Battery insulation sheet and manufacturing method therefor
The battery insulation sheet with an airgel layer and fibrous support addresses thermal insulation and dust issues in high-capacity batteries, offering improved safety and durability through uniform airgel distribution and binding.
Patent Information
- Application Number
- JP2023133476
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2023-08-18
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-08-18
AI Technical Summary
Conventional insulation methods for high-capacity batteries, such as lithium-ion secondary batteries, fail to provide effective thermal insulation and are prone to dust generation, which can lead to thermal runaway and safety issues.
A battery insulation sheet comprising a base material with an airgel layer coated on its surface, incorporating a fibrous support, airgel, binder, and dispersant, adhering to the ratio T_i/D_s = 50 to 100,000, where T_i is the thickness of the airgel layer and D_s is the average diameter of the fibrous support, ensuring uniform distribution and high binding force.
The solution provides excellent heat insulation, compression properties, and prevents dust generation, enhancing safety by blocking flame propagation and improving the durability of battery modules.
Smart Images

Figure 2024152552000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery insulation sheet and a method for producing the same. [Background technology]
[0002] Secondary batteries are power storage systems that provide excellent energy density by converting electrical energy into chemical energy and storing it. Unlike primary batteries, which cannot be recharged, secondary batteries can be recharged and are widely used in IT devices such as smartphones, cellular phones, laptops, and tablet PCs. Recently, interest in electric vehicles has increased to prevent environmental pollution, and high-capacity secondary batteries are being adopted for electric vehicles. Such secondary batteries are required to have characteristics such as high density, high output, and stability.
[0003] Furthermore, when a battery contains a large number of high-capacity cells such as lithium-ion secondary batteries, there is a risk that one cell may overheat for some reason and go into thermal runaway, adversely affecting other adjacent cells, so it is necessary to thermally insulate adjacent cells from each other.
[0004] For this reason, conventionally, plates or insulating resin plates have been placed between the cells to insulate and heat the adjacent cells.
[0005] The above information disclosed in the Background of the Invention section is intended to enhance the understanding of the background of the present invention and may therefore include information that does not constitute prior art. Summary of the Invention [Problem to be solved by the invention]
[0006] One embodiment provides a battery insulation sheet having excellent insulation properties, compression properties and dust properties, and a manufacturing method thereof. [Means for solving the problem]
[0007] One embodiment provides a battery insulation sheet including a substrate and an aerogel layer formed on the substrate, the aerogel layer including a fibrous support, an aerogel, and a functional material including a binder, a dispersant, or a combination thereof, and satisfies the following formula 1: [Formula 1] 50≦A≦100000, A=T i / D s In the above formula 1, the above T i is the thickness of the aerogel layer, and D s is the average diameter of the fibrous support.
[0008] The aerogel layer may have a thickness of 1 mm to 10 mm.
[0009] The average diameter of the fibrous support may be 0.1 μm to 20 μm.
[0010] The A may be 200 to 10,000.
[0011] The surface of the fibrous support may be coated with an aerogel.
[0012] The substrate may contain one or more materials selected from the group consisting of resins, metals, and inorganic materials other than metals.
[0013] The fibrous support may comprise one or more fibers selected from the group consisting of natural fibers, silica fibers, glass fibers, carbon fibers, basalt fibers, and polymeric fibers.
[0014] The aerogel has a BET specific surface area of 500 m 2 / g~1,000m 2 / g.
[0015] The binder includes a water-based polymer binder, and the water-based polymer binder may include one or more selected from the group consisting of a water-based polymer, an anionic water-soluble polymer, a cationic water-soluble polymer, and a water-dispersible polymer.
[0016] The binder may be contained in an amount of 0.5% by weight to 20% by weight based on the total amount of the aerogel layer.
[0017] The binder may include a water-based polymer and a water-dispersible polymer, and the water-based polymer and the water-dispersible polymer may be included in a weight ratio of 1:1 to 1:5.
[0018] The dispersant may include one or more selected from the group consisting of surfactants and phosphate-based salts.
[0019] The dispersant may be contained in an amount of 0.1% by weight to 6% by weight based on the total amount of the aerogel layer.
[0020] The binder and the dispersant may be included in a weight ratio of 1:0.001 to 1:0.67.
[0021] The aerogel layer may contain 5% by weight to 70% by weight of the fibrous support, 10% by weight to 90% by weight of the aerogel, and 0.5% by weight to 20% by weight of the functional material, based on the total amount of the aerogel layer.
[0022] The aerogel layer may contain, relative to the total amount of the aerogel layer, 25% by weight to 60% by weight of the fibrous support, 30% by weight to 70% by weight of the aerogel, and 2% by weight to 15% by weight of the binder.
[0023] The aerogel layer may contain, relative to the total amount of the aerogel layer, 25% by weight to 60% by weight of the fibrous support, 30% by weight to 70% by weight of the aerogel, 2% by weight to 15% by weight of the binder, and 0.1% by weight to 5% by weight of the dispersant.
[0024] Another embodiment provides a method for manufacturing an insulation sheet for a battery, the method comprising: coating an aerogel composition on a substrate; and drying the aerogel composition coated on the substrate to form an aerogel layer, the aerogel layer including a fibrous support; an aerogel; and a functional material including a binder, a dispersant, or a combination thereof, and satisfying the following formula 1: [Formula 1] 50≦A≦100000, A=T i / D s In the above formula 1, the above T i is the thickness of the aerogel layer, and D s is the average diameter of the fibrous support.
[0025] The method for producing the aerogel composition may include the steps of: mixing a functional material, including a binder, a dispersant, or a combination thereof, with a solvent to produce a solvent mixture; mixing the solvent mixture with an aerogel to produce an aerogel mixture; and mixing the aerogel mixture with a fibrous support to produce an aerogel composition.
