Fluorescence sensor, fluorescence sensor device and fluorescence sensor element

Polycrystalline nanocomposite materials, produced via high-pressure sintering, address the accuracy and stability issues of existing sensors by offering enhanced optical signals and reduced hysteresis for precise temperature measurements in harsh environments.

JP2024156892APending Publication Date: 2024-11-06ジェイムスダリル +2

Patent Information

Application Number
JP2024128847
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-03-01
Filing Date
2024-08-05
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Existing fluorescent temperature sensors face challenges in providing accurate and stable temperature measurements at high temperatures due to issues with binder materials, hysteresis, and variations in time decay responses, particularly when exposed to harsh environments.

Method used

The development of polycrystalline nanocomposite fluorescent materials, produced through high-pressure sintering and controlled atmosphere processing, which are denser, more stable, and exhibit minimal hysteresis, enhancing the optical signal and accuracy of temperature sensors.

Benefits of technology

The polycrystalline nanocomposite materials provide brighter and more stable temperature measurements at high temperatures, ensuring precise and repeatable readings even in extreme conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156892000001_ABST
    Figure 2024156892000001_ABST
Patent Text Reader

Abstract

To provide a fluorescence sensor used for phosphor thermometry.SOLUTION: The sensor includes an optical light guide having a distal end, and a sensor element. The sensor element is attached to the distal end or close to the distal end of the optical light guide, and is aligned with the distal end. The sensor element contains polycrystal nanocomposite. The polycrystal nanocomposite contains at least one base material, at least one dopant, and at least one filler.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present technology relates to a temperature probe capable of sensing temperature accurately using nanocomposite fluorescent materials for use in phosphor thermometry. More particularly, the present technology relates to a method of fabricating a nanocomposite material that results in a polycrystalline sensor element and a fluorescent temperature sensor including a polycrystalline sensor element. [Background technology]

[0002] Fluorescence Temperature Sensor Fluorescence can be very easily defined as the emission of light when a material is exposed to electromagnetic radiation. This emission can continue for a period of time after the initial excitation. The length of time the material emits is the result of several interactions occurring at the atomic level and the amount of energy absorbed. Both the excitation and emission intensity behave exponentially with time. This dual behavior over time is a unique property and can be used to indicate the temperature of a fluorescent material.

[0003] Fluorescence temperature sensors exploit the proportional relationship between the time decay of a fluorophore's luminescence and the maintained temperature. For a fiber optic temperature sensor, an excitation light pulse is coupled into the optical fiber at one end and travels down the fiber to excite the fluorescent material at the other end. The excited light is coupled back into the same fiber and travels back towards the light source and split off onto a photodetector which produces an electrical signal that can be analyzed. The luminous intensity of the fluorophore is thereby analyzed over a period of time to determine its time decay rate. This time decay rate is then compared in a look-up table to known time decay values ​​for different reference temperatures. In this way, the time decay is converted to temperature and the fluorophore at the end of the fiber acts as the sensor element.

[0004] Fluorescence Sensing Materials When attached to the end of an optical fiber or mounted on a target substrate, phosphor powder can be used to sense temperature. However, phosphor powder in a loose form is unstable and cannot provide an accurate temperature reading. The powder can be strengthened and stabilized by mixing it with a liquid binder such as an epoxy before applying it to the end of the optical fiber and allowing it to solidify.

[0005] Bonding the phosphor powder to a solid matrix improves its stability against hysteresis effects from thermal cycling and also protects the phosphor from external influences that may change over time, such as the presence of moisture and various gas concentrations in the surrounding atmosphere that interact with the phosphor powder and affect its time fade characteristics.

[0006] Processing variations in the production of different batches of phosphor powders, having the same chemical composition, will result in different time fade values ​​at the same controlled temperature. Some of this variation is a result of differences in particle size, differences in fine dopant concentrations, sintering and grinding process variations, presence of impurities, phosphor particle density, and microstructure absorption and scattering properties.

[0007] Higher temperature fluorescent sensors Adding binder material to the phosphor powder works well in lower temperature regimes (below 250°C) because there are many optically clear organic binders to choose from, such as epoxies, silicones, and thermoplastics. However, at higher temperatures, these organic binders oxidize and degrade the phosphor, resulting in lower signal levels and changes in time fade response. Therefore, it is desirable to use an inorganic binder. A variety of liquid inorganic binders have been proposed, including sodium silicate, HPC, LK, and ZAP, manufactured by Zyp Coatings, Inc., Oak Ridge, Tennessee. Although these materials can withstand high temperatures, all of them suffer from one or more of the following drawbacks: a) Chemical inertness - they can react to moisture, oxygen or other gases in the environment, altering the time fade behavior of the phosphor matrix. b) Mechanical weaknesses - they are weak adhesives, which easily crack and result in a phosphor matrix that does not adhere well to the substrate. c) Phase transitions - for example sodium silicate undergoes a phase transition from a glass to a crystalline structure which is partially reversible in the presence of moisture, thereby introducing large hysteresis into the time fade behavior. d) Organic Additives - Many high temperature binder solutions contain organic solvents or other organic additives that dissipate at high temperatures but leave behind contaminants that degrade the optical signal and contribute to hysteretic behavior. e) Dehydration - Many binder solutions contain water that must be slowly removed in order to solidify. The result is a porous physical structure with density variations that produce a weaker optical signal and a variable time-fading response. f) Moisture resorption - In particular, the water absorption properties of silicate binders contribute to hysteresis and significantly alter the time fade response of the phosphor matrix at temperatures below 100°C.

