Method for producing polymer layer, film, sheet and laminate
A controlled heating process for tetrafluoroethylene polymer particles forms a polymer layer with enhanced adhesion and low transmission loss, addressing adhesion and frequency loss issues in printed circuit boards.
Patent Information
- Application Number
- JP2023066604
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Printed circuit board materials require improved adhesion between conductive and insulating layers, reduced transmission loss in high frequency ranges, and enhanced physical properties such as low dielectric constant and low dielectric loss tangent.
A method involving a base material layer with tetrafluoroethylene polymer particles and controlled heating processes to form a polymer layer with specific particle sizes and surface properties, using a dispersion containing tetrafluoroethylene polymer particles, water, and optional additives to achieve adhesion and low transmission loss.
The method produces a polymer layer with excellent adhesion to conductive layers and low transmission loss in high frequencies, exhibiting heat resistance and electrical properties like low dielectric constant and low dielectric loss tangent.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polymer layer containing a tetrafluoroethylene-based polymer, a film or sheet containing a tetrafluoroethylene-based polymer, and a laminate having a layer containing a tetrafluoroethylene-based polymer. [Background technology]
[0002] In recent years, in order to cope with the increasing speed and frequency of mobile communication devices such as mobile phones, materials with high thermal conductivity, low linear expansion coefficient, low dielectric constant and low dielectric loss tangent are required for printed circuit boards of communication devices, and tetrafluoroethylene-based polymers with low dielectric constant and low dielectric loss tangent have attracted attention. In addition, with the increasing density of printed wiring boards, there is a demand for printed wiring boards with excellent adhesion between the conductive layer and the insulating layer, suppressing peeling of the fine conductive pattern from the insulating layer, and excellent circuit formation properties. Patent Document 1 proposes a printed wiring board having a polyimide base film that is insulating and has a specific surface property, and a conductive layer on at least one surface of the polyimide base film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2016 / 104420 Summary of the Invention [Problem to be solved by the invention]
[0004] Printed circuit board materials are required to have high adhesion between conductive and insulating layers as well as to further reduce transmission loss in the high frequency range. The present inventors have discovered that, when forming an insulating layer having a low linear expansion coefficient, low dielectric constant and low dielectric tangent from an aqueous dispersion containing tetrafluoroethylene-based polymer particles, coating a base layer with an aqueous dispersion containing a predetermined amount of tetrafluoroethylene-based polymer particles in a specific particle size range and controlling the baking of the coating layer under specific conditions is an effective method for controlling the surface properties that affect physical properties such as adhesion to a conductive layer and obtaining a printed circuit board material having low transmission loss even in the high frequency range. The present inventors also found that a laminate having such a polymer layer has excellent physical properties such as heat resistance and electrical properties (low linear expansion coefficient, low dielectric constant and low dielectric tangent) based on the tetrafluoroethylene polymer, which led to the present invention. An object of the present invention is to provide a method for producing a polymer layer containing a tetrafluoroethylene-based polymer and having excellent adhesion to a conductive layer and low transmission loss in the high frequency range, a film or sheet which is the polymer layer, and a laminate including the polymer layer. [Means for solving the problem]
[0005] The present invention has the following aspects. [1] A method for producing a polymer layer, comprising: coating a substrate layer with a dispersion liquid containing 100 parts by mass of tetrafluoroethylene-based polymer particles having an average particle size of 1 μm or more and less than 10 μm, and 80 to 300 parts by mass of water, the dispersion liquid having a particle concentration of 5 to 100 particles / ml of particles having particle sizes of 20 to 80 μm as measured with a particle counter; forming a coating layer made of the dispersion liquid on the surface of the substrate layer; first heating the substrate layer having the coating layer in a temperature range of 25° C. or more, less than the boiling point of the water, and less than [the glass transition temperature of the tetrafluoroethylene-based polymer + 10° C.]; subsequently, second heating in a temperature range higher than the temperature range and less than the melting temperature of the tetrafluoroethylene-based polymer to obtain the substrate layer having a layer containing tetrafluoroethylene-based polymer particles on its surface; and further heating in a temperature range equal to or higher than the melting temperature to form a polymer layer containing the tetrafluoroethylene-based polymer on the surface of the substrate layer. [2] The method according to [1], wherein the tetrafluoroethylene-based polymer contains units based on perfluoro(alkyl vinyl ether). [3] The method according to [1] or [2], wherein the tetrafluoroethylene-based polymer is a heat-fusible tetrafluoroethylene-based polymer having a carbonyl group-containing group. [4] The method according to any one of [1] to [3], wherein the content of the tetrafluoroethylene-based polymer particles is 30% by mass or more. [5] The method according to any one of [1] to [4], wherein the dispersion further contains 5 to 20 parts by mass of a water-soluble solvent having a surface tension of 20 to 30 mN / m. [6] The method according to any one of [1] to [5], wherein the dispersion liquid further contains a nonionic surfactant. [7] The method according to any one of [1] to [6], wherein the dispersion further contains a water-soluble polymer. [8] The method according to any one of [1] to [7], wherein the polymer layer has a maximum height Sz defined by ISO 25178 of 0.1 μm or more and less than 10 μm. [9] The method according to any one of [1] to [8], wherein the substrate layer is a long substrate.
[10] A film or sheet comprising a polymer layer formed on the surface of a base layer, the polymer layer comprising a molten-sintered product of particles of a tetrafluoroethylene-based polymer having an average particle size of 1 μm or more and less than 10 μm, and the maximum height Sz of the polymer layer as defined by ISO 25178 is 0.1 μm or more and less than 10 μm.
[11] A laminate having a base layer and a polymer layer formed on a surface of the base layer, the polymer layer containing a molten-sintered product of particles of a tetrafluoroethylene-based polymer having an average particle diameter of 1 μm or more and less than 10 μm, and the maximum height Sz of the polymer layer defined in ISO 25178 is 0.1 μm or more and less than 10 μm.
[12] The laminate according to
[11] , wherein the substrate is a heat-resistant substrate.
[13] The laminate according to
[11] or
[12] , wherein the heat-resistant substrate is a metal foil or a heat-resistant resin film.
