Solar cell, method for preparing solar cell, and photovoltaic module

The solar cell design addresses low efficiency by using a doped conductive layer concentration gradient and a blocking layer to enhance carrier transport and reduce recombination, improving overall performance.

JP2024155726AActive Publication Date: 2024-10-31JINKO SOLAR (HAINING) CO LTS +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024016212
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-02-06
Publication Date
2024-10-31
Estimated Expiration
2043-06-20

Smart Images

  • Figure 2024155726000001_ABST
    Figure 2024155726000001_ABST
Patent Text Reader

Abstract

To provide, in the field of solar cells, particularly a solar cell, a method for preparing the same, and a photovoltaic module.SOLUTION: A solar cell comprises: a substrate having a first surface; a tunneling layer formed on the first surface; a first doped conductive layer formed on the tunneling layer; a second doped conductive layer formed on the first doped conductive layer, where the second doped conductive layer comprises a plurality of first portions and a plurality of second portions, where a doping element concentration of the first doped conductive layer is lower than a doping element concentration of the first portions, and the doping element concentration of the first portions is lower than a doping element concentration of the second portions; and a plurality of first electrodes each extending along a preset direction, and each electrically contacting corresponding one of the second portions. Embodiments of the present application are advantageous in improving the photoelectric conversion performance of the solar cell.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] TECHNICAL FIELD The present application relates to the field of solar cells, and more particularly to solar cells and methods for manufacturing the same, and photovoltaic modules. [Background technology]

[0002] Solar cells have good photoelectric conversion capacity, and in order to suppress carrier recombination on the substrate surface in solar cells and improve the passivation performance of the substrate, currently a tunnel layer and a doped conductive layer are fabricated on the substrate surface, of which the tunnel layer has good chemical passivation effect and the doped conductive layer has good field passivation effect.

[0003] The doped conductive layer is doped with a certain concentration of doping elements, which can form a sufficiently high potential barrier between the doped conductive layer and the substrate. This potential barrier allows majority carriers in the substrate to easily tunnel through the tunneling layer, while minority carriers in the substrate escape through the interface, reducing the minority carrier concentration and realizing selective carrier transport. Therefore, the doping element concentration in the doped conductive layer plays an important role in the performance of the doped conductive layer, which may ultimately affect the performance of the entire solar cell.

[0004] However, the photoelectric conversion performance of current solar cells remains poor. Summary of the Invention [Problem to be solved by the invention]

[0005] In the embodiments of the present application, a solar cell, a manufacturing method thereof, and a photovoltaic module are provided, which are advantageous in improving at least the photoelectric conversion efficiency of the solar cell. [Means for solving the problem]

[0006] In an embodiment of the present application, a solar cell is provided, the solar cell including a substrate having a first surface, a tunnel layer formed on the first surface, a first doped conductive layer formed on a surface of the tunnel layer remote from the substrate, and a second doped conductive layer formed on a side of the first doped conductive layer remote from the substrate, the second doped conductive layer including a plurality of first portions and a plurality of second portions, the first portions and the second portions being alternately arranged along a predetermined direction and a direction perpendicular to a thickness direction of the second doped conductive layer, and each of the first portions and each of the second portions being predetermined. a second doped conductive layer extending along a predetermined direction, wherein a doping element concentration of the first doped conductive layer is smaller than a doping element concentration of the first portion, and the doping element concentration of the first portion is smaller than a doping element concentration of the second portion, and wherein the predetermined direction is parallel to the first surface; and a plurality of first electrodes, each of which extends along the predetermined direction, each of which corresponds to each of the second portions in a one-to-one relationship, and each of which is in electrical contact with a corresponding one of the second portions.

[0007] The ratio of the doping element concentration in the first portion to the doping element concentration in the second portion is 1:50 to 3:4.

[0008] The ratio of the doping element concentration in the first doped conductive layer to the doping element concentration in the second portion is 1:100 to 1:2.

[0009] The first doped conductive layer includes a plurality of third portions and a plurality of fourth portions, and the third portions and the fourth portions are alternately arranged along a predetermined direction and a direction perpendicular to a thickness direction of the second doped conductive layer, wherein the predetermined direction is parallel to the first surface, the third portions and the fourth portions both extend along the predetermined direction, one third portion faces one first portion, one fourth portion faces one second portion, and the doping element concentration of the third portions is lower than the doping element concentration of the fourth portions.

[0010] Furthermore, when the doping element type of the first doped conductive layer is N-type, the ratio of the doping element concentration of the third portion to the doping element concentration of the fourth portion is 1:30 to 5:6, and when the doping element type of the first doped conductive layer is P-type, the ratio of the doping element concentration of the third portion to the doping element concentration of the fourth portion is 1:100 to 2:3.

[0011] The ratio of the doping element concentration in the fourth portion to the doping element concentration in the second portion is 1:10 to 5:6.

[0012] The doping element types of the first doped conductive layer and the second doped conductive layer are both P-type, and the doping element concentration of the first portion is 5×10 18 atom / cm 3 ~5×10 19 atom / cm 3 and the doping element concentration of the second portion is 5×10 19 atom / cm 3 ~3×10 20 atom / cm 3 and the doping element concentration of the first doped conductive layer is 1×10 18 atom / cm 3 ~4.5×10 19 atom / cm 3 is.

[0013] The doping element type of the first doped conductive layer and the second doped conductive layer is N-type, and the doping element concentration of the first portion is 1×10 20 atom / cm 3 ~2×10 21 atom / cm 3 and the doping element concentration of the second portion is 2×10 20 atom / cm 3 ~5×10 21 atom / cm 3 and the doping element concentration of the first doped conductive layer is 5×10 19 atom / cm3 ~5×10 20 atom / cm 3 is.

[0014] The semiconductor device further includes a blocking layer, the blocking layer being located between the first doped conductive layer and the second doped conductive layer, the surface of the blocking layer facing the substrate being in contact with the surface of the first doped conductive layer away from the substrate, and the surface of the blocking layer facing the substrate being in contact with the surface of the second doped conductive layer away from the substrate.

[0015] Additionally, the surface of the blocking layer away from the substrate is in contact with each of the second portions, and the orthogonal projection of the blocking layer on the first surface overlaps with the orthogonal projection of the second portions on the first surface.

[0016] Furthermore, the surface of the blocking layer away from the substrate is in contact with each of the first portions and each of the second portions, and the orthogonal projection of the blocking layer on the first surface overlaps with the orthogonal projection of each of the first portions on the first surface and the orthogonal projection of each of the second portions on the first surface.

[0017] Additionally, the material of the blocking layer includes at least one of silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, and magnesium fluoride.

[0018] Furthermore, the material of the first doped conductive layer includes at least one of amorphous silicon, polycrystalline silicon, or silicon carbide, and the material of the second doped conductive layer includes at least one of amorphous silicon, polycrystalline silicon, or silicon carbide.

[0019] Furthermore, the first doped conductive layer is made of first polycrystalline silicon, the first portion is made of second polycrystalline silicon, and the second portion is made of third polycrystalline silicon, and the average crystal grain size of the first polycrystalline silicon is larger than the average crystal grain size of the second polycrystalline silicon and is also larger than the average crystal grain size of the third polycrystalline silicon.

[0020] Furthermore, the third portion is made of fourth polycrystalline silicon, the fourth portion is made of fifth polycrystalline silicon, the first portion is made of second polycrystalline silicon, and the second portion is made of third polycrystalline silicon, wherein the average crystal grain size of the fourth polycrystalline silicon is larger than the average crystal grain size of the fifth polycrystalline silicon, the average crystal grain size of the fifth polycrystalline silicon is larger than the average crystal grain size of the third polycrystalline silicon, and the average crystal grain size of the second polycrystalline silicon is larger than the average crystal grain size of the third polycrystalline silicon.

[0021] In addition, the doping element type of the substrate is an N-type doping element, and the second portion includes a main body portion doped with the N-type doping element and an inversion doping portion located within the main body portion and doped with a P-type doping element, and the volume ratio of the inversion doping portion within the main body portion is less than 1 / 2.

[0022] The ratio of the thickness of the first doped conductive layer to the thickness of the second doped conductive layer is 2:1 to 1:12.

[0023] In response to the above, an embodiment of the present application further provides a photovoltaic module, which includes at least one cell string formed by connecting a plurality of solar cells described in any one of the above items, at least one sealing layer for covering the at least one cell string, and at least one cover plate for covering the at least one sealing layer.

[0024] In response to the above, an embodiment of the present application further provides a method for manufacturing a solar cell, the method including: providing a substrate having a first surface; forming a tunnel layer on the first surface; forming a first doped conductive layer on the tunnel layer; and forming a second doped conductive layer on the first doped conductive layer, the second doped conductive layer including a plurality of first portions and a plurality of second portions, the first portions and the second portions being alternately arranged along a predetermined direction and a direction perpendicular to a thickness direction of the second doped conductive layer, and the first portions and the second portions being alternately arranged along a predetermined direction and a direction perpendicular to a thickness direction of the second doped conductive layer, extending along a predetermined direction, wherein a doping element concentration of the first doped conductive layer is smaller than a doping element concentration of the first portion, and the doping element concentration of the first portion is smaller than a doping element concentration of the second portion, wherein the predetermined direction is parallel to the first surface; and forming a plurality of first electrodes, each of which extends along the predetermined direction, each of which corresponds to each of the second portions one-to-one, and one of which is in electrical contact with a corresponding one of the second portions.

[0025] Also, before the step of forming the second doped conductive layer, the method further includes forming a blocking layer located on a surface of the first doped conductive layer away from the substrate, and the material of the blocking layer includes at least one of silicon oxide, silicon nitride, silicon oxynitride, or silicon carbide.

[0026] Also, the method of forming the first doped conductive layer, the second doped conductive layer, and the blocking layer includes: forming a first intrinsic silicon layer on a surface of the tunnel layer; forming the blocking layer on the surface of the first intrinsic silicon layer; forming a second intrinsic silicon layer on the surface of the blocking layer; depositing a doping source containing a first doping element on a surface of the second intrinsic silicon layer away from the substrate; and simultaneously depositing the doping source, by flowing oxygen gas, converting a partial thickness of the second intrinsic silicon layer into a glass layer, the glass layer being silicon oxide containing the first doping element; diffusing an element into the first intrinsic silicon layer to form the first doped conductive layer, and diffusing the first doping element into the second intrinsic silicon layer excluding the glass layer to form an initial second doped conductive layer; performing a second doping process on a portion of the glass layer, in which the first doping element in the glass layer that has undergone the second doping process diffuses into the initial second doped conductive layer along a direction perpendicular to the first surface, converting this portion of the initial second doped conductive layer into a second portion of the second doped conductive layer, and the remaining portion of the initial second doped conductive layer forming a first portion.

[0027] The second doping process includes a laser process, and the laser wavelength used in the laser process is 300 nm to 532 nm, the laser frequency is 120 kHz to 1500 kHz, the scan rate is 1000 mm / s to 40000 mm / s, and the laser energy is 0.1 J / cm 2 ~1.5J / cm 2 is. [Effects of the Invention]

[0028] The technical solutions provided in the embodiments of the present application have at least the following advantages:

[0029] In the solar cell technical solution provided in the embodiments of the present application, the first doped conductive layer is closer to the substrate than the second doped conductive layer, and the doping element concentration of the first doped conductive layer is lower than that of the second doped conductive layer, thereby reducing the probability of impurity elements in the first doped conductive layer penetrating into the tunneling layer, ensuring good tunneling performance of the tunneling layer for carriers in the substrate, increasing the number of carriers tunneled into the first doped conductive layer and the second doped conductive layer, improving the carrier collection ability of the first electrode, increasing the open circuit voltage and short circuit current of the solar cell, and improving the photoelectric conversion performance of the solar cell.

[0030] The second doped conductive layer includes a first portion and a second portion, and the doping element concentrations of the first portion and the second portion are both greater than the doping element concentration of the first doped conductive layer. That is, in a direction perpendicular to the first surface, the first portion and the second portion form a concentration gradient with the first doped conductive layer, which is useful for driving the longitudinal transport of carriers, reinforces the transport of carriers in the substrate to the second doped conductive layer, and improves the carrier collection ability of the first electrode, thereby improving the photoelectric conversion performance of the solar cell.

[0031] The doping element concentration in the first portion is smaller than the doping element concentration in the second portion, i.e., a concentration gradient is also formed between the first portion and the second portion in the direction perpendicular to the first surface, which helps to reinforce the lateral transport of carriers in the second doped conductive layer, further improving the carrier collection ability of the first electrode, and ultimately improving the photoelectric conversion performance of the solar cell.