[0008] A variety of solid crystal fluorescent materials have been proposed for time-fading temperature sensing at temperatures above 350°C. Such crystals include Y2O3 (yttria), Y3Al5O 12 (yttria aluminum garnet or YAG), YAlO3 (yttria aluminum perovskite or YAP), and Al2O3 (sapphire) doped with one or more rare earth elements. For example, a sensor may be fabricated from a YAG light guide with YAG-Er (erbium) grown on the end (U.S. Pat. No. 6,045,259). One advantage of this type of sensor is its use for extreme temperature applications in excess of 700°C.

[0009] However, this type of sensor suffers from the following drawbacks: 1. Time consuming and high cost to grow YAG light guides. 2. Time-consuming and high cost for growing YAG-Er crystals. 3. By undergoing ionic charge transfer and hysteresis, the crystals may develop color centers.

[0010] US Patent No. 8,123,403 discloses a temperature sensor probe capable of performing stable measurements, and a method for manufacturing the same. The temperature sensor probe provides: a fluorescent material, which is a mixture of a fluorescent material and a transparent material; a heat-sensitive portion having a recess in which the fluorescent material is disposed; a waveguide root rod that transmits an excitation light irradiated to the fluorescent material and a fluorescence generated by the fluorescent material; and a protective tube that covers the side of the waveguide root rod. The fluorescent material is then attached to the tip of the waveguide root rod using a transparent material, and the waveguide root rod is embedded in the fluorescent material. The fluorescent sensor is not a polycrystalline or solidified sintered sensor. The method does not include a step of producing a polycrystalline sensor element. The disclosed sensor relies on a recess for receiving the mixture of the fluorescent material and the transparent material, a waveguide root member that is embedded in the sensor material, and an undescribed process of "sintering" to attach the waveguide to the fluorescent material.

[0011] US Patent No. 9,599,518 discloses a fiber optic temperature sensor system incorporating a phosphor-based temperature probe in the form of a microsphere. The microsphere is positioned in air to create a lens effect in both coupling the excitation light delivered by the fiber to the microsphere and in coupling the fluorescence generated by the phosphor microsphere back into the fiber. The temperature probe can be implemented in either flexible or rigid form. Materials for the phosphor microsphere include, but are not limited to, rare earth doped single crystal, rare earth doped ceramic, and ruby. When coupled to a suitable controller, these temperature probes can provide reliable temperature measurements even in environments characterized by strong electrical noise or electromagnetic interference. The fluorescent sensor is not a sintered, polycrystalline, or solidified sintered sensor.

[0012] The technique of US Patent No. 9,599,518 allows for the growth of large quantities of YAG crystal material, somewhat reducing the cost of fabrication. The optical signal is weaker and has poor resolution and accuracy. This is due to the following: 1. The microspheres are small and match the fibers. 2. The excitation light travels through the microsphere, most of the excitation light escapes, and very little excitation light couples back into the fiber, so that it is not absorbed much by the microsphere. 3. The mechanical difficulty of attaching the microsphere to the end of the optical fiber so that it does not shift around. Even small shifts can result in changes in the fluorescent signal and affect the time decay characteristics.

[0013] US Patent No. 6,045,259 discloses a crystalline structure comprising an optical waveguide region, a crystalline fluorescent temperature sensor region, and a crystalline junction between the optical waveguide region and the crystalline fluorescent temperature sensor region. An embodiment of the invention is a novel fiber optic temperature sensor that functions under high temperature conditions. The fiber optic temperature sensor comprises a continuous crystal fiber optic high temperature sensor probe having a crystalline optical waveguide region with first and second ends and a crystalline fluorescent temperature sensor tip at one end. The crystalline optical waveguide region and the crystalline fluorescent temperature sensor tip are preferably crystallographically and thermomechanically compatible with one another. The fluorescent temperature sensor tip contains fluorescent ions that can be excited to fluoresce and produce fluorescence. The fiber optic high temperature sensor probe also includes a crystalline junction, preferably having a continuous crystal structure throughout. The crystalline junction is positioned and attached between the crystalline fluorescent temperature sensor tip and a first end of the crystalline optical waveguide region, thereby forming a preferably continuous crystal fiber optic high temperature sensor probe. The fluorescent sensor is a non-sintered, non-polycrystalline, non-solidified sintered sensor.