[0026] The solvent may include one or more selected from the group consisting of polar solvents and non-polar solvents. Effect of the Invention
[0027] The battery insulation sheet according to one embodiment includes an aerogel layer in which the surface of a fibrous support is coated with aerogel, and has excellent heat insulation properties and compression characteristics, low manufacturing costs, and can prevent the generation of aerogel dust during the manufacturing process or actual use. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a schematic diagram showing a battery insulation sheet formed between a plurality of cells according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram illustrating a structure of a battery insulation sheet according to an embodiment. [Diagram 3]FIG. 3 is a schematic diagram illustrating a structure of a battery insulation sheet according to an embodiment. [Figure 4] FIG. 4 is an SEM image of a cross section of the battery insulation sheet of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Although the present invention is described in detail below so that those skilled in the art can easily implement the present invention, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0030] Insulation is a material used to prevent the flow of heat from high to low places, and is used not only in the construction of refrigerators, freezer warehouses, and buildings, but also in various industrial fields including the aircraft, electronic parts, and automotive industries.
[0031] Such a thermal insulation material must have excellent thermal insulation performance through low thermal conductivity, and also must have sufficient mechanical strength to sustain such thermal insulation performance.
[0032] Aerogel is a transparent or translucent advanced material with a nanoporous structure, and has very low density and low thermal conductivity. As a result, it not only has great potential as an insulating material, but is also considered to be a highly efficient super-insulating material that can be used in a variety of industrial fields.
[0033] The biggest advantage of aerogel is that it has lower thermal conductivity than conventional organic insulation materials such as styrofoam, and it solves the fatal weaknesses of organic insulation materials, namely, vulnerability to fire and the generation of harmful gases during a fire.
[0034] However, in general, aerogel has very low strength, i.e., it is easily broken even by a small impact due to its high brittleness, and it is difficult to process it into a very thin thickness and shape. Therefore, despite its excellent thermal insulation properties, it is very difficult to manufacture a thermal insulation material by using aerogel alone.
[0035] According to an embodiment, the battery insulation sheet includes a substrate and an aerogel layer formed on the substrate. The aerogel layer includes a fibrous support, an aerogel, and a functional material including a binder, a dispersant, or a combination thereof, and may satisfy the following formula 1: [Formula 1] 50≦A≦100000, A=T i / D s In the above formula 1, the above T i is the thickness of the aerogel layer, and D s is the average diameter of the fibrous support.
[0036] The battery insulation sheet formed with the above structure has excellent insulation properties and compression characteristics, has low manufacturing process costs, and can prevent dust generation from aerogel during manufacturing and actual use. In addition, the surface of the fibrous support in the aerogel layer is coated with aerogel, the aerogel and the fibrous support are uniformly distributed, and the binding force between the aerogel and the fibrous support is strong, so that dust generation due to detachment of aerogel can be reduced.
[0037] FIG. 1 is a schematic diagram showing a battery insulation sheet formed between a plurality of cells according to an embodiment. 1, the battery insulation sheet 100 according to an embodiment may be formed between each of the cells 200 in a battery module including the cells 200. Here, the upper and lower surfaces of the battery insulation sheet may be disposed to face each of the adjacent cells. By forming the battery insulation sheet 100 according to an embodiment between each of the cells 200, it is possible to provide a battery module and a battery pack including the same that are further improved in safety by blocking a flame inside the cell in advance and maximally suppressing the flame from spreading to other cells.
[0038] FIG. 2 is a schematic diagram illustrating a structure of a battery insulation sheet according to an embodiment. Referring to FIG. 2, the battery insulation sheet 100 includes a substrate 110; and an aerogel layer 120 formed on the substrate 110; where the upper and lower surfaces of the battery insulation sheet may be arranged to face adjacent cells, respectively. By forming an aerogel layer using the aerogel composition according to an embodiment on the substrate, the battery insulation sheet has improved heat insulation properties as well as compression characteristics, and the aerogel can be prevented from detaching and generating dust when the battery insulation sheet is manufactured or installed inside an apparatus.
[0039] FIG. 3 is a schematic diagram showing the structure of a battery insulation sheet according to another embodiment. 3, in one embodiment, the battery insulation sheet 100 may have a structure including a first substrate 130, an aerogel layer 120 formed on the first substrate 130, and a second substrate 140 formed on the aerogel layer 120. Here, the first substrate and the second substrate may be disposed to face the adjacent cells, respectively. The first substrate and the second substrate may be formed of the same or different materials.
[0040] In the above formula 1, the value of A may be, for example, 50 to 100,000, 100 to 30,000, or 200 to 10,000. By satisfying the value of A within the above range, the ratio of the thickness of the aerogel layer to the average diameter of the fibrous support can be controlled, and the structure of the aerogel layer can be formed firmly, in which case it is easy to withstand high pressure during heat transmission between multiple cells. In addition, by controlling the ratio of the thickness of the aerogel layer to the average diameter of the fibrous support, the coating property of the aerogel layer is improved, and it is easy to install a heat insulating sheet between multiple cells.
[0041] The substrate may be of any type, such as a resin, a metal, an inorganic material other than a metal, or a composite of these. The substrate may be in any form, such as a film, a thin film, or a sheet.
[0042] The resin may include, for example, one or more selected from the group consisting of polyethylene, polypropylene, polystyrene, polyethylene terephthalate, and polyamide.
[0043] The metal may include, for example, one or more selected from the group consisting of copper, nickel, cobalt, iron, chromium, vanadium, palladium, ruthenium, rhodium, molybdenum, tungsten, iridium, silver, gold, and platinum. When using a substrate made of a metal material, the substrate may be subjected to anti-corrosion treatment, insulation treatment, etc., as necessary.
[0044] The inorganic material may include one or more selected from the group consisting of calcium carbonate (CaCO3), talc, and mica.
[0045] As a specific example, the substrate may include an inorganic material, and as a further specific example, the substrate may include mica, which can improve the heat insulating property and durability of the heat insulating sheet.
[0046] The thickness of the substrate may be 0.01 mm to 5 mm, 0.05 mm to 3 mm, or 0.1 mm to 1 mm. By forming an aerogel layer on a substrate having a thickness within the above range, a heat insulating sheet can be formed.