[14] The laminate according to any one of
[11] to
[13] , wherein the polymer layer is disposed on both surfaces of the base layer. Effect of the Invention
[0006] According to the present invention, there is provided a method for producing a polymer layer containing a tetrafluoroethylene-based polymer, which has excellent adhesion to a conductive layer and has low transmission loss in the high frequency range. The polymer layer, which is a film or sheet, and a laminate including the polymer layer can be effectively used, for example, as a material for a printed wiring board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The following terms have the following meanings. "Average particle size (D50)" is the volume-based cumulative 50% diameter of particles determined by laser diffraction / scattering. In other words, particle size distribution is measured by laser diffraction / scattering, and a cumulative curve is calculated with the total volume of the particle group as 100%, and the particle size is the point on the cumulative curve where the cumulative volume is 50%. The D50 of particles is determined by dispersing the particles in water and analyzing them by the laser diffraction / scattering method using a laser diffraction / scattering type particle size distribution measuring device (LA-920 measuring device, manufactured by Horiba, Ltd.). "Average particle size (D90)" is the volume-based cumulative 90% diameter of the particles, calculated in the same manner as for D50. The specific surface area of a particle is a value calculated by measuring the particle by a gas adsorption (constant volume method) BET multipoint method, and is determined using a NOVA4200e (manufactured by Quantachrome Instruments). "Melting temperature" is the temperature corresponding to the maximum of the melting peak of a polymer as measured by differential scanning calorimetry (DSC). The "glass transition temperature (Tg)" is a value measured by analyzing a polymer using the dynamic mechanical analysis (DMA) method. The "viscosity" is determined by measuring the composition using a Brookfield viscometer at 25° C. and 30 rpm. The measurement is repeated three times, and the average value of the three measured values is calculated. The "thixotropy ratio" is a value calculated by dividing the viscosity η1 of the composition measured at a rotation speed of 30 rpm by the viscosity η2 measured at a rotation speed of 60 rpm. Each viscosity measurement is repeated three times, and the average value of the three measured values is used. The "surface tension" of a solvent or solution is a value measured by the Wilhelmy method at 25°C using a surface tensiometer. The term "unit" in a polymer means an atomic group based on a monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by processing the polymer. Hereinafter, a unit based on monomer a is also referred to simply as a "monomer a unit."
[0008] The manufacturing method of the present invention (hereinafter also referred to as "this method") comprises coating a base layer with a dispersion (hereinafter also referred to as "this dispersion") containing 100 parts by mass of particles (hereinafter also referred to as "F particles") of a tetrafluoroethylene polymer (hereinafter also referred to as "F polymer") having an average particle diameter of 1 μm or more and less than 10 μm and 80 to 300 parts by mass of water, and having a particle concentration of 5 to 100 particles / ml having a particle diameter of 20 to 80 μm as measured by a particle counter, and coating the surface of the base layer with a coating liquid made of the dispersion. a coating layer is formed on the substrate, the substrate layer having the coating layer is first heated in a temperature range of 25°C or higher, lower than the boiling point of water and lower than [the glass transition temperature of the F polymer + 10°C], and then second heated in a temperature range higher than the above temperature range and lower than the melting temperature of the F polymer to obtain the substrate layer having a layer containing F particles on its surface, and further heated in a temperature range equal to or higher than the melting temperature to form a polymer layer containing the F polymer on the surface of the substrate layer.
[0009] According to this method, a polymer layer having excellent adhesion to a conductive layer and low transmission loss in the high frequency range can be obtained. The film or sheet of such a polymer layer and the laminate including the polymer layer have excellent physical properties such as heat resistance and electrical properties (low linear expansion coefficient, low dielectric constant and low dielectric loss tangent) based on the tetrafluoroethylene polymer, and further have excellent properties as described above. The reason why the polymer layer obtained by this method has excellent adhesion to the conductive layer and has low transmission loss in the high frequency range is not entirely clear, but is thought to be as follows.
[0010] In this method, a coating layer is first formed from the present dispersion containing F particles with a particle size of 20 to 80 μm and a particle concentration of 5 to 100 particles / ml, and then dried in a predetermined temperature range in stages. Specifically, in the first heating step, the coating layer is heated near the glass transition temperature while maintaining the diffusion state of the F particles in the coating layer, giving priority to reducing the change in the state of the F particles themselves. On the other hand, in the second heating step, the diffusion and removal of liquid dispersion medium such as water or a water-soluble solvent described later from the coating layer is given priority to form a layer containing F particles, which is a dry coating with little distortion overall. Then, the dry coating is baked to form a polymer layer containing an F polymer. This stepwise drying is believed to balance the diffusion of the F particles and the diffusion of the liquid dispersion medium while keeping the aggregation of the F particles in a highly de-aggregated state, and to facilitate the convergence of the maximum height Sz of the polymer layer to 0.1 μm or more and less than 10 μm as specified in ISO25178, and to facilitate the formation of a polymer layer with high adhesion and low transmission loss. In addition, a polymer layer having Sz in this specific range is believed to be densely and firmly adhered to a substrate layer such as copper foil in a laminate due to the anchor effect and increased contact area, and therefore to further reduce dielectric loss. This tendency becomes more pronounced when the dispersion liquid further contains one or more of a water-soluble solvent, a nonionic surfactant, or a water-soluble polymer having a specific surface tension, because the surface of the F particles becomes more easily wetted, and the F particle aggregates are more easily broken down and uniformly dispersed.
[0011] The F polymer in the present invention is a polymer containing units based on tetrafluoroethylene (hereinafter also referred to as "TFE") (hereinafter also referred to as "TFE units"). The F polymer is preferably heat-fusible. Here, a heat-fusible polymer means a polymer that has a temperature at which the melt flow rate is 1 to 1000 g / 10 min under a load of 49 N. The melting temperature of the F polymer is preferably 200° C. or higher, more preferably 260° C. or higher. The melting temperature of the F polymer is preferably 325° C. or lower, more preferably 320° C. or lower. The melting temperature of the F polymer is preferably 200 to 320° C. In this case, the present dispersion is likely to have excellent processability, and the polymer layer formed from the present dispersion is likely to have excellent heat resistance.
[0012] The glass transition point of the F polymer is preferably 50° C. or higher, more preferably 75° C. or higher. The glass transition point of the F polymer is preferably 150° C. or lower, more preferably 125° C. or lower. The fluorine content of the F polymer is preferably 70% by mass or more, more preferably 72 to 76% by mass. The surface tension of the F polymer is preferably 16 to 26 mN / m. The surface tension of the F polymer can be measured by placing a droplet of a mixture for wetting tension testing (manufactured by Wako Pure Chemical Industries, Ltd.) specified in JIS K 6768 on a flat plate made of the F polymer.
[0013] F polymer is preferably a polymer containing TFE unit and ethylene-based unit (ETFE), a polymer containing TFE unit and propylene-based unit, a polymer containing TFE unit and perfluoro(alkyl vinyl ether) (PAVE)-based unit (PAVE unit) (PFA), a polymer containing TFE unit and hexafluoropropylene-based unit (FEP), more preferably PFA and FEP, and even more preferably PFA. These polymers may further contain units based on other comonomers. PAVE is preferably CF2=CFOCF3, CF2=CFOCF2CF3 or CF2=CFOCF2CF2CF3 (hereinafter also referred to as "PPVE"), and more preferably PPVE.
