Stretch blow molded product, toner bottle and method for producing stretch blow molded product, molded product, and pellet
By using inorganic layered double hydroxides and zeolites to adsorb wax in PET resin, the migration of wax to the inner surface of stretch blow-molded toner bottles is prevented, addressing chemical attack and ensuring image quality in electrophotographic devices.
Patent Information
- Application Number
- JP2023069974
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
AI Technical Summary
The migration of wax from recycled PET containing toner bottles to the inner surface of stretch blow-molded products causes chemical attack on toner particles, leading to development defects and density unevenness in electrophotographic images.
Incorporating inorganic layered double hydroxides and zeolites into the PET resin mixture to adsorb and prevent the migration of wax to the surface during the stretch blow molding process.
Prevents chemical attack on toner particles, maintaining image quality by suppressing wax migration and ensuring the integrity of the toner bottle.
Smart Images

Figure 2024155330000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a stretch blow molded article, a toner bottle, and a method for manufacturing a stretch blow molded article. The present disclosure also relates to a molded article and a pellet. [Background technology]
[0002] In electrophotographic image forming devices, toner bottles for supplying toner and the like need to be strong enough not to break even when dropped, so molded products made by injection stretch blow molding polyethylene terephthalate (hereinafter sometimes referred to as "PET"), a polyester resin, are often used. For example, Patent Document 1 discloses a toner bottle made by stretch blow molding.
[0003] In recent years, from the viewpoint of environmental protection, it has become common to recycle PET beverage bottles into PET bottles again. Here, as described in paragraphs
[0008] and
[0009] of Patent Document 3, chemical recycling and material recycling are known as methods for recycling PET.
[0004] Chemical recycling requires a multi-stage process as disclosed in Patent Document 2, and requires decomposition and polymerization equipment for this purpose, resulting in high recycling costs. It also places a heavy burden on the environment. On the other hand, PET obtained by material recycling (hereinafter also referred to as "material recycled PET" or "MR-PET") may have a reduced molecular weight due to hydrolysis caused by the absorption of moisture in the air by the PET resin and subsequent heating for pelletization. In addition, the time it takes for PET resin to crystallize decreases as the molecular weight decreases (Non-Patent Document 1). Furthermore, even if stretch blow molding is performed using a preform molded from low molecular weight PET, the PET rapidly crystallizes during the stretching process, making molding defects likely to occur. As a method for compensating for such shortcomings of material recycling, mechanical recycling, which adds a process of adjusting the intrinsic viscosity by repolymerization, as described in paragraph
[0010] of Patent Document 3, is known. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-042626 A [Patent Document 2] JP 2000-169623 A [Patent Document 3] JP 2014-198422 A [Non-patent literature]
[0006] [Non-Patent Document 1] Nikkan Kogyo Shimbun, Saturated Polyester Resin Handbook, edited by Kazuo Yuki, December 22, 1989, first edition, P224~P225 Summary of the Invention [Problem to be solved by the invention]
[0007] The solid-state polymerization process that repolymerizes the above-mentioned low-molecular-weight PET requires a large amount of heat energy, which places a large burden on the environment. In addition, a process of washing bottles is generally carried out in material recycling. However, bottle washing may be carried out multiple times using water, acid, alkali, etc., and a drying process is also required. Therefore, bottle washing may also increase the environmental burden. Therefore, from the viewpoint of reducing the environmental load, the present inventors simplified or omitted the washing of the toner bottles to be recycled, obtained MR-PET from the toner bottles with toner still attached inside, and used the MR-PET to manufacture toner bottles again. Then, when toner was stored in the toner bottle obtained in this way, it was found that the surface of the toner particles may be deformed at the contact point between the toner in the toner bottle and the inner surface of the toner bottle. Toner particles with deformed surfaces may cause development defects, and development defects may cause density unevenness in electrophotographic images.
[0008] The present inventors speculate as follows as to why deformation occurs on the surface of the toner contained in a toner bottle molded using MR-PET obtained from a toner bottle with toner still attached thereto. That is, it is believed that the wax contained in the toner is mixed into the toner bottle. It is believed that at least a part of the mixed wax is present on the inner surface of the toner bottle. It is believed that the toner contained in the toner bottle comes into contact with the wax exposed on the inner surface of the toner bottle, which causes the surface of the toner particles to deform. The phenomenon of deformation of the toner particle surface due to wax may be referred to as chemical attack hereinafter.
[0009] At least one aspect of the present disclosure is directed to providing a stretch blow molded article that can prevent migration of wax to the surface of the blow molded article, assuming that a polyester containing wax is used as a raw material. At least one aspect of the present disclosure is directed to providing a toner bottle that can prevent deterioration of toner contained therein. Furthermore, at least one aspect of the present disclosure is directed to providing a manufacturing method for a stretch blow molded article that can prevent migration of wax to the surface of the blow molded article, assuming that a polyester containing wax is used as a raw material. Furthermore, at least one aspect of the present disclosure is directed to providing a molded article that can prevent migration of wax to a surface, assuming that a polyester containing wax is used as a raw material. Still further, at least one aspect of the present disclosure is directed to providing pellets that contribute to suppression of migration of wax to the surface of a molded article. [Means for solving the problem]
[0010] According to at least one embodiment of the present disclosure, there is provided a stretch blow molded article comprising at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, a polyester, and a wax.
[0011] According to at least one embodiment of the present disclosure, there is provided a toner bottle, the toner bottle comprising at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, A toner bottle is provided that includes polyester and a wax.