[0032] Because the doping element concentration in the second portion is relatively high, good ohmic contact is formed between the second portion and the first electrode, reducing contact recombination loss between the first electrode and the second portion. Because the doping element concentration in the first portion is relatively low, parasitic absorption of incident light in the first portion that is not in contact with the first electrode is reduced, increasing the utilization rate of the substrate for incident light and improving the photoelectric conversion performance of the solar cell. [Brief explanation of the drawings]

[0033] One or more embodiments are illustratively described in corresponding figures in the accompanying drawings, and these illustrative descriptions do not limit the embodiments, and unless otherwise specified, the figures in the accompanying drawings do not form proportional limitations. In order to more clearly describe the embodiments of the present disclosure or technical solutions in the prior art, the following will briefly describe the drawings that need to be used in the embodiments. Obviously, the drawings in the following description are only some embodiments of the present disclosure, and those skilled in the art can obtain other drawings based on these drawings without paying creative labor. [Figure 1] FIG. 1 is a diagram showing the cross-sectional structure of a solar cell. [Figure 2] FIG. 2 is a diagram showing a top view structure of a solar cell provided according to an embodiment of the present application. [Figure 3] FIG. 3 is a diagram showing a cross-sectional structure of a first solar cell provided by an embodiment of the present application. [Figure 4] FIG. 4 is a diagram showing a cross-sectional structure of a second solar cell provided by an embodiment of the present application. [Figure 5] FIG. 5 is a diagram showing a top view configuration of another solar cell provided by an embodiment of the present application. [Figure 6] FIG. 6 is a diagram showing a cross-sectional structure of a third solar cell provided by an embodiment of the present application. [Figure 7] FIG. 7 is a diagram showing a cross-sectional structure of a fourth solar cell provided by an embodiment of the present application. [Figure 8] FIG. 8 is a diagram showing a cross-sectional structure of a fifth solar cell provided by an embodiment of the present application. [Figure 9] FIG. 9 is a diagram showing a cross-sectional structure of a sixth solar cell provided by an embodiment of the present application. [Figure 10] FIG. 10 is a diagram showing a cross-sectional structure of a seventh solar cell provided by an embodiment of the present application. [Figure 11]FIG. 11 is a diagram showing a cross-sectional structure of a photovoltaic module provided by another embodiment of the present application. [Figure 12] FIG. 12 is a diagram showing a cross-sectional structure corresponding to a step of providing a substrate in a method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 13] FIG. 13 is a diagram showing a cross-sectional structure corresponding to a step of forming an emitter in a method for manufacturing a solar cell according to an embodiment of the present application. [Figure 14] FIG. 14 is a diagram showing a cross-sectional structure corresponding to a step of forming a tunnel layer in a method for manufacturing a solar cell according to an embodiment of the present application. [Figure 15] FIG. 15 is a diagram showing a cross-sectional structure corresponding to a step of forming an intrinsic silicon layer in a method for manufacturing a solar cell according to an embodiment of the present application. [Figure 16] FIG. 16 is a diagram showing a cross-sectional structure corresponding to a step of forming a glass layer in a method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 17] FIG. 17 is a diagram showing a cross-sectional structure corresponding to a step of forming an initial silicon doped layer in a method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 18] FIG. 18 is a diagram illustrating a cross-sectional structure corresponding to a step of forming a first doped conductive layer and a silicon-doped layer in another method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 19] FIG. 19 is a diagram showing cross-sectional structures corresponding to the step of forming the first portion and the second portion in the method for manufacturing a solar cell provided by one embodiment of the present application. [Figure 20] FIG. 20 is a diagram illustrating a cross-sectional structure corresponding to a step of forming a first intrinsic silicon layer in another method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 21] FIG. 21 is a diagram illustrating a cross-sectional structure corresponding to a step of forming a blocking layer and a second intrinsic silicon layer in another method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 22] FIG. 22 is a diagram showing a cross-sectional structure corresponding to a step of forming a glass layer in another method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 23] FIG. 23 is a diagram illustrating a cross-sectional structure corresponding to a step of forming a first doped conductive layer and an initial second doped conductive layer in another method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 24] FIG. 24 is a diagram showing a cross-sectional structure corresponding to a step of forming a mask layer in another method for manufacturing a solar cell provided by an embodiment of the present application. [Figure 25] FIG. 25 is a diagram showing a cross-sectional structure corresponding to a step of forming the first portion 11 and the second portion 12 in another method for manufacturing a solar cell provided according to an embodiment of the present application. [Figure 26] FIG. 26 is a diagram illustrating a cross-sectional structure corresponding to a step of forming a first passivation layer and a second passivation layer in another method for manufacturing a solar cell provided by an embodiment of the present application. DETAILED DESCRIPTION OF THE INVENTION

[0034] As can be seen from the background art, conventional solar cells have a problem of low photoelectric conversion efficiency.

[0035] Analysis reveals that one of the reasons for the low photoelectric conversion efficiency of current solar cells is that, as shown in Figure 1, in current TOPCON (Tunnel Oxide Passivated Contact) cells, the first surface 1 of the substrate 100 has a passivation contact structure. This passivation contact structure includes a tunnel layer 2 and a doped conductive layer 3. The doped conductive layer 3 has a certain concentration of doping elements, which creates a band bending on the surface of the substrate 100 and realizes selective carrier transport. A metal electrode 4 is in electrical contact with the doped conductive layer 3. Carriers in the substrate 100 are transported into the doped conductive layer 3 and collected by the metal electrode 4. The doping element concentration in the doped conductive layer 3 is an important factor in controlling the performance of the doped conductive layer 3. If the doping concentration is too low, a sufficiently high potential barrier cannot be formed between the doped conductive layer 3 and the substrate 100, preventing carriers in the substrate 100 from tunneling through the second surface 2, resulting in a rapid decrease in carrier collection efficiency. On the other hand, if the concentration of the doping element in the doped conductive layer 3 is too high, the doped conductive layer 3 will have a large parasitic absorption of incident light, which will reduce the utilization of the substrate 100 for incident light and significantly reduce the passivation quality of the doped conductive layer 3. Therefore, controlling the concentration of the doping element in the doped conductive layer 3 is key to improving the photoelectric conversion performance of the solar cell.

[0036] In an embodiment of the present application, a solar cell is provided, in which the doping element concentration of the first doped conductive layer is lower than the doping element concentration of the second doped conductive layer, thereby reducing the probability of impurities in the first doped conductive layer penetrating into the tunneling layer and ensuring good tunneling performance of the tunneling layer. Furthermore, in a direction perpendicular to the first surface, the first and second portions of the second doped conductive layer form a concentration gradient with the first doped conductive layer, which is beneficial to vertical carrier transport, enhances carrier transport in the substrate to the second doped conductive layer, and improves the carrier collection ability of the first electrode. Because the doping element concentration of the first portion is lower than the doping element concentration of the second portion, a concentration gradient is also formed between the first and second portions, which is beneficial to lateral carrier transport in the second doped conductive layer, further improving the carrier collection ability of the first electrode. Furthermore, the relatively high doping element concentration of the second portion can improve contact recombination loss between the first electrode and the second portion, and the relatively low doping element concentration of the first portion can reduce parasitic absorption of incident light in the first portion that is not in contact with the first electrode, thereby improving the utilization rate of incident light of the substrate. By adjusting and controlling the doping element concentration of the first doped conductive layer and the doping element concentrations of the first and second portions of the second doped conductive layer, interactions can be achieved between the first doped conductive layer and the first and second portions, which have different doping element concentrations, to improve carrier transport ability and overall improve the photoelectric conversion performance of the solar cell.

[0037] Hereinafter, each embodiment of the present application will be described in detail with reference to the accompanying drawings. However, as will be understood by those skilled in the art, although many technical details are proposed in each embodiment of the present application to facilitate a better understanding of the present application, the technical solution claimed for protection by the present application can be realized without these technical details and various changes and modifications based on the following embodiments.

[0038] FIG. 2 is a diagram showing a top view structure of a solar cell provided by an embodiment of the present application, FIG. 3 is a diagram showing a cross-sectional structure of a first solar cell provided by an embodiment of the present application, and FIG. 3 is a diagram showing a cross-sectional structure along the AA' direction of FIG.

[0039] 2 and 3, the solar cell includes a substrate 100 having a first surface 1 and a tunnel layer 110 formed on the first surface 1. The solar cell further includes a first doped conductive layer 120 formed on the tunnel layer 110. The solar cell further includes a second doped conductive layer 130 formed on the first doped conductive layer 120. The second doped conductive layer 130 includes a plurality of first portions and a plurality of second portions, the first portions 11 and the second portions 12 being alternately arranged along a predetermined direction X and a direction perpendicular to a thickness direction of the second doped conductive layer 130, and the first portions 11 and the second portions 12 both extend along the predetermined direction X, where the doping element concentration of the first doped conductive layer 120 is lower than the doping element concentration of the first portions 11, and the doping element concentration of the first portions 11 is lower than the doping element concentration of the second portions 12, and the predetermined direction X is parallel to the first surface 1. The solar cell further includes a plurality of first electrodes, each of which, a first electrode 140, extends along a predetermined direction X, each of which has a one-to-one correspondence with each of the second portions 12, and each of which has a first electrode 140 in electrical contact with a corresponding second portion 12.

[0040] Substrate 100 is used to receive incident light and generate photo-generated carriers. In some embodiments, substrate 100 may be a silicon substrate, and the material of the silicon substrate may be at least one of monocrystalline silicon, polycrystalline silicon, amorphous silicon, or microcrystalline silicon. In some embodiments, the material of substrate 100 may be a semiconductor material. In some embodiments, the material of substrate 100 may be silicon carbide, an organic material, or a multi-component compound. Examples of multi-component compounds include, but are not limited to, perovskite, gallium arsenide, cadmium telluride, copper indium selenide, and the like.

[0041] In some embodiments, the solar cell may be a TOPCON cell, and the substrate 100 has a second surface 2 opposite the first surface 1. In some embodiments, the solar cell is a bifacial cell, and both the first surface 1 and the second surface 2 can be used to receive incident light. In some embodiments, the solar cell is a monofacial cell, and either the first surface 1 or the second surface 2 can be used to receive incident light.

[0042] In some embodiments, when the solar cell is a monofacial solar cell and the second surface 2 is a light-receiving surface, the second surface 2 of the substrate 100 can be textured, e.g., a pyramidal texture, so as to reduce the reflectivity of the second surface 2 of the substrate 100 to incident light and increase the absorption efficiency of the light. In some embodiments, the first surface 1 of the substrate 100 can be polished, i.e., the first surface 1 of the substrate 100 is flat compared to the second surface 2 of the substrate 100. In some embodiments, when the first surface 1 is a light-receiving surface, the first surface 1 can be textured, e.g., a pyramidal texture, and the second surface 2 can be polished. In some embodiments, the solar cell is a monofacial solar cell and both the first surface 1 and the second surface 2 can be textured, e.g., a pyramidal texture.

[0043] In some embodiments, the solar cell is a bifacial cell, and both the second surface 2 of the substrate 100 and the first surface 1 of the substrate 100 can be pyramidal textured.

[0044] In some embodiments, the substrate 100 includes doping elements, and the type of the doping elements is N-type or P-type, where the N-type elements may be Group V elements such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As), and the P-type elements may be Group III elements such as boron (B), aluminum (Al), gallium (Ga), or indium (In). For example, if the substrate 100 is a P-type substrate, the type of the doping elements therein is P-type. Alternatively, if the substrate 100 is an N-type substrate, the type of the doping elements therein is N-type.

[0045] One first electrode 140 is in electrical contact with one second portion 12, and carriers in the substrate 100 tunnel into the first doped conductive layer 120 through the tunneling layer 110. Carriers in the first doped conductive layer 120 are transported to the second portion 12 and collected by the first electrode 140 in electrical contact with the second portion 12, and carriers in the first doped conductive layer 120 can also be transported to the first portion 11, and carriers in the first portion 11 are transported to the second portion 12 and further collected by the first electrode 140 in electrical contact with the second portion 12.

[0046] In some embodiments, the orthogonal projection of the first electrode 140 on the first surface 1 can be located within the orthogonal projection of the second portion 12 on the first surface 1, i.e., the width dimension of the first electrode 140 can be smaller than the width dimension of the second portion 12. In some embodiments, the orthogonal projection of the first electrode 140 on the first surface 1 can overlap with the orthogonal projection of the second portion 12 on the first surface 1. The first portion 11 is a portion of the second doped conductive layer 130 other than the second portion 12.

[0047] The first doped conductive layer 120 and the second doped conductive layer 130 can form a band bending at the first surface 1 and form a built-in electric field, so that the potential barrier for majority carriers is lower than the potential barrier for minority carriers, allowing holes to escape from the interface and reducing the hole concentration. However, the majority carriers in the substrate 100 can easily tunnel into the first doped conductive layer 120 and the second doped conductive layer 130 through the tunneling layer 110, thereby realizing selective carrier transport.

