Cu-Ni-Co-Si BASED COPPER ALLOY SHEET MATERIAL AND METHOD FOR PRODUCING THE SAME, AND ELECTRICALLY ENERGIZING COMPONENT

By dispersing Mg-S particles in Cu-Ni-Co-Si copper alloy sheets through controlled manufacturing processes, the alloy achieves a high strength-conductivity balance, improving press punchability and die life for thinner current-carrying parts.

JP2024153807AActive Publication Date: 2024-10-29DOWA METALTECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024123188
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-29
Estimated Expiration
2040-02-25

AI Technical Summary

Technical Problem

Existing Cu-Ni-Co-Si copper alloy sheets struggle to achieve a high balance of tensile strength (900 MPa or more) and electrical conductivity (40% IACS or more) while maintaining improved press punchability, which is crucial for manufacturing thinner and smaller current-carrying parts with high dimensional accuracy.

Method used

Incorporating trace amounts of Mg and S into the Cu-Ni-Co-Si alloy to disperse Mg-S particles with specific size and density, combined with a manufacturing process involving hot rolling, solution treatment, and aging treatment, to create a microstructure that enhances strength and conductivity.

Benefits of technology

The solution stabilizes a high strength-conductivity balance, significantly reduces sheared surfaces during press punching, and extends press die life, ensuring high dimensional accuracy and quality in mass-produced parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153807000001_ABST
    Figure 2024153807000001_ABST
Patent Text Reader

Abstract

To provide a Cu-Ni-Co-Si based copper alloy sheet material which materializes strength / conductivity balance, that is, tensile strength of 900 MPa or more and conductivity of 40% IACS or more, and has significantly improved press punchability.SOLUTION: A copper alloy sheet material is provided which has a chemical composition composed of, in mass%, the total of Ni and Co: 1.50 to 5.50%, Si: 0.50 to 1.20%, S: 0.0005 to 0.20%, Mg: 0.01 to 0.20%, Cr: 0 to 0.50%, Zn: 0 to 1.00%, Sn: 0 to 1.00%, Mn: 0 to 0.20%, B: 0 to 0.10%, P: 0 to 0.10%, Ag: 0 to 0.20%, Al: 0 to 0.20%, Zr: 0 to 0.20%, Ti: 0 to 0.50%, Fe: 0 to 0.30%, the balance composed of Cu and unavoidable impurities, and in which Mg-S based particles having a circle-equivalent diameter of 0.5 μm or more are present at a number density of 300 pieces / mm2 or more, and the average particle size of the Mg-S based particles is 3.0 μm or less in terms of the circle-equivalent diameter.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high-strength Cu-Ni-Co-Si copper alloy sheet material having improved press punching properties, a manufacturing method thereof, and an electrical-conducting part using said Cu-Ni-Co-Si copper alloy sheet material. [Background technology]

[0002] Among copper alloys, Cu-Ni-Co-Si copper alloys have a relatively good balance between strength and electrical conductivity, and are useful for current-carrying parts such as connectors and lead frames. In recent years, connector materials have become thinner as electronic devices become smaller and lighter, and the copper alloy sheets that are the raw materials for these connectors are required to have even higher strength. In the case of Cu-Ni-Co-Si copper alloy sheets, it is expected that a high level of strength-electrical conductivity balance will be achieved, for example, with a tensile strength of 900 MPa or more in the rolling direction and electrical conductivity of 40% IACS or more. However, strength and electrical conductivity are generally in a trade-off relationship, and it is not easy to achieve both high levels of strength and electrical conductivity in the copper alloy sheets.

[0003] On the other hand, when copper alloy sheets are processed into current-carrying parts, they are generally subjected to a press punching process. Recently, parts have become smaller and have narrower pitches, and high dimensional accuracy is required for punched parts. In order to improve the dimensional accuracy in the punching process, it is important to extend the life of the die. The cut surface (cut edge) of a metal sheet formed by press punching usually has a shear surface and a fracture surface (see Figure 2). When punching is performed with an appropriate clearance, the smaller the proportion of the shear surface in the cut surface is, the more advantageous it is for extending the life of the die. In this specification, it is expressed that the material has better "press punchability" when the same sheet thickness is punched with a press die with an appropriate clearance, and the smaller the proportion of the shear surface in the cut surface is. In Cu-Ni-Co-Si-based copper alloy sheets with high strength, there is room for improvement in press punchability.

[0004] Patent Document 1 describes a Cu-Ni-Co-Si-based copper alloy sheet material that achieves both bending workability and high strength by controlling the texture. However, it does not disclose a material that has a high strength of tensile strength of 900 MPa or more with electrical conductivity of 40% IACS or more. There is no intention to improve press punchability, and there is no description of the S content.

[0005] Patent Document 2 describes a Cu-(Ni)-Co-Si-based copper alloy sheet material that has high electrical conductivity and reduced die wear by controlling the particle size and number density of precipitates in the surface and center. The electrical conductivity is increased to 55% IACS or more, but the tensile strength remains at 750 MPa or less. The die life is evaluated by the burr height and sagging amount. There is no idea of ​​reducing the proportion of sheared surfaces or using S-containing particles.