[0012] According to at least one aspect of the present disclosure, there is provided a method for producing the stretch blow molded article, comprising the steps of: preparing a preform containing at least one selected from the group consisting of the inorganic layered double hydroxide and the zeolite, the polyester, and the wax; and There is also provided a method for producing a stretch blow molded article, comprising a molding step of stretch blow molding the preform to obtain the stretch blow molded article.
[0013] Furthermore, according to at least one embodiment of the present disclosure, there is provided a molded article, the molded article comprising at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, a polyester, and a wax.
[0014] Furthermore, according to at least one embodiment of the present disclosure, there is provided a composition comprising at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, a polyester, and a wax, Pellets are provided. Effect of the Invention
[0015] According to at least one embodiment of the present disclosure, a stretch blow molded article capable of preventing migration of the wax to the surface of the blow molded article can be obtained, on the premise that a polyester containing wax is used as a raw material. Also, according to at least one embodiment of the present disclosure, a toner bottle capable of preventing deterioration of the toner contained therein can be obtained. Furthermore, according to at least one embodiment of the present disclosure, a manufacturing method for a stretch blow molded article capable of preventing migration of the wax to the surface of the blow molded article can be obtained, on the premise that a polyester containing wax is used as a raw material. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic diagram of an image forming apparatus. [Diagram 2] FIG. 2 is a schematic diagram showing a method for molding a preform. [Diagram 3] FIG. 1 is a schematic diagram showing a blow molding method. [Figure 4] FIG. 1 is a schematic diagram of a one-stage blow molding process. [Diagram 5] FIG. 2 is a schematic diagram showing the migration of a wax component. [Figure 6] FIG. 1 is a schematic diagram of a blow bottle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, with reference to the drawings, an embodiment for carrying out the present disclosure will be described in detail by way of example. However, the scope of the present invention is not limited to the following embodiment. In this disclosure, the description "XX or more and YY or less" and "XX to YY" representing a numerical range means a numerical range including a lower limit and an upper limit, which are endpoints, unless otherwise specified, and when a numerical range is described in stages, any combination of the upper limit and the lower limit of each numerical range is also disclosed.
[0018] As mentioned above, it is believed that wax mixed into recycled polyester such as MR-PET causes chemical attacks. As shown in Figure 5, during the toner bottle molding process, when the PET resin 201 reaches or exceeds its glass transition temperature, the wax 202 migrates to the surface of the bottle. Above the glass transition temperature of the PET resin, the PET resin becomes more active in thermal motion. This causes the wax to migrate to the surface of the bottle through the gaps in the PET resin. Therefore, the present inventors recognized that it is necessary to develop a technology for obtaining a stretch-blow molded article that is unlikely to cause chemical attack on toner that comes into contact with its surface, even if the stretch-blow molded article is made from a raw material containing recycled polyester derived from toner bottles. Based on this recognition, the present inventors conducted extensive research and found that the following stretch-blow molded article is unlikely to cause chemical attack on toner that comes into contact with its surface. That is, the stretch blow molded article according to at least one embodiment of the present disclosure includes at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, a polyester, and a wax.
[0019] As a result of investigations by the present inventors, it has been found that chemical attack can be prevented by causing at least one selected from the group consisting of inorganic layered double hydroxides and zeolites to be present in a polyester containing wax. The reason for this is believed to be that at least one selected from the group consisting of inorganic layered double hydroxides and zeolites (hereinafter also referred to as zeolites, etc.) adsorbs the wax and inhibits the transfer of the wax to the surface of the toner bottle. In particular, since toner is easily charged by friction with other members, it is believed that at least a portion of the toner remaining in the toner bottle is electrically charged. The charged state of the toner is believed to be maintained even after it becomes MR-PET, and at least a portion of the wax contained in the MR-PET is also It is believed that the wax is electrically charged. Such an electrically charged wax is likely to be adsorbed by zeolite and the like.
[0020] During the process of using a toner bottle in an electrophotographic image forming apparatus, the toner is subjected to friction, and thus the toner, including the wax contained therein, is charged. The charged state is maintained even after the toner bottle is converted into MR-PET, so the wax contained in the MR-PET is usually charged. It is believed that at least one selected from the group consisting of inorganic layered double hydroxides and zeolites (hereinafter also referred to as zeolite, etc.) can ionically adsorb the charged wax, thereby suppressing the transfer of the wax to the bottle surface.
[0021] Therefore, the stretch blow molded article according to the present disclosure can be obtained by stretch blow molding a preform as a molded product molded from a resin mixture containing at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, polyester, and wax.
[0022] (Preform) The preform used in the stretch blow molding preferably contains the following (a), (b) and (c): (a) Wax (b) at least one selected from the group consisting of inorganic layered double hydroxides and zeolites; (c) Polyester Zeolite and the like are covered with a polyester skin layer during molding of the bottle precursor preform, and are therefore less likely to precipitate on the bottle surface, thus inhibiting the migration of adsorbed wax to the bottle surface, which makes it easier to prevent chemical attack by wax.
[0023] <Polyester> The polyester is not particularly limited, and a known polyester resin can be used. The polyester may be a thermoplastic polyester. The polyester preferably includes at least one selected from the group consisting of polyethylene terephthalate and polyethylene naphthalate. The polyester more preferably includes polyethylene terephthalate (PET). PET is obtained, for example, by a condensation reaction or an ester exchange reaction between terephthalic acid or an ester-forming derivative thereof and 1,2-ethanediol or an ester-forming derivative thereof. The polyester may also be a mixture with other resins. The polyester preferably contains PET in an amount of 60 to 100% by mass, more preferably 80 to 100% by mass, and even more preferably 90 to 100% by mass.
[0024] The polyester is, for example, recycled polyester. The polyester may be MR-PET, or may be virgin PET that has not undergone molecular weight reduction. However, the effect of the present disclosure is more pronounced when the polyester is MR-PET obtained by recycling toner bottles. Therefore, the polyester is preferably material recycled polyester, and more preferably material recycled PET.
