METHOD FOR PRODUCING w-BN SINTERED BODY USING SHOCK PRESSURE

By applying ultra-high pressure through explosive explosions and annealing, the method produces dense, high-hardness w-BN sintered bodies, addressing equipment limitations and maintaining w-BN's hardness, suitable for cutting tools and abrasive applications.

JP2024154195AActive Publication Date: 2024-10-30TOMEI DIAMOND +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023067901
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Existing methods for producing wurtzite boron nitride (w-BN) sintered bodies are limited by the need for expensive, high-pressure equipment with short lifespan, and result in mixed crystal structures that do not exhibit the original hardness of w-BN, due to phase transitions to cubic boron nitride (c-BN) under high pressure and temperature.

Method used

A method involving the application of instantaneous ultra-high pressure of 8 to 100 GPa to w-BN particles, using explosive explosions to bond adjacent particles without the need for static ultra-high pressure devices, allowing for the production of dense, 100% w-BN sintered bodies with added materials, and incorporating stress relief annealing to improve bonding strength.

Benefits of technology

The method enables the production of w-BN sintered bodies with hardness exceeding 20 GPa, overcoming dimensional and cost limitations of traditional equipment, and maintaining the hardness of w-BN by preventing phase transitions to c-BN, suitable for cutting tools and abrasive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154195000001_ABST
    Figure 2024154195000001_ABST
Patent Text Reader

Abstract

To obtain: a w-BN-based sintered body having good properties without upper limit of producible dimension and without high equipment cost; or a w-BN-based composite impact sintered body added with a material having hardness of 20 GPa or more.SOLUTION: A method for producing a w-BN-based sintered body includes subjecting a starting particle aggregate containing wurtzite-type boron nitride (hereinafter referred to as w-BN) particles and a hard material single crystal particle to an instantaneous ultra-high pressure of 8 to 100 GPa to make the adjacent particles bond with each other, thereby collecting a sintered body of integrated particles, wherein: the particle aggregate comprises, in terms of composition ratio, 10 mass% or more of w-BN (raw material composition); and an ultra-high pressure is applied under close contact between w-BN and the hard material single crystal particle.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel compound sintered body based on wurtzite-type boron nitride and a method for producing the same. [Background technology]

[0002] Wurtzite boron nitride (w-BN) particles are an aggregate of fine crystal particles with excellent mechanical properties, and are industrially produced by applying shock pressure from explosive explosions to low-pressure phase h-BN. Because the shock pressure application time is extremely short, on the order of microseconds, the product is obtained in the form of agglomerated particles of 200 nm (0.2 μm) or more, in which fine primary particles of about several tens of nm are entangled.

[0003] The hardness of w-BN is 114 GPa according to theoretical analysis, which is higher than the hardness of diamond (90 GPa) and is known to be significantly harder than the approximately 50 GPa of cubic boron nitride (hereafter c-BN), which is the high-pressure phase of the same compound and is considered to be a high-hardness material. In terms of heat resistance, diamond is about 600°C in air, whereas c-BN is said to not undergo phase transformation to the low-pressure phase h-BN even at 1400°C (Non-Patent Documents 1 and 2).

[0004] On the other hand, although there is no data on w-BN itself, in addition to excellent hardness, it has low reactivity with iron-group metals, just like c-BN. Therefore, sintered materials sintered either alone (Patent Document 1) or mixed with c-BN (Patent Documents 2 and 3) are suitable materials for manufacturing various tool components for cutting and grinding steel, etc.

[0005] Sintered bodies or chunks of w-BN, c-BN or diamond are mainly obtained by adding sintering aids such as metals to powders or particles of these materials, loading them into a high-pressure, high-temperature apparatus (hereafter referred to as a high-pressure apparatus), and treating them under high-pressure, high-temperature conditions of several GPa and 1200°C or higher (Patent Documents 1-3).

[0006] As mentioned above, the high-pressure equipment used for sintering high-hardness materials is designed to withstand ultra-high pressures of several GPa and severe high pressures and high temperatures of several thousand degrees Celsius, so the spatial shape and volume in which the sintered raw material is stored is restricted, and it is limited to a disk with a diameter of 100 mm and a thickness of 10 mm at most. In addition, the special structure of such equipment increases the manufacturing costs, and the component parts are subjected to large stresses, resulting in a short lifespan, which inevitably makes the sintered products expensive.

