Thermoplastic resin film, adhesive film, adhesive film for semiconductor manufacturing process and method for manufacturing the same
A three-layer thermoplastic resin film with specific resin compositions addresses compatibility and stability issues, providing heat resistance, transparency, and flexibility for semiconductor manufacturing, while minimizing blocking and laser scattering.
Patent Information
- Application Number
- JP2023181602
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2023-10-23
- Publication Date
- 2024-10-31
AI Technical Summary
Existing adhesive films used in semiconductor manufacturing processes face issues with poor compatibility and stability due to plasticizer bleed-out, lack of heat resistance, and difficulties in preventing laser light scattering and blocking between films, especially with the trend towards smaller and thinner semiconductor devices.
A thermoplastic resin film composed of at least three layers, with specific resin compositions for each layer, including high-density polyethylene, homopolypropylene, and thermoplastic elastomers, is produced by nipping molten resin between a metal and a rubber roll to achieve low surface roughness, high transparency, and sufficient heat resistance, while minimizing blocking and enhancing handleability and flexibility.
The film exhibits excellent heat resistance, low surface roughness, and transparency, effectively preventing blocking and laser light scattering, with improved handleability and flexibility, making it suitable for semiconductor manufacturing processes.
Smart Images

Figure 2024155685000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to a thermoplastic resin film that is suitable for use as a substrate for adhesive films (tapes) and the like used in semiconductor manufacturing processes, an adhesive film in which an adhesive layer is provided on the film, an adhesive film for semiconductor manufacturing processes made of the film, and a method for manufacturing the thermoplastic resin film. [Background technology]
[0002] BACKGROUND ART Films made of polyvinyl chloride resin (hereinafter also referred to as "PVC-based films"), which have excellent colorability, processability, scratch resistance, weather resistance, etc., have traditionally been widely used as the substrate for adhesive films (tapes) used in semiconductor manufacturing processes, decorative adhesive films (tapes) such as stickers, labels, and marking films attached to signs, automobiles, etc. to add design features, and decorative sheets.
[0003] The PVC film itself has rigidity, but a plasticizer is added to impart flexibility so that it can function as an adhesive film. However, depending on the plasticizer used, there are problems such as poor compatibility with the adhesive, poor stability when used as an adhesive film, and significant bleeding out of the plasticizer. In addition, there is a tendency for regulations on the use of plasticizers themselves to be strengthened. Therefore, polyolefin resin films have come to be widely used as an alternative to PVC films.
[0004] Furthermore, in the process of manufacturing semiconductors, adhesive films for semiconductor wafer processing are used when cutting semiconductor wafers, packages, etc., and due to the above-mentioned problems, polyolefin resin films are increasingly being used (e.g., Patent Document 1).
[0005] In recent years, semiconductor elements have become smaller and thinner, and in addition to the flexibility required for films to be easy to handle and expand, heat resistance is also required for films used in semiconductor manufacturing processes, as it is anticipated that heating processes will be used, such as heating the wafer and adhesive film to bond them more firmly together and heating the expansion process after dicing, in order to prevent chip breakage and loss during expansion. In addition to blade dicing, which uses a rotating blade, there are also cases where it is required to apply it to processes such as laser dicing, which modifies part of a semiconductor wafer by irradiating it with laser light and then divides the wafer by stretching it, and stealth dicing. In such processes using laser light, the laser light may be irradiated through a film or tape used in semiconductor manufacturing processes, and in such cases, there is a tendency for highly transparent films to be required to prevent the laser light from scattering and to accurately focus it on the wafer.
[0006] Patent Document 2 discloses a dicing substrate film that uses a polyethylene resin to maintain expandability even at low temperatures. Patent Document 3 discloses a substrate film for use in semiconductor manufacturing processes that is provided with antistatic properties and has excellent flexibility and heat resistance. Patent Document 4 discloses a dicing sheet that has small surface roughness and excellent transparency.
[0007] However, the film described in Patent Document 2 uses only a polyethylene resin with a relatively low melting point, and although it is thought to have excellent low-temperature expandability, it is thought that there is room for improvement in heat resistance. Also, the film described in Patent Document 3 has excellent antistatic properties and heat resistance, but there is room for improvement in terms of suppressing problems caused by blocking between films when obtaining a film with low surface roughness and high transparency. The sheet described in Patent Document 4 is a film having small surface roughness and excellent transparency, but like the sheet described in Patent Document 3, it is presumed that there is room for improvement in terms of suppressing defects due to blocking and also in terms of the heat resistance of the resin. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 09-008111 [Patent Document 2] Japanese Patent Application Publication No. 2018-125521 [Patent Document 3] Japanese Patent Publication No. 2020-84143 [Patent Document 4] Patent No. 6980684 DISCLOSURE OF THE INVENTION [Problem to be solved by the invention]
[0009] In view of the above problems, the present invention aims to provide a film with a good appearance that has low surface roughness, high transparency, and sufficient heat resistance when used in heating processes in semiconductor manufacturing processes or when suppression of scattering of laser light is required, and further to provide a thermoplastic resin film that can suppress blocking between films when handling the film and has excellent handleability and flexibility. Another object of the present invention is to provide a pressure-sensitive adhesive film that can be suitably used in semiconductor manufacturing processes by providing a pressure-sensitive adhesive layer on the thermoplastic resin film. [Means for solving the problem]
[0010] The present inventors have conducted extensive research into a method for producing a thermoplastic resin film, which uses a specific resin composition in each layer of a thermoplastic resin film obtained by nipping the molten resin extruded during film production between a metal roll and a rubber roll, thereby making it possible to obtain a thermoplastic resin film that not only has heat resistance, ease of handling, and flexibility, but also has low surface roughness, high transparency, and a good appearance with suppressed blocking between films.As a result, they have completed the present invention.
[0011] That is, the gist of the present invention is as follows. [1] A thermoplastic resin film consisting of at least three layers, namely, two outer layers and an intermediate layer, obtained by nipping an extruded molten resin between a metal roll and a rubber roll, The resin composition constituting the outer layer on the side that comes into contact with the metal roll contains high-density polyethylene and homopolypropylene, The intermediate layer contains at least one selected from the group consisting of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, The thermoplastic resin film is characterized by satisfying the following requirements: (1) When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of both outer layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less. [2] The thermoplastic resin film according to [1], wherein the thermoplastic elastomer is a styrene-based elastomer and / or an olefin-based elastomer. [3] The thermoplastic resin film according to [1] or [2], wherein the haze of the thermoplastic resin film is 50% or less. [4] The thermoplastic resin film according to any one of [1] to [3], wherein the thermoplastic resin film has a tensile modulus in the range of 100 to 600 MPa. [5] An adhesive film comprising a thermoplastic resin film according to any one of [1] to [4], and an adhesive layer provided on at least one surface of the thermoplastic resin film. [6] The adhesive film for semiconductor manufacturing processes according to [5], which is used in semiconductor manufacturing processes. [7] A method for producing a thermoplastic resin film consisting of at least three layers, two outer layers and an intermediate layer, comprising: The production method includes nipping an extruded molten resin between a metal roll and a rubber roll to obtain the thermoplastic resin film, The surface roughness (Ra) of the metal roll and the rubber roll used to nip the extruded molten resin is 0.5 μm or less, The resin composition constituting the outer layer on the side in contact with the metal roll contains high-density polyethylene and homopolypropylene, the intermediate layer contains at least one selected from the group consisting of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene; The manufacturing method, wherein the thermoplastic resin film satisfies the following requirements: (1) When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of both outer layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less. [8] The manufacturing method according to [7], characterized in that the surface of the rubber roll is made of silicone resin or fluororesin. [Effects of the Invention]
[0012] By using a specific thermoplastic resin composition in the manufacturing method of nipping with a metal roll and a rubber roll described in the present invention, it is possible to provide a thermoplastic resin film that has sufficient heat resistance, low surface roughness, high transparency, and can suppress blocking between films, and that has excellent handleability, flexibility, and appearance, even when heating steps are performed in the semiconductor manufacturing process or suppression of laser light scattering is required. Furthermore, the present invention makes it possible to provide a thermoplastic resin film that can suppress adhesion to a metal roll and also suppress the occurrence of appearance defects such as unevenness in the film caused by air entrapment. Furthermore, the present invention makes it possible to provide a pressure-sensitive adhesive film that can be suitably used in semiconductor manufacturing processes by providing a pressure-sensitive adhesive layer on the thermoplastic resin film. DETAILED DESCRIPTION OF THE INVENTION
[0013] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be practiced with various modifications within the scope of the gist. In this specification, when the expression "to" is used, it is used as an expression including the numerical values or physical property values before and after it.
[0014] 1. Thermoplastic resin film The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers, namely, two outer layers and an intermediate layer, obtained by nipping an extruded molten resin between a metal roll and a rubber roll, in which the resin composition constituting the outer layer on the side in contact with the metal roll contains high-density polyethylene and homopolypropylene, and the intermediate layer contains high-density polyethylene, homopolypropylene, and at least one selected from the group consisting of a thermoplastic elastomer and a random polypropylene, and is characterized by satisfying the following requirements (hereinafter also referred to as the "thermoplastic resin film of the present invention"). (1) When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of both outer layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
[0015] The resins constituting the thermoplastic resin film of the present invention will be described in detail below.
[0016] <High-density polyethylene> The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers: two outer layers and an intermediate layer, and the resin composition constituting each of the outer layer and the intermediate layer on the side that comes into contact with the metal roll contains high-density polyethylene. By incorporating high-density polyethylene into the outer layer on the side that comes into contact with the metal roll, the elastic modulus of the front and / or back layers can be improved, and even if the surface roughness of the front and back sides of the film is small, blocking between films when the film is wound into a roll can be suppressed. Furthermore, by using a predetermined amount of high-density polyethylene, it is possible to prevent the resin composition from adhering too closely to the metal roll when the film is obtained by a molding method in which a metal roll and a rubber roll are nipped together, making it possible to obtain a film without the film wrapping around the metal roll. In addition, air may be entrapped when the resin composition adheres to the metal roll, and the entrapped air may become bubbles, causing unevenness due to the bubbles on the surface of the resulting film facing the metal roll. By using a predetermined amount of high-density polyethylene, adhesion to the metal roll and the entrapment of air are suppressed, making it possible to suppress defects in appearance due to unevenness caused by the bubbles.
[0017] By incorporating high-density polyethylene into the intermediate layer of the present thermoplastic resin film, it is possible to improve compatibility with the outer layer containing high-density polyethylene, and to improve adhesion to the intermediate layer. There are no particular restrictions on the high-density polyethylene used, and high-density polyethylene composed of an ethylene homopolymer or a copolymer of ethylene as the main component and other monomers copolymerizable with ethylene (hereinafter referred to as other monomers) can be used. Examples of other monomers include α-olefins having 3 or more carbon atoms. Examples of α-olefins having 3 or more carbon atoms include propylene, 1-butene, isobutene, 1-pentene, 2-methyl-butene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-pentene, 1-octene, 1-decene, and 1-dodecene. From the viewpoints of availability of the monomer and the performance of the resulting high-density polyethylene, α-olefins having 3 or more carbon atoms are preferably in the range of 3 to 20.