[0006] Patent Document 3 describes a Cu-Ni-Co-Si-based copper alloy sheet material that has improved stress relaxation resistance by adjusting the structure using a method of controlling the heating rate and cooling rate in solution treatment. There is no intention to improve press punchability, and there is no description of the S content.

[0007] Patent Document 4 describes a Cu-Ni-Co-Si-based copper alloy sheet material that improves the spring limit value by controlling the morphology of precipitates using a three-stage aging treatment method. Among the specifically described sheets, some have a relatively high 0.2% yield strength (YS) of 882 MPa among those with electrical conductivity of 40% IACS or more (Table 2-7, Example 138), but no method is disclosed for stably obtaining a strength level of tensile strength of 900 MPa or more. There is no intention to improve press punchability, and there is no description of the S content.

[0008] Patent Document 5 describes a Cu-(Ni)-Co-Si-based copper alloy sheet material with an S content of about 0.002%. The solution treatment temperature is 750°C (paragraph 0033). These materials have low strength levels and low electrical conductivity.

[0009] Patent Document 6 shows manufacturing examples of Nos. 6, 8, 15, 19, 38, 41, and 46 in the table of the specification as Cu-(Ni)-Co-Si-based copper alloy sheet materials containing S in the range of 50 ppm (0.005%) or less and Mg. Of these, No. 8 has a relatively high electrical conductivity of 46% IACS. However, there is no particular description regarding hot rolling, and the temperature of the finish heat treatment equivalent to the solution treatment is low at 775°C, so there is insufficient in terms of notable improvement in strength and press punchability. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP2011-117034A [Patent Document 2] JP 2012-224922 A [Patent Document 3] JP 2015-187308 A [Patent Document 4] JP 2011-214088 A [Patent Document 5] Japanese Patent Application Publication No. 11-222641 [Patent Document 6] JP 2016-44344 A Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention aims to achieve a high level of balance between strength and electrical conductivity, i.e., a tensile strength in the rolling direction of 900 MPa or more and an electrical conductivity of 40% IACS or more, in a Cu-Ni-Co-Si-based copper alloy sheet material, and to significantly improve the press-punching properties. [Means for solving the problem]

[0012] The inventors have found that the above object can be achieved by adding trace amounts of Mg and S to a Cu-Ni-Co-Si based copper alloy and creating a structure in which Mg-S based inclusions of a predetermined size are dispersed.

[0013] That is, the above object is to provide a steel sheet having a chemical composition consisting of, in mass%, the total of Ni and Co: 1.50 to 5.50%, preferably 2.00 to 4.00%, Si: 0.50 to 1.20%, S: 0.0005 to 0.20%, Mg: 0.01 to 0.20%, Cr: 0 to 0.50%, Zn: 0 to 1.00%, Sn: 0 to 1.00%, Mn: 0 to 0.20%, B: 0 to 0.10%, P: 0 to 0.10%, Ag: 0 to 0.20%, Al: 0 to 0.20%, Zr: 0 to 0.20%, Ti: 0 to 0.50%, Fe: 0 to 0.30%, with the balance being Cu and unavoidable impurities, and having 300 Mg-S based particles / mm2 with a circle equivalent diameter of 0.5 μm or more in a cross section parallel to the rolling direction and the plate thickness direction (referred to as the "TD surface"). 2 The copper alloy sheet material has a number density of 1 to 900 MPa, the Mg-S particles have an average particle size of 3.0 μm or less in terms of circle equivalent diameter, and the tensile strength in the rolling direction is 900 MPa or more. In this structure state, a conductivity of 40% IACS or more can be obtained. In the cross section (LD surface) perpendicular to the rolling direction of this sheet material, the average crystal grain size measured by a cutting method according to JIS H0501-1986 is, for example, 1 to 20 μm.

[0014] In the present invention, a method for producing the above-mentioned Cu-Ni-Co-Si-based copper alloy sheet material is provided, which comprises producing the sheet material from a cast slab having the above-mentioned chemical composition by a process including hot rolling, cold rolling, solution treatment, and aging treatment in the above-mentioned order, In the hot rolling process, the rolling reduction rate per pass in all rolling passes performed at a temperature of 800°C or higher is 20% or less, and the total rolling reduction rate in all rolling passes performed at a temperature of 900°C or higher is 38% or more; A method for producing a copper alloy sheet is provided, in which, in the solution treatment step, the average heating rate from 300°C to 800°C is 10°C / s or more, the temperature is held at 800 to 1,020°C for 10 seconds or more, and the average cooling rate from 800°C to 500°C is 50°C / s or more. The aging treatment temperature may be, for example, 400 to 550°C.

