Metal oxide nanoparticles dispersible in non-polar solvent, electron transfer layer ink composition for inkjet printing containing the same and method for producing the same and light emitting device and display containing the same

JP2024154428AActive Publication Date: 2024-10-30SAMSUNG ELECTRONICS CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024067545
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-18
Publication Date
2024-10-30
Estimated Expiration
2044-04-18

AI Technical Summary

Benefits of technology

【0036】 本発明の実施形態によれば、金属酸化物ナノ粒子の表面改質を通じて2種の非極性溶剤に混合することができ、インクジェット法による均一な吐出が容易である。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154428000001_ABST
    Figure 2024154428000001_ABST
Patent Text Reader

Abstract

To provide metal oxide nanoparticles dispersible in a non-polar solvent, an electron transport layer ink composition for inkjet printing containing the same and a method for producing the same, and a light emitting device and a display containing the same.SOLUTION: There are provided metal oxide nanoparticles, an electron transport layer ink composition for inkjet printing containing the same and a method for producing the same and a light emitting device and a display containing the same, specifically, metal oxide nanoparticles which can be dispersed in a non-polar solvent and can prevent etching of a polar solvent type light emitting layer, an electron transport layer ink composition for inkjet printing containing the same and a method for producing the same and a light emitting device and a display containing the same.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to metal oxide nanoparticles, an ink composition for an electron transport layer for inkjet printing including the same and a method for preparing the same, and a light emitting device and a display including the same. More specifically, the present invention relates to metal oxide nanoparticles that are dispersible in a non-polar solvent and can prevent a light emitting layer of a polar solvent type from being etched, an ink composition for an electron transport layer for inkjet printing including the same and a method for preparing the same, and a light emitting device and a display including the same. [Background technology]

[0002] Quantum dots (QDs) are so-called semiconductor nanocrystals, and can produce various colors by generating light of different wavelengths according to particle size without changing the type of material. They have advantages of higher color purity and light stability than existing light-emitting bodies, so they are attracting attention as a next-generation light-emitting device.

[0003] In particular, quantum dots, which have become a new trend in the display field, are dispersed in a polymer matrix and can be applied in the form of a complex to various displays and electronic devices in addition to TVs and LEDs. Meanwhile, materials for color filters are required to have high sensitivity, adhesion to substrates, chemical resistance, heat resistance, etc. Conventionally, color filters applied to displays have generally been formed through a patterning process in which a desired pattern is formed using a photosensitive resist composition through an exposure process using a photomask, and then the non-exposed areas are dissolved and removed through a development process, but this has led to a problem of increased costs due to the waste of materials.

[0004] Recently, in order to solve the problem of increasing the quality of materials used for pixels and the associated cost increases, methods that use materials only in desired areas and minimize the use of materials have been attracting attention, rather than the conventional patterning methods such as spin coating or slit coating. The most representative method is the inkjet method, which can be broadly classified into the bubble jet method and the piezo method. The inkjet method uses materials only in desired pixels, thereby preventing unnecessary waste of materials.

[0005] Thus, although there has been much research on quantum dot solutions for inkjet printing, there has been little research on electron transport layer (ETL) compositions for inkjet printing. A prior invention relating to an electron transport layer (ETL) composition for inkjet printing is disclosed in Korean Patent Publication No. 10-2007-0078615 (August 1, 2007). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Korean Patent Publication No. 10-2007-0078615 Summary of the Invention [Problem to be solved by the invention]

[0007] Currently, the type of solvent for the quantum dot emitting layer used in the self-luminous display for inkjet printing is unclear, and various types of solvents are being researched and developed, but when a polar solvent type emitting layer is used, there is a technical problem that the emitting layer is etched if a polar solvent type electron transport layer ink composition having the same properties is used. Therefore, there is a demand for metal oxide nanoparticles and electron transport layer (ETL) compositions that can be dispersed in non-polar solvents.

[0008] The problem to be solved by the present invention is to provide metal oxide nanoparticles and an electron transport layer ink composition that can be dispersed in a non-polar solvent by modifying the surface of hydrophilic metal oxide nanoparticles when a polar solvent type light emitting layer is used, and that can be easily inkjet printed because the viscosity is easily adjusted. [Means for solving the problem]

[0009] According to one aspect of the present invention for solving the above-mentioned problems, there is provided a metal oxide nanoparticle, The metal oxide nanoparticles are surface-modified; Metal oxide nanoparticles for inkjet printing are provided that are dispersible in non-polar solvents.

[0010] Preferably, the surface of the metal oxide nanoparticles is modified with organic ligands having hydrophobic moieties to provide metal oxide nanoparticles for inkjet printing.

[0011] Preferably, the non-polar solvent is a mixture of at least two solvents to provide metal oxide nanoparticles for inkjet printing.

[0012] Preferably, the non-polar solvent comprises cyclohexylbenzene to provide metal oxide nanoparticles for inkjet printing.

