Polishing pad having adjusted chlorine content, and method for manufacturing semiconductor element using the same

A polishing pad with controlled chlorine content addresses debris-related defects and scratches in the CMP process by using a urethane-based composition, ensuring high performance and safety.

JP2024152644AActive Publication Date: 2024-10-25SK ENPULSE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024055095
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-03-28
Publication Date
2024-10-25
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

During the chemical mechanical planarization (CMP) process, debris generated from the friction between the polishing surface and semiconductor substrates or diamond disks for conditioning causes defects and scratches on the polishing surface.

Method used

A polishing pad with a controlled chlorine content of 10,000 ppm or less, utilizing a urethane-based prepolymer, blowing agent, and curing agent, is developed to minimize debris size and maintain excellent physical properties, avoiding the use of chlorine-based components like bis(4-amino-3-chlorophenyl)methane and vinylidene chloride.

Benefits of technology

The polishing pad effectively reduces debris size and minimizes defects and scratches, ensuring high performance and reliability in the CMP process while being environmentally friendly and safe for human health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152644000001_ABST
    Figure 2024152644000001_ABST
Patent Text Reader

Abstract

To provide a polishing pad which reduces the size of debris while maintaining various physical properties and performance of the polishing pad in excellent states by adjusting a chlorine content to be within a specific range, and can minimize generation of defects and scratches in a CMP process.SOLUTION: A polishing pad includes a polishing layer and a support layer, wherein the polishing layer contains a urethane-based prepolymer, a foaming agent and a curing agent, and a chlorine (Cl) content obtained by analyzing the polishing layer on the basis of IEC 62321-3-2 standard is 10,000 ppm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiment relates to a polishing pad having an adjusted chlorine content that can reduce defects and scratches during a chemical mechanical planarization (CMP) process, and a method for manufacturing a semiconductor device using the same. [Background technology]

[0002] Among semiconductor manufacturing processes, the chemical mechanical planarization (CMP) process is a process in which a semiconductor substrate such as a wafer is attached to a head and brought into contact with the surface of a polishing pad formed on a platen, and a slurry is supplied to chemically react with the semiconductor substrate surface while the platen and head are moved relative to each other to mechanically planarize uneven portions of the semiconductor substrate surface.

[0003] Polishing pads are essential components that play an important role in such CMP processes. They are usually made of polyurethane resin and have grooves on their surface that allow for large slurry flow and pores that support fine flow.

[0004] To manufacture the polishing pad, a prepolymer is obtained by reacting diisocyanate with a polyol, and then a curing agent and a foaming agent are mixed with the prepolymer and cured to obtain a polyurethane foam sheet. The polyurethane foam sheet is then sliced ​​at the top and bottom to obtain an upper pad according to the desired thickness, and a groove is formed on the surface of the upper pad by digging a groove in a specific shape using a tip or the like, and then the upper pad is bonded to a polyurethane-based lower pad to complete the polishing pad.

[0005] The CMP process can be applied in multiple ways in the manufacturing process of semiconductor devices. In the case of semiconductor devices, the device includes multiple layers, each of which includes a complex and fine circuit pattern. In recent years, the size of individual chips in semiconductor devices has been reduced, and the patterns of each layer have been made more complex and fine. As a result, the purpose of the CMP process in the manufacturing process of semiconductor devices has expanded beyond the planarization of circuit wiring to include the separation of circuit wiring and the improvement of wiring surfaces, and as a result, more sophisticated and reliable CMP performance is required.

[0006] During the CMP process of such a polishing pad, debris is generated when the polishing surface is rubbed against the semiconductor substrate or when the polishing surface is cut by a diamond disk for conditioning. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Korean Patent Publication No. 2016-0027075 Summary of the Invention [Problem to be solved by the invention]

[0008] During the CMP process of the polishing pad, debris is generated during the friction process between the polishing surface and the semiconductor substrate, or when the polishing surface is cut by a diamond disk for conditioning. Such debris can cause defects and scratches on the polishing surface during the CMP process.

[0009] As a result of research conducted by the present inventors, it was found that the chlorine (Cl) content in the polishing pad affects the size and surface characteristics of debris generated during conditioning of the polishing pad. By adjusting the chlorine content within a specific range, it was possible to reduce the size of debris while maintaining excellent physical properties and performance of the polishing pad, thereby minimizing the occurrence of defects and scratches during the CMP process.

[0010] Therefore, the problem to be solved by the present invention relates to a polishing pad having a chlorine content adjusted to a certain range, and a method for manufacturing a semiconductor device using the polishing pad. [Means for solving the problem]

[0011] According to one embodiment, a polishing pad is provided that includes a polishing layer and a support layer, the polishing layer including a urethane-based prepolymer, a foaming agent, and a curing agent, and the polishing layer has a chlorine (Cl) content of 10,000 ppm or less when analyzed based on the IEC 62321-3-2 standard.

[0012] According to another embodiment, the method includes the steps of preparing a polishing pad composition including a urethane-based prepolymer, a foaming agent, and a curing agent, injecting the polishing pad composition into a mold and curing it to produce a polishing layer, and laminating the polishing layer with a support layer, wherein the foaming agent includes a solid-phase foaming agent, and the solid-phase foaming agent includes at least one selected from the group consisting of acrylonitrile-based copolymers, methyl methacrylate-based copolymers, methacrylonitrile-based copolymers, and acrylic-based copolymers, and the curing agent includes diethyltoluenediamine (DETDA), 3,5-dimethylthio-2,6-diaminotoluene (DMTDA), 1,2-dimethylphenyl ether (DMTH ... The present invention provides a method for producing a polishing pad comprising one or more compounds selected from the group consisting of 4-(4-aminobenzoyl)oxyphenyl 4-aminobenzoate, 4-(4-aminobenzoyl)oxybutyl 4-aminobenzoate, 4-[4-(4-aminobenzoyl)oxy-3-methylbutoxy]butyl 4-aminobenzoate, and methylene bis-methylanthranilate (MBNA).

[0013] According to another embodiment, a method for manufacturing a semiconductor device is provided, the method including polishing a surface of a semiconductor substrate using the polishing pad. Effect of the Invention

[0014] The polishing pad according to the above embodiment has a chlorine content adjusted within a specific range, thereby reducing the size of debris while maintaining excellent physical properties and performance of the polishing pad, thereby minimizing the occurrence of defects and scratches during the CMP process.

[0015] Furthermore, the polishing pad according to the above embodiment does not use or minimizes the use of chlorine-based components such as bis(4-amino-3-chlorophenyl)methane (MOCA) and vinylidene chloride (VDC), which are commonly used as raw materials in the past, and therefore does not pose any harmful issues to humans and the environment. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a semiconductor device manufacturing process using a polishing pad according to one implementation. [Diagram 2] FIG. 2 is a diagram showing the occurrence of defects due to debris during the semiconductor device manufacturing process. [Diagram 3] FIG. 3 is an apparatus for measuring the chlorine content of a polishing pad according to one implementation. [Figure 4] FIG. 4 is a diagram illustrating a solid phase foaming agent used in a polishing pad according to one implementation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Various implementations and embodiments will now be described in detail with reference to the drawings.

[0018] In describing the implementation examples, if a detailed description of related known configurations or functions is determined to make the gist of the implementation example unclear, the detailed description will be omitted. In addition, the size of each component in the drawings may be exaggerated or omitted for the purpose of explanation, and may differ from the size actually applied.

[0019] In this specification, a description that one component is formed above / below another component, or is connected or joined to each other includes being formed, connected or joined directly between these components, or indirectly through other components. It should be understood that the reference regarding the above / below of each component may change depending on the direction in which the object is observed.

[0020] In this specification, the terms referring to each component are used to distinguish it from other components and are not intended to limit the implementation examples. Furthermore, in this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise.

[0021] In this specification, the terms "first", "second", etc. are used to describe various components, and the components should not be limited by the terms. The terms are used for the purpose of distinguishing one component from another.

[0022] In this specification, the term "comprising" is intended to embody certain features, regions, steps, steps, elements and / or components, and does not exclude the presence or inclusion of other features, regions, steps, steps, elements and / or components therein, unless specifically stated to the contrary.

[0023] The molecular weights of the compounds and polymers described herein, for example, number average molecular weight or weight average molecular weight, are, as is well known, expressed as relative masses based on carbon-12 without units, but may be understood to be the same numerical molar mass (g / mol) as necessary.

[0024] In the numerical ranges limiting the size, physical properties, etc. of the components described in this specification, when a numerical range limited only by an upper limit value and a numerical range limited only by a lower limit value are separately exemplified, it should be understood that the numerical range combining these upper and lower limits is also included in the exemplary range.

