Method for producing concrete-sludge-treated product containing organic material

A method combining protein-containing organic waste with concrete sludge, divalent iron, and phosphoric acid compounds at a pH of 10 to 12.5, addresses ammonia and metal leaching issues, facilitating safe disposal and reuse of concrete sludge.

JP2024155631AActive Publication Date: 2024-10-31ENVIRONMENTAL INNOVATION CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023070506
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

The disposal of protein-containing organic waste, such as seafood processing residues, poses challenges due to ammonia generation, landfill odors, pest emergence, increased BOD and COD, and leaching of toxic metals, while concrete sludge disposal is hindered by hexavalent chromium content requiring costly pretreatment.

Method used

A method involving mixing protein-containing organic matter with concrete sludge, a divalent iron compound, and a phosphoric acid compound, maintaining a pH of 10 to 12.5, to produce a treated concrete sludge that suppresses ammonia generation and elution of toxic metals.

Benefits of technology

The method effectively reduces ammonia generation and suppresses the elution of hexavalent chromium and toxic metals like cadmium and arsenic, enabling safe landfill disposal and reuse of concrete sludge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155631000015
    Figure 2024155631000015
  • Figure 2024155631000001
    Figure 2024155631000001
  • Figure 2024155631000002
    Figure 2024155631000002
Patent Text Reader

Abstract

To provide a method for treating a protein-containing organic material while suppressing generation of ammonia, by utilizing concrete sludge.SOLUTION: The present invention provides: a method for producing a concrete-sludge-treated product containing an organic material, in which ammonia generation is suppressed, and which includes a step of preparing a mixture of a protein-containing organic material, concrete sludge, a divalent iron compound, and a phosphate compound, and a step of retaining the mixture for at least one hour; a method for suppressing ammonia generation from a protein-containing organic material; a kit for use in these methods; and a method for suppressing hydrogen sulfide emission using a concrete-sludge-treated product. The present invention enables performing treatment of a protein-containing organic material while suppressing ammonia generation, and furthermore, the obtained concrete-sludge-treated product suppresses elution of harmful metals, and therefore, can be subjected to disposal by land-filing at a final disposal site.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a treated concrete sludge product containing protein-containing organic matter, a method for suppressing the generation of ammonia from protein-containing organic matter, a kit for use in these methods, and utilization of the produced treated concrete sludge product. [Background technology]

[0002] Although various efforts have been made to utilize organic waste containing protein, such as fishery processing residues and food waste, as resources, such as for livestock feed and composting, they are still often disposed of as waste. In particular, fishery processing residues, such as squid innards and scallop midgut glands, contain high concentrations of cadmium and arsenic and cannot be used for human or livestock consumption, so most of them are disposed of as industrial waste.

[0003] When organic waste is treated as industrial waste, it is usually reduced in volume through intermediate treatment such as crushing and dehydration, and then disposed of in landfills along with other industrial waste. Problems that arise when disposing of organic waste in landfills include the generation of foul odors such as ammonia due to the decomposition of the organic matter, and the emergence of pests. Furthermore, depending on the amount of organic matter, the BOD (biochemical oxygen demand) and COD (chemical oxygen demand) of the leachate may rise, increasing the burden on wastewater treatment. Furthermore, there is a problem in terms of work, as the landfill material softens due to the rapid decomposition of the organic matter, causing it to sink when heavy machinery is placed on it.

[0004] In addition to the problems mentioned above, when organic waste containing hazardous metals is disposed of in landfills, there is also the problem that the hazardous metals trapped in the organic matter are eluted into leachate as the organic matter decomposes. Since such leachate requires wastewater treatment to reduce the concentration of hazardous metals to a level that meets the wastewater standards, accepting organic waste containing hazardous metals places a heavy burden on managed final disposal sites. Due to the existence of such various problems, organic waste, especially seafood processing residues such as squid innards and scallop mid-intestinal glands, is rarely disposed of in landfills at final disposal sites.

[0005] On the other hand, concrete sludge (also called ready-mixed concrete sludge) is the residue left over after aggregate is removed from wastewater generated during the cleaning of mixers, agitators, and leftover concrete (remaining concrete) not used at work sites in ready-mixed concrete plants, as well as concrete that has failed unloading inspections (returned concrete).

[0006] Concrete sludge is classified as industrial waste under the Waste Management and Public Cleansing Law, and is generally disposed of by landfill at controlled final disposal sites. However, the cost of disposing of the large amounts of concrete sludge generated is a heavy burden for concrete manufacturers, and in recent years the remaining capacity of controlled final disposal sites has been decreasing, so there is a demand for effective use of concrete sludge.

[0007] The effective use of concrete sludge is challenged by its nature of containing harmful hexavalent chromium. For example, when using concrete sludge as backfill material, pretreatment is required to reduce the amount of eluted hexavalent chromium to below the environmental standard value, which is an obstacle to effective use.

