Biaxially oriented polyester film, method for manufacturing sand mat film, and method for manufacturing printed label

A biaxially oriented polyester film with controlled resin layer thickness and surface roughness, combined with strategic manufacturing processes, addresses blocking and adhesion issues, ensuring effective print adhesion and slipperiness in low-gloss designs.

JP2024154842AInactive Publication Date: 2024-10-31TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023068989
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing biaxially oriented polyester films face issues with blocking and poor adhesion after deep sand matting, particularly when an easy-to-adhesive layer peels off, leading to insufficient matte finish and print adhesion, especially in low-gloss designs.

Method used

A biaxially oriented polyester film with a resin layer (A) of specific thickness and surface roughness (Sku) properties, combined with a B layer of controlled exposure, ensures both blocking resistance and print adhesion, achieved through precise manufacturing processes like in-line coating and biaxial stretching.

Benefits of technology

The film achieves both blocking and slipperiness with excellent print adhesion after deep sand matting, suitable for low-gloss designs, by maintaining the resin layer integrity and optimizing surface texture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154842000001
    Figure 2024154842000001
  • Figure 2024154842000002
    Figure 2024154842000002
  • Figure 2024154842000003
    Figure 2024154842000003
Patent Text Reader

Abstract

To provide a biaxially oriented polyester film which achieves both blocking and slipperiness, and printing adhesion after deep sand mat treatment, a sand mat film using the same, and a printed label using the same.SOLUTION: A biaxially oriented polyester film has a resin layer (A layer) having a thickness of 150 nm or more and 400 nm or less on the outermost layer on at least one side of the polyester film, wherein the A layer is in contact with a B layer containing polyester as the main component, and the kurtosis Sku measured on the surface on the A layer side is 20 or more and 250 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biaxially oriented polyester film that satisfies both blocking resistance and slipperiness, and print adhesion after deep sand matte treatment, a method for producing a sand matte film, and a method for producing a printed label. [Background technology]

[0002] Polyester films are widely used as base films for labels, etc., because of their excellent heat resistance, printability, and adhesive properties. In addition, in order to improve the texture of the label and the clarity of the print, it is sometimes necessary to apply a process to the surface of the polyester film to reduce the gloss (matte finish).

[0003] Typical processes (matte finishes) that reduce the gloss of a film include sandblasting and hairline finishes. Sandblasting involves colliding powder (sand) with the film surface at high speed to change the shape of the film surface and reduce the gloss of the film. Hairline finishes involve using a metal lathe to create hair-like scratches on the surface to reduce gloss. Both processes create unevenness on the film surface, resulting in a surface shape that diffuses light. The strength of the matte finish is adjusted appropriately depending on the required gloss level, but in order to meet the demand for more advanced low-gloss designs in recent years, there is an increasing need to form a surface shape with deeper unevenness and more denseness.

[0004] On the other hand, when a polyester film is used as a base film for a label or the like, an easy-adhesion layer may be provided on the surface of the polyester film in order to improve adhesion with a printing layer. However, when the film having an easy-adhesion layer is subjected to the above-mentioned matte processing, the easy-adhesion layer peels off, and there is a problem that the easy-adhesion after the matte processing is insufficient. When the intensity of the matte processing is adjusted in order to prevent the easy-adhesion layer from peeling off, the matte feeling may become insufficient, and it is often difficult to achieve both, which is a major problem especially in labels with a lower gloss design.

[0005] In order to solve such problems, studies have been conducted to ensure the easy adhesion after sand matting by making the easy adhesion layer thicker (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-124875 A [Patent Document 2] Japanese Patent Application Publication No. 2-42475 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the films of Patent Documents 1 and 2, the thickening of the easy-adhesion layer is accompanied by the smoothing of the film surface, which can cause blocking, where the films adhere to each other before the sand matte processing. In addition, particles of the easy-adhesion layer remaining on the surface after deep sand matte processing to achieve a lower gloss, which is particularly required in recent years, can fall off after printing processing, causing poor adhesion and missing prints. Thus, there is room for improvement in the characteristics of the substrate to be matte processed.

[0008] Therefore, an object of the present invention is to provide a biaxially oriented polyester film that combines blocking resistance, slipperiness, and printing adhesion after deep sand matte treatment, as well as a sand matte film using the same, and a printed label using the same. [Means for solving the problem]

[0009] In order to solve the above problems, a preferred embodiment of the present invention has the following configuration. (1) A biaxially oriented polyester film having a resin layer (layer A) having a thickness of 150 nm or more and 400 nm or less as the outermost layer on at least one side of the polyester film, the layer A being in contact with layer B containing polyester as a main component, and having a kurtosis Sku of 20 or more and 250 or less measured on the surface on the layer A side. (2) The biaxially oriented polyester film according to (1), wherein the surface crystallinity measured on the layer A side by attenuated total reflection infrared spectroscopy (ATR-IR) is 0.70 or more and less than 1.10. (3) The biaxially oriented polyester film according to (1) or (2), wherein the layer A contains resin particles. (4) The biaxially oriented polyester film according to any one of (1) to (3), wherein the curl amount measured at 23° C. is 0.2 mm or more and 3.0 mm or less. (5) The biaxially oriented polyester film according to any one of (1) to (4), wherein the thickness of the layer B is from 0.5 μm to 4.0 μm. (6) A method for producing a sand-matte film, comprising a step of subjecting a biaxially oriented polyester film according to any one of (1) to (5) to a sand-matte treatment, in which the B layer is exposed at a ratio of 0.5% or more and 10.0% or less. (7) A method for producing a printed label, comprising: a biaxially oriented polyester film according to any one of (1) to (5) that has been subjected to a sand-matt treatment so that the B layer is exposed at a ratio of 0.5% to 10.0%; and a printed layer, the printed layer being in contact with both the A layer and the B layer. Effect of the Invention

[0010] According to the present invention, it is possible to provide a biaxially oriented polyester film that combines blocking resistance, slipperiness, and print adhesion after deep sand matte treatment, as well as a sand matte film using the same, and a printed label using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] A preferred embodiment of the present invention will be described in detail below.

[0012] The polyester resin used in the biaxially oriented polyester film of the present invention (hereinafter, sometimes simply referred to as the "film of the present invention") refers to a polymer having an ester bond in the main chain, and the polyester resin used in the present invention is preferably a polyester resin having a structure obtained by condensation polymerization of a dicarboxylic acid and a diol. Examples of the dicarboxylic acid component include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenoxyethanedicarboxylic acid, and 5-sodiumsulfonedicarboxylic acid, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid, alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, and oxycarboxylic acids such as paraoxybenzoic acid. Examples of the dicarboxylate derivative component include esters of the above dicarboxylate compounds, such as dimethyl terephthalate, diethyl terephthalate, 2-hydroxyethyl methyl terephthalate, dimethyl 2,6-naphthalenedicarboxylate, dimethyl isophthalate, dimethyl adipate, diethyl maleate, and dimethyl dimerate. Examples of the diol component include aliphatic dihydroxy compounds such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 2,2-dimethyl-1,3-propanediol (neopentyl glycol), polyoxyalkylene glycols such as diethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, alicyclic dihydroxy compounds such as 1,4-cyclohexanedimethanol and spiroglycol, and aromatic dihydroxy compounds such as bisphenol A and bisphenol S. These may be used alone or in combination of two or more. In addition, as long as the film formability is not adversely affected, a small amount of one or more of trimellitic acid, pyromellitic acid and their ester derivatives may be copolymerized.

[0013] Specific examples of polyester resins include polyethylene terephthalate (hereinafter abbreviated as PET), polyethylene-2,6-naphthalenedicarboxylate, polypropylene terephthalate, polybutylene terephthalate, and poly-1,4-cyclohexylene dimethylene terephthalate, which are inexpensive and have good film-forming properties and can therefore be particularly suitably used.

[0014] The polyester resin may be a homopolymer or a copolymer. Examples of copolymer components in the copolymer include aromatic dicarboxylic acids, aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and diol components having 2 to 15 carbon atoms, and examples of these include isophthalic acid, adipic acid, sebacic acid, phthalic acid, sulfonate group-containing isophthalic acid, and ester-forming compounds thereof, ethylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, spiroglycol, and polyalkylene glycols having a number average molecular weight of 400 to 20,000.

