Sheath material for power storage devices

The exterior material for power storage devices uses mixed particles with specified sizes and a lubricant to enhance moldability by reducing contact area and ensuring consistent slip properties, addressing issues of slipperiness and delamination in conventional materials.

JP2024153434AActive Publication Date: 2024-10-29LISSENOK PACKAGING CO LTD

Patent Information

Application Number
JP2023067332
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Conventional exterior materials for power storage devices suffer from unstable moldability due to variations in slipperiness and delamination, especially at right-angle corners, and inconsistent slip properties over the entire surface.

Method used

The exterior material incorporates a heat-sealing layer with mixed particles of different volume average particle diameters, including small, medium, and large incompatible particles, specified weight content, and a lubricant, to create uniform convex portions that reduce contact area with molds, enhancing slipperiness and moldability.

Benefits of technology

The solution provides stable and good moldability by dispersing particles uniformly, reducing contact area, and ensuring consistent slip properties, resulting in high-quality power storage devices with improved operational reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153434000001_ABST
    Figure 2024153434000001_ABST
Patent Text Reader

Abstract

To provide a sheath material for power storage devices improved in moldability.SOLUTION: A sheath material for power storage devices includes a metal foil layer 4, a substrate layer 2 provided at an outer surface side of the metal foil layer 5, and a thermal fusion layer 3 provided at an inner surface side of the metal foil layer 4. A seal layer 31 disposed at an innermost surface side in the thermal fusion layer 3 contains at least two or more kinds of mixed grains of different volume average grain diameters as D50 to be a 50% grain diameter of cumulative distribution in granularity distribution measurement using a laser diffraction-scattering method. When counted from a smallest grain diameter in the cumulative distribution of the mixed grains, D10 to be a 10% grain diameter of the cumulative distribution is 2 μm or less and D90 to be a 90% grain diameter of the cumulative distribution is 6 μm or more. Only one peak is included in a range of D10-D90 in the granularity distribution of the mixed grains, and a peak value in the granularity distribution of the mixed grains is 1 μm to 10 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an exterior material for electricity storage devices such as batteries and capacitors used in mobile devices such as smartphones and tablet terminals, and batteries and capacitors used for storing electricity in hybrid automobiles, electric automobiles, wind power generation, solar power generation, and nighttime electricity. [Background technology]

[0002] In recent years, as mobile devices such as smartphones and tablet terminals become thinner and lighter, a laminate consisting of a heat-resistant resin layer (base material layer) / adhesive layer / metal foil layer (barrier layer) / adhesive layer / thermoplastic resin layer (heat fusion layer) is used as the exterior material of the electric storage device such as lithium ion secondary battery, lithium polymer secondary battery, lithium ion capacitor, and electric double layer capacitor mounted thereon, instead of the conventional metal can. In addition, there is an increasing tendency for the power source of an electric vehicle, a large power source for electric storage, a capacitor, etc. to be exteriorized with a laminate (exterior material) of the above configuration. When forming an exterior material for an electric storage device, the laminate is subjected to cold forming such as stretch forming or deep drawing forming, thereby being formed into a three-dimensional shape such as a substantially rectangular parallelepiped shape. By forming into such a three-dimensional shape, it is possible to secure a storage space for accommodating the main body of the electric storage device. Therefore, in order to secure a highly accurate storage space, it is preferable to improve the formability.

[0003] For example, the exterior packaging material for an electricity storage device shown in Patent Document 1 below ensures good moldability by adding a lubricant to the exposed surface of the inner layer (thermal adhesive layer) to improve slipperiness.

[0004] In addition, the exterior material for an electricity storage device shown in Patent Document 2 below has an appropriate adjustment of the center line average roughness (Ra) and ensures good formability by phase-separating the exposed surface of the heat-sealing layer or adding fine particles to the layer of the exposed surface. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3774163 [Patent Document 2] Patent No. 5380762 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the conventional exterior material for an electrical storage device shown in Patent Document 1, the layer on the exposed surface to which the lubricant is added is a surface layer that is easily transferred, and so the amount of the lubricant varies during use, causing variations in the lubricity and making it impossible to obtain stable, good formability. Furthermore, in places where molding is performed at angles close to a right angle, such as the corners of the molded part, delamination is likely to occur, and from this point of view, good formability cannot be obtained.

[0007] Furthermore, in the conventional exterior material for an electricity storage device shown in Patent Document 2, unevenness such as undulations is required over a wide area of ​​the exposed surface. However, merely adjusting the center line average roughness (Ra) improves slipperiness partially, but it is not possible to obtain consistent slipperiness over the entire area, and there is a problem in that stable and good formability cannot be obtained.

[0008] The present invention has been made in view of the above problems, and has an object to provide an exterior material for an electricity storage device that can obtain stable and excellent formability. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention comprises the following means.

[0010] [1] An exterior material for an electricity storage device, comprising a metal foil layer, a resin base layer provided on the outer surface side of the metal foil layer, and a thermoplastic resin heat-sealing layer provided on the inner surface side of the metal foil layer, The seal layer disposed on the innermost side of the heat-sealing layer contains at least two or more kinds of mixed particles having different volume average particle diameters as D50, which is the 50% particle diameter of a cumulative distribution in particle size distribution measurement by a laser diffraction scattering method, In the cumulative distribution of the mixed particles, counting from the smaller particle size, D10, which is the 10% particle size of the cumulative distribution, is 2 μm or less, and D90, which is the 90% particle size of the cumulative distribution, is 6 μm or more, The particle size distribution of the mixed particles includes only one peak in the range of D10 to D90, The exterior material for an electricity storage device, wherein the mixed particles have a peak value in particle size distribution of 1 μm to 10 μm.

[0011] [2] The mixed particles include small particles, medium particles, and large particles, which are incompatible particles having three different volume average particle sizes, The small particles have a volume average particle size of 0.05 μm to 5 μm, The medium particles have a volume average particle size of 3 μm to 8 μm, 2. An exterior material for an electricity storage device according to item 1, wherein the large particles have a volume average particle diameter of 7 to 15 μm.

[0012] [3] The exterior material for an electricity storage device according to item 1 or 2, wherein the sealing layer has a weight content of the mixed particles of 3,000 ppm to 20,000 ppm.

[0013] [4] The exterior packaging material for an electricity storage device according to any one of items 1 to 3 above, wherein the sealing layer has a thickness of 5 μm or more.

[0014] [5] The exterior material for an electricity storage device according to any one of items 1 to 4 above, wherein the mixed particles have an aspect ratio of 0.2 to 1.

[0015] [6] The exterior packaging material for an electricity storage device according to any one of items 1 to 5 above, wherein the sealing layer contains a lubricant.

[0016] [7] An exterior packaging material for an electricity storage device according to any one of items 1 to 6 above, which satisfies the relational formula (D90-D10) / D50=0.5 to 5.

[0017] [8] A film used in a heat-sealing layer in the exterior material for an electricity storage device according to any one of items 1 to 7, A film for a heat-sealing layer of an exterior material for an electrical storage device, wherein a portion corresponding to the sealing layer is constituted by a resin layer containing the mixed particles.

[0018] [9] A method for producing a film used for a heat-sealing layer in the exterior material for an electricity storage device according to any one of items 1 to 7, comprising the steps of: A method for producing a film for a heat-sealing layer of an exterior material for an electrical storage device, characterized in that a portion corresponding to the sealing layer is formed by a resin layer containing the mixed particles.

[0019]

[10] A main body of an electricity storage device; The packaging material according to any one of items 1 to 7, A power storage device, characterized in that the power storage device main body is exteriorly covered with the exterior material. Effect of the Invention

[0020] According to the exterior material for an electricity storage device of the invention [1], mixed particles with different particle sizes are added to the sealing layer on the inner side of the heat-sealing layer, so that it is possible to form large and small convex parts. Furthermore, since the mixed particles can be measured as particles having one peak within the conditions at a certain particle size distribution width in the particle size distribution measurement results, the mixed particles are less likely to aggregate, and each particle is dispersed on the inner surface of the heat-sealing layer to form convex parts without bias. This reduces the contact area with the molding tool such as a mold during molding, improves the slipperiness, and provides stable and good moldability.

[0021] According to the exterior packaging material for an electricity storage device of invention [2], the sealing layer contains small, medium and large particles with specific particle sizes, which makes it easier to blend mixed particles with the desired particle size distribution, and allows the desired unevenness to be formed on the inner surface of the heat-sealing layer. This makes it possible to further reduce the contact area with the molding tool during molding, thereby further improving moldability.

[0022] According to the exterior packaging material for an electricity storage device of the invention [3], the content of the mixed particles in the sealing layer is specified, so that the mixed particles can be appropriately dispersed and arranged in a well-balanced manner within the sealing layer, and the desired unevenness can be formed on the inner surface of the heat-sealing layer, thereby further improving moldability.

[0023] According to the exterior packaging material for an electricity storage device of invention [4], the thickness of the sealing layer is specified, so that the mixed particles can be firmly fixed to the sealing layer in a stable state, and defects such as the mixed particles falling off can be prevented, thereby more reliably improving the moldability.

[0024] According to the exterior packaging material for an electricity storage device of the invention [5], the aspect ratio of the mixed particles is specified, so that convex portions can be formed sufficiently regardless of the direction in which the mixed particles are tilted, and falling off is less likely to occur, thereby further improving formability.

[0025] According to the exterior packaging material for an electricity storage device of invention [6], since the sealing layer contains a lubricant, when the temperature reaches or exceeds a certain level, the lubricant precipitates and appears on the inner surface of the heat-sealing layer, thereby further improving the lubricating properties and further improving the formability.

[0026] According to the exterior packaging material for an electricity storage device of invention [7], the relationship of (D90-D10) / D50=0.5 to 5 is satisfied, so that the volume distribution of the mixed particles can be made broader with greater certainty, and the moldability during molding can be further improved.

[0027] According to the film for a heat-sealing layer of the exterior packaging material for an electricity storage device of the invention [8], the exterior packaging material of the above invention can be reliably produced using the film.

[0028] According to the method for producing a film for a heat-sealing layer of an exterior material for an electricity storage device of the invention [9], the exterior material of the invention can be reliably produced.

[0029] According to the invention

[10] , since the exterior material has excellent sliding properties against a molding jig, a high-quality electricity storage device with high operational reliability can be provided. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a cross-sectional view showing an exterior material for an electricity storage device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating a heat seal layer of an exterior material for an electricity storage device according to an embodiment. [Diagram 3] FIG. 3 is a graph showing the particle size distribution of each particle and the entire mixed particle in the embodiment. [Figure 4] FIG. 4 is a graph showing the particle size distribution and cumulative distribution of mixed particles in an embodiment. [Diagram 5] FIG. 5 is a graph for explaining a peak value in the particle size distribution of mixed particles in the embodiment. [Figure 6] FIG. 6 is a schematic cross-sectional view for explaining a seal layer in which a lubricant is precipitated in the heat-sealing layer of the embodiment. [Figure 7] FIG. 7 is a cross-sectional view showing an electricity storage device produced using the exterior material of the embodiment. [Figure 8] FIG. 8 is an exploded perspective view of the electricity storage device according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Fig. 1 is a cross-sectional view showing an exterior material for an electricity storage device according to an embodiment of the present invention. As shown in the figure, the exterior material for an electricity storage device 1 includes a metal foil layer 4 made of metal foil, a base layer 2 made of heat-resistant resin provided on the outer surface side of the metal foil layer 4 and serving as an outer layer, an adhesive layer 5 provided on the inner surface side of the metal foil layer 4, and a heat-sealing layer (sealant layer) 3 made of heat-sealing resin and serving as an inner layer provided on the inner surface side of the adhesive layer 5.

[0032] In this specification, when describing the position of each layer constituting the battery packaging material in terms of a direction (upward in Figure 1), the direction of the base material layer 2 is referred to as the outside, and the direction of the heat-sealing layer 3 (downward in Figure 1) is referred to as the inside.

[0033] The base layer 2 is preferably made of a polyamide resin, a polyester resin, a polyolefin resin, a polyimide resin, or the like, and can be formed as a coating film or a film. The base layer 2 is preferably made of a biaxially oriented film of the above resin, and is preferably made of a biaxially oriented polyamide film or a biaxially oriented polyester film. Among these, the biaxially oriented polyamide film is not particularly limited, but biaxially oriented nylon 6 film, biaxially oriented nylon 6,6 film, biaxially oriented MXD nylon film, or the like can be preferably used, and the polyester film is preferably made of a biaxially oriented polybutylene terephthalate (PBT) film, biaxially oriented polyethylene terephthalate (PET) film, biaxially oriented polyethylene naphthalate (PEN) film, or the like.

[0034] As the heat-resistant resin constituting the base layer 2, it is preferable to use a thermoplastic resin having a temperature of 10° C. or higher, and more preferably a thermoplastic resin having a temperature of 20° C. or higher, relative to the heat-sealing resin constituting the heat-sealing layer 3. The thickness of the base layer 2 is preferably set to 9 μm to 50 μm.

[0035] The metal foil layer 4 may be made of a single metal foil such as aluminum (Al) foil, copper (Cu) foil, stainless steel (SUS) foil, titanium (Ti) foil, or nickel (Ni) foil, or may be a clad material made by bonding two or more metals together. The thickness of the metal foil layer 4 is preferably set to 20 μm to 150 μm. That is, if the thickness is too thin, there is a risk of reduced durability due to pinholes, and conversely, if the thickness is too thick, there is a risk of reduced formability.

[0036] It is preferable to form an undercoat layer on at least one of the inner and outer surfaces of the metal foil layer 4, particularly on the surface on the thermal adhesive layer 3 side (inner surface).

[0037] The underlayer can be formed by carrying out a coating treatment of a silane coupling agent, a chemical conversion treatment such as a chromate treatment, etc. The thickness of the underlayer is preferably set to 0.01 μm to 1 μm.

[0038] By forming the undercoat layer in this manner, the corrosion resistance of the metal foil layer 4 can be improved, and the adhesive strength with the adhesive layer 5 provided on the inner surface can be improved, thereby effectively preventing peeling of the adhesive layer 5.

[0039] When the base layer is formed by a coating by chemical conversion treatment (chemical conversion coating), the chemical conversion coating may be selected depending on the combination with the adhesive layer 5. For example, a coating by chromic acid treatment, a coating by chromate phosphate treatment, a coating by zinc phosphate treatment, a coating by a non-chromate treatment in which zirconium or titanium is used as a metal component instead of Cr, or an oxide coating by boehmite treatment can be suitably used.

[0040] The above-mentioned base material layer 2 is attached to the outer surface of this metal foil layer 4, if necessary via an adhesive, for integral lamination.

[0041] An adhesive layer formed of a two-liquid curing adhesive can be suitably used as an adhesive for bonding the base layer 2 and the metal foil layer 4, and as an adhesive between films when the base layer 2 is formed of a plurality of films. For example, a two-liquid curing adhesive composed of a first liquid (base agent) made of one or more polyols selected from the group consisting of polyurethane polyols, polyester polyols, polyether polyols, and polyester urethane polyols, and a second liquid (curing agent) made of isocyanate can be used. The thickness of this adhesive is preferably set to 2 μm to 5 μm.

[0042] The adhesive layer 5 provided on the inner surface of the metal foil layer 4 may be an adhesive containing one or more of polyurethane resin, acrylic resin, epoxy resin, polyolefin resin, elastomer resin, fluorine resin, and acid-modified polypropylene resin, and among them, it is particularly preferable to use an adhesive made of a polyurethane composite resin containing acid-modified polyolefin as a main component. The thickness of the adhesive layer 5 is preferably set to 2 μm to 5 μm.

[0043] The adhesive layer 5 may be formed by heat lamination using a modified polyolefin (for example, acid-modified polypropylene). In this case, the preferred thickness is 10 μm to 30 μm.

[0044] Examples of the thermoplastic resin constituting the heat-sealing layer 3 include polyethylene-based resins such as LDPE (low density polyethylene), LLDPE (linear low density polyethylene), HDPE (high density polyethylene), and polyethylene-based copolymers, polypropylene-based resins such as rPP (random polypropylene), bPP (block polypropylene), hPP (homopolypropylene), and polypropylene-based copolymers, polybutene-based copolymers, and ionomers. Among them, polypropylene-based resins are preferably used because of their electrolyte resistance, water resistance, and oxygen barrier resistance. In addition, from the viewpoint of handling, it is preferable that the resin is in the form of a film, and it is particularly preferable to use a non-oriented polypropylene film such as CPP (cast polypropylene) or IPP (inflation polypropylene).

[0045] Fig. 2 is a cross-sectional view showing the heat-sealing layer 3 in the packaging material 1 of this embodiment. As shown in Fig. 1 and Fig. 2, in this embodiment, the heat-sealing layer 3 is composed of a three-layer laminate including a sealing layer 31 arranged on the innermost side, an outer layer 33 also called a metal foil side layer, a laminate layer, etc. arranged on the outermost side, and an intermediate layer 32 arranged between the sealing layer 31 and the outer layer 33.

[0046] In the present invention, the thermal adhesive layer 3 is not limited to three layers, and may be a single layer, two layers, or four or more layers. However, in the present invention, when the thermal adhesive layer 3 has a laminated structure, it is easier to form a desired laminated structure when the thermal adhesive layer 3 has multiple layers.

[0047] In addition, in the present invention, it is not necessarily necessary to change the resin for each layer. For example, the resin of the innermost layer to which mixed particles are added and the resin of an adjacent layer to which mixed particles are not added may be the same type of resin, and the sealing layer 31, intermediate layer 32, and outer layer 33 may be constructed using this same type of resin.

[0048] As described above, the film for the heat-sealing layer 3 may be a single layer or a multi-layer, but considering the heat sealability, delamination resistance, and insulation, it is preferable to form it from a multi-layer film such as a co-extruded product. For example, in this embodiment, a three-layer co-extruded CPP film in which an rPP layer is arranged on both sides of an hPP layer or a bPP layer can be suitably used. In the heat-sealing layer 3 made of this three-layer co-extruded CPP film, the middle hPP layer or bPP layer is configured as the middle layer 32, one of the rPP layers on both sides (inner and outer surfaces) is configured as the seal layer 31, and the other rPP layer is configured as the outer layer 33.

[0049] In this embodiment, the thickness of the entire heat-sealing layer 3 is preferably set to 20 μm to 120 μm. The thickness of the sealing layer 31 is preferably set to 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. In other words, when the thickness of the sealing layer 31 is specified within this range, the mixed particles contained in the sealing layer 31, which will be described later, can be reliably held in a stable state in the sealing layer, and problems such as the mixed particles falling off can be reliably prevented.

[0050] In this embodiment, the sealing layer 31 contains, as mixed particles, three types of particles M1 to M3 that are incompatible particles, that is, incompatible particles having immiscibility.

[0051] As the mixed particles M1 to M3, metal oxides, resin beads, etc. can be used. Specific examples that can be suitably used include silica, alumina, calcium carbonate, barium carbonate, titanium oxide, aluminum silicate, talc, kaolin, acrylic resin beads, polyethylene resin beads, and polyethylene elastomers. It is preferable that the particles M1 to M3 are made by combining two or more types of the above-mentioned particles. By using particles of two or more different compositions, the mixed particles are less likely to aggregate due to van der Waals forces, and the mixed particles can be dispersed in the seal layer 31 to form appropriate unevenness.

[0052] The content of the mixed particles M1 to M3 in the sealing layer 31 is preferably set to 3000 ppm to 20000 ppm, more preferably 7000 ppm to 18000 ppm, by weight. In other words, when the content of the mixed particles M1 to M3 is set within this range, the mixed particles M1 to M3 can be appropriately dispersed and arranged in a well-balanced manner in the sealing layer 31, and desired irregularities can be formed on the inner surface of the heat-sealing layer 3.

[0053] In this embodiment, the mixed particles (incompatible particles) contained in the sealing layer 31 are composed of three types of particles with different volume average particle diameters (median diameters), which are the 50% particle diameter D50 of the cumulative distribution, namely small particles M1, medium particles M2, and large particles M3.

[0054] The sealing layer 31, which contains small particles M1, medium particles M2 and large particles M3 of different sizes, is arranged so that a portion of each particle M1 to M3 protrudes inward (downward in the figures) from the inner surface (the lower surface in Figures 1 and 2) of a resin component such as rPP, and the inner surface of the sealing layer 31 is uneven.

[0055] The small particles M1 preferably have a volume average particle size (D50) of 0.05 μm to 5 μm, and more preferably 0.5 μm to 3 μm.

[0056] As the medium particles M2, those having a volume average particle size (D50) of 3 μm to 8 μm are preferably used, and those having a volume average particle size (D50) of 4 μm to 7 μm are more preferably used.

[0057] The large particles M3 preferably have a volume average particle size (D50) of 7 μm to 15 μm, and more preferably 8 μm to 13 μm.

[0058] In this embodiment, the sealing layer 31 contains three types of particles M1 to M3 with different particle diameters D50. The small particles M1 and large particles M3 broaden the particle size distribution, and the medium particles M2 combine them into a single distribution. This contributes to the formation of unevenly sized protrusions by dispersing particles of each size throughout the entire material, thereby reducing the contact area with a mold such as a molding jig when molding the exterior material 1, improving slipperiness, and achieving stable and favorable moldability.

[0059] If particles of the same size are mixed rather than particles of different sizes, the size of the protrusions will be uniform, which may result in a monotonous surface shape, resulting in reduced slipperiness and formability, or the protrusions may imprint on the exterior material 1.

[0060] Furthermore, in this embodiment, the small particles M1 can form fine irregularities on the surface (inner surface) of the heat-sealing layer 3, which can suppress adhesion to a mold when molding the exterior packaging material 1.

[0061] Furthermore, the large particles M3 ensure the formation of convex portions (protrusions) on the inner surface of the heat-sealing layer 3, making it possible to reduce the kinetic frictional force with a die when molding the exterior packaging material 1.

[0062] Furthermore, the medium particles M2 form small protrusions on the inner surface of the heat-sealing layer 3 and prevent the protrusions from being biased, thereby further enhancing the effects of the small particles M1 and the large particles M3.

[0063] Furthermore, in this embodiment, by specifying the particle size (D50) of each of the particles M1 to M3 within the above range, it becomes easier to blend mixed particles having a desired particle size distribution, and the desired unevenness can be formed on the inner surface of the heat-sealing layer 3. This makes it possible to further reduce the contact area with the mold during molding of the exterior packaging material 1, thereby further improving moldability.

[0064] Furthermore, in this embodiment, when the content of the mixed particles is specified within the above range, or when the thickness of the sealing layer 31 is specified within the above range, it is possible to prevent each particle from falling off from the sealing layer 31, and the effect of the convex portions can be fully exerted, so that good moldability can be obtained more reliably.

[0065] In this embodiment, the blending ratio (weight ratio) of large particles M3:medium particles M2:small particles M1 is preferably adjusted to 0.5-1.5:1-3:0.5-1.5, and more preferably adjusted to 0.8-1.2:1.5-2.5:0.8-1.2. In other words, by adjusting the blending ratio within this range, the above-mentioned effects due to the blending of particles M1-M3 can be obtained more reliably.

[0066] 3 is a graph showing the particle size distribution of each of the small particles M1, the medium particles M2, and the large particles M3 in this embodiment, and the particle size distribution of a mixed particle obtained by mixing the small particles M1, the medium particles M2, and the large particles M3. As shown in the figure, the small particles M1 and the medium particles M2 have smaller particle diameters than the large particles M3, so when mixed in the same blending amount (weight or volume) as the large particles M3, the particle amount (number of particles), which is the amount present in the particle size distribution, becomes larger.

[0067] In the present invention, the particle size distribution and cumulative distribution are measured based on the laser diffraction method (laser diffraction scattering method).

[0068] In this embodiment, the mixed particles are described by taking three types of particles M1 to M3 with different volume average particle diameters (D50) as an example, but the present invention is not limited thereto. As long as the mixed particles satisfy the conditions of particle size distribution, at least two types of particles with different volume average particle diameters (D50) may be used as the mixed particles. For example, the mixed particles may be made of two types of particles, small particles M1 and medium particles M2, or small particles M1 and large particles M3. Furthermore, the mixed particles may be formed using four or more types of particles with different volume average particle diameters (D50).

[0069] 4 is a graph showing the particle size distribution and cumulative distribution of the mixed particles in this embodiment. As shown in the figure, the particle size distribution of the mixed particles, counting from the smaller particle size, includes only one peak (mountain part) within the range of 10% particle size (D10) to 90% particle size (D90) of the cumulative distribution, and there are no two or more peaks within that range.

[0070] Here, in the present invention, the particle size distribution of the mixed particles includes only one peak within the range of D10 to D90, and even if there is a peak outside the range of D10 to D90, the peak outside the range is irrelevant to the present invention. For example, in the particle size distribution in Figure 5, a peak exists at a position below D10, but this peak is not counted in the present invention. In other words, the particle size distribution in the figure includes only one peak within the range of D10 to D90, and is the subject of the present invention.

[0071] In this embodiment, in the cumulative distribution of the mixed particles, the D10 particle size is 2 μm or more and the D90 particle size is 6 μm or more. Furthermore, in this embodiment, the mode diameter as a peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.

[0072] In this embodiment, the particle diameters D10 and D90 and the mode diameter are specified to the above values, so that the mixed particles as a whole can have one broad distribution that is not sharp, and the convex portions of the particles M1 to M3 can be formed uniformly and without bias on the inner surface of the heat-sealing layer 3. Therefore, when molding the exterior material 1, stress concentration on the mold is unlikely to occur, improving the slipperiness and further increasing the moldability.

[0073] In this embodiment, it is preferable to satisfy the relationship of (D90-D10) / D50 = 0.5 to 5, and more preferably the relationship of (D90-D10) / D50 = 1.5 to 3. In other words, when this relationship is satisfied, the volume distribution of the mixed particles as a whole can be more reliably made broad, and irregularities of various sizes can be provided, thereby further improving the moldability when molding the exterior packaging material 1.

[0074] Furthermore, in this embodiment, it is preferable to employ particles M1 to M3 constituting the mixed particles each having an aspect ratio (minor axis / major axis) of 0.2 to 1. In other words, in this case, since the particles form a certain amount of clumps, convex portions can be sufficiently formed no matter in which direction the particles M1 to M3 are inclined, and falling off is unlikely to occur, so that the moldability can be improved more reliably when molding the exterior packaging material 1.

[0075] In this embodiment, it is preferable that the seal layer 31 of the heat-sealing layer 3 contains a lubricant.

[0076] Examples of the lubricant include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylol amides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides.

[0077] More specifically, examples of saturated fatty acid amides include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide.

[0078] Further, examples of the unsaturated fatty acid amide include oleic acid amide and erucic acid amide.

[0079] Further, examples of the substituted amide include N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, and N-stearyl erucic acid amide.

[0080] Further, the methylol amide may, for example, be methylol stearic acid amide.

[0081] Further examples of saturated fatty acid bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipic acid amide, and N,N'-distearyl sebacic acid amide.

[0082] Further, examples of unsaturated fatty acid bisamides include ethylene bisoleamide, ethylene biserucamide, hexamethylene bisoleamide, N,N'-dioleyl adipamide, and N,N'-dioleyl sebacamide.

[0083] Further, an example of the fatty acid ester amide is stearamide ethyl stearate.

[0084] Examples of aromatic bisamides include m-xylylene bisstearic acid amide, m-xylylene bishydroxystearic acid amide, and N,N'-cystearylisophthalic acid amide.

[0085] The amount of lubricant deposited on the inner surface of the heat-sealing layer 3 is 0.1 μg / cm 2 ~1μg / cm2 (0.1μg / cm 2 and 1 μg / cm 2 It is preferable to adjust the lubricant amount to 0.05 to 0.05% (including the amount of lubricant precipitated). If the amount of lubricant precipitated is too small, it is likely that good slip properties cannot be obtained, which is not preferable. Conversely, if the amount of lubricant precipitated is too large, it is likely that the frequency of occurrence of white powder and equipment contamination due to the lubricant increases, which is not preferable.

[0086] As shown in FIG. 6, the inner surface of the heat-sealing layer 3 is formed into an uneven structure by the particles M1 to M3, so that excessive precipitation of the lubricant on the inner surface of the heat-sealing layer 3 is suppressed, and at a predetermined temperature or higher, an appropriate amount of lubricant is precipitated, and the inner surface of the heat-sealing layer 3 is covered with a lubricant layer 6 of the lubricant, thereby further improving the slipperiness against the molding jig.

[0087] Furthermore, when the packaging material 1 of this embodiment is wound up, for example, into a roll, the heat-sealing layer 3 comes into contact with the outermost layer, such as the base layer 2, and the positions of the convex portions of each of the particles M1 to M3 are preferentially brought into contact with other parts (such as the base layer 2), thereby suppressing the amount of lubricant transferred to other parts.

[0088] In the present invention, in order to further improve the slipperiness during molding, a substrate protective layer formed of a binder resin containing fine particles may be provided on the outer side of the substrate layer 2. As the fine particles, the incompatible particles used as the mixed particles in this embodiment may be used, and as the binder resin, a urethane resin, an acrylic resin, an acrylic urethane resin, a fluorine resin, etc. may be used.

[0089] The exterior material 1 for an electricity storage device of this embodiment configured as described above is used as an exterior case for an electricity storage device either in sheet form or, if necessary, formed into a predetermined shape by thermoforming such as deep drawing or stretch forming.

[0090] For example, Fig. 7 and Fig. 8 are a cross-sectional view and an exploded perspective view showing an electricity storage device 30 manufactured using the exterior material 1 of this embodiment. As shown in both figures, this electricity storage device 30 is a lithium ion secondary battery. In this embodiment, an exterior case 15 is configured by a tray member 14 obtained by molding the exterior material 1 and a lid member 10 configured by a planar (sheet-shaped) exterior material 1. Thus, an electricity storage device main body part (electrochemical element, etc.) 35 having a substantially rectangular parallelepiped shape is accommodated in the accommodation recess of the tray member 14 obtained by molding the exterior material 1 of the present invention, and the lid member 10 (exterior material 1) of the present invention is placed on the electricity storage device main body part 35 with its heat fusion layer 3 side facing inward (lower side), and the outer peripheral edge part of the heat fusion layer 3 of the lid member 10 and the heat fusion layer 3 of the flange part (sealing peripheral part) 29 of the tray member 14 are sealed and joined by heat sealing to form a electricity storage device 30. The inner surface of the accommodating recess of the tray member 14 is the heat-sealing layer 3, and the outer surface of the accommodating recess faces the base layer 2.

[0091] 7, reference numeral "39" denotes a heat seal portion at which the outer peripheral edge of the cover member 10 and the flange portion (sealing peripheral portion) 29 of the tray member 14 are joined (welded) to each other. Note that in the electricity storage device 30, the tip of a tab lead connected to the electricity storage device main body 35 is led out to the outside of the exterior case 15, but is not shown in the figure.

[0092] The energy storage device 30 manufactured using the exterior material 1 of this embodiment has an exterior material 1 that has excellent slip resistance against a molding die and has high adhesive strength between the heat-sealing layer 3 and the adhesive layer 5, and therefore has high operational reliability and can reliably provide a high-quality energy storage device product.

[0093] The power storage device main body 35 is not particularly limited, but examples thereof include a battery main body, a capacitor main body, and a condenser main body.

[0094] In the above embodiment, the exterior case 15 is composed of a tray member 14 obtained by molding the exterior material 1 and a planar lid member 10, but the present invention is not limited to such a combination. For example, the exterior case 15 may be composed of a pair of planar (sheet-like) exterior materials 1, or may be composed of a pair of tray members 14 stacked opposite each other. EXAMPLES

[0095] [Table 1]

[0096] [Table 2]

[0097] 1. Preparation of film for heat-sealing layer <Example 1> As shown in Tables 1 and 2, a film for the heat-sealing layer 3 of Example 1 in the exterior packaging material 1 for an electricity storage device was produced. That is, as the film for the heat-sealing layer 3, a CPP film was produced in which a 16 μm-thick rPP for the sealing layer, a 48 μm-thick bPP for the intermediate layer, and a 16 μm-thick rPP for the outer layer were laminated by three-layer coextrusion using a T-die.

[0098] In the heat-sealing layer film of Example 1, 3000 ppm of silica particles having an average particle size of 1.5 μm were added to the sealing layer 31 as small particles M1, 6000 ppm of silica particles having an average particle size of 6 μm as medium particles M2, and 3000 ppm of HDPE (high-density polyethylene) particles having an average particle size of 12 μm as large particles M3.

[0099] As shown in Table 2, for the mixed particles M1 to M3 added to the sealing layer 31, the 10% particle size (D10) is 0.8 μm, the 50% particle size (D50) is 3.8 μm, the 90% particle size is 8.2 μm, (D90-D10) / D50 is 1.9, the aspect ratio is 0.8, the number of peaks within the range of D10 to D90 in the volume distribution is one, and the peak position is 4.1 μm.

[0100] The particle size distribution of the mixed particles was measured using the laser diffraction method. Specifically, the device used was a Microtrac MT3000II, the measurement conditions were a measurement range of 0.02μm-2000μm, a measurement time of 30 seconds, two measurements, a solvent of methanol (refractive index 1.33), and particle settings of non-spherical particles (refractive index 1.54).

[0101] The aspect ratio of each particle was measured using FPIA-3000 manufactured by Sysmex Corporation.

[0102] <Examples 2 to 17> The resins for the seal layer, intermediate layer and outer layer shown in Tables 1 and 2 were laminated in the same manner as in Example 1 above to prepare films for the heat-sealing layer of Examples 2 to 17.

[0103] <Examples 18 and 19> Using the resins for the seal layer shown in Tables 1 and 4, single-layer unstretched films were produced using a T-die to prepare the heat-sealable films of Examples 18 and 19.

[0104] <Comparative Examples 1 to 4> A film for a heat-sealing layer was prepared by laminating the resins for the sealing layer, intermediate layer, and outer layer shown in Tables 1 and 2 in the same manner as in Example 1. In the mixed particles of Comparative Example 1, the number of peaks in the range of D10 to D90 of the volume distribution was two, and the respective peak positions were 1.9 μm and 9.3 μm.

[0105] 2. Preparation of exterior materials for energy storage devices A chemical conversion coating was formed by applying a chemical conversion solution consisting of phosphoric acid, polyacrylic acid (acrylic resin), a chromium (III) salt compound, water, and alcohol to both sides of a 40 μm-thick aluminum foil (A8021-O) as the metal foil layer 4, and then drying at 180° C. The chromium deposition amount of this chemical conversion coating was 10 mg / m per side. 2 It was.

[0106] Next, a 15 μm-thick biaxially oriented 6 nylon (ONy) film was dry laminated (attached) to one side (outer side) of the chemically treated aluminum foil (metal foil layer 4) via a two-component curing urethane adhesive (3 μm) as the base layer 2.

[0107] Next, the outer surface of the outer layer of the CPP film for the heat-sealing layer prepared in the above Examples and Comparative Examples was superimposed on the other surface (inner surface) of the aluminum foil (metal foil layer) after the above dry lamination via a two-liquid curing adhesive (2 μm) of maleic acid-modified polypropylene resin and isocyanate, and dry laminated by pressing and sandwiching between a rubber nip roll and a laminating roll heated to 100° C. After that, it was aged at 40° C. for 10 days to obtain the exterior materials (laminates) of the Examples and Comparative Examples as samples.

[0108] 3.Evaluation test for each exterior material

[0109] [Table 3]

[0110] <Moldability test> Each of the exterior packaging materials of the Examples and Comparative Examples was cut into a predetermined size to perform a deep drawing test on the exterior packaging material test pieces, using a deep drawing mold, in an area of ​​55 mm length x 35 mm width, while increasing the forming height (drawing depth) in 0.5 mm increments. The gauge pressure for the wrinkle holding pressure during this forming was 0.475 MPa, and the actual pressure (calculated value) was 0.7 MPa.

[0111] It was visually confirmed using transmitted light whether or not pinholes were formed in the corners of the drawn recess by this molding.

[0112] Then, pinholes were observed when the molding depth was 7 mm or more, and were evaluated as "◎", pinholes were observed when the molding depth was 6 mm or more but less than 7 mm, and were evaluated as "○", pinholes were observed when the molding depth was 5 mm or more but less than 6 μm, and pinholes were observed when the molding depth was less than 5 mm, and were evaluated as "×". In this evaluation, "◎", "○", and "△" were considered to be acceptable in this example. The results are shown in Table 3.

[0113] <Lamination strength (sealing property) test> Each of the exterior materials of the examples and comparative examples was cut into a strip of 15 mm width, and the peel strength between the metal foil layer and the heat-sealing layer was measured according to JIS K6854-3 (1999). The peel strength was evaluated as 4.0 N / 15 mm or more as "◎", 3.0 N / 15 mm or more and less than 4.0 N / 15 mm as "○", 2.0 N / 15 mm or more and less than 3.0 N / 15 mm as "△", and less than 2.0 N / 15 mm as "×". In this evaluation, "◎", "○", and "△" were considered to be acceptable in this example. The results are shown in Table 3.

[0114] <Slipperiness test (dynamic friction coefficient)> Each exterior material of the examples and comparative examples was cut to a size of 80 mm x 200 mm, and the dynamic friction coefficient was measured in accordance with JIS K 7125. The measurement conditions were a low cell weight of 100 N and a weight of 200 g (including the weight of the sliding piece). The results of the dynamic friction coefficient are shown in Table 3.

[0115] <Overall Review> As shown in Table 3, although there was some variation in the results for the exterior materials of the examples, all of the examples were evaluated as having no problems and reached the pass level.

[0116] In contrast, the packaging materials of Comparative Examples 1 to 4, which deviate from the gist of the present invention, were evaluated as being poor in any one of formability, sealability, and slipperiness. [Industrial Applicability]

[0117] The exterior packaging material for an electricity storage device of the present invention can be suitably used when producing electricity storage devices such as batteries and capacitors used in mobile devices such as smartphones and tablets, and batteries and capacitors used for storing electricity in hybrid automobiles, electric automobiles, wind power generation, solar power generation, and night-time electricity. [Explanation of symbols]

[0118] 1: Exterior material 2: Base material layer 3: Heat-sealing layer 30: Energy storage device 31: Sealing layer 35: Device body 4: Metal foil layer 6: Lubricant layer M1: Small particles M2: Medium particle M3: large particles

Claims

1. An exterior material for an electricity storage device, comprising: a metal foil layer; a resin base layer provided on an outer surface side of the metal foil layer; and a thermoplastic resin heat-sealing layer provided on an inner surface side of the metal foil layer, The seal layer disposed on the innermost side of the heat-sealing layer contains at least two or more types of mixed particles having different volume average particle diameters as D50, which is the 50% particle diameter of a cumulative distribution in particle size distribution measurement by a laser diffraction scattering method, In a cumulative distribution of the mixed particles, counting from the smaller particle size, D10, which is a 10% particle size of the cumulative distribution, is 2 μm or less, and D90, which is a 90% particle size of the cumulative distribution, is 6 μm or more, The particle size distribution of the mixed particles includes only one peak in the range of D10 to D90, The outer casing material for an electricity storage device is characterized in that the mixed particles have a peak value in a particle size distribution of 1 μm to 10 μm.

2. The mixed particles include small particles, medium particles, and large particles, which are incompatible particles having three different volume average particle sizes, The small particles have a volume average particle size of 0.05 μm to 5 μm; The medium particles have a volume average particle size of 3 μm to 8 μm, 2. The exterior material for an electricity storage device according to claim 1, wherein the large particles have a volume average particle diameter of 7 to 15 μm.

3. 3. The exterior packaging material for an electricity storage device according to claim 1, wherein the sealing layer has a weight content of the mixed particles of 3000 ppm to 20000 ppm.

4. The packaging material for an electricity storage device according to claim 1 or 2, wherein the sealing layer has a thickness of 5 μm or more.

5. 3. The electrical storage device packaging material according to claim 1, wherein the mixed particles have an aspect ratio of 0.2 to 1.

6. The packaging material for an electricity storage device according to claim 1 or 2, wherein the sealing layer contains a lubricant.

7. The exterior packaging material for an electricity storage device according to claim 1 or 2, which satisfies the relationship (D90-D10) / D50=0.5 to 5.

8. A film used for a heat-sealing layer in the electrical storage device packaging material according to claim 1 or 2, A film for a heat-sealing layer of an exterior material for an electrical storage device, wherein a portion corresponding to the sealing layer is constituted by a resin layer containing the mixed particles.

9. A method for producing a film used for a heat-sealing layer in the exterior material for an electrical storage device according to claim 1 or 2, A method for producing a film for a heat-sealing layer of an exterior material for an electrical storage device, characterized in that a portion corresponding to the sealing layer is formed by a resin layer containing the mixed particles.

10. A power storage device main body; The exterior material according to claim 1 or 2, A power storage device, characterized in that the power storage device main body is exteriorly covered with the exterior material.

Citation Information

Patent Citations

  • Battery pack

    JP2014032966A

  • Sheath material for secondary battery

    JP2017004765A

  • Exterior material for power storage device, outer casing for power storage device and power storage device

    JP2019061938A

  • Sealant film for battery external material

    JP2021103679A

  • Exterior materials for energy storage devices

    JP2023017866A

Cited By

  • Exterior material for power storage device, exterior case for power storage device, and power storage device

    WO2026126911A1