[0014] US Patent No. 9,537,047 discloses a method for assembling an LED / phosphor structure in which an array of blue light emitting diode (LED) dies are attached to a submount wafer. The phosphor powder is mixed with an organic polymer filler, such as acrylate or nitrocellulose. The liquid or paste mixture is then deposited as a substantially uniform layer on the LED dies or other substrate. The organic filler is then removed or decomposed by baking in air or by subjecting it to O.sub.2 plasma treatment, leaving a porous layer of phosphor particles sintered together. The porous phosphor layer is impregnated with a sol-gel (e.g., TEOS or MTMS sol-gel) or a liquid glass (e.g., sodium silicate or potassium silicate), also known as water glass, which saturates the porous structure. The structure is then heated to solidify the inorganic glass filler, leaving a robust glass filler that resists yellowing, among other desirable properties. The phosphor element is an LED phosphor coating. It is not polycrystalline, nor is it a solidified sintered sensor. The method does not include the step of producing a polycrystalline or solidified sintered sensor.

[0015] US Patent No. 9,434,876 discloses a phosphor-dispersed glass, which includes a glass material and a phosphor dispersed in the glass material. The glass material is substantially free of Nb2O5 and includes 15-40% by weight of SiO2, 10-30% by weight of B2O3, 1-35% by weight of ZnO, 0-20% by weight of Al2O3, 2-30% by weight of at least one selected from the group consisting of BaO, CaO, and SrO, 0-1% by weight of MgO, 5-35% by weight of R2O (at least one selected from the group consisting of Li2O, Na2O, and K2O), and 0-15% by weight of at least one of antimony oxide and tin oxide. The fluorescent sensor is not a polycrystalline or solidified sintered sensor. The method does not include a step of producing a polycrystalline or solidified sintered sensor.

[0016] U.S. Patent No. 4,652,143 discloses an optical temperature measurement technique that utilizes the decaying luminescence intensity properties of a sensor constructed from a luminescent material that is excited to emit light by a light pulse or other periodic or other intermittent radiation source. The luminescence of the preferred sensor exhibits a roughly exponential decay in time that is the average of a distribution of chemically reproducible crystals and is repeatable with a high degree of accuracy regardless of the excitation level or prior temperature history of the sensor. The fluorescent sensor is not a sintered, polycrystalline, or solidified sintered sensor.

[0017] US Patent No. 7,374,335 discloses a light emitting temperature sensor comprising: (i) an object having a recess; (ii) a layer of luminescent material disposed in the recess, the luminescent material emitting electromagnetic radiation having detectable optical characteristics functionally dependent on the temperature of the object; and (iii) an optical waveguide in optical communication with the luminescent material layer. A test device for measuring temperature during a process step is provided comprising: (i) an object having a surface and a recess on the surface; (ii) a layer of luminescent material disposed in the recess, the luminescent material emitting electromagnetic radiation having detectable optical characteristics functionally dependent on the temperature of the object in response to an excitation radiation source; and (iii) an optical window sealing the luminescent material layer in the recess on the surface of the object. The fluorescent sensor is not sintered, is not polycrystalline, and is not a solidified sintered sensor.

[0018] Ogi et al. (ECS Journal of Solid State Science and Technology,2(5) R91-R95 (2013) Optical Materials Vo.75, pp814-820) discloses that rare earth doped yttria aluminum garnet (YAG:RE) phosphors have good photoluminescence (PL) properties and are widely used in light emitting diodes. However, the RE elements used in these phosphors are expensive and scarce. Therefore, it is important to develop phosphors that incorporate less amount of RE material. One approach is to produce nanocomposite phosphors in which cheaper and more readily available materials are used as the matrix for the RE oxide. In this work, they produced YAG:Ce / SiO2 nanocomposites using a sol-gel method. Poly(ethylene glycol) and urea were added to improve micelle formation and aggregation, respectively. The nanocomposites were characterized using X-ray diffraction, scanning and transmission electron microscopy (TEM), and energy dispersive X-ray spectroscopy. They determined the concentration of SiO2 that provided the greatest PL enhancement and proposed an explanation for this enhancement using a geometrical model as well as characterization results. Their results showed that a SiO2 concentration of 10 vol.% provided a PL intensity of 120% that of pure YAG:Ce. TEM analysis showed that the SiO2 nanoparticles filled the cavities between the single grain boundaries of the YAG:Ce crystals, thereby suppressing the scattering of light and resulting in enhanced PL. This method will be useful for large-scale synthesis of low RE, high PL phosphors. A sol-gel process was used to synthesize the phosphor. The phosphor is neither sintered nor polycrystalline.

[0019] What is needed is a method for fabricating the nanocomposite fluorescent material for higher temperature applications, a method for producing multiple sensor elements with substantially the same precision, and a method for tuning the time decay response of the fluorescent material. It would be preferable that the nanocomposite fluorescent material be capable of being used in high temperature fluorescent sensors and improve the optical signal of high temperature fluorescent sensors. It would further be preferable that the nanocomposite fluorescent material be dense, stable and precise over time with minimal hysteresis in its time decay to temperature response. [Prior art documents] [Patent documents]

[0020] [Patent Document 1] U.S. Patent No. 6,045,259 [Patent Document 2] U.S. Pat. No. 8,123,403 [Patent Document 3] U.S. Pat. No. 9,599,518 [Patent Document 4] U.S. Pat. No. 9,537,047 [Patent Document 5] U.S. Pat. No. 9,434,876 [Patent Document 6] U.S. Pat. No. 4,652,143 [Patent Document 7] U.S. Patent No. 7,374,335 [Non-patent literature]