[0007] Previously, there have been attempts to bond w-BN, c-BN or diamond particles by using the high shock pressure associated with the explosion of explosives without using a static ultra-high pressure device, but no results suitable for industrial production have been obtained. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Laid-Open No. 61-100302 [Patent Document 2] Japanese Patent Publication No. 63-266030 [Patent Document 3] Japanese Patent Application Publication No. 176769 / 1983 [Non-patent literature]

[0009] [Non-Patent Document 1] DeVries, General Electric Report No. 72-CRD, 178, June (1972) [Non-Patent Document 2] Z. Pan et al., Physical Review Letters 102 (5), 055503-1, (2009). The American Physical Society Summary of the Invention [Problem to be solved by the invention]

[0010] w-BN is a thermodynamically metastable phase, and it is believed that a transition to c-BN is observed from around 1000°C in the pressure and temperature range of the c-BN stable phase, which is the stable phase under high pressure. Therefore, the w-BN sintered body obtained by static pressing always exhibits a w-BN / c-BN mixed crystal structure, and no sintered body exhibiting the inherent hardness of w-BN has been obtained.

[0011] The present invention aims to obtain a w-BN based sintered body with good properties without any upper limit on the manufacturable dimensions and without requiring high equipment costs, or a w-BN based composite impact sintered body with added material having a hardness of 20 GPa or more. Another object of the present invention is to obtain a dense sintered body consisting essentially of 100% w-BN. [Means for solving the problem]

[0012] The gist of the present invention lies in a method for producing a w-BN-based sintered body, in which a starting particle aggregate containing wurtzite-type boron nitride (hereinafter referred to as w-BN) particles and hard material single crystal particles is subjected to an instantaneous ultra-high pressure of 8 to 100 GPa to bond adjacent particles together, and a sintered body of the integrated particles is recovered, in which the particle aggregate contains w-BN at a composition ratio of 10 mass% or more (raw material composition), and the ultra-high pressure is applied under intimate contact between the w-BN and the hard material single crystal particles. Effect of the Invention

[0013] In the present invention, the w-BN powder mixture is subjected to an impact pressure of a scale that cannot be achieved by a normal industrial-scale static pressure method during an explosive explosion, thereby densifying the w-BN powder. In addition, the instantaneous and short-term nature of the heating under this explosion suppresses the phase transition to c-BN, making it possible to obtain a sintered body that is essentially 100% w-BN.

[0014] Previously, there have been attempts to bond high-hardness particles of c-BN and diamond using the high shock pressure from explosive explosions without relying on static ultra-high pressure equipment, but no results suitable for industrial production have been achieved. The main reason for this is believed to be that, for example, when attempting to bond only c-BN particles, since most c-BN and other high-hardness material particles are polyhedral crystals, it is difficult for adjacent particles to blend together, and it is not possible to bond them together without gaps.

[0015] In contrast, in the present invention, w-BN is used as a high-hardness material to form the sintered body. W-BN is synthesized by narrowing the lattice spacing of hexagonal boron nitride (hereafter referred to as h-BN) by applying a momentary high pressure for about 1 μs, causing a phase transition, and the individual particles are 100 nm (1×10 -4 It is an irregular polycrystalline particle formed by an aggregation of minute crystals of size 0.1m or less, and therefore does not have the cleavage that is unavoidably present in single crystal particles.

[0016] On the other hand, w-BN, which is an aggregate of fine crystals, does not have the sharp corners and edges that single crystal particles have to function as cutting edges. Therefore, when w-BN alone is formed into a lump by impact pressure and used as a cutting tool, it is suitable for machining the surface of a workpiece to a fine finish, but is not suitable for highly efficient cutting processes that require deep cuts. Therefore, it is preferable to use w-BN as a lump integrated with single crystal particles other than w-BN that have sharp corners and edges when making cutting tools. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a configuration for the direct impact pressure method of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a configuration for the indirect impact pressure method of the present invention. EMBODIMENTS OF THE PRESENTINVENTION

[0018] The starting w-BN particles used in the shock pressurization treatment in the present invention are suitable for bonding with cleavable single crystal particles such as diamond, c-BN, and other high hardness substances with Vickers hardness of 20 GPa or more to form a sintered body, taking advantage of the characteristic that w-BN does not have cleavage even when sintered alone. The reason is that since it has no sharp corners or flat surfaces and is amorphous, it easily penetrates between single crystal particles, and is suitable for compressing the whole body to a high density without cleaving the single crystal particles.