[0025] The weight average molecular weight of the polyester is preferably from 20,000 to 80,000, and more preferably from 35,000 to 45,000. For example, the weight average molecular weight is measured by using gel permeation chromatography (GPC).
[0026] <Inorganic layered double hydroxide> The stretch-blow molded product, the molded product, and the pellets each contain at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite. The presence of the inorganic layered double hydroxide and the zeolite in the stretch-blow molded product, the molded product, and the pellets can be confirmed by a measurement using a microscopic FT-IR. It is possible.
[0027] Examples of inorganic layered double hydroxides include kaolin and mica, but as a compound that is more effective and easily available, there is a hydrotalcite compound represented by the following general formula (1): The inorganic layered double hydroxide preferably contains a hydrotalcite compound. General formula (1): M 2+ (1-X) M 3+ X (OH)2A n- (X / n) mH2O (However, 0 <X≦0.5、m≧0、M 2+ ;Mg 2+ ,Zn 2+ Divalent metal ions such as M 3+ ;Al 3+ ,Fe 3+ Trivalent metal ions such as A n- ;CO3 2-,Cl - ,NO3 - (n-valent anions such as these, n being an integer of 1 or greater)
[0028] The hydrotalcite compound represented by the general formula (1) has a positively charged base layer [M 2+ (1-X) M 3+ x (OH)2] x+ and the negatively charged intermediate layer [A n- (x / n) mH2O] x- It is a layered compound consisting of a basic layer and an intermediate layer inserted therein, and can be considered as an intercalation compound. Intercalation compounds are generally known to exhibit unique chemical properties (reactivity). In the case of hydrotalcite compounds represented by the general formula (1), the anions (A n- It is known that the anion exchange between the base layer and anions occurs easily (anion exchange). The mechanism of anion exchange is unclear, but it is assumed to involve a combination of factors such as the electrical interaction (attraction) between the base layer and anions, the size of the voids in the intermediate layer (the thickness of the intermediate layer), and adsorption.
[0029] In the general formula (1), a divalent metal ion M 2+ As for Mg 2+ is a trivalent metal ion M 3+ As for Al 3+ As the n-valent anion, CO3 2- ,Cl - is preferred.
[0030] The content of the inorganic layered double hydroxide is preferably 0.09 to 1.2 mass%, more preferably 0.1 to 1.0 mass%, based on the mass of the stretch blow molded product, molded product, or pellets. If it is 0.09 mass% or more, the wax can be more sufficiently adsorbed, and the wax is less likely to migrate to the bottle surface. If it is 1.2 mass% or less, the inorganic layered double hydroxide is less likely to become a starting point for rupture when blowing the preform. By setting the blending amount within the above range, it becomes easier to achieve both chemical attack suppression and blowability.
[0031] <Zeolite> Zeolite is a hydrated aluminosilicate containing an alkali or alkaline earth metal, which consists of a rigid anionic framework having regular channels (tubular pores) and cavities (voids). It is not particularly limited, and natural or artificial (synthetic) zeolite can be used.
[0032] Also, zeolite preferably has the following composition.
Chemical formula
[0033] The content of zeolite is preferably 0.09 to 1.2% by mass, more preferably 0.1 to 1.0% by mass, based on the mass of the stretch blow molded product (molded product or pellet). When it is 0.09% by mass or more, wax can be adsorbed more sufficiently, and it is more difficult for wax to migrate to the bottle surface. When it is 1.2% by mass or less, zeolite is less likely to be a starting point for rupture when blowing the preform. By setting the compounding amount within the above range, it becomes easier to balance chemical attack suppression and blowability.
[0034] From the viewpoint of achieving both suppression of chemical attack and blowability, the total content of the inorganic layered double hydroxide and the zeolite is preferably 0.09 to 1.2 mass%, and more preferably 0.1 to 1.0 mass%, based on the mass of the stretch-blow molded article (molded article or pellets).
[0035] The content ratio of inorganic layered double hydroxide and zeolite in the stretch blow molded product (molded product or pellet) can be measured by the following means. After measuring the mass of the stretch blow molded product, the stretch blow molded product is placed in a stainless steel container and then left in an oven at 480°C for 1 hour to burn the resin of the blow molded product. After that, ion-exchanged water is added to the stainless steel container containing the residue and thoroughly stirred, and then filtered through a nylon mesh with an opening that does not allow the inorganic layered double hydroxide and zeolite to pass through. The opening may be selected taking into consideration the size of materials other than the inorganic layered double hydroxide and zeolite. After filtration, the moisture is removed in an oven at 100°C, the mass is measured, and the content ratio can be measured by subtracting the mass of the nylon mesh. In this method, the catalyst and carbon black contained in the resin pass through the nylon mesh, so the content ratio of inorganic layered double hydroxide and zeolite can be accurately measured. If the inorganic layered double hydroxide and zeolite cannot be separated by filtration alone, the content can be measured by further combining known means.
[0036] The number-average particle size of the inorganic layered double hydroxide and zeolite is preferably 0.05 to 2.00 μm, more preferably 0.10 to 1.50 μm. When the number-average particle size is 0.05 μm or more, the dispersibility in the resin is good. When the number-average particle size is 2.00 μm or less, the inorganic layered double hydroxide and zeolite are less likely to become foreign matter during blow molding, and the bursting of the molded product is easily suppressed.
