Positive electrode plate for lithium ion secondary battery and lithium ion secondary battery

The lithium ion secondary battery's positive electrode plate uses scale-like carbon nanotube aggregates to enhance heat dissipation and prevent overheating, addressing the insufficiency of conventional carbon nanotubes in dissipating heat, thereby improving overcharge resistance.

JP2024153484APending Publication Date: 2024-10-29TOYOTA BATTERY CO LTD +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023067408
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries face issues with insufficient heat dissipation during overcharging due to the use of carbon nanotubes, which, despite their high thermal conductivity, require a small amount to form an effective conductive network, leading to potential overheating and electrolyte decomposition.

Method used

The positive electrode plate incorporates a fibrous conductive material, specifically carbon nanotubes, formed into scale-like aggregates that do not adhere to the active material, with a planar area of 2.84 μm² or more, thickness of 0.4 μm or less, and porosity of 30% or less, allowing for efficient heat dissipation through increased contact with the non-aqueous electrolyte.

Benefits of technology

This configuration effectively suppresses heat generation and temperature rise on the electrode surface, preventing electrolyte decomposition and enhancing the battery's overcharge resistance, even with a minimal amount of fibrous conductive material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153484000001_ABST
    Figure 2024153484000001_ABST
Patent Text Reader

Abstract

To manufacture a positive electrode plate for a lithium ion secondary battery according to the present invention that can dissipate heat sufficiently even when a small amount of fibrous conductive material is blended.SOLUTION: A positive electrode composite layer 32 of a positive electrode plate 3 of a lithium ion secondary battery includes a positive electrode active material 33 and a fibrous conductive material 34 dispersed on the surface of the positive electrode active material 33, and the fibrous conductive material 34 includes flat scale-like aggregates 35 that are aggregated into scales and are not adhered to the positive electrode active material 33.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode plate for a lithium ion secondary battery and a lithium ion secondary battery, and more particularly to a positive electrode plate for a lithium ion secondary battery and a lithium ion secondary battery that are highly resistant to overcharge. [Background technology]

[0002] Lithium ion secondary batteries have a large capacity and a high voltage, and are therefore used, for example, as driving power sources for electric vehicles, hybrid vehicles, etc. They are also used as stationary batteries in homes and factories. Such lithium ion secondary batteries are required to have even higher output.

[0003] Therefore, in order to improve input and output, it is considered to reduce the reaction resistance by using a positive electrode active material with a high specific surface area. Therefore, the use of a fibrous conductive material to utilize the high specific surface area of ​​the conductive active material can further contribute to reducing the reaction resistance. Such fibrous conductive materials, such as carbon nanotubes (CNTs) and carbon nanofibers (CNFs), can form a conductive network between particles of the positive electrode active material even in small amounts due to their conductivity and shape. As a result, an invention has been disclosed that can increase the ratio of the positive electrode active material in the positive electrode mixture layer.

[0004] For example, Patent Document 1 discloses a fine carbon fiber dispersion in which fine carbon fibers having extremely high cohesive power and in the form of aggregates are uniformly dispersed and defibrated in an organic solvent, and in a stable dispersion state. The use of such fine carbon fibers as an additive for electrode films in the field of secondary battery electrode materials has been proposed. For example, it has been disclosed that fine carbon fibers are mixed with positive electrode active materials such as lithium cobalt oxide and lithium iron phosphate as an additive for positive electrode films of high-output, high-capacity secondary batteries used in hybrid cars and electric cars. The addition of such fine carbon fibers is expected to provide a conductive auxiliary effect, improve the strength of the positive electrode film, increase density, and improve the permeability of the electrode solution. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2012 / 036172 Summary of the Invention [Problem to be solved by the invention]

[0006] Such fibrous conductive materials have the advantage that they can build an effective conductive network even in small amounts due to their high electrical conductivity, and function sufficiently as conductive materials. Carbon nanotubes in particular have high thermal conductivity (3000 to 5500 W / m K), which is also advantageous for heat dissipation.

[0007] However, the positive electrode active material has a large specific surface area, which increases the amount of heat generated during overcharging, making the electrolyte more susceptible to decomposition reactions. However, although carbon nanotubes have high thermal conductivity, as described above, they have high electrical conductivity, so the amount of fibrous conductive material required can be small, which can actually result in insufficient heat dissipation. This can lead to a problem of concern about the deterioration of the so-called overcharge resistance.

[0008] Therefore, the problem that the positive electrode plate for a lithium ion secondary battery and the lithium ion secondary battery of the present invention aim to solve is to produce a positive electrode plate that can dissipate heat sufficiently even when a small amount of fibrous conductive material is used. [Means for solving the problem]

[0009] In order to solve the above problems, the positive electrode plate for a lithium ion secondary battery of the present invention is characterized in that, in a positive electrode mixture layer of the positive electrode plate of a lithium ion secondary battery, it comprises a positive electrode active material and a fibrous conductive material dispersed on the surface of the positive electrode active material, and the fibrous conductive material comprises flat, scale-like agglomerates that are aggregated into scales that are not adhered to the positive electrode active material.

[0010] The planar area of ​​the scale-like aggregate is 2.84 [μm 2] or higher is desirable. It is desirable that the thickness of the scale-like aggregate is 0.39 μm or less. It is desirable that the porosity of the scale-like aggregates be 30% or less.

[0011] The amount of the scale-like agglomerates is preferably 0.04 wt% or more of the entire fibrous conductive material, and is preferably 1.47 wt% or less of the entire fibrous conductive material.

[0012] The length of the fibrous conductive material is desirably 100 nm or more. Also, the length of the fibrous conductive material is desirably 1000 nm or less. The fibrous conductive material is preferably a carbon nanotube.

[0013] The positive electrode active material is desirably lithium nickel cobalt manganese oxide. It is desirable for the lithium ion secondary battery to use the positive electrode plate of this embodiment. Effect of the Invention

[0014] According to the positive electrode plate for a lithium ion secondary battery and the lithium ion secondary battery of the present invention, a positive electrode plate that dissipates heat sufficiently even with a small amount of fibrous conductive material blended therein can be obtained. [Brief description of the drawings]

[0015] [Figure 1] 1 is a perspective view showing an outline of the configuration of a lithium ion secondary battery according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic diagram showing the configuration of a wound electrode body of the present embodiment. [Diagram 3] FIG. 2 is a schematic diagram of the surface of a positive electrode plate according to the present embodiment. [Figure 4] FIG. 1 is a schematic diagram of the surface of a conventional positive electrode plate. [Diagram 5] 4 is a micrograph of the surface of a positive electrode plate according to the present embodiment. [Figure 6]1 is a micrograph of the surface of a conventional positive electrode plate. [Figure 7] 1 is a graph comparing the heat generation rate (maximum) [°C / sec] when the scale-like aggregates of this embodiment are present and when they are not present. [Figure 8] This is a table comparing the rate of change [%] in heat generation rate [°C / sec] depending on the planar area [μm2] of the scaly aggregates. [Figure 9] This is a graph comparing the rate of change [%] in heat generation rate [°C / sec] depending on the planar area [μm2] of the scaly aggregates. [Figure 10] This is a table comparing the rate of change [%] in heat generation rate [°C / sec] due to differences in the ratio of scale-like aggregates (vs. conductive material). [Figure 11] 1 is a graph comparing the rate of change [%] in heat generation rate [°C / sec] due to differences in the ratio of scale-like aggregates (vs. conductive material). [Figure 12] This is a table comparing the rate of change [%] in heat generation rate [°C / sec] depending on the thickness [μm] of the scale-like aggregates. [Figure 13] 1 is a graph comparing the rate of change [%] in heat generation rate [°C / sec] depending on the thickness [μm] of the scale-like aggregates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the positive electrode plate for a lithium ion secondary battery and the lithium ion secondary battery of the present invention will be described with reference to one embodiment of the positive electrode plate 3 of the lithium ion secondary battery 1 with reference to FIGS.