[0008] Patent Document 1 discloses a method for neutralizing ready-mixed concrete sludge, which is characterized by comprising a mixing step of adding and mixing ferrous sulfate, a polymer flocculant, and inorganic powder to ready-mixed concrete sludge, and a curing step of curing the mixture obtained by this mixing step. Patent Document 2 discloses a hydrogen sulfide gas adsorbent, which is characterized by containing neutralized soil obtained by the neutralization method of Patent Document 1. This neutralization method can reduce hexavalent chromium in concrete sludge, but has the problem of requiring a large amount of ferrous sulfate.

[0009] Furthermore, Patent Document 3 discloses a method for producing treated concrete sludge by adding and mixing a divalent iron compound and a phosphate compound to concrete sludge. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2014-087723 A [Patent Document 2] JP 2017-064613 A [Patent Document 3] Patent No. 7117809 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention provides a method for treating protein-containing organic matter while suppressing the generation of ammonia, by utilizing concrete sludge. [Means for solving the problem]

[0012] The inventors have discovered that by mixing a protein-containing organic matter, concrete sludge, a divalent iron compound, and a phosphate compound, it is possible to produce a treated concrete sludge product in which the generation of ammonia is suppressed.

[0013] The present invention provides the following inventions. Item 1. A method for producing a treated concrete sludge product containing organic matter, in which generation of ammonia is suppressed, comprising the steps of preparing a mixture of protein-containing organic matter, concrete sludge, a divalent iron compound, and a phosphate compound, and maintaining the mixture for at least one hour, wherein the mass ratio of iron in the divalent iron compound to phosphoric acid in the phosphate compound used in preparing the mixture is 1:2 to 1:8, and the pH of the prepared mixture is 10 to 12.5. Item 2. The method according to Item 1, wherein the mass of the solid content of the concrete sludge is three times or more the mass of the protein in the organic matter. Item 3. The method according to item 1 or 2, wherein the mixture is prepared by mixing a protein-containing organic matter, concrete sludge, and a liquid in which a divalent iron compound and a phosphate compound are dissolved. Item 4. The method according to any one of Items 1 to 3, wherein the divalent iron compound is iron sulfate (II) or iron chloride (II). Item 5. The method according to any one of Items 1 to 4, wherein the phosphoric acid compound is orthophosphoric acid or a salt thereof. Item 6. The method according to any one of Items 1 to 5, wherein the protein-containing organic matter is a fish and shellfish residue. Item 7. The method according to any one of Items 1 to 6, wherein the protein-containing organic matter is fish or shellfish viscera, shell attachments, or starfish. Item 8. The method according to any one of Items 1 to 7, wherein elution of harmful metals from treated concrete sludge is suppressed. Item 9. A method for suppressing generation of ammonia from protein-containing organic matter, comprising the steps of preparing a mixture of protein-containing organic matter, concrete sludge, a divalent iron compound, and a phosphate compound, and maintaining the mixture for at least 1 hour, wherein the mass ratio of iron in the divalent iron compound to phosphoric acid in the phosphate compound used in the preparation of the mixture is 1:2 to 1:8, and the pH of the prepared mixture is 10 to 12.5. Item 10. A kit for use in the method according to any one of Items 1 to 9, comprising a liquid in which a divalent iron compound and a phosphate compound are dissolved, the mass ratio of iron in the divalent iron compound to phosphoric acid in the phosphate compound being 1:2 to 1:8. Item 11. The kit according to Item 10, wherein the divalent iron compound is iron sulfate (II) or iron chloride (II). Item 12. The kit according to Item 10 or 11, wherein the phosphate compound is orthophosphoric acid or a salt thereof. Item 13. A method for suppressing release of hydrogen sulfide from landfill waste, comprising a step of burying a treated concrete sludge produced by the method according to any one of items 1 to 8 together with landfill waste. Effect of the Invention

[0014] According to the present invention, the organic matter containing protein can be treated while suppressing the generation of ammonia. Furthermore, the resulting treated concrete sludge has suppressed elution of hexavalent chromium, and even if the organic matter contains harmful metals such as cadmium and arsenic, the elution of these harmful metals is suppressed, making it possible to dispose of the treated concrete sludge in a landfill site. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic diagram of a hydrogen sulfide gas adsorption test device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The following description may be based on a representative embodiment or specific example, but the present invention is not limited to such an embodiment or specific example. The upper and lower limit values ​​of each numerical range shown in this specification can be combined arbitrarily. In addition, a numerical range expressed using "~" or "-" in this specification means a range including the numerical values ​​at both ends as the upper and lower limits, unless otherwise specified.

[0017] The present invention provides a method for producing a treated concrete sludge product containing organic matter, in which generation of ammonia is suppressed, comprising the steps of preparing a mixture of protein-containing organic matter, concrete sludge, a divalent iron compound, and a phosphate compound, and holding the mixture for at least one hour, wherein the mass ratio of iron in the divalent iron compound to phosphoric acid in the phosphate compound used in preparing the mixture is 1:2 to 1:8, and the pH of the prepared mixture is 10 to 12.5.

[0018] The method for producing a treated concrete sludge product of the present invention includes a step of preparing a mixture of protein-containing organic matter, concrete sludge, a divalent iron compound, and a phosphate compound (hereinafter referred to as a mixture preparation step).