[0037] <Wax> Examples of waxes include aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, polyolefin copolymers, polyolefin wax, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax; or block copolymers thereof; vegetable waxes such as candelilla wax, carnauba wax, Japan wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; waxes mainly composed of aliphatic esters such as montan acid ester wax and castor wax; and waxes in which aliphatic esters have been partially or completely deoxidized, such as deoxidized carnauba wax. Further, saturated straight-chain fatty acids such as palmitic acid, stearic acid, montanic acid, or long-chain alkyl carboxylic acids having an even longer alkyl chain; unsaturated fatty acids such as brassidic acid, eleostearic acid, and valinaric acid; saturated alcohols such as stearyl alcohol, eicosyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, melissyl alcohol, or alkyl alcohols having an even longer alkyl chain; Examples of such compounds include polyhydric alcohols such as sorbitol; aliphatic amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; saturated aliphatic bisamides such as methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, and hexamethylene bisstearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipic acid amide, and N,N'-dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N'-distearyl isophthalic acid amide; fatty acid metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes obtained by grafting aliphatic hydrocarbon waxes with vinyl monomers such as styrene and acrylic acid; partial esterification products of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.
[0038] In addition, the waxes having a sharp molecular weight distribution obtained by subjecting them to a press sweating method, a solvent method, a recrystallization method, a vacuum distillation method, a supercritical gas extraction method, or a melt crystal precipitation method are preferably used, and those from which low molecular weight solid fatty acids, low molecular weight solid alcohols, low molecular weight solid compounds, and other impurities have been removed are also preferably used. The presence of wax in the stretch blow molded article (molded article or pellets) can be confirmed by GPC-FTIR.
[0039] Specific examples of waxes include Viscol (registered trademark) 330-P, 550-P, 660-P, and TS-200 (Sanyo Chemical Industries, Ltd.), Hiwax 400P, 200P, 100P, 410P, 420P, 320P, 220P, 210P, and 110P (Mitsui Chemicals, Inc.), Sasol H1, H2, C80, C105, and C77 (Schumann-Sasol), HNP-1, HNP- 3, HNP-9, HNP-10, HNP-11, HNP-12 (Nippon Seiro Co., Ltd.), Unilin (registered trademark) 350, 425, 550, 700, Unicid (registered trademark) 350, 425, 550, 700 (Toyo Petrolite Co., Ltd.), wood wax, beeswax, rice wax, candelilla wax, and carnauba wax (available from Cerarica NODA Co., Ltd.).
[0040] The wax content in the stretch blow molded product (molded product or pellets) is, for example, 0.001 to 0.100 mass%, 0.002 to 0.050 mass%, or 0.002 to 0.030 mass% based on the mass of the stretch blow molded product (molded product or pellets). If the wax content is within the above range, it is possible to more reliably prevent the wax from affecting the stretch blow moldability of the preform. The presence and quantity of wax in PET resin can be determined, for example, by measurement using pyrolysis GC / MS.
[0041] In the stretch blow molded product (molded product or pellets), the total content of the inorganic layered double hydroxide and the zeolite per 100 parts by mass of wax is preferably 400 to 5000 parts by mass, more preferably 450 to 4600 parts by mass.
[0042] The stretch blow molded article (molded article or pellets) may contain carbon black. For example, carbon black may be added to the stretch blow molded article for reasons of appearance. The carbon black content (blending amount) in the stretch blow molded article (molded article or pellets) is, for example, 0.01 to 0.20 mass%, or 0.02 to 0.10 mass%.
[0043] (Manufacturing of stretch blow molded products) Next, a method for manufacturing stretch blow molded products such as toner bottles by biaxial stretch blow molding is described. The method for producing a stretch-blow molded article includes a step of preparing a preform containing at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, polyester, and wax, and a molding step of stretch-blow molding the preform to obtain a stretch-blow molded article.
[0044] First, an example of a method for producing pellets that are the material of the preform used for biaxial stretch blow molding of the stretch blow molded product will be described. For example, in the process of preparing the preform, at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, polyester, and wax are melt-kneaded to form pellets. By forming the material into pellets, the material composition is made uniform, making it easier to mold. The wax may be a toner containing the wax. More specifically, at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, polyester, and an electrophotographic toner containing the wax are melted and kneaded to form pellets. At least one selected from the group consisting of inorganic layered double hydroxides and zeolites may be mixed or melt-kneaded with polyester in advance to obtain a modified polyester, and then a toner containing a wax may be mixed or melt-kneaded therewith.
[0045] Furthermore, for example, a toner bottle containing polyester with an electrophotographic toner containing wax attached thereto may be used. That is, the step of preparing the preform preferably includes a step of pulverizing a recycled toner bottle with an electrophotographic toner attached thereto to obtain a pulverized material, a step of melting and kneading the pulverized material with at least one selected from the group consisting of inorganic layered double hydroxides and zeolites to form pellets, and a step of forming the preform from the formed pellets. It is also preferable that the electrophotographic toner contains wax and the toner bottle contains polyester. The amount of electrophotographic toner is preferably 0.100 to 1.000 mass %, and more preferably 0.150 to 0.500 mass %, based on the total amount of the toner bottle and the electrophotographic toner attached to the toner bottle.
[0046] The melt kneading means is not particularly limited, and known means such as a twin-screw extruder can be used. The temperature during melt kneading is not particularly limited as long as the polyester can be melt kneaded. For example, it is 120 to 300°C, preferably 260 to 280°C. The melt kneading conditions are also not particularly limited. After melt kneading, the mixture is cooled and molded into pellets that can be injection molded using known means such as a pelletizer.
[0047] After forming pellets by melt kneading, a step of crystallizing the pellets may be adopted. Crystallizing the pellets improves the workability during preform production. The pellets can be crystallized by maintaining them at preferably about 100 to 180°C, more preferably about 130 to 170°C, for preferably 1 to 12 hours, more preferably about 3 to 7 hours. Note that even if the pellets are crystallized, they may become amorphous due to heating during preform production.