[0047] In the battery insulation sheet, the aerogel layer may include a fibrous support; an aerogel; and a functional material including a binder, a dispersant, or a combination thereof.
[0048] The thickness of the aerogel layer may be 1 mm to 10 mm, 1 mm to 5 mm, or 1 mm to 3 mm. By forming an aerogel layer on a substrate having a thickness within the above range, a heat insulating sheet having excellent heat insulating and compression properties can be produced.
[0049] In one embodiment, the fibrous support may be included in the aerogel layer to improve durability of the battery insulation sheet.
[0050] The fibrous support may include fibers used in supports of ordinary heat insulating materials. For example, the fibrous support may include one or more selected from the group consisting of natural fibers, silica fibers, glass fibers, carbon fibers, graphite fibers, mineral fibers, and polymer fibers. As a specific example, the fibrous support may include glass fibers, but is not limited thereto.
[0051] The natural fibers may include, for example, one or more selected from the group consisting of hemp, jute, flax, coir, kenaf, and cellulose.
[0052] The mineral fibers may be, for example, mineral fibers comprising one or more selected from the group consisting of basalt, wollastonite, alumina, silica, slag, and rock.
[0053] The polymer fiber may include at least one selected from the group consisting of nylon, polyimide, polyamide, polybenzimidazole, polybenzoxazole, polyamideimide, polyethyleneterephthalate, polybutyleneterephthalate, polyester, polyethylene (PE), and polypropylene (PP). As a specific example, the polymer fiber may include at least one of polyimide, polyamide, and polybenzimidazole, but is not limited thereto.
[0054] The fibrous support may be, for example, in the form of wool or chopped strands, but is not limited thereto.
[0055] The average diameter of the fibrous support may be, for example, 0.1 μm to 20 μm, 0.1 μm to 15 μm, 0.1 μm to 5 μm, 1 μm to 15 μm, or 3 μm to 10 μm. By including a fibrous support having an average diameter within the above range, the structure of the aerogel layer can be made robust and production costs can be reduced.
[0056] The average length of the fibrous support may be, for example, 50 μm to 1000 μm, 70 μm to 800 μm, or 100 μm to 600 μm. By including a fibrous support having an average length within the above range, the aerogel layer can be formed firmly and durability can be improved.
[0057] The content of the fibrous support may be 5% by weight to 70% by weight, 25% by weight to 60% by weight, or 30% by weight to 50% by weight based on the total amount of the aerogel layer. A battery insulation sheet including an aerogel layer containing a fibrous support within the above range can improve durability.
[0058] In one embodiment, the aerogel has a BET specific surface area of 500 m 2 / g~1,000m 2 For example, the aerogel may have a BET specific surface area of 500 m 2 / g~950m 2 / g, 550m 2 / g~950m 2 / g or 600m 2 / g~900m 2 By including an aerogel having a BET specific surface area value within the above range, it is possible to provide a heat insulating sheet capable of effectively preventing heat transfer and heat propagation between a plurality of cells.
[0059] The average particle size (D50) of the aerogel may be 5 μm to 200 μm, 10 μm to 100 μm, or 20 μm to 50 μm. By including aerogel having an average particle size within the above range, the heat insulating properties can be improved and the heat transfer between multiple cells can be delayed.
[0060] In the present disclosure, when a particle is spherical, "particle size" refers to the particle size or average particle size, and when a particle is non-spherical, "particle size" refers to the major axis length or average major axis length. The particle size (or size) of a particle can be measured using a scanning electron microscope or a particle size analyzer. For example, a laser particle size distribution measuring device LA-950 manufactured by Horiba, Ltd. can be used as a particle size distribution measuring device. When particle size is measured using a particle size distribution measuring device, the average particle size (or particle size) is called D50. D50 refers to the average particle size (or particle size) of particles whose cumulative volume corresponds to 50 vol% in a particle size distribution (e.g., cumulative distribution), and refers to the particle size value corresponding to 50% from the smallest particle when the total number of particles is 100% in a distribution curve accumulated in order from small to large particle sizes.
[0061] The content of the aerogel may be 10% by weight to 90% by weight, 30% by weight to 70% by weight, or 40% by weight to 60% by weight based on the total amount of the aerogel layer. When a battery insulation sheet is manufactured using an aerogel composition containing aerogel within the above range, the heat insulating property of the battery insulation sheet can be improved.
[0062] In an embodiment, the binder may include a water-based polymer binder, for example, the water-based polymer binder may include at least one selected from the group consisting of a water-based polymer, an anionic water-soluble polymer, a cationic water-soluble polymer, and a water-dispersible polymer.
[0063] The aqueous polymer may include, but is not limited to, one or more selected from the group consisting of polyvinyl alcohol, polyethylene oxide, polyacrylamide, and polyvinylpyrrolidone.
[0064] The anionic water-soluble polymer may include at least one selected from the group consisting of polymers having functional groups of carboxylic acid, sulfonic acid, sulfate, phosphate, and salts thereof. For example, the anionic water-soluble polymer may be a polymer having a carboxylic acid group, and a specific example thereof may include, but is not limited to, polymaleic acid.
[0065] The cationic water-soluble polymer may include at least one selected from the group consisting of polymers having functional groups such as amine, ammonium, phosphonium, sulfonium, and salts thereof. For example, the cationic water-soluble polymer may be a polymer having an amine group, and specific examples thereof include at least one selected from the group consisting of polyethylene amine and polyamine, but are not limited thereto.
[0066] The water-dispersible polymer may include, but is not limited to, one or more selected from the group consisting of water-dispersible polyurethane and water-dispersible polyester.
[0067] The binder may include a water-based polymer and a water-dispersible polymer, for example, a water-based polymer having binder properties as well as dispersing properties and a water-dispersible polyurethane having fire-resistant properties, or a specific example thereof may include polyvinyl alcohol and a water-dispersible polyurethane.
