Multilayer type electronic component

By using LiF as a sintering aid in the dielectric layer with controlled Li content, the reliability and connectivity issues in multilayer electronic components are addressed, achieving improved performance and reduced shrinkage differences.

JP2024155766APending Publication Date: 2024-10-31SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024062632
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-09
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The difference in firing temperatures and shrinkage behavior between internal electrodes and dielectric layers in multilayer electronic components leads to agglomeration and stress, causing reliability issues and short circuits.

Method used

Incorporating LiF as a low-temperature sintering aid into the dielectric layer, with a specific Li content of 0.02 to 0.36 mol per 100 mol of Ba, to reduce the firing temperature and minimize volatilization, thereby improving the reliability and connectivity of the components.

Benefits of technology

The addition of LiF as a sintering aid helps in reducing the firing temperature, enhancing the reliability and insulation resistance of multilayer electronic components by minimizing shrinkage differences and maintaining density, even at low thicknesses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155766000001_ABST
    Figure 2024155766000001_ABST
Patent Text Reader

Abstract

To provide a multilayer type electronic component in which, when a low-temperature sintering assistant agent for relieving the reliability decrease of the multilayer type electronic component due to the difference in sintering temperature between an internal electrode and a dielectric layer and reducing the sintering temperature of the dielectric layer is added to a dielectric composition, the excess evaporation of the low-temperature sintering assistant agent in the process of sintering the multilayer type electronic component is prevented, and a manufacturing method for the multilayer type electronic component.SOLUTION: A multilayer type electronic component in one embodiment of the present invention includes a main body including a dielectric layer containing Ba and Ti and internal electrodes alternately disposed with the dielectric layer, and an external electrode disposed on the main body. The dielectric layer further contains Li and F. The content of Li in the dielectric layer is 0.02 moles or more and 0.36 moles or less per 100 moles of Ba in the dielectric layer.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer electronic component. [Background technology]

[0002] Multilayer ceramic capacitors (MLCCs), which are one type of multilayer electronic component, are chip-type capacitors that are mounted on printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones to charge and discharge electricity.

[0003] When forming a thin dielectric layer to miniaturize and increase the capacity of a multilayer electronic component, there is a trend to require stable capacitance and high reliability. In particular, when forming a thin dielectric layer, it is effective to reduce the difference in firing temperature between the dielectric layer and the internal electrodes in order to reduce the difference in shrinkage behavior with the internal electrodes.

[0004] Generally, since the firing temperature of the conductive metal contained in the internal electrodes is lower than that of the ceramic contained in the dielectric layers, agglomeration may occur in the internal electrodes during the firing process of the multilayer electronic components, which may cause a short circuit in the multilayer electronic components. In addition, the difference in shrinkage behavior between the internal electrodes and the dielectric layers may cause stress inside the multilayer electronic components, which may cause a decrease in reliability of the multilayer electronic components.

[0005] Therefore, a method is required to simultaneously sinter the internal electrodes and the dielectric layers at a relatively low temperature and reduce the difference in shrinkage behavior between the internal electrodes and the dielectric layers. Summary of the Invention [Problem to be solved by the invention]

[0006] One of the various objects of the present invention is to mitigate the deterioration of reliability of a multilayer electronic component caused by the difference in firing temperature between the internal electrodes and the dielectric layers.

[0007] One of the various objects of the present invention is to prevent the low-temperature sintering aid from being excessively volatilized during the sintering process of a multilayer electronic component when the low-temperature sintering aid is added to a dielectric composition to lower the sintering temperature of a dielectric layer.

[0008] However, the scope of the present invention is not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Means for solving the problem]

[0009] A multilayer electronic component according to one embodiment of the present invention includes a main body including dielectric layers containing Ba and Ti and internal electrodes arranged alternately with the dielectric layers, and an external electrode arranged on the main body, wherein the dielectric layers further contain Li and F, and the content of Li contained in the dielectric layers is 0.02 mol or more and 0.36 mol or less per 100 mol of Ba contained in the dielectric layers. Effect of the Invention

[0010] One of the various effects of the present invention is that the reliability of the multilayer electronic component can be improved by adding LiF to the dielectric layer and adjusting the content of Li or F contained in the dielectric layer.

[0011] As one of the various effects of the present invention, LiF is added as a low-temperature sintering aid to the dielectric composition forming the dielectric layer, and the difference in sintering temperature between the internal electrodes and the dielectric layer can be reduced by adjusting the form or composition of LiF added, thereby improving the reliability of the multilayer electronic component.