[0019] Since the reaction time of w-BN particles synthesized using impact pressure is short, they have many defects inside the crystals in addition to the fineness of the primary particles, and the surface is active, and it is presumed that these factors work in the direction of promoting the bonding between particles during sintering. The smaller the aggregate particle size, the larger the overall surface area and the more active it is in the sintering reaction, so in the present invention, it is particularly preferable to use an average particle size of 5 μm or less.

[0020] Other than sintering w-BN alone, in order to create a composite sintered body by bonding cleavable single crystal particles with w-BN, which is a polycrystalline particle, it is preferable to interpose w-BN particles between the single crystal particles. From this perspective, it is appropriate that the average particle size of the w-BN particles is smaller than the average particle size of the single crystal particles to be combined, and in particular it is preferable that it is 1 / 2 or less.

[0021] The problem with the mechanism of sintering particle aggregates by explosive pressure is that the material is compressed strongly by the instantaneous pressure, causing the temperature of the entire material to rise rapidly, and the temperature to drop during the compression pressure release process, and localized residual stresses are generated due to factors such as uneven compression. Therefore, it is preferable to perform stress relief annealing as a post-process as necessary.

[0022] Annealing is also effective for improving the bonding strength in sintered bodies obtained by adding sintering aids and applying impact. The annealing conditions are set based on the material composition of the pressure sintered product, but generally, heating to a temperature range of 700°C to 1700°C for 1 hour to 24 hours is also effective.

[0023] In the present invention, the mechanism of sintering w-BN particles or w-BN particles and added single crystal particles by explosion pressure is considered to be the same as in the case of explosive pressure welding (explosive pressure bonding, explosive welding, explosive bonding, etc.), a metallurgical method that uses the explosion pressure of explosives to bond metals together, and it is believed that the bonding is performed without generating compounds between the bonding surfaces. However, some compounds are inevitably generated due to the molten state caused by the jet generated by the collision between particles, and bonding by these compounds cannot be excluded. If a decrease in hardness of the resulting sintered body can be tolerated to a certain extent, it is also possible to add metal materials such as Al, Si, Ti, Zr, Hf, Ta, etc. as sintering aids, either alone or in combination, and sinter under a lower pressure load by using less explosives.

[0024] By adding the above metals, bonding occurs with the formation of metal nitrides or borides with w-BN, or bonding occurs due to the affinity between the metals. In these cases, sintering is possible at lower pressures and temperatures than the sintering conditions for w-BN alone, and the hardness of the resulting sintered body is lower than that of a sintered body made of w-BN alone, but since the sintered body can be made with a small explosive force, it is within the range of choice if the product objective can be achieved even with a sintered body with a slightly lower hardness.

[0025] In addition, when stress relief annealing is performed according to the present invention, it is assumed that the material sintered with the addition of the sintering aid will not react with w-BN during the sintering process due to the impact pressure and will remain as a metal, but in this case too, it is expected that the annealing heat will stabilize the material while reacting with w-BN to form a compound. It is also expected that the sintered body will be stabilized by adding an appropriate amount of ceramics such as carbides, nitrides, borides, and oxides of specific metals that have chemical activity against boron nitride.

[0026] The stress relief annealing operation in the present invention can be carried out in a non-oxidizing atmosphere under normal pressure, but it is more effective for promoting densification if it is carried out under pressure. As the pressure application method, various means such as hot pressing, HIP, and ultra-high pressure can be used.

[0027] In the present invention, the pressure applied to the treated material is the impact pressure generated when an explosive explodes. By using this method according to the present invention, although there are environmental restrictions on the amount of explosive that can cause an explosion, there are no dimensional restrictions in principle, and since no static ultra-high pressure device is used, various problems such as restrictions on manufacturable dimensions and high manufacturing costs due to the use of such devices can be avoided.

[0028] In the present invention, the impact pressure applied to the w-BN or a mixture of w-BN and a sintering aid is calculated by first determining the explosion pressure of the explosive, then calculating the pressure value applied to the container of the impact object due to that pressure, and then determining the pressure transmitted from the container to the w-BN or the mixture of w-BN and a sintering aid contained therein. In the present invention, the direct method and indirect method described in detail below can be used as a method for transmitting the explosion pressure of an explosive to a material sealed in a metal tube.

[0029] The direct method involves detonating explosives placed around a metal tube containing the material to be sintered, thereby transmitting pressure to the impacted material. On the other hand, the indirect method involves arranging metal tubes (flying tubes) with an inner diameter larger than the outer diameter of the metal tube containing the impacted material to be sintered in a concentric pattern, detonating explosives placed around the outside of the tube, and causing the flying tube to collide centripetally with the material storage tube at high speed, thereby transmitting pressure.