[0018] The density of high density polyethylene is 0.940 to 0.970 g / cm 3 It is preferable that the density is in the range of 0.940 to 0.970 g / cm 3 By using a high-density polyethylene within this range, it becomes easy to adjust the elastic modulus of the surface layer and / or back layer and intermediate layer of the obtained thermoplastic resin film. It is more preferably 0.942 to 0.968 g / cm 3 The density is preferably in the range of 0.944 to 0.966, and more preferably in the range of 0.944 to 0.966. Methods for measuring the density include Method A (underwater displacement method), Method B (pycnometer method), Method C (float-sink method), and Method D (density gradient tube method) described in "JIS K 7112." There are no particular restrictions on the measurement method, and an appropriate method can be selected and used.
[0019] The high-density polyethylene preferably has a crystalline melting peak of 120°C or higher. Having a crystalline melting peak of 120°C or higher makes it possible to impart sufficient heat resistance to the resulting thermoplastic resin film. The peak is more preferably 125°C or higher, and even more preferably 130°C or higher. The crystalline melting peak can be measured using a differential scanning calorimeter according to JIS K 7122.
[0020] Regarding the strength of the high-density polyethylene, the tensile modulus of a film obtained from high-density polyethylene alone is preferably in the range of 600 to 1800 MPa. If the tensile modulus is in the range of 600 to 1800 MPa, it is possible to impart appropriate strength and flexibility to the thermoplastic resin film of the present invention. It is more preferably in the range of 650 to 1750 MPa, and even more preferably in the range of 700 to 1700 MPa. The tensile modulus can be measured according to the method described in "JIS K 7127." Appropriate conditions such as the shape of the test piece, the test speed, and the distance between chucks during measurement can be selected and used.
[0021] The melt flow rate of high-density polyethylene is selected appropriately depending on the molding method and application, but preferably is 0.1 to 50 g / 10 min as measured at a temperature of 190°C under a load of 2.16 kg. A melt flow rate of 0.1 g / 10 min or higher provides good film formability, while a melt flow rate of 50 g / 10 min or lower enables the thickness precision of the film to be maintained at a high level. A melt flow rate of 0.5 to 40 g / 10 min is more preferable, and 1.0 to 30 g / 10 min is even more preferable. The melt flow rate can be measured using the method described in "JIS K 7210." The measurement conditions, such as temperature and load, can be selected appropriately depending on the material used and its properties.
[0022] Commercially available high-density polyethylenes include, for example, Novatec HD "HJ360," Novatec HD "HJ491," Novatec HD "HF560," and Novatec HD "HY350" (all manufactured by Japan Polyethylene Corporation), Santech HD "B161," Santech HD "J340," and Santech HD "J241" (all manufactured by Asahi Kasei Corporation), Nipolon Hard "4000," Nipolon Hard "2000," Nipolon Hard "2500," and Nipolon Hard "LW13D" (all manufactured by Tosoh Corporation). These high-density polyethylenes may be used alone or in combination of two or more. They can be appropriately selected as needed, taking into consideration the film-forming properties when obtaining a thermoplastic resin film, the heat resistance and flexibility of the resulting film, and blocking between films.
[0023] <Homopolypropylene> The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers: two outer layers and an intermediate layer, and the resin composition constituting each of the outer layer and the intermediate layer on the side that comes into contact with the metal roll contains homopolypropylene. By incorporating homopolypropylene into the outer layer on the side that comes into contact with the metal roll, it is possible to improve the elastic modulus of the layer and impart heat resistance to the layer. Furthermore, even if the surface roughness of the front and back of the film is small, it is possible to prevent blocking between films when the film is wound into a roll. Furthermore, by incorporating homopolypropylene into the intermediate layer, it is possible to improve compatibility with the outer layer containing homopolypropylene, and it is also possible to improve adhesion to the intermediate layer. The homopolypropylene used in the present invention is a homopolymer of propylene.
[0024] The crystalline melting peak of the homopolypropylene preferably exhibits a temperature of 140°C or higher. Having a crystalline melting peak of 140°C or higher makes it possible to impart sufficient heat resistance to the resulting multilayer film. The temperature is more preferably 145°C or higher, and even more preferably 150°C or higher. The crystalline melting peak can be measured using the same method as described in the section on high-density polyethylene. Regarding the strength of homopolypropylene, the tensile modulus of a film obtained from the resin alone is preferably in the range of 600 to 1800 MPa. If the tensile modulus is in the range of 600 to 1800 MPa, it is possible to impart appropriate strength to the film of the present invention. It is more preferably in the range of 650 to 1750 MPa, and even more preferably in the range of 700 to 1700 MPa. The tensile modulus can be measured using the same method as described in the section on high-density polyethylene. The melt flow rate of homopolypropylene is selected appropriately depending on the molding method and application, but is preferably 0.1 to 50 g / 10 min as measured at a temperature of 230°C under a load of 2.16 kg. A melt flow rate of 0.1 g / 10 min or higher provides good film formability, while a melt flow rate of 50 g / 10 min or lower makes it possible to maintain good film thickness precision. A melt flow rate of 0.5 to 40 g / 10 min is more preferred, and a melt flow rate of 1.0 to 30 g / 10 min is even more preferred. The melt flow rate can be measured using the same method as described in the high-density polyethylene section.
[0025] Commercially available homopolypropylene products include, for example, Novatec PP "MA3U" and Novatec PP "FY6HA" (all manufactured by Japan Polypropylene Corporation), PC412A, PC600A, PC600S, and PLA00A (all manufactured by SunAllomer Co., Ltd.), F-730NV and F-744NP (all manufactured by Prime Polypropylene Co., Ltd.), Sumitomo Noblen "WF836DG3," and Sumitomo Noblen "FLX80H5" (all manufactured by Sumitomo Chemical Co., Ltd.). The homopolypropylene may be used alone or in combination of two or more types, and can be appropriately selected as needed, taking into consideration the film-forming properties when obtaining a thermoplastic resin film, the heat resistance and flexibility of the obtained film, blocking between films, etc.
[0026] <Thermoplastic elastomer> The intermediate layer of the thermoplastic resin film of the present invention contains, as an essential component, at least one selected from the group consisting of a thermoplastic elastomer and random propylene, in addition to the high-density polyethylene and homopolypropylene described above. By incorporating the thermoplastic elastomer, it becomes possible to adjust the flexibility and expandability of the resulting film within appropriate ranges.
[0027] Examples of the thermoplastic elastomer include olefin elastomers, styrene elastomers, acrylic elastomers, vinyl chloride elastomers, urethane elastomers, polyester elastomers, polyamide elastomers, fluorine elastomers, and silicone elastomers. Among the above thermoplastic elastomers, it is preferable to use an olefin-based elastomer or a styrene-based elastomer from the viewpoints of compatibility with the aforementioned high-density polyethylene and homopolypropylene, imparting flexibility to the resulting film, and transparency. The olefin-based elastomer and the styrene-based elastomer may be used alone, or they may be used in combination, taking into consideration the film-forming properties when obtaining a thermoplastic resin film and the flexibility of the resulting film. Furthermore, multiple types, such as two or more types of olefin-based elastomers and two or more types of styrene-based elastomers, may be used. Among these, it is more preferable to use an olefin-based elastomer and a styrene-based elastomer in combination from the viewpoint of adjusting flexibility.
[0028] The olefin elastomer is a soft resin containing a polyolefin resin and a rubber component, and may be a polyolefin resin in which the rubber component is dispersed, or a polyolefin resin in which the two components are copolymerized. Specific examples of olefin-based elastomers include amorphous elastic copolymers containing olefins as a main component, such as ethylene-propylene copolymer elastomers, ethylene-1-butene copolymer elastomers, ethylene-propylene-1-butene copolymer elastomers, ethylene-1-hexene copolymer elastomers, ethylene-1-octene copolymer elastomers, ethylene-styrene copolymer elastomers, ethylene-norbornene copolymer elastomers, propylene-1-butene copolymer elastomers, ethylene-propylene-non-conjugated diene copolymer elastomers, ethylene-1-butene-non-conjugated diene copolymer elastomers, and ethylene-propylene-1-butene-non-conjugated diene copolymer elastomers, as well as derivatives and acid-modified derivatives thereof.
[0029] Commercially available olefin-based elastomers include, for example, Wellnex "RFG4VM," Wellnex "RFX4V," and Wellnex "RMG02" (all manufactured by Japan Polypropylene Corporation), Tafmer "A-4070S," Tafmer "A-4085S," Tafmer "BL2481M," Tafmer "BL3450M," Tafmer "XM7070," Tafmer "XM7080," and Milastomer (all manufactured by Mitsui Chemicals, Inc.), as well as ENGAGE, AFFINITY, and VERSIFY (all manufactured by The Dow Chemical Company). The olefin-based elastomer may be used alone or in combination of two or more types, and can be appropriately selected as needed, taking into consideration the film-forming properties when obtaining a thermoplastic resin film, the flexibility of the obtained film, blocking between films, etc.
[0030] Regarding the strength of the olefin-based elastomer, the tensile modulus of a film obtained from the resin alone is preferably in the range of 30 to 400 MPa. If the tensile modulus is in the range of 30 to 400 MPa, it is possible to impart appropriate flexibility to the film of the present invention. It is more preferably in the range of 30 to 300 MPa, and even more preferably in the range of 30 to 200 MPa. The tensile modulus can be measured using the same method as described in the section on high-density polyethylene.
[0031] The melt flow rate of the olefin elastomer is selected appropriately depending on the molding method and application, but preferably is 0.1 to 50 g / 10 min as measured at a temperature of 190°C or 230°C under a load of 2.16 kg. A melt flow rate of 0.1 g / 10 min or higher provides good film formability, while a melt flow rate of 50 g / 10 min or lower makes it possible to maintain good film thickness precision. A melt flow rate of 0.5 to 40 g / 10 min is more preferred, and a melt flow rate of 1.0 to 30 g / 10 min is even more preferred. The melt flow rate can be measured using the same method as described in the section on high-density polyethylene.
[0032] The styrene elastomer is preferably a block copolymer represented by the following formula (I) or (II). X-(YX)n …(I) (XY)n …(II) In general formulas (I) and (II), X represents an aromatic vinyl polymer block (hereinafter referred to as the styrene component), typically styrene, and in formula (I), the degrees of polymerization at both ends of the molecular chain may be the same or different. Y represents at least one selected from the group consisting of a butadiene polymer block, an isoprene polymer block, a butadiene / isoprene copolymer block, a hydrogenated butadiene polymer block, a hydrogenated isoprene polymer block, a hydrogenated butadiene / isoprene copolymer block, a partially hydrogenated butadiene polymer block, a partially hydrogenated isoprene polymer block, and a partially hydrogenated butadiene / isoprene copolymer block. n represents an integer of 1 or greater.