[0012] However, the various and beneficial advantages and effects of the present invention are not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0013] [Figure 1] 1 is a perspective view showing a schematic configuration of a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] 2 is a cross-sectional view taken along line II' in FIG. [Diagram 3] 2 is a cross-sectional view taken along line II-II' in FIG. [Figure 4] This is a graph showing the thermodynamic calculation of the behavior of a mixture containing 1 mol each of LiF and H2O as a function of temperature. [Diagram 5] 1 is a graph showing the shrinkage start temperature depending on the LiF content of LiF samples. [Figure 6] 1 is a graph showing the shrinkage behavior of LiF samples depending on the LiF content and temperature. [Figure 7] 1A is a graph showing the results of a TG-DTA test according to an embodiment, and FIG. 1B is a graph showing the results of a TG-DTA test according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into several other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shapes and sizes of elements in the drawings may be enlarged or reduced (or highlighted or simplified) for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0015] In addition, in the drawings, parts that are not relevant to the description are omitted in order to clearly explain the present invention, and the size and thickness of each component shown in the drawings are arbitrarily shown for the convenience of explanation, so the present invention is not necessarily limited by the drawings. Furthermore, components having the same function within the same concept may be described using the same reference numerals. Furthermore, throughout the specification, when a part "includes" a certain component, it does not mean that the part excludes other components, but that the part may further include other components, unless otherwise specified to the contrary.

[0016] In the drawings, a first direction may be defined as a direction in which first and second internal electrodes are alternately arranged with a dielectric layer therebetween, or a thickness (T) direction, and among second and third directions perpendicular to the first direction, the second direction may be defined as a length (L) direction and the third direction may be defined as a width (W) direction.

[0017] Multilayer Electronic Components FIG. 1 is a perspective view showing a schematic configuration of a multilayer electronic component according to one embodiment of the present invention, FIG. 2 is a cross-sectional view taken along line II' in FIG. 1, and FIG. 3 is a cross-sectional view taken along line II-II' in FIG. 1.

[0018] Hereinafter, a multilayer electronic component and a method for manufacturing a multilayer electronic component according to one embodiment of the present invention will be described in detail with reference to FIGS.

[0019] A multilayer electronic component 100 according to one embodiment of the present invention includes a body 110 including dielectric layers 111 containing Ba and Ti and internal electrodes 121, 122 arranged alternately with the dielectric layers, and external electrodes 130, 140 arranged on the body, wherein the dielectric layers further contain Li and F, and the content of Li in the dielectric layers is 0.02 mol or more and 0.36 mol or less per 100 mol of Ba contained in the dielectric layers.

[0020] The body 110 includes dielectric layers 111 containing Ba and Ti, and internal electrodes 121 , 122 alternating with the dielectric layers 111 .

[0021] Although there is no particular limitation on the specific shape of the main body 110, as shown in FIGS. 1 to 3, the main body 110 can be formed in a hexahedron shape or a shape similar thereto. Due to the shrinkage of the ceramic material contained in the main body 110 during the firing process, the main body 110 may not have a perfect straight-edge hexahedron shape but can substantially have a hexahedron shape.

[0022] The main body 110 can include a first surface 1 and a second surface 2 facing each other in a first direction, a third surface 3 and a fourth surface 4 connected to the first surface 1 and the second surface 2 and facing each other in a second direction, and a fifth surface 5 and a sixth surface 6 connected to the first surface 1 and the second surface 2 and connected to the third surface 3 and the fourth surface 4 and facing each other in a third direction.

[0023] The plurality of dielectric layers 111 forming the main body 110 are in a fired state, and the boundaries between adjacent dielectric layers 111 can be integrated to such an extent that it is difficult to confirm without using a scanning electron microscope (SEM).

[0024] The raw material for forming the dielectric layer 111 is not particularly limited as long as sufficient capacitance can be obtained. For example, a barium titanate-based material can be used. The barium titanate-based material can include BaTiO3-based ceramic powder. Examples of the ceramic powder include BaTiO3, (Ba 1-x Ca x )TiO3 (0 < x < 1) in which Ca (calcium), Zr (zirconium), etc. are partially solid-solved in BaTiO3, Ba(Ti 1-y Ca y )O3 (0 < y < 1), (Ba 1-x Ca x )(Ti 1-y Zr y )O3 (0 < x < 1, 0 < y < 1), or Ba(Ti 1-y Zr y )O3 (0 < y < 1), etc. Thereby, the dielectric layer 111 according to an embodiment of the present invention can contain Ba and Ti.

[0025] In addition, various ceramic additives, organic solvents, binders, dispersants, etc. may be added to the dielectric layer 111 according to the purpose of the present invention.

[0026] Generally, the dielectric layer 111 included in the main body 110 of the multilayer electronic component 100 is formed through a firing process at a high temperature of 1100 degrees or more, so that it may be difficult to form a thin dielectric layer 111. In addition, the dielectric layers 111 are arranged alternately with the internal electrodes 121 and 122 described below, so that a difference in shrinkage behavior occurs between the dielectric layers 111 and the internal electrodes 121 and 122. Such a difference in shrinkage behavior between the dielectric layers 111 and the internal electrodes 121 and 122 may cause stress inside the multilayer electronic component 100, which may cause cracks to occur inside the multilayer electronic component 100.

[0027] Conventionally, Li2CO3 has been used as a sintering aid for the dielectric layer 111 to enable firing at low temperatures and improve the properties of the dielectric layer, but this has problems such as easily volatilizing during the firing process of the dielectric layer, causing discoloration and poor reliability. Therefore, the present invention aims to facilitate the thinning of the multilayer electronic component and improve its electrical and mechanical properties by using LiF instead of Li2CO3 as a low-temperature sintering aid and adjusting the Li content or F content contained in the dielectric layer of the multilayer electronic component after firing.