[0015] Furthermore, the present invention provides an electric-conducting part using the above-mentioned copper alloy sheet material, and is particularly suitable for use in an electric-conducting part having a press-punched portion. Effect of the Invention

[0016] According to the present invention, it is possible to stably impart a high level of strength-conductivity balance, such as a tensile strength of 900 MPa or more in the rolling direction and a conductivity of 40% IACS or more, to a Cu-Ni-Co-Si-based copper alloy sheet material. Furthermore, it is possible to significantly reduce the proportion of sheared surfaces generated at the cut edge during press punching, thereby improving the life of the press die. The improvement in die life leads to stabilization of quality by maintaining high dimensional accuracy in mass production of press punched parts. The present invention has realized the simultaneous improvement of conductivity, strength, and press punchability, which was desired for sheet materials for manufacturing current-carrying parts that are becoming thinner and narrower in pitch. [Brief description of the drawings]

[0017] [Figure 1] 1 is an SEM image of a cross section of a Cu-Ni-Co-Si-based copper alloy sheet material according to the present invention, in which particles have been made clear by binarization processing. [Diagram 2] FIG. 4 is a diagram showing a schematic shape of a cut edge of a metal plate after being punched by a press. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] [Chemical composition] In the present invention, a Cu-Ni-Co-Si based copper alloy is used. Hereinafter, "%" regarding the alloy components means "mass %" unless otherwise specified.

[0019] Ni and Co form Ni-Co-Si-based precipitates, Co-Si-based precipitates, and Ni-Si-based precipitates, improving the strength and electrical conductivity of the copper alloy sheet material. The Ni-Co-Si-based precipitates are considered to be compounds mainly composed of (Ni, Co)2Si. The Co-Si-based precipitates and the Ni-Si-based precipitates are considered to be precipitates mainly composed of Co2Si and Ni2Si, respectively. In order to sufficiently disperse fine precipitate particles effective for improving strength, the total content of Ni and Co needs to be 1.50% or more, and is more preferably 2.00% or more. The Ni content is more preferably 0.50% or more, and even more preferably 0.75% or more, and may be controlled to 1.00% or more. The Co content is also more preferably 0.50% or more, and even more preferably 1.00% or more. On the other hand, if the total content of Ni and Co is excessive, coarse precipitates are easily generated, which is disadvantageous for improving strength. The total content of Ni and Co is limited to 5.50% or less, and may be controlled to 4.00% or less.

[0020] Silicon forms Ni-Co-Si precipitates. In order to sufficiently disperse fine precipitate particles, which are effective in improving strength, the silicon content must be 0.50% or more. On the other hand, excessive silicon easily generates coarse precipitates, which are prone to cracking during hot rolling. The silicon content is limited to 1.20% or less. It may be controlled to less than 1.00%.

[0021] S is an important component element in the present invention. In general, in copper alloys, S is often treated as an impurity from the viewpoint of suppressing deterioration of hot workability and deterioration of material properties. In the manufacturing process of copper alloys, the S content is usually reduced by methods such as degreasing of raw materials and floating separation in molten metal. However, in the present invention, Mg-S particles are dispersed in the material to improve press punchability. Therefore, a predetermined amount of S is contained in the copper alloy as a source of generation of Mg-S particles. As a result of various studies, it is necessary to control the S content to a range of 0.0005 to 0.20%. If the S content is too small, the amount of Mg-S particles generated becomes insufficient, and the improvement effect of press punchability cannot be obtained. It is more effective to set the S content to 0.01% or more. When comparing copper alloys with the same content of alloy elements other than S and the same manufacturing conditions, setting the S content to 0.01% or more is advantageous in obtaining a more excellent improvement effect of press punchability. Excessive S content deteriorates hot workability and makes the material more susceptible to cracking during hot rolling. Excessive addition of S also tends to cause coarsening of Mg-S particles, which is a factor in reducing strength.

[0022] Mg is an element that has the effect of improving the stress relaxation resistance of Cu-Ni-Co-Si copper alloys, and has been added as necessary. However, in the present invention, Mg is used as a source of Mg-S particles, so the inclusion of Mg is essential. In addition, the inclusion of Mg is important in order to increase the tensile strength to 900 MPa or more while suppressing the decrease in electrical conductivity by utilizing the solid solution strengthening of Mg. As a result of various investigations, it is necessary to ensure that the Mg content is 0.01% or more. A large amount of Mg content causes a decrease in hot workability or cold workability. The Mg content is limited to a range of 0.20% or less, and may be controlled to 0.15% or less.

[0023] Other elements such as Cr, Zn, Sn, Mn, B, P, Ag, Al, Zr, Ti, and Fe may be contained as necessary. The content ranges of these elements are preferably as follows: Cr: 0-0.50%, Zn: 0-1.00%, Sn: 0-1.00%, Mn: 0-0.20%, B: 0-0.10%, P: 0-0.10%, Ag: 0-0.20%, Al: 0-0.20%, Zr: 0-0.20%, Ti: 0-0.50%, and Fe: 0-0.30%.

[0024] Cr, Mn, B, P, Al, Zr, and Ti have the effect of further increasing the alloy strength and reducing stress relaxation. Sn and Ag are effective in improving stress relaxation resistance. Zn improves the solderability and castability of copper alloy sheet materials. Cr, Mn, Zr, Ti, and Fe are likely to form high melting point compounds with Pb and other elements present as unavoidable impurities, and B, P, Zr, and Ti have the effect of refining the cast structure, each of which can contribute to improving hot workability.

[0025] When adding one or more of Cr, Zn, Sn, Mn, B, P, Ag, Al, Zr, Ti, and Fe, it is more effective to set the total content to 0.01% or more. However, adding a large amount will adversely affect hot or cold workability and will be disadvantageous in terms of cost. It is more preferable to set the total content of these optional added elements to 1.0% or less, or 0.5% or less.

