Crystallizable shrinkable films and thermoformable sheets made of resins blends
Crystallizable polyester blends with specific glycol monomer combinations address the challenges of shrink film performance and recyclability by ensuring controlled shrinkage and compatibility with PET recycling, preventing agglomeration and maintaining film integrity.
Patent Information
- Application Number
- JP2024121143
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-12-20
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-10-08
AI Technical Summary
Existing shrink films and thermoformable sheets face challenges in achieving low shrinkage onset temperature, controlled shrinkage rate, high shrinkage force, recyclability, and compatibility with PET bottle recycling processes without forming agglomerates during high-temperature drying.
Development of crystallizable polyester blends comprising specific combinations of terephthalic acid, neopentyl glycol, 1,4-cyclohexanedimethanol, and ethylene glycol, which allow for amorphous films to crystallize at high strain-induced melting points, ensuring compatibility with PET recycling and maintaining film performance.
The crystallizable polyester blends provide excellent shrink film properties, prevent agglomeration with PET flakes, and enable seamless recycling without additional operational steps, enhancing recyclability and film performance.
Smart Images

Figure 2024153767000009 
Figure 2024153767000010 
Figure 2024153767000001
Abstract
Description
FIELD OF THEINVENTION
[0001] This disclosure relates to crystallizable shrinkable films and thermoformable sheets comprising mixtures of polyester compositions containing residues of terephthalic acid, neopentyl glycol (NPG), 1,4-cyclohexanedimethanol (CHDM), ethylene glycol (EG), and diethylene glycol (DEG) in specific compositional ranges that have certain advantages and improve properties. [Background technology]
[0002]
[0002] There is a commercial demand for shrink films having at least one of the following desirable properties: (1) a low shrink onset temperature; (2) a shrink rate that increases gradually and in a controlled manner with increasing temperature over the temperature range over which shrinkage occurs; (3) a shrink force low enough to prevent crushing of the underlying container; (4) a high maximum shrink rate (shrink rate at the highest temperature), e.g., greater than 50% in the main shrink direction at 95°C; (5) a low shrink rate in a direction perpendicular to the high shrink rate direction; (6) high film toughness to prevent undesirable crushing, breaking, tearing, splitting, bubbling, or wrinkling of the film during manufacture and before and after shrinking; and (7) recyclability.
[0003]
[0003] There is a commercial need for thermoformable sheets having superior properties and recyclability.
[0004]
[0004] It has been found that blends made of polyesters containing specific combinations of glycol monomers in shrink film resin compositions can produce films with excellent shrink film performance, and can be crystallized so as not to affect the recycling of the PET flakes that occur simultaneously during recycling. These crystallizable shrink film resin blends can be processed with PET bottles and become a component of the recyclable PET flakes after the recycling process is completed. It has been found that the selection of the specific combinations of polyesters and their amounts in the blends containing specific glycol monomers is important to produce films with excellent shrink film properties and to produce crystallizable films. The optimized polyester resin blend compositions of the present disclosure are amorphous but crystallizable. Thus, these compositions exhibit excellent properties in film applications, including shrink films, but because these strain-induced crystals have high melting points, they perform well in the recycling process. The shrink film labels of the present disclosure do not need to be removed during the recycling process and do not affect the recycling process.
[0005]
[0005] To be used in this application, heat shrinkable films must meet various standards of suitability. The film must be strong, shrink in a controlled manner, and provide sufficient shrink force to hold itself against the bottle surface without crushing the contents. Furthermore, when these labels are applied to polyester containers, the polyester shrink film labels must not interfere with the bottle recycling process. It would be advantageous if the labels could be recycled, i.e., the entire bottle, including the label, could be recycled and converted into a new product without requiring additional handling requirements or creating new environmental problems. Heat shrink films are made from a variety of raw materials to meet a range of material demands. This disclosure describes the unique and unexpected effects of blends of polyesters made with specific monomer combinations for shrink film resin compositions.
[0006] Polyester shrink film compositions have been used commercially as shrink film labels for food, beverages, personal care products, household goods, and the like. Often these shrink films are used in combination with bottles or containers made of clear polyethylene terephthalate (PET). After use, the entire product (bottle and label) is put into a recycling process. At a typical recycling station, due to their similar composition and density, the PET and shrink film materials may end up mixed together at the end of the process. Drying of the PET flakes is necessary to remove the residual water that is carried by the PET during the recycling process. Typically, PET is dried at temperatures in excess of 200°C. At these temperatures, typical polyester shrink film resins soften and become sticky, and the PET flakes often form clumps. These clumps must be removed before further processing. These clumps reduce the yield of PET flakes from the process and require additional handling steps.
[0007]
[0007] It has also been found that a particular combination of glycol monomers in a film or sheet resin composition can produce a film or sheet with excellent performance properties, and that this combination is crystallizable so as not to affect the recyclability of the PET flakes. These crystallizable film or sheet resins can be processed with recycled PET and become a component of the recyclable PET flakes after the recycling process is completed. It has also been found that the selection of a particular combination of glycol monomers and their amounts are important to produce a film or sheet with excellent performance properties and to produce a crystallizable film or sheet. That is, although these polyester compositions are amorphous, they are "crystallizable" in the sense that they have a high strain-induced crystalline melting point. Thus, these compositions exhibit excellent properties in film or sheet applications, such as forming, thermoforming, or as-molded parts and / or articles, but they also have a high strain-induced crystalline melting point so that they can be recycled with PET. Because when recycled PET flakes are subjected to high temperature drying conditions, the crystallizable polyesters of the present invention do not form agglomerates that would interfere with the normal mechanical operations of grinding, drying, and feeding the flakes to an extruder for subsequent processing into (recycled) polyester pellets. Similarly, the sheet of the present disclosure does not need to be removed during the recycling process because it does not adversely affect the recycling process. (e.g., https: / / www.thebalancesmb.com / recycling-polyethylene-terephthalate-pet-2877869 (see
[0008] One embodiment of the present disclosure is a crystallizable film comprising a mixture of polyester compositions comprising: (1) at least one crystallizable polyester comprising residues of terephthalic acid, neopentyl glycol (NPG), 1,4-cyclohexanedimethanol (CHDM), ethylene glycol (EG), and diethylene glycol (DEG) in a particular compositional range; and (2) at least one amorphous polyester comprising residues of terephthalic acid, neopentyl glycol (NPG), 1,4-cyclohexanedimethanol (CHDM), ethylene glycol (EG), and diethylene glycol (DEG) in a particular compositional range.
[0008]
[0009] One embodiment of the present disclosure relates to a crystallizable polyester blend composition. In one embodiment, the crystallizable polyester blend composition comprises: (a) 5 to 95 wt % of a crystallizable polyester composition; and (b) 5 to 95 wt % of at least one amorphous polyester composition.
[0009]
[0010] One embodiment of the present disclosure is a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and a diol component selected from either (b) or (b'); (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 75 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 25 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 25 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 25 mol % or less of other glycols, including one or more of from about 0 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (b') The diol component is about 75 mole percent or more of ethylene glycol residues, and (i) from about 0.1 to less than about 24 mole percent neopentyl glycol residues; (ii) from about 0.1 to less than about 24 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 25 mol % or less of other glycols, including one or more of from about 1 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 60 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 40 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 40 mol % or less of other glycols, including one or more of from about 0 to less than about 15 mol % of the total diethylene glycol residues in the final polyester composition; The total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the (1) and (2) polyesters are different.
[0010]
[0011] One embodiment of the present disclosure is a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 80 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 20 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 20 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 20 mol % or less of other glycols, including one or more of from about 0 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 70 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 30 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 30 mol % or less of other glycols, including one or more of from about 0 to less than about 15 mol % of the total diethylene glycol residues in the final polyester composition; The total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the (1) and (2) polyesters are different.
[0011]
[0012] One embodiment of the present disclosure is a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 85 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 15 mole % neopentyl glycol residues; (ii) from about 0 to less than about 15 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 15 mol % or less of other glycols, including one or more of from about 0 to less than about 5 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 60 mole percent or more of ethylene glycol residues, and (i) a neopentyl glycol residue, (ii) 1,4-cyclohexanedimethanol residue, and (iii) not more than about 40 mole % of other glycols, whether generated in situ or not, including one or more diethylene glycol residues in the final polyester composition. Including, The total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the (1) and (2) polyesters are different.
[0012]
[0013] One embodiment of the present disclosure is a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) from about 0 to about 30 mol % neopentyl glycol residues; (ii) from about 0 to less than about 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) contains a diethylene glycol residue, The remainder of the glycol component is (iv) ethylene glycol residues, and (v) containing 0.1 to 20 mol % of at least one modifying glycol residue; the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the glycol component is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) from about 0 to about 40 mol % neopentyl glycol residues; (ii) from about 0 to less than about 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) Contains diethylene glycol residues, whether or not generated in situ; The remainder of the glycol component is (iv) ethylene glycol residues, and (v) 0-20 mol %, or 0-10 mol %, or 0-5 mol % of at least one modifying glycol residue; The total mole % of the dicarboxylic acid components is 100 mole %, the total mole % of the glycol components is 100 mole %, and the (1) and (2) polyesters are different.
[0013]
[0014] In another embodiment of the present disclosure, the mixed composition has a crystalline melting point in the range of about 200 to about 255°C.
[0015] In other embodiments of the present disclosure, the mixture has a crystalline melting point in the range of about 220° C. to about 230° C., or in the range of about 245° C. to about 255° C. In other embodiments, component (1) has a crystalline melting point of about 220° C. to about 230° C.
[0014]
[0016] One embodiment of the present disclosure is a crystallizable film of the previous embodiment, which is stretched in at least one direction, the stretched film having a melting point of strain-induced crystals of 200° C. or greater.
[0015]
[0017] One embodiment of the present disclosure is a thermoformed or thermoformable film or sheet comprising a mixture of polyester compositions comprising: (1) at least one crystallizable polyester comprising residues of terephthalic acid, neopentyl glycol (NPG), 1,4-cyclohexanedimethanol (CHDM), ethylene glycol (EG), and diethylene glycol (DEG) in a particular compositional range; and (2) at least one amorphous polyester comprising residues of terephthalic acid, neopentyl glycol (NPG), 1,4-cyclohexanedimethanol (CHDM), ethylene glycol (EG), 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD), and diethylene glycol (DEG) in a particular compositional range.
[0016]
[0018] One embodiment of the present disclosure relates to a thermoformed or thermoformable film or sheet comprising a crystallizable polyester blend composition. In one embodiment, the thermoformed or thermoformable film or sheet comprises a crystallizable polyester blend composition comprising: (a) 5 to 95 weight percent of a crystallizable polyester composition; and (b) 5 to 95 weight percent of at least one amorphous polyester composition.
[0017]
[0019] One embodiment of the present disclosure is a thermoformed sheet having a thickness of about 0.25 mm to about 6.4 mm, comprising a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and a diol component selected from either (b) or (b'); (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 75 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 25 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 25 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 25 mol % or less of other glycols, including one or more of from about 0 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (b') The diol component is about 75 mole percent or more of ethylene glycol residues, and (i) from about 0.1 to less than about 24 mole percent neopentyl glycol residues; (ii) from about 0.1 to less than about 24 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 25 mol % or less of other glycols, including one or more of from about 1 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 60 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 40 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 40 mol % or less of other glycols, including one or more of from about 0 to less than about 15 mol % of the total diethylene glycol residues in the final polyester composition; The total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the (1) and (2) polyesters are different.
[0018]
[0020] One embodiment of the present disclosure is a thermoformed sheet having a thickness of about 0.25 mm to about 6.4 mm, comprising a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 80 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 20 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 20 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 20 mol % including one or more of from about 0 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition, whether or not generated in situ. Other glycols include: the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 70 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 30 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 30 mol % or less of other glycols, including one or more of from about 0 to less than about 15 mol % of the total diethylene glycol residues in the final polyester composition; The total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the (1) and (2) polyesters are different.
[0019]
[0021] One embodiment of the present disclosure is a thermoformed sheet having a thickness of about 0.25 mm to about 6.4 mm, comprising a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 80 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 15 mole % neopentyl glycol residues; (ii) from about 0 to less than about 15 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 15 mol % or less of other glycols, including one or more of from about 0 to less than about 5 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 60 mole percent or more of ethylene glycol residues, and (i) a neopentyl glycol residue, (ii) 1,4-cyclohexanedimethanol residue, and (iii) one or more diethylene glycol residues in the final polyester composition and about 40 mole % or less of other glycols, including The total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the (1) and (2) polyesters are different.
[0022] One embodiment of the present disclosure is a thermoformed sheet having a thickness of about 0.25 mm to about 6.4 mm, comprising a crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) from about 0 to about 30 mol % neopentyl glycol residues; (ii) from about 0 to less than about 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) contains a diethylene glycol residue, The remainder of the glycol component is (iv) ethylene glycol residues, and (v) optionally, 0.1 to 10 mole % of at least one modifying glycol residue; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) from about 0 to about 40 mol % neopentyl glycol residues; (ii) from about 0 to less than about 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) contains a diethylene glycol residue, The remainder of the glycol component is (iv) ethylene glycol residues, and (v) optionally, 0.1 to 10 mole % of at least one modifying glycol residue; The total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the (1) and (2) polyesters are different.
[0020]
[0023] One embodiment of the present disclosure is an extruded or calendered film comprising a mixture of the crystallizable compositions of any of the preceding embodiments.
[0024] One embodiment of the present disclosure is a molded, thermoformed, or shaped article comprising or prepared from a sheet of any of the preceding embodiments.
[0021]
[0025] One embodiment of the present disclosure is medical device packaging, medical related packaging, healthcare product packaging, commercial food supply packaging, trays, containers, food plates, tumblers, storage bins, bottles, cookware, mixing bowls, household items, water bottles, crisper trays, dishwasher parts, refrigerator parts, vacuum cleaner parts, ophthalmic lenses, and frames or toys comprising or prepared from the thermoformed or thermoformable sheets of any of the preceding embodiments.
[0022]
[0026] One embodiment of the present disclosure is an article of manufacture comprising or prepared from a thermoformed or thermoformable sheet of any of the preceding claims.
[0027] One embodiment of the present disclosure is a method of making a thermoformed film or sheet of any of the previous embodiments, the method including A) heating a polyester film or sheet, B) applying air pressure, vacuum, and / or physical pressure to the heat-softened film or sheet, C) conforming the sheet to the shape of a mold with vacuum or pressure, D) cooling the thermoformed part, and E) removing the thermoformed part or article from the mold.