[0028] In an embodiment of the present invention, the dielectric layer 111 may further contain Li and F in addition to Ba and Ti. Li and F are added to the dielectric layer 111 and may play a role in adjusting microstructures such as the average crystal grain size and porosity of the dielectric layer and variables in the sintering process such as the sintering temperature and sintering pressure.

[0029] When the content of Li contained in the dielectric layer 111 is less than 0.02 moles relative to 100 moles of Ba contained in the dielectric layer 111, the effect of lowering the sintering start temperature of the dielectric layer 111 may be insufficient. When the content of Li contained in the dielectric layer 111 is more than 0.36 moles relative to 100 moles of Ba contained in the dielectric layer 111, it may be difficult to form the dielectric layer 111 with a sufficiently high insulation resistance. According to an embodiment of the present invention, the dielectric layer 111 contains Li and F, and the content of Li contained in the dielectric layer is 0.02 moles or more and 0.36 moles or less relative to 100 moles of Ba contained in the dielectric layer. This can improve the density of the dielectric layer 111, and can improve the connectivity of the internal electrodes by reducing the difference in the shrinkage behavior between the dielectric layer 111 and the internal electrodes 121 and 122, prevent a decrease in capacitance, and suppress deterioration of the insulation resistance. This effect is more pronounced when the content of F contained in the dielectric layer 111 is 0.49 moles or more and 0.88 moles or less relative to 100 moles of Ba contained in the dielectric layer 111.

[0030] An example of a method for measuring the Li and F contents is inductively coupled plasma-mass spectrometry (ICP-MS).

[0031] Meanwhile, a more specific example of measuring the Li content per Ba100 mole and the F content per Ba100 mole contained in the dielectric layer 111 included in the multilayer electronic component 100 of the present invention includes a method of irradiating a laser beam onto the surface of the cross section in the first and second directions polished to the center in the second direction of the multilayer electronic component 100 or the cross section in the first and third directions polished to the center in the third direction, and analyzing the surface through LA-ICP-MS (Laser Ablation-Inductively Coupled Plasma-Mass Spectrometry). In this case, the laser irradiation can be performed on the central region of the dielectric layer 111 arranged at the center of each region after dividing the capacitance forming portion Ac into three equal regions in the first direction. The contents of Ba, Li, and F calculated by irradiating each region with a laser are converted into the Li content per Ba100 mole and the F content per Ba100 mole, and the average value is calculated, so that the Li content per Ba100 mole and the F content per Ba100 mole contained in the dielectric layer 111 can be further generalized.

[0032] Meanwhile, the manner in which Li and F are added to the dielectric layer 111 is important. Specifically, materials such as Li2CO3, which are generally added to the dielectric layer as sintering aids, are easily volatilized during the sintering process, and therefore cannot sufficiently aid the mass transfer of BaTiO3, the main component of the dielectric layer, in the region of about 1100°C, which is close to the firing temperature of multilayer electronic components. Specifically, materials such as Li2CO3, which is an existing sintering aid, suffer a mass loss of about -55% in the region of about 1100°C, making it difficult for them to properly fulfill their role as sintering aids.

[0033] LiF, which is a sintering aid added to the dielectric layer 111, has a low melting point of 1000° C. or less, and can form a liquid phase in a temperature range lower than the firing temperature (1100 to 1200° C.) of the multilayer electronic component, and has a relatively high boiling point of 1600° C. or more, so that a small amount of it volatilizes during firing. Therefore, in one embodiment, by adding LiF to the dielectric layer 111 as a sintering aid, discoloration defects and deterioration of reliability of the multilayer electronic component can be suppressed.

[0034] Meanwhile, when LiF is used as a sintering aid for the dielectric layer 111, it is possible to minimize a phase change of LiF before and after the sintering process of the multilayer electronic component 100. That is, in one embodiment, at least a portion of Li and F contained in the dielectric layer 111 may exist in the form of LiF.

[0035] In one embodiment, the dielectric layer 111 includes a plurality of dielectric crystal grains, and the average crystal grain size of the plurality of dielectric crystal grains may be 150 nm or more and 250 nm or less, thereby ensuring the insulation resistance and reliability of the multilayer electronic component 100 at the same time.

[0036] As an example of a method for measuring the average crystal grain size of a plurality of dielectric crystal grains, a method can be used in which, in a cross section in the first and third directions polished to the center in the second direction of the laminated electronic component 100 or a cross section in the first and second directions polished to the center in the third direction, the capacitance forming portion Ac is divided into three equal parts in the first direction into three regions, and then a central 10 μm×10 μm region of the dielectric layer 111 arranged at the center of each region is observed with a scanning electron microscope (SEM) to obtain an average value of the crystal grain size. In this case, the average crystal grain size can be obtained by measuring the lengths of the short axis and the long axis of each crystal grain and averaging them, or by measuring the area of ​​the crystal grain in pixels and converting it into a circle equivalent diameter.