[0017] (Principle of this embodiment) First, the principle of the invention of the positive electrode plate 3 of this embodiment will be described. As described in the prior art, in the positive electrode plate 3 of the lithium ion secondary battery 1 shown in FIG. 3, a fibrous conductive material 34 such as carbon nanotubes or carbon nanofibers is used. In recent years, the specific surface area of ​​the positive electrode active material 33 is increased, and the area in contact with the non-aqueous electrolyte 13 is increased to improve battery performance. In this case, it is desired to form a conductive network that electrically connects the surfaces of the positive electrode active material 33 to each other. The fibrous conductive material 34 is not limited to carbon nanotubes, but carbon nanotubes in particular are used in various applications as a material that has electrical, thermal, mechanical and composite effects. Therefore, in this embodiment, carbon nanotubes are also used as the fibrous conductive material 34. In general, in order to maximize the effect of addition, it is desirable that the carbon nanotubes are uniformly dispersed. Carbon nanotubes that are defibrated into individual strands are subject to a very strong cohesive force (van der Waals force). For this reason, in order to prevent aggregation, they are often distributed in a state where they are defibrated into individual fibers and dispersed in a dispersion medium such as water, an organic solvent, or a resin solution.

[0018] Conventionally, the positive electrode composite paste is produced by kneading the positive electrode active material 33, the fibrous conductive material 34 dispersed in a medium, an organic solvent, and a binder, and then applying the kneaded positive electrode composite paste to the positive electrode current collector 31 and drying it. By producing the positive electrode composite paste in this manner, it is possible to produce a positive electrode composite paste in which the carbon nanotubes are uniformly dispersed.

[0019] In this case, carbon nanotubes, as described above, have excellent electrical conductivity, and because of their fibrous shape, they form an effective conductive network even in small amounts. Therefore, a sufficient conductive network is formed with a smaller amount than with conventional conductive materials.

[0020] Furthermore, if the amount of conductive material can be reduced, the amount of positive electrode active material 33 in positive electrode mixture layer 32 can be relatively increased, which has the advantage that the capacity of positive electrode plate 3 can be increased.

[0021] Incidentally, the lithium ion secondary battery 1 used as the driving power source for electric vehicles and hybrid vehicles may be overcharged due to rapid charging or a large regenerative current. In the overcharged state, the temperature rises on the surface of the positive electrode active material 33 of the positive electrode, causing decomposition of the nonaqueous electrolyte 13, which causes deterioration of the battery. Therefore, the positive electrode plate 3 of this embodiment is designed to suppress such a temperature rise during overcharging.

[0022] 4 is a schematic diagram of the surface of a conventional positive electrode plate 3. In the conventional positive electrode plate 3, dispersed fibrous conductive material 34 is attached to the surface of a positive electrode active material 33. The fibrous conductive material 34 forms a conductive path with adjacent fibrous conductive material 34, forming a conductive network within the positive electrode plate 3.

[0023] On the other hand, overcharging causes a rise in temperature on the surface of the positive electrode active material 33 in contact with the nonaqueous electrolyte 13. In this case, the fibrous conductive material 34 conducts the heat generated from the surface of the positive electrode active material 33 in accordance with the thermal gradient. The fibrous conductive material 34 then dissipates the heat to the nonaqueous electrolyte 13. However, the fibrous conductive material 34 cannot dissipate heat to the nonaqueous electrolyte 13 from the portion of the fibrous conductive material 34 that is in contact with the surface of the positive electrode active material 33. For this reason, the surface area that can dissipate heat to the nonaqueous electrolyte 13 is limited, and the heat dissipation performance is relatively low.

[0024] Fig. 3 is a schematic diagram of the surface of a positive electrode plate 3 of this embodiment. The basic configuration of the positive electrode plate 3 of this embodiment is the same as that of a conventional positive electrode plate 3 shown in Fig. 4. The difference is that the positive electrode plate 3 of this embodiment includes scale-like aggregates 35 formed by agglomeration of fibrous conductive material 34.

[0025] The scale-like aggregates 35 are formed by agglomerating a portion of the fibrous conductive material 34 before the fibrous conductive material 34 is manufactured into a positive electrode mixture paste, to form thin, scale-like (disk-like) plate-like aggregates. Conventionally, attention was focused only on the conductive network, and those skilled in the art paid attention to how to maintain the conductive material in a dispersed state so that it would not aggregate. However, in this embodiment, attention is paid to a viewpoint that was not considered in the past, namely, suppressing the decomposition of the nonaqueous electrolyte 13 due to the temperature rise on the surface of the positive electrode active material 33 during overcharging. This invention is based on knowledge obtained as a result of repeated experiments and research on the fibrous conductive material 34.

[0026] <Basic configuration of this embodiment> <Shape of scale-like aggregate 35> The positive electrode mixture layer 32 of the positive electrode plate 3 of the lithium ion secondary battery 1 of this embodiment includes a positive electrode active material 33 and a fibrous conductive material 34 dispersed on the surface of the positive electrode active material 33. The fibrous conductive material 34 forms a flat scale-like aggregate 35 that aggregates in a scale-like shape and is not in contact with the positive electrode active material 33 for the most part. The term "scale-like" used here is a figurative expression and refers to a shape formed in a generally thin plate shape. The reason for making the aggregate scale-like is that, unlike a fibrous one, it does not stick to the surface of the positive electrode active material 33 and can maintain a separated state. In other words, the contact area of ​​the scale-like aggregate 35 with the nonaqueous electrolyte 13 can be utilized to the maximum.

[0027] < Planar area A of scale-like aggregate 35 [μm 2 ]> Specifically, the planar area A [μm 2 ] is 2.8 [μm 2 In this embodiment, the planar area A [μm 2 ] is the area of ​​the bottom surface perpendicular to one of the thickness directions of the scale-like aggregates 35. In this embodiment, unless otherwise specified, the "average" is the median value (D 50 The "average" of other numerical values ​​is also the same unless otherwise specified. Thus, the planar area A [μm 2 ] is 2.8 [μm 2When the thickness is equal to or greater than 100 nm, the contact area between the scale-like aggregates 35 and the non-aqueous electrolyte 13 can be increased, and heat can be dissipated effectively.

[0028] <Thickness T of scale-like aggregate 35 [μm]> On the other hand, it is desirable that the average thickness T [μm] of the scale-like agglomerate 35 is 0.4 [μm] or less. By forming the scale-like agglomerate 35 to be thin in this manner, the amount of heat stored inside the scale-like agglomerate 35 is reduced, and heat is not trapped inside, allowing heat to be dissipated effectively.