[0015] Furthermore, various additives such as antioxidants, heat stabilizers, weathering agents, ultraviolet absorbers, infrared absorbers, organic lubricants, pigments, dyes, organic or inorganic fine particles, fillers, antistatic agents, nucleating agents, etc. may be appropriately selected and added to the polyester.

[0016] The thickness of the biaxially oriented polyester film of the present invention is not particularly limited and is appropriately selected depending on the application and type, but is usually 10 μm to 500 μm, more preferably 23 μm to 125 μm, from the viewpoints of mechanical strength, handleability, etc. The polyester film may be a composite film obtained by coextrusion, or may be a composite film obtained by laminating the obtained films by various methods.

[0017] The biaxially oriented polyester film of the present invention must have a resin layer (hereinafter referred to as layer A) as the outermost layer on at least one side, and layer A must be laminated in contact with layer B, which is mainly composed of polyester resin. Layer A can be provided by applying a coating composition for layer A to a substrate film containing layer B. In the film of the present invention, the surface layer is a layer that is present on at least one air side of the film. Furthermore, layer B, which is mainly composed of polyester, refers to a layer that contains 60% by mass or more of polyester in 100% by mass of the layer.

[0018] Layer A of the present invention preferably contains a binder resin, since this can improve adhesion with layer B and the printed layer. The binder resin preferably contains one or more types selected from the group consisting of epoxy resins, melamine resins, oxazoline compounds, carbodiimide compounds, polyester resins, acrylic resins, urethane resins, and polyamide resins.

[0019] The polyester resin that can be used as the binder resin is one having an ester bond in the main chain or side chain, and is preferably one obtained by polycondensation of a dicarboxylic acid and a diol.

[0020] As the dicarboxylic acid raw material of the polyester resin, aromatic, aliphatic, and alicyclic dicarboxylic acids can be used. As the aromatic dicarboxylic acid, terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 2,5-dimethylterephthalic acid, 1,4-naphthalenedicarboxylic acid, biphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,2-bisphenoxyethane-p-p'-dicarboxylic acid, phenylindanedicarboxylic acid, and the like can be used. As the aliphatic and alicyclic dicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, dimer acid, 1,3-cyclopentanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and the like, and their ester-forming derivatives can be used.

[0021] Diol components that are raw materials for the polyester resin include ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2,4-dimethyl-2-ethylhexane-1,3-diol, neopentyl glycol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2-isobutyl-1, 3-propanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 4,4'-thiodiphenol, bisphenol A, 4,4'-methylenediphenol, 4,4'-(2-norbornylidene)diphenol, 4,4'-dihydroxybiphenol, o-, m-, and p-dihydroxybenzene, 4,'-isopropylidenephenol, 4,4'-isopropylidenebindiol, cyclopentane-1,2-diol, cyclohexane-1,2'-diol, cyclohexane-1,2-diol, cyclohexane-1,4-diol, and the like can be used.

[0022] Furthermore, as the polyester resin, it is also possible to use modified polyester copolymers, for example, block copolymers and graft copolymers modified with acrylic, urethane, epoxy, or the like.

[0023] The acrylic resin that can be used as the binder resin is not particularly limited, but is preferably composed of an alkyl methacrylate and / or an alkyl acrylate.

[0024] As the alkyl methacrylate and / or alkyl acrylate, it is preferable to use methacrylic acid, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, acrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate, maleic acid, itaconic acid, acrylamide, N-methylolacrylamide, diacetoneacrylamide, etc. These can be used alone or in combination of two or more.

[0025] Examples of epoxy resins that can be used as binder resins include sorbitol polyglycidyl ether-based crosslinking agents, polyglycerol polyglycidyl ether-based crosslinking agents, diglycerol polyglycidyl ether-based crosslinking agents, and polyethylene glycol diglycidyl ether-based crosslinking agents. As epoxy resins, commercially available ones may be used, for example, epoxy compounds "Denacol" (registered trademark) EX-611, EX-614, EX-614B, EX-512, EX-521, EX-421, EX-313, EX-810, EX-830, EX-850, etc., manufactured by Nagase Chemtec Corporation, diepoxy / polyepoxy compounds (SR-EG, SR-8EG, SR-GLG, etc.) manufactured by Sakamoto Pharmaceutical Co., Ltd., epoxy crosslinking agents "EPICLON" (registered trademark) EM-85-75W or CR-5L, etc., manufactured by Dainippon Ink Mfg. Co., Ltd., and among them, those having water solubility are preferably used.

[0026] Examples of melamine resins that can be used as binder resins include melamine, methylolated melamine derivatives obtained by condensing melamine with formaldehyde, compounds obtained by reacting methylolated melamine with lower alcohols to partially or completely etherify them, and mixtures thereof. The melamine resin may be any of condensates consisting of monomers or dimers or higher, or mixtures thereof. Examples of lower alcohols that can be used for etherification include methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, and isobutanol. Examples of functional groups include those having an imino group, a methylol group, or an alkoxymethyl group such as a methoxymethyl group or a butoxymethyl group in one molecule, such as imino group-type methylated melamine resin, methylol group-type methylated melamine resin, methylol group-type methylated melamine resin, and fully alkylated methylated melamine resin. Among these, methylolated melamine resin is most preferably used.

[0027] The oxazoline compound that can be used as the binder resin has an oxazoline group as a functional group in the compound, and is preferably an oxazoline group-containing copolymer obtained by copolymerizing at least one monomer containing an oxazoline group and at least one other monomer. As the monomer containing an oxazoline group, 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline can be used, and one or a mixture of two or more of these can also be used. Among them, 2-isopropenyl-2-oxazoline is suitable because it is easily available industrially.

[0028] In the oxazoline compound, at least one other monomer used for the monomer containing an oxazoline group is a monomer copolymerizable with the monomer containing an oxazoline group, and examples thereof include acrylic acid esters or methacrylic acid esters such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, and 2-ethylhexyl methacrylate, unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, and maleic acid, unsaturated nitriles such as acrylonitrile and methacrylonitrile, unsaturated amides such as acrylamide, methacrylamide, N-methylol acrylamide, and N-methylol methacrylamide, vinyl esters such as vinyl acetate and vinyl propionate, vinyl ethers such as methyl vinyl ether and ethyl vinyl ether, olefins such as ethylene and propylene, halogen-containing α,β-unsaturated monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride, and α-unsaturated monomers such as styrene and α-methylstyrene. , β-unsaturated aromatic monomers, etc. can be used, and these can be used alone or in combination of two or more kinds.

[0029] The carbodiimide compound that can be used as the binder resin is a compound having one or more carbodiimide groups or cyanamide groups in a tautomeric relationship therewith as functional groups in the molecule. Specific examples of such carbodiimide compounds include dicyclohexylmethanecarbodiimide, dicyclohexylcarbodiimide, tetramethylxylylenecarbodiimide, and urea-modified carbodiimide, and these can be used alone or in a mixture of two or more kinds.

[0030] The urethane resin that can be used as the binder resin is preferably a resin obtained by reacting a polyhydroxy compound with a polyisocyanate compound by a known urethane resin polymerization method such as emulsion polymerization or suspension polymerization.

[0031] Examples of polyhydroxy compounds include polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene glycol, hexamethylene glycol, tetramethylene glycol, 1,5-pentanediol, diethylene glycol, triethylene glycol, polycaprolactone, polyhexamethylene adipate, polyhexamethylene sebacate, polytetramethylene adipate, polytetramethylene sebacate, trimethylolpropane, trimethylolethane, pentaerythritol, polycarbonate diol, and glycerin.

[0032] Examples of the polyisocyanate compound that can be used include hexamethylene diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, isophorone diisocyanate, an adduct of tolylene diisocyanate and trimethylenepropane, and an adduct of hexamethylene diisocyanate and trimethylolethane.