[0048] Next, the obtained pellets are used to mold a preform 104 having a test tube shape by injection molding as shown in Fig. 2. Specifically, a heating cylinder 105 heats the material fed into an injection molding machine 101 to make it molten, and an extrusion screw 207 injects the molten material into preform molds 102 and 103, and after cooling, the material is removed from the molds to obtain a preform 104. In the step of preparing a preform, it is preferable to obtain a preform from the obtained pellets by injection molding. In addition, the preform preferably has a test tube shape.
[0049] Next, the molding process will be described. In the molding process, biaxial stretch blow (biaxial stretch molding) is performed on the preform 104 as shown in FIG. 3. First, the preform 104 is placed in a heating furnace 107. The preform 104 is placed in the heating furnace 107 and heated to a temperature at which it can be stretched. The heating time is preferably within 3 minutes. By keeping the heating time within 3 minutes, it is possible to prevent the progress of crystallization of the polyester in the preform during heating. The heated preform 104 is taken out of the heating furnace 107 and placed in the mouth of a blow mold 108 in which a cavity is formed by combining a left mold 108-1 and a right mold 108-2.
[0050] It is preferable to place the heated preform at the mouth of the blow mold in a short time (for example, within 10 seconds) so that the temperature of the preform does not drop before the start of the biaxial stretching process, which can prevent the progress of crystallization of the polyester in the preform due to the slow cooling of the preform.
[0051] The heated preform placed in the blow mold 108 is stretched in the vertical direction using a stretch rod 109. This stretching is called the first stretching. In the first stretching, it is preferable to inject gas so that the preform 104 does not come into contact with the stretch rod 109, and the pressure of the gas at this time is called the first blow pressure.
[0052] After the first stretching, gas 110 is introduced from the preform mouth 106 to expand the preform in the lateral direction (circumferential direction). This is called the second stretching. The pressure of the gas at this time is called the second blow pressure. Examples of the gas to be blown include air, nitrogen, carbon dioxide, and argon.
[0053] By carrying out these primary and secondary stretching steps, preform 104 expands in each direction indicated by arrows 301 and adheres to the inner wall of blow mold 108, and is cooled and solidified in this state to become blow-molded product 112. The molding process preferably includes a step of stretching the preform in the longitudinal direction of the preform using a stretching rod, and a step of injecting gas into the preform stretched in the longitudinal direction to stretch the preform in the circumferential direction. Next, the left mold 108-1 and the right mold 108-2 of the blow mold 108 are separated, and the blow-molded article 112 is removed from the blow mold 108. Since this blow-molded article 112 is stretched in both the vertical and horizontal directions, it becomes a molded article with high strength.
[0054] Thus, it is preferable that the preform is not crystallized (non-crystalline, i.e., amorphous) during the stretching process of injection stretch blow molding. If the preform is in an amorphous state and is at the blow molding temperature, the resin will stretch and crystallize in the stretched direction when it is blown, i.e., biaxially stretched, making it possible to form a bottle with high strength.
[0055] There are two types of injection stretch blow molding: one-stage and two-stage. The one-stage method uses the residual heat of the preform immediately after it is removed from the mold to stretch blow mold it as is, or after adjusting the temperature. The two-stage method cools the preform down to room temperature, and then stretch blow molds it again after adjusting the temperature.
[0056] In the one-stage method, as shown in Fig. 4, after injection molding of a preform 104 from an injection molding machine 101, cooling during injection molding is completed in a short time of 10 seconds or less so that the preform 104 does not fall below the glass transition temperature of the resin. Then, the preform is immediately heated and kept at a blow molding temperature (for example, 90°C to 120°C) and blow molded to obtain a blown bottle 112. An apparatus in which an injection molding device and a blow molding device are integrated is used.
[0057] In the two-stage method, after injection molding the preform, the preform is cooled below the glass transition temperature of the resin, removed, and then heated to the blow molding temperature (for example, 90°C to 120°C) in a separate blow molding machine for blow molding. After the preform is molded, the preform is cooled below the glass transition temperature of the polyester before the molding step is carried out.
[0058] The one-stage method is preferable because it does not cool the preform below its glass transition temperature and therefore requires less energy to reheat than the two-stage method.
[0059] Next, a method for checking chemical attack in a toner bottle obtained by biaxial stretch blow molding will be described. Toner is placed in a toner bottle obtained by biaxial stretch blow molding. The toner bottle containing the toner is left in the usage environment. For the evaluation of chemical attack, the usage environment is set at 50°C for 72 hours, and the toner bottle is left in a thermostatic chamber for testing. The toner bottle exposed to the usage environment is removed, and the toner adhering to the inner surface of the bottle is removed. The toner is discharged from the bottle by turning the toner storage opening of the bottle upside down, and the toner adhering to the inner surface of the bottle is easily removed by attaching it with adhesive tape or the like. When the removed toner is observed with an electron microscope or the like to observe the deformation of the toner particle surface, the toner particles that have been subjected to chemical attack can be observed to have deformation marks on the contact surface with the toner bottle.
[0060] (Image forming device) The image forming apparatus will be described below with reference to the drawings. Fig. 1 is a schematic diagram showing a four-color image forming apparatus using an electrophotographic method, with 80 being the main body of the image forming apparatus. This image forming apparatus 80 is configured as a so-called intermediate transfer tandem type image forming apparatus in which four color image forming units are arranged side by side on an intermediate transfer belt.