[0048] The first doped conductive layer 120 is closer to the tunnel layer 110 than the second doped conductive layer 130, and the doping element concentration of the first doped conductive layer 120 is lower than the doping element concentration of the second doped conductive layer 130, thereby reducing the probability that impurity elements in the first doped conductive layer 120 will enter the tunnel layer 110, ensuring good tunneling performance of the tunnel layer 110, and ultimately ensuring that a large number of carriers tunnel from the substrate 100 through the tunnel layer 110, thereby ensuring good chemical passivation effect on the first surface 1 of the tunnel layer 110.

[0049] The impurity element here refers to the doping element in the first doped conductive layer 120. If the doping element concentration is too high, the impurity element in the first doped conductive layer 120 will diffuse into the tunnel layer 110 and form an impurity element in the tunnel layer 110, which will affect the tunneling performance of the tunnel layer 110, causing a sharp decrease in the passivation ability of the tunnel layer 110 to the first surface 1 and a sharp increase in Auger recombination at the first surface 1. In some embodiments, the material of the tunnel layer 110 includes at least one of silicon oxide, aluminum oxide, silicon nitride, silicon oxynitride, amorphous silicon, or polycrystalline silicon.

[0050] The second doped conductive layer 130 includes a first portion 11 and a second portion 12. The doping element concentrations of the first portion 11 and the second portion 12 are both greater than that of the first doped conductive layer 120. As a result, the first portion 11 and the second portion 12 form a concentration gradient with the first doped conductive layer 120 in a direction perpendicular to the first surface 1. That is, the second doped conductive layer 130 also forms a surface electric field on the surface of the first doped conductive layer 120, realizing selective transport of carriers in the first doped conductive layer 120 to the second doped conductive layer 130. This reinforces the vertical transport of carriers, reinforces the transport of carriers in the substrate 100 to the second doped conductive layer 130, increases the number of carriers transported to the second doped conductive layer 130, and further increases the number of carriers collected in the first electrode 140, thereby increasing the short-circuit current and open-circuit voltage of the solar cell and improving the photoelectric conversion performance of the solar cell.

[0051] The doping element concentration in the first portion 11 is lower than the doping element concentration in the second portion 12, so that a concentration gradient is also formed between the first portion 11 and the second portion 12 in a direction perpendicular to the predetermined direction X and the thickness direction of the second doped conductive layer 130. That is, a built-in electric field is also formed in the second doped conductive layer 130, reinforcing the transport of carriers from the first portion 11 to the second portion 12. Carriers in the portion of the second doped conductive layer 130 that is not in contact with the first electrode 140 are also transported to the second portion 12 and collected by the first electrode 140, further increasing the number of carriers collected by the first electrode 140 and further increasing the short-circuit current and open-circuit voltage of the solar cell.

[0052] The doping element concentration of the second portion 12 is higher than that of the first portion 11, and the sheet resistance of the second portion 12 is lower than that of the first portion 11. This reduces the contact resistance between the first electrode 140 and the second portion 12, realizes good ohmic contact between the first electrode 140 and the second portion 12, reduces contact recombination loss between the first electrode 140 and the second portion 12, reduces carrier transport loss to the first electrode 140, and helps improve the carrier collection ability of the first electrode 140. The doping element concentration of the first portion 11 is relatively low, which reduces parasitic absorption of incident light in the first portion 11 that is not in contact with the first electrode 140, increases the utilization rate of the substrate 100 for incident light, and improves the photoelectric conversion performance of the solar cell.

[0053] In some embodiments, the doping element type of the first doped conductive layer 120 is the same as the doping element type of the substrate 100, and the doping element type of the second doped conductive layer 130 is the same as the doping element type of the substrate 100. This allows the first doped conductive layer 120 and the second doped conductive layer 130 to form a band bending at the first surface 1 of the substrate 100, thereby realizing selective carrier transport. In some embodiments, if the doping element of the substrate 100 is P-type, the doping element type of the first doped conductive layer 120 and the doping element type of the second doped conductive layer 130 are both P-type. In some embodiments, if the doping element of the substrate 100 is N-type, the doping element type of the first doped conductive layer 120 and the doping element type of the second doped conductive layer 130 are both N-type. The doping element of the first doped conductive layer 120 and the doping element of the second doped conductive layer 130 may be the same or different.

[0054] In the present embodiment, the specific doping elements of the first doped conductive layer 120 and the second doped conductive layer 130 are not limited, but the doping element type of the first doped conductive layer 120 and the second doped conductive layer 130 may be the same as the doping element type of the substrate 100. For example, the P-type doping element may be any of Group III elements such as boron (B), aluminum (Al), gallium (Ga), or indium (In). The N-type doping element may be any of Group V elements such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As).

[0055] In some embodiments, the ratio of the doping element concentration in the first portion 11 to the doping element concentration in the second portion 12 is 1:50 to 3:4, and may be, for example, 1:50 to 1:45, 1:45 to 1:40, 1:40 to 1:30, 1:30 to 1:25, 1:25 to 1:20, 1:20 to 1:15, 1:15 to 1:10, 1:10 to 1:5, 1:5 to 1:3, 1:3 to 1:2, 1:2 to 2:3, or 2:3 to 3:4. Within the above range, the doping element concentration of the second portion 12 is greater than that of the first portion 11, which results in a smaller sheet resistance of the second portion 12 than that of the first portion 11, a smaller contact resistance between the second portion 12 and the first electrode 140, an improved ohmic contact between the second portion 12 and the first electrode 140, a reduced metal contact recombination loss between the first electrode 140 and the second portion 12, and a reduced transport loss of carriers to the first electrode 140.

[0056] Within the above range, the doping element concentration of the second portion 12 is not too large compared to the doping element concentration of the first portion 11, thereby preventing the passivation performance of the second portion 12 from being impaired due to the doping element concentration of the second portion 12 being too large, improving the ohmic contact between the second portion 12 and the first electrode 140, while maintaining good passivation performance of the second portion 12, including passivation for the first surface 1 and passivation between the contact interface of the first electrode 140 and the second electrode.

[0057] Within the above range, the doping element concentration of the first portion 11 is lower than that of the second portion 12, which weakens the parasitic absorption ability of the first portion 11 for incident light and ensures a high absorption utilization ability for incident light of the substrate 100. Furthermore, the doping element concentration of the first portion 11 is relatively low, and compared with the second portion 12, the first portion 11 has better passivation performance for the first surface 1, which can reduce Auger recombination at the first surface 1 and suppress carrier recombination at the first surface 1.

[0058] The second doped conductive layer 130 has a plurality of first portions and a plurality of second portions, and the doping element concentration of each first portion 11 among the plurality of first portions is greater than the doping element concentration of each second portion 12 among the plurality of second portions, and the ratio of the doping element concentrations of each first portion 11 to each second portion 12 is 1:50 to 3:4.

[0059] In some embodiments, the doping element types of the first doped conductive layer 120 and the second doped conductive layer 130 are both P-type, and the doping element concentration of the first portion 11 is 5×10 18 atom / cm 3 ~5×10 19 atom / cm 3 For example, 5 × 10 18 atom / cm 3 ~9×10 18 atom / cm 3 , 9×10 18 atom / cm 3 ~1×10 19 atom / cm 3 , 1×10 19 atom / cm 3 ~2×10 19 atom / cm 3 or 2×10 19 atom / cm 3 ~5×10 19 atom / cm 3 The doping element concentration of the second portion 12 may be 5×10 19 atom / cm 3 ~3×10 20 atom / cm3 For example, 5 × 10 19 atom / cm 3 ~9×10 19 atom / cm 3 , 9×10 19 atom / cm 3 ~1×10 20 atom / cm 3 , 1×10 20 atom / cm 3 ~2×10 20 atom / cm 3 or 2×10 20 atom / cm 3 ~3×10 20 atom / cm 3 When the doping element type is P-type, within the above range, both the first portion 11 and the second portion 12 have good passivation performance, and the sheet resistance of the second portion 12 is reduced, which helps to improve the ohmic contact between the second portion 12 and the first electrode. In some embodiments, the P-type doping element may be boron, aluminum, nitrogen, gallium, or indium.

[0060] In some embodiments, the doping element types of the first doped conductive layer 120 and the second doped conductive layer 130 are both N-type, and the doping element concentration of the first portion 11 is 1×10 20 atom / cm 3 ~2×10 21 atom / cm 3 For example, 1×10 20 atom / cm 3 ~2×10 20 atom / cm 3 , 2 × 10 20 atom / cm 3 ~5×10 20 atom / cm 3 , 5×10 20 atom / cm 3 ~9×10 20 atom / cm 3 , 9×10 20 atom / cm 3 ~1×10 21 atom / cm 3or 1×10 21 atom / cm 3 ~2×10 21 atom / cm 3 The doping element concentration of the second portion 12 may be 2×10 atoms / cm to 5×10 atoms / cm, for example, 2×10 20 atom / cm 3 ~3×10 20 atom / cm 3 , 3×10 20 atom / cm 3 ~5×10 20 atom / cm 3 , 5×10 20 atom / cm 3 ~9×10 20 atom / cm 3 , 9×10 20 atom / cm 3 ~1×10 21 atom / cm 3 , 1×10 21 atom / cm 3 ~3×10 21 atom / cm 3 or 3×10 20 atom / cm 3 ~5×10 21 atom / cm 3 In some embodiments, the N-type doping element may be phosphorus, bismuth, antimony, or arsenic. When the doping element type is N-type within the above range, both the first portion 11 and the second portion 12 can have good passivation performance, and the sheet resistance of the second portion 12 can be low, improving the ohmic contact with the first electrode 140.

[0061] By setting the doping element concentrations of the first portion 11 and the second portion 12 with different types of doping elements, the doping element concentration of the first portion 11 is small within the above range, which weakens the parasitic absorption of incident light in the first portion 11 and increases the absorption utilization rate of the incident light in the substrate 100. Furthermore, within the above range, the first portion 11 has good passivation performance, which prevents excessive Auger recombination at the first surface 1 and suppresses carrier recombination at the first surface 1.

[0062] Within the above range, the doping element concentration of the second portion 12 is high and the sheet resistance of the second portion 12 is low, thereby forming a good ohmic contact between the second portion 12 and the first electrode 140, improving the metal contact recombination loss between the first electrode 140 and the second portion 12, and reducing the transport loss during carrier transport to the first electrode 140. Furthermore, within the above range, the doping element concentration of the second portion 12 is not too high, which prevents excessive Auger recombination at the first surface 1 and serious carrier recombination at the first surface 1 due to an excessively high doping element concentration in the second portion 12.

[0063] Within the above range, the concentration difference between the first portion 11 and the second portion 12 forms a concentration gradient within the second doped conductive layer 130. Due to the presence of this concentration gradient, a built-in electric field is also formed within the second doped conductive layer 130 from the second portion 12 toward the first portion 11, reinforcing the lateral transport of carriers in the first portion 11 into the second portion 12, increasing the carrier collection number of the first electrode 140, and thus increasing the open circuit voltage and short circuit current of the solar cell, thereby improving the photoelectric conversion performance of the solar cell.

[0064] In the present embodiment, the doping element concentrations of the first portion 11 and the second portion 12 refer to the surface doping concentration of the first portion 11 at a surface away from the substrate 100 and the surface doping concentration of the second portion 12 at a surface away from the substrate 100. When the doping element types of the first doped conductive layer 120 and the second doped conductive layer 130 are both P-type, the doping element concentration of each first portion 11 among the plurality of first portions is 5×10 18 atom / cm 3 ~5×10 19 atom / cm 3 and the doping element concentration of each of the second portions 12 among the plurality of second portions is 5×10 19 atom / cm 3 ~3×10 20 atom / cm 3 When the doping element types of the first doped conductive layer and the second doped conductive layer are both N-type, the doping element concentration of each of the first portions 11 among the plurality of first portions is 1×10 20 atom / cm 3 ~2×10 21 atom / cm 3 and the doping element concentration of each of the second portions 12 among the plurality of second portions is 2×10 20 atom / cm 3 ~5×10 21 atom / cm 3 is.

[0065] In some embodiments, the ratio of the doping element concentration of the first doped conductive layer 120 to the doping element concentration of the second portion 12 is 1:100 to 1:2, such as 1:100 to 1:85, 1:85 to 1:70, 1:70 to 1:60, 1:60 to 1:50, 1:50 to 1:40, 1:40 to 1:25, 1:25 to 1:15, 1:15 to 1:10, 1:10 to 1:5, or 1:5 to 1:2. Within the above range, the doping element concentration of the first doped conductive layer 120 is lower than the doping element concentration of the second portion 12, thereby preventing the doping element in the first doped conductive layer 120 from diffusing into the tunnel layer 110 and thereby preventing problems that could impair the tunneling and passivation performance of the tunnel layer 110. The tunnel layer 110 has good chemical passivation effect on the first surface 1.