[0037] In one embodiment, the average density of the dielectric layer 111 may be 95% or more and 99% or less. According to an embodiment of the present invention, the dielectric layer 111 contains Li and F, and the content of Li contained in the dielectric layer 111 is adjusted to 0.02 mol or more and 0.36 mol or less with respect to 100 mol of Ba contained in the dielectric layer, so that sintering is possible even at a relatively low temperature of 1080°C or less, and the density of the dielectric layer 111 can be improved even through such a low-temperature sintering process. In this case, the average density of the dielectric layer 111 may be 95% or more and 99% or less.

[0038] In one embodiment, the density of the dielectric layer may refer to the area ratio of the region excluding pores in the dielectric layer. As an example of a method for measuring the average density of the dielectric layer 111, in a cross section in the first and third directions polished to the center in the second direction of the laminated electronic component 100 or in a cross section in the first and second directions polished to the center in the third direction, the capacitance forming portion Ac is divided into three equal parts in the first direction into three regions, and then a central 10 μm×10 μm region of the dielectric layer 111 arranged at the center of each region is observed with a scanning electron microscope (SEM) to measure the ratio of the pore area, and the average value of the measured values ​​is calculated, and the value of “100-pore area ratio” is defined as the average density of the dielectric layer in the present invention, but the method is not limited thereto.

[0039] On the other hand, there is no need to particularly limit the average thickness td of the dielectric layer 111. However, in general, when the dielectric layer is formed thin, with an average thickness of less than 0.6 μm, particularly when the multilayer electronic component is miniaturized, such as when the average thickness td of the dielectric layer is 0.35 μm or less, it may be difficult to control the sintering shrinkage of the dielectric layer 111.

[0040] According to one embodiment of the present invention, the Li content in the dielectric layer 111 is adjusted to be 0.02 mol or more and 0.36 mol or less relative to 100 mol of Ba in the dielectric layer. Therefore, even when the average thickness td of the dielectric layer is 0.35 μm or less, the sintering shrinkage of the dielectric layer 111 can be adjusted to improve the capacitance characteristics and reliability of the multilayer electronic component 100.

[0041] Therefore, when the average thickness td of the dielectric layer 111 is 0.35 μm or less, the effect of improving the capacitance characteristics and reliability according to the present invention becomes more remarkable.

[0042] The average thickness td of the dielectric layer 111 may refer to the average thickness of the dielectric layer 111 disposed between the first and second internal electrodes 121 and 122.

[0043] The average thickness of the dielectric layer 111 may be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, in the scanned image, the thickness of one dielectric layer may be measured at 30 equally spaced points in the length direction to obtain an average value. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 dielectric layers to measure the average value, the average thickness of the dielectric layer may be further generalized.

[0044] The body 110 may include a capacitance forming portion Ac that is disposed inside the body 110 and includes a first internal electrode 121 and a second internal electrode 122 that are disposed to face each other with a dielectric layer 111 interposed therebetween to form a capacitance.

[0045] The capacitance forming portion Ac is a portion that contributes to forming the capacitance of the capacitor, and can be formed by repeatedly laminating a plurality of first and second internal electrodes 121, 122 with the dielectric layer 111 interposed therebetween.

[0046] 2, cover parts 112 and 113 may be disposed on one surface and the other surface in the first direction of the capacitance forming part Ac. The cover parts 112 and 113 may be formed by laminating a single dielectric layer or two or more dielectric layers in the thickness direction on the upper and lower surfaces of the capacitance forming part Ac, respectively, and may basically play a role in preventing damage to the internal electrodes due to physical or chemical stress.

[0047] The cover parts 112, 113 do not include internal electrodes and may include the same material as the dielectric layer 111. That is, the cover parts 112, 113 may include a ceramic material, for example, a barium titanate (BaTiO3) based ceramic material.

[0048] There is no need to particularly limit the average thickness tc of the covers 112, 113. However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the average thickness tc of the covers 112, 113 can be 15 μm or less.

[0049] The average thickness tc of the cover parts 112, 113 may mean the size in the first direction, and may be the average value of the size in the first direction of the cover parts 112, 113 measured at five equally spaced points on the upper or lower part of the capacitance forming part Ac.

[0050] Referring to FIG. 3, margin portions 114 and 115 may be disposed on one and the other surfaces of the capacitance forming portion Ac in the third direction.

[0051] The margin portions 114, 115 include a margin portion 114 disposed on the fifth surface 5 of the body 110 and a margin portion 115 disposed on the sixth surface 6. That is, the margin portions 114, 115 can be disposed on both side surfaces of the ceramic body 110 in the width direction.

[0052] The margin portions 114 and 115 may refer to the regions between both ends of the first and second internal electrodes 121 and 122 and the boundary surface of the body 110 in a cross section of the body 110 cut in the width-thickness (WT) direction, as shown in FIG. 3.

[0053] The margins 114 and 115 essentially serve to prevent damage to the internal electrodes due to physical or chemical stress.

[0054] The margin portions 114 and 115 may be formed by applying a conductive paste to the ceramic green sheets except for the areas where the margin portions are to be formed, to form internal electrodes.