[0029] <Porosity of scale-like aggregate 35 [%]> The porosity [%] of the scale-like agglomerate 35 is preferably 30[%] or less. Here, "porosity [%]" refers to the ratio of the volume of voids to the total volume of the scale-like agglomerate 35. For example, it is measured by optical measurement or mercury intrusion porosimetry. If the porosity [%] of the scale-like agglomerate 35 exceeds 30[%], a sufficient surface area cannot be obtained. Also, a porosity of at least 10[%] is preferable. If the porosity [%] of the scale-like agglomerate 35 is less than 10[%], the flow of the nonaqueous electrolyte 13 becomes poor. As a result, the resistance to ion movement becomes large.

[0030] <Ratio of scale-like aggregates 35 to the entire conductor [wt%]> The amount of the scale-like agglomerates 35 is desirably 0.04 [wt %] or more relative to the entire fibrous conductive material 34. If the amount of the scale-like agglomerates 35 is less than 0.04 [wt %] relative to the entire fibrous conductive material 34, it is difficult to obtain a sufficient heat dissipation effect.

[0031] The amount of the scale-like agglomerates 35 is desirably 1.50 wt% or less with respect to the entire fibrous conductive material 34. If the amount of the scale-like agglomerates 35 exceeds 1.50 wt% with respect to the entire fibrous conductive material 34, the shape of the scale-like agglomerates 35 makes it difficult for them to contribute to the conductive network. Also, the resistance to ion migration increases.

[0032] <Length of fibrous conductive material 34 [nm]> It is desirable that the length of the fibrous conductive material 34 be 100 nm or more. If the length of the fibrous conductive material 34 is less than 100 nm, it is difficult to form a conductive path between adjacent fibrous conductive material 34, making it difficult to form an efficient conductive network.

[0033] It is desirable that the length of the fibrous conductive material 34 be 1000 nm or less. If the length of the fibrous conductive material 34 exceeds 1000 nm, the fibrous conductive material 34 will frequently aggregate into balls due to intermolecular forces and hydrogen bonds between the individual fibrous conductive materials 34. This may make it difficult to ensure sufficient conductivity.

[0034] <Cathode active material 33> In the present invention, the positive electrode active material 33 is not particularly limited, but is particularly suitable for use in granular lithium nickel-cobalt manganese oxide having a large surface area, because it is a material that is prone to oxygen desorption and to generate heat of decomposition.

[0035] (Configuration of this embodiment) <Configuration of lithium-ion secondary battery> First, an example of the overall configuration of a lithium ion secondary battery 1 that is the premise of this embodiment will be briefly described.

[0036] FIG. 1 is a perspective view showing an outline of the configuration of a lithium ion secondary battery 1 of this embodiment. As shown in FIG. 1, the lithium ion secondary battery 1 is configured as a cell battery. The lithium ion secondary battery 1 includes a rectangular parallelepiped battery case 11 having an opening on the upper side. An electrode body 12 is housed inside the battery case 11. A nonaqueous electrolyte 13 is filled into the battery case 11 through a filling hole. The battery case 11 is made of a metal such as an aluminum alloy, and forms a sealed battery container. The lithium ion secondary battery 1 also includes a positive electrode external terminal 14 and a negative electrode external terminal 15 used for charging and discharging power. The shapes of the positive electrode external terminal 14 and the negative electrode external terminal 15 are not limited to those shown in FIG. 1.

[0037] <Electrode body 12> 2 is a schematic diagram showing the configuration of a wound electrode assembly 12. The electrode assembly 12 is formed by winding a large number of negative electrode plates 2 and positive electrode plates 3, with separators 4 arranged between them, flatly. The negative electrode plates 2 have a negative electrode composite layer 22 formed on a negative electrode current collector 21 that serves as a base material. A negative electrode connection part 23 is provided at one end in a width direction W (winding axis direction) perpendicular to the winding direction (winding direction L), where the negative electrode composite layer 22 is not formed and the negative electrode current collector 21 is exposed.

[0038] <Layer structure of electrode body 12> As shown in FIG. 2, an electrode assembly 12 of a lithium ion secondary battery 1 includes a negative electrode plate 2, a positive electrode plate 3, and a separator 4.

[0039] The negative electrode plate 2 includes a negative electrode mixture layer 22 on both sides of a negative electrode current collector 21 serving as a negative electrode base material. One end of the negative electrode current collector 21 serves as a negative electrode connection portion 23 where the metal is exposed. The positive electrode plate 3 includes a positive electrode mixture layer 32 on both sides of a positive electrode current collector 31 serving as a positive electrode base material. The other end of the positive electrode current collector 31 is a positive electrode connection portion 31a where the metal is exposed.

[0040] A laminate is formed by stacking the negative electrode plate 2 and the positive electrode plate 3 with a separator 4 interposed therebetween. This laminate is wound in the longitudinal direction around the winding axis, and formed into a flat wound electrode body 12.

[0041] <Nonaqueous electrolyte 13> As shown in FIG. 1, the nonaqueous electrolyte 13 is filled in a battery container formed by a battery case 11. The nonaqueous electrolyte 13 of the lithium ion secondary battery 1 is a composition in which a lithium salt is dissolved in an organic solvent. Examples of the lithium salt that can be used include LiClO4, LiPF6, LiAsF6, LiBF4, and LiSO3CF3. Examples of the organic solvent include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, and trifluoropropylene carbonate (F.PC), chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and dipropyl carbonate (DPC), ether compounds such as tetrahydrofuran (TFH), 2-methyltetrahydrofuran (2-MeTHF), and dimethoxyethane, sulfur compounds such as ethyl methyl sulfone and butane sultone, and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. The nonaqueous electrolyte solution may be one of these or a mixture of a plurality of these. The composition of the nonaqueous electrolyte solution 13 is not limited to these.

[0042] <Components of electrode body 12> Next, the negative electrode plate 2, the positive electrode plate 3, and the separator 4, which are the components that make up the electrode assembly 12, will be described.

[0043] In this embodiment, unless otherwise specified, the "average diameter" refers to the median diameter (D 50 Average particle size (50% volume average particle size) refers to the average particle size in the range of approximately 1 μm or more, which can be determined by the laser diffraction / light scattering method. In addition, average particle size in the range of approximately 1 μm or less can be determined by the dynamic light scattering (DLS) method. The average particle size based on the DLS method can be measured in accordance with JIS Z 8828:2013.

[0044] <Negative electrode plate 2> The negative electrode plate 2 is constituted by forming a negative electrode mixture layer 22 on both sides of a negative electrode current collector 21, which is a negative electrode base material. In this embodiment, the negative electrode current collector 21 is made of Cu foil. The negative electrode current collector 21 serves as a base for the aggregate of the negative electrode mixture layer 22, and also functions as a current collecting member that collects electricity from the negative electrode mixture layer 22. In this embodiment, the negative electrode active material is a material capable of absorbing and releasing lithium ions, and a powdered carbon material made of graphite or the like is used.