[0066] In addition, by arranging the first doped conductive layer 120 close to the tunnel layer 110 and reducing the doping element concentration of the first doped conductive layer 120, the problem of excessive Auger recombination occurring at the first surface 1 due to an excessively high doping element concentration of the first doped conductive layer 120 can be avoided, and the recombination of carriers at the first surface 1 can be effectively suppressed.

[0067] It should be noted that the doping element concentration of the first doped conductive layer 120 in the examples of the present application refers to the surface doping concentration of the surface of the first doped conductive layer 120 that is farther away from the substrate 100 .

[0068] The ratio of the doping element concentration of the first doped conductive layer 120 to the doping element concentration of each second portion 12 is 1:100 to 1:2.

[0069] In some embodiments, the doping element types of the first doped conductive layer 120 and the second doped conductive layer 130 are both P-type, and the doping element concentration of the first doped conductive layer 120 is 1×10 18 atom / cm 3 ~4.5×10 19 atom / cm 3For example, 1×10 18 atom / cm 3 ~2×10 18 atom / cm 3 , 2 × 10 18 atom / cm 3 ~5×10 18 atom / cm 3 , 5×10 18 atom / cm 3 ~9×10 18 atom / cm 3 , 9×10 18 atom / cm 3 ~1×10 19 atom / cm 3 , 1×10 19 atom / cm 3 ~3×10 19 atom / cm 3 or 3×10 19 atom / cm 3 ~4.5×10 19 atom / cm 3 The doping element concentration of the second portion 12 may be 5×10 19 atom / cm 3 ~3×10 20 atom / cm 3 For example, 5 × 10 19 atom / cm 3 ~9×10 19 atom / cm 3 , 9×10 19 atom / cm 3 ~1×10 20 atom / cm 3 , 1×10 20 atom / cm 3 ~2×10 20 atom / cm 3 or 2×10 20 atom / cm 3 ~3×10 20 atom / cm 3 The doping element concentration of the first portion 11 may be 5×10 18 atom / cm 3 ~5×10 19 atom / cm 3 For example, 5 × 1018 atom / cm 3 ~9×10 18 atom / cm 3 , 9×10 18 atom / cm 3 ~1×10 19 atom / cm 3 , 1×10 19 atom / cm 3 ~2×10 19 atom / cm 3 or 2×10 19 atom / cm 3 ~5×10 19 atom / cm 3 When the doping element type is P-type, within the above range, the first doping conductive layer 120, the first portion 11, and the second portion 12 have good performance, so that the first doping conductive layer 120, the first portion 11, and the second portion 12 can form a band bending at the first surface 1 and realize carrier transport, and the first doping conductive layer 120, the first portion 11, and the second portion 12 all have good passivation performance. In some embodiments, the P-type doping element may be boron, aluminum, nitrogen, gallium, or indium.

[0070] In some embodiments, the doping element types of the first doped conductive layer 120 and the second doped conductive layer 130 are both N-type, and the doping element concentration of the first doped conductive layer 120 is 5×10 19 atom / cm 3 ~5×10 20 atom / cm 3 For example, 5 × 10 19 atom / cm 3 ~9×10 19 atom / cm 3 , 9×10 19 atom / cm 3 ~1×10 20 atom / cm 3 , 1×10 20 atom / cm 3 ~2×10 20 atom / cm 3 or 2×10 20atom / cm 3 ~5×10 20 atom / cm 3 The doping element concentration of the first portion 11 may be 1×10 20 atom / cm 3 ~2×10 21 atom / cm 3 For example, 1×10 20 atom / cm 3 ~2×10 20 atom / cm 3 , 2 × 10 20 atom / cm 3 ~5×10 20 atom / cm 3 , 5×10 20 atom / cm 3 ~9×10 20 atom / cm 3 , 9×10 20 atom / cm 3 ~1×10 21 atom / cm 3 or 1×10 21 atom / cm 3 ~2×10 21 atom / cm 3 The doping element concentration of the second portion 12 may be 2×10 20 atom / cm 3 ~5×10 21 atom / cm 3 For example, 2 × 10 20 atom / cm 3 ~3×10 20 atom / cm 3 , 3×10 20 atom / cm 3 ~5×10 20 atom / cm 3 , 5×10 20 atom / cm 3 ~9×10 20 atom / cm 3 , 9×10 20 atom / cm 3 ~1×10 21 atom / cm 3 , 1×10 21 atom / cm 3 ~3×1021 atom / cm 3 or 3×10 20 atom / cm 3 ~5×10 21 atom / cm 3 When the doping element type is N-type, within the above range, the first doping conductive layer 120, the first portion 11, and the second portion 12 all have good performance, so that the first doping conductive layer 120, the first portion 11, and the second portion 12 can form a band bending at the first surface 1 and realize carrier transport, and the first doping conductive layer 120, the first portion 11, and the second portion 12 all have good passivation performance. In some embodiments, the N-type doping element may be phosphorus, bismuth, antimony, or arsenic.

[0071] The doping element concentration ranges of the first doped conductive layer 120, the first portion 11, and the second portion 12 are set by using different types of doping elements, so that within the above range, the doping element concentration of the first doped conductive layer 120 is lower than the doping element concentration of the second doped conductive layer 130. This reduces the probability that the doping element in the first doped conductive layer 120 will be transported to the tunneling layer 110, thereby maintaining good tunneling performance of the tunneling layer 110. Furthermore, within the above range, the doping element concentration of the first doped conductive layer 120 is not too low, ensuring that the doping element concentration of the first doped conductive layer 120 is sufficiently high, forming a sufficiently high potential barrier with the substrate 100 and allowing carriers to pass through the tunneling layer 110 to reach the first doped conductive layer 120.

[0072] Furthermore, within the above range, the concentration differences between the first doped conductive layer 120 and the first portion 11 and between the first doped conductive layer 120 and the second portion 12 are sufficiently large, thereby forming concentration gradients between the first doped conductive layer 120 and the first portion 11 and between the first doped conductive layer 120 and the second portion 12. Because the doping element concentration of the first portion 11 is greater than that of the first doped conductive layer 120, the first portion 11 can form a surface electric field on the surface of the first doped conductive layer 120, and the second portion 12 can form a surface electric field on the surface of the first doped conductive layer 120, thereby enhancing the transport of carriers in the first doped conductive layer 120 to the first portion 11 and the second portion 12.

[0073] 4 is a diagram showing a cross-sectional structure of a second solar cell according to an embodiment of the present disclosure, and is a diagram showing a cross-sectional structure along the AA' direction in FIG. 2. In some embodiments, the first doped conductive layer 120 includes a plurality of third portions and a plurality of fourth portions, where the third portions 13 and the fourth portions 14 are alternately arranged along a direction parallel to the first surface 1, and the third portions 13 and the fourth portions 14 extend along a predetermined direction X, with one third portion 13 facing one first portion 11 and one fourth portion 14 facing one second portion 12, and the doping element concentration of the third portion 13 being lower than the doping element concentration of the fourth portion 14. That is, the doping element concentration of the first doped conductive layer 120 facing the first electrode 140 is higher than the doping element concentration of the first doped conductive layer 120 not facing the first electrode 140.

[0074] Because the doping element concentration in the third portion 13 is lower than that in the fourth portion 14, a concentration gradient is formed between the third portion 13 and the fourth portion 14. The presence of this concentration gradient forms a built-in electric field in the first doped conductive layer 120 from the fourth portion 14 to the third portion 13, thereby enhancing lateral transport of carriers in the third portion 13 to the fourth portion 14. Because the fourth portion 14 faces the first electrode 140, the efficiency of carrier transport from the fourth portion 14 to the second portion 12 is higher than that of the third portion 13, allowing more carriers to be collected by the first electrode 140. Based on this, the lateral transport of carriers in the third portion 13 to the fourth portion 14 can be enhanced, thereby enhancing the carrier collection efficiency of the first electrode 140.

[0075] In some embodiments, the doping element type of the first doped conductive layer 120 is P-type, and the ratio of the doping element concentration of the third portion 13 to the doping element concentration of the fourth portion 14 is 1:100 to 2:3, for example, 1:90, 1:80, 1:70, 1:65, 1:55, 1:50, 1:40, 1:30, 1:25, 1:20, 1:18, 1:15, 1:10, 1:5, 1:3 or 2:3. In some embodiments, the doping element type of the first doped conductive layer 120 is N-type, and the ratio of the doping element concentration of the third portion 13 to the doping element concentration of the fourth portion 14 is 1:30 to 5:6, for example, 1:30 to 1:25, 1:25 to 1:20, 1:20 to 1:15, 1:15 to 1:10, 1:10 to 1:8, 1:8 to 1:5, 1:5 to 1:3, 1:3 to 2:3, or 2:3 to 5:6.

[0076] By setting different ratios of the doping element concentrations in the third portion 13 and the fourth portion 14 to different values ​​using different doping elements, the third portion 13 and the fourth portion 14 can have good passivation performance for the first surface 1, whether they are P-type doped or N-type doped. Furthermore, within the above ratio range, a concentration gradient can be formed between the third portion 13 and the fourth portion 14, thereby improving the carrier collection efficiency of the first electrode 140. In some embodiments, the P-type doping element can be boron, aluminum, nitrogen, gallium, or indium. In some embodiments, the N-type doping element can be phosphorus, bismuth, antimony, or arsenic.

[0077] In some embodiments, the doping element type of the first doped conductive layer 120 is P-type, the number of third portions 13 is multiple, the number of fourth portions 14 is multiple, and the ratio of the doping element concentration of each third portion 13 among the multiple third portions to the doping element concentration of each fourth portion 14 among the multiple fourth portions is 1:100 to 2:3. In some embodiments, the doping element type of the first doped conductive layer 120 is N-type, the number of third portions 13 is multiple, the number of fourth portions 14 is multiple, and the ratio of the doping element concentration of each third portion 13 among the multiple third portions to the doping element concentration of each fourth portion 14 among the multiple fourth portions is 1:30 to 5:6.

[0078] Note that the doping element concentrations of the third portion 13 and the fourth portion 14 referred to here are the surface doping concentrations of the surface of the third portion 13 away from the substrate 100 and the surface doping concentrations of the surface of the fourth portion 14 away from the substrate 100.

[0079] In some embodiments, when the doping element type of the first doped conductive layer 120 is P-type, the doping element concentration of each third portion 13 of the plurality of third portions is 1×10 18 atom / cm 3 ~5×10 19 atom / cm 3 For example, 1×1018 atom / cm 3 ~2×10 18 atom / cm 3 , 2 × 10 18 atom / cm 3 ~5×10 18 atom / cm 3 , 5×10 18 atom / cm 3 ~9×10 18 atom / cm 3 , 9×10 18 atom / cm 3 ~1×10 19 atom / cm 3 , 1×10 19 atom / cm 3 ~3×10 19 atom / cm 3 or 3×10 19 atom / cm 3 ~5×10 19 atom / cm 3 The doping element concentration of each of the fourth portions 14 of the plurality of fourth portions may be 1×10 19 atom / cm 3 ~1×10 20 atom / cm 3 For example, 1×10 19 atom / cm 3 ~2×10 19 atom / cm 3 , 2 × 10 19 atom / cm 3 ~5×10 19 atom / cm 3 , 5×10 19 atom / cm 3 ~7×10 19 atom / cm 3 , 7×10 19 atom / cm 3 ~9×10 19 atom / cm 3 or 9×10 19 atom / cm 3 ~1×10 20 atom / cm 3 may be.

[0080] In some embodiments, the doping element type of the first doped conductive layer 120 is N-type, and the doping concentration of each third portion 13 of the plurality of third portions is 2×10 19 atom / cm 3 ~5×10 20 atom / cm 3 For example, 2 × 10 19 atom / cm 3 ~3×10 19 atom / cm 3 , 3×10 19 atom / cm 3 ~5×10 19 atom / cm 3 , 5×10 19 atom / cm 3 ~9×10 19 atom / cm 3 , 9×10 19 atom / cm 3 ~1×10 20 atom / cm 3 , 1×10 20 atom / cm 3 ~3×10 20 atom / cm 3 or 3×10 20 atom / cm 3 ~5×10 20 atom / cm 3 The doping element concentration of each of the fourth portions 14 of the plurality of fourth portions may be 5×10 19 atom / cm 3 ~6×10 20 atom / cm 3 For example, 5 × 10 19 atom / cm 3 ~7×10 19 atom / cm 3 , 7×10 19 atom / cm 3 ~9×10 19 atom / cm 3 , 9×10 19 atom / cm 3 ~1×10 20 atom / cm 3 , 1×10 20 atom / cm 3 ~3×1020 atom / cm 3 , 3×10 20 atom / cm 3 ~5×10 20 atom / cm 3 or 5×10 20 atom / cm 3 ~6×10 20 atom / cm 3 may be.

