LCP resin composition for circuit board, and LCP film for circuit board
By forming an LCP film with controlled linear expansion using a specific resin composition and pressurization, the film achieves improved mechanical and thermal properties with enhanced adhesion to metal foils, addressing the limitations of existing LCP resin compositions.
Patent Information
- Application Number
- JP2024140570
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-11-20
AI Technical Summary
Existing LCP resin compositions for circuit boards, particularly those used in flexible printed circuit boards (FPCs) and millimeter wave radars, lack sufficient mechanical strength, dimensional stability, and adhesion to metal foils while maintaining high frequency properties and heat resistance.
A composition of liquid crystal polyester, oxazoline group-containing polymer, and optionally polyarylate is melt-extruded and pressurized to form an LCP film with controlled linear expansion coefficients, enhancing dimensional stability and adhesion to metal foils.
The LCP film achieves reduced linear expansion, improved adhesion to metal foils, and maintains excellent mechanical, electrical, and thermal properties, enhancing productivity and economic efficiency.
Smart Images

Figure 2024155964000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an LCP resin composition for circuit boards, an LCP film for circuit boards, and a method for producing the same. [Background technology]
[0002] Liquid crystal polymers (LCPs) are polymers that exhibit liquid crystallinity in a molten state or in a solution state. In particular, thermotropic liquid crystal polymers that exhibit liquid crystallinity in a molten state have excellent properties such as high gas barrier properties, high film strength, high heat resistance, high insulation, and low water absorption, and therefore are being rapidly put to practical use in gas barrier film materials, electronic materials, and electrical insulating materials.
[0003] As a resin composition using a liquid crystal polymer, for example, Patent Document 1 discloses a liquid crystal polyester resin composition consisting of (A) a liquid crystal polyester and (B) an oxazolyl group-containing polymer, in which the ratio of component (A) to component (B) is 99.9 to 0.1% by weight for component (A) and 0.1 to 99.9% by weight for component (B).
[0004] Furthermore, as a resin composition using a liquid crystal polymer, for example, Patent Document 2 discloses a polymer alloy characterized by comprising 97.1 to 99.0% by weight of a thermoplastic polymer capable of forming an optically anisotropic molten phase and 1.0 to 2.9% by weight (based on the total amount of polymers) of an amorphous polymer.
[0005] On the other hand, for example, Patent Document 3 discloses a liquid crystal polymer blend film formed from a blend of a liquid crystal polymer and at least one thermoplastic resin selected from polyethersulfone, polyetherimide, polyamideimide, polyetheretherketone, polyarylate, and polyphenylene sulfide, the ratio of the thermoplastic resin in the blend being 25 to 55% by weight, the linear expansion coefficient of the film in both MD and TD being 5 to 25 ppm / K, and the linear expansion coefficient in the thickness direction of the film not exceeding 270 ppm / K. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 09-286903 [Patent Document 2] JP 2000-290512 A [Patent Document 3] JP 2004-175995 A Summary of the Invention [Problem to be solved by the invention]
[0007] Liquid crystal polymers, especially LCP resin compositions using liquid crystal polyesters, have been attracting attention in recent years as insulating materials for circuit boards such as flexible printed circuit boards (FPCs), flexible printed circuit board laminates, and fiber-reinforced flexible laminates in the upcoming fifth-generation mobile communication systems (5G) and millimeter-wave radars due to their excellent high-frequency characteristics and low dielectric properties.
[0008] However, Patent Document 1 focuses on the gas barrier properties and mechanical strength of the LCP resin composition and only considers applications to gas barrier molded products, containers, tubes, meat, fibers, coating materials, electronic material packaging films, and the like, but does not consider at all applications as insulating materials for flexible printed circuit boards (FPCs) and the like.
[0009] Furthermore, although Patent Document 2 mentions the usefulness of the LCP resin composition as an electrical insulating material or an electrical circuit board material, in reality, it merely proposes improvements to improve the mechanical strength of the LCP film (edge tear strength, i.e., strength against chipping or tearing that occurs at the edges of the film, etc.).
[0010] On the other hand, in Patent Document 3, a resin composition of a liquid crystal polymer and a specific thermoplastic resin is melt-extruded through a T-die to obtain an LCP blend film, which is then biaxially stretched to obtain a liquid crystal polymer blend film that has no anisotropy in the linear expansion coefficient in the plane directions (TD direction and MD direction) and a small linear expansion coefficient in the thickness direction. However, since the obtained liquid crystal polymer blend film contains a large amount of a thermoplastic resin such as polyarylate, the heat resistance, dielectric properties, tensile strength, etc. are reduced, and the practical use is poor.
[0011] The present invention has been made in view of the above problems. An object of the present invention is to provide an LCP resin composition for circuit boards, which can realize an LCP film for circuit boards having a small linear expansion coefficient and excellent dimensional stability without excessively impairing the excellent basic properties of liquid crystal polyester, such as mechanical properties, electrical properties, and heat resistance.
[0012] Another object of the present invention is to provide an LCP film for circuit boards, which has a small linear expansion coefficient and excellent dimensional stability without excessively impairing the excellent basic properties of liquid crystal polyester, such as mechanical properties, electrical properties, and heat resistance, and a method for producing the same. [Means for solving the problem]
[0013] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have found that by using a specific LCP resin composition and by subjecting an LCP film obtained by melt-extruding this specific LCP resin composition to a pressure-heat treatment, the linear expansion coefficient can be reduced, thereby improving dimensional stability and also improving adhesion to metal foil. These findings have led to the completion of the present invention, which has solved the above-mentioned problems.
[0014] That is, the present invention provides various specific embodiments as shown below. (1) A method for producing an LCP film for circuit boards, comprising at least the steps of: preparing an LCP resin composition containing at least 100 parts by mass of a liquid crystal polyester and 1 to 20 parts by mass of an oxazoline group-containing polymer; melt-extruding the LCP resin composition to form an LCP film having a linear expansion coefficient (α2) of 50 ppm / K or more in the TD direction; and pressurizing and heating the LCP film to obtain an LCP film for circuit boards having a linear expansion coefficient (α2) of 16.8±12 ppm / K in the TD direction.
