Method for producing tool steel

The method addresses the issues of undesirable metallographic structures and high costs in conventional spheroidizing annealing by using specific temperature controls and compositions, resulting in improved tool steel with enhanced mechanical and processing properties.

JP2024154276APending Publication Date: 2024-10-30DAIDO STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023068022
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

Conventional spheroidizing annealing methods for tool steel result in undesirable metallographic structures, such as the presence of bainite, and require additional heat treatment steps, increasing manufacturing costs.

Method used

A method involving specific chemical compositions and a four-step temperature control process during spheroidizing annealing, including heating above the Ac3 temperature, cooling to a lower temperature, and maintaining at a constant temperature, to promote spheroidization and refine the α structure without additional steps.

Benefits of technology

Achieves a suitable metallographic structure with reduced bainite and martensite, enabling tool steel with improved mechanical properties and processing characteristics while omitting additional heat treatment steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154276000001_ABST
    Figure 2024154276000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a tool steel capable of obtaining a tool steel suitably softened by spheroidizing annealing and having an improved metallic structure.SOLUTION: A method for producing tool steel comprises a step of preparing a steel material having a predetermined chemical composition, and a step of subjecting the steel material to spheroidizing annealing by performing a heating treatment for heating the steel material at a first temperature higher than the Ac3 point of the steel material, a cooling treatment for lowering the first temperature to a second temperature lower than the A1 point of the steel material, and a constant temperature holding treatment for holding the steel material at the second temperature for a predetermined time.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a tool steel. [Background technology]

[0002] Known examples of tool steel include hot die steel, cold die steel, plastic mold steel, etc. In general, a manufacturing process for tool steel first involves a step of melting various metallic raw materials in an electric arc furnace or the like to obtain molten steel, a step of refining the molten steel, and a step of casting the refined molten steel to obtain a steel material.

[0003] The steel is then subjected to homogenization heat treatment and hot working such as forging, and then spheroidizing annealing (SA) is performed to improve the mechanical properties and processing characteristics of the tool steel. The spheroidizing annealing is mainly performed for the purpose of softening the steel by spheroidizing the carbides in the metal structure of the steel.

[0004] Conventionally, various techniques related to spheroidizing annealing have been proposed. For example, the following Patent Document 1 discloses a technique of applying a magnetic field to a steel material before or during spheroidizing annealing in order to shorten the heat treatment time in spheroidizing annealing. In addition, Patent Document 2 discloses a technique of performing quenching after spheroidizing annealing in order to manufacture a tool steel for a die having the desired hardenability and spheroidizing annealing property. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-298640 [Patent Document 2] JP 2008-121032 A Summary of the Invention [Problem to be solved by the invention]

[0006] As described in the above Patent Documents 1 and 2, in one example of conventional spheroidizing annealing, a steel material is heated to a predetermined temperature higher than the A1 point of the steel material, and then slowly cooled at a predetermined cooling rate. However, even if the desired softening of the steel material can be achieved with such conventional temperature control of spheroidizing annealing, there is still room for improvement in the state of the metal structure, for example, traces of bainite remaining in the metal structure are observed.

[0007] In the past, in order to improve the metal structure of the steel after spheroidizing annealing, an additional heat treatment process such as low temperature annealing (LA) was sometimes performed, but such an additional process increases the manufacturing cost of the tool steel.

[0008] An object of the present invention is to provide a manufacturing method that can obtain tool steel that is appropriately softened and has a good metal structure without performing any additional steps by performing spheroidizing annealing in a manner different from the conventional method. [Means for solving the problem]

[0009] The inventors of the present invention have conducted extensive research into spheroidizing annealing and have discovered a method of spheroidizing annealing that is different from conventional methods and that can achieve the desired softening of steel and improve the state of the metal structure of the steel. The present invention can be realized, for example, in the following forms.

[0010] [First aspect] The first aspect is provided as a method for producing a tool steel. The first embodiment of the manufacturing method includes the steps of preparing a steel material having a chemical composition containing, in mass%, C: 0.25% or more and 1.50% or less, Si: 0.10% or more and 1.50% or less, Mn: 0.20% or more and 1.50% or less, P: 0.050% or less, S: 0.050% or less, Cu: 0.30% or less, Ni: 0.30% or less, Cr: 4.00% or more and 9.00% or less, Mo: 0.50% or more and 3.00% or less, and V: 0.15% or more and 1.50% or less, with the balance being Fe and unavoidable impurities, and performing spheroidizing annealing on the steel material by performing a heat treatment at a first temperature higher than the Ac3 point of the steel material, a cooling treatment to reduce the temperature from the first temperature to a second temperature lower than the A1 point of the steel material, and a isothermal holding treatment to hold the steel material at the second temperature for a predetermined time.