[0045] The negative electrode plate 2 is produced, for example, by kneading a negative electrode active material, a solvent, and a binding material (binder), applying the kneaded negative electrode mixture paste to the negative electrode current collector 21, and drying it. <Positive electrode plate 3> FIG. 3 is a schematic diagram of the surface of the positive electrode plate 3 of this embodiment.

[0046] The positive electrode plate 3 is composed of a positive electrode current collector 31 (FIG. 2) and a positive electrode mixture layer 32 applied thereto. <Positive electrode current collector 31> 2, a positive electrode plate 3 is formed by forming a positive electrode mixture layer 32 on both sides of a positive electrode current collector 31, which is a positive electrode base material. In this embodiment, the positive electrode current collector 31 is made of aluminum foil. The positive electrode current collector 31 serves as a base material for the positive electrode mixture layer 32, and also functions as a current collecting member that collects electricity from the positive electrode mixture layer 32.

[0047] Although the positive electrode base material constituting the positive electrode current collector 31 is exemplified by aluminum foil, it may be made of, for example, a conductive material made of a metal having good electrical conductivity. As the conductive material, for example, a material containing aluminum or a material containing an aluminum alloy may be used. The configuration of the positive electrode current collector 31 is not limited to this.

[0048] <Positive electrode mixture layer 32> 5, positive electrode mixture layer 32 is formed by applying a positive electrode mixture paste to positive electrode current collector 31 and drying it. Positive electrode mixture layer 32 contains, in addition to positive electrode active material 33, fibrous conductive material 34, scaly aggregates 35, and additives such as a binder and a dispersant.

[0049] <Composition of Positive Electrode Active Material 33> The particles of the positive electrode active material 33 contain a lithium transition metal oxide having a layered crystal structure, without being limited to those exemplified in the embodiment. The lithium transition metal oxide contains one or more predetermined transition metal elements in addition to Li. The transition metal element contained in the lithium transition metal oxide is preferably at least one of Ni, Co, and Mn. A suitable example of the lithium transition metal oxide is a lithium transition metal oxide containing all of Ni, Co, and Mn.

[0050] The positive electrode active material 33 may additionally contain one or more elements in addition to a transition metal element (i.e., at least one of Ni, Co, and Mn). Examples of the additional element of the positive electrode active material 33 include any element belonging to Group 1 (alkali metals such as sodium), Group 2 (alkaline earth metals such as magnesium and calcium), Group 4 (transition metals such as titanium and zirconium), Group 6 (transition metals such as chromium and tungsten), Group 8 (transition metals such as iron), Group 13 (metalloid element boron or metals such as aluminum), and Group 17 (halogens such as fluorine) of the periodic table.

[0051] In this embodiment, granular lithium nickel cobalt manganese oxide having a large surface area is used, which is a material that is prone to oxygen desorption and generates heat of decomposition. <Fibrous conductive material 34> The fibrous conductive material 34 is a material for forming a conductive path in the positive electrode mixture layer 32. By mixing an appropriate amount of the fibrous conductive material 34 into the positive electrode mixture layer 32, the conductivity inside the positive electrode can be increased, and the charge / discharge efficiency and output characteristics of the battery can be improved. As the conductor of this embodiment, for example, a fibrous conductive material 34 made of a carbon material such as carbon nanotube (CNT) or carbon nanofiber (CNF) can be used. In addition, it is desirable to use a string-like material with an aspect ratio of length to diameter of 30 or more. The length is preferably 100 [nm] or more and 1000 [nm]. If it is less than 100 [nm], a sufficient conductive network cannot be formed. If it exceeds 1000 [nm], it becomes difficult to disperse.

[0052] In this embodiment, carbon nanotubes having a length [nm] of 100 [nm] or more, up to 1000 [nm], are used. <Scaly aggregate 35> The scale-like aggregate 35 of this embodiment is formed in a generally disk-like thin plate shape. 2 ] is 2.8 [μm 2 ] or more. The average thickness T [μm] of the scale-like agglomerates 35 is 0.4 [μm] or less. The porosity [%] of the agglomerates of the scale-like agglomerates 35 is 10 to 30 [%]. The ratio [wt%] of the scale-like agglomerates 35 to the entire conductor is 0.04 [wt%] or more and 1.50 [wt%] or less with respect to the entire fibrous conductive material 34.

[0053] <Binding material (binder)> The binder may be, for example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid, polyacrylate, or the like.

[0054] <Manufacturing method of positive electrode plate> 2, the positive electrode plate 3 is composed of a positive electrode current collector 31 and a positive electrode mixture layer 32 applied thereto. The positive electrode mixture layer 32 is formed by applying a positive electrode mixture paste to the positive electrode current collector 31 and drying it. The positive electrode mixture paste is prepared by mixing and kneading a positive electrode active material 33, a fibrous conductive material 34, a scaly aggregate 35, and additives such as a binder and a dispersant.

[0055] Conventionally, carbon nanotubes uniformly dispersed in a dispersion medium such as an organic solvent are mixed with the positive electrode active material 33 as well as additives such as a binder and a dispersant, and the solid content NV [%] and viscosity [Pa s] are adjusted with a solvent before being kneaded. By manufacturing in this manner, a positive electrode composite paste in which carbon nanotubes are uniformly dispersed can be produced.

[0056] On the other hand, in this embodiment, carbon nanotubes that have been uniformly dispersed in advance in a dispersion medium such as an organic solvent are aggregated. A very strong cohesive force (van der Waals force) acts between the carbon nanotubes that have been defibrated into individual pieces or between aggregates of several nm to several tens of nm. Therefore, the carbon nanotubes are distributed in a dispersion medium such as an organic solvent in a state where they are defibrated into individual pieces. In this embodiment, a shear force is applied to the dispersed carbon nanotubes to intentionally cause aggregation. This can be performed on a paste-like material, but it is performed on fibrous conductive material 34 that has been dispersed in a medium in advance.

[0057] To apply such shear force, a colloid mill can be used. A colloid mill is a general term for a grinding machine that produces ultrafine particles. It is a device that performs subdivision that is impossible with ordinary grinding means, and it is designed to pour solid particles together with a liquid into a gap between two surfaces that rotate very close to each other, and apply a shear force to the liquid to finely pulverize the solid and disperse it in the liquid. Some have toothed rotating surfaces, which can produce a colloid-like product of 1 μm or less. In addition to these wet types, there are various types such as dry types. It is used in the industries of fillers for paper, rubber, cosmetics, and food, pigments, paints, and enamel. An example of the colloid mill of this embodiment is a carbon nanotube wet grinding machine such as the MK2000 by IKA Japan Co., Ltd.

[0058] Colloid mills are usually used for the purpose of breaking down large solid particles, but the inventors have discovered that by using a colloid mill on carbon nanotubes that have been defibrated into individual strands in a dispersion medium, it is actually possible to form aggregates.

[0059] <Formation of scale-like aggregates 35> In this embodiment, the conditions for controlling aggregation with a colloid mill include the solid content rate NV (Nonvolatile content) [%] and viscosity [Pa s], which are physical properties of the carbon nanotube dispersion. In addition, the equipment conditions for the colloid mill include the size of the gap [μm] between the pair of rotors, as well as the stirring speed [rpm], temperature [°C], and stirring time [sec], and the state of aggregation differs depending on these.

