Thermoplastic resin film, adhesive film, and adhesive film for semiconductor manufacturing process
A three-layer thermoplastic resin film with specific resin compositions addresses heat resistance, surface roughness, and blocking issues in semiconductor manufacturing, enhancing handling and flexibility while maintaining transparency.
Patent Information
- Application Number
- JP2023181601
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2023-10-23
- Publication Date
- 2024-10-31
AI Technical Summary
Existing adhesive films used in semiconductor manufacturing processes face issues with heat resistance, surface roughness, transparency, and blocking between films, particularly during heating and laser dicing processes, which affect handling and flexibility.
A thermoplastic resin film composed of at least three layers, including a surface layer, a back layer, and an intermediate layer, utilizing high-density polyethylene, homopolypropylene, and thermoplastic elastomers, with specific resin composition ratios to achieve heat resistance, low surface roughness, and high transparency while preventing film blocking.
The film provides sufficient heat resistance, excellent handling and flexibility, and suppresses blocking between films, ensuring high transparency and ease of use in semiconductor manufacturing processes.
Smart Images

Figure 2024155684000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin film that is suitably used as a substrate for adhesive films (tapes) and the like used in semiconductor manufacturing processes, an adhesive film in which an adhesive layer is provided on the film, and an adhesive film for semiconductor manufacturing processes made of the film. [Background technology]
[0002] Conventionally, films made of polyvinyl chloride resin (hereinafter also referred to as "PVC-based films"), which have excellent colorability, processability, scratch resistance, weather resistance, etc., have been widely used as the substrate for adhesive films (tapes) used in the semiconductor manufacturing process, decorative adhesive films (tapes) such as stickers, labels, and marking films attached to signs, automobiles, etc. to add design to them, decorative sheets, etc.
[0003] The PVC film itself has rigidity, but a plasticizer is added to impart flexibility so that the film can function as an adhesive film. However, depending on the plasticizer used, the film may have poor compatibility with the adhesive, resulting in poor stability when used as an adhesive film, and the plasticizer may bleed out significantly. In addition, there is a tendency for restrictions on the use of plasticizers to be strengthened. Therefore, polyolefin resin films have come to be widely used as an alternative material to PVC films.
[0004] Furthermore, in the process of manufacturing semiconductors, adhesive films for semiconductor wafer processing are used when cutting semiconductor wafers, packages, etc., and due to the problems described above, there are an increasing number of cases in which polyolefin-based resin films are used (e.g., Patent Document 1).
[0005] In recent years, semiconductor elements have become smaller and thinner, and in addition to the flexibility required for films to be easy to handle and expand, in order to prevent chip damage and loss during expansion, heat resistance is also required for films used in the semiconductor manufacturing process, as heating is anticipated in processes such as heating the wafer and adhesive film to bond them more firmly together, and heating the expansion process after dicing. In addition to blade dicing using a rotating blade, there are also cases where it is required to apply the film to processes such as laser dicing, in which a part of a semiconductor wafer is modified by irradiating it with laser light and then the wafer is divided by stretching it, and stealth dicing. In such processes using laser light, the laser light may be irradiated through a film or tape used in the semiconductor manufacturing process, and in such cases, there is a tendency for a highly transparent film to be required in order to prevent the laser light from scattering and to focus it accurately on the wafer.
[0006] Patent Document 2 discloses a substrate film for dicing that uses a polyethylene resin in order to maintain expandability even at low temperatures. Patent Document 3 discloses a substrate film for use in semiconductor manufacturing processes that is provided with antistatic properties and has excellent flexibility and heat resistance. Patent Document 4 discloses a dicing sheet that has small surface roughness and excellent transparency.
[0007] However, the film described in Patent Document 2 uses only a polyethylene resin with a relatively low melting point, and although it is considered to have excellent low-temperature expandability, it is considered that there is room for improvement in heat resistance. Also, the film described in Patent Document 3 has excellent antistatic performance and heat resistance, but there is room for improvement in terms of suppressing problems caused by blocking between films when obtaining a film with small surface roughness and high transparency. The sheet described in Patent Document 4 is described as a film having small surface roughness and excellent transparency. However, like the sheet described in Patent Document 3, it is presumed that there is room for improvement in terms of suppressing defects due to blocking, as well as in terms of the heat resistance of the resin. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 09-008111 [Patent Document 2] JP 2018-125521 A [Patent Document 3] JP 2020-84143 A [Patent Document 4] Patent No. 6980684 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0009] In view of the above problems, the present invention aims to provide a film that has sufficient heat resistance, small surface roughness and high transparency even in cases where heating is performed in the semiconductor manufacturing process or where suppression of scattering of laser light is required, and further to provide a thermoplastic resin film that can suppress blocking between films when handling the film and has excellent handleability and flexibility. Another object of the present invention is to provide a pressure-sensitive adhesive film that can be suitably used in semiconductor manufacturing processes by providing a pressure-sensitive adhesive layer on the thermoplastic resin film. [Means for solving the problem]
[0010] The present inventors have conducted extensive research into thermoplastic resin films that use specific resin compositions in each layer, thereby achieving not only heat resistance, ease of handling, and flexibility, but also suppression of blocking between films, even in films with low surface roughness and high transparency, and have completed the present invention.
[0011] That is, the gist of the present invention is as follows. [1] A thermoplastic resin film consisting of at least three layers: a surface layer, a back layer, and an intermediate layer, At least one of the front and back layers contains high density polyethylene and homopolypropylene, The intermediate layer contains high density polyethylene and homopolypropylene, and also contains at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes, The thermoplastic resin film is characterized by satisfying the following requirements. (1) When the total amount of thermoplastic resins contained in the resin composition constituting at least one of the front and back layers is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of the front and back layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less. [2] The thermoplastic resin film according to [1], wherein the thermoplastic elastomer is a styrene-based elastomer and / or an olefin-based elastomer. [3] The thermoplastic resin film according to [1] or [2], wherein the haze of the thermoplastic resin film is 50% or less. [4] The thermoplastic resin film according to any one of [1] to [3], wherein the thermoplastic resin film has a tensile modulus within a range of 100 to 600 MPa. [5] An adhesive film comprising the thermoplastic resin film according to any one of [1] to [4] and an adhesive layer provided on at least one surface of the thermoplastic resin film. [6] The adhesive film for semiconductor manufacturing process according to [5], which is used in the semiconductor manufacturing process. Effect of the Invention
[0012] By using the resin composition described in the present invention to produce a thermoplastic resin film, it is possible to provide a film that has sufficient heat resistance, small surface roughness, and high transparency even when a heating step or suppression of scattering of laser light is required in the semiconductor manufacturing process, and further, it is possible to provide a thermoplastic resin film that can suppress blocking between films when the film is handled, and has excellent handleability and flexibility. In addition, the present invention can provide an adhesive film that can be suitably used in the semiconductor manufacturing process by providing an adhesive layer on the thermoplastic resin film.
[0013] According to the present invention, it is possible to obtain a thermoplastic resin film which has sufficient heat resistance even when a heating step is expected to be performed in the semiconductor manufacturing process, is excellent in handleability and flexibility, and suppresses blocking between films even when the film has a small surface roughness and is highly transparent, and the thermoplastic resin film can be suitably used in the semiconductor manufacturing process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified and practiced in various ways within the scope of the gist. In addition, when the expression "~" is used in this specification, it is used as an expression including the numerical value or physical property value before and after it.
[0015] The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers, namely, a front layer, a back layer, and an intermediate layer, in which at least one of the front layer and the back layer contains high density polyethylene and homopolypropylene, and the intermediate layer contains high density polyethylene and homopolypropylene, and also contains at least one selected from the group consisting of a thermoplastic elastomer and a random polypropylene, and which satisfies the following requirements described later. (1) When the total amount of thermoplastic resins contained in the resin composition constituting at least one of the front and back layers is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of the front and back layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
[0016] The resins constituting the thermoplastic resin film of the present invention will be described in detail below.
[0017] <High density polyethylene> The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers, a surface layer, a back layer and an intermediate layer, and at least one of the surface layer and the back layer and the intermediate layer contain high-density polyethylene. By incorporating high density polyethylene in at least one of the front and back layers, the elastic modulus of the front and back layers can be improved, and even if the surface roughness of the front and back layers of the film is small, blocking between the films when the film is wound into a roll can be suppressed. In addition, by incorporating high density polyethylene in the intermediate layer, it is possible to improve compatibility with the front and / or back layer, and to improve adhesion between each layer. There are no particular limitations as long as it is a high-density polyethylene, and high-density polyethylene composed of an ethylene homopolymer or a copolymer of ethylene, mainly composed of ethylene and other monomers copolymerizable with ethylene (hereinafter referred to as other monomers) can be used. Examples of the other monomers include α-olefins having 3 or more carbon atoms. Examples of α-olefins having 3 or more carbon atoms include propylene, 1-butene, isobutene, 1-pentene, 2-methyl-butene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-pentene, 1-octene, 1-decene, and 1-dodecene. From the viewpoint of availability of the monomer and the performance of the resulting high-density polyethylene, it is preferable that the number of carbon atoms is within the range of 3 to 20, among those having 3 or more carbon atoms.