[0030] The present invention will now be described in detail with reference to the accompanying drawings. In Fig. 1, which shows an outline of the components of the direct method, the opening at one end of a steel treated material storage tube 1 is sealed with a metal plug 2, filled with starting material 3 consisting of w-BN or a powder mixture of w-BN and a sintering aid, and the other end is plugged with a similar metal plug 4. The whole is placed coaxially inside a larger diameter, bottomed steel explosive storage tube 5, filled with explosive 6, sealed with an end plate 7 made of any material, and an electric detonator 8 is attached.

[0031] When the explosive 6 is detonated by the detonator 8, a detonation wave travels from the detonated side to the opposite side at a high speed characteristic of the explosive, and the steel tube 1 is compressed toward the central axis at high speed by the generated explosion pressure, and at the same time, the starting material containing w-BN contained therein is integrated by the compression load.

[0032] On the other hand, in the indirect method, metal tubes (flying tubes) with an inner diameter larger than the outer diameter of the metal tube containing the material to be sintered are arranged concentrically, and explosives placed around the outside of the tubes are detonated to transmit pressure by causing the flying tubes to collide centripetally with the material storage tube at high speed. In Fig. 2, elements 1 to 8 are configured in the same way as in Fig. 1, but a metal cylinder 11 is arranged around the outer periphery of the steel tube 1 containing the material to be treated in order to fly the tubes and cause them to collide with the steel tube 1. There is a space 12 between the steel tube 1 and the metal cylinder 11.

[0033] When the explosive 6 is detonated by the detonator 8, a detonation wave travels from the detonated side to the opposite side at a speed specific to the explosive, and the generated explosion pressure causes the flying metal cylinder 11 to contract at high speed, and then passes through the space 12 and impact compresses the surface of the treated material storage tube 1, thereby compressing and integrating the w-BN or the powder mixture of w-BN and single crystal particles and / or these with sintering aids inside the steel tube.

[0034] The pressures generated in the direct and indirect methods are calculated below. As a special example in the present invention, there is also a method in which impact pressure is applied to a flat material, and the pressure applied in that case can also be calculated in the same manner by referring to the following description.

[0035] The explosion pressure P of the explosive required for both the direct and indirect methods can be roughly calculated using the following formula, assuming that the initial density of the explosive is ρ0 and the explosion velocity is D. P = ρD 2 / 4 ..... 1) P: Pressure N / m 2 , ρ0: density kg / m 3 , D: Explosion velocity m / s Density 1.1×10 3 kg / m 3, explosion speed 2.8×10 3 The pressure P generated by an explosive of m / s is P = ρD 2 / 4 = 1.1×10 3 kg / m 3 ×(2.8×10 3 m / s) 2 / 4 = 2.156×10 9 kgm / m 2 s 2 = 2.156 GPa The pressure obtained is an estimate and may be rounded to 2.2 GPa.

[0036] In both the direct and indirect methods, it is considered that 60% of the explosive energy is transferred to the metal tube in contact with the explosive, and this value is called the Gurney energy (US Pat. 3,667,911). In addition, when the material to be impacted is contained in a cylinder, the energy consumed by the deformation of the cylinder due to the impact is a small amount of the loaded energy and can be ignored.

[0037] In the direct method, when the metal tube that contains the material (hereinafter referred to as the material storage tube) receives the impact of the explosion, it contracts toward the central axis of the tube, compressing the stored material. Strictly speaking, since the material storage tube is in contact with the material, it does not fly through space, but since it is possible to calculate the speed at which metal is accelerated by the explosion pressure, as a convenience method, it is assumed that the material storage tube flies a small distance and collides with the material.

[0038] In order to understand the behavior of w-BN particles subjected to impact pressure through a material storage tube, it is first necessary to determine the impact properties of w-BN. Since the impact properties of w-BN cannot be obtained from published data, we will use those of cubic boron nitride (hereafter c-BN), which is also a high-pressure phase of boron nitride, instead. The specific volume V of c-BN having a true density under high pressure at each pressure can be obtained by the following procedure.