[0021] [Non-Patent Document 1] Ogi et al.(ECS Journal of Solid State Science and Technology,2(5) R91-R95 (2013) Optical Materials Vo.75,pp814-820) Summary of the Invention [Problem to be solved by the invention]

[0022] The present technology provides methods for fabricating nanocomposite fluorescent materials for higher temperature applications, methods for producing multiple sensor elements of substantially the same accuracy, and methods for tuning the time fade response of the fluorescent material. The methods utilize high pressure prior to high temperature sintering to produce polycrystalline sensor elements. The polycrystalline nanocomposite fluorescent materials can be used in high temperature fluorescent sensors to improve the optical signal of high temperature fluorescent sensors. Polycrystalline nanocomposite fluorescent materials are dense, stable and accurate over time with minimal hysteresis in their time fade to temperature response. Furthermore, they are brighter and more stable with respect to time fade at high temperatures, and therefore suitable as sensor materials for phosphor thermometry. [Means for solving the problem]

[0023] In an embodiment, a fluorescent sensor for use in phosphor thermometry is provided, the sensor comprising an optical light guide including a distal end and a sensor element including a proximal end and an outer surface, the proximal end of the sensor element being attached to or located adjacent the distal end of the optical light guide, the sensor element comprising one of a single crystal solid, a polycrystalline solid, or a polycrystalline nanocomposite.

[0024] In embodiments, the sensor element of the fluorescent sensor may be a nanocomposite with a solid phase density greater than about 90% or a polycrystalline solid with a solid phase density greater than about 90%.

[0025] In the fluorescent sensor, the polycrystalline nanocomposite can include at least one host material, at least one dopant, and at least one filler material.

[0026] In a fluorescent sensor, the sensor element may be mounted at the distal end of an optical light guide.

[0027] The fluorescent sensor may further comprise a glass bonding material between the distal end of the optical light guide and the sensor element.

[0028] In a fluorescent sensor, the optical light guide may be an optical fiber.

[0029] In the fluorescent sensor, the host material may be at least one of YSO, YSZ, Y2O3, YVO4, YAG, YAP, YAM, YGG, Al2O3, La2O2S, Gd2O2S, Mg2TiO4, 3.5MgO0.5MgF2GeO2, Mg4FGeO6, and K2SiF6.

[0030] In the fluorescent sensor, the dopant may be at least one of Ce, Cr, Dy, Er, Eu, Gd, Ho, Mn, Nd, Pr, Sm, Tb, Ti, and Yb.

[0031] In the fluorescent sensor, the filler material may be at least one of silica, glass, borosilicate glass, diamond, and an undoped host.

[0032] In the fluorescent sensor, the undoped host may be at least one of YSO, YSZ, Y2O3, YVO4, YAG, YGG, YAP, YAM, Al2O3, La2O2S, Gd2O2S, MgO, GeO2, TiO2, SiO2, and MgF2.

[0033] In a fluorescent sensor, the filler may be silicon dioxide.

[0034] In the fluorescent sensor, the silicon dioxide concentration may be about 0.1 to 10% by weight.

[0035] In the fluorescent sensor, the silicon dioxide may be doped with at least one of Ce, Cr, Dy, Er, Eu, Gd, Ho, Mn, Nd, Pr, Sm, Tb, Ti, and Yb.

[0036] The fluorescence sensor may further comprise a protective sheath in which at least the sensor element is housed.

[0037] In another embodiment, a polycrystalline nanocomposite for use in fluorescence time decay sensing is provided, the polycrystalline nanocomposite comprising a mixture of at least one host material, at least one dopant, and at least one filler material.

[0038] In another embodiment, a polycrystalline nanocomposite for use in fluorescence time decay sensing is provided, the polycrystalline nanocomposite comprising a mixture of at least one host material, at least one dopant, and at least one filler material, the mixture having a density of at least about 5 tonnes per inch. 2 It is compressed by increasing the pressure.

[0039] In the polycrystalline nanocomposite, the polycrystalline nanocomposite can be sintered.

[0040] In the polycrystalline nanocomposite, the host may be at least one of YSO, YSZ, Y2O3, YVO4, YAG, YAP, YAM, YGG, Al2O3, La2O2S, Gd2O2S, Mg2TiO4, 3.5MgO0.5MgF2GeO2, Mg4FGeO6, and K2SiF6.

[0041] In the polycrystalline nanocomposite, the dopant may be at least one of Ce, Cr, Dy, Er, Eu, Gd, Ho, Mn, Nd, Pr, Sm, Tb, Ti, and Yb.

[0042] In polycrystalline nanocomposites, the filler may be at least one of silica, glass, borosilicate glass, diamond, and an undoped host.

[0043] In the polycrystalline nanocomposite, the undoped host may be at least one of YSO, YSZ, Y2O3, YVO4, YAG, YGG, YAP, YAM, Al2O3, La2O2S, Gd2O2S, MgO, GeO2, TiO2, SiO2, and MgF2.

[0044] In a polycrystalline nanocomposite, the filler may be silicon dioxide.