[0061] In this image forming apparatus 80, image formation is performed as follows. First, in this image forming apparatus 80, an electrostatic latent image is formed on a photosensitive drum 17 (17y, 17m, 17c, 17bk) by an exposure device 50 (50y, 50m, 50c, 50bk) based on print data. Then, in this image forming apparatus 80, the formed electrostatic latent image is developed by a developing device 21 (21y, 21m, 21c, 21bk) to form a toner image.
[0062] In this image forming apparatus 80, the toner image is transferred onto an intermediate transfer body 62 by a primary transfer device 60 (60y, 60m, 60c, 60bk), and then transferred onto a sheet material S supplied from a paper feeder 63 by a secondary transfer section 64 (64a, 64b). Next, in this image forming apparatus 80, the toner image transferred onto the sheet S is fixed onto the sheet material S by a fixing means 68, and then the sheet material S is discharged onto a paper discharge tray 70.
[0063] In addition, in this image forming apparatus 80, a toner image is formed by the developing device 21, and detachable toner bottles 3 (3Y, 3M, 3C, 3Bk) are used to supply toner to the developing device 21. The toner bottle according to at least one embodiment of the present disclosure is a toner bottle used in this manner. The toner bottle contains at least one selected from the group consisting of inorganic layered double hydroxides and zeolites, polyester, and wax. EXAMPLES
[0064] The present disclosure will be described in detail below using examples and comparative examples. However, the present disclosure is not limited to these examples. In the following examples and comparative examples, "%" means "mass %" unless otherwise specified.
[0065] <Toner bottle manufacturing> One-stage blow molding equipment (ASB-70DPH manufactured by Nissei ASB Machinery Co., Ltd.) ) was used to prepare a toner bottle 3 (total length 439.5 mm, diameter 101 mm) shown in Fig. 6. The blow stretching ratio was "vertical ratio x horizontal ratio = 6.7". The "longitudinal ratio" of the blow stretch ratio is a value calculated by dividing the "total length after stretching" by the "total length (before stretching) of the part (heated part) of the preform that reaches the stretching temperature." The "lateral ratio" of the blow stretch ratio is a value calculated by dividing the "diameter of the middle part after stretching" by the "diameter of the middle part of the preform (before stretching)".
[0066] First, the materials shown in Table 1 below were melt-kneaded and then pelletized to prepare a master batch with a carbon black concentration of 5 mass %. [Table 1]
[0067] Next, the master batch with a carbon black concentration of 5% by mass prepared above and PET were mixed in the ratio shown in Table 2 below, melt-kneaded, and pelletized to obtain pellets of a resin mixture. The obtained pellets were dried at a temperature of 150° C. for 5 hours. [Table 2]
[0068] <Blow molding conditions> The pellets of the resin mixture dried above were fed into an injection molding device of a one-step stretch blow molding machine (product name: ASB-70DPH; manufactured by Nissei ASB Machinery Co., Ltd.), and a toner bottle was molded by biaxial stretch blow molding. The one-step stretch blow molding machine can continuously carry out (one-stage method) a process of obtaining a test tube-shaped preform by injection molding, and a process of obtaining a bottle-shaped molded product by biaxial stretch blow molding of the preform. The screw diameter of the injection molding machine in the molding machine was 54 mm.
[0069] First, a mold capable of molding a preform having an outer diameter of 30 mm, a wall thickness of 3.7 mm, and a length of 220 mm was prepared as a mold for molding a preform. Then, a preform was molded under the following molding conditions. Screw diameter: 54mm Screw position before filling the cavity with resin mixture: 95mm ·Injection speed Up to 5mm of screw advance: 50% of maximum speed Advance the screw another 20mm: 30% of maximum speed Until the screw advances another 35mm: 25% of maximum speed PV switching position: 35mm Injection pressure Up to PV switching: 12.0MPa After PV switching: 4.5MPa (holding pressure) - Pressure retention time after PV switching ·4.57 seconds ·Heating tube temperature: 280℃ ·Cooling time: 8.0 seconds Mold temperature: 18℃
[0070] After a cooling time of 8.0 seconds had elapsed, the preform was demolded and transported to the biaxial stretch blow station of the one-step stretch blow molding machine. The temperature of the preform during transportation was controlled as follows. Preform heating temperature 10% of the preform's total length from the top of the preform 180℃ 25% of the preform's total length from the top of the preform 200℃ 50% of the preform's total length from the top of the preform 200℃ 75% of the preform's total length from the top of the preform 180℃ Next, the preform adjusted to the above temperature was placed in a cylindrical mold adjusted to a temperature of 18°C and having a size corresponding to the size of the toner bottle, and was subjected to biaxial stretch blow molding to produce a blown bottle. The preform was heated during transportation, so that the surface temperature of the center of the preform immediately before being placed in the cylindrical mold was 100°C.
[0071] First, the stretch bar was inserted from the retreated position into the preform through the opening of the preform and advanced until it contacted the top of the preform. Next, the air pressure driving the stretch bar was set to 1.2 MPa and the stretch bar was advanced further. Next, 0.5 seconds after the start of the further advancement of the stretch bar, primary air was introduced into the preform through the opening of the preform. The pressure of the primary air was set to 1.0 MPa. Next, 0.15 seconds after the introduction of the primary air, secondary air was introduced. The pressure of the secondary air was set to 2.9 MPa. Then, air was introduced into the preform for 7.0 seconds from the start of the introduction of the primary air. Next, the pressure inside the preform was returned to normal pressure over 2.5 seconds. In this way, a toner bottle was produced by blow molding. This bottle is a toner bottle using virgin PET that has not been recycled. Using the above method, 200 toner bottles were produced using virgin PET.