[0023]
[0028] The Association for Plastic Recyclers (APR) is a non-profit organization that provides a comprehensive evaluation of the suitability of plastics for recycling in the current recycling process (PET-CG-02). A test has been established to measure label (minimum 3% by weight) and bottles. In this test, labels (minimum 3% by weight) and bottles are crushed to 1 / 4-1 / 2 inch flake size. The bottle flakes are then mixed 50:50 with unlabeled control bottle flakes. The samples are then wet sized under conditions that allow no more than 1.2% of the PET with the label to be carried over. The flakes are washed in 0.3% Triton X-100 and 1.0% caustic at 88°C for 15 minutes. All suspended solids are then crushed to 1 / 4-1 / 2 inch flake size. The bottle flakes are then mixed 50:50 with unlabeled control bottle flakes. The samples are then wet sized under conditions that allow no more than 1.2% of the PET with the label to be carried over. The flakes are then washed in 0.3% Triton X-100 and 1.0% caustic at 88°C for 15 minutes. All suspended solids are then crushed to 1 / 4-1 / 2 inch flake size. After removing the particles, the flakes are washed with water and then strained to remove excess water. The flakes are wet screened again as before. Two pounds of the washed flakes are then placed into a Teflon coated baking dish for each washed sample, adding flakes to a layer thickness of 1.5 inches. The dish containing the flakes is placed in a circulating oven at 208°C for 1.5 hours. The flakes are cooled and passed through a sieve with 0.0625 inch openings. If the material passes through the sieve, it is not agglomerated, i.e., it is not too large to pass through the sieve. This test is followed by extrusion / pelletization and molding steps to ensure the quality of the flakes.
[0024]
[0029] As a result, the crystallizable mixture of the present disclosure provides an effective component of the PET recycling process stream to the extent that the composition is capable of accompanying the PET in the recycling process stream without the need for an additional separation step. Thus, in one embodiment of the present disclosure, a polyester recycling process stream is provided that includes recycled polyethylene terephthalate flakes mixed together with at least about 0.1% by weight of the crystallizable mixture of the present disclosure. In another embodiment, the process stream has passed Document No. PET-CG-02, dated April 11, 2019, entitled "Critical Guidance Protocol for Clear PET Articles with Labels and Closures." [Brief description of the drawings]
[0025] [Figure 1]
[0030] FIG. 1 shows the PET aggregation percentage versus crystallinity for blends made with Resin No. 1 and Resin No. 2. [Diagram 2]
[0031] FIG. 2 shows the PET aggregation percentage versus crystallinity for blends made with Resin No. 2 and Resin No. 3. Detailed Description of the Invention
[0026]
[0032] The present disclosure will be more readily understood by reference to the following detailed description of certain embodiments and examples of the present disclosure. In accordance with the purposes of this disclosure, certain embodiments of the present disclosure are described in the Summary of the Invention and further described herein below. Other embodiments of the present disclosure are also described herein.
[0027]
[0033] Heat shrinkable plastic films are used as coverings to hold multiple objects together and as outer wrappings for bottles, cans, and other types of containers. For example, the films are used to cover the lid, neck, shoulder, body, or entire bottle for the purpose of labeling, protecting, packaging, or adding value to the product, and for other reasons. In addition, the films can be used as coverings to pack objects together as a group, such as boxes, bottles, boards, bars, or notebooks, and the films can also be tightly attached as wrappings. The above uses take advantage of the shrinkability and internal shrinkage stress of the film.
[0028]
[0034] Historically, polyvinyl chloride (PVC) film has dominated the shrink film market. However, polyester film has become a viable alternative because it does not have the environmental issues associated with PVC film. Ideally, polyester shrink film would have properties very similar to PVC film, so polyester can act as a "drop-in" film replacement and replace existing heat shrink tunnels. The desired PVC film properties for replication include: (1) a relatively low shrink onset temperature, (2) a total shrinkage percentage that increases in a gradual and controlled manner with increasing temperature, (3) a low shrink force to prevent crushing of the underlying container, (4) a high total shrinkage percentage (e.g., 50% or more), and (5) inherent film toughness to prevent undue tearing and splitting of the film before and after shrinkage.
[0029]
[0035] To be used in this application, heat shrinkable films must meet various standards of suitability. The film must be strong, shrink in a controlled manner, and provide sufficient shrink force to hold itself on the bottle surface without crushing the contents. Furthermore, when these labels are applied to polyester containers, they must not interfere with the recycling process of PET bottles. In fact, it would be advantageous if the labels were also recyclable, and the entire bottle could be recycled and converted into a new product without creating additional operating requirements or new environmental problems. Heat shrinkable films are manufactured from a variety of raw materials to meet a range of material needs. This disclosure describes the unique and unexpected effects of blends of polyesters, including combinations with specific monomers, that improve the recyclability of labels made of polyester shrink films.
[0030]
[0036] Shrink film compositions are used commercially as shrink film labels for food, beverages, personal care products, household products, and the like. Often these shrink films are used in combination with clear polyethylene terephthalate (PET) bottles or containers. The entire product (bottle and label) is then put into a recycling process. In a typical recycling station, due to their similar composition and density, the PET and shrink film materials may be mixed at the end of the process. Drying of the PET flakes is necessary to remove the residual water that is attached to the PET during the recycling process. Typically, PET is dried at temperatures above 200°C, and at these temperatures, typical polyester shrink film resins soften and become sticky, often forming agglomerates with the PET flakes. These agglomerates must be removed prior to further processing. These agglomerates reduce the yield of PET flakes from the process, necessitating additional handling steps.
[0031]
[0037] It has been found that polyesters with specific combinations of glycol monomers in the polyester resin blend composition of shrink film provide films with excellent shrink film performance, and are crystallizable so as not to affect the recyclability of PET flakes during recycling. These crystallizable shrink film resin blends can be processed with PET bottles and become a component of the recyclable PET flakes after the recycling process is completed. It has been found that the selection of the specific combinations of glycol monomers and their amounts in each composition (amorphous composition and crystallizable composition) in the crystallizable polyester blend composition is important to produce films with excellent shrink film properties and to produce crystallizable films.
[0032]
[0038] The term "polyester" as used herein is intended to include "copolyester" and is understood to mean a synthetic polymer prepared by reacting one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds, such as branching agents. In general, the difunctional carboxylic acids may be dicarboxylic acids and the difunctional hydroxyl compounds may be dihydric alcohols, such as glycols and diols. The term "glycol" as used herein includes, but is not limited to, diols, glycols, and / or polyfunctional hydroxyl compounds, such as branching agents. Alternatively, the difunctional carboxylic acids may be hydroxycarboxylic acids, such as p-hydroxybenzoic acid, and the difunctional hydroxyl compounds may have an aromatic nucleus bearing two hydroxyl substituents, such as hydroquinone. The term "residue" as used herein means any organic structure incorporated into a polymer by polycondensation and / or esterification reactions from the corresponding monomers. The term "repeating unit" as used herein means an organic structure having dicarboxylic acid residues and diol residues linked through ester groups. Thus, for example, the dicarboxylic acid residues may be derived from a dicarboxylic acid monomer or its associated acid halides, esters, salts, anhydrides, and / or mixtures thereof. The term "diacid" as used includes polyfunctional acids, such as branching agents. Thus, the term "dicarboxylic acid" as used herein is intended to encompass any dicarboxylic acid derivative useful for reactive processing with diols to obtain polyesters, such as the associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, and / or mixtures thereof. The term "terephthalic acid" as used herein is intended to encompass any terephthalic acid derivative useful for reactive processing with diols to obtain polyesters, such as terephthalic acid itself and its residues, as well as the associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, and / or mixtures thereof or residues thereof.
[0033]
[0039] The polyesters used in the present disclosure can typically be prepared from dicarboxylic acids and diols that react in substantially equal proportions and are incorporated into the polyester polymer as the corresponding residues. Thus, the polyesters of the present disclosure may contain substantially equal molar ratios of acid residues (100 mol%) and diol (and / or multifunctional hydroxyl compound) residues (100 mol%), such that the total moles of repeat units equal 100 mol%. Thus, the mole percentages given in the present disclosure may be based on the total moles of acid residues, the total moles of diol residues, or the total moles of repeat units. For example, a polyester containing 10 mol% isophthalic acid based on the total acid residues means that the polyester contains 10 mol% isophthalic acid residues out of a total of 100 mol% acid residues. That is, there are 10 moles of isophthalic acid residues in each 100 moles of acid residues. As another example, a polyester containing 25 mole percent 1,4-cyclohexanedimethanol based on total diol residues means that the polyester contains 25 mole percent 1,4-cyclohexanedimethanol residues out of a total of 100 mole percent diol residues, i.e., there are 25 moles of 1,4-cyclohexanedimethanol residues in every 100 moles of diol residues.
[0034]
[0040] In certain embodiments, terephthalic acid or an ester thereof, such as dimethyl terephthalate or a mixture of terephthalic acid residues and their esters, can comprise all or part of the dicarboxylic acid component used to form the polyesters useful in the present disclosure. In certain embodiments, terephthalic acid residues can comprise all or part of the dicarboxylic acid component used to form the polyesters useful in the present disclosure. For purposes of this disclosure, the terms "terephthalic acid" and "dimethyl terephthalate" are used interchangeably herein. In one embodiment, dimethyl terephthalate is all or part of the dicarboxylic acid component used to make the polyesters useful in the present disclosure. In some embodiments, 70-100 mol%; or 80-100 mol%; or 90-100 mol%; or 99-100 mol%; or 100 mol% terephthalic acid and / or dimethyl terephthalate and / or mixtures thereof may be used.
[0035]
[0041] In addition to terephthalic acid, the dicarboxylic acid component of the polyesters useful in the present disclosure may include up to 30 mol%, up to 20 mol%, up to 10 mol%, up to 5 mol%, or up to 1 mol% of one or more modified aromatic dicarboxylic acids. Yet another embodiment includes 0 mol% modified aromatic dicarboxylic acids. Thus, it is contemplated that the amount of one or more modified aromatic dicarboxylic acids, if present, may vary between any of these above endpoint values, such as 0.01-10 mol%, 0.01-5 mol%, 0.01-1 mol%. In one embodiment, modified aromatic dicarboxylic acids that may be used in the present disclosure include, but are not limited to, those having up to 20 carbon atoms and which may be linear, para-oriented, or symmetric. Examples of modified aromatic dicarboxylic acids that may be used in the present disclosure include, but are not limited to, isophthalic acid, 4,4'-biphenyl dicarboxylic acid, 1,4-, 1,5-, 2,6-, 2,7-naphthalenedicarboxylic acid, and trans-4,4'-stilbene dicarboxylic acid, and esters thereof. In one embodiment, the modifying aromatic dicarboxylic acid is isophthalic acid.
[0036]
[0042] The carboxylic acid component of the polyesters useful in the present disclosure can be further modified with up to 10 mol%, such as up to 5 mol% or up to 1 mol% of one or more aliphatic dicarboxylic acids containing 2 to 16 carbon atoms, such as cyclohexanedicarboxylic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and / or dodecanedioic acid. Certain embodiments may also include 0.01 to 10 mol%, such as 0.1 to 10 mol%, 1 or 10 mol%, 5 to 10 mol%, etc. of one or more modified aliphatic dicarboxylic acids. Yet another embodiment includes 0 mol% modified aliphatic dicarboxylic acids. The total mol% of the dicarboxylic acid component is 100 mol%. In one embodiment, adipic acid and / or glutaric acid are provided in the modified aliphatic dicarboxylic acid component of the polyesters useful in the present disclosure.
[0037]
[0043] Esters of terephthalic acid and other modified dicarboxylic acids or their corresponding esters and / or salts may be used in place of the dicarboxylic acids. Suitable examples of dicarboxylic acid esters include, but are not limited to, dimethyl, diethyl, dipropyl, diisopropyl, dibutyl, and diphenyl esters. In one embodiment, the esters are selected from at least one of methyl, ethyl, propyl, isopropyl, and phenyl esters.
[0038]
[0044] In one embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure may include 1,4-cyclohexanedimethanol. In another embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure includes 1,4-cyclohexanedimethanol and 1,3-cyclohexanedimethanol. The molar ratio of cis / trans 1,4-cyclohexanedimethanol may vary within the range of 50 / 50 to 0 / 100, for example, 40 / 60 to 20 / 80.
[0039]
[0045] The diol component of the crystallizable polyester compositions and crystallizable polyester blend compositions useful in the present disclosure include, but are not limited to, 1 to 30 mol %, or 1 to 25 mol %, or 1 to 20 mol %, or 1 to 15 mol %, or 1 to 10 mol %, or 2 to 30 mol %, or 2 to 25 mol %, or 2 to 20 mol %, or 2 to 15 mol %, or 2 to 10 mol %, or 3 to 30 mol %, or 3 to 2 ... 5 mol%, or 3 to 20 mol%, or 3 to 15 mol%, or 3 to 10 mol%, 4 to 30 mol%, or 4 to 25 mol%, or 4 to 20 mol%, or 4 to 15 mol%, or 4 to 10 mol%, 5 to 30 mol%, or 5 to 25 mol%, or 5 to 20 mol%, or 5 to 15 mol%, or 5 to 10 mol%, or 6 to 30 mol%, or 6 to 25 mol%, or 6 to 20 mol%, or 6 to 15 mol%, or 6 to 10 mol%, or 7 to 30 mol%, or 7 to 25 mol%, 7 to 20 mol%, or 7 to 15 mol%, or 7 to 10 mol%, or 8 to 30 mol%, or 8 to 25 mol%, or 8 to 20 mol%, or 8 to 15 mol%, or 8 to 10 mol%, or 9 to 30 mol%, or 9 to 25 mol%, or 9 to 20 mol%, or 9 to 15 mol%, or 9 to 10 mol%, or 10 to 30 mol%, or 10 to 25 mol%, or 10 to 20 mol%, or 10 to 15 mol%, or 11 to 30 mol%, or 11 to 30 mol%, or 11 to 25 mol%, or 11 to 20 mol%, or 11 to 15 mol%, or 12 to 30 mol%, or 12 25 mol%, or 12 to 20 mol%, or 12 to 15 mol%, or 13 to 30 mol%, or 13 to 25 mol%, or 13 to 20 mol%, or 13 to 15 mol%, or 14 to 30 mol%, or 14 to 25 mol%, or 14 to 20 mol%, or 14 to 15 mol%, or 15 to 30 mol%, or 15 to 25 mol%, or 15 to 20 mol%, or 16 to 20 mol%, or 18 to 20 mol%, or 10 to 18 mol%, or 16 to 18 mol%, or 12 to 16 mol%, or 16 to 20 mol%, or 1 4-18 mol%, or 11-30 mol%, or 13-30 mol%, or 14-30 mol%, or 10-29 mol%, or 11-29 mol%, or 12-29 mol%, or 13-29 mol%, or 14-29 mol%, or 15-29 mol%, or 10-28 mol%, or 11-28 mol%, or 12-28 mol%, or 13-28 mol%, or 14-28 mol%, or 15-28 mol%. In one embodiment, the sum of 1,4-cyclohexanedimethanol residues and neopentyl glycol residues in the final polyester composition can be from 4 to 15 mol %, or from 2 to 21 mol %, or from 2 to less than 20 mol %, or from 4 to 20 mol %, or from 5 to 18 mol %, or from 10 to 21 mol %, or from 12 to 21 mol %, where the total mol % of the diol components is 100 mol %.