[0018] The density of high density polyethylene is 0.940 to 0.970 g / cm 3 It is preferable that the density is within the range of 0.940 to 0.970 g / cm 3 By using a high-density polyethylene within this range, it is easy to adjust the elastic modulus of the surface layer and / or back layer and intermediate layer of the obtained thermoplastic resin film. More preferably, it is 0.942 to 0.968 g / cm 3 and more preferably in the range of 0.944 to 0.966. Methods for measuring density include Method A (underwater displacement method), Method B (pycnometer method), Method C (floating-sink method), and Method D (density gradient tube method) described in "JIS K 7112". There are no particular limitations on the measurement method, and an appropriate method can be selected and used.
[0019] The high density polyethylene preferably has a crystalline melting peak of 120° C. or higher. By having a crystalline melting peak of 120° C. or higher, it is possible to impart sufficient heat resistance to the obtained thermoplastic resin film. The crystalline melting peak is more preferably 125° C. or higher, and even more preferably 130° C. or higher. The crystalline melting peak can be measured using a differential scanning calorimeter according to "JIS K 7122".
[0020] Regarding the strength of the high density polyethylene, the tensile modulus of the film obtained from the high density polyethylene alone is preferably within the range of 600 to 1800 MPa. If the tensile modulus is within the range of 600 to 1800 MPa, it is possible to impart appropriate strength and flexibility to the thermoplastic resin film of the present invention. More preferably, it is within the range of 650 to 1750 MPa, and further preferably within the range of 700 to 1700 MPa. The tensile modulus can be measured according to the method described in "JIS K 7127". Various conditions such as the shape of the test piece, the test speed, and the distance between the chucks during measurement can be appropriately selected and used.
[0021] The melt flow rate of the high density polyethylene is appropriately selected depending on the molding method and application, but is preferably 0.1 to 50 g / 10 min, measured at a temperature of 190° C. and a load of 2.16 kg. If it is 0.1 g / 10 min or more, the moldability of the film is good, and if it is 50 g / 10 min or less, the thickness precision of the film can be maintained at a good level. More preferably, it is 0.5 to 40 g / 10 min, and even more preferably, it is 1.0 to 30 g / 10 min. The melt flow rate can be measured by the method described in "JIS K 7210". The conditions such as temperature and load during measurement can be appropriately selected depending on the material used and its characteristics.
[0022] Examples of commercially available high density polyethylene include Novatec HD "HJ360", Novatec HD "HJ491", Novatec HD "HF560", Novatec HD "HY350" (all manufactured by Japan Polyethylene Co., Ltd.), Santech HD "B161", Santech HD "J340", Santech HD "J241" (all manufactured by Asahi Kasei Corporation), Nipolon Hard "4000", Nipolon Hard "2000", Nipolon Hard "2500", and Nipolon Hard "LW13D" (all manufactured by Tosoh Corporation). These high density polyethylenes may be used alone or in combination of two or more types. They can be appropriately selected as needed, taking into consideration the film formability when obtaining a thermoplastic resin film, the heat resistance and flexibility of the obtained film, and blocking between films.
[0023] <Homopolypropylene> The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers, a surface layer, a back layer and an intermediate layer, and contains homopolypropylene on at least one side of the surface layer or the back layer and on the intermediate layer. By incorporating homopolypropylene into at least one of the surfaces of the front and back layers, it is possible to improve the elastic modulus of the front and back layers while imparting heat resistance. Furthermore, even if the surface roughness of the front and back layers of the film is small, it is possible to suppress blocking between the films when the film is wound into a roll. Furthermore, by incorporating homopolypropylene into the intermediate layer, it is possible to improve compatibility with the front and / or back layer, and it is possible to improve adhesion between each layer. The homopolypropylene used in the present invention is a homopolymer of propylene.
[0024] The homopolypropylene preferably has a crystalline melting peak of 140° C. or higher. By having a crystalline melting peak of 140° C. or higher, it is possible to impart sufficient heat resistance to the multilayer film obtained. It is more preferably 145° C. or higher, and even more preferably 150° C. or higher. The crystalline melting peak can be measured by the same method as described in the section on high-density polyethylene. Regarding the strength of homopolypropylene, the tensile modulus of a film obtained from the resin alone is preferably within the range of 600 to 1800 MPa. If the tensile modulus is within the range of 600 to 1800 MPa, it is possible to impart an appropriate strength to the film of the present invention. It is more preferably within the range of 650 to 1750 MPa, and further preferably within the range of 700 to 1700 MPa. The tensile modulus can be measured by the same method as described in the section on high density polyethylene. The melt flow rate of homopolypropylene is appropriately selected depending on the molding method and application, but is preferably 0.1 to 50 g / 10 min, measured at a temperature of 230° C. and a load of 2.16 kg. If it is 0.1 g / 10 min or more, the moldability of the film is good, and if it is 50 g / 10 min or less, the thickness precision of the film can be kept good. It is more preferably 0.5 to 40 g / 10 min, and even more preferably 1.0 to 30 g / 10 min. The melt flow rate can be measured by the same method as described in the section on high density polyethylene.
[0025] Commercially available homopolypropylene products include, for example, Novatec PP "MA3U" and Novatec PP "FY6HA" (both manufactured by Japan Polypropylene Corporation), PC412A, PC600A, PC600S, PLA00A (all manufactured by SunAllomer Corporation), F-730NV, F-744NP (all manufactured by Prime Polypropylene Corporation), Sumitomo Noblen "WF836DG3", and Sumitomo Noblen "FLX80H5" (all manufactured by Sumitomo Chemical Co., Ltd.). The homopolypropylene may be used alone or in combination of two or more kinds. It can be appropriately selected as necessary in consideration of film formability when obtaining a thermoplastic resin film, heat resistance and flexibility of the obtained film, blocking between films, etc.
[0026] <Thermoplastic elastomer> The intermediate layer of the thermoplastic resin film of the present invention contains at least one selected from the group consisting of a thermoplastic elastomer and random propylene as an essential component in addition to the above-mentioned high density polyethylene and homopolypropylene. By containing the thermoplastic elastomer, it becomes possible to adjust the flexibility and expandability of the obtained film to an appropriate range.
[0027] Examples of the thermoplastic elastomer include olefin-based elastomers, styrene-based elastomers, acrylic-based elastomers, vinyl chloride-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, fluorine-based elastomers, and silicone-based elastomers. Among the above thermoplastic elastomers, it is preferable to use an olefin-based elastomer or a styrene-based elastomer from the viewpoint of compatibility with the above-mentioned high density polyethylene and homopolypropylene, imparting flexibility to the obtained film, and transparency. The olefin-based elastomer and the styrene-based elastomer may be used alone, or may be used in combination, taking into consideration the film formability when obtaining a thermoplastic resin film and the flexibility of the obtained film. In addition, a plurality of types, such as two or more types of olefin-based elastomers and two or more types of styrene-based elastomers, may be used. Among them, it is more preferable to use an olefin-based elastomer and a styrene-based elastomer in combination from the viewpoint of adjusting flexibility.
[0028] The olefin-based elastomer is a soft resin containing a polyolefin-based resin and a rubber component, and may be one in which the rubber component is dispersed in the polyolefin-based resin, or one in which the two are copolymerized with each other. Specific examples of olefin-based elastomers include amorphous elastic copolymers mainly composed of olefins, such as ethylene-propylene copolymer elastomers, ethylene-1-butene copolymer elastomers, ethylene-propylene-1-butene copolymer elastomers, ethylene-1-hexene copolymer elastomers, ethylene-1-octene copolymer elastomers, ethylene-styrene copolymer elastomers, ethylene-norbornene copolymer elastomers, propylene-1-butene copolymer elastomers, ethylene-propylene-non-conjugated diene copolymer elastomers, ethylene-1-butene-non-conjugated diene copolymer elastomers, and ethylene-propylene-1-butene-non-conjugated diene copolymer elastomers, as well as derivatives and acid-modified derivatives thereof.
[0029] Commercially available examples of olefin-based elastomers include Wellnex "RFG4VM", Wellnex "RFX4V", Wellnex "RMG02" (all manufactured by Japan Polypropylene Corporation), Tufmer "A-4070S", Tufmer "A-4085S", Tufmer "BL2481M", Tufmer "BL3450M", Tufmer "XM7070", Tufmer "XM7080", Mirastomer (all manufactured by Mitsui Chemicals), ENGAGE, AFFINITY, and VERSIFY (all manufactured by The Dow Chemical Company). The olefin-based elastomer may be used alone or in combination of two or more kinds. It can be appropriately selected as necessary in consideration of film formability when obtaining a thermoplastic resin film, flexibility of the obtained film, blocking between films, etc.
[0030] Regarding the strength of the olefin-based elastomer, the tensile modulus of a film obtained from the resin alone is preferably within the range of 30 to 400 MPa. If the tensile modulus is within the range of 30 to 400 MPa, it is possible to impart appropriate flexibility to the film of the present invention. It is more preferably within the range of 30 to 300 MPa, and even more preferably within the range of 30 to 200 MPa. The tensile modulus can be measured by the same method as described in the section on high-density polyethylene.
[0031] The melt flow rate of the olefin elastomer is appropriately selected depending on the molding method and application, but is preferably 0.1 to 50 g / 10 min, measured under a temperature condition of 190°C or 230°C and a load of 2.16 kg. If it is 0.1 g / 10 min or more, the moldability of the film is good, and if it is 50 g / 10 min or less, the thickness precision of the film can be kept good. It is more preferably 0.5 to 40 g / 10 min, and even more preferably 1.0 to 30 g / 10 min. The melt flow rate can be measured by the same method as described in the section on high density polyethylene.