[0015] (2) The method for producing an LCP film for circuit boards according to (1), wherein the LCP resin composition further contains 1 to 20 parts by mass of polyarylate. (3) The LCP film has a tensile modulus Y MD and tensile modulus Y in the TD direction TD Ratio of (Y MD / Y TD ) is 2 or more and 10 or less, and in the pressurizing and heating step, the LCP film is pressurized and heated to thereby obtain a tensile modulus Y MD and tensile modulus Y in the TD direction TD Ratio of (Y MD / Y TD ) is 0.8 or more and 2.0 or less. (4) The method for producing an LCP film for circuit boards according to any one of (1) to (3), wherein in the pressurizing and heating step, the LCP film is pressurized and heated to obtain an LCP film for circuit boards having a linear expansion coefficient in the TD direction of 5.0 ppm / K or more and 16.0 ppm / K or less. (5) The method for producing an LCP film for circuit boards according to any one of (1) to (4), wherein the LCP film has a thickness of 10 μm or more and 500 μm or less. (6) The LCP film for circuit boards has a relative dielectric constant ε r The method for producing an LCP film for circuit boards according to any one of (1) to (5), having dielectric properties (36 GHz) of 3.0 to 3.9 and a dielectric tangent tan δ of 0.0005 to 0.003.
[0016] (7) An LCP resin composition for circuit boards, comprising at least 100 parts by mass of a liquid crystal polyester and 1 to 20 parts by mass of an oxazoline group-containing polymer. (8) The LCP resin composition for circuit boards according to (7), further comprising 1 to 20 parts by mass of a polyarylate.
[0017] (9) An LCP film for circuit boards, comprising at least 100 parts by mass of a liquid crystal polyester and 1 to 20 parts by mass of an oxazoline group-containing polymer, and having a linear expansion coefficient (α2) in the TD direction of 16.8±12 ppm / K.
[0018] (10) The LCP film for circuit boards according to (9), further comprising 1 to 20 parts by mass of polyarylate. (11) Tensile modulus Y in MD direction MD and tensile modulus Y in the TD direction TD Ratio of (Y MD / Y TD ) is 0.8 or more and 2.0 or less. (12) The LCP film for circuit boards according to any one of (9) to (11), having a linear expansion coefficient in the TD direction of 5.0 ppm / K or more and 16.0 ppm / K or less. (13) Specific permittivity ε r The LCP film for circuit boards according to any one of (9) to (12), having dielectric properties (36 GHz) of 3.0 to 3.9 and a dielectric tangent tan δ of 0.0005 to 0.003. (14) The LCP film for circuit boards according to any one of (9) to (13), having a thickness of 10 μm or more and 500 μm or less. Effect of the Invention
[0019] According to the present invention, it is possible to provide an LCP film for circuit boards, which has a small coefficient of linear expansion and thus improved dimensional stability without excessively impairing the excellent basic properties of liquid crystal polyester, such as mechanical properties, electrical properties, high frequency properties, and heat resistance, and a method for producing the same. In addition, according to a preferred embodiment of the present invention, it is possible to easily and reproducibly provide an LCP film for circuit boards, which not only has excellent basic properties, such as mechanical properties, electrical properties, high frequency properties, and heat resistance, but also has small anisotropy in the in-plane direction of the film and can improve adhesion to metal foil, thereby improving productivity and economy. [Brief description of the drawings]
[0020] [Figure 1] 1 is a flowchart showing a method for producing an LCP film 11 for circuit boards according to one embodiment. [Diagram 2] 1 is a schematic diagram showing an LCP film 11 for circuit boards according to one embodiment. [Diagram 3] 1 is a schematic diagram showing a metal foil-clad laminate 31 according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. The positional relationships such as up, down, left and right are based on the positional relationships shown in the drawings unless otherwise specified. The dimensional ratios of the drawings are not limited to the ratios shown. However, the following embodiments are examples for explaining the present invention, and the present invention is not limited to these. That is, the present invention can be practiced with any changes within the scope of the gist of the present invention. In this specification, for example, the expression of a numerical range such as "1 to 100" includes both the lower limit "1" and the upper limit "100". The same applies to the expression of other numerical ranges.
[0022] (LCP film) FIG. 1 is a flow chart showing a method for producing an LCP film 11 for circuit boards of this embodiment, and FIG. 2 is a schematic diagram showing an LCP film 11 for circuit boards of this embodiment.
[0023] The manufacturing method of this embodiment includes at least a composition preparation step (S1) of preparing a specified LCP resin composition, a film formation step (S2) of melt-extruding this LCP resin composition to form a specified LCP film, and a pressurizing and heating step (S3) of pressurizing and heating the LCP film to obtain a specified LCP film 11 for circuit boards.
[0024] <Composition preparation step (S1)> In this composition preparation step (S1), an LCP resin composition is prepared that contains at least 100 parts by mass of a liquid crystal polyester as a liquid crystal polymer, and 1 to 20 parts by mass of an oxazoline group-containing polymer.
[0025] As the liquid crystal polyester, those known in the art can be used, and the type is not particularly limited. A liquid crystal polyester exhibiting thermotropic liquid crystal-like properties and having a melting point of 250°C or more, preferably 280°C to 380°C, is preferably used. As such liquid crystal polyester, for example, an aromatic polyester that is synthesized from monomers such as aromatic diol, aromatic carboxylic acid, and hydroxycarboxylic acid and exhibits liquid crystallinity when melted is known. Representative examples thereof include polycondensates of ethylene terephthalate and parahydroxybenzoic acid, polycondensates of phenol and phthalic acid and parahydroxybenzoic acid, and polycondensates of 2,6-hydroxynaphthoic acid and parahydroxybenzoic acid, but are not particularly limited thereto. The liquid crystal polyesters can be used alone or in any combination and ratio of two or more.
[0026] Among liquid crystal polyesters, from the viewpoint of excellent basic performance such as mechanical properties, electrical properties, and heat resistance, aromatic polyester-based liquid crystal polymers having a basic structure of 6-hydroxy-2-naphthoic acid and its derivatives (hereinafter, sometimes simply referred to as "monomer component A") and at least one monomer component selected from the group consisting of parahydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalenedicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate, and derivatives thereof (hereinafter, sometimes simply referred to as "monomer component B") are preferred.