[0033] Furthermore, the A layer of the film of the present invention may contain an isocyanate compound as a resin or compound. Examples of the isocyanate compound include tolylene diisocyanate, diphenylmethane-4,4'-diisocyanate, metaxylylene diisocyanate, hexamethylene-1,6-diisocyanate, 1,6-diisocyanatehexane, an adduct of tolylene diisocyanate and hexanetriol, an adduct of tolylene diisocyanate and trimethylolpropane, polyol-modified diphenylmethane-4,4'-diisocyanate, carbodiimide-modified diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, 3,3'-bitrylene-4,4' diisocyanate, 3,3'dimethyldiphenylmethane-4,4'-diisocyanate, and metaphenylene diisocyanate.

[0034] Furthermore, since isocyanate groups easily react with water, in terms of the pot life of the coating material, it is preferable to use blocked isocyanate compounds in which the isocyanate groups are masked with a blocking agent, etc. In this case, when heat is applied in the drying process after the coating composition is applied to the polyester film, the blocking agent is dissociated and the isocyanate groups are exposed, which causes the crosslinking reaction to proceed.

[0035] The polyamide resin that can be used as the binder resin is preferably a polymer having a heterocyclic amine skeleton in the main chain. The polyamide resin may have a substituent at any position in the main chain or side chain, or may have a substituent at any position in the heterocyclic amine skeleton such as piperazine, pyridine, imidazole or carbazole. When the polyamide resin has a piperazine skeleton in the main chain, it is preferable that the piperazine skeleton is present between the carbonyl groups of the main chain, and the nitrogen in the heterocycle of the piperazine skeleton and the carbonyl group form an amide bond. When the polyamide resin has another heterocyclic amine skeleton having two or more primary or secondary amino groups such as a pyridine, imidazole or carbazole skeleton in the main chain, it is also preferable that the heterocyclic amine skeleton is present between the carbonyl groups.

[0036] When the polyamide resin used as the binder resin of the present invention has a piperazine skeleton, the piperazine skeleton may be directly bonded to the carbon linking the amide group, or the piperazine skeleton may be bonded via an alkyl group or an amino group.When the polyamide resin has a heterocyclic amine skeleton other than the piperazine skeleton, such as a pyridine, imidazole or carbazole skeleton, the heterocyclic amine skeleton such as a pyridine, imidazole or carbazole skeleton may be directly bonded to the carbon linking the amide group, or the heterocyclic amine skeleton such as a pyridine, imidazole or carbazole skeleton may be bonded via an alkyl group or an amino group.

[0037] The polyamide resin used as the binder resin of the present invention is preferably a polymer having a piperazine skeleton in the main chain or side chain, more preferably a polymer having a piperazine skeleton in the main chain. The polyamide having a piperazine skeleton in the main chain used in the present invention is preferably obtained by a polycondensation reaction between an amine having a piperazine skeleton and a dicarboxylic acid.

[0038] Preferred examples of amines having a piperazine skeleton include piperazine, aminomethylpiperazine, aminoethylpiperazine, aminopropylpiperazine, aminobutylpiperazine, 1,4-bis(aminomethyl)piperazine, 1,4-bis(2-aminoethyl)piperazine, 1,4-bis(3-aminopropyl)piperazine, and 1,4-bis(4-aminobutyl)piperazine. Among these, aminoethylpiperazine and 1,4-bis(3-aminopropyl)piperazine are more preferred. In addition, these amines may have a substituent at any position other than the nitrogen that can form an amide bond.

[0039] Preferred examples of dicarboxylic acids include 1H-imidazole-2,4-dicarboxylic acid, 1H-imidazole-2,5-dicarboxylic acid, 1H-imidazole-4,5-dicarboxylic acid, pyridine-2,3-dicarboxylic acid, pyridine-2,4-dicarboxylic acid, pyridine-2,5-dicarboxylic acid, pyridine-2,6-dicarboxylic acid, pyridine-3,4-dicarboxylic acid, pyridine-3,5-dicarboxylic acid, adipic acid, sebacic acid, dodecadicarboxylic acid, terephthalic acid, isophthalic acid, etc. Furthermore, these dicarboxylic acids may have a substituent at any position other than the carboxyl group capable of forming an amide bond.

[0040] The polyamide resin used as the binder resin in the present invention can be preferably a polyamide obtained by combining the above-mentioned amine and dicarboxylic acid, and a polyamide obtained by combining aminoethylpiperazine and adipic acid is particularly preferred.

[0041] The polyamide resin used as the binder resin of the present invention may have a polyalkylene glycol structure in the main chain. Specific examples thereof include polyamides having a skeleton of aminoethylpiperazine, adipic acid, and bisaminopropylpolyethylene glycol.

[0042] The polyamide resin used as the binder resin in the present invention may be a mixture or copolymer of a polyamide having a piperazine, pyridine, imidazole or carbazole skeleton with another polymer. In this case, specific examples of other polymers include polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polypentamethylene adipamide (nylon 5 6), polypentamethylene sebacamide (nylon 510), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (nylon 66 / 6 T), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 6I), polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 6T / 6 I), polyxylylene adipamide (nylon XD6), etc.

[0043] The biaxially oriented polyester film of the present invention must have a kurtosis Sku measured on the surface of the A layer side of 20 or more and 250 or less. Sku is a parameter related to the tip shape of the peaks and valleys in the surface roughness height distribution curve, and is generally 3 when the surface roughness height distribution curve is a normal distribution, and when it is less than 3, the distribution is gradual and has a short tail, and when it is more than 3, the distribution is steep and has a long tail. Sku is an extension of the definition of kurtosis in JIS B0601-2013 to a three-dimensional parameter, and is obtained by the method described in the examples. The biaxially oriented polyester film of the present invention has an Sku of 20 or more, so that it can have sharp and uniform protrusion shapes and a smooth base surface shape in parallel, and can achieve both blocking resistance and easy adhesion after deep sand mat processing. In particular, even when the resin layer is locally scraped off to an uneven shape during deep sand mat processing, the remaining amount of the resin layer can be averaged by having a flat area with a longer tail, and easy adhesion failure after sand mat processing can be suppressed in some cases. In addition, by having Sku of 250 or less, local concentration of load and friction load on the protrusions is reduced, and the phenomenon in which the protrusions fall off during transportation in the film forming process and processing process, causing frequent scratches, can be suppressed. In addition, in a design with a large thickness of the A layer, which is a feature of the present invention, the absolute value of the film thickness unevenness is likely to become large, and in particular, in an extremely flat surface with Sku exceeding 250, there may be cases where adhesion failure after sand matting occurs due to local film thickness unevenness. Sku is more preferably 40 to 235, and most preferably 60 to 220. Methods for setting Sku within the above specific range include a method in which large diameter particles are sparsely included, but it is preferable to carry out the following methods in combination. (i) The balance between the average particle size of the particles contained in layer A and the thickness of layer A is within a specific range described below. (ii) The solids concentration of the A layer resin composition solution before drying and curing is set to a specific viscosity region of 6.0 to 15.0 mass %. (iii) In the in-line coating method described below, the wet thickness reduction rate in the section from application of the A layer resin composition solution to the start of stretching is 0.5 μm / sec or more and 8.0 μm / sec or less.

[0044] The thickness of the A layer of the biaxially oriented polyester film of the present invention must be 150 nm or more and 400 nm or less. By setting the thickness of the A layer in the above range, the numerical range of the Sku can be realized, and both the suppression of blocking and the easy adhesion after sand matting can be achieved. If the thickness of the A layer is less than 150 nm, the resin layer may not remain sufficiently after deep sand matting, resulting in insufficient easy adhesion. If the thickness of the A layer is greater than 400 nm, the particles are buried, making it difficult to satisfy the numerical value of the Sku, and in the in-line coating method described below, the film thickness unevenness due to stretching may become large. The thickness of the A layer is more preferably 170 nm or more and 380 nm or less, and most preferably 180 nm or more and 360 nm or less.

[0045] In order to control the Sku within a specific range, the A layer of the biaxially oriented polyester film of the present invention contains inorganic and / or resin particles, and the content is preferably 0.15 to 3.0 mass% based on the total solid mass in the coating composition. The average particle size of the particles is preferably 0.30 μm or more and 1.00 μm or less, and most preferably 0.45 μm or more and 0.85 μm or less. If the average particle size of the particles is less than 0.30 μm or more and more than 1.00, it may be difficult to satisfy the Sku.