[0026] [Mg-S particles] In this specification, "Mg-S particles" refer to compound particles present in a copper alloy, in which Mg and S are observed by EDX (energy dispersive X-ray fluorescence analysis) when the center of the particle is irradiated with an electron beam. The particle is considered to be mainly composed of the compound MgS. Press formability is improved by dispersing Mg-S particles with a particle diameter of about 0.5 to 3.0 μm. In this specification, the particle diameter of Mg-S particles means the circle equivalent diameter unless otherwise specified. In other words, the area of ​​a certain particle observed in the cross section of a copper alloy sheet is defined as S (μm 2 ), the diameter D (μm) of a perfect circle with an area S is called the equivalent circle diameter of the particle. Here, S = π × D2 / 4.

[0027] According to the research of the inventors, in a cross section (TD surface) parallel to the rolling direction and the plate thickness direction, Mg-S-based particles having a circle equivalent diameter of 0.5 μm or more are present at 300 particles / mm 2 It was found that when Mg-S particles are present at a number density of 0.5 μm or more, the proportion of sheared surfaces is significantly reduced in the cut edge formed when shear processing (press punching) is performed with an appropriate clearance. In other words, press punching properties are significantly improved. This extends the life of the press die, maintains high dimensional accuracy of punched parts in mass production, and stabilizes the quality of the parts. However, if the average particle size of Mg-S particles with a circle equivalent diameter of 0.5 μm or more exceeds 3.0 μm in circle equivalent diameter, it hinders high strength and in some cases the effect of improving press punching properties cannot be fully obtained. The average particle size and number density of the Mg-S based particles can be determined by the following analytical method.

[0028] (Method of analyzing Mg-S particles) A cross section (TD surface) parallel to the rolling direction and thickness direction of the copper alloy sheet material is polished to obtain a sample surface for EDX measurement. The sample surface is observed by an FE-SEM (field emission scanning electron microscope) equipped with an EDX device, and a measurement area is randomly determined. EDX analysis is performed on all particles with a circular equivalent diameter of 0.5 μm or more that are entirely present within the measurement area, and particles in which Mg and S are detected are identified as "Mg-S-based particles" and their number is counted. In EDX analysis, an electron beam is irradiated to the center of the particle. In addition, the circular equivalent diameter of each particle present within the measurement area is measured by processing the FE-SEM image of the measurement area with software. This operation is performed for multiple non-overlapping measurement areas, and the total number of particles identified as "Mg-S-based particles" with a circular equivalent diameter of 0.5 μm or more is divided by the total area of ​​the measurement area to obtain the "number density (pieces / mm 2 The arithmetic mean of the equivalent circle diameters of those particles is calculated, and this value is taken as the "average particle diameter (μm) of Mg-S particles with an equivalent circle diameter of 0.5 μm or more." Here, the area of ​​one measurement region is 0.03 mm 2The total area of ​​the measurement area is 0.75 mm 2 In the FE-SEM observation, a region in one visual field may be set as one measurement region, or a region obtained by joining several adjacent visual fields together without interruption may be set as one measurement region.

[0029] [Tensile strength / conductivity] The present invention is directed to a copper alloy sheet material having a tensile strength of 900 MPa or more in the rolling direction. By applying a manufacturing method under the conditions described below to a Cu-Ni-Co-Si-based copper alloy adjusted to the above-mentioned chemical composition, a high strength of tensile strength of 900 MPa or more can be obtained. At the same time, a conductivity of 40% IACS or more can be obtained. Such a high level of balance between strength and conductivity can meet the needs for thinner and smaller current-carrying parts. It is also possible to obtain a conductivity of 43% IACS or more, or even 46% IACS or more.

[0030] [Average grain size] In general, making the crystal grain size finer is advantageous for improving strength and bending workability. On the other hand, when stress relaxation properties, which are a type of creep phenomenon, are important, an excessively small crystal grain size is disadvantageous. When processing into current-carrying parts that require thinning and narrow pitch is assumed, the average crystal grain size of the cross section perpendicular to the rolling direction (LD surface) according to a cutting method in accordance with JIS H0501-1986 is preferably in the range of, for example, 1 to 20 μm. The average crystal grain size can be measured by the following method.

[0031] (Method of measuring average crystal grain size) The cross section (LD surface) perpendicular to the rolling direction of the plate material is polished and then etched to prepare an observation surface. The observation surface is observed with an optical microscope to obtain an observation image. On the obtained observation image, a total of three straight lines parallel to the rolling surface are drawn at the 1 / 4, 1 / 2 (center of plate thickness), and 3 / 4 positions in the plate thickness direction, and the average crystal grain size is calculated by counting the number of crystal grain boundaries cut by each straight line using a cutting method in accordance with JIS H0501-1986. This operation is performed for five randomly selected fields of view, and the arithmetic mean of the average crystal grain size obtained in each field of view is adopted as the average crystal grain size of the plate material. A confocal laser microscope can be used as the optical microscope.