[0040]
[0046] In one embodiment, the diol component of the crystallizable polyester compositions and crystallizable polyester blend compositions useful in the present disclosure may comprise 0-30 mol % neopentyl glycol, based on the total mol % of the diol components being 100 mol %. In one embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure may comprise 0-25 mol % neopentyl glycol, based on the total mol % of the diol components being 100 mol %. In one embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure may comprise 0-17 mol % neopentyl glycol, based on the total mol % of the diol components being 100 mol %. In one embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure may comprise 5-20 mol % neopentyl glycol, based on the total mol % of the diol components being 100 mol %. In one embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure may comprise 10-20 mol % neopentyl glycol, based on the total mol % of the diol component being 100 mol %. In one embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure may comprise 10-15 mol % neopentyl glycol, based on the total mol % of the diol component being 100 mol %. In one embodiment, the diol component of the polyester compositions and polyester blend compositions useful in the present disclosure may comprise 15-25 mol % neopentyl glycol, based on the total mol % of the diol component being 100 mol %.
[0041]
[0047] In one embodiment, the diol component of the crystallizable polyester compositions and crystallizable polyester blend compositions useful in this disclosure may comprise from 0 to 30 mol%, or from 0.01 to 30 mol%, or from 0 to 20 mol%, or from 0.1 to 20 mol%, or from 2 to 20 mol%, or from 0.01 to 15 mol%, or from 0.01 to 14 mol%, or from 0.01 to 13 mol%, or from 0.01 to 12 mol%, or from 0.01 to 11 mol%, or from 0.01 to 10 mol%, or from 0.01 to 9 mol%, or from 0.01 to 16 mol%, based on the total mol% of the diol component being 100 mol%. 8 mol%, or 0.01 to 7 mol%, or 0.01 to 6 mol%, or 0.01 to 5 mol%, or 3 to 15 mol%, or 3 to 14 mol%, or 3 to 13 mol%, or 3 to 12 mol%, or 3 to 11 mol%, or 3 to 10 mol%, or 3 to 9 mol%, or 3 to 8 mol%, or 3 to 7 mol%, or 2 to 10 mol%, or 2 to 9 mol%, or 2 to 8 mol%, or 2 to 7 mol%, or 2 to 5 mol%, or 1 to 7 mol%, or 1 to 5 mol%, or 1 to 3 mol% of 1,4-cyclohexanedimethanol residues.
[0042]
[0048] In one embodiment, the diol component of the crystallizable polyester compositions of the crystallizable polyester compositions and polyester blend compositions useful in this disclosure may comprise 0 to 15 mole % of 1,4-cyclohexanedimethanol, based on the total mole % of the diol components being 100 mole %. In one embodiment, the diol component of the polyester compositions useful in this disclosure may comprise 0.01 to less than ... The diol component of the polyester compositions useful in the present disclosure may comprise 0 to 10 mol % of 1,4-cyclohexanedimethanol, based on the total mole % of the diol components being 100 mol %. In one embodiment, the diol component of the polyester compositions useful in the present disclosure may comprise 0.01 to less than 10 mol % of 1,4-cyclohexanedimethanol, based on the total mole % of the diol components being 100 mol %. In one embodiment, the diol component of the polyester compositions useful in the present disclosure may comprise 0.01 to 5 mol % of 1,4-cyclohexanedimethanol, based on the total mole % of the diol components being 100 mol %. In one embodiment, the diol component of the polyester compositions useful in the present disclosure may comprise 0 to less than 5 mol % of 1,4-cyclohexanedimethanol, based on the total mole % of the diol components being 100 mol %.
[0043]
[0049] Some other diol residues may of course be generated in situ during processing. The total amount of diethylene glycol residues, whether generated in situ during processing or intentionally added, or both, may be present in any amount in the crystallizable polyester blend composition useful in the present disclosure, for example, based on the total mole percent of the diol component being 100 mole percent, 1-15 mole%, or 2-12 mole%, or 2-11 mole%, or 2-10 mole%, or 2-9 mole%, or 3-12 mole%, or 3-11 mole%, or 3-10 mole%, or 3-9 mole%, or 4-12 mole%, or 4-11 mole%, or 4-10 mole%, or 4-9 mole%, or 5-12 mole%, or 5-11 mole%, or 5-10 mole%, or 5-9 mole% of diethylene glycol residues.
[0044]
[0050] In one embodiment, the total amount of diethylene glycol residues that may be present in the polyesters useful in the present disclosure, whether generated in situ during processing, intentionally added, or both, based on the total mole percent of the diol component being 100 mole%, may be 5 mole% or less, 4 mole% or less, or 3.5 mole% or less, or 3.0 mole% or less, or 2.5 mole% or less, or 2.0 mole% or less, or 1.5 mole% or less, or 1.0 mole% or less, or from 1 to 4 mole%, or from 1 to 3 mole%, or from 1 to 2 mole%, or from 2 to 8 mole%, or from 2 to 7 mole%, or from 2 to 6 mole%, or from 2 to 5 mole%, or from 3 to 8 mole%, or from 3 to 7 mole%, or from 3 to 6 mole%, or from 3 to 5 mole%, or in some embodiments, there are no intentionally added diethylene glycol residues. In certain embodiments, no modifying diols are added to the polyesters. In certain embodiments, the crystallizable polyester composition of the polyester blend composition may have diethylene glycol residues of 5 mole percent or less.
[0045]
[0051] In one embodiment, the diol component of the crystallizable polyester blend composition useful in the present disclosure may contain up to 20 mol%, or up to 19 mol%, or up to 18 mol%, or up to 17 mol%, or up to 16 mol%, or up to 15 mol%, or up to 14 mol%, or up to 13 mol%, or up to 12 mol%, or up to 11 mol%, or up to 10 mol%, or up to 9 mol%, or up to 8 mol%, or up to 7 mol%, or up to 6 mol%, or up to 5 mol%, or up to 4 mol%, or up to 3 mol%, or up to 2 mol%, or up to 1 mol% of one or more modified diols (modified diols are defined as diols that are not ethylene glycol, diethylene glycol, neopentyl glycol, or 1,4-cyclohexanedimethanol). In certain embodiments, the polyesters useful in the present disclosure may contain up to 10 mol% of one or more modified diols. In certain embodiments, the polyesters useful in the present disclosure may contain up to 5 mol% of one or more modified diols. In certain embodiments, polyesters useful in the present disclosure may contain up to 3 mole percent of one or more modified diols. In other embodiments, polyesters useful in the present disclosure may contain 0 mole percent modified diols. However, some other diol residues may be generated in situ, so the amount of residues generated in situ may also be determined by the mole percent of the modified diol. This may be considered an embodiment of the present disclosure.
[0046]
[0052] In some embodiments, the modifying diols used in the crystallizable polyester blend composition defined herein, if used, contain 2 to 16 carbon atoms. Examples of modifying diols include, but are not limited to, 1,2-propanediol, 1,3-propanediol, isosorbide, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol, polytetramethylene glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD), and mixtures thereof. In one embodiment, isosorbide is the modifying diol. In another embodiment, the modifying diols include, but are not limited to, at least one of 1,3-propanediol and 1,4-butanediol. In one embodiment, 1,3-propanediol and / or 1,4-butanediol may be excluded. When 1,4- or 1,3-butanediol is used, in one embodiment, it may provide more than 4 mol% or more than 5 mol%. In one embodiment, the at least one modifying diol is 1,4-butanediol present in an amount of 5 to 25 mole %.
[0053] In all embodiments, the remainder of the diol component may contain any amount of ethylene glycol residues, based on the total mole percent of the diol component being 100 mole percent. In one embodiment, the crystallizable polyester blend composition useful in the present disclosure may contain 50 mole percent or more, or 55 mole percent or more, or 60 mole percent or more, or 65 mole percent or more, or 70 mole percent or more, or 75 mole percent or more, or 80 mole percent or more, or 85 mole percent or more, or 90 mole percent or more, or 95 mole percent or more, or 50-80 mole percent, or 55-80 mole percent, or 60-80 mole percent, or 50-75 mole percent, or 55-75 mole percent, or 60-75 mole percent, or 65-75 mole percent, of ethylene glycol residues, based on the total mole percent of the diol component being 100 mole percent.
[0047]
[0054] In one embodiment, there is provided a shrink film comprising a crystallizable polyester blend composition (i.e., components (1) and (2)) further comprising: 1,4-cyclohexanedimethanol residues present in an amount of 0.01 to about 10 mole %, diethylene glycol residues present in an amount of 2-9 mole %, neopentyl glycol residues present in an amount of 5-30 mole %, and ethylene glycol residues present in an amount of 60 mole % or greater, based on the total mole % of the diol component being 100 mole %.
[0048]
[0055] In one embodiment, the crystallizable polyester blend composition comprises: The present invention provides a shrink film comprising 1,4-cyclohexanedimethanol residues present in an amount of 0.01 to about 5 mole %, diethylene glycol residues present in an amount of 1 to 9 mole %, neopentyl glycol residues present in an amount of 5 to 25 mole %, and ethylene glycol residues present in an amount of 60 mole % or greater, based on the total mole % of the diol component being 100 mole %.
[0049]
[0056] In one embodiment, there is provided a shrink film comprising a crystallizable polyester blend composition comprising: 1,4-cyclohexanedimethanol residues present in an amount of about 10 to about 20 mole %, diethylene glycol residues present in an amount of 1 to 10 mole %, neopentyl glycol residues present in an amount up to about 1 mole %, and ethylene glycol residues present in an amount of 60 mole % or greater, based on the total mole % of the diol component being 100 mole %.
[0050]
[0057] In one embodiment, there is provided a shrink film comprising a crystallizable polyester blend composition comprising: 1,4-cyclohexanedimethanol residues are present in an amount of 2-7 mole %, diethylene glycol residues are present in an amount less than 10 mole %, neopentyl glycol residues are present in an amount of 5-20 mole %, and ethylene glycol residues are present in an amount greater than 60 mole %, based on the total mole % of the diol component being 100 mole %.
[0051]
[0058] In one embodiment, there is provided a shrink film comprising a crystallizable polyester blend composition comprising: 1,4-cyclohexanedimethanol residues are present in an amount less than 10 mole %, diethylene glycol residues are present in an amount between 1 and 10 mole %, neopentyl glycol residues are present in an amount greater than 5 mole %, and ethylene glycol residues are present in an amount equal to or greater than 60 mole %, based on the total mole % of the diol component being 100 mole %.
[0052]
[0059] In one embodiment, a shrink film is provided in which the total amount of one or more diol monomer components capable of forming an amorphous polyester composition in the polyester blend composition is 20-45 mol%, or 22-45 mol%, or 20-40 mol%, or 24-40 mol%, or 30-45 mol%, or 25-45 mol%, or 25-40 mol%, or 25-35 mol%, where the total mol% of the diol component content is 100 mol%.
[0053]
[0060] In one embodiment, a shrink film is provided in which the combined total of residues of 1,4-cyclohexanedimethanol and neopentyl glycol residues in the amorphous polyester composition of the polyester blend is 12-35 mol %, or 15-40 mol %, or 15-35 mol %, or 20-40 mol %, or 25-40 mol %, or 20-45 mol %, or 25-35 mol %, where the total mole % of the diol component is 100 mol %.
[0054]
[0061] In one embodiment of the present disclosure, a crystallizable film is provided that includes a mixture of polyester compositions that include: (1) at least one crystallizable polyester that includes terephthalic acid residues, and 0 to about 20 mol %, or 0 to about 17 mol %, or about 1 to about 20 mol %, or about 1 to about 17 mol %, or about 5 to about 20 mol % neopentyl glycol (NPG) residues, and 0 to about 20 mol %, or 0 to about 17 mol %, or about 1 to about 20 mol %, or about 1 to about 17 mol %, or about 5 to about 20 mol % 1,4-cyclohexanedimethanol (CHDM), and less than about 5 mol % diethylene glycol (DEG) residues, with the balance being ethylene glycol (EG) residues; and (2) terephthalic acid residues, and 0 to about 40 mol % %, or 0 to about 30 mol %, or about 1 to about 40 mol %, or about 10 to about 20 mol %, or about 10 to about 40 mol %, or about 5 to about 30 mol % neopentyl glycol (NPG), and 0 to about 40 mol %, or 0 to about 35 mol %, or about 1 to about 30 mol %, or about 10 to about 40 mol %, or about 20 to about 40 mol % 1,4-cyclohexanedimethanol (CHDM), and 1 to about 15 mol %, or 2 to about 10 mol %, or about 5 to about 15 mol %, or about 5 to about 10 mol % diethylene glycol (DEG), the remainder being ethylene glycol (EG) residues.
[0055]
[0062] In some embodiments, polyester compositions according to the present disclosure may include 0-10 mol %, e.g., 0.01-5 mol %, 0.01-1 mol %, 0.05-5 mol %, 0.05-1 mol %, or 0.1-0.7 mol % of one or more branching monomer residues, based on the total mol % of either diol residues or diacid residues, respectively, the branching monomer, also referred to herein as a branching agent, having three or more carboxyl substituents, hydroxyl substituents, or combinations thereof. In certain embodiments, the branching monomer or branching agent may be added prior to and / or during and / or after the polymerization of the polyester. Thus, in some embodiments, the polyesters useful in the present disclosure may be linear or branched.