[0046] In the A layer of the biaxially oriented polyester film of the present invention, the difference between the average particle size of the particles contained in the A layer and the thickness of the A layer is preferably 100 nm or more and 500 nm or less. If the difference between the average particle size of the particles contained in the A layer and the thickness of the A layer is less than 100 nm, the particles may fall off during the process and the film may be easily scratched, and if it is more than 500 nm, blocking may worsen, and in either case, it may be difficult to set the Sku value to the preferred range characteristic of the present application. It is more preferable that the difference between the average particle size of the particles contained in the A layer and the thickness of the A layer is 200 nm or more and 400 nm or less.

[0047] The particles contained in the layer A of the present invention are preferably inorganic particles such as silica, alumina, kaolin, calcium carbonate, titanium oxide, calcium phosphate, barium sulfate, silicon oxide, aluminum oxide, magnesium oxide, talc, clay, mica, zirconia, and aluminosilicate particles, and resin particles such as crosslinked polystyrene particles, acrylic particles, and polyester particles. From the viewpoint that the particles fall off and are unlikely to remain on the outermost surface when the film surface is scraped by sand mat processing, resin particles are preferred because they have lower adhesion to the binder resin of the layer A than inorganic particles, and non-polar crosslinked polystyrene particles are particularly preferred. When the film surface is scraped by sand mat processing, the particles fall off, partially exposing the base layer, and the adhesion to the printing layer can be further improved.

[0048] Furthermore, within the scope of the present invention, layer A may contain, as necessary, an antifoaming agent, a release agent, a coatability improving agent, a thickener, an organic lubricant, an antistatic agent, an antioxidant, an ultraviolet absorber, a foaming agent, a dye, etc.

[0049] The biaxially oriented polyester film of the present invention preferably has a surface crystallinity of 0.70 or more and less than 1.10 as determined by ATR-IR measured on the A layer side. If the surface crystallinity is less than 0.70, the amorphousness near the film surface layer is excessive, and while the adhesion after sand matting is improved, the quality aspects such as scratches and thickness unevenness during film formation and processing and transportation may deteriorate. In addition, if the surface crystallinity is 1.10 or more, the crystallization near the film surface layer is excessive, and the adhesion with the printing layer after sand matting may be insufficient. The surface crystallinity is determined by the method described in the examples. The method for making the surface crystallinity into the specific range is not particularly limited, but examples include a method in which the A layer is provided and a B layer mainly composed of biaxially oriented polyester is provided adjacent to the A layer.

[0050] The thickness of the B layer of the biaxially oriented polyester film of the present invention is preferably 0.5 μm or more and 4.0 μm or less. If the thickness is less than 0.5 μm, the B layer may be scraped off after deep sand mat processing, and the desired adhesiveness of the present invention may not be fully realized. If the thickness is more than 4.0 μm, curling may become an issue during processing and transportation or when used as a label.

[0051] The B layer of the biaxially oriented polyester film of the present invention is mainly composed of biaxially oriented polyester, and preferably contains 80 mol% or more and less than 95 mol% of ethylene glycol component as glycol component in the polyester in the B layer, 5 mol% or more and less than 20 mol% of at least one of diethylene glycol component, 1,4-cyclohexanedimethanol component, and neopentyl glycol component, and 90 mol% or more of terephthalic acid component as dicarboxylic acid component. More preferably, the glycol component contains 85 mol% or more and less than 95 mol% of ethylene glycol component, 5 mol% or more and less than 15 mol% of at least one of diethylene glycol component, 1,4-cyclohexanedimethanol component, and neopentyl glycol component, and 95 mol% or more of terephthalic acid component as dicarboxylic acid component, and more preferably, 98 mol% or more of the dicarboxylic acid component among the above glycol components is terephthalic acid component. By using such composition, the surface crystallinity measured from the A layer side can be controlled to a preferred range.

[0052] The surface crystallinity determined by ATR-IR measured on the A layer side of the biaxially oriented polyester film of the present invention is a parameter reflecting the higher-order structure of each resin in both A layer and B layer, and is particularly strongly affected by B layer, whose orientation state varies greatly under biaxial stretching conditions. By making B layer have the above composition, biaxial orientation by stretching is moderate, which contributes to the easy adhesion after sand matting, which is the objective of the present application, but it is preferably used from the viewpoint of further improving this characteristic to provide an orientation relaxation process by high-temperature stretching of 135°C or more in the biaxial stretching process described below.

[0053] The biaxially oriented polyester film of the present invention preferably has a curl amount measured at 23°C of 0.2 mm to 3.0 mm. If the curl amount is greater than 3.0 mm, a process defect may occur in which the film end portion rises during processing and transport, and if the curl amount is less than 0.2 mm, curling to the opposite side may occur during processing of the opposite side after sand mat processing. The curl amount is determined by the method described in the examples. The method for setting the curl amount within the specific range is not particularly limited, but examples include a method of performing a relaxation heat treatment at a temperature 20°C to 60°C lower than the heating crystallization temperature Tcc of the B layer to fix the amorphous structure.

[0054] Next, a preferred embodiment of the method for producing the biaxially oriented polyester film of the present invention will be described. The film of the present invention is not limited to that obtained by the following production method. Preferred methods for forming a laminated structure of an A layer and a biaxially oriented B layer include a method of co-extruding two or more kinds of raw materials and laminating them, a method of bonding two or more kinds of films together, an in-line coating method, an off-coating method, etc. Among them, in consideration of productivity, the in-line coating method is the most suitable.

[0055] Here, the in-line coating method is a method of coating within the manufacturing process of the base film. When a polyester film is used as the base film, it is preferable to manufacture the base film by a manufacturing method in which a coating composition is applied to at least one surface layer of the polyester film before the crystal orientation is completed, and then the polyester film is stretched at least in one axial direction and then heat-treated to complete the crystal orientation of the polyester film. In addition, the off-coating method is a method of forming the base film by applying the above-mentioned coating composition to at least one surface layer of the polyester film after the manufacturing is completed, followed by drying and curing. The method of applying the resin composition to the base film can be any known coating method. For example, a wire bar coating method, a reverse coating method, a gravure coating method, a die coating method, a blade coating method, a dip coating method, an air knife coating method, a curtain coating method, a roller coating method, and the like can be mentioned.

[0056] In the present invention, it is preferable to form a surface layer by applying a coating composition to at least one side of a polyester film that is a base film, and then drying the coating composition. In the present invention, when a solvent is contained in the coating composition, it is preferable to use an aqueous solvent as the solvent. By using an aqueous solvent, it is possible to suppress rapid evaporation of the solvent in the drying process, and not only can a uniform resin layer be formed, but also it is excellent in terms of environmental load.

[0057] Here, the aqueous solvent refers to water or a mixture of water and a water-soluble organic solvent, such as alcohols (e.g., methanol, ethanol, isopropyl alcohol, butanol, etc.), ketones (e.g., acetone, methyl ethyl ketone, etc.), or glycols (e.g., ethylene glycol, diethylene glycol, propylene glycol, etc.), in any ratio.

[0058] The method of applying the coating composition to the film is not particularly limited, but as mentioned above, it is preferably an in-line coating method. Specifically, it refers to a method of applying the coating at any stage from melt extrusion of the polyester resin to biaxial stretching, heat treatment, and winding up, and is usually applied to any of the following films: an unstretched (unoriented) film (A film) in a substantially amorphous state obtained by melt extrusion and rapid cooling, a uniaxially stretched (uniaxially oriented) film (B film) that is subsequently stretched in the longitudinal or width direction, or a biaxially stretched (biaxially oriented) film (C film) that is further stretched in the width direction or longitudinal direction and before heat treatment.

[0059] In the present invention, it is preferable to adopt a method in which a coating composition is applied to either the above-mentioned film A or film B before the crystal orientation is completed, and then the film is stretched in a uniaxial or biaxial direction and heat-treated at a temperature higher than the boiling point of the solvent to complete the crystal orientation of the film and provide a resin layer. This method has the advantage of being able to simultaneously perform film formation and the coating and drying of the coating composition (i.e., the formation of the resin layer), and therefore has the advantage in terms of production costs.