[0014] The F polymer preferably has an oxygen-containing polar group, more preferably has a hydroxyl- or carbonyl-containing group, and even more preferably has a carbonyl-containing group. In this case, the dispersion tends to have excellent dispersion stability and ease of handling, and the polymer layer formed from the dispersion tends to have excellent physical properties such as heat resistance and electrical properties (low linear expansion coefficient, low dielectric constant and low dielectric tangent). The hydroxyl-containing group is preferably a group containing an alcoholic hydroxyl group, more preferably -CF2CH2OH or -C(CF3)2OH. The carbonyl group-containing group is preferably a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH2), an acid anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)-, etc.), a formyl group, a halogenoformyl group, a urethane group (-NHC(O)O-), a carbamoyl group (-C(O)-NH2), a ureido group (-NH-C(O)-NH2), an oxamoyl group (-NH-C(O)-C(O)-NH2) or a carbonate group (-OC(O)O-), and more preferably an acid anhydride residue. When the F polymer has an oxygen-containing polar group, the number of oxygen-containing polar groups in the F polymer is 1×10 6 The number of oxygen-containing polar groups per unit is preferably 10 to 5000, more preferably 100 to 3000. The number of oxygen-containing polar groups in the F polymer can be quantified by the composition of the polymer or the method described in WO 2020 / 145133.
[0015] The oxygen-containing polar group may be contained in a unit based on a monomer in the F polymer, or may be contained in a terminal group of the main chain of the F polymer, the former being preferred. The latter embodiment includes an F polymer having an oxygen-containing polar group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., and an F polymer obtained by subjecting an F polymer to plasma treatment or ionizing radiation treatment.
[0016] The F polymer is preferably a polymer (1) that does not have an oxygen-containing polar group and contains TFE units and PAVE units, and contains 2.0 to 5.0 mol% of PAVE units based on the total units, or a polymer (2) that contains TFE units and PAVE units and has an oxygen-containing polar group. If such an F polymer is used, spherulites having a relatively small radius are easily formed, so that the surface property of the polymer layer formed from the composition is easily increased, and the maximum height Sz is easily controlled to a predetermined range described later.
[0017] It is more preferable that the polymer (1) is composed only of TFE units and PAVE units, and contains more than 2.5 mol % and 5.0 mol % or less of PAVE units based on the total units. In addition, the fact that the polymer (1) does not have an oxygen-containing polar group means that the number of the oxygen-containing polar groups is 1×10 of the carbon atoms constituting the polymer main chain. 6 This means that the number of oxygen-containing polar groups in the polymer is less than 500 per unit. The number of the oxygen-containing polar groups is preferably 100 or less, more preferably less than 50. The lower limit of the number of the oxygen-containing polar groups is 1. The polymer (1) may be produced by using a polymerization initiator or a chain transfer agent that does not generate an oxygen-containing polar group as a terminal group of the polymer chain, or by fluorinating an F polymer having an oxygen-containing polar group (such as an F polymer having an oxygen-containing polar group derived from a polymerization initiator at the terminal group of the polymer main chain). Examples of the fluorination method include a method using fluorine gas (see JP 2019-194314 A, etc.).
[0018] The polymer (2) is preferably a polymer having a carbonyl group-containing group containing TFE units and PAVE units, more preferably a polymer containing TFE units, PAVE units, and units based on a monomer having a carbonyl group-containing group, and more preferably a polymer containing these units in this order in an amount of 90 to 99 mol%, 0.99 to 9.97 mol%, and 0.01 to 3 mol% based on all units. Specific examples of such F polymers include the polymers described in WO 2018 / 16644. The monomer having a carbonyl group-containing group is preferably itaconic anhydride, citraconic anhydride, or 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH"), and more preferably NAH.
[0019] In this method, the F particles contained in the dispersion are particles that include an F polymer, and preferably consist of an F polymer. The D50 of the F particles is 1 μm or more and less than 10 μm. The F particles may be solid particles or non-hollow particles. The F particles may be secondary particles formed from nanometer-order fine particles. The D50 of the F particles is preferably 1.0 μm or more, more preferably 1.5 μm or more. The D50 of the F particles is preferably 6 μm or less, more preferably 5 μm or less. Furthermore, D90 of the F particles is preferably 8 μm or less, and more preferably 6 μm or less. When the D50 and D90 of the F particles are within the above ranges, the above-mentioned mechanism of action is more easily manifested, and it is easier to obtain a dispersion having a particle concentration of 5 to 100 particles / ml having a particle diameter of 20 to 80 μm as measured with a particle counter. One type of F particle may be used, or two or more types of F particles may be used.
[0020] The specific surface area of F particles is 1 to 25 m 2 / g, and 6 to 15m 2 When the specific surface area of the F particles is within the above range, it is considered that the F particle surfaces are easily wetted and F particle aggregates are easily disintegrated, making it easier to realize the above-mentioned mechanism of action, and making it easier to obtain a dispersion liquid in which the particle concentration of particles having particle diameters of 20 to 80 μm measured with a particle counter is 5 to 100 particles / ml. In addition, the polymer layer formed on the coating layer made of this dispersion through a specific heating process is more likely to satisfy the specified range of maximum height Sz specified in ISO25178, and is more likely to have excellent adhesion to the substrate layer in addition to the physical properties inherent to the F polymer, such as heat resistance and electrical properties (low linear expansion coefficient, low dielectric constant and low dielectric tangent).
[0021] This dispersion contains 100 parts by mass of F particles and 80 to 300 parts by mass of water, and has a particle concentration of 5 to 100 particles / ml having a particle diameter of 20 to 80 μm as measured with a particle counter. The content of F particles in the present dispersion is preferably 25% by mass or more, more preferably 30% by mass or more, and is preferably 55% by mass or less, more preferably 50% by mass or less. The water content in the present dispersion is preferably 25% by mass or more, and more preferably 40% by mass or more. The water content is preferably less than 70% by mass, and more preferably 65% by mass or less. The water content in the present dispersion is preferably 60 to 180% by mass relative to the F particle content. In the present dispersion, the particle concentration of particles having a particle diameter of 20 to 80 μm as measured by a particle counter is preferably 10 particles / ml or more. The particle concentration is preferably 80 particles / ml or less, more preferably 60 particles / ml or less. When the particle concentration is within the above range, the above-mentioned mechanism of action is more easily expressed, and the maximum height Sz of the polymer layer obtained by the present method can be easily controlled within a specific range.