[0045] In the polycrystalline nanocomposite, the silicon dioxide concentration may be about 0.01 to 10 wt %.

[0046] In the polycrystalline nanocomposite, the silicon dioxide can be doped with at least one of Ce, Cr, Dy, Er, Eu, Gd, Ho, Mn, Nd, Pr, Sm, Tb, Ti, and Yb.

[0047] In another embodiment, a method is provided for producing a polycrystalline nanocomposite fluorescent solid, the method comprising: providing a phosphor powder by doping at least one host body with at least one dopant; mixing at least one filler material with the phosphor powder to provide a phosphor and filler mixture; The mixture is heated to at least about 5 tons / in. 2 to provide a solid or nearly solid matrix, and sintering the solid or nearly solid matrix in a controlled atmosphere to provide a polycrystalline nanocomposite fluorescent solid.

[0048] In this method, the at least one filler may be SiO2 nanoparticles.

[0049] The method may further include grinding the polycrystalline nanocomposite fluorescent solid to a substantially uniform particle size.

[0050] The method may further include processing the polycrystalline nanocomposite fluorescent solid into a sensor element.

[0051] In another embodiment, a method is provided for producing a plurality of devices by fine-tuning the time decay to temperature response of a batch of fluorescent temperature sensor material, the method comprising: providing bin values ​​to a predetermined precision; mixing a batch of fluorescent temperature sensor material; Obtaining a sample from this batch; allowing the samples to clot; testing the sample by recording a time decay response at a reference temperature; comparing the time decay response to a bin value of a predetermined precision for each of the samples; determining whether a majority of the samples fall within a bin value of a given precision; adjusting the batch material based on the test results by adding and mixing additional material to the batch to provide a new batch if a majority of the samples do not fall within the bin values ​​of the predetermined precision; Obtaining new samples from this new batch and Allowing the new sample to clot; and testing the new samples to determine a bin value for each of the new samples; comparing the bin value of each new sample with the bin value of a predetermined precision; determining whether a majority of new samples fall within a bin value of a given precision; further adjusting the batch material based on the test results by adding and mixing additional material into the batch if a majority of the new samples do not fall within the bin values ​​of the predetermined precision; repeating the above steps until a majority of new samples fall within a bin value of a given accuracy; and coagulating the entire batch when the majority of the test samples fall within a predetermined precision bin value.

[0052] In the method, the step of preparing the batch material may include adding a filler material to the phosphor powder one or more times; or adding a second batch of phosphor powder having a different dopant concentration; or adding a second batch of phosphor powder of a different particle size than the original phosphor powder.

[0053] In the method, the step of preparing the batch materials comprises preparing the following materials: a phosphor powder of the same chemical composition but with a larger particle size; a phosphor powder of the same chemical composition but with a smaller particle size; A filler material; a phosphor powder of the same chemical composition but with a higher dopant concentration; and phosphor powders of the same chemical composition but with lower dopant concentrations. The method may include adding one or more of:

[0054] In a fluorescent sensor, the optical light guide may comprise a bundle of optical fibers.

[0055] In a fluorescence sensor, the proximal end of the sensor element may be polished.

[0056] In a fluorescence sensor, the outer surface of the sensor element may be polished.

[0057] In a fluorescent sensor, the outer surface may be a reflective surface.

[0058] The fluorescence sensor may further include a sensor cap that houses the sensor element.

[0059] In a fluorescent sensor, the sensor element may be formed within the sensor cap or may be bonded to the sensor cap.

[0060] The fluorescent sensor may further comprise a space between a distal end of the optical light guide and a proximal end of the sensor element, the optical light guide being bonded to the sensor cap.

[0061] The fluorescent sensor may further comprise a bonding layer between the distal end of the optical light guide and the proximal end of the sensor element, the bonding layer comprising at least one of silica, glass, or a lithium, potassium, or sodium loaded silicate.

[0062] In a fluorescent sensor, the protective sheath may have a similar coefficient of thermal expansion as the optical light guide.

[0063] In a fluorescent sensor, a protective sheath may be bonded to an optical light guide to define a cavity.

[0064] In a fluorescent sensor, the cavity may hold an inert gas or a vacuum.

[0065] In a fluorescent sensor, the sensor element may be coated with a glass or silica coating, or a silicate coating.

[0066] In a fluorescent sensor, the optical light guide may comprise one or more high numerical aperture optical fibers.

[0067] In a fluorescence sensor, the optical fiber may comprise a germanium-doped silica core and a fluorosilicate-doped silica cladding.

[0068] In the fluorescent sensor, the optical fiber can be thermoformed into a stress-free shape with one or more bends.

[0069] This technology is A fluorescence time decay sensor device, more particularly a temperature sensor device; A method for synthesizing a fluorescent sensor element, and A method for producing a device by bonding a crystalline or polycrystalline fluorescent sensor element to the end of an optical fiber. is directed towards.