[0055] In addition, in order to suppress steps caused by the internal electrodes 121, 122, after stacking, the internal electrodes can be cut so as to be exposed on the fifth and sixth faces 5, 6 of the main body, and then a single dielectric layer or two or more dielectric layers can be stacked in the width direction on both side faces of the capacitance forming portion Ac to form margin portions 114, 115.

[0056] On the other hand, there is no need to particularly limit the width of the marginal portions 114, 115. However, in order to more easily achieve a smaller size and higher capacity of the multilayer electronic component, the average width of the marginal portions 114, 115 can be 15 μm or less.

[0057] The average width of the margin portions 114, 115 may mean the average size of the margin portions 114, 115 in the third direction, and may be the average value of the sizes of the margin portions 114, 115 in the third direction measured at five equally spaced points on the side of the capacitance forming portion Ac.

[0058] The internal electrodes 121 , 122 are arranged alternately with the dielectric layers 111 .

[0059] The internal electrodes 121, 122 may include first and second internal electrodes 121, 122. The first and second internal electrodes 121, 122 may be alternately arranged to face each other across the dielectric layer 111 constituting the body 110, and may be exposed to third and fourth surfaces 3, 4 of the body 110, respectively.

[0060] Referring to FIG. 2, the first internal electrode 121 may be spaced apart from the fourth surface 4 and exposed through the third surface 3, and the second internal electrode 122 may be spaced apart from the third surface 3 and exposed through the fourth surface 4.

[0061] At this time, the first and second internal electrodes 121 and 122 may be electrically isolated from each other by the dielectric layer 111 disposed therebetween.

[0062] There are no particular limitations on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity can be used. For example, the internal electrodes 121 and 122 can include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0063] On the other hand, there is no need to particularly limit the average thickness te of the internal electrodes 121, 122. However, in general, when the internal electrodes are formed to a thickness of less than 0.6 μm, particularly when the multilayer electronic component is miniaturized such as when the thickness of the internal electrodes is 0.35 μm or less, it is difficult to adjust the difference in shrinkage behavior between the internal electrodes 121, 122 and the dielectric layer 111, and therefore it may be difficult to improve the reliability of the multilayer electronic component 100.

[0064] According to one embodiment of the present invention, the dielectric layer 111 contains Li and F, and the Li content in the dielectric layer 111 is adjusted to be 0.02 mol or more and 0.36 mol or less per 100 mol of Ba contained in the dielectric layer, so that excellent reliability can be ensured even when the average thickness of the internal electrodes 121, 122 is 0.35 μm or less.

[0065] Therefore, when the internal electrodes 121, 122 have an average thickness of 0.35 μm or less, the effects of the present invention become more pronounced, and miniaturization and high capacity of the multilayer electronic component can be more easily achieved.

[0066] The average thickness te of the internal electrodes 121, 122 may refer to the average thickness of the internal electrodes 121, 122.

[0067] The average thickness of the internal electrodes 121, 122 may be measured by scanning an image of a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, in the scanned image, the thickness of one internal electrode may be measured at 30 equally spaced points in the length direction to obtain an average value. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 internal electrodes and an average value is measured, the average thickness of the internal electrodes may be further generalized.

[0068] In one embodiment, the internal electrodes 121 and 122 may contain Ni. The firing temperature (about 950° C.) of Ni contained in the internal electrodes 121 and 122 is much lower than the firing temperature (about 1100 to 1200° C.) of the barium titanate-based material that may be the main component of the dielectric layer 111. Therefore, in the process of firing the main body 110, the internal electrodes 121 and 122 may experience electrode aggregation, a decrease in electrode connectivity, a decrease in electrode coverage, and electrode oxidation. As a result, the multilayer electronic component 100 may have a decreased capacitance or a decreased insulation resistance. However, according to one embodiment of the present invention, the content of Li contained in the dielectric layer 111 is adjusted to 0.02 mol to 0.36 mol with respect to 100 mol of Ba contained in the dielectric layer, so that the firing temperature of the main body 110 can be set to be 20° C. or more lower than conventionally, and therefore the electrode aggregation, the decrease in electrode connectivity, the decrease in electrode coverage, and the electrode oxidation of the internal electrodes 121 and 122 may be mitigated. Such an effect becomes more prominent when the content of F contained in the dielectric layer 111 is 0.49 mol or more and 0.88 mol or less per 100 mol of Ba contained in the dielectric layer 111.

[0069] In one embodiment, the content of Ni contained in the internal electrodes 121, 122 may be 95 at% or more with respect to the total content of other elements excluding Ni contained in the internal electrodes 121, 122. According to an embodiment of the present invention, the content of Li contained in the dielectric layer 111 is adjusted to 0.02 mol to 0.36 mol with respect to 100 mol of Ba contained in the dielectric layer, so that when the content of Ni contained in the internal electrodes is 95 at% or more with respect to the total content of other elements excluding Ni contained in the internal electrodes, the difference in contraction behavior between the dielectric layer 111 and the internal electrodes 121, 122 can be minimized. Similarly, this effect is more prominent when the content of F contained in the dielectric layer 111 is 0.49 mol to 0.88 mol with respect to 100 mol of Ba contained in the dielectric layer 111, as in one embodiment.