[0027] The aromatic polyester liquid crystal polymer containing the above-mentioned monomer component A and monomer component B forms an anisotropic molten phase in which the linear chains of the molecules are regularly arranged in a molten state, typically exhibiting thermotropic liquid crystal-like properties and having excellent basic performance in mechanical properties, electrical properties, high frequency properties, heat resistance, moisture absorption, etc. The properties of the anisotropic molten phase of the aromatic polyester liquid crystal polymer described above can be confirmed by a known method such as a polarized light inspection method using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by using a Leitz polarizing microscope and observing a sample placed on a Leitz hot stage at a magnification of 40 times under a nitrogen atmosphere.
[0028] The aromatic polyester liquid crystal polymer described above can have any configuration as long as it has the monomer component A and the monomer component B as essential units. For example, it may have two or more kinds of monomer components A, or it may have three or more kinds of monomer components A. The aromatic polyester liquid crystal polymer described above may contain other monomer components other than the monomer components A and B. That is, the aromatic polyester liquid crystal polymer may be a two-component or more polycondensate consisting of only the monomer components A and B, or a three-component or more polycondensate consisting of the monomer components A, B, and other monomer components. The other monomer components (hereinafter, may be simply referred to as "monomer component C") include those other than the monomer components A and B described above, specifically, aromatic or aliphatic dihydroxy compounds and derivatives thereof; aromatic or aliphatic dicarboxylic acids and derivatives thereof; aromatic hydroxycarboxylic acids and derivatives thereof; aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids and derivatives thereof; and the like, but are not particularly limited thereto.
[0029] In this specification, the term "derivative" refers to a monomer component having a modification group such as a halogen atom (e.g., fluorine atom, chlorine atom, bromine atom, iodine atom), an alkyl group having 1 to 5 carbon atoms (e.g., methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, s-butyl group, t-butyl group, etc.), an aryl group such as a phenyl group, a hydroxyl group, an alkoxy group having 1 to 5 carbon atoms (e.g., methoxy group, ethoxy group, etc.), a carbonyl group, -O-, -S-, -CH2-, etc., introduced therein (hereinafter, this may be referred to as a "monomer component having a substituent"). Here, the "derivative" may be an ester-forming monomer such as an acylation product, an ester derivative, or an acid halide of the monomer components A and B which may have the above-mentioned modification group.
[0030] More preferred aromatic polyester liquid crystal polymers include binary polycondensates of parahydroxybenzoic acid and its derivatives and 6-hydroxy-2-naphthoic acid and its derivatives; ternary or higher polycondensates of parahydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, and monomer component C; and polycondensates of parahydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, and terephthalic acid, isophthalic acid, 6-naphthalenedicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybenzoic acid, ... and ternary or higher polycondensates consisting of one or more selected from the group consisting of parahydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, terephthalic acid, isophthalic acid, 6-naphthalenedicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate, and their derivatives, and one or more monomer components C. These can be obtained as having a relatively low melting point compared to, for example, homopolymers of parahydroxybenzoic acid, and therefore, LCP films using these have excellent moldability when thermocompressed to an adherend.
[0031] From the viewpoint of lowering the melting point of the aromatic polyester liquid crystal polymer, improving the moldability during thermocompression bonding of the LCP film to the adherend, or obtaining high peel strength when the LCP film is thermocompression bonded to a metal foil, the molar ratio of the monomer component A to the aromatic polyester liquid crystal polymer is preferably 10 mol% or more and 70 mol% or less, more preferably 10 mol% or more and 50 mol% or less, even more preferably 10 mol% or more and 40 mol% or less, and more preferably 15 mol% or more and 30 mol% or less. Similarly, the molar ratio of the monomer component B to the aromatic polyester liquid crystal polymer is preferably 30 mol% or more and 90 mol% or less, more preferably 50 mol% or more and 90 mol% or less, even more preferably 60 mol% or more and 90 mol% or less, and more preferably 70 mol% or more and 85 mol% or less.
[0032] In addition, the content of monomer component C that may be contained in the aromatic polyester-based liquid crystal polymer is preferably 10 mass% or less, more preferably 8 mass% or less, even more preferably 5 mass% or less, and preferably 3 mass% or less, in terms of molar ratio.
[0033] The synthesis method of the liquid crystal polyester can be a known method and is not particularly limited. Known polycondensation methods for forming ester bonds by the above-mentioned monomer components, such as melt polymerization, melt acidolysis, and slurry polymerization, can be used. When applying these polymerization methods, an acylation or acetylation process may be performed according to a conventional method.
[0034] The oxazoline group-containing polymer is a polymer having at least two or more oxazoline groups in the molecule. By containing the oxazoline group-containing polymer, the anisotropy in the in-plane direction of the LCP film generated in the film forming step (S2) can be effectively reduced by crosslinking with the liquid crystal polyester or promoting compatibility with the liquid crystal polyester in the pressurizing and heating step (S3). The oxazoline group-containing polymer can be appropriately selected from known ones and is not particularly limited in type. For example, it can be obtained by polymerization of a monomer containing an oxazoline compound having a polymerizable group such as 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, and 2-isopropenyl-2-oxazoline, copolymerization of an oxazonyl group-containing unsaturated monomer and a vinyl monomer (e.g., styrene and / or acrylonitrile), graft copolymerization of an oxazonyl group-containing unsaturated monomer and a thermoplastic resin other than liquid crystal polyester and liquid crystal polyester resin composition (e.g., polystyrene, styrene-acrylonitrile copolymer), etc. In addition, oxazoline group polymers are used in various applications such as modifiers and crosslinking agents for thermoplastic resins, and can be appropriately selected from these known polymers for use. Commercially available oxazoline group-containing polymers include, for example, EPOCROS (registered trademark), EPOCROS (registered trademark) RPS series, and EPOCROS (registered trademark) RAS series manufactured by Nippon Shokubai Co., Ltd. The oxazoline group-containing polymers can be used alone or in any combination and ratio of two or more types.