[0068] The weight ratio of the aqueous polymer and the water-dispersible polymer may be 1:1 to 1:5, 1:1 to 1:4, or 1:2 to 1:3. When the aqueous polymer and the water-dispersible polymer are mixed and used in a weight ratio within the above range, the heat insulation property, dust resistance, and compressibility of the heat insulating sheet can be further improved as well as the fire resistance and mechanical properties.
[0069] The content of the binder may be 0.5% by weight to 20% by weight, 2% by weight to 15% by weight, or 8% by weight to 15% by weight based on the total amount of the aerogel layer. When the aerogel composition containing the binder within the above range is used to manufacture the battery insulation sheet, the dust characteristics of the battery insulation sheet can be improved.
[0070] In one embodiment, the dispersant may include at least one selected from the group consisting of surfactants and phosphate-based salts. As a specific example, the dispersant may include at least one of a nonionic surfactant, an anionic surfactant, an amphoteric surfactant, a natural surfactant such as lecithin, and a phosphate, but is not limited thereto.
[0071] When the dispersant is further included, the dispersion of the aerogel in the composition can be further improved, and the fibrous support and the aerogel can be uniformly dispersed.
[0072] The content of the dispersant may be 0.1% by weight to 6% by weight, 0.1% by weight to 5% by weight, or 0.1% by weight to 3% by weight, based on the total amount of the aerogel layer. When the dispersant is contained within the above range, a battery insulation sheet having excellent heat insulation properties, compression properties, and dust properties can be produced.
[0073] In an embodiment, the binder and the dispersant may be included in a weight ratio of 1:0.001 to 1:0.67, 1:0.001 to 1:0.5, or 1:0.001 to 1:0.3. When the binder and the dispersant are mixed in a weight ratio within this range, the aerogel may be more uniformly dispersed in the aerogel layer.
[0074] In one embodiment, the aerogel layer may contain 5 wt % to 70 wt % of the fibrous support, 10 wt % to 90 wt % of the aerogel, and 0.5 wt % to 20 wt % of the functional material, based on the total weight of the aerogel layer.
[0075] As an example, the aerogel layer may contain 25% by weight to 60% by weight of the fibrous support, 30% by weight to 70% by weight of the aerogel, and 2% by weight to 15% by weight of the binder, based on the total amount of the aerogel layer.
[0076] Specifically, the aerogel layer may contain 30% to 50% by weight of the fibrous support, 40% to 60% by weight of the aerogel, and 8% to 15% by weight of the binder, based on the total amount of the aerogel layer. When the aerogel layer is formed within the above ranges, excellent heat insulation can be realized, durability can be improved, and the bonding force between the fibrous support and the aerogel can be improved to prevent dust generation.
[0077] As another example, the aerogel layer may contain, relative to the total amount of the aerogel layer, 25% by weight to 60% by weight of the fibrous support, 30% by weight to 70% by weight of the aerogel, 2% by weight to 15% by weight of the binder, and 0.1% by weight to 5% by weight of the dispersant.
[0078] Specifically, the aerogel layer may contain 30% to 50% by weight of the fibrous support, 40% to 60% by weight of the aerogel, 5% to 10% by weight of the binder, and 0.1% to 3% by weight of the dispersant, based on the total amount of the aerogel layer. When the aerogel layer is formed within the above ranges, the dispersibility of the aerogel can be improved, excellent heat insulation can be realized, and durability can be improved at the same time, and the cohesive force between the fibrous support and the aerogel can be improved to prevent dust generation.
[0079] In an embodiment, the aerogel layer may be formed in a single layer structure or a multi-layer structure. When the aerogel layer is formed in a multi-layer structure, the aerogel layer may be formed in 2 to 10 layers, 2 to 7 layers, or 2 to 5 layers.
[0080] A method for manufacturing a battery insulation sheet according to an embodiment includes: coating an aerogel composition on a substrate; and drying the aerogel composition coated on the substrate to form an aerogel layer, the aerogel layer including a fibrous support; an aerogel; and a functional material including a binder, a dispersant, or a combination thereof; and may satisfy the following formula 1. Here, the specific description related to the substrate and the aerogel layer is as described above. Also, the substrate may be any one of the substrate of FIG. 2 or the first substrate and the second substrate of FIG. 3.
[0081] [Formula 1] 50≦A≦100000, A=T i / D s
[0082] In the above formula 1, the above T i is the thickness of the aerogel layer, and D s is the average diameter of the fibrous support.
[0083] The method for producing the aerogel composition may include the steps of: mixing a functional material, including a binder, a dispersant, or a combination thereof, with a solvent to produce a solvent mixture; mixing the solvent mixture with an aerogel to produce an aerogel mixture; and mixing the aerogel mixture with a fibrous support to produce an aerogel composition.
[0084] In the step of preparing the solvent mixture by mixing the functional material with the solvent, a binder may be mixed with the solvent, or a binder and a dispersant may be mixed with the solvent, as described above.
[0085] In one embodiment, the solvent may include at least one selected from the group consisting of polar solvents and non-polar solvents.
[0086] The polar solvent may include one or more selected from the group consisting of water and alcohol-based solvents.
[0087] The water may include, for example, purified water, deionized water, or a combination thereof.
[0088] The alcohol-based solvent may include, for example, one or more selected from the group consisting of methanol, ethanol, propanol, pentanol, butanol, hexanol, ethylene glycol, propylene glycol, diethylene glycol, and glycerol, but is not limited thereto.
[0089] The non-polar solvent may include a hydrocarbon-based solvent, for example, one or more selected from the group consisting of hexane, pentane, heptane, toluene, and benzene, and more preferably, an alkane solvent such as hexane or a mixture containing an alkane solvent, but is not limited thereto.
[0090] The solvent may include water. When water is used as the solvent, raw material costs and post-treatment costs can be effectively reduced. However, when water is used as the solvent, there is a problem that it is not easy to mix with hydrophobic aerogel. In one embodiment, the aerogel is uniformly dispersed by controlling the design of the mixing step, the mixing conditions, the addition and the amount of the binder and the dispersant, etc. When the aerogel is uniformly dispersed in the composition in this way, a battery insulation sheet having excellent insulation properties, compression properties, and low dust properties can be formed with a thin thickness without using a large amount of binder.