[0022] The dispersion may further contain 5 to 20 parts by mass of a water-soluble solvent having a surface tension of 20 to 30 mN / m. The water-soluble solvent having a surface tension of 20 to 30 mN / m is a compound that is liquid at 25°C under atmospheric pressure, preferably a compound having a boiling point of 160°C or less, more preferably a compound having a boiling point of 120°C or less. Such a water-soluble solvent is preferably azeotropic with water. In this specification, the water-soluble solvent means a solvent having a solubility in water of 100 g / L or more. The water-soluble solvent is preferably a monool having 1 to 6 carbon atoms, more preferably methanol (23 mN / m), ethanol (23 mN / m), 1-propanol (24 mN / m), 2-propanol (22 mN / m), 1-butanol (25 mN / m), 2-butanol (24 mN / m), isobutanol (23 mN / m), 1-methoxy-2-propanol (26 mN / m), 2-propoxy-ethanol (27 mN / m), 1-propoxy-2-propanol (25 mN / m), 2-ethoxyethanol (26 mN / m), and even more preferably ethanol. The numerical values in parentheses are the surface tensions of the monools. When the present dispersion further contains a water-soluble solvent, the amount is preferably 0.1 to 5 mass % or less based on the total amount of the present dispersion. The content of the water-soluble solvent in the present dispersion is preferably 1 to 10 mass % based on the content of the F particles. In the present dispersion, the water-soluble solvent is considered to play a role in adjusting the concentration of particles with a particle size of 20 to 80 μm, and also to play a role as an antifoaming agent such as a foam suppressing action or a foam breaking action.
[0023] The dispersion may further contain a nonionic surfactant, such as a glycol surfactant, an acetylene surfactant, a silicone surfactant, or a fluorine surfactant. Among these, nonionic surfactants having a hydroxyl group in the hydrophilic site are preferred, and organopolysiloxanes having a hydroxyl group or a polyoxyalkylene group, whose mass loss rate at 200 to 300° C. is 20% by mass / ° C. or more, are more preferred. The mass loss rate is preferably 90% by mass / ° C. or less. When the present dispersion contains the above-mentioned nonionic surfactant, the above-mentioned mechanism of action is more easily manifested, and the dispersion stability and handleability of the F particles are more likely to be excellent. Furthermore, the rheological properties of the dispersion are improved, and handling properties such as film-forming properties tend to improve. The "mass loss rate at 200 to 300°C" of an organopolysiloxane is a value determined as a percentage of the mass loss amount when the temperature is raised from 200°C to 300°C using a thermogravimetry device (TG) and a thermogravimetry-differential thermal analyzer (TG-DTA) at a heating rate of 10°C / min, a sample weight of 10 mg, and an atmosphere of a mixed gas consisting of 90% by volume of helium and 10% by volume of oxygen, divided by the heating time (10 minutes) and the sample weight (10 mg). The organopolysiloxane is more preferably a polyoxyalkylene-modified dimethylsiloxane having a polyoxyalkylene structure as the hydrophilic portion and a polydimethylsiloxane structure as the hydrophobic portion. Polyoxyalkylene-modified dimethylsiloxane has a polydimethylsiloxane unit (-(CH3)2SiO 2 / 2 -), may have polydimethylsiloxane units in the side chain, or may have polydimethylsiloxane units in both the main chain and the side chain.
[0024] Specific examples of nonionic surfactants include the "Ftergent" series (manufactured by Neos), the "Surflon" series (manufactured by AGC Seimi Chemical Co., Ltd.), the "Megafac" series (manufactured by DIC Corporation), the "Unidyne" series (manufactured by Daikin Industries, Ltd.), "BYK-347", "BYK-349", "BYK-378", "BYK-3450", "BYK-3451", "BYK-3455", "BYK-3456" (manufactured by BYK Japan), "KF-6011", "KF-6043" (manufactured by Shin-Etsu Chemical Co., Ltd.), and the "Tergitol" series (manufactured by The Dow Chemical Company, "Tergitol TMN-100X", etc.). The nonionic surfactant may be used alone or in combination of two or more kinds. When the present dispersion further contains a nonionic surfactant, the amount thereof is preferably within the range of 1 to 15 parts by mass relative to 100 parts by mass of the present dispersion.
[0025] The dispersion may further contain a water-soluble polymer. Examples of the water-soluble polymer include at least one selected from the group consisting of vinyl alcohol-based polymers, acrylic polymers, polyvinylpyrrolidone, polypyrrole, polythiophene, polyethyleneimine, and cellulose ether. In addition, a water-soluble polymer having a polar functional group and having a mass reduction rate of less than 40 mass% / °C at 200 to 300°C is more preferable. The mass reduction rate is preferably 35 mass% / °C or less, more preferably 30 mass% / °C or less. In addition, the mass reduction rate is preferably 5 mass% / °C or more. The "mass reduction rate at 200 to 300°C" of the water-soluble polymer is determined in the same manner as the "mass reduction rate at 200 to 300°C" of the organopolysiloxane described above. In this specification, the term "water-soluble polymer" refers to a polymer having a solubility in water of 20 g / L or more. When the present dispersion contains the above-mentioned water-soluble polymer, the above-mentioned mechanism of action is more easily exhibited, and the concentration of particles having a particle size of 20 to 80 μm in the present dispersion can be easily adjusted to a predetermined range, and the rheological properties of the present dispersion are improved, and the handling properties such as film-forming properties are easily improved.
[0026] Examples of vinyl alcohol-based polymers include polyvinyl alcohol, polyvinyl acetate, partially acetylated or partially acetalized polyvinyl alcohol, and copolymers of vinyl alcohol, vinyl butyral, and vinyl acetate. Specific examples of vinyl alcohol-based polymers include the "S-LEC (registered trademark) B" series, the "S-LEC (registered trademark) K (KS)" series, and the "S-LEC (registered trademark) SV" series (all manufactured by Sekisui Chemical Co., Ltd.), and the "Mobital (registered trademark)" series (manufactured by Kuraray Co., Ltd.). Examples of acrylic acid-based polymers include polyacrylic acid, salts of polyacrylic acid such as sodium polyacrylate, sodium acrylic acid / maleic acid copolymer, and sodium acrylic acid / sulfonic acid monomer copolymer; polyacrylates such as methyl polyacrylate and ethyl polyacrylate; poly-α-haloacrylate; poly-α-cyanoacrylate; and polyacrylamide.