[0039] Shock wave velocity U of the material under impacts , sound speed C0, particle speed U p The relation between the coefficient S and U s = C0+ SU p ..... 2) P = ρU s U p = ρ0(C0U p +SU p 2 ) ..... 3) from, U p = [{(ρ0C0) 2 +4ρ0SP} 1 / 2 ] / 2ρ0S ..... 4) In c-BN, C0 = 1.19 × 10 4 m / s, S = 1.11, ρ0 = 3.48×10 3 kg / m 3 and [4] Therefore, equation 4) becomes: U p = [{(3.48×10 3 × 1.19×10 4 ) 2 + 4 × 3.48×10 3 × 1.1 × P} 1 / 2 and the specific volume V is given by the following equation: V = V0(U s - U p ) / U s ..... 5) [4] : N. Kawai et al., Shock compression of cubic boron nitride, J. Appl. Phys. 106, 033508 (2009)

[0040] The true density w-BN (substituted with the value of c-BN) at each pressure can be obtained by equations 3), 4), and 5). However, the material subjected to impact is a powder filled material and has a low density. The behavior of the material with voids under impact is different from that of the true density material under high pressure. The behavior of the material under impact must be calculated by the following equation. [5] . P = P H [1-ρ γ (V0-V) / 2] / [1- ρ γ (V0* - V) / 2] ..... 6) P: Pressure of the material with voids P H : Pressure of the material at true density ρ γ : Defined in Equation 7) V0: Initial specific volume of the material with true density V0*: Initial specific volume of the material with voids [5] : RG McQueen et al. (1970) "The equation of solids from shock wave studies" in High-Velocity Impact Phenomena (ed. R. Kinslow), Academic Press, New York, pp.293-417

[0041] ρ in Equation 6 γ is defined by equation 7), and γ or γ0 is called the Gruneisen coefficient and is defined by equation 7). ρ0γ0= ρ γ ..... 7) ρ0: initial density of material ρ: density at any pressure γ0: Gruneisen coefficient at the initial density of the material γ: Gruneisen coefficient at density ρ The meaning of this formula is that even if the material density changes due to pressure, the value obtained as the product of density and the Gruneisen coefficient does not change. The initial value of the Gruneisen coefficient γ0 is defined by the following formula from physical considerations.

[0042] γ0= 2S-1 ..... 8) S in formula 8) is S in formula 2). Therefore, γ0 of c-BN is γ0= 2S - 1 = 2 × 1.11 - 1 = 1.22 It is.

[0043] When calculating the various values ​​when impact is applied to c-BN having voids using formula 6), the ratio of the packing density to the true density is taken as the packing rate, which in the present invention is set to 75% based on past experience. V0= 1 / ρ0= 1 / 3480 = 0.2874 ×10 -4 m 3 / kg V0* = 1 / (ρ0× 0.75) = 1 / (3480×0.75) = 1 / 2610 = 0.3831×10 -3 m 3 / kg

[0044] Once the PV relationship for c-BN with voids is obtained, the particle velocity U at each pressure can be calculated using equations 9) and 10). p1 and shock wave speed U s1 It is possible to obtain the following. U p = [(P - P0)(V0- V)] 1 / 2 ..... 9) U s = V0[(P - P0) / (V0- V)] 1 / 2 ..... 10) Table 1 shows the true density of c-BN calculated by equations 2) to 5). H , U p .U s , V are calculated, and then, using equations 6) to 10), P, U of c-BN with voids are calculated. p1 .U s1 The results of the relationship are shown below.

[0045] [Table 1]

[0046] High pressure data for true density c-BN P H , U p , U s , V High pressure data P, U for c-BN with voids p1 , U s1 , V (true density same as high pressure data for c-BN) Table 1 U of c-BN with voids p1 and Us1 The two-dimensional correlation was analyzed with a reliability of r = 0.994. U s1 = 1446.5 + 2.504U p ..... 11) The relationship was obtained.

[0047] The metal tube inscribed in the cylindrical explosive contracts toward its central axis, and in the direct method, high pressure is applied directly to the material stored in the metal tube, while in the indirect method, the material flies through space and collides with the metal tube containing the material. In both the direct and indirect methods, it can be considered that most of the energy generated by the explosion and directed toward the central axis is transferred to the stored material, and in the indirect method, the speed of the metal tube flying under the explosion pressure can be calculated using the following formula. V pm =(2E g ) 1 / 2 [{(1+2M d / M x ) 3 +1} / {6(1+M d / M x )}+M d / M x ] -1 / 2 ... 12) however V pm : The maximum flight tube speed obtainable by the system E g :Explosive explosion energy × 0.6 M d : explosive mass per unit area of ​​the flight tube kg / m 2 M x : Mass per unit area of ​​the flight tube kg / m 2 YP x / (M d V pm 2 ) = -ln(1 - V p / V pm )-V p / V pm .....13) Y: Flight distance until the flying tube hits the material storage tube m P x:Explosion pressure of explosive P a V p : The speed when the tube reaches the flight distance Y (m / s)