[0011] [Second aspect] In the method for producing a tool steel according to the first aspect, the first temperature may be 870°C or higher and 920°C or lower.

[0012] [Third Feature] In the method for producing a tool steel according to the first or second feature, the second temperature may be 680°C or higher and 780°C or lower.

[0013] [Fourth feature] In the method for producing a tool steel according to the first, second or third feature, the difference between the A1 point of the steel material and the second temperature may be 30°C or more and 140°C or less.

[0014] [Fifth feature] In the method for producing a tool steel according to any one of the first, second, third or fourth features, the second temperature is a temperature within a range of a predetermined reference temperature ±20°C, and the reference temperature may be an approximation of a temperature at which the isothermal transformation of the steel can be completed in the shortest time.

[0015] [Sixth Feature] In the method for producing a tool steel according to the fifth feature, the reference temperature may be set to a value of A1 point of the steel material -70°C. Effect of the Invention

[0016] According to the present invention, by carrying out spheroidizing annealing with a temperature control different from that of the conventional method, it is possible to obtain a tool steel having a good metal structure in which the steel is appropriately softened, the carbides are appropriately spheroidized, and the ferrite (α structure) of the parent phase is refined. According to the present invention, it is possible to omit the implementation of an additional process for improving the state of the metal structure of the steel during or after spheroidizing annealing.

[0017] The present invention can be realized in various forms other than the method for manufacturing tool steel. For example, the present invention can be realized in the form of an apparatus for manufacturing tool steel, a method for spheroidizing annealing, an apparatus for performing spheroidizing annealing, etc. Furthermore, the present invention can also be realized in the form of a tool steel, or a tool, instrument, machine, device, etc. manufactured using the tool steel. [Brief description of the drawings]

[0018] [Figure 1] FIG. 4 is an explanatory diagram for explaining temperature control of spheroidizing annealing according to the embodiment. [Diagram 2] FIG. 4 is an explanatory diagram for explaining how to determine the minimum isothermal transformation completion temperature. [Diagram 3] FIG. 4 is an explanatory diagram for explaining temperature control of spheroidizing annealing in a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the method for producing tool steel according to the present invention will be described.

[0020] 1.First step: In the first step, a steel material having the following chemical composition is prepared. The steel material prepared in the first step has a chemical composition containing at least carbon (C), silicon (Si), manganese (Mn), phosphorus (P), sulfur (S), copper (Cu), nickel (Ni), chromium (Cr), molybdenum (Mo), and vanadium (V), with the balance being iron (Fe) and unavoidable impurities. In the first step, the steel material is prepared in a state in which it has been formed into a shape such as an ingot after being subjected to hot working such as hot forging.

[0021] 1-1. Chemical composition of steel: The preferred range of the content of each of the above chemical components and the reasons for limiting the range are described in detail below. In the following description, unless otherwise specified, the content is the mass content, and "%" means "mass%".

[0022] C: 0.25% or more and 1.50% or less C is an element effective for ensuring the strength, wear resistance, and hardness required for tool steel. C combines with carbide-forming elements such as Cr, Mo, and V to form carbides. By containing 0.25% or more of C, the strength generally required for tool steel can be obtained. It is more preferable that C is contained at 0.30% or more. This makes it possible to obtain a tool steel with higher strength. However, if the C content exceeds 1.50%, it may cause coarse carbides to remain or may cause the hot workability of the steel to decrease. Therefore, the C content in this embodiment is set to 1.50% or less. In order to suppress the above-mentioned problems, it is more preferable that the C content is 1.10% or less.

[0023] Si: 0.10% or more and 1.50% or less Si is an element effective in promoting the precipitation of carbides and promoting the secondary hardening of steel material. By including 0.10% or more of Si, the precipitation of carbides can be further promoted. The Si content is more preferably 0.13% or more. However, if the Si content exceeds 1.50%, the hardenability may decrease. Therefore, the Si content in the steel material of this embodiment is set to 1.50% or less. From the viewpoint of suppressing the decrease in hardenability, the Si content is more preferably 1.30% or less.

[0024] Mn: 0.20% or more and 1.50% or less Mn is an element effective in improving hardenability. In order to obtain high hardenability of the steel material, the Mn content is set to 0.20% or more. In order to improve the hardenability of the steel material, the Mn content is more preferably 0.23% or more. However, if the Mn content exceeds 1.50%, there is a possibility that the hot workability may be deteriorated. Therefore, the Mn content in the steel material of this embodiment is set to 1.50% or less. In order to suppress the deterioration of the hot workability, the Mn content is more preferably 1.30% or less.