[0033] Specific examples of styrene-based elastomers include styrene-ethylene-butylene-styrene copolymer, styrene-ethylene-propylene-styrene copolymer, styrene-ethylene-ethylene-propylene-styrene copolymer, styrene-butadiene-butene-styrene copolymer, styrene-butadiene-styrene copolymer, styrene-isoprene-styrene copolymer, styrene-hydrogenated butadiene diblock copolymer, styrene-hydrogenated isoprene diblock copolymer, styrene-butadiene diblock copolymer, and styrene-isoprene diblock copolymer, among which styrene-ethylene-butylene-styrene copolymer, styrene-ethylene-propylene-styrene copolymer, styrene-ethylene-ethylene-propylene-styrene copolymer, and styrene-butadiene-butene-styrene copolymer are preferred. Furthermore, styrene-ethylene-butylene-crystalline olefin copolymer block copolymers can also be used.
[0034] The melt flow rate of the styrene elastomer (measured at a temperature of 230°C under a load of 2.16 kg) is preferably 0.1 to 20 g / 10 min, more preferably 0.15 to 15 g / 10 min, and particularly preferably 0.2 to 10 g / 10 min. If the melt flow rate of the styrene elastomer is 0.1 g / 10 min or more and 20 g / 10 min or less, it has good compatibility with other resins and is preferable in terms of film formability. The melt flow rate can be measured using the same method as described in the section on high-density polyethylene.
[0035] The styrene content of the styrene elastomer is preferably 50% by mass or less. If the styrene content is 50% by mass or less, flexibility can be imparted to the resulting film. It is preferably 47% by mass or less, and more preferably 44% by mass or less.
[0036] The content of styrene components and other components is as follows: 1 H-NMR and 13 It can be measured by C-NMR. Here, the "styrene component content" refers to the content (mass %) of aromatic vinyl polymer blocks, typically styrene, based on the mass of the styrene-based elastomer.
[0037] Examples of commercially available styrene-based elastomers having a styrene component content of 50% by mass or less include Tuftec H1221, Tuftec H1062, Tuftec H1521, Tuftec H1517, Tuftec H1052, Tuftec H1041, Tuftec P1083, Tuftec P1913, and P5051 (all manufactured by Asahi Kasei Corporation), Septon 2004F, Septon 2063, Hybler 7311, Hybler 7311F, Hybler 7125F, Hybler 5127, and Hybler 5125 (all manufactured by Kuraray Co., Ltd.), Dynaron 1320P, Dynaron 4600P, Dynaron 8300P, and Dynaron 8903P (all manufactured by JSR Corporation).
[0038] The styrene-based elastomer may be used alone or in combination of two or more types, and can be appropriately selected as needed, taking into consideration the film-forming properties when obtaining a thermoplastic resin film, and the flexibility, handleability, and expandability of the obtained film.
[0039] It is preferable to use an olefin-based elastomer and a styrene-based elastomer in combination, since this makes it easier to adjust the flexibility and film-forming properties of the resulting thermoplastic resin film and also makes it easier to reduce cutting debris generated when cutting a wafer with a blade.
[0040] <Random polypropylene> The intermediate layer of the thermoplastic resin film of the present invention contains, as an essential component, at least one selected from the group consisting of a thermoplastic elastomer and a random polypropylene, in addition to the high-density polyethylene and homopolypropylene described above. By including the random polypropylene, it becomes possible to adjust the flexibility and expandability of the resulting film within appropriate ranges.
[0041] Examples of random polypropylenes include copolymers of propylene as the main component with other monomers copolymerizable with propylene, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 4-methyl-1-pentene, and 1-decene, and one or more of these may be used.
[0042] The random polypropylene preferably has a crystalline melting peak of 110°C or higher. Having a crystalline melting peak of 110°C or higher makes it easy to adjust the heat resistance of the resulting thermoplastic resin film. It is more preferably 115°C or higher, and even more preferably 120°C or higher. The crystalline melting peak can be measured using the same method as described in the section on high-density polyethylene.
[0043] Regarding the strength of random polypropylene, the tensile modulus of a film obtained from the resin alone is preferably in the range of 200 to 800 MPa. If the tensile modulus is in the range of 200 to 800 MPa, it is possible to impart appropriate strength and flexibility to the thermoplastic resin film of the present invention. It is more preferably in the range of 200 to 700 MPa, and even more preferably in the range of 200 to 600 MPa. The tensile modulus can be measured using the same method as described in the section on high-density polyethylene.
[0044] The melt flow rate of random polypropylene is selected appropriately depending on the molding method and application, but preferably is 0.1 to 50 g / 10 min as measured at a temperature of 230°C under a load of 2.16 kg. If it is 0.1 g / 10 min or higher, film formability is good, and if it is 50 g / 10 min or lower, it is possible to maintain good film thickness precision. It is more preferably 0.5 to 40 g / 10 min, and even more preferably 1.0 to 30 g / 10 min. The melt flow rate can be measured using the same method as described in the section on high-density polyethylene.
[0045] Commercially available random polypropylene products include, for example, Novatec PP "FW4BA" and Novatec PP "FX3B" (both manufactured by Japan Polypropylene Corporation), PC630A and PC630S (both manufactured by SunAllomer Co., Ltd.), F-730NV and F-744NP (both manufactured by Prime Polypropylene Co., Ltd.), Sumitomo Noblen "FL6737" and Sumitomo Noblen "S131" (both manufactured by Sumitomo Chemical Co., Ltd.), and the like.
[0046] <Other thermoplastic resins> In addition to high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, other thermoplastic resins may be added to the thermoplastic resin film of the present invention as long as the heat resistance and flexibility are not impaired. Examples of other thermoplastic resins include polyethylene-based resins, cyclic olefin-based resins, and polymethylpentene-based resins.
[0047] Examples of polyethylene resins include ethylene homopolymers, copolymers of ethylene, primarily composed of ethylene, with other monomers copolymerizable with ethylene (low-density polyethylene (LDPE), high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), ethylene copolymers obtained by polymerization using a metallocene catalyst (metallocene polyethylene), ethylene-vinyl acetate copolymers, ethylene-methyl (meth)acrylate copolymers, ethylene-ethyl (meth)acrylate copolymers, ethylene-butyl (meth)acrylate copolymers, ethylene-(meth)acrylic acid copolymers, and metal ion-crosslinked resins (ionomers) of ethylene-(meth)acrylic acid copolymers. Among these, it is preferable to use low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE) from the viewpoints of ease of availability, ease of handling of the resin, and ease of adjusting the flexibility and heat resistance of the resulting film.
[0048] The density of low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE) is 0.900 to 0.940 g / cm 3 It is preferable that the density is in the range of 0.900 to 0.940 g / cm 3 By using a material in this range, it is easy to adjust the heat resistance and flexibility of the resulting thermoplastic resin film. More preferably, it is 0.902 to 0.938 g / cm 3 The density is preferably in the range of 0.904 to 0.936, and more preferably in the range of 0.904 to 0.936. The density can be measured by the same method as described in the section on high-density polyethylene.
[0049] The crystalline melting peak of low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE) preferably exhibits a temperature of 70°C or higher. Having a crystalline melting peak of 70°C or higher makes it easy to adjust the heat resistance of the resulting thermoplastic resin film. The temperature is more preferably 75°C or higher, and even more preferably 80°C or higher. The crystalline melting peak can be measured using the same method as described in the section on high-density polyethylene.
[0050] Regarding the strength of low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE), the tensile modulus of a film obtained from these resins alone is preferably within the range of 30 to 400 MPa. If the tensile modulus is within the range of 30 to 400 MPa, it becomes easy to adjust the flexibility of the thermoplastic resin film of the present invention. It is more preferably within the range of 40 to 350 MPa, and even more preferably within the range of 50 to 300 MPa. The tensile modulus can be measured using the same method as described in the section on high-density polyethylene.
[0051] Commercially available low-density polyethylene (LDPE) products include, for example, Novatec LD "LC500," Novatec LD "LC520," and Novatec LD "LC720" (all manufactured by Japan Polyethylene Co., Ltd.), as well as F224N, F324C, and F522N (all manufactured by Ube Maruzen Polyethylene Co., Ltd.). Commercially available linear low-density polyethylene (LLDPE) products include, for example, Novatec LL "UF420" and Novatec LL "UF641" (both manufactured by Japan Polyethylene Co., Ltd.), Yumerit "0540F" and Yumerit "4040F" (both manufactured by Ube Maruzen Polyethylene Co., Ltd.).
[0052] Examples of cyclic olefin resins include norbornene polymers, vinyl alicyclic hydrocarbon polymers, and cyclic conjugated diene polymers. Among these, norbornene polymers are preferred. Examples of norbornene polymers include ring-opening polymers of norbornene monomers and norbornene copolymers obtained by copolymerizing norbornene monomers with α-olefins such as ethylene. Hydrogenated products of these may also be used.
[0053] The polymethylpentene resin is preferably a homopolymer containing methylpentene as a monomer or a copolymer with other monomers, such as a copolymer of α-olefins and 4-methylpentene-1, which are listed as examples of other monomers copolymerizable with propylene for polypropylene resins. When the polymethylpentene resin is a copolymer, the content of the α-olefin component used in the copolymerization is preferably 20% by mass or less. By setting the content to 20% by mass or less, it is possible to suppress a decrease in the crystalline melting peak. It is more preferably 10% by mass or less.
[0054] <Other ingredients> The thermoplastic resin film of the present invention may contain various additives to impart antistatic properties, heat resistance, weather resistance, and the like. Specific examples of the additives that may be used include antistatic agents, antioxidants, neutralizing agents, lubricants, antiblocking agents, plasticizers, heat stabilizers, light stabilizers, dyes and pigments, nucleating agents, ultraviolet absorbers, bulking agents, inorganic fillers that impart rigidity, and elastomers other than those described above that impart flexibility, within the scope of not impairing the effects of the present invention.
[0055] Known polymer antistatic agents can be used, such as block copolymers of a hydrophobic block and a hydrophilic block, in which the hydrophobic block and the hydrophilic block form a block copolymer via ester bonds, ether bonds, amide bonds, imide bonds, urethane bonds, urea bonds, etc.
[0056] As the ultraviolet absorber, known ones can be used, and examples thereof include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, and triazine-based ultraviolet absorbers.
[0057] As the light stabilizer, known ones can be used, and examples thereof include hindered amine light stabilizers.
[0058] As the lubricant or antiblocking agent, it is preferable to use a silicone-olefin copolymer, since it has excellent compatibility with the above-mentioned polypropylene-based resins, polyethylene-based resins, etc., and can prevent defects caused by bleed-out onto the surface of the resulting film and can impart long-term scratch resistance and slip properties.
