Battery insulation sheet, manufacturing method thereof, and battery module comprising the same
The airgel-based battery insulation sheet with a fibrous polymer matrix and dry binder addresses thermal insulation and safety challenges in high-capacity batteries by providing excellent heat resistance, flexibility, and low dust properties, enhancing safety in electric vehicles.
Patent Information
- Application Number
- JP2024065538
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-14
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2044-04-15
AI Technical Summary
Existing battery insulation materials face challenges in providing effective thermal insulation, heat resistance, flexibility, and preventing dust generation, especially in high-capacity lithium secondary batteries used in electric vehicles, where thermal runaway can occur, affecting adjacent cells.
A battery insulation sheet comprising an airgel layer with a fibrous polymer matrix and airgel particles, using a dry binder like polytetrafluoroethylene, is developed to ensure excellent insulation, heat resistance, and flexibility, with a manufacturing process that avoids water-based binders to maintain dispersion and prevent particle detachment.
The insulation sheet achieves enhanced thermal insulation, heat resistance, and flexibility while minimizing dust generation, effectively preventing heat transfer and flame propagation between battery cells, ensuring safety and performance in dynamic environments.
Smart Images

Figure 2024155790000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery insulation sheet, a manufacturing method thereof, and a battery module including the same. [Background technology]
[0002] Secondary batteries are power storage systems that provide excellent energy density by converting electrical energy into chemical energy and storing it. Unlike primary batteries, which cannot be recharged, secondary batteries can be recharged, and are widely used in IT devices such as smartphones, cellular phones, laptops, and tablet PCs. In recent years, interest in electric vehicles has increased to prevent environmental pollution, and high-capacity secondary batteries are being adopted for electric vehicles. Such secondary batteries are required to have characteristics such as high density, high output, and stability.
[0003] On the other hand, when a battery contains a large number of high-capacity cells such as lithium secondary batteries, one cell may overheat for some reason and experience thermal runaway, adversely affecting other adjacent cells, so it is required that adjacent cells are thermally insulated from each other.
[0004] Therefore, conventionally, a plate material or an insulating resin plate is placed between the cells to insulate and heat the adjacent cells.
[0005] The above information disclosed in the Background of the Invention is intended to enhance the understanding of the background of the present invention only, and may therefore include information that does not constitute prior art. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Korean Patent Publication No. 10-2016-0107572 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of one embodiment of the present invention is to provide a battery insulation sheet having at least one or more properties selected from the group consisting of excellent insulation properties, heat resistance, low dust properties, and flexibility, a manufacturing method thereof, and a battery module including the same. [Means for solving the problem]
[0008] One embodiment of the present invention provides a battery insulation sheet including an aerogel layer, the aerogel layer including a fiberized polymer matrix and aerogel particles distributed in the fiberized polymer matrix, the fiberized polymer matrix including a dry binder.
[0009] The dry binder includes a fluorine-based binder, and the fluorine-based binder may be one or more selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexapropylene copolymer, and polyvinylidene fluoride.
[0010] The fiberized polymer matrix may be contained in an amount of 10% by weight to 90% by weight, and the aerogel particles may be contained in an amount of 10% by weight to 90% by weight, based on the total amount of the aerogel layer.
[0011] The aerogel particles have a BET specific surface area of 500m 2 / g or more 1,000m 2 / g or less.
[0012] The average particle size (D50) of the aerogel particles may be 5 μm or more and 100 μm or less.
[0013] The aerogel particles may be dispersed within the fiberized polymer matrix.
[0014] The aerogel layer can satisfy the following formula (1). 0.1≦W FB / TPM ≦18···(1) In the above formula (1), W FB represents the content (wt%) of the dry binder relative to the total amount of the aerogel layer, and T PM represents the average particle size (μm) of the aerogel particles.
[0015] The battery insulation sheet may further include a substrate provided on the upper surface, lower surface, or both surfaces of the aerogel layer.
[0016] The battery insulation sheet may have a structure in which a first substrate, an aerogel layer, and a second substrate are laminated in this order.
[0017] Another embodiment provides a method for producing a battery insulation sheet, the method including: preparing a raw material mixture including a powdered dry binder and powdered aerogel particles; and extruding the raw material mixture using an extruder to prepare an aerogel layer, the aerogel layer including a fiberized polymer matrix having the aerogel particles distributed therein, the fiberized polymer matrix including the fiberized dry binder.
[0018] The step of preparing the raw material mixture may include a first dry mixing step and a second dry mixing step, and the stirring speed in the second dry mixing step may be at least twice as fast as the stirring speed in the first dry mixing step.