[0091] The solvent may be contained in such a way that the weight ratio of the solvent to the total amount of solids in the aerogel composition is 1:1 to 1:90. For example, the weight ratio of the solvent to the total amount of solids may be 1:50 to 1:70, 1:20 to 1:30, or 1:2 to 1:10. By controlling the weight ratio of the solvent to the total amount of solids within the above range, the viscosity can be controlled and the aerogel layer can be coated.
[0092] In the step of preparing the aerogel mixture by mixing the solvent mixture with the aerogel, the aerogel may be added in a powder form, and the detailed description of the aerogel is as described above.
[0093] In the step of preparing an aerogel composition by mixing the aerogel mixture with the fibrous support, the specific description of the fibrous support is as described above.
[0094] In an embodiment, the aerogel composition may further include a silane-based compound. The silane-based compound may include at least one selected from the group consisting of 3-(trimethoxysilyl)propylmethacrylate, methyltriethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, octadecyltrimethoxysilane, ethyltriethoxysilane, and 3-glycidoxypropyltrimethoxysilane. When the silane-based compound is further included, the dispersibility can be further improved.
[0095] In each of the steps of mixing the solvent with a functional material including a binder, a dispersant, or a combination thereof to prepare a solvent mixture, mixing the solvent mixture with an aerogel to prepare an aerogel mixture, and mixing the aerogel mixture with a fibrous support to prepare an aerogel composition, a mixer may be used during mixing. For example, the mixer may include, but is not limited to, a planetary mixer and a thinky mixer.
[0096] As a specific example, a planetary mixer can be used to mix the solvent mixture with the aerogel. When the solvent mixture and the aerogel are mixed using the planetary mixer, the aerogel can be uniformly dispersed in the solvent.
[0097] The planetary mixer may be a piece of equipment that can be used to mix or stir other materials to produce a homogenous mixture. It may include blades capable of planetary motion.
[0098] In one embodiment, the planetary mixer may include one or more planetary blades and one or more high-speed dispersion blades. As a specific example, the planetary mixer may include one or more planetary blades and one or more high-speed dispersion blades.
[0099] The planetary blades and high speed dispersion blades rotate continuously about their axes, and the rotational speed can be expressed in units of rotations per minute (rpm).
[0100] In one embodiment, the planetary mixer may include a first blade and a second blade having different rotation axes. For example, the first blade may be a low-speed blade, and the second blade may be a high-speed blade. Here, low speed and high speed refer to the relative rotation speed between the first blade and the second blade. As a specific example, the first blade may be an open blade, and the second blade may be a Despa blade.
[0101] The rotation speed of the first blade may be, for example, 10 rpm to 100 rpm, 10 rpm to 60 rpm, or 30 rpm to 70 rpm, and the rotation speed of the second blade may be, for example, 100 rpm to 2000 rpm, 100 rpm to 1000 rpm, 300 rpm to 1700 rpm, or 500 rpm to 1700 rpm.
[0102] When the functional material is mixed in the solvent, the rotation speed of the first blade of the mixer may be 10 rpm to 60 rpm, 20 rpm to 50 rpm, or 30 rpm to 40 rpm, and the rotation speed of the second blade may be 300 rpm to 1700 rpm, 600 rpm to 1000 rpm, or 700 rpm to 800 rpm. When the solvent and the functional material are mixed as described above, a solvent mixture in which the binder, dispersant, or a combination thereof is uniformly dispersed is prepared, and aerogel mixing can be more easily performed in the subsequent step.
[0103] When the solvent mixture and the aerogel are mixed, the rotation speed of the first blade of the mixer may be 30 rpm to 70 rpm, 40 rpm to 70 rpm, or 60 rpm to 70 rpm, and the rotation speed of the second blade may be 500 rpm to 1700 rpm, 600 rpm to 1600 rpm, or 800 rpm to 1500 rpm. When the aerogel is mixed into the solvent mixture as described above, it is possible to prevent the aerogel from agglomerating with each other and induce uniform dispersion.
[0104] When the aerogel mixture and the fibrous support are mixed, the rotation speed of the first blade of the mixer may be 10 rpm to 60 rpm, 20 rpm to 50 rpm, or 30 rpm to 40 rpm, and the rotation speed of the second blade may be 300 rpm to 1700 rpm, 400 rpm to 1500 rpm, or 800 rpm to 1200 rpm. When the aerogel mixture and the fibrous support are mixed as described above, air bubbles in the composition are removed, the viscosity is adjusted, and the fibrous support is easily dispersed among the uniformly dispersed aerogel, and the aerogel may be present in a form in which the periphery of the fibrous support is wrapped in the composition. Here, a binder is present between the aerogel and the fibrous support, which can improve the binding force between the aerogel and the fibrous support.
[0105] The coating step may be performed by applying an aerogel slurry onto a conventional substrate.
[0106] The coating step may be carried out once or repeated two or more times.
[0107] The drying step may be performed at a temperature of, for example, 25° C. to 100° C., 45° C. to 90° C., or 60° C. to 85° C. By drying at the above temperature conditions, a robust aerogel layer may be formed on the substrate without a separate adhesive member or bonding agent while preventing detachment between the substrate and the aerogel layer, and a coating layer may be formed in a shape in which the aerogel is coated around a plurality of dispersed fibrous supports.
[0108] In an embodiment, the method for manufacturing the battery insulation sheet may further include laminating a substrate on the coated aerogel composition before drying. In this case, a battery insulation sheet may be manufactured in a structure in which a plurality of substrates, for example, a first substrate and a second substrate, are formed on both sides of the aerogel layer without an adhesive layer.
[0109] According to a manufacturing method of a battery insulation sheet according to an embodiment, a battery insulation sheet can be manufactured by a simple method of coating on a substrate and drying, without using a separate adhesive or forming an adhesive layer. The aerogel is uniformly dispersed and has excellent compression properties, so that the battery insulation sheet can realize excellent insulation properties and low dust properties even with a thin thickness.