[0025] P:0.050% or less P is an inevitable impurity that can cause embrittlement due to grain boundary segregation and reduce the toughness of the steel material. Therefore, the upper limit of the P content in this embodiment is set to 0.050% or less. The upper limit of the P content is more preferably 0.040% or less.

[0026] S: 0.050% or less S is an unavoidable impurity, but may be added intentionally to improve the machinability of tool steel. However, if S is contained in excess, it may cause a decrease in hot workability, so the upper limit of the S content in this embodiment is set to 0.050% or less. It is more preferable that the upper limit of the S content is 0.040% or less.

[0027] Cu:0.30% or less Cu is an element effective for stabilizing austenite. However, if Cu is contained excessively, the hot workability of the steel material may be deteriorated, so the upper limit of the Cu content in this embodiment is set to 0.30% or less. In order to ensure the hot workability, the Cu content is more preferably 0.28% or less.

[0028] Ni: 0.30% or less Ni, like Cu, is an element effective in stabilizing austenite. However, if Ni is contained in excess, there is a possibility that the softening of the steel material by spheroidizing annealing may be hindered, so the upper limit of the Ni content in this embodiment is set to 0.30% or less. The upper limit of the Ni content is more preferably 0.28% or less.

[0029] Cr:4.00% or more and 9.00% or less Cr is an element that contributes to improving the strength of tool steel by forming carbides, and is also an element that is effective in improving the hardenability of steel. In order to improve the strength of tool steel and the hardenability of steel, the Cr content is set to 4.00% or more. It is more preferable that the Cr content is 4.50% or more. However, excessive Cr content may reduce the hardness of the tool steel. Therefore, the Cr content in this embodiment is set to 9.00% or less. It is more preferable that the upper limit of the Cr content is 8.80% or less.

[0030] Mo: 0.50% or more and 3.00% or less Like Cr, Mo is an element that is effective in improving hardenability, and contributes to improving the strength of tool steel by forming carbides. In order to improve hardenability and the strength of tool steel, the Mo content is set to 0.50% or more. It is more preferable that the Mo content is 0.80% or more. However, if Mo is contained in excess, there is a possibility that the softening of the steel material is inhibited. Therefore, the Mo content in this embodiment is set to 3.00% or less. It is more preferable that the Mo content is 2.80% or less.

[0031] V: 0.15% or more and 1.50% or less Like Cr and Mo, V is an element that contributes to improving the strength of tool steel by forming carbides, and is also an element that is effective in preventing grain growth during quenching. In order to ensure the strength of the tool steel and the hardenability of the steel material, the V content in this embodiment is set to 0.15% or more. It is more preferable that the V content is 0.18% or more. However, if V is contained in excess, coarse carbonitrides are formed, which may reduce the brittleness and toughness of the tool steel. Therefore, the V content in this embodiment is set to 1.50% or less. It is more preferable that the upper limit of the V content is 1.20% or less.

[0032] 2.Second process: Fig. 1 is an explanatory diagram showing an example of temperature control of the steel material in the spheroidizing annealing in the second step. In the second step, the steel material prepared in the above-mentioned first step is subjected to spheroidizing annealing. In the spheroidizing annealing of this embodiment, a four-stage temperature control process of steps S1 to S4 shown in Fig. 1 is performed.

[0033] In step S1, a heat treatment is performed. In the heat treatment, the steel material is heated to a first temperature Th higher than the Ac3 point. The Ac3 point may be, for example, an actual measurement value obtained by a Formaster test. In step S1, the heating time during which heating is continued at the first temperature Th may be, for example, about 3 to 8 hours.

[0034] Through repeated research, the inventors of the present invention have found that the first temperature Th, which corresponds to the heating temperature in the heat treatment, is important for creating a metal structure in the spheroidizing annealing, and have discovered that by setting the first temperature Th to a temperature higher than the Ac3 point, the transformation from bainite to austenite during the heat treatment is promoted, and the tempering of austenite to bainite after the heat treatment can be suppressed.

[0035] In the heat treatment of step S1, if the first temperature Th is set to a temperature higher than the Ac3 point of the steel, it is possible to reduce bainite in the metal structure of the steel after spheroidizing annealing, and to promote the refinement of the α structure, which is the parent phase.

[0036] The first temperature Th is preferably at least 10°C higher than the Ac3 point, and more preferably at least 30°C higher. In general, the Ac3 point is about 850 to 900°C. Therefore, the first temperature Th is preferably at least 870°C. If the first temperature Th is set to a value of 870°C or higher, it is possible to further reduce bainite in the metal structure of the steel material after spheroidizing annealing, and it is possible to further promote the refinement of the α structure.