[0070] A method for producing multiple devices by fine tuning the time decay to temperature response in a batch of fluorescent sensor elements comprises the following steps: mixing a batch of phosphor material; obtaining a sample from the batch; allowing the sample to clot; testing the samples to determine whether a majority of the samples fall within parameters for a given accuracy bin value; adjusting the batch material based on the results of the previous test by adding and mixing additional material into the batch; obtaining a new sample from this batch; and Allowing the new sample to clot; testing new samples to determine whether a majority of the new samples fall within parameters for a given accuracy bin value; repeating the above steps until a majority of the test samples fall within the parameters at the predetermined accuracy bin values; · A step of solidifying the entire batch; Through.

[0071] The objective of this method is to finely tune the time decay versus temperature response of a batch of fluorescent sensor elements by following the steps above.

[0072] The present technology is also directed to a method of making the device by bonding a sintered phosphor disk or crystal to the end of an optical fiber to maintain intimate contact and protection from the chemical environment. [Brief description of the drawings]

[0073] [Figure 1] 1 illustrates an embodiment of a temperature sensor of the present technology. [Diagram 2] FIG. 1 illustrates another embodiment of a temperature sensor of the present technology. [Diagram 3] FIG. 1 illustrates another embodiment of a temperature sensor of the present technology. [Figure 4] FIG. 1 illustrates another embodiment of a temperature sensor of the present technology. [Diagram 5] FIG. 1 illustrates another embodiment of a temperature sensor of the present technology. [Figure 6] FIG. 1 illustrates another embodiment of a temperature sensor of the present technology. [Figure 7]FIG. 1 illustrates another embodiment of a temperature sensor of the present technology. [Figure 8] FIG. 1 illustrates another embodiment of a temperature sensor of the present technology. [Figure 9] 1 shows a sensor element in a sensor cap during manufacturing and testing. [Figure 10] FIG. 1 shows a sensor element coated with a transparent silica, silicate, or glass coating. [Figure 11] FIG. 2 is a schematic diagram of a sheet and disk of sensor material. [Figure 12] A histogram of grouped bins. [Figure 13] FIG. 1 is a schematic diagram of an apparatus of the present technology. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0074] Unless otherwise expressly stated, the following rules of interpretation apply to this specification (the written description and the claims): (a) words used herein shall be construed as to gender or number (singular or plural) appropriate to the context; (b) the singular terms "a," "an," and "the" used in this specification and the appended claims shall include the plural, unless the context clearly supports otherwise; (c) the estimation term "about" applied to a recited range or value represents an approximation within a deviation in the range or value known or expected in the art from the measurement method; (d) the words "herein," "in the present specification," "in the present The words "hereby," "hereof," "hereto," "hereinbefore," "hereinafter," and words of similar import refer to this specification as a whole and not to any particular paragraph, claim, or other portion, unless otherwise expressly stated; (e) the recited details are for convenience only and do not control or affect the meaning or construction of any portion of this specification; (f) "or" and "any" are not exclusive, and "include" and "including" are not limiting. Further, the terms "comprising," "having," "including," and "containing" are to be construed as open-ended terms (i.e., meaning "including but not limited to"), unless otherwise specified.

[0075] The recitation of ranges of values ​​herein is intended only as a shorthand method of individually referring to each separate value falling within the range, unless otherwise noted herein. Each separate value is incorporated herein as if it were individually recited herein. When a specific range of values ​​is provided, each intervening value is included, to the tenth of the unit of the lower limit, between the upper and lower limit of the range and any other stated or intervening value within the stated range, unless the context clearly dictates otherwise. All smaller subranges are also included. The lower and upper limits of these smaller ranges are also included therein, subject to any specifically excluded limitations within the stated range.

[0076] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the relevant art. Although any methods and materials similar or equivalent to those described herein can also be used, acceptable methods and materials are described below.

[0077] definition Phosphor Powder - In the context of the present technology, a phosphor powder is a combination of at least one host and at least one dopant, in other words a doped host that absorbs energy from incident light of certain wavelengths and emits light at other wavelengths.

[0078] Fluorescent Material - In the context of the present technology, the fluorescent material is composed of phosphor powder and filler.

[0079] Fluorescence Sensor Element - In the context of the present technology, the fluorescence sensor element is one of a single crystal solid, a polycrystalline solid, or a polycrystalline nanocomposite of either a mixture of phosphor powder and glass, or phosphor powder.

[0080] Single Crystal Solids - In the context of the present technology, single crystal solids are sintered phosphor crystals of phosphor powder. They are understood to have a grain size greater than about 100 microns, but generally lack any grain boundaries. Single crystal solids ideally have a solid phase density greater than about 90%.

[0081] Polycrystalline solids - in the context of the present technology, a polycrystalline solid is a sintered phosphor powder resulting in a polycrystalline structure having a particle size ranging from about 10 nanometers to about 100 microns. Polycrystalline solids ideally have a solid phase density of greater than about 90%.

[0082] Polycrystalline Nanocomposite - In the context of the present technology, a polycrystalline nanocomposite is a sintered phosphor material (phosphor powder and at least one filler) that results in a polycrystalline structure having particle sizes ranging from about 10 nanometers to about 100 microns. Polycrystalline solid nanocomposites ideally have a solid phase density of greater than about 90%.

[0083] High Pressure - With respect to the present technology, high pressure is at least about 5 tons / inch 2 , preferably about 100 tons / inch 2 It is.