[0060] Among these, the method of applying the coating composition to a film (B film) uniaxially stretched in the longitudinal direction, then stretching in the transverse direction and heat treating is superior. In this method, compared to the method of applying the coating composition to an unstretched film and then biaxially stretching, there is one less stretching step after applying the coating composition, so defects and cracks in the resin layer due to stretching are less likely to occur, and a surface layer with excellent smoothness can be formed. In addition, as mentioned above, by applying the coating composition to a film before the completion of crystal orientation, adhesion between the surface layer and the film can be imparted.

[0061] Therefore, the preferred method for forming the surface layer in the present invention is to apply a coating composition using an aqueous solvent onto the base film by in-line coating, followed by drying and heat treatment, and more preferably to in-line coat the coating composition onto the uniaxially stretched B film.

[0062] Next, the method for producing the film of the present invention will be described by taking a polyester film as an example, but the present invention should not be construed as being limited to this example.

[0063] The raw materials used are vacuum dried to a moisture content of 50 ppm or less, and then fed to a single-screw extruder for melt extrusion. At this time, it is preferable to control the resin temperature to 265°C to 295°C. In addition, in a composite film-forming device having at least two single-screw or twin-screw extruders, or a main extruder and a sub-extruder, the resin that is the raw material for layer B is fed to the main extruder, and the resin that is the raw material for layer A is fed to the sub-extruder, and melt extrusion is performed, and a laminated film such as A / B or A / B / A can be formed, for example, by a feed block or multi-manifold installed above a die (T-die) having two extruders and a linear lip. Thereafter, the film is in close contact with a cooled drum and cooled and solidified to produce an unstretched (unoriented) PET film (A film). This film is heated to a temperature above the glass transition temperature (Tg) of the polymer by infrared heating or the like as necessary, and stretched in the longitudinal direction (hereinafter referred to as MD) (MD stretching). In the case of sequential biaxial stretching, MD stretching is performed by utilizing the peripheral speed difference between two or more rolls. The MD stretching ratio is preferably 1.5 to 6.0 times. By setting it to 1.5 times or more, more preferably 2.0 times or more, and even more preferably 2.8 times or more, a film with small thickness unevenness within a practical range can be obtained. By setting it to 6.0 times or less, more preferably 4.0 times or less, the occurrence of breakage during film formation can be prevented. In addition, the MD stretching temperature is preferably from Tg of the film to Tg+20°C from the viewpoint of uniform stretching and suppression of roll adhesion. In addition, the stretching speed is preferably from 1,000% / min to 200,000% / min.

[0064] When a resin layer is further provided on the PET film, a coating composition prepared to a predetermined concentration may be applied to one side of the B film, and further, the coating surface of the PET film may be subjected to a surface treatment such as a corona discharge treatment before coating. By performing a surface treatment such as a corona discharge treatment, the wettability of the resin composition to the PET film can be improved, the resin composition can be prevented from repelling, and a uniform coating thickness can be achieved.

[0065] Here, in order to control the Sku of the biaxially oriented polyester film of the present invention within the above-mentioned preferred range, the solid content concentration of the coating composition is preferably 6% by mass or more and 15% by mass or less. If the solid content concentration is less than 6% by mass, the viscosity of the coating composition is low, and the particles of the A layer aggregate or settle before curing, resulting in a form different from the desired surface shape, which may make it difficult to set the Sku within the preferred range. In addition, if the solid content concentration is more than 15% by mass, the viscosity of the coating composition may become excessive, resulting in a large variation in Sku. The solid content concentration represents the ratio of the mass of the coating composition to the mass of the coating composition minus the mass of the solvent (i.e., [solid content concentration (mass%)] = [(mass of coating composition) - (mass of solvent)] / [mass of coating composition] × 100).

[0066] In addition, for the purpose of controlling the Sku of the biaxially oriented polyester film of the present invention within the above-mentioned preferred range, when the coating composition is applied to the B film and then stretched, it is preferable that the wet thickness reduction rate in the coating-stretching start section is 0.5 μm / sec or more and 8.0 μm / sec or less. If the wet thickness reduction rate in the coating-stretching start section is less than 0.5 μm / sec, the particles in the coating composition may aggregate or settle during the drying process, resulting in a form different from the desired surface shape, making it difficult to set the Sku within the preferred range. If the wet thickness reduction rate in the coating-stretching start section is greater than 8.0 μm / sec, the particle concentration in the thickness direction of the A layer is likely to be non-uniform, and similarly, it is difficult to realize the surface shape as designed, and it may be difficult to control the Sku within the preferred range. The wet thickness reduction rate in the coating-stretching start section is more preferably 1.0 μm / sec or more and 7.0 μm / sec or less, and most preferably 1.5 μm / sec or more and 6.5 μm / sec or less. The rate of decrease in wet thickness in the section from coating to the start of stretching can be adjusted by setting the drying temperature, the length of the drying section, the line speed, and the thickness of layer A or the entire film.

[0067] After the MD stretching, the film can be stretched in a direction perpendicular to the MD (hereinafter referred to as TD stretching) and then heat-set and heat-relaxed in order to obtain a biaxially oriented film. These processes are performed while the film is running. At this time, the preheating and stretching temperature for TD stretching is preferably Tg or higher and Tg+50°C or lower with respect to the glass transition temperature Tg of the polymer. The TD stretching ratio is preferably 2.5 to 6.0 times. By setting the ratio to 2.5 times or higher, more preferably 3.0 times or higher, the mechanical properties and heat resistance required for processing and use as a printed label, which is the final application, can be made sufficient. By setting the ratio to 6.0 times or lower, more preferably 4.0 times or lower, it is possible to suppress the occurrence of breakage during film formation and achieve high productivity by forming a wide film all at once. In addition, the stretching speed in the TD direction is preferably 1,000% / min or higher and 200,000% / min or lower.

[0068] In the biaxially oriented polyester of the present invention, in order to control the orientation and crystalline state of the polyester in the base film and improve the easy adhesion after sand mat processing, it is preferable to provide an orientation relaxation process in which the final temperature in the TD stretching is in the range of 135 ° C. or more and 150 ° C. or less. If the final temperature in the TD stretching is less than 135 ° C., the orientation relaxation is insufficient, and if it is higher than 150 ° C., crystallization proceeds too much, so in either case, it may be difficult to control the surface crystallinity measured by the ATR-IR method to a preferred range. The final temperature in the TD stretching is more preferably 140 ° C. or more and 150 ° C. or less. By applying this stretching condition, the surface crystallinity measured by the ATR-IR method can be set to a preferred range, especially in a polyester system in which the polyester resin of the B layer is a glycol component of the specific composition, but the effect may not be sufficient in a highly crystalline polyester composition such as homo-PET.

[0069] Furthermore, the film is heat-treated after the biaxial stretching. The film is introduced into a heat treatment zone (heat setting zone) at 180 to 240°C and heat-treated for 1 to 60 seconds to complete the crystal orientation. In this heat treatment step (heat setting step), a relaxation treatment of 1 to 15% may be performed in the width direction or the length direction as necessary. In addition, slight stretching in the width direction or the length direction at a ratio of 0.1% to 10% is also an effective method for improving the uniformity of physical properties in the width direction. The heat treatment can be performed by any conventionally known method, such as in an oven or on a heated roll.

[0070] Then, the film is uniformly cooled, cooled to room temperature, and wound on a roll. In this process, it is preferable to perform a relaxation heat treatment for 1 to 10 seconds at a temperature 20 to 60°C lower than the heating crystallization temperature Tcc of the B layer. The high-temperature heat treatment process is a process that involves crystallization, but in order to improve the easy adhesion after sand mat processing, it is ideal to relax the orientation by high-temperature heat treatment while suppressing crystallization. As a result of intensive research by the inventors, it was found that a more effective orientation relaxation process is a slow cooling condition in which the film is exposed to a temperature near the stretching temperature and below the heating crystallization temperature Tcc for a certain period of time. The temperature condition may give more preferable results if it is a temperature 30 to 50°C lower than the heating crystallization temperature Tcc.