[0059] <Thermoplastic resin film> The thermoplastic resin film of the present invention is a thermoplastic resin film consisting of at least three layers: two outer layers and an intermediate layer, in which the resin composition constituting the outer layer on the side that comes into contact with the metal roll contains high-density polyethylene and homopolypropylene, and the intermediate layer contains high-density polyethylene and homopolypropylene, and also contains at least one member selected from the group consisting of a thermoplastic elastomer and a random polypropylene, and is characterized by satisfying the following requirements: (1) When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of both outer layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
[0060] The total mass of the thermoplastic resin contained in the resin composition constituting the outer layer on the side that comes into contact with the metal roll means the total mass of the high-density polyethylene, homopolypropylene, and the aforementioned thermoplastic elastomer, random polypropylene, and other thermoplastic resins (hereinafter also referred to as "other thermoplastic resins") that may be optionally contained, and the content of the high-density polyethylene, homopolypropylene, and other thermoplastic resins is specified with the total mass of the thermoplastic resins being 100% by mass.
[0061] Here, the contents of high-density polyethylene, homopolypropylene, and other thermoplastic resins in the resin composition constituting the outer layer on the side that comes into contact with the metal roll can be specified as follows: high-density polyethylene content of 20 to 90 mass%, homopolypropylene content of 10 to 75 mass%, and other thermoplastic resins content of 0 to 30 mass% (the total mass of high-density polyethylene, homopolypropylene, and other thermoplastic resins is 100 mass%). Furthermore, the total mass of the thermoplastic resin contained in the resin composition constituting the intermediate layer means the total mass of the high-density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and the masses of the other thermoplastic resins mentioned above that may be optionally contained, and the content of the high-density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and other thermoplastic resins is specified with the mass of the total thermoplastic resin being 100% by mass. Here, the contents of high-density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and other thermoplastic resins in the resin composition constituting the intermediate layer can be specified as follows: high-density polyethylene content of 3 to 15 mass%, homopolypropylene content of 10 to 50 mass%, at least one selected from the group consisting of thermoplastic elastomer and random polypropylene content of 10 to 85 mass%, and other thermoplastic resin content of 0 to 40 mass% (the total amount of high-density polyethylene, homopolypropylene, thermoplastic elastomer, random polypropylene, and other thermoplastic resins is 100 mass%).
[0062] By incorporating the aforementioned high-density polyethylene and homopolypropylene in predetermined amounts into the resin composition constituting the outer layer on the side that contacts the metal roll, it is possible to adjust the heat resistance and flexibility of the resulting film and further suppress blocking between films. When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side that contacts the metal roll is taken as 100% by mass, the high-density polyethylene content is 20 to 90% by mass and the homopolypropylene content is 10 to 75% by mass. By containing high-density polyethylene in a range of 20 to 90% by mass, flexibility can be imparted to the film without impairing its heat resistance, and blocking between films can be improved. Furthermore, as described above, adhesion to the metal roll can be suppressed, and at the same time, the occurrence of appearance defects such as unevenness in the film due to air entrapment can be suppressed. The high-density polyethylene content is preferably in a range of 25 to 85% by mass, more preferably 30 to 80% by mass. By having the homopolypropylene content within the range of 10 to 75% by mass, it is possible to impart heat resistance to the film without impairing flexibility, and to improve the blocking resistance between films. The homopolypropylene content is preferably within the range of 12 to 65% by mass, more preferably within the range of 14 to 60% by mass. Furthermore, it is preferable that the total amount of high-density polyethylene and homopolypropylene is 45% by mass or more. By having the high-density polyethylene and homopolypropylene content be 45% by mass or more, it is possible to impart heat resistance and flexibility to the film, and to improve the blocking resistance between films. It is more preferable that the total amount is 50% by mass or more, and even more preferably 55% by mass or more.
[0063] The resin composition constituting the outer layer on the side in contact with the metal roll can contain the aforementioned other thermoplastic resins and other components in addition to high-density polyethylene and homopolypropylene. Adding other thermoplastic resins can impair flexibility and heat resistance, and can also increase the likelihood of blocking between films. Therefore, the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll must be adjusted to fall within the range of 0 to 30% by mass, assuming that the total amount is 100% by mass. It is more preferably within the range of 0 to 25% by mass, and even more preferably within the range of 0 to 20% by mass. The resin compositions used for the front and back layers may be the same or different, and may be high-density polyethylene, homopolypropylene, or other thermoplastic resins within a specified range, as long as the heat resistance, flexibility, and blocking properties of the resulting film are not impaired.
[0064] Regarding the hardness of the resin composition constituting the outer layer on the side that comes into contact with the metal roll, the tensile modulus of a film obtained from the resin composition alone is preferably in the range of 500 to 1800 MPa. If the tensile modulus is in the range of 500 to 1800 MPa, blocking between the thermoplastic resin films of the present invention can be easily suppressed. It is more preferably in the range of 550 to 1750 MPa, and even more preferably in the range of 600 to 1700 MPa. The tensile modulus can be measured using the same method as described in the section on high-density polyethylene.
[0065] The resin composition constituting the layer of the two outer layers that comes into contact with the rubber roll may be the same as or different from the resin composition constituting the layer that comes into contact with the metal roll. A preferred resin composition can be used as long as it does not affect the performance of the thermoplastic resin film, such as the blocking property between films, flexibility, and heat resistance. As the rubber material for the rubber roll, silicone resins and fluororesins are preferably used, as described below, and therefore adhesion to the thermoplastic resin tends to be inferior compared to the metal roll. Whether or not to use the same resin composition as the outer layer on the metal roll side can be selected based on the performance of the resulting film and ease of film formation. When it is necessary to eliminate differences in performance between the front and back sides, it is preferable to use the same resin composition for both outer layers. When different performances are required between the front and back sides, it is preferable to use different resin compositions for the two outer layers. Furthermore, from the viewpoint of suppressing blocking between films, it is preferable that the resin compositions constituting the layer that comes into contact with the metal roll and the layer that comes into contact with the rubber roll each have a tensile modulus within the above-mentioned range.
[0066] By including a predetermined amount of at least one selected from the group consisting of the aforementioned high-density polyethylene and homopolypropylene, thermoplastic elastomer and random polypropylene in the resin composition used for the intermediate layer, it becomes possible to adjust the flexibility of the resulting film while maintaining heat resistance, and further to improve the adhesion between each layer. The contents of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene are 3 to 15 mass% of high-density polyethylene, 10 to 50 mass% of homopolypropylene, 10 to 85 mass% of at least one selected from the group consisting of thermoplastic elastomer and random polypropylene, and 0 to 40 mass% of other thermoplastic resins, when the total thermoplastic resins contained in the resin composition constituting the intermediate layer of the film is taken as 100 mass%. By setting the content of high-density polyethylene within the range of 3 to 15% by mass, the heat resistance and flexibility of the film are not impaired and adhesion between the front and back layers can be imparted. The content of high-density polyethylene is preferably within the range of 5 to 13% by mass, more preferably within the range of 7 to 11% by mass. When the homopolypropylene content is within the range of 10 to 50% by mass, it is possible to impart heat resistance to the film. The homopolypropylene content is preferably within the range of 13 to 47% by mass, and more preferably within the range of 16 to 44% by mass. The flexibility of the film can be easily adjusted by setting the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes within the range of 10 to 85% by mass. The content of the thermoplastic elastomer and random polypropylene is preferably within the range of 15 to 80% by mass, more preferably within the range of 20 to 75% by mass, and even more preferably within the range of 25 to 70% by mass. In this specification, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is in the range of 10 to 85 mass%. This means that when either a thermoplastic elastomer or random polypropylene is selected, the content of that one is in the range of 10 to 85 mass%. When two or more of a thermoplastic elastomer and random polypropylene are selected, the total content of those two or more is in the range of 10 to 85 mass%. Either case is within the scope of the present invention. Furthermore, when two or more of a thermoplastic elastomer and a random polypropylene are selected, it is preferable that the content of at least one of the two or more is in the range of 10 to 85 mass%, and that the total content of the two or more is in the range of more than 10 mass% and not more than 85 mass%. When the content of at least one of the two or more types is within the range of 10 to 85 mass %, and the total content of the two or more types is within the range of more than 10 mass % and not more than 85 mass %, it becomes easy to achieve both heat resistance and flexibility. Furthermore, when two or more of a thermoplastic elastomer and a random polypropylene are selected, it is more preferable that the content of each of the two or more is in the range of 10 to 85 mass %, and that the total content of the two or more is in the range of 20 to 85 mass %. By ensuring that the content of at least one of the two or more types is within the range of 10 to 85 mass % and that the total content of the two or more types is within the range of 20 to 85 mass % or less, it becomes easier to achieve both heat resistance and flexibility. Regarding the strength of the resin composition used in the intermediate layer, the tensile modulus of a film obtained from the resin composition alone is preferably in the range of 30 to 600 MPa. If the tensile modulus is in the range of 30 to 600 MPa, it becomes easy to adjust the flexibility of the thermoplastic resin films of the present invention. It is more preferably in the range of 40 to 550 MPa, and even more preferably in the range of 50 to 500 MPa. The tensile modulus can be measured by the same method as described in the section on high-density polyethylene.
[0067] The resin composition used in the intermediate layer can contain the above-mentioned other thermoplastic resins and other components in addition to high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene. The content of other thermoplastic resins is 0 to 40% by mass. When it is necessary to adjust the heat resistance and flexibility of the resulting film or to impart film formability, the resin used can be appropriately selected and used. The amount used can be adjusted within a range that does not impair heat resistance or flexibility, and is more preferably 0 to 38% by mass, and even more preferably 0 to 36% by mass.
[0068] The thermoplastic resin film of the present invention has a basic structure of at least a three-layer film, comprising an outer layer on the side that comes into contact with the metal roll, which contains high-density polyethylene and homopolypropylene; an intermediate layer that contains at least one selected from the group consisting of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene; and an outer layer on the side that comes into contact with the rubber roll. In this at least three-layer film configuration, the resin compositions constituting both outer layers may be the same or different, as described above. The intermediate layer may also be composed of two or more layers. In this case, a film configuration consisting of three or more layers is also included. In this case, all of the intermediate layers consisting of two or more layers must contain a predetermined amount of at least one selected from the group consisting of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, and the resin compositions constituting each layer may be the same or different. From the viewpoint of productivity and economic efficiency of the film, a three-layer film consisting of two outer layers and one intermediate layer is preferable. In this case, whether to use a two-kind three-layer film in which the front and back layers are made of the same resin composition or a three-kind three-layer film in which the front and back layers are made of different resin compositions can be selected appropriately as needed, taking into consideration the required performance and use of each of the front and back layers of the film, and the processability when providing an adhesive layer or a printed layer, which will be described later.