[0032] The styrene-based elastomer is preferably a block copolymer represented by the following formula (I) or (II). X-(YX)n …(I) (XY)n …(II) In general formulas (I) and (II), X is an aromatic vinyl polymer block (hereinafter, styrene component) typified by styrene, and in formula (I), the degree of polymerization at both ends of the molecular chain may be the same or different. Y is at least one selected from a butadiene polymer block, an isoprene polymer block, a butadiene / isoprene copolymer block, a hydrogenated butadiene polymer block, a hydrogenated isoprene polymer block, a hydrogenated butadiene / isoprene copolymer block, a partially hydrogenated butadiene polymer block, a partially hydrogenated isoprene polymer block, and a partially hydrogenated butadiene / isoprene copolymer block. n is an integer of 1 or more.
[0033] Specific examples of styrene-based elastomers include styrene-ethylene-butylene-styrene copolymers, styrene-ethylene-propylene-styrene copolymers, styrene-ethylene-ethylene-propylene-styrene copolymers, styrene-butadiene-butene-styrene copolymers, styrene-butadiene-styrene copolymers, styrene-isoprene-styrene copolymers, styrene-hydrogenated butadiene diblock copolymers, styrene-hydrogenated isoprene diblock copolymers, styrene-butadiene diblock copolymers, styrene-isoprene diblock copolymers, etc., among which styrene-ethylene-butylene-styrene copolymers, styrene-ethylene-propylene-styrene copolymers, styrene-ethylene-ethylene-propylene-styrene copolymers, and styrene-butadiene-butene-styrene copolymers are preferred. Also usable are block copolymers that are styrene-ethylene-butylene-crystalline olefin copolymers.
[0034] The melt flow rate of the styrene elastomer (measured at a temperature of 230°C under a load of 2.16 kg) is preferably 0.1 to 20 g / 10 min, more preferably 0.15 to 15 g / 10 min, and particularly preferably 0.2 to 10 g / 10 min. If the melt flow rate of the styrene elastomer is 0.1 g / 10 min or more and 20 g / 10 min or less, it is favorable in terms of compatibility with other resins and film formability. The melt flow rate can be measured by the same method as that described in the section on high density polyethylene.
[0035] The content of the styrene component in the styrene-based elastomer is preferably 50% by mass or less. If the content of the styrene component is 50% by mass or less, it is possible to impart flexibility to the obtained film. It is preferably 47% by mass or less, more preferably 44% by mass or less.
[0036] The content of styrene components and other components is as follows: 1 H-NMR and 13It can be measured by C-NMR. Here, the "styrene component content" refers to the content ratio (mass%) of aromatic vinyl polymer blocks, typically styrene, based on the mass of the styrene-based elastomer.
[0037] Examples of commercially available styrene-based elastomers having a styrene component content of 50% by mass or less include Tuftec H1221, Tuftec H1062, Tuftec H1521, Tuftec H1517, Tuftec H1052, Tuftec H1041, Tuftec P1083, Tuftec P1913, P5051 (all manufactured by Asahi Kasei Corporation), Septon 2004F, Septon 2063, Hybler 7311, Hybler 7311F, Hybler 7125F, Hybler 5127, Hybler 5125 (all manufactured by Kuraray Co., Ltd.), Dynaron 1320P, Dynaron 4600P, Dynaron 8300P, Dynaron 8903P (all manufactured by JSR Corporation), and the like.
[0038] The styrene-based elastomer may be used alone or in combination of two or more kinds. It can be appropriately selected as necessary in consideration of film-forming properties when obtaining a thermoplastic resin film, and flexibility, handling properties, and expandability of the obtained film.
[0039] It is preferable to use an olefin-based elastomer and a styrene-based elastomer in combination, since this makes it easier to adjust the flexibility and film-forming properties of the resulting thermoplastic resin film and also makes it easier to reduce cutting debris generated when cutting a wafer with a blade.
[0040] <Random polypropylene> The intermediate layer of the thermoplastic resin film of the present invention contains, as an essential component, at least one selected from the group consisting of a thermoplastic elastomer and a random propylene, in addition to the above-mentioned high density polyethylene and homopolypropylene. By including the random polypropylene, it becomes possible to adjust the flexibility and expandability of the obtained film to an appropriate range.
[0041] Examples of random polypropylene include copolymers of propylene, which are mainly composed of propylene, and other monomers copolymerizable with propylene. Examples of other monomers copolymerizable with propylene include ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 4-methyl-1-pentene, and 1-decene, and one or more of these are used.
[0042] The crystalline melting peak of the random polypropylene is preferably 110° C. or higher. By having a crystalline melting peak of 110° C. or higher, it becomes easy to adjust the heat resistance of the obtained thermoplastic resin film. It is more preferably 115° C. or higher, and even more preferably 120° C. or higher. The crystalline melting peak can be measured by the same method as described in the section on high density polyethylene.
[0043] Regarding the strength of the random polypropylene, the tensile modulus of a film obtained from the resin alone is preferably within the range of 200 to 800 MPa. If the tensile modulus is within the range of 200 to 800 MPa, it is possible to impart appropriate strength and flexibility to the thermoplastic resin film of the present invention. It is more preferably within the range of 200 to 700 MPa, and even more preferably within the range of 200 to 600 MPa. The tensile modulus can be measured by the same method as described in the section on high density polyethylene.
[0044] The melt flow rate of the random polypropylene is appropriately selected depending on the molding method and application, but is preferably 0.1 to 50 g / 10 min, measured at a temperature of 230° C. and a load of 2.16 kg. If it is 0.1 g / 10 min or more, the moldability of the film is good, and if it is 50 g / 10 min or less, the thickness precision of the film can be kept good. It is more preferably 0.5 to 40 g / 10 min, and even more preferably 1.0 to 30 g / 10 min. The melt flow rate can be measured by the same method as described in the section on high density polyethylene.
[0045] Commercially available random polypropylene products include, for example, Novatec PP "FW4BA", Novatec PP "FX3B" (both manufactured by Japan Polypropylene Corporation), PC630A, PC630S (both manufactured by SunAllomer Corporation), F-730NV, F-744NP (both manufactured by Prime Polypropylene Corporation), Sumitomo Noblen "FL6737", Sumitomo Noblen "S131" (all manufactured by Sumitomo Chemical Co., Ltd.), and the like.
[0046] <Other thermoplastic resins> In addition to high density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, other thermoplastic resins may be added to the thermoplastic resin film of the present invention as long as the heat resistance and flexibility are not impaired. Examples of other thermoplastic resins include polyethylene resins, cyclic olefin resins, and polymethylpentene resins.
[0047] Examples of polyethylene-based resins include ethylene homopolymers, copolymers of ethylene mainly composed of ethylene and other monomers copolymerizable therewith (low-density polyethylene (LDPE), high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), ethylene-based copolymers obtained by polymerization using a metallocene catalyst (metallocene-based polyethylene), ethylene-vinyl acetate copolymers, ethylene-methyl (meth)acrylate copolymers, ethylene-ethyl (meth)acrylate copolymers, ethylene-butyl (meth)acrylate copolymers, ethylene-(meth)acrylic acid copolymers, and metal ion crosslinked resins (ionomers) of ethylene-(meth)acrylic acid copolymers. Of these, it is preferable to use low density polyethylene (LDPE) and linear low density polyethylene (LLDPE) from the viewpoints of ease of availability, ease of handling of the resin, and ease of adjusting the flexibility and heat resistance of the resulting film.
[0048] The density of low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE) is 0.900 to 0.940 g / cm 3It is preferable that the density is in the range of 0.900 to 0.940 g / cm 3 By using one within this range, it is easy to adjust the heat resistance and flexibility of the resulting thermoplastic resin film. More preferably, it is 0.902 to 0.938 g / cm 3 and more preferably in the range of 0.904 to 0.936. The density can be measured by the same method as described in the section on high density polyethylene.
[0049] The crystalline melting peak of low density polyethylene (LDPE) and linear low density polyethylene (LLDPE) is preferably 70°C or higher. By having a crystalline melting peak of 70°C or higher, it becomes easy to adjust the heat resistance of the obtained thermoplastic resin film. It is more preferably 75°C or higher, and even more preferably 80°C or higher. The crystalline melting peak can be measured by the same method as described in the section on high density polyethylene.
[0050] Regarding the strength of low density polyethylene (LDPE) and linear low density polyethylene (LLDPE), the tensile modulus of a film obtained from these resins alone is preferably within the range of 30 to 400 MPa. If the tensile modulus is within the range of 30 to 400 MPa, it is easy to adjust the flexibility of the thermoplastic resin film of the present invention. It is more preferably within the range of 40 to 350 MPa, and even more preferably within the range of 50 to 300 MPa. The tensile modulus can be measured by the same method as described in the section on high density polyethylene.
[0051] Commercially available low-density polyethylene (LDPE) products include, for example, Novatec LD "LC500", Novatec LD "LC520", Novatec LD "LC720" (all manufactured by Japan Polyethylene Co., Ltd.), F224N, F324C, F522N (all manufactured by Ube Maruzen Polyethylene Co., Ltd.), and the like. Commercially available linear low-density polyethylene (LLDPE) products include, for example, Novatec LL "UF420" and Novatec LL "UF641" (both manufactured by Japan Polyethylene Co., Ltd.), Yumerit "0540F", and Yumerit "4040F" (both manufactured by Ube Maruzen Polyethylene Co., Ltd.).