[0071] Here, the case where stretching is performed by the sequential biaxial stretching method has been described in detail as an example, but either the sequential biaxial stretching method or the simultaneous biaxial stretching method may be adopted.

[0072] In addition, to the extent that the effects of the present invention are not impaired, various coating liquids may be applied to the surface of at least one of the layers A using known techniques in order to impart lubricity, antistatic properties, ultraviolet light absorption performance, etc., or a hard coat layer may be provided to enhance impact resistance. The coating may be applied during film production (in-line coating) or may be applied to the biaxially oriented polyester film after film production (off-line coating).

[0073] The biaxially oriented polyester film of the present invention can be suitably used as a label characterized by low gloss design by subjecting the surface to a matte treatment. In particular, even after dense matte treatment with a 60° gloss of 5 or less, the film has good adhesion and can achieve both high ink adhesion and design, and can be suitably used as a biaxially oriented polyester film for matte treatment, and more suitably used as a biaxially oriented polyester film for matte treatment with a 60° gloss of 5 or less. In addition, the biaxially oriented polyester film of the present invention has excellent blocking and slip properties, and achieves both printing adhesion after deep sand matte treatment, and can be suitably used as a biaxially oriented polyester film for sand matte, and more suitably used as a sand matte biaxially oriented polyester film for printing.

[0074] In the sand matte film obtained by subjecting the biaxially oriented polyester film of the present invention to a sand matte treatment, the B layer is partially exposed to the outermost surface, and the ratio of the exposed portion is preferably 0.5% or more and 10.0% or less. The ratio of the exposed portion is determined by the method described in the Examples. By the B layer being exposed to the outermost surface, the easy adhesion due to the B layer having a controlled orientation structure in the biaxial stretching process is expressed, and the adhesion to a wide range of inks can be improved by combining the easy adhesion of the A layer. The ratio of the B layer being exposed to the outermost surface is more preferably 1.5% or more and 8.0% or less. If the ratio of the B layer being exposed to the outermost surface is less than 0.5%, the easy adhesion characteristic derived from the B layer may be insufficient, and if it is higher than 10.0%, the easy adhesion characteristic derived from the A layer may be insufficient. In other words, a preferred embodiment of the method for producing a sand matte film of the present invention is a method for producing a sand matte film including a step of subjecting the biaxially oriented polyester film to a sand matte treatment, in which the B layer is exposed at a ratio of 0.5% or more and 10.0% or less. Furthermore, since printing on such a sand-matte film provides high design properties and easy adhesion, a preferred embodiment of the method for producing a printed label of the present invention is a method for producing a printed label comprising a sand-matte film that has been sand-matted so that the B layer is exposed to a ratio of 0.5% to 10.0% of the biaxially oriented polyester film, and a printing layer, wherein the printing layer is in contact with both the A layer and the B layer. EXAMPLES

[0075] The present invention will be described in detail below with reference to examples. The respective property values ​​were measured by the following methods.

[0076] (1) Film thickness and film layer structure Five cross sections were cut out from the center of the film in the width direction and observed using a scanning electron microscope (Hitachi Field Emission Scanning Electron Microscope (FE-SEM) S-4000) at magnifications of 500 to 5,000 times so that the entire thickness of the film was within the field of view. The cross-sectional photographs taken were used to determine the film thickness and, in the case of a layered structure, the film layer structure (thickness of each layer).

[0077] (2) Resin composition The film was dissolved in hexafluoroisopropanol (HFIP), 1 H-NMR and 13 The content of each monomer residue component and by-product diethylene glycol can be quantified using C-NMR. In the case of a laminated film, each layer of the film can be scraped off depending on the laminate thickness to sample and evaluate the components constituting each layer alone. For the film of the present invention, the resin composition was calculated from the mixing ratio at the time of film production.

[0078] (3) Resin layer (A layer) thickness The film was stained with RuO4 and / or OsO4. Next, the film was frozen and cut in the film thickness direction to obtain 10 ultrathin slice samples for observing the cross section of the resin layer. The cross section of each sample was observed at 10,000 to 1,000,000 magnifications with a TEM (transmission electron microscope: H7100FA type manufactured by Hitachi, Ltd.) to obtain a cross-sectional photograph. The measured values ​​of the resin layer thickness of the 10 samples were averaged to obtain the resin layer thickness of the film.

[0079] (4) Solid content in the coating composition An appropriate amount of the coating composition was weighed out and heated at 150° C. until the mass of the remaining matter (solid content) reached a constant weight, and the solid content was calculated.

[0080] (5) Sku on the surface of layer A Measurements were performed using a three-dimensional surface roughness meter (ET4000AK, manufactured by Kosaka Laboratory) under the following conditions in accordance with JIS B0601-2013 using the three-dimensional stylus method. Needle diameter 2 (μmR) Stylus pressure 10(mg) Measurement length 500(μm) Vertical magnification: 20000 (times) CUTOFF 250(μm) Speed ​​100(μm / s) Measurement interval 5(μm) Record number: 80 Hysteresis width ±6.25(nm) Reference area 0.1(mm 2 ).

[0081] (6) Surface crystallinity of the A layer surface measured by ATR-IR The spectrum of the surface of Layer A was measured by the ATR method of FT-IR using the following equipment and conditions, and then the spectrum of the polyester film "Lumirror" (registered trademark) #50T60 manufactured by Toray Industries, Inc., measured in the same manner, was divided to obtain a difference spectrum.

[0082] The surface crystallinity is at 1340 cm, which corresponds to the bending vibration of the trans structure of ethylene glycol. -1 Absorption around 1410cm is independent of the structure factor of the crystal and orientation. -1 Dividing the spectral intensity of the absorption near (1340 cm -1 / 1410cm -1 ) was calculated.

[0083] If there are two or more maximum absorbance values ​​in the vicinity of the relevant wavenumber, the larger absorbance value is used for the calculation. Apparatus: Nicolet 6700 (Thermo Fisher Scientific) Light source: Ever-Glo (mid-infrared) Detector: DTGS KBr Resolution: 4cm -1 Number of times: 16 Attachment: Single reflection ATR measurement attachment (Smart iTR) ATR crystal; diamond Angle of incidence: 45°

[0084] (7) Curl amount The film was cut into a size of 150 mm x 150 mm so that the length direction and width direction of the roll were perpendicular to each other. After leaving the sample at 23°C x 65% RH (room temperature) for 24 hours, the sample was placed on a glass plate and the average height of the lifting amount at the four corners (four places) in the vertical direction from the glass plate surface was measured. The same measurement was performed at 10 different sampling locations, and the average value of all the data was adopted as the curl amount. If the direction of the film was unclear, a preliminary measurement was performed in three directions rotated 30 degrees from an arbitrary direction, and the sample was sampled in the direction with the largest curl amount among the three measurements, and the above measurement was performed.

[0085] (7-2) 60 degree gloss According to the method specified in JIS-Z-8741 (1997), the 60° specular gloss was measured with a digital variable angle glossmeter UGV-5D manufactured by Suga Test Instruments Co., Ltd., N=3, and the average value was used. For the film of the present invention, the measurement was performed on the side that had been subjected to sand matt treatment.

[0086] (7-3) Tcc of B layer The measurements were carried out using a Hitachi High-Tech Science EXSTAR DSC6220 (differential scanning calorimeter). First, about 10 mg of the B layer identified by the method described in (1) was sampled and placed in the device. The measurement sample was then heated from 25°C to 280°C at a rate of 20°C / min in a nitrogen atmosphere, held for 5 minutes, and then quenched with liquid nitrogen for 5 minutes. The sample was heated at 20°C / min, and the crystallization exothermic peak temperature (Tcc(°C)) from the glass state was detected.

[0087] (8) Sand mat processing Fine sand with a particle size of about 1 mm was supplied to the rotating blade of the shot blast (centrifugal blast), and the film was transported from roll to roll using three rotor-type sand throwers, while the sand throwing strength and transport speed were adjusted so that the 60 degree gloss level was 3 or less, and a matte finish was applied to the surface.The film was then washed with water using a high-pressure shower and dried to obtain a sand matte processed sample.