[0048] For example, the density explained in 0035 is 1.1×10 3 kg / m 3 , explosion speed 2.8×10 3 An explosive of 1.5 m / s is filled between an SGP150A steel explosive storage tube (outer diameter 165.2 mm x inner diameter 155.2 mm) and an STPG370 125A steel flight tube (outer diameter 139.8 mm x inner diameter 126.6 mm) and collided with an STPG370 80A steel material storage tube (outer diameter 89.1 mm x inner diameter 78.1 mm). Explosives explosion energy E is 4×10 3 In kJ / kg, the Gurney energy E g teeth, Eg = E × 0.6 = 2.4 × 10 3 kJ / kg Amount of explosive per unit area of ​​the flight tube M x and the mass per unit area of ​​the flight tube M d teeth, M x = 24.9kg / m 2 ; M d = 54.5kg / m 2 And by equation 12), V pm = 680.4m / s is obtained.

[0049] The flight distance of the flight tube is (Inner diameter of flight tube - outer diameter of material storage tube) / 2 = (0.1266 - 0.0891) / 2 = 0.01875 Therefore, the left side of equation 13) becomes: YP x / (M d V pm 2 ) = 0.01875 × 2.2×10 9 / (54.5 × 680.4 2 ) = 1.6349 Find the right hand side that is equal to that value, V = 627.5m / s Therefore, we can assume that the flight tube collides with the material storage tube at 627.5 m / s.

[0050] When the flying tube collides with the material storage tube, it shrinks and becomes thicker. The collision mass per surface area of ​​the material storage tube is calculated as M d When the flying tube with an outer diameter of 139.8 mm and an inner diameter of 126.6 mm collides with the material storage tube, the inner diameter becomes equal to the outer diameter of the material storage tube, which is 89.1 mm. d M d1 Then, M d1 = 77.4kg / m 2 It becomes.

[0051] The energy of a moving object is E = MV 2 / 2 ..... 14) In this case, E = 77.4kg / m 2 × (627.5m / s) 2 / 2 = 15.2MJ / m 2 The flight tube consumes energy due to deformation during the contraction process, but this amount is a small portion of the total energy and can be ignored. The material storage tube also deforms due to the impact, but this can also be ignored. Therefore, we will consider that all of the flight tube's kinetic energy is transferred to the material through the material storage tube.

[0052] Surface area of ​​material storage pipe 1m 2 The mass of the 75% w-BN per unit mass is 45.68 kg, and the energy provided by the flight tube is 15.2 MJ / m 2 When the energy received by w-BN per kg is E1= 332.7kJ / kg The impact properties of c-BN, which is assumed to have similar impact properties to w-BN, at a filling rate of 75%, are as follows: Us1 = 1446.5 + 2.504U p ..... 11) From U s1 If we set the explosion speed to 2800m / s, U p = 550.5m / s From equations 2) and 3), P = 4.06GPa V0 = 0.6061 x 10 -3 m 3 / kg V = 0.4891 x 10 -3 From 5), E = (P+P0)(V0-V) / 2 ..... 15) = 231kJ / kg The energy of the speed is 2.8 × 10 3 A shock wave of m / s is generated in the material.

[0053] This value is calculated based on the shock wave velocity U generated by the energy input from the flight tube of 332.7 kJ / kg. s = 3409 m / s. Therefore, in this case, for the w-BN with a filling rate of 75% located at the collision point of the flight tube, there is a U s =3409m / s, particle velocity U p At the pressure point where the pressure drops to P=4.06GPa in the direction of explosion, centered on the maximum pressure P=7.266GPa equivalent to P=816m / s, the velocity is 2.8×10 3 It forms a shock wave front of m / s.