[0052] Examples of cyclic olefin resins include norbornene polymers, vinyl alicyclic hydrocarbon polymers, and cyclic conjugated diene polymers. Among these, norbornene polymers are preferred. Examples of norbornene polymers include ring-opening polymers of norbornene monomers and norbornene copolymers obtained by copolymerizing norbornene monomers with α-olefins such as ethylene. Hydrogenated products of these may also be used.
[0053] As the polymethylpentene-based resin, it is preferable to use a homopolymer having methylpentene as a monomer or a copolymer with other monomers.Specific examples include a copolymer of α-olefin and 4-methylpentene-1, which are exemplified as other monomers copolymerizable with propylene for the polypropylene-based resin. When the polymethylpentene resin is a copolymer, the content of the α-olefin component used in the copolymerization is preferably 20% by mass or less. By making it 20% by mass or less, it is possible to suppress the decrease in the crystal melting peak. It is more preferably 10% by mass or less.
[0054] <Other ingredients> The thermoplastic resin film of the present invention may contain various additives in order to impart antistatic properties, heat resistance, weather resistance, and the like. Specific examples of the additives that may be used include antistatic agents, antioxidants, neutralizing agents, lubricants, antiblocking agents, plasticizers, heat stabilizers, light stabilizers, dyes and pigments, crystal nucleating agents, ultraviolet absorbers, fillers, inorganic fillers that impart rigidity, and elastomers other than those mentioned above that impart flexibility, within the scope of not impairing the effects of the present invention.
[0055] The polymer-type antistatic agent may be a known one, for example, a block copolymer of a hydrophobic block and a hydrophilic block. Examples of the polymer-type antistatic agent include a block copolymer formed by an ester bond, an ether bond, an amide bond, an imide bond, a urethane bond, a urea bond, or the like between the hydrophobic block and the hydrophilic block.
[0056] As the ultraviolet absorbing agent, known agents can be used, and examples thereof include benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, and triazine-based ultraviolet absorbing agents.
[0057] As the light stabilizer, a known one can be used, and examples thereof include hindered amine light stabilizers.
[0058] As the lubricant or antiblocking agent, it is preferable to use a silicone-olefin copolymer, since this has excellent compatibility with the above-mentioned polypropylene-based resins, polyethylene-based resins, etc., and makes it possible to prevent defects due to bleed-out on the surface of the obtained film and to impart long-term scratch resistance and slipperiness.
[0059] <Thermoplastic resin film> The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers, namely a front layer, a back layer, and an intermediate layer, in which at least one of the front layer and the back layer contains high density polyethylene and homopolypropylene, and the intermediate layer contains high density polyethylene and homopolypropylene, and also contains at least one member selected from the group consisting of a thermoplastic elastomer and a random polypropylene, and which satisfies the following requirements. (1) When the total amount of thermoplastic resins contained in the resin composition constituting at least one of the front and back layers is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of the front and back layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
[0060] The total mass of the thermoplastic resin contained in the resin composition constituting at least one of the front and back layers means the combined total mass of high-density polyethylene, homopolypropylene, and the aforementioned thermoplastic elastomers, random polypropylene, and other thermoplastic resins (hereinafter also referred to as "other thermoplastic resins") that may be optionally contained, and the content of high-density polyethylene, homopolypropylene, and other thermoplastic resins is specified with the total mass of the thermoplastic resins being 100 mass%. Here, the contents of high-density polyethylene, homopolypropylene, and other thermoplastic resins in the resin composition constituting at least one of the front and back layers can be specified as follows: high-density polyethylene is 20 to 90 mass%, homopolypropylene is 10 to 75 mass%, and other thermoplastic resins are 0 to 30 mass% (the total mass of high-density polyethylene, homopolypropylene, and other thermoplastic resins is 100 mass%). In addition, the mass of the entire thermoplastic resin contained in the resin composition constituting the intermediate layer means the total mass of the high-density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and the masses of the other thermoplastic resins mentioned above that may be optionally contained, and the contents of the high-density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and other thermoplastic resins are specified with the mass of the entire thermoplastic resin being 100 mass%. Here, the contents of high density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and other thermoplastic resins in the resin composition constituting the intermediate layer can be specified as follows: high density polyethylene content is 3 to 15 mass%, homopolypropylene content is 10 to 50 mass%, at least one selected from the group consisting of thermoplastic elastomer and random polypropylene content is 10 to 85 mass%, and other thermoplastic resin content is 0 to 40 mass% (the total amount of high density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and other thermoplastic resins is 100 mass%).
[0061] By containing a predetermined amount of the high density polyethylene and homopolypropylene in the resin composition constituting at least one of the front and back layers, it is possible to adjust the heat resistance and flexibility of the obtained film, and furthermore, it is possible to suppress blocking between the films. When the total amount of the thermoplastic resin contained in the resin composition constituting at least one of the front and back layers of the film is taken as 100 mass%, the high density polyethylene is 20 to 90 mass% and the homopolypropylene is 10 to 75 mass%. By containing the high density polyethylene in the range of 20 to 90 mass%, it is possible to impart flexibility without impairing the heat resistance of the film, and furthermore, it is possible to improve the blocking property between the films. The preferred range of the high density polyethylene content is more preferably 25 to 85 mass%, and even more preferably 30 to 80 mass%. By setting the homopolypropylene content within the range of 10 to 75% by mass, it is possible to impart heat resistance to the film without impairing flexibility, and to improve the blocking properties between films. The homopolypropylene content is more preferably within the range of 12 to 65% by mass, and even more preferably within the range of 14 to 60% by mass. In addition, the total amount of high density polyethylene and homopolypropylene is preferably 45% by mass or more. By making the total amount of high density polyethylene and homopolypropylene 45% by mass or more, it is possible to impart heat resistance and flexibility to the film, and it is possible to improve the blocking property between the films. It is more preferably 50% by mass or more, and even more preferably 55% by mass or more.
[0062] The resin composition constituting at least one of the front and back layers can contain the above-mentioned other thermoplastic resins and other components in addition to high density polyethylene and homopolypropylene. When other thermoplastic resins are added, there is a possibility that flexibility and heat resistance are impaired, and furthermore, blocking between films may easily occur, so it is necessary to adjust the total amount of thermoplastic resins contained in the resin composition constituting at least one of the front and back layers to be within the range of 0 to 30% by mass when the total amount is taken as 100% by mass. It is more preferably within the range of 0 to 25% by mass, and even more preferably within the range of 0 to 20% by mass. In addition, the resin composition used for the front layer and the back layer may be the same or different. As long as the heat resistance, flexibility, and blocking property between films of the obtained film are not impaired, it is possible to use high density polyethylene, homopolypropylene, and other thermoplastic resins within a predetermined range. When different performance is required on the front and back, it is preferable to use different resin compositions within a range that does not impair flexibility, heat resistance, and blocking property between films. Regarding the strength of the resin composition constituting at least one layer of the front layer and the back layer, it is preferable that the tensile modulus of the film obtained from the resin composition alone is in the range of 500 to 1800 MPa. If the tensile modulus is in the range of 500 to 1800 MPa, it is easy to suppress blocking between the thermoplastic resin films of the present invention. It is more preferable that the tensile modulus is in the range of 550 to 1750 MPa, and even more preferable that it is in the range of 600 to 1700 MPa. From the viewpoint of suppressing blocking between films, it is preferable that both the front layer and the back layer are in the above tensile modulus range. The tensile modulus can be measured by the same method as described in the section on high density polyethylene.
[0063] By containing a predetermined amount of at least one selected from the group consisting of the aforementioned high-density polyethylene and homopolypropylene, thermoplastic elastomer and random polypropylene in the resin composition used for the intermediate layer, it becomes possible to adjust the flexibility of the obtained film while maintaining heat resistance, and further to improve the adhesion between each layer. The contents of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene are, when the total thermoplastic resins contained in the resin composition constituting the intermediate layer of the film is taken as 100% by mass, 3 to 15% by mass of high-density polyethylene, 10 to 50% by mass of homopolypropylene, 10 to 85% by mass of at least one selected from the group consisting of thermoplastic elastomer and random polypropylene, and 0 to 40% by mass of other thermoplastic resins. By setting the content of high density polyethylene within the range of 3 to 15% by mass, the heat resistance and flexibility of the film are not impaired, and it is possible to impart adhesion to the front and back layers. The content of high density polyethylene is preferably within the range of 5 to 13% by mass, more preferably within the range of 7 to 11% by mass. When the homopolypropylene content is within the range of 10 to 50% by mass, it is possible to impart heat resistance to the film. The homopolypropylene content is preferably within the range of 13 to 47% by mass, more preferably within the range of 16 to 44% by mass. The flexibility of the film can be easily adjusted by setting the content of at least one selected from the group consisting of thermoplastic elastomer and random polypropylene within the range of 10 to 85% by mass. The content of the thermoplastic elastomer and random polypropylene is preferably within the range of 15 to 80% by mass, more preferably within the range of 20 to 75% by mass, and further preferably within the range of 25 to 70% by mass. In this specification, the content of at least one selected from the group consisting of thermoplastic elastomer and random polypropylene is within the range of 10 to 85 mass%, meaning that when either one of thermoplastic elastomer or random polypropylene is selected, the content of said one is within the range of 10 to 85 mass%, or when two or more of thermoplastic elastomer and random polypropylene are selected, the total content of said two or more is within the range of 10 to 85 mass%. Either case is within the scope of the present invention. Furthermore, when two or more of a thermoplastic elastomer and a random polypropylene are selected, it is preferable that the content of at least one of the two or more is in the range of 10 to 85 mass%, and that the total content of the two or more is in the range of more than 10 mass% and 85 mass% or less. By ensuring that the content of at least one of the two or more types is within the range of 10 to 85 mass % and that the total content of the two or more types is greater than 10 mass % and equal to or less than 85 mass %, it becomes easy to achieve both heat resistance and flexibility. Furthermore, when two or more of a thermoplastic elastomer and a random polypropylene are selected, it is more preferable that the content of each of the two or more is within the range of 10 to 85 mass%, and that the total content of the two or more is within the range of 20 to 85 mass%. By ensuring that the content of at least one of the two or more types is within the range of 10 to 85 mass % and that the total content of the two or more types is within the range of 20 to 85 mass %, it becomes easier to achieve both heat resistance and flexibility. Regarding the strength of the resin composition used in the intermediate layer, the tensile modulus of elasticity of the film obtained from the resin composition alone is preferably within the range of 30 to 600 MPa. If the tensile modulus is within the range of 30 to 600 MPa, it becomes easy to adjust the flexibility of the thermoplastic resin films of the present invention. It is more preferably within the range of 40 to 550 MPa, and even more preferably within the range of 50 to 500 MPa. The tensile modulus can be measured by the same method as described in the section on high density polyethylene.