[0069] The total thickness of the thermoplastic resin film of the present invention is preferably 30 to 250 μm. If it is 30 μm or more, the film production properties and the handleability of the resulting film are good, and flexibility and heat resistance can be maintained at a good level. If it is 250 μm or less, the handleability and processability of the film can be maintained at a good level in the step of laminating a printing layer or an adhesive layer to the film. The total thickness of the thermoplastic resin film of the present invention is more preferably 40 to 230 μm, and even more preferably 50 to 210 μm. The thickness of each of the outer layers is preferably within a range of 1 to 30% of the total thickness of the thermoplastic resin film. By making the thickness 1% or more of the total thickness, it is possible to impart the effect of suppressing blocking between the films, and by making the thickness 30% or less, the flexibility of the obtained film is not impaired, which is preferable. The thickness is more preferably within a range of 3 to 25%, and even more preferably within a range of 5 to 20%. The thickness of each of the outer layers may be the same or different, as long as it satisfies the performance required of each of the outer layers of the obtained thermoplastic resin film and can suppress blocking between the films. From the viewpoints of film productivity and economic efficiency, it is preferable that the thickness of both outer layers is the same.
[0070] The thermoplastic resin film of the present invention is a film characterized by having a high transparency with small surface irregularities, and having a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less in both outer layers of the film, where the surface roughness (Ra) is also referred to as the arithmetic mean surface roughness (Ra). By making the surface roughness (Ra) 0.5 μm or less and the maximum height (Rz) 3.0 μm or less, it is possible to obtain a film with a nearly smooth surface and high transparency. More preferred values for the surface roughness (Ra) and maximum height (Rz) are a surface roughness (Ra) of 0.4 μm or less and a maximum height (Rz) of 2.5 μm or less, and even more preferred values are a surface roughness (Ra) of 0.3 μm or less and a maximum height (Rz) of 2.0 μm or less.
[0071] The surface roughness (Ra) and maximum height (Rz) of both outer layers may be adjusted so that they are approximately the same, or may be adjusted so that they are different values within the above-mentioned range. When adjusting to have different values, which layer should have a higher (lower) value can be adjusted appropriately as needed, taking into consideration the application and the processability when providing the adhesive layer and printing layer described below.
[0072] There are no particular limitations on the method for measuring the surface roughness (Ra) and maximum height (Rz), and any known method can be used. For example, a commonly used stylus, contact, or non-contact surface roughness meter can be used according to the method specified in JIS B0601, etc.
[0073] Regarding the transparency of the thermoplastic resin film, the haze of the film is preferably 50% or less. If the haze is 50% or less, scattering of laser light or the like irradiated from the light source can be suppressed, enabling the light to be accurately focused on the wafer. It is more preferably 36% or less, and even more preferably 32% or less. Furthermore, it is preferable that the total light transmittance is 70% or more. A total light transmittance of 70% or more is preferable because attenuation of laser light when passing through the film is suppressed. It is more preferably 75% or more, and even more preferably 80% or more.
[0074] The method for measuring the total light transmittance and haze is not particularly limited, and known methods can be used. For example, a commonly used transmittance measuring device, a haze meter, etc., can be used according to the method specified in JIS K7361, JIS K7136, etc.
[0075] The tensile modulus of the thermoplastic resin film of the present invention is preferably within the range of 80 to 600 MPa. If it is 80 MPa or more, the film is not too flexible and can maintain good handleability, and if it is 600 MPa or less, the flexibility of the film is not impaired and the film can maintain good handleability and processability in the step of laminating a printing layer or an adhesive layer onto the film. It is more preferably within the range of 100 to 550 MPa, and even more preferably within the range of 120 to 500 MPa.
[0076] The thermoplastic resin film of the present invention preferably has a tensile elongation at break of 300% or more. A tensile elongation of 300% or more prevents breakage during handling of the film, thereby preventing problems due to breakage when adhesive processing or the like is performed, and is also preferable because breakage during expansion is less likely to occur in the expanding step of semiconductor manufacturing processes. A tensile elongation of 400% or more is more preferable, and 500% or more is even more preferable. The tensile modulus and elongation at break can be measured using the same methods as those described in the section on high-density polyethylene.
[0077] 2. Thermoplastic resin film manufacturing method Although known methods can be used to form the thermoplastic resin film of the present invention, it is necessary to use a melt extrusion molding method in which a film is formed by nipping between a metal roll and a rubber roll. By nipping, the surface shapes of the rolls can be transferred to the film, making it easier to maintain uniform surface roughness and appearance of the film. The surface roughness (Ra) of the metal roll and rubber roll used for nipping is preferably 0.5 μm or less. By using rolls with a surface roughness of 0.5 μm or less, it is possible to easily suppress blocking between films while improving the transparency of the resulting film. The surface roughness (Ra) is more preferably 0.45 μm or less, and even more preferably 0.40 μm or less. Furthermore, when nipping is performed between metal rolls, the rolls may come into contact with each other and be damaged if the film breaks.Furthermore, when nipping is performed between rubber rolls, both rolls may deform during nipping, making pressure adjustment and control unstable, and the appearance of the film may also be unstable.Therefore, it is preferable to nip using a metal roll and a rubber roll. As a molding method other than the nip method, known methods can be used, such as air knife molding and air chamber molding. Air knife molding and air chamber molding are molding methods in which a gas is supplied and the molten resin is pressed against a roll by pressure, and can be selected when a film with low surface roughness (Ra) and high transparency is to be obtained.
[0078] That is, another aspect of the present invention is a method for producing a thermoplastic resin film consisting of at least three layers, namely, two outer layers and an intermediate layer, comprising the steps of: The production method includes nipping an extruded molten resin between a metal roll and a rubber roll to obtain the thermoplastic resin film, The surface roughness (Ra) of the metal roll and the rubber roll used to nip the extruded molten resin is 0.5 μm or less, The resin composition constituting the outer layer on the side in contact with the metal roll contains high-density polyethylene and homopolypropylene, the intermediate layer contains at least one selected from the group consisting of high-density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene; The thermoplastic resin film produced by this method satisfies the following requirements (hereinafter also referred to as the "thermoplastic resin film producing method of the present invention"). (1) When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll is taken as 100% by mass, the content of high-density polyethylene is 20 to 90% by mass, the content of homopolypropylene is 10 to 75% by mass, and the content of other thermoplastic resins is 0 to 30% by mass. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of both outer layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
[0079] Among the melt extrusion molding methods for producing the thermoplastic resin film of the present invention, the T-die molding method is more preferred, in which a molten resin is extruded from an extruder having a T-die, nipped with rolls, and cooled and solidified to obtain a film. To obtain a multilayer film consisting of both outer layers and an intermediate layer, it is preferable to use a co-extrusion T-die molding method using multiple extruders. By using a co-extrusion T-die molding method using multiple extruders, it is possible to obtain a multilayer film, which can be the film of the present invention consisting of both outer layers and an intermediate layer. It is also possible to obtain an intermediate layer consisting of two or more layers.
[0080] Examples of co-extrusion T-die molding methods include a method in which multiple resin layers are formed into a film using a multi-manifold die, and then the layers are brought into contact within the T-die to form a multi-layered film; and a method in which multiple resins are brought into contact with each other using a device that combines molten resins called a feed block, and then the resins are brought into contact with each other to form a multi-layered film.
[0081] To cool and solidify the resin extruded in a molten state from a T-die, it is necessary to use a method in which the resin is nipped and contacted between a metal roll and a rubber roll set at a predetermined temperature to solidify it. By obtaining a film by nipping with rolls having the surface roughness described below, it is possible to adjust the surface roughness and transparency of the film to a preferred range.
[0082] The set temperatures of the metal roll and the rubber roll are not particularly limited, but are preferably set to 80°C or less. If the temperature is 80°C or less, it is possible to prevent the phenomenon in which the molten resin remains stuck to the chill roll and cannot be peeled off. The temperature is more preferably 70°C or less, and even more preferably 60°C or less. Furthermore, the surface temperature of the chill roll is preferably 100°C or less from the viewpoint of preventing problems caused by the same film sticking.
[0083] The metal roll and rubber roll used in the method for producing a thermoplastic resin film of the present invention preferably have a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less. By using such metal rolls and rubber rolls, it is possible to obtain a film with a predetermined surface roughness. More preferred values for the surface roughness (Ra) and maximum height (Rz) of the roll are a surface roughness (Ra) of 0.4 μm or less and a maximum height (Rz) of 2.5 μm or less, and even more preferred values are a surface roughness (Ra) of 0.3 μm or less and a maximum height (Rz) of 2.0 μm or less. The metal roll and the rubber roll may have the same roughness, or may have different roughnesses as long as they are within the above-mentioned roughness range. When adjusting the roughness values to be different, the value of which layer should be higher (lower) can be adjusted as needed, taking into consideration the application and the processability when providing the adhesive layer and the printing layer described below. The roughness of the metal roll and the rubber roll can be adjusted by a known method, for example, buff polishing, belt polishing, blasting methods such as sandblasting and glass bead blasting, laser processing, etc. From the viewpoint of ease of processing and ease of adjusting the surface roughness, it is preferable to use polishing using a buff, belt, etc., or blasting. The material of the metal roll is not particularly limited, and known materials can be selected and used, such as iron, steel, stainless steel, nickel, etc. From the viewpoints of ease of handling and economy, it is preferable to use steel, stainless steel, or nickel. Furthermore, in order to improve the durability of the metal roll, it is more preferable that the surface of the metal roll is chrome-plated. The method for cooling the metal roll is not particularly limited, and any known method can be used, such as cooling with air, a method using a liquid refrigerant such as water or oil, or a cooling method using an electric heater or dielectric heating. From the viewpoint of cooling efficiency and ease of handling, it is preferable to use a method using a liquid refrigerant such as water or oil, or a method using an electric heater or dielectric heating. The material of the rubber roll is not particularly limited, and any known material can be selected and used, for example, natural rubber, nitrile rubber, butyl rubber, ethylene propylene diene rubber (EPDM), silicone resin, fluororesin such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), perfluoroethylenepropene (FEP), ethylene tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), etc. Among these, from the viewpoint of releasability of the film from the roll, it is preferable to use a rubber roll made of silicone resin or fluororesin. The rubber roll can be cooled by the same method as the above-mentioned metal roll.
[0084] Furthermore, if necessary, one or both sides of the present thermoplastic resin film may be subjected to a surface treatment such as plasma treatment, corona treatment, ozone treatment, flame treatment, etc. From the viewpoint of the intended use of the resulting film and the prevention of blocking between films, it is possible to select whether to perform a surface treatment on one or both sides, or whether to perform no corona treatment on either side.
[0085] 3. Adhesive film The thermoplastic resin film of the present invention can be made into a pressure-sensitive adhesive film by providing a pressure-sensitive adhesive layer on at least one of the outer and inner surfaces (hereinafter also referred to as "pressure-sensitive adhesive film of the present invention"). The adhesive used in the adhesive layer is not particularly limited, and various adhesives such as natural rubber resins, acrylic resins, styrene resins, silicone resins, polyvinyl ether resins, etc. may be used. Furthermore, a functional layer such as an adhesive layer or a thermosetting resin layer may be further provided on the adhesive layer.