[0081] Within the above range, the doping element concentration of the fourth portion 14 is ensured to be greater than the doping element concentration of the third portion 13, which can enhance the lateral transport of carriers in the third portion 13 to the fourth portion 14. At the same time, within the above range, the doping element concentrations of the third portion 13 and the fourth portion 14 are not too high, which can ensure that the doping element concentration of the entire first doped conductive layer 120 is small, which can reduce the probability of the doping elements in the first doped conductive layer 120 being transported to the tunnel layer 110.

[0082] In some embodiments, the ratio of the doping element concentration in the fourth portion 14 to the doping element concentration in the second portion 12 is 1:10 to 5:6, and may be, for example, 1:10 to 1:8, 1:8 to 1:6, 1:6 to 1:4, 1:4 to 1:3, 1:3 to 1:2, 1:2 to 2:3, 2:3 to 3:4, or 3:4 to 5:6. Within this range, the doping element concentration in the fourth portion 14 is lower than the doping element concentration in the second portion 12, forming a concentration gradient between the fourth portion 14 and the second portion 12, which enhances the transport of carriers in the fourth portion 14 to the second portion 12 and thus improves the collection ability of the first electrode 140 for carriers in the second portion 12.

[0083] There are multiple fourth portions 14 and multiple second portions 12, and the ratio of the doping element concentration of each fourth portion 14 among the multiple fourth portions to the doping element concentration of each second portion 12 among the multiple second portions is 1:10 to 5:6.

[0084] In some embodiments, the thickness ratio of the first doped conductive layer 120 and the second doped conductive layer 130 is controlled to ensure that the first electrode 140 is unlikely to penetrate the second doped conductive layer 130, while ensuring that the total thickness of the first doped conductive layer 120 and the second doped conductive layer 130 is not too large, thereby avoiding the problem of excessive stress being caused in the tunnel layer 110 due to the total thickness of the first doped conductive layer 120 and the second doped conductive layer 130 being too large, and maintaining good performance of the tunnel layer 110.

[0085] In some embodiments, the ratio of the thickness d1 of the first doped conductive layer 120 to the thickness d2 of the second doped conductive layer 130 is 2:1 to 1:12, such as 2:1 to 3:2, 3:2 to 4:3, 4:3 to 1:1, 1:1 to 1:3, 1:3 to 1:2, 1:2 to 1:5, 1:5 to 1:7, 1:7 to 1:9, or 1:9 to 1:12. Within this range, it is difficult for the actually manufactured first electrode 140 to penetrate the second doped conductive layer 130 to electrically contact the first doped conductive layer 120 and achieve good ohmic contact between the first electrode 140 and the second portion 12. Furthermore, the thickness d1 of the first doped conductive layer 120 is not too large, and the total thickness of the first doped conductive layer 120 and the second doped conductive layer 130 is not too large, so as to avoid excessive stress being applied to the tunnel layer 110 due to the total thickness of the first doped conductive layer 120 and the second doped conductive layer 130 being too large.

[0086] In some embodiments, the material of the first doped conductive layer 120 includes at least one of amorphous silicon, polycrystalline silicon, or silicon carbide. In some embodiments, the first doped conductive layer 120 includes a third portion 13 and a fourth portion 14, which are obtained by doping different portions of the first doped conductive layer 120 with different concentrations, and therefore the third portion 13 and the fourth portion 14 are an integrated structure.

[0087] In some embodiments, the material of the second doped conductive layer 130 includes at least one of amorphous silicon, polycrystalline silicon, or silicon carbide. The first portion 11 and the second portion 12 are obtained by doping different portions of the second doped conductive layer 130 at different concentrations, and the first portion 11 and the second portion 12 are an integrated structure.

[0088] In some embodiments, the first doped conductive layer 120 is made of a first polycrystalline silicon, the first portion 11 is made of a second polycrystalline silicon, and the second portion 12 is made of a third polycrystalline silicon, and the first polycrystalline silicon has an average grain size larger than the average grain size of the second polycrystalline silicon and larger than the average grain size of the third polycrystalline silicon, and the second polycrystalline silicon has an average grain size larger than the average grain size of the third polycrystalline silicon.

[0089] In polycrystalline silicon, silicon atoms are arranged in a diamond crystal lattice in a number of crystal nuclei, which grow into crystal grains with different crystal plane orientations. When these crystal grains combine, they are crystallized into polycrystalline silicon. In other words, the first polycrystalline silicon, the second polycrystalline silicon, and the third polycrystalline silicon are all formed by combining multiple crystal grains. The contact interface between crystal grains of the first polycrystalline silicon, the second polycrystalline silicon, and the third polycrystalline silicon that have the same structure but different orientations can be called a grain boundary.

[0090] That is, the grain density of the first polycrystalline silicon in the first doped conductive layer 120 per unit volume is smaller than the grain density of the second polycrystalline silicon and the grain density of the third polycrystalline silicon in the second doped conductive layer 130. As a result, the number of grain boundaries in the first doped conductive layer 120 per unit volume is smaller than the number of grain boundaries in the second doped conductive layer 130 per unit volume. Grain boundaries act as diffusion paths for the doping element, and the greater the number of grain boundaries, the greater the diffusion of the doping element and the higher the doping element concentration. Because the number of grain boundaries in the first doped conductive layer 120 is relatively small, the degree of diffusion of the doping element in the first doped conductive layer 120 is low during the doping process to actually form the first doped conductive layer 120, ensuring a low doping element concentration in the first doped conductive layer 120. Since the number of grain boundaries in the second doped conductive layer 130 is relatively large, the degree of diffusion of the doping element in the second doped conductive layer 130 is high, and the concentration of the doping element in the second doped conductive layer 130 is high.

[0091] Furthermore, the number of crystal grains in the second doped conductive layer 130 per unit volume is greater than the number of crystal grains in the first doped conductive layer 120, i.e., the crystallinity of the second doped conductive layer 130 is high, which allows the second doped conductive layer 130 to have better passivation performance and further improves the metal contact composite between the second portion 12 and the first electrode 140.

[0092] As shown in FIG. 4 , in some embodiments, the first doped conductive layer 120 may include a third portion 13 facing the first portion 11 and a fourth portion 14 facing the second portion 12, where the third portion 13 is made of fourth polycrystalline silicon, the fourth portion 14 is made of fifth polycrystalline silicon, the first portion 11 is made of second polycrystalline silicon, and the second portion 12 is made of third polycrystalline silicon, where the average grain size of the fourth polycrystalline silicon is larger than the average grain size of the fifth polycrystalline silicon, the average grain size of the fifth polycrystalline silicon is larger than the average grain size of the third polycrystalline silicon, the average grain size of the second polycrystalline silicon is larger than the average grain size of the third polycrystalline silicon, and the average grain size of the fifth polycrystalline silicon is larger than the average grain size of the second polycrystalline silicon.

[0093] The average crystal grain size of the fourth polycrystalline silicon is larger than the average crystal grain size of the fifth polycrystalline silicon, i.e., the average crystal grain size in the first doped conductive layer 120 facing the first electrode 140 is smaller than the average crystal grain size in the first doped conductive layer 120 not facing the first electrode 140. As a result, the number of grain boundaries per unit volume in the first doped conductive layer 120 facing the first electrode 140 is larger than the number of grain boundaries per unit volume in the first doped conductive layer 120 not facing the first electrode 140. As a result, in the step of actually performing doping to form the first doped conductive layer 120, the degree of diffusion of the doping element in the first doped conductive layer 120 directly facing the first electrode 140 is greater than the degree of diffusion of the doping element in the first doped conductive layer 120 not directly facing the first electrode 140, which helps to ensure that the doping element concentration in the third portion 13 is lower than the doping element concentration in the fourth portion 14, forming a concentration gradient between the third portion 13 and the fourth portion 14 and helping to transport carriers laterally from the third portion 13 to the fourth portion 14.

[0094] The average grain sizes of the first polycrystalline silicon, the second polycrystalline silicon, the third polycrystalline silicon, the fourth polycrystalline silicon, and the fifth polycrystalline silicon in the examples of the present application can be measured in accordance with the Chinese national standard "GB / T6394-2017 Method for Determining Average Grain Size of Metals."

[0095] FIG. 5 is a diagram showing a top view configuration of another solar cell provided by an embodiment of the present application, FIG. 6 is a diagram showing a cross-sectional structure of a third solar cell provided by an embodiment of the present application, and FIG. 6 is a diagram showing a cross-sectional structure along the AA' direction of FIG.

[0096] As shown in Figures 5 and 6, in some embodiments, the doping element type of the substrate 100 is an N-type doping element, and the second portion 12 includes a main body portion 20 doped with the N-type doping element and an inverse doping portion 21 located within the main body portion 20 and doped with a P-type doping element.

[0097] In some embodiments, the material of the first electrode 140 is metal, including copper, silver, nickel, or aluminum. The material of the second portion 12 is silicon, such as polycrystalline silicon, amorphous silicon, or single-crystalline silicon. The actual process for fabricating the first electrode 140 involves first forming a metal paste, and then the metal in the metal paste reacts with oxygen to form metal ions. When the metal ions migrate into the second portion 12 and provide electrons, a reduction reaction occurs between the metal ions and silicon in the second portion 12, reducing the metal ions to metal. The resulting metal is located in the second portion 12, thereby establishing electrical contact between the formed first electrode 140 and the second portion 12. However, if too much metal is reduced, the formed first electrode 140 may penetrate the entire second portion 12, damaging the second portion 12 and potentially contacting the first electrode 140 with the substrate 100, which could adversely affect the photoelectric conversion performance of the solar cell.

[0098] The second doped conductive layer 130 includes a main body 20 containing an N-type doping element and an inversion doping portion 21 located within the main body 20. The inversion doping portion 21 is doped with a P-type doping element, so that holes are dominant in the inversion doping portion 21, providing more hole positions. Meanwhile, some of the electrons transported to the second portion 12 recombine with holes, resulting in a reduced number of electrons compared to a case where the inversion doping portion 21 is not provided. As a result, in the step of actually forming the first electrode 140, the reduced number of electrons weakens the reaction between metal ions and silicon, preventing the problem of excessive damage to the second portion 12 due to the metal being generated by the reduction of the metal ions and silicon. This maintains good photoelectric conversion performance of the solar cell.

[0099] In some embodiments, the volume ratio of the counter-doped regions 21 within the body region 20 is less than 1 / 2. That is, because the counter-doped regions 21 are in a minority within the body region 20, the volume of the body region 20 is large enough to form a band bending at the first surface 1, and the first electrode 140 can contact most of the body region 20 to form a metal contact, which helps ensure normal transport of carriers within the second region 12 and collection of carriers by the first electrode 140.

[0100] FIG. 7 is a diagram showing the cross-sectional structure of a fourth solar cell in one embodiment of the present application, and FIG. 8 is a diagram showing the cross-sectional structure of a fifth solar cell in one embodiment of the present application, and both FIG. 7 and FIG. 8 are diagrams showing the cross-sectional structure along the AA' direction in FIG. 2.

[0101] As shown in Figures 7 and 8, in some embodiments, the semiconductor device further includes a blocking layer 150, which is located between the first doped conductive layer 120 and the second doped conductive layer 130, and the surface of the blocking layer 150 facing the substrate 100 is in contact with the surface of the first doped conductive layer 120 away from the substrate 100, and the surface of the blocking layer 150 facing the substrate 100 is in contact with the surface of the second doped conductive layer 130 facing the substrate 100. Since the doping element concentration of the second doped conductive layer 130 is higher than that of the first doped conductive layer 120, a blocking layer 150 is provided between the first doped conductive layer 120 and the second doped conductive layer 130 to prevent the doping element in the second doped conductive layer 130 from diffusing excessively into the first doped conductive layer 120, and serves to block the diffusion of the doping element in the second doped conductive layer 130 into the first doped conductive layer 120, thereby maintaining a low doping element concentration in the first doped conductive layer 120.

[0102] In addition, in some embodiments, the material of the first electrode 140 includes a metal, the substrate 100 is an N-type substrate 100, and the blocking layer 150 serves to block the transport of electrons in the substrate 100 to the second portion 12, thereby reducing the degree to which metal ions in the metal paste used to form the first electrode 140 react with silicon under conditions that supply electrons, thereby reducing the probability that the formed first electrode 140 will penetrate the second doped conductive layer 130.

[0103] 7 , in some embodiments, the surface of the blocking layer 150 away from the substrate 100 is in contact with each second portion 12, and the orthogonal projection of the blocking layer 150 on the first surface 1 overlaps with the orthogonal projection of the second portion 12 on the first surface 1. That is, the blocking layer 150 is located only between a portion of the first doped conductive layer 120 and a portion of the second doped conductive layer 130, and faces the second portion 12. This is because the doping element concentration in the second portion 12 is higher than that in the first portion 11. Therefore, by arranging the blocking layer 150 so as to face only the second portion 12, it is possible to prevent the doping element in the second portion 12, which has a relatively higher doping element concentration, from diffusing into the first doped conductive layer 120.