[0054] As a concrete example, the direct method in which explosives are directly attached to the material storage tube shown in Figure 1 will be explained. (1) Impact material: 100% by mass w-BN, packing density 50% of theoretical density (2) Explosives storage steel pipe: SPG65A, outer diameter 76.3 mm, inner diameter 69.6 mm, length 300 mm (3) Filled explosive: outer diameter 69.6 mm, inner diameter 27.2 mm, loading density 1450 kg / m 3, length 300mm Explosion Speed ​​5×10 3 m / s, explosive energy 5×10 3 KJ (4) Impact material storage tube: Carbon steel STPG370 SCH40 20A, outer diameter 27.2 mm, inner diameter 21.4 mm, Length: 250mm (5) Metal plug to seal the material: outer diameter 21.4 mm, length 25 mm

[0055] From the above, the amount of explosives per unit area of ​​the material storage tube M x and the mass per unit area of ​​the flight tube M d teeth, M x = 55.44kg / m 2 , M d = 20.51kg / m 2 Then, according to equation 12, V pm teeth, V pm = 230m / s According to 0037, if we consider that the material storage tube flies a very small distance of 1 mm and collides with the material, then according to formula 13), the material storage tube will be V p = 816m / s The object will collide with the material at a speed of

[0056] The kinetic energy of the material storage tube is given by equation 14): E = 20.51 kg / m 2 × (2300m / s) 2 / 2 = 54.2MJ / m 2 It is assumed that all of this is transmitted to the material in the material storage pipe. The surface area of ​​the material storage pipe is 1m 2 Amount of material per unit M s teeth, M s = 17.5kg / m 2 It becomes. M s If the kinetic energy E of the material storage tube is transmitted to the material, the energy E per unit of material mass is s teeth, Es = E / E s = 54.2MJ / m 2 / 17.5kg / m 2 = 3.10MJ / kg It is.

[0057] When analyzing the impact conditions where the material subjected to the impact is 100% w-BN by mass and the filling density is 75% of the theoretical density, the w-BN density and hardness are extremely close to those of w-BN and c-BN, so the impact characteristics at high pressure shown by c-BN with a filling rate of 50% obtained earlier are: U s1 = 1.4465×10 3 + 2.504U p ..... 11) Here, let us assume that the explosive velocity of the explosive in the material is 5×10 3 E s If a shock wave is generated, the pressure generated in the material is 3) and 11). From this, the estimated energy was 18.5 GPa, and the introduced energy E s1 From equation 15), E s1 = 1.0MJ / kg Then, the introduced energy E s This is less than 3.10MJ / kg.

[0058] Energy introduced E s When the shock wave speed U is 3.10MJ / kg s and particle velocity U p The pressure P corresponding to the sequence is U s = 7435E s , U p = 2490E s , P = 48.5GPa and the shock wave velocity U s The explosion speed is 5×10 3The pressure is much faster than m / s, and at the highest pressure point close to the explosion impact point, it reaches 48.5 GPa. A shock wave precedes the explosion impact point, and when the pressure decays, it becomes a shock wave with a speed equal to the explosion speed. The following examples are provided to illustrate the embodiments of the present invention. Example 1

[0059] Using the configuration in Figure 2, w-BN powder consisting of 45% average grain size of 10 μm, 40% average grain size of 3 μm, and 15% grain size of 1 μm was sintered to obtain a sintered body by indirect impact pressure. 150 g of w-BN powder with the above grain size distribution was pressurized and filled into a material storage tube made of STPG37015A steel with an outer diameter of 27.2 mm, an inner diameter of 21.4 mm, and a length of 300 mm, and the inside of the tube was evacuated to below 1 Torr, sealed, and subjected to impact treatment.

[0060] The explosive tube was made of SGP 90A steel, with an outer diameter of 101.6 mm, an inner diameter of 93.2 mm, and a length of 400 mm, and the flight tube was made of STPG370 50A steel, with an outer diameter of 60.5 mm, an inner diameter of 52.7 mm, and a length of 400 mm, and was filled with 1.9 kg of ANFO explosive. The impact pressure due to this configuration was estimated to be about 35 GPa.

[0061] The w-BN was in the form of a tightly sintered round bar with a diameter of about 15 mm. This was cut using a diamond blade to take out 15 mm long specimens from three locations: the starting point of the explosive shock, the center of the tube, and the end of the tube. The density was measured and found to be 3.43 g / cm3 in the above order. 3 , 3.44g / cm 3 , 3.46g / cm 3 These values ​​give a true density of c-BN of 3.48 g / cm 3 These correspond to 98.6%, 98.9%, and 99.4%, respectively. The micro Vickers hardness of each of these samples was measured, and the average value of five points was in the range of 56 GPa to 58 GPa, with no difference observed depending on the location of the sample. Example 2