[0056]
[0063] Examples of branching monomers include, but are not limited to, polyfunctional acids or polyfunctional alcohols such as trimellitic acid, trimellitic anhydride, pyromellitic dianhydride, trimethylolpropane, glycerol, pentaerythritol, citric acid, tartaric acid, 3-hydroxyglutaric acid, etc. In one embodiment, the branching monomer residue is trimellitic anhydride, pyromellitic dianhydride, glycerol, sorbitol, 1,2,6-hexanetriamine ... The branching monomer may comprise 0.1 to 0.7 mole % of one or more residues selected from at least one of ethanol, pentaerythritol, trimethylolethane, and / or trimesic acid. The branching monomer may be added to the polyester reaction mixture in the form of a concentrate or may be mixed with the polyester, for example, as explained in U.S. Patent Nos. 5,654,347 and 5,696,176, the disclosures of which are incorporated herein by reference with respect to branching monomers.
[0057]
[0064] The polyesters useful in the present disclosure may include at least one chain extender. Suitable chain extenders include, but are not limited to, polyfunctional (such as, but not limited to, difunctional) isocyanates, polyfunctional epoxides such as epoxidized novolacs, and phenoxy resins. In certain embodiments, the chain extender may be added at the end of the polymerization process or after the polymerization process. If added after the polymerization process, the chain extender may be incorporated by compounding or by adding during a conversion process such as injection molding or extrusion.
[0058]
[0065] The amount of chain extender used may vary depending on the particular monomer composition used and the physical properties desired, but is generally from about 0.1% to about 10% by weight, for example from about 0.1% to about 5% by weight, based on the total weight of the polyester.
[0059]
[0066] It is believed that the polyester blend composition useful in the present disclosure may have at least one of the intrinsic viscosity ranges described herein, and at least one of the monomer ranges of the polyester composition described herein, unless otherwise specified. It is also believed that the polyester blend composition useful in the present disclosure may have at least one of the Tg ranges described herein, and at least one of the monomer ranges of the polyester composition described herein, unless otherwise specified. It is also believed that the polyester composition useful in the present disclosure may have at least one of the intrinsic viscosity ranges described herein, at least one of the Tg ranges described herein, and at least one of the monomer ranges of the polyester composition described herein, unless otherwise specified.
[0060]
[0067] In embodiments of the present disclosure, the polyester compositions useful in the present disclosure may exhibit at least one of the following intrinsic viscosity values measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at 25° C. and a concentration of 0.5 g / dL: 0.50-1.2 dL / g; 0.50-1.0 dL / g; 0.50-0.90 dL / g; 0.50-0.80 dL / g; 0.55-0.80 dL / g; 0.60-0.80 dL / g; 0.65-0.80 dL / g; 0.70-0.80 dL / g; 0.50-0.75 dL / g; 0.55-0.75 dL / g; or 0.60-0.75 dL / g.
[0061]
[0068] The glass transition temperature (Tg) of the polyester of the polyester blend composition is measured using a TA DSC 2920 manufactured by Thermal Analyst Instrument at a scan rate of 20° C. / min. The value of the glass transition temperature is measured during the second heating.
[0062]
[0069] In certain embodiments, the oriented or shrink films of the present disclosure comprise polyester / polyester compositions in which the polyester has a Tg of 60-80° C., 70-80° C., 65-80° C., or 65-75° C. In certain embodiments, these Tg ranges can be met regardless of whether or not at least one plasticizer is added during polymerization.
[0063]
[0070] In an embodiment of the present disclosure, a particular oriented film and / or shrinkable film comprising a polyester and / or polyester composition useful in the present disclosure may have all of the following properties: excellent stretchability, controlled shrinkage properties, particular toughness, particular intrinsic viscosity, particular glass transition temperature (Tg), particular strain-induced crystalline melting point, particular flexural modulus, particular density, particular The composition may have a unique combination of a certain tensile modulus, a particular surface tension, excellent melt viscosity, excellent clarity, and excellent color.
[0064]
[0071] In one embodiment, certain polyester blend compositions useful in the present disclosure may be visually clear, the term "visually clear" being defined herein as the apparent absence of haze, mist, and / or turbidity upon visual inspection.
[0065]
[0072] The polyester portion of the polyester blend composition useful in the present disclosure (both amorphous and crystallizable compositions) may be prepared by methods known from the literature, such as in homogeneous solution, by transesterification in the melt, and by two-phase interface. Suitable methods include, but are not limited to, reacting one or more dicarboxylic acids with one or more diols at temperatures between 100° C. and 315° C. and pressures between 0.1 and 760 mm Hg for a time sufficient to produce a polyester. For methods of producing polyesters, see U.S. Pat. No. 3,772,405, the disclosure of which is incorporated herein by reference. Can be enjoyed.
[0066]
[0073] Generally, polyesters may be prepared by condensing dicarboxylic acids or dicarboxylic esters with diols in the presence of a catalyst at elevated temperatures, gradually increasing during the condensation to temperatures of about 225° C. to 310° C. in an inert atmosphere, and at lower pressures during the latter part of the condensation, as explained in more detail in U.S. Pat. No. 2,720,507, which is incorporated herein by reference. It may also be prepared by condensation with
[0067]
[0074] In some embodiments, during the manufacturing process of the polyester blend compositions useful in the present disclosure, certain chemicals that color the polymer may be added to the melt containing the toner or pigment. In one embodiment, the resulting polyester polymer melt phase product b * Bluing toners are added to the melt to reduce the bluing effect. Such bluing agents include blue inorganic and organic toners and / or pigments. Red toners and / or pigments are also used to reduce the bluing effect. * The color tone of the polyester may be adjusted. Organic toners, such as those described in U.S. Patent Nos. 5,372,864 and 5,384,377, which are incorporated by reference in their entirety, may be used, for example, blue and red organic toners. The organic toners may be provided as a premixed composition. The premixed composition may be a neat mixture of the red and blue compounds, or the composition may be pre-dissolved or pre-slurried in one of the raw materials of the polyester, such as ethylene glycol.
[0068]
[0075] The total amount of toner components added depends on the amount of inherent yellow color in the base polyester and the potency of the toner. In one embodiment, mixed organic toner components may be used at a maximum concentration of about 15 ppm and a minimum concentration of about 0.5 ppm. In one embodiment, the total amount of bluing additive may range from 0.5 to 10 ppm. In one embodiment, the toner may be added to the esterification reaction zone or the polycondensation reaction zone. Preferably, the toner is added to the esterification reaction zone or at an early stage of the polycondensation zone, such as in a prepolymerization reactor, or the toner may be added during compounding or during the extrusion process after polymerization.
[0069]
[0076] The present disclosure further relates to a polymer blended with a crystallizable polyester composition as part of a polyester blend composition, in one embodiment, the blended composition comprises (a) 5 to 80 weight percent of the crystallizable polyester composition of the present disclosure described herein, and (b) 20 to 95 weight percent of at least one polymer component (i.e., a component other than the blend of the present disclosure).
[0070]
[0077] Suitable examples of polymeric components include, but are not limited to, nylon; polyesters other than those described herein; polyamides such as ZYTEL® from DuPont; polystyrene; Polystyrene copolymers; styrene-acrylonitrile copolymers; acrylonitrile butadiene styrene copolymers; polymethyl methacrylate; acrylic copolymers; polyetherimides such as ULTEM® (polyetherimides manufactured by SABIC); poly(2,6-dimethylphenyl Polyphenylene oxides such as NORYL 1000(R) (a mixture of poly(2,6-dimethylphenylene oxide) and polystyrene resins manufactured by SABIC) or polyphenylene oxide / polystyrene blends such as NORYL 1000(R) (a mixture of poly(2,6-dimethylphenylene oxide) and polystyrene resin manufactured by SABIC); polyphenylene sulfide; polyphenylene sulfide / sulfone; polyester carbonate; LEXAN(R) (a polycarbonate manufactured by SABIC) polycarbonates such as polycarbonates (polycarbonates); polysulfones; polysulfone ethers; and polyether ketones of aromatic dihydroxy compounds; or mixtures of any of the aforementioned polymers. In one embodiment, aliphatic-aromatic polyesters may be excluded from the polyester compositions useful in the present disclosure. The following polyesters that can be blended to make the polyester compositions of the present disclosure may be excluded as polymeric components for addition and blending if the blending exceeds the composition ranges of the present disclosure: polyethylene terephthalate (PET), glycol-modified PET (PETG), glycol-modified polycyclohexylene dimethylene terephthalate (PCTG), polycyclohexylene dimethylene terephthalate (PCT), acid-modified polycyclohexylene dimethylene terephthalate (PCTA), polybutylene terephthalate, and / or diethylene glycol-modified PET (East BONDE TM Copolymer polyester ).
[0071]
[0078] The mixture may be prepared by conventional processing techniques known in the art such as melt blending or solution blending.
[0079] In some embodiments, the polyester compositions and polymer blend compositions may also contain common additives such as colorants, toners, pigments, release agents, flame retardants, plasticizers, glass bubbles, nucleating agents, stabilizers such as, but not limited to, UV stabilizers, heat stabilizers, and / or reaction products thereof, fillers, and impact modifiers, at 0.01 to 25% by weight of the total composition. Examples of commercially available impact modifiers include, but are not limited to, ethylene / propylene terpolymers, functionalized polyolefins such as methyl acrylate and / or glycidyl methacrylate, styrenic block copolymer impact modifiers, and various acrylic core / shell impact modifiers. Residues of such additives are also contemplated as part of the polyester composition.
[0072]
[0080] Reinforcing materials may be added to the compositions useful in the present disclosure. Reinforcing materials may include, but are not limited to, carbon fibers, silicates, mica, clays, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, polymeric fibers, and combinations thereof. In one embodiment, reinforcing materials include glass materials such as mixtures of fibrous glass filaments, glass and talc, glass and mica, and glass and polymeric fibers.
[0073]
[0081] In one embodiment, films and shrink films according to the present disclosure may comprise 0.01 to 10 weight percent polyester plasticizer. In one embodiment, shrink films may comprise 0.1 to 5 weight percent polyester plasticizer. In general, shrink films may comprise 90 to 99.99 weight percent copolyester. In a particular embodiment, shrink films may comprise 95 to 99.9 weight percent copolyester.
[0074]
[0082] In one aspect, the present disclosure relates to methods of shrink film and molded articles of the present disclosure comprising the polyester compositions and / or polymer blends useful in the present disclosure. Methods of forming the polyesters and / or blends into films and / or sheets are well known in the art. Examples of films and / or sheets useful in the present disclosure include, but are not limited to, extruded films and / or sheets, compression molded films and / or sheets, calendered films and / or sheets, solution cast films and / or sheets. In one aspect, methods of making films and / or sheets useful for making the shrink films of the present disclosure include, but are not limited to, methods of making films and / or sheets useful for making the shrink films of the present disclosure. These include, but are not limited to, extrusion, compression molding, calendaring, and casting.
[0075]
[0083] In one embodiment, the polyester compositions useful in this disclosure are made into films using any method known in the art for making films from polyesters, such as solution casting, extrusion, compression molding, or calendaring.
[0076]
[0084] In one embodiment, the as-formed film is subsequently oriented in one or more directions (e.g., as a uniaxially and / or biaxially oriented film). This orientation of the film can be carried out by any method known in the art using standard orientation conditions. For example, an oriented film of the present disclosure may be produced from a film having a thickness of about 100-400 μm, such as an extruded, cast, or calendered film, which may be oriented at a temperature of Tg to Tg+55° C. in a ratio of 5:1 to 3:1, such as a ratio of 5:1 or 3:1 at a temperature of 70° C. to 125° C., and the film may be oriented to a thickness of 20 to 80 μm. In one embodiment, the orientation of the initial as-formed film may be carried out in a tenter frame according to these orientation conditions.
[0077]
[0085] Shrink films of the present disclosure may have a shrink initiation temperature of from about 55 to about 80° C., or from about 55 to about 75° C., or from about 55 to about 70° C. The shrink initiation temperature is the temperature at which the initiation of shrinkage occurs.
[0078]
[0086] In certain embodiments, polyester compositions useful in the present disclosure may have a density of 1.6 g / cc or less, or 1.5 g / cc or less, or 1.4 g / cc or less, or from 1.1 g / cc to 1.5 g / cc, or from 1.2 g / cc to 1.4 g / cc, or from 1.2 g / cc to 1.35 g / cc.
[0079]
[0087] In one embodiment, many small voids or holes are introduced into the film or molded article to reduce the density of the film. This process is called "voiding" and This is sometimes called "cavitating" or "microvoiding". These pores are obtained by incorporating about 1 to about 50% by weight of small organic or inorganic (including glass microspheres) particles or "inclusions" (known in the art as "pore-forming" or "void-forming" agents) into a matrix polymer and stretching in at least one direction to orient the polymer. During stretching, small cavities or voids are formed around the void-forming agents. When voids are introduced into a polymer film, the resulting voided film is not only less dense than a nonvoided film, but also becomes opaque and develops a paper-like surface. This surface also has the advantage of improving printability, i.e., the surface can accept more ink in a substantially larger volume than a nonvoided film. Typical examples of holed films are shown in U.S. Patent Nos. 3,426,754; 3,944,699; 4,138,459; 4,582,752; 4,632,869; 4,770,931; 5,176,954; 5,435,955; 5,843,578; 6,004,664; 6,287,68 0; 6,500,533; 6,720,085; U.S. Patent Application Publication Nos. 2001 / 0036545; 2003 / 0068453; 2003 / 0165671; 2003 / 0170427; Japanese Patent Application Publication Nos. 61-037827; 63-193822; 2004-181863; European Patent Application Publication No. 0 581 970 B1; and European Patent Application Publication No. 0 214 859 A2.
[0080]
[0088] In certain embodiments, the as-formed or as-extruded film is oriented during stretching. The oriented or shrinkable films of the present disclosure can be made from films of any thickness depending on the desired end use. In one embodiment, a desirable condition is that the oriented and / or shrinkable film can be printed with ink for applications such as labels, photographic films that can be adhered to substrates such as paper, and / or other applications in which they may be useful. The polyesters useful in the present disclosure are P It may be desirable to coextrude with another polymer, such as ET, to enable the film to be used as an oriented film and / or a shrink film of the present disclosure. One advantage of performing the latter coextrusion is that, in some embodiments, a tie layer is not required. That's a good thing.