[0013] Preferably, the organic ligand is contained in an amount of 0.0001 to 10 mol per 1 mol of the metal contained in the metal oxide nanoparticles, thereby providing metal oxide nanoparticles for inkjet printing.

[0014] Preferably, the metal oxide nanoparticles are zinc (Zn)-containing metal oxide nanoparticles for inkjet printing.

[0015] Preferably, the zinc (Zn)-containing metal oxide nanoparticles are alloyed with a metal that can increase the band gap of zinc oxide (ZnO) to provide metal oxide nanoparticles for inkjet printing.

[0016] Preferably, the zinc (Zn)-containing metal oxide nanoparticles are zinc magnesium oxide (ZnMgO), to provide metal oxide nanoparticles for inkjet printing.

[0017] In another aspect of the invention, a metal oxide nanoparticle surface-modified with an organic ligand; a non-polar solvent, Electron transport layer ink compositions for ink jet printing are provided that are jettable by ink jet.

[0018] Preferably, the non-polar solvent is a mixture of at least two solvents.

[0019] Preferably, the non-polar solvent comprises cyclohexylbenzene.

[0020] Preferably, the non-polar solvent further comprises one or more solvents selected from the group consisting of styrene, hexadecane, anisole, and cyclohexanone.

[0021] Preferably, the mixed non-polar solvent comprises: The viscosity at 20°C is 1 to 6 cps, The vapor pressure at 20°C is 0.001 to 0.1 mmHg. An electron transport layer ink composition for ink jet printing is provided, which has a surface tension of 30 to 40 dyn / cm at 20°C.

[0022] Preferably, the volume ratio of cyclohexylbenzene to other solvents is from 7:3 to 20:1 in the electron transport layer ink composition for inkjet printing.

[0023] Preferably, the composition comprises: The viscosity at 20°C is 1.0 to 5.0 cps, The vapor pressure at 20°C is 0.6 to 45 mmHg. An electron transport layer ink composition for ink jet printing is provided having a solids content of 5 to 30 weight percent.

[0024] Preferably, the organic ligand is an organic ligand having a hydrophobic moiety.

[0025] Preferably, the metal oxide nanoparticles are zinc (Zn) containing metal oxide nanoparticles.

[0026] Preferably, the zinc (Zn) containing metal oxide nanoparticles are alloyed with a metal that can increase the band gap of zinc oxide (ZnO) to provide an electron transport layer ink composition for inkjet printing.

[0027] Preferably, the zinc (Zn) containing metal oxide nanoparticles are zinc magnesium oxide (ZnMgO).

[0028] Preferably, the organic ligand is contained in an amount of 0.0001 to 10 moles per mole of metal contained in the metal oxide nanoparticles, in an electron transport layer ink composition for inkjet printing.

[0029] In yet another aspect of the present invention, there is provided a method for preparing an ink composition for an electron transport layer for inkjet printing, comprising preparing metal oxide nanoparticles, adding an organic ligand to modify the surface of the metal oxide nanoparticles, and mixing the resulting mixture with a non-polar solvent.

[0030] Preferably, the organic ligand is contained in an amount of 0.0001 to 10 moles per mole of the main metal contained in the metal oxide nanoparticles.

[0031] Preferably, the non-polar solvent is Cyclohexylbenzene, and at least one solvent selected from the group consisting of styrene, hexadecane, anisole, and cyclohexanone.

[0032] Preferably, the volume ratio of cyclohexylbenzene to other solvents is 7:3 to 20:1.

[0033] In yet another aspect of the present invention, there is provided a light-emitting device comprising an electron transport layer made from the aforementioned composition.

[0034] Preferably, the electron transport layer is formed through inkjet printing to provide a light emitting device.

[0035] In yet another aspect of the present invention, there is provided a display including the light-emitting device. Effect of the Invention

[0036] According to an embodiment of the present invention, the metal oxide nanoparticles can be mixed into two non-polar solvents through surface modification, and can be easily discharged uniformly by an inkjet method.

[0037] In addition, when a polar solvent-based light-emitting layer is used, an ink composition for an electron transport layer for inkjet printing can be provided that can form a uniform film on the top of the light-emitting layer, thereby eliminating the etching problem of the polar solvent-based light-emitting layer.

[0038] As a result, the electron transport layer ink composition of the present invention can be usefully applied to the preparation of light-emitting devices, specifically, self-emissive displays, through an inkjet printing process, and can also be advantageously applied to commercialization and large-scale production through the application of a simple and inexpensive inkjet process.