[0032] [Manufacturing method] The copper alloy sheet material described above can be produced, for example, by the following manufacturing process. Melting / casting → hot rolling → cold rolling → (intermediate annealing → cold rolling) → solution treatment → aging treatment → finish cold rolling → low temperature annealing Although not described in the above steps, facing is performed as necessary after hot rolling, and pickling, polishing, or further degreasing is performed as necessary after each heat treatment. Each step will be described below.

[0033] [Melting and Casting] The cast pieces may be produced by continuous casting, semi-continuous casting, or the like. To prevent oxidation of Si, Mg, etc., it is preferable to carry out the casting in an inert gas atmosphere or in a vacuum melting furnace. In the production of copper alloys, S is generally treated as an impurity, and the raw materials and refining methods are usually controlled so as to reduce the S content as much as possible. In contrast, in the present invention, it is necessary to strictly control the S content so that the S content within the above-mentioned predetermined content range is incorporated into the copper alloy. For example, a Cu-S mother alloy prepared in advance can be used to add S.

[0034] [Hot rolling] Since S tends to cause the formation of coarse Mg-S compound phases in the slab, it is important to break up the coarse compound phases in the hot rolling process in order to finally obtain a desired metal structure with dispersed Mg-S particles. In order to break up the coarse compound phases, it is advantageous to obtain as large a degree of processing as possible in a high temperature region where the deformation resistance is small. However, since S is also an element that reduces hot workability, it is necessary to carefully manage the pass schedule in hot rolling to prevent cracks from occurring. Therefore, the inventors conducted detailed hot rolling experiments. As a result, it was found that by following the following conditions, it is possible to break up the coarse compound phases and prevent cracks during hot rolling for copper alloys in the above-mentioned composition range.

[0035] (i) The rolling reduction rate per pass in all rolling passes performed at a temperature of 800°C or higher is 20% or less. (ii) And the total rolling reduction rate in the rolling passes performed at a temperature of 900°C or more is 38% or more. Here, the rolling temperature in each rolling pass can be the surface temperature of the material immediately before it is bitten by the rolling rolls, measured by a radiation thermometer. The rolling reduction ratio from the plate thickness t0 (mm) to the plate thickness t1 (mm) is determined by the following formula (1). Reduction ratio (%) = 100 × (t0-t1) / t0…(1) The reduction ratio per pass in a certain rolling pass can be determined by substituting the plate thickness before rolling in that rolling pass into t0 and the plate thickness after rolling in that rolling pass into t1 and applying formula (1). The total reduction ratio in rolling passes performed at a temperature of 900°C or higher can be determined by substituting the initial plate thickness before the start of rolling into t0 and the plate thickness after rolling in the last rolling pass where the rolling temperature is 900°C or higher into t1 and applying formula (1).

[0036] Heating before hot rolling can be performed under conditions of, for example, holding at 920 to 1060°C for 60 to 600 minutes. The lower limit of the rolling ratio per pass in (i) above is not particularly specified, but since a large number of passes is uneconomical, the rolling ratio may be set in the range of, for example, 5 to 20%. It is more preferable to set it in the range of 10 to 20%. It is more effective to set the total rolling ratio by the rolling passes performed at a temperature of 900°C or higher in (ii) above to 40% or more. The upper limit of the total rolling ratio by the rolling passes performed at a temperature of 900°C or higher is not particularly specified, but it may be set in the range of, for example, 65% or less. The rolling temperature of the final pass is preferably 700°C or higher. After the hot rolling is completed, it is preferable to rapidly cool the product by water cooling or the like.

[0037] [Cold rolling] Cold rolling is performed by a conventional method to obtain an intermediate product sheet material for the next step of solution treatment. If necessary, intermediate annealing and cold rolling may be performed once or multiple times to adjust the sheet thickness. The reduction ratio of the cold rolling is preferably set in the range of 90.0 to 99.5%.

[0038] [Solution treatment] The solution treatment is carried out under the conditions of an average heating rate of 10°C / s or more from 300°C to 800°C, a holding time of 10 seconds or more at 800 to 1020°C, and an average cooling rate of 50°C / s or more from 800°C to 500°C, for the purpose of maximizing precipitation strengthening and ultimately obtaining a distribution form of Mg-S-based particles that improves press punchability. In addition, water cooling or oil cooling can be used as a means to increase the average cooling rate. If the heating rate or cooling rate is slower than the above range, it becomes difficult to stably achieve a high strength of 900MPa or more. The reason for this is not necessarily clear at present, but it is presumed that the presence of Mg-S-based precipitates in the parent phase causes the solid solution behavior of Ni, Co, and Si to be different from normal, and that the heat pattern, including the heating process and cooling process, must be controlled more strictly than before. If the heating rate or cooling rate is slow, if the holding temperature for solution treatment is lower than 800°C, or if the holding time at 800°C or higher is too short, the solution treatment will be insufficient and it will be difficult to stably obtain a high strength of tensile strength of 900 MPa or more. In addition, the final result will be that "the number of Mg-S particles with a circle equivalent diameter of 0.5 μm or more is 300 / mm 2 It becomes difficult to obtain a structural state in which Mg-S particles having a number density of 0.5 μm or more and an average particle diameter of Mg-S particles having a circle equivalent diameter of 0.5 μm or more are 3.0 μm or less in circle equivalent diameter, and it becomes impossible to achieve both high strength and improved press formability. In addition, these Mg-S particles have the effect of suppressing the coarsening of crystal grains, and preventing a decrease in strength and bending workability. If the holding time of the solution treatment is higher than 1020°C, the crystal grains may become coarse, which may lead to a decrease in strength and bending workability. Holding time at 800°C or higher for too long is uneconomical. The holding time at 800 to 1020°C is preferably set in the range of 10 to 600 seconds.