[0037] The first temperature Th is preferably 920° C. or less. If the first temperature Th is higher than 920° C., the amount of carbon dissolved in solid solution increases, which may take a long time for carbon to diffuse during the cooling stage, resulting in insufficient softening. Also, the crystal grains in the metal structure of the steel material after spheroidizing annealing may become excessively coarse.

[0038] Step S2 is a cooling treatment. In the cooling treatment, the steel material is cooled in a furnace from a first temperature Th to a second temperature Tc lower than the A1 point of the steel material. The A1 point here may be a value determined by, for example, regression calculation. The cooling rate in the cooling treatment may be, for example, 10 to 50°C / hour. The cooling rate is not particularly limited because it has little effect on the finish of spheroidizing annealing.

[0039] Step S3 is a constant temperature holding process. In the constant temperature holding process, the steel material is held at a second temperature Tc for a predetermined time t hold During this isothermal treatment, carbides grow into spheroids in the metal structure of the steel, and the transformation of austenite to an α structure progresses. Therefore, in order to soften the steel and create a metal structure by spheroidizing annealing, the treatment conditions of the isothermal treatment, along with the first temperature Th of the heat treatment described above, are important.

[0040] Hereinafter, in step S3, the time for which the steel material is held at the second temperature Tc is referred to as the “constant temperature holding time t hold It is also called "constant temperature holding time t hold The isothermal holding time t may be appropriately determined within a range of, for example, 5 hours to 20 hours depending on the chemical composition and dimensions of the steel material.hold The lower limit of the constant temperature holding time t is more preferably 10 hours or more. hold It is more preferable that the upper limit is 18 hours or less.

[0041] In various steel types, in order to enhance the softening effect by spheroidizing annealing and to make the metal structure after spheroidizing annealing in an appropriate state, the second temperature Th is preferably in the range of approximately 680° C. or more and 780° C. or less. As shown in the examples described later, the second temperature Th is more preferably 700° C. or more and 760° C. or less.

[0042] In order to promote the transformation from austenite to an α structure in the isothermal holding treatment, the second temperature Th is preferably at least 30°C lower than the A1 point of the steel material. It is more preferable that the difference between the A1 point and the second temperature Th is at least 40°C. If the difference between the A1 point and the second temperature Th is at least 40°C, it is possible to further suppress austenite from remaining in the metal structure of the steel material after spheroidizing annealing. Therefore, it is possible to achieve the desired softening of the steel material.

[0043] The difference between the A1 point and the second temperature Th is preferably 140°C or less, and more preferably 100°C or less. If the difference between the A1 point and the second temperature Th is 140°C or less, an ideal metal structure state can be easily obtained. If the difference between the A1 point and the second temperature Th is 100°C or less, austenite is transformed into martensite during cooling of the steel material after the heat treatment in step S1, and the steel material is prevented from becoming hard. In addition, it is possible to prevent the spherical carbides from growing sufficiently during the constant temperature holding treatment, and the steel material from becoming insufficiently soft.

[0044] The inventors of the present invention have found that by setting the second temperature Th to a value within the range of a predetermined reference temperature Ts ±20°C, the metal structure of the steel material can be made into a more suitable state. Hereinafter, the "reference temperature Ts" is an approximation of the temperature at which the isothermal transformation of the steel material can be completed in the shortest time. Hereinafter, the "temperature at which the isothermal transformation of the steel material can be completed in the shortest time" will also be referred to as the "shortest isothermal transformation completion temperature". The shortest isothermal transformation completion temperature can be experimentally determined by the method described below. As described below, according to the inventors, the shortest isothermal transformation completion temperature is an approximation of the value of A1 point -70°C.

[0045] Step S4 is a quenching treatment. In the quenching treatment, the steel material is cooled from the second temperature Th. The treatment conditions of the quenching treatment are not particularly limited. In the quenching treatment of this embodiment, the steel material is carried out from the furnace and cooled by air cooling.

[0046] By carrying out the above-mentioned steps S1 to S4, the spheroidal annealing of the second step is completed. According to the spheroidal annealing of this embodiment, it is possible to obtain a suitable metal structure in which spheroidized carbides are appropriately present in the steel material, the mother phase is a fine α structure, and the presence of bainite and martensite is suppressed, and the steel material can be appropriately softened.

[0047] 3. How to determine the minimum completion temperature of isothermal transformation: Fig. 2 is an explanatory diagram for explaining an example of a method for experimentally determining the above-mentioned minimum isothermal transformation completion temperature. In this method, a spheroidizing annealing test is performed in which a steel material is heated at various heating temperatures and then slowly cooled, and the minimum isothermal transformation completion temperature is determined based on the temperature at which the spheroidizing annealing test is completed and the cooling time determined for each heating temperature.