[0039] The effects of the present invention are not limited to the above-mentioned examples, and more diverse effects are included in the present specification. [Brief description of the drawings]

[0040] [Figure 1] 1 is a diagram showing absorption spectra of metal oxide nanoparticles (ZnMgO) prepared according to Example 1 of the present invention and a comparative example. [Diagram 2] 1 is a diagram showing TGA graphs of ZnMgO prepared in Examples 1 and 2 according to the present invention and a comparative example, respectively. [Diagram 3] 1 is a diagram showing FT-IR graphs of ZnMgO prepared in Examples 1 and 3 according to the present invention and a comparative example, respectively. [Figure 4] 1 shows a one-drop image formed on a substrate using the electron transport layer ink composition prepared in Example 1 according to the present invention. [Diagram 5] 1 is a diagram showing the shape of an ink formed on a substrate using an electron transport layer ink composition according to Example 1 of the present invention and a coffee ring factor (CRF) result. [Figure 6] 13 is a diagram showing the ink profile and CRF results formed on a substrate using an electron transport layer ink composition of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] The present invention will now be described.

[0042] All terms (including technical and scientific terms) used in this specification may be used as commonly understood by those having ordinary knowledge in the technical field to which the present invention belongs, unless otherwise defined. Furthermore, terms defined in commonly used dictionaries are not interpreted ideally or excessively unless otherwise clearly defined.

[0043] Furthermore, throughout this specification, when a part "comprises" a certain component, this does not mean to exclude other components, but means that it may further include other components, unless specifically stated to the contrary.

[0044] In this specification, the term "organic group" refers to a C1-C30 linear or branched alkyl group, a C2-C30 linear or branched alkenyl group, or a C2-C30 linear or branched alkynyl group, each of which may be substituted or unsubstituted.

[0045] As used herein, "alkyl" refers to a monovalent substituent derived from a straight or branched chain saturated hydrocarbon having 1 to 30 carbon atoms, examples of which include, but are not limited to, methyl, ethyl, propyl, isobutyl, sec-butyl, pentyl, iso-butyl, hexyl, and the like.

[0046] As used herein, "alkenyl" refers to a monovalent substituent derived from a straight-chain or branched-chain unsaturated hydrocarbon having 2 to 30 carbon atoms and one or more carbon-carbon double bonds. Examples include, but are not limited to, vinyl, allyl, isopropenyl, 2-butenyl, etc.

[0047] As used herein, "alkynyl" refers to a monovalent substituent derived from a straight-chain or branched-chain unsaturated hydrocarbon having 2 to 30 carbon atoms and one or more carbon-carbon triple bonds. Examples include, but are not limited to, ethynyl, n-propynyl, n-but-2-enyl, n-hex-3-enyl, and the like.

[0048] <Electron Transport Layer Ink Composition> The electron transport layer ink composition according to one embodiment of the present invention is an ink composition that can be jetted by a general ink jet method and can form an electron transport layer (ETL).

[0049] An electron transport layer ink composition according to one embodiment of the present invention can include metal oxide nanoparticles that are surface modified with organic ligands and a non-polar solvent.

[0050] The composition of the electron transport layer ink composition is described in detail below.

[0051] Metal Oxide Nanoparticles The metal oxide nanoparticles may be any material used in the art for an electron transport layer without limitation. For example, conventional metal oxide nanoparticles used as dopant materials may be used, and non-limiting examples thereof include In 2 S 3 , Cu 2 S, Ag 2 S, ZnSe, ZnS, ZnO, ZnTe, ZnSe, TiO 2 , SnO 2 , ZnS, or a form in which at least one element is added to the aforementioned components.

[0052] In one specific example, the metal oxide nanoparticles are zinc (Zn)-containing metal oxide nanoparticles, and more specifically, may be alloyed with a metal (M) capable of increasing the band gap of zinc oxide (ZnO) [ZnMO (M=Ca, Mg)]. The metal (M) capable of increasing the band gap of ZnO is calcium (Ca) or magnesium (Mg). These metals have an ionic radius similar to that of Zn, so they can be mixed into the ZnO lattice without inducing stress and increase the band gap of ZnO through the reduction in the size of ZnO, and are preferably zinc magnesium oxide (ZnMgO).

[0053] In this way, when the band gap of ZnO nanoparticles is increased by alloying and applied to the electron transport layer, an upshift of the conduction band minimum (CBM) level occurs, resulting in energy proximity between the CBM of the quantum dot light emitting layer and the electron transport layer, which reduces the electron energy barrier and promotes the injection of electrons into the quantum dot region. As a result, a light emitting device having an electron transport layer containing alloyed ZnO nanoparticles is superior in terms of luminance and efficiency compared to a device having an electron transport layer containing ZnO nanoparticles, and can have a higher luminous efficiency even at a lower driving voltage. That is, when the above-mentioned electron transport layer is applied, the electron injection barrier is reduced, and the effects of reducing the driving voltage of the QLED, improving efficiency, and further reducing power consumption can be obtained. If the driving voltage of the device is reduced, the heat generation of the device is also reduced, and thus an increase in the life of the device can be expected.

[0054] In one embodiment, organic ligands having hydrophobic moieties may be attached to all or part of the surface of the metal oxide nanoparticles.