[0104] In some embodiments, the number of barrier layers 150 may be multiple, and each barrier layer 150 of the multiple barrier layers 150 contacts one second portion 12 .

[0105] 8 , in some embodiments, the surface of the blocking layer 150 facing away from the substrate 100 is in contact with each of the first portions 11 and each of the second portions 12, and the orthogonal projection of the blocking layer 150 on the first surface 1 overlaps with the orthogonal projection of each of the first portions 11 on the first surface 1 and the orthogonal projection of each of the second portions 12 on the first surface 1. That is, the front surface of the blocking layer 150 is covered by the surface of the first doped conductive layer 120 facing away from the substrate 100 and the surface of the second doped conductive layer 130 facing toward the substrate 100. This allows the blocking layer 150 to act as a barrier against the doping elements in the first portions 11 and the second portions 12, preventing the doping elements in the first portions 11 and the second portions 12 from diffusing into the first doped conductive layer 120.

[0106] In some embodiments, whether the blocking layer 150 faces only the second portion 12 or both the first portion 11 and the second portion 12, the material of the blocking layer 150 may be a wide bandgap material, which can effectively prevent the doping elements in the second doped conductive layer 130 from diffusing into the first doped conductive layer 120. In some embodiments, the material of the blocking layer 150 includes at least one of silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, and magnesium fluoride. The use of these materials can provide the blocking layer 150 with a good blocking effect and also provide a good passivation effect on the first surface 1, suppressing carrier recombination on the first surface 1. Furthermore, these materials have relatively high hardness, which makes it difficult for the formed first electrode 140 to burn through the blocking layer 150 during sintering during the actual manufacturing step of the first electrode 140, thereby reducing the risk of contact between the formed first electrode 140 and the substrate 100.

[0107] In some embodiments, whether the blocking layer 150 faces only the second portion 12 or faces both the first portion 11 and the second portion 12, the thickness of the blocking layer 150 is 0.5 nm to 5 nm, and may be, for example, 0.5 nm to 0.8 nm, 0.8 nm to 1 nm, 1 nm to 1.5 nm, 1.5 nm to 2 nm, 2 nm to 2.5 nm, 2.5 nm to 3 nm, 3 nm to 3.5 nm, 3.5 nm to 4 nm, 4 nm to 4.5 nm, or 4.5 nm to 5 nm. Within the above range, the doping elements in the second doped conductive layer 130 can be effectively prevented from diffusing into the first doped conductive layer 120, while not adversely affecting the performance of the entire passivation contact structure composed of the first doped conductive layer 120, the second doped conductive layer 130 and the tunnel layer 110, and maintaining the selective transport of carriers in the passivation contact structure and good passivation effect on the first surface 1.

[0108] FIG. 9 is a diagram showing a cross-sectional structure of a sixth solar cell provided by an embodiment of the present application, and FIG. 9 is a diagram showing a cross-sectional structure along the direction AA′ of FIG.

[0109] 9 , in some embodiments, the solar cell further includes a first passivation layer 160, which covers surfaces of the first portion 11 and the second portion 12 that are remote from the substrate 100. The first electrode 140 penetrates the first passivation layer 160 and is in electrical contact with the second portion 12. The first passivation layer 160 can provide a good passivation effect for the first surface 1, such as providing good chemical passivation for dangling bonds on the first surface 1, reducing the defect state density on the first surface 1, and suppressing carrier recombination on the first surface 1.

[0110] In some embodiments, first passivation layer 160 may have a single layer structure. In some embodiments, first passivation layer 160 may have a multi-layer structure. In some embodiments, the material of first passivation layer 160 may be at least one of silicon oxide, aluminum oxide, silicon nitride, or silicon oxynitride.

[0111] In some embodiments, the solar cell may include an emitter 170 located on the second surface 2 of the substrate 100. The doping element type of the emitter 170 is opposite to the doping element type of the substrate 100 and forms a PN junction with the substrate 100. In some embodiments, the material of the emitter 170 is the same as the material of the substrate 100.

[0112] FIG. 10 is a diagram showing a cross-sectional structure of a seventh solar cell in one embodiment of the present invention, and FIG. 10 is a diagram showing a cross-sectional structure taken along the direction AA′ in FIG.

[0113] 10 , in some embodiments, the solar cell may not have an emitter 170, but may have a second passivation contact structure on the second surface 2, which includes a second tunneling layer 111 and a third doped conductive layer 112 located on the surface of the second tunneling layer 111, so that the solar cell is a bifacial TOPCON cell. The doping element type of the third doped conductive layer 112 is opposite to that of the substrate 100, i.e., the doping element of the third doped conductive layer 112 is P-type, forming a PN junction with the substrate 100.

[0114] In some embodiments, the material of the second tunneling layer 111 may include at least one of silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or magnesium fluoride.

[0115] In some embodiments, the material of the third doped conductive layer 112 includes at least one of amorphous silicon, polycrystalline silicon, or silicon carbide.

[0116] As shown in FIGS. 9 and 10, in some embodiments, the solar cell further comprises a second passivation layer 180 .

[0117] 9, in some embodiments, the emitter 170 is provided within the substrate 100, and the upper surface of the emitter 170 overlaps the second surface 2. This allows the second passivation layer 180 to be located on the surface of the emitter 170 that is remote from the substrate 100.

[0118] 10 , in some embodiments, the substrate 100 does not include an emitter 170, but instead includes a second passivation contact structure. The second passivation layer 180 is located on the surface of the third doped conductive layer 112 that is remote from the substrate 100. The second passivation layer 180 provides a good passivation effect for the second surface 2 of the substrate 100, reducing the defect state density at the second surface 2 and effectively suppressing carrier recombination at the second surface 2 of the substrate 100. The second passivation layer 180 also provides a reflection reduction effect, which helps reduce the reflection of incident light and increase the utilization rate of the incident light.

[0119] In some embodiments, second passivation layer 180 may be a single layer structure, and in some embodiments, second passivation layer 180 may be a multi-layer structure. In some embodiments, the material of second passivation layer 180 may be at least one of silicon oxide, aluminum oxide, silicon nitride, or silicon oxynitride.

[0120] As shown in FIGS. 9-10, some embodiments further include a second electrode 190 located on the second surface 2 of the substrate 100.

[0121] 9, in some embodiments, the emitter 170 is in the substrate 100. Thus, the second electrode 190 extends through the second passivation layer 180 to make electrical contact with the emitter 170.

[0122] 10, in some embodiments, the substrate 100 does not include an emitter 170, but instead includes a second passivation contact structure, such that the second electrode penetrates the second passivation layer 180 and makes electrical contact with the third doped conductive layer 112. In some embodiments, the material of the second electrode may be a metal, such as copper, silver, nickel, or aluminum.

[0123] In the solar cell provided in the above embodiment, the doping element concentration of the first doped conductive layer 120 is lower than that of the second doped conductive layer, thereby reducing the probability that impurity elements in the first doped conductive layer 120 will enter the tunnel layer 110. Furthermore, in the direction perpendicular to the first surface 1, the first portion 11 and the second portion 12 of the second doped conductive layer 130 form a concentration gradient with the first doped conductive layer 120, which helps drive vertical carrier transport and enhance carrier transport in the substrate 100 to the second doped conductive layer 130. The doping element concentration of the first portion 11 is lower than that of the second portion 12, which also forms a concentration gradient between the first portion 11 and the second portion 12, which helps enhance lateral carrier transport in the second doped conductive layer 130. The doping element concentration of the second portion 12 is relatively high, which can improve contact recombination loss between the first electrode 140 and the second portion 12. Since the doping element concentration in the first portion 11 is relatively low, parasitic absorption of incident light in the first portion 11 that is not in contact with the first electrode 140 can be reduced.

[0124] Another aspect of the present embodiment provides a photovoltaic module. As shown in Fig. 11, the photovoltaic module includes a cell string formed by connecting a plurality of solar cells 101 provided in the above embodiment, an encapsulation layer 102 for covering the surface of the cell string, and a cover plate 103 for covering the surface of the encapsulation layer 102 away from the cell string. The solar cells 101 are electrically connected as a whole or in the form of a plurality of divided slices to form a plurality of cell strings, and the plurality of cell strings are electrically connected in series and / or parallel.

[0125] Specifically, in some embodiments, multiple cell strings may be electrically connected via conduction bands 104. The encapsulation layer 102 covers the first surface 1 and the second surface 2 of the substrate 100 of the solar cell 101. Specifically, the encapsulation layer 102 may be an organic encapsulation film such as an ethylene vinyl acetate copolymer (EVA) film, an ethylene octene copolymer (POE) film, a polyethylene terephthalate (PET) film, or a polyvinyl butyral (PVB) film. In some embodiments, the cover plate 103 may be a light-transmitting cover plate such as a glass cover plate or a plastic cover plate. Specifically, the surface of the cover plate 103 facing the encapsulation layer 102 may be textured to increase the utilization efficiency of incident light.

[0126] Furthermore, the present invention also provides a method for manufacturing a solar cell, which is used to manufacture the solar cell provided in the above-described embodiment.

[0127] As shown in FIG. 12, a substrate 100 having a first surface 1 is provided.

[0128] The substrate 100 is used to receive incident light and generate photo-generated carriers, and the substrate 100 has a first surface 1 and a second surface 2 opposite to the first surface 1 .

[0129] In some embodiments, the substrate 100 is doped with an N-type doping element, which may be a Group V element such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As). In some embodiments, the substrate is doped with a P-type doping element, which may be a Group III element such as boron (B), aluminum (Al), gallium (Ga), or indium (In).

[0130] In some embodiments, the second surface 2 of the substrate 100 may be textured, such as a pyramidal texture, which reduces the reflectivity of the second surface 2 of the substrate 100 to incident light and increases its absorption efficiency for the light. The first surface 1 of the substrate 100 may be polished, i.e., the first surface 1 of the substrate 100 is flatter than the second surface 2 of the substrate 100. In some embodiments, both the second surface 2 of the substrate 100 and the first surface 1 of the substrate 100 may be pyramidal textured.

[0131] In some embodiments, the substrate 100 may be subjected to a first doping step, for example an ion implantation step, to diffuse doping elements into the substrate 100 .

[0132] In some embodiments, the solar cell formed is a TOPCON cell.

[0133] 13 , in some embodiments, a method for fabricating a solar cell includes forming an emitter 170 in a substrate 100, with an upper surface of the emitter 170 exposed in the substrate 100 and overlapping the second surface 2. The emitter 170 has a doping element type opposite to that of the substrate 100 and forms a PN junction with the substrate 100.

[0134] In some embodiments, the method for forming the emitter 170 may include performing a diffusion process on the second surface 2 side of the substrate 100, diffusing a P-type element from the second surface 2 of the substrate 100 into the portion of the substrate 100, thereby converting the portion of the substrate 100 into which the P-type doping element is diffused into the emitter 170. In some embodiments, the diffusion process may be an ion implantation process. In some embodiments, a phosphorus diffusion process may be performed on the second surface 2 side of the substrate 100.

[0135] As shown in FIG. 14, after the emitter 170 is formed, a tunnel layer 110 is formed on the first surface 1 .

[0136] In some embodiments, the tunnel layer 110 can be formed at the first surface 1 using a deposition process, which may include either atomic layer deposition or chemical vapor deposition.

[0137] In some embodiments, the material of the tunnel layer 110 may include at least one of silicon oxide, aluminum oxide, silicon nitride, silicon oxynitride, amorphous silicon, or polycrystalline silicon.

[0138] 15 to 25 , a first doped conductive layer 120 is formed on a tunnel layer 110. A second doped conductive layer 130 is formed on the side of the first doped conductive layer 120 away from the substrate 100. The second doped conductive layer 130 includes a plurality of first portions and a plurality of second portions, and the first portions 11 and the second portions 12 are alternately arranged along a predetermined direction X and a direction perpendicular to the thickness direction of the second doped conductive layer 130, and both the first portions 11 and the second portions 12 extend along the predetermined direction X, where the doping element concentration of the first doped conductive layer 120 is lower than the doping element concentration of the first portions 11, which is lower than the doping element concentration of the second portions 12.

[0139] Compared with the second doped conductive layer 130, the first doped conductive layer 120 is closer to the substrate 100, and the doping element concentration of the first doped conductive layer 120 is lower than the doping element concentration of the second doped conductive layer 130, thereby reducing the probability that the impurity elements in the first doped conductive layer 120 will enter the tunnel layer 110.

[0140] In some embodiments, a method for forming the first doped conductive layer 120 and the second doped conductive layer 130 may include the following.