[0086] The pressure-sensitive adhesive layer can be provided by directly coating the pressure-sensitive adhesive onto the thermoplastic resin film of the present invention, or by laminating the pressure-sensitive adhesive layer onto a separator or the like having a release layer, and then bonding the pressure-sensitive adhesive layer side of the separator to either of the two outer layers of the film of the present invention, thereby transferring the pressure-sensitive adhesive layer. In the pressure-sensitive adhesive film of the present invention, one or both surfaces of the film may be subjected to the above-described surface treatment before the pressure-sensitive adhesive layer is provided. Furthermore, a primer layer may be provided between the film and the pressure-sensitive adhesive layer, if necessary. The thickness of the adhesive layer and the primer layer can be appropriately determined as needed.
[0087] The present invention provides a film that has low surface roughness, high transparency, and sufficient heat resistance, which is obtained by nipping between a metal roll and a rubber roll.Furthermore, it is possible to suppress blocking between films when handling the film, making it possible to obtain a thermoplastic resin film that has excellent handleability, flexibility, and a good appearance. Furthermore, the present invention also makes it possible to provide a pressure-sensitive adhesive film that can be suitably used in semiconductor manufacturing processes by providing a pressure-sensitive adhesive layer on the thermoplastic resin film. [Example]
[0088] The present invention will be specifically explained below by showing examples and comparative examples, but the present invention is not limited to these examples. The materials used in the following examples and comparative examples and the methods for measuring the evaluated properties are as follows.
[0089] [Materials used] As the thermoplastic resin, a polypropylene-based resin, a polyethylene-based resin, and a styrene-based elastomer were used as shown below.
[0090] <High-density polyethylene> "HF560" manufactured by Japan Polyethylene Corporation (high-density polyethylene, melt flow rate at 190°C and 2.16 kg: 7.0 g / 10 min, crystalline melting peak: 134°C, density: 0.963 g / cm 3 , Tensile modulus of the film alone: 1000 MPa) <Linear low-density polyethylene> "0540F" (linear low-density polyethylene, melt flow rate at 190°C and 2.16 kg: 4.0 g / 10 min, crystalline melting peaks at 91°C and 111°C, density: 0.904 g / cm), manufactured by Ube Maruzen Polyethylene Co., Ltd. 3 , Tensile modulus of the film alone: 90 MPa) <Low-density polyethylene> "Novatec LC500" manufactured by Japan Polyethylene Corporation (low-density polyethylene, melt flow rate at 190°C and 2.16 kg: 4.0 g / 10 min, crystalline melting peak: 106°C, density: 0.923 g / cm 3 , Tensile modulus of the film alone: 140 MPa) <Homopolypropylene> Sumitomo Chemical Co., Ltd., "FLX80H5" (homopolypropylene, melt flow rate at 230°C and 2.16 kg: 8.0 g / 10 min, crystalline melting peak: 162°C, tensile modulus of film: 900 MPa) <Random polypropylene> SunAllomer Corporation's "PC630A" (random polypropylene, melt flow rate at 230°C and 2.16 kg: 7.5 g / 10 min, crystalline melting peak: 135°C, tensile modulus of film: 600 MPa) <Olefin elastomer> RFG4VM (olefin elastomer, melt flow rate at 230°C and 2.16 kg: 6.0 g / 10 min, crystalline melting peak: 129°C, tensile modulus of film: 250 MPa) manufactured by Japan Polypropylene Corporation <Styrene-based elastomer> Styrene elastomer (α) Asahi Kasei's "Tuftec H1221" (melt flow rate at 230°C and 2.16 kg: 4.5 g / 10 min, styrene content: 12% by mass, styrene-ethylene-butylene-styrene copolymer) Styrene elastomer (β) Asahi Kasei's "Tuftec H1517" (melt flow rate at 230°C and 2.16 kg: 5.0 g / 10 min, styrene content: 43% by mass, styrene-ethylene-butylene-styrene copolymer)
[0091] <Preparation of Resin Composition> The above thermoplastic resins were blended so that the total amount was 100 parts by mass. When two or more types were used, they were mixed by dry blending, and it was confirmed by visual inspection that the mixture was uniform.
[0092] <Film production method> Each resin composition was charged into the hopper of three Toshiba Machine single-screw extruders (surface layer: 35φmm, L / D=25mm, middle layer: 50φmm, L / D=32, back layer: 35φmm, L / D=25mm), and the extruder temperature of each extruder was set to 190-230°C. The three-layer structure of surface layer / middle layer / back layer was merged in the feed block section and extruded through a 650mm wide T-die (temperature setting 210-230°C, lip opening 0.5mm). The rotation speed of each extruder was set to obtain the thickness structure shown in Table 1. The extruded molten resin was nipped between a matte metal roll (surface chrome plated, surface roughness Ra approximately 0.3 μm, 700 mm wide x φ350 mm) through which cooling water set at 30°C was passed, and a matte rubber roll (fluororesin coated roll, surface roughness Ra approximately 0.3 μm, 700 mm wide x φ200 mm) through which cooling water was passed, and after cooling and solidifying into a film, it was taken up on a winding machine to obtain films with a thickness of approximately 80 μm, consisting of 3 layers of type 1, 3 layers of type 2, and 3 layers of type 3. In the present invention, the metal roll side of the obtained film is referred to as the surface layer, and the rubber roll side is referred to as the back layer.
[0093] [Thickness of each layer] The thickness of each layer was calculated from the amount of resin extruded from each extruder. [Total film thickness] The thickness of the film was measured at the center and both ends using a contact thickness meter to confirm that the film had the desired thickness.
[0094] [Surface roughness (Ra), maximum height (Rz)] The surface roughness and maximum height of the front and back layers of the obtained film were measured using a Tokyo Seimitsu SURFCOM FLEX-50A in accordance with JIS B0601 (2001) using a stylus tip with a tip radius of 2 μm and a conical taper angle of 60° at a measuring force of 0.7 mN.
[0095] [Total light transmittance, haze] The total light transmittance and haze of the film were measured under the following conditions. The total light transmittance was measured in accordance with JIS K7361-1, and the haze was measured in accordance with JIS K7136 using NDH2000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0096] Tensile modulus Test pieces were taken from the obtained thermoplastic resin film using a dumbbell "SDK-600" manufactured in accordance with JIS K6732, and the tensile modulus (MPa) was measured at a tension speed of 50 mm / min using an autograph (Shimadzu Corporation AGS-X) under the following conditions, which refer to JIS K7127: 23°C, 50% RH. The tensile modulus was measured in the extrusion direction (MD) of the film.
[0097] [Tensile elongation at break] Test pieces were taken from the obtained film using a dumbbell "SDK-600" manufactured in accordance with JIS K6732, and the tensile elongation at break (%) was measured at a tension speed of 300 mm / min using a small tabletop testing machine (Shimadzu EZ-L) in an atmosphere of 23°C and 50% RH. The tensile elongation at break was measured in the extrusion direction (MD) of the film.
[0098] [Blocking evaluation] The obtained film was wound into a roll of 50 m, and after storage for one day, the film was pulled out from the roll and evaluated for the presence or absence of blocking between the films according to the following criteria. ◎: No blocking and easy to unwind 〇: Slight blocking is observed, but the film can be easily unwound. △: Blocking is observed, but unwinding is possible ×: Significant blocking was observed, and unwinding was not possible
[0099] [Unevenness of metal roll surface] The metal roll side of the obtained film was observed at a magnification of approximately 270x using a microscope "SKM-Z200C-PC" manufactured by Saito Optical Co., Ltd., and the irregularities caused by air bubbles observed in the film were evaluated according to the following criteria. ◎: No irregularities are observed ○: Minute irregularities caused by air bubbles can be observed, but their size cannot be measured △: Multiple irregularities caused by bubbles smaller than 30 μm are observed. ×: Multiple irregularities caused by bubbles of 30 μm or more are observed.
[0100] [Crystal melting peak] Using a differential scanning calorimeter (DSC823e manufactured by Mettler-Toledo), approximately 5 mg of test pieces taken from the films obtained in the Examples and Comparative Examples were heated from 25°C to 230°C at a heating rate of 10°C / min, then cooled to 25°C at a cooling rate of 10°C / min, and then heated again to 230°C at a heating rate of 10°C / min. The crystalline melting peak was calculated from the chart measured.