[0039] [Aging process] Next, aging treatment is performed. The aging treatment conditions may be set according to the required properties within the range of an aging temperature of 400 to 550°C and a holding time in that temperature range of 1 to 24 hours.

[0040] [Finishing cold rolling] The final cold rolling performed after the aging treatment is referred to as "finish cold rolling" in this specification. The rolling reduction ratio of the finish cold rolling is preferably set in the range of 10 to 80%. Considering the processing application to small current-carrying parts such as connectors, the final plate thickness is preferably set in the range of, for example, 0.05 to 0.40 mm. The plate thickness setting range may be 0.05 to 0.25 mm, or 0.06 to 0.15 mm.

[0041] [Low temperature annealing] As the final heat treatment, it is preferable to perform low-temperature annealing for the purpose of reducing residual stress, improving bending workability, improving stress relaxation resistance by reducing voids and dislocations on slip planes, etc. The conditions for low-temperature annealing may be heating conditions that do not cause recrystallization within a holding temperature range of 150 to 500°C and a holding time range of 5 seconds to 5 hours. EXAMPLES

[0042] Copper alloys having the chemical compositions shown in Tables 1A, 1B, 2A, and 2B (hereinafter abbreviated as "Tables 1A to 2B") were melted and cast using a vertical semi-continuous casting machine. A Cu-20.1 mass% S alloy was used to add S. The resulting cast pieces were heated at 1000°C for 3 hours, extracted, hot rolled to a thickness of 10 mm, and water-cooled. The hot rolling conditions are shown in Tables 1A to 2B. The total hot rolling reduction was 90 to 95%. The rolling temperature of the final pass of hot rolling was 700°C or higher in all cases. Except for some comparative examples (No. 41) in which cracks occurred during hot rolling, after hot rolling, the oxide layer on the surface was removed by mechanical polishing (face cutting), and cold rolling was performed to obtain intermediate product sheets to be subjected to solution treatment. Each intermediate product sheet was subjected to solution treatment under the conditions shown in Tables 1A to 2B. After that, aging treatment, finish cold rolling, and low-temperature annealing were performed to obtain a plate product (test material) with a thickness of 0.10 mm. The main manufacturing conditions for the processes other than hot rolling and solution treatment are also shown in Tables 1A to 2B. Note that the hot rolling and cold rolling reduction ratios shown in the tables are rounded off to the nearest whole number.

[0043] The following investigations were carried out on each test material.

[0044] [Number density and average particle size of Mg-S particles] According to the above-mentioned "Analysis method of Mg-S-based particles", the cross section (TD surface) parallel to the rolling direction and plate thickness direction of the test material was observed with an FE-SEM equipped with an EDX device and EDX analysis was performed. The sample surface was prepared by mechanical polishing using 0.04 μm colloidal silica and then ion milling. The ion milling conditions were SVM-741 manufactured by Sanyu Electronics, accelerating voltage 6 kV, irradiation current 120 μA, time 30 minutes, and tilt angle 60°. In the FE-SEM observation, a backscattered electron image was obtained with a JSM-7200F manufactured by JEOL, magnification 500 times, voltage 15 kV, current level 12 to 14, and dead time 30 to 60%. One field of view was a rectangular area of ​​170 μm × 240 μm. The constituent elements of the particles, Mg, S, Co, Ni, and Si, are lighter than the metal base, Cu, so in the backscattered electron image, Mg-S, Ni-Co-Si, Ni-Si, and Co-Si particles all appear darker than the metal base. By binarizing the backscattered electron image, the particles present in the metal base can be clearly identified. Here, the backscattered electron image was binarized with the contrast set to 3800-4000 and the brightness set to 300-800.

[0045] All particles in the field of view with a circle equivalent diameter of 0.5 μm or more were subjected to elemental analysis by EDX. The EDX device used was X-MaxN50 manufactured by Oxford Instruments. The analysis software used was AZtec (Ver.4.0 SP2 HF1) manufactured by the same company. The measurement conditions were exposure time of 2 seconds per particle, energy range of 0-20 keV, number of channels 2048, and process time mode 4 was selected. In the EDX measurement of particles using this device, the electron beam was programmed to automatically aim at the center of each measurement target particle in the field of view. Particles with a circle equivalent diameter of 0.5 μm or more in which both Mg and S were detected were selected as "Mg-S-based particles." Here, the area of ​​four consecutive fields of view overlapping with an area ratio of 10% in the long side direction was set as one measurement area. The area of ​​one measurement area is the area of ​​four fields of view minus the area of ​​the overlapping parts, so (0.17mm x 0.24mm x 4) - (0.17mm x 0.24mm x 0.1 x 3) = 0.151mm 2 The number density of Mg-S particles (particles / mm 2 The average particle size (μm) was calculated based on the diameter of the particle and the equivalent circle diameter. This operation was repeated n = 5 times for different non-overlapping measurement areas set randomly. The total area of ​​the measurement areas was 0.151 mm 2 ×5=0.755mm 2 It is.

[0046] For reference, FIG. 1 shows an example of an SEM image of one measurement area in which the particles have been made clear by binarization processing. This is a stitched-together image of four fields of view for the sample material No. 1, which is an example of the present invention, as described above. The original image, in which the Mg-S-based particles are displayed in red, has been converted to monochrome and is shown here. Of the particles displayed, approximately 42% by number are Mg-S-based particles displayed in red. The remaining particles are almost all either Ni-Co-Si-based particles, Ni-Si-based particles, or Co-Si-based particles.

[0047] [Average grain size] According to the above-mentioned "Method of measuring average crystal grain size", the average crystal grain size was determined for a cross section (LD surface) perpendicular to the rolling direction of the test material sheet by a cutting method in accordance with JIS H0501-1986.

[0048] [conductivity] The electrical conductivity of each test material was measured by the double bridge, average cross-sectional area method in accordance with JIS H0505. Considering the electrical conductivity required for current-carrying parts such as small connectors, materials with electrical conductivity of 40% IACS or more were judged to pass.

[0049] [Tensile strength] Tensile test pieces (JIS No. 5) were taken from each test material in the rolling direction, and tensile tests were conducted in accordance with JIS Z2241 with n=3 tests to measure tensile strength. The average value of n=3 was used as the performance value for the test material. From the perspective of ensuring high reliability as an electrical conductive part such as a connector, which is becoming thinner, a test material with a tensile strength of 900 MPa or more in the rolling direction was judged to pass.

[0050] [Press punching ability] A test was conducted to punch out a square test piece of 5mm x 5mm using a press die for a test material with a thickness of 0.10mm. The clearance was set to two levels, 4% and 10% of the plate thickness. The square test piece was punched out so that two of the four cuts (end faces) formed on it were parallel to the rolling direction. Figure 2 shows the shape of the cut of the punched test piece. The size of the burrs is exaggerated. For the cuts parallel to the rolling direction of the test piece, the surface height as seen in the normal direction of the cut was measured on a line over the entire length in the plate thickness direction (punch axial direction) using a laser microscope, and a profile of the surface unevenness was created. From the profile, the length of the shear surface shown by symbol A in Figure 2 was determined, and the ratio of the shear surface to the shear surface and the fracture surface was calculated. Here, for the convenience of measurement, the length including the burr part shown by symbol B in Figure 2 was considered to be the length of the fracture surface, and the "shear surface ratio" was calculated using the following formula (2). In this press punching test, the height of the burrs is usually less than 1 μm, so there is no problem in evaluating the press punchability by including the burrs in the length of the fracture surface. Shear surface ratio (%) = 100 × A / (A+B) …(2) This measurement was performed at 10 locations on the cut surface (end face) parallel to the rolling direction of the test piece, and the shear surface ratio was calculated at each location using formula (2). The arithmetic mean of these values ​​was calculated, and this mean value was adopted as the shear surface ratio of the test material. In conventional Cu-Ni-(Co)-Si copper alloy sheet materials, the shear surface ratio in this test is about 50 to 60%. Test materials with a shear surface ratio of 40% or less under both clearance conditions of 4% and 10% can be judged to have a significant improvement in press punchability.

[0051] The results are shown in Tables 1A to 2B.

[0052] [Table 1A]

[0053] [Table 1B]

[0054] [Table 2A]

[0055] [Table 2B]

[0056] The test materials of the examples of the present invention, which contained the specified amounts of Mg and S and were hot-rolled and solution-treated under conditions within the ranges specified by the present invention, all had high tensile strength in the rolling direction of 900 MPa or more, electrical conductivity of 40% IACS or more, and a shear area ratio of 40% or less, demonstrating a significant improvement in press-punchability.