[0048] Fig. 2(a) shows an example of a graph showing a temperature control pattern in a spheroidizing annealing test for determining the minimum isothermal transformation completion temperature. In this spheroidizing annealing test, a steel material is heated at a heating temperature higher than the A3 point for a predetermined time, and then cooled at a predetermined cooling rate by furnace cooling to a spheroidizing annealing completion temperature (hereinafter referred to as "SA completion temperature"). After reaching the SA completion temperature, the steel material is rapidly cooled by air cooling. The SA completion temperature is the temperature at which the transformation of austenite to an α structure is completed and softening of the steel material can be confirmed.

[0049] When determining the reference temperature Ts, the above spheroidizing annealing test is performed at various heating temperatures Tt1, Tt2, …, Tt n The subscript n is an arbitrary natural number. The heating temperatures Tt1, Tt2, ..., Tt n For each SA completion temperature Tf1, Tf2, …, Tt n and cooling times t1, t2, …, t n Calculate the cooling time t1, t2, …, t n After the heat treatment is completed, the SA completion temperatures Tf1, Tf2, …, Tf n corresponds to the time it takes to reach

[0050] Figure 2(b) shows the SA completion temperatures Tf1, Tf2, ..., Tf n and cooling times t1, t2, …, t n An example of a graph plotting SA completion temperatures Tf1, Tf2, ..., Tf3 is shown. In this graph, the vertical axis is temperature, and the horizontal axis is time, which is shown on a logarithmic scale. The subscript m in the graph in FIG. 2(b) is an arbitrary natural number. SA completion temperatures Tf1, Tf2, ..., Tf4 are n and cooling times t1, t2, …, t n By performing a TTT conversion on the graph plotting and, the minimum completion temperature of isothermal transformation can be obtained, as described below.

[0051] FIG. 2(c) shows an example of a graph obtained by converting the graph in FIG. 2(b) into a TTT graph. In the graph in FIG. 2(c), the minimum time t minThe temperature Tm for this represents the minimum completion temperature Tm of the isothermal transformation.

[0052] As described above, the metal structure of the steel material can be improved by determining the reference temperature Ts as an approximation of the minimum isothermal transformation completion temperature Tm and setting the second temperature Tc to a value within the range of the reference temperature Ts ±20° C. The approximation of the minimum isothermal transformation completion temperature Tm may be set to a value within the range of the minimum isothermal transformation completion temperature Tm ±3%, for example.

[0053] The inventors of the present invention have found through experiments that the minimum completion temperature of isothermal transformation Tm is an approximate value of A1 point -70° C. for all steel materials. If the reference temperature Ts is set to a value of A1 point -70° C., it is possible to easily determine the second temperature Tc of the isothermal holding treatment that can more effectively improve the metal structure of the steel material after spheroidizing annealing.

[0054] 4. Comparative Example of Spheroidizing Annealing: Temperature control of spheroidizing annealing as a comparative example to the spheroidizing annealing of the above-mentioned embodiment will be described with reference to Fig. 3. The spheroidizing annealing of the comparative example corresponds to that generally performed in the conventional manufacturing of tool steels.

[0055] In the spheroidizing annealing of the comparative example, the steel material is first heated for a predetermined time at a heating temperature Ta lower than the Ac3 point of the steel material in the heat treatment of step S1a. Then, the steel material is cooled at a predetermined cooling rate from the heating temperature Ta to a cooling temperature Tb by furnace cooling in the slow cooling treatment of step S2a. The cooling temperature Tb is a temperature just below the Ac1 point of the steel material. The cooling rate in step S2a may be, for example, about 15°C / hour. The steel material is cooled by air cooling in the rapid cooling treatment of step S3a. After step S3a, if the softening of the steel material is not sufficient, a quenching treatment of step S4a is performed.

[0056] In the spheroidizing annealing of the comparative example, in many cases, when the cooling treatment of step S2a is completed, the metal structure of the steel material is in a state in which α structure and γ structure (austenite) are mixed. The γ structure is likely to become martensite in the rapid cooling treatment of step S3a, which causes the softening of the steel material to be hindered. In addition, in the spheroidizing annealing of the comparative example, since the heating temperature Ta is lower than the Ac3 point, there is a possibility that bainite will remain in the metal structure of the steel material.

[0057] 5. Summary of embodiments: As described above, according to the manufacturing method of the tool steel of this embodiment, spheroidizing annealing is performed with a temperature control different from that of conventional spheroidizing annealing. According to the spheroidizing annealing of this embodiment, the steel is heated to a first temperature Th higher than the Ac3 point in the heat treatment, and then held at a second temperature Tc lower than the A1 point for a constant temperature holding time. This temperature control can reduce bainite in the metal structure of the steel, and can promote refinement of the α structure, which is the parent phase. In addition, it can promote spheroidization of carbides. Therefore, it is possible to obtain a metal structure in a better state than the spheroidizing annealing of the above comparative example, and the steel can be suitably softened. Therefore, it is possible to obtain a tool steel with improved mechanical properties and processing characteristics. EXAMPLES

[0058] Next, an embodiment of the method for producing tool steel according to the present invention will be described.

[0059] A. Chemical composition of steel: In this example, three steel types SA, SB, and SC shown in Table 1 below were prepared as steel materials used in the manufacturing method of tool steel according to the present invention.

[0060] [Table 1]

[0061] The lower and upper limits of the content of each element contained in each of the steel types SA, SB, and SC are shown in mass% in Table 1. Although not shown in Table 1, the chemical composition of each of the steel types SA, SB, and SC is the remainder Fe and unavoidable impurities.

[0062] Steel grades SA and SB are hot work tool steels, and steel grade SA is cold work die steel. Steel grade SA is a secondary melted material produced through primary and secondary melting. Steel grades SB and SC are primary melted materials produced through primary melting.

[0063] B. Steel transformation point, reference temperature, and minimum completion temperature of isothermal transformation: Table 2 below summarizes the A3 point, Ac3 point, A1 point, reference temperature Ts, and isothermal transformation completion temperature Tm for each of the steel types SA, SB, and SC.

[0064] [Table 2]

[0065] In Table 2, points A1 and A3 are values ​​calculated by regression calculation. Point Ac3 is an actual measured value obtained by a Formaster test. The isothermal transformation completion temperature Tm is a value experimentally obtained by the method explained in Figure 2. The reference temperature Ts in Table 2 is set to a value 70°C lower than point A1. For all steel types SA, SB, and SC, the reference temperature Ts is an approximation within the range of ±3% of the isothermal transformation completion temperature Tm.

[0066] C. Evaluation of the effect of the first temperature of heat treatment: Table 3 below summarizes the evaluation results of the steel materials after spheroidizing annealing when the first temperature Th in the heat treatment was 870°C, 900°C, and 920°C and the treatment conditions for the constant temperature holding treatment were the same.

[0067] [Table 3]

[0068] In the manufacturing examples E1, E2, and E3, the steel type SA was used as the steel material, in the manufacturing examples E4, E5, and E6, the steel type SB was used as the steel material, and in the manufacturing examples E7, E8, and E9, the steel type SC was used as the steel material. For the steel types SA and SB, two types of steel materials, "coarse grain" and "ultra-coarse grain", which have different crystal grain sizes in the metal structure of the steel material before spheroidal annealing, were prepared and evaluated. That is, for example, in the manufacturing example E1, two types of steel materials, the "coarse grain" steel material of the steel type SA and the "ultra-coarse grain" steel material of the steel type SA, were each subjected to spheroidal annealing at a first temperature Th of 870°C and evaluated. The "coarse grain" steel material was observed with a digital microscope and had an average grain size of 200 μm measured visually. The "ultra-coarse grain" steel material was observed with a digital microscope and had an average grain size of 2000 μm measured visually. For steel type SC, only the coarse grain steel was evaluated.

[0069] In each of the manufacturing examples E1 to E9, the heating time in the heat treatment was 4 hours. The second temperature Th in the constant temperature holding treatment was 720° C., and the constant temperature holding time T hold The second temperature Th of 720° C. is lower than the A1 point of any of the steel types SA, SB, and SC shown in Table 2 by 30° C. or more.

[0070] The "Evaluation Results" in Table 3 are the results of observing the metal structure of the steel after spheroidizing annealing under a 400x microscope, and evaluating it according to the following guidelines: "○" in the evaluation results indicates that defects were observed in less than 30% of the observed field of view, "△" indicates that defects were observed in 30% to less than 50% of the observed field of view, and "×" indicates that defects were observed in 50% or more of the observed field of view.

[0071] In Production Example E1, where the heating temperature was lower than the Ac3 point, a large amount of bainite was present in a range of 50% or more of the observation field for both the "coarse grains" and the "ultra-coarse grains," and the evaluation result was "X." In Production Example E1, it is presumed that because the first temperature Th in the heat treatment was lower than the Ac3 point, a large amount of bainite was tempered from austenite after the heat treatment.