[0062] The material subjected to the impact load in Example 1 was placed in a high-pressure device, and the pressure and temperature were raised to 2 GPa and 1350°C, and held for 15 minutes, and then the pressure and temperature were returned to normal and the sample was collected. The density of the collected sample was 3.47 g / cm3 regardless of the impact position, as measured by the Archimedes method. 3 ~3.48g / cm 3 This was almost equal to the theoretical density of c-BN (Non-Patent Document 1). The Vickers hardness was also 78 GPa to 81 GPa regardless of the impact position, which was significantly higher than before treatment with the high-pressure device, and is thought to be due to the treatment further tightening the bonds between the constituent particles. X-ray diffraction measurement revealed a single phase of w-BN. Example 3

[0063] Ten types of samples were prepared by mixing w-BN powder with the metals, diamond, c-BN, metal carbides, oxides, or nitrides shown in Table 2. Each sample was packed into a material storage tube made of STPG37015A steel with an outer diameter of 27.2 mm, an inner diameter of 21.4 mm, and a length of 300 mm, and the tube was evacuated to a pressure of 1 Torr or less and sealed. Each sample was subjected to impact pressure treatment by indirect pressure using the configuration shown in Example 1. The ultimate pressure and the products identified by X-ray diffraction of the recovered materials are also shown in the same table.

[0064] [Table 2]

[0065] In Table 2, (1) The composition ratio of each component is expressed in mass%. (2) The particle size is the average value (μm). Single crystal particles other than w-BN include composite crystals consisting of unit single crystals of 1 μm or more. (3) Hardness is measured by the Vickers hardness GPa (Hv) of the sintered body. (4) Hardness and load pressure values ​​are rounded off. (5) The hardness of sintered products containing Al, Mg, Ti, Hf, Si, Ta, and Mo was measured after impact and subsequent heating at 1400°C for 1 hour in a nitrogen atmosphere. [Industrial Applicability]

[0066] Sintered w-BN is an ultra-hard material that is expected to find many applications in a variety of fields, including as an abrasive tool component or a wear-resistant component. [Explanation of symbols]

[0067] 1 Processing material storage tube 2 Metal plug 3 Starting material 4 Metal stopper 5 Explosives-containing steel pipe 6 Explosives 7 Metal end plate 8 Electric detonator 11 Metal cylinder 12 Space

Claims

1. This method for producing a w-BN-based sintered body involves subjecting a starting particle aggregate containing wurtzite-type boron nitride (hereinafter referred to as w-BN) particles and single crystal particles of a hard material to an instantaneous ultra-high pressure of 8 to 100 GPa to bond adjacent particles together, and then recovering a sintered body of the integrated particles. The particle aggregate contains 10 mass% or more w-BN in terms of composition (raw material composition), and the ultra-high pressure is applied under intimate contact between the w-BN and the single crystal particles of the hard material.

2. The hard material single crystal particles are H v The method according to claim 1, wherein the pressure is 20 GPa or more and the grain size is at least twice that of the w-BN grains.

3. The method according to claim 1, wherein the w-BN is fine particles having an average particle size of 5 μm or less, prepared by phase transformation of low-pressure phase boron nitride (h-BN) under ultra-high pressure.

4. The method of claim 1 , wherein the ultra-high pressure is due to the detonation of an explosive.

5. The method of claim 1 , wherein the hard material is diamond or cubic boron nitride (c-BN).

6. 2. The method according to claim 1, wherein the hard material is one or more selected from the group consisting of nitrides, carbides, borides, and oxides of specific metals that have chemical activity with boron nitride.

7. The method of claim 1 , wherein the particle assembly further contains the specified metal as a sintering aid.

8. 8. The method according to claim 1, wherein the specific metal is one to four selected from Al, Mg, Ti, Hf, Si, Ta, and Mo.

9. 10. The method of claim 1, further comprising heating the sintered body to a temperature of 700 to 1700°C in a non-oxidizing atmosphere.

10. 2. A w-BN-based sintered body according to claim 1, which contains three-dimensionally distributed, sized w-BN particles, and includes portions where adjacent w-BN particles are directly bonded to each other and are integrated as a whole.

11. 2. The w-BN based sintered body according to claim 1, further comprising a portion where adjacent w-BN particles are bonded to each other via particles of another kind.

Citation Information

Patent Citations

  • Production of high hardness sintered body

    JP1988266030A

  • Bonded body of highly pure boron nitride having wurtzite structure

    JP1989024074A

  • Shock pressurization / heat treatment method of porous material and apparatus therefor

    JP2005013838A

  • Method for producing high-purity boron nitride sintered compact having high hardness and high toughness

    JP2010024103A

  • Solidified body (sintered body) of high-toughness / high-pressure phase boron nitride and method of producing the same

    JP2021130589A