[0035] The total content of the above-mentioned oxazoline group-containing polymer can be appropriately set according to the desired performance, and is not particularly limited, but is preferably 1 to 20 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 1.5 to 10 parts by mass in terms of solid content, relative to 100 parts by mass of the total amount of the LCP resin composition. When the content of the oxazoline group-containing polymer is within the above preferred range, the effect of reducing the anisotropy in the in-plane direction of the LCP film tends to be effectively exhibited. When the content of the oxazoline group-containing polymer exceeds the above preferred range, the content of the liquid crystal polyester is relatively reduced, and basic performance such as mechanical properties, electrical properties, high frequency properties, and heat resistance tends to decrease, so the content of the oxazoline group-containing polymer may be adjusted in consideration of the balance between the effect of reducing anisotropy according to the present invention and the decrease in the basic performance of the liquid crystal polyester.
[0036] In addition, the LCP resin composition of the present embodiment preferably further contains polyarylate in addition to the liquid crystal polyester and the oxazoline group-containing polymer described above. By containing polyarylate, which is an amorphous polymer, it is possible to effectively reduce the amount of the liquid crystal polyester in the pressurizing and heating step (S3) by promoting compatibility with the liquid crystal polyester. The polyarylate can be appropriately selected from known ones and is not particularly limited in type. For example, amorphous polyester carbonate composed of aromatic dicarboxylic acid units such as isophthalic acid, terephthalic acid, or a mixture thereof and diphenol units such as bisphenol is preferable. In addition, as commercially available polyarylate, for example, U-Polymer (registered trademark) manufactured by Unitika Ltd. and Durel (registered trademark) manufactured by Celanese Corporation of the United States are known. The polyarylate can be used alone or in any combination and ratio of two or more kinds.
[0037] The total content of the polyarylate described above can be appropriately set according to the desired performance, and is not particularly limited, but is preferably 1 to 20 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 1.5 to 10 parts by mass in terms of solid content, relative to 100 parts by mass of the total amount of the LCP resin composition. When the content of the polyarylate is within the above preferred range, the effect of reducing the anisotropy in the in-plane direction of the LCP film tends to be effectively exhibited. When the content of the polyarylate exceeds the above preferred range, the content of the liquid crystal polyester and the oxazoline group-containing polymer tends to be relatively reduced, and basic performance such as mechanical properties, electrical properties, high frequency properties, and heat resistance tends to decrease, and the effect of reducing the anisotropy according to the present invention tends to decrease, so the content of the polyarylate may be adjusted in consideration of the balance between the effect of reducing the anisotropy according to the present invention and the decrease in the basic performance of the liquid crystal polyester.
[0038] In addition to the above-mentioned components, the LCP resin composition of the present embodiment may contain additives known in the art, such as release improvers such as higher fatty acids having 10 to 25 carbon atoms, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, and fluororesins, colorants such as dyes, pigments, and carbon black, organic fillers, inorganic fillers, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, flame retardants, lubricants, antistatic agents, surfactants, rust inhibitors, foaming agents, defoamers, and fluorescent agents, within the range that does not excessively impair the effects of the present invention. These additives can be added to the molten resin composition during film formation of the LCP film. These additives can be used alone or in combination of two or more. The content of the additives is not particularly limited, but from the viewpoints of moldability, heat stability, and the like, it is preferably 0.01 to 10 mass%, more preferably 0.1 to 7 mass%, and even more preferably 0.5 to 5 mass% relative to the total amount of the LCP film.
[0039] The preparation of the LCP resin composition of the present embodiment may be carried out according to a conventional method, and is not particularly limited. The above-mentioned components may be produced and processed by known methods, such as kneading, melt kneading, granulation, extrusion molding, pressing, or injection molding. When melt kneading, kneading devices such as commonly used single-screw or twin-screw extruders and various kneaders may be used. When supplying each component to these melt kneading devices, the liquid crystal polyester and polymer materials may be dry-blended in advance using a mixing device such as a tumbler or Henschel mixer. When melt kneading, the cylinder setting temperature of the kneading device may be appropriately set, and is not particularly limited, but is generally preferably in the range of the melting point of the liquid crystal polyester to 360°C, and more preferably in the range of the melting point of the liquid crystal polyester +10°C to 360°C.
[0040] <Film formation process (S2)> In this film forming step (S2), the above-mentioned LCP resin composition is formed into a film shape by a known melt extrusion film forming method such as the T-die method, to form an LCP film having a linear expansion coefficient (α2) of 50 ppm / K or more in the TD direction. In this specification, the linear expansion coefficient means a value when the LCP film or the LCP film for circuit boards 11 is heated (1st heating) at a heating rate of 5°C / min, cooled (1st cooling) to the measurement environment temperature (23°C), and then heated a second time (2nd heating) at a heating rate of 5°C / min in order to see the value after removing the thermal history. In addition, the other conditions are in accordance with the measurement conditions described in the examples described later.
[0041] Specifically, for example, the above-mentioned LCP resin composition is melt-kneaded in an extruder, and the molten resin is extruded through a die (for example, a T-die) to obtain an LCP film. At this time, the components are dry-blended in advance without going through the melt-kneading process, and the LCP resin composition is prepared and the LCP film is obtained as it is by kneading during the melt extrusion operation. The setting conditions of the extruder during such film formation may be appropriately set according to the type and composition of the LCP resin composition used, the desired performance of the target LCP film, etc., and are not particularly limited, but generally, the setting temperature of the cylinder of the extruder is preferably 230 to 360 ° C, more preferably 280 to 350 ° C. Similarly, for example, the slit gap of the T-die may be appropriately set according to the type and composition of the LCP resin composition used, the desired performance of the target LCP film, etc., and are not particularly limited. Generally, it is preferably 0.1 to 1.5 mm, more preferably 0.1 to 0.5 mm.
[0042] The thickness of the obtained LCP film can be appropriately set according to requirements and is not particularly limited. In consideration of the handleability and productivity during T-die melt extrusion molding, the thickness is preferably 10 μm to 500 μm, more preferably 20 μm to 300 μm, and even more preferably 30 μm to 250 μm.