[0064] The resin composition used in the intermediate layer can contain the above-mentioned other thermoplastic resins and other components in addition to high density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene. The content of other thermoplastic resins is 0 to 40% by mass. When it is necessary to adjust the heat resistance and flexibility of the obtained film or to impart film formability, the resin used can be appropriately selected and used. The amount used can be adjusted within a range that does not impair heat resistance and flexibility, and is more preferably 0 to 38% by mass, and even more preferably 0 to 36% by mass.
[0065] The basic structure of the thermoplastic resin film of the present invention is a three-layer film structure comprising a layer (at least one of the front and back layers) containing high-density polyethylene and homopolypropylene, and a layer (middle layer) containing at least one selected from the group consisting of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene. By making at least one of the front and back layers a layer containing high density polyethylene or homopolypropylene, it becomes easy to improve heat resistance and flexibility, and to suppress blocking between films. In addition, by making the intermediate layer a layer containing at least one selected from the group consisting of high density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, it becomes easy to adjust heat resistance and flexibility. In this three-layer film configuration, the resin compositions constituting the front layer and the back layer may be the same or different. The intermediate layer may be composed of two or more layers. In that case, a film configuration composed of three or more layers is also included. In that case, all layers of the intermediate layer composed of two or more layers must be layers containing a predetermined amount of at least one selected from the group consisting of high density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, as described above, and the resin compositions constituting each layer may be the same or different. From the viewpoint of film productivity and economic efficiency, a three-layer film consisting of a front layer, a back layer, and one intermediate layer is preferable. In this case, whether to use a two-kind three-layer film in which the front layer and the back layer are made of the same resin composition or a three-kind three-layer film in which the front layer and the back layer are made of different resin compositions can be appropriately selected as needed, taking into consideration the performance and use of each layer of the front and back of the film required, and the processability when providing an adhesive layer or a printed layer described later.
[0066] The total thickness of the thermoplastic resin film of the present invention is preferably 30 to 250 μm. If it is 30 μm or more, the film formability during film production and the handleability of the obtained film are good, and flexibility and heat resistance can be maintained good, and if it is 250 μm or less, the handleability and processability of the film in the process of laminating a printing layer or an adhesive layer on the film can be maintained good. The total thickness of the thermoplastic resin film of the present invention is more preferably 40 to 230 μm, and further preferably 50 to 210 μm. The thickness of each of the front layer and the back layer is preferably within the range of 1 to 30% of the total thickness of the thermoplastic resin film. By making it 1% or more of the total thickness, it is possible to impart the effect of suppressing blocking between the films, and by making it 30% or less, it is preferable that the flexibility of the obtained film is not impaired. More preferably, it is within the range of 3 to 25%, and further preferably within the range of 5 to 20%. The thickness of each of the front layer and the back layer may be the same thickness or different thicknesses as long as it can suppress the performance required for each of the front layer and the back layer of the obtained thermoplastic resin film and the blocking between the films. From the viewpoint of the productivity and economic efficiency of the film, it is preferable that the thickness of the front layer and the back layer is the same thickness.
[0067] The thermoplastic resin film of the present invention is a film having a small surface irregularity and high transparency, and is characterized in that the surface roughness (Ra) of the front layer and the back layer of the film is 0.5 μm or less and the maximum height (Rz) is 3.0 μm or less. Here, the surface roughness (Ra) is also called the arithmetic mean surface roughness (Ra). By making the surface roughness (Ra) 0.5 μm or less and the maximum height (Rz) 3.0 μm or less, it is possible to obtain a film with a nearly smooth surface and high transparency. More preferred values of the surface roughness (Ra) and the maximum height (Rz) are a surface roughness (Ra) of 0.4 μm or less and a maximum height (Rz) of 2.5 μm or less, and even more preferred values are a surface roughness (Ra) of 0.3 μm or less and a maximum height (Rz) of 2.0 μm or less.
[0068] The surface roughness (Ra) and maximum height (Rz) of the front layer and back layer may be adjusted so that each layer is approximately the same, or may be adjusted so that the front layer and back layer have different values within the above values. When adjusting to have different values, the value of the front or back layer should be higher (lower), and can be adjusted appropriately as needed, taking into consideration the application and the processability when providing the adhesive layer and printing layer described later.
[0069] The method for measuring the surface roughness (Ra) and the maximum height (Rz) is not particularly limited, and any known method can be used. For example, a commonly used stylus type, contact type, or non-contact type surface roughness meter can be used according to the method specified in JIS B0601, etc.
[0070] Regarding the transparency of the thermoplastic resin film, the haze of the film is preferably 50% or less. If the haze is 50% or less, scattering of the laser light or the like irradiated from the light source can be suppressed, and the light can be accurately focused on the wafer. It is more preferably 36% or less, and even more preferably 32% or less. Furthermore, it is preferable that the total light transmittance is 70% or more. With a total light transmittance of 70% or more, attenuation of the laser light when passing through the film is suppressed, which is preferable. It is more preferably 75% or more, and even more preferably 80% or more.
[0071] The method for measuring the total light transmittance and haze is not particularly limited, and any known method can be used. For example, a commonly used transmittance measuring device, a haze meter, etc., can be used according to the method specified in JIS K7361, JIS K7136, etc.
[0072] The tensile modulus of the thermoplastic resin film of the present invention is preferably within the range of 100 to 600 MPa. If it is 100 MPa or more, the film is not too flexible and can maintain good handleability, and if it is 600 MPa or less, the flexibility of the film is not impaired and the film can maintain good handleability and processability in the process of laminating a printing layer or an adhesive layer on the film. It is more preferably within the range of 100 to 550 MPa, and even more preferably within the range of 120 to 500 MPa.
[0073] The tensile elongation at break of the thermoplastic resin film of the present invention is preferably 300% or more. If the tensile elongation at break is 300% or more, breakage during handling of the film is suppressed, and therefore defects due to breakage are suppressed even when adhesive processing or the like is performed, and breakage during expansion is less likely to occur in the expansion step of the semiconductor manufacturing process, which is preferable. It is more preferably 400% or more, and even more preferably 500% or more. The tensile modulus and breakage elongation can be measured by the same method as described in the section on high density polyethylene.
[0074] The thermoplastic resin film of the present invention can be formed by any known method, but it is preferable to use a melt extrusion method. Among the melt extrusion methods, a T-die molding method in which a molten resin is extruded from an extruder having a T-die and cooled and solidified to obtain a film is more preferable. In order to obtain a film, it is preferable to use a co-extrusion T-die molding method using a plurality of extruders. By using a co-extrusion T-die molding method using a plurality of extruders, it is possible to obtain a multi-layer film, and it is possible to obtain a film of the present invention consisting of a front layer, a back layer, and an intermediate layer. It is also possible to obtain an intermediate layer consisting of two or more layers.
[0075] Examples of coextrusion T-die molding methods include a method in which multiple resin layers are formed into a film using a multi-manifold die, and then the layers are brought into contact inside the T-die to form a multi-layered film; and a method in which multiple resins are joined and bonded together using a device that joins molten resins called a feed block, to obtain a multi-layered film.
[0076] The resin extruded in a molten state from the T-die can be cooled and solidified by contacting it with a cooling roll set at a predetermined temperature. The set temperature of the cooling roll is not particularly limited, but it is preferably set to 80°C or less. If it is 80°C or less, it is possible to suppress the phenomenon that the molten resin remains stuck to the cooling roll and cannot be peeled off. It is more preferably 70°C or less, and even more preferably 60°C or less. Furthermore, the surface temperature of the cooling roll is preferably 100°C or less from the viewpoint of suppressing defects caused by the same film sticking. When using a molding method using a rubber roll or metal roll and a nip as described later, it is preferable to adjust the temperature setting and surface temperature of these rolls to be approximately the same as that of the cooling roll. The method for adhering the film to the cooling roll is not particularly limited, and examples thereof include an air knife, an air chamber, electrostatic pinning, and a nip between a roll such as a rubber roll or a metal roll. When using a nip forming method using rubber or metal rolls, in order to adjust the surface roughness (Ra) and maximum height (Rz) of the film to those described above, it is preferable to use rolls whose surface roughness (Ra) and maximum height (Rz) are similar to those of the desired film. Among the above-mentioned molding methods, from the viewpoints of adjusting the surface roughness (Ra) and maximum height (Rz) and film productivity, it is more preferable to use a molding method using an air knife or an air chamber, or a molding method using a nip with a rubber roll or a metal roll with a touch roll.