[0141] As shown in FIGS. 15 to 19 , an intrinsic silicon layer 30 is formed on the surface of the tunnel layer 110. In some embodiments, the intrinsic silicon layer 30 may be polycrystalline silicon, amorphous silicon, single crystal silicon, or silicon carbide. A first doping process is performed on the intrinsic silicon layer 30 to form an initial silicon-doped layer 32. A second doping process is performed on the initial silicon-doped layer 32 to diffuse the doping element into only a portion of the initial silicon-doped layer 32, forming a silicon-doped layer 33. The remaining initial silicon-doped layer 32 is designated as the first doped conductive layer 120. Finally, a third doping process is performed on a portion of the silicon-doped layer 33 to form a second portion 12, and the remaining portion of the silicon-doped layer 33 is designated as the first portion 11.

[0142] In some embodiments, the first doping process may be an ion implantation process. In some embodiments, the second doping process may be a laser doping process, in which the laser wavelength, laser frequency, laser energy, or scan rate is controlled to control the depth to which the doping element reaches the initial silicon-doped layer 32, thereby controlling the thicknesses of the first doped conductive layer 120 and the silicon-doped layer 33 to be formed. In some embodiments, the third doping process may be a laser doping process, in which laser irradiation is performed on only a portion of the silicon-doped layer 33, and the doping element is re-injected into this portion of the silicon-doped layer 33 to form the second portion 12 and the first portion 11.

[0143] 15 , in some embodiments, the intrinsic silicon layer 30 may be intrinsic polycrystalline silicon, and in the first doping step, a doping source containing a first doping element is deposited on the surface of the intrinsic silicon layer 30. In some embodiments, the first doping element is an N-type doping element. In some embodiments, the N-type doping source may be an element or compound containing a pentavalent element, such as phosphorus or a compound containing phosphorus, such as phosphorus trichloride.

[0144] Prior to the doping source deposition step, the substrate 100 is subjected to a quartz carrier deposition process. After the substrate 100 is deposited in the quartz carrier, the temperature is increased, a doping source is deposited on the first surface 1 of the substrate 100, and oxygen is introduced. In some embodiments, the doping source may be nitrogen gas carrying phosphorus trichloride. As shown in FIG. 16, in this step, oxygen reacts with the polycrystalline silicon to convert a portion of the intrinsic silicon layer 30 into a glass layer 31, which is silicon oxide containing a first doping element. For example, if the first doping element is phosphorus, the glass layer 31 is silicon phosphate glass, i.e., phosphorus-containing silicon oxide. As shown in FIG. 17, after a large amount of the first doping element is accumulated in the glass layer 31, the temperature is increased and the first doping element accumulated in the glass layer 31 is diffused into the intrinsic polycrystalline silicon, forming an initial silicon-doped layer 32.

[0145] As shown in FIG. 18, in the second doping process, the glass layer 31 is retained and laser light is used to irradiate the glass layer 31, causing the first doping element in the laser-treated glass layer 31 to re-diffuse into part of the initial silicon-doped layer 32, thereby forming a first doped conductive layer 120 and a silicon-doped layer 33.

[0146] As shown in Figure 19, in the third doping process, the glass layer 31 is still retained, and a portion of the glass layer 31 is irradiated with laser light, causing the first doping element in the laser-treated glass layer 31 to re-diffuse into a portion of the silicon-doped layer 33, thereby forming the first portion 11 and the second portion 12.

[0147] In some embodiments, the laser used in the laser process may be an infrared laser, a green laser, or an ultraviolet laser, which may be generated from a CO2 laser, an excimer laser, a titanium sapphire laser, a semiconductor laser, a copper vapor laser, or any other laser capable of emitting laser light.

[0148] The surface of the glass layer 31 is irradiated with laser light emitted from a laser, and the first doping element in the glass layer 31 diffuses into the initial silicon-doped layer 32 or the silicon-doped layer 33 due to the laser thermal effect.

[0149] After forming the first portion 11 and the second portion 12, the glass layer 31 is removed. The glass layer 31 can be removed by an acid cleaning process.

[0150] 21 , in some embodiments, before the step of forming the second doped conductive layer 130, a blocking layer 150 located on a surface of the first doped conductive layer 120 away from the substrate 100 is further formed, and the material of the blocking layer 150 includes at least one of silicon oxide, silicon nitride, silicon oxynitride, and silicon carbide. The blocking layer 150 serves to block the diffusion of the doping element in the second doped conductive layer 130 into the first doped conductive layer 120, thereby maintaining a small doping element concentration in the first doped conductive layer 120.

[0151] In some embodiments, a method for forming the first doped conductive layer 120, the second doped conductive layer 130, and the blocking layer 150 includes the following.

[0152] 20, a first intrinsic silicon layer 41 is formed on the surface of the tunnel layer 110. In some embodiments, the first intrinsic silicon layer 41 may be polycrystalline silicon, amorphous silicon, single crystal silicon, or silicon carbide. In some embodiments, the first intrinsic silicon layer 41 may be formed on the surface of the tunnel layer 110 using a deposition process, which may be, for example, an atomic layer deposition process.

[0153] 21 , a blocking layer 150 is formed on the surface of the first intrinsic silicon layer 41. In some embodiments, the blocking layer 150 can be formed using a deposition process, such as an atomic layer deposition process or a chemical vapor deposition process. In some embodiments, the blocking layer 150 can be formed over the entire surface of the first intrinsic silicon layer 41, facing the first portion 11 and the second portion 12 that will be formed later. In some embodiments, the blocking layer 150 can be formed only on a portion of the surface of the first intrinsic silicon layer 41, facing the second portion 12 that will be formed later.

[0154] 21, a second intrinsic silicon layer 42 is formed on the surface of the blocking layer 150. In some embodiments, the second intrinsic silicon layer 42 may be any of polycrystalline silicon, amorphous silicon, single crystal silicon, or silicon carbide. In some embodiments, the second intrinsic silicon layer 42 may be formed on the surface of the tunnel layer 110 using a deposition process, which may be, for example, an atomic layer deposition process.

[0155] A doping source containing a first doping element is deposited on the surface of the second intrinsic silicon layer 42 away from the substrate 100. Simultaneously with the deposition of the doping source, oxygen gas is introduced to convert a portion of the second intrinsic silicon layer 42 into a glass layer 31. The glass layer 31 is silicon oxide containing the first doping element.

[0156] In some embodiments, the doping source may be an N-type doping source and the first doping element may be an N-type doping element. In some embodiments, the N-type doping source may be an element or compound containing a pentavalent element, such as phosphorus or a phosphorus-containing compound, such as phosphorus trichloride.

[0157] Before the doping source deposition step, the substrate 100 is subjected to a quartz carrier entry process, and after entering the quartz carrier, the substrate is heated to a first preset temperature, which may be 500° C. to 900° C. After heating to the first preset temperature, the doping source is deposited on the first surface 1 of the substrate 100, and oxygen gas is introduced, and the deposition time of the doping source is 50 seconds to 800 seconds. In some embodiments, the doping source may be nitrogen gas containing phosphorus trichloride, where the concentration of phosphorus trichloride may be 0.1% to 3 wt %, and the flow rate of the nitrogen gas may be 2000 sccm to 4000 sccm.

[0158] 22, in the above steps, oxygen reacts with silicon to convert the partial thickness of the second intrinsic silicon layer 42 into a glass layer 31, which is a silicon oxide containing a first doping element. For example, if the first doping element is phosphorus, the glass layer 31 is a phosphorus silicon glass, i.e., a phosphorus-containing silicon oxide, and a large amount of the first doping element is accumulated in the glass layer 31.

[0159] 23 , a first doping process is performed to diffuse the first doping element accumulated in the glass layer 31 into the first intrinsic silicon layer 41 to form a first doped conductive layer 120, and the first doping element is diffused into the second intrinsic silicon layer 42 excluding the glass layer 31 to form an initial second doped conductive layer 43. In some embodiments, the first doping process is performed after the temperature is raised to a second preset temperature, which may be higher than the first preset temperature, for example, 900°C to 1200°C, and simultaneously, diffusion is performed in a nitrogen gas atmosphere to diffuse the first doping element accumulated in the glass layer 31 into the first intrinsic silicon layer 41 to form the first doped conductive layer 120.

[0160] As can be seen, due to the presence of the blocking layer 150, during the process in which the first doping element in the glass layer 31 diffuses from the second intrinsic silicon layer 42 to the first intrinsic silicon layer 41, the blocking layer 150 acts as a barrier to the first doping element, and the number of doping elements diffusing into the first intrinsic silicon layer 41 is smaller than the number of doping elements diffusing into the second intrinsic silicon layer 42. As a result, the doping element concentration of the formed first doped conductive layer 120 is smaller than the doping element concentration of the initial second doped conductive layer 43.

[0161] As shown in Figures 24 and 25, a second doping process is performed on a portion of the glass layer 31, and the first doping element in the glass layer 31 that has undergone the second doping process diffuses into the initial second doped conductive layer 43 along a direction perpendicular to the first surface 1, converting this portion of the initial second doped conductive layer 43 into the second portion 12 of the second doped conductive layer 130, and the remaining portion of the initial second doped conductive layer 43 forms the first portion 11.

[0162] As shown in FIG. 24, in some embodiments, before performing the second doping process, a mask layer 50 is formed on the surface of the glass layer 31, the mask layer 50 has a first opening 51, and the first opening 51 is exposed from a portion of the surface of the glass layer 31, and in some embodiments, a photoetching process can be performed on the mask layer 50 to form the first opening 51.

[0163] In some embodiments, the material of mask layer 50 may be either silicon oxide or silicon oxynitride, and a deposition process may be used to form mask layer 50 .

[0164] 25 , in some embodiments, a second doping step is performed on the initial second doped conductive layer 43 (see FIG. 24 ) along the first opening 51, and the first doping element in the glass layer 31 directly facing the first opening 51 is diffused into the initial second doped conductive layer 43 to form the second portion 12 with a relatively high doping concentration, while the remaining portion of the initial second doped conductive layer 43 is blocked by the mask layer 50. As a result, the doping element in the glass layer 31 hardly diffuses into this portion of the initial second doped conductive layer 43, and the remaining portion of the initial second doped conductive layer 43 forms the first portion 11 with a relatively low doping concentration.

[0165] As can be easily understood, since the doping element concentration of the initial second doped conductive layer 43 is greater than the doping element concentration of the first doped conductive layer 120, the doping element concentrations of the formed first portion 11 and second portion 12 are both greater than the doping element concentration of the second doped conductive layer 130.

[0166] In some embodiments, the second doping step includes a laser step. The parameters of the laser step include a laser wavelength of 300 nm to 532 nm, for example, 300 nm to 330 nm, 330 nm to 350 nm, 350 nm to 380 nm, 380 nm to 420 nm, 420 nm to 480 nm, or 480 nm to 532 nm; a laser frequency of 120 kHz to 1500 kHz, for example, 120 kHz to 180 kHz, 180 kHz to 240 kHz, 240 kHz to 330 kHz, 330 kHz to 480 kHz, 480 kHz to 600 kHz, 600 kHz to 700 kHz, 700 kHz to 800 kHz, 800 kHz to 900 kHz, 900 kHz to 1050 kHz, or 1050 kHz to 1200 kHz; and a scan laser frequency of 120 kHz to 1500 kHz, for example, 120 kHz to 180 kHz, 180 kHz to 240 kHz, 240 kHz to 330 kHz, 330 kHz to 480 kHz, 480 kHz to 600 kHz, 600 kHz to 700 kHz, 700 kHz to 800 kHz, 800 kHz to 900 kHz, 900 kHz to 1050 kHz, or 1050 kHz to 1200 kHz. The speed is 1000mm / s to 40000mm / s, for example, 1000mm / s to 2000mm / s, 2000mm / s to 5000mm / s, 5000mm / s to 6000mm / s, 6000mm / s to 7500mm / s, 7500mm / s to 9000mm / s, 9000mm / s to 12000mm / s, 12000mm / s to 18000mm / s, 1800 0mm / s to 25000mm / s, 25000mm / s to 28000mm / s, 28000mm / s to 32000mm / s, 32000mm / s to 34000mm / s, 34000mm / s to 36000mm / s, 36000mm / s to 38500mm / s or 38500mm / s to 40000mm / s, and the laser energy is 0.1J / cm 2 ~1.5J / cm 2 For example, 0.1 J / cm 2 ~0.3J / cm 2 , 0.3J / cm 2 ~0.5J / cm 2 , 0.5J / cm 2 ~0.8J / cm 2 , 0.8J / cm 2 ~1J / cm 2 , 1 J / cm 2 ~1.2J / cm 2 , 1.2J / cm 2 ~1.3J / cm 2 or 1.3 J / cm 2 ~1.5J / cm2 Within the above range, a sufficient laser thermal effect can be generated so that the first doping element in the glass layer 31 diffuses into the initial second doped conductive layer 43 by the laser thermal effect. Furthermore, within the above range, the degree of diffusion of the first doping element in the glass layer 31 is not too great, which prevents the first doping element from diffusing too much into the first doped conductive layer 120, thereby preventing an increase in the doping element concentration of the first doped conductive layer 120 that is formed.