[0110] In an embodiment, the aerogel layer may further include additives such as wetting agents, emulsifiers, compatibilizers, viscosity adjusters, pH adjusters, stabilizers, antioxidants, acidic or basic scavengers, metal deactivators, defoamers, antistatic agents, thickeners, adhesion improvers, binders, flame retardants, impact modifiers, pigments, dyes, colorants, and deodorizers.
[0111] Specific examples of the present invention will be presented below. However, the examples described below are merely for the purpose of specifically illustrating and explaining the present invention, and the present invention is not limited thereto. Furthermore, since the contents not described here can be sufficiently inferred by those skilled in the art, the description thereof will be omitted.
[0112] (Manufacture of battery insulation sheets) Example 1 1. Preparation of Aerogel Composition Polyvinyl alcohol (Sigma Aldrich, Poly(vinyl alcohol)) was added as a binder to ultrapure water as a solvent, and mixed under conditions of an open blade of 30 rpm and a despa blade of 700 rpm to produce a solvent mixture. After that, the solvent mixture was mixed to obtain a BET value of 800m 2 / g of aerogel was added and mixed under the conditions of open blade 70 rpm and Despa blade 1500 rpm to produce an aerogel mixture. Glass wool with an average diameter of 0.12 μm to 5 μm was added as a fibrous support to the aerogel mixture and mixed under the conditions of open blade 30 rpm and Despa blade 1200 rpm to produce an aerogel composition. Here, a planetary mixer (DNTEK, PT-005) was used for mixing.
[0113] The solid content of the prepared aerogel composition was confirmed to be 50 wt % aerogel, 40 wt % glass wool, and 10 wt % polyvinyl alcohol.
[0114] 2. Manufacturing of battery insulation sheets The aerogel composition prepared above was applied as a slurry onto a 0.1 mm thick mica sheet (Famica, Muscovite), and then a 0.1 mm thick mica sheet was laminated in a sandwich type and coated by a roll rolling method. Then, it was dried at 60° C. for 24 hours to form an aerogel layer, and a battery insulation sheet was prepared. Here, it was confirmed that the thickness of the aerogel layer was 1.18 mm, and the total thickness of the prepared battery insulation sheet was 1.38 mm.
[0115] Example 2 The aerogel composition was prepared in the same manner as in Example 1, except that the amounts of raw materials added were adjusted to prepare an aerogel composition having a solid content of 60 wt % aerogel, 25 wt % glass wool, and 15 wt % polyvinyl alcohol.
[0116] Example 3 The aerogel composition was prepared in the same manner as in Example 1, except that the amounts of raw materials added were adjusted to prepare an aerogel composition having a solid content of 65 wt % aerogel, 25 wt % glass wool, and 10 wt % polyvinyl alcohol.
[0117] Example 4 The aerogel composition was prepared in the same manner as in Example 1, except that the amounts of raw materials added were adjusted to prepare an aerogel composition having a solid content of 45 wt % aerogel, 50 wt % glass wool, and 5 wt % polyvinyl alcohol.
[0118] Example 5 An aerogel composition was prepared in the same manner as in Example 1, except that the amounts of raw materials added were adjusted to prepare an aerogel composition having a solid content of 50 wt % aerogel, 49.7 wt % glass wool, and 0.3 wt % polyvinyl alcohol.
[0119] Example 6 The aerogel composition was prepared in the same manner as in Example 1, except that the amounts of raw materials added were adjusted to prepare an aerogel composition having a solid content of 40 wt % aerogel, 35 wt % glass wool, and 25 wt % polyvinyl alcohol.
[0120] Example 7 The aerogel composition was prepared using glass wool having an average diameter of 0.1 μm to 3 μm as a fibrous support, and the thickness of the aerogel layer was adjusted to 1.3 mm when preparing the battery insulation sheet, except that the battery insulation sheet was prepared in the same manner as in Example 1.
[0121] Example 8 The aerogel composition was prepared by using glass wool having an average diameter of 10 μm to 15 μm as a fibrous support, and the thickness of the aerogel layer was adjusted to 1.3 mm when preparing the battery insulation sheet, except that the battery insulation sheet was prepared in the same manner as in Example 1.
[0122] Example 9 The aerogel composition was prepared in the same manner as in Example 1, except that water-dispersible polyurethane was used instead of polyvinyl alcohol as a binder.
[0123] Example 10 1. Preparation of Aerogel Composition Polyvinyl alcohol (Sigma Aldrich, Poly(vinyl alcohol)) as a binder and a surfactant (Triton-X100, Sigma Aldrich) as a dispersant were added to the ultrapure water solvent, and mixed under conditions of an open blade of 30 rpm and a despa blade of 700 rpm to produce a solvent mixture. After that, the solvent mixture was measured to have a BET value of 800m 2 / g of aerogel was added and mixed under the conditions of open blade 70 rpm and Despa blade 1500 rpm to produce an aerogel mixture. Glass wool with an average diameter of 0.12 μm to 5 μm was added as a fibrous support to the aerogel mixture and mixed under the conditions of open blade 30 rpm and Despa blade 1200 rpm to produce an aerogel composition. Here, a planetary mixer (DNTEK, PT-005) was used for mixing.
[0124] The solid contents of the prepared aerogel composition were confirmed to be 50 wt % aerogel, 40 wt % glass wool, 9.9 wt % polyvinyl alcohol, and 0.1 wt % dispersant.
[0125] 2. Manufacturing of battery insulation sheets The aerogel composition prepared above was applied as a slurry onto a 0.1 mm thick mica sheet (Famica, Muscovite), and then a 0.1 mm thick mica sheet was laminated in a sandwich type and coated by a roll rolling method. Then, it was dried at 60° C. for 24 hours to form an aerogel layer, and a battery insulation sheet was prepared. Here, it was confirmed that the thickness of the aerogel layer was 1.18 mm, and the total thickness of the prepared battery insulation sheet was 1.38 mm.