[0027] The cellulose ether includes carboxyalkyl cellulose, hydroxyalkyl cellulose, or hydroxyalkyl alkyl cellulose, and is preferably carboxyalkyl cellulose, hydroxyalkyl cellulose, or hydroxyalkyl alkyl cellulose. Examples of the carboxyalkyl cellulose include carboxymethyl cellulose, etc. Examples of the hydroxyalkyl cellulose include hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, etc. Examples of the hydroxyalkyl alkyl cellulose include hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl ethyl cellulose, and hydroxyethyl ethyl methyl cellulose. Specific examples of cellulose ethers include the "Sunrose (registered trademark)" series (manufactured by Nippon Paper Industries Co., Ltd.), the "Metolose (registered trademark)" series (manufactured by Shin-Etsu Chemical Co., Ltd.), and "HEC CF Grade" (manufactured by Sumitomo Seika Chemicals Co., Ltd.). The water-soluble polymer may be used alone or in combination with two or more kinds. When the present dispersion further contains a water-soluble polymer, the amount thereof is preferably within a range of 1 to 15 parts by mass relative to 100 parts by mass of the present dispersion.
[0028] In addition to water and the above-mentioned water-soluble solvent, the present dispersion may contain other dispersion media within the range that does not impair the effects of the present invention. Such other dispersion media are preferably miscible with the above-mentioned water-soluble solvent and water. Examples of other dispersion media include amides such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylpropanamide, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-diethylformamide, hexamethylphosphoric triamide, and 1,3-dimethyl-2-imidazolidinone; and ketones such as acetone and methyl ethyl ketone.
[0029] The present dispersion may further contain inorganic particles, in which case the polymer layer formed from the present dispersion is likely to have excellent electrical properties and low linear expansion. Examples of inorganic particles include silicon compounds such as quartz powder, silica, wollastonite, talc, silicon nitride, silicon carbide, and mica; nitrogen compounds such as boron nitride and aluminum nitride; metal oxides such as aluminum oxide, zinc oxide, titanium oxide, cerium oxide, beryllium oxide, magnesium oxide, nickel oxide, vanadium oxide, copper oxide, iron oxide, and silver oxide; carbon fibers; carbon allotropes such as graphite, graphene, and carbon nanotubes; and metals such as silver and copper. One type of inorganic particle may be used, or two or more types may be used in combination. The inorganic particles preferably have a D50 of 0.1 to 50 μm. The surfaces of the inorganic particles may be treated with a silane coupling agent. When the present dispersion contains inorganic particles, the content of the inorganic particles in the present dispersion is preferably 1 to 25% by mass.
[0030] The present dispersion may further contain another resin different from the F polymer. Such another resin may be contained in the present dispersion as non-hollow particles, or may be dissolved or dispersed in a liquid dispersion medium (hereinafter also referred to as "liquid dispersion medium") such as water, a water-soluble solvent, or another dispersion medium that constitutes the present dispersion. Examples of other resins include polyester resins such as liquid crystalline aromatic polyesters, polyimide resins, polyamideimide resins, epoxy resins, maleimide resins, urethane resins, polyphenylene ether resins, polyphenylene oxide resins, and polyphenylene sulfide resins. The other resin is preferably an aromatic polymer, more preferably at least one aromatic imide polymer selected from the group consisting of aromatic polyimide, aromatic polyamic acid, aromatic polyamideimide, and a precursor of aromatic polyamideimide. The aromatic polymer is preferably contained in the present dispersion as a varnish dissolved in a liquid dispersion medium.
[0031] Specific examples of aromatic imide polymers include the "UPIA-AT" series (manufactured by UBE), the "NEOPLUMI (registered trademark)" series (manufactured by Mitsubishi Gas Chemical Company, Inc.), the "SPIXELIA (registered trademark)" series (manufactured by Somar), the "Q-PILON (registered trademark)" series (manufactured by PI Technical Research Institute), the "WINGO" series (manufactured by Wingo Technology Co., Ltd.), the "TOMAID (registered trademark)" series (manufactured by T&K TOKA Corporation), the "KPI-MX" series (manufactured by Kawamura Sangyo Co., Ltd.), "HPC-1000" and "HPC-2100D" (all manufactured by Showa Denko Materials Co., Ltd.). When the present dispersion further contains another resin, the content of the other resin relative to the F particles is preferably 1 to 25% by weight.
[0032] The present dispersion may further contain additives such as a thixotropic agent, a viscosity modifier, an antifoaming agent, a dehydrating agent, a plasticizer, a weathering agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a whitening agent, a colorant, a conductive agent, a release agent, and a flame retardant.
[0033] The present dispersion is obtained by mixing 100 parts by mass of F particles, 80 to 300 parts by mass of water, and, if necessary, the water-soluble solvent, nonionic surfactant, other dispersion medium, inorganic particles, other resins, additives, etc. The present dispersion may be obtained by mixing F particles and water all at once, or by dividing and mixing them several times. In addition, there is no particular limitation on the order of mixing when the water-soluble solvent, nonionic surfactant, other dispersion medium, inorganic particles, other resins, additives, etc. are further mixed as necessary, and they may be mixed with the F particles in advance, may be added to water in advance and then mixed with the F particles, or may be mixed when the F particles and water are mixed.
[0034] Examples of mixing devices for obtaining the present dispersion include stirring devices equipped with blades, such as a Henschel mixer, a pressure kneader, a Banbury mixer, and a planetary mixer; grinding devices equipped with media, such as a ball mill, an attritor, a basket mill, a sand mill, a sand grinder, a Dyno Mill, a Dispermat, an SC Mill, a spike mill, and an agitator mill; and dispersing devices equipped with other mechanisms, such as a microfluidizer, a nanomizer, an ultimizer, an ultrasonic homogenizer, a dissolver, a disperser, a high-speed impeller, a thin film swirling high-speed mixer, a planetary stirrer, and a V-type mixer.
[0035] The viscosity of the present dispersion is preferably 10 mPa·s or more, more preferably 100 mPa·s or more. The viscosity of the present dispersion is preferably 10,000 mPa·s or less, more preferably 3,000 mPa·s or less. In this case, the present dispersion has excellent coatability and is easy to form a polymer layer of any thickness. In addition, the present dispersion having a viscosity in this range is easy to highly express the physical properties of the F polymer in the polymer layer formed therefrom. The thixotropy ratio of the present dispersion is preferably 1.0 to 3.0, in which case the present dispersion has excellent coatability and homogeneity and is likely to form a denser polymer layer. These liquid properties are likely to be improved when the present dispersion further contains the above-mentioned water-soluble polymer.
[0036] From the viewpoint of improving long-term storage stability, the pH of the present dispersion is more preferably 8 to 10. The pH of the present dispersion can be adjusted with a pH adjuster (amine, ammonia, citric acid, etc.) or a pH buffer (tris(hydroxymethyl)aminomethane, ethylenediaminetetraacetic acid, ammonium hydrogen carbonate, ammonium carbonate, ammonium acetate, etc.).