[0081]
[0089] In one embodiment, the uniaxially and biaxially oriented films of the present disclosure may be made from a film, such as an extruded, cast, or calendered film, having a thickness of about 100-400 μm, which may be stretched in one or more directions at a ratio of 6.5:1 to 3:1 at a temperature from the Tg of the film to Tg+55° C., and may have a thickness of 20-80 μm. In one embodiment, orientation of the initial as-extruded film may be performed in a tenter frame according to these orientation conditions. Shrink films of the present disclosure can be made from the oriented films of the present disclosure.
[0082]
[0090] In certain embodiments, the shrink films of the present disclosure shrink slowly with little or no wrinkling. In certain embodiments, the shrink films of the present disclosure have a shrink percentage in the main shrink direction of 40% or less per 5° C. increment of temperature increase.
[0083]
[0091] In certain embodiments of the present disclosure, the shrink films of the present disclosure have a shrinkage in the machine direction (i.e., perpendicular to the main shrink direction) of 10% or less, or 5% or less, or 3% or less, or 2% or less, or no shrinkage, when immersed in water at 65° C. for 10 seconds. In certain embodiments of the present disclosure, the shrink films of the present disclosure have a shrinkage in the machine direction of -5% to 10%, -5% to 5%, or -5% to 3%, or -5% to 2%, or -4% to 5%, or -3% to 5%, or -2% to 5%, or -2% to 3%, or -2% to 2%, or 0 to 2%, or no shrinkage, when immersed in water at 65° C. for 10 seconds. A negative shrinkage in the machine direction indicates expansion in the machine direction. A positive shrinkage in the machine direction indicates shrinkage in the machine direction.
[0084]
[0092] In certain embodiments of the present disclosure, the shrink films of the present disclosure have a shrink percentage in the main shrink direction when immersed in 95° C. water for 10 seconds of 50% or more, or 60% or more, or 70% or more.
[0085]
[0093] In certain embodiments of the present disclosure, the shrink film of the present disclosure has a shrinkage percentage of 50-90% in the main shrink direction and a shrinkage percentage of 10% or less, or -10% to 10%, in the machine direction when immersed in 95° C. water for 10 seconds.
[0086]
[0094] In one embodiment, the polyesters useful in the present disclosure are made into a film using any method known in the art for making films from polyesters, such as solution casting, extrusion, compression molding, or calendaring. The as-extruded (or as-formed) film is then oriented in one or more directions (e.g., uniaxially and / or biaxially oriented film). This orientation of the film may be carried out by any method known in the art using standard orientation conditions. For example, a uniaxially oriented film of the present disclosure may be made from a film, such as an extruded, cast, or calendared film, having a thickness of about 100-400 μm, which may be stretched at a ratio of 6.5:1 to 3:1 at a temperature from the Tg of the film to Tg+55° C., and stretched to a thickness of 20-80 μm. In one embodiment, the orientation of the initial as-extruded film may be carried out in a tenter frame according to these orientation conditions.
[0087]
[0095] In certain embodiments of the present disclosure, the shrink films of the present disclosure may have a shrink initiation temperature of from about 55 to about 80° C., or from about 55 to about 75° C., or from 55 to about 70° C. The shrink initiation temperature is the temperature at which the initiation of shrinkage occurs.
[0088]
[0096] In certain embodiments of the present disclosure, the shrink films of the present disclosure may have a shrink initiation temperature of from 55°C to 70°C.
[0097] In certain embodiments of the present disclosure, the shrink films of the present disclosure may have a breaking strain of greater than 200% at a stretch rate of 500 mm / min in the direction perpendicular to the main shrink direction according to ASTM method D882.
[0089]
[0098] In certain embodiments of the present disclosure, the shrink films of the present disclosure may have a breaking strain of greater than 300% at a stretch rate of 500 mm / min in the direction perpendicular to the main shrink direction according to ASTM method D882.
[0090]
[0099] In certain embodiments of the present disclosure, the shrink films of the present disclosure may have a tensile stress at break (stress at break) measured according to ASTM method D882 of from 20 to 400 MPa, or from 40 to 260 MPa, or from 42 to 260 MPa, or from 20 to 100 MPa.
[0091]
[0100] In certain embodiments of the present disclosure, the shrink films of the present disclosure are Depending on the end use of the label, the label may have a shrink force of 4-18 MPa, or 4-15 MPa, as measured by ISO Method 14616. For example, a particular label made for plastic bottles may have a shrink force of 4-8 MPa, and a particular label made for glass bottles may have a shrink force of 10-14 MPa, as measured by ISO Method 14616 at 80° C. using a LabThink shrink force tester.
[0092]
[0101] In one embodiment of the present disclosure, the polyester composition is typically The monomers may be reacted by known methods to produce polyesters, which are referred to as compositions of the invention.
[0093]
[0102] In one embodiment of the present disclosure, the polyester composition of the present disclosure is phthalate (PET), glycol modified PET (PETG), glycol modified polycyclohexylene dimethylene terephthalate (PCTG), polycyclohexylene dimethylene terephthalate (PCT), acid modified polycyclohexylene dimethylene terephthalate (PCTA), polybutylene terephthalate, and / or diethylene glycol modified PET (EASTOBOND TM Polyesters such as copolymer polyesters are included in the monomer range of these compositions. The mixture may be mixed to reach the desired range.
[0094]
[0103] In certain embodiments, the polyester compositions and polymer blend compositions also include Common additives such as colorants, toners, pigments, release agents, flame retardants, plasticizers, glass bubbles, nucleating agents, stabilizers including but not limited to UV stabilizers, heat stabilizers, and / or reaction products thereof, fillers, and impact modifiers may be included at 0.01 to 25% by weight of the total composition. Examples of commercially available impact modifiers include but are not limited to ethylene / propylene terpolymers, functionalized polyolefins such as polyolefins containing methyl acrylate and / or glycidyl methacrylate, styrenic block copolymer impact modifiers, and various acrylic core / shell impact modifiers. Residues of such additives are also contemplated as part of the polyester composition.
[0095]
[0104] Reinforcing materials may be added to the polyester compositions useful in the present disclosure. Reinforcing materials include: These may include, but are not limited to, carbon fibers, silicates, mica, clays, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, polymeric fibers, and combinations thereof. In one embodiment, the reinforcing material includes glass materials such as mixtures of fibrous glass filaments, glass and talc, glass and mica, and glass and polymeric fibers.
[0096]
[0105] Molded articles can be made from any of the polyester compositions disclosed herein, which may consist of or include a shrink film, and are included within the scope of this disclosure.
[0097]
[0106] Generally, shrink films according to the present disclosure may comprise 0.01 to 10 weight percent polyester plasticizer. In one embodiment, the shrink film may comprise 0.1 to 5 weight percent polyester plasticizer. Generally, the shrink film may comprise 90 to 99.99 weight percent copolyester. In a particular embodiment, the shrink film may comprise 95 to 99.9 weight percent copolyester.
[0098]
[0107] In one embodiment, when having a pre-oriented thickness of about 100-400 μm and then oriented in a tenter frame at a temperature of from Tg to Tg+55° C. and a ratio of 6.5:1 to 3:1 to a thickness of about 20 to about 80 μm, the shrink film of the present disclosure exhibits the following properties: (1) when immersed in water at 95° C. for 10 seconds, it shrinks by an amount greater than 50% (or greater than 60%) in the main shrinkage or transverse direction and shrinks by 10% or less (or −10% to 10%) in the machine direction; (2) when immersed in water at about 55° C. to about (3) a shrink onset temperature of 70° C., (4) a strain at break of greater than 200%, or 200-600%, or 200-500%, or 226-449%, or 250-455%, in the transverse direction, machine direction, or both, at a stretch rate of 500 mm / min, in accordance with ASTM method D882, (5) a shrinkage of 40% or less per 5° C. temperature increase increment, and / or (6) a melting point of strain-induced crystallinity of greater than 190° C., as measured on the first heat of a DSC scan in accordance with ASTM. Any combination of these properties, or all of these properties, may be present in a shrink film of the present disclosure. A shrink film of the present disclosure may have a combination of two or more of the shrink film properties described above. A shrink film of the present disclosure may have a combination of three or more of the shrink film properties described above. A shrink film of the present disclosure may have a combination of four or more of the shrink film properties described above. In certain embodiments, properties (1)-(2) are present. In certain embodiments, characteristics (1)-(5) are present. In certain embodiments, characteristics (1)-(3), etc. are present.
[0099]
[0108] The shrinkage percentages herein are based on initial as-produced films having a thickness of about 20-80 μm that have been oriented in a tenter frame at a ratio of 6.5:1 to 3:1 at temperatures from Tg to Tg+55° C., such as a ratio of 5:1 at temperatures from 70° C. to 85° C. In one embodiment, the shrink properties of the oriented films used to make the shrink films of the present disclosure were unchanged when the films were annealed at a temperature higher than the temperature at which they were oriented. In other embodiments, the shrink properties may be adjusted by heat treatment.
[0100]
[0109] The shape of the film useful for making the oriented or shrink film of the present disclosure is not subject to any limitations. For example, the shape may be a flat film or a film formed into a tube. To produce a shrink film useful in the present disclosure, the polyester is first formed into a flat film and then "uniaxially stretched", which means that the polyester film is oriented in one direction. The ends of the stretched film are then joined using a stitching solvent or stitching adhesive to form a shrinkable tube. The film may also be "biaxially oriented", which means that the polyester film is oriented in two different directions, for example, the film is stretched in both the machine direction and a direction different from the machine direction. Typically, the two directions are substantially perpendicular, but this is not always the case. For example, in one embodiment, the two directions are the longitudinal or machine direction ("MD") of the film (the direction in which the film is produced on the film-making machine) and the transverse direction ("TD") of the film (the direction perpendicular to the MD of the film). Biaxially oriented films may be sequentially oriented, simultaneously oriented, or some combination of simultaneous and sequential stretching. It may be oriented by
[0101]
[0110] The film is stretched by rolls, long-gap stretching, tenter, etc. Orientation may be accomplished by any conventional method, such as frame stretching, and tubular stretching. Any of these methods may be used to achieve sequential biaxial stretching, simultaneous biaxial stretching, uniaxial stretching, or a combination thereof. Biaxial stretching as described above may achieve simultaneous machine and transverse stretching. Stretching may also be accomplished first in one direction and then in the other direction, effectively resulting in biaxial orientation. In one embodiment, film stretching is accomplished by preheating the films to 5° C. to 80° C. above their glass transition temperature (Tg). In one embodiment, the films may be preheated to 10° C. to 30° C. above their Tg. In one embodiment, the stretching speed is 5 to 20 inches (12.7 to 50.8 cm) per second. The film may then be oriented, for example, to 2 to 6 times its original dimensions in either the machine direction, the transverse direction, or both directions. The film may be oriented as a single film layer or may be coextruded with another polymeric material such as PET (polyethylene terephthalate) or polyester as a multilayer film and then oriented.
[0102]
[0111] In one embodiment, the present disclosure provides a method for producing a shrink film comprising the steps of: In another embodiment, the present disclosure includes an article of manufacture or a molded article comprising an oriented film of any of the embodiments of the oriented films of the present disclosure.
[0103]
[0112] In certain embodiments, the present disclosure includes, but is not limited to, shrink films applied to containers, plastic bottles, glass bottles, packaging, batteries, hot-fill containers, and / or industrial products or other applications. In one embodiment, the present disclosure includes, but is not limited to, oriented films applied to containers, packaging, plastic bottles, glass bottles, photographic substrates such as paper, batteries, hot-fill containers, and / or industrial products or other applications.
[0104]
[0113] In certain embodiments of the present disclosure, the shrink films of the present disclosure may be formed into a label or sleeve, which may then be applied to the wall of a container, an article of manufacture such as a battery, or over a sheet or film.
[0105]
[0114] The oriented or shrink films of the present disclosure can be used in the form of sheets, films, tubes, bottles, etc. and are commonly used in a variety of packaging applications. For example, films and sheets made from polymers such as polyolefins, polystyrene, polyvinyl chloride, polyester, polylactic acid (PLA), etc. are frequently used to make shrinkable labels for plastic beverage or food containers. For example, the shrinkable films of the present disclosure can be used in many packaging applications, where the molded article exhibits properties such as excellent printability, high opacity, excellent shrink force, excellent texture, and high stiffness after application of the shrink film.
[0106]
[0115] The combination of improved shrink properties and increased toughness can be used in applications including, but not limited to, containers. The present invention could provide new commercial options for applications such as plastic bottles, glass bottles, packaging, batteries, hot fill containers, and / or shrink films applied to industrial products or other uses.
[0107]
[0116] In one aspect of the present disclosure, the disclosed polyester blend composition is a thermoformed, and / or thermoformable films or sheets. The present disclosure is also directed to articles of manufacture incorporating the thermoformed films and / or sheets of the present disclosure. In one embodiment, the polyester blend compositions of the present disclosure are useful as films and sheets that are easily formed into molded or shaped articles. In one embodiment, the films and / or sheets of the present disclosure can be processed into molded articles or parts by thermoforming. The polyester blend compositions of the present disclosure are useful as films and sheets that are easily formed into molded or shaped articles. In one embodiment, the films and / or sheets of the present disclosure can be processed into molded articles or parts by thermoforming. The polyester compositions can be used in a variety of molding and extrusion applications.
[0108]
[0117] Further, in one embodiment, polyester compositions useful in the thermoformed sheets of the present disclosure include The polyester blend composition may also contain common additives such as colorants, lubricants, antiblocking agents, release agents, flame retardants, plasticizers, nucleating agents, stabilizers such as, but not limited to, UV stabilizers, heat stabilizers, fillers, and impact modifiers, in amounts of 0.1 to 25% by weight of the total composition.
[0109]
[0118] In one embodiment, the reinforcement is a thermoformed polyester comprising the polyester composition of the present disclosure. For example, suitable reinforcing materials may include carbon fibers, silicates, mica, clays, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, polymeric fibers, and combinations thereof.
[0110]
[0119] In one embodiment, the thermoformed film or sheet of the present disclosure is a multi-layer film. In one embodiment, at least one layer of the multilayer film or sheet is a foam layer, or a foamed polymer or polyester layer.
[0111]
[0120] One aspect of the present disclosure is to provide parts and articles formed or molded using thermoforming. Methods of Manufacture Any thermoforming technique or process known to one of ordinary skill in the art can be used to manufacture the formed or molded articles of the present disclosure.