[0072] In Production Example E2, the heating temperature was 10°C higher than the Ac3 point, but the evaluation results for both "coarse grains" and "ultra-coarse grains" were "△". In Production Example E2, the presence of bainite was confirmed in an area between 30% and 50% of the observation field. However, in Production Example E2, the α structure, which is the parent phase, was sufficiently refined. It is presumed that the bainite observed in Production Example E2 was retained without transforming into austenite during heat treatment.

[0073] The first temperature Th of the other manufacturing examples E3 to E9 was 870°C or higher and 920°C or lower, all of which were higher than the Ac3 point. The evaluation results of manufacturing examples E3 to E9 were all "○". In all of manufacturing examples E3 to E9, the presence of bainite was confirmed only in less than 30% of the observation field, the α structure was sufficiently refined, and the carbides were appropriately granulated. From these results, it can be seen that the first temperature Th is preferably 870°C or higher and 920°C or lower.

[0074] From the above, it was found that the state of the metal structure can be improved by combining a heat treatment in which the first temperature Th is higher than the Ac3 point with a constant temperature treatment. The evaluation results of the manufacturing examples E3, E5, E6, E8, and E9 in which the first temperature Th is 30°C or more higher than the Ac3 point were all "○". From this, it can be said that it is more preferable that the first temperature Th is 30°C or more higher than the Ac3 point.

[0075] D. The effect of the second temperature on the isothermal treatment: Table 4 below summarizes the evaluation results of steel materials after spheroidizing annealing when the heat treatment conditions were the same and the second temperature Tc in the isothermal holding treatment was 780°C, 760°C, 740°C, 720°C, 700°C, and 680°C.

[0076] [Table 4]

[0077] In manufacturing examples E10, E11, E12, E13, E14, and E15, steel type SA was used as the steel material. In manufacturing examples E16, E17, E18, E19, E20, and E21, steel type SB was used as the steel material. In manufacturing examples E22, E23, E24, E25, E26, and E27, steel type SC was used as the steel material. "Coarse grain" and "ultra-coarse grain" in Table 4 refer to two types of steel with different crystal grain sizes in the metal structure before spheroidizing annealing, as explained in Table 3.

[0078] In the heat treatment, the first temperature Th was set to 900°C and the heating time was set to 4 hours for all of the Production Examples E10 to E27. The first temperature Th of 900°C was higher than the Ac3 point of all of the steel types SA, SB, and SC, as shown in Table 2. The constant temperature holding time of the constant temperature holding treatment was set to 5 hours for all of the Production Examples E10 to E27.

[0079] The second temperature Tc of each of the manufacturing examples E10 to E27 was lower than the A1 point. In each of the manufacturing examples E10 to E27, the softening required for spheroidizing annealing was achieved, and an appropriate state was obtained for the metal structure. This shows that by performing heat treatment at the first temperature Th, which is higher than the Ac3 point, and then performing spheroidizing annealing by isothermal holding treatment at the second temperature Tc, which is lower than the A1 point, it is possible to easily soften the steel appropriately and improve the metal structure of the steel.

[0080] Moreover, the second temperature Tc of all of Production Examples E10 to E27 was not less than 680° C. and not more than 780° C. This shows that the second temperature Tc is preferably not less than 680° C. and not more than 780° C.

[0081] The "Evaluation Results" in Table 4 are based on the measurement results of the Brinell hardness of the steel material after spheroidizing annealing. Evaluation result "A" indicates that the measured Brinell hardness was 220HB or less, "B" indicates that the measured Brinell hardness was greater than 220HB and less than 250HB, and "C" indicates that the measured Brinell hardness was 250HB or more. Below, more suitable temperature conditions for the constant temperature treatment will be explained based on these evaluation results.

[0082] All of the manufacturing examples E11, E12, E13, E14, E17, E18, E19, E20, E23, E24, E25, and E26, in which the second temperature Tc was 700° C. or more and 760° C. or less, were evaluated as “A.” This shows that it is more preferable for the second temperature Tc to be 700° C. or more and 760° C. or less.

[0083] The evaluation result for "coarse grains" of Manufacturing Example E15 was "C", and the evaluation result for "ultra-coarse grains" was "B". In Manufacturing Example E15, more martensite was observed in the metal structure than in the other Manufacturing Examples E10 to E14 and E16 to E27, and it is believed that this martensite is the cause of the higher Brinell hardness than the others. The reason why there was a relatively large amount of martensite in the metal structure of Manufacturing Example E15 is believed to be that in Manufacturing Example E15, the decrease in the second temperature Tc from point A1 was the largest at 145°C, making it easier for austenite to become martensite during isothermal treatment.