[0037] In this method, the present dispersion is applied to a substrate layer to form a coating layer made of the present dispersion on the surface of the substrate layer. Examples of the method for applying the present dispersion include a coating method, a droplet ejection method, and a dipping method, and the present dispersion is preferably applied to a substrate layer by a roll coating method, a knife coating method, a bar coating method, a die coating method, or a spray method.
[0038] The substrate layer is preferably a heat-resistant substrate. Examples of the heat-resistant substrate include metal substrates such as metal foils of copper, nickel, aluminum, titanium, and alloys thereof; heat-resistant resin films such as polyimide, polyamide, polyetheramide, polyphenylene sulfide, polyaryl ether ketone, polyamideimide, liquid crystal polymers such as liquid crystal polyester, and tetrafluoroethylene-based polymers other than F polymers such as polytetrafluoroethylene; prepreg substrates (precursors of fiber-reinforced resin substrates), ceramic substrates such as silicon carbide, aluminum nitride, and silicon nitride; and glass substrates. Among these, the heat-resistant substrate is preferably a film of any one of heat-resistant resins such as polyimide, liquid crystal polymer, and polytetrafluoroethylene, and a polyimide film is more preferable.
[0039] The shape of the substrate may be flat, curved, or uneven, and may be any of a foil, plate, film, and fiber shape. In this method, the substrate layer may be a long substrate, which is preferable from the viewpoint of improving productivity because a roll-to-roll process can be applied and the film or sheet and laminate of the present invention described later can be produced as a roll-shaped product in a long form. The ten-point average roughness of the surface of the substrate is preferably 0.01 to 0.05 μm. The surface of the substrate may be surface-treated with a silane coupling agent or plasma-treated. As the silane coupling agent, a silane coupling agent having a functional group such as 3-aminopropyltriethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, or 3-isocyanatepropyltriethoxysilane is preferable.
[0040] Next, the substrate layer having the coating layer is first heated in a temperature range of 25°C or higher, lower than the boiling point of water constituting the dispersion and lower than [the glass transition temperature of the F polymer + 10°C], and then secondly heated in a temperature range higher than the above temperature range and lower than the melting temperature of the F polymer to obtain a substrate layer having a layer containing F particles on its surface. The lower limit of the initial heating temperature is preferably 40° C. or higher. The upper limit of the initial heating is preferably below the glass transition temperature of the F polymer. The second heating is preferably carried out in a temperature range that is at least 50° C. higher than the temperature range of the first heating and is at most [the melting temperature of the F polymer −100° C.]. Specifically, it is preferable that the temperature range of the first heating is 45 to 95°C, and the temperature range of the second heating is 100 to 150°C.
[0041] The above-mentioned first heating and second heating are both preferably performed for 1 to 30 minutes. In the first heating and second heating, the liquid dispersion medium does not need to be completely removed, and it is sufficient to remove it to the extent that the layer formed by the packing of the F particles can maintain a self-supporting film. In addition, in the first heating and second heating, air may be blown to promote removal of the liquid dispersion medium by air drying.
[0042] The substrate layer having the layer containing F particles on its surface obtained by the second heating is further heated (hereinafter also referred to as "third heating") in a temperature range equal to or higher than the melting temperature of the F polymer to form a polymer layer containing the molten and sintered body of F particles (hereinafter also referred to as "F layer") on the surface of the substrate layer. In other words, a laminate having an F layer and a substrate layer in this order is obtained. Specifically, the temperature range of the third heating is preferably 340 to 400° C. The heating time of the third heating is preferably 0.1 to 30 minutes.
[0043] The heating device for each of the first heating, the second heating, and the third heating may be an oven or a ventilation drying furnace. The heat source in the device may be a contact type heat source (hot air, hot plate, etc.) or a non-contact type heat source (infrared rays, etc.). In this method, each heating step may be performed under normal pressure (atmospheric pressure) or reduced pressure, and the atmosphere in each heating step may be either air or inert gas (helium gas, neon gas, argon gas, nitrogen gas, etc.).
[0044] The F layer is formed through the steps of coating the present dispersion on the substrate layer, and the first, second and third heating. These steps may be performed once each, or may be repeated two or more times. For example, the present dispersion may be coated on the surface of the substrate layer to obtain a coating layer, the F layer may be formed by the first, second and third heating, the present dispersion may be further coated on the surface of the F layer to form a coating layer, and the second F layer may be formed by the above-mentioned heating. Alternatively, the present dispersion may be coated on the surface of the substrate layer to obtain a coating layer, and at the stage where the liquid dispersion medium is removed by the above-mentioned first and second heating, the present dispersion may be further coated on the surface, and the F layer may be formed by the above-mentioned heating. The first heating may be carried out stepwise at a plurality of temperatures within the temperature range of the first heating, and the second heating may be carried out stepwise at a plurality of temperatures within the temperature range of the second heating.
[0045] The dispersion may be disposed on only one surface of the substrate layer, or on both surfaces of the substrate layer. In the former case, a laminate having a substrate layer and an F layer on one surface of the substrate layer is obtained, and in the latter case, a laminate having a substrate layer and an F layer on both surfaces of the substrate layer is obtained. By separating the substrate layer from such a laminate, a film or sheet containing the F polymer, which is a molten and sintered product of the F particles, can be obtained.
[0046] Suitable specific examples of the laminate include a metal-clad laminate having a metal foil and an F layer on at least one surface of the metal foil, and a multilayer film having a polyimide film and an F layer on both surfaces of the polyimide film.
[0047] The thickness of the F layer is preferably 25 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more. The thickness of the F layer is preferably 300 μm or less. The dielectric constant of the F layer is preferably 2.4 or less, more preferably 2.0 or less. Also, the dielectric constant is preferably greater than 1.0. The dielectric tangent of the F layer is preferably 0.0022 or less, more preferably 0.0020 or less. Also, the dielectric tangent is preferably greater than 0.0010. The thermal conductivity of the F layer is preferably 1 W / m·K or more, more preferably 3 W / m·K or more. The thermal conductivity of the F layer means the thermal conductivity in the in-plane direction of the F layer.
[0048] The linear expansion coefficient of the F layer is preferably 100 ppm / ° C. or less, more preferably 80 ppm / ° C. or less. The lower limit of the linear expansion coefficient of the F layer is 30 ppm / ° C. The linear expansion coefficient means a value obtained by measuring the linear expansion coefficient of a test piece in the range of 25° C. or more and 260° C. or less according to the measurement method specified in JIS C 6471:1995. The peel strength between the F layer and the base layer is preferably 10 N / cm or more, more preferably 15 N / cm or more, and is preferably 100 N / cm or less.