[0019] In the first dry mixing step, the temperature may be from 20° C. to 65° C., the stirring speed may be from 2000 rpm to 2000 rpm, and the stirring time may be from 5 minutes to 15 minutes. In the second dry mixing step, the temperature may be from 20° C. to 65° C., the stirring speed may be from 4000 rpm to 10,000 rpm, and the stirring time may be from 10 minutes to 60 minutes.
[0020] In the step of producing the aerogel layer, the raw material mixture can be fed into an extruder and extruded into a sheet shape.
[0021] The step of preparing the aerogel layer may be carried out under conditions of a temperature of 25° C. to 150° C. and a pressure of 1 MPa to 100 MPa.
[0022] The method may further include laminating a substrate on the top surface, bottom surface, or both top and bottom surfaces of the aerogel layer.
[0023] A first substrate and a second substrate can be laminated on the top and bottom surfaces of the aerogel layer, respectively.
[0024] Yet another embodiment provides a battery module including a plurality of cells and battery insulation sheets respectively provided between the plurality of cells, with upper and lower surfaces of the battery insulation sheets being arranged to face adjacent cells, respectively. Effect of the Invention
[0025] The battery insulation sheet according to one embodiment of the present invention includes a fiberized polymer matrix in which aerogel is distributed by a dry process using a dry binder and aerogel having excellent heat resistance, and therefore has excellent insulation properties, heat resistance, low dust properties, and flexibility. [Brief description of the drawings]
[0026] [Figure 1] 1 is a schematic diagram showing a structure of a battery insulation sheet according to an embodiment. FIG. [Diagram 2] FIG. 4 is a schematic diagram showing a structure of a battery insulation sheet according to another embodiment. [Diagram 3] FIG. 4 is a schematic diagram showing the structure of a battery insulation sheet according to still another embodiment. [Figure 4] FIG. 2 is a schematic diagram illustrating a battery insulation sheet formed between a plurality of cells according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Although the present invention will be described in detail below so as to be easily understood by those skilled in the art, the present invention may be embodied in various different forms and should not be construed as being limited to the embodiments set forth herein.
[0028] Insulation materials are materials that prevent the flow of heat from a high temperature area to a low temperature area, and are used in refrigerators, freezer warehouses, and buildings as well as in various industrial fields including the aircraft, electronic parts, and automotive industries.
[0029] Such a heat insulating material should have excellent heat insulating performance due to low thermal conductivity, and is also required to have sufficient mechanical strength to maintain such heat insulating performance.
[0030] Meanwhile, aerogel is a transparent or translucent cutting-edge material with a nanoporous structure, and has very low density and low thermal conductivity. As such, it not only has great potential as an insulating material, but is also considered a highly efficient super-insulating material that can be used in a variety of industrial fields.
[0031] Furthermore, the greatest advantage of aerogel is that it exhibits lower thermal conductivity than conventional organic insulation materials such as styrofoam, and that it solves the fatal weaknesses of organic insulation materials, namely, vulnerability to fire and the generation of harmful gases during a fire.
[0032] A battery insulation sheet according to an embodiment is a battery insulation sheet including an aerogel layer, the aerogel layer including a fiberized polymer matrix and aerogel particles distributed in the fiberized polymer matrix, the fiberized polymer matrix may include a dry binder.
[0033] The battery insulation sheet formed in the above structure can contain a high content of a heat-resistant dry binder, and therefore has improved heat resistance as well as insulation properties. Since the dry binder is present in a fiberized polymer matrix structure and aerogel particles are dispersed inside the fiberized polymer matrix, the battery insulation sheet can have excellent flexibility and low dust properties by preventing the aerogel particles from falling off.
[0034] In particular, although dry binders generally have excellent heat resistance, they have the limitation that they are relatively difficult to disperse in water. However, the battery insulation sheet according to an embodiment of the present invention can contain a high content of dry binder without being affected by its dispersibility through a dry process, and can be easily contained in the insulation sheet, thereby exhibiting better heat resistance. As a result, the insulation sheet can achieve the desired heat resistance with a relatively thin thickness, and the phenomenon of aerogel particles detaching can be reduced.
[0035] In one embodiment, the fiberized polymer matrix may not include a water-based binder, where the water-based binder may mean a common water-soluble binder, and may include, for example, an inorganic binder, a water-based polymer, an anionic water-soluble polymer, a cationic water-soluble polymer, and a water-dispersible polymer.
[0036] Specifically, the fiberized polymer matrix is produced by a dry process and does not need to contain an aqueous binder. By not containing an aqueous binder, it is possible to form an aerogel layer having a structure in which the aerogel is dispersed in the fiberized polymer matrix by extrusion in a dry process.
[0037] In this connection, the inorganic binder may include soluble silicates, and may be understood to mean, for example, common water-based polymers such as sodium silicate, potassium silicate, and lithium silicate.
[0038] The water-soluble polymer may refer to a typical water-soluble polymer such as polyvinyl alcohol, polyethylene oxide, polyacrylamide, and polyvinylpyrrolidone.