[0084] The evaluation results for Production Example E16 were "C" for both "coarse grains" and "ultra-coarse grains". In the metal structure of Production Example E16, many structures were observed that did not transform into α structure and remained as austenite. It is believed that the presence of this austenite was the cause of the inhibition of softening of the steel. Also, in Production Example E16, the second temperature Tc was relatively high compared to point A1, and the difference between point A1 and second temperature Tc was the smallest at 13°C, so it is presumed that the transformation from austenite to α structure did not progress sufficiently during the isothermal treatment.

[0085] The results of the above manufacturing examples E15 and E16 show that better results of spherical annealing can be obtained by appropriately setting the second temperature Tc within a range in which the difference from point A1 is not too small and not too large.

[0086] In Production Examples E10 to E14, and E17 to E27, the difference between the second temperature Tc and the A1 point was 30° C. or more and 140° C. or less, and all of them were evaluated as “A” or “B.” This shows that it is more preferable that the difference between the A1 point and the second temperature Tc is 30° C. or more and 140° C. or less.

[0087] Moreover, the evaluation results of the manufacturing examples E10, E11, E12, E18, E19, E20, E23, E24, and E25, in which the difference between the A1 point and the second temperature Tc was 40° C. or more and 100° C. or less, were all "A." From this, it can be seen that it is even more preferable that the difference between the A1 point and the second temperature Tc is 40° C. or more and 100° C. or less.

[0088] The reference temperature Ts in Table 4 is 70°C lower than point A1. In manufacturing examples E10, E11, E12, E18, E19, E20, E23, and E24, the second temperature Tc was within the range of the reference temperature Ts ±20°C. The evaluation results for manufacturing examples E10, E11, E12, E18, E19, E20, E23, and E24 were all "A". From this, it can be seen that in order to achieve the desired softening of the steel material and improve the state of the metal structure, it is even more preferable to set the second temperature Tc to a value within the range of the reference temperature Ts ±20°C.

[0089] E. Summary: From the above results, it is clear that the spheroidizing annealing carried out in the method for producing tool steel according to the present invention makes it possible to achieve the desired softening of the steel material and improve the state of the metal structure of the steel material. Therefore, the method for producing tool steel according to the present invention makes it possible to obtain tool steel that is appropriately softened, has a good metal structure, and is excellent in mechanical properties and processing characteristics.

[0090] The present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible within the scope of the present invention. For example, it is possible to omit some of the elements that are not essential, add elements other than those mentioned above to the extent that they do not significantly affect the main elements, and change some of the manufacturing conditions that are not essential. [Explanation of symbols]

[0091] S1...heat treatment, S2...cooling treatment, S3...constant temperature maintenance treatment, S4...quenching treatment, Th...first temperature, Tc...second temperature, Tm...shortest completion temperature of isothermal transformation, Ts...standard temperature, t hold …Constant temperature holding time

Claims

1. In mass percent, C: 0.25% or more and 1.50% or less, Si: 0.10% or more and 1.50% or less, Mn: 0.20% or more and 1.50% or less, P: 0.050% or less, S: 0.050% or less, Cu: 0.30% or less, Ni: 0.30% or less, Cr: 4.00% or more and 9.00% or less, Mo: 0.50% or more and 3.00% or less, and V: 0.15% or more and 1.50% or less, and the balance being Fe and unavoidable impurities; For the steel material, the Ac of the steel material 3 a heat treatment for heating the steel material at a first temperature higher than the A point; 1 a step of performing a spheroidizing annealing process by performing a cooling process to reduce the temperature to a second temperature lower than the temperature point and a constant temperature holding process to hold the second temperature for a predetermined time; A method for producing a tool steel comprising the steps of:

2. The method of claim 1 , wherein the first temperature is greater than or equal to 870° C. and less than or equal to 920° C.

3. The method of claim 2 , wherein the second temperature is greater than or equal to 680° C. and less than or equal to 780° C.

4. The above steel material A 1 3. The method for producing tool steel according to claim 1, wherein a difference between the point and the second temperature is 30°C or more and 140°C or less.

5. The second temperature is a temperature within a range of a predetermined reference temperature ±20° C., 3. The method of manufacturing a tool steel according to claim 1, wherein the reference temperature is an approximation of a temperature at which the isothermal transformation of the steel material can be completed in the shortest time.

6. The reference temperature is the A 1 The method for producing a tool steel according to claim 5, wherein the temperature is −70° C.

Citation Information

Patent Citations

  • Method for spheroidize-annealing steel material

    JP1998298640A

  • Die steel superior in spheroidizing annealing property and hardenability

    JP2008121032A