[0055] The organic ligand may be any organic ligand known in the art, and some of the organic ligands may have functional groups with excellent affinity to the quantum dot surface, such as carboxylic acid, acrylate, pyridine, thiol, phosphine, phosphine oxide, primary amine, secondary amine, or a combination thereof.

[0056] The organic ligand may contain a hydrophobic moiety, specifically, a C1-C30 linear or branched alkyl group, a C2-C30 linear or branched alkenyl group, or a C2-C30 linear or branched alkynyl group, preferably a C5-C30 linear or branched alkyl group, a C5-C30 linear or branched alkenyl group, or a C5-C30 linear or branched alkynyl group.

[0057] Non-limiting examples of organic ligands that can be used include oleic acid, myristic acid, lauric acid, palmitic acid, stearic acid, oleylamine, n-octylamine, hexadecylamine, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, or combinations thereof.

[0058] Such organic ligands are attached to the surface of metal oxide nanoparticles, surrounding the surface of the nanoparticles with hydrophobic moieties, allowing them to be mixed and dispersed in non-polar solvents, and can play a role in ensuring film uniformity by improving the coffee ring effect (CRE) during inkjet ejection.

[0059] Here, the coffee ring effect (CRE) refers to the phenomenon in which colloidal particles move to the edge due to the hydrodynamic effect of the evaporation process, resulting in an uneven particle density distribution. That is, the smaller the particle size, the more it can move to the edge, so small particles are distributed closer to the edge of the droplet, and relatively large particles are distributed closer to the center of the droplet.

[0060] The content of the organic ligand is not particularly limited and may be appropriately adjusted within a range of contents known in the art. In consideration of dispersibility and film uniformity, the organic ligand is contained in the metal oxide nanoparticles in a range of 0.001 to 10 mol, specifically, 0.001 to 5 mol, per mol of the metal, for example, zinc (Zn), contained therein.

[0061] Meanwhile, in the present invention, metal oxide nanoparticles are mainly described as materials constituting the electron transport layer, but the present invention is not limited to the above materials, and the application of organic materials or organic-inorganic composite materials that can be used as electron transport layer materials in the relevant field also falls within the scope of the present invention.

[0062] In the present invention, the content of the metal oxide nanoparticles is not particularly limited and may be appropriately adjusted within a range known in the art, for example, 5 to 30 parts by weight, specifically 10 to 20 parts by weight, based on the total weight (e.g., 100 parts by weight) of the electron transport layer ink composition.

[0063] Non-polar solvents Conventional metal oxide nanoparticles, for example ZnMgO, use alcohol-based solvents as a dispersion medium due to the characteristics of the material. When ethanol is used alone, the device characteristics are realized but inkjet ejection is not performed. In addition, when a light-emitting layer of the same polar solvent type as ethanol is used, the inevitable problem of etching the light-emitting layer due to the use of the same solvent cannot be avoided. Finding a non-polar solvent that can disperse metal oxide nanoparticles and meets the inkjet ejection conditions has been a persistent and very difficult problem in the industry.

[0064] Meanwhile, the ejection conditions of the inkjet equipment are largely divided into viscosity and vapor pressure. If the viscosity is too high or low, a uniform film cannot be obtained, and the degree of ejection is determined by the vapor pressure. In the present invention, taking into consideration the viscosity and vapor pressure appropriate for inkjet ejection, at least two mixed solvents that can satisfy such physical properties are selected, and the mixing ratio of these is controlled within a predetermined range to constitute the solvent of the electron transport layer ink composition.

[0065] As a specific example, the electron transport layer ink composition of the present invention containing at least two solvents has a viscosity of 1.0 to 5.0 cps at 20° C., a vapor pressure of 0.6 to 45 mmHg at 20° C., and a solids content of 5 to 30% by weight. More specifically, the ink composition may have a viscosity of 1.2 to 3.0 cps, a vapor pressure of 1.0 to 30 mmHg, and a solids content of 5 to 25% by weight.

[0066] When the ink has the above-mentioned physical properties of solid content, viscosity, and vapor pressure, not only is ink jet ejection easy, but the ejected ink is uniform in quality, allowing device characteristics to be realized.

[0067] The electron transport layer ink composition according to the present invention is not particularly limited in terms of the specific components and / or contents of the at least two solvents constituting the composition, so long as the composition satisfies the above-mentioned properties of solid content, viscosity, and vapor pressure.

[0068] In one specific example, the non-polar solvent may include cyclohexylbenzene (CHB).

[0069] That is, in the present invention, CHB having good dispersibility can be used as the main solvent, and considering the application of inkjet ejection, when CHB solvent is used alone, it is not suitable in terms of viscosity. Therefore, other non-polar solvents having a viscosity different from that of CHB are mixed, and the volume ratio of each is adjusted so that the final composition simultaneously satisfies the above-mentioned properties of solid content, viscosity, and vapor pressure.