[0049] The present invention also relates to a polymer layer formed on the surface of a base layer, the polymer layer comprising a molten-sintered product of F particles having a D50 of 1 μm or more and less than 10 μm, and a film or sheet having a maximum height Sz of the polymer layer defined in ISO 25178 of 0.1 μm or more and less than 10 μm. The maximum height Sz is preferably 0.9 μm or more, more preferably 1.0 μm or more. On the other hand, the maximum height Sz is preferably less than 8 μm, more preferably less than 5 μm. When the maximum height Sz of the polymer layer surface as defined by ISO25178 is within the above range, the above-mentioned effects are more effectively achieved, and the adhesive force between the polymer layer and the base layer can be maintained. The maximum height Sz can be measured, for example, by a laser microscope.
[0050] As described above, the film or sheet which is the polymer layer is preferably obtained by first forming a coating layer made of the dispersion on the surface of the substrate layer by applying the present dispersion to the substrate layer, and then forming a polymer layer containing the molten-sintered product of F particles through the steps of the first heating, the second heating, and the third heating. In other words, it is only by going through such steps that a film or sheet which is the polymer layer containing the molten-sintered product of F particles and which satisfies the above-mentioned predetermined range of Sz can be obtained. Here, the concentration of particles having a particle diameter of 20 to 80 μm as measured by a particle counter in this dispersion can be controlled to 5 to 100 particles / ml by, for example, using F particles having a specific specific surface area using a specific F polymer and dispersing them by controlling the blend ratio with water, and further including one or more of the above-mentioned water-soluble solvents, nonionic surfactants, and water-soluble polymers. The preferred ranges of the thickness, dielectric constant, dielectric dissipation factor, thermal conductivity, and linear expansion coefficient of such a film or sheet are the same as the preferred ranges of the thickness, dielectric constant, dielectric dissipation factor, thermal conductivity, and linear expansion coefficient of the F layer in the laminate formed from the above-mentioned dispersion.
[0051] The present invention also relates to a laminate having a base layer and a polymer layer formed on a surface of the base layer, the polymer layer comprising a molten-sintered product of F particles having a D50 of 1 μm or more and less than 10 μm, and the maximum height Sz of the polymer layer as defined by ISO25178 is 0.1 μm or more and less than 10 μm. In such a laminate, the substrate layer is preferably a heat-resistant substrate, and the heat-resistant substrate is more preferably a metal foil or a heat-resistant resin film. Details of the heat-resistant substrate, metal foil or heat-resistant resin film are the same as those described above in the description of this method. The maximum height Sz of the polymer layer defined by ISO25178 is as described above. Moreover, such a laminate preferably has a polymer layer on both surfaces of the substrate layer. The preferred ranges of the thickness, dielectric constant, dielectric dissipation factor, thermal conductivity, linear expansion coefficient, and peel strength between the polymer layer and the base layer in such a laminate are the same as the preferred ranges of the thickness, dielectric constant, dielectric dissipation factor, thermal conductivity, linear expansion coefficient, and peel strength between the F layer and the base layer in the laminate formed from the above-mentioned dispersion.
[0052] The polymer layers, which are films or sheets, and laminates formed by this method are useful as antenna parts, printed circuit boards, aircraft parts, automobile parts, sports equipment, food industry products, heat dissipation parts, and the like. Specifically, these include electric wire coating materials (aircraft electric wires, rectangular wires, FFC (Flexible Flat Cable), etc.), enameled wire coating materials used in motors for electric vehicles, etc., power generation coating materials, electrical insulating tapes, insulating tapes for oil drilling, oil transport hoses, hydrogen tanks, materials for printed circuit boards, separation membranes (microfiltration membranes, ultrafiltration membranes, reverse osmosis membranes, ion exchange membranes, dialysis membranes, gas separation membranes, etc.), electrode binders (for lithium secondary batteries, for fuel cells, etc.), carrier films for fuel cells, tape base films for the semiconductor manufacturing process (dicing tape, pick-up tape, etc.), release films for semiconductor molding, liquid crystal antennas, reflectors, transmission lines, COF (Chip on Fuel) base films for electrostatic chucks for semiconductor manufacturing processes, electrostatic chucks for display manufacturing processes, copy rolls, furniture, automobile dashboards, covers for home appliances, etc., sliding parts (load bearings, yaw bearings, sliding shafts, valves, bearings, bushes, seals, thrust washers, wear rings, pistons, slide switches, gears, cams, belt conveyors, food transport belts, etc.), tension ropes, wear pads, wear strips, tube lamps, test sockets, wafer guides, wear parts for centrifugal pumps, chemical and water supply pumps, tools (shovels, files, drills, saws, etc.), boilers, hoppers, pipes, ovens, baking molds, chutes, racket strings, dies, toilets, container coating materials, heat dissipation boards for mounting power devices, heat dissipation parts for wireless communication devices, transistors, thyristors, rectifiers, transformers, power MOS They are useful as FETs, CPUs, heat dissipation fins, metal heat sinks, blades for wind turbines, wind power generation equipment, and aircraft, housings for personal computers and displays, electronic device materials, interior and exterior parts of automobiles, sealing materials for processing machines and vacuum ovens that perform heat treatment under low oxygen conditions, plasma processing equipment, heat dissipation parts in processing units for sputtering and various dry etching equipment, and electromagnetic wave shielding.
[0053] The polymer layers (films or sheets) and laminates formed by this method are useful as electronic substrate materials such as flexible printed wiring boards and rigid printed wiring boards, protective films and heat dissipation substrates, particularly heat dissipation substrates for automobiles. EXAMPLES
[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. 1. Preparation of each ingredient [F Polymer] F particle 1: containing 97.9 mol% of TFE units, 0.1 mol% of NAH units, and 2.0 mol% of PPVE units, in that order, and having a carbonyl group-containing group with a main chain carbon number of 1×10 6 Particles of tetrafluoroethylene polymer (melting point: 300°C) with 1000 particles per particle (D50: 2.0 μm, specific surface area: 7 m 2 / g)
[0055] 2. Dispersion liquid production example [Example 1] F particles 1, organopolysiloxane (a nonionic surfactant with an HLB value of 13 and a mass reduction rate of 25%), hydroxyethyl cellulose with a mass reduction rate of 20%, and water were added to the pot, and zirconia balls were added. The pot was then rolled at 150 rpm for 1 hour to obtain dispersion 1 containing F particles 1 (35 parts by mass), organopolysiloxane (5 parts by mass), hydroxyethyl cellulose (0.1 parts by mass), and water (59.9 parts by mass). 1.44 ml of dispersion 1 was taken and diluted 250 times. The entire amount was then passed through a particle size distribution measuring device (AccuSizer (registered trademark) A7000APS manufactured by Japan Entegris Co., Ltd., using an LE400 sensor) to measure the particle concentration with particle diameters of 20 to 80 μm, which was 20 particles / ml.