[0039] The anionic water-soluble polymer can refer to a typical anionic water-soluble polymer, such as a polymer having functional groups of carboxylic acid, sulfonic acid, sulfate, phosphate, and salts thereof.
[0040] The cationic water-soluble polymer may include at least one selected from the group consisting of polymers having functional groups of amine, ammonium, phosphonium, sulfonium, and salts thereof. For example, the cationic water-soluble polymer may be a polymer having an amine group, and specific examples thereof may be understood to mean ordinary cationic water-soluble polymers such as polyethylene amine and polyamine.
[0041] The water-dispersible polymer may be understood to mean a conventional water-dispersible polymer such as a water-dispersible polyurethane and a water-dispersible polyester.
[0042] The dry binder may be, for example, a fibrillized binder. In particular, the dry binder may be understood to mean a binder that can be fibrillized or that can be fibrillated to form a matrix.
[0043] The dry binder can refer to a binder that is not impregnated, dissolved, or dispersed in a solvent. The dry binder is a fiberized binder and can act as a matrix that supports and binds the aerogel. The aspect ratio of the dry binder can be 10 or more, 20 or more, 50 or more, or 100 or more.
[0044] The dry binder may include, for example, one or more selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexapropylene (PVDF-HFP) copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, cellulose, polyvinylpyrrolidone, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), and fluororubber, or may include a copolymer of two or more selected therefrom, but is not limited thereto.
[0045] As a specific example, the dry binder may include a fluorine-based binder. The fluorine-based binder may include, for example, one or more selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexapropylene (PVDF-HFP) copolymer, and polyvinylidene fluoride (PVDF). By including the dry binder, fiberization is possible by a dry process. Specifically, in the dry process, a raw material mixture is extruded using an extruder to produce an aerogel layer, and here, when a water-based binder is included, fiberization of the binder may be difficult.
[0046] In one embodiment, the aerogel particles have a BET specific surface area of 500 m 2 / g or more 1,000m 2 For example, the aerogel particles may have a BET specific surface area of 500 m 2 / g or more 950m 2 / g or less, 550m 2 / g or more 950m 2 / g or less, or 600m 2 / g or more 900m 2 By including aerogel particles having a BET specific surface area value within this range, heat transfer and heat propagation between multiple cells can be effectively prevented, and the heat insulating property of the battery insulation sheet can be improved.
[0047] The average particle size (D50) of the aerogel may be 5 μm to 100 μm, 10 μm to 100 μm, or 50 μm to 100 μm. By including aerogel particles having a particle size within this range, it is possible to improve the heat insulation while preventing the aerogel particles from agglomerating and the thickness of the heat insulating sheet from becoming too thick, and to retard heat transfer between a plurality of cells.
[0048] The average particle size (D50) can be measured, for example, by a laser diffraction method or a scanning electron microscope (SEM), and the average particle size (D50) of particles can be defined as the particle size at 50% of the particle size distribution (the particle size corresponding to 50% of the cumulative volume of the particle size distribution).
[0049] The aerogel particles may be dispersed inside the fiberized polymer matrix. Specifically, when the aerogel layer is formed by the manufacturing method described later, the aerogel layer may be formed in a structure in which the aerogel particles are uniformly dispersed inside the fiberized polymer matrix.
[0050] In one embodiment, the fiberized polymer matrix may be present in an amount of 10% by weight to 90% by weight, and the aerogel particles may be present in an amount of 10% by weight to 90% by weight, based on the total weight of the aerogel layer.
[0051] Specifically, the fiberized polymer matrix may be contained in an amount of 20% by weight to 90% by weight, 20% by weight to 75% by weight, or 20% by weight to 65% by weight, based on the total amount of the aerogel layer, and the aerogel particles may be contained in an amount of 10% by weight to 80% by weight, 25% by weight to 80% by weight, or 35% by weight to 80% by weight. By controlling the content of the fiberized polymer matrix and the aerogel particles in the aerogel layer within the range, a battery insulation sheet having excellent heat insulation, heat resistance, flexibility, and low dust properties can be provided.
[0052] In one embodiment, the content of the dry binder may be adjusted according to the size of the aerogel particles. Specifically, the aerogel layer may satisfy the following formula (1): 0.1≦W FB / T PM ≦18···(1) In the above formula (1), W FB represents the content of dry binder (wt%) relative to the total amount of the aerogel layer, and T PM represents the average particle size (μm) of the aerogel particles.
[0053] Specifically, W FB / T PM The value may be 0.1 to 18, 0.1 to 10, 0.1 to 5, or 0.2 to 1.3. FB / T PM The value can indicate the relationship between the average particle size of the aerogel particles and the content of the dry binder that can be contained in the aerogel layer. For example, the larger the size of the aerogel particles, the more difficult it is to pack the dry binder into the fiberized matrix, and the smaller the size of the aerogel particles, the larger the specific surface area becomes, requiring an excessive amount of binder, which may result in a deterioration in the insulating properties of the insulating sheet. Therefore, the aerogel particle size affects the content of the dry binder that can be contained. Therefore, W FB / T PM By adjusting the value within the above range, it is possible to provide a battery insulation sheet having excellent heat insulation, heat resistance, flexibility, and low dust properties despite its thin thickness.
[0054] The aerogel layer has a structure in which aerogel particles are uniformly distributed inside a polymer matrix fiberized by a manufacturing method described later, and since the aerogel layer does not have many vacant spaces inside, it can have excellent heat resistance even when formed to a thin thickness because it can contain a high content of dry binder having excellent heat insulation and heat resistance. In addition, the aerogel particles are uniformly distributed inside the fiberized polymer matrix, and dust generation due to detachment of the aerogel particles can be prevented. In addition, while the vacant spaces inside the aerogel layer function to absorb vibrations and impacts, they also cause an increase in the thickness of the insulation sheet. However, the battery insulation sheet according to an embodiment can be used as an insulation sheet for various types of batteries because the aerogel layer can realize excellent flexibility due to the fiberized polymer matrix even if the vacant spaces inside are not many. In particular, even when the battery is applied to an environment in which it moves without being fixed during operation, such as an electric vehicle, detachment of the aerogel particles can be prevented.
[0055] The thickness of the aerogel layer may be 1 mm to 10 mm, 1 mm to 5 mm, or 1 mm to 3 mm. By forming an aerogel layer on a substrate having a thickness within the range, a heat insulating sheet having excellent heat insulating properties, heat resistance, flexibility, and low dust properties at a thin thickness can be produced.
[0056] In one embodiment, the battery insulation sheet may further include a substrate provided on the upper surface, the lower surface, or both upper and lower surfaces of the aerogel layer.
[0057] As an example, FIG. 1 is a schematic diagram showing the structure of a battery insulation sheet according to one embodiment.
[0058] Referring to FIG. 1, a battery insulation sheet 100 includes an aerogel layer 110, where the upper and lower surfaces of the aerogel layer 110 may be disposed to face adjacent cells, respectively.
[0059] As another example, FIG. 2 is a schematic diagram showing the structure of a battery insulation sheet according to an embodiment.
[0060] Referring to FIG. 2, the battery insulation sheet 100 includes a substrate 120 and an aerogel layer 110 formed on the substrate 120, where the upper surface of the battery insulation sheet, for example the upper surface of the aerogel layer 110 and the lower surface of the substrate 120, may be disposed to face the adjacent cells, respectively.
[0061] As yet another example, FIG. 3 is a schematic diagram showing the structure of a battery insulation sheet according to an embodiment.
[0062] Referring to FIG. 3, in one embodiment, the battery insulation sheet 100 may have a structure including a first substrate 130, an aerogel layer 110 formed on the first substrate 130, and a second substrate 140 formed on the aerogel layer 110. Specifically, the battery insulation sheet may have a structure in which the first substrate 130, the aerogel layer 110, and the second substrate 140 are sequentially laminated. Here, the first substrate 130 and the second substrate 140 may be disposed to face the adjacent cell, respectively. The first substrate 130 and the second substrate 140 may be formed of the same or different materials.
[0063] The substrate may include a resin, a metal, an inorganic material other than a metal, or a composite of these, and the type is not limited. The form of the substrate is not particularly limited, and may be a film, a thin film, a sheet, etc. Here, the substrate may refer to the substrate 120 in FIG. 2, the first substrate 130 in FIG. 2, and the second substrate 140.
[0064] The resin may include, for example, one or more selected from the group consisting of polyethylene, polypropylene, polystyrene, polyethylene terephthalate, and polyamide.
[0065] The metal may include, for example, one or more selected from the group consisting of copper, nickel, cobalt, iron, chromium, vanadium, palladium, ruthenium, rhodium, molybdenum, tungsten, iridium, silver, gold, and platinum. When using a substrate made of a metal material, the substrate may be subjected to anti-corrosion treatment, insulation treatment, etc., as necessary.
[0066] The inorganic material may include one or more selected from the group consisting of calcium carbonate (CaCO3), talc, and mica.
[0067] As a specific example, the substrate may include an inorganic material, and more specifically, may include mica, in which case the thermal insulation properties and durability of the heat insulating sheet can be improved.
[0068] The thickness of the substrate may be 0.01 mm or more and 5 mm or less, 0.05 mm or more and 3 mm or less, or 0.1 mm or more and 1 mm or less. By including a substrate having a thickness within the range, the durability of the battery insulation sheet can be improved.
[0069] According to an embodiment, a method for manufacturing a battery insulation sheet includes: preparing a raw material mixture including a powdered dry binder and powdered aerogel particles; and extruding the raw material mixture using an extruder to prepare an aerogel layer. The aerogel layer may include a fiberized polymer matrix having the aerogel particles distributed therein, and the fiberized polymer matrix may include the dry binder.
[0070] In the method for producing the battery insulation sheet, all steps may be performed by a dry process, and the specific description of the components of the aerogel layer may be as described above.
[0071] In the step of preparing a raw material mixture containing a powdered dry binder and powdered aerogel particles, the specific description of the dry binder and the aerogel particles may be as described above.
[0072] In the step of preparing the raw material mixture, the dry binder and the aerogel particles may be mixed in a powder form without containing a solvent.
[0073] The step of preparing the raw material mixture may be carried out by a first or second or more mixing steps. Specifically, the step of preparing the raw material mixture includes a first dry mixing step and a second dry mixing step, and the stirring speed in the second dry mixing step may be 2 times or more, 2 times or more and 8 times or less, or 4 times or more and 6 times or less than the stirring speed in the first dry mixing step.
[0074] In the primary dry mixing stage, the temperature may be from 20° C. to 65° C., from 25° C. to 50° C., or from 25° C. to 35° C., the stirring speed may be from 2000 rpm to 2000 rpm, from 500 rpm to 1800 rpm, or from 800 rpm to 1300 rpm, and the stirring time may be from 5 minutes to 15 minutes.
[0075] In the secondary dry mixing step, the temperature may be from 20° C. to 65° C., from 25° C. to 50° C., or from 25° C. to 35° C., the stirring speed may be from 4000 rpm to 10,000 rpm, from 4000 rpm to 8000 rpm, or from 4000 rpm to 6000 rpm, and the stirring time may be from 10 minutes to 60 minutes, from 10 minutes to 40 minutes, or from 20 minutes to 30 minutes.
[0076] By extruding the raw material mixture that has been through the first and second dry mixing steps under the above conditions, an aerogel layer can be formed in which aerogel particles are distributed inside a fiberized polymer matrix.
[0077] In the step of preparing the raw material mixture, a stirrer can be used for stirring. The stirrer may include, for example, a kneader. The stirrer may have a structure including, for example, a chamber, one or more rotating shafts arranged inside the chamber and rotating, and a blade rotatably coupled to the rotating shaft and arranged in the longitudinal direction of the rotating shaft. The blade may include, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. By including the blade, the aerogel and the dry binder can be effectively mixed without a solvent to prepare a dough-like raw material mixture.
[0078] When the raw material mixture is produced, the dry binder may be contained in an amount of 20% by weight to 70% by weight, 30% by weight to 60% by weight, or 40% by weight to 60% by weight, and the aerogel particles may be contained in an amount of 30% by weight to 80% by weight, 40% by weight to 70% by weight, or 40% by weight to 60% by weight, based on the total amount of the raw material mixture. When the raw material mixture is produced within these ranges, an aerogel layer having excellent heat insulation, heat resistance, flexibility, and low dust properties can be produced.
[0079] In one embodiment, the step of producing the aerogel layer may be to feed a raw material mixture into an extruder and extrude it into a sheet.
[0080] The step of producing the aerogel layer can be carried out at a temperature of 25° C. to 150° C., 30° C. to 100° C., or 30° C. to 70° C. In addition, in the step of producing the aerogel layer, the pressure during extrusion can be 1 MPa to 100 MPa, 20 MPa to 80 MPa, or 30 MPa to 70 MPa. By extruding the raw material mixture under such conditions, an aerogel layer having a structure in which the aerogel is uniformly distributed in the dry binder can be formed.
[0081] The method for manufacturing a battery insulation sheet according to an embodiment is performed by a dry process and does not include a process solvent, so that there is an advantage that an additional process for removing residual solvent is not required.
[0082] In one embodiment, when the raw material mixture is extruded from the extruder in the step of producing the aerogel layer, the temperature may be 20° C. to 90° C., 30° C. to 60° C., or 35° C. to 55° C. The pressure during the extrusion may be 30 MPa to 70 MPa, 40 MPa to 65 MPa, or 40 MPa to 60 MPa. By extruding the raw material mixture under conditions within the range, an aerogel layer including a fiberized polymer matrix in which aerogel is dispersed can be produced.
[0083] The extruder used may be a common extruder without any particular limitation, and for example, a single screw extruder or a twin screw extruder may be used.
[0084] In one embodiment, the method may further include laminating a substrate on the upper surface, the lower surface, or both surfaces of the aerogel layer. As one example, a battery insulation sheet may be manufactured by laminating the aerogel layer on the substrate, and as another example, a first substrate and a second substrate may be laminated on the upper and lower surfaces of the aerogel layer, respectively, to manufacture a battery insulation sheet. Here, the specific description of the substrate, the first substrate, and the second substrate may be as described above.
[0085] The step of laminating the substrate can be performed by laminating the substrate on the upper surface, lower surface, or upper and lower surfaces of the aerogel layer using an adhesive. Specifically, the step of laminating the substrate can be performed by coating an adhesive layer on the upper surface, lower surface, or upper and lower surfaces of the aerogel layer using a conventional adhesive, and laminating the substrate on the adhesive layer.
[0086] A battery module according to an embodiment may include a plurality of cells and battery insulation sheets respectively provided between the plurality of cells, and upper and lower surfaces of the battery insulation sheets may be disposed to face adjacent cells, respectively.
[0087] FIG. 4 is a schematic diagram showing a battery insulation sheet according to an embodiment formed between a plurality of cells.
[0088] Referring to FIG. 4, the battery insulation sheet 100 according to an embodiment may be formed between each of the cells 200 in a battery module including a plurality of cells 200. Here, the battery insulation sheet 100 may include an upper surface, a lower surface, and an edge side between the upper surface and the lower surface, and the upper and lower surfaces of the battery insulation sheet 100, i.e., the upper and lower surfaces, may be arranged to face each of the adjacent cells 200. For example, the upper and lower surfaces of the aerogel layer 110 in FIG. 1 described above may be arranged to face each of the cells 200 formed on the left and right in FIG. 4. As another example, the upper surface of the aerogel layer 110 and the lower surface of the substrate 120 in FIG. 2 described above may be arranged to face each of the cells 200 formed on the left and right in FIG. 4. As yet another example, the lower surface of the first substrate 130 and the upper surface of the second substrate 140 in FIG. 3 described above may be arranged to face each of the cells 200 formed on the left and right in FIG. 4. By forming the battery insulation sheet 100 according to the above embodiment between each of the multiple cells 200, it is possible to provide a battery module and a battery pack including the same, which can prevent the flame from spreading to other cells by blocking the flame first inside the cell. EXAMPLES
[0089] Specific examples of the present invention will be presented below. However, the examples described below are merely for the purpose of specifically illustrating or explaining the present invention, and the present invention should not be limited thereto. Furthermore, since the contents not described here can be sufficiently inferred by a person skilled in the art, the description thereof will be omitted.
[0090] (Battery insulation sheet manufacturing) Example 1 1. Raw material mixture production Powdered polytetrafluoroethylene and aerogel particles (D50 50μm) were mixed as a dry binder to prepare a raw material mixture. The raw material mixture was first dry mixed at 25°C and a stirring speed of 1000 rpm for 10 minutes to prepare a first mixture. The first mixture was then further mixed at 25°C and a stirring speed of 5000 rpm for 20 minutes to prepare a second mixture.
[0091] Here, the content of polytetrafluoroethylene was 50% by weight, and the content of aerogel particles was 50% by weight, based on the total amount of the raw material mixture.
[0092] 2. Aerogel Layer Fabrication The prepared second mixture was put into an extruder and extruded under a temperature condition of 45°C and a pressure condition of 50 MPa to form an aerogel layer in which aerogel particles are distributed inside a fiberized polytetrafluoroethylene matrix. Here, the thickness of the aerogel layer was confirmed to be 2 mm.
[0093] 3. Battery insulation sheet manufacturing A 0.1 mm thick mica sheet (Famica, Muscovite) was laminated on the top and bottom of the aerogel layer using an adhesive coating method to produce a battery insulation sheet.
[0094] Example 2 The same procedure as in Example 1 was repeated, except that the raw material mixture was changed to a composition of 20% by weight of polytetrafluoroethylene and 80% by weight of aerogel particles.
[0095] Example 3 The same procedure as in Example 1 was repeated, except that the raw material mixture was changed to a composition of 35% by weight of polytetrafluoroethylene and 65% by weight of aerogel particles.
[0096] Example 4 The same procedure as in Example 1 was repeated, except that the raw material mixture was changed to a composition of 65% by weight of polytetrafluoroethylene and 35% by weight of aerogel particles.
[0097] Example 5 The same procedure as in Example 1 was carried out, except that aerogel particles having an average particle size (D50) of 5 μm were used and the raw material mixture was made to have a composition of 80% by weight of polytetrafluoroethylene and 20% by weight of aerogel particles.
[0098] Example 6 The same procedure as in Example 1 was carried out, except that aerogel particles having an average particle size (D50) of 100 μm were used.
[0099] Comparative Example 1 1. Aerogel Composition Preparation An aerogel composition was prepared by adding polyvinyl alcohol (Sigma Aldrich, Poly(vinyl alcohol)) as an aqueous binder, polytetrafluoroethylene as a dry binder, and aerogel particles to an ultrapure water solvent and mixing them.
[0100] The solids content of the aerogel composition was determined to be 85% aerogel, 10% polyvinyl alcohol, and 5% polytetrafluoroethylene by weight.
[0101] 2. Battery insulation sheet manufacturing The aerogel composition was applied as a slurry onto a 0.1 mm-thick mica sheet (Famica, Muscovite), and then a 0.1 mm-thick mica sheet was laminated in a sandwich type and coated by a roll rolling method.Then, the aerogel layer was formed by drying, and a battery insulation sheet was manufactured.
[0102] Comparative Example 2 The aerogel composition was produced in the same manner as in Comparative Example 1, except that the amount of raw materials added was adjusted during the production of the aerogel composition in Comparative Example 1 to produce an aerogel composition with a solid content of 50% by weight of aerogel and 50% by weight of polytetrafluoroethylene. In this case, it was difficult to disperse polytetrafluoroethylene, so a battery insulation sheet could not be produced.
[0103] Comparative Example 3 In Comparative Example 1, the amount of raw materials added was adjusted during the preparation of the aerogel composition, and an aerogel composition having a solid content of 85% by weight of aerogel, 5% by weight of polyvinyl alcohol, and 10% by weight of polytetrafluoroethylene was prepared by the same method as in Comparative Example 1. In this case, it was also difficult to disperse polytetrafluoroethylene, and a battery insulation sheet could not be produced.
[0104] (Experimental Example) Experimental example 1: Thermal insulation evaluation The battery insulation sheets manufactured in Examples 1 to 6 and Comparative Examples 1 to 3 were used to evaluate the insulation properties in the following manner, and the results are shown in Table 1 below.
[0105] Thermal conductivity at room temperature (23±5℃) (mW / mK): The insulation sheet was cut into pieces with a width of 125mm~150mm and a width of 125mm~150mm to prepare test pieces, and the thermal conductivity at room temperature (23±5℃) was measured using a NETZSCH HFM436 Lambda instrument. The lower the thermal conductivity at room temperature, the better the insulation of the insulation sheet.
[0106] Experimental example 2: Dustiness evaluation The battery insulation sheets manufactured in Examples 1 to 6 and Comparative Examples 1 to 3 were evaluated for dust resistance in the following manner, and the results are shown in Table 1 below.
[0107] Dust resistance test: Using a vibration tester (ASTMC592-04), the weight loss rate due to vibration was measured under vibration conditions of 24Hz / 3mm for 6hr. - Sample preparation: 12 x 12 inch insulation sheet preparation - Weight reduction rate [%] = [(Weight of insulation sheet before evaluation) - (Weight of insulation sheet after evaluation)] / (Weight of insulation sheet before evaluation) x 100
[0108] Experimental example 3: Flexibility evaluation The battery insulation sheets manufactured in Examples 1 to 6 and Comparative Examples 1 to 3 were used to evaluate the flexural modulus, and the results are shown in Table 1 below.
[0109] Flexural modulus (Mpa): Each heat insulating sheet was manufactured as a test piece based on the ASTM D790 standard, and measured using MTDI UTM (UT-005E). Specifically, the manufactured test piece was placed on a support table, and a force was applied to the center of the test piece at a speed of 1 mm / min to 10 mm / min by a three-point bending analysis method, the load was recorded, and the initial gradient value was measured by dividing this by 15% strain, and the flexural modulus at 15% strain was measured. The lower the flexural modulus, the more flexible the heat insulating sheet is.
[0110] [Table 1]
[0111] From Table 1 above, it was confirmed that the examples have excellent heat insulation, dust resistance, and flexibility. In addition, it is expected that the examples have excellent heat resistance because they contain a high content of binder with excellent heat resistance.
[0112] Here, it was confirmed from Examples 1 to 6 that the changes in heat insulation, dust resistance, and flexibility due to the content of aerogel particles and polytetrafluoroethylene were observed. Specifically, it was confirmed that better physical property measurement results were obtained when the average particle size of the aerogel particles was 50 μm or more and 100 μm or less, and the content of polytetrafluoroethylene was 20% by weight or more and 65% by weight or less.
[0113] On the other hand, it was confirmed from Comparative Example 1 that when the aerogel layer was formed by a wet process using a solvent, the heat insulation was at a similar level, and flexibility and dust resistance were also reduced, despite the high content of aerogel particles compared to Example 2. In addition, as can be confirmed from Comparative Examples 1 to 3, when the aerogel layer was manufactured by a wet process, the polytetrafluoroethylene could only be contained at a maximum of 5 wt %, and when it exceeds this, it is difficult to form the aerogel layer due to dispersibility problems. It was also confirmed that when the aerogel layer was formed by a wet process, it was difficult to manufacture a battery insulation sheet with a thin thickness as in the Examples.
[0114] Therefore, it was confirmed that the aerogel composition according to one embodiment has excellent heat insulation, heat resistance, flexibility, and low dust properties.
[0115] Although the above describes preferred embodiments of the present invention, the present invention is not limited thereto, and can be embodied in various modified forms within the scope of the claims, the detailed description of the invention, and the accompanying drawings, which of course also fall within the scope of the present invention. [Explanation of symbols]
[0116] 100 Battery insulation sheet 110 Aerogel layer 120 Base material 130 1st base material 140 Second base material 200 cells
Claims
1. A battery insulation sheet including an aerogel layer, The aerogel layer includes a fiberized polymer matrix and aerogel particles distributed in the fiberized polymer matrix; The fiberized polymer matrix includes a dry binder.
2. 2. The battery insulation sheet according to claim 1, wherein the dry binder includes a fluorine-based binder, and the fluorine-based binder is at least one selected from the group consisting of polytetrafluoroethylene, polyvinylidene fluoride-hexapropylene copolymer, and polyvinylidene fluoride.
3. 2. The battery insulation sheet according to claim 1, wherein the fiberized polymer matrix is contained in an amount of 10% by weight to 90% by weight, and the aerogel particles are contained in an amount of 10% by weight to 90% by weight, based on the total amount of the aerogel layer.
4. The aerogel particles have a BET specific surface area of 500 m 2 / g or more 1,000m 2 The battery insulating sheet according to claim 1, wherein the elastic modulus is 0.05 to 0.15 μm.
5. The battery insulating sheet according to claim 1 , wherein the aerogel particles have an average particle size (D50) of 5 μm or more and 100 μm or less.
6. The battery insulation sheet according to claim 1 , wherein the aerogel particles are dispersed within the fiberized polymer matrix.
7. The battery insulation sheet according to claim 1 , wherein the aerogel layer satisfies the following formula (1): 0.1≦W FB / T PM ≦18・・・(1) In the above formula (1), W FB represents the content (wt%) of the dry binder relative to the total amount of the aerogel layer, T PM represents the average particle size (μm) of the aerogel particles.
8. The battery insulation sheet according to claim 1 , further comprising a substrate provided on the upper surface, the lower surface, or both surfaces of the aerogel layer.
9. The battery insulation sheet according to claim 8 , wherein the battery insulation sheet has a structure in which a first substrate, the aerogel layer, and a second substrate are sequentially laminated.
10. preparing a raw mix comprising a powdered dry binder and powdered aerogel particles; and extruding the raw material mixture using an extruder to produce an aerogel layer. the aerogel layer comprises a fiberized polymer matrix having aerogel particles distributed therein; The fiberized polymer matrix includes a dry binder.
11. The method of claim 10, wherein the step of preparing the raw material mixture is performed by one or more dry mixing steps.
12. 11. The method of claim 10, wherein the step of preparing the raw material mixture includes a first dry mixing step and a second dry mixing step, and a stirring speed in the second dry mixing step is at least twice as fast as a stirring speed in the first dry mixing step.
13. In the first dry mixing step, the temperature is 20° C. or more and 65° C. or less, the stirring speed is 2000 rpm or less, and the stirring time is 5 minutes or more and 15 minutes or less; 13. The method of claim 12, wherein in the second dry mixing, the temperature is 20° C. to 65° C., the stirring speed is 4,000 rpm to 10,000 rpm, and the stirring time is 10 minutes to 60 minutes.
14. The method for manufacturing a battery insulation sheet according to claim 10, wherein in the step of manufacturing the aerogel layer, the raw material mixture is fed into the extruder and extruded into a sheet shape.
15. The method of claim 10, wherein the aerogel layer is formed at a temperature of 25° C. to 150° C. and a pressure of 1 MPa to 100 MPa.
16. The method for manufacturing a battery insulation sheet according to claim 10, further comprising laminating a substrate on the upper surface, the lower surface, or both surfaces of the aerogel layer.
17. The method for manufacturing a battery insulation sheet according to claim 10, further comprising laminating a first substrate and a second substrate on upper and lower surfaces of the aerogel layer, respectively.
18. A plurality of cells; and a battery insulating sheet according to any one of claims 1 to 9 provided between each of the plurality of cells; The upper and lower surfaces of the battery insulation sheet are arranged to face adjacent cells, respectively.
Citation Information
Patent Citations
Aerogel / PTFE composite insulating material
JP2007510794A
Insulating material for battery pack and battery pack
JP2021144879A
Electrode, lithium battery including the same, and manufacturing method therefore
JP2022137005A
Articles useful in the circular economy and comprising silicone elastomers having releasable and cleanly releasable properties
JP2023512060A
High temperature insulative composites and articles thereof
WO2022261579A1