[0077] If necessary, one or both sides of the film may be subjected to a surface treatment such as a plasma treatment, corona treatment, ozone treatment, flame treatment, etc. From the viewpoint of the use of the obtained film and the prevention of blocking between films, it is possible to select whether to perform a surface treatment on one or both sides, or to perform no corona treatment on either side.
[0078] <Adhesive film> The thermoplastic resin film of the present invention can be made into an adhesive film by providing an adhesive layer on at least one of the front and back surfaces (hereinafter also referred to as "adhesive film of the present invention"). The adhesive used in the adhesive layer is not particularly limited, and various adhesives such as natural rubber resins, acrylic resins, styrene resins, silicone resins, polyvinyl ether resins, etc. may be used. In addition, a functional layer such as an adhesive layer or a thermosetting resin layer may be further provided on the adhesive layer.
[0079] The pressure-sensitive adhesive layer can be provided by directly coating the pressure-sensitive adhesive on the thermoplastic resin film of the present invention, or by laminating the pressure-sensitive adhesive layer on a separator or the like having a release layer, attaching the pressure-sensitive adhesive layer side of the separator to the surface layer of the film of the present invention, and transferring the pressure-sensitive adhesive layer. In the pressure-sensitive adhesive film of the present invention, one or both sides of the film may be subjected to the above-mentioned surface treatment before the pressure-sensitive adhesive layer is provided. In addition, a primer layer may be provided between the film and the pressure-sensitive adhesive layer, if necessary. The thickness of the adhesive layer and the primer layer can be appropriately determined according to need.
[0080] The thermoplastic resin film of the present invention is a thermoplastic resin film that uses a specific resin composition in each layer, and thus has excellent heat resistance, handleability, and flexibility, and also has low surface roughness and high transparency, and in which blocking between films is suppressed. Furthermore, it is also possible to obtain an adhesive film by laminating an adhesive layer on the film, and the adhesive film can be suitably used in the semiconductor manufacturing process. EXAMPLES
[0081] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples. The materials used in the following examples and comparative examples and the methods for measuring the evaluated properties are as follows.
[0082] [Materials used] As the thermoplastic resin, a polypropylene-based resin, a polyethylene-based resin, and a styrene-based elastomer were used as shown below.
[0083] <High density polyethylene> "HF560" manufactured by Japan Polyethylene Corporation (high density polyethylene, melt flow rate at 190°C and 2.16 kg: 7.0 g / 10 min, crystal melting peak: 134°C, density: 0.963 g / cm 3 , Tensile modulus of single film: 1000MPa) <Linear low density polyethylene> "0540F" (linear low-density polyethylene, melt flow rate at 190°C and 2.16 kg: 4.0 g / 10 min, crystal melting peaks at 91°C and 111°C, density: 0.904 g / cm) manufactured by Ube Maruzen Polyethylene Co., Ltd. 3 , Tensile modulus of single film: 90MPa) <Low density polyethylene> "Novatec LC500" manufactured by Japan Polyethylene Corporation (low density polyethylene, melt flow rate at 190°C, 2.16 kg: 4.0 g / 10 min, crystal melting peak: 106°C, density: 0.923 g / cm 3 , Tensile modulus of single film: 140MPa) <Homopolypropylene> Sumitomo Chemical Co., Ltd., "FLX80H5" (homopolypropylene, melt flow rate at 230°C and 2.16 kg: 8.0 g / 10 min, crystal melting peak: 162°C, tensile modulus of single film: 900 MPa) <Random polypropylene> SunAllomer Corporation, "PC630A" (random polypropylene, melt flow rate at 230°C and 2.16 kg: 7.5 g / 10 min, crystal melting peak: 135°C, tensile modulus of single film: 600 MPa) <Olefin elastomer> Japan Polypropylene, "RFG4VM" (olefin elastomer, melt flow rate at 230°C and 2.16 kg: 6.0 g / 10 min, crystal melting peak: 129°C, tensile modulus of single film: 250 MPa) <Styrene-based elastomer> Styrene-based elastomer (α) Asahi Kasei Corporation's "Tuftec H1221" (Melt flow rate at 230°C and 2.16 kg: 4.5 g / 10 min, styrene content: 12% by mass, styrene-ethylene-butylene-styrene copolymer) Styrene elastomer (β) Asahi Kasei Corporation's "Tuftec H1517" (Melt flow rate at 230°C and 2.16 kg: 5.0 g / 10 min, styrene content: 43% by mass, styrene-ethylene-butylene-styrene copolymer)
[0084] <Preparation of Resin Composition> The above thermoplastic resins were mixed so that the total amount was 100 parts by mass. When two or more types were used, they were mixed by dry blending, and it was confirmed by visual inspection that the mixture was homogeneous.
[0085] <Film production method> Each resin composition was charged into each hopper of three Toshiba Machine single-screw extruders (surface layer: 35φmm, L / D=25mm, middle layer: 50φmm, L / D=32, back layer: 35φmm, L / D=25mm), the extruder temperature of each extruder was set to 190-230°C, and the three-layer structure of surface layer / middle layer / back layer was merged in the feed block section and extruded from a 650mm wide T-die (temperature setting 210-230°C, lip opening 0.5mm). The rotation speed of each extruder was set so that the thickness configuration was as shown in Table 1. The extruded molten resin was nipped between a matte (surface roughness Ra approximately 0.3 μm) metal cooling roll (metal cooling roll: 700 mm width x φ350 mm) and a matte (surface roughness Ra approximately 0.3 μm) rubber roll (rubber cooling roll: 700 mm width x φ200 mm) through which cooling water set at 30°C had passed, and after cooling and solidifying into a film, it was taken up on a winding machine to obtain films with a thickness of approximately 80 μm, consisting of 3 layers of type 1, 3 layers of type 2, and 3 layers of type 3. In the present invention, the surface of the obtained film facing the metallic cooling roll is expressed as the surface layer.
[0086] [Thickness of each layer] The thickness of each layer was calculated from the amount of resin extruded from each extruder. [Total film thickness] The thickness of the film was measured at the center and both ends using a contact thickness meter to confirm that the film had the desired thickness. [Surface roughness (Ra), maximum height (Rz)] The surface roughness and maximum height of the front and back layers of the obtained film were measured using a Tokyo Seimitsu SURFCOM FLEX-50A with a measuring force of 0.7 mN using a stylus tip with a tip radius of 2 μm and a conical taper angle of 60° in accordance with JIS B0601 (2001).
[0087] [Total light transmittance, haze] The total light transmittance and haze of the film were measured under the following conditions. The total light transmittance was measured in accordance with JIS K7361-1, and the haze was measured in accordance with JIS K7136 using NDH2000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0088] [Tensile modulus] Test pieces were prepared from the obtained thermoplastic resin film using a dumbbell "SDK-600" manufactured in accordance with JIS K6732, and the tensile modulus (MPa) was measured at a tension speed of 50 mm / min using an autograph (Shimadzu Corporation AGS-X) under the following conditions referring to JIS K7127, under an atmosphere of 23°C and 50% RH. The tensile modulus was measured in the extrusion direction (MD) of the film.
[0089] [Tensile elongation at break] Test pieces were taken from the obtained film using a dumbbell "SDK-600" manufactured in accordance with JIS K6732, and the tensile breaking elongation (%) was measured at a tensile speed of 300 mm / min using a small tabletop testing machine (Shimadzu EZ-L) in an atmosphere of 23°C and 50% RH. The tensile elongation at break was measured in the extrusion direction (MD) of the film.
[0090] [Blocking rating] The obtained film was wound into a roll of 50 m, and after storage for one day, the film was pulled out from the roll and evaluated for the presence or absence of blocking between the films according to the following criteria. ◎: No blocking, easy to unwind 〇: Slight blocking is observed, but the film can be easily unwound. △: Blocking is observed, but unwinding is possible ×: Significant blocking was observed, and unwinding was not possible.
[0091] [Crystal melting peak] Using a differential scanning calorimeter (DSC823e manufactured by Mettler Toledo), approximately 5 mg of test pieces taken from the films obtained in the Examples and Comparative Examples were heated from 25°C to 230°C at a heating rate of 10°C / min, then cooled to 25°C at a cooling rate of 10°C / min, and then heated again to 230°C at a heating rate of 10°C / min. The crystal melting peak was calculated from the chart measured.