[0057] In contrast, Comparative Examples Nos. 31, 32, and 46 had insufficient number density of Mg-S particles with a circle equivalent diameter of 0.5 μm or more due to low Mg and S contents, and the improvement of press punchability (reduction of shear surface ratio) was insufficient. Among these, Nos. 31 and 32 also had low Si contents, which resulted in insufficient formation of precipitates that contribute to strength, and the tensile strength was low. Nos. 33, 34, 36, and 40 had low S content, so the number density of Mg-S particles with a circle equivalent diameter of 0.5 μm or more was insufficient, and the improvement of press punchability (reduction of shear surface ratio) was insufficient. Of these, No. 34 had low strength because the holding time of the solution treatment was short, which resulted in insufficient solid solution formation. It is thought that the strength improvement effect of fine Mg-S precipitates was not fully exerted due to the very low S content, resulting in insufficient strength. In No. 35, the solid solution behavior of Ni, Co, and Si is different from normal due to the presence of Mg-S phase, but the heating rate of the solution treatment was slower than the range specified in the present invention, which is thought to have resulted in insufficient solid solution of Ni, Co, and Si. In addition, the S content was too high, resulting in the formation of many coarse Mg-S particles. For these reasons, the strength was low. No. 37, 43, and 45 had low total reduction ratios in passes over 900℃ during hot rolling, which resulted in insufficient division of the Mg-S phase in the slab and made the average particle size of the Mg-S particles too large. As a result, the strength was low. No. 43 in particular had a large decrease in strength because the cooling rate during solution treatment was also slow. No. 38 had a low Mg content, and therefore the strength-improving effect of the solid solution strengthening of Mg and the synergistic effect with the (Ni,Co)2Si, Ni2Si, and Co2Si precipitates was not fully exerted, resulting in low strength. No.39 had low electrical conductivity due to too much Mg content. In addition, it had a lot of coarse Mg-S particles, which resulted in low strength. No. 41 had a high S content and the reduction ratio per pass in hot rolling at 800°C or higher was large, so cracks occurred during hot rolling and the experiment was discontinued. Nos. 42 and 44 had low S content, which resulted in an insufficient number density of Mg-S particles with a circular equivalent diameter of 0.5 μm or more, and the improvement in press punchability was insufficient. Of these, No. 42 had low strength because the cooling rate in the solution treatment was slow, which resulted in insufficient formation of precipitates that contribute to strength. No. 44 had low strength because the total content of Ni and Co was too low, which is thought to have resulted in a shortage of fine (Ni,Co)2Si precipitates that contribute to strength. No. 47 had low strength because the solution treatment temperature was low, and the total reduction ratio at 900℃ or higher was not sufficiently ensured in the hot rolling, so the Mg-S phase in the slab was not sufficiently divided, and the improvement of press punchability was not fully achieved.

Claims

1. The steel has a chemical composition, in mass%, of 1.50 to 5.50% total of Ni and Co, 1.00% or more Ni, 0.50 to 1.20% Si, 0.001 to 0.20% S, 0.01 to 0.20% Mg, 0 to 0.03% Cr, 0 to 0.01% Zn, 0 to 0.07% Mn, 0 to 0.05% B, 0 to 0.05% P, 0 to 0.01% Ag, 0 to 0.04% Al, 0 to 0.04% Zr, 0 to 0.04% Ti, the balance being Cu and unavoidable impurities, and has 300 Mg-S based particles per mm having a circle equivalent diameter of 0.5 μm or more in a cross section parallel to the rolling direction and the plate thickness direction. 2 the Mg-S based particles are present at a number density of at least 100% by mass, the Mg-S based particles have an average particle diameter of at most 3.0 μm in terms of equivalent circle diameter, and the copper alloy sheet has a tensile strength in the rolling direction of at least 900 MPa.

2. The copper alloy sheet material according to claim 1, wherein the total amount of Ni and Co in the chemical composition is 2.00 to 4.00%.

3. 3. The copper alloy sheet material according to claim 1, having an electrical conductivity of 40% IACS or more.

4. The copper alloy sheet material according to any one of claims 1 to 3, wherein the average crystal grain size in a cross section perpendicular to the rolling direction is 1 to 20 µm, as measured by a cutting method in accordance with JIS H0501-1986.

5. A plate material is manufactured from a cast slab having a chemical composition consisting of, in mass%, the sum of Ni and Co: 1.50 to 5.50%, Ni: 1.00% or more, Si: 0.50 to 1.20%, S: 0.001 to 0.20%, Mg: 0.01 to 0.20%, Cr: 0 to 0.03%, Zn: 0 to 0.01%, Mn: 0 to 0.07%, B: 0 to 0.05%, P: 0 to 0.05%, Ag: 0 to 0.01%, Al: 0 to 0.04%, Zr: 0 to 0.04%, Ti: 0 to 0.02%, the balance being Cu and unavoidable impurities, by a process including hot rolling, cold rolling, solution treatment, and aging treatment in the above order, In the hot rolling process, the rolling ratio per pass in all rolling passes performed at a temperature of 800° C. or higher is 20% or less, and the total rolling ratio in all rolling passes performed at a temperature of 900° C. or higher is 38% or more; In the solution treatment process, the average heating rate from 300°C to 800°C is 10°C / s or more, the temperature is held at 800 to 1020°C for 10 seconds or more, and the average cooling rate from 800°C to 500°C is 50°C / s or more. The method for producing the copper alloy sheet material according to any one of claims 1 to 4.

6. The method for producing a copper alloy sheet according to claim 5, wherein the aging treatment is performed at a temperature of 400 to 550°C.

7. A current-carrying part using the copper alloy sheet material according to any one of claims 1 to 4.

8. An electric current-carrying part having a press-punched part, using the copper alloy sheet material according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • High strength and high conductivity copper alloy having excellent fatigue and intermediate temperature property

    JP2004225112A

  • Wiring material, insulation cable and method of producing insulation cable

    JP2014137950A

  • HIGH INTENSITY Cu-Ni-Co-Si BASED COPPER ALLOY SHEET MATERIAL AND PRODUCTION METHOD THEREOF, AND CONDUCTIVE COMPONENT

    JP2014156623A

  • High-strength high-conductivity copper alloy wire rod of excellent resistance to stress relaxation characteristics

    WO2003076672A1

  • Copper alloy material excellent in strength, bending workability and stress relaxation resistance, and method for producing the same