[0043] The melting point (melting temperature) of the LCP film is not particularly limited, but from the viewpoint of heat resistance and processability of the film, the melting point (melting temperature) is preferably 200 to 400°C, and from the viewpoint of improving the thermal compression bonding to metal foil, the melting point (melting temperature) is preferably 250 to 360°C, more preferably 260 to 355°C, even more preferably 270 to 350°C, and particularly preferably 275 to 345°C. In this specification, the melting point of the LCP film means the melting peak temperature in differential scanning calorimetry (DSC) when the LCP film to be subjected to compression bonding is heated (1st heating) at a heating rate of 20°C / min, cooled (1st cooling) at a temperature drop rate of 50°C / min, and then heated for the second time (2nd heating) at a heating rate of 20°C / min in order to see the value after removing the thermal history. In addition, the other conditions are the same as those described in the examples described later.
[0044] When the above LCP resin composition is melt extruded to form an LCP film by T-die melt extrusion, it is easy to obtain an LCP film having a linear expansion coefficient (CTE, α2) in the MD (machine direction; longitudinal direction) of -40 to 40 ppm / K and a linear expansion coefficient (CTE, α2) in the TD (transverse direction; transverse direction) of 50 to 120 ppm / K. In addition, when ... MD and tensile modulus Y in the TD direction TD Ratio of (Y MD / Y TD ) is easily obtained in an LCP film having a value of 2 or more and 10 or less. Such physical properties are obtained because the main chain of the liquid crystal polyester tends to be easily oriented in the MD direction during T-die melt extrusion molding, and because an anisotropic molten phase of the liquid crystal polyester exists during T-die melt extrusion molding.
[0045] Thus, in the film forming step (S2), an LCP film with a high degree of orientation (large anisotropy) is likely to be formed. In the present invention, even in the case of an LCP film with such a high degree of orientation, the orientation (anisotropy) can be significantly reduced by performing the pressurizing and heating step (S3) using the LCP resin composition of the above composition, so that the LCP film with a high degree of orientation, which has been considered to have poor industrial applicability, can be used as a semi-finished product (intermediate product). Therefore, when an LCP film with an extremely high degree of orientation (extremely large anisotropy) is used, the effect of the present invention tends to be more pronounced. The linear expansion coefficient (CTE, α2) of the LCP film in the MD direction is not particularly limited, but is preferably -40 to 0 ppm / K, more preferably -30 to 0 ppm / K. The linear expansion coefficient (CTE, α2) of the LCP film in the TD direction is not particularly limited, but is preferably 50 to 120 ppm / K, more preferably 50 to 100 ppm / K. Furthermore, the tensile modulus Y in the MD direction of the obtained LCP film MD and tensile modulus Y in the TD direction TD Ratio of (Y MD / Y TD ) is not particularly limited, but is preferably 2 to 9, and more preferably 3 to 8.
[0046] <Pressure and heating process (S3)> In this pressurizing and heating step (S3), the LCP film with a high degree of orientation (large anisotropy) described above is pressurized and heated to reduce the degree of orientation (anisotropy) and obtain an LCP film for circuit boards 11 with a linear expansion coefficient in the TD direction (CTE, α2) of 16.8±12 ppm / K. This pressurizing and heating relaxes the orientation of the polymer chains of the liquid crystal polyester, improving the dimensional stability of the film in advance and providing excellent adhesion to the metal foil.
[0047] The heat and pressure treatment may be performed by a method known in the art, such as a contact heat treatment or a non-contact heat treatment, and the type is not particularly limited. For example, heat setting may be performed using known equipment such as a non-contact heater, an oven, a blowing device, a heat roll, a cooling roll, a heat press, or a double-belt heat press. At this time, if necessary, a release film or a porous film known in the art may be arranged on the surface of the LCP film and the heat treatment may be performed. In addition, when performing this heat treatment, from the viewpoint of controlling the orientation, a heat and pressure molding method is preferably used in which a release film or a porous film is arranged on the front and back of the LCP film, the film is sandwiched between a pair of endless belts of a double-belt press machine, and the film is then heat-pressed and the release film or the porous film is removed. The heat and pressure molding method may be performed by referring to, for example, JP-A-2010-221694. The processing temperature when the LCP film using the above LCP resin composition is thermocompressed between the endless belt pair of the double belt press is preferably higher than the melting point of the liquid crystal polyester and lower than 70°C higher than the melting point, more preferably higher than +5°C higher than the melting point and lower than 60°C higher than the melting point, and even more preferably higher than +10°C higher than the melting point and lower than 50°C higher than the melting point. The thermocompression bonding conditions at this time can be appropriately set according to the desired performance and are not particularly limited, but are preferably performed under conditions of a surface pressure of 0.5 to 10 MPa and a heating and pressing time of 250 to 430°C, more preferably under conditions of a surface pressure of 0.6 to 8 MPa and a heating and pressing time of 260 to 400°C, and even more preferably under conditions of a surface pressure of 0.7 to 6 MPa and a heating and pressing time of 270 to 370°C. On the other hand, when a non-contact heater or oven is used, it is preferable to perform the thermocompression bonding under conditions of, for example, 200 to 320°C and 1 to 20 hours.
[0048] (LCP film for circuit boards) The thickness of the LCP film 11 for circuit boards obtained after the pressurizing and heating step (S3) can be appropriately set according to requirements and is not particularly limited. In consideration of the ease of handling and productivity during the pressurizing and heating treatment, the thickness is preferably 10 μm to 500 μm, more preferably 20 μm to 300 μm, and even more preferably 30 μm to 250 μm.
[0049] The linear expansion coefficient (CTE, α2) in the TD direction of the LCP film 11 for circuit boards is not particularly limited, but is preferably 16.8±12 ppm / K, more preferably 16.8±10 ppm / K, and even more preferably 16.8±8 ppm / K, from the viewpoint of enhancing adhesion to the metal foil. The present invention has a remarkable effect in that the linear expansion coefficient (CTE, α2) in the TD direction can be significantly reduced, even though a highly anisotropic LCP film with a linear expansion coefficient (CTE, α2) in the TD direction of 50 ppm / K or more is used as the processing object from the beginning. In addition, from the viewpoint of enhancing adhesion to the electrolytic copper foil, in one embodiment of the LCP film 11 for circuit boards, the linear expansion coefficient (CTE, α2) in the TD direction is preferably 5.0 ppm / K or more and 16.0 ppm / K or less, more preferably 6.0 ppm / K or more and 16.0 ppm / K or less, and even more preferably 7.0 ppm / K or more and 16.0 ppm / K or less.