[0126] Example 11 1. Preparation of Aerogel Composition Polyvinyl alcohol (Sigma Aldrich, Poly(vinyl alcohol)) as a binder, water-dispersible polyurethane, and a surfactant (Triton-X100, Sigma Aldrich) as a dispersant were added to the ultrapure water solvent, and mixed under conditions of an open blade of 30 rpm and a despa blade of 700 rpm to produce a solvent mixture. After that, the solvent mixture was mixed to obtain a BET value of 800m 2 / g of aerogel was added and mixed under conditions of open blade 70 rpm and Despa blade 1500 rpm to produce an aerogel mixture. Glass wool with an average diameter of 0.12 μm to 5 μm was added as a fibrous support to the aerogel mixture and mixed under conditions of open blade 30 rpm and Despa blade 1200 rpm to produce an aerogel composition. Here, a planetary mixer (DNTEK, PT-005) was used for mixing.
[0127] The solid contents of the prepared aerogel composition were confirmed to be 50 wt % aerogel, 40 wt % glass wool, 3 wt % polyvinyl alcohol, 6.9 wt % water-dispersible polyurethane, and 0.1 wt % dispersant.
[0128] 2. Manufacturing of battery insulation sheets The aerogel composition prepared above was applied as a slurry onto a 0.1 mm thick mica sheet (Famica, Muscovite), and then a 0.1 mm thick mica sheet was laminated in a sandwich type and coated by a roll rolling method. Then, it was dried at 60° C. for 24 hours to form an aerogel layer, and a battery insulation sheet was prepared. Here, it was confirmed that the thickness of the aerogel layer was 1.18 mm, and the total thickness of the prepared battery insulation sheet was 1.38 mm.
[0129] Comparative Example 1 The aerogel composition was prepared by using glass wool having an average diameter of 30 μm to 40 μm as the fibrous support in Example 1, and the thickness of the aerogel layer was adjusted to 1.18 mm when preparing the battery insulation sheet, except that the battery insulation sheet was prepared in the same manner as in Example 1.
[0130] Comparative Example 2 The aerogel composition was prepared by using glass wool having an average diameter of 0.01 μm to 0.015 μm as the fibrous support, and the thickness of the aerogel layer was adjusted to 1.18 mm when preparing the battery insulation sheet, except that the battery insulation sheet was prepared in the same manner as in Example 1.
[0131] (Experimental Example) Experimental example 1: SEM analysis The cross section of the aerogel layer of the battery insulation sheet manufactured in Example 1 was observed using Hitachi's S-4800 SEM, and an analysis was performed after Pt coating. The results are shown in Figure 4 below. Specifically, Figure 4 shows SEM images of the battery insulation sheet according to Example 1 at 300 magnifications (X300) and 800 magnifications (X800).
[0132] 4, it can be seen that the battery insulation sheet of Example 1 manufactured by the method of the present invention has a unique structure. Specifically, when an aerogel layer is formed by impregnating a fiber blanket with an aerogel precursor at low temperature under reduced pressure, gelling the aerogel precursor, and then drying the aerogel under supercritical drying, there is a limit to the amount of aerogel that can be added, making it difficult to add a fixed amount, and the aerogel is applied to the surface of the blanket in large particle sizes, which makes it easy to fall off and generates a large amount of dust. However, it can be seen from FIG. 4 that the aerogel coats a fibrous support, and therefore the battery insulation sheet of the present invention can exhibit excellent insulation, compression properties, and low dust properties.
[0133] Experimental example 2: Evaluation of thermal insulation The heat insulating properties were evaluated using the heat insulating sheets produced in Examples 1 to 11 and Comparative Examples 1 and 2.
[0134] Specifically, each heat insulating sheet was inserted between a pair of opposing 1 mm thick aluminum plates and placed on a heat press, and the upper plate of the heat press was heated to 350° C., while the lower plate of the heat press was not heated and was maintained at an initial temperature of 40° C. Then, a pressure of 20 kN was applied to the lower plate of the heat press, and the temperature of the lower plate of the heat press after 11 minutes was measured and shown in Table 1 below.
[0135] Experimental example 3: Dustiness evaluation The heat insulating sheets produced in Examples 1 to 11 and Comparative Examples 1 and 2 were used to evaluate dustiness.
[0136] Specifically, the weight of each heat insulation sheet was measured before the evaluation. After that, the heat insulation sheet was placed on a rubber plate and hit with a rubber hammer at a total of five places, including the top and center of the heat insulation sheet, to remove dust and then measure the weight of the heat insulation sheet. Next, the weight before and after the physical impact was compared to calculate the weight loss rate, and the results are shown in Table 1 below.
[0137] Experimental Example 4: Evaluation of compression characteristics The heat insulating sheets manufactured in Examples 1 to 11 and Comparative Examples 1 and 2 were used to evaluate compression characteristics.
[0138] Specifically, the zero point was taken using UTM equipment, and each insulation sheet was sandwiched between 1mm thick aluminum plates, and the compression rate was measured from 0kN to 80kN at a compression speed of 0.02mm / sec. The thickness was then measured at 5kN and 40kN, and the reduction rate of thickness was expressed as the compression rate. The results are shown in Table 1 below.
[0139] [Table 1]
[0140] Referring to Table 1, it was confirmed that in the cases of Examples 1 to 11, the heat insulation, dust resistance, and compression characteristics were all excellent. Here, looking at Examples 1 to 4, it was confirmed that the heat insulation, dust resistance, and compression characteristics changed according to the component content of the aerogel composition. In addition, in the case of Example 5, it was confirmed that the dust resistance and compression characteristics were somewhat decreased according to the change in the components of the aerogel composition, but the heat insulation was improved, and in the case of Example 6, it was confirmed that the heat insulation and compression characteristics were somewhat decreased. In addition, looking at Examples 1, 7, and 8, it was confirmed that the heat insulation, dust resistance, and compression characteristics changed according to the A value, and it was confirmed that when the A value was 200 to 10,000, the heat insulation and dust resistance were excellent without a decrease in compression characteristics. In addition, in the case of Example 9, since it was not possible to act as a dispersant as a fire-resistant binder, the dust resistance was somewhat decreased, but it was confirmed that the heat insulation was improved. In addition, looking at Example 10, it was confirmed that the heat insulation, dust resistance, and compression characteristics were improved in the case of using a mixture of a binder and a dispersant. In addition, in Example 11, it was confirmed that when polyvinyl alcohol, which can act as a dispersant, was mixed with a water-dispersible polyurethane binder, which cannot act as a dispersant, the insulation properties, dust resistance, and compression properties were further improved.