[0084] Controlled Atmosphere - In the context of the present technique, the controlled atmosphere is one of an inert gas atmosphere, an oxygen atmosphere, or a vacuum.

[0085] Device FIG. 1 shows an embodiment of a fluorescent temperature sensor for high temperature applications, generally designated 10. The fluorescent temperature sensor includes an optical light guide 12, which may be a silica optical fiber, a sensor element 14, and a protective sheath 16, which is preferably opaque, but need not be transparent. The protective sheath 16 is preferably an end-sealed fused silica tube having the same or similar coefficient of thermal expansion as the optical light guide 12. The protective sheath is fusion bonded to the light guide 12 at fusion joint 18 and defines a cavity 15. The cavity 15 houses at least the sensor element 14. The cavity 15 holds an inert gas or vacuum. The sensor element 14 may have any shape, such as, but not limited to, a small disk sized to fit into the distal end 20 of the optical light guide 12 at a proximal end 22 of the sensor element 14. Without being bound by theory, the disk has a thickness of about 50 to about 1000 microns to maximize thermal conductivity throughout the disk, minimize thermal gradients across the disk, and maximize absorption and emission of the fluorescent signal. In one embodiment, the sensor element 14 is a polycrystalline solid. In another embodiment, the sensor element 14 is a polycrystalline nanocomposite. In all embodiments, the sensor element 14 can withstand temperatures in excess of 350 degrees Celsius while producing a monotonic time decay response to temperatures beyond the preferred temperature range. Without being bound by theory, the cavity 15 creates a controlled environment for the sensor element. A controlled environment is desirable because oxidation can occur at high temperatures, which can lead to charge migration and hysteresis of the dopant ions. Because the cavity 15 is very small (on the order of a few microns), there is no need to bond or mount the sensor element 14 to the optical light guide 12. This reduces the number of steps to fabricate the fluorescent temperature sensor 10.

[0086] As shown in FIG. 2, in another embodiment of the fluorescent temperature sensor 10, there is a glass bonding layer 24 between the distal end 20 of the optical light guide 12 and the proximal end 22 of the sensor element 14. The glass bonding material has a similar or lower melting temperature as the light guide 12 or the sensor element 14 and serves to fuse the distal end 20 of the optical light guide 12 to the proximal end 22 of the sensor element 14. This layer 24 may include the same fillers used to create the polycrystalline nanocomposite sensor element 14, but may also be any solid, substantially transparent glass material that forms a mechanical bond between the sensor element 14 and the optical light guide 12. Examples of materials for the glass bonding layer 22 may include, but are not limited to, borosilicate glass, glass compositions including specialty silica, or liquid glasses such as potassium silicate, lithium silicate, or sodium silicate, or combinations thereof.

[0087] 3, the sensor element 14 has a larger diameter than the optical light guide 12. In this embodiment, there is a space 26 between the distal end 20 of the optical light guide 12 and the sensor element 14. The distance between the distal end of the optical light guide 12 and the sensor element 14, and the diameter of the sensor element 14, are preferably calculated to match the numerical aperture of the optical light guide 12 such that the cone of light emitted from the optical light guide 12 is focused at the sensor element 14. One advantage of this embodiment is that it eliminates the need for an intermediate bonding layer while maximizing the optical signal.

[0088] As shown in FIG. 4, in another embodiment of the fluorescence temperature sensor 10, the sensor element 14 is a single crystal solid crystal, with or without a glass bonding layer 24, attached to the distal end 20 of the optical light guide 12. The sensor element 14 has a hemispherical shape as shown, or a disk shape as shown in FIG. 2, and the outer surface 32 of the sensor element 14 may be either polished or ground. Without being bound by theory, the polishing of the outer surface promotes back scattering of the excitation light within the sensor element 14, thereby improving its absorption and emission intensity. A reflective surface coating 34 is also applied to the outer surface 32, which helps capture light within the sensor element 14, further improving its absorption and emission intensity. The distal end 20 of the optical light guide 12 has a polished surface 36. The proximal end 38 of the sensor element 22 also has a polished end. The protective sheath 16 may have thinner end walls 40 for faster response time, but thicker rearward extending side walls 42 to help protect the fragile optical light guide 12. For high temperature applications, the protective sheath 16 may be fused silica, a ceramic such as alumina, or a metal such as Inconel. For low temperature applications, the protective sheath may be a polymer coating such as Teflon.

[0089] As shown in Figure 5, when a more flexible probe structure is required, a smaller diameter optical fiber bundle 60 is used. The individual optical fibers 62 typically have diameters in the range of about 40 to about 200 microns. In this case, the bundle 60 of borosilicate or silica-based optical fibers 62 has a diameter of about 1000 microns and has a fused distal end 64 and a sensor element 14 attached as described above.

[0090] Without being bound by theory, a bundle of optical fibers has the advantage that it accommodates a smaller bend radius while delivering more light to the sensor element 14 than a single optical fiber with the same minimum bend radius.