[0112]
[0121] In one embodiment, the thermoforming process can be carried out in several ways, for example as taught in "Technology of Thermoforming" (Throne, James; Hanser Publishers; 1996; pp. 16-29), which is incorporated herein by reference. In some embodiments, the process is a male thermoforming process in which gas or air pressure is applied to the softened sheet, which then stretches and draws the sheet like a bubble, and a male mold is placed inside the bubble from the inside. A vacuum is then applied to further draw the part to conform to the surface of the male mold. In this thermoforming process, biaxial stretching / orientation is primarily performed in one step as gas or air pressure is applied to the softened sheet. The forming step is then completed using vacuum and a male mold to lock the orientation into the sheet after cooling for a good balance of physical and cosmetic properties. In another embodiment, the process is a female mold process where a vacuum or physical plug is applied to the heat softened sheet to stretch and draw the sheet to approximately the final part dimensions, then internal positive air pressure or additional external vacuum is applied to draw the sheet into an external female mold, fixing the orientation in the polymer after cooling and forming the sheet into an article.
[0113]
[0122] In some embodiments, the bubble formation is further induced by utilizing a plug assist device. Following this, a sheet is covered and molded over the rising male mold, and then a vacuum is applied to pull the corners, sleeve guides, etc. into the mold. In some embodiments, after removal from the mold, the formed part or article can be cut, punched, cornered, etc., as needed.
[0114]
[0123] In another embodiment, the thermoforming is carried out on a film or a composition of the polyester of the present disclosure. It is a process in which a sheet is heated to a temperature sufficient to allow it to deform, and then the heated sheet is forced to conform to the contours of a mold by means such as vacuum assistance, air pressure assistance, and mating mold assistance. In another embodiment, the heated film or sheet is placed into a mold and forced to conform to the contours of the mold, for example, by applying air pressure, using a vacuum plug aid, or using a mating mold. In some embodiments, thin-walled articles are produced by thermoforming.
[0115]
[0124] In one embodiment, the thermoforming process comprises forming a film or sheet on a heated male mold. The film or sheet is formed into the desired shape by forcing it into the mold. In this embodiment, thermoforming involves having the male mold of the article supported between surfaces or tables that are evacuated. In this embodiment, heat from an external heat source, such as a hot air blower, heat lamps, or other radiant heat source, is directed at the film or sheet. In this embodiment, the film or sheet is heated to its softening point. In this embodiment, a vacuum is then applied to the table, under the table, and around the mold, drawing the heat-softened film or sheet towards the table, placing the softened film or sheet in contact with the mold surface. In this embodiment, the vacuum draws the softened film or sheet into intimate contact with and conforms to the contours of the mold surface. This causes the film or sheet to take the shape of the mold. In this embodiment, after the film or sheet cools, the film or sheet solidifies and the resulting article or part can be removed from the mold.
[0116]
[0125] In one embodiment, the thermoforming process comprises forming a ?ber from the polyester blend composition of the present disclosure. heating the film or sheet until it softens and placing the film or sheet over a mold; drawing the preheated film or sheet over the heated mold surface; cooling the film or sheet; and then removing the formed article or part from the mold cavity or, in some cases, heat fixing the formed film or sheet by continuing the film or sheet in contact with the heated mold for a time sufficient to partially crystallize the film or sheet.
[0117]
[0126] In one embodiment, the thermoforming process comprises forming a ?ber from the polyester blend composition of the present disclosure. heating the film or sheet to a temperature above the Tg of the polyester; applying gas pressure, vacuum, and / or physical pressure to the heat-softened film or sheet to stretch the film or sheet to approximately the final part dimensions; forcing the sheet to conform to the shape of the mold with the vacuum or pressure; cooling the film or sheet to a temperature below the Tg of the polyester; and then removing the thermoformed article or part from the mold.
[0118]
[0127] The films and sheets used in the thermoforming process may be made in any suitable manner known to those skilled in the art. The film may be made by conventional methods. In one embodiment, the sheet or film is formed by extrusion. In one embodiment, the sheet or film is formed by calendaring. In one embodiment, during the thermoforming process, the film or sheet is heated to a temperature equal to or greater than the Tg of the polyester. In one embodiment, this temperature is about 10° C. to about 60° C. higher than the Tg of the polyester. In one embodiment, in order to achieve shorter forming times, it is necessary to heat the film or sheet before placing it on the thermoforming mold. In one embodiment, the sheet needs to be heated above its Tg but below a temperature at which the sheet sags excessively while being placed over the mold cavity. In one embodiment, the formed film or sheet may be cooled to a temperature below the Tg of the polyester before being removed from the mold. In one embodiment, the thermoforming process may include a vacuum assist, an air assist, a mechanical plug assist, or a mating mold. In some embodiments, the mold is heated to a temperature equal to or greater than the Tg of the film or sheet. Selection of the optimum mold temperature depends on the mold of the thermoforming device, the structure and wall thickness of the article being formed, and other factors.
[0119]
[0128] In some embodiments, the heated film or sheet is subjected to a vacuum application; And then introduce and stretch.
[0129] In one embodiment, heat setting is performed by subjecting the polyester to no apparent orientation. Heat setting is a process of thermally inducing partial crystallization of a polymer film or sheet. In one embodiment, heat setting is accomplished by maintaining contact of the film or sheet with a heated mold surface for a time sufficient to achieve a level of crystallinity that will impart suitable physical properties to the finished part. In one embodiment, the level of crystallinity should be about 10 to about 30%.
[0120]
[0130] In one embodiment, the heat set parts are then removed by known means. It may be removed from the mold cavity. For example, in one embodiment, a blowback is used, which involves introducing compressed air to break the vacuum established between the mold and the formed film or sheet. In some embodiments, the excess of the formed article or part is then cut off, and the waste is crushed and recycled.
[0131] In some embodiments, the addition of a nucleating agent provides faster crystallization during thermoforming. , thus providing faster molding. In one embodiment, a nucleating agent such as a fine particle sized inorganic or organic material may be used. For example, in one embodiment, suitable nucleating agents include talc, titanium dioxide, calcium carbonate, and immiscible or crosslinked polymers. In one embodiment, the nucleating agent may be used in an amount ranging from about 0.01% to about 20% based on the weight of the article. In one embodiment, other conventional additives such as pigments, dyes, plasticizers, crack inhibitors, and stabilizers may be used as needed for thermoforming. In some embodiments, the crack inhibitor improves impact strength, and the nucleating agent provides faster crystallization. In some embodiments, crystallization is necessary to achieve high temperature stability.
[0121]
[0132] In one embodiment, the foamed polyester film or sheet is made by foaming the polyester composition of the present disclosure with chemical and / or physical foaming agents, extruding the foamed polyester into a sheet or film, and thermoforming the foamed polyester film or sheet. Additives to improve the properties of the foamed polyester film may be added to the polyester before foaming. Examples of such additives include lubricants, antiblocking agents, plasticizers, optical brighteners, and UV inhibitors. In one embodiment, the foamed polyester film may be an extrusion or laminate coated on one or both sides using conventional techniques to improve its properties. In one embodiment, the coating material may be applied to the printed surface that provides product labeling, rather than to the foamed film itself.
[0122]
[0133] The blended compositions of the present disclosure can be used as formed or molded plastic parts, and are useful as solid plastic articles. The blended compositions of the present disclosure are useful as thermoformed parts or articles. The blended compositions of the present disclosure are suitable for use in any application where a clear, rigid plastic is required. Examples of such parts include disposable knives, forks, spoons, plates, cups, straws, as well as eyeglass frames, toothbrush handles, toys, automotive accessories, tool handles, camera parts, electronic equipment parts, razor parts, ink pen holders, disposable syringes, bottles, and the like. In one embodiment, the blended compositions of the present disclosure are useful as plastics, films, fibers, and sheets. In one embodiment, the compositions are useful as plastics for making bottles, bottle caps, eyeglass frames, cutlery, disposable cutlery, cutlery handles, shelves, shelf dividers, electronic equipment housings, electronic equipment cases, computer monitors, printers, keyboards, tubes, automotive parts, automotive interior parts, automotive accessories, signs, thermoformed letters, sidings, toys, thermally conductive plastics, ophthalmic lenses, tools, tool handles, and household items. In another embodiment, the blended compositions of the present disclosure can be used in the manufacture of films, sheets, fibers, formed articles, molded articles, formed parts, molded parts, medical devices, dental trays, dental instruments, containers, food containers, shipping containers, packaging, bottles, bottle caps, eyeglass frames, cutlery, disposable cutlery, cutlery handles, shelves, shelf dividers, furniture parts, electronics enclosures, electronics cases, computer monitors, printers, keyboards, tubes, toothbrush handles, automotive parts, automotive interior parts, automotive trim, signs, outdoor signs, skylights, multi-walled films, multi-layer ... films, insulation components, insulation articles, insulation containers, thermoformed letters, wallboard, toys, toy parts, trays, food trays, dental trays, thermally conductive plastics, ophthalmic lenses and framing materials, tools, tool handles, and household items, healthcare products, commercial food supply products, boxes, film for graphic arts, plastic film for plastic glass laminates, point of purchase displays, skylights, smoke vents, laminate cards, fenestrations, glazing, partitions, ceiling tiles, lighting, machine guards, graphs Suitable for use as visual art, lenses, extruded laminate sheet or film, decorative laminates, office furniture, face shields, medical packaging, display shelf sign holders, and shelf price holders.
[0123]
[0134] The thermoformed or thermoformable blended composition can be used to form films, formed articles, formed articles, or molded articles. It is useful for forming parts, molded articles, molded parts, and sheets. The method of manufacturing the thermoformed or thermoformable mixed composition into films, formed articles, formed parts, molded articles, molded parts, and sheets may follow any method known in the art. Examples of formed articles include, but are not limited to, medical device packaging, medical packaging, healthcare product packaging, commercial food service products such as trays, containers, food plates, tumblers, storage boxes, bottles, food processors, mixing bowls, household products, water bottles, crisper trays, washing machine parts, refrigerator parts, vacuum cleaner parts, ophthalmic lenses and frames, and toys.
[0124]
[0135] The present disclosure further provides films and and / or sheets. In embodiments, the films and / or sheets of the present disclosure may be of any thickness required for the intended use.
[0125]
[0136] The present disclosure further relates to the films and / or sheets described herein. The method of forming the polyester blend composition into film and / or sheet includes any method known in the art.The examples of the film and / or sheet of the present disclosure include, but are not limited to, extruded film and / or sheet, calendered film and / or sheet, compression molded film and / or sheet, and solution cast film and / or sheet.The method of making the film and / or sheet of the present disclosure includes, but is not limited to, extrusion, calendering, compression molding, wet block processing, dry block processing, and solution casting.
[0126]
[0137] The present disclosure further relates to formed or molded articles described herein. Methods of forming the stell composition into a formed or molded article include any method known in the art. Examples of formed or molded articles of the present disclosure include, but are not limited to, thermoformed or thermoformable articles, injection molded articles, extrusion molded articles, injection blow molded articles, injection stretch blow molded articles, and extrusion blow molded articles. Methods of making formed articles include, but are not limited to, thermoforming, injection molding, extrusion, injection blow molding, injection stretch blow molding, and extrusion blow molding. The process of the present disclosure may include any thermoforming process known in the art. The process of the present disclosure may include any blow molding process known in the art, including, but not limited to, extrusion blow molding, extrusion stretch blow molding, injection blow molding, and injection stretch blow molding.
[0127]
[0138] The present disclosure includes any injection blow molding manufacturing process known in the art. Although not intended to be limiting, a typical description of an injection blow molding (IBM) manufacturing process includes: 1) melting a composition in a reciprocating screw extruder; 2) injecting the molten composition into an injection mold to form a partially cooled tube (i.e., a preform) closed at one end; 3) moving the preform into a blow mold having the desired final shape around the preform and closing the blow mold around the preform; 4) blowing air into the preform to stretch and expand it to fill the mold; 5) cooling the molded article; and 6) removing the article from the mold.
[0128]
[0139] This disclosure includes any injection stretch blow molding manufacturing process known in the art. A typical, but non-limiting, description of the injection stretch blow molding (ISBM) manufacturing process includes: 1) melting the composition in a reciprocating screw extruder; 2) injecting the molten composition into an injection mold to form a partially cooled tube (i.e., a preform) closed at one end. 3) transferring the preform to a blow mold that has the desired final shape around the preform and closing the blow mold around the preform; 4) stretching the preform using an internal stretch rod and blowing air into the preform to stretch and expand the preform to fill the mold; 5) cooling the molded article; and 6) removing the article from the mold.
[0129]
[0140] The present disclosure includes any extrusion blow molding manufacturing process known in the art. Although not intended to be limiting, a typical description of the extrusion blow molding manufacturing process includes: 1) melting the composition in an extruder, 2) extruding the molten composition through a die to form a tube of molten polymer (i.e., a molten preform), 3) clamping a mold having the desired final shape around the molten preform, 4) blowing air into the molten preform to stretch and expand the extrudate to fill the mold, 5) cooling the molded article, 6) removing the article from the mold, and 7) removing excess plastic (commonly referred to as flash) from the article.
[0130]
[0141] The following examples illustrate how the polyesters of the present disclosure can be made and evaluated. The examples further illustrate how the present invention can be used in a wide variety of applications, and these examples are intended to be purely illustrative and not intended to limit the scope thereof. Unless indicated otherwise, parts are parts by weight, temperature is in °C (centigrade) or is at room temperature, and pressure is at or near atmospheric. EXAMPLES
[0131]
[0142] Copolyester resin samples were prepared using procedures described elsewhere herein. In all cases the resin samples are dried prior to extrusion.
[0143] The test film samples were then attached to a 2.5-inch Davis and Standard uniaxial screen. Resin samples were extruded into 10 mil (250 μm) films using a Bruckner extruder. These 10 mil films were cut and stretched to a final thickness of 50 μm in a Bruckner Karo 4 tenter frame at 5-15°C above the glass transition temperature (Tg) of the extruded film and at a stretch ratio of approximately 5:1.
[0132]
[0144] The film samples on the tenter frame were prepared by extruding the resin samples and using a commercially available tenter (located at Marshall and Williams, a division of Parkinson Technologies, Inc.). The films were made by stretching on a 3-frame extrusion machine, where the films were extruded using 3 layers from ABC die sets, the B layer extruded from a 2.5 inch single screw extruder, and the A and C layers extruded from separate 1.25 inch single screw satellite extruders. The films were cast at a thickness of approximately 10 mils (250 μm) and then stretched to a thickness of 50 μm with a 5:1 stretch ratio. Typically, the cast thickness is 250 μm with a final film thickness of 50 μm. The line speed was 45 fpm.
[0133]
[0145] The glycol content of the extruded film compositions was determined by NMR. All NMR spectra were recorded on a JEOL Eclipse Plus 600 MHz nuclear magnetic resonance spectrometer using chloroform-trifluoroacetic acid (70-30:vol / vol) on all polymers with deuterated chloroform added for locking. The acid component of the interpolymers used in the examples herein was 100 mol% terephthalic acid. The total mol% of glycol components was equal to 100 mol%, and the total mol% of acid components was equal to 100 mol%.
[0134]
[0146] The intrinsic viscosity of the polyesters herein is defined as the viscosity at 25° C. and a concentration of 0.5 g / dL. It was measured in 60 / 40 (w / w) phenol / tetrachloroethane and values are given in dL / g.
[0135]
[0147] In this specification, the shrinkage rate is measured by subjecting a square film sample of 50 mm×50 mm to a shrinkage rate of 65 The film is placed in water at temperatures between 100°C and 95°C in 5°C increments and the shrinkage (or expansion) of the film sample is measured by immersing the film in water for 10 seconds without restricting shrinkage in either direction. The shrinkage percentage is calculated using the following formula: Shrinkage rate (%) = [(50 mm - length after shrinkage) / 50 mm] x 100%
[0148] Shrinkage was measured in the direction perpendicular to the main shrinkage direction (machine direction: MD) and Measurements were also taken in the transverse direction (TD).
[0136]
[0149] The shrinkage force was measured using a LabThink FST-02 heat shrinkage tester as described in the examples of this specification. It is measured in units of MPa at the same temperature used to stretch the film.
[0150] Tensile film properties were measured using ASTM method D882 for the examples herein. The films were evaluated using multiple film stretching speeds (300 mm / min and 500 mm / min).
[0137]
[0151] The glass transition temperature and strain-induced crystal melting point (Tg and Tc, respectively) of polyesters The Tm and Tg were measured using a Thermal Analyst Instruments TA DSC 2920 at a scan rate of 20°C / min. The Tm was measured on the first heat of the stretched sample and the Tg was measured on the second heating step. Additionally, samples can be crystallized at 165°C for 30 minutes in a forced air oven and then analyzed by DSC. For all samples, the crystalline melting point is generally absent during the second heat of the DSC scan at a heating rate of 20°C / min.
[0138]
[0152] The suitability of materials for recycling processes is verified by the Association of Plastic Recyclers (AP R: the Association for Plastic Recyclers (PARP) In the case of PETG resin, PET clumping is the primary issue addressed by this invention. A laboratory process was developed to mimic this industry standard. The experimental clumping test parameters are as follows: 582g of PET flakes are combined with 18g of shrink flake film (3% film relative to the PET flakes) in its shrink state (the film is immersed in 85°C water for 10 seconds to shrink it before combining). ·PET flakes + film were placed in an aluminum dish to a depth of 1.5 inches. The dish with the slices was placed in a forced air oven at 208°C for 1.5 hours. The flakes were then carefully poured through a 0.5 inch sieve and the amount of flakes that remained on the dish or could not pass through the sieve was measured and the percent agglomeration was calculated as a percentage of the starting weight.
[0139]
[0153] The Association of Plastic Recyclers (APR) is committed to ensuring that materials are recycled in accordance with current recycling processes. A test was established to measure compliance with the (Important Instructions for Transparent PET Articles with Labels and Seals, revised or enacted on April 11, 2019; PET-CG-02). This method refers to the method for measuring PET cohesion (PET Thin Strip Cohesion Evaluation, revised on November 16, 2018; PET-S-08). The details of this test are as follows: · Prepare labeled bottle slices by crushing the label (minimum weight: 3% by weight, pre-shrunk at 85°C for 10 seconds) and bottle into slices of 1 / 4 to 1 / 2 inch. · Mix the labeled bottle slices 50:50 with the unlabeled reference bottle slices. · Samples were then wet classified under conditions that allowed less than 1.2% labeled PET to be carried over. The sections are then washed in 0.3% Triton X-100 and 1.0% caustic at 88°C for 15 minutes. · The flakes are then washed with water after removing all suspended solids and then filtered to remove excess water. · Wet classify the flakes again as before. · Place 2 pounds of cleaned slices (including labels) into a Teflon-lined baking dish for each cleaned sample, adding slices to a layer thickness of 1.5 inches. Place the dish containing the slices in a circulating oven at 208°C for 1.5 hours. Cool the flakes and pass them through a sieve with 0.0625 inch openings. If the material passes through the sieve, it is not agglomerated, i.e., it is not too large to pass through the sieve. This test was followed by an extrusion / pelletization and molding process to confirm the quality of the flakes.
[0140]
[0154] Modulated Differential Scanning Calorimetry (MDSC) is a method for measuring the thermal and chemical properties of a sample as a function of time and temperature. MDSC is a technique that measures the difference in heat flow between the sample and an inert reference sample. In addition, the same heat flux cell design is used as in conventional DSC. However, in MDSC, a different heating regime (temperature state) is applied to the sample and reference sample. Specifically, a sinusoidal modulation (amplitude) is superimposed on the conventional linear heating or cooling ramp to produce a regime in which the average sample temperature varies continuously with time, but not linearly. The net effect of subjecting the sample to this more complex heating regime is as if two tests, one with a conventional linear (average) heating rate and one with a sinusoidal (instantaneous) heating rate, were run on the material simultaneously. The actual rate of these two simultaneous tests depends on three operator-selectable variables: · Base heating rate (3°C / min) Modulation period (60 seconds) ·Temperature amplitude of modulation (±1℃)
[0155] The glass transition temperature and the area of the melting peak were analyzed using reversing heat flow. The heat of fusion (Hf) upon heating was measured as the integrated reversing heat flow signal. The heat of crystallization (Hc) upon heating was integrated from the total heat flow signal. The relative crystallinity (C) of the sample was measured by subtracting the heat of fusion (Hf) from the heat of crystallization (Hc) upon heating. Examples 1 to 12
[0156] Test film samples were prepared using the resin blends and evaluated in experimental cohesion tests. Details of the resin compositions and the film properties obtained from those compositions are described in the examples below.
[0141]
[0157] Polymer blends are commonly used to modify the properties of resins. It has been found that by mixing a crystalline resin with an amorphous resin capable of forming a shrinkable film, a new resin that can be used as a shrinkable film having an unexpectedly high melting point of strain-induced crystals can be provided, which helps improve the suitability of the shrinkable film for the recycling process. The compositions of the three resins used in the preparation of these test mixtures are shown below. Resin 1 or Resin 3 Shrink films made solely from Resin 1 and Resin 2 have acceptable shrink film properties, but are not designed to minimize PET agglomeration during the recycling process. Resin 2 is an example of a crystallizable copolyester resin that can be used to improve the recyclability of Resin 1 and Resin 3. Clear, conformable films were formed using an extruder with blends made from Resin 1 and Resin 2, or Resin 2 and Resin 3.
[0142] [Table 1]
[0143]
[0158] Using a laboratory scale process, mixtures 1, 2, and 3 were prepared as shown in Table 2. Combinations were made by mixing Resin 1 with Resin 2 and Resin 2 with Resin 3. Mixtures using these unmixed starting materials together were converted into shrinkable films using a laboratory scale process and the properties of these films were measured. The results are summarized in Table 3. Films made with Resin 1 or Resin 3 alone are not compatible with the PET recycling process and exhibit PET clumping rates greater than 1%. The properties of shrinkable films made with these mixtures are shown in Tables 4 and 5.
[0144] [Table 2]
[0145] [Table 3]
[0146] [Table 4]
[0147] [Table 5]
[0148]
[0159] * As used herein, "crystallinity" is calculated by subtracting the heat of crystallization from the heat of fusion. where the value is greater than 8, this corresponds to a composition that is sufficiently crystalline and recyclable in the context of the present disclosure. Examples 13 to 16
[0160] Tenter frame film samples were then examined for suitability for recycling processes. Mixtures were made in a commercial tenter frame to form sufficient material to be evaluated using the APR test procedure. In this commercial tenter frame process, the resins were dried, mixed, and extruded into a 10 mil film, which was then stretched directly in the tenter frame. The resin compositions used to make these mixes are listed in Table 6. The mix combinations used to make these shrinkable films are listed in Table 7. The film properties of these mixes are listed in Table 8.
[0149] [Table 6]
[0150] [Table 7]
[0151] [Table 8]
[0152]
[0161] Films made with these blends exhibit excellent shrink film properties and high The melting points of strain-induced crystallinity are higher than 200°C for these compositions. Typically, the melting points of strain-induced crystallinity must be higher than 200°C to withstand the drying temperature of PET and remain free-flowing. The melting points of strain-induced crystallinity for these resin blends are much higher than would be expected for reactor-grade materials made with the same composition. This higher melting point of strain-induced crystallinity may be advantageous in applications where a higher melting point is required. For example, when PET flakes are dried at a temperature higher than the APR test temperature (e.g., 420F or 210°C), the label does not become sticky and can still be recycled with the PET. These films were tested for compatibility with the recycling process (results are shown in Table 11). The films made with these compositions are considered compatible with the recycling process because they have passed lower and higher drying temperatures (a target agglomeration rate of less than 1% is considered "compatible with the recycling process").
[0153]
[0162] Aspect 1 A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and a diol component selected from either (b) or (b'); (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 75 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 25 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 25 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 25 mol % or less of other glycols, including one or more of from about 0 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (b') The diol component is about 75 mole percent or more of ethylene glycol residues, and (i) from about 0.1 to less than about 24 mole percent neopentyl glycol residues; (ii) from about 0.1 to less than about 24 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 25 mol % or less of other glycols, including one or more of from about 1 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 60 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 40 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 40 mol % or less of other glycols, including one or more of from about 0 to less than about 15 mol % of the total diethylene glycol residues in the final polyester composition; A composition, wherein the total mole % of said dicarboxylic acid components is 100 mole %, the total mole % of said diol components is 100 mole %, and said (1) and (2) polyesters are different. Aspect 2 A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 80 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 20 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 20 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 20 mol % or less of other glycols, including one or more of from about 0 to less than about 10 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 70 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 30 mole percent neopentyl glycol residues; (ii) from about 0 to less than about 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 30 mol % or less of other glycols, including one or more of from about 0 to less than about 15 mol % of the total diethylene glycol residues in the final polyester composition; A composition, wherein the total mole % of said dicarboxylic acid components is 100 mole %, the total mole % of said diol components is 100 mole %, and said (1) and (2) polyesters are different. Aspect 3 A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 85 mole percent or more of ethylene glycol residues, and (i) from about 0 to less than about 15 mole % neopentyl glycol residues; (ii) from about 0 to less than about 15 mole percent 1,4-cyclohexanedimethanol residues, and (iii) about 15 mol % or less of other glycols, including one or more of from about 0 to less than about 5 mol % of the total diethylene glycol residues in the final polyester composition; the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is about 60 mole percent or more of ethylene glycol residues, and (i) a neopentyl glycol residue, (ii) 1,4-cyclohexanedimethanol residue, and (iii) containing up to about 40 mol % of other glycols, including one or more diethylene glycol residues in the final polyester composition; A composition, wherein the total mole % of said dicarboxylic acid components is 100 mole %, the total mole % of said diol components is 100 mole %, and said (1) and (2) polyesters are different. Aspect 4 A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 5-80% of at least one crystallizable polyester; and (2) 20-95% of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) from about 0 to about 30 mol % neopentyl glycol residues; (ii) from about 0 to less than about 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) contains a diethylene glycol residue, The remainder of the glycol component is (iv) ethylene glycol residues, and (v) optionally, 0.1 to 10 mole % of at least one modifying glycol residue; the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the glycol component is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) about 70 to about 100 mole percent terephthalic acid residues, and (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) from about 0 to about 40 mol % neopentyl glycol residues; (ii) from about 0 to less than about 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) contains a diethylene glycol residue, The remainder of the glycol component is (iv) ethylene glycol residues, and (v) optionally, 0.1 to 10 mole % of at least one modifying glycol residue; A composition, wherein the total mole % of said dicarboxylic acid components is 100 mole %, the total mole % of said glycol components is 100 mole %, and said (1) and (2) polyesters are different. Aspect 5 The composition according to any one of aspects 1 to 4, wherein the mixture has a crystalline melting point of about 200 to about 255°C. Aspect 6 Aspect 5. The composition of any one of aspects 1-4, wherein the mixture has a heat of fusion minus a heat of crystallization greater than about 8.0. Aspect 7 The composition of any one of the preceding embodiments, wherein the composition is in the form of a crystallizable film. Aspect 8 8. The crystallizable film of embodiment 7, wherein the intrinsic viscosity of the film is 0.50-0.80 dL / g, measured in a 60 / 40 (wt / wt) phenol / tetrachloroethane solution at a concentration of 0.5 g / dL at 25° C. Aspect 9 8. The crystallizable film of embodiment 7, wherein the Tg of the film is between 65° C. and 80° C. as measured using a Thermal Analyst Instrument TA DSC 2920 at a scan rate of 20° C. / min. Aspect 10 8. The crystallizable film of claim 7, wherein the sum of the diol contents of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester is 15 to 40 mol %, and the total diol content is 100 mol %. Aspect 11 8. The crystallizable film of claim 7, wherein the sum of the diol contents of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester is 20 to 40 mol %, and the total diol content is 100 mol %. Aspect 12 8. The crystallizable film of claim 7, wherein the sum of the diol contents of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester is 30 to 40 mol %, and the total diol content is 100 mol %. Aspect 13 8. The crystallizable film of embodiment 7, wherein the film is stretched in at least one direction. Aspect 14 The crystallizable