[0072] (Example 1-1) <Production of recycled pellets> 200 unused toner cartridges (product name: Toner NPG-67, manufactured by Canon Inc.) filled with black toner were prepared. The black toner contained wax. The entire amount of black toner in each toner cartridge was transferred to the 200 toner bottles prepared above. After that, the opening of the toner bottle was turned vertically downward to discharge the black toner inside. Even after this operation, a small amount of black toner was still attached to the inner wall of each toner bottle. At this time, the amount of black toner remaining in the toner bottle was 0.321% by mass, based on the mass of the toner bottle itself, on the average of 200 toner bottles. Note that the mass of the toner bottle itself here refers to the mass of the toner bottle and only the toner remaining inside it, after all supply parts and other items attached to the toner bottle have been removed. Next, each toner bottle was crushed into pieces of about 5 to 10 mm square using a crusher to obtain crushed products (hereinafter also referred to as "flake products"). The wax content of the obtained flake products was measured using GPC and FT-IR, and was found to be 0.022 parts by mass per 100 parts by mass of the flake products. This flake product contains 99.5% by mass of hydrotalcite as an inorganic layered double hydroxide. A compound (trade name: DHT-4C; manufactured by Kyowa Chemical Industry Co., Ltd.) was added at 0.5% by mass, and the mixture was melt-kneaded using a twin-screw extruder (manufactured by Ikegai Co., Ltd., PC-46) at a temperature of 260°C, a screw rotation speed of 200 rpm, and a discharge rate of 50 kg / h, and then pelletized. The inorganic layered double hydroxide used here was in the form of a filler, and had a number-average particle size of 0.38 μm. The pellets obtained by melt kneading in an extruder were maintained at a temperature of 150° C. for 5 hours to crystallize the molding pellets (this recycled material is referred to as MR-PET (1-1)).
[0073] <Making a blow bottle> The MR-PET (1-1) was placed in the one-step stretch blow molding machine and biaxial stretch blow molding was performed under the same blow molding conditions as described above (the obtained toner bottle is referred to as toner bottle (1-1)). Toner was placed in the toner bottle (1-1) and a chemical attack confirmation test was performed in an environment of 50°C for 72 hours. As a result, no deformation of the toner particle surface was confirmed even when observing the toner attached to the inner surface of the toner bottle.
[0074] Toner bottles (1-2), (1-3) and a comparative toner bottle (1-4) were obtained by blow molding in the same manner as in Example 1-1, except that the compounding ratio of the flakes and the inorganic layered double hydroxide (hydrotalcite compound) was changed as shown in Table 3. Blow molding could be performed without any problems for all of the toner bottles. For each of the obtained toner bottles, the deformation of the toner particle surface was observed in the same manner as in Example 1-1. [Table 3]
[0075] Toner bottle (1-2) When the amount of inorganic layered double hydroxide added was 1.0 mass%, biaxial stretch blow molding of the preform was performed, and blow molding was possible without any problems. When this toner bottle (1-2) was used to evaluate chemical attack, no deformation of the toner particle surface was confirmed even when observing the toner adhering to the inner surface of the toner bottle.
[0076] Toner bottle (1-3) When the amount of inorganic layered double hydroxide added was 0.1% by mass, biaxial stretch blow molding of the preform was performed, and blow molding was possible without any problems. When this toner bottle (1-3) was used to evaluate chemical attack, no deformation of the toner particle surface was confirmed even when observing the toner adhering to the inner surface of the toner bottle.
[0077] Comparison toner bottle (1-4) When the amount of inorganic layered double hydroxide added was 0.0 mass %, the preform was subjected to biaxial stretch blow molding, and the blow molding was possible without any problem. When the comparative toner bottle (1-4) was used to evaluate chemical attack, the toner adhering to the inner surface of the toner bottle was Deformation was confirmed on the particle surface, and chemical attack occurred. The reason for this is thought to be that if inorganic layered double hydroxide is not added, the wax, which is the cause of chemical attack, is not adsorbed by the inorganic layered double hydroxide, and the wax migrates to the inner surface of the toner bottle, causing chemical attack.
[0078] <Production of recycled pellets> (Example 2-1) 0.5% by mass of zeolite (product name: Silton MT-8000, manufactured by Mizusawa Chemical Industries, Ltd.) was added to 99.5% by mass of flakes prepared in the same manner as in Example 1-1, and the mixture was melt-kneaded at a temperature of 260°C, a screw rotation speed of 200 rpm, and a discharge rate of 50 kg / h using a twin-screw extruder (PC-46, manufactured by Ikegai Corporation), and then pelletized. The zeolite used here was in the form of a filler. The pellets obtained by melt-kneading in the extruder were maintained at a temperature of 150°C for 5 hours to crystallize the molding pellets (this recycled material is referred to as MR-PET (2-1)).
[0079] <Making a blow bottle> The MR-PET (2-1) was placed in the one-step stretch blow molding machine and biaxial stretch blow molding was performed under the same blow molding conditions as described above (the obtained toner bottle is referred to as toner bottle (2-1)). Toner was placed in the toner bottle (2-1) and a chemical attack confirmation test was performed in an environment of 50°C for 72 hours. As a result, no deformation of the toner particle surface was confirmed even when observing the toner attached to the inner surface of the toner bottle.
[0080] Toner bottles (2-2), (2-3) and a comparative toner bottle (2-4) were obtained by blow molding in the same manner as in Example 2-1, except that the compounding ratio of the flakes and zeolite was changed as shown in Table 4. Blow molding could be performed without any problems for all of the toner bottles. For each of the obtained toner bottles, the deformation of the toner particle surface was observed in the same manner as in Example 2-1. [Table 4]
[0081] Toner bottle (2-2) When the amount of zeolite added was 1.0 mass%, the preform was subjected to biaxial stretch blow molding, and the blow molding was possible without any problems. When the toner attached to the inner surface of the toner bottle was observed to evaluate chemical attack using this toner bottle (2-2), no deformation of the toner particle surface was confirmed.