[0167] In some embodiments, the parameters of the laser process are controlled to diffuse the first doping element into the first doped conductive layer 120, forming a third portion 13 (see FIG. 4) directly opposite the first portion 11 and a fourth portion 14 (see FIG. 4) directly opposite the second portion 12 in the first doped conductive layer 120, the fourth portion 14 directly opposite the second portion 12, and in the step of performing the laser process to form the second portion 12, a portion of the first doping element diffuses into the first doped conductive layer 120 directly opposite the second portion 12 to form the fourth portion 14 with a relatively high doping element concentration, and the remaining portion of the first doped conductive layer 120 forms the third portion 13 with a relatively low doping element concentration.

[0168] In some embodiments, the parameters of the laser process can be controlled so that the crystal grains of the formed second portion 12 are recrystallized, and the average crystal grain size in the second portion 12 is smaller than the average crystal grain size in the first portion 11. This increases the amount of the first doping element diffusing into the second portion 12, making it easier to achieve a doping element concentration in the second portion 12 that is higher than the doping element concentration in the first portion 11. In some embodiments, the parameters of the laser process can be controlled so as to recrystallize the crystal grains of the second portion 12 and the fourth portion 14, and thereby achieve a doping element concentration in the fourth portion 14 that is smaller than the average crystal grain size in the third portion 13 and a doping element concentration in the fourth portion 14 that is higher than the doping element concentration in the third portion 13.

[0169] In some embodiments, the laser used in the laser process may be an infrared laser, a green laser, or an ultraviolet laser, which may be generated from a CO2 laser, an excimer laser, a titanium sapphire laser, a semiconductor laser, a copper vapor laser, or any other laser capable of emitting laser light.

[0170] The surface of the glass layer 31 is irradiated with laser light emitted from a laser, and the first doping element in the glass layer 31 diffuses into the initial second doped conductive layer 43 due to the laser thermal effect.

[0171] In some embodiments, after forming the first portion 11 and the second portion 12, the sacrificial layer and the glass layer 31 are removed. In some embodiments, the glass layer 31 may be removed using an acid cleaning process, for example, an HCl solution or an HF solution may be used to clean the sacrificial layer and the glass layer 31 and remove the sacrificial layer and the glass layer 31.

[0172] 26 , in some embodiments, the method for manufacturing a solar cell further includes forming a first passivation layer 160 on a surface of the second doped conductive layer 130 away from the substrate 100. In some embodiments, the first passivation layer 160 may have a single-layer structure. In some embodiments, the first passivation layer 160 may have a multi-layer structure.

[0173] In some embodiments, the first passivation layer 160 has a single layer structure, and the material of the first passivation layer 160 may be any one of silicon oxide, aluminum oxide, silicon nitride, or silicon oxynitride. In some embodiments, the first passivation layer 160 has a multi-layer structure, and the material of the first passivation layer 160 may be at least one of silicon oxide, aluminum oxide, silicon nitride, or silicon oxynitride.

[0174] In some embodiments, the method of forming the first passivation layer 160 may include forming the first passivation layer 160 on the surface of the second doped conductive layer 130 using a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.

[0175] In some embodiments, the method may further include forming a second passivation layer 180 on the surface of the emitter 170, where the second passivation layer 180 can provide a good passivation effect. In some embodiments, the second passivation layer 180 may have a single-layer structure. In some embodiments, the second passivation layer 180 may have a multi-layer structure.

[0176] In some embodiments, the second passivation layer 180 has a single layer structure, and the material of the second passivation layer 180 may be any one of silicon oxide, aluminum oxide, silicon nitride, or silicon oxynitride. In some embodiments, the second passivation layer 180 has a multi-layer structure, and the material of the second passivation layer 180 may be at least one of silicon oxide, aluminum oxide, silicon nitride, or silicon oxynitride.

[0177] In some embodiments, a PECVD process may be used to form a second passivation layer 180 on the surface of the emitter 170 .

[0178] As shown in FIG. 9, a plurality of first electrodes are formed, and each of the first electrodes 140 among the plurality of first electrodes extends along a predetermined direction X, and each of the first electrodes 140 corresponds one-to-one to each of the second portions 12, and one first electrode 140 is in electrical contact with the corresponding second portion 12.

[0179] In some embodiments, a method of forming the first electrode 140 includes the following.

[0180] A metal paste is formed on the side of each second portion away from the substrate 100. In some embodiments, a screen printing process can be used to print the metal paste on the surface of the first passivation layer 160 facing the second portion. In some embodiments, the metal paste may include at least one of silver, aluminum, copper, tin, gold, lead, or nickel.

[0181] A sintering process is performed on the metal paste, and the metal paste is burned through a portion of the thickness of the second portion 12 from the side of the second portion 12 away from the substrate 100 to form the first electrode 140. In some embodiments, the metal paste contains a material with a highly corrosive component, such as glass. As a result, during the sintering process, the corrosive component corrodes the first passivation layer 160 and a portion of the second portion 12, and the metal paste penetrates the first passivation layer 160 and a portion of the second portion 12.

[0182] In some embodiments, the method further includes forming a second electrode 190, where the second electrode 190 penetrates the second passivation layer 180 and makes electrical contact with the emitter 170. In some embodiments, the process of forming the second electrode 190 may be the same as the process of forming the first electrode 140, and reference may be made to the above description of the method of forming the first electrode 140.

[0183] Although the present application has been disclosed as above in preferred embodiments, it does not limit the scope of the claims, and a person skilled in the art may make some possible variations and modifications without departing from the idea of ​​the present application, so the protection scope of the present application should be in accordance with the scope defined by the claims of the present application.

[0184] Those skilled in the art will understand that the above embodiments are specific examples of realizing the present application, but that various changes in form and details are possible in practice without departing from the spirit and scope of the present application. Since anyone skilled in the art can make changes and modifications without departing from the spirit and scope of the present application, the scope of protection of the present application should be based on the scope limited by the claims.

Claims

1. a substrate having a first surface; a tunnel layer formed on the first surface; a first doped conductive layer formed on a surface of the tunnel layer remote from the substrate; a second doped conductive layer formed on a side of the first doped conductive layer away from the substrate, the second doped conductive layer including a plurality of first portions and a plurality of second portions, the first portions and the second portions alternately arranged along a predetermined direction and a direction perpendicular to a thickness direction of the second doped conductive layer, and the first portions and the second portions extend along the predetermined direction, wherein a doping element concentration of the first doped conductive layer is lower than a doping element concentration of the first portions, and a doping element concentration of the first portions is lower than a doping element concentration of the second portions; a plurality of first electrodes, each of which extends along the predetermined direction, each of the first electrodes and each of the second portions are in one-to-one correspondence with each other, and each of the first electrodes is in electrical contact with a corresponding one of the second portions; the predetermined direction is parallel to the first surface and perpendicular to a direction in which the first portions and the second portions are alternately arranged, and a ratio of a doping element concentration of the first portion to a doping element concentration of the second portion is 1:50 to 3:

4. A solar cell characterized by:

2. a ratio of a doping element concentration of the first doped conductive layer to a doping element concentration of the second portion is 1:100 to 1:2; The solar cell according to claim 1 .

3. the first doped conductive layer includes a plurality of third portions and a plurality of fourth portions, the third portions and the fourth portions being alternately arranged along a predetermined direction and a direction perpendicular to a thickness direction of the second doped conductive layer, the predetermined direction being parallel to the first surface, the third portions and the fourth portions both extending along the predetermined direction, one of the third portions facing one of the first portions, one of the fourth portions facing one of the second portions, and a doping element concentration of the third portions being lower than a doping element concentration of the fourth portions; The solar cell according to claim 1 .

4. When the doping element type of the first doped conductive layer is N-type, the ratio of the doping element concentration of the third portion to the doping element concentration of the fourth portion is 1:30 to 5:6, and when the doping element type of the first doped conductive layer is P-type, the ratio of the doping element concentration of the third portion to the doping element concentration of the fourth portion is 1:100 to 2:

3. The solar cell according to claim 3 .

5. the ratio of the doping element concentration of the fourth portion to the doping element concentration of the second portion is 1:10 to 5:6; The solar cell according to claim 4 .

6. a blocking layer, the blocking layer being located between the first doped conductive layer and the second doped conductive layer, the surface of the blocking layer facing the substrate being in contact with the surface of the first doped conductive layer away from the substrate, and the surface of the blocking layer facing the substrate being in contact with the surface of the second doped conductive layer away from the substrate. The solar cell according to any one of claims 1 to 5.

7. a surface of the barrier layer facing away from the substrate is in contact with each of the second portions, and an orthogonal projection of the barrier layer on the first surface overlaps with an orthogonal projection of each of the second portions on the first surface. The solar cell according to claim 6 .

8. a surface of the barrier layer away from the substrate is in contact with each of the first portions and each of the second portions, and an orthogonal projection of the barrier layer on the first surface overlaps with an orthogonal projection of each of the first portions on the first surface and an orthogonal projection of each of the second portions on the first surface; The solar cell according to claim 6 .

9. The material of the blocking layer includes at least one of silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or magnesium fluoride; The solar cell according to claim 6 .

10. The material of the first doped conductive layer includes at least one of amorphous silicon, polycrystalline silicon, or silicon carbide, and the material of the second doped conductive layer includes at least one of amorphous silicon, polycrystalline silicon, or silicon carbide; The solar cell according to claim 9 .

11. the first doped conductive layer is made of first polycrystalline silicon, the first portion is made of second polycrystalline silicon, the second portion is made of third polycrystalline silicon, and an average crystal grain size of the first polycrystalline silicon is larger than an average crystal grain size of the second polycrystalline silicon and is also larger than an average crystal grain size of the third polycrystalline silicon; The solar cell according to claim 10 .

12. the third portion is made of fourth polycrystalline silicon, the fourth portion is made of fifth polycrystalline silicon, the first portion is made of second polycrystalline silicon, and the second portion is made of third polycrystalline silicon, wherein an average crystal grain size of the fourth polycrystalline silicon is larger than an average crystal grain size of the fifth polycrystalline silicon, an average crystal grain size of the fifth polycrystalline silicon is larger than an average crystal grain size of the third polycrystalline silicon, and an average crystal grain size of the second polycrystalline silicon is larger than an average crystal grain size of the third polycrystalline silicon; The solar cell according to claim 3 .

13. a ratio of a thickness of the first doped conductive layer to a thickness of the second doped conductive layer is 2:1 to 1:12; The solar cell according to any one of claims 1 to 5.

14. At least one battery string formed by connecting a plurality of solar cells according to claim 1; at least one encapsulation layer for covering the at least one battery string; and at least one cover plate for covering the at least one sealing layer. A photovoltaic module comprising:

15. Providing a substrate having a first surface; forming a tunnel layer on the first surface; forming a first doped conductive layer on a surface of the tunnel layer remote from the substrate; forming a second doped conductive layer on a side of the first doped conductive layer away from the substrate, the second doped conductive layer including a plurality of first portions and a plurality of second portions, the first portions and the second portions being alternately arranged along a predetermined direction and a direction perpendicular to a thickness direction of the second doped conductive layer, and the first portions and the second portions both extending along the predetermined direction, wherein a doping element concentration of the first doped conductive layer is lower than a doping element concentration of the first portions, and a doping element concentration of the first portions is lower than a doping element concentration of the second portions; forming a plurality of first electrodes, each of the plurality of first electrodes extending along the predetermined direction, each of the first electrodes corresponding to each of the second portions in a one-to-one relationship, and one of the first electrodes being in electrical contact with a corresponding one of the second portions; the predetermined direction is a direction parallel to the first surface and perpendicular to a direction in which the first portions and the second portions are alternately arranged, the ratio of the doping element concentration of the first portion to the doping element concentration of the second portion is 1:50 to 3:4; A method for producing a solar cell comprising the steps of:

16. Before the step of forming the second doped conductive layer, the method further includes forming a blocking layer located on a surface of the first doped conductive layer away from the substrate, the material of the blocking layer including at least one of silicon oxide, silicon nitride, silicon oxynitride, or silicon carbide. The method for producing a solar cell according to claim 15 .

Citation Information

Patent Citations

  • TOPCon battery and preparation method thereof

    CN115692533A

  • Film structure for crystalline silicon solar cell, crystalline silicon solar cell, photovoltaic module and photovoltaic system

    CN218548445U

  • Manufacture of polycrystalline semiconductor film

    JP1995263340A

  • Solar battery, solar battery module, and method of manufacturing solar battery

    JP2016111357A

  • Solar cell

    JP2022073810A