[0019] In the present invention, the protein-containing organic matter is not limited as long as it is desired to be treated as waste, and examples thereof include waste derived from animals such as livestock and poultry (e.g., meat, skin, internal organs, etc.), waste derived from plants (e.g., vegetable scraps, soybean meal), marine waste (e.g., fish and shellfish internal organs, shellfish attachments, aquatic pests such as starfish, seaweed), food waste from restaurants, etc.

[0020] In addition, these wastes correspond to solid animal waste, animal and plant residues, animal carcasses, etc. in the industrial waste category, and to seafood residues, agricultural residues, food residues, etc. in the general waste category. However, in the present invention, any organic matter containing protein can be used without distinction between industrial waste and general waste.

[0021] The protein-containing organic matter may contain harmful metals. Examples of such organic matter include the innards of fish and shellfish, such as the mid-gut gland of a scallop (known as uro) and the innards of a squid (known as goro). Cadmium and arsenic accumulate in the mid-gut gland of a scallop and the innards of a squid, and there is a risk that these harmful metals will elute during the waste treatment process. However, according to the present invention, the elution of these harmful metals can be suppressed.

[0022] In the present invention, there is no limitation on the protein content or the composition of the amino acids in the organic matter. According to the present invention, even organic matter containing a large amount of protein, such as the midgut gland of a scallop, can be treated while suppressing the generation of ammonia.

[0023] The protein-containing organic matter can be used in the preparation of the mixture in the form in which it is discarded, or in the form that has been subjected to processing such as crushing, pulverization, heating, dehydration, etc.

[0024] In the present invention, concrete sludge may be either sludge or sludge solids. In ready-mix concrete plants, wastewater containing concrete components (concrete washing wastewater) is generated by washing fresh mortar and residual fresh concrete adhering to transport vehicles, mixers, hoppers, etc. of the plant, and returned concrete. The suspended water recovered by removing coarse aggregate and fine aggregate from this concrete washing wastewater is called sludge water, and sludge water that has been concentrated and lost its fluidity is called sludge, and the sludge obtained by drying it at 105 to 110°C is called sludge solids.

[0025] For example, concrete sludge includes sludge obtained by concentrating sludge water using a sedimentation thickener or the like, sludge solids obtained by drying these, or sludge cake (solid matter) obtained by dehydrating the sludge or sludge water and compressing and molding it. Note that in the present invention, concrete sludge is not limited to concrete sludge from which coarse aggregate and fine aggregate have been completely removed, and may contain an amount of aggregate that does not interfere with mixing, which will be described later, or with the use of the treated concrete sludge.

[0026] Concrete sludge usually contains hexavalent chromium at about several ppm to 10 ppm. Hexavalent chromium may be concentrated to about several tens of ppm in the concrete sludge by reusing a part of the sludge water as circulating sludge water for washing mixers and agitators. In the present invention, in addition to ordinary concrete sludge, concrete sludge in which hexavalent chromium is concentrated can be used. The hexavalent chromium content of concrete sludge can be measured by a water quality test kit (e.g., Pack Test (registered trademark)) commercially available for business use such as wastewater testing, or a method specified in 65.2 of Japanese Industrial Standard K0102 described in Environment Agency Notification No. 46 Soil Environmental Standards (diphenylcarbazide absorptiometry, flame atomic absorption spectrometry, ICP emission spectrometry, etc.).

[0027] In the present invention, the concrete sludge may be the sludge or sludge solids generated in a ready-mix concrete plant, or may be sludge or sludge solids to which water or recovered water has been added. The moisture content of the concrete sludge used in the present invention may be about 0 to 90%, and may be, for example, 0% or more, 5% or more, 10% or more, 15% or more, or 20% or more, and may be 90% or less, 80% or less, 70% or less, 60% or less, or 50% or less. In one embodiment, the moisture content of the concrete sludge is 40 to 50%.

[0028] Concrete sludge contains cement hydrates formed when cement is mixed with water. Examples of cement hydrates include calcium silicate hydrate (tobermorite, 3CaO·2SiO2·3H2O, calcium hydroxide (Ca(OH)2), calcium aluminate hydrate, and calcium aluminate trisulfate hydrate (ettringite, 3CaO·Al2O3·3CaSO4·32H2O).

[0029] The amount of concrete sludge used in preparing the mixture may be such that the mass of the sludge solids relative to the mass of the protein in the organic matter is 3 times or more, preferably 3.5 times or more, more preferably 4 times or more, even more preferably 4.5 times or more, and particularly preferably 5 times or more.

[0030] Ferrous iron (Fe(I)) is a compound of ferrous iron (Fe 2+ Any compound capable of supplying iron (II ions) may be used, and inorganic iron salts such as iron sulfate (II), iron chloride (II), and iron nitrate (II), particularly iron sulfate (II) or iron chloride (II), are preferred. The inorganic iron salt divalent iron compound may be anhydrous or hydrated. In preparing the mixture, the divalent iron compound is preferably used in the form of a liquid, for example, in the form of an aqueous solution.