[0088] (9) Ratio of areas where layer B is exposed on the top surface A cross-sectional image was obtained at a magnification of 5000 times by the method described in (1) of a film that had been sand-matted by the method described in (8). A 30 μm-long area in the plane direction of the cross-sectional image was divided into 30 sections, and the number of sections where 30% or more of the B layer was exposed in the plane direction length on the sand-matted surface was counted and divided by 30. The same operation was performed on 15 points at different positions on the film, and the average value obtained x 100 (%) was used as the sample value.

[0089] (10) Blocking resistance The film was cut into a size of 200 cm x 200 cm. When a coating layer was applied to one side of the two cut-out films, the coating layer side and the side without the coating layer were overlapped. When a coating layer was applied to both sides of the film, the coating layers were overlapped and the two were subjected to a load of 1.5 kg / cm under an atmosphere of 60°C x 80% RH. 2 After applying this pressure for 65 hours, the peel strength is measured. The peel strength was measured using a tensile tester (Orientec Tensilon UCT-100) with an initial tensile chuck distance of 100 mm and a tensile speed of 20 mm / min, and a 180° peel test was performed. Measurements were continued until the peel length reached 130 mm (chuck distance 230 mm), and the average value of the load from a peel length of 25 mm to 125 mm was taken as the peel strength. Measurements were performed with N=3, and the average value was evaluated (g per 5 cm). Evaluation was performed based on the peel strength according to the following criteria, with A to C being considered as passing. A: Less than 2g B: 2g or more - less than 3g C: 3g or more, but less than 5g D: Over 5g - torn.

[0090] (11) Dignity The A4 cut size film was observed under fluorescent lighting and evaluated according to the following criteria, with A to C being acceptable. A: 0 scratches longer than 1cm B: 1 to 3 scratches with a length of 1 cm or more C: 4 to 9 scratches longer than 1 cm D: 10 or more scratches longer than 1 cm.

[0091] (12) Matte finish The 60 degree gloss of the sand-matted surface of the film subjected to the sand-matt treatment according to the method described in (8) was measured and evaluated according to the following criteria. A: 3.0 or less B: 4.0 or less C: 5.0 or less D: Greater than 5.0.

[0092] (13) Ink adhesion The following three types of inks were applied to the surface of the film that had been subjected to a sand matte treatment by the method described in (8) above, to a thickness of 5.0 μm using an applicator. For inks A and B, an ultraviolet lamp was used at an irradiation intensity of 80 W / cm. 2 The ink was cured at a distance of 9 cm for 5 seconds. Ink C was dried at 40°C for 30 minutes. 2 One hundred crosscuts of the above were inserted, Nichiban cellophane adhesive tape (CT405AP-24) was attached on top of them, and a rubber roller was used to roll the tape back and forth three times with a load of 19.6 N. After pressing the tape, it was peeled off in a 90° direction, and the number of remaining ink films was counted for the three types of ink. The number of remaining ink films for the ink with the smallest number was evaluated according to the following criteria, with A to C being deemed acceptable. Ink A: Jujo Chemical Co., Ltd. "Raycure" (registered trademark) SL6100 Ink B: "FLASH DRY" (registered trademark) FD MP ink M manufactured by Toyo Ink Mfg. Co., Ltd. Ink C: CAV Meiban made by Seiko Advance Co., Ltd. A:100 (passed) B:80~99(pass) C:50~79(pass) D: 0~49 (fail).

[0093] (14) Processability A film that had been sand-matted using the method described in (8) was transported from roll to roll under conditions of a roll-to-roll distance of 500 mm and a transport tension of 1.2 MPa. The amount of lift of the film end between the rolls (the vertical position of the end part based on the height of the center part of the transported film) was evaluated according to the following criteria, and A to C were deemed to be acceptable. A: No lift B: Floating is 2mm or less C: Floating is 5mm or less D: The lift is greater than 5 mm.

[0094] (raw materials) The polyester resin used had the following characteristics:

[0095] (Polyester A) 100 parts by mass of dimethyl terephthalate, 57.5 parts by mass of ethylene glycol, 0.03 parts by mass of magnesium acetate dihydrate, and 0.03 parts by mass of antimony trioxide were melted at 150°C under a nitrogen atmosphere. The melt was heated to 230°C over 3 hours while stirring, and methanol was distilled off to terminate the transesterification reaction. After the transesterification reaction was completed, an ethylene glycol solution (pH 5.0) in which 0.005 parts by mass of phosphoric acid was dissolved in 0.5 parts by mass of ethylene glycol was added. The intrinsic viscosity of the polyester composition at this time was less than 0.2. Thereafter, the polymerization reaction was carried out at a final temperature of 285°C and a vacuum degree of 0.1 Torr to obtain polyethylene terephthalate with an intrinsic viscosity of 0.65.

[0096] (Polyester B) A copolymer polyester (GN001, manufactured by Eastman Chemical Co.) in which 1,4-cyclohexanedimethanol was copolymerized at 33 mol% relative to the glycol component was used as cyclohexanedimethanol-copolymerized polyethylene terephthalate (intrinsic viscosity 0.75).

[0097] (Polyester C) A neopentyl glycol copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.75) having 100 mol % terephthalic component as a dicarboxylic acid component, 70 mol % ethylene glycol component as a glycol component, and 30 mol % neopentyl glycol component as a glycol component.

[0098] (Polyester D) An isophthalic acid copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.7) having, as the dicarboxylic acid component, 82.5 mol % of a terephthalic component, 17.5 mol % of an isophthalic component, and as the glycol component, 100 mol % of an ethylene glycol component.

[0099] (Particle Master E) When producing the polyester A, an ethylene glycol slurry of aggregated silica particles having an average particle size of 2.2 μm was added after the transesterification reaction, and then a polycondensation reaction was carried out to produce a particle master having a particle concentration of 2 mass % in the polymer.

[0100] (Resin layer forming solution) The coating materials shown below were mixed in the mass ratios and solid content concentrations shown in the table, and then diluted with pure water.

[0101] Binder resin 1 (acrylic modified polyester resin): The polyester resin component was 50 parts by mass of terephthalic acid, 50 parts by mass of isophthalic acid, 50 parts by mass of ethylene glycol, and 30 parts by mass of neopentyl glycol, together with 0.3 parts by mass of antimony trioxide and 0.3 parts by mass of zinc acetate, which were used as polymerization catalysts, in a nitrogen-purged reactor, and polymerization reaction was carried out for 12 hours at 190 to 220°C under normal pressure while removing water to obtain polyester glycol. Next, 5 parts by mass of 5-sodium sulfoisophthalic acid and xylene as a solvent were added to the obtained polyester glycol in the reactor, and polymerization was carried out for 3 hours while distilling off xylene at 260°C under a reduced pressure of 0.2 mmHg to obtain a polyester resin component. This polyester resin component was dissolved in water containing ammonia water and butyl cellulose. Next, 40 parts by mass of methyl methacrylate and 10 parts by mass of methacrylamide were added as a total of 50 parts by mass of the acrylic resin component to the aqueous dispersion containing the above-mentioned polyester resin component, so that the mass ratio of the acrylic resin component / polyester resin component was 50 / 50. Furthermore, 5 parts by mass of benzoyl peroxide was added as a polymerization initiator, and a polymerization reaction was carried out at 70 to 80° C. for 3 hours in a nitrogen-purged reactor, to obtain a coating liquid containing an acrylic-modified polyester.

[0102] Binder resin 2 (melamine resin): Cross-linked resin of methylated melamine / urea copolymer ("Nicalac" (registered trademark) "MW12LF" manufactured by Sanwa Chemical Co., Ltd.)

[0103] Binder resin 3 (polyester resin): A dispersion obtained by diluting a mixed polymer of 25 mol % terephthalic acid, 24 mol % isophthalic acid, 1 mol % 5-Na sulfoisophthalic acid, 25 mol % ethylene glycol, and 25 mol % neopentyl glycol with water to 25 mass %.