[0101] [Example 1] The thermoplastic resins for the surface, intermediate and back layers were high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer (α) in the amounts shown in Table 1, and resin compositions for each layer were prepared. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by nip molding using the matte metal cooling roll and the matte fluororesin-coated rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.11 μm and the maximum height (Rz) was 1.08 μm, and the surface roughness (Ra) of the back layer side was 0.12 μm and the maximum height (Rz) was 0.92 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 90.0% and the haze was 27.0%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The front and back layers of this film contain a specified amount of high-density polyethylene and homopolypropylene, and the film obtained from only the resin composition of each of the front and back layers exhibited a tensile modulus of 870 MPa. Therefore, no blocking was observed when the film was unwound from the roll, and it could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when subsequent adhesive and printing layers are applied. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 200 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 260 MPa and a tensile breaking elongation of 820%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0102] [Example 2] The thermoplastic resins for the surface, intermediate and back layers were high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer (α) in the amounts shown in Table 1, and resin compositions for each layer were prepared. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.10 μm and the maximum height (Rz) was 0.84 μm, and the surface roughness (Ra) of the back layer side was 0.15 μm and the maximum height (Rz) was 1.04 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.4% and the haze was 22.0%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The front and back layers of this film contain a specified amount of high-density polyethylene and homopolypropylene, and the film obtained from only the resin composition of each of the front and back layers exhibited a tensile modulus of 860 MPa. Therefore, no blocking was observed when the film was unwound from the roll, and it could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 200 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 260 MPa and a tensile breaking elongation of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0103] [Example 3] The thermoplastic resins for the surface, intermediate and back layers were high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer and styrene-based elastomer (α) in the amounts shown in Table 1, and resin compositions for each layer were prepared. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.06 μm, and the surface roughness (Ra) of the back layer side was 0.18 μm and the maximum height (Rz) was 1.31 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.3% and the haze was 23.4%, and the film had excellent matte transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The front and back layers of this film contain a specified amount of high-density polyethylene and homopolypropylene, and the film obtained from only the resin composition of each of the front and back layers exhibited a tensile modulus of 880 MPa. Therefore, no blocking was observed when the film was unwound from the roll, and it could be easily unwound. Therefore, it is presumed that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 200 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 260 MPa and a tensile breaking elongation of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0104] [Example 4] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and styrene-based elastomer (α), the thermoplastic resins for the middle layer were high-density polyethylene, homopolypropylene, random polypropylene, and styrene-based elastomer (α), and the thermoplastic resins for the back layer were homopolypropylene and random polypropylene, and the resin compositions for each layer were prepared in the amounts listed in Table 1. Using the resin compositions for the surface, middle, and back layers, a three-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.13 μm and the maximum height (Rz) was 1.05 μm, and the surface roughness (Ra) of the back layer side was 0.10 μm and the maximum height (Rz) was 0.91 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 90.1% and the haze was 23.3%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The surface layer of this film contains a specified amount of high-density polyethylene and homopolypropylene. Furthermore, a film obtained from only the resin composition of the surface layer exhibited a tensile modulus of 800 MPa, while a film obtained from only the resin composition of the back layer exhibited a tensile modulus of 790 MPa. Furthermore, when unwinding the film from the roll obtained by winding up the film having this surface and back layers, no blocking was observed, and it could be easily unwound. Therefore, it is inferred that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, random polypropylene, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 270 MPa, suggesting that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 320 MPa and a tensile breaking elongation of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 162°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0105] [Example 5] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and a styrene-based elastomer (α); the thermoplastic resins for the middle layer were high-density polyethylene, homopolypropylene, an olefin-based elastomer, and a styrene-based elastomer (α); and the thermoplastic resins for the back layer were homopolypropylene and an olefin-based elastomer, and the resin compositions for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface, middle, and back layers, a three-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.01 μm, and the surface roughness (Ra) of the back layer side was 0.12 μm and the maximum height (Rz) was 0.95 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.5% and the haze was 30.0%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The surface layer of this film contains a specified amount of high-density polyethylene and homopolypropylene. Furthermore, a film obtained from only the resin composition of the surface layer exhibited a tensile modulus of 800 MPa, while a film obtained from only the resin composition of the back layer exhibited a tensile modulus of 650 MPa. Furthermore, when unwinding the film from the roll obtained by winding up the film having this surface and back layers, no blocking was observed, and it could be easily unwound. Therefore, it is inferred that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 260 MPa, suggesting that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 300 MPa and a tensile breaking elongation of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0106] [Example 6] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and a styrene-based elastomer (α); the thermoplastic resins for the middle layer were high-density polyethylene, homopolypropylene, an olefin-based elastomer, and a styrene-based elastomer (α); and the thermoplastic resins for the back layer were homopolypropylene and an olefin-based elastomer, and the resin compositions for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface, middle, and back layers, a three-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.13 μm and the maximum height (Rz) was 1.22 μm, and the surface roughness (Ra) of the back side was 0.12 μm and the maximum height (Rz) was 1.11 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.5% and the haze was 29.9%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The surface layer of this film contains a specified amount of high-density polyethylene and homopolypropylene. Furthermore, a film obtained from only the resin composition of the surface layer exhibited a tensile modulus of 800 MPa, while a film obtained from only the resin composition of the back layer exhibited a tensile modulus of 650 MPa. Furthermore, when unwinding the film from the roll obtained by winding up the film having this surface and back layers, no blocking was observed, and it could be easily unwound. Therefore, it is inferred that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains specified amounts of high-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 220 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 270 MPa and a tensile breaking elongation of 800%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 129°C and 163°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0107] [Example 7] The thermoplastic resins for the surface layer were high-density polyethylene, linear low-density polyethylene, and homopolypropylene. The thermoplastic resins for the middle layer were high-density polyethylene, linear high-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer (β). The thermoplastic resins for the back layer were homopolypropylene and olefin-based elastomer. These were blended in the amounts shown in Table 1 to prepare the resin compositions for each layer. Using the resin compositions for the surface, middle, and back layers, a three-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.32 μm, and the surface roughness (Ra) of the back layer side was 0.12 μm and the maximum height (Rz) was 0.96 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.6% and the haze was 31.2%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The surface layer of this film contains a specified amount of high-density polyethylene and homopolypropylene. Furthermore, a film obtained from only the resin composition of the surface layer exhibited a tensile modulus of 900 MPa, while a film obtained from only the resin composition of the back layer exhibited a tensile modulus of 650 MPa. Furthermore, when unwinding the film from the roll obtained by winding up the film having this surface and back layers, no blocking was observed, and it could be easily unwound. Therefore, it is inferred that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains specified amounts of high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 410 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 440 MPa and a tensile breaking elongation of 790%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 129°C and 162°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0108] [Example 8] The thermoplastic resins for the surface layer were high-density polyethylene, homopolypropylene, and styrene-based elastomer (α); the thermoplastic resins for the middle layer were high-density polyethylene, low-density polyethylene, homopolypropylene, random polypropylene, and styrene-based elastomer (α); and the thermoplastic resins for the back layer were homopolypropylene and random polypropylene, and the resin compositions for each layer were prepared in the amounts shown in Table 1. Using the resin compositions for the surface, middle, and back layers, a three-layer, three-kind film with a total thickness of 80 μm was obtained by nip molding using the matte metal cooling roll and the matte fluororesin-coated rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.13 μm and the maximum height (Rz) was 1.21 μm, and the surface roughness (Ra) of the back layer side was 0.14 μm and the maximum height (Rz) was 1.00 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.4% and the haze was 21.8%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The surface layer of this film contains a specified amount of high-density polyethylene and homopolypropylene. Furthermore, a film obtained from only the resin composition of the surface layer exhibited a tensile modulus of 890 MPa, while a film obtained from only the resin composition of the back layer exhibited a tensile modulus of 720 MPa. Furthermore, when unwinding the film from the roll obtained by winding up the film having this surface and back layers, no blocking was observed, and it could be easily unwound. Therefore, it is inferred that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains specified amounts of high-density polyethylene, linear low-density polyethylene, homopolypropylene, olefin-based elastomer, and styrene-based elastomer, and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 250 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 290 MPa and a tensile breaking elongation of 830%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 162°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0109] [Example 9] The thermoplastic resins for the surface layer were high-density polyethylene, linear low-density polyethylene, and homopolypropylene. The thermoplastic resins for the middle layer were high-density polyethylene, linear low-density polyethylene, homopolypropylene, random polypropylene, and styrene-based elastomer (α). The thermoplastic resins for the back layer were homopolypropylene and random polypropylene. These were blended in the amounts shown in Table 1 to prepare the resin compositions for each layer. Using the resin compositions for the surface, middle, and back layers, a three-layer, three-kind film with a total thickness of 80 μm was obtained by nip molding using the matte metal cooling roll and the matte fluororesin-coated rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.11 μm and the maximum height (Rz) was 1.18 μm, and the surface roughness (Ra) of the back layer side was 0.12 μm and the maximum height (Rz) was 1.02 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 88.8% and the haze was 15.4%, and the film had excellent matte transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The surface layer of this film contains a specified amount of high-density polyethylene and homopolypropylene. Furthermore, a film obtained from only the resin composition of the surface layer exhibited a tensile modulus of 890 MPa, while a film obtained from only the resin composition of the back layer exhibited a tensile modulus of 720 MPa. Furthermore, when unwinding the film from the roll obtained by winding up the film having this surface and back layers, no blocking was observed, and it could be easily unwound. Therefore, it is inferred that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains a predetermined amount of high-density polyethylene, linear low-density polyethylene, homopolypropylene, random polypropylene, and styrene-based elastomer (α), and the tensile modulus of the film obtained from only the resin composition of the intermediate layer was 240 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 280 MPa and a tensile breaking elongation of 840%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 161°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0110] [Example 10] The thermoplastic resins for the surface layer were high-density polyethylene, linear low-density polyethylene, and homopolypropylene. The thermoplastic resins for the middle layer were high-density polyethylene, linear low-density polyethylene, homopolypropylene, random polypropylene, and styrene-based elastomer (α). The thermoplastic resins for the back layer were homopolypropylene and random polypropylene. These were blended in the amounts shown in Table 1 to prepare the resin compositions for each layer. Using the resin compositions for the surface, middle, and back layers, a three-layer, three-kind film with a total thickness of 80 μm was obtained by nip molding using the matte metal cooling roll and the matte fluororesin-coated rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.30 μm, and the surface roughness (Ra) of the back layer side was 0.12 μm and the maximum height (Rz) was 0.95 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.0% and the haze was 16.5%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The surface layer of this film contains a specified amount of high-density polyethylene and homopolypropylene. Furthermore, a film obtained from only the resin composition of the surface layer exhibited a tensile modulus of 890 MPa, while a film obtained from only the resin composition of the back layer exhibited a tensile modulus of 720 MPa. Furthermore, when unwinding the film from the roll obtained by winding up the film having this surface and back layers, no blocking was observed, and it could be easily unwound. Therefore, it is inferred that this film can be easily handled during processing when subsequent adhesive layers and printed layers are provided. The intermediate layer contains a predetermined amount of high-density polyethylene, linear low-density polyethylene, homopolypropylene, random polypropylene, and styrene-based elastomer (α), and the film obtained from only the resin composition of the intermediate layer exhibited a tensile modulus of 160 MPa, which suggests that the film has good heat resistance and flexibility, as well as excellent adhesion to the front and back layers. The film consisting of the above-mentioned surface, middle, and back layers had a tensile modulus of 210 MPa and a tensile breaking elongation of 820%, providing sufficient flexibility and breaking properties.Furthermore, the crystalline melting peaks of the obtained film were 128°C and 160°C, confirming that it also exhibited good heat resistance. Therefore, it was confirmed that this film has sufficient heat resistance, excellent handling properties and flexibility, and has a good appearance and transparency with small surface roughness and no irregularities caused by air bubbles, while also suppressing blocking between films.
[0111] [Comparative Example 1] As the thermoplastic resins for the surface, intermediate and back layers, high density polyethylene, linear low density polyethylene, homopolypropylene and olefin elastomer were used in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front side of the obtained film was 0.12 μm and the maximum height (Rz) was 1.05 μm, and the surface roughness (Ra) of the back side was 0.15 μm and the maximum height (Rz) was 1.10 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.3% and the haze was 29.2%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was found that due to the low content of high-density polyethylene, there were irregularities caused by air bubbles due to adhesion to the metal roll and air entrapment. The surface and back layers of this film contained small amounts of high-density polyethylene and homopolypropylene, and the film obtained from only the resin compositions of the surface and back layers showed a tensile modulus of 280 MPa. Therefore, there was significant blocking between the films in the roll obtained by winding, and the film could not be unwound. Therefore, it was confirmed that although this film has heat resistance and flexibility, it has poor handling properties, as it cannot be unwound during processing when the subsequent adhesive layer and printed layer are provided.
[0112] Comparative Example 2 As the thermoplastic resins for the surface, intermediate and back layers, high density polyethylene, linear low density polyethylene and an olefin-based elastomer were mixed in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.15 μm and the maximum height (Rz) was 1.20 μm, and the surface roughness (Ra) of the back layer side was 0.10 μm and the maximum height (Rz) was 0.98 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.4% and the haze was 28.7%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which was in contact with the metal roll, was observed under a microscope, only slight irregularities of an unmeasurable size were confirmed, which were thought to be due to adhesion to the metal roll and air bubbles caused by air entrapment, and it was confirmed that the film had a good appearance. The surface and back layers of this film contained only a small amount of high-density polyethylene, and the tensile modulus of the film obtained from only the resin composition of each of the surface and back layers was 270 MPa, so blocking between the films in the roll obtained by winding was significant and the film could not be unwound. Furthermore, since neither the surface layer, middle layer, nor back layer contained homopolypropylene, and no crystalline melting peak derived from homopolypropylene was observed, it was also confirmed that the film had poor heat resistance. Therefore, since this film has poor blocking properties and heat resistance, it cannot be unwound during processing when applying the subsequent adhesive layer or printing layer, and it was confirmed that the film is difficult to handle as it is likely to suffer from problems due to heat during processing.