[0031] Phosphate compounds consist of phosphate ions (PO4 3- Any compound capable of supplying ions (ions) may be used. Examples of the phosphate compound include orthophosphoric acid (H3PO4) or a salt thereof, such as monopotassium phosphate, dipotassium phosphate, tripotassium phosphate, monosodium phosphate, disodium phosphate, trisodium phosphate, monoammonium phosphate, diammonium phosphate, etc. In preparing the mixture, the phosphate compound is preferably used in the form of a liquid, for example, in the form of an aqueous solution.

[0032] In preparing the mixture, the iron compound and the phosphate compound are used so that the mass ratio of iron in the iron compound to phosphoric acid in the phosphate compound is 1:2 to 1:8, preferably 1:3 to 1:6, and more preferably 1:3 to 1:5.

[0033] The amounts of the divalent iron compound and the phosphate compound used in the mixture preparation step may be amounts that make the pH of the mixture prepared 12.5 or less. The pH of the mixture prepared in the mixture preparation step may be 10 or more, preferably 10.5 or more, more preferably 11 or more, and even more preferably 11.5 or more, in order to prevent putrefaction of organic matter. The pH of the mixture may be measured immediately after preparation or after leaving it to stand for about one day after preparation, by adding about the same amount of water as necessary.

[0034] In one embodiment, the amount of the divalent iron compound and the phosphate compound used in the preparation of the mixture may be an amount that makes the pH of the concrete sludge 12.5 or less when added to the concrete sludge. The amount of the divalent iron compound and the phosphate compound may be determined in advance before the preparation of the mixture by performing a preliminary test of adding them to the concrete sludge, or the amount added may be adjusted by adding the divalent iron compound and the phosphate compound little by little to the concrete sludge while measuring the pH during the preparation of the mixture. The pH of the concrete sludge can be measured by using the sludge or sludge solids generated in a ready-mix concrete plant, or by adding water or recovered water to the sludge or sludge solids, and adding about the same amount of water as necessary.

[0035] In one embodiment, the amount of the divalent iron compound used in the mixture preparation step corresponds to the amount of a solution of a divalent iron compound having a concentration of 0.1 mass% or more, preferably 0.2 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.8 mass% or more, calculated as iron, added to a concrete sludge having a moisture content of 40 to 50% by mass or more. In another embodiment, the amount of the phosphoric acid compound used in the mixture preparation step corresponds to the amount of a solution of a phosphoric acid compound having a concentration of 0.4 mass% or more, preferably 0.8 mass% or more, more preferably 2.0 mass% or more, and even more preferably 3.2 mass% or more, added to a concrete sludge having a moisture content of 40 to 50% by mass or more.

[0036] When preparing the mixture, there is no restriction on the order of mixing the four components, the protein-containing organic matter, the concrete sludge, the divalent iron compound, and the phosphate compound, and all of them may be mixed at the same time, any two of the components may be mixed first, and then the remaining two components may be added simultaneously or sequentially and mixed, or a mixture of the remaining two components may be added and mixed, or any three of the components may be mixed first, and then the remaining components may be added and mixed.

[0037] When preparing the mixture, the divalent iron compound and the phosphate compound can be added and mixed with other components, preferably in a form dissolved in a liquid, for example, in the form of an aqueous solution, in order to facilitate uniform mixing. In the present invention, the divalent iron compound and the phosphate compound dissolved in a liquid are also called liquids. The liquid may be one in which the divalent iron compound and the phosphate compound are dissolved separately, or one in which both the divalent iron compound and the phosphate compound are dissolved.

[0038] The amount of the liquid agent used to prepare the mixture and the concentration of the divalent iron compound and the phosphate compound in the liquid agent are not limited as long as the divalent iron compound and the phosphate compound are added to the protein-containing organic matter and the concrete sludge in an amount that makes the pH of the mixture to be prepared 10 to 12.5. The liquid agent is mixed uniformly even if the amount added is very small, for example, at least 1 mL, for example, about 1 to 10 mL, per 100 g of concrete sludge. Without being bound by theory, it is believed that even if the amount of the liquid agent added is small, free water is generated by the reaction between the phosphoric acid contained in the liquid agent and the cement hydrate such as ettringite contained in the concrete sludge, and as a result, the water content of the concrete sludge is improved and uniform mixing is achieved.

[0039] The production method of the present invention includes a step of holding the mixture for at least 1 hour (hereinafter referred to as the holding step). The holding time is not limited as long as it is 1 hour or more, and may be, for example, 1 hour or more, 3 hours or more, 6 hours or more, 12 hours or more, or 24 hours or more, and may be 14 days or less, 10 days or less, 7 days or less, 5 days or less, 3 days or less, or 2 days or less. The holding is typically performed under atmospheric pressure and at ambient temperature. During the holding step, the mixture may be left to stand or may be stirred continuously or intermittently. There is no particular limitation on the stirring means, and the stirring may be performed manually, with a stirring device, or with a mechanical means such as a backhoe, depending on the volume of the mixture.

[0040] According to the manufacturing method of the present invention, it is possible to manufacture a treated concrete sludge product containing the organic matter, in which the generation of ammonia is suppressed. The treated concrete sludge product referred to in the present invention is a composition containing a protein-containing organic matter, concrete sludge, a divalent iron compound, a phosphate compound, and a substance generated from these. The suppression of ammonia generation can be confirmed by comparing with a case in which the protein-containing organic matter is directly treated as waste, or by comparing with a case in which the protein-containing organic matter is mixed with concrete sludge and treated without adding a divalent iron compound and a phosphate compound.

[0041] The treated concrete sludge produced by the manufacturing method of the present invention is capable of suppressing the generation of ammonia, as well as adsorbing hydrogen sulfide gas and stably retaining harmful metals such as chromium, cadmium, and arsenic.

[0042] Without being bound by theory, the reaction that occurs in the manufacturing method of the present invention is presumed to be as follows. The mixture has a high pH because it contains concrete sludge, which is a strong alkali, and this inhibits the decay of organic matter. In addition, the phosphoric acid in the mixture reacts with the calcium contained in the concrete sludge to form hydroxyapatite, which adsorbs ammonia and inhibits the generation of ammonia from organic matter.

[0043] Hexavalent chromium contained in concrete sludge is reduced to trivalent chromium by divalent iron, and then binds to hydroxyapatite, thereby suppressing elution. Even if the organic matter contains harmful metals such as cadmium or arsenic, these harmful metals are retained in the treated concrete by the strong alkaline environment caused by the concrete sludge or by binding to hydroxyapatite, thereby suppressing elution. Even if the pH of the treated concrete sludge decreases over time, creating an environment in which harmful metals are more likely to elute, the elution of harmful metals is still suppressed by binding to hydroxyapatite.

[0044] The production method of the present invention may include a step of dehydrating or drying the mixture to form a solid after the holding step. The dehydration or drying step can be performed using, for example, a precipitation thickener, a dehydrator, or a dryer.

[0045] The treated concrete sludge produced by the production method of the present invention has the ability to adsorb hydrogen sulfide gas as described above, and therefore by burying the treated concrete sludge together with industrial waste, it is possible to adsorb hydrogen sulfide gas that may be generated from the industrial waste, for example hydrogen sulfide gas generated by the action of sulfate-reducing microorganisms from sulfate compounds in gypsum boards, etc. The present invention provides an invention relating to a method for suppressing release of hydrogen sulfide from landfill waste, which includes a step of burying the treated concrete sludge produced by the above-mentioned production method together with landfill waste.

[0046] The present invention also provides a method for suppressing generation of ammonia from an organic matter containing a protein, the method comprising the steps of preparing the mixture and holding the mixture.Furthermore, the present invention provides a method for suppressing elution of a harmful metal from an organic matter containing a protein and the harmful metal.

[0047] In addition, the present invention provides a kit for use in the above-mentioned method, comprising a divalent iron compound and a phosphate compound. The kit of the present invention preferably comprises the divalent iron compound and the phosphate compound in a form dissolved in a liquid, i.e., as a liquid preparation. The liquid preparation may be a combination of a liquid in which a divalent iron compound is dissolved and a plurality of liquids in which a phosphate compound is dissolved, or may be a single liquid in which both a divalent iron compound and a phosphate compound are dissolved.

[0048] For example, the concentration of the divalent iron compound in the solution is 0.1 mass% or more, preferably 0.2 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.8 mass% or more, calculated as iron. For example, the concentration of the phosphate compound in the solution is 0.4 mass% or more, preferably 0.8 mass% or more, more preferably 2.0 mass% or more, and even more preferably 3.2 mass% or more, calculated as phosphoric acid. In a preferred embodiment, the kit of the present invention, which is a solution, is used in an amount of at least 1 mL, for example 1 to 10 mL, per 100 g of concrete sludge.

[0049] The treated concrete sludge produced by the above-mentioned production method can be used as a substitute for concrete sludge, as a backfill material, a recycled roadbed material, a neutralizer for acidic soil, a neutralizer for acidic substances generated during garbage incineration, a soil cover material, and the like, which are generally expected as a method for reusing concrete sludge. In particular, the treated concrete sludge produced by the above-mentioned production method can adsorb harmful substances that may be generated from industrial waste, such as hydrogen sulfide gas generated by the action of sulfate-reducing microorganisms from sulfate compounds in gypsum boards, and is suitable for use as a soil cover material for covering industrial waste. A soil cover material containing the treated concrete sludge produced by the above-mentioned production method is also disclosed as a further invention.

[0050] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto. EXAMPLES

[0051] [Example 1] (1) Preparation of treated concrete sludge containing organic matter A solution was prepared by adding water to 5 g of iron (II) sulfate heptahydrate (Wako Pure Chemical Industries, Ltd.) and 5 g of 85% aqueous phosphoric acid solution (H3PO4, Wako Pure Chemical Industries, Ltd.) to make a 100 mL solution, and this solution was used as a treatment agent. The treatment agent contained 1.00% by mass of iron and 4.12% by mass of phosphoric acid.

[0052] The following five types of samples were prepared using the above treatment agent, concrete sludge (a) (water content 43%, taken about one year after being collected from a ready-mix concrete factory), and boiled scallop midgut gland (a) (protein content 20% by mass) discarded from a fishery processing plant. The scallop midgut gland (a) had decayed after being boiled and stored in a refrigerator, and was crushed in a mixer before use. Samples 1 to 5 were prepared by first mixing the concrete sludge and treatment agent, then adding the midgut gland and further mixing. 1: 1 part by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 2: 1.2 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 3: 1.5 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 4: 1.7 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 5: 2 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge

[0053] Table 1 shows information on each sample, such as the amount and ratio of each component. [Table 1]

[0054] (2) Evaluation of ammonia generation and fly larvae infestation Each sample was placed in a beaker, lightly covered with aluminum foil, and left to stand at room temperature. After 7 days, the intensity of the ammonia odor and the emergence of fly larvae were observed. The results are shown in Table 2. Samples 3 to 5 had a weaker ammonia odor than samples 1 and 2, and it was observed that the ammonia odor tended to weaken as the ratio of sludge solids to protein added increased. Samples 2 to 5 also suppressed the emergence of fly larvae. [Table 2]

[0055] [Example 2] (1) Preparation of treated concrete sludge containing organic matter The following four types of samples were prepared using the treatment agent prepared in Example 1(1) and the concrete sludge (a) and scallop midgut gland (a) used in Example 1(1). Samples C and D were prepared by first mixing the concrete sludge and treatment agent, then adding the midgut gland and further mixing. A: Concrete sludge + 2.0% by mass of treatment agent B: 1 part by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge C: 2 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge D: 2 parts by mass of concrete sludge + 1 part by mass of midgut gland

[0056] Table 3 shows information on each sample, such as the amount and ratio of each component. [Table 3]

[0057] (2)pH measurement Samples A to C with the treatment agent added were left to stand at room temperature, and the pH was measured over time. The pH was measured after sampling each sample, adding the same amount of water as the sampled amount, and leaving it to stand for one hour. For all of samples A to C, the pH after one day of standing was in the range of 10.8 to 11.6, and after 30 days of standing was in the range of 10.4 to 11.3, and no significant pH fluctuations were observed over time.

[0058] (3) Ammonia measurement Samples C and D, which were prepared separately from those for pH measurement, were each placed in a 300 ml Erlenmeyer flask and left to stand at room temperature, and ammonia gas was measured over time. Measurements were performed by sampling gas from the top of the Erlenmeyer flask using a Kitagawa gas detector tube (measurement range 5-260 ppm). The results are shown in Table 4. Sample C, which had the treatment agent added, had a lower ammonia gas concentration after 5 days compared to sample D, which had no treatment agent added. [Table 4]

[0059] [Example 3] (1) Preparation of treated concrete sludge containing organic matter The following two types of samples were prepared using the treatment agent prepared in Example 1(1), the concrete sludge (a) used in Example 1(1), and boiled scallop midgut gland (b) (protein content 20% by mass) discarded from a fishery processing plant. The scallop midgut gland (b) was frozen and stored immediately after boiling, and was then thawed, indicating that no decay had occurred. It was crushed in a mixer and used. Sample b was prepared by first mixing the concrete sludge and treatment agent, then adding the midgut gland and further mixing. a: 2 parts by mass of concrete sludge + 1 part by mass of midgut gland b: 2 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge

[0060] Table 5 shows information on each sample, such as the amount and ratio of each component. [Table 5]

[0061] (2) Ammonia measurement Each sample was placed in a 300 ml Erlenmeyer flask and left to stand at room temperature, and ammonia gas was measured over time. Measurements were performed by sampling gas from the top of the Erlenmeyer flask using a Kitagawa gas detector (measurement range 5-260 ppm). The results are shown in Table 6. Sample b, which had the treatment agent added, had a lower ammonia gas concentration after 5 days compared to sample a, which had no treatment agent added. [Table 6]

[0062] The midgut gland (b) used in Example 3 was fresher than the midgut gland (a) used in Examples 1 and 2, and no decay had occurred at the start of the test. From the results of Examples 1 to 3, it was confirmed that the generation of ammonia gas originating from the midgut gland at a wide range of concentrations can be suppressed by mixing concrete sludge and a treatment agent with the midgut gland.

[0063] [Example 4] (1) Preparation of treated concrete sludge containing organic matter The following two types of samples were prepared using the treatment agent prepared in Example 1(1), the concrete sludge (a) used in Example 1(1), and starfish (protein content 8% by mass) exterminated as pests. Raw starfish were crushed in a mixer before use. Sample d was prepared by first mixing the concrete sludge and treatment agent, then adding the starfish and further mixing. c: 2 parts by mass of concrete sludge + 1 part by mass of starfish d: 2 parts by mass of concrete sludge + 1 part by mass of starfish + 2.0% by mass of treatment agent relative to the sludge

[0064] Table 7 shows information on each sample, such as the amount and ratio of each component. [Table 7]

[0065] (2) Ammonia measurement Each sample was placed in a 300 ml Erlenmeyer flask and left to stand at room temperature, and ammonia gas was measured over time starting immediately after mixing. Measurements were performed by sampling gas from the top of the Erlenmeyer flask using a Kitagawa gas detector tube (measurement range 5-260 ppm). The results are shown in Table 8. Sample d, which contained the treatment agent, had a lower ammonia gas concentration after two days compared to sample c, which did not contain the treatment agent. [Table 8] [Example 5] (1) Preparation of treated concrete sludge containing organic matter The following six types of samples were prepared using the treatment agent prepared in Example 1(1), concrete sludge (b) (water content 43%, immediately after collection at a ready-mix concrete factory), and the scallop midgut gland (a) used in Example 1(1). Samples 1' to 5' were prepared by first mixing the concrete sludge and the treatment agent, then adding the midgut gland and further mixing. 0': Midgut gland only 1': 1 part by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 2': 1.2 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 3': 1.5 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 4': 1.7 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge 5': 2 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge

[0066] Table 9 shows information on each sample, such as the amount and ratio of each component. [Table 9]

[0067] (2) Ammonia measurement Each sample was placed in a 300 ml Erlenmeyer flask and allowed to stand in a thermostatic chamber at 25°C, and ammonia gas was measured after 15 and 25 days. Measurements were performed by collecting gas from the top of the beaker using a Kitagawa gas detector (measurement range 5-260 ppm). The results are shown in Table 10. Samples 1'-5' had lower ammonia gas concentrations after both 15 and 25 days compared to sample 0', which did not contain concrete sludge or treatment agent. In addition, in the samples after 15 days, a tendency was observed for the ammonia gas concentration to decrease as the ratio of sludge solids to protein added increased. [Table 10]

[0068] [Example 6] (1) Preparation of treated concrete sludge containing organic matter The following six types of samples were prepared using the treatment agent prepared in Example 1(1), the concrete sludge (b) (water content 43%) used in Example 3(1), and the scallop midgut gland (b) used in Example 3(1). Samples C' and D' were prepared by first mixing the concrete sludge and the treatment agent, then adding the midgut gland and further mixing. A': Concrete sludge only B': Concrete sludge + 2.0% by mass of treatment agent relative to the sludge C': 1 part by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge D': 2 parts by mass of concrete sludge + 1 part by mass of midgut gland + 2.0% by mass of treatment agent relative to the sludge E': 2 parts by mass of concrete sludge + 1 part by mass of midgut gland F': 1 part by mass of concrete sludge + 1 part by mass of midgut gland + water equivalent to 2.0% by mass of sludge

[0069] Table 11 shows information on each sample, such as the amount and ratio of each component. [Table 11]

[0070] (2)pH measurement Samples A' to D' were left to stand at room temperature, and the pH was measured over time. The pH was measured by taking a sample from each sample, adding the same amount of water as the sampled amount, and leaving it to stand for one hour. The results are shown in Table 12. No significant pH change over time was observed in any of the samples. [Table 12]

[0071] (3) Ammonia measurement Samples D' and E', which were prepared separately from those for pH measurement, were each filled into a 300 ml Erlenmeyer flask and left to stand at room temperature, and ammonia gas was measured over time starting immediately after mixing. Measurements were performed by sampling gas from the top of the Erlenmeyer flask using a Kitagawa gas detector tube (measurement range 5-260 ppm). The results are shown in Table 13. The ammonia gas concentration was lower at all times in sample D', which had the treatment agent added, compared to sample E', which had no treatment agent added. [Table 13]

[0072] (4)Measurement of hazardous metal elution concentration Samples C' and F', which were prepared separately from those for pH measurement, were left to stand at room temperature. After three days, twice the amount of water was added, mixed, and then left to stand to collect the supernatant. The supernatant was filtered through Advantec filter paper type 5A (retention particle size 7 μm), and the filtrate was further pressure filtered using Advantec DISMIC syringe filter (pore size 0.8 μm, cellulose acetate). The obtained filtrate was used as is or adjusted to pH 5 as an analytical sample to calculate the concentrations (ppm) of eluted cadmium, arsenic, and hexavalent chromium.

[0073] Cadmium was measured by flame atomic absorption spectrometry as specified in JIS K 0102-55.1. Arsenic was measured using Pack Test (registered trademark) Arsenic (low concentration) (Kyoritsu Chemical Laboratory), and hexavalent chromium was measured using Pack Test (registered trademark) Cr 6+ (Kyoritsu Chemical Laboratory) was used.

[0074] The results are shown in Table 14. For cadmium, sample C' to which a treatment agent was added had a lower elution concentration than sample F' to which no treatment agent was added, both when the pH was adjusted to 5 and when the pH was not adjusted. For arsenic, when the pH was not adjusted, the elution concentration did not change whether a treatment agent was added or not, but when the pH was adjusted to 5, the elution concentration was lower in sample C' to which a treatment agent was added than in sample F' to which no treatment agent was added. For hexavalent chromium, sample C' to which a treatment agent was added had a lower elution concentration than sample F' to which no treatment agent was added. [Table 14]

[0075] These results confirmed that by mixing concrete sludge and a treatment agent into the mid-gut gland, the leaching of hexavalent chromium and cadmium originating from the mid-gut gland can be suppressed, and that even when the pH of the treated concrete sludge decreases over time, creating an environment prone to the leaching of harmful metals, the leaching of cadmium and arsenic can be suppressed.

[0076] (5) Hydrogen sulfide gas adsorption test A hydrogen sulfide gas adsorption test was conducted using crushed sample C' prepared separately for pH measurement and hazardous metal elution concentration measurement. The configuration of the device used in the test is explained with reference to Figure 1. 200 mL of a 1% by mass aqueous solution of sodium sulfide nonahydrate (Wako Pure Chemical Industries) was placed in a Muenke-type washing bottle 11 and connected to a micropipette 12 and column 13 via a tube. The column 13 is a cylindrical column with a diameter of 65 mm, a top diameter of 100 mm, and a length of 165 mm, and the bottom of the column is filled with cotton 15, and a hole is made in the top of the column to connect a gas detector 14 (Cure 2 suction type / PGM-2400P). When hydrochloric acid is dropped from the micropipette 12, hydrogen sulfide gas is generated in the washing bottle 11 and is sucked into the gas detector 14 through the column 13.

[0077] When 5 mL of 35% hydrochloric acid was dropped into the sodium sulfide aqueous solution, the hydrogen sulfide gas concentration measured by gas detector 14 exceeded 100 ppm after 5 seconds. When the hydrogen sulfide gas concentration at this point was measured by suction using a Kitagawa gas detector tube, it was confirmed that 200 ppm of hydrogen sulfide gas had been generated.

[0078] After the tube connecting the column 13 and the washing bottle 11 was closed, 3 g of crushed material of sample C' was filled on top of the cotton 15 at the bottom of the column 13. The tube connecting the column 13 and the washing bottle 11 was opened, and hydrogen sulfide gas was passed through the crushed material to conduct an adsorption test. The hydrogen sulfide gas concentration measured by the gas detector 14 was 0 ppm for up to 12 hours after the start of passing hydrogen sulfide gas through the crushed material. From this result, it was confirmed that the treated concrete sludge obtained by mixing concrete sludge and a treatment agent in the midgut gland has the ability to adsorb hydrogen sulfide gas. [Explanation of symbols]

[0079] 1. Muenke washing bottle 2 Micropipettes 3 Glass columns 4 Gas detectors 5 Cotton plug 6 Test items 7 Rubber stopper

Claims

1. A method for producing a treated concrete sludge product containing organic matter, in which generation of ammonia is suppressed, comprising the steps of preparing a mixture of a protein-containing organic matter, concrete sludge, a divalent iron compound, and a phosphate compound, and holding the mixture for at least one hour, The method according to claim 1, wherein the mass ratio of iron in the divalent iron compound to phosphoric acid in the phosphoric acid compound used in the preparation of the mixture is 1:2 to 1:8, and the pH of the prepared mixture is 10 to 12.

5.

2. The method according to claim 1, wherein the mass of the solids in the concrete sludge is three times or more the mass of the protein in the organic matter.

3. 2. The method according to claim 1, wherein the mixture is prepared by mixing a protein-containing organic matter, concrete sludge, and a liquid having dissolved therein a divalent iron compound and a phosphate compound.

4. 2. The method according to claim 1, wherein the divalent iron compound is iron sulfate (II) or iron chloride (II).

5. The method of claim 1 , wherein the phosphoric acid compound is orthophosphoric acid or a salt thereof.

6. The method according to claim 1, wherein the protein-containing organic matter is seafood residue.

7. 2. The method of claim 1, wherein the protein-containing organic matter is fish or shellfish viscera, shell attachments, or starfish.

8. 2. The method according to claim 1, wherein elution of harmful metals from treated concrete sludge is suppressed.

9. A method for suppressing ammonia generation from protein-containing organic matter, the method comprising the steps of preparing a mixture of protein-containing organic matter, concrete sludge, a divalent iron compound, and a phosphate compound, and holding the mixture for at least one hour, The method according to claim 1, wherein the mass ratio of iron in the divalent iron compound to phosphoric acid in the phosphoric acid compound used in the preparation of the mixture is 1:2 to 1:8, and the pH of the prepared mixture is 10 to 12.

5.

10. A kit for use in the method according to any one of claims 1 to 9, comprising a liquid in which a divalent iron compound and a phosphate compound are dissolved, the mass ratio of iron in the divalent iron compound to phosphoric acid in the phosphate compound being 1:2 to 1:

8.

11. The kit according to claim 10, wherein the divalent iron compound is iron sulfate (II) or iron chloride (II).

12. The kit according to claim 10, wherein the phosphate compound is orthophosphoric acid or a salt thereof.

13. A method for suppressing release of hydrogen sulfide from landfill waste, comprising a step of burying treated concrete sludge produced by the method according to any one of claims 1 to 8 together with the landfill waste.

Citation Information

Patent Citations

  • Ammoniac odor remover for cement blend

    JP2000203908A

  • Building material and method for producing the same

    JP2006001795A

  • Waste treatment method, waste treatment apparatus for executing the method, fired pellets manufactured by the method or the apparatus, and bottom sediment improving method using the fired pellets

    JP2015123402A

  • Method for manufacturing treated concrete sludge

    JP7117809B1

  • Neutralization treatment method for ready-mixed concrete sludge, and neutralization treatment material

    JP2014087723A