[0104] Binder resin 4 (acrylic resin): Methyl methacrylate (α), hydroxyethyl methacrylate (β), and urethane acrylate oligomer (manufactured by Negami Chemical Industries, Ltd., "Art Resin" (registered trademark) UN-3320HA, number of acryloyl groups is 6) (γ) were charged in a mass ratio of (α) / (β) / (γ)=94 / 1 / 5 in a stainless steel reaction vessel, and 2 parts by mass of sodium dodecylbenzenesulfonate was added as an emulsifier to a total of 100 parts by mass of (α) to (γ) and stirred to prepare mixed solution 1. Next, a reaction apparatus equipped with a stirrer, a reflux condenser, a thermometer, and a dropping funnel was prepared. 60 parts by mass of the above mixed solution 1, 200 parts by mass of isopropyl alcohol, and 5 parts by mass of potassium persulfate as a polymerization initiator were charged in the reaction apparatus and heated to 60°C to prepare mixed solution 2. Mixed solution 2 was kept heated at 60°C for 20 minutes. Next, mixed solution 3 consisting of 40 parts by mass of mixed solution 1, 50 parts by mass of isopropyl alcohol, and 5 parts by mass of potassium persulfate was prepared. Then, mixed solution 3 was dropped into mixed solution 2 over 2 hours using a dropping funnel to prepare mixed solution 4. Then, mixed solution 4 was heated to 60°C and held for 2 hours. After cooling the obtained mixed solution 4 to 50°C or less, it was transferred to a container equipped with a stirrer and a pressure reducing device. 60 parts by mass of 25% ammonia water and 900 parts by mass of pure water were added thereto, and isopropyl alcohol and unreacted monomers were collected under reduced pressure while heating to 60°C, and an acrylic resin dispersed in pure water was obtained.

[0105] Binder resin 4 (urethane resin): 70 parts by mass of 1,6-hexane diisocyanate as an aliphatic polyisocyanate compound, 30 parts by mass of polyisobutylene glycol as a polyol compound, 60 parts by mass of acetonitrile, and 30 parts by mass of N-methylpyrrolidone as a solvent were charged in a four-neck flask equipped with a reflux condenser, a nitrogen inlet tube, a thermometer, and a stirrer. Next, under a nitrogen atmosphere, the reaction liquid temperature was adjusted to 75 to 78°C, 0.06 parts by mass of stannous octylate was added as a reaction catalyst, and the reaction was allowed to proceed for 7 hours. Next, the reaction liquid was cooled to 30°C to obtain an isocyanate-terminated aliphatic urethane resin. Next, water was added to a reaction vessel equipped with a homodisperser capable of high-speed stirring, and the temperature was adjusted to 25°C. The isocyanate-terminated aliphatic urethane resin was added and dispersed in water while stirring and mixing at 2000 rpm. Then, a coating liquid containing a urethane resin was prepared by removing a portion of the acetonitrile and water under reduced pressure.

[0106] Inorganic particles 1: Spherical silica particles with an average particle size of 1000 nm Inorganic particles 2: Spherical silica particles with an average particle size of 700 nm Inorganic particles 3: Spherical silica particles with an average particle size of 200 nm Inorganic particles 4: Silica particles with an average particle size of 100 nm (Catalysts and Chemical Industries Co., Ltd. "Cataloid" (registered trademark)) Resin particles 1: Spherical polystyrene particles with an average particle size of 700 nm Resin particles 2: Spherical PMMA (polymethyl methacrylate) particles with an average particle size of 500 nm Resin particles 3: Spherical PMMA particles with an average particle size of 350 nm.

[0107] Example 1 The raw materials of the compositions shown in the table were vacuum dried for 6 hours at a temperature of 180° C. Then, the raw materials for layer B were fed to the main extruder, melt-extruded at a temperature of 280° C., and filtered through a 30 μm cut filter. The raw materials for layer C were fed to the sub-extruder, melt-extruded at a temperature of 290° C., and filtered through a 30 μm cut filter.

[0108] Subsequently, these molten polymers were merged in a T-die composite die so that layer B was laminated to layer C (B / C). The merged molten polymers were extruded into a sheet to form a molten sheet, which was then attached to a drum whose surface temperature was kept at 25°C by electrostatic application using a wire electrode with a diameter of 0.1 mm, and cooled and solidified to form an unstretched film.

[0109] Next, before stretching in the longitudinal direction, the film temperature was raised using a heating roll, and the film was stretched 3.3 times in the longitudinal direction at a preheating temperature of 85°C and a stretching temperature of 92°C, and then immediately cooled using a metal roll whose temperature was controlled at 40°C.

[0110] Thereafter, a corona discharge treatment was performed, and a resin layer forming solution (aqueous dispersion) having the composition shown in the table was applied onto layer B using a metalling bar to a wet thickness of 13.5 μm.

[0111] Next, the film was stretched 3.8 times in the width direction in a tenter-type transverse stretching machine at a preheating temperature of 120°C and a stretching temperature of 145°C, and then heat-treated at a temperature of 227°C at a constant length in the tenter, and then relaxed by 3% at the same temperature, and then relaxed by 2% at a temperature of 220°C. The wet thickness reduction rate in the section from application of the resin layer forming solution to the start of stretching was 2.3 μm / sec. The film was then introduced into a zone at a temperature of 150°C and heat-treated, and then cooled to room temperature to obtain a biaxially oriented polyester film with a film thickness of 50 μm. The layer formed by coating and drying was layer A.

[0112] (Examples 2 to 17, Comparative Example 3) A polyester film having a thickness of 50 μm was obtained in the same manner as in Example 1, except that the raw materials and conditions were used as shown in the table. The evaluation results of the obtained polyester film are shown in the table.

[0113] (Comparative Examples 1 and 4) The raw material of the B layer having the composition shown in the table was vacuum dried at a temperature of 180°C for 6 hours. Thereafter, the raw material of the B layer was fed to the main extruder, melt extruded at a temperature of 280°C, and then filtered through a 30 μm cut filter. Thereafter, a polyester film having a film thickness of 50 μm was obtained in the same manner as in Example 1, except that the raw materials and conditions were as shown in the table. The evaluation results of the obtained polyester film are shown in the table.

[0114] Comparative Example 2 The biaxially oriented polyester film described in Comparative Example 1 was subjected to a sand matt finish by adjusting the conditions so that the 60° gloss level was 6. The evaluation results of the obtained polyester film are shown in the table.

[0115] [Table 1]

[0116] [Table 2]

[0117] [Table 3]

[0118] [Table 4]

[0119] [Table 5] [Industrial Applicability]

[0120] According to the present invention, it is possible to obtain a biaxially oriented polyester film that combines blocking resistance, slipperiness, and print adhesion after deep sand matte treatment, a sand matte film using the same, and a printed label using the same.

Claims

1. A biaxially oriented polyester film having a resin layer (layer A) having a thickness of 150 nm or more and 400 nm or less as the outermost layer on at least one side of the polyester film, the layer A being in contact with layer B containing polyester as a main component, and having a kurtosis (Sku) measured on the surface on the layer A side of 20 or more and 250 or less.

2. 2. The biaxially oriented polyester film according to claim 1, wherein the surface crystallinity measured on the A layer side by attenuated total reflection infrared spectroscopy (ATR-IR) is 0.70 or more and less than 1.

10.

3. The biaxially oriented polyester film according to claim 1 or 2, wherein the layer A contains resin particles.

4. 3. The biaxially oriented polyester film according to claim 1, wherein the curl amount measured at 23° C. is 0.2 mm or more and 3.0 mm or less.

5. 3. The biaxially oriented polyester film according to claim 1, wherein the thickness of the layer B is 0.5 μm or more and 4.0 μm or less.

6. A method for producing a sand matte film, comprising a step of subjecting the biaxially oriented polyester film according to claim 1 or 2 to a sand matte treatment, wherein the B layer is exposed at a ratio of 0.5% to 10.0%.

7. 3. A method for producing a printed label comprising: a biaxially oriented polyester film according to claim 1 or 2, which has been subjected to a sand matte treatment so that the B layer is exposed at a ratio of 0.5% to 10.0%; and a printed layer, wherein the printed layer is in contact with both the A layer and the B layer.

Citation Information

Patent Citations

  • label

    JP1990042475A

  • Biaxially oriented polyester film

    JP2020124875A