[0141] In addition, looking at Comparative Examples 1 and 2, it was confirmed that since the A value was not satisfied, the heat insulation property, dust resistance, and compression property were all significantly reduced.
[0142] Therefore, it was confirmed that the aerogel composition according to an embodiment has excellent heat insulation properties, compression properties, and low dust properties.
[0143] Although a preferred embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible within the scope of the claims, the detailed description of the invention, and the accompanying drawings, which of course also fall within the scope of the present invention. [Explanation of symbols]
[0144] 100 Battery insulation sheet 110 Base material 120 Aerogel layer 130 1st base material 140 Second base material 200 cells
Claims
1. A substrate; and an aerogel layer formed on the substrate; the aerogel layer comprises a fibrous support; an aerogel; and a functional material comprising a binder, a dispersant, or a combination thereof; A battery insulation sheet that satisfies the following formula 1: [Formula 1] 50≦A≦100000, A=T i / D s In the above formula 1, the T i is the thickness of the aerogel layer, and D s is the average diameter of the fibrous support.
2. The battery insulation sheet according to claim 1 , wherein the aerogel layer has a thickness of 1 mm to 10 mm.
3. The battery insulation sheet according to claim 1 , wherein the average diameter of the fibrous support is 0.1 μm to 20 μm.
4. The battery insulating sheet according to claim 1, wherein A is 200 to 10,000.
5. The battery insulating sheet according to claim 1 , wherein a surface of the fibrous support is coated with an aerogel.
6. The battery insulating sheet according to claim 1 , wherein the substrate comprises at least one material selected from the group consisting of a resin, a metal, and an inorganic material other than a metal.
7. 2. The battery insulating sheet according to claim 1, wherein the fibrous support comprises at least one selected from the group consisting of natural fibers, silica fibers, glass fibers, carbon fibers, basalt fibers, and polymeric fibers.
8. The aerogel has a BET specific surface area of 500 m 2 / g to 1,000m 2 The battery insulating sheet according to claim 1, wherein the elastic modulus is 1 / g.
9. The binder comprises a water-based polymer binder, The battery insulating sheet according to claim 1 , wherein the water-based polymer binder comprises at least one selected from the group consisting of a water-based polymer, an anionic water-soluble polymer, a cationic water-soluble polymer, and a water-dispersible polymer.
10. The battery insulation sheet according to claim 1 , wherein the binder is contained in an amount of 0.5% by weight to 20% by weight based on the total amount of the aerogel layer.
11. The binder includes a water-soluble polymer and a water-dispersible polymer, The battery insulating sheet according to claim 1 , wherein the water-based polymer and the water-dispersible polymer are contained in a weight ratio of 1:1 to 1:
5.
12. The battery insulating sheet according to claim 1 , wherein the dispersing agent comprises at least one selected from the group consisting of a surfactant and a phosphate-based salt.
13. The battery insulation sheet according to claim 1 , wherein the dispersant is contained in an amount of 0.1% by weight to 6% by weight based on the total amount of the aerogel layer.
14. The battery insulation sheet according to claim 1 , wherein the binder and the dispersant are contained in a weight ratio of 1:0.001 to 1:0.
67.
15. 2. The battery insulation sheet according to claim 1, wherein the aerogel layer comprises, with respect to a total amount of the aerogel layer, 5% by weight to 70% by weight of the fibrous support, 10% by weight to 90% by weight of the aerogel, and 0.5% by weight to 20% by weight of the functional material.
16. 2. The battery insulation sheet according to claim 1, wherein the aerogel layer comprises, with respect to a total amount of the aerogel layer, 25% by weight to 60% by weight of the fibrous support, 30% by weight to 70% by weight of the aerogel, and 2% by weight to 15% by weight of the binder.
17. 2. The battery insulation sheet according to claim 1, wherein the aerogel layer comprises, relative to the total amount of the aerogel layer, 25% by weight to 60% by weight of the fibrous support, 30% by weight to 70% by weight of the aerogel, 2% by weight to 15% by weight of the binder, and 0.1% by weight to 5% by weight of the dispersant.
18. Coating an aerogel composition onto a substrate; and drying the aerogel composition coated on the substrate to form an aerogel layer. the aerogel layer comprises a fibrous support; an aerogel; and a functional material comprising a binder, a dispersant, or a combination thereof; A method for producing a battery insulation sheet that satisfies the following formula 1: [Formula 1] 50≦A≦100000, A=T i / D s In the above formula 1, the T i is the thickness of the aerogel layer, and D s is the average diameter of the fibrous support.
19. The method for producing the aerogel composition includes: mixing a functional material, including a binder, a dispersant, or a combination thereof, with a solvent to produce a solvent mixture; mixing the solvent mixture with an aerogel to prepare an aerogel mixture; The method for producing a battery insulation sheet according to claim 18, further comprising: mixing the aerogel mixture with a fibrous support to produce an aerogel composition.
20. The method for producing a battery insulation sheet according to claim 19, wherein the solvent includes at least one selected from the group consisting of polar solvents and non-polar solvents.
Citation Information
Patent Citations
Composite thermal insulation material integrally formed with battery shell and preparation process of composite thermal insulation material
CN113998983A
Heat insulating material and method of manufacturing heat insulating material
JP2015163815A
Method for burdock beverage containing with saponin and weight loss method using the beverage
KR1020210056618A
Three-dimensional porous polyurea networks and methods of manufacture
US20200071482A1
Thermal insulation material for battery pack, and battery pack
WO2021181951A1