film of embodiment 7, wherein the film is stretched and oriented in at least one direction. Aspect 15 8. The crystallizable film of embodiment 7, wherein the film is annealed. Aspect 16 8. The crystallizable film of embodiment 7, wherein the film is annealed at a temperature from about its Tg to about 15° C. above its Tg. Aspect 17 8. The crystallizable film of embodiment 7, wherein the film is annealed at a temperature of about 75°C to about 110°C. Aspect 18 8. The crystallizable film of embodiment 7, wherein the sum of the diol content of 1,4-cyclohexanedimethanol residues and neopentyl glycol residues in the crystallizable polyester component in the final polyester is 4 to 15 mol %, and the total diol content is 100 mol %. Aspect 19 8. The crystallizable film of embodiment 7, wherein the film is stretched in at least one direction, and the melting point of strain-induced crystals in the stretched film is 200° C. or higher. Aspect 20 8. The crystallizable film of embodiment 7, wherein the film has a shrinkage percentage of 60% or more in the main shrinkage direction when immersed in water at 85° C. for 10 seconds. Aspect 21 8. The crystallizable film of embodiment 7, wherein the film has a shrinkage of 50% or more in the main shrinkage direction when immersed in water at 85° C. for 10 seconds. Aspect 22 8. The crystallizable film of embodiment 7, wherein the film has a shrinkage percentage of 40% or more in the main shrinkage direction when immersed in water at 85° C. for 10 seconds. Aspect 23 8. The crystallizable film of embodiment 7, wherein the film has a shrink force of 5 MPa or more. Aspect 24 The crystallizable film of embodiment 7, which is oriented in one or more directions. Aspect 25 The crystallizable film of embodiment 7, having a pre-oriented thickness of about 50 to 400 μm, and being oriented in a tenter frame at a temperature of from Tg of said film to Tg+55° C. and a ratio of 5:1 to 3:1 to a thickness of about 10 to about 80 μm. Aspect 26 8. The crystallizable film of claim 7, wherein the film has a shrinkage rate of 50 to 90% in the main shrinkage direction and a shrinkage rate of 10% or less in the direction perpendicular to the main shrinkage direction when immersed in water at 95° C. for 10 seconds. Aspect 27 A shrink film comprising the crystallizable film of any one of embodiments 7 to 26. Aspect 28 8. A stretched film comprising the crystallizable film of embodiment 7. Aspect 29 An oriented film comprising the crystallizable film of embodiment 7. Aspect 30 A flexible packaging film for lidding films, extrusion blow molded containers, extruded sheets, thermoformed sheets, stand-alone bags, comprising the crystallizable film of embodiment 7. Aspect 31 A label or sleeve comprising the crystallizable film of embodiment 7, applied to an article of manufacture, a molded article, a container, a plastic bottle, a glass bottle, a packaging material, a battery, a hot fill container, or an industrial product. Aspect 32 An extruded or calendered film comprising the crystallizable film of embodiment 7. Aspect 33 A thermoformed sheet having a thickness of about 0.25 mm to about 6.4 mm comprising the crystallizable composition of any one of embodiments 1 to 4. Aspect 34 34. The thermoformed sheet of embodiment 33, wherein the intrinsic viscosity of the film is 0.50-0.80 dL / g, measured in a 60 / 40 (wt / wt) phenol / tetrachloroethane solution at a concentration of 0.5 g / dL at 25° C. Aspect 35 34. The thermoformable sheet of embodiment 33, wherein the film has a Tg of 65°C to 120°C as measured using a Thermal Analyst Instrument TA DSC 2920 at a scan rate of 20°C / min. Aspect 36 34. The thermoformed sheet of claim 33, wherein the sum of the diol contents of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester is 15 to 90 mol %, and the total diol content is 100 mol %. Aspect 37 34. The thermoformed sheet of claim 33, wherein the sheet is stretched in at least one direction. Aspect 38 34. The thermoformed sheet of claim 33, wherein the sheet is stretched and oriented in at least one direction. Aspect 39 34. The thermoformed sheet of claim 33, wherein the sheet is annealed. Aspect 40 34. The thermoformed sheet of embodiment 33, wherein the sheet is annealed at a temperature from about its Tg to about 15° C. above its Tg. Aspect 41 34. The thermoformed sheet of embodiment 33, wherein the sheet is annealed at a temperature of from about 75° C. to about 110° C. Aspect 42 34. The thermoformed sheet of embodiment 33, wherein the sum of the diol content of 1,4-cyclohexanedimethanol residues and neopentyl glycol residues in the crystallizable polyester component in the final polyester is 4 to 15 mol %, and the total diol content is 100 mol %. Aspect 43 A shaped or molded article comprising or prepared from the thermoformed sheet of embodiment 33. Aspect 44 A thermoformed sheet according to any one of embodiments 33 to 43, or prepared from the same. Medical equipment packaging, medical related packaging, healthcare product packaging, commercial food supply packaging, trays, containers, food plates, tumblers, storage bins, bottles, cookware, mixing bowls, household items, water bottles, vegetable trays, dishwasher parts, refrigerator parts, vacuum cleaner parts, ophthalmic lenses, and frameworks or toys. Aspect 45 A polyester recycling stream comprising recycled polyethylene terephthalate flakes mixed with at least about 0.1 wt. % of the recycled crystallizable film of any one of embodiments 1-7.
[0154] Aspect 46 46. A polyester recycling stream as described in embodiment 45, wherein the stream has passed document number PET-CG-02, “Important Instructions for Transparent PET Articles with Labels and Seals,” dated April 11, 2019.
Claims
1. A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 50 to 80 weight percent of at least one crystallizable polyester; and (2) 20 to 50 weight percent of at least one amorphous polyester; (1) At least one crystallizable polyester comprises (a) a dicarboxylic acid component and a diol component selected from either (b) or (b'); (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is 75 mole percent or more of ethylene glycol residues, and (i) 0 to less than 25 mole percent neopentyl glycol residues; (ii) 0 to less than 25 mole percent 1,4-cyclohexanedimethanol residues, and (iii) 0 to less than 10 mol % total diethylene glycol residues in the final polyester composition, the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and The diol component (b') is 75 mole percent or more of ethylene glycol residues, and (i) 0.1 to less than 24 mole percent neopentyl glycol residues; (ii) from 0.1 to less than 24 mole percent of 1,4-cyclohexanedimethanol residues, and (iii) 1 to less than 10 mol % total diethylene glycol residues in the final polyester composition, the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is 60 mole percent or more of ethylene glycol residues, and (i) 0 to less than 40 mole percent neopentyl glycol residues; (ii) 0 to less than 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) 0 to less than 15 mol % total diethylene glycol residues in the final polyester composition, the total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the polyesters (1) and (2) are different; The final polyester composition comprises residues of neopentyl glycol and residues of 1,4-cyclohexanedimethanol.
2. A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 50 to 80 weight percent of at least one crystallizable polyester; and (2) 20 to 50 weight percent of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is at least 80 mole percent ethylene glycol residues, and (i) 0 to less than 20 mole percent neopentyl glycol residues; (ii) 0 to less than 20 mole percent 1,4-cyclohexanedimethanol residues, and (iii) 0 to less than 10 mol % total diethylene glycol residues in the final polyester composition, the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is 70 mole percent or more of ethylene glycol residues, and (i) 0 to less than 30 mole percent neopentyl glycol residues; (ii) 0 to less than 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) 0 to less than 15 mol % total diethylene glycol residues in the final polyester composition, the total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the polyesters (1) and (2) are different; The final polyester composition comprises residues of neopentyl glycol and residues of 1,4-cyclohexanedimethanol.
3. A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 50 to 80 weight percent of at least one crystallizable polyester; and (2) 20 to 50 weight percent of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is at least 85 mole percent ethylene glycol residues, and (i) 0 to less than 15 mole percent neopentyl glycol residues; (ii) 0 to less than 15 mole percent 1,4-cyclohexanedimethanol residues, and (iii) 0 to less than 5 mol % total diethylene glycol residues in the final polyester composition, the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is 60 mole percent or more of ethylene glycol residues, and (i) a neopentyl glycol residue, (ii) 1,4-cyclohexanedimethanol residue, and (iii) diethylene glycol residues in the final polyester composition, the total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the diol component is 100 mole %, and the polyesters (1) and (2) are different; The final polyester composition comprises residues of neopentyl glycol and residues of 1,4-cyclohexanedimethanol.
4. A crystallizable composition comprising a mixture of polyester compositions, the mixture comprising: (1) 50 to 80 weight percent of at least one crystallizable polyester; and (2) 20 to 50 weight percent of at least one amorphous polyester; (1) at least one crystallizable polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) 0 to 30 mole % neopentyl glycol residues; (ii) 0 to less than 30 mole percent 1,4-cyclohexanedimethanol residues, and (iii) contains a diethylene glycol residue, The remainder of the glycol component is (iv) an ethylene glycol residue, and (v) optionally, containing 0.1 to 10 mole % of at least one modifying glycol residue; the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the glycol component is 100 mole %; and (2) the at least one amorphous polyester comprises (a) a dicarboxylic acid component and (b) a diol component; (a) The dicarboxylic acid component is (i) 70 to 100 mole percent terephthalic acid residues, and (ii) contains 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; (b) The diol component is (i) 0 to 40 mole % neopentyl glycol residues; (ii) 0 to less than 40 mole percent 1,4-cyclohexanedimethanol residues, and (iii) contains a diethylene glycol residue, The remainder of the glycol component is (iv) an ethylene glycol residue, and (v) optionally, containing 0.1 to 10 mole % of at least one modifying glycol residue; the total mole % of the dicarboxylic acid component is 100 mole %, the total mole % of the glycol component is 100 mole %, and the (1) and (2) polyesters are different; The final polyester composition comprises residues of neopentyl glycol and residues of 1,4-cyclohexanedimethanol.
5. The mixture has a crystalline melting point of 200 to 255° C.; or the heat of fusion minus the heat of crystallization of the mixture is greater than 8.0; The composition according to any one of claims 1 to 4.
6. The composition of any one of claims 1 to 5, in the form of a crystallizable film.
7. 7. The crystallizable film of claim 6, the intrinsic viscosity of the film is 0.50 to 0.80 dL / g, measured in a 60 / 40 (w / w) phenol / tetrachloroethane solution at a concentration of 0.5 g / dL at 25° C.; or the Tg of the film is between 65° C. and 80° C., as measured using a Thermal Analyst Instrument TA DSC 2920 at a scan rate of 20° C. / min; or the sum of the diol content of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester composition is 15-40 mol %, with the total diol content being 100 mol %; or the sum of the diol content of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester composition is 20-40 mol %, the total diol content being 100 mol %, or the sum of the diol content of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester composition is 30-40 mol %, and the total diol content is 100 mol %, or the film is stretched in at least one direction; or the film is stretched and oriented in at least one direction; or the film is annealed, or The film has been annealed at a temperature between its Tg and 15° C. above its Tg; or The film is annealed at a temperature of from 75° C. to 110° C.; or the sum of the diol content of 1,4-cyclohexanedimethanol residues and neopentyl glycol residues in the crystallizable polyester component in said final polyester is 4 to 15 mole percent, with the total diol content being 100 mole percent; or The film is stretched in at least one direction, and the melting point of the strain-induced crystals of the stretched film is 200° C. or higher; or The film has a shrinkage percentage of 60% or more in the main shrinkage direction when immersed in water at 85° C. for 10 seconds; or The film has a shrinkage percentage of 50% or more in the main shrinkage direction when immersed in water at 85° C. for 10 seconds; or The film has a shrinkage percentage of 40% or more in the main shrinkage direction when immersed in water at 85° C. for 10 seconds; or The film has a shrinkage force of 5 MPa or more; or Oriented in one or more directions, or having a pre-oriented thickness of 50 to 400 μm and being oriented in a tenter frame at a temperature from the Tg of the film to Tg+55° C. and a ratio of 5:1 to 3:1 to a thickness of 10 to 80 μm; or The film has a shrinkage rate of 50 to 90% in the main shrinkage direction and a shrinkage rate of 10% or less in a direction perpendicular to the main shrinkage direction when immersed in water at 95° C. for 10 seconds. Crystallizable films.
8. A shrink film comprising the crystallizable film of claim 6 or 7.
9. The crystallizable film according to claim 6, Stretched film, Oriented film, Lidding films, extrusion blow molded containers, extruded sheets, thermoformed sheets, flexible packaging films for stand up bags, A label or sleeve affixed to an article of manufacture, molded article, container, plastic bottle, glass bottle, packaging material, battery, hot-fill container, or industrial product; or Extruded or calendared film.
10. A thermoformed sheet having a thickness of 0.25 mm to 6.4 mm comprising the crystallizable composition of any one of claims 1 to 4.
11. 11. The thermoformable sheet of claim 10, The intrinsic viscosity of the sheet, measured in a 60 / 40 (wt / wt) phenol / tetrachloroethane solution at a concentration of 0.5 g / dL at 25° C., is 0.50 to 0.80 dL / g; or the Tg of the sheet is between 65°C and 120°C, as measured using a Thermal Analyst Instrument TA DSC 2920 at a scanning rate of 20°C / min; or the sum of the diol content of the one or more diol monomer components capable of forming the amorphous polyester in the final polyester composition is 15 to 90 mol %, with the total diol content being 100 mol %; or the sheet is stretched in at least one direction; or the sheet is stretched and oriented in at least one direction; or the sheet is annealed, or The sheet has been annealed at a temperature between its Tg and 15° C. above its Tg; or The sheet is annealed at a temperature between 75°C and 110°C; or the sum of the diol content of 1,4-cyclohexanedimethanol residues and neopentyl glycol residues in the crystallizable polyester component in the final polyester composition is 4-15 mole %, with the total diol content being 100 mole %; Thermoforming sheet.
12. A formed or molded article comprising or prepared from the thermoformed sheet of claim 10.
13. 12. A thermoformed sheet comprising or prepared from the thermoformed sheet of claim 10 or 11. Medical equipment packaging, medical related packaging, healthcare product packaging, commercial food supply packaging, trays, containers, food plates, tumblers, storage bins, bottles, cookware, mixing bowls, household items, water bottles, vegetable trays, dishwasher parts, refrigerator parts, vacuum cleaner parts, ophthalmic lenses, and frameworks or toys.
14. 7. A polyester recycling stream comprising recycled polyethylene terephthalate flakes mixed with at least 0.1 wt. % of the crystallizable composition of any one of claims 1 to 6.
15. 15. The polyester recycling stream of claim 14, wherein the stream passes Document No. PET-CG-02, dated April 11, 2019, "Important Instructions for Transparent PET Articles with Labels and Seals."
Citation Information
Patent Citations
Heat-shrinkable polyester-based film roll
JP2003113257A
Heat-shrinkable polyester-based film
JP2005206730A
Polyester-based resin composition, and thermally shrinkable film using the composition, thermally shrinkable label, and container having the label attached thereto
JP2006233092A
Heat-shrinkable polyester film
JP2011184690A
Blendable polyester blends and shrinkable films manufactured therefrom
JP2011513550A