[0050] The linear expansion coefficient (CTE, α2) in the MD direction of the LCP film for circuit boards 11 is not particularly limited, but from the viewpoint of improving adhesion to the metal foil, it is preferably 0 to 40 ppm / K, more preferably 0 to 30 ppm / K, and even more preferably 0 to 20 ppm / K. The linear expansion coefficient (CTE, α2) in the film thickness direction is not particularly limited, but is preferably 150 ppm / K or less.
[0051] On the other hand, the tensile modulus Y in the MD direction of the LCP film 11 for circuit boards MD and tensile modulus Y in the TD direction TD Ratio of (Y MD / Y TD ) is preferably 0.8 or more and 2.0 or less, more preferably 0.9 or more and 1.5 or less, and even more preferably 0.95 or more and 1.2 or less, from the viewpoint of reducing the anisotropy in the in-plane direction of the film.
[0052] The dielectric properties of the LCP film for circuit boards 11 can be appropriately set according to the desired performance, and are not particularly limited. ris preferably 3.0 to 3.9, and more preferably 3.0 to 3.6. In addition, the dielectric tangent tan δ(36 GHz) is preferably 0.0005 to 0.0030, and more preferably 0.0005 to 0.0025.
[0053] The melting point (melting temperature) of the LCP film 11 for circuit boards is not particularly limited, but from the viewpoints of the heat resistance and processability of the film, the melting point (melting temperature) is preferably 200 to 400° C., and from the viewpoint of improving the thermocompression bondability to metal foil in particular, the melting point is preferably 250 to 360° C., more preferably 260 to 355° C., even more preferably 270 to 350° C., and particularly preferably 275 to 345° C. In this specification, the melting point of the LCP film 11 for circuit boards means a value measured under the same measurement conditions as the melting point of the above-mentioned LCP film.
[0054] (Metal foil laminate) 3 is a schematic diagram showing an example of a metal foil-clad laminate 31 of this embodiment. The metal foil-clad laminate 31 (metal foil laminated LCP film) of this embodiment includes the above-mentioned LCP film 11 for circuit boards and one or more metal foils 21 provided on at least one surface of the LCP film 11 for circuit boards. In this specification, the phrase "provided on one (other) surface side of ..." is a concept that includes not only an embodiment in which the metal foil 21 is provided only on one surface 11a of the LCP film 11 for circuit boards, but also an embodiment in which the metal foil 21 is provided on the other surface 11b of the LCP film 11 for circuit boards, and an embodiment in which the metal foil 21 is provided on both surfaces 11a, 11b of the LCP film 11 for circuit boards.
[0055] The material of the metal foil 21 is not particularly limited, but includes gold, silver, copper, copper alloy, nickel, nickel alloy, aluminum, aluminum alloy, iron, iron alloy, etc. Among these, copper foil, aluminum foil, stainless steel foil, and copper-aluminum alloy foil are preferred, and copper foil is more preferred. As such copper foil, any foil manufactured by rolling method or electrolysis method can be used, but electrolytic copper foil or rolled copper foil having a relatively large surface roughness is preferred. The thickness of the metal foil 21 can be appropriately set according to the desired performance, and is not particularly limited. Usually, it is preferably 1.5 to 1000 μm, more preferably 2 to 500 μm, even more preferably 5 to 150 μm, and particularly preferably 7 to 100 μm. In addition, the metal foil 21 may be subjected to a surface treatment such as a chemical surface treatment such as acid washing, as long as the effect of the present invention is not impaired.
[0056] The method of providing the metal foil 21 on the surfaces 11a and 11b of the LCP film 11 for circuit boards can be performed according to a conventional method, and is not particularly limited. Any of a method of laminating the metal foil 21 on the LCP film 11 for circuit boards and adhering or pressing the two layers together, a physical method (dry method) such as sputtering or vapor deposition, a chemical method (wet method) such as electroless plating or electrolytic plating after electroless plating, a method of applying a metal paste, and the like may be used.
[0057] A preferred lamination method is to overlap the LCP film 11 for circuit boards and the metal foil 21 to form a laminate in which the metal foil 21 is placed on the LCP film 11 for circuit boards, and then to perform thermocompression molding while sandwiching this laminate between a pair of endless belts of a double belt press. As described above, the LCP film 11 for circuit boards used in this embodiment has a significantly reduced linear expansion coefficient (CTE, α2) in the TD direction without excessively impairing the excellent basic performance of the liquid crystal polyester, and in a preferred embodiment, the tensile modulus Y in the MD direction is reduced. MD and tensile modulus Y in the TD direction TD Since the anisotropy of the metal foil 21 is sufficiently reduced, a higher peel strength can be obtained for the metal foil 21 than in the past. Therefore, the process tolerance during the manufacture of the circuit board or the metal foil-clad laminate 31 can be increased, and the productivity and economy can be improved.
[0058] The temperature during the thermocompression bonding of the metal foil 21 can be appropriately set according to the required performance, and is not particularly limited, but is preferably 50°C lower than the melting point of the liquid crystal polyester or higher and below the melting point, more preferably 40°C lower than the melting point or higher and below the melting point, even more preferably 30°C lower than the melting point or higher and below the melting point, and particularly preferably 20°C lower than the melting point or higher and below the melting point. The temperature during the thermocompression bonding of the metal foil 21 is a value measured at the surface temperature of the LCP film of the laminate described above. The pressure bonding conditions at this time can be appropriately set according to the desired performance, and are not particularly limited, but for example, when using a double belt press machine, it is preferable to perform the bonding under conditions of a surface pressure of 0.5 to 10 MPa and a heating time of 200 to 360°C.