[0070] External electrodes 130 and 140 are disposed on the body 110 .

[0071] The external electrodes 130 , 140 may include a first external electrode 130 in contact with the third surface 3 of the body 110 and a second external electrode 140 in contact with the fourth surface 4 .

[0072] In this embodiment, a structure in which the multilayer electronic component 100 has two external electrodes 130, 140 is described, but the number and shapes of the external electrodes 130, 140 can be changed depending on the shape of the internal electrodes 121, 122 and other purposes.

[0073] Meanwhile, the external electrodes 130 and 140 may be formed using any material having electrical conductivity, such as a metal, and the specific material may be determined in consideration of electrical characteristics, structural stability, etc., and may further have a multi-layer structure.

[0074] For example, the external electrodes 130, 140 may include an electrode layer disposed on the body 110 and a plating layer formed on the electrode layer.

[0075] More specifically, the electrode layer may be a fired electrode containing a conductive metal and glass, or a resin-based electrode containing a conductive metal and resin.

[0076] The electrode layer may be formed by sequentially forming a fired electrode and a resin-based electrode on the main body, and may be formed by transferring a sheet containing a conductive metal onto the main body, or by transferring a sheet containing a conductive metal onto the fired electrode.

[0077] The conductive metal contained in the electrode layer may be a material having excellent electrical conductivity, and is not particularly limited. For example, the conductive metal may be one or more of nickel (Ni), copper (Cu) and alloys thereof, and may preferably be copper (Cu) to improve adhesion to the main body.

[0078] The plating layer serves to improve mounting characteristics. The type of the plating layer is not particularly limited, and may be a plating layer containing at least one of Ni, Sn, Pd, and alloys thereof, and may be formed of a plurality of layers.

[0079] More specifically, the plating layer may be a Ni plating layer or a Sn plating layer, and may be a form in which a Ni plating layer and a Sn plating layer are sequentially formed on an electrode layer, or a form in which a Sn plating layer, a Ni plating layer and a Sn plating layer are sequentially formed. The plating layer may also include a plurality of Ni plating layers and / or a plurality of Sn plating layers.

[0080] Manufacturing method for multilayer electronic components A method for manufacturing the multilayer electronic component 100 according to one embodiment of the present invention will now be described in detail.

[0081] However, it should be noted that the manufacturing method for manufacturing the multilayer electronic component 100 according to the embodiment of the present invention described above is not limited to the manufacturing method described below. Also, content that overlaps with the content described above may be omitted to avoid redundant description.

[0082] A method for producing a multilayer electronic component 100 according to one embodiment of the present invention includes the steps of forming a body including dielectric layers containing Ba and Ti and internal electrodes arranged alternately with the dielectric layers, and forming external electrodes arranged on the body, wherein the dielectric layers further contain Li and F, and the content of Li contained in the dielectric layers is 0.02 mol or more and 0.36 mol or less per 100 mol of Ba contained in the dielectric layers.

[0083] Forming the body 110 A method for manufacturing a multilayer electronic component according to an embodiment of the present invention includes forming a body 110 including dielectric layers containing Ba and Ti, and internal electrodes alternately arranged with the dielectric layers.

[0084] As an example of a method for forming the main body 110 to include a dielectric layer 111 containing Ba and Ti, and internal electrodes 121, 122 arranged alternately with the dielectric layer 111, a conductive paste for the internal electrodes can be printed on one side and the other side of a dielectric green sheet containing a barium titanate-based component.

[0085] The internal electrodes 121 and 122 may be formed by printing a conductive paste for internal electrodes containing at least one of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti) and alloys thereof on a dielectric green sheet, but it is preferable that the conductive paste for internal electrodes contains Ni as a main component in order to minimize the difference in shrinkage behavior with the dielectric layer 111 of the present invention. In this case, containing Ni as a main component may mean that the at% of Ni is the highest among conductive metals other than glass and dispersant that can be contained in the conductive paste for internal electrodes.

[0086] The method for printing the conductive paste for the internal electrodes may be a screen printing method, a gravure printing method, or the like, but the present invention is not limited thereto.

[0087] Forming the external electrodes 130 and 140 After forming the body 110, external electrodes 130 and 140 may be formed on the body 110.

[0088] There is no particular limitation on the method of forming the external electrodes 130 and 140. For example, the electrode layer that can be included in the external electrodes 130 and 140 can be formed by using a method of dipping in a paste containing a conductive metal and glass, or by transferring a sheet containing a conductive metal. Also, the electrode layer can be formed by using a paste containing a conductive metal and a resin, or by using an atomic layer deposition (ALD) method, a molecular layer deposition (MLD) method, a chemical vapor deposition (CVD) method, a sputtering method, or the like.

[0089] In addition, when a plating layer is disposed on the electrode layer, the plating layer can be formed using a method such as electrolytic plating or electroless plating.