[0056] [Example 2] Dispersion liquid 2 containing F particles 1 (35 parts by mass), organopolysiloxane (5 parts by mass), hydroxyethyl cellulose (1.0 part by mass) and water (59.0 parts by mass) was obtained in the same manner as in Example 1, except that the amount of hydroxyethyl cellulose was changed. 1.44 ml of Dispersion Liquid 2 was taken, and the concentration of particles with particle sizes of 20 to 80 μm was measured in the same manner as in Example 1, and was found to be 100 particles / ml.
[0057] [Example 3] Dispersion 3 containing F particles 1 (35 parts by mass), organopolysiloxane (5 parts by mass), polyacrylic acid (0.1 parts by mass) and water (59.9 parts by mass) was obtained in the same manner as in Example 1, except that polyacrylic acid having a mass reduction rate of 40% was used instead of hydroxyethyl cellulose. 1.44 ml of Dispersion Liquid 3 was taken, and the concentration of particles with particle sizes of 20 to 80 μm was measured in the same manner as in Example 1, and was found to be 4 particles / ml.
[0058] 3. Example of laminate production and evaluation of polymer layer A laminate was produced using each of the dispersions 1 to 3, and the formed polymer layer was evaluated. Specifically, each dispersion was coated on one side of a polyimide film (thickness 25 μm) by a roll-to-roll process using a small-diameter gravure reverse method to form a coating layer, and the coating layer was passed through a ventilated drying oven at an oven temperature of 70° C. for 5 minutes to perform the first heating, and then passed through a ventilated drying oven at an oven temperature of 150° C. for 5 minutes to perform the second heating, forming a polyimide film having a layer containing F particles 1 on its surface. Next, the other side of the polyimide film was subjected to the same operation to form a polyimide film having layers containing F particles 1 on both surfaces. Furthermore, this polyimide film was passed through a far-infrared furnace at a furnace temperature of 350°C for 5 minutes to melt and sinter the F particles 1, forming a polymer layer containing the molten and sintered F particles 1 on one side of the substrate 1, thereby obtaining laminates 1 to 3 having a polymer layer (thickness 25 μm) and the substrate 1. Using a laser microscope (Keyence Corporation's shape analysis laser microscope "VK-X150"), the maximum height Sz of the surface of the polymer layer was measured in accordance with ISO 25178. As a result, the Sz of the polymer layer produced from Dispersion 1 was 1.5 μm, the Sz of the polymer layer produced from Dispersion 2 was 10 μm, and the Sz of the polymer layer produced from Dispersion 3 was 0.08 μm.
[0059] Electrolytic copper foil (Fukuda Metal Foil & Powder Co., Ltd., "CF-T49A-DS-HD2", thickness: 12 μm) was placed on both sides of each laminate, and pressed under vacuum at 340° C. for 20 minutes to obtain double-sided copper-clad laminates. The interlayer adhesion of the double-sided copper-clad laminate obtained from Laminate 1 was significantly higher than the interlayer adhesion of Laminate 2 and Laminate 3, respectively. In addition, when the transmission loss of the printed wiring board obtained from the double-sided copper clad laminate at a frequency of 40 GHz was measured, it was found that the transmission loss of the double-sided copper clad laminate obtained from laminate 1 was significantly lower than the transmission loss of the double-sided copper clad laminate obtained from laminate 3. [Industrial Applicability]
[0060] The polymer layer obtained by this method and the laminate having the polymer layer exhibit the physical properties of the F polymer to a high degree and have excellent adhesion to the base layer, and therefore can be effectively used for applications such as printed wiring boards.
Claims
1. A method for producing a polymer layer, comprising: coating a substrate layer with a dispersion liquid containing 100 parts by mass of tetrafluoroethylene-based polymer particles having an average particle size of 1 μm or more and less than 10 μm, and 80 to 300 parts by mass of water, the dispersion liquid having a particle concentration of 5 to 100 particles / ml having a particle size of 20 to 80 μm as measured with a particle counter, to form a coating layer made of the dispersion liquid on the surface of the substrate layer; first heating the substrate layer having the coating layer in a temperature range of 25° C. or more, lower than the boiling point of the water, and lower than [glass transition temperature of the tetrafluoroethylene-based polymer + 10° C.], subsequently performing a second heating in a temperature range higher than the above temperature range and lower than the melting temperature of the tetrafluoroethylene-based polymer, to obtain the substrate layer having a layer containing tetrafluoroethylene-based polymer particles on its surface, and further heating in a temperature range equal to or higher than the melting temperature to form a polymer layer containing the tetrafluoroethylene-based polymer on the surface of the substrate layer.
2. The process of claim 1 , wherein the tetrafluoroethylene-based polymer comprises units based on perfluoro(alkyl vinyl ether).
3. The process according to claim 1 , wherein the tetrafluoroethylene-based polymer is a heat-fusible tetrafluoroethylene-based polymer having a carbonyl group-containing group.
4. The method according to claim 1 , wherein the content of the tetrafluoroethylene-based polymer particles is 30% by mass or more.
5. The method according to claim 1, wherein the dispersion further comprises 5 to 20 parts by mass of a water-soluble solvent having a surface tension of 20 to 30 mN / m.
6. The method according to claim 1 , wherein the dispersion further comprises a nonionic surfactant.
7. The method according to claim 1 , wherein the dispersion further comprises a water-soluble polymer.
8. The method according to claim 1 , wherein the polymer layer has a maximum height Sz defined by ISO 25178 of 0.1 μm or more and less than 10 μm.
9. The method according to any one of claims 1 to 9, wherein the substrate layer is a long substrate.
10. A film or sheet comprising a polymer layer formed on a surface of a base layer, the polymer layer comprising a molten-sintered product of particles of a tetrafluoroethylene-based polymer having an average particle diameter of 1 μm or more and less than 10 μm, and the maximum height Sz of the polymer layer as defined in ISO 25178 is 0.1 μm or more and less than 10 μm.
11. A laminate comprising a base layer and a polymer layer formed on a surface of the base layer, the polymer layer comprising a molten-sintered product of particles of a tetrafluoroethylene-based polymer having an average particle diameter of 1 μm or more and less than 10 μm, and the polymer layer having a maximum height Sz defined in ISO 25178 of 0.1 μm or more and less than 10 μm.
12. The laminate according to claim 11 , wherein the substrate is a heat resistant substrate.
13. The laminate according to claim 12, wherein the heat-resistant substrate is a metal foil or a heat-resistant resin film.
14. The laminate according to any one of claims 11 to 13, comprising the polymer layers on both surfaces of the base layer.
Citation Information
Patent Citations
Substrate for printed wiring board and method for manufacturing same, printed wiring board and method for manufacturing same, and resin base material