[0070] Other non-polar solvents having a viscosity different from that of CHB may include one or more solvents selected from the group including styrene, hexadecane, anisole, and cyclohexanone.

[0071] In this case, CHB is the main solvent and may be configured to have 70 volume % or more based on 100 volume % of the total solvent. The volume ratio of cyclohexylbenzene to other non-polar solvents is 7:3 to 20:1, preferably 7:3 to 9.5:0.5, and more preferably 7:3 to 9:1. If the other non-polar solvent other than cyclohexylbenzene exceeds 30 volume % of the total solvent, the viscosity of the total solvent may increase, and the inkjet dischargeability may decrease.

[0072] The mixed nonpolar solvent in the present invention is characterized in that it has a viscosity of 1 to 6 cps at 20° C., a vapor pressure of 0.001 to 0.1 mmHg at 20° C., and a surface tension of 30 to 40 dyn / cm at 20° C. When the properties of the mixed nonpolar solvent are within the above ranges, it is suitable for use in an ink composition for inkjet printing.

[0073] In the present invention, the total content of the non-polar solvent in the ink composition is not particularly limited and can be appropriately adjusted within a range known in the art. For example, the total content is the balance that satisfies 100 parts by weight of the electron transport layer ink composition, specifically, 70 to 95 parts by weight.

[0074] Other Additives In addition to the above-mentioned components, the electron transport layer ink composition of the present invention can contain at least one additive known in the art, without any restrictions, as long as the additive does not impair the effects of the present invention.

[0075] Examples of usable additives include light stabilizers, heat stabilizers, light initiation accelerators, heat initiation accelerators, smoothing agents, toughening agents, thickeners, colorants, reactive diluents, coupling agents, dispersants, etc. These may be used alone or in combination of two or more. In this case, the content of the additives may be appropriately adjusted within a range known in the art and is not particularly limited. For example, the at least one additive is included in an amount of 0.01 to 5 parts by weight, specifically 0.01 to 2 parts by weight, based on the total weight of the electron transport layer ink composition.

[0076] <Method of Manufacturing Electron Transport Layer Ink Composition> The electron transport layer ink composition for ink jet printing according to the present invention can be prepared by mixing and stirring the surface-modified metal oxide nanoparticles described above, at least two non-polar solvents, and other additives, if desired, by any conventional method known in the art.

[0077] In one embodiment of the present invention, after preparing metal oxide nanoparticles, an organic ligand can be added to modify the surface of the metal oxide nanoparticles, centrifuged, and mixed with a non-polar solvent to prepare an electron transport layer ink composition for inkjet printing.

[0078] In this case, the organic ligand can be added in an amount of 0.0001 to 10 mol per 1 mol of the main metal contained in the metal oxide nanoparticles.

[0079] The nonpolar solvent is a mixture of two nonpolar solvents, specifically, a mixture of cyclohexylbenzene and another nonpolar solvent, in a volume ratio of 7:3 to 20:1.

[0080] In one embodiment of the electron transport layer ink composition, (i) a basic substance is added to a reaction solution in which a zinc-containing compound and a metal-containing compound capable of increasing the band gap of ZnO are dissolved in a solvent, and the reaction solution is stirred and heated at about 50 to 80° C. for 30 minutes to 2 hours at a uniform speed, (ii) an organic ligand is added to the reaction solution in a molar amount ranging from 10 to 70% of the molar amount of zinc ions contained in the zinc-containing compound, and the reaction solution is stirred and heated at about 80 to 120° C. for 10 minutes to 1 hour at a uniform speed, (iii) hexane and acetone are added to the reaction solution after the reaction is completed, and the solution is centrifuged to obtain surface-modified metal oxide nanoparticles. (iv) The surface-modified metal oxide nanoparticles can be mixed and dispersed in a solvent in which cyclohexylbenzene and another non-polar solvent are mixed in a volume ratio of 7:3 to produce an electron transport layer ink composition.

[0081] In the above embodiment, the zinc-containing compound and the metal-containing compound are not particularly limited, and any substance known in the art can be used without limitation. For example, zinc acetate, zinc acetate dihydrate, zinc chloride, zinc nitrate, zinc sulfate, magnesium acetate tetrahydrate, etc. can be used.

[0082] The basic substance is not particularly limited, and any substance known in the art may be used without limitation. For example, at least one substance selected from the group consisting of tetramethylammonium hydroxide (TMAH), potassium hydroxide (KOH), sodium hydroxide (NaOH), and amines may be used.

[0083] Non-limiting examples of solvents that can be used to separate surface-modified metal oxide nanoparticles using their solvent and non-solvent properties include hexane, benzene, xylene, toluene, octane, chloroform, chlorobenzene, tetrahydrofuran (THF), methylene chloride, 1,4-dioxane, diethyl ether, cyclohexane, dichlorobenzene, etc., which may be used alone or in combination of two or more. Non-limiting examples of non-solvents that can be used include acetone, ethanol, methanol, butanol, propanol, isopropyl alcohol, tetrahydrofuran, dimethyl sulfoxide, dimethylformamide, etc., which may be used alone or in combination of two or more.