[0060] Therefore, the parameters for the physical properties of these dispersions are the solid content rate NV [%] and viscosity [Pa s]. In addition, the size of the gap [μm], as well as equipment conditions such as the stirring speed [rpm], temperature [°C], and stirring time [sec] are also used as parameters. By changing these parameters, the desired shape, planar area A [μm 2The mixture is then mixed in a colloid mill to achieve the desired shape, planar area A [μm], void ratio [%], and blending amount [wt%]. In particular, the solid content NV [%] and viscosity [Pa s] are easy to adjust, and increasing the solid content NV [%] and viscosity [Pa s] promotes aggregation. By adjusting these factors, the desired shape, planar area A [μm 2 ], thickness T [μm], etc. can be obtained. However, excessive stirring may result in the formation of amorphous aggregates.

[0061] <Solid content NV[%]> When the solid content rate NV [%] is high, the planar area A [μm 2 ] tends to increase, and the thickness T [μm] tends to increase. This is thought to be because the carbon nanotubes come into contact with each other more frequently. On the other hand, when the solid content rate NV [%] is low, the planar area A [μm 2 ] tends to become smaller and the thickness T [μm] tends to become thinner. However, this is a tendency within a certain range, so it does not necessarily apply to all cases, and actual experiments are required.

[0062] <Viscosity [Pa s]> When the viscosity [Pa·s] is low, the thickness T [μm] tends to be thin. This is presumably because the contact in the thickness direction is reduced when the paste has high fluidity. Plane area A [μm 2 No clear trend was observed for viscosity [Pa s]. On the other hand, there was a tendency for thickness T [μm] to increase as viscosity [Pa s] increased. This is also a tendency within a certain range, so it does not necessarily apply to all cases, and actual experiments are required.

[0063] <Gap [μm]> When the gap [μm] between the pair of rotors is wide, the planar area [μm 2 ] tends to be large and the thickness T [μm] also tends to be thick. It is presumed that the wider the gap [μm], the higher the frequency of contact between the carbon nanotubes in each direction. On the other hand, when the gap [μm] between the pair of rotating bodies is narrow, the planar area [μm 2] tends to be small and the thickness T [μm] also tends to be thin. It is presumed that this is because the shear force increases when the gap [μm] is narrow. This is also a tendency within a certain range, so it does not necessarily apply to all cases, and actual experiments are required.

[0064] <Stirring speed [rpm]> When the stirring speed (rotation speed) [rpm] is slow, the planar area A [μm 2 ] tends to increase. No significant tendency was observed for the thickness T [μm]. On the other hand, when the stirring speed (rotation speed) [rpm] is high, the planar area A [μm 2 ] tended to be smaller. It is assumed that this is because the faster the rotation, the more the agglomerates are broken down. However, this is a tendency that is within a certain range, so it does not necessarily apply to all cases, and actual experiments are required.

[0065] <Processing temperature [°C]> The higher the treatment temperature [°C], the greater the planar area A [μm 2 ] tended to increase. This is presumably because the higher the temperature [°C], the greater the kinetic energy, which increases the frequency of contact between the carbon nanotubes. On the other hand, the lower the treatment temperature [°C], the greater the planar area A [μm 2 ] tended to become smaller. No strong tendency was observed for the thickness T [μm]. This is also a tendency within a certain range, so it does not necessarily apply to all cases, and actual experiments are required.

[0066] <Mixing time [sec]> The longer the stirring time [sec], the larger the planar area A [μm 2 ] tended to be smaller. It is presumed that this is because the longer the stirring time, the more the agglomerates are loosened. On the other hand, when the stirring time [sec] was short, the planar area A [μm 2] tended to become larger. However, no strong tendency was observed for the thickness T [μm]. This is also a tendency within a certain range, so it does not necessarily apply to all cases, and actual experiments are required.

[0067] <Control of formation of scale-like aggregates 35> As described above, the degree of aggregation changes depending on the solid content NV [%], viscosity [Pa s], gap [μm], stirring speed [rpm], temperature [°C], stirring time [sec], etc. By changing the conditions, a certain tendency was observed in the formation of scale-like aggregates 35. Therefore, the planar area A [μm 2 It was confirmed that the thickness T [μm] and solid content NV [%] and viscosity [Pa s] can be controlled by adjusting the solvent. In particular, the solid content NV [%] and viscosity [Pa s] can be easily adjusted by adjusting the solvent. However, changing these conditions does not result in a linear relationship between the conditions and the results, and the relationship is limited to a certain range. For this reason, it is necessary to actually measure the surface area A [μm] of the desired scale-like aggregate 35 in advance through experiments and reflect the resulting tendency. 2 ] and thickness T [μm] can be achieved.

[0068] <Configuration of scale-like aggregate 35> FIG. 5 is a micrograph of the surface of the positive electrode plate 3 of this embodiment. FIG. 6 is a micrograph of the surface of the conventional positive electrode plate 3. As shown in FIG. 6, granular positive electrode active material 33 can be seen on the surface of the conventional positive electrode plate 3 as surrounded by a white line. A large number of fibrous conductive materials 34 that look like threads are attached to the surface of this granular positive electrode active material 33. On the other hand, in the positive electrode plate 3 of this embodiment shown in FIG. 5, a large number of fibrous conductive materials 34 are attached to the surface of the granular positive electrode active material 33, and a large black scale-like aggregate 35 surrounded by a white line can be seen. The scale-like aggregate 35 is not attached to the granular positive electrode active material 33, and its periphery can be contacted with the nonaqueous electrolyte 13.

[0069] 7 is a graph comparing the rate of change [%] in heat generation rate (maximum) [°C / sec] between the case with and without the scale-like aggregates 35 of this embodiment. For a conventional positive electrode plate 3, the rate of change [%] in heat generation rate (maximum) [°C / sec] in an overcharged state under constant conditions was set to 100, and the rate of change [%] in heat generation rate (maximum) [°C / sec] in the positive electrode plate 3 of this embodiment in the same overcharged state was compared.

[0070] As can be seen from this graph, the surface temperature [°C] of the positive electrode active material 33 is the same for both the conventional positive electrode plate 3 and the positive electrode plate 3 of this embodiment, which generate heat under the same conditions and in the same state.

[0071] This proves that the rate of change [%] in the heat generation rate (maximum) [°C / sec] is due to the presence or absence of scale-like aggregates 35. (Experimental Example of the Present Embodiment) Next, the planar area A [μm 2 The change rate [%] in heat generation rate (maximum) [°C / sec] was measured by changing the conditions of the thickness T [μm], and the ratio R [wt%] of the scale-like aggregates 35 to the entire conductive material.

[0072] (Experiment 1: Plane area A [μm 2 ] Difference in heat generation rate (max) [°C / sec] [%]) <Conditions of Experiment 1> FIG. 8 shows the planar area A [μm 2 9 is a table comparing the rate of change [%] in heat generation rate [°C / sec] due to differences in the planar area A [μm 2 13 is a graph comparing the rate of change [%] in the heat generation rate [°C / sec] of the positive electrode plate 3 due to differences in the temperature.