[0059] The metal foil-clad laminate 31 of this embodiment may have a further laminated structure as long as it has a two-layer structure of the LCP film 11 for circuit boards and the metal foil 21. For example, it can have a multilayer structure having at least the above-mentioned two-layer structure, such as a two-layer structure of metal foil 21 / LCP film 11 for circuit boards; a three-layer structure such as metal foil 21 / LCP film 11 for circuit boards / metal foil 21 or LCP film 11 for circuit boards / metal foil 21 / LCP film 11 for circuit boards; or a five-layer structure such as metal foil 21 / LCP film 11 for circuit boards / metal foil 21 / LCP film 11 for circuit boards / metal foil 21. In addition, a plurality of (for example, 2 to 50) metal foil-clad laminates 31 can be laminated and thermocompressed.
[0060] In the metal foil-clad laminate 31 of this embodiment, the peel strength between the LCP film 11 for circuit boards and the metal foil 21 is not particularly limited, but from the viewpoint of providing a higher peel strength, it is preferably 1.0 (N / mm) or more, more preferably 1.1 (N / mm) or more, and even more preferably 1.2 (N / mm) or more. As described above, the metal foil-clad laminate 31 of this embodiment can realize a higher peel strength than the conventional technology, so that peeling between the LCP film 11 for circuit boards and the metal foil 21 can be suppressed, for example, during the heating process of substrate manufacturing. In addition, since it is possible to apply mild manufacturing conditions to obtain a peel strength equivalent to that of the conventional technology, it is possible to suppress deterioration of the basic performance of the liquid crystal polyester while maintaining the same level of peel strength as before.
[0061] The metal foil-clad laminate 31 of this embodiment can be used as a material for electronic circuit boards, multilayer boards, etc. by pattern-etching at least a part of the metal foil 21, and can also be used for applications such as high heat dissipation boards, antenna boards, optoelectronic hybrid boards, IC packages, etc. Furthermore, the metal foil-clad laminate 31 of this embodiment has excellent high-frequency characteristics and low dielectric constant, excellent adhesion between the LCP film 11 for circuit boards and the metal foil 21, and good dimensional stability, making it a particularly useful material as an insulating material for flexible printed circuit boards (FPCs) in fifth-generation mobile communication systems (5G), millimeter-wave radars, etc. EXAMPLES
[0062] The features of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. That is, the materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. In addition, the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limits in the embodiment of the present invention, and the preferred numerical range may be a range defined by a combination of the above-mentioned upper or lower limit and the values of the following examples or the values of the examples.
[0063] Example 1 Synthesis of LCPs A reaction vessel equipped with a stirrer and a vacuum distillation apparatus was charged with p-hydroxybenzoic acid (74 mol%), 6-hydroxy-2-naphthoic acid (26 mol%), and acetic anhydride in an amount of 1.025 times the molar amount of the total monomers. The reaction vessel was heated to 150°C under a nitrogen atmosphere, held for 30 minutes, and then heated to 190°C quickly while distilling off the by-product acetic acid, and held for 1 hour to obtain an acetylated reaction product. The obtained acetylated reaction product was heated to 320°C over 3.5 hours, and then the pressure was reduced to 2.7 kPa over about 30 minutes to perform melt polycondensation, and then the pressure was gradually reduced to normal pressure to obtain a polymer solid. The obtained polymer solid was pulverized and granulated at 300°C using a twin-screw extruder to obtain LCP pellets of an aromatic polyester liquid crystal polymer (molar ratio 74:26) consisting of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid.
[0064] Preparation of LCP resin composition The obtained LCP pellets and an oxazoline group-containing polymer (polystyrene containing 5% by mass of oxazoline component, product name: EPOCROS RPS-1005, manufactured by Nippon Shokubai Co., Ltd.) were supplied in the ratio shown in Table 1, and mixed, reacted and granulated at 300°C using a twin-screw extruder to obtain LCP resin composition pellets.
[0065] Manufacturing of LCP film The obtained LCP resin composition pellets were used to form a film at 300° C. by a T-die casting method, to obtain an LCP melt-extruded film having a melting temperature of 280° C. and a thickness of 50 μm.
[0066] Manufacturing of pressurized and heated LCP film The obtained LCP melt-extruded film was subjected to contact heat treatment at 320°C for 30 seconds using a double-belt heat press to obtain a pressurized and heat-treated LCP film having a melting temperature of 280°C and a thickness of 50 μm.
[0067] Example 2 Preparation of LCP resin composition The LCP pellets obtained in Example 1, an oxazoline group-containing polymer (polystyrene containing 5 mass% of oxazoline component, product name: EPOCROS RPS-1005, manufactured by Nippon Shokubai Co., Ltd.), and a polyarylate (product name: U Polymer POWDER CK, manufactured by Unitika Ltd.) (PAR) were supplied in the ratios shown in Table 1, and mixed, reacted, and granulated at 300°C using a twin-screw extruder, to obtain LCP resin composition pellets.
[0068] Manufacturing of LCP film The obtained LCP resin composition pellets were used to form a film at 300° C. by a T-die casting method, to obtain an LCP melt-extruded film having a melting temperature of 280° C. and a thickness of 50 μm.
[0069] Manufacturing of pressurized and heated LCP film The obtained LCP melt-extruded film was subjected to contact heat treatment at 320°C for 30 seconds using a double-belt heat press to obtain a pressurized and heat-treated LCP film having a melting temperature of 280°C and a thickness of 50 μm.
[0070] Comparative Example 1 An LCP resin composition was prepared in the same manner as in Example 1, except that the blending of the oxazoline group-containing polymer was omitted, and an LCP film having a melting temperature of 280°C and a thickness of 50 μm, and a pressurized and heat-treated LCP film having a melting temperature of 280°C and a thickness of 50 μm were obtained.
[0071] <Performance evaluation> The performance evaluation was carried out on the LCP films obtained in Examples 1 and 2 and Comparative Example 1 and the LCP film that had been subjected to the pressure and heat treatment. The measurement conditions were as follows.
[0072] [Linear expansion coefficient] Measuring equipment: TMA 4000SE (NETZSCH) Measurement method: Tensile mode Measurement conditions: Sample size 20mm x 4mm x thickness 50μm Temperature range: Room temperature to 200℃ (2nd RUN) Heating rate: 5℃ / min Atmosphere: Nitrogen (flow rate 50ml / min) Test load: 5gf *The value from the 2nd run was used to see the value after eliminating the thermal history.