[0092] [Example 1] The thermoplastic resins for the surface layer, intermediate layer and back layer were high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer (α) in the amounts shown in Table 1, and resin compositions for each layer were prepared. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of two types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.11 μm and the maximum height (Rz) was 1.08 μm, and the surface roughness (Ra) of the back side was 0.12 μm and the maximum height (Rz) was 0.92 μm. It was confirmed that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 90.0% and the haze was 27.0%, showing that the film had a matte appearance and excellent transparency. The front and back layers of this film contain a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of each of the front and back layers was 870 MPa, so no blocking was observed when the film was unwound from the roll obtained by winding, and it could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when the subsequent adhesive layer and printing layer are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 200 MPa. As a result, it is presumed that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 260 MPa and a tensile breaking elongation of 820%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibits good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0093] [Example 2] The thermoplastic resins for the surface layer, intermediate layer and back layer were high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer (α) in the amounts shown in Table 1, and resin compositions for each layer were prepared. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of two types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.10 μm and the maximum height (Rz) was 0.84 μm, and the surface roughness (Ra) of the back side was 0.15 μm and the maximum height (Rz) was 1.04 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.4% and the haze was 22.0%, showing that the film had a matte appearance and excellent transparency. The front and back layers of this film contain a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of each of the front and back layers was 860 MPa, so no blocking was observed when the film was unwound from the roll obtained by winding, and it could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when the subsequent adhesive layer and printing layer are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 200 MPa. As a result, it is presumed that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 260 MPa and a tensile elongation at break of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0094] [Example 3] The thermoplastic resins for the surface layer, intermediate layer and back layer were high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer (α) in the amounts shown in Table 1, and resin compositions for each layer were prepared. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of two types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.06 μm, and the surface roughness (Ra) of the back side was 0.18 μm and the maximum height (Rz) was 1.31 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.3% and the haze was 23.4%, showing that the film had a matte appearance and excellent transparency. The front and back layers of this film contain a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of each of the front and back layers was 880 MPa, so no blocking was observed when the film was unwound from the roll obtained by winding, and it could be easily unwound. Therefore, it is assumed that this film can be easily handled during processing when the subsequent adhesive layer and printing layer are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 200 MPa. As a result, it is presumed that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 260 MPa and a tensile elongation at break of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0095] [Example 4] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and a styrene-based elastomer (α); the thermoplastic resins for the middle layer were high-density polyethylene, homopolypropylene, random polypropylene, and a styrene-based elastomer (α); and the thermoplastic resins for the back layer were homopolypropylene and random polypropylene. These were mixed in the amounts shown in Table 1 to prepare the resin compositions for use in each layer. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.13 μm and the maximum height (Rz) was 1.05 μm, and the surface roughness (Ra) of the back side was 0.10 μm and the maximum height (Rz) was 0.91 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 90.1% and the haze was 23.3%, showing that the film had a matte appearance and excellent transparency. The surface layer of this film contains a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of the surface layer was 800 MPa, and the tensile modulus of the film obtained only from the resin composition of the back layer was 790 MPa. Furthermore, when the film having this surface layer and back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when a subsequent adhesive layer or printing layer is provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, random polypropylene and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 270 MPa. As a result, it is presumed that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 320 MPa and a tensile breaking elongation of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 162°C, confirming that it also exhibits good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0096] [Example 5] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and a styrene-based elastomer (α); the thermoplastic resins for the middle layer were high-density polyethylene, homopolypropylene, an olefin-based elastomer, and a styrene-based elastomer (α); and the thermoplastic resins for the back layer were homopolypropylene and an olefin-based elastomer.The resin compositions for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.01 μm, and the surface roughness (Ra) of the back side was 0.12 μm and the maximum height (Rz) was 0.95 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.5% and the haze was 30.0%, showing that the film had a matte appearance and excellent transparency. The surface layer of this film contains a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of the surface layer was 800 MPa, and the tensile modulus of the film obtained only from the resin composition of the back layer was 650 MPa. Furthermore, when the film having this surface layer and back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when a subsequent adhesive layer or printing layer is provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 260 MPa. As a result, it is presumed that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 300 MPa and a tensile elongation at break of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibits good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0097] [Example 6] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and a styrene-based elastomer (α); the thermoplastic resins for the middle layer were high-density polyethylene, homopolypropylene, an olefin-based elastomer, and a styrene-based elastomer (α); and the thermoplastic resins for the back layer were homopolypropylene and an olefin-based elastomer.The resin compositions for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.13 μm and the maximum height (Rz) was 1.22 μm, and the surface roughness (Ra) of the back side was 0.12 μm and the maximum height (Rz) was 1.11 μm, confirming that the surface roughness (Ra) of both the front and back sides was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.5% and the haze was 29.9%, showing that the film had a matte appearance and excellent transparency. The surface layer of this film contains a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of the surface layer was 800 MPa, and the tensile modulus of the film obtained only from the resin composition of the back layer was 650 MPa. Furthermore, when the film having this surface layer and back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when a subsequent adhesive layer or printing layer is provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 220 MPa. As a result, it is presumed that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 270 MPa and a tensile breaking elongation of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 129°C and 163°C, confirming that it also exhibits good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0098] [Example 7] The thermoplastic resins used for the surface layer were high density polyethylene, linear low density polyethylene, and homopolypropylene. The thermoplastic resins used for the middle layer were high density polyethylene, linear high density polyethylene, homopolypropylene, an olefin-based elastomer, and a styrene-based elastomer (β). The thermoplastic resins used for the back layer were homopolypropylene and an olefin-based elastomer. The resin compositions used for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.32 μm, and the surface roughness (Ra) of the back side was 0.12 μm and the maximum height (Rz) was 0.96 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.6% and the haze was 31.2%, showing that the film had a matte appearance and excellent transparency. The surface layer of this film contains a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of the surface layer was 900 MPa, and the tensile modulus of the film obtained only from the resin composition of the back layer was 650 MPa. Furthermore, when the film having this surface layer and back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when a subsequent adhesive layer or printing layer is provided. The intermediate layer contains specified amounts of high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 410 MPa, suggesting that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 440 MPa and a tensile breaking elongation of 790%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 129°C and 162°C, confirming that it also exhibits good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0099] [Example 8] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and a styrene-based elastomer (α); the thermoplastic resins for the middle layer were high-density polyethylene, low-density polyethylene, homopolypropylene, random polypropylene, and a styrene-based elastomer (α); and the thermoplastic resins for the back layer were homopolypropylene and random polypropylene.The resin compositions for each layer were prepared in the amounts listed in Table 1. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.13 μm and the maximum height (Rz) was 1.21 μm, and the surface roughness (Ra) of the back side was 0.14 μm and the maximum height (Rz) was 1.00 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.4% and the haze was 21.8%, showing that the film had a matte appearance and excellent transparency. The surface layer of this film contains a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of the surface layer was 890 MPa, and the tensile modulus of the film obtained only from the resin composition of the back layer was 720 MPa. Furthermore, when the film having the surface layer and the back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. Therefore, it is presumed that the film can be easily handled during processing when the subsequent adhesive layer and printing layer are provided. The intermediate layer contains specified amounts of high-density polyethylene, low-density polyethylene, homopolypropylene, random polypropylene and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 250 MPa, suggesting that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 290 MPa and a tensile breaking elongation of 830%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 162°C, confirming that it also exhibits good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0100] [Example 9] The thermoplastic resins used for the surface layer were high-density polyethylene, homopolypropylene, and linear low-density polyethylene. The thermoplastic resins used for the middle layer were high-density polyethylene, homopolypropylene, random polypropylene, styrene-based elastomer (α), and linear low-density polyethylene. The thermoplastic resins used for the back layer were homopolypropylene and random polypropylene. The resin compositions used for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.11 μm and the maximum height (Rz) was 1.18 μm, and the surface roughness (Ra) of the back side was 0.12 μm and the maximum height (Rz) was 1.02 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 88.8% and the haze was 15.4%, showing that the film had a matte appearance and excellent transparency. The surface layer of this film contains a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of the surface layer was 890 MPa, and the tensile modulus of the film obtained only from the resin composition of the back layer was 720 MPa. Furthermore, when the film having the surface layer and the back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. Therefore, it is presumed that the film can be easily handled during processing when the subsequent adhesive layer and printing layer are provided. The intermediate layer contains specified amounts of high-density polyethylene, linear low-density polyethylene, homopolypropylene, random polypropylene and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 240 MPa, suggesting that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 280 MPa and a tensile breaking elongation of 840%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0101] [Example 10] The thermoplastic resins used for the surface layer were high-density polyethylene, homopolypropylene, and linear low-density polyethylene. The thermoplastic resins used for the middle layer were high-density polyethylene, homopolypropylene, random polypropylene, styrene-based elastomer (α), and linear low-density polyethylene. The thermoplastic resins used for the back layer were homopolypropylene and random polypropylene. The resin compositions used for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.30 μm, and the surface roughness (Ra) of the back side was 0.12 μm and the maximum height (Rz) was 0.95 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.0% and the haze was 16.5%, showing that the film had a matte appearance and excellent transparency. The surface layer of this film contains a specified amount of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained only from the resin composition of the surface layer was 890 MPa, and the tensile modulus of the film obtained only from the resin composition of the back layer was 720 MPa. Furthermore, when the film having the surface layer and the back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. Therefore, it is presumed that the film can be easily handled during processing when the subsequent adhesive layer and printing layer are provided. The intermediate layer contains specified amounts of high-density polyethylene, linear low-density polyethylene, homopolypropylene, random polypropylene and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer showed a tensile modulus of 160 MPa, suggesting that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface layer, middle layer, and back layer had a tensile modulus of 210 MPa and a tensile breaking elongation of 820%, providing sufficient flexibility and breaking properties.Furthermore, the crystal melting peaks of the obtained film were 128°C and 160°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handleability and flexibility, has small surface roughness and good transparency, while suppressing blocking between films.