[0082] Toner bottle (2-3) When the amount of zeolite added was 0.1% by mass, the preform was subjected to biaxial stretch blow molding, and the blow molding was possible without any problems. When the toner attached to the inner surface of the toner bottle was observed to evaluate chemical attack using this toner bottle (2-3), no deformation of the toner particle surface was confirmed.
[0083] Comparison toner bottle (2-4) When the preform was biaxially stretched and blow molded with 0.0% by mass of added zeolite, blow molding was possible without any problems. When chemical attack was evaluated using this comparative toner bottle (2-4), deformation was confirmed on the surface of the toner particles attached to the inner surface of the toner bottle, and chemical attack had occurred. The reason for this is thought to be that if zeolite is not added, the wax, which is the cause of chemical attack, is not adsorbed by the zeolite, and the wax migrates to the inner surface of the toner bottle, causing chemical attack.
[0084] The present disclosure relates to the following configurations. (Configuration 1) A stretch blow molded article, The stretch blow molded product is At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A stretch blow molded article comprising: (Configuration 2) 2. The stretch blow molded article according to claim 1, wherein the total content of the inorganic layered double hydroxide and the zeolite is 0.09 to 1.2% by mass based on the mass of the stretch blow molded article. (Configuration 3) 3. The stretch blow molded article according to claim 1 or 2, wherein the inorganic layered double hydroxide comprises a hydrotalcite compound. (Configuration 4) 4. The stretch blow molded product according to any one of configurations 1 to 3, wherein the polyester is a material recycled polyester. (Configuration 5) 5. The stretch blow molded article according to any one of configurations 1 to 4, wherein the polyester comprises at least one selected from the group consisting of polyethylene terephthalate and polyethylene naphthalate. (Configuration 6) 6. The stretch blow molded article according to any one of configurations 1 to 5, which is a toner bottle. (Configuration 7) A toner bottle, The toner bottle is At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A toner bottle comprising: (Configuration 8) A method for producing a stretch blow molded article according to any one of configurations 1 to 6, preparing a preform containing at least one selected from the group consisting of the inorganic layered double hydroxide and the zeolite, the polyester, and the wax; and A molding step of stretch-blow molding the preform to obtain the stretch-blow molded product. A method for producing a stretch blow molded product comprising the steps of: (Configuration 9) The step of preparing the preform comprises: A step of crushing the recycled toner bottles to which electrophotographic toner has been attached to obtain crushed material; A step of melting and kneading the ground product with at least one selected from the group consisting of the inorganic layered double hydroxide and the zeolite to form pellets; and forming the preform from the formed pellet; the electrophotographic toner comprises the wax, 9. The method for producing a stretch blow molded article according to claim 8, wherein the toner bottle comprises the polyester. (Configuration 10) A molded article, The molded article is At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A molded article comprising: (Configuration 11) At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A pellet comprising: [Explanation of symbols]
[0085] 3: toner bottle, 21: developing device, 80: image forming device, 60: primary transfer device, 62: intermediate transfer body, 63: paper feeder, 64: secondary transfer section, 68: fixing means, 70: paper discharge tray, 101: injection molding machine, 102: preform mold, 103: preform mold, 104: preform, 105: heating cylinder, 106: preform mouth, 107: heating furnace, 108: blow mold, 109: stretch rod, 110: gas, 112: blow molded product, 201: PET resin, 202: wax, 207: extrusion screw
Claims
1. A stretch blow molded article, The stretch blow molded product is At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A stretch blow molded article comprising:
2. 2. The stretch blow molded article according to claim 1, wherein the total content of the inorganic layered double hydroxide and the zeolite is 0.09 to 1.2 mass% based on the mass of the stretch blow molded article.
3. The stretch blow molded article according to claim 1 , wherein the inorganic layered double hydroxide comprises a hydrotalcite compound.
4. The stretch blow molded product according to claim 1 , wherein the polyester is a material recycled polyester.
5. The stretch blow molded article according to claim 1 , wherein the polyester comprises at least one selected from the group consisting of polyethylene terephthalate and polyethylene naphthalate.
6. The stretch blow molded article according to claim 1 , wherein the stretch blow molded article is a toner bottle.
7. A toner bottle, The toner bottle is At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A toner bottle comprising:
8. A method for producing the stretch blow molded article according to any one of claims 1 to 6, preparing a preform containing at least one selected from the group consisting of the inorganic layered double hydroxide and the zeolite, the polyester, and the wax; and A method for producing a stretch blow molded article, comprising the step of stretch blow molding the preform to obtain the stretch blow molded article.
9. The step of preparing the preform comprises: A step of crushing the recycled toner bottles to which electrophotographic toner has been attached to obtain crushed material; A step of melting and kneading the ground product with at least one selected from the group consisting of the inorganic layered double hydroxide and the zeolite to form pellets; and forming the preform from the formed pellet; the electrophotographic toner comprises the wax, The method for producing a stretch blow molded article according to claim 8, wherein the toner bottle comprises the polyester.
10. A molded article, The molded article is At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A molded article comprising:
11. At least one selected from the group consisting of inorganic layered double hydroxides and zeolites; Polyester and Wax and A pellet comprising:
Citation Information
Patent Citations
Chemical recycle of polyethylene terephthalate waste
JP2000169623A
Toner bottle, electrophotographic device fitting the same, and manufacture of the toner bottle
JP2001042626A
Injection stretch blow molded bottle and method for manufacturing the same
JP2014198422A