[0084] The mixing method in the above-mentioned production method is not particularly limited, and as an example, a mixer such as a general homodisper, homomixer, universal mixer, planetary mixer, kneader, or three-roll mixer known in the art can be used.

[0085] The prepared electron transport layer ink composition may further include at least one other additive, such as a dispersant.

[0086] The ink composition for an electron transport layer of the present invention, configured as described above, has optimized viscosity and vapor pressure properties, thereby providing excellent workability and processability. In particular, the ink composition for an electron transport layer of the present invention can be effectively used in inkjet printing by ensuring uniformity and stability in terms of inkjet ejection, the shape of the ejected ink, and the shape of the ink formed on a substrate.

[0087] Other than that, to the extent that they overlap, they are as described above for the electron transport layer ink composition.

[0088] <Light Emitting Device and Display Device> The light emitting device according to one embodiment of the present invention is distinguished from conventional light emitting devices in that it includes an electron transport layer formed from the above-described electron transport layer ink composition.

[0089] The light emitting device according to an embodiment of the present invention may be, but is not limited to, a quantum dot light emitting device, an organic light emitting device, or the like, and may be applied to various types of light emitting devices.

[0090] In general, a light emitting device includes a first electrode, a second electrode facing the first electrode, a light emitting layer between the first electrode and the second electrode, a hole transport layer between the first electrode and the light emitting layer, and an electron transport layer between the light emitting layer and the second electrode and formed by inkjet printing the electron transport layer ink composition described above. If necessary, the light emitting device may further include at least one layer selected from the group consisting of a hole injection layer and an electron injection layer.

[0091] In this case, the electron transport layer serves to facilitate the injection of electrons from the second electrode and to transport the electrons to the light emitting layer. Such an electron transport layer includes Zn-containing metal oxide nanoparticles alloyed with a metal capable of increasing the band gap of ZnO. For example, the electron transport layer may be formed by inkjet printing the electron transport layer ink composition on the light emitting layer and then volatilizing the solvent. The electron transport layer of the present invention may be provided as a single layer structure that also serves as an electron injection layer, or may be formed as a laminate structure with a separate electron injection layer.

[0092] The present invention also provides a display device including the quantum dot composition, which may be, but is not limited to, a liquid crystal display (LCD), an electroluminescent display (EL), a plasma display panel (PDP), a field emission display (FED), an organic light emitting device (OLED), or the like.

[0093] The present invention will be described in more detail with reference to the following examples. However, the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention. EXAMPLES

[0094] Example 1. Non-polar Solvent Inkjet Electron Transport Layer Ink Composition Zinc acetate (Zn(OAc) 2 ) and magnesium acetate tetrahydrate were dissolved in dimethyl sulfoxide (DMSO), and then the basic substance tetramethylammonium hydroxide (TMAH) was poured in, heated to about 60°C, and reacted for about 1 hour. 2 Oleic acid was added so that the molar ratio was about 30% relative to the molar ratio of the olefin, and the reaction was carried out at about 100° C. for about 30 minutes. After the reaction, the solution was centrifuged and dispersed in a solvent in which cyclohexylbenzene:styrene was mixed in a volume ratio of 7:3.

[0095] Example 2. Similar to Example 1, the solution after surface modification was centrifuged twice and then dispersed in a non-polar solvent.

[0096] Example 3. The same as in Example 1, except that the moles of oleic acid were changed to Zn(OAc) 2 The production was carried out by adding about 50% by mole of the above.

[0097] Comparative Example: Conventional Inkjet Electron Transport Layer Ink Composition (Polar Solvent Type) The reaction was terminated without adding any additional organic ligand to the solution after the reaction was completed in the same manner as in Example 1, and hexane and acetone were added to the solution, and the particles were centrifuged and then dispersed in a solvent containing DMSO, ethanol, 2-methoxyethanol, and butanol in a volume ratio of 5:3:1:1.

[0098] Test Example 1: Spectroscopic Evaluation The absorption spectra were measured using the electron transport layer compositions prepared in Example 1 and Comparative Example.

[0099] Referring to Figure 1, the UV-visible absorption spectrum of the ZnMgO nanoparticles synthesized in Example 1 (blue line) and the UV-visible absorption spectrum of the ZnMgO nanoparticles synthesized in the Comparative Example (orange line) are shown together. As shown in Figure 1, it can be seen that both have similar absorption spectra, especially the maximum absorption wavelength at about 305 nm.

[0100] Therefore, it was confirmed that the metal oxide nanoparticles of Example 1 can exhibit the same spectral characteristics as the existing polar solvent-based inkjet electron transport layer ink composition.