[0090] In the following, a method for manufacturing such a multilayer electronic component 100 will be described in which the dielectric layer 111 contains Li and F, and the Li content in the dielectric layer 111 is adjusted to be 0.02 mol or more and 0.36 mol or less per 100 mol of Ba contained in the dielectric layer 111.

[0091] As described above, the dielectric green sheet can contain barium titanate-based materials such as BaTiO3. Examples of barium titanate-based materials include BaTiO3, (Ba 1-x Ca x )TiO3 (0 < x < 1) in which Ca (calcium), Zr (zirconium), etc. are partially solid-solved in BaTiO3, Ba(Ti 1-y Ca y )O3 (0 < y < 1), (Ba 1-x Ca x )(Ti 1-y Zr y )O3 (0 < x < 1, 0 < y < 1), or Ba(Ti 1-y Zr y )O3 (0 < y < 1), etc. can be used. Therefore, after firing the main body 110, the dielectric layer 111 can contain Ba and Ti.

[0092] On the other hand, as in the above-described embodiment, the content of Li or F contained in the dielectric layer 111 can be adjusted according to the amount and form of the additive added to the dielectric ceramic green sheet.

[0093] In one embodiment, the dielectric layer 111 can be formed by adding LiF, preferably by adding LiF in the form of a sol. At this time, when adjusting the amount of LiF added, the content of Li or F that can be contained in the dielectric layer 111 can be adjusted.

[0094] By increasing the content of LiF added to the dielectric layer 111, the shrinkage start temperature of the dielectric layer 111 can be lowered. Specifically, the content of LiF added to the dielectric layer 111 is preferably 0.2 mol or more with respect to 100 mol of the barium titanate-based component of the dielectric layer 111 so that the shrinkage start temperature of the dielectric layer 111 is lowered and the density of the dielectric layer 111 is improved. However, if the content of LiF added to the dielectric layer 111 exceeds 1.8 mol with respect to 100 mol of the barium titanate-based component of the dielectric layer 111, a problem may occur in that it is difficult to form the insulation resistance of the dielectric layer 111 to be sufficiently high because the content of LiF is excessively high. Therefore, the content of LiF added to the dielectric layer 111 is preferably 0.2 mol or more and 1.8 mol or less with respect to 100 mol of the barium titanate-based component of the dielectric layer 111.

[0095] When the content of LiF added to the dielectric layer 111 is 0.2 mol to 1.8 mol with respect to 100 mol of the barium titanate-based component of the dielectric layer 111, the content of Li or F that can be contained in the dielectric layer 111 after firing of the main body 110 can be appropriately adjusted. Specifically, when the content of LiF added to the dielectric layer 111 is 0.2 mol to 1.8 mol with respect to 100 mol of the barium titanate-based component of the dielectric layer 111, the content of Li contained in the dielectric layer 111 after firing can be 0.02 mol to 0.36 mol with respect to 100 mol of Ba contained in the dielectric layer, and when the content of LiF added to the dielectric layer 111 is 0.2 mol to 1.8 mol with respect to 100 mol of the barium titanate-based component of the dielectric layer 111, the content of F contained in the dielectric layer 111 after firing can be 0.49 mol to 0.88 mol with respect to 100 mol of Ba contained in the dielectric layer.

[0096] A step of firing the body may be performed between the step of forming the body and the step of forming the external electrodes, but is not limited thereto, and may be performed after the step of forming the external electrodes 130 and 140. In addition, the firing process is not limited to being performed once, but may be performed multiple times by changing the firing atmosphere.

[0097] In one embodiment, when the firing of the body is performed between the forming of the body and the forming of the external electrodes, the temperature at which the body is fired may be 1080° C. or less.

[0098] LiF, which is a sintering aid added to the dielectric layer 111, has a low melting point of 1000°C or less, and can form a liquid phase in a temperature range lower than the firing temperature (1100 to 1200°C) of the multilayer electronic component, and has a relatively high boiling point of 1600°C or more, so that a small amount of it volatilizes during firing. Therefore, in one embodiment, by adding LiF as a sintering aid to the dielectric layer 111 and adjusting the content, it is possible to lower the firing temperature of the main body 110 to 1080°C or less, and to suppress discoloration and reliability deterioration of the multilayer electronic component.

[0099] There is no need to particularly limit the size of the multilayer electronic component 100. Since the present invention is advantageous for miniaturization and high capacity, it can be applied to the size of small IT products, and since high reliability can be ensured in various environments, it can also be applied to the size of automotive electrical equipment products that require high reliability.

[0100] (Experimental Example 1) Figure 4 is a graph showing the thermodynamic calculation of the behavior of a mixture containing 1 mol each of LiF and H2O as a function of temperature.

[0101] Referring to Figure 4, when LiF and H2O were added at 1 mole each at the same content and reacted, H2O changed from liquid to gas phase as the temperature increased, and LiF underwent a first-order phase transition from solid to liquid near its melting point (845°C) and began to volatilize above 1050°C. However, it was confirmed that the degree of volatilization of LiF was negligible at 1100°C, which is the firing temperature range for multilayer electronic components. In other words, when LiF is added to the dielectric composition to form a dielectric layer, it is expected that the volatilization of LiF, a low-temperature sintering aid, can be minimized even after the firing process.