[0073] Below, Examples 1 to 3 are compared with Comparative Examples 1 and 2. The total amount of fibrous conductive material 34 (including scale-like aggregates 35) in positive electrode mixture layer 32 is commonly 0.8 [wt %]. In Comparative Example 1, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.78 [wt%].2 ] to 0.20 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.10 [μm]. The rate of change [%] was set to 100 [%] based on the heat generation rate [°C / sec] of the positive electrode plate 3 at this time.

[0074] In Comparative Example 2, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.87 [wt%]. 2 ] to 1.77 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.15 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 99 [%].

[0075] In Example 1, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.75 [wt%]. 2 ] to 2.84 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.20 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 85 [%].

[0076] In Example 2, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.47 [wt%]. 2 ] to 4.91 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.15 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 80 [%].

[0077] In Example 3, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.77 [wt%]. 2 ] to 39.6 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.19 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 83 [%].

[0078] <Summary of Experiment 1> FIG. 9 shows the planar area A [μm 2 9 is a graph comparing the rate of change [%] in the heat generation rate [°C / sec] of the positive electrode plate 3 due to differences in the temperature. As is clear from Fig. 9, the rate of change [%] in the heat generation rate [°C / sec] is 100 [%] in Comparative Example 1 and 99 [%] in Comparative Example 2. In contrast, it is 85 [%] in Example 1, 80 [%] in Example 2, and 83 [%] in Example 3, which shows that heat generation is significantly suppressed.

[0079] In this case, the total amount of the fibrous conductive material 34 (including the scale-like aggregates 35) is 0.8 [wt%] in the positive electrode mixture layer 32. The ratio R [wt%] of the scale-like aggregates 35 to the entire conductive material including the scale-like aggregates 35 is in the range of 0.75 to 0.87 [wt%] except for 0.47 [wt%] in Example 2. The thickness T [μm] of the scale-like aggregates 35 is in the range of 0.10 to 0.20 in all cases. In particular, the ratio R [wt%] of the scale-like aggregates 35 is small, 0.47 [wt%], in Example 2. That is, it can be seen that the ratio R [wt%] of the scale-like aggregates 35 to the entire conductive material including the scale-like aggregates 35 is a relatively small value of 0.47 [wt%] in Example 2, that is, even under unfavorable conditions in which the amount of the scale-like aggregates 35 is small, heat generation is significantly suppressed.

[0080] On the other hand, the planar area A [μm 2 ] is 0.20 [μm in Comparative Example 1 2 ], and 1.77 [μm 2 ], which is relatively small. 2 ], and Example 2 is 4.91 [μm 2 ], which is relatively large, and in Example 3, it is 39.6 [μm 2 ] and has become extremely large.

[0081] From these experimental results, it is concluded that the planar area A of the scale-like aggregate 35 is 2.84 [μm 2] From the above, it can be seen that heat generation was significantly suppressed, 85[%] in Example 1, 80[%] in Example 2, and 83[%] in Example 3.

[0082] <Conclusion of Experiment 1> Therefore, from Experiment 1, in order to effectively suppress heat generation, the planar area A of the scale-like aggregate 35 must be 2.84 [μm 2 It was found that it is desirable for the

[0083] (Experiment 2: Change in heat generation rate (maximum) [°C / sec] [%] due to differences in the ratio R [wt%] of scale-like aggregates 35 to the entire conductive material) <Conditions of Experiment 2> Fig. 10 is a table comparing the rate of change [%] in heat generation rate [°C / sec] due to differences in the ratio R (vs. conductive material) of scale-like agglomerates 35. Fig. 11 is a graph comparing the rate of change [%] in heat generation rate [°C / sec] due to differences in the ratio R (vs. conductive material) of scale-like agglomerates 35.

[0084] Below, Examples 4 to 8 are compared with Comparative Example 3. The total amount of fibrous conductive material 34 (including scale-like aggregates 35) in positive electrode mixture layer 32 is commonly 0.8 [wt %]. In Comparative Example 3, the ratio R [wt%] of the scale-like aggregates 35 to the entire conductive material was set to 0 [wt%]. In other words, the scale-like aggregates 35 were not formed. At this time, the heat generation rate [°C / sec] of the positive electrode plate 3 was used as the standard, and the rate of change [%] was set to 100 [%].

[0085] In Example 4, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.04 [wt%]. 2 ] to 6.3 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.15 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 92 [%].

[0086] In Example 5, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 1.00 [wt%]. 2 ] to 9.2 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.11 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 74 [%].

[0087] In Example 6, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.64 [wt%]. 2 ] to 8.0 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.12 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 78 [%].

[0088] In Example 7, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 1.47 [wt%]. 2 ] to 5.2 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.11 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 91 [%].

[0089] In Example 8, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.37 [wt%]. 2 ] to 5.4 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.13 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 76 [%].

[0090] <Summary of Experiment 2> 11 is a graph comparing the rate of change [%] in heat generation rate [°C / sec] due to differences in the ratio R (vs. conductive material) R of scale-like aggregates 35. As shown in Fig. 11, the rate of change [%] in heat generation rate [°C / sec] is 100 [%] in Comparative Example 3, whereas it is 92 [%] in Example 4. It is clear that heat generation is significantly suppressed, with 74 [%] in Example 5, 78 [%] in Example 6, 91 [%] in Example 7, and 76 [%] in Example 8.

[0091] In this case, the total amount of fibrous conductive material 34 (including scale-like aggregates 35) in positive electrode mixture layer 32 is commonly 0.8 [wt %]. On the other hand, the planar area A [μm 2 In Comparative Example 3, since there is no scale-like aggregate 35, the value is 0 [μm 2 In Example 4, it is 6.3 [μm 2 ], and in Example 5, 9.2 [μm 2 ], and in Example 6, 8.0 [μm 2 ], and in Example 7, 5.2 [μm 2 ], and in Example 8, 5.4 [μm 2 ] and 5.2 to 9.2 [μm 2 ] range, but in all cases, fever is suppressed.

[0092] The thickness T [μm] of the scaly agglomerates 35 is 0 [μm] in Comparative Example 3 since there are no scaly agglomerates 35. The thickness is in the range of 0.11 to 0.15 [μm], that is, 0.15 [μm] in Example 4, 0.11 [μm] in Example 5, 0.12 [μm] in Example 6, 0.11 [μm] in Example 7, and 0.13 [μm] in Example 8, and heat generation is suppressed in all cases.

[0093] It can be seen that when the ratio R of scale-like aggregates 35 is 0.04 [wt%] or more, heat generation is significantly suppressed by 92 [%] in Example 4, 74 [%] in Example 5, 78 [%] in Example 6, 91 [%] in Example 7, and 76 [%] in Example 8.

[0094] Therefore, from Experiment 2, it was derived that in order to effectively suppress heat generation, it is desirable for the ratio R of scale-like aggregates 35 to be 0.04[%] or more, as shown in FIG. It should be noted that a desirable upper limit for the ratio R of the scale-like agglomerates 35 is derived for a reason different from that of Experiment 2. That is, the scale-like agglomerates 35 are desirably 1.50 [wt%] or less with respect to the entire fibrous conductive material 34. The reason is that if the ratio R of the scale-like agglomerates 35 is 1.50 [wt%] or less, the inhibition of the movement of Li ions can be suppressed. In addition, the combination of the fibrous conductive material 34 and the scale-like agglomerates 35 allows the fibrous conductive material 34 to efficiently form paths between the positive electrode active material 33 and the scale-like agglomerates 35 to form a conductive network, and the conductivity is not impaired.

[0095] <Conclusion of Experiment 2> From the above Experiment 2, it was found that in order to effectively suppress heat generation, it is desirable for the scale-like aggregates 35 to be 0.04 [wt %] or more and 1.50 [wt %] or less of the entire fibrous conductive material 34.

[0096] (Experiment 3: Change in heat generation rate (maximum) [°C / sec] [%] due to difference in thickness T [μm] of scale-like aggregate 35) <Conditions of Experiment 3> Fig. 12 is a table comparing the rate of change [%] in heat generation rate [°C / sec] depending on the thickness T [μm] of the scale-like agglomerate 35. Fig. 13 is a graph comparing the rate of change [%] in heat generation rate [°C / sec] depending on the thickness T [μm] of the scale-like agglomerate 35.

[0097] Below, Examples 9 to 12 are compared with Comparative Example 4. The total amount of fibrous conductive material 34 (including scale-like aggregates 35) in positive electrode mixture layer 32 is commonly 0.8 [wt %]. In Comparative Example 4, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.70 [wt%]. 2 ] to 9.7 [μm 2The thickness T [μm] of the scale-like aggregate 35 was set to 0.57 [μm]. At this time, the heat generation rate [°C / sec] of the positive electrode plate 3 was set as the standard, and the rate of change [%] was set to 100 [%].

[0098] In Example 9, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.76 [wt%]. 2 ] to 9.4 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.20 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 68 [%].

[0099] In Example 10, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.79 [wt%]. 2 ] to 8.0 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.35 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 72 [%].

[0100] In Example 11, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.88 [wt%]. 2 ] to 9.3 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.10 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 76 [%].

[0101] In Example 12, the ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material was set to 0.53 [wt%]. 2 ] to 9.2 [μm 2 The thickness T [μm] of the scale-like aggregate 35 was set to 0.39 [μm]. At this time, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 was 70 [%].

[0102] <Summary of Experiment 3> The thickness T [μm] of the scale-like aggregate 35 is 0.57 [μm] in Comparative Example 4. It is 0.20 [μm] in Example 9, 0.35 [μm] in Example 10, 0.10 [μm] in Example 11, and 0.39 [μm] in Example 12, and is in the range of 0.10 to 0.39 [μm] in Examples 9 to 12 compared to 0.57 [μm] in Comparative Example 4.

[0103] 13, the rate of change [%] of heat generation rate [°C / sec] of the positive electrode plate 3 of Comparative Example 4 was 100 [%]. In contrast, the rate of change [%] of heat generation rate [°C / sec] of the positive electrode plate 3 of Examples 9 to 12 was 68 to 76 [%], indicating that heat generation was significantly suppressed in all cases.

[0104] In this case, the total amount of fibrous conductive material 34 (including scale-like aggregates 35) in positive electrode mixture layer 32 is commonly 0.8 [wt %]. The ratio R [wt%] of the scale-like aggregate 35 to the entire conductive material is 0.70 [wt%] in Comparative Example 4, whereas it is 0.53 to 0.88 [wt%] in Examples 9 to 12, with 0.70 [wt%] in Comparative Example 4 being approximately the median value. In particular, in Example 12, the ratio R [wt%] of the scale-like aggregate 35 is 0.53 [wt%], which is an unfavorable condition, but despite this, the rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 of Example 12 is 70 [%]. The rate of change [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 of Examples 9 to 12 is 68 to 76 [%], and it was found that heat generation was significantly suppressed in all cases.

[0105] In addition, the planar area A [μm 2 In Comparative Example 4, the thickness is 9.7 [μm]. In contrast, in Examples 9 to 12, the thickness is 8.0 to 9.4 [μm], which is smaller than that of Comparative Example 4. In particular, in Example 10, the thickness is 8.0 [μm]. 2 ], which are unfavorable conditions compared to Comparative Example 4. Nevertheless, the change rate [%] of the heat generation rate [°C / sec] of the positive electrode plate 3 of Examples 9 to 12 compared to the heat generation rate [°C / sec] of the positive electrode plate 3 of Comparative Example 4 was 68 to 76 [%], and it was found that heat generation was significantly suppressed in all cases.

[0106] Therefore, from Experiment 3, it was derived that in order to effectively suppress heat generation, it is desirable for the thickness T [μm] of the scale-like aggregates 35 to be 0.39 [%] or less, as shown in FIG. <Conclusion of Experiment 3> From the above Experiment 3, it was found that in order to effectively suppress heat generation, the thickness T [μm] of the scale-like aggregates 35 needs to be 0.39 [%] or less.

[0107] (Action of this embodiment) In the positive electrode plate 3 for a lithium ion secondary battery of this embodiment, in the positive electrode mixture layer 32, fibrous conductive material 34 made of carbon nanotubes forms a conductive network so as to electrically connect the positive electrode active materials 33 to each other. Furthermore, some of the fibrous conductive material 34 is aggregated to form a scale-like aggregate 35. This scale-like aggregate 35 is roughly disc-shaped and has a planar area A corresponding to its bottom surface of 2.84 [μm 2 The agglomerates are formed so that the thickness T [μm] of the scale-like agglomerates 35 is 0.4 [μm] or less and the porosity of the scale-like agglomerates 35 is 30 [%] or less. The porosity of the scale-like agglomerates 35 is 0.04 [wt%] or more and 1.47 [wt%] or less with respect to the entire fibrous conductive material 34.

[0108] Such scale-like aggregates 35 do not adhere to granular positive electrode active material 33 , and almost the entire surface thereof is in contact with nonaqueous electrolyte solution 13 . When the surface temperature of the positive electrode active material 33 rises due to overcharging or the like, a thermal gradient occurs in the fibrous conductive material 34 with good thermal conductivity that is entangled with the surface of the positive electrode active material 33, and heat is transferred. Conventionally, heat is dissipated directly from the fibrous conductive material 34 that is entangled with the surface of the positive electrode active material 33 to the non-aqueous electrolyte 13. In this embodiment, in addition to this heat dissipation, heat is also dissipated from the scale-like aggregate 35 to the non-aqueous electrolyte 13. The scale-like aggregate 35 has a porosity of 30% or less and a volume larger than that of each individual fibrous conductive material 34, so that the heat capacity is also large. The fibrous conductive material 34 attached to the positive electrode active material 33 is connected to the scale-like aggregate 35 so as to form a conductive network. In other words, the scale-like aggregate 35 generates thermal conduction with the fibrous conductive material 34 attached to the positive electrode active material 33. Since carbon nanotubes have extremely good thermal conductivity, heat is transferred quickly from the fibrous conductive material 34 to the scale-like aggregate 35 according to the thermal gradient. In addition, since the thickness T [μm] of the scale-like aggregate 35 is 0.4 [μm] or less, heat is not accumulated inside the scale-like aggregate 35 and is quickly dissipated to the non-aqueous electrolyte 13. In other words, it can be said that the scale-like aggregate 35 acts as a heat dissipation fin for the positive electrode active material 33. Therefore, by quickly dissipating the heat of the positive electrode active material 33, the temperature rise of the positive electrode active material 33 is suppressed. Then, even if heat is generated on the surface of the positive electrode active material 33 due to overcharging, the temperature rise is suppressed, and the thermal decomposition of the non-aqueous electrolyte 13 can be effectively suppressed. As a result, there is an effect that the deterioration of the lithium ion secondary battery can be effectively suppressed.

[0109] (Effects of this embodiment) Since the present embodiment has the above-described configuration, it has the following advantages. (1) In the positive electrode plate 3 of the lithium ion secondary battery of this embodiment, there is an effect that sufficient heat dissipation can be performed even with a small amount of fibrous conductive material 34. Therefore, it is possible to suppress decomposition of the nonaqueous electrolyte 13 due to the surface of the positive electrode active material 33 becoming hot during overcharging. Therefore, there is an effect that it is possible to suppress deterioration of the lithium ion secondary battery due to overcharging.

[0110] (2) In this embodiment, fibrous conductive material 34 is dispersed on the surface of positive electrode active material 33, and fibrous conductive material 34 has flat, scaly agglomerates 35 that are aggregated into scales and do not adhere to positive electrode active material 33. This has the effect that scaly agglomerates 35 can effectively transfer heat generated on the surface of positive electrode active material 33 to scaly agglomerates 35 and dissipate the heat.

[0111] (3) The planar area A of the scale-like aggregate 35 is 2.84 [μm 2 For this reason, there is an effect that high heat dissipation properties can be obtained over a wide area compared to fibrous conductive material that is not aggregated.

[0112] (4) The thickness T [μm] of the scale-like aggregate 35 is set to 0.39 [μm] or less. This has the effect of preventing heat from being trapped inside the scale-like aggregate 35, thereby achieving a preferable high heat dissipation property.

[0113] (5) The porosity of the scale-like aggregate 35 is set to 30% or less, which has the effect of providing a large heat capacity and a preferable high heat dissipation property. (6) The amount of the scale-like aggregates 35 is set to 0.04 [wt %] or more relative to the entire fibrous conductive material 34. This has the effect of providing a desirable high heat dissipation property.

[0114] (7) The amount of scale-like aggregates 35 is set to 1.47 wt% or less of the total amount of fibrous conductive material 34. This makes it possible to suppress the inhibition of the movement of lithium ions. In addition, fibrous conductive material 34 that is in the form of fibers itself is combined with fibrous conductive material 34 that has scale-like aggregates 35 formed therein. This has the effect that fibrous conductive material 34 forms a path between positive electrode active material 33 and scale-like aggregates 35, making it possible to efficiently transfer heat from positive electrode active material 33 to scale-like aggregates 35.

[0115] (8) The length of the fibrous conductive material 34 is set to 100 nm or more. This makes it easier for the fibrous conductive material 34 to form conductive paths between each other, and has the effect of forming a conductive network to obtain sufficient conductivity.

[0116] (9) The length of the fibrous conductive material 34 is set to 1000 nm or less. This has the effect of suppressing the aggregation of the fibrous conductive material into "lumps" due to the intermolecular forces between the fibers and hydrogen bonds, thereby ensuring sufficient conductivity.

[0117] (10) The fibrous conductive material 34 of the present embodiment is a carbon nanotube, which has the effect of providing desirable physical properties, such as chemical properties, electrical properties, mechanical properties, thermal conductivity properties, and structural properties.

[0118] (11) The positive electrode active material 33 of the present embodiment is made of granular lithium nickel-cobalt manganese oxide having a large surface area. Therefore, the effect of the present embodiment can be exhibited in the positive electrode active material 33, which is prone to oxygen desorption and to generate heat of decomposition.

[0119] (12) In addition, the lithium ion secondary battery 1 of this embodiment uses the positive electrode plate 3 of this embodiment. This has the effect of making the lithium ion secondary battery highly resistant to overcharging.

[0120] (Another example) In the present embodiment, the lithium ion secondary battery 1 is used to drive a vehicle. However, the battery is not limited to being used in a vehicle and may be used as a stationary battery or a battery for other purposes.

[0121] Although the lithium ion secondary battery 1 having a flat wound electrode body 12 has been illustrated, the battery may have a cylindrical electrode body or a planar electrode body. The lithium ion secondary battery 1 exemplified in this embodiment is merely an example for explaining the present invention, and is not intended to limit the materials and shape constituting the battery.

[0122] Furthermore, the numerical values, their ranges, threshold values, etc. set forth in this embodiment are given as preferred examples, and are not limited to these. Needless to say, these values ​​can be optimized as appropriate by those skilled in the art depending on the configuration of the lithium ion secondary battery.

[0123] In addition, those skilled in the art may add, delete, or modify the configuration without departing from the scope of the claims. [Explanation of symbols]

[0124] 1...Lithium-ion secondary battery 11…Battery case 12...Electrode body 13...Nonaqueous electrolyte 14…Positive external terminal 15...Negative external terminal 2...Negative electrode plate 21...Negative electrode current collector 22...Negative electrode composite material layer 23...Negative electrode connection part 3…Positive electrode plate 31...Positive electrode current collector 32...Positive electrode mixture layer 33...Cathode active material 34...Fiber conductive material 35…scaly aggregate 32a…Positive electrode mixture paste 31a…Positive electrode connection part 4…Separator A [μm 2 ]…Plane area of ​​scale-like aggregate T [μm]: Thickness of scale-like aggregate L [μm]…(average length of fibrous conductor) R [wt%]: Ratio of scale-like aggregates to the entire conductive material

Claims

1. A positive electrode mixture layer of a positive electrode plate of a lithium ion secondary battery includes a positive electrode active material and a fibrous conductive material dispersed on a surface of the positive electrode active material, A positive electrode plate for a lithium ion secondary battery, characterized in that the fibrous conductive material has flat, scale-like aggregates that are aggregated into scales and do not adhere to the positive electrode active material.

2. The planar area of ​​the scale-like aggregate is 2.84 [μm 2 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the positive electrode is at least 0.1% by mass.

3. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the thickness of the scale-like aggregate is 0.39 [μm] or less.

4. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the porosity of the scale-like aggregate is 30% or less.

5. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the scale-like aggregates account for 0.04 wt % or more of the entire fibrous conductive material.

6. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the scale-like aggregates account for 1.47 wt % or less of the total amount of the fibrous conductive material.

7. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the length of the fibrous conductive material is 100 nm or more.

8. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the length of the fibrous conductive material is 1000 nm or less.

9. The positive electrode plate for a lithium ion secondary battery according to any one of claims 1 to 8, characterized in that the fibrous conductive material is a carbon nanotube.

10. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the positive electrode active material is lithium nickel cobalt manganese oxide.

11. A lithium ion secondary battery, comprising the positive electrode plate for lithium ion secondary batteries according to claim 9.

Citation Information

Patent Citations

  • Electrode active material-carbon nanotube composite and manufacturing method thereof

    JP2017084759A

  • Active material composite, electrode, power storage device and method for manufacturing active material composite

    JP2021036508A

  • Carbon microfiber dispersion liquid

    WO2012036172A1