[0025] [Polishing pad] According to one implementation, the polishing pad includes a polishing layer and a support layer, and an adhesive layer may be interposed between the polishing layer and the support layer.

[0026] In one embodiment of the polishing pad, the polishing layer has a chlorine (Cl) content of 10,000 ppm or less when analyzed according to the IEC 62321-3-2 standard.

[0027] Specifically, the chlorine content can be measured by measuring the chlorine content in a sample according to IEC62321-3-2, an international standard for measuring specific substances in a polymer by combustion-ion chromatography (C-IC). In this case, the sample for measuring the chlorine content can be a circular sample with a diameter of 3 cm and a height of 0.3 cm taken from the polishing layer of the polishing pad.

[0028] The IEC62321-3-2 standard is a halogen component screening test method developed to comply with regulations on halogen use. This test method is more precise / accurate and reproducible than conventional halogen analysis methods (e.g., oxygen bomb-IC, oxygen flask-IC), and is automated, so the test results are more reliable.

[0029] 3 is a diagram showing a method for measuring the chlorine content of a polishing pad according to one embodiment. Referring to FIG. 3, a sample 110 containing organic chlorine (C-Cl) components is put into a combustion tube 730, burned in an electric furnace 750, and the resultant is sent to an adsorption tube 770 to extract chlorine ions (Cl - ) will be measured by ion chromatography.

[0030] In the polishing pad according to the embodiment, the chlorine content in the polishing layer is 10,000 ppm or less, for example, 5,000 ppm or less, 1,000 ppm or less, 500 ppm or less, 200 ppm or less, 100 ppm or less, 80 ppm or less, or 50 ppm or less. By adjusting the chlorine content within the above range, the size of debris can be reduced while maintaining the various physical properties and performance of the polishing pad in an excellent state, thereby minimizing the occurrence of defects and scratches during the CMP process.

[0031] Furthermore, the lower limit of the chlorine content range in the polishing layer according to the above embodiment may be, for example, 0 ppm or more, more than 0 ppm, 1 ppm or more, 5 ppm or more, 10 ppm or more, 20 ppm or more, 50 ppm or more, or 100 ppm or more. Within the above preferred range, debris can be aggregated to an appropriate size, the surface area and adhesive force can be adjusted, and adhesion and desorption to the wafer and pad can be facilitated, and the electrical attraction / chucking force can be adjusted to provide more appropriate polishing performance.

[0032] As a specific example, the chlorine (Cl) content of the polishing layer analyzed according to the IEC 62321-3-2 standard may be 10 ppm to 1000 ppm. As another specific example, the chlorine (Cl) content of the polishing layer analyzed according to the IEC 62321-3-2 standard may be 10 ppm to 100 ppm, 20 ppm to 80 ppm, or 20 ppm to 50 ppm. As yet another specific example, the chlorine (Cl) content of the polishing layer analyzed according to the IEC 62321-3-2 standard may be 50 ppm to 10000 ppm, or 100 ppm to 10000 ppm.

[0033] In this manner, the polishing pad according to the above embodiment can reduce the size of debris by adjusting the chlorine content within a specific range, thereby minimizing the occurrence of defects and scratches during the CMP process.

[0034] 2 shows how defects are caused by debris during the semiconductor device manufacturing process. Referring to FIG. 2, defects 650 and scratches are caused on the surface of the semiconductor device by debris 150 generated from the polishing layer, but according to the above embodiment, the size of the debris generated from the polishing layer is controlled within a specific range, so that the occurrence of defects and scratches can be minimized.

[0035] For example, polishing pads according to the above implementations can have debris particle sizes of 30 μm or less, 25 μm or less, 20 μm or less, 19 μm or less, 18 μm or less, or 17 μm or less, and can be 5 μm or more, 10 μm or more, or 15 μm or more.

[0036] Specifically, the debris was obtained when the polishing pad was conditioned under the conditions of a platen speed of 93 rpm, a conditioner load of 9 lb, a conditioner speed of 64 rpm, and 19 sweeps / min while supplying 300 cc / min of deionized water, and the particle size of the debris may be the average particle size, i.e., the D50 particle size.

[0037] As a specific example, the D50 particle size of the polishing pad debris obtained when the polishing pad is conditioned under conditions of a platen speed of 93 rpm, a conditioner load of 9 lb, a conditioner speed of 64 rpm, and 19 sweeps / min while supplying 300 cc / min of deionized water may be 30 μm or less.

[0038] As another specific example, the D50 particle size of the polishing pad debris obtained when the polishing pad is conditioned under conditions of a platen speed of 93 rpm, a conditioner load of 9 lb, a conditioner speed of 64 rpm, and 19 sweeps / min while supplying 300 cc / min of deionized water may be 10 μm to 30 μm, 10 μm to 25 μm, or 10 μm to 18 μm.

[0039] Furthermore, the polishing pad according to the above implementations may have a zeta potential value of the debris that is measured within a specific range of values.

[0040] For example, the zeta potential value of a pH 5.5 aqueous solution containing the debris obtained by conditioning the polishing layer at a concentration of 0.01% by weight may be -20 mV or more, -10 mV or more, -5 mV or more, 0 mV or more, 5 mV or more, 7 mV or more, or 10 mV or more, and may be 40 mV or less, 30 mV or less, 20 mV or less, 15 mV or less, 10 mV or less, or 8 mV or less. Specifically, the zeta potential value of the aqueous solution of the debris may be a positive (+) value.

[0041] As a specific example, the zeta potential value of a pH 5.5 aqueous solution containing the debris obtained by conditioning the polishing layer at a concentration of 0.01 wt % may be -10 mV to 30 mV. As another specific example, the zeta potential value of a pH 5.5 aqueous solution containing the debris obtained by conditioning the polishing layer at a concentration of 0.01 wt % may be 7 mV to 15 mV. As yet another specific example, the zeta potential value of a pH 5.5 aqueous solution containing the debris obtained by conditioning the polishing layer at a concentration of 0.01 wt % may be -10 mV to 8 mV.

[0042] Within the above preferred range, the zeta potential of the debris is similar to that of the abrasive particles (e.g., ceria particles) in the CMP polishing composition (slurry), and the occurrence of defects can be further reduced. Specifically, the zeta potential quantitatively indicates the magnitude of the repulsive and attractive forces between particles generated by the positive / negative ions of the particles in the suspension, and when the zeta potentials of the debris and the abrasive particles are similar, the repulsive forces between the particles are large, preventing aggregation, and thus the particle size in the composition can be reduced to reduce the occurrence of defects and scratches.

[0043] In addition, the polishing pad according to the embodiment can maintain excellent polishing pad performance and various physical properties even if the chlorine content is adjusted within a specific range.

[0044] For example, when the polishing pad is used to polish a silicon oxide layer of a silicon wafer in a ceria slurry, the removal rate may be 2000 Å / min or more, 2200 Å / min or more, 2300 Å / min or more, or 2400 Å / min or more, and may be 3000 Å / min or less, 2800 Å / min or less, 2600 Å / min or less, or 2500 Å / min or less.

[0045] As a specific example, when the polishing pad is used to polish a silicon oxide layer of a silicon wafer in a ceria slurry, the polishing rate according to the following Equation 1 may be 2200 Å / min to 2600 Å / min. [Number 1] Polishing rate (Å / min) = polished thickness of silicon wafer (Å) / polishing time (min)

[0046] Specifically, the polishing rate may be a polishing rate for a silicon wafer having a diameter of 300 mm on which silicon oxide is deposited. The polishing rate may be measured under conditions of a polishing load of 4.0 psi, a polishing pad rotation speed of 150 rpm, and a calcined ceria slurry being fed at 250 mL / min while rotating a platen at 150 rpm for 60 seconds. The temperature condition when measuring the polishing rate is not particularly limited, and may be, for example, a room temperature condition.

[0047] In addition, the pad cut rate of the polishing layer can be 30 μm / hr to 60 μm / hr, 30 μm / hr to 50 μm / hr, 40 μm / hr to 60 μm / hr, or 40 μm / hr to 50 μm / hr.

[0048] The thickness of the polishing pad may be 0.8 mm to 5.0 mm, 1.0 mm to 4.0 mm, 1.0 mm to 3.0 mm, 1.5 mm to 2.5 mm, 1.7 mm to 2.3 mm, or 2.0 mm to 2.1 mm. Within this range, the particle size deviation between the upper and lower parts of the pores can be minimized, while the basic physical properties of the polishing pad can be sufficiently exhibited.

[0049] [Polishing layer] The polishing layer provides a polishing surface that contacts a semiconductor substrate during a CMP process, and constitutes a top pad of a polishing pad.

[0050] The polishing layer includes a urethane-based prepolymer, a foaming agent, and a curing agent. Specifically, the polishing layer includes a polyurethane resin that is a reaction product of a urethane prepolymer, a foaming agent, and a curing agent, i.e., a cured product of a composition in which the above components are mixed, and more specifically, includes a porous polyurethane resin. The polishing layer may also include a plurality of pores formed from the foaming agent.

[0051] The thickness of the polishing layer may be, for example, 0.8 mm or more, 1 mm or more, 1.2 mm or more, or 1.5 mm or more, and 5 mm or less, 3 mm or less, 2.5 mm or less, or 2 mm or less. As a specific example, the thickness of the polishing layer may be 0.8 mm to 5 mm, or 1.5 mm to 3 mm.

[0052] The specific gravity of the polishing layer is, for example, 0.6 g / cm 3 More than 0.7g / cm 3 or more than 0.75g / cm 3 More than 0.9g / cm 3 Below, 0.85g / cm 3 or less than 0.8g / cm 3 In one specific example, the specific gravity of the polishing layer may be 0.6 g / cm 3 ~0.9g / cm 3 or 0.7 g / cm 3 ~0.9g / cm 3 It could be.

[0053] The hardness of the polishing layer may be, for example, 30 Shore D or more, 40 Shore D or more, or 50 Shore D or more, and 80 Shore D or less, 70 Shore D or less, 65 Shore D or less, or 60 Shore D or less. As a specific example, the hardness of the polishing layer may be 30 Shore D to 80 Shore D, or 50 Shore D to 65 Shore D.

[0054] The tensile strength of the polishing layer is, for example, 5 N / mm 2 More than 10N / mm 2 or more than 15N / mm 2 Above 30N / mm 2 Below, 25N / mm 2 or less than 20N / mm 2 As a specific example, the tensile strength of the polishing layer may be 5 N / mm 2 ~30N / mm 2 or 15N / mm 2 ~25N / mm 2 It could be.

[0055] The elongation of the polishing layer may be, for example, 50% or more, 70% or more, 90% or more, 106% or more, or 120% or more, and 300% or less, 250% or less, 200% or less, or 150% or less. As a specific example, the elongation of the polishing layer may be 50% to 300% or 90% to 130%. The elongation may be the breaking elongation.

[0056] As a specific example, the abrasive layer has a hardness of 50 Shore D to 65 Shore D and a surface roughness of 15 N / mm 2 ~25N / mm 2 and an elongation of 90% to 130%.

[0057] The pores are present in a dispersed state within the polishing layer. The average diameter of the pores can be, for example, 10 μm to 60 μm, 10 μm to 50 μm, 20 μm to 50 μm, 20 μm to 40 μm, 10 μm to 30 μm, 20 μm to 25 μm, or 30 μm to 50 μm.

[0058] The total area of ​​the pores may be 30% to 60%, 35% to 50%, or 35% to 43% of the total area of ​​the polishing layer, and the total volume of the pores may be 30% to 70%, or 40% to 60% of the total volume of the polishing layer.

[0059] The polishing layer may have grooves for mechanical polishing on the surface thereof. The grooves may have a depth, width and interval appropriate for mechanical polishing, and are not particularly limited.

[0060] [Urethane prepolymer] The polishing pad according to one implementation includes a urethane-based prepolymer. A prepolymer is a polymer having a relatively low molecular weight whose polymerization degree is stopped at an intermediate stage in order to facilitate molding in the production of a cured product. A prepolymer can be molded into a final cured product by itself or after reacting with other polymerizable compounds.

[0061] In one implementation, the urethane-based prepolymer can be prepared by reacting an isocyanate compound with a polyol.

[0062] The isocyanate compound used in the preparation of the urethane-based prepolymer may be one selected from the group consisting of aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, and combinations thereof.

[0063] The isocyanate compound may include, for example, one selected from the group consisting of toluene 2,4-diisocyanate (2,4-TDI), toluene 2,6-diisocyanate (2,6-TDI), naphthalene-1,5-diisocyanate, para-phenylene diisocyanate, tolidine diisocyanate, 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, and combinations thereof.

[0064] The polyol is a compound containing at least two hydroxyl groups (—OH) per molecule, and may include, for example, one selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, polycaprolactone polyols, and combinations thereof.

[0065] The polyol may include, for example, one selected from the group consisting of polytetramethylene ether glycol, polypropylene ether glycol, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, tripropylene glycol, and combinations thereof.

[0066] The polyol may have a weight average molecular weight (Mw) of 100 to 3000. The polyol may have a weight average molecular weight (Mw) of, for example, 100 to 3000, for example, 100 to 2000, for example, 100 to 1800.

[0067] In one embodiment, the polyol may include a low molecular weight polyol having a weight average molecular weight (Mw) of 100-300 and a high molecular weight polyol having a weight average molecular weight (Mw) of 300-1800.

[0068] The urethane-based prepolymer may have a weight average molecular weight of 500 to 3000. The urethane-based prepolymer may have a weight average molecular weight (Mw) of, for example, 1000 to 2000, for example, 1000 to 1500.

[0069] In one embodiment, the isocyanate compound for preparing the urethane-based prepolymer includes an aromatic diisocyanate compound, and the aromatic diisocyanate compound can include, for example, 2,4-toluene diisocyanate (2,4-TDI) and 2,6-toluene diisocyanate (2,6-TDI).The polyol compound for preparing the urethane-based prepolymer can include polytetramethylene ether glycol (PTMEG) and diethylene glycol (DEG).

[0070] In another embodiment, the isocyanate compound for preparing the urethane-based prepolymer can include an aromatic diisocyanate compound and an alicyclic diisocyanate compound, for example, the aromatic diisocyanate compound can include 2,4-toluene diisocyanate (2,4-TDI) and 2,6-toluene diisocyanate (2,6-TDI), and the alicyclic diisocyanate compound can include dicyclohexylmethane diisocyanate (H12MDI).The polyol compound for preparing the urethane-based prepolymer can include polytetramethylene ether glycol (PTMEG) and diethylene glycol (DEG).

[0071] The urethane-based prepolymer may have an isocyanate terminal group content (NCO%) of 5% by weight or more, 8% by weight or more, or 10% by weight or more, and 13% by weight or less, 12% by weight or less, or 11% by weight or less. As a specific example, the urethane-based prepolymer may have an isocyanate terminal group content (NCO%) of 10% by weight to 11% by weight.

[0072] The isocyanate terminal group content (NCO%) of the urethane prepolymer can be designed by comprehensively adjusting the types and contents of the isocyanate compound and polyol compound for preparing the urethane prepolymer, process conditions such as temperature, pressure, and time in the process for preparing the urethane prepolymer, and the types and contents of additives used in the preparation of the urethane prepolymer.

[0073] When the isocyanate terminal group content (NCO%) of the urethane prepolymer satisfies the above range, the reaction rate, reaction time, and final cured structure when the urethane prepolymer is subsequently reacted with a curing agent can be adjusted in a direction favorable to the polishing performance depending on the application and purpose of the final polishing pad.

[0074] In one embodiment, the isocyanate end group content (NCO%) of the urethane-based prepolymer may be 8% by weight to 10% by weight, for example, 8% by weight to 9.4% by weight. If the NCO% is less than the above range, the desired polishing performance may not be achieved in terms of polishing rate and flatness, and there may be a problem of shortening the life of the polishing pad due to an excessive increase in cutting rate, etc. On the other hand, if the NCO% exceeds the above range, surface defects such as scratches and chatter marks on the semiconductor substrate may increase.

[0075] [Foaming agent] The foaming agent may include one selected from the group consisting of a solid-phase foaming agent, a gas-phase foaming agent, a liquid-phase foaming agent, and combinations thereof, as a component for forming a pore structure in the polishing layer.

[0076] According to one embodiment, the foaming agent is a non-chlorine foaming agent that does not contain a chlorine component, and in particular, does not contain or minimizes the use of a chlorine foaming agent component that is commonly used in polishing pad manufacturing, such as vinylidene chloride (VDC). For example, the content of the non-chlorine foaming agent based on the total weight of the foaming agent is 50 wt% or more, 80 wt% or more, 90 wt% or more, 95 wt% or more, 97 wt% or more, 99 wt% or more, or 99.5 wt% or more, and 100 wt% or less or 99.5 wt% or less, and specific examples include 80 wt% to 100 wt%, 90 wt% to 100 wt%, or 80 wt% to 99.5 wt%. The content of the chlorine-based blowing agent based on the total weight of the blowing agent is 20% by weight or less, 10% by weight or less, 5% by weight or less, 1% by weight or less, or 0.5% by weight or less, 0.3% by weight or less, or 0% by weight or more, 0.1% by weight or more, 0.5% by weight or more, and specific examples thereof may be 0 to 20% by weight, 0 to 1% by weight, 0 to 0.5% by weight, or 0.5 to 20% by weight.

[0077] The foaming agent may be one or more selected from a solid-phase foaming agent containing particles having a hollow structure, a liquid-phase foaming agent using a volatile liquid, and an inert gas.

[0078] For example, the solid foaming agent may include particles having a hollow structure, the size of which is adjusted by expanding with heat. Such a solid foaming agent is added to the raw material in an already expanded form and has a uniform particle size, which is advantageous in that the particle size of the pores can be uniformly adjusted.

[0079] The solid-phase foaming agent may also include expandable particles. The expandable particles are particles that have the property of being expandable by heat or pressure, etc., and the size of the expandable particles in the final polishing layer may be determined by the heat or pressure applied during the manufacturing process of the polishing layer. The expandable particles are added to the raw material in a pre-unexpanded particle state, and are expanded by the heat or pressure applied during the manufacturing process of the polishing layer, so that the final size of the expandable particles may be determined.

[0080] The average particle diameter of the solid-phase foaming agent may be, for example, 5 μm to 100 μm, specifically 5 μm to 50 μm or 20 μm to 50 μm. The average particle diameter of the solid-phase foaming agent means the average particle diameter of the expanded particles themselves when the solid-phase foaming agent is particles added to the raw material in an expanded state as described below, and may mean the average particle diameter of the particles after expansion by heat or pressure during the manufacturing process when the solid-phase foaming agent is particles added to the raw material in an unexpanded state as described below.

[0081] 4 is a diagram showing an expandable particle type solid-phase foaming agent used in a polishing pad according to an embodiment. Referring to FIG. 4, the expandable particle type solid-phase foaming agent 130 may include a resin material outer shell 131 and an expansion-inducing component 132 present inside and enclosed by the outer shell 131. Such expandable particles may be formed into a hollow structure by vaporizing the internal expansion-inducing component due to heat during the manufacturing process.

[0082] For example, the outer shell may include a thermoplastic resin, which may be one or more selected from the group consisting of an acrylonitrile-based copolymer, a methacrylonitrile-based copolymer, and an acrylic-based copolymer.

[0083] The thickness of the skin is, for example, 0.1 μm or more, 0.5 μm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and 15 μm or less, 12 μm or less, or 10 μm or less, and as a specific example, it can be 2 μm to 15 μm.

[0084] The expansion-inducing component may include one selected from the group consisting of a hydrocarbon compound, a tetraalkylsilane compound, and a combination thereof. Specifically, the hydrocarbon compound may include one selected from the group consisting of ethane, ethylene, propane, propene, n-butane, isobutene, n-butene, isobutene, n-pentane, isopentane, neopentane, n-hexane, heptane, petroleum ether, and a combination thereof. The tetraalkylsilane compound may include one selected from the group consisting of tetramethylsilane, trimethylethylsilane, trimethylisopropylsilane, trimethyl-n-propylsilane, and a combination thereof.

[0085] The solid-phase blowing agent may include inorganic component-treated particles. In one implementation, the solid-phase blowing agent may have a surface treated with silica (SiO2) particles. The inorganic component treatment of the solid-phase blowing agent may prevent agglomeration between multiple particles. The inorganic component-treated solid-phase blowing agent may have different chemical, electrical and / or physical properties of the blowing agent surface from a solid-phase blowing agent that is not inorganic component-treated.

[0086] Commercially available solid phase blowing agents include 920DE20d70, 051DET40d25, 051DET40d42 and the like manufactured by Nouryon, and F-65DE, F-80DE, FN-80SDE and the like manufactured by Matsumoto.

[0087] As a specific example, the foaming agent used in the polishing pad according to the above embodiment includes a solid-phase foaming agent, and the solid-phase foaming agent may include one or more selected from the group consisting of acrylonitrile-based copolymers, methyl methacrylate-based copolymers, methacrylonitrile-based copolymers, and acrylic-based copolymers.

[0088] The content of the solid-phase blowing agent may be 0.1 parts by weight or more, 0.5 parts by weight or more, or 1 part by weight or more, and 5 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less, based on 100 parts by weight of the urethane-based prepolymer. As a specific example, the content of the solid-phase blowing agent may be 0.1 to 5 parts by weight or 0.5 to 2 parts by weight, based on 100 parts by weight of the urethane-based prepolymer.

[0089] The type and content of the solid-phase foaming agent can be designed depending on the desired pore structure and physical properties of the polishing layer.

[0090] Meanwhile, the liquid foaming agent is added during the process of mixing and reacting the prepolymer and the curing agent to form pores, but is not involved in the reaction between the prepolymer and the curing agent. Also, the liquid foaming agent is physically vaporized by heat generated during the process of mixing and reacting the prepolymer and the curing agent to form pores.

[0091] The volatile liquid phase blowing agent does not react with isocyanate groups, amide groups, and alcohol groups, and may be in a liquid phase at 25° C. Specifically, the volatile liquid phase blowing agent may be selected from the group consisting of perfluoro compounds such as cyclopentane, n-pentane, cyclohexane, n-butyl acetate, bis(nonafluorobutyl)(trifluoromethyl)amine, perfluorotributylamine, perfluoro-N-methylmorpholine, perfluorotripentylamine, and perfluorohexane. Commercially available perfluoro compounds include FC-40, FC-43, FC-70, FC-72, FC-770, FC-3283, and FC-3284 from 3M.

[0092] In addition, the blowing agent may include a gas phase blowing agent. For example, the blowing agent may include a solid phase blowing agent and a gas phase blowing agent.

[0093] The gas-phase blowing agent may include an inert gas, and may be used as a pore-forming agent by being added during the reaction of the urethane-based prepolymer with the curing agent.

[0094] The inert gas is not particularly limited as long as it is a gas that does not participate in the reaction between the urethane prepolymer and the curing agent. For example, the inert gas may include one selected from the group consisting of nitrogen gas (N2), carbon dioxide gas (CO2), argon gas (Ar), helium gas (He), and combinations thereof.

[0095] The type and content of the gas-phase foaming agent can be designed depending on the desired pore structure and physical properties of the polishing layer.

[0096] The inert gas may be added in a volume equivalent to 10% to 30% of the total volume of the composition. Specifically, the inert gas may be added in a volume equivalent to 15% to 30% of the total volume of the composition. Specifically, the gas-phase blowing agent may be injected through a predetermined injection line during the process of mixing the urethane-based prepolymer, the solid-phase blowing agent, and the curing agent. The injection rate of the gas-phase blowing agent may be about 0.8 L / min to about 2.0 L / min, for example, about 0.8 L / min to about 1.8 L / min, for example, about 0.8 L / min to about 1.7 L / min, for example, about 1.0 L / min to about 2.0 L / min, for example, about 1.0 L / min to about 1.8 L / min, for example, about 1.0 L / min to about 1.7 L / min.

[0097] [Hardening agent] The curing agent is a compound that chemically reacts with the urethane-based prepolymer to form a final cured structure in the polishing layer, and may include, for example, an amine compound or an alcohol compound. Specifically, the curing agent may include one selected from the group consisting of aromatic amines, aliphatic amines, aromatic alcohols, aliphatic alcohols, and combinations thereof.

[0098] According to one embodiment, the curing agent may include a non-chlorine curing agent that does not contain a chlorine component. For example, the content of the non-chlorine curing agent based on the total weight of the curing agent may be 50% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, 97% by weight or more, 99% by weight or more, or 99.5% by weight or more, and may be 100% by weight or less or 99.5% by weight or less, and may be 80% by weight to 100% by weight, 90% by weight to 100% by weight, or 80% by weight to 99.5% by weight, for example. The content of the chlorine-based curing agent based on the total weight of the curing agent is 20% by weight or less, 10% by weight or less, 5% by weight or less, 1% by weight or less, or 0.5% by weight or less, 0.3% by weight or less, or 0% by weight or more, 0.1% by weight or more, 0.5% by weight or more, and specific examples thereof may be 0% by weight to 20% by weight, 0% by weight to 1% by weight, 0% by weight to 0.5% by weight, or 0.5% by weight to 20% by weight.

[0099] The curing agent may be at least one selected from a solid-phase curing agent and a liquid-phase curing agent.

[0100] The solid-phase hardener may contain an active hydrogen group. The solid-phase hardener may contain an amine group (-NH2) as the active hydrogen group.

[0101] In addition, the solid-phase hardener may be an ester compound having two or more benzene rings. Specifically, the solid-phase hardener may contain two or more ester groups in the molecule.

[0102] The solid-phase curing agent may have a weight average molecular weight of 150 to 400, for example, 150 to 350, for example, 200 to 350, for example, 250 to 350, for example, 300 to 350. The solid-phase curing agent may have a melting point (mp) of 100°C to 150°C, for example, 100°C to 140°C, for example, 110°C to 130°C.

[0103] In one implementation, the solid-phase curing agent may include one or more selected from the group consisting of 1,3-propanediol bis(4-aminobenzoate) (PDPAB), 4-(4-aminobenzoyl)oxyphenyl 4-aminobenzoate, 4-(4-aminobenzoyl)oxybutyl 4-aminobenzoate, 4-[4-(4-aminobenzoyl)oxy-3-methylbutoxy]butyl 4-aminobenzoate, and methylene bis-methylanthranilate (MBNA).

[0104] The liquid-phase curing agent may contain an active hydrogen group, which may be one or more selected from the group consisting of an amine group (-NH2), a hydroxyl group (-OH), a carboxylic acid group (-COOH), an epoxy group, and combinations thereof, and may specifically contain an amine group (-NH2).

[0105] The liquid phase curing agent may contain sulfur in the molecule, specifically, may contain two or more sulfur elements in the molecule.

[0106] The liquid phase curing agent has a weight average molecular weight of 50-300, for example, 100-250, for example, 150-250, for example, 200-250.

[0107] The liquid-phase hardener may be in a liquid phase at room temperature, or may have a boiling point (bp) of 160°C to 240°C, specifically 170°C to 240°C, more specifically 170°C to 220°C.

[0108] Examples of the liquid phase curing agent may include one or more selected from the group consisting of 3,5-dimethylthio-2,6-diaminotoluene (DMTDA), 2,6-bis(methylthio)-4-methyl-1,3-benzenediamine, and N,N'-bis(sec-butylamino)diphenylmethane.

[0109] In addition, the curing agent may further include other curing agents in addition to the liquid-phase curing agent and the solid-phase curing agent. The other curing agents may be, for example, one or more of an amine compound and an alcohol compound. Specifically, the other curing agents may include one or more compounds selected from the group consisting of aromatic amines, aliphatic amines, aromatic alcohols, and aliphatic alcohols.

[0110] For example, the other curing agent may be one or more selected from the group consisting of diaminodiphenyl methane, diaminodiphenyl sulphone, m-xylylene diamine, isophoronediamine, ethylenediamine, diethylenetriamine, triethylenetetramine, polypropylenediamine, polypropylenetriamine, ethylene glycol, diethyleneglycol, dipropyleneglycol, butanediol, hexanediol, glycerine, and trimethylolpropane.

[0111] As a specific example, the curing agent may include one or more selected from the group consisting of diethyltoluenediamine (DETDA), 3,5-dimethylthio-2,6-diaminotoluene (DMTDA), 1,3-propanediol bis(4-aminobenzoate) (PDPAB), N,N'-bis(sec-butylamino)diphenylmethane, 2,6-bis(methylthio)-4-methyl-1,3-benzenediamine, 4-(4-aminobenzoyl)oxyphenyl 4-aminobenzoate, 4-(4-aminobenzoyl)oxybutyl 4-aminobenzoate, 4-[4-(4-aminobenzoyl)oxy-3-methylbutoxy]butyl 4-aminobenzoate, and methylene bis-methylanthranilate (MBNA).

[0112] The content of the curing agent may be 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, or 20 parts by weight or more, and 50 parts by weight or less, 45 parts by weight or less, 40 parts by weight or less, 35 parts by weight or less, 30 parts by weight or less, or 25 parts by weight or less, based on 100 parts by weight of the urethane-based prepolymer. Specifically, the content of the curing agent may be 10 parts by weight to 40 parts by weight, more specifically, 15 parts by weight to 35 parts by weight or 15 parts by weight to 25 parts by weight, based on 100 parts by weight of the urethane-based prepolymer.

[0113] [Additives] The composition for preparing the polishing layer may further include other additives such as a surfactant, a reaction rate modifier, etc. The names "surfactant", "reaction rate modifier", etc. are arbitrary names based on the main role of the corresponding substance, and each corresponding substance does not necessarily perform only the function limited to the role of the corresponding name.

[0114] The surfactant is not particularly limited as long as it is a substance that serves to prevent phenomena such as pore aggregation or overlapping, etc. For example, the surfactant may include a silicone-based surfactant.

[0115] The surfactant may be used in an amount of 0.2 to 2 parts by weight based on 100 parts by weight of the urethane-based prepolymer. Specifically, the surfactant may be used in an amount of 0.2 to 1.9 parts by weight, for example, 0.2 to 1.8 parts by weight, for example, 0.2 to 1.7 parts by weight, for example, 0.2 to 1.6 parts by weight, for example, 0.2 to 1.5 parts by weight, for example, 0.5 to 1.5 parts by weight based on 100 parts by weight of the urethane-based prepolymer. When the surfactant is included in an amount within the above range, pores derived from the gas phase blowing agent can be stably formed and maintained in the mold.

[0116] The reaction rate regulator plays a role of accelerating or retarding the reaction, and may be a reaction promoter, a reaction retarder, or both, depending on the purpose. The reaction rate regulator may include a reaction promoter. For example, the reaction promoter may be one or more reaction promoters selected from the group consisting of tertiary amine compounds and organometallic compounds.

[0117] Specifically, the reaction rate regulator may include one or more selected from the group consisting of triethylenediamine, dimethylethanolamine, tetramethylbutanediamine, 2-methyl-triethylenediamine, dimethylcyclohexylamine, triethylamine, triisopropanolamine, 1,4-diazabicyclo(2,2,2)octane, bis(2-methylaminoethyl)ether, trimethylaminoethylethanolamine, N,N,N,N,N″-pentamethyldiethylenetriamine, dimethylaminoethylamine, dimethylaminopropylamine, benzyldimethylamine, N-ethylmorpholine, N,N-dimethylaminoethylmorpholine, N,N-dimethylcyclohexylamine, 2-methyl-2-azanorbornene, dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, dioctyltin diacetate, dibutyltin maleate, dibutyltin di-2-ethylhexanoate, and dibutyltin dimercaptide. Specifically, the reaction rate regulator may include one or more selected from the group consisting of benzyldimethylamine, N,N-dimethylcyclohexylamine, and triethylamine.

[0118] The reaction rate adjuster may be used in an amount of 0.05 parts by weight to 2 parts by weight based on 100 parts by weight of the urethane-based prepolymer. Specifically, the reaction rate adjuster may be used in an amount of 0.05 parts by weight to 1.8 parts by weight, for example, 0.05 parts by weight to 1.7 parts by weight, for example, 0.05 parts by weight to 1.6 parts by weight, for example, 0.1 parts by weight to 1.5 parts by weight, for example, 0.1 parts by weight to 0.3 parts by weight, for example, 0.2 parts by weight to 1.8 parts by weight, for example, 0.2 parts by weight to 1.7 parts by weight, for example, 0.2 parts by weight to 1.6 parts by weight, for example, 0.2 parts by weight to 1.5 parts by weight, for example, 0.5 parts by weight to 1 part by weight based on 100 parts by weight of the urethane-based prepolymer. When the reaction rate adjuster is used in the above content range, the curing reaction rate of the prepolymer composition can be appropriately adjusted to form a polishing layer having pores of a desired size and hardness.

[0119] [Support layer] The support layer constitutes a sub pad and serves to absorb and disperse external impacts applied to the polishing layer while supporting the polishing layer, thereby minimizing damage and defects to an object to be polished during a polishing process using the polishing pad.

[0120] The support layer may include, but is not limited to, a nonwoven fabric or suede. In one embodiment, the support layer may be a resin-impregnated nonwoven fabric. The nonwoven fabric may be a fibrous nonwoven fabric comprising one selected from the group consisting of polyester fibers, polyamide fibers, polypropylene fibers, polyethylene fibers, and combinations thereof.

[0121] The resin impregnated into the nonwoven fabric may include one selected from the group consisting of polyurethane resin, polybutadiene resin, styrene-butadiene copolymer resin, styrene-butadiene-styrene copolymer resin, acrylonitrile-butadiene copolymer resin, styrene-ethylene-butadiene-styrene copolymer resin, silicone rubber resin, polyester-based elastomer resin, polyamide-based elastomer resin, and combinations thereof.

[0122] The thickness of the support layer may be, for example, 0.3 mm or more, or 0.5 mm or more, and 3 mm or less, 2 mm or less, or 1 mm or less. As a specific example, the thickness of the support layer may be 0.3 mm to 3 mm, or 0.5 mm to 1 mm.

[0123] The hardness of the support layer may be, for example, 50 Asker C or more, 60 Asker C or more, or 70 Asker C or more, and 100 Asker C or less, 90 Asker C or less, or 80 Asker C or less. As a specific example, the hardness of the support layer may be 50 Asker C to 100 Asker C or 60 Asker C to 90 Asker C.

[0124] Also, an adhesive layer may be inserted between the polishing layer (upper pad) and the support layer (lower pad).

[0125] The adhesive layer may include a hot melt adhesive. The hot melt adhesive may be one or more selected from the group consisting of polyurethane resins, polyester resins, ethylene-vinyl acetate resins, polyamide resins, and polyolefin resins. Specifically, the hot melt adhesive may be one or more selected from the group consisting of polyurethane resins and polyester resins.

[0126] In addition, a double-sided tape is attached to the lower part of the support layer, and when the double-sided tape is applied to a CMP device, the release paper of the double-sided tape can be removed and the double-sided tape can be attached to a platen for use.

[0127] [Polishing pad manufacturing method] A method for manufacturing a polishing pad according to one embodiment includes preparing a polishing pad composition including a urethane-based prepolymer, a foaming agent, and a curing agent, injecting the polishing pad composition into a mold and curing it to produce a polishing layer, and bonding the polishing layer to a support layer.

[0128] The specific types and contents of the urethane-based prepolymer, the curing agent, and the foaming agent are as exemplified above.

[0129] As a specific example, the foaming agent includes a solid-phase foaming agent, and the solid-phase foaming agent includes at least one selected from the group consisting of an acrylonitrile-based copolymer, a methyl methacrylate-based copolymer, a methacrylonitrile-based copolymer, and an acrylic-based copolymer. The curing agent may include at least one selected from the group consisting of diethyltoluenediamine (DETDA), 3,5-dimethylthio-2,6-diaminotoluene (DMTDA), 1,3-propanediol bis(4-aminobenzoate) (PDPAB), N,N'-bis(sec-butylamino)diphenylmethane, 2,6-bis(methylthio)-4-methyl-1,3-benzenediamine, 4-(4-aminobenzoyl)oxyphenyl 4-aminobenzoate, 4-(4-aminobenzoyl)oxybutyl 4-aminobenzoate, 4-[4-(4-aminobenzoyl)oxy-3-methylbutoxy]butyl 4-aminobenzoate, and methylene bis-methylanthranilate (MBNA).

[0130] The polishing pad composition may be prepared by sequentially or simultaneously mixing the urethane-based prepolymer, the foaming agent, and the curing agent.

[0131] As an example, the step of preparing the polishing pad composition may be performed by mixing a urethane-based prepolymer with a curing agent and then further mixing it with a foaming agent, or by mixing the urethane-based prepolymer with the foaming agent and then further mixing it with the curing agent.

[0132] As another example, the urethane-based prepolymer, the curing agent, and the blowing agent are added to the mixing process at substantially the same time, and when a blowing agent, a surfactant, and an inert gas are further added, they may also be added to the mixing process at substantially the same time.

[0133] As another example, the urethane prepolymer, the blowing agent and the surfactant may be premixed and then the curing agent may be added, or the curing agent and the inert gas may be added together.

[0134] In the mixing, the urethane prepolymer and the curing agent are mixed to start the reaction, and the foaming agent and the inert gas are uniformly dispersed in the raw material. In this case, the reaction rate regulator can be intervened in the reaction between the urethane prepolymer and the curing agent from the early stage of the reaction to adjust the reaction rate. Specifically, the mixing can be performed at a speed of 1000 rpm to 10000 rpm or 4000 rpm to 7000 rpm. When the speed is within the above range, it is more advantageous for the inert gas and the foaming agent to be uniformly dispersed in the raw material.

[0135] The step of preparing the polishing pad composition may be carried out at a temperature of 50° C. to 150° C., and may be carried out under vacuum degassing conditions as necessary.

[0136] When the foaming agent includes a solid-phase foaming agent, the step of preparing the polishing pad composition may include a step of preparing a first preliminary composition by mixing the urethane-based prepolymer and the solid-phase foaming agent, and a step of preparing a second preliminary composition by mixing the first preliminary composition and a curing agent.

[0137] The viscosity of the first preliminary composition at about 80° C. may be about 1000 cps to about 2000 cps, for example, about 1000 cps to about 1800 cps, for example, about 1000 cps to about 1600 cps, for example, about 1000 cps to about 1500 cps.

[0138] When the foaming agent includes a gas-phase foaming agent, the step of preparing the polishing pad composition may include the steps of preparing a third preliminary composition including the urethane-based prepolymer and the curing agent, and injecting the gas-phase foaming agent into the third preliminary composition to prepare a fourth preliminary composition. In one implementation, the third preliminary composition may further include a solid-phase foaming agent.

[0139] In one implementation example, the process for manufacturing the polishing layer may include preparing a mold preheated to a first temperature, injecting and curing the polishing pad composition into the preheated mold, and post-curing the hardened polishing pad composition under a second temperature condition higher than the preheat temperature.

[0140] In one embodiment, the temperature difference between the first temperature and the second temperature is about 10° C. to about 40° C., for example, about 10° C. to about 35° C., for example, about 15° C. to about 35° C. In one embodiment, the first temperature is about 60° C. to about 100° C., for example, about 65° C. to about 95° C., for example, about 70° C. to about 90° C. In one embodiment, the second temperature is about 100° C. to about 130° C., for example, about 100° C. to about 125° C., for example, about 100° C. to about 120° C.

[0141] The step of curing the polishing pad composition at the first temperature may be performed for about 5 minutes to about 60 minutes, such as about 5 minutes to about 40 minutes, such as about 5 minutes to about 30 minutes, for example, about 5 minutes to about 25 minutes.

[0142] The step of post-curing the polishing pad composition cured at the first temperature at the second temperature may be carried out for about 5 hours to about 30 hours, for example, about 5 hours to about 25 hours, for example, about 10 hours to about 30 hours, for example, about 10 hours to about 25 hours, for example, about 12 hours to about 24 hours, for example, about 15 hours to about 24 hours.

[0143] Then, the step of injecting the polishing pad composition into the mold and curing it is performed under a temperature condition of 60° C. to 120° C. and a pressure of 50 kg / m 2 ~200kg / m 2 The reaction may be carried out under pressure conditions of 0.1 to 1000 MPa.

[0144] The manufacturing method may further include a step of cutting the surface of the obtained polishing pad, a step of processing grooves in the surface, a step of bonding with a lower layer, a step of inspecting, a step of packaging, etc. These steps may be performed by a normal polishing pad manufacturing method.

[0145] As an example, the method for manufacturing the polishing pad may include processing at least one surface of the polishing layer, which may include at least one of forming grooves on the at least one surface of the polishing layer, lathe turning the at least one surface of the polishing layer, and roughening the at least one surface of the polishing layer.

[0146] The grooves may include at least one of concentric grooves formed at a predetermined interval from the center of the polishing layer and radial grooves continuously connected from the center of the polishing layer to the edge of the polishing layer. The turning may be performed by a method of cutting off a predetermined thickness of the polishing layer using a cutting tool. The roughening may be performed by processing the surface of the polishing layer with a sanding roller.

[0147] [Method of manufacturing semiconductor devices] A method for manufacturing a semiconductor device according to one implementation includes polishing a surface of a semiconductor substrate using a polishing pad according to the implementation.

[0148] Specifically, the method for manufacturing the semiconductor device may include a step of providing a polishing pad according to the above embodiment, and a step of polishing the surface of the semiconductor substrate by rotating the polishing surface of the polishing layer and the surface of the semiconductor substrate relative to each other so as to abut against each other.

[0149] FIG. 1 is a diagram showing a semiconductor device manufacturing process using a polishing pad according to an embodiment. Referring to FIG. 1, a polishing pad 100 according to an embodiment is mounted on a platen 200, and then a semiconductor substrate 600 to be polished is placed on the polishing pad 100. At this time, the surface to be polished of the semiconductor substrate 600 directly contacts the polishing surface of the polishing pad 100. For polishing, a polishing slurry 400 may be sprayed onto the polishing pad through a nozzle. The flow rate of the polishing slurry 400 supplied through the nozzle is about 10 cm. 3 / min ~ approx. 1000cm 3 / min., for example, about 50 cm 3 / min ~ approx. 500cm 3 / min, but is not limited to this.

[0150] Thereafter, the semiconductor substrate 600 and the polishing pad 100 may rotate relative to each other to polish the surface of the semiconductor substrate 600. At this time, the rotating direction of the semiconductor substrate 600 and the rotating direction of the polishing pad 100 may be the same or opposite to each other. The rotating speeds of the semiconductor substrate 600 and the polishing pad 100 may be selected according to the purpose within a range of about 10 rpm to about 500 rpm, respectively, and may be, for example, about 30 rpm to about 200 rpm, but are not limited thereto.

[0151] The semiconductor substrate 600 may be attached to the polishing head 510 and brought into contact with the polishing surface of the polishing pad 100 under a predetermined load, and then the surface of the semiconductor substrate 600 may be polished. The load applied to the polishing surface of the polishing pad 100 by the polishing head 510 is about 1 gf / cm. 2 ~About 1000gf / cm 2 For example, the range is about 10 gf / cm 2 ~About 800gf / cm 2 It can be, but is not limited to, these.

[0152] In one embodiment, the semiconductor substrate 600 to be polished may include an oxide film, a tungsten film, or a composite film thereof. Specifically, the semiconductor substrate 600 may include an oxide film, a tungsten film, or a composite film of an oxide film and a tungsten film. The composite film of an oxide film and a tungsten film may be a multi-layer film in which the tungsten film is stacked on one side of the oxide film, or may be a single layer film in which an oxide region and a tungsten region are mixed in one layer. When the polishing object has such film quality characteristics and the polishing pad has the characteristics according to the embodiment, defects in the semiconductor device manufactured by the manufacturing method of the semiconductor device may be minimized.

[0153] In one embodiment, the method for manufacturing a semiconductor device may further include, in the step of polishing the object to be polished, a step of supplying either one of the oxide film polishing slurry and the tungsten film polishing slurry, or a step of sequentially supplying the oxide film polishing slurry and the tungsten film polishing slurry to a polishing surface.

[0154] For example, when the semiconductor substrate to be polished includes an oxide film, the method for manufacturing a semiconductor device may include a step of supplying the oxide film polishing slurry. When the semiconductor substrate includes a tungsten film, the method for manufacturing a semiconductor device may include a step of supplying the tungsten film polishing slurry. When the semiconductor substrate includes a composite film of an oxide film and a tungsten film, the method for manufacturing a semiconductor device may include a step of supplying the oxide film polishing slurry and the tungsten film polishing slurry sequentially to the polishing surface. At this time, depending on the process, the oxide film polishing slurry may be supplied first and then the tungsten film polishing slurry may be supplied later, or the tungsten film polishing slurry may be supplied first and then the oxide film polishing slurry may be supplied later.

[0155] In one embodiment, the method for manufacturing a semiconductor device may further include a step of processing the polishing surface of the polishing pad 100 with a conditioner 300 simultaneously with polishing the semiconductor substrate 600 in order to maintain the polishing surface of the polishing pad 100 in a state suitable for polishing.

[0156] The polishing pad according to one embodiment has a chlorine content in its polishing layer adjusted within a specific range, thereby maintaining the physical properties and performance of the polishing pad in excellent condition while reducing the size of debris and minimizing the occurrence of defects and scratches during the CMP process, so that semiconductor devices of excellent quality can be efficiently manufactured using the polishing pad.

[0157] (Example) Examples are described below, but the feasible scope is not limited to these.

[0158] (Examples and Comparative Examples: Production of Polishing Pads) Step (1) Preparation of prepolymer Toluene diisocyanate (TDI), dicyclohexylmethane diisocyanate (H12MDI), polytetramethylene ether glycol (PTMEG) and diethylene glycol (DEG) were charged into a four-neck flask and reacted at 80°C for 3 hours to prepare a urethane prepolymer. The NCO% of the prepolymer was measured and is shown in Table 1 below.

[0159] Step (2) Manufacturing the polishing pad A casting machine was prepared, equipped with tanks and supply lines for supplying raw materials such as prepolymer, curing agent, inert gas, and foaming agent. The urethane-based prepolymer, foaming agent, curing agent, inert gas (N2), and silicone-based surfactant (Evonik) prepared above were filled into each tank. The raw materials were stirred while being fed into the mixing head at a constant speed through each feeding line. The foaming agent and curing agent used were those listed in Table 1 below, and the prepolymer and curing agent were fed in an equivalent ratio of 1:1 at a total rate of 10 kg / min.

[0160] A mold (1000 mm x 1000 mm x 3 mm) was prepared and preheated at 80°C, and the raw material stirred above was discharged into the mold and reacted to obtain a solid cake-like molded body. Then, the upper and lower ends of the molded body were cut to obtain an upper pad polishing layer.

[0161] Thereafter, the polishing layer was subjected to surface milling and groove forming processes, and then attached to a lower pad support layer with a hot melt adhesive to produce a polishing pad.

[0162] A double-sided tape (442JS, 3M) was attached to the lower part of the support layer so that it could be attached to the platen of a CMP device.

[0163] The curing agents and foaming agents used in the examples and comparative examples are as follows. - DMTDA: 3,5-dimethylthio-2,6-diaminotoluene, Covestro - MOCA: 4,4'-methylenebis(2-chloroaniline), Ishihara - F-65DE: Acrylonitrile / Methyl Methacrylate / Methacrylonitrile Copolymer, Expanded Cell Type, Matsumoto - F-80DE: Acrylonitrile / Methyl Methacrylate / Methacrylonitrile Copolymer, Expanded Cell Type, Matsumoto - 051DET40d25: Acrylonitrile / Methacrylonitrile Copolymer, Expanded Cell Type, Nouryon - 051DET40d42: Acrylonitrile / Methacrylonitrile Copolymer, Expanded Cell Type, Nouryon - 461DET40d25: Acrylonitrile / Dichloroethane, Expanded Cell Type, Nouryon

[0164] The configurations of the above-mentioned Examples and Comparative Examples are summarized in Table 1 below.

[0165] JPEG2024152644000002.jpg153164

[0166] (Test Example 1) The polishing layer, support layer, and polishing pad formed by laminating these thus produced were subjected to the following tests.

[0167] (1)Hardness The samples were cut into 5 cm x 5 cm (thickness: 2 mm) and stored at room temperature, 30°C, 50°C, and 70°C for 12 hours, respectively, and then the Shore D hardness and Asker C hardness were measured using a hardness tester.

[0168] (2) Specific gravity The sample was cut into a size of 2 cm x 5 cm (thickness: 2 mm) and stored at 25°C for 12 hours, after which the specific gravity was measured using a hydrometer.

[0169] (3) Tensile strength The sample was cut into a size of 4 cm×1 cm (thickness: 2 mm), and the maximum strength value just before the breakage of the polishing pad was measured using a universal testing meter (UTM) at a speed of 50 mm / min.

[0170] (4) Growth rate The sample was cut to 4 cm x 1 cm (thickness: 2 mm), and the maximum deformation just before the abrasive pad broke was measured using a universal testing meter (UTM) at a speed of 50 mm / min. The ratio of the maximum deformation to the initial length was then expressed as a percentage (%). The results are summarized in the table below.

[0171] JPEG2024152644000003.jpg127162

[0172] As can be seen from the above table, the polishing pads of Examples 1 to 7 were at levels equal to or higher than those of the polishing pads of Comparative Examples 1 and 2 in terms of hardness, specific gravity, tensile strength, and elongation.

[0173] (Test Example 2) Each of the polishing pads thus manufactured was subjected to the following tests.

[0174] (1)Removal rate A silicon wafer having a diameter of 300 mm on which silicon oxide had been deposited by a CVD process was placed in a CMP polishing apparatus, and then the silicon wafer was placed with the silicon oxide film facing down on the platen to which the porous polyurethane polishing pad had been attached.

[0175] Thereafter, the silicon oxide film was polished by rotating the platen at 150 rpm for 60 seconds while feeding calcined ceria slurry onto the polishing pad at a rate of 250 mL / min under conditions of a polishing load of 4.0 psi and a polishing pad rotation speed of 150 rpm.

[0176] After polishing, the silicon wafer was removed from the carrier, attached to a spin dryer, washed with deionized water (DIW), and then dried with nitrogen for 15 seconds. The change in film thickness of the dried silicon wafer before and after polishing was measured using a spectroscopic interference wafer thickness meter (model name: SI-F80R, Keyence Corporation).

[0177] Then, the polishing rate was calculated using the following mathematical formula 1. [Number 1] Polishing rate (Å / min) = polished thickness of silicon wafer (Å) / polishing time (min)

[0178] (2) Defects Polishing was performed in the same manner as in the polishing rate test using a CMP polishing device. After polishing, the silicon wafer was moved to a cleaning device and washed with 1% HF, deionized water (DIW), 1% H2NO3, and deionized water (DIW) for 10 seconds each. It was then moved to a spin dryer and washed with deionized water (DIW), and then dried with nitrogen for 15 seconds. The dried silicon wafer was measured for defect changes before and after polishing using a defect measuring device (model name: XP+, KLA-TENCOR). Specifically, the total number of scratches, chatter marks, pits, and residues on the wafer was measured.

[0179] (3) Chlorine content A circular sample with a diameter of 3 cm and a height of 0.3 cm was prepared from the polishing layer of the polishing pad. The chlorine content in the sample was measured according to IEC62321-3-2, an international standard for the measurement of specific substances in polymers by combustion ion chromatography (C-IC) (see Figure 3).

[0180] (4) Debris size A porous polyurethane polishing pad was attached and set on the platen of a CMP polishing device. Then, the operation of the carrier was removed and only the conditioner and deionized water (DIW) were used to collect debris from the polishing layer. The platen speed was set to 93 rpm, the conditioner load was 9 lb, the rotation speed was 64 rpm, and the sweep speed was 19 times / min, and deionized water was injected at 300 cc / min to condition the polishing layer. The debris from the polishing layer that came out with the deionized water during conditioning was collected. The D50 particle size of the collected debris was obtained using a particle size analyzer (Mastersize 3000, Malvern) and a medium-capacity automatic wet disperser (Hydro MV, Malvern). The analyzer settings were polyurethane 1.55 as the refractive index of the analyte, deionized water 1.33 as the refractive index of the dispersant, and the stirring speed was 2500 rpm.

[0181] (5) Zeta potential A porous polyurethane polishing pad was attached to the platen of a CMP polishing device and set on it. After that, the carrier was removed and debris from the polishing layer was collected using only conditioner and deionized water (DIW).

[0182] The platen speed was set to 93 rpm, the conditioner load was 9 lb, the rotation speed was 64 rpm, the sweep speed was 19 times / min, deionized water was injected at 300 cc / min, and the disk was set to CI45, and the polishing layer was conditioned. The debris of the polishing layer generated during conditioning was collected in a solution state mixed with deionized water, and after storing for 24 hours, the supernatant liquid located within 10 mm from the upper surface of the solution was taken as a sample. The obtained sample was approximately pH 6.5 level, and the pH was adjusted to 5.5 using nitric acid and potassium hydroxide. At this time, the concentration of the nitric acid aqueous solution used was 35%, and the concentration of the potassium hydroxide aqueous solution used was 10%. The debris concentration in the liquid phase sample was confirmed to be about 0.01% by weight. The concentration was measured using a heating type moisture meter (MX-50, AND Co.) after placing about 5 g of the liquid phase sample in an aluminum dish.

[0183] The zeta potential of the sample was measured using a Zetasizer (Nano-ZS90, Malvern). Specifically, 1 mL of the sample was placed in a Zetasizer cuvette and the measurement was repeated three times to obtain the zeta potential. At this time, the instrument settings were set to RI 1.550 and Absorption 0.010 based on the polyurethane value. The test results are summarized in the table below.

[0184] JPEG2024152644000004.jpg100164

[0185] As can be seen from the table, the polishing pads of Examples 1 to 7 were measured to have a chlorine (Cl) content within a preferred range, and performance such as removal rate was at a level equal to or higher than that of Comparative Examples 1 and 2. In particular, the debris size of the polishing pads of Examples 1 to 7 was measured to be smaller than that of Comparative Examples 1 and 2, and the number of defects / scratches was measured to be significantly smaller. Furthermore, the zeta potential of the polishing pads of Examples 1 to 7 was also measured to be within a preferred range. [Explanation of symbols]

[0186] 100: Polishing pad 110: Polishing layer (sample) 130: Solid phase blowing agent 131: Hull 132: Expansion-inducing component 150: Debris 200: Platen 300: Conditioner 400: Abrasive slurry 510: Polishing head 520: Career 600: Semiconductor substrate (wafer) 650: Defect 700: Apparatus for measuring the chlorine content of polishing pads 710: Injection gas (Ar / O2) 730: Combustion tube 750: Electric furnace 770: Adsorption tube 790: Valve for transferring to ion chromatography

Claims

1. A polishing pad comprising a polishing layer and a support layer, The polishing layer includes a urethane-based prepolymer, a foaming agent, and a curing agent, The polishing pad has a chlorine (Cl) content of 10,000 ppm or less when the polishing layer is analyzed based on the IEC 62321-3-2 standard.

2. 2. The polishing pad according to claim 1, wherein the polishing layer has a chlorine (Cl) content of 10 ppm to 1000 ppm as analyzed based on IEC 62321-3-2 standard.

3. The blowing agent comprises a solid phase blowing agent; The polishing pad according to claim 1, wherein the solid-phase foaming agent comprises at least one selected from the group consisting of acrylonitrile-based copolymers, methyl methacrylate-based copolymers, methacrylonitrile-based copolymers, and acrylic-based copolymers.

4. The curing agent is 2. The polishing pad according to claim 1, comprising one or more selected from the group consisting of diethyltoluenediamine (DETDA), 3,5-dimethylthio-2,6-diaminotoluene (DMTDA), 1,3-propanediol bis(4-aminobenzoate) (PDPAB), N,N'-bis(sec-butylamino)diphenylmethane, 2,6-bis(methylthio)-4-methyl-1,3-benzenediamine, 4-(4-aminobenzoyl)oxyphenyl 4-aminobenzoate, 4-(4-aminobenzoyl)oxybutyl 4-aminobenzoate, 4-[4-(4-aminobenzoyl)oxy-3-methylbutoxy]butyl 4-aminobenzoate, and methylene bis-methylanthranilate (MBNA).

5. The polishing layer is Hardness of 50 Shore D to 65 Shore D; 15N / mm 2 ~25N / mm 2 and a tensile strength of 2. The polishing pad of claim 1, having an elongation of 90% to 130%.

6. 2. The polishing pad according to claim 1, wherein the zeta potential value of an aqueous solution of pH 5.5 containing debris obtained by conditioning the polishing layer at a concentration of 0.01% by weight is −10 mV to 30 mV.

7. 2. The polishing pad according to claim 1, wherein the D50 particle size of the polishing pad debris obtained when the polishing pad is conditioned under the conditions of a platen speed of 93 rpm, a conditioner load of 9 lb, a conditioner speed of 64 rpm, and a sweep rate of 19 times / min while supplying 300 cc / min of deionized water is 30 μm or less.

8. 2. The polishing pad according to claim 1, wherein when a silicon oxide layer of a silicon wafer is polished in a ceria slurry using the polishing pad, the polishing rate is 2200 Å / min to 2600 Å / min according to the following mathematical formula 1: [Equation 1] Polishing rate (Å / min)=polished thickness of silicon wafer (Å) / polishing time (min).

9. preparing a polishing pad composition comprising a urethane-based prepolymer, a foaming agent, and a curing agent; Injecting the polishing pad composition into a mold and curing it to produce a polishing layer; and bonding the polishing layer to a support layer. The foaming agent includes a solid-phase foaming agent, and the solid-phase foaming agent includes at least one selected from the group consisting of an acrylonitrile-based copolymer, a methyl methacrylate-based copolymer, a methacrylonitrile-based copolymer, and an acrylic-based copolymer; The curing agent is selected from the group consisting of diethyltoluenediamine (DETDA), 3,5-dimethylthio-2,6-diaminotoluene (DMTDA), 1,3-propanediol bis (4-aminobenzoate) (PDPAB), N,N'-bis (sec-butylamino) diphenylmethane, 2,6-bis (methylthio) -4-methyl-1,3-benzenediamine, 4- (4-aminobenzoyl) oxyphenyl 4-aminobenzoate, 4- (4-aminobenzoyl) oxybutyl 4-aminobenzoate, 4- [4- (4-aminobenzoyl) oxy-3-methylbutoxy] butyl 4-aminobenzoate, and methylene bis - methyl anthranilate (MBNA), comprising at least one selected from the group consisting of. The method for producing a polishing pad according to claim 1.

10. 10. A method for manufacturing a semiconductor device, comprising the step of polishing a surface of a semiconductor substrate with the polishing pad of claim 1.

Citation Information

Patent Citations

  • Polishing composition

    JP2021152138A

  • Polishing pad and method for preparing semiconductor device using the same

    JP2022185571A

  • Cmp polishing pad

    JP2023008827A

  • KR2016-0027075