[0102] (Experimental Example 2) FIG. 5 is a graph showing the shrinkage starting temperature depending on the LiF content of the LiF sample, and FIG. 6 is a graph showing the shrinkage behavior depending on the LiF content and temperature of the LiF sample.

[0103] 5 and 6, it can be seen that as the LiF content increases, the onset of shrinkage and high temperature shrinkage occur at low temperatures, and even with a small amount of LiF added, the shrinkage temperature drops sharply. That is, it can be seen that as the amount of LiF added increases, density improves and grain growth occurs even at low temperatures, and therefore it is expected that sintering at a lower temperature than conventional sintering temperatures is possible.

[0104] (Experimental Example 3) FIG. 7(a) is a graph showing the results of a TG-DTA test according to an embodiment, and FIG. 7(b) is a graph showing the results of a TG-DTA test according to a comparative example.

[0105] Referring to Fig. 7(a), which is the experimental result for a sample to which LiF was added as a sintering aid, about -7.5% volatilization of LiF occurred in the region of 1100 degrees, which is the appropriate firing temperature region for multilayer electronic components, and referring to Fig. 7(b), which is the experimental result for a sample to which Li2CO3 was added as a sintering aid, it can be seen that an explosive mass loss occurred near the melting point of Li2CO3, and that in the region of 1100 degrees, which is the appropriate firing temperature region, there was a mass loss of -55% or more. In other words, when LiF is used as a sintering aid, the degree of volatilization can be reduced compared to when Li2CO3 is used as a sintering aid, and therefore the content of Li and F in the dielectric layer after firing can be maintained high.

[0106] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments and the accompanying drawings, but is limited by the scope of the accompanying claims. Therefore, within the scope of the technical idea of ​​the present invention described in the claims, various substitutions, modifications, and changes are possible by a person having ordinary knowledge in the art, and these also belong to the scope of the present invention.

[0107] In addition, the expression "one embodiment" used in the present invention does not mean the same embodiment, but is provided to emphasize and describe each unique feature that is different from the others. However, the above-mentioned one embodiment does not exclude being realized in combination with the features of another embodiment. For example, even if a matter described in a specific embodiment is not described in another embodiment, it can be understood as a description related to the other embodiment, unless there is a description that is opposite or contradictory to the matter in the other embodiment.

[0108] The terms used in the present invention are merely for the purpose of describing one embodiment and are not intended to limit the present invention. In this case, the singular expression includes the plural expression unless the context clearly indicates otherwise. [Explanation of symbols]

[0109] 100 Multilayer electronic components 110 Main unit 111 Dielectric layer 121, 122 Internal electrode 112, 113 Cover part 114, 115 Margin 130, 140 external electrode

Claims

1. a body including dielectric layers including Ba and Ti and internal electrodes interleaved with the dielectric layers; an external electrode disposed on the body; the dielectric layer further comprises Li and F; A multilayer electronic component, wherein the content of Li contained in the dielectric layer is 0.02 mol or more and 0.36 mol or less per 100 mol of Ba contained in the dielectric layer.

2. 2. The multilayer electronic component according to claim 1, wherein the content of F contained in said dielectric layers is 0.49 mol or more and 0.88 mol or less per 100 mol of Ba contained in said dielectric layers.

3. the dielectric layer includes a plurality of dielectric crystal grains; 2. The multilayer electronic component according to claim 1, wherein an average crystal grain size of the plurality of dielectric crystal grains is 150 nm or more and 250 nm or less.

4. When the area ratio of the region excluding pores in the dielectric layer is defined as density, 2. The multilayer electronic component according to claim 1, wherein the average density of the dielectric layers is 95% or more and 99% or less.

5. 2. The multilayer electronic component according to claim 1, wherein the internal electrodes contain Ni.

6. 2. The multilayer electronic component according to claim 1, wherein the average thickness of said dielectric layers is 0.35 μm or less.

7. 2. The multilayer electronic component according to claim 1, wherein the internal electrodes have an average thickness of 0.35 μm or less.

8. forming a body including dielectric layers including Ba and Ti and internal electrodes interleaved with the dielectric layers; forming an external electrode disposed on the body; the dielectric layer further comprises Li and F; A method for producing a multilayer electronic component, wherein the content of Li contained in the dielectric layer is 0.02 mol or more and 0.36 mol or less per 100 mol of Ba contained in the dielectric layer.

9. 9. The method for producing a multilayer electronic component according to claim 8, wherein the content of F contained in said dielectric layer is 0.49 mol or more and 0.88 mol or less per 100 mol of Ba contained in said dielectric layer.

10. The method for producing a multilayer electronic component according to claim 9 , wherein the dielectric layer is formed by adding LiF.

11. The method for producing a multilayer electronic component according to claim 10, wherein the LiF is added in the form of a sol.

12. Between the step of forming the body and the step of forming the external electrodes, a step of firing the body is performed. The method for producing a multilayer electronic component according to claim 8, wherein the temperature for firing the body is 1080° C. or lower.