[0073] [Tensile modulus] Measuring equipment: Strograph VE1D (manufactured by Toyo Seiki Co., Ltd.) Measurement method: Tensile test Measurement environment: Temperature 23℃, relative humidity 50% Measurement conditions: Sample size: dumbbell type, thickness: 50 μm Test speed: 50mm / min Gauge distance 25mm
[0074] [Relative permittivity ε r , dielectric tangent tanδ(36GHz) Electrical properties] Measurement method: Cylindrical cavity resonator method Measurement environment: Temperature 23℃, relative humidity 50% Measurement conditions: Sample size 15mm x 15mm x thickness 200μm Cavity 36GHz
[0075] [Heat resistance] Measurement equipment: DSC8500 (PerkinElmer) Measurement method: Differential scanning calorimetry (DSC) Measurement conditions: Temperature range 30~400℃ 1st heating 20℃ / min 1st cooling 50℃ / min 2nd heating 20℃ / min *The value from the 2nd run was used to see the value after eliminating the thermal history.
[0076] The measurement results are shown in Table 1. [Table 1]
[0077] (Examples 3 to 5) An LCP resin composition was prepared in the same manner as in Example 1, except that the blending ratio of the oxazoline group-containing polymer and the polyarylate was changed as shown in Table 2, and an LCP film having a melting temperature of 280°C and a thickness of 50 μm, and a pressurized and heat-treated LCP film having a melting temperature of 280°C and a thickness of 50 μm were obtained.
[0078] <Performance evaluation> The performance of the LCP films obtained in Examples 1 to 5 and Comparative Example 1 and the LCP film that had been subjected to the pressurization and heat treatment was evaluated.
[0079] The measurement results are shown in Table 2. [Table 2] [Industrial Applicability]
[0080] The LCP film for circuit boards of the present invention can be widely and effectively used in applications such as electronic circuit boards, multilayer boards, high heat dissipation boards, flexible printed wiring boards, antenna boards, optoelectronic hybrid boards, and IC packages. In particular, because of their excellent high-frequency characteristics and low dielectric properties, they can be widely and effectively used as insulating materials for flexible printed wiring boards (FPCs) in fifth-generation mobile communication systems (5G), millimeter-wave radar, and the like. [Explanation of symbols]
[0081] 11 LCP film for circuit boards 11a...Surface 11b...Surface 21 Metal foil 31 Metal foil laminate
Claims
1. A composition preparation step of preparing an LCP resin composition containing at least 100 parts by mass of a liquid crystal polyester and 1 to 20 parts by mass of an oxazoline group-containing polymer; A film forming step of melt-extruding the LCP resin composition to form an LCP film having a linear expansion coefficient (α2) in the TD direction of 50 ppm / K or more; The LCP film is pressurized and heated to obtain an LCP film for circuit boards having a linear expansion coefficient (α2) of 16.8±12 ppm / K in the TD direction. A manufacturing method for LCP film for circuit boards.
2. The LCP resin composition further contains 1 to 20 parts by mass of polyarylate. A method for producing the LCP film for circuit boards according to claim 1.
3. The LCP film has a tensile modulus Y MD and tensile modulus Y in the TD direction TD The ratio (Y MD / Y TD ) is 2 or more and 10 or less, In the pressurizing and heating step, the LCP film is pressurized and heated to reduce the tensile modulus Y in the MD direction. MD and tensile modulus Y in the TD direction TD The ratio (Y MD / Y TD ) is 0.8 to 2.0 to obtain an LCP film for circuit boards. A method for producing the LCP film for circuit boards according to claim 1 or 2.
4. In the pressurizing and heating step, the LCP film is pressurized and heated to obtain an LCP film for circuit boards having a linear expansion coefficient in the TD direction of 5.0 ppm / K or more and 16.0 ppm / K or less. A method for producing the LCP film for circuit boards according to any one of claims 1 to 3.
5. The LCP film has a thickness of 10 μm or more and 500 μm or less. A method for producing the LCP film for circuit boards according to any one of claims 1 to 4.
6. The LCP film for circuit boards has a relative dielectric constant ε r has dielectric properties (36 GHz) of 3.0 to 3.9 and a dielectric tangent tan δ of 0.0005 to 0.
003. A method for producing the LCP film for circuit boards according to any one of claims 1 to 5.
7. Contains at least 100 parts by mass of a liquid crystal polyester and 1 to 20 parts by mass of an oxazoline group-containing polymer; LCP resin composition for circuit boards.
8. The LCP resin composition further contains 1 to 20 parts by mass of polyarylate. The LCP resin composition for circuit boards according to claim 7.
9. Contains at least 100 parts by mass of a liquid crystal polyester and 1 to 20 parts by mass of an oxazoline group-containing polymer; The linear expansion coefficient (α2) in the TD direction is 16.8±12 ppm / K. LCP film for circuit boards.
10. Further contains 1 to 20 parts by mass of polyarylate The LCP film for circuit boards according to claim 9 .
11. Tensile modulus Y in MD MD and tensile modulus Y in the TD direction TD The ratio (Y MD / Y TD ) is 0.8 or more and 2.0 or less The LCP film for circuit boards according to claim 9 or 10.
12. The linear expansion coefficient in the TD direction is 5.0 ppm / K or more and 16.0 ppm / K or less. The LCP film for circuit boards according to any one of claims 9 to 11.
13. Relative permittivity ε rhas dielectric properties (36 GHz) of 3.0 to 3.9 and a dielectric tangent tan δ of 0.0005 to 0.
003. The LCP film for circuit boards according to any one of claims 9 to 12.
14. The thickness is 10 μm or more and 500 μm or less. The LCP film for circuit boards according to any one of claims 9 to 13.
Citation Information
Patent Citations
Resin composition
JP1993005054A
Liquid crystal polyester resin composition and film therefrom
JP1997286903A
Liquid crystal polymer film and its laminate
JP1998034742A
Liquid crystal polymer blend film
JP2004175995A
Aromatic liquid crystalline polyester film
JP2005097591A