[0102] [Comparative Example 1] As the thermoplastic resins for the surface layer, intermediate layer and back layer, high density polyethylene, linear low density polyethylene, homopolypropylene and an olefin-based elastomer were mixed in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of two types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.05 μm, and the surface roughness (Ra) of the back side was 0.15 μm and the maximum height (Rz) was 1.10 μm, confirming that the surface roughness (Ra) of both the front and back sides was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.3% and the haze was 29.2%, showing that the film had a matte appearance and excellent transparency. The surface and back layers of this film contained small amounts of high density polyethylene and homopolypropylene, and the tensile modulus of the film obtained from only the resin composition of each of the surface and back layers was 280 MPa, so that the film in the roll obtained by winding had significant blocking between the films and could not be unwound. Therefore, it was confirmed that although this film has heat resistance and flexibility, it has poor handling properties and cannot be unwound during processing when the subsequent adhesive layer and printing layer are provided.
[0103] [Comparative Example 2] As the thermoplastic resins for the surface layer, intermediate layer and back layer, high density polyethylene, linear low density polyethylene and an olefin-based elastomer were mixed in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of two types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.15 μm and the maximum height (Rz) was 1.20 μm, and the surface roughness (Ra) of the back layer side was 0.10 μm and the maximum height (Rz) was 0.98 μm. It was confirmed that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.4% and the haze was 28.7%, showing that the film had a matte appearance and excellent transparency. The surface and back layers of this film contained only a small amount of high density polyethylene, and the tensile modulus of the film obtained from only the resin composition of the surface and back layers was 270 MPa, so that the film in the roll obtained by winding had significant blocking between the films, and the film could not be unwound. In addition, since none of the surface, middle, or back layers contained homopolypropylene, and no crystalline melting peak derived from homopolypropylene was observed, it was confirmed that the film had poor heat resistance. Therefore, since this film has poor blocking properties and heat resistance, it cannot be unwound during processing when the subsequent adhesive layer and printing layer are applied, and it was confirmed that the film is difficult to handle as it is highly likely to suffer from defects due to heat during processing.
[0104] [Comparative Example 3] As the thermoplastic resins for the surface layer, intermediate layer and back layer, high density polyethylene, linear low density polyethylene and an olefin-based elastomer were mixed in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of two types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.15 μm and the maximum height (Rz) was 0.99 μm, while the surface roughness (Ra) of the back side was 0.15 μm and the maximum height (Rz) was 1.11 μm. It was confirmed that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.3% and the haze was 32.1%, showing that the film had a matte appearance and excellent transparency. The front and back layers of this film contain a large amount of high-density polyethylene, and furthermore, the film obtained from only the resin composition of each of the front and back layers showed a tensile modulus of 820 MPa. Therefore, even when the film having the front and back layers was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. However, since none of the surface, middle, or back layers contained homopolypropylene, and no crystalline melting peak derived from homopolypropylene was observed, it was confirmed that the film had poor heat resistance. Therefore, although this film has excellent blocking properties and can be unwound during processing when the subsequent adhesive layer and printing layer are applied, it was confirmed that the film has poor handleability and is likely to develop problems due to heat during processing.
[0105] [Comparative Example 4] As the thermoplastic resins for the surface layer, intermediate layer and back layer, high density polyethylene, linear low density polyethylene and homopolypropylene were used in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of two types and three layers and having a total thickness of 80 μm was obtained by the manufacturing method using the matte metal cooling roll and the matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.10 μm and the maximum height (Rz) was 0.98 μm, and the surface roughness (Ra) of the back layer side was 0.10 μm and the maximum height (Rz) was 0.95 μm, confirming that the surface roughness (Ra) of both the front and back sides of the film was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less. The total light transmittance was 89.5% and the haze was 27.0%, showing that the film had a matte appearance and excellent transparency. The front and back layers of this film contain specified amounts of high-density polyethylene and homopolypropylene, and furthermore, the tensile modulus of the film obtained from only the resin composition of each of the front and back layers was 550 MPa. Therefore, although slight blocking was observed when the film was unwound from the roll obtained by winding, it could be easily unwound. The middle layer contains high-density polyethylene and homopolypropylene, but the homopolypropylene content is higher. The tensile modulus of the film obtained from only the resin composition of the middle layer was 870 MPa, and the tensile modulus of the film consisting of the front layer, middle layer, and back layer was also high at 830 MPa, and the tensile breaking elongation was 730%, indicating that the film has sufficient flexibility and breaking properties, but is not very flexible. Therefore, although this film has excellent blocking properties and heat resistance, it was confirmed that it has poor flexibility and is likely to be difficult to handle during processing when subsequent adhesive layers and printed layers are provided.
[0106] [Comparative Example 5] As the resin compositions for the surface layer, the intermediate layer and the back layer, the same resin compositions as those in Example 5 were prepared. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by a manufacturing method using the above-mentioned matte metal cooling roll and a different matte silicone rubber roll (surface roughness Ra is about 1.0 μm) by nip molding. The film formation conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the surface layer of the obtained film was 0.14 μm and the maximum height (Rz) was 1.11 μm, while the surface roughness (Ra) of the back layer side was 1.01 μm and the maximum height (Rz) was 7.21 μm. It was confirmed that while the surface layer had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less, the surface roughness of the back layer exceeded the specified range. This film had a total light transmittance of 89.3%, but because the surface of the back layer was rough, the haze was 93.8%, making it a film with high haze and poor transparency. Therefore, it was confirmed that the film has sufficient heat resistance, and is excellent in handleability and flexibility, but has a rough back layer and poor transparency.
[0107] [Comparative Example 6] As the resin compositions for the surface layer, the intermediate layer and the back layer, the same resin compositions as those in Example 5 were prepared. Using the resin compositions for the surface layer, intermediate layer, and back layer, a film consisting of three types and three layers and having a total thickness of 80 μm was obtained by a manufacturing method using a matte metal cooling roll (surface roughness Ra is about 1.0 μm) different from the above-mentioned one and a matte silicone rubber roll (surface roughness Ra is about 1.0 μm) different from the above-mentioned one by nip molding. The film formation conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the intermediate layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer of the obtained film was 0.84 μm and the maximum height (Rz) was 5.51 μm, while the surface roughness (Ra) of the back layer was 1.05 μm and the maximum height (Rz) was 7.53 μm, confirming that the surface roughness of both the front and back layers of the film exceeded the specified range. This film had a total light transmittance of 89.4%, but because the surfaces of the front and back layers were rough, the haze was 94.4%, making it a film with high haze and poor transparency. Therefore, it was confirmed that the film had sufficient heat resistance and was excellent in handleability and flexibility, but both the front and back layers were rough and the film had poor transparency.
[0108] [Table 1]
[0109] [Example 11] An acrylic adhesive (SK Dyne 1502C manufactured by Soken Chemical Industries, Ltd.) was applied onto the separator using the comma coat method so that the adhesive layer would be 25 μm thick after drying, and the adhesive layer was then dried for 5 minutes in a hot air dryer at 80°C to form an adhesive layer. The adhesive layer side of the prepared separator was bonded to the surface side of the film obtained in Example 1 after corona treatment, whereby the film of the present invention and the adhesive layer were sufficiently adhered to each other, thereby obtaining a laminated adhesive film. Since an adhesive film was obtained that has sufficient heat resistance, excellent handleability and flexibility, as well as low surface roughness and high transparency, it is presumed that an adhesive film was obtained that can be suitably used in semiconductor manufacturing processes that include steps using laser light, such as laser dicing, where a highly transparent film is required.
[0110] [Industrial Applicability] The present invention aims to provide a thermoplastic resin film that has sufficient heat resistance, small surface roughness, and high transparency even when suitability for a heating step in a semiconductor manufacturing process and suppression of scattering of laser light are required, and further, that can suppress blocking between films when the film is handled and has excellent handleability and flexibility. Another object of the present invention is to provide an adhesive film that can be suitably used in a semiconductor manufacturing process by providing an adhesive layer on the thermoplastic resin film.
Claims
1. A thermoplastic resin film consisting of at least three layers: a surface layer, a back layer, and an intermediate layer, At least one of the front and back layers contains high density polyethylene and homopolypropylene, The intermediate layer contains high density polyethylene and homopolypropylene, and also contains at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes; The thermoplastic resin film is characterized by satisfying the following requirements. (1) When the total amount of thermoplastic resins contained in the resin composition constituting at least one of the front and back layers is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of the front layer and the back layer is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
2. 2. The thermoplastic resin film according to claim 1, wherein the thermoplastic elastomer is a styrene-based elastomer and / or an olefin-based elastomer.
3. 3. The thermoplastic resin film according to claim 1, wherein the haze of the thermoplastic resin film is 50% or less.
4. 3. The thermoplastic resin film according to claim 1, wherein the thermoplastic resin film has a tensile modulus in the range of 100 to 600 MPa.
5. 3. An adhesive film comprising the thermoplastic resin film according to claim 1 or 2 and an adhesive layer provided on at least one surface of the thermoplastic resin film.
6. The adhesive film for use in a semiconductor manufacturing process according to claim 5, which is used in a semiconductor manufacturing process.
Citation Information
Patent Citations
Semiconductor wafer fixing adhesive tape
JP1997008111A
Dicing-base film
JP2018125521A
Base film for semiconductor manufacturing process and adhesive film for dicing using base film
JP2020084143A
Dicing Sheet
JP6980684B2