[0101] Test Example 2. TGA analysis of ZnMgO produced in Examples 1 and 2 and Comparative Example TGA analysis is a thermal analysis technique that measures the mass change of a sample due to temperature change. The temperature at which a sudden change in weight occurs can be interpreted as the decomposition temperature of the organic matter, and the weight percentage occupied by the organic matter can be numerically confirmed based on the degree of total weight loss.

[0102] The ZnMgO prepared in Examples 1 and 2 and Comparative Example were subjected to TGA analysis, and the results are shown in Table 1 and FIG.

[0103] [Table 1]

[0104] There was a weight loss of about 10% of the organic matter contained in the nanoparticles produced in the comparative example.

[0105] In the case of Example 1, the weight of the organic matter was reduced by about 30%, and in the case of Example 2, the weight of the organic matter was reduced by about 15%. This shows that the more centrifugation is performed, the more the organic ligands attached to the ZnMgO surface are separated from the nanoparticles.

[0106] In addition, the nanoparticles produced in the Comparative Example did not contain any organic ligands and had a decomposition temperature of about 300° C., while the decomposition temperatures in the Examples were all the same at about 360° C. Therefore, it is believed that the organic matter removed from the Comparative Example is the organic matter that was removed in small amounts during the centrifugation process, and that the organic matter removed from the Examples is the organic ligand that was attached to the surface of the ZnMgO.

[0107] Test Example 3: FT-IR analysis of ZnMgO produced in Examples 1, 3 and Comparative Example FT-IR analysis was carried out using the ZnMgO produced in Examples 1 and 3 and the Comparative Example, and the results are shown in FIG.

[0108] 3, similarly shaped peaks are observed at 2800-2900 nm in Examples 1 and 3, but no peak is observed in this range in the Comparative Example, confirming that organic ligands are well attached to the surface of the ZnMgO prepared in the Examples.

[0109] Test Example 4. Evaluation of dispersibility of ZnMgO produced in Examples 1, 3 and Comparative Example The ZnMgO prepared in Examples 1 and 3 and Comparative Example was mixed and stirred with a non-polar solvent to check whether it could be dispersed. The non-polar solvent used was a mixture of cyclohexylbenzene and styrene in a volume ratio of 7:3. The results are shown in Table 2 below.

[0110] [Table 2]

[0111] Both Examples 1 and 3 were able to be dispersed in non-polar solvents regardless of the amount of organic ligand added, but the nanoparticles of the comparative example were shown to separate into layers when mixed with a non-polar solvent and not to be mixed at all.

[0112] Test Example 5. Inkjet ejection evaluation The ejection properties by inkjet printing were evaluated using the electron transport layer ink composition of Example 1. Specifically, each ink composition was ejected using an inkjet printing device (OMNIJET200), and ejected in the form of one drop. The results are shown in FIG.

[0113] Referring to FIG. 4, each dot is derived in a circular shape, and no deformations have been found that encroach on the area of ​​other dots or change the spacing between dots.

[0114] Test Example 6. Inkjet Shape (CRF) Evaluation The electron transport layer ink compositions of Example 1 and Comparative Example were ejected using an inkjet printing device (OMNIJET200), and the inks formed on the substrate were analyzed using a three-dimensional surface profiler (NV9000, Zygo). The degree of the coffee-ring effect was quantified using the following Equation 1, and the results are shown in FIGS. 5 and 6.

[0115] [Formula 1] CRF (Coffee Ring Factor)=Hmax / Hmin In the above formula, Hmax indicates the maximum thickness of the pattern, Hmin indicates the minimum thickness of the pattern, and the CRF value indicates the degree of the coffee ring effect, i.e., CRF=1 indicates that the coffee ring effect is completely removed.

[0116] 5, the Hmax of the inkjet shape of Example 1 was about 11.86 nm, and Hmin was about 9.49 nm (not shown). Therefore, the CRF was about 1.25, which is very close to 1, and it can be seen that the three-dimensional shape is not a single cross section but has a uniform shape overall.

[0117] 6, the Hmax of the inkjet shape of the comparative example was about 15.26 nm, and Hmin was about 9.66 nm (not shown). Therefore, the CRF was about 1.58, which is a value far from 1. Even when looking at the three-dimensional shape, it can be seen that the coffee ring effect is not clearly seen in only one cross section, but is seen overall.

[0118] For reference, even though the same amount was ejected, Hmax was approximately 11.86 nm in Example 1 and 15.26 nm in the comparative example. Comparing these, it can be expected that the deviation in height of the inkjet shape is very large in the comparative example.

[0119] It will be obvious to those having ordinary skill in the art to which the present invention pertains that the present invention is not limited to the above-described embodiments and can be modified or altered in various ways without departing from the technical scope of the present invention.

Claims

1. 1. A metal oxide nanoparticle comprising: The metal oxide nanoparticles are surface-modified; Metal oxide nanoparticles dispersible in non-polar solvents for inkjet printing.

2. 10. The metal oxide nanoparticles of claim 1, wherein the surface of the metal oxide nanoparticles is modified with organic ligands having hydrophobic moieties.