[0091] To further increase the optical signal, in an embodiment, an optical fiber having a larger diameter of 1000 microns can be formed into a final shape with an applicable bend. Heat is applied to the optical fiber to create a bend with a radius large enough to avoid optical loss through the bend. The preforming step is done to reduce bending stresses in the optical fiber, which can lead to breakage over time or under sudden temperature changes. In this case, a higher numerical aperture optical fiber is also desirable to accommodate a smaller bend radius without signal loss.

[0092] As shown in FIG. 6, the light guide 12 is a heat-formed optical fiber with a high numerical aperture (NA). Standard commercial grade silica-based optical fibers for high temperature applications typically have a numerical aperture of 0.22, which limits the light acceptance angle and restricts the minimum bend radius. It is desirable to use a germanium-doped silica core fiber with an increased NA of about 0.37 or higher to provide an improved optical signal and smaller bend radius. The optical fiber diameter is about 200-1000 microns, and the germanium-doped silica core is typically coated with a phosphor-doped silica cladding 17. An annealing step after heat-forming the light guide allows complex bends to be formed while eliminating bending stresses that may lead to failure in high temperature applications.

[0093] As shown in FIG. 7, in an alternative embodiment, the sensor element 14 is attached to a sensor target 50 to be sensed and illuminated by a light guide 12 some distance away from the target 50. The sensor target 50 may be individually accuracy tested as part of the manufacturing process before being placed on a surface 66 to be measured. In another embodiment shown in FIG. 8, a lens system 68 is positioned between the optical light guide 12 and the sensor element 14 bonded to the target 66. One or more optical lenses 68 may also be utilized between the distal end of the optical light guide 12 and the sensor element 14 to further extend the distance between the light guide 12 and the sensor element 14 in remote sensing applications. In this way, the temperature of the target 66 may be very high, but the lens and light guide 12 may remain at a lower temperature because they are located far away.

[0094] 9, in an embodiment, the sensor element 14 is made of phosphor powder and at least one filler material that is compressed and sintered into a polycrystalline solid or polycrystalline nanocomposite within the cap 72. When manufactured in this manner, the cap 72 can be individually tested for accuracy before being assembled into the fluorescent temperature sensor 10. The distal region 70 can house the optical light guide 12, which is temporarily inserted during testing of the sensor cap.

[0095] In an embodiment, the sensor element 14 comprises a fluorescent polycrystalline solid or polycrystalline nanocomposite material. The polycrystalline solid or polycrystalline nanocomposite includes a host crystal material, a dopant, and a filler material. Table 1 shows examples of host crystals, dopants, and filler materials. The polycrystalline solid or polycrystalline nanocomposite material may include any combination of host crystals, dopants, and filler materials as listed in Table 1.

[0096] For example, in embodiments, the phosphor powder portion of a polycrystalline solid or polycrystalline nanocomposite material may include any combination of any of the host crystals listed in Table 1 (or any other host crystal materials known in the art) with one or more dopants listed in Table 1 (or any other dopants known in the art), such as, for example, YAG:Er and YAG:Nd. Further for example, in embodiments, the filler material portion of a polycrystalline solid or polycrystalline nanocomposite may include any of the filler materials listed in Table 1 (or any filler materials known in the art).

[0097] In embodiments, the relative amount of filler material to other materials may be from about 0.1 to about 10% by weight of the total amount of materials.

[0098] In embodiments, the particle shape of the filler material may be in the form of microspheres or randomly ground powder. The particle size may range from about 10 nanometers to about 10 microns.

[0099] In an embodiment, the filler material may be an undoped host crystal as set forth in Table 1. In another embodiment, the filler material may be a doped host crystal as set forth in Table 1.

[0100] In embodiments, the specialty glass is a custom-composed glass with a lower melting point than the host crystal.

[0101] Various factors are considered in selecting the fill material, such as thermal conductivity, chemical compatibility with the doped host crystal, susceptibility to oxidation and ionic charge transfer, effect on time fade response, and useful operating temperature range. In addition, to maximize the optical signal, the fill material is ideally selected to be optically transparent at the excitation and emission wavelengths of the doped host crystal.

[0102] Another consideration is the chemical compatibility of the filler material with the operating environment in which the sensor may be deployed. Inertness is important because at high temperatures the host crystal can absorb gas molecules from the atmosphere into its crystal lattice, thereby altering its time-fading response. Adding nanoparticle filler materials in high density combinations can greatly reduce this effect.

[0103] In addition, ionic charge transfer can occur within the crystal lattice as a result of exposure to incident light energy of a particular wavelength, either at high temperatures or for long periods of time. For example, the amount of Er3+ relative to Er2+ ionic charge changes with incident light intensity in the YAG crystal lattice over temperature. This alters the fluorescence time decay response of the host crystal, resulting in irreversible drift and hysteresis over time. To stabilize this behavior, a fill material that includes oxygen is selected to provide additional oxygen ions to the crystal lattice and keep the erbium in the Er3+ state.

[0104] [Table 1]

[0105] In a preferred embodiment, silicon dioxide is added at a concentration of about 0.1 to about 10% (see Table 2). The particle size is about 10 nanometers to about 10 microns. Without being bound by theory, adding a small amount of silicon dioxide to the crystal lattice or crystals of various phosphor powders helps to prