Developing roller, process cartridge, electrophotographic image forming apparatus, and electrophotographic image forming system
By using an aluminum alloy with a silicon content of over 0.6% in the developing sleeve to reduce eddy currents, the developing roller addresses image defects and ensures high-quality, low-temperature fixing in electrophotographic image forming devices.
Patent Information
- Application Number
- JP2023066096
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Existing developing rollers in electrophotographic image forming devices experience image defects such as white streaks and black spots due to heat generation from eddy currents, which are exacerbated by increased printing speeds and compact machine designs, leading to issues with toner aggregation and clogging.
Incorporating an aluminum alloy with a silicon content of more than 0.6% by mass into the developing sleeve to increase resistance and suppress eddy current generation, thereby reducing heat and preventing toner scattering and low concentration.
The solution effectively suppresses image defects like white streaks and black spots, enabling high-quality, low-temperature fixing over extended periods by maintaining magnetic flux density and proper toner charging.
Smart Images

Figure 2024152113000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a developing roller, a process cartridge, an electrophotographic image forming apparatus, and an electrophotographic image forming system. [Background technology]
[0002] In recent years, there has been a demand for technology that reduces the thermal energy required for fixing a toner image in order to meet the needs of higher print speeds, a wider range of paper types, and reduced environmental impact.
[0003] In order to reduce the thermal energy required for fixing a toner image, it is necessary to improve the low-temperature fixing property of the toner.
[0004] For example, Patent Document 1 discloses a technique that addresses the issue of low-temperature fixability.
[0005] One of the means for improving the low-temperature fixing property of a toner is to cause the molecular motion of a resin to start at a lower temperature, and for this purpose, a resin having a low glass transition temperature is used.
[0006] However, it was found that using a resin with a low glass transition temperature causes the developer and toner to aggregate on the sleeve, which can lead to clogging of the doctor blade when a thin layer is formed, resulting in poor image quality, such as white streaks caused by clogging of the doctor blade and black spots caused by coarse toner particles being transferred.
[0007] In particular, with the recent trend toward higher printing speeds and more compact machines, it has become apparent that this image defect becomes more pronounced. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2017-156544 A Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is a developing roller, a process cartridge, an electrophotographic image forming apparatus, and an electrophotographic image forming system that suppress image defects such as white streaks and black spots and enable low-temperature fixing of high-quality images over a long period of time. The purpose of this project is to provide [Means for solving the problem]
[0010] In order to solve the above problems, the inventors investigated the causes of the above problems and found that the above problems can be solved by having a developing sleeve of a developing roller with an aluminum alloy containing more than 0.6 mass % silicon, thereby arriving at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0011] 1. A developing roller for an electrophotographic image forming apparatus that transports a developer, the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, The developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon. A developing roller characterized by:
[0012] 2. The silicon content of the aluminum alloy is greater than 0.8% by mass. 2. The developing roller according to claim 1,
[0013] 3. The lithium content of the aluminum alloy is less than 1% by mass. 2. The developing roller according to claim 1,
[0014] 4. A process cartridge including a developing roller for transporting a developer, the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, The developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon. A process cartridge comprising:
[0015] 5. An electrophotographic image forming apparatus including a developing roller for transporting a developer, the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, 13. An electrophotographic image forming apparatus, wherein the developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon.
[0016] 6. An electrophotographic image forming system having a device including a developing roller for transporting a developer and a toner for developing an electrostatic latent image, the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, the developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon; and The glass transition temperature of the toner for developing an electrostatic latent image is within a range of 0 to 40° C. 23. An electrophotographic imaging system comprising:
[0017] 7. The binder resin contained in the toner particles contained in the electrostatic latent image developing toner contains polyester in the range of 50 to 95% by mass. 7. The electrophotographic imaging system according to claim 6, Effect of the Invention
[0018] By the above-mentioned means of the present invention, it is possible to provide a developing roller, a process cartridge, an electrophotographic image forming apparatus, and an electrophotographic image forming system which are capable of suppressing image defects such as white streaks and black spots and enabling low-temperature fixing of high-quality images over a long period of time. Although the mechanism by which the effects of the present invention are expressed or the mechanism of action has not been clarified, it is speculated as follows.
[0019] The developing roller of the present invention comprises a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and is characterized in that the developing sleeve comprises an aluminum alloy containing more than 0.6 mass % silicon.
[0020] When a developing roller with a magnetic flux generating member inserted inside the developing sleeve is used, heat is generated on the developing sleeve due to eddy currents. This heat causes the toner and carrier to thermally fuse and begin to aggregate, and the aggregates clog the doctor blade, resulting in the appearance of white streaks. In addition, the aggregates of toner particles cause image defects such as black spots, and worsen the graininess (GI value) of halftones.
[0021] In particular, in response to recent demands for faster printing speeds and more compact machines, the developing sleeve is required to have a small diameter. In addition, the developing sleeve is also required to rotate at high speed while maintaining a high magnetic flux density.
[0022] This causes the developing sleeve to generate more heat due to eddy currents, which in turn makes image defects such as white streaks and black spots more noticeable.
[0023] In the present invention, the aluminum alloy of the developing sleeve contains more than 0.6% by mass of silicon, which increases the surface resistance of the developing sleeve, thereby suppressing the generation of eddy currents and heat generation even if the developing sleeve has a member that generates magnetic flux inside, thereby suppressing the generation of image defects such as white streaks and black spots.
[0024] Furthermore, the aluminum alloy of the developing sleeve contains more than 0.6% by mass of silicon, which prevents toner scattering and low density. Since silicon has almost the same chargeability as aluminum, it does not interfere with the chargeability between the toner carrier. This is presumably what prevents toner scattering and low density due to excessive charging.
[0025] In other words, the toner should be charged correctly using only the toner and carrier, but if an element with a significantly different charging property from aluminum, such as lithium, is contained, it tends to disturb the charging between the toner and carrier, widening the charge distribution of the toner.
[0026] The components that spread to the low charge side are scattered because the carrier cannot hold the toner due to the centrifugal force of the sleeve, while the components that spread to the high charge side electrostatically stick to the positive surfaces of the carrier and sleeve, preventing proper development, which means a reduced amount of development and lower density.
[0027] It is presumed that silicon according to the present invention, having a chargeability similar to that of aluminum, suppresses the spread of the charge distribution as described above, and also prevents toner scattering and low density due to excessive charging. [Brief description of the drawings]
[0028] [Figure 1] External view of a developing roller equipped with a developing sleeve [Diagram 2] A cross-sectional view of the developing sleeve in Figure 1 as seen from the axial direction and perpendicular direction. [Diagram 3] Cross-sectional view of the developing sleeve in FIG. 1 as seen from the axial direction [Figure 4] An explanatory diagram showing the magnetic pattern of a magnet roller [Diagram 5] FIG. 1 is a perspective view of a main part of a developing roller for explaining the principle of generation of eddy currents; [Figure 6] Vertical section of developing sleeve with grooves [Figure 7] FIG. 1 is a schematic diagram showing an example of an image forming apparatus according to the present invention; [Figure 8] Schematic diagram of the charge amount measuring device DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The developing roller of the present invention is a developing roller for an electrophotographic image forming apparatus that transports a developer, and is characterized in that the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % of silicon. This characteristic is a technical characteristic common to or corresponding to each of the following embodiments (modes).
[0030] In an embodiment of the present invention, it is preferable that the silicon content of the aluminum alloy is more than 0.8 mass %, from the viewpoint of increasing the resistance value of the developing sleeve surface and suppressing the generation of eddy currents, thereby enhancing the effect of suppressing heat generation.
[0031] It is preferable that the lithium content of the aluminum alloy is less than 1% by mass from the viewpoints of reducing the influence of the positive charging property of lithium and suppressing the heat generation effect of the developing sleeve.
[0032] The process cartridge of the present invention is a process cartridge including a developing roller that transports a developer, the developing roller having a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon.
[0033] The electrophotographic image forming apparatus of the present invention is an electrophotographic image forming apparatus including a developing roller that transports a developer, the developing roller having a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon.
[0034] The electrophotographic image forming system of the present invention is an electrophotographic image forming system equipped with a device including a developing roller that transports a developer and a toner for developing an electrostatic latent image, characterized in that the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon, and the glass transition temperature of the toner for developing an electrostatic latent image is within the range of 0 to 40°C.
[0035] In the electrophotographic image forming system of the present invention, it is preferable that the binder resin contained in the toner particles contained in the electrostatic latent image developing toner contains polyester in the range of 50 to 95 mass %, from the viewpoints of low-temperature fixing property, negative chargeability, and appropriate hydrophilicity of the toner.
[0036] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as the lower limit and upper limit.
[0037] 1.Developing roller The developing roller of the present invention is a developing roller for an electrophotographic image forming apparatus that transports a developer, the developing roller having a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon.
[0038] (1.1) Structure The developing roller of the present invention includes a developing sleeve. The "developing sleeve" is a means having a function of carrying a moderately charged developer and supplying the developer to a photoconductor on which an electrostatic latent image is formed. It is also a part of a developing roller included in a developing device included in an electrophotographic image forming apparatus, for example, and the developing roller is composed of a developing sleeve, a flange, a shaft, and a member that generates a magnetic flux.
[0039] Incidentally, since the above-mentioned "member generating magnetic flux" is generally used as a magnet roller, in the following description, the "member generating magnetic flux" will be simply referred to as a "magnet roller."
[0040] Fig. 1 is an external view of a developing roller equipped with a developing sleeve, Fig. 2 is a cross-sectional view of the developing sleeve of Fig. 1 as viewed from a direction perpendicular to the axial direction, and Fig. 3 is a cross-sectional view of the developing sleeve of Fig. 1 as viewed from the axial direction.
[0041] The developing sleeve is rotatable and cylindrical, and serves to carry and transport the developer on its surface.
[0042] As shown in FIG. 1, a substantially cylindrical developing sleeve 11 is provided, and a first flange 18 and a second flange 19 are fixedly attached to both ends of the developing sleeve 11.
[0043] The first flange 18 is formed with a shaft portion 18a extending in a protruding manner to the left, and a recess 18b is formed in the approximate center of the right part of the first flange 18. A through hole is formed in the approximate center of the second flange 19, and a shaft 16 is provided coaxially with the developing sleeve 11 in the center of the developing sleeve 11.
[0044] The left end of shaft 16 is rotatably supported by first flange 18 via bearing 17 mounted in recess 18b. The right end of shaft 16 is rotatably supported by second flange 19 via bearing 17 mounted in a through hole, and extends rightward through the through hole.
[0045] A substantially cylindrical magnet roller 12 is fixed to the shaft 16 in the developing sleeve 11 in a non-contact manner with the inner peripheral surface of the developing sleeve 11 (see FIG. 3). The magnet roller 12 fixed to the shaft 16 is supported via a first flange 18 and a second flange 19 to be rotatable relative to the developing sleeve 11.
[0046] The magnet roller 12 is a typical structure made of a resin magnet or a sintered magnet with multiple magnetic poles formed in the circumferential direction of the outer periphery. For example, magnets with S and N poles alternately arranged in the circumferential direction of the outer periphery, or magnets with S and N poles arranged to form a predetermined magnetic pattern are used.
[0047] (1.2) Eddy current Aluminum alloy is a conductive material with a relatively small electrical resistance, and when the developing sleeve is rotated relative to the magnet roller, the developing sleeve crosses the magnetic field lines generated by the magnet roller, which causes electromagnetic induction and generates eddy currents around the surface of the developing sleeve.
[0048] FIG. 4 is an explanatory diagram showing the magnetic pattern of the magnet roller, and FIG. 5 is a perspective view of the main part of the developing roller for explaining the principle of generation of eddy currents.
[0049] 4 and 5, the magnet roller 12 has magnetic S poles and N poles alternately formed in the circumferential direction. Magnetic field lines G from the adjacent N pole reach any S pole of the magnet roller 12 by penetrating the developing sleeve 11 made of an aluminum alloy.
[0050] In this state, when the developing sleeve 11 rotates in the direction of the arrow Y, an eddy current indicated as Ia is generated in the front part of the rotation direction to compensate for the decrease in the magnetic field lines G. At the same time, an eddy current indicated as Ib is generated in the rear part of the rotation direction to compensate for the increase in the magnetic field lines G. This eddy current generates a force in the direction of the arrow X in FIG. 5, which is the opposite direction to the rotation direction of the developing sleeve 11. Note that if the current density of the eddy current is high, the generation of heat increases, causing image defects.
[0051] (1.3) Aluminum alloys The developing sleeve of the developing roller of the present invention contains an aluminum alloy. The developing sleeve preferably contains an aluminum alloy as a main component, and the aluminum alloy content is preferably 80% by mass or more. More preferably, the aluminum alloy content is 100% by mass.
[0052] (Silicon content) The aluminum alloy of the developing sleeve of the developing roller of the present invention contains more than 0.6% by mass of silicon when the total amount of the aluminum alloy is taken as 100% by mass.
[0053] When the silicon content in the aluminum alloy is low, the resistance value of the surface of the developing sleeve is low and eddy current increases, so that the heat generation amount of the developing sleeve increases. In particular, when the silicon content is 0.6 mass % or less, the resistance value of the surface of the developing sleeve is too low and the heat generation amount of the developing sleeve is too large.
[0054] When the aluminum alloy has a high silicon content, the resistance value of the surface of the developing sleeve increases, and the generation of eddy currents can be suppressed, so that the amount of heat generated on the surface of the developing sleeve decreases. Therefore, the higher the resistance value, the more the heat generation of the developing sleeve can be suppressed.
[0055] The silicon content of the aluminum alloy is preferably more than 0.8% by mass, because it increases the resistance of the developing sleeve surface and suppresses the generation of eddy currents, thereby enhancing the effect of suppressing heat generation. However, if the silicon content is too high, although the eddy currents can be suppressed, heat generation begins to occur due to the voltage during toner image formation. Therefore, it is preferable that the silicon content is less than 30.0% by mass, from the viewpoint of suppressing the amount of heat generation.
[0056] (Lithium content) The lithium in the aluminum alloy exerts an effect of suppressing heat generation on the surface of the developing sleeve with increasing content, but on the other hand, unlike silicon, lithium has a strong positive chargeability with respect to aluminum, so that excessive addition of lithium in the aluminum alloy tends to affect the chargeability of the toner and broaden the charge amount distribution of the toner. Therefore, it is preferable that the lithium content of the aluminum alloy is less than 1 mass % from the viewpoint of suppressing the heat generation effect of the developing sleeve while suppressing the influence of the chargeability of lithium.
[0057] (Method of measuring element content in aluminum alloy) The elements and their contents in aluminum alloys can be measured by inductively coupled plasma atomic emission spectrometry. Inductively coupled plasma atomic emission spectrometry is a method in which a solution sample in which metals are dissolved in acid or alkali is sprayed into Ar plasma, the excited light is separated into different wavelengths, and the type and content of elements are quantified from the light intensity. With this method, there is a linear relationship between light intensity and content from trace to high concentrations, and each element can be analyzed simultaneously.
[0058] The measurement equipment for the high-frequency inductively coupled plasma optical emission spectrometry is the ULTIMA2000. (manufactured by Horiba Ltd.) can be used.
[0059] The silicon and lithium contents of the developing sleeve according to the present invention are values measured after cutting the alloy of the developing sleeve into chips, dissolving them in acid, and then measuring the values.
[0060] (1.4) Surface Fig. 6 is a vertical cross section of a developing sleeve when grooves are formed. Thus, grooves 20 are provided on the outer peripheral surface of the developing sleeve of the developing roller of the present invention in order to improve the transport ability of the developer. That is, as shown in Fig. 3, a cutting process is performed on the outer peripheral surface of the developing sleeve 11 to form a plurality of grooves 20 at predetermined circumferential intervals over substantially the entire length of the developing sleeve 11, and the developer is carried by these grooves 20 as if scooping it up. Note that the depth of the grooves 20 is preferably 0.5 mm or less, taking into consideration the thickness of the developing sleeve 11 and the transportability of the developer.
[0061] (Sandblasting) Alternatively, the outer peripheral surface of the developing sleeve 11 may be sandblasted to form a plurality of projections and recesses on the outer peripheral surface of the developing sleeve 11, and the developer may be supported on the recesses of the plurality of projections and recesses. By forming projections and recesses on the surface of the developing sleeve through sandblasting, the roughness of the outer peripheral surface can be appropriately maintained, and excellent transportability can be ensured.
[0062] As a means for imparting roughness to the surface of the developing sleeve, it is more preferable to impart surface roughness by sandblasting, which has been conventionally used. When silicon is contained, the silicon is scraped differently on the surface of the developing sleeve during sandblasting treatment between the part containing silicon and the part not containing silicon, so that an appropriate surface roughness can be imparted.
[0063] Sandblasting is a process in which a blasting material is projected onto the surface of a developing sleeve to indent the surface with the blasting material, thereby forming an uneven shape. More specifically, examples of sandblasting include air blasting, wet sandblasting, and shot blasting.
[0064] Materials applicable to sandblasting are not particularly limited, and known materials can be used as appropriate. Specific examples include glass beads, alumina particles, silica particles, titania particles, and zirconia particles. Organic fine particles can also be used, such as melamine resin particles, benzoguanamine resin particles, and crosslinked acrylic resin particles. In addition, from the viewpoint of imparting an impact force that dents the elastic layer but does not tear the surface of the outer layer, spherical glass beads and alumina beads are particularly preferred. These materials may be used alone or in combination of two or more.
[0065] The volume average particle size of the above material varies depending on the size of the desired irregularities on the surface of the developing sleeve, but is preferably within the range of 3 to 200 μm, more preferably within the range of 10 to 100 μm, and even more preferably within the range of 20 to 80 μm.
[0066] 2. Electrophotographic image forming apparatus The electrophotographic image forming apparatus of the present invention is an electrophotographic image forming apparatus including a developing roller that transports a developer, the developing roller having a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon.
[0067] The image forming apparatus includes, for example, a charging unit (first charging unit), an exposure unit, a developing unit, a transfer unit, and a cleaning unit. The image forming apparatus may also include a second charging unit between the transfer unit and the cleaning unit.
[0068] FIG. 7 is a schematic diagram showing an example of the image forming apparatus of the present invention.
[0069] The image forming apparatus 100 is called a tandem type color image forming apparatus, and includes four process cartridges 10Y, 10M, 10C, and 10Bk, an intermediate transfer unit 7, a paper feeding means 21, a fixing means 24, etc. An original image reading device SC is disposed on the upper portion of the main body A of the image forming apparatus.
[0070] (2.1) Process cartridge The process cartridge according to the present invention is a process cartridge including a developing roller that transports developer, the developing roller having a developing sleeve and a member that generates magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon.
[0071] The process cartridge 10Y, which forms a yellow image, has a first charging means 2Y, an exposure means 3Y, a developing means 4Y, a primary transfer roller 5Y, a second charging means 9Y, and a cleaning means 6Y, which are arranged in sequence around the drum-shaped photoreceptor 1Y in the direction of rotation of the photoreceptor 1Y.
[0072] The process cartridge 10M, which forms a magenta image, has a first charging means 2M, an exposure means 3M, a developing means 4M, a primary transfer roller 5M, a second charging means 9M and a cleaning means 6M, which are arranged in sequence around the drum-shaped photosensitive member 1M in the direction of rotation of the photosensitive member 1M.
[0073] The process cartridge 10C, which forms a cyan image, has a first charging means 2C, an exposure means 3C, a developing means 4C, a primary transfer roller 5C, a second charging means 9C and a cleaning means 6C, which are arranged in sequence around the drum-shaped photosensitive member 1C in the direction of rotation of the photosensitive member 1C.
[0074] The process cartridge 10Bk, which forms a black image, has a first charging means 2Bk, an exposure means 3Bk, a developing means 4Bk, a primary transfer roller 5Bk, a second charging means 9Bk and a cleaning means 6Bk, which are arranged in sequence around the drum-shaped photosensitive member 1Bk along the direction of rotation of the photosensitive member 1Bk.
[0075] The process cartridges 10Y, 10M, 10C, and 10Bk are configured similarly, except that the colors of the toner images formed on the photoconductors 1Y, 1M, 1C, and 1Bk are different. Therefore, the process cartridge 10Y will be described in detail as an example, and the description of the process cartridges 10M, 10C, and 10Bk will be omitted.
[0076] The process cartridge 10Y has a first charging means 2Y, an exposure means 3Y, a developing means 4Y, a primary transfer roller 5Y, a second charging means 9Y, and a cleaning means 6Y arranged around a photoconductor 1Y which is an image forming body, and forms a yellow (Y) toner image on the photoconductor 1Y. The process cartridge 10Y may be detachable from the image forming apparatus 100.
[0077] In this embodiment, in the process cartridge 10Y, at least the photoconductor 1Y, the first charging means 2Y, the developing means 4Y, the second charging means 9Y and the cleaning means 6Y are integrally provided.
[0078] (First charging means) The first charging means 2Y is a means for applying a uniform potential to the photoconductor 1Y, and for example, a corona discharge type charger is used.
[0079] (Exposure means) The exposure means 3Y is a means for exposing the photoconductor 1Y, to which a uniform potential has been applied by the first charging means 2Y, based on an image signal (yellow) to form an electrostatic latent image corresponding to the yellow image. As the exposure means 3Y, for example, one consisting of LEDs in which light emitting elements are arranged in an array in the axial direction of the photoconductor 1Y and an imaging element, or a laser optical system is used.
[0080] (Developing means) The developing means 4Y is composed of, for example, a developing sleeve incorporating a magnet and rotating while holding a developer, and a voltage application device for applying a DC and / or AC bias voltage between the photoreceptor 1Y and this developing sleeve.
[0081] (Primary transfer roller) The primary transfer roller 5Y is a means for transferring the toner image formed on the photoconductor 1Y to an endless belt-like intermediate transfer body 70. The primary transfer roller 5Y is disposed in contact with the intermediate transfer body 70.
[0082] (Second charging means) The second charging means 9Y is a discharging means for charging (discharging) the surface of the photoreceptor 1Y after the toner image is transferred to the intermediate transfer body 70, and is provided as a pre-cleaning member. As the second charging means 9Y, for example, a corona discharge type charger is used.
[0083] (Cleaning Means) The cleaning means 6Y is composed of a cleaning blade and a brush roller provided upstream of the cleaning blade.
[0084] (2.2) Intermediate transfer unit The intermediate transfer unit 7 has an endless belt-like intermediate transfer body 70 wound around a plurality of rollers 71, 72, 73, and 74 and rotatably supported as a semiconductive endless belt-like second image carrier.
[0085] The intermediate transfer unit 7 is provided with a cleaning means 6b for removing toner from the intermediate transfer unit 70. The process cartridges 10Y, 10M, 10C, and 10Bk and the intermediate transfer unit 7 form a housing 8. The housing 8 is configured so as to be removable from the main body A of the image forming apparatus via support rails 82L and 82R.
[0086] The image forming apparatus 100 includes a secondary transfer roller 5b that transfers a color image formed on the intermediate transfer body 70 onto a transfer material P.
[0087] (2.3) Paper feeding means The paper feed means 21 is a means for supplying the transfer material P to the secondary transfer roller 5b. The paper feed means 21 includes a paper feed cassette 20 that stores the transfer material P, a plurality of intermediate rollers 22A, 22B, 22C, and 22D for transporting the transfer material P to the secondary transfer roller 5b, and a registration roller 23.
[0088] (2.4) Fixing means The fixing means 24 is a means for fixing the color image transferred to the transfer material P onto the transfer material P, and may be, for example, a heat roller fixing type consisting of a heating roller having an internal heat source and a pressure roller that is placed in pressure contact with the heating roller so as to form a fixing nip portion.
[0089] The image forming apparatus 100 has a paper discharge tray 26 for taking out the transfer material P on which an image has been formed, and is provided with paper discharge rollers 25 downstream of the fixing means 24 for transporting the transfer material P after the fixing process to the paper discharge tray 26. Note that, although the image forming apparatus 100 is a color laser printer in the above-described embodiment, it may also be a monochrome laser printer, copier, multifunction machine, etc.
[0090] 3. Electrophotographic Image Forming System The electrophotographic image forming system of the present invention is an electrophotographic image forming system equipped with a device including a developing roller that transports a developer and a toner for developing an electrostatic latent image, characterized in that the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon, and the glass transition temperature of the toner for developing an electrostatic latent image is within the range of 0 to 40°C.
[0091] The "electrophotographic image forming system" of the present invention refers to an assembly that is composed of devices or apparatuses having predetermined functions as means elements required for each step of image formation, toner for developing electrostatic latent images, etc., and that performs at least the function of image formation as a whole. Each means element may be disposed separately in different locations, or may be disposed together in a certain space as one device to be integrated into a system device.
[0092] That is, the device used in the present invention is not particularly limited as long as it satisfies the above conditions, and it is not necessarily required to use an electrophotographic image forming device exclusively for the toner for developing electrostatic latent images that satisfies the specific conditions of the present invention. In addition, it is also preferable that the image forming system of the present invention is provided with a means for recording and storing the recording and copying information as electronic data, and a means for wirelessly transmitting the electronic data.
[0093] For example, it is also preferable that the toner has a wireless interface for transmitting and receiving data to and from an information processing device by wireless communication such as Bluetooth (registered trademark), Wi-Fi (registered trademark), etc. The electrophotographic image forming system of the present invention can use the same developing sleeve as described above, and can be used in combination with a toner for developing electrostatic latent images having a glass transition temperature in the range of 0 to 40°C.
[0094] (3.1) Toner for developing electrostatic latent images (3.1.1) Toner base particles The toner base particles constituting the electrostatic latent image developing toner according to the present invention contain, for example, a binder resin, and may also contain a colorant, a release agent and other additives as required.
[0095] In the present invention, "toner particles" refers to toner base particles to which an external additive has been added, and an aggregate of toner particles is called "toner". Toner base particles can generally be used as toner particles as they are, but in the present invention, toner base particles to which an external additive has been added are used as toner particles. In the following description, when there is no particular need to distinguish between toner base particles and toner particles, they are also simply referred to as "toner particles".
[0096] Hereinafter, the glass transition temperature will be described, and then each of the constituent materials of the toner base particles according to the present invention will be described in detail.
[0097] (3.1.2) Glass transition temperature of toner for developing electrostatic latent images The "glass transition temperature" is defined as the temperature at which the free volume of molecules increases and micro-Brownian motion begins as the temperature of the resin components constituting the toner changes from a low temperature to a high temperature.
[0098] In order to improve the low-temperature fixing ability of a toner, it is necessary to design the toner so as to lower the glass transition temperature, which allows molecular motion at a lower temperature. It is also preferable to devise further measures to improve heat-resistant storage properties and suppress fusion of toner particles.
[0099] For example, it is preferable to change the composition of the surface and the inside of the toner to form a core-shell toner composition using a resin with a low glass transition temperature in the core and a resin with a high glass transition temperature in the shell. It is also preferable to harden only the surface by using a means for fixing inorganic fine particles as an external additive in the part corresponding to the shell, thereby ensuring heat-resistant storage properties and resistance to fusion and aggregation.
[0100] The glass transition temperature of the toner for developing electrostatic latent images according to the present invention is within the range of 0 to 40° C. If the glass transition temperature is lower than 0° C., the toner is too soft, causing image defects, and if it is higher than 40° C., the low-temperature fixing property of the toner deteriorates. Note that the core resin constituting the toner according to the present invention needs to be designed to have a lower glass transition temperature, and the shell resin needs to be designed to have a higher glass transition temperature.
[0101] (Control Method) The glass transition temperature of a resin is controlled by changing the composition and molecular weight of the molecules that make up the resin, the component ratio of different resins, and the like. (Measurement method) The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC). More specifically, it is determined from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K-7121-1987 "Method for measuring transition temperature of plastics."
[0102] (3.1.3) Binder resin The toner particles contained in the toner for developing electrostatic latent images preferably contain polyester as a binder resin. Polyester is a dehydration condensation reaction system, and is particularly compatible with paper and has high internal cohesion. Therefore, since the folding fixability after fixing is particularly high, it is possible to achieve even lower temperature fixation.
[0103] The "folding fixability" refers to the property that indicates the ease with which the toner layer peels off at the fold line when, for example, a black band-like toner image is formed with toner using paper as a recording medium, the paper is folded in half, and then unfolded again after fixing. If the "folding fixability" is high, the toner layer will not be destroyed as described above, and good fixability can be achieved.
[0104] In addition, polyester has both a high negative chargeability and moderate hydrophilicity compared to other resins. Therefore, even if there are parts with high resistance values partially on the surface of a developing sleeve containing more than 0.6% by mass of silicon, the charge stability inside the toner is further improved. As a result, image quality is also stabilized at a higher level.
[0105] The above-mentioned effects can be confirmed when the polyester content is 60% by mass or more. If the polyester content exceeds 98% by mass, for example, the remaining 2% by mass is considered to be an external additive, the amount of external additive is relatively small, which causes problems with heat-resistant storage and image quality and makes the film unusable.
[0106] In view of the above, in the electrophotographic image forming system of the present invention, it is preferable that the binder resin contained in the toner particles contained in the electrostatic latent image developing toner contains polyester in the range of 50 to 95 mass % from the viewpoints of low-temperature fixing property, negative chargeability, and appropriate hydrophilicity of the toner.
[0107] The toner particles may contain a non-crystalline polyester and a crystalline polyester as a binder resin. Either a crystalline resin or a non-crystalline resin may be used, but it is the crystalline resin that provides sharp melting properties.
[0108] The term "crystalline" refers to a state in which a clear endothermic peak is present rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC), and specifically refers to a state in which the half-width of the endothermic peak is within 10°C when measured at a heating rate of 10 (°C / min).
[0109] On the other hand, "amorphous" refers to a half-width exceeding 10°C, a stepwise change in endothermic heat, or no clear endothermic peak.
[0110] (amorphous polyester) The content of the amorphous polyester is preferably within the range of 50 to 88% by mass, more preferably within the range of 60 to 80% by mass, based on the total amount of the binder resin. Examples of the amorphous polyester include condensation polymers of polyvalent carboxylic acids and polyhydric alcohols. The amorphous polyester may be a commercially available product or a synthesized product.
[0111] [Polycarboxylic acid] Examples of the polycarboxylic acid include aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, aromatic dicarboxylic acids, their anhydrides, and their lower alkyl esters. Among these, the polycarboxylic acid is preferably, for example, an aromatic dicarboxylic acid.
[0112] Examples of the aliphatic dicarboxylic acid include oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, and sebacic acid.
[0113] The alicyclic dicarboxylic acid may, for example, be cyclohexanedicarboxylic acid.
[0114] Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, phthalic acid, and naphthalenedicarboxylic acid.
[0115] The lower alkyl esters include, for example, those having 1 to 5 carbon atoms.
[0116] The polyvalent carboxylic acid may be used in combination with a dicarboxylic acid and a trivalent or higher carboxylic acid having a crosslinked or branched structure. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, their anhydrides, and their lower alkyl esters. Examples of the lower alkyl ester include those having 1 to 5 carbon atoms. The polyvalent carboxylic acid may be used alone or in combination of two or more kinds.
[0117] [Polyhydric alcohol] Examples of the polyhydric alcohol include aliphatic diols, alicyclic diols, and aromatic diols. Among these, aromatic diols and alicyclic diols are preferred, and aromatic diols are more preferred.
[0118] Examples of the aliphatic diol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, and neopentyl glycol.
[0119] Examples of the alicyclic diol include cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, and the like.
[0120] Examples of the aromatic diol include an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A.
[0121] As the polyhydric alcohol, a trihydric or higher polyhydric alcohol having a crosslinked or branched structure may be used in combination with the diol. Examples of the trihydric or higher polyhydric alcohol include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohol may be used alone or in combination of two or more kinds.
[0122] [Glass transition temperature of amorphous polyester] The amorphous polyester may be used inside the toner or as a shell material on the surface of the toner. When used inside the toner, the glass transition temperature (Tg) is preferably in the range of -5 to 40°C, more preferably in the range of 0 to 30°C. When used as a shell material, the glass transition temperature (Tg) of the amorphous polyester is preferably in the range of 50 to 80°C, more preferably in the range of 50 to 65°C.
[0123] The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC). More specifically, it is determined from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K-7121-1987 "Method for measuring transition temperature of plastics."
[0124] 〔others〕 In this embodiment, two or more kinds of amorphous polyesters may be used in combination. In this case, the absolute value of the difference in SP value between the amorphous polyester showing the largest SP value and the amorphous polyester showing the smallest SP value is preferably 0.25 or less, more preferably within the range of 0.01 to 0.25, and even more preferably within the range of 0.10 to 0.25. If the absolute value of the difference in SP value is 0.25 or less, it is possible to adjust the compatibility between the crystalline polyester and the amorphous polyester to an appropriate range.
[0125] The amorphous polyester can be obtained by a known manufacturing method, for example, by setting the polymerization temperature within a range of 180 to 230° C., reducing the pressure in the reaction system as necessary, and removing water and alcohol generated during condensation.
[0126] If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present in the copolymerization reaction, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.
[0127] In the present embodiment, the SP value of the amorphous polyester can be adjusted by selecting the types of polyvalent carboxylic acid and polyhydric alcohol constituting the amorphous polyester so that the SP value of the amorphous polyester is a desired value.
[0128] (Crystalline polyester) The crystalline polyester may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester may be a commercially available product or a synthesized product. Here, the crystalline polyester is preferably a polycondensate using a polymerizable monomer having a linear aliphatic group rather than a polymerizable monomer having an aromatic group, since it easily forms a crystal structure.
[0129] [Polycarboxylic acid] Examples of the polycarboxylic acid include aliphatic dicarboxylic acids, aromatic dicarboxylic acids, anhydrides thereof, and lower alkyl esters thereof.
[0130] Examples of the aliphatic dicarboxylic acid include oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid.
[0131] Examples of aromatic dicarboxylic acids include dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalene-2,6-dicarboxylic acid.
[0132] The lower alkyl esters include, for example, those having 1 to 5 carbon atoms.
[0133] The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid.
[0134] Examples of the trivalent carboxylic acid include aromatic carboxylic acids, their anhydrides, and their lower alkyl esters.
[0135] Examples of aromatic carboxylic acids include 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, and 1,2,4-naphthalenetricarboxylic acid.
[0136] The lower alkyl esters include, for example, those having 1 to 5 carbon atoms.
[0137] As the polycarboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polycarboxylic acid may be used alone or in combination of two or more kinds.
[0138] [Polyhydric alcohol] The polyhydric alcohol includes, for example, an aliphatic diol, and for example, a straight-chain aliphatic diol having a main chain portion with 7 to 20 carbon atoms is preferable.
[0139] Examples of the aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred.
[0140] The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0141] The polyhydric alcohol may be used alone or in combination of two or more kinds. Here, the polyhydric alcohol may have an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.
[0142] [Melting temperature of crystalline polyester] The melting temperature of the crystalline polyester is preferably within the range of 55 to 80°C, more preferably within the range of 55 to 78°C, and even more preferably within the range of 55 to 76°C. If the melting temperature of the crystalline polyester is 72°C or higher, the thermal storage property is further improved. If the melting temperature of the crystalline polyester is 80°C or lower, the low-temperature fixation is further improved. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) by the "melting peak temperature" described in the method for determining the melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics".
[0143] 〔others〕 The crystalline polyester can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester. In the present embodiment, the SP value of the crystalline polyester can be adjusted by selecting the types of polyvalent carboxylic acid and polyhydric alcohol constituting the crystalline polyester so that the SP value of the crystalline polyester is a desired value.
[0144] (Other resins) In the present embodiment, resins other than the amorphous polyester and crystalline polyester may be used as the binder resin. Examples of other binder resins include vinyl resins made of homopolymers of monomers such as styrenes, (meth)acrylic acid esters, ethylenically unsaturated nitriles, vinyl ethers, vinyl ketones, and olefins, or copolymers of two or more of these monomers.
[0145] Examples of styrenes include styrene, parachlorostyrene, and α-methylstyrene.
[0146] Examples of (meth)acrylic acid esters include methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, and 2-ethylhexyl methacrylate.
[0147] Examples of the ethylenically unsaturated nitriles include acrylonitrile and methacrylonitrile.
[0148] Examples of the vinyl ethers include vinyl methyl ether and vinyl isobutyl ether.
[0149] Examples of vinyl ketones include vinyl methyl ketone, vinyl ethyl ketone, and vinyl isopropenyl ketone.
[0150] Examples of the olefins include ethylene, propylene, and butadiene.
[0151] Examples of other binder resins include non-vinyl resins such as epoxy resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosins. In addition, mixtures of the above-mentioned resins with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the presence of these resins, etc. These other binder resins may be used alone or in combination of two or more.
[0152] In the present embodiment, a styrene-(meth)acrylic copolymer resin may be used as the other binder resin. By using a styrene-(meth)acrylic copolymer resin as the other binder resin, fixing characteristics such as hot offset and heat storage properties are further improved.
[0153] When a styrene-(meth)acrylic copolymer resin is used as another binder resin, the proportion of the styrene-(meth)acrylic copolymer resin in the binder resin is preferably within a range of 5 to 25% by mass, more preferably within a range of 5 to 20% by mass, and even more preferably within a range of 10 to 15% by mass.
[0154] If the proportion of the styrene-(meth)acrylic copolymer resin in the binder resin is 5% by mass or more, the fixing properties such as hot offset and the thermal storage properties are further improved. If the proportion of the styrene-(meth)acrylic copolymer resin in the binder resin is 25% by mass or less, the low-temperature fixing properties are further improved.
[0155] In this embodiment, (meth)acrylic means acrylic or methacrylic.
[0156] The styrene-(meth)acrylic copolymer resin can be synthesized by various polymerization methods, such as solution polymerization, precipitation polymerization, suspension polymerization, precipitation polymerization, bulk polymerization, and emulsion polymerization. The polymerization reaction can be carried out by known operations such as batch, semi-continuous, and continuous.
[0157] (3.1.4) Colorants The colorant may be, for example, a pigment or a dye.
[0158] Examples of pigments include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, chalco oil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate.
[0159] Examples of dyes include acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes.
[0160] The colorant may be used alone or in combination of two or more. The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of colorants may be used in combination. The content of the colorant is preferably within a range of 1 to 30% by mass, more preferably within a range of 3 to 15% by mass, based on the total mass of the toner particles.
[0161] (3.1.5) Release agents Examples of the release agent include, but are not limited to, hydrocarbon waxes, natural waxes, synthetic or mineral / petroleum waxes, and ester waxes.
[0162] Examples of natural waxes include carnauba wax, rice wax, and candelilla wax.
[0163] An example of the synthetic or mineral / petroleum wax is montan wax.
[0164] Examples of the ester wax include fatty acid esters and montanic acid esters.
[0165] The melting temperature of the release agent is preferably within a range of 50 to 110° C., and more preferably within a range of 60 to 100° C. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the “melting peak temperature” described in the method for determining the melting temperature in JIS K-7121-1987 “Method for measuring transition temperature of plastics.”
[0166] The content of the release agent is, for example, preferably within a range of 1 to 20% by mass, and more preferably within a range of 5 to 15% by mass, based on the total mass of the toner particles.
[0167] (3.1.6) Other additives Examples of other additives include well-known additives such as magnetic materials, charge control agents, and inorganic powders, and these additives are contained in the toner particles as internal additives.
[0168] (magnetic material) Magnetic materials include iron oxides such as magnetite, hematite, and ferrite, metals such as iron, cobalt, and nickel, and alloys of these metals with metals such as aluminum, cobalt, copper, lead, magnesium, tin, zinc, antimony, bismuth, calcium, manganese, titanium, tungsten, and vanadium, and mixtures thereof.
[0169] The shape of the magnetic material may be polyhedral, octahedral, hexahedral, spherical, needle-like, scale-like, etc., and those with less anisotropy such as polyhedral, octahedral, hexahedral, and spherical shapes are preferred in terms of increasing image density.
[0170] The magnetic material preferably has a number-average particle size in the range of 0.10 to 0.40 μm. In general, the smaller the particle size of the magnetic material, the higher the coloring power, but the magnetic material is more likely to aggregate, so the above range is preferable from the viewpoint of the balance between coloring power and aggregation. The number-average particle size of the magnetic material can be measured using a transmission electron microscope.
[0171] Specifically, the toner particles to be observed are thoroughly dispersed in an epoxy resin, and then the resin is cured for two days in an atmosphere at 40°C to obtain a cured product. The cured product is cut into thin slices using a microtome, and the diameters of 100 magnetic particles in the field of view are measured using a transmission electron microscope (TEM) at a magnification of 10,000 to 40,000. The number-average particle diameter is then calculated based on the equivalent diameter of a circle that is equal to the projected area of the magnetic particles. It is also possible to measure the particle diameter using an image analyzer.
[0172] The magnetic material used in the toner of the present invention can be produced, for example, by the following method.
[0173] An aqueous solution containing ferrous hydroxide is prepared by adding an equivalent or greater amount of alkali such as sodium hydroxide to an aqueous solution of ferrous salt. While maintaining the pH of the prepared aqueous solution at 7 or higher, air is blown in and the aqueous solution is heated to 70°C or higher to carry out an oxidation reaction of the ferrous hydroxide, thereby first producing seed crystals that will become the cores of the magnetic iron oxide powder.
[0174] Next, an aqueous solution containing about 1 equivalent of ferrous sulfate is added based on the amount of alkali added previously to the slurry liquid containing the seed crystals. While maintaining the pH of the liquid within the range of 5 to 10, the reaction of ferrous hydroxide is allowed to proceed while blowing in air, and magnetic iron oxide powder is grown around the seed crystals as cores. At this time, the shape and magnetic properties of the magnetic material can be controlled by selecting any pH, reaction temperature, and stirring conditions.
[0175] As the oxidation reaction proceeds, the pH of the solution shifts to the acidic side, but it is preferable not to make the pH of the solution less than 5. The magnetic material thus obtained can be filtered, washed, and dried in a standard manner to obtain the desired magnetic material. In addition, when producing a toner in an aqueous medium in the present invention, it is highly preferable to subject the surface of the magnetic material to a hydrophobic treatment.
[0176] When performing the surface treatment by the dry method, the magnetic material is treated with a coupling agent after washing, filtering, and drying. When performing the surface treatment by the wet method, the dried material is redispersed after the oxidation reaction is completed. Alternatively, the iron oxide material obtained by washing and filtering after the oxidation reaction is redispersed in another aqueous medium without drying, thereby performing the coupling treatment. In the present invention, either the dry method or the wet method can be appropriately selected.
[0177] The content of the magnetic material in the toner can be measured using a thermal analyzer, TGA7, manufactured by PerkinElmer, as follows.
[0178] The toner is heated in a nitrogen atmosphere from room temperature to 900° C. at a temperature increase rate of 25° C. / min. The mass percent loss between 100° C. and 750° C. is taken as the amount of binder resin, and the remaining mass is taken as approximately the amount of magnetic material.
[0179] (Charge control agent) In order to stabilize the chargeability, it is preferable to use a charge control agent. As such a charge control agent, any known charge control agent can be used alone or in combination.
[0180] Considering the suitability for color toners (the charge control agent itself is colorless or light-colored and does not interfere with the color tone of the toner), quaternary ammonium salt compounds are preferred for their positive chargeability.
[0181] As the negatively charged material, preferred are metal salts or metal complexes of salicylic acid or alkylsalicylic acid with chromium, zinc, aluminum, etc., metal salts or metal complexes of benzilic acid, amide compounds, phenol compounds, naphthol compounds, phenolamide compounds, etc. Furthermore, polymers that exhibit negative charging properties, such as sulfonates, carboxylates, and halogens, may also be used.
[0182] (3.1.7) Characteristics of toner particles The toner particles may be toner particles of a single layer structure, or may be toner particles of a so-called core-shell structure composed of a core (core particle) and a coating layer (shell layer) that coats the core. Here, the toner particles of the core-shell structure may be composed of a core composed of, for example, a binder resin and, if necessary, other additives such as a colorant and a release agent, and a coating layer composed of a binder resin.
[0183] Volume average particle size of toner particles (D 50 v) is preferably in the range of 2 to 10 μm, more preferably in the range of 4 to 8 μm. The various average particle sizes and various particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.).
[0184] For the measurement, 0.5 to 50 mg of the measurement sample is added to 2 mL of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is added to 100 to 150 mL of the electrolyte.
[0185] The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with a particle size in the range of 2 to 60 μm is measured using a Coulter Multisizer II with an aperture of 100 μm in diameter. The number of particles sampled is 50,000.
[0186] Based on the particle size distribution measured, the cumulative distribution of volume and number is drawn for each divided particle size range (channel) from the small particle size side. The particle size at which the cumulative 16% occurs is called the volume particle size D 16 v, number particle size D 16 p, the particle size at which the cumulative 50% is reached is the volume average particle size D 50 v, cumulative number average particle diameter D 50 p, the particle size at which the cumulative 84% occurs is the volume particle size D 84 v, number particle size D 84 Using these, the volume average particle size distribution index (GSDv) is defined as (D 84 v / D 16 v)1 / 2, the number average particle size distribution index (GSDp) is (D 84 p / D 16 p)1 / 2.
[0187] (3.1.8) External additives The external additive may be, for example, inorganic particles. Examples of inorganic particles include SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2) n , Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, MgSO 4、 In addition to the above, inorganic chlorides such as titanates can also be used.
[0188] The surface of the inorganic particles as an external additive is preferably subjected to a hydrophobic treatment. The hydrophobic treatment is performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobic treatment agent is usually within the range of 1 part by mass to 10 parts by mass, for example, relative to 100 parts by mass of the inorganic particles.
[0189] Examples of the external additive include resin particles and cleaning lubricants. Examples of the resin particles include resin particles such as polystyrene, polymethyl methacrylate (PMMA), melamine resin, etc. Examples of the cleaning lubricant include metal salts of higher fatty acids such as zinc stearate, and particles of fluorine-based polymers.
[0190] The amount of the external additive added is preferably within a range of 0.01 to 5% by mass, and more preferably within a range of 0.01 to 2.0% by mass, based on the toner particles.
[0191] (3.1.9) Method for producing toner for developing electrostatic latent images Next, a method for producing the toner according to the present embodiment will be described.
[0192] The toner according to the present embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles. The toner particles may be produced by any of a dry production method (e.g., a kneading and grinding method, etc.) and a wet production method (e.g., an aggregation and coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). The method for producing the toner particles is not particularly limited, and any well-known production method may be used. Some examples of the method for producing the toner particles are given below.
[0193] (3.1.9.1) Agglomeration coalescence method The aggregation and coalescence method includes, for example, three steps: (1) a resin particle dispersion preparation step, (2) an aggregate particle formation step, and (3) a fusion and coalescence step. Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.
[0194] (1) Resin particle dispersion preparation process The resin particle dispersion preparation step is a step of preparing a resin particle dispersion in which resin particles that will become a binder resin are dispersed.
[0195] First, a colorant particle dispersion in which colorant particles are dispersed and a release agent particle dispersion in which release agent particles are dispersed are prepared together with a resin particle dispersion in which resin particles serving as a binder resin are dispersed. Here, the resin particle dispersion is prepared by dispersing resin particles in a dispersion medium using a surfactant, for example.
[0196] (dispersion medium) Examples of the dispersion medium used in the resin particle dispersion liquid include aqueous media. Examples of the aqueous media include water such as distilled water and ion-exchanged water, and alcohols. These may be used alone or in combination of two or more.
[0197] (Surfactant) Examples of the surfactant include anionic surfactants, cationic surfactants, and nonionic surfactants, and anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactant may be used in combination with an anionic surfactant or a cationic surfactant. The surfactant may be used alone or in combination with two or more kinds.
[0198] Examples of the anionic surfactant include sulfates, sulfonates, phosphates, and soaps.
[0199] Examples of cationic surfactants include amine salt types and quaternary ammonium salt types.
[0200] Examples of nonionic surfactants include polyethylene glycol surfactants, alkylphenol ethylene oxide adduct surfactants, polyhydric alcohol surfactants, and the like.
[0201] (Distribution method) In the resin particle dispersion, the resin particles are dispersed in the dispersion medium by a general dispersion method such as a rotary shear homogenizer, a ball mill having a medium, a sand mill, or a dyno mill. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion by a phase inversion emulsification method. The phase inversion emulsification method is as follows.
[0202] The resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, and a base is added to the organic continuous phase (O phase) to neutralize it.Then, an aqueous medium (W phase) is added to convert the resin from W / O to O / W (so-called phase inversion), forming a discontinuous phase, and the resin is dispersed in the aqueous medium in the form of particles.
[0203] (Volume average particle size of resin particles) The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably in the range of 0.01 to 1 μm, more preferably in the range of 0.08 to 0.8 μm, and further preferably in the range of 0.1 to 0.6 μm. The volume average particle size of the resin particles can be measured by a laser diffraction particle size distribution measuring device.
[0204] An example of a laser diffraction particle size distribution measuring device is the "LA-700" (manufactured by Horiba, Ltd.). Using the particle size distribution obtained by measuring with the above-mentioned device, the cumulative distribution is drawn for the divided particle size range (channel) from the small particle size side for the volume. The particle size that is cumulatively 50% of all particles is then called the volume average particle size D 50 The volume average particle size of particles in other dispersions is measured in the same manner.
[0205] (Resin particle content) The content of the resin particles in the resin particle dispersion is, for example, preferably in the range of 5 to 50% by mass, and more preferably in the range of 10 to 40% by mass.
[0206] (Other preparation methods) In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.
[0207] (2) Agglomerated particle formation process The aggregated particle forming step is a step of aggregating resin particles in a resin particle dispersion to form aggregated particles. The resin particle dispersion may be a mixture of other particle dispersions as required, and may be aggregated to form aggregated particles.
[0208] Next, the colorant particle dispersion and the release agent particle dispersion are mixed with the resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles. Specifically, the aggregated particles are formed as follows.
[0209] For example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic, and a dispersion stabilizer is added as necessary. At this time, the pH is adjusted to a range of 2 to 5. Thereafter, the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles, and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. At this time, the above glass transition temperature is within a range of (glass transition temperature of the resin particles - 30°C) to (glass transition temperature - 10°C).
[0210] In the aggregated particle formation step, for example, the mixed dispersion may be stirred with a rotary shear homogenizer, the above-mentioned aggregating agent may be added at room temperature (e.g., 25°C), the pH of the mixed dispersion may be adjusted to an acidic state (e.g., a pH in the range of 2 to 5), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.
[0211] (Flocculant) The flocculant may be, for example, a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion. The above surfactant may be, for example, an inorganic metal salt or a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. An additive that forms a complex with the metal ion of the flocculant or a bond similar to the metal ion may be used as necessary. A chelating agent is preferably used as this additive.
[0212] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide.
[0213] The chelating agent may be a water-soluble chelating agent. Examples of the chelating agent include oxycarboxylic acids such as tartaric acid, citric acid, and gluconic acid, iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), and ethylenediaminetetraacetic acid (EDTA). The amount of the chelating agent added is preferably within a range of 0.01 to 5.0 parts by mass, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.
[0214] (3) Fusion / unification process The fusion / coalescence process is a process in which the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated to fuse and coalesce the aggregated particles to form toner particles. After the aggregated particle formation process, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the resin particles to fuse and coalesce the aggregated particles to form toner particles. Toner particles are obtained through the above processes. Note that, after obtaining the aggregated particle dispersion liquid in which the aggregated particles are dispersed, toner particles may be manufactured through a process of forming second aggregated particles and a process of fusing and coalescing the second aggregated particles to form toner particles having a core / shell structure.
[0215] The step of forming the second aggregated particles is a step of further mixing the aggregated particle dispersion liquid with the resin particle dispersion liquid in which the resin particles are dispersed, and aggregating the aggregated particles so that the resin particles are further attached to the surfaces of the aggregated particles.
[0216] In addition, the process of fusing and coalescing the second aggregate particles to form toner particles having a core / shell structure is a process of fusing and coalescing the second aggregate particles by heating the second aggregate particle dispersion liquid in which the second aggregate particles are dispersed, thereby forming toner particles having a core / shell structure.
[0217] Here, after the fusion and coalescence process is completed, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain dried toner particles. In the washing process, it is preferable to carry out sufficient substitution washing with ion-exchanged water from the viewpoint of chargeability. Furthermore, the solid-liquid separation process is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. Furthermore, the drying process is also not particularly limited, but it is preferable to carry out freeze drying, flash jet drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.
[0218] In the present embodiment, after the toner particles are produced, the toner particles may be subjected to an annealing treatment under predetermined temperature and heating time conditions. The toner according to the present embodiment is produced by, for example, adding an external additive to the obtained toner particles in a dry state and mixing them.
[0219] The mixing may be carried out by, for example, a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed by using a vibration separator or an air separator, etc.
[0220] (3.1.9.2) Grinding method When preparing a toner by a pulverization method, first, the binder resin, wax, charge control agent, etc. contained in the toner particles are thoroughly mixed in a mixer such as a Henschel mixer or a ball mill to obtain a mixture. The toner particles may be magnetic toner particles, and may contain a magnetic material in addition to the binder resin, wax, and charge control agent.
[0221] The mixture is then melted and kneaded using a thermal kneader such as a twin-screw kneading extruder, a heating roll, a kneader, or an extruder, cooled and solidified, and then pulverized and classified. This gives toner particles. The toner can be produced by externally adding and mixing an external additive to the toner particles.
[0222] Examples of mixers include Henschel Mixer (manufactured by Mitsui Mining Co., Ltd.); Super Mixer (manufactured by Kawata Co., Ltd.); Ribocone (manufactured by Okawara Manufacturing Co., Ltd.); Nauta Mixer, Turbulizer, Cyclomix (manufactured by Hosokawa Micron Corporation); Spiral Pin Mixer (manufactured by Pacific Machinery Co., Ltd.); and Loedige Mixer (manufactured by Matsubo Co., Ltd.).
[0223] Examples of kneading machines include the KRC kneader (manufactured by Kurimoto Iron Works); the Buss-Co kneader (manufactured by Buss); the TEM type extruder (manufactured by Toshiba Machine Co., Ltd.); the TEX twin-screw kneader (manufactured by Japan Steel Works); the PCM kneader (manufactured by Ikegai Iron Works); the three-roll mill, mixing roll mill, kneader (manufactured by Inoue Seisakusho Co., Ltd.); the Kneadex (manufactured by Mitsui Mining Co., Ltd.); the MS-type pressure kneader, the Niderruder (manufactured by Moriyama Seisakusho Co., Ltd.); and the Banbury mixer (manufactured by Kobe Steel, Ltd.).
[0224] Examples of grinding machines include counter jet mills, micron jets, and innomizers (manufactured by Hosokawa Micron Corporation); IDS type mills, PJM jet grinders (manufactured by Japan Pneumatic Mfg. Co., Ltd.); cross jet mills (manufactured by Kurimoto Iron Works); Urumax (manufactured by Nisso Engineering Co., Ltd.); SK Jet-O-Mill (manufactured by Seishin Enterprise Co., Ltd.); Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.); Turbo Mill (manufactured by Turbo Industrial Co., Ltd.); and Super Rotor (manufactured by Nisshin Engineering Co., Ltd.).
[0225] Examples of classifiers include Classeal, Micron Classifier, and Spedic Classifier (manufactured by Seishin Enterprise Co., Ltd.); Turbo Classifier (manufactured by Nisshin Engineering Co., Ltd.); Micron Separator, Turboplex (ATP), and TSP Separator (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), Dispersion Separator (manufactured by Nippon Pneumatic Industry Co., Ltd.); and YM Microcut (manufactured by Yaskawa Shoji Co., Ltd.).
[0226] As a mixing processing device for mixing the external additives, a known mixing processing device such as the above mixer can be used.
[0227] In addition, when the pulverized toner is designed to be soft, the surface needs to be hardened separately, so there is a technique to fix and coat the pulverized toner surface with fine particles such as silica, which has a uniform particle size distribution of about 110 nm, such as "X24". Then, the toner base particles produced in this way can be further treated with an external additive for the purpose of a fluidizing agent.
[0228] (3.1.9.3) Suspension polymerization method The method for producing toner particles by the suspension polymerization method includes a dissolving step in which these additives are uniformly dissolved or dispersed to form a polymerizable monomer composition, a granulation step in which this polymerizable monomer composition is dispersed in an aqueous medium containing a dispersion stabilizer using an appropriate stirrer and granulated, a polymerization reaction step in which an aromatic solvent and a polymerization initiator are added as necessary to carry out a polymerization reaction, a cooling step in which the location and size of microdomains of the crystalline material are controlled, and a holding (annealing) step in which the degree of crystallinity of the crystalline material is controlled, thereby obtaining toner particles having a desired particle size.
[0229] (3.1.9.4) Toner surface modification The toner produced by the above-mentioned method can also be fixed by, for example, adhering fine particles to the core surface. The adhesion of fine particles to the core surface can be achieved, for example, by uniformly mixing the core material and inorganic fine particles, electrostatically attaching the inorganic fine particles to the surface of the core material to produce an ordered mixture, and then applying a mechanical or thermal impact force to drive the inorganic fine particles into the core material to fix them.
[0230] The inorganic fine particles are not completely embedded in the core material, but are fixed so that a part of them protrudes from the core material. Such an inorganic fine particle fixing device is commercially available as a surface modification device or system, and examples thereof include the following.
[0231] (1) Dry mechanochemical method: Mechanochemical (Okada Seiko Co., Ltd.), Mechanofusion System (Hosokawa Micron Co., Ltd.) (2) High-velocity airflow impact method: Hybridization System (Nara Machinery Works, Ltd.), Cryptron System (Kawasaki Heavy Industries, Ltd.) (3) Wet method: Dispercoat (Nisshin Flour Milling Co., Ltd.), Coatmizer (Freund Corporation) (4) Heat treatment method: Surfusing (Nippon Pneumatic Mfg. Co., Ltd.) (5) Others: Spray dryer (Okawahara Chemical Engineering Co., Ltd.)
[0232] (3.2) Developer The electrostatic latent image developer according to the present embodiment contains at least the toner for developing electrostatic latent images according to the present embodiment. The electrostatic latent image developer according to the present embodiment may be a one-component developer containing only the toner for developing electrostatic latent images according to the present embodiment, or may be a two-component developer in which the toner for developing electrostatic latent images is mixed with a carrier.
[0233] (Career) One of the main roles of the carrier in two-component developer is to agitate and mix with the toner in the developer box and give the toner the desired charge. Another role of the carrier is to act as an electrode between the developer and the photoreceptor, and to carry the charged toner to the electrostatic latent image on the photoreceptor, forming a toner image.
[0234] The carrier is held on a magnet roller by magnetic force, for example, and after acting on the development, it returns to the development box, where it is stirred and mixed again with new toner, and is used repeatedly for a certain period of time. Therefore, in order to stably maintain the desired image characteristics (image density, fog, white spots, gradation, resolution, etc.), it is naturally required that the characteristics of the carrier are stable throughout the period of use.
[0235] The carrier is not particularly limited, and may be any known carrier. Examples of the carrier include conductive particles, coated carriers in which the surface of a core material made of magnetic powder is coated with a coating resin, magnetic powder dispersion type carriers in which magnetic powder is dispersed and mixed in a matrix resin, and resin impregnated type carriers in which porous magnetic powder is impregnated with resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be carriers in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.
[0236] Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.
[0237] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.
[0238] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin.
[0239] The coating resin and the matrix resin may contain other additives such as conductive materials.
[0240] Here, the method of coating the surface of the core material with the coating resin includes a method of coating with a solution for forming a coating layer in which the coating resin and, if necessary, various additives are dissolved in an appropriate solvent, etc. The solvent is not particularly limited and may be selected taking into consideration the coating resin to be used, the suitability for application, etc.
[0241] Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.
[0242] In the two-component developer, the mixing ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100. EXAMPLES
[0243] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they are "parts by mass" or "% by mass" unless otherwise specified. The pH value is a value measured at 25°C unless otherwise specified.
[0244] A. Preparation of the developing roller (A.1) Preparation of developing roller 1 (A.1.1) Preparation of developing sleeve 1 The developing sleeve 1 was prepared according to the following procedure.
[0245] (Preparation of the support) A cylindrical support made of an aluminum alloy was prepared. The silicon content of the aluminum alloy of this cylindrical support was 0.61 mass%. The cylindrical support was a thin-walled support having an outer diameter of 16 mm, an inner diameter of 14 mm, and a wall thickness of 1 mm.
[0246] (Sandblasting) The cylindrical support made of the aluminum alloy was sandblasted on the outer peripheral surface of the cylinder by spraying glass beads with a blast gun, to prepare the developing sleeve 1. The processing conditions for the sandblasting were as follows:
[0247] <Processing conditions> Glass bead type: FGB#80 (manufactured by Fuji Manufacturing) Glass beads feed rate: 200g / min Distance from blast gun to cylinder: 100mm Blast gun movement speed: 5.0cm / sec Compressed air pressure: 0.23MPa Cylinder rotation speed: 545 rpm
[0248] (A.1.2) Installation of magnetic rollers A magnetic roller was provided on the inside of the developing sleeve 1 as shown in FIG.
[0249] (A.2) Preparation of developing rollers 2 to 12 Developing sleeves 2 to 12 were produced in the same manner as the producing procedure of developing sleeve 1, except that the silicon content in the aluminum alloy was set to the amount shown in Table I. In addition, the magnet roller was also installed in the same manner as developing roller 1, and developing rollers 2 to 12 were produced.
[0250] [Table 1]
[0251] B. Toner Preparation (B.1) Resins and dispersions used for each toner (preparation for producing toners 1 to 3) (B.1.1) Amorphous polyester (B.1.1.1) Preparation of each amorphous polyester (Preparation of amorphous polyester [a1]) The following components were placed in a reaction vessel equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube, and the atmosphere in the reaction vessel was replaced with dry nitrogen gas. Then, tin dioctanoate was added in an amount of 0.3% based on the total amount of the components.
[0252] <Ingredients> Ethylene glycol 106 parts by weight Dimethyl terephthalate 245 parts by mass 1,10-Decanedicarboxylic acid 105 parts by mass
[0253] The temperature was raised to 235°C over 1 hour under a nitrogen gas stream, and the reaction was carried out for 3 hours. The pressure inside the reaction vessel was then reduced to 10.0 mmHg, and the reaction was continued with stirring. When the desired molecular weight was reached, the reaction was stopped to produce amorphous polyester [a1].
[0254] (Preparation of amorphous polyester [a2]) Amorphous polyester [a2] was prepared in the same manner as for amorphous polyester [a1], except that the following components were added.
[0255] <Ingredients> Bisphenol A ethylene oxide adduct 30 parts by mass Bisphenol A propylene oxide adduct 270 parts by mass Terephthalic acid 60 parts by mass Fumaric acid 40 parts by mass Tetrapropenylsuccinic anhydride 40 parts by mass
[0256] (Preparation of amorphous polyester [a3]) Amorphous polyester [a3] was prepared in the same manner as for amorphous polyester [a1], except that the following components were added.
[0257] <Ingredients> Bisphenol A ethylene oxide adduct 210 parts by mass Bisphenol A propylene oxide adduct 230 parts by mass Terephthalic acid 30 parts by mass Fumaric acid 135 parts by mass Tetrapropenylsuccinic anhydride 40 parts by mass
[0258] (Preparation of amorphous polyester [a4]) Amorphous polyester [a4] was prepared in the same manner as for amorphous polyester [a1], except that the following components were added.
[0259] <Ingredients> Bisphenol A ethylene oxide adduct 150 parts by mass Bisphenol A propylene oxide adduct 250 parts by mass Terephthalic acid 100 parts by mass Tetrapropenylsuccinic anhydride 130 parts by mass Trimellitic acid 15 parts by mass
[0260] (Preparation of amorphous polyester [a5]) Amorphous polyester [a5] was prepared in the same manner as for amorphous polyester [a1], except that the following components were added.
[0261] <Ingredients> Bisphenol A propylene oxide adduct 350 parts by mass Terephthalic acid 35 parts by mass Fumaric acid 90 parts by mass Tetrapropenylsuccinic anhydride 13 parts by mass
[0262] (B.1.1.2) Preparation of each amorphous polyester dispersion (Preparation of amorphous polyester dispersion (A1)) The following components were placed in a reaction vessel equipped with a stirrer and dissolved at 60°C.
[0263] <Ingredients> Amorphous polyester [a1] 100 parts by mass Methyl ethyl ketone 60 parts by weight Isopropyl alcohol 10 parts by weight
[0264] After confirming dissolution, the reaction vessel was cooled to 35°C, and 3.5 parts by mass of 10% aqueous ammonia solution was added. Then, 300 parts by mass of ion-exchanged water was dropped into the reaction vessel over 3 hours. Then, methyl ethyl ketone and isopropyl alcohol were removed using an evaporator to prepare an amorphous polyester dispersion (A1).
[0265] (Preparation of amorphous polyester dispersion (A2)) Amorphous polyester dispersion (A2) was prepared in the same manner as in the preparation of amorphous polyester dispersion (A1), except that the amorphous polyester (a1) was replaced with amorphous polyester (a2).
[0266] (Preparation of amorphous polyester dispersion (A3)) Amorphous polyester dispersion (A3) was prepared in the same manner as in the preparation of amorphous polyester dispersion (A1), except that the amorphous polyester (a1) was replaced with amorphous polyester (a3).
[0267] (Preparation of amorphous polyester dispersion (A4)) Amorphous polyester dispersion (A4) was prepared in the same manner as in the preparation of amorphous polyester dispersion (A1), except that the amorphous polyester (a1) was replaced with amorphous polyester (a4).
[0268] (Preparation of amorphous polyester dispersion (A5)) Amorphous polyester dispersion (A5) was prepared in the same manner as in the preparation of amorphous polyester dispersion (A1), except that the amorphous polyester (a1) was replaced with amorphous polyester (a5).
[0269] (B.1.2) Crystalline polyester (B.1.2.1) Preparation of each crystalline polyester (Preparation of crystalline polyester [c1]) The following components were charged into a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube, and the atmosphere in the reaction vessel was replaced with dry nitrogen gas. Then, 0.3 parts by mass of tin dioctanoate was charged per 100 parts by mass of the following components.
[0270] <Ingredients> 1,10-Decanedicarboxylic acid 300 parts by mass Ethylene glycol 100 parts by mass
[0271] After stirring and reacting for 3 hours at 160°C under a nitrogen gas flow, the temperature was further raised to 180°C over 1.5 hours, the pressure inside the reaction vessel was reduced to 3 kPa, and the reaction was terminated when the desired molecular weight was reached to produce crystalline polyester [c1].
[0272] (Preparation of crystalline polyester [c2]) Crystalline polyester [c2] was prepared in the same manner as for crystalline polyester [c1], except that the following components were added.
[0273] <Ingredients> 1,10-Decanedicarboxylic acid 350 parts by mass 1,6-Hexanediol 170 parts by mass
[0274] (Preparation of crystalline polyester [c3]) Crystalline polyester [c3] was prepared in the same manner as for crystalline polyester [c1], except that the following components were added.
[0275] <Ingredients> 1,10-Decanedicarboxylic acid 350 parts by mass 1,9-nonanediol 240 parts by mass
[0276] (B.1.2.2) Preparation of each crystalline polyester dispersion (Preparation of Crystalline Polyester Dispersion (C1)) The following components were placed in a reaction vessel equipped with a stirrer and dissolved at 65°C.
[0277] <Ingredients> Crystalline polyester [c1] 100 parts by mass Methyl ethyl ketone 60 parts by weight Isopropyl alcohol 15 parts by weight
[0278] After confirming dissolution, the reaction vessel was cooled to 60°C, and then 5 parts by mass of 10% aqueous ammonia solution was added. Then, 300 parts by mass of ion-exchanged water was dropped into the reaction vessel over 3 hours. Then, methyl ethyl ketone and isopropyl alcohol were removed using an evaporator to prepare a crystalline polyester dispersion (C1).
[0279] (Preparation of Crystalline Polyester Dispersion (C2)) A crystalline polyester dispersion (C2) was prepared in the same manner as in the preparation of the crystalline polyester dispersion (C1), except that the crystalline polyester (c1) was changed to the crystalline polyester (c2).
[0280] (Preparation of Crystalline Polyester Dispersion (C3)) A crystalline polyester dispersion (C3) was prepared in the same manner as in the preparation of the crystalline polyester dispersion (C1), except that the crystalline polyester (c1) was replaced with the crystalline polyester (c3).
[0281] (B.1.3) Styrene-acrylic copolymer resin (Preparation of styrene-acrylic copolymer resin dispersion (S1)) The following components were placed in a vessel and emulsified using a homogenizer to prepare a monomer emulsion (S).
[0282] <Ingredients> Styrene 126 parts by weight n-Butyl acrylate 14 parts by weight Dodecanethiol 2.1 parts by mass Isopropyl alcohol 0.88 parts by weight Anionic surfactant (Dowfax, manufactured by The Dow Chemical Company) 4 parts by weight Ion-exchanged water 59.2 parts by weight
[0283] Meanwhile, the following components were placed in a polymerization reaction vessel.
[0284] <Ingredients> Anionic surfactant (Dowfax, manufactured by The Dow Chemical Company) 0.6 parts by mass Ion-exchanged water 133 parts by weight
[0285] Thereafter, a reflux condenser was installed, and the mixture was slowly stirred while injecting nitrogen, and the polymerization flask was heated in a water bath to 75° C. and maintained at that temperature. 10 parts by mass of the monomer emulsion (S) was added dropwise to the container over a period of 10 minutes using a metering pump.
[0286] Next, 1.05 parts by mass of ammonium persulfate was dissolved in 10 parts by mass of ion-exchanged water and added dropwise to the polymerization flask over 10 minutes using a metering pump. Stirring was continued for 1 hour under this condition. Furthermore, the remaining monomer emulsion (S) was added dropwise over 2 hours using a metering pump.
[0287] After the addition was complete, stirring was continued for an additional 3 hours to prepare a styrene-acrylic copolymer resin dispersion (S1).
[0288] (B.1.4) Release agent dispersion (Preparation of release agent dispersion (W1)) The following components were mixed, and the release agent was dissolved in a pressure discharge homogenizer (Gaulin Homogenizer, manufactured by Gaulin Co., Ltd.) at an internal liquid temperature of 120°C. The mixture was then dispersed at a dispersion pressure of 5 MPa for 120 minutes and then at 40 MPa for 360 minutes, and cooled to prepare a release agent dispersion (W1).
[0289] <Ingredients> Hydrocarbon wax 270.0 parts by mass Anionic surfactant 13.5 parts by mass (3.0% of the active ingredient in the release agent) Ion-exchanged water 700.0 parts by mass
[0290] The hydrocarbon wax in the above components is "FNP0090" (manufactured by Nippon Seiro Co., Ltd.) having a melting temperature Tw of 90.2°C.
[0291] The anionic surfactant in the above ingredients is "Teika Power BN2060" (manufactured by Teika Co., Ltd.), which has an active ingredient content of 60%.
[0292] The volume average particle size D of the particles in the release agent dispersion (W1) 50 v was 220 nm.
[0293] Thereafter, ion-exchanged water was added to adjust the solid content to 20.0%.
[0294] (B.1.5) Colorant dispersion (Preparation of Black Colorant Dispersion (B1)) The following components were placed in a stainless steel container large enough that the liquid level would be 1 / 3 of the container's height when all of the components were added, and 280 parts by mass of ion-exchanged water and an anionic surfactant were added and the surfactant was thoroughly dissolved.
[0295] Thereafter, all of the pigment was added and stirred with a stirrer until there was no unwetted pigment, after which the remaining ion-exchanged water was added and further stirred to thoroughly defoam the mixture.
[0296] <Ingredients> Carbon black 200 parts by weight Anionic surfactant 33 parts by weight (10% of the active ingredient, based on colorant) Ion-exchanged water 750 parts by weight
[0297] The carbon black in the above components is "REGAL330" (manufactured by Cabot Japan Co., Ltd.).
[0298] The anionic surfactant in the above ingredients is "Neogen SC" (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), with an active ingredient content of 60%.
[0299] After defoaming, the mixture was dispersed at 5,000 rpm for 10 minutes using a homogenizer "Ultra Turrax T50" (manufactured by IKA), and then stirred overnight with a stirrer to defoam the mixture.
[0300] After degassing, the mixture was dispersed again using a homogenizer at 6,000 rpm for 10 minutes, and then stirred overnight with a stirrer to degas the mixture.
[0301] After degassing, the mixture was dispersed at a pressure of 240 MPa using a high-pressure impact disperser, Ultimizer HJP30006 (manufactured by Sugino Machine Co., Ltd.) The dispersion was performed for the equivalent of 25 passes, calculated based on the total charge amount and the processing capacity of the device.
[0302] The obtained dispersion liquid was left for 72 hours to remove the precipitate, and ion-exchanged water was added to adjust the solid content to 15%, to prepare a black colorant particle dispersion liquid (B1). 50 v was 110 nm.
[0303] (B.2) Preparation of Toner 1 (Preparation of toner base particles [1]) As the toner core components, each dispersion was weighed so that the solid content was the following amount.
[0304] <Core Ingredients> Amorphous polyester [a1] 47.5 parts by mass Crystalline polyester [c1] 22.0 parts by mass Black colorant [B1] (solid content) 6.0 parts by weight Release agent [W1] (solid content) 1.5 parts by weight
[0305] Each dispersion was poured into a round stainless steel flask, ion-exchanged water was added so that the solid content concentration was 12.5%, and 6.3 parts of a 10% aqueous aluminum sulfate solution was further poured in. Next, the mixture was mixed and dispersed at 5000 rpm for 10 minutes using a homogenizer (Ultra Turrax T50, manufactured by IKA), and the contents in the flask were heated to 40°C while stirring.
[0306] After that, the temperature was raised at 0.5° C. per minute, and the temperature was maintained when the particle size reached 6.1 μm. Next, each dispersion was weighed and mixed so that the solid content of the toner shell component was as follows, and the resulting dispersion was then added and maintained for 60 minutes.
[0307] <Shell component> Amorphous polyester [a5] 20 parts by mass Release agent dispersion [W1] (solid content) 3 parts by weight
[0308] When the resulting content was observed under an optical microscope, it was confirmed that aggregated particles were formed.
[0309] After adding 11 parts of tetrasodium ethylenediaminetetraacetic acid (EDTA) "Chilest 40" (Chilest Co., Ltd.), an aqueous solution of sodium hydroxide was added to adjust the pH to 8. The temperature was then raised to 82.5°C, after which the pH was lowered by 0.05 every 10 minutes with nitric acid and stirring was continued for 45 minutes. After cooling, the mixture was filtered, thoroughly washed with ion-exchanged water, and dried to prepare toner base particles [1].
[0310] (Addition of external additives) To 100 parts by mass of the toner base particles [1] obtained above, 1.5 parts by mass of hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd.) was added and mixed for 30 seconds at 13,000 rpm using a sample mill. The mixture was then sieved using a vibrating sieve with 45 μm openings to produce toner 1.
[0311] (Measurement of glass transition temperature) The glass transition temperature (Tg) of Toner 1 was 0.4°C.
[0312] The glass transition temperatures of Toner 1 and other toners were measured by differential scanning calorimetry in accordance with JIS K7121-1987.
[0313] The substances to be measured (each toner) were set in a differential scanning calorimeter "DSC-50" (manufactured by Shimadzu Corporation) equipped with an automatic tangent processing system. Liquid nitrogen was also set as a cooling medium.
[0314] The sample was heated from 0°C to 150°C at a rate of 10°C / min (first heating process) to determine the relationship between temperature (°C) and heat amount (mW).
[0315] Next, the sample was cooled to 0°C at a rate of -10°C / min, and then heated again to 150°C at a rate of 10°C / min (second heating process) to collect data. The sample was held at 0°C and 150°C for 10 minutes each.
[0316] The melting temperature of the mixture of indium and zinc was used to correct the temperature of the detection part of the measuring device, and the heat of fusion of indium was used to correct the amount of heat.
[0317] The samples were placed in aluminum pans, and the aluminum pans containing the samples were set up alongside an empty aluminum pan as a control.
[0318] The glass transition temperature was determined as the temperature at the intersection of the baseline and the extended line of the rising edge in the endothermic portion of the DSC curve obtained during the second heating process.
[0319] (B.3) Preparation of Toners 2 and 3 Toner base particles [2] and [3] were prepared in the same manner as in the preparation of toner base particles [1], so that the components of the toner base particles were those shown in Table II.
[0320] The solid content [S1] of the styrene-acrylic copolymer resin dispersion (S1) in the preparation of the toner base particles [2] was set to 4.5 parts by mass.
[0321] [Table 2]
[0322] Further, toners 2 and 3 were prepared by adding external additives to the above toner base particles [2] and [3], and the glass transition temperatures (Tg) were measured.
[0323] The types and amounts of the external additives of Toners 1 to 3, the polyester content in the toner containing the external additives, and the glass transition temperatures are shown in Table III.
[0324] [Table 3]
[0325] (B.4) Resins and dispersions used for each toner (preparation for producing toners 4 to 6) (B.4.1) Amorphous polyester (Preparation of amorphous polyester [a7]) The following components were placed in a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and reacted at 230°C under normal pressure for 10 hours.
[0326] <Ingredients> Ethylene glycol 106 parts by weight Dimethyl terephthalate 245 parts by mass 1,10-Decanedicarboxylic acid 105 parts by mass Dibutyltin oxide 2 parts by mass
[0327] After that, the mixture was reacted for 5 hours under a reduced pressure of 10 to 15 mmHg, and then 30 parts by mass of trimellitic anhydride was added to the reaction vessel and reacted for 3 hours at 180°C and normal pressure to produce amorphous polyester [a7], which is a low molecular weight polyester having hydroxyl groups.
[0328] (Preparation of amorphous polyester [a8]) The following components were placed in a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and reacted at 230°C under normal pressure for 10 hours.
[0329] <Ingredients> Bisphenol A ethylene oxide side 2 mole adduct 229 parts by mass Bisphenol A propylene oxide 3 mole adduct 529 parts by mass Isophthalic acid 100 parts by mass Terephthalic acid 108 parts by mass Adipic acid 46 parts by mass Dibutyltin oxide 2 parts by mass
[0330] After that, the mixture was reacted for 5 hours under a reduced pressure of 10 to 15 mmHg, and then 30 parts by mass of trimellitic anhydride was added to the reaction vessel and reacted for 3 hours at 180°C and normal pressure to produce amorphous polyester [a8], which is a low molecular weight polyester having hydroxyl groups.
[0331] (Preparation of amorphous polyester [a9]) The following components were placed in a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and reacted at 240° C. for 10 hours under normal pressure.
[0332] <Ingredients> Bisphenol A ethylene oxide side 2 mole adduct 235 parts by mass Bisphenol A propylene oxide 3 mole adduct 535 parts by mass Terephthalic acid 215 parts by mass Adipic acid 50 parts by mass Dibutyltin oxide 3 parts by mass
[0333] After that, the mixture was reacted for 5 hours under a reduced pressure of 10 to 20 mmHg, and then 45 parts by mass of trimellitic anhydride was added to the reaction vessel and reacted for 3 hours at 185°C and normal pressure to produce amorphous polyester [a9], which is a low molecular weight polyester having a hydroxyl group.
[0334] (B.4.2) Crystalline polyester (B.4.2.1) Preparation of each crystalline polyester (Preparation of crystalline polyester [c4]) The following ingredients were placed in a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and reacted at 180° C. for 10 hours.
[0335] <Ingredients> 1,10-Decanedioic Acid 2300g 1,8-Octanediol 2530g Hydroquinone 4.9g
[0336] Thereafter, the temperature was raised to 200° C. and the reaction was carried out for 3 hours, and further for 2 hours at 8.3 kPa to produce crystalline polyester [c4].
[0337] (Preparation of crystalline polyester [c5]) Crystalline polyester [c5] was prepared in the same manner as for crystalline polyester [c4].
[0338] (Preparation of crystalline polyester [c6]) The following components were placed in a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and reacted at 150° C. for 6 hours.
[0339] <Ingredients> 1,4-butanediol 50 moles Fumaric acid 50 moles Hydroquinone 6.0g
[0340] Thereafter, the temperature was raised to 200° C. and the reaction was carried out for 1 hour, and further for 1 hour at 8.3 kPa to produce a crystalline polyester [c6].
[0341] (B.4.2.2) Preparation of each crystalline polyester dispersion (Preparation of Crystalline Polyester Dispersion (C4)) The following ingredients were placed in a 2 L metal container and dissolved by heating at 75°C, then rapidly cooled in an ice-water bath at a rate of 27°C / min.
[0342] <Ingredients> Crystalline polyester [c4] 100g 400g ethyl acetate
[0343] Thereafter, 500 mL of glass beads (3 mm diameter) was added, and the mixture was ground for 10 hours using a batch-type sand mill (Kanpe Hapio Co., Ltd.) to prepare a crystalline polyester dispersion (C4).
[0344] (Preparation of Crystalline Polyester Dispersion (C5)) The following ingredients were placed in a 2 L metal container and dissolved by heating at 75°C, then rapidly cooled in an ice-water bath at a rate of 27°C / min.
[0345] <Ingredients> Crystalline polyester [c5] 100g 400g ethyl acetate
[0346] Thereafter, 500 mL of glass beads (3 mm diameter) was added, and the mixture was ground for 10 hours using a batch-type sand mill (Kanpe Hapio Co., Ltd.) to prepare a crystalline polyester dispersion (C5).
[0347] (Preparation of Crystalline Polyester Dispersion (C6)) The following ingredients were placed in a 2 L metal container and dissolved by heating at 80°C, then rapidly cooled in an ice-water bath at a rate of 27°C / min.
[0348] <Ingredients> Crystalline polyester [c6] 110g 450g ethyl acetate
[0349] Thereafter, 500 mL of glass beads (3 mm diameter) was added, and the mixture was ground for 10 hours using a batch-type sand mill (Kanpe Hapio Co., Ltd.) to prepare a crystalline polyester dispersion (C6).
[0350] (B.4.3) Polyester prepolymer (B.4.3.1) Preparation of intermediate polyester (Preparation of intermediate polyester [p1]) The following components were placed in a reaction vessel equipped with a condenser, a stirrer, and a nitrogen inlet tube, and reacted at normal pressure and 230°C for 8 hours.
[0351] <Ingredients> Ethylene glycol 106 parts by weight Dimethyl terephthalate 245 parts by mass 1,10-Decanedicarboxylic acid 105 parts by mass Dibutyltin oxide 2 parts by mass
[0352] Thereafter, the mixture was reacted for 5 hours under a reduced pressure of 10 to 15 mmHg to prepare an intermediate polyester [p1].
[0353] (Preparation of intermediate polyester [p2]) The following components were placed in a reaction vessel equipped with a condenser, a stirrer, and a nitrogen inlet tube, and reacted at normal pressure and 230°C for 8 hours.
[0354] <Ingredients> Bisphenol A ethylene oxide 2 mole adduct 682 parts by mass Bisphenol A propylene oxide 2 mole adduct 81 parts by mass Terephthalic acid 283 parts by mass Trimellitic anhydride 22 parts by weight Dibutyltin oxide 2 parts by mass
[0355] Thereafter, the mixture was reacted for 5 hours under a reduced pressure of 10 to 15 mmHg to prepare an intermediate polyester [p2].
[0356] (Preparation of intermediate polyester [p3]) The following components were placed in a reaction vessel equipped with a condenser, a stirrer, and a nitrogen inlet tube, and reacted at normal pressure and 240°C for 10 hours.
[0357] <Ingredients> Bisphenol A ethylene oxide 2 mole adduct 700 parts by mass Bisphenol A propylene oxide 2 mole adduct 85 parts by mass Terephthalic acid 300 parts by mass Trimellitic anhydride 25 parts by mass Dibutyltin oxide 3 parts by mass
[0358] Thereafter, the mixture was reacted for 6 hours under a reduced pressure of 10 to 20 mmHg to prepare an intermediate polyester [p3].
[0359] (B.4.3.2) Preparation of polyester prepolymer dispersions (Preparation of polyester prepolymer dispersion (P1)) Next, the following components were placed in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, and reacted at 100° C. for 5 hours.
[0360] <Ingredients> Intermediate polyester [p1] 410 parts by weight Isophorone diisocyanate 89 parts by weight Ethyl acetate 500 parts by weight
[0361] In this way, a polyester prepolymer dispersion (P1) having an isocyanate group was prepared.
[0362] (Preparation of polyester prepolymer dispersion (P2)) Next, the following components were placed in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, and reacted at 100° C. for 5 hours.
[0363] <Ingredients> Intermediate polyester [p2] 410 parts by weight Isophorone diisocyanate 89 parts by weight Ethyl acetate 500 parts by weight
[0364] In this way, a polyester prepolymer dispersion (P2) having an isocyanate group was prepared.
[0365] (Preparation of polyester prepolymer dispersion (P3)) Next, the following components were placed in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, and reacted at 110° C. for 6 hours.
[0366] <Ingredients> Intermediate polyester [p3] 400 parts by weight Isophorone diisocyanate 90 parts by weight Ethyl acetate 500 parts by weight
[0367] This resulted in a polyester prepolymer dispersion (P3) having an isocyanate group.
[0368] (B.4.4) Ketimine compounds (Synthesis of ketimine compound (K1)) The following components were placed in a reaction vessel equipped with a stirring bar and a thermometer, and the mixture was reacted at 50° C. for 5 hours to synthesize ketimine compound (K1).
[0369] <Ingredients> Isophoronediamine 170 parts by mass Methyl ethyl ketone 75 parts by mass
[0370] (Synthesis of ketimine compound (K2)) Ketimine compound (K2) was synthesized in exactly the same manner as for ketimine compound (K1).
[0371] (Synthesis of ketimine compound (K3)) The following components were placed in a reaction vessel equipped with a stirring bar and a thermometer, and the mixture was reacted at 50° C. for 6 hours to synthesize the ketimine compound (K3).
[0372] <Ingredients> Isophoronediamine 180 parts by mass Methyl ethyl ketone 80 parts by mass
[0373] (B.4.5) Water phase (B.4.5.1) Preparation of fine particle dispersion for aqueous phase preparation (Preparation of organic fine particle emulsion (1)) The following components were added to a reaction vessel equipped with a stirring rod and a thermometer and stirred at 400 rpm for 15 minutes, resulting in a white emulsion. <Ingredients> Water 683 parts by mass "Eleminol RS-30" (manufactured by Sanyo Chemical Industries) 11 parts by weight Styrene 138 parts by weight Methacrylic acid 138 parts by mass Ammonium persulfate 1.0 parts by mass
[0374] Incidentally, "Eleminol RS-30" (manufactured by Sanyo Chemical Industries, Ltd.) among the above ingredients is the sodium salt of methacrylic acid ethylene oxide adduct sulfate ester.
[0375] The white emulsion was heated to raise the system temperature to 75° C. and reacted for 5 hours. Then, 30 parts by mass of a 1% aqueous solution of ammonium persulfate was added and aged at 75° C. for 5 hours to prepare an organic fine particle emulsion (1), which is an aqueous dispersion of a vinyl resin (a copolymer of styrene-methacrylic acid-sodium salt of ethylene oxide adduct of methacrylic acid sulfate).
[0376] When the organic fine particle emulsion (1) was measured using a laser diffraction / scattering type particle size distribution measuring device "LA-920" (manufactured by Horiba, Ltd.), the volume average particle size was found to be 0.14 μm.
[0377] (Preparation of organic fine particle emulsion (2)) The following components were added to a reaction vessel equipped with a stirring rod and a thermometer and stirred at 400 rpm for 15 minutes, resulting in a white emulsion.
[0378] <Ingredients> Water 683 parts by mass "Eleminol RS-30" (manufactured by Sanyo Chemical Industries) 11 parts by weight Styrene 138 parts by weight Methacrylic acid 138 parts by mass Ammonium persulfate 1.0 parts by mass
[0379] Incidentally, "Eleminol RS-30" (manufactured by Sanyo Chemical Industries, Ltd.) among the above ingredients is the sodium salt of methacrylic acid ethylene oxide adduct sulfate ester.
[0380] The white emulsion was heated to raise the system temperature to 75° C. and reacted for 5 hours. Then, 30 parts by mass of a 1% aqueous solution of ammonium persulfate was added and aged at 75° C. for 5 hours to obtain an organic fine particle emulsion (2) which is an aqueous dispersion of a vinyl resin (a copolymer of styrene-methacrylic acid-sodium salt of ethylene oxide adduct of methacrylic acid sulfate).
[0381] When the organic fine particle emulsion (2) was measured using a laser diffraction / scattering type particle size distribution measuring device "LA-920" (manufactured by Horiba, Ltd.), the volume average particle size was found to be 0.14 μm.
[0382] (Preparation of organic fine particle emulsion (3)) The following components were added to a reaction vessel equipped with a stirring bar and a thermometer and stirred at 450 rpm for 20 minutes, resulting in a white emulsion.
[0383] <Ingredients> 700 parts by mass of water "Eleminol RS-30" (manufactured by Sanyo Chemical Industries) 12 parts by weight Styrene 140 parts by weight Methacrylic acid 140 parts by mass Ammonium persulfate 1.5 parts by weight
[0384] Incidentally, "Eleminol RS-30" (manufactured by Sanyo Chemical Industries, Ltd.) among the above ingredients is the sodium salt of methacrylic acid ethylene oxide adduct sulfate ester.
[0385] The white emulsion was heated to raise the system temperature to 75° C. and reacted for 5 hours. Then, 35 parts by mass of a 1% aqueous solution of ammonium persulfate was added and aged at 75° C. for 5 hours to prepare an organic fine particle emulsion (3), which is an aqueous dispersion of a vinyl resin (a copolymer of styrene-methacrylic acid-sodium salt of ethylene oxide adduct of methacrylic acid sulfate).
[0386] When the organic fine particle emulsion (3) was measured using a laser diffraction / scattering type particle size distribution measuring device "LA-920" (manufactured by Horiba, Ltd.), the volume average particle size was found to be 0.30 μm.
[0387] (B.4.5.2) Preparation of the aqueous phase (Preparation of Aqueous Phase (1)) A part of the organic fine particle emulsion (1) was dried to isolate the resin content.
[0388] The following ingredients were then mixed and stirred:
[0389] <Ingredients> Water 990 parts by mass Organic fine particle emulsion (1) 83 parts by weight "Eleminol MON-7" (manufactured by Sanyo Chemical Industries) 37 parts by weight Ethyl acetate 90 parts by weight
[0390] The above-mentioned "Eleminol MON-7" (manufactured by Sanyo Chemical Industries, Ltd.) is an aqueous solution of sodium dodecyldiphenyletherdisulfonate. A milky white liquid, water phase (1), was prepared using this.
[0391] (Preparation of aqueous phase (2)) A part of the organic fine particle emulsion (2) was dried to isolate the resin content.
[0392] The following ingredients were then mixed and stirred:
[0393] <Ingredients> Water 990 parts by mass Organic fine particle emulsion (2) 83 parts by weight "Eleminol MON-7" (manufactured by Sanyo Chemical Industries) 37 parts by weight Ethyl acetate 90 parts by weight
[0394] The above-mentioned "Eleminol MON-7" (manufactured by Sanyo Chemical Industries, Ltd.) is an aqueous solution of sodium dodecyldiphenyletherdisulfonate. A milky white liquid, water phase (2), was prepared using this.
[0395] (Preparation of aqueous phase (3)) The following ingredients were mixed and stirred:
[0396] <Ingredients> 1000 parts by mass of water Organic fine particle emulsion (3) 85 parts by weight "Eleminol MON-7" (Sanyo Chemical Industries, Ltd.) 40 parts by weight Ethyl acetate 95 parts by weight
[0397] The above-mentioned "Eleminol MON-7" (manufactured by Sanyo Chemical Industries, Ltd.) is an aqueous solution of sodium dodecyldiphenyletherdisulfonate. A milky white liquid, the aqueous phase (3), was prepared using this solution.
[0398] (B.4.6) Preparation of oil phase (release agent / masterbatch dispersion) (B.4.6.1) Preparation of release agent dispersion (Preparation of release agent dispersion (W2)) The following ingredients were placed in a vessel equipped with a stirring bar and thermometer, heated to 80°C with stirring, maintained at 80°C for 5 hours, and then cooled to 30°C over 1 hour.
[0399] <Ingredients> Amorphous polyester [a7] 378 parts by mass Carnauba wax (release agent) 110 parts by weight CCA 22 parts by mass Ethyl acetate 947 parts by mass
[0400] In addition, the "carnauba wax" in the above components is refined carnauba wax No. 1 powder manufactured by Kato Yoko Co., Ltd. In addition, the "CCA" in the above components is salicylic acid metal complex E-84 (Orient Chemical Industry Co., Ltd.). In this way, a release agent dispersion (W2) was prepared.
[0401] (Preparation of release agent dispersion (W3)) The following ingredients were placed in a vessel equipped with a stirring bar and thermometer, heated to 80°C with stirring, maintained at 80°C for 5 hours, and then cooled to 30°C over 1 hour.
[0402] <Ingredients> Amorphous polyester [a8] 378 parts by mass Carnauba wax (release agent) 110 parts by weight CCA 22 parts by mass Ethyl acetate 947 parts by mass
[0403] In addition, the "carnauba wax" in the above components is refined carnauba wax No. 1 powder manufactured by Kato Yoko Co., Ltd. In addition, the "CCA" in the above components is salicylic acid metal complex E-84 (Orient Chemical Industry Co., Ltd.). In this way, a release agent dispersion (W3) was prepared.
[0404] (Preparation of release agent dispersion (W4)) The following ingredients were placed in a vessel equipped with a stirring bar and thermometer, heated to 80°C with stirring, held at 80°C for 8 hours, and then cooled to 24°C over 1 hour.
[0405] <Ingredients> Amorphous polyester [a9] 400 parts by mass Microcrystalline wax (release agent) 100 parts by weight CCA 20 parts by mass Ethyl acetate 1000 parts by mass
[0406] The "microcrystalline wax" in the above components has an acid value of 0.1 mgKOH / g, a melting point of 65°C, a carbon number of 80, and a linear hydrocarbon ratio of 70% by weight. The "CCA" in the above components is salicylic acid metal complex E-84 (Orient Chemical Industry). A release agent dispersion (W4) was prepared in this manner.
[0407] (B.4.6.2) Masterbatches (Preparation of Masterbatch [1]) The following ingredients were added and mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.).
[0408] <Ingredients> Carbon black (pigment) 540 parts by weight Amorphous polyester [a7] 1200 parts by mass
[0409] The carbon black used is "Printex35" (manufactured by Dexa) [DBP oil absorption: 43 mL / 100 mg, pH: 9.5].
[0410] The mixture was then kneaded using two rolls at 150°C for 30 minutes, further rolled and cooled, and pulverized in a pulverizer to produce master batch [1].
[0411] (Preparation of Masterbatch [2]) The following ingredients were added and mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.).
[0412] <Ingredients> Carbon black (pigment) 540 parts by weight Amorphous polyester [a8] 1200 parts by mass
[0413] The carbon black used is "Printex35" (manufactured by Dexa) [DBP oil absorption: 43 mL / 100 mg, pH: 9.5].
[0414] The mixture was then kneaded using two rolls at 150°C for 30 minutes, further rolled and cooled, and pulverized in a pulverizer to produce master batch [2].
[0415] (Preparation of Masterbatch [3]) The following ingredients were added and mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.).
[0416] <Ingredients> Carbon black (pigment) 550 parts by weight Amorphous polyester [a9] 1,300 parts by mass
[0417] The carbon black used is "Printex35" (manufactured by Dexa) [DBP oil absorption: 43 mL / 100 mg, pH: 9.5].
[0418] The mixture was then kneaded using two rolls at 160°C for 45 minutes, further rolled and cooled, and pulverized in a pulverizer to produce master batch [3].
[0419] (B.4.6.3) Raw material solution (Preparation of raw material solution (1)) The following components were charged into the vessel containing the release agent dispersion (W2) and mixed for 1 hour to prepare a raw material solution (1).
[0420] <Ingredients> Masterbatch [1] 480 parts by mass Ethyl acetate 550 parts by weight
[0421] (Preparation of raw material solution (2)) The following components were charged into the vessel containing the release agent dispersion (W3) and mixed for 1 hour to prepare a raw material solution (2).
[0422] <Ingredients> Masterbatch [2] 480 parts by mass Ethyl acetate 550 parts by weight
[0423] (Preparation of raw material solution (3)) The following components were charged into the vessel containing the release agent dispersion (W4) and mixed for 1 hour to prepare a raw material solution (3).
[0424] <Ingredients> Masterbatch [3] 480 parts by mass Ethyl acetate 550 parts by weight
[0425] (B.4.6.4) Dispersion and addition of each solution (Preparation of Oil Phase (1)) 1324 parts by mass of the raw material solution (1) was transferred to another container, and the carbon black and the release agent were dispersed using a bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.) under the following conditions.
[0426] <Condition> Liquid delivery speed: 1kg / hour Disk speed: 6m / sec 0.5mm zirconia beads, 80% by volume, 3 passes
[0427] Next, 1042.3 parts by mass of a 65% ethyl acetate solution of amorphous polyester [a7] (a solution in which amorphous polyester [a7] was dissolved in ethyl acetate at 65% by mass) was added, and the mixture was passed once through the bead mill under the above conditions to prepare an oil phase (1).
[0428] The solid content concentration of the oil phase (1) (130° C., 30 minutes) was 50 mass %.
[0429] (Preparation of Oil Phase (2)) 1324 parts by mass of the raw material solution (2) was transferred to another container, and the carbon black and the release agent were dispersed using a bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.) under the following conditions.
[0430] <Condition> Liquid delivery speed: 1kg / hour Disk speed: 6m / sec 0.5mm zirconia beads, 80% by volume, 3 passes
[0431] Next, 1042.3 parts by mass of a 65% ethyl acetate solution of amorphous polyester [a8] (a solution in which amorphous polyester [a8] was dissolved in ethyl acetate at 65% by mass) was added, and the mixture was passed once through the bead mill under the above conditions to prepare oil phase (2).
[0432] The solid content concentration of the oil phase (2) (130° C., 30 minutes) was 50 mass %.
[0433] (Preparation of Oil Phase (3)) 1324 parts by mass of the raw material solution (3) was transferred to another container, and the carbon black and the release agent were dispersed using a bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.) under the following conditions.
[0434] <Condition> Liquid delivery speed: 1kg / hour Disk speed: 6m / sec 0.5mm zirconia beads, 80% by volume, 3 passes
[0435] Next, 1,000 parts by mass of a 65% ethyl acetate solution of amorphous polyester [a9] (a solution in which amorphous polyester [a9] was dissolved in ethyl acetate at 65% by mass) was added, and the mixture was passed once through the bead mill under the above conditions to prepare an oil phase (3).
[0436] The solid content concentration of the oil phase (3) (130° C., 30 minutes) was 53 mass %.
[0437] (B.5) Preparation of Toner 4 (B.5.1) Preparation of toner base particles [4] (emulsification process) The following ingredients were placed in a container and mixed for 1 minute at 5,000 rpm using a TK Homomixer (manufactured by Tokushu Kika).
[0438] <Ingredients> Oil phase (1) 664 parts by mass Polyester prepolymer dispersion (P1) 109.4 parts by weight Crystalline polyester dispersion (C4) 73.9 parts by weight Ketimine compound (K1) 4.6 parts by mass
[0439] Thereafter, 1,200 parts by mass of the aqueous phase (1) was added to the vessel and mixed with a TK homomixer at a rotation speed of 13,000 rpm for 20 minutes to obtain an emulsified slurry [1].
[0440] (Desolution process) The emulsified slurry [1] was placed in a vessel equipped with a stirrer and a thermometer, and the mixture was desolvated at 30° C. for 8 hours, and then aged at 45° C. for 4 hours to obtain a dispersed slurry [1].
[0441] (Washing and drying process) 100 parts by mass of the dispersion slurry [1] is filtered under reduced pressure, (1) 100 parts by mass of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes), and then filtered.
[0442] (2): 100 parts by mass of a 10% aqueous sodium hydroxide solution was added to the filter cake of (1), and the mixture was mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 30 minutes), followed by filtration under reduced pressure.
[0443] (3): 100 parts by mass of 10% hydrochloric acid was added to the filter cake of (2), and the mixture was mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes) and then filtered.
[0444] (4): 300 parts by mass of ion-exchanged water was added to the filter cake of (3), and the mixture was mixed in a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes), followed by filtering twice to obtain a filter cake [1].
[0445] The filtered cake [1] was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a 75 μm mesh to prepare toner base particles [4].
[0446] (B.5.2) Addition of external additives and measurement of glass transition temperature External additives were added in the same manner as in Toner 1. The glass transition temperature was also measured in the same manner, and the glass transition temperature (Tg) of Toner 4 was found to be 0.1°C.
[0447] (B.6) Preparation of Toner 5 (B.6.1) Preparation of toner base particles [5] (emulsification process) The following ingredients were placed in a container and mixed for 1 minute at 5,000 rpm using a TK Homomixer (manufactured by Tokushu Kika).
[0448] <Ingredients> Oil phase (2) 664 parts by mass Polyester prepolymer dispersion (P2) 109.4 parts by weight Crystalline polyester dispersion (C5) 73.9 parts by weight Ketimine compound (K2) 4.6 parts by mass
[0449] Thereafter, 1,200 parts by mass of the aqueous phase (2) was added to the vessel and mixed with a TK homomixer at a rotation speed of 13,000 rpm for 20 minutes to obtain an emulsified slurry [2].
[0450] (Desolution process) The emulsified slurry [2] was placed in a vessel equipped with a stirrer and a thermometer, and the mixture was desolvated at 30° C. for 8 hours, and then aged at 45° C. for 4 hours to obtain a dispersed slurry [2].
[0451] (Washing and drying process) 100 parts by mass of the dispersion slurry [2] is filtered under reduced pressure, (1) 100 parts by mass of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes), and then filtered.
[0452] (2): 100 parts by mass of a 10% aqueous sodium hydroxide solution was added to the filter cake of (1), and the mixture was mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 30 minutes), followed by filtration under reduced pressure.
[0453] (3): 100 parts by mass of 10% hydrochloric acid was added to the filter cake of (2), and the mixture was mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes) and then filtered.
[0454] (4): 300 parts by mass of ion-exchanged water was added to the filter cake of (3), mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes), and then filtered twice to obtain a filter cake [2].
[0455] The filtered cake [2] was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a 75 μm mesh to prepare toner base particles [5].
[0456] (B.6.2) Addition of external additives and measurement of glass transition temperature The external additives were added in the same manner as in Toner 1. The glass transition temperature was also measured in the same manner, and the glass transition temperature (Tg) of Toner 5 was found to be 26.3°C.
[0457] (B.7) Preparation of Toner 6 (B.7.1) Preparation of toner base particles [6] (emulsification process) The following ingredients were placed in a container and mixed for 1 minute at 6,000 rpm using a TK Homomixer (manufactured by Tokushu Kika).
[0458] <Ingredients> Oil phase (3) 700 parts by mass Polyester prepolymer dispersion (P2) 120 parts by weight Crystalline polyester dispersion (C6) 80 parts by weight Ketimine compound (K3) 5 parts by mass
[0459] Thereafter, 1,300 parts by mass of the aqueous phase (3) was added to the vessel and mixed with a TK homomixer at a rotation speed of 13,000 rpm for 20 minutes to obtain an emulsified slurry [3].
[0460] (Desolution process) The emulsified slurry [3] was placed in a vessel equipped with a stirrer and a thermometer, and the mixture was desolvated at 30° C. for 10 hours, and then aged at 45° C. for 5 hours to obtain a dispersed slurry [3].
[0461] (Washing and drying process) 100 parts by mass of the dispersion slurry [3] is filtered under reduced pressure, (1) 100 parts by mass of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes), and then filtered.
[0462] (2): 100 parts by mass of a 10% aqueous sodium hydroxide solution was added to the filter cake of (1), and the mixture was mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 30 minutes), followed by filtration under reduced pressure.
[0463] (3): 100 parts by mass of 10% hydrochloric acid was added to the filter cake of (2), and the mixture was mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes) and then filtered.
[0464] (4): 300 parts by mass of ion-exchanged water was added to the filter cake of (3), mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered twice to obtain a filter cake [3].
[0465] The filtered cake [3] was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a 75 μm mesh to prepare toner base particles [6].
[0466] (B.7.2) Addition of external additives and measurement of glass transition temperature The external additives were added in the same manner as in Toner 1. The glass transition temperature was also measured in the same manner, and the glass transition temperature (Tg) of Toner 6 was 37.2°C.
[0467] The components of the toner base particles [4] to [6] are shown in Table IV. The types and amounts of external additives of toners 4 to 6, as well as the polyester content and glass transition temperature in the toners containing the external additives, are shown in Table V.
[0468] [Table 4]
[0469] [Table 5]
[0470] (B.8) Preparation of Toner 7 (B.8.1) Preparation of dispersion for core part (B.8.1.1) Vinyl resin dispersions (Preparation of vinyl resin dispersion (D1)) (1) First-stage polymerization A 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device was charged with 8 parts by mass of sodium dodecyl sulfate and 3,000 parts by mass of ion-exchanged water, and the internal temperature was raised to 80° C. while stirring at a speed of 230 rpm under a nitrogen stream. After the temperature was raised, a solution in which 10 parts by mass of potassium persulfate was dissolved in 200 parts by mass of ion-exchanged water was added, the liquid temperature was again raised to 80° C., and the following components were added dropwise over 1 hour.
[0471] <Ingredients> n-Butyl acrylate 526 parts by weight Methacrylic acid 474 parts by mass
[0472] After the dropwise addition, polymerization was carried out by heating and stirring at 80° C. for 2 hours to prepare a dispersion liquid of vinyl resin particles [d1].
[0473] (2) Second-stage polymerization: formation of the intermediate layer A solution of 7 parts by mass of sodium dodecyl sulfate dissolved in 3,000 parts by mass of ion-exchanged water was charged into a 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and heated to 98° C. After heating, 300 parts by mass, calculated as solid content, of the dispersion of vinyl resin particles [d1] prepared by the above first-stage polymerization and a mixed solution of the following monomers, chain transfer agent, and release agent dissolved at 90° C. were added thereto.
[0474] <Ingredients> 2-Ethylhexyl acrylate 90.5 parts by mass Methacrylic acid 33.1 parts by mass n-Octyl mercaptan (chain transfer agent) 5.5 parts by mass Behenyl behenate (release agent, melting point 73°C) 130.0 parts by mass
[0475] A mixing and dispersion process was carried out for 1 hour using a mechanical disperser CLEARMIX (manufactured by M-Technique Co., Ltd.) with a circulation path to prepare a dispersion containing emulsified particles (oil droplets). A polymerization initiator solution in which 6 parts by mass of potassium persulfate was dissolved in 200 parts by mass of ion-exchanged water was added to this dispersion, and the system was heated and stirred at 78°C for 1 hour to polymerize, preparing a dispersion of vinyl resin particles [d2].
[0476] (3) Third-stage polymerization: formation of the outer layer 400 parts by mass of ion-exchanged water was further added to the dispersion of vinyl resin particles [d2] obtained by the second-stage polymerization and mixed thoroughly. Then, a solution of 6.0 parts by mass of potassium persulfate dissolved in 400 parts by mass of ion-exchanged water was added. Furthermore, the following components were added dropwise over 1 hour at a temperature of 81°C.
[0477] <Ingredients> n-Butyl acrylate 143.2 parts by mass Methacrylic acid 52.0 parts by mass n-Octyl mercaptan (chain transfer agent) 8.0 parts by mass
[0478] After the dropwise addition was completed, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28° C. to prepare a vinyl resin dispersion (D1).
[0479] The weight average molecular weight (Mw) of the vinyl resin in the vinyl resin dispersion (D1) was 35,000.
[0480] (Preparation of vinyl resin dispersions (D2) and (D3)) Vinyl resin dispersions (D2) and (D3) were prepared in the same manner as in the preparation of vinyl resin dispersion (D1), except that the components in the first, second and third polymerization stages were as follows.
[0481] [Components in the preparation of vinyl resin dispersion (D2)] <Components of the first polymerization step> n-Butyl acrylate 396 parts by weight Methacrylic acid 604 parts by mass
[0482] <Components of the second stage polymerization> 2-Ethylhexyl acrylate 90.5 parts by mass Methacrylic acid 33.1 parts by mass n-Octyl mercaptan (chain transfer agent) 5.5 parts by mass Behenyl behenate (release agent, melting point 73°C) 130.0 parts by mass
[0483] <Components of the third polymerization step> n-Butyl acrylate 143.2 parts by mass Methacrylic acid 200.5 parts by mass n-Octyl mercaptan (chain transfer agent) 8.0 parts by mass
[0484] [Components in the preparation of vinyl resin dispersion (D3)] <Components of the first polymerization step> Styrene 480.0 parts by mass n-Butyl acrylate 250.0 parts by mass Methacrylic acid 68.0 parts by mass
[0485] <Components of the second stage polymerization> Styrene 243.0 parts by mass 2-Ethylhexyl acrylate 90.5 parts by mass Methacrylic acid 33.1 parts by mass n-Octyl mercaptan (chain transfer agent) 5.5 parts by mass Behenyl behenate (release agent, melting point 73°C) 130.0 parts by mass
[0486] <Components of the third polymerization step> Styrene 354.8 parts by mass n-Butyl acrylate 143.2 parts by mass Methacrylic acid 52.0 parts by mass n-Octyl mercaptan (chain transfer agent) 8.0 parts by mass
[0487] (B.8.1.2) Crystalline polyester dispersions (Preparation of Crystalline Polyester Dispersion (E1)) The following components for the vinyl polymerization segment (styrene·acrylic polymerization segment, St·Ac segment) containing bireactive monomers were placed in a dropping funnel.
[0488] <Ingredients> n-Butyl acrylate 12 parts by weight Acrylic acid 2 parts by mass Radical polymerization initiator (di-t-butyl peroxide) 7 parts by mass
[0489] Furthermore, the raw material monomers for the crystalline polyester polymerized segment (CPEs segment) described below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and were heated to 170° C. to dissolve.
[0490] <Raw material monomer> Ethylene glycol 106 parts by weight Dimethyl terephthalate 245 parts by mass 1,10-Decanedicarboxylic acid 105 parts by mass
[0491] Next, the raw material monomer for the vinyl polymerization segment was dropped over 90 minutes while stirring, and the mixture was aged for 60 minutes. After that, the unreacted raw material monomer for the vinyl polymerization segment was removed under reduced pressure (8 kPa). The amount of the monomer removed was very small compared to the amount of the monomer for the vinyl polymerization segment.
[0492] Thereafter, 0.8 parts by mass of Ti(On-Bu)4 was added as an esterification catalyst, the temperature was raised to 235°C, and the reaction was carried out under normal pressure (101.3 kPa) for 5 hours, and further under reduced pressure (8 kPa) for 1 hour.
[0493] Next, after cooling to 200°C, the mixture was reacted for 1 hour under reduced pressure (20 kPa) to produce crystalline polyester [e1], which is a hybrid crystalline polyester.
[0494] The crystalline polyester (e1) contained 8 mass% of polymerized segments other than CPEs segments (St·Ac segments) relative to the total mass of the polyester, and was a resin in which the CPEs segments were grafted to the St·Ac segments.
[0495] 30 parts by mass of the crystalline polyester [e1] was melted and transferred in the molten state to an emulsifying and dispersing machine "Cavitron CD1010" (manufactured by Eurotech Co., Ltd.) at a transfer rate of 100 parts by mass per minute. Simultaneously with the transfer of the crystalline polyester [e1] in the molten state, dilute ammonia water with a concentration of 0.37% by mass, which was obtained by diluting 70 parts by mass of reagent ammonia water with ion-exchanged water in a separate aqueous solvent tank, was transferred to the emulsifying and dispersing machine "Cavitron CD1010" (manufactured by Eurotech Co., Ltd.) at a transfer rate of 0.1 liters per minute while being heated to 100°C by a heat exchanger.
[0496] The emulsion dispersion machine was then operated at a rotor speed of 60Hz and a pressure of 5kg / cm 2 A crystalline polyester dispersion (E1) having a solid content of 30 mass% was prepared by operating under the above conditions. At this time, the volume-based median diameter of the crystalline polyester particles contained in the crystalline polyester dispersion (E1) was 200 nm.
[0497] (Preparation of Crystalline Polyester Dispersion (E2)) A crystalline polyester dispersion (E2) was prepared in the same manner as the preparation of the crystalline polyester dispersion (E1), except that the components of the vinyl polymer segment (styrene·acrylic polymer segment, St·Ac segment) and the raw material monomers of the crystalline polyester polymer segment (CPEs segment) were as follows.
[0498] <Components of the St·Ac segment> 12 parts by mass of n-butyl acrylate 2 parts by mass of acrylic acid 7 parts by mass of a radical polymerization initiator (di-t-butyl peroxide)
[0499] <Components of the CPEs segment> 210 parts by mass of bisphenol A ethylene oxide adduct 230 parts by mass of bisphenol A propylene oxide adduct 30 parts by mass of terephthalic acid 135 parts by mass of fumaric acid 40 parts by mass of tetrapropenyl succinic anhydride
[0500] (Preparation of crystalline polyester dispersion (E3)) A crystalline polyester dispersion (E3) was prepared in the same manner as the preparation of the crystalline polyester dispersion (E1), except that the components of the vinyl polymer segment (styrene·acrylic polymer segment, St·Ac segment) and the raw material monomers of the crystalline polyester polymer segment (CPEs segment) were as follows.
[0501] <Components of the St·Ac segment> 34 parts by mass of styrene 12 parts by mass of n-butyl acrylate 2 parts by mass of acrylic acid 7 parts by mass of a radical polymerization initiator (di-t-butyl peroxide)
[0502] <Components of the CPEs segment> 281 parts by mass of hexadecanedioic acid 1,4-butanediol 94 parts by mass
[0503] (B.8.2) Dispersion for shell layer (Preparation of amorphous polyester dispersion (F)) The following components for the vinyl polymerization segment (St·Ac segment), containing both reactive monomers, were placed in a dropping funnel.
[0504] <Ingredients> Styrene 80 parts by weight n-Butyl acrylate 20 parts by weight Acrylic acid 10 parts by mass Radical polymerization initiator (di-t-butyl peroxide) 16 parts by mass
[0505] Furthermore, the raw material monomers for the amorphous polyester polymer segment (APEs segment) described below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and were heated to 170° C. to dissolve.
[0506] <Raw material monomer> Bisphenol A propylene oxide 2 mole adduct 228.6 parts by mass Bisphenol A ethylene oxide 2 mole adduct 57.1 parts by mass Terephthalic acid 66.9 parts by mass Fumaric acid 47.4 parts by mass
[0507] Next, the raw material monomer of the vinyl polymerization segment was dropped under stirring over 90 minutes, and after aging for 60 minutes, the unreacted raw material monomer of the vinyl polymerization segment was removed under reduced pressure (8 kPa). Then, 0.4 parts by mass of Ti(On-Bu)4 was added as an esterification catalyst, and the temperature was raised to 235°C, and the reaction was carried out at normal pressure (101.3 kPa) for 5 hours and further at reduced pressure (8 kPa) for 1 hour.
[0508] Next, after cooling to 200° C., the reaction was carried out under reduced pressure (20 kPa) until the desired softening point was reached. Next, desolvation was carried out to produce an amorphous polyester [f1].
[0509] The amorphous polyester [f1] contained 8 mass% of polymerized segments other than APEs segments (St·Ac segments) relative to the total mass of the polyester, and was a hybrid amorphous polyester in which the APEs segments were grafted to the St·Ac segments.
[0510] 100 parts by mass of the prepared amorphous polyester [f1] was dissolved in 400 parts by mass of ethyl acetate (manufactured by Kanto Chemical Co., Ltd.), and further mixed with 638 parts by mass of a 0.26% by mass concentration sodium lauryl sulfate solution prepared in advance, and ultrasonically dispersed for 30 minutes at V-LEVEL 300μA with stirring using an ultrasonic homogenizer "US-150T" (manufactured by Nippon Seiki Co., Ltd.).
[0511] After that, the mixture was heated to 40°C and stirred under reduced pressure for 3 hours using a diaphragm vacuum pump "V-700" (manufactured by BUCHI) to completely remove the ethyl acetate, thereby preparing an amorphous polyester dispersion (F) with a solid content of 13.5 mass%.
[0512] (B.8.3) Colorant dispersions (Preparation of Black Colorant Dispersion (B2)) 90 parts by mass of sodium dodecyl sulfate was dissolved in 1600 parts by mass of ion-exchanged water by stirring. While stirring this solution, 420 parts by mass of carbon black "Regal 330R" (manufactured by Cabot Corporation) was gradually added, and then the solution was dispersed using a stirring device "Clearmix" (manufactured by M Technique Co., Ltd.) to prepare black colorant dispersion (B2). The particle size of the colorant particles in the black colorant dispersion (B2) was measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.) and found to be 110 nm.
[0513] (B.8.4) Preparation of toner base particles [7] Into a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube, 285 parts by mass (solid content equivalent) of the vinyl resin dispersion (D1) for the core part, 40 parts by mass (solid content equivalent) of the crystalline polyester dispersion (E1) for the other core part, and 2,000 parts by mass of ion-exchanged water were added.
[0514] Furthermore, dodecyldiphenyletherdisulfonic acid sodium salt was added in an amount of 1 mass % (solid content equivalent) based on the total amount of the vinyl resin and the crystalline polyester, and then the pH was adjusted to 10 by adding a 5 mol / L aqueous sodium hydroxide solution.
[0515] Then, 30 parts by mass (solid content equivalent) of black colorant dispersion (B2) was added, and then an aqueous solution in which 60 parts by mass of magnesium chloride was dissolved in 60 parts by mass of ion-exchanged water was added under stirring over 10 minutes at 30° C. After that, the mixture was left for 3 minutes, and then heating was started, and the temperature of this system was raised to 80° C. over 60 minutes.
[0516] After the temperature reached 80°C, the stirring speed was adjusted so that the particle size growth rate was 0.01 μm / min. At this time, the particle size of the associated particles was measured using a Coulter Multisizer 3 (Beckman Coulter, Inc.), and the particles were allowed to grow until the volume-based median diameter reached 6.0 μm.
[0517] Then, 37 parts by mass (solid content equivalent) of amorphous polyester dispersion (F) for the shell layer was added over 30 minutes, and when the supernatant of the reaction solution became transparent, an aqueous solution of 190 parts by mass of sodium chloride dissolved in 760 parts by mass of ion-exchanged water was added to stop particle growth. The temperature was then raised and the mixture was heated and stirred at 80°C to promote particle fusion, and the average circularity of the toner was measured (HPF detection number: 4000) using a measuring device "FPIA-3000" (manufactured by Sysmex Corporation), and when the average circularity reached 0.970, the mixture was cooled to 30°C at a cooling rate of 2.5°C / min.
[0518] Next, the toner cake was subjected to solid-liquid separation, and the dehydrated toner cake was redispersed in ion-exchanged water and subjected to solid-liquid separation. This procedure was repeated three times to wash the toner cake, and then the toner cake was dried at 40°C for 24 hours to prepare toner base particles [7].
[0519] (B.8.5) Addition of external additives and measurement of glass transition temperature External additives were added in the same manner as for Toner 1. Furthermore, the glass transition temperature was measured in the same manner as for Toner 1, and the glass transition temperature (Tg) of Toner 7 was 0.3°C.
[0520] (B.9) Preparation of Toners 8 and 9 Toner base particles [8] and [9] were prepared in the same manner as in the preparation of toner base particles [7], except that the components of the toner base particles were those shown in Table VI.
[0521] In Table VI, the amorphous PEs [D1], [D2], [D3], and [F] are the solid content equivalents of the amorphous polyester dispersions (D1), (D2), (D3), and (F), the crystalline PEs [E1], [E2], and [E3] are the solid content equivalents of the crystalline polyester dispersions [E1], [E2], and [E3], and the colorant [B2] is the solid content equivalent of the colorant dispersion (B2).
[0522] [Table 6]
[0523] Further, toners 8 and 9 were prepared by adding external additives to the above toner base particles [8] and [9] in the same manner as in the case of toner 1, and the glass transition temperatures were measured.
[0524] Table VII shows the types and amounts of external additives, the polyester content in the toner containing the external additives, and the glass transition temperatures of toners 7 to 9.
[0525] [Table 7]
[0526] (B.10) Preparation of Toner 10 (B.10.1) Preparation of amorphous polyester [a10] The following polyester monomer was added, and 2 parts by mass of tetrabutyl titanate was added as a condensation catalyst, and the reaction was carried out at 220° C. in a nitrogen stream while distilling off the generated water.
[0527] <Polyester Monomer> Ethylene glycol 108 parts by weight Dimethyl terephthalate 245 parts by mass 1,10-decanedicarboxylic acid 105 parts by mass
[0528] Then, the mixture was cooled to 180° C. After the reaction was completed, the mixture was taken out of the vessel, cooled, and pulverized to prepare the amorphous polyester a10.
[0529] (B.10.2) Preparation of magnetic material [1] The magnetic material used to prepare the magnetic toner core base particles has a number average particle diameter D1 of 120 nm, an octahedral shape, and a saturation magnetization of 88 Am at 796 kA / m. 2 A magnetic material [1] weighing 1.0 g / kg was prepared.
[0530] (B.10.3) Preparation of magnetic toner core base particles [10c] The following components were premixed in a Henschel mixer, and then melt-kneaded using a PCM-30 (manufactured by Ikegai Iron Works) with the temperature set so that the molten temperature at the discharge outlet was 150°C.
[0531] <Ingredients> Amorphous polyester [a10] 100 parts by mass Magnetic material [1] 60 parts by mass Sasol Wax C105 (manufactured by Sasol) 1 part by weight Charge control agent "T-77" (manufactured by Hodogaya Chemical Co., Ltd.) 2 parts by weight
[0532] In addition, Sasolwax C105 (manufactured by Sasol) in the above ingredients is a Fischer-Tropsch wax with a melting point of 105°C.
[0533] The resulting kneaded product was cooled, coarsely pulverized with a hammer mill, and then finely pulverized with a Turbo Mill T250 (manufactured by Turbo Kogyo Co., Ltd.) The finely pulverized powder was classified with a multi-division classifier utilizing the Coanda effect to produce magnetic toner core base particles [10c] with a weight average particle size (D4) of 6.5 μm.
[0534] (B.10.4) Preparation of toner base particles
[10] (Surface modification of magnetic toner core particles using inorganic particles) The following materials were put into the "High-velocity air current impact method: Hybridization system (Nara Machinery Manufacturing Co., Ltd.)" to prepare an ordered mixture.
[0535] Magnetic toner core base particles [10c] 100 parts by weight Inorganic fine particles "X24" (for surface modification) 4.5 parts by weight
[0536] The inorganic fine particles "X24" used herein are sol-gel silica spherical fine particles "X24-9163A" manufactured by Shin-Etsu Chemical Co., Ltd., and have an average particle size of 110 nm.
[0537] After that, the blade rotation speed and product temperature were controlled to fix the inorganic fine particles "X24" on the surface of the magnetic toner core base particle [10c], producing the toner base particle
[10] . At this time, the weight average particle size of the toner base particle
[10] with the inorganic fine particles "X24" fixed thereon was 6.7 μm.
[0538] (B.10.5) Addition of external additives and measurement of glass transition temperature The following fine particles were externally added to 100 parts by mass of the toner base particles
[10] and mixed using a Henschel mixer (FM-10, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.).
[0539] <Fine particles> Hydrophobic silica particles [1] 0.5 parts by weight Hydrophobic silica fine particles [2] 0.5 parts by weight
[0540] The above hydrophobic silica fine particles [1] are hydrophobic silica fine particles having a number-average primary particle size of 20 nm and surface-treated with 25% by mass of hexamethyldisilazane.
[0541] The hydrophobic silica fine particles [2] are hydrophobic silica fine particles having a number-average primary particle size of 40 nm and surface-treated with 15% by mass of hexamethyldisilazane.
[0542] The glass transition temperature (Tg) of Toner 10 was measured in the same manner as for Toner 1, and it was found to be 0.2°C.
[0543] (B.11) Preparation of Toner 11 (B.11.1) Preparation of amorphous polyester [a11] The following polyester monomer was added, and 2 parts by mass of tetrabutyl titanate was added as a condensation catalyst, and the reaction was carried out at 220° C. in a nitrogen stream while distilling off the generated water.
[0544] <Polyester Monomer> Ethylene glycol 108 parts by weight Dimethyl terephthalate 280 parts by mass 1,10-decanedicarboxylic acid 70 parts by mass
[0545] Then, the mixture was cooled to 180° C. After the reaction was completed, the mixture was taken out of the vessel, cooled, and pulverized to prepare the amorphous polyester a11.
[0546] (B.11.2) Preparation of magnetic material [2] The magnetic material used to prepare the magnetic toner core base particles has a number average particle diameter D1 of 120 nm, an octahedral shape, and a saturation magnetization of 88 Am at 796 kA / m. 2 A magnetic material [2] with a mass of 1.0 g / kg was prepared.
[0547] (B.11.3) Preparation of magnetic toner core base particles [11c] The following components were premixed in a Henschel mixer, and then melt-kneaded using a PCM-30 (manufactured by Ikegai Iron Works) with the temperature set so that the molten temperature at the discharge outlet was 150°C.
[0548] <Ingredients> Amorphous polyester [a11] 100 parts by mass Magnetic material [2] 60 parts by mass Sasol Wax "C105" (manufactured by Sasol) 1 part by weight Charge control agent "T-77" (manufactured by Hodogaya Chemical Co., Ltd.) 2 parts by weight
[0549] In addition, the Sasol wax "C105" (manufactured by Sasol) in the above ingredients is a Fischer-Tropsch wax with a melting point of 105°C.
[0550] The resulting kneaded product was cooled, coarsely pulverized with a hammer mill, and then finely pulverized with a Turbo Mill T250 (manufactured by Turbo Kogyo Co., Ltd.) The finely pulverized powder was classified with a multi-division classifier utilizing the Coanda effect to produce magnetic toner core base particles [11c] with a weight average particle size (D4) of 6.5 μm.
[0551] (B.11.4) Preparation of toner base particles
[11] (Surface modification of magnetic toner core particles using inorganic particles) The following materials were put into the "High-velocity air current impact method: Hybridization system (Nara Machinery Manufacturing Co., Ltd.)" to prepare an ordered mixture.
[0552] Magnetic toner core base particles [11c] 100 parts by weight Inorganic fine particles "X24" (for surface modification) 3.5 parts by weight
[0553] The inorganic fine particles "X24" used herein are sol-gel silica spherical fine particles "X24-9600A-80" manufactured by Shin-Etsu Chemical Co., Ltd., and have an average particle size of 80 nm.
[0554] Thereafter, the blade rotation speed and the product temperature were controlled to fix the inorganic fine particles "X24" onto the surface of the magnetic toner core base particle [11c], thereby producing the toner base particle
[11] .
[0555] (B.11.5) Addition of external additives and measurement of glass transition temperature The external additives were added in the same manner as in Toner 10. The glass transition temperature was measured in the same manner as in Toner 1, and the glass transition temperature (Tg) of Toner 11 was 28.6°C.
[0556] (B.12) Preparation of Toner 12 (B.12.1) Preparation of amorphous polyester particles [a12] The following polyester monomer was added, and 2 parts by mass of tetrabutyl titanate was added as a condensation catalyst, and the reaction was carried out at 220° C. in a nitrogen stream while distilling off the generated water.
[0557] <Polyester Monomer> Bisphenol A propylene oxide 2 mole adduct 400 parts by mass Bisphenol A propylene oxide 3 mole adduct 280 parts by mass Terephthalic acid 120 parts by mass Isophthalic acid 120 parts by weight
[0558] Then, the mixture was cooled to 180° C., and 250 parts by mass of trimellitic anhydride was added thereto to carry out a reaction. After the reaction was completed, the mixture was taken out of the vessel, cooled, and pulverized to prepare an amorphous polyester (a12).
[0559] (B.12.2) Preparation of magnetic material [3] The magnetic material used to prepare the magnetic toner core base particles has a number average particle diameter D1 of 120 nm, an octahedral shape, and a saturation magnetization of 88 Am at 796 kA / m. 2 A magnetic material [3] with a mass of 1.0 g / kg was prepared.
[0560] (B.12.3) Preparation of magnetic toner core base particles [12c] The following components were premixed in a Henschel mixer, and then melt-kneaded using a PCM-30 (manufactured by Ikegai Iron Works) with the temperature set so that the molten temperature at the discharge outlet was 150°C.
[0561] <Ingredients> Amorphous polyester [a12] 100 parts by mass Magnetic material [3] 60 parts by mass Sasol Wax C105 (manufactured by Sasol) 1 part by weight Charge control agent "T-77" (manufactured by Hodogaya Chemical Co., Ltd.) 2 parts by weight
[0562] In addition, Sasolwax C105 (manufactured by Sasol) in the above ingredients is a Fischer-Tropsch wax with a melting point of 105°C.
[0563] The kneaded product thus obtained was cooled, coarsely pulverized in a hammer mill, and then finely pulverized using a Turbo Mill T250 (manufactured by Turbo Kogyo Co., Ltd.) as a pulverizer. The finely pulverized powder thus obtained was classified using a multi-division classifier utilizing the Coanda effect to produce magnetic toner core base particles [12c] having a weight average particle size (D4) of 6.7 μm.
[0564] (B.12.4) Preparation of toner base particles
[12] For the toner base particles
[12] , the magnetic toner core base particles were not subjected to surface modification treatment with inorganic particles, and the magnetic toner core base particles [12c] were used as they were as the toner base particles
[12] . The weight average particle size of the toner base particles
[12] was 6.7 μm.
[0565] (B.12.5) Addition of external additives and measurement of glass transition temperature The external additives were added in the same manner as in Toner 10. The glass transition temperature was measured in the same manner as in Toner 1, and the glass transition temperature (Tg) of Toner 12 was 38.2°C.
[0566] The components and amounts added of the magnetic toner core base particles [10c], [11c] and [12c] are shown in Table VIII.
[0567] In addition, the magnetic toner core base particles [10c] and [11c] used to prepare the toner base particles
[10] and the toner base particles
[11] were subjected to a surface modification treatment using the "High-velocity airflow impact method: Hybridization System (Nara Machinery Manufacturing Co., Ltd.)", and the combinations and amounts added are summarized in Table IX.
[0568] Table X shows the toner base particles of toners 10 to 12, the magnetic toner core base particles, the presence or absence of surface modification treatment by the above-mentioned hybridization system, the type and amount of external additives, the polyester content in the toner containing the external additives, and the glass transition temperature.
[0569] [Table 8]
[0570] [Table 9]
[0571] [Table 10]
[0572] (B.13) Preparation of Toner 13 (B.13.1) Preparation of magnetic iron oxide particles [1] Fe 2+ 50 L of an aqueous solution of ferrous sulfate containing 2.0 mol / L of ferrous hydroxide was mixed with 55 L of an aqueous solution of sodium hydroxide containing 4.0 mol / L, and stirred to prepare an aqueous solution of ferrous salt containing ferrous hydroxide colloid. This aqueous solution was kept at 85°C and an oxidation reaction was carried out while blowing in air at 20 L / min, to obtain a slurry containing core particles.
[0573] The obtained slurry was filtered and washed using a filter press, and the core particles were redispersed in water to reslurry. Sodium silicate was added to this reslurry in an amount of 0.20 mass% silicon per 100 mass parts of core particles, the pH of the slurry was adjusted to 6.0, and the mixture was stirred to prepare a reslurry containing magnetic iron oxide particles with a silicon-rich surface.
[0574] The prepared reslurry liquid was filtered and washed with a filter press, and then reslurried with ion-exchanged water. 500 g (10% by mass relative to the magnetic iron oxide) of ion-exchange resin SK110 (manufactured by Mitsubishi Chemical) was added to the reslurry liquid (solid content 50 g / L) and stirred for 2 hours to perform ion exchange.
[0575] Thereafter, the ion exchange resin was removed by filtration through a mesh, and the mixture was filtered and washed using a filter press, dried, and crushed to produce magnetic iron oxide particles [1] with a number-average diameter of 0.23 μm.
[0576] (B.13.2) Preparation of silane compound aqueous solution 30 parts by mass of iso-butyltrimethoxysilane was dropped into 70 parts by mass of ion-exchanged water while stirring. Then, this aqueous solution was kept at pH 5.5 and temperature 55°C, and dispersed for 120 minutes at a peripheral speed of 0.46 m / s using a dispersing blade to carry out hydrolysis. Then, the pH of the aqueous solution was adjusted to 7.0, and the solution was cooled to 10°C to stop the hydrolysis reaction. Thus, a silane compound aqueous solution (1) containing a silane compound was prepared.
[0577] (B.13.3) Preparation of magnetic material [4] 100 parts by mass of the magnetic iron oxide particles [1] were placed in a high-speed mixer (LFS-2 model, manufactured by Fukae Powtec Co., Ltd.) and stirred at a rotation speed of 2000 rpm. 8.0 parts by mass of the silane compound aqueous solution (1) were added dropwise over a period of 2 minutes, and then the mixture was mixed and stirred for 5 minutes to obtain a mixture [1].
[0578] Next, in order to increase the adhesion of the silane compound, the mixture was dried at 40°C for 1 hour to reduce the moisture, and then the mixture [1] was dried at 110°C for 3 hours to promote the condensation reaction of the silane compound. After that, the mixture was crushed and passed through a sieve with 100 μm openings to produce magnetic material [4].
[0579] (B.13.4) Preparation of crystalline polyester [c7] The following components were placed in a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple.
[0580] <Ingredients> 1,9-Nonanediol 49mol% 1,10-Decanedioic acid 49mol% n-Octadecanoic acid 2mol%
[0581] Then, 1 part by mass of tin dioctylate was added as a catalyst for 100 parts by mass of the total amount of monomers, and the mixture was heated to 140°C in a nitrogen atmosphere and reacted for 6 hours while distilling off water under normal pressure. Next, the mixture was reacted while increasing the temperature to 200°C at a rate of 10°C / hour, and reacted for 2 hours after reaching 200°C.
[0582] The pressure in the reaction vessel was then reduced to 5 kPa or less, and the mixture was reacted at 200° C. for 3 hours to produce crystalline polyester c7. The acid value of the crystalline polyester c7 was 2.2 mg KOH / g, and the weight average molecular weight (Mw) was 34,200.
[0583] (B.13.5) Preparation of first aqueous medium [1] 2.9 parts by mass of sodium phosphate 12-hydrate was added to 353.8 parts by mass of ion-exchanged water, and the mixture was heated to 60° C. while being stirred using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.).
[0584] Thereafter, an aqueous calcium chloride solution prepared by adding 1.7 parts by mass of calcium chloride dihydrate to 11.7 parts by mass of ion-exchanged water, and an aqueous magnesium chloride solution prepared by adding 0.5 parts by mass of magnesium chloride to 15.0 parts by mass of ion-exchanged water were added and stirred to prepare a first aqueous medium [1].
[0585] (B.13.6) Preparation of polymerizable monomer composition [1] The following components were uniformly dispersed and mixed using an Attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.).
[0586] <Ingredients> Stearyl methacrylate 90.0 parts by weight Methyl methacrylate 10.0 parts by mass Magnetic material [4] 95.0 parts by mass Crystalline polyester [c7] 5.0 parts by mass
[0587] Thereafter, the mixture was heated to 60° C., and the following components were added, mixed, and dissolved to prepare a polymerizable monomer composition [1].
[0588] <Ingredients> Behenyl stearate wax 15.0 parts by weight "HNP-9" (manufactured by Nippon Seirosha) 8.0 parts by mass
[0589] The above-mentioned component, behenyl stearate wax, is an ester wax with a melting point of 68° C. The above-mentioned component, “HNP-9,” is a hydrocarbon wax (paraffin wax).
[0590] (B.13.7) Preparation of second aqueous medium [1] 0.6 parts by mass of sodium phosphate 12-hydrate was added to 166.8 parts by mass of ion-exchanged water, and the mixture was heated to 60° C. while being stirred with a paddle impeller.
[0591] Thereafter, an aqueous calcium chloride solution prepared by adding 0.3 parts by mass of calcium chloride dihydrate to 2.3 parts by mass of ion-exchanged water was added and stirred to prepare a second aqueous medium [1].
[0592] (B.13.8) Preparation of granulation liquid [1A] containing polymerizable monomer composition The polymerizable monomer composition [1] was added to the first aqueous medium [1] to obtain a granulation liquid [1a].
[0593] The granulation liquid [1a] was treated with a Cavitron (manufactured by Eurotech) at a rotor speed of 29 m / s for 1 hour to uniformly disperse and mix. Further, 7.0 parts by mass of t-butyl peroxypivalate was added as a polymerization initiator, and the mixture was granulated with a Clearmix (manufactured by M Technique) at a rotor speed of 22 m / s for 10 minutes at 60°C under a N2 atmosphere to prepare a granulation liquid [1A] containing a polymerizable monomer composition.
[0594] (B.13.9) Polymerization / Distillation / Drying / External Addition The granulation liquid [1A] containing the polymerizable monomer composition was added to the second aqueous medium [1], and the mixture was reacted for 3 hours at 74° C. while stirring with a paddle impeller. After the reaction was completed, the mixture was heated to 98° C. and distilled for 3 hours to obtain a reaction slurry [1].
[0595] Then, in the cooling step, 0°C water was added to the reaction slurry [1], and the reaction slurry [1] was cooled from 98°C to 45°C at a rate of 100°C / min. The temperature was then further increased and maintained at 50°C for 3 hours. Then, the reaction slurry [1] was allowed to cool to 25°C at room temperature.
[0596] The reaction slurry [1] was allowed to cool, washed with hydrochloric acid, filtered and dried to prepare magnetic toner core base particles [13c] having a weight average particle size of 6.1 μm.
[0597] (B.13.10) Surface modification of magnetic toner core base particles with inorganic particles The following materials were put into the "High-velocity air current impact method: Hybridization system (Nara Machinery Manufacturing Co., Ltd.)" to prepare an ordered mixture.
[0598] Magnetic toner core base particles [13c] 100 parts by weight Inorganic fine particles "X24" (for surface modification) 4.5 parts by weight The inorganic fine particles "X24" used herein are sol-gel silica spherical fine particles "X24-9163A" manufactured by Shin-Etsu Chemical Co., Ltd., and have an average particle size of 110 nm.
[0599] Thereafter, the blade rotation speed and product temperature were controlled to fix the inorganic fine particles "X24" onto the surface of the magnetic toner core base particle [13c], producing the toner base particle
[13] . At this time, the weight average particle size of the toner base particle
[13] with the inorganic fine particles "X24" fixed thereto was 6.4 μm.
[0600] (B.13.11) Addition of external additives and measurement of glass transition temperature The external additives were added in the same manner as in Toner 10. The glass transition temperature was measured in the same manner as in Toner 1, and the glass transition temperature (Tg) of Toner 13 was 0.3°C.
[0601] (B.14) Preparation of Toner 14 (B.14.1) Preparation of magnetic iron oxide particles [2] Fe 2+ 50 L of an aqueous ferrous sulfate solution containing 2.0 mol / L of ferric sulfate was mixed with 55 L of a 4.0 mol / L aqueous sodium hydroxide solution and stirred to prepare an aqueous ferrous salt solution containing ferrous hydroxide colloid.
[0602] This aqueous solution was kept at 85° C., and an oxidation reaction was carried out while blowing air into it at 20 L / min, to obtain a slurry containing core particles.
[0603] The obtained slurry was filtered and washed using a filter press, and the core particles were then redispersed in water to form a reslurry.
[0604] To this reslurry liquid, sodium silicate was added in an amount equivalent to 0.20 mass% silicon per 100 mass parts of core particles, the pH of the slurry liquid was adjusted to 6.0, and the slurry liquid was stirred to prepare a reslurry liquid containing magnetic iron oxide particles with a silicon-rich surface.
[0605] The resulting reslurry liquid was filtered and washed using a filter press, and then reslurried with ion-exchanged water. 500 g (10% by mass relative to the magnetic iron oxide) of ion-exchange resin SK110 (manufactured by Mitsubishi Chemical) was added to the reslurry liquid (solid content 50 g / L) and stirred for 2 hours to perform ion exchange.
[0606] Thereafter, the ion exchange resin was removed by filtration through a mesh, and the mixture was filtered and washed using a filter press, and then dried and crushed to produce magnetic iron oxide particles [2] with a number-average diameter of 0.23 μm.
[0607] (B.14.2) Preparation of silane compound aqueous solution 30 parts by mass of iso-butyltrimethoxysilane was dropped into 70 parts by mass of ion-exchanged water while stirring. Then, this aqueous solution was kept at pH 5.5 and temperature 55°C, and dispersed for 120 minutes at a peripheral speed of 0.46 m / s using a dispersing blade to carry out hydrolysis. Then, the pH of the aqueous solution was adjusted to 7.0, and the solution was cooled to 10°C to stop the hydrolysis reaction. In this way, a silane compound aqueous solution (2) containing a silane compound was prepared.
[0608] (B.14.3) Preparation of magnetic material [5] 100 parts by mass of the magnetic iron oxide particles [2] were placed in a high-speed mixer (LFS-2 model, manufactured by Fukae Powtec Co., Ltd.) and stirred at a rotation speed of 2000 rpm. 8.0 parts by mass of the silane compound aqueous solution (2) were added dropwise over a period of 2 minutes, and then the mixture was mixed and stirred for 5 minutes to obtain a mixture [2].
[0609] Next, in order to increase the adhesion of the silane compound, the mixture was dried at 40°C for 1 hour to reduce the moisture, and then the mixture [2] was dried at 110°C for 3 hours to promote the condensation reaction of the silane compound. After that, the mixture was crushed and passed through a sieve with 100 μm openings to produce magnetic material [5].
[0610] (B.14.4) Preparation of crystalline polyester [c8] The following components were placed in a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple.
[0611] <Ingredients> 1,9-Nonanediol 49mol% 1,10-Decanedioic acid 49mol% n-Octadecanoic acid 2mol%
[0612] Then, 1 part by mass of tin dioctylate was added as a catalyst for 100 parts by mass of the total amount of monomers, and the mixture was heated to 140°C in a nitrogen atmosphere and reacted for 6 hours while distilling off water under normal pressure. Next, the mixture was reacted while increasing the temperature to 200°C at a rate of 10°C / hour, and reacted for 2 hours after reaching 200°C.
[0613] Thereafter, the pressure in the reaction vessel was reduced to 5 kPa or less, and the mixture was reacted at 200° C. for 3 hours to produce crystalline polyester [c8]. At this time, the acid value of the crystalline polyester [c8] was 2.2 mg KOH / g, and the weight average molecular weight (Mw) was 34,200.
[0614] (B.14.5) Preparation of first aqueous medium [2] 2.9 parts by mass of sodium phosphate dodecahydrate was added to 353.8 parts by mass of ion-exchanged water, and the mixture was heated to 60° C. while stirring using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.). Then, an aqueous calcium chloride solution prepared by adding 1.7 parts by mass of calcium chloride dihydrate to 11.7 parts by mass of ion-exchanged water, and an aqueous magnesium chloride solution prepared by adding 0.5 parts by mass of magnesium chloride to 15.0 parts by mass of ion-exchanged water were added, and stirring was continued to obtain a first aqueous medium [2].
[0615] (B.14.6) Preparation of polymerizable monomer composition [2] The following components were uniformly dispersed and mixed using an Attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.).
[0616] <Ingredients> Stearyl methacrylate 67.0 parts by weight Methyl methacrylate 33.0 parts by mass Magnetic material [5] 95.0 parts by mass Crystalline polyester [c8] 5.0 parts by mass
[0617] Thereafter, the mixture was heated to 60° C., and the following components were added, mixed, and dissolved to prepare a polymerizable monomer composition [2].
[0618] <Ingredients> Behenyl stearate wax 15.0 parts by weight "HNP-9" (manufactured by Nippon Seirosha) 8.0 parts by mass
[0619] The above-mentioned component, behenyl stearate wax, is an ester wax with a melting point of 68° C. The above-mentioned component, “HNP-9,” is a hydrocarbon wax (paraffin wax).
[0620] (B.14.7) Preparation of second aqueous medium [2] 0.6 parts by mass of sodium phosphate 12-hydrate was added to 166.8 parts by mass of ion-exchanged water, and the mixture was heated to 60° C. while stirring using a paddle impeller. Thereafter, an aqueous calcium chloride solution prepared by adding 0.3 parts by mass of calcium chloride dihydrate to 2.3 parts by mass of ion-exchanged water was added, and stirring was continued to prepare a second aqueous medium [2].
[0621] (B.14.8) Preparation of granulation liquid [2A] containing polymerizable monomer composition The polymerizable monomer composition [2] was added to the first aqueous medium [2] to obtain a granulation liquid [2a]. The granulation liquid [2a] was treated for 1 hour using a Cavitron (manufactured by Eurotech) at a rotor speed of 29 m / s to uniformly disperse and mix. Furthermore, 7.0 parts by mass of t-butyl peroxypivalate was added as a polymerization initiator, and the mixture was granulated at 60°C and a N2 atmosphere with a Clearmix (manufactured by M Technique) at a peripheral speed of 22 m / s for 10 minutes to prepare a granulation liquid [2A] containing a polymerizable monomer composition.
[0622] (B.14.9) Polymerization / Distillation / Drying / External Addition The granulation liquid [2A] containing the polymerizable monomer composition was added to the second aqueous medium [2], and the mixture was reacted for 3 hours at 74° C. while stirring with a paddle impeller. After the reaction was completed, the mixture was heated to 98° C. and distilled for 3 hours to obtain a reaction slurry [2].
[0623] Then, in the cooling step, 0°C water was added to the reaction slurry [2], and the reaction slurry [2] was cooled from 98°C to 45°C at a rate of 100°C / min. The temperature was then further increased and maintained at 50°C for 3 hours. Then, the reaction slurry [2] was allowed to cool to 25°C at room temperature.
[0624] The reaction slurry [2] was allowed to cool, washed with hydrochloric acid, filtered and dried to prepare magnetic toner core base particles [14c] having a weight average particle size of 6.1 μm.
[0625] (B.14.10) Surface modification of magnetic toner core base particles with inorganic particles The following materials were put into the "High-velocity air current impact method: Hybridization system (Nara Machinery Manufacturing Co., Ltd.)" to prepare an ordered mixture.
[0626] Magnetic toner core base particles [14c] 100 parts by weight Inorganic fine particles "X24" (for surface modification) 3.5 parts by weight
[0627] The inorganic fine particles "X24" used herein are sol-gel silica spherical fine particles "X24-9600A-80" manufactured by Shin-Etsu Chemical Co., Ltd., and have an average particle size of 80 nm.
[0628] Then, the blade rotation speed and product temperature were controlled to fix the inorganic fine particles "X24" on the surface of the magnetic toner core base particle [11c], producing the toner base particle
[14] . The weight average particle size of the toner base particle
[14] was 6.4 μm.
[0629] (B.14.11) Addition of external additives and measurement of glass transition temperature The external additives were added in the same manner as in Toner 10. The glass transition temperature was measured in the same manner as in Toner 1, and the glass transition temperature (Tg) of Toner 14 was 25.6°C.
[0630] (B.15) Preparation of Toner 15 (B.15.1) Preparation of magnetic iron oxide particles
[15] Fe 2+50 L of an aqueous solution of ferrous sulfate containing 2.0 mol / L of ferrous hydroxide was mixed with 55 L of an aqueous solution of sodium hydroxide containing 4.0 mol / L, and stirred to prepare an aqueous solution of ferrous salt containing ferrous hydroxide colloid. This aqueous solution was kept at 85°C and an oxidation reaction was carried out while blowing in air at 20 L / min, to obtain a slurry containing core particles.
[0631] The obtained slurry was filtered and washed using a filter press, and the core particles were redispersed in water to reslurry. Sodium silicate was added to this reslurry in an amount of 0.20 mass% silicon per 100 mass parts of core particles, the pH of the slurry was adjusted to 6.0, and the mixture was stirred to prepare a reslurry containing magnetic iron oxide particles with a silicon-rich surface.
[0632] The prepared reslurry liquid was filtered and washed with a filter press, and then reslurried with ion-exchanged water. 500 g (10% by mass relative to the magnetic iron oxide) of ion-exchange resin SK110 (manufactured by Mitsubishi Chemical) was added to the reslurry liquid (solid content 50 g / L) and stirred for 2 hours to perform ion exchange.
[0633] Thereafter, the ion exchange resin was removed by filtration through a mesh, and the mixture was filtered and washed using a filter press, dried, and crushed to produce magnetic iron oxide particles [3] with a number-average diameter of 0.23 μm.
[0634] (B.15.2) Preparation of silane compound aqueous solution 30 parts by mass of iso-butyltrimethoxysilane was dropped into 70 parts by mass of ion-exchanged water while stirring. Then, this aqueous solution was kept at pH 5.5 and temperature 55°C, and dispersed for 120 minutes at a peripheral speed of 0.46 m / s using a dispersing blade to carry out hydrolysis. Then, the pH of the aqueous solution was adjusted to 7.0, and the solution was cooled to 10°C to stop the hydrolysis reaction. In this way, a silane compound aqueous solution (3) containing a silane compound was prepared.
[0635] (B.15.3) Preparation of magnetic material [6] 100 parts by mass of the magnetic iron oxide particles [3] were placed in a high-speed mixer (LFS-2 model, manufactured by Fukae Powtec Co., Ltd.) and stirred at a rotation speed of 2000 rpm. 8.0 parts by mass of the silane compound aqueous solution (3) were added dropwise over a period of 2 minutes, and then the mixture was mixed and stirred for 5 minutes to obtain a mixture [3].
[0636] Next, in order to increase the adhesion of the silane compound, the mixture was dried at 40°C for 1 hour to reduce the moisture, and then the mixture [3] was dried at 110°C for 3 hours to promote the condensation reaction of the silane compound. After that, the mixture was crushed and passed through a sieve with 100 μm openings to produce magnetic material [6].
[0637] (B.15.4) Preparation of crystalline polyester [c9] The following components were placed in a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple.
[0638] <Ingredients> 1,9-Nonanediol 49mol% 1,10-Decanedioic acid 49mol% n-Octadecanoic acid 2mol%
[0639] Then, 1 part by mass of tin dioctylate was added as a catalyst for 100 parts by mass of the total amount of monomers, and the mixture was heated to 140°C in a nitrogen atmosphere and reacted for 6 hours while distilling off water under normal pressure. Next, the mixture was reacted while increasing the temperature to 200°C at a rate of 10°C / hour, and reacted for 2 hours after reaching 200°C.
[0640] Thereafter, the pressure in the reaction vessel was reduced to 5 kPa or less, and the mixture was reacted at 200° C. for 3 hours to produce a crystalline polyester [c9]. At this time, the acid value of the crystalline polyester [c9] was 2.2 mg KOH / g, and the weight average molecular weight (Mw) was 34,200.
[0641] (B.15.5) Preparation of first aqueous medium [3] 2.9 parts by mass of sodium phosphate 12-hydrate was added to 353.8 parts by mass of ion-exchanged water, and the mixture was heated to 60° C. while being stirred using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.).
[0642] Thereafter, an aqueous calcium chloride solution prepared by adding 1.7 parts by mass of calcium chloride dihydrate to 11.7 parts by mass of ion-exchanged water, and an aqueous magnesium chloride solution prepared by adding 0.5 parts by mass of magnesium chloride to 15.0 parts by mass of ion-exchanged water were added and stirred to prepare a first aqueous medium [3].
[0643] (B.15.6) Preparation of polymerizable monomer composition [3] The following components were uniformly dispersed and mixed using an Attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.).
[0644] <Ingredients> Styrene 75.0 parts by mass n-Butyl acrylate 25.0 parts by mass 1-6 Hexanediol diacrylate 0.5 parts by mass Magnetic material [6] 95.0 parts by mass Crystalline polyester [c9] 5.0 parts by mass
[0645] Thereafter, the mixture was heated to 60° C., and the following components were added, mixed, and dissolved to prepare a polymerizable monomer composition [3].
[0646] <Ingredients> Behenyl stearate wax 15.0 parts by weight "HNP-9" (manufactured by Nippon Seirosha) 8.0 parts by mass
[0647] The above-mentioned component, behenyl stearate wax, is an ester wax with a melting point of 68° C. The above-mentioned component, “HNP-9,” is a hydrocarbon wax (paraffin wax).
[0648] (B.15.7) Preparation of second aqueous medium [3] 0.6 parts by mass of sodium phosphate 12-hydrate was added to 166.8 parts by mass of ion-exchanged water, and the mixture was heated to 60° C. while being stirred with a paddle impeller.
[0649] Thereafter, an aqueous calcium chloride solution prepared by adding 0.3 parts by mass of calcium chloride dihydrate to 2.3 parts by mass of ion-exchanged water was added and stirred to prepare a second aqueous medium [3].
[0650] (B.15.8) Preparation of granulation liquid
[15] containing polymerizable monomer composition The polymerizable monomer composition [3] was added to the first aqueous medium [3] to obtain a granulation liquid [3a]. The granulation liquid [3a] was treated with a Cavitron (manufactured by Eurotech) at a rotor speed of 29 m / s for 1 hour to uniformly disperse and mix the granulation liquid [3a].
[0651] Furthermore, 7.0 parts by mass of t-butyl peroxypivalate was added as a polymerization initiator, and the mixture was granulated at 60°C under a N2 atmosphere with a Clearmix (manufactured by M Technique) at a peripheral speed of 22 m / s for 10 minutes to prepare a granulation liquid [3A] containing a polymerizable monomer composition.
[0652] (B.15.9) Polymerization / Distillation / Drying / External Addition The granulation liquid [3A] containing the polymerizable monomer composition was added to the second aqueous medium [3], and the mixture was reacted for 3 hours at 74° C. while stirring with a paddle impeller. After the reaction was completed, the mixture was heated to 98° C. and distilled for 3 hours to obtain a reaction slurry [3].
[0653] Then, in the cooling step, 0°C water was added to the reaction slurry [3], and the reaction slurry [3] was cooled from 98°C to 45°C at a rate of 100°C / min. The temperature was then further increased and maintained at 50°C for 3 hours. Then, the reaction slurry [3] was allowed to cool to 25°C at room temperature.
[0654] The cooled reaction slurry [3] was washed with hydrochloric acid, filtered and dried to produce magnetic toner core base particles [15c] with a weight average particle size of 6.1 μm. The magnetic toner core base particles [15c] were not surface-modified, and the magnetic toner core base particles [15c] were used as they were as toner base particles
[15] . The weight average particle size of the toner base particles
[15] was 6.4 μm.
[0655] (B.15.10) Addition of external additives and measurement of glass transition temperature The external additives were added in the same manner as in Toner 10. The glass transition temperature was measured in the same manner as in Toner 1, and the glass transition temperature (Tg) of Toner 15 was 39.1°C.
[0656] The components and amounts of the magnetic toner core base particles [13c], [14c] and [15c] are shown in Table XI. The magnetic toner core base particles [13c] and [14c] used to prepare the toner base particles
[13] and
[14] were subjected to a surface modification treatment by the "High-speed airflow impact method: Hybridization system (Nara Machinery Manufacturing Co., Ltd.)", and the combinations and amounts of the components are shown in Table XII.
[0657] The toner base particles of toners 13 to 15, the magnetic toner core base particles, the presence or absence of surface modification treatment by the above-mentioned hybridization system, the type and amount of external additives, the polyester content in the toner containing the external additives, and the glass transition temperature are shown in Table XIII.
[0658] [Table 11]
[0659] [Table 12]
[0660] [Table 13]
[0661] (B.16) Preparation of Toner 16 (B.16.1) Preparation of amorphous polyester [Ha] The following components were placed in a reaction vessel equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube, and the atmosphere in the reaction vessel was replaced with dry nitrogen gas. Then, tin dioctanoate was added in an amount of 0.3% based on the total amount of the components.
[0662] <Ingredients> Ethylene glycol 106 parts by weight Dimethyl terephthalate 228 parts by mass 1,10-Decanedicarboxylic acid 123 parts by mass
[0663] The temperature was raised to 235°C under a nitrogen gas stream over the course of one hour, and the reaction was carried out for three hours. The pressure inside the reaction vessel was then reduced to 10.0 mmHg, and the reaction was continued with stirring. When the desired molecular weight was reached, the reaction was terminated to produce amorphous polyester [Ha].
[0664] (B.16.2) Preparation of amorphous polyester dispersion (HA) The following components were placed in a reaction vessel equipped with a stirrer and dissolved at 60°C.
[0665] <Ingredients> Amorphous polyester [Ha] 100 parts by mass Methyl ethyl ketone 60 parts by weight Isopropyl alcohol 10 parts by weight
[0666] After confirming dissolution, the reaction vessel was cooled to 35°C, and 3.5 parts by mass of 10% aqueous ammonia solution was added. Then, 300 parts by mass of ion-exchanged water was dropped into the reaction vessel over 3 hours. Then, methyl ethyl ketone and isopropyl alcohol were removed using an evaporator to prepare an amorphous polyester dispersion (A1).
[0667] (B.16.3) Preparation of toner base particles
[16] As the toner core components, each dispersion was weighed so that the solid content was the following amount.
[0668] <Core Ingredients> Amorphous polyester [Ha] 47.5 parts by mass Crystalline polyester [c1] 22.0 parts by mass Black colorant [B1] (solid content) 6.0 parts by weight Release agent [W1] (solid content) 1.5 parts by weight
[0669] Each dispersion was poured into a round stainless steel flask, ion-exchanged water was added so that the solid content concentration was 12.5%, and 6.3 parts of a 10% aqueous aluminum sulfate solution was further poured in. Next, the mixture was mixed and dispersed at 5000 rpm for 10 minutes using a homogenizer (Ultra Turrax T50, manufactured by IKA), and the contents in the flask were heated to 40°C while stirring.
[0670] After that, the temperature was raised at 0.5° C. per minute, and the temperature was maintained when the particle size reached 6.1 μm. Next, each dispersion was weighed and mixed so that the solid content of the toner shell component was as follows, and the resulting dispersion was then added and maintained for 60 minutes.
[0671] <Shell component> Amorphous polyester [a5] 20 parts by mass Release agent dispersion [W1] (solid content) 3 parts by weight
[0672] Observation of the resulting contents under an optical microscope confirmed the formation of aggregated particles. 11 parts of tetrasodium ethylenediaminetetraacetic acid (EDTA) "Chilest 40" (manufactured by Chelest Co., Ltd.) was added, and then an aqueous solution of sodium hydroxide was added to adjust the pH to 8.
[0673] After that, the temperature was raised to 82.5°C, and the pH was lowered by 0.05 with nitric acid every 10 minutes, and stirring was continued for 45 minutes. After cooling, the mixture was filtered, thoroughly washed with ion-exchanged water, and then dried to prepare toner base particles
[16] .
[0674] (B.16.4) Addition of external additives and measurement of glass transition temperature Toner base particles
[16] were mixed with hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd.) in an amount of 3.0 parts by mass, and mixed for 30 seconds at 13,000 rpm using a sample mill. The mixture was then sieved using a vibrating sieve with 45 μm openings to produce toner 16.
[0675] The glass transition temperature (Tg) of Toner 16 was −1.5° C. The glass transition temperature of Toner 16 was measured in the same manner as Toner 1.
[0676] (B.17) Preparation of Toner 17 (B.17.1) Preparation of amorphous polyester [Hb] Amorphous polyester [Hb] was prepared in the same manner as for amorphous polyester [Ha], except that the following components were added.
[0677] <Ingredients> Bisphenol A ethylene oxide adduct 140 parts by mass Bisphenol A propylene oxide adduct 260 parts by mass Terephthalic acid 100 parts by mass Tetrapropenylsuccinic anhydride 130 parts by mass Trimellitic acid 16 parts by mass
[0678] (B.17.2) Preparation of amorphous polyester dispersion (HB) An amorphous polyester dispersion (HB) was prepared in the same manner as in the preparation of the amorphous polyester dispersion (HA), except that the amorphous polyester (Ha) was replaced by an amorphous polyester (Hb).
[0679] (B.17.3) Preparation of toner base particles
[17] Toner base particles
[17] were prepared in the same manner as toner base particles
[16] , except that the core component and shell component were changed to those shown below.
[0680] <Core Ingredients> Amorphous polyester [Hb] 26.0 parts by mass Amorphous polyester [a5] 26.0 parts by mass Crystalline polyester [c3] 19.5 parts by mass Black colorant [B1] (solid content) 6.0 parts by weight Release agent [W1] (solid content) 1.5 parts by weight
[0681] <Shell component> Amorphous polyester [a5] 18 parts by mass Release agent dispersion [W1] (solid content) 3 parts by weight
[0682] (B.17.4) Addition of external additives and measurement of glass transition temperature Toner base particles
[17] were mixed with hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd.) in an amount of 3.0 parts by mass, and mixed at 13,000 rpm for 30 seconds using a sample mill. The mixture was then sieved using a vibrating sieve with 45 μm openings to produce toner 17.
[0683] The glass transition temperature (Tg) of Toner 16 was 41.2° C. The glass transition temperature of Toner 17 was measured in the same manner as Toner 1.
[0684] The components and amounts of the toner base particles
[16] and
[17] are summarized in Table XIV. The types and amounts of the external additives of the toners 16 and 17, the polyester content in the toners containing the external additives, and the glass transition temperatures are shown in Table XV.
[0685] [Table 14]
[0686] [Table 15]
[0687] C. Preparation of the Carrier (Preparation of Resin-Coated Carrier [C]) The following components [1] excluding the ferrite particles and glass beads (φ1 mm, the same amount as toluene) were stirred at 1200 rpm for 30 minutes using a sand mill (manufactured by Kansai Paint Co., Ltd.) to prepare a resin coating layer forming solution (c1).
[0688] <Ingredient [1]> Ferrite particles [f1] 100.0 parts by mass Toluene 14.0 parts by weight ·Copolymer A 2.0 parts by mass
[0689] The ferrite particles [f1] are Mn-Mg-Sr ferrite particles having an average particle size of 40 μm. The copolymer A is a cyclohexyl methacrylate / dimethylaminoethyl methacrylate copolymer (weight ratio 99:1, Mw 80000).
[0690] Furthermore, this resin coating layer forming solution (c1) and the ferrite particles [f1] were placed in a vacuum degassing kneader, the pressure was reduced, and the toluene was distilled off to dry the mixture. In this way, a resin-coated carrier [C] was produced.
[0691] D. Preparation of developer (D.1) Preparation of Developer 1 Toner 1 and carrier [C] were placed in a 2 liter V blender in the amounts shown below, and stirred for 20 minutes in an environment of normal temperature and humidity. Thereafter, developer 1 was prepared by sieving through a 105 μm sieve.
[0692] Carrier 1 100 parts by weight Toner 1 7 parts by weight
[0693] (D.2) Preparation of developers 2 to 9, 16 and 17 Developers 2 to 9, 16 and 17 were prepared in the same manner as in the preparation of developer 1, except that the type of toner was changed from toner 1 as shown in Table XVI.
[0694] (D.3) Preparation of developers 10 to 15 In the developers 10 to 15, a one-component developer was used without using a carrier [C], and the toners 10 to 15 were used as the developers 10 to 15 as they were.
[0695] [Table 16]
[0696] (D.3) Summary of developer composition These developers are summarized in Table XVII.
[0697] [Table 17]
[0698] E. Evaluation (E.1) Preparation of evaluation equipment (E.1.1) Two-component developing device (Preparation of evaluation device when using developers 1 to 9, 16 and 17 during image formation) As an image forming device, we prepared a "bizhub C650i" (manufactured by Konica Minolta), and modified it so that it could output images by replacing the black developing roller with a specified developing roller. Hereinafter, this device will be referred to as a two-component developing device.
[0699] (E.1.2) Magnetic one-component developing device (Preparation of evaluation device when using developers 10 to 15 during image formation) A commercially available laser printer, HP LaserJet Enterprise M506 (manufactured by Hewlett-Packard), was prepared as an image forming device, and the black developing roller installed in this device was replaced with a specified developing roller to enable image output. Hereinafter, this device will be referred to as a magnetic single-component developing device.
[0700] The cartridge was removed from each of the above main bodies, the product toner was removed from the cartridge, and 300 g of each developer was filled in. The main body and cartridge were left in the respective temperature and humidity controlled environments for 24 hours before the image output evaluation.
[0701] (E.2) Evaluation method and criteria (E.2.1) Change in charge (Evaluation method using two-component developing device: Evaluation method for developers 1 to 9, 16 and 17) The developing roller and developer in the combination shown in Table XVIII were set in a two-component developing device.
[0702] The charge amount of the developer on the developing roller was measured at the start of continuous printing using a chart with a print rate of 2% and after printing 5,000 sheets, and the degree of decrease in the charge amount was compared by calculating the absolute value of the difference, and evaluated according to the following evaluation criteria. A and B were considered to be acceptable, and C was considered to be unacceptable. The results are shown in Table XVIII.
[0703] The absolute value of the difference was calculated using the following formula (1).
[0704] Equation (1) Absolute value of difference = |(charge amount value at the start of printing - charge amount value after printing 5000 sheets)|
[0705] (Evaluation Criteria) A The absolute value of the difference is 4μC / g or less. B The absolute value of the difference is greater than 4 μC / g and less than or equal to 10 μC / g. C The absolute value of the difference is greater than 10 μC / g.
[0706] The measurement was performed using a measuring device as shown in Fig. 8. The measuring device used was a small suction type charge amount measuring device "Model 212HS" (manufactured by West One Co., Ltd.) The measurement method was as follows.
[0707] First, 1 g of two-component developer weighed with a precision balance was placed evenly on the entire surface of the conductive sleeve 11. A voltage of 2 kV was supplied from the bias power source 13 to the conductive sleeve 11, and the rotation speed of the magnet roller 12 provided inside the conductive sleeve 11 was set to 1000 rpm.
[0708] The developer was left for 30 seconds under the above conditions, and the two-component developer was collected in the cylindrical electrode 14. After 30 seconds, the potential Vm of the cylindrical electrode 14 was read and the charge amount of the two-component developer was calculated. Furthermore, the mass of the collected two-component developer was measured with a precision balance, and the average charge amount (-μC / g) was calculated and used as the measured value.
[0709] (Evaluation method using magnetic single-component developing device: Evaluation method for developers 10 to 15) The developing roller and developer were set in a magnetic one-component developing device according to the combination in Table XVIII. The charge amount of the toner on the developing roller was measured at the start of printing and after printing 5,000 sheets, and the degree of decrease in the charge amount was compared by calculating the absolute value of the difference, and evaluated according to the following evaluation criteria. A and B were considered to be acceptable, and C was considered to be unacceptable. The results are shown in Table XVIII. The absolute value of the difference was calculated using the above-mentioned formula (1), and the evaluation criteria were the same as those used in the evaluation method using the two-component developing device. The measuring device used was also the same as that used in the evaluation using the two-component developing device.
[0710] [Table 18]
[0711] (E.2.2) Check for scattering inside the aircraft (Evaluation method using two-component developing device and magnetic one-component developing device) Before printing started, double-sided tape was attached to the top of the developing unit, and after printing 5,000 sheets, the toner stains caused by toner scattering inside the machine were measured with a reflection densitometer (RD-918; Macbeth Co., Ltd.). The difference between the start of printing and the end of 5,000 sheets was quantified and evaluated according to the following evaluation criteria. A and B were considered to be acceptable, and C was considered to be unacceptable. The results are shown in Table XIX.
[0712] (Evaluation Criteria) A: Almost no increase in density due to toner scattering from the start of printing is observed, and the difference in density is 0.1 or less. B: Although some toner scattering is observed from the start of printing, this does not pose a problem in practical use, and the differential density is 0.8 or less. C: The amount of toner scattering from the start of printing is large, which is problematic for practical use, and the differential density exceeds 0.8.
[0713] (E.2.3) Image quality assessment (Evaluation method using two-component developing device and magnetic one-component developing device) Graininess was evaluated using the GI value published in the Journal of the Imaging Society of Japan 39(2), 84-93 (2000) to evaluate the quality of halftones, i.e., image quality. Specifically, an image with a gradation pattern with 32 levels of gradation was output for each evaluation after 5,000 sheets of endurance printing. Graininess in this image was evaluated by reading the gradation pattern with a CCD, applying Fourier transform processing to the obtained readings with MTF (Modulation Transfer Function) correction taken into account, measuring the GI (Graininess Index) value, which is adjusted to the relative visual sensitivity of humans, and determining the maximum GI value.
[0714] The smaller the GI value, the better, and the less graininess of the image, but when the toner particles begin to heat-fuse on the developing roller, graininess appears and the value becomes high. Also, when the aggregates become large, the thin layer of the developer begins to become clogged with the aggregates, causing image defects such as white streaks.
[0715] The graininess of the gradation pattern in the image was evaluated for each of the evaluation devices at the beginning of printing (0 sheets) and after 5,000 sheets of durable printing according to the following evaluation criteria. The images of the gradation pattern output at the beginning and after durable printing were judged according to the following evaluation criteria based on the maximum GI value of the image. A and B were considered to be acceptable, and C and D were considered to be unacceptable. The results are shown in Table XIX.
[0716] (Evaluation Criteria) A GI value is less than 0.26. B GI value is 0.26 or greater but less than 0.30. C GI value is 0.30 or higher. D Aggregates are visible and white streaks appear on the image.
[0717] (E.2.4) Evaluation of low-temperature fixability (Evaluation method) To evaluate the low-temperature fixing property of this embodiment, the fixing device of each actual machine used in the actual shooting was modified to control the fixing temperature to (normal temperature -30° C.) In addition, Konica Minolta J paper was used as the recording medium, and a solid image (25 mm×25 mm) was formed and fixed.
[0718] After printing 5,000 sheets, the image surface of the fixed image was folded in a valley shape to observe the degree of peeling of the image at the fold, and the width of the paper that appeared at the fold as a result of the image peeling was measured. The evaluation criteria were as follows. A and B were considered to be acceptable, and C was considered to be unacceptable. The results are shown in Table XIX.
[0719] (Evaluation Criteria) A: The width of the paper is not visible at the fold, and the fixation is good. B: The width of the paper at the fold is confirmed to be 1 mm or less, and fixing is possible. C: The width of the paper at the fold is greater than 1 mm (not suitable for practical use).
[0720] [Table 19]
[0721] (E.3) Summary Regarding the above evaluation, the combinations of the developing sleeves and the toners and the evaluation results thereof are summarized and shown in Table XX.
[0722] [Table 20]
[0723] F. Overall Review As is clear from Table XX, the examples of the present invention are superior to the comparative examples, and the evaluations of the charge amount, in-machine scattering, image quality and low-temperature fixability in the examples are all A or B, and therefore no problem is found in practical use. [Explanation of symbols]
[0724] 1Y, 1M, 1C, 1Bk: Photoreceptor 2Y, 2M, 2C, 2Bk: 1st charging means 3Y, 3M, 3C, 3Bk: Exposure means 4Y, 4M, 4C, 4Bk: Developing means 5Y, 5M, 5C, 5Bk: Primary transfer roller 5b: Secondary transfer roller 6Y, 6M, 6C, 6Bk, 6b: cleaning means 7: Intermediate transfer unit 8: Housing 9Y, 9M, 9C, 9Bk: second charging means 10Y, 10M, 10C, 10Bk: Process cartridge 11: Developing sleeve, conductive sleeve 12:Magnetic roller 13: Bias power supply 14: Cylindrical electrode 16: Shaft 17: Bearings 18: First flange 18a: Shaft 18b: Recess 19: Second flange 21:Paper feeding means 20: Paper feed cassette 22A, 22B, 22C, 22D: Intermediate rollers 23: Resist roller 24: Fixing method 25: Paper ejection roller 26: Paper output tray 70: Intermediate transfer body 71, 72, 73, 74: Intermediate rollers 82L, 82R: Support rail 100: Image forming device P: Transfer material A: Main body of the image forming device space:space Original image reading device SC
Claims
1. A developing roller for an electrophotographic image forming apparatus that transports a developer, comprising: the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, The developing sleeve has an aluminum alloy containing more than 0.6% by weight of silicon. A developing roller characterized by:
2. The aluminum alloy has a silicon content of more than 0.8% by mass.
2. The developing roller according to claim 1 .
3. The lithium content of the aluminum alloy is less than 1% by mass.
2. The developing roller according to claim 1 .
4. A process cartridge including a developing roller for transporting a developer, the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, The developing sleeve has an aluminum alloy containing more than 0.6% by weight of silicon. A process cartridge comprising:
5. An electrophotographic image forming apparatus including a developing roller for transporting a developer, the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, 11. An electrophotographic image forming apparatus, wherein the developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon.
6. An electrophotographic image forming system including a device including a developing roller for transporting a developer and a toner for developing an electrostatic latent image, the developing roller has a developing sleeve and a member that generates a magnetic flux inside the developing sleeve, the developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon; and The glass transition temperature of the toner for developing an electrostatic latent image is within a range of 0 to 40° C.
23. An electrophotographic imaging system comprising:
7. The toner particles contained in the electrostatic latent image developing toner contain a binder resin containing polyester in the range of 50 to 95% by mass.
7. An electrophotographic imaging system according to claim 6.
Citation Information
Patent Citations
Method for manufacturing toner for electrostatic charge image development
JP2017156544A