3. The metal oxide nanoparticles for inkjet printing of claim 1 , wherein the non-polar solvent is a mixture of at least two solvents.

4. The metal oxide nanoparticles for inkjet printing of claim 3 , wherein the non-polar solvent comprises cyclohexylbenzene.

5. 3. The metal oxide nanoparticles for inkjet printing according to claim 2, wherein the organic ligand is contained in an amount ranging from 0.0001 to 10 moles per mole of the metal contained in the metal oxide nanoparticles.

6. The metal oxide nanoparticles for inkjet printing according to claim 1 , wherein the metal oxide nanoparticles are zinc (Zn)-containing metal oxide nanoparticles.

7. The metal oxide nanoparticles for inkjet printing according to claim 6, wherein the zinc (Zn)-containing metal oxide nanoparticles are alloyed with a metal capable of increasing the band gap of zinc oxide (ZnO).

8. 7. The metal oxide nanoparticles for inkjet printing of claim 6, wherein the zinc (Zn)-containing metal oxide nanoparticles are zinc magnesium oxide (ZnMgO).

9. Metal oxide nanoparticles surface-modified with organic ligands; a non-polar solvent, An electron transport layer ink composition for ink jet printing that is ink jet jettable.

10. 10. The electron transport layer ink composition for ink jet printing of claim 9, wherein the non-polar solvent is a mixture of at least two solvents.

11. 11. The electron transport layer ink composition for ink jet printing of claim 10 wherein the non-polar solvent comprises cyclohexylbenzene.

12. 12. The electron transport layer ink composition for ink jet printing of claim 11 wherein the non-polar solvent further comprises one or more solvents selected from the group consisting of styrene, hexadecane, anisole, and cyclohexanone.

13. The mixed non-polar solvent is The viscosity at 20°C is 1 to 6 cps, The vapor pressure at 20°C is 0.001 to 0.1 mmHg, 11. The electron transport layer ink composition for ink jet printing of claim 10 having a surface tension of from 30 to 40 dyn / cm at 20.degree.

14. 12. The electron transport layer ink composition for ink jet printing of claim 11, wherein a volume ratio of cyclohexylbenzene to the other solvent is from 7:3 to 20:

1.

15. The composition comprises: The viscosity at 20°C is 1.0 to 5.0 cps, The vapor pressure at 20°C is 0.6 to 45 mmHg, 10. The electron transport layer ink composition for ink jet printing of claim 9 having a solids content of from 5 to 30 weight percent.

16. 10. The electron transport layer ink composition for ink jet printing of claim 9 wherein the organic ligand is an organic ligand having a hydrophobic moiety.

17. 10. The electron transport layer ink composition for ink jet printing of claim 9, wherein the metal oxide nanoparticles are zinc (Zn) containing metal oxide nanoparticles.

18. 20. The electron transport layer ink composition for ink jet printing of claim 17, wherein the zinc (Zn)-containing metal oxide nanoparticles are alloyed with a metal capable of increasing the band gap of zinc oxide (ZnO).

19. 20. The electron transport layer ink composition for ink jet printing of claim 17, wherein the zinc (Zn) containing metal oxide nanoparticles are zinc magnesium oxide (ZnMgO).

20. 10. The electron transport layer ink composition for ink jet printing of claim 9, wherein the organic ligand is present in an amount of 0.0001 to 10 moles per mole of metal contained in the metal oxide nanoparticles.

21. A method for preparing an electron transport layer ink composition for inkjet printing, comprising preparing metal oxide nanoparticles, adding an organic ligand to modify the surface of the metal oxide nanoparticles, and mixing the metal oxide nanoparticles with a non-polar solvent.

22. 22. The method of claim 21, wherein the organic ligand is present in an amount of 0.0001 to 10 moles per mole of the main metal contained in the metal oxide nanoparticles.

23. The non-polar solvent is Cyclohexylbenzene, 22. The method of claim 21 , wherein the ink composition is prepared by mixing one or more solvents selected from the group consisting of styrene, hexadecane, anisole, and cyclohexanone.

24. 24. The method for preparing an electron transport layer ink composition for ink jet printing according to claim 23, wherein a volume ratio of cyclohexylbenzene to the other solvent is from 7:3 to 20:

1.

25. 21. A light emitting device comprising an electron transport layer made with the composition of any one of claims 9 to 20.

26. The light emitting device of claim 25, wherein the electron transport layer is formed through inkjet printing.

27. A display comprising the light-emitting device of claim 26.

Citation Information

Patent Citations

  • Coloring particle and ink-jet ink

    JP2001192582A

  • inkjet ink composition

    JP2017519056A

  • Quantum dot emitting diode and quantum dot display device including the same

    US20190081262A1

  • Ink for use in ink jet recording

    WO1991007470A1

  • Display device and method for manufacturing same

    WO2020121398A1