[0113] Comparative Example 3 As the thermoplastic resins for the surface, intermediate and back layers, high density polyethylene, linear low density polyethylene and an olefin-based elastomer were mixed in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.15 μm and the maximum height (Rz) was 0.99 μm, and the surface roughness (Ra) of the back layer side was 0.15 μm and the maximum height (Rz) was 1.11 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.3% and the haze was 32.1%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The front and back layers of this film contain a large amount of high-density polyethylene, and furthermore, the film obtained from only the resin composition of each of the front and back layers showed a tensile modulus of 820 MPa. Therefore, when the film having this front and back layer was wound up and unwound from the resulting roll, no blocking was observed and the film could be easily unwound. However, since neither the surface layer, intermediate layer, nor the outer layer contained homopolypropylene, and no crystalline melting peak derived from homopolypropylene was observed, it was confirmed that the film had poor heat resistance. Therefore, although this film has excellent handleability and flexibility, has small surface roughness, and has a good appearance and transparency with no irregularities caused by air bubbles, it was confirmed that the film has poor handleability and is likely to develop defects due to heat during processing.
[0114] Comparative Example 4 As the thermoplastic resins for the surface, intermediate and back layers, high density polyethylene, linear low density polyethylene and homopolypropylene were used in the amounts shown in Table 1 to prepare resin compositions for each layer. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by the nip molding method using the matte metal cooling roll and matte silicone rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.10 μm and the maximum height (Rz) was 0.98 μm, and the surface roughness (Ra) of the back layer side was 0.10 μm and the maximum height (Rz) was 0.95 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.5% and the haze was 27.0%, and the film had a matte appearance and excellent transparency. Furthermore, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was confirmed that the film had a good appearance, with no irregularities due to air bubbles caused by adhesion to the metal roll or air entrapment being observed. The front and back layers of this film contain a specified amount of high-density polyethylene and homopolypropylene, and furthermore, the film obtained from only the resin composition of each of the front and back layers exhibited a tensile modulus of 550 MPa. Therefore, although slight blocking was observed when the film was unwound from the roll obtained by winding, it could be easily unwound. The middle layer contains high-density polyethylene and homopolypropylene, but the homopolypropylene content is higher. The film obtained from only the resin composition of the middle layer exhibited a tensile modulus of 870 MPa, while the film consisting of the surface, middle, and back layers also exhibited a high tensile modulus of 830 MPa and a tensile breaking elongation of 820%, confirming that the film has sufficient flexibility and breaking properties, but is not very flexible. Therefore, although this film has excellent appearance, transparency, blocking resistance, and heat resistance, it has been confirmed that it is poor in flexibility and is likely to be difficult to handle during processing when subsequent adhesive layers and printed layers are applied.
[0115] Comparative Example 5 The resin composition described in Example 5 was prepared, and a film was produced under the same production conditions and by the same method as in Example 5, except that a matte rubber cooling roll (surface roughness Ra: approximately 1.0 μm) was used instead of the matte rubber cooling roll (surface roughness Ra: approximately 0.3 μm). A three-layer, three-kind film with a total thickness of 80 μm was obtained. The film production conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the surface side of the obtained film was 0.14 μm and the maximum height (Rz) was 1.11 μm, and the surface roughness (Ra) of the back side was 1.01 μm and the maximum height (Rz) was 7.21 μm.It was confirmed that the surface roughness (Ra) of the surface side was 0.5 μm or less and the maximum height (Rz) was 3.0 μm or less, but the back side was a film with a surface roughness that exceeded the specified value. The total light transmittance of this film was 89.3% and the haze was 93.8%, confirming that the film had high haze, a matte appearance, and poor transparency. Therefore, although this film has excellent blocking properties and heat resistance, it is difficult to use this film in semiconductor processes that involve the use of laser light due to its poor transparency.
[0116] Comparative Example 6 The resin composition described in Comparative Example 5 was prepared, and a film was produced under the same production conditions and by the same method as in Comparative Example 5, except that a matte metal cooling roll (surface roughness Ra: approximately 0.8 μm) was used instead of the matte metal cooling roll described above (surface roughness Ra: approximately 0.3 μm), to obtain a film consisting of three types of three layers with a total thickness of 80 μm. The film production conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the surface layer of the obtained film was 0.84 μm and the maximum height (Rz) was 5.51 μm, and the surface roughness (Ra) of the back layer was 1.05 μm and the maximum height (Rz) was 7.53 μm, confirming that both the surface and back layers of the film exceeded the specified surface roughness. The total light transmittance of this film was 89.4% and the haze was 94.4%, confirming that the film had high haze, a matte appearance, and poor transparency. Therefore, although this film has excellent blocking properties and heat resistance, it is difficult to use this film in semiconductor processes that involve the use of laser light due to its poor transparency.
[0117] Comparative Example 7 A resin composition was prepared in the same manner as in Example 1, except that high-density polyethylene was not used as the thermoplastic resin for the surface layer. Using the resin compositions for the surface, middle, and back layers, a two-type, three-layer film with a total thickness of 80 μm was obtained by nip molding using the matte metal cooling roll and the matte fluororesin-coated rubber roll described above. The film-forming conditions were adjusted so that the thickness of each layer was 4 μm for the surface layer, 72 μm for the middle layer, and 4 μm for the back layer. The surface roughness (Ra) of the front layer side of the obtained film was 0.14 μm and the maximum height (Rz) was 1.06 μm, and the surface roughness (Ra) of the back layer side was 0.12 μm and the maximum height (Rz) was 0.94 μm, confirming that the film had a surface roughness (Ra) of 0.5 μm or less and a maximum height (Rz) of 3.0 μm or less on both the front and back sides. The total light transmittance was 89.9% and the haze was 26.6%, and the film had a matte appearance and excellent transparency. However, when the surface layer of the obtained film, which is the side that comes into contact with the metal roll, was observed under a microscope, it was found that the surface layer did not contain high-density polyethylene, and there were noticeable irregularities caused by air bubbles due to adhesion to the metal roll and air entrapment, confirming that the film had an inferior appearance due to the irregularities caused by the air bubbles. Therefore, although this film has sufficient heat resistance, is easy to handle and has excellent flexibility, has small surface roughness, and suppresses blocking between films, it was confirmed that the film has poor appearance, with noticeable unevenness due to air bubbles.
[0118] [Table 1]
[0119] [Example 11] An acrylic adhesive (SK Dyne 1502C manufactured by Soken Chemical & Engineering Co., Ltd.) was applied onto the separator using the comma coating method so that the adhesive layer would be 25 μm thick after drying, and the adhesive layer was then dried for 5 minutes in a hot air dryer at 80°C to form the adhesive layer. The adhesive layer side of the prepared separator was then subjected to corona treatment and bonded to the surface of the film obtained in Example 1, thereby achieving sufficient adhesion between the film of the present invention and the adhesive layer, and obtaining a laminated adhesive film. Since an adhesive film was obtained that has sufficient heat resistance, excellent handling and flexibility, and high transparency with low surface roughness, it is presumed that an adhesive film has been obtained that can be suitably used in semiconductor manufacturing processes that involve steps using laser light, such as laser dicing, where highly transparent films are required.
[0120] [Industrial Applicability] The present invention aims to provide a thermoplastic resin film that has sufficient heat resistance, low surface roughness, high transparency, and good appearance even when suitability for heating steps in semiconductor manufacturing processes and suppression of laser light scattering are required, and that can suppress blocking between films when handled, and that has excellent handleability and flexibility. Another object of the present invention is to provide a pressure-sensitive adhesive film that can be suitably used in semiconductor manufacturing processes by providing the thermoplastic resin film with a pressure-sensitive adhesive layer.
Claims
1. A thermoplastic resin film having at least three layers, namely, two outer layers and an intermediate layer, obtained by nipping an extruded molten resin with a metal roll and a rubber roll, The resin composition constituting the outer layer on the side in contact with the metal roll contains high density polyethylene and homopolypropylene, The intermediate layer contains at least one selected from the group consisting of high density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, The thermoplastic resin film is characterized by satisfying the following requirements. (1) When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll is taken as 100 mass%, the content of high-density polyethylene is 20 to 90 mass%, the content of homopolypropylene is 10 to 75 mass%, and the content of other thermoplastic resins is 0 to 30 mass%. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of both outer layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
2. 2. The thermoplastic resin film according to claim 1, wherein the thermoplastic elastomer is a styrene-based elastomer and / or an olefin-based elastomer.
3. 3. The thermoplastic resin film according to claim 1, wherein the haze of the thermoplastic resin film is 50% or less.
4. 3. The thermoplastic resin film according to claim 1, wherein the thermoplastic resin film has a tensile modulus in the range of 100 to 600 MPa.
5. 3. An adhesive film comprising the thermoplastic resin film according to claim 1 or 2 and an adhesive layer provided on at least one surface of the thermoplastic resin film.
6. The adhesive film for use in a semiconductor manufacturing process according to claim 5, which is used in a semiconductor manufacturing process.
7. A method for producing a thermoplastic resin film having at least three layers, including two outer layers and an intermediate layer, comprising the steps of: The production method includes nipping an extruded molten resin with a metal roll and a rubber roll to obtain the thermoplastic resin film, The surface roughness (Ra) of each of the metal roll and the rubber roll used to nip the extruded molten resin is 0.5 μm or less; The resin composition constituting the outer layer on the side in contact with the metal roll contains high-density polyethylene and homopolypropylene, The intermediate layer contains at least one selected from the group consisting of high density polyethylene, homopolypropylene, thermoplastic elastomer, and random polypropylene, The manufacturing method, wherein the thermoplastic resin film satisfies the following requirements: (1) When the total amount of thermoplastic resins contained in the resin composition constituting the outer layer on the side in contact with the metal roll is taken as 100 mass%, the content of high-density polyethylene is 20 to 90 mass%, the content of homopolypropylene is 10 to 75 mass%, and the content of other thermoplastic resins is 0 to 30 mass%. (2) When the total amount of thermoplastic resins contained in the resin composition constituting the intermediate layer is taken as 100% by mass, the content of high-density polyethylene is 3 to 15% by mass, the content of homopolypropylene is 10 to 50% by mass, the content of at least one selected from the group consisting of thermoplastic elastomers and random polypropylenes is 10 to 85% by mass, and the content of other thermoplastic resins is 0 to 40% by mass. (3) The surface roughness (Ra) of both outer layers is 0.5 μm or less, and the maximum height (Rz) is 3.0 μm or less.
8. 8. The method according to claim 7, wherein the surface of the rubber roll is made of silicone resin or fluororesin.
Citation Information
Patent Citations
Semiconductor wafer fixing adhesive tape
JP1997008111A
Dicing-base film
JP2018125521A
Base film for semiconductor manufacturing process and adhesive film for dicing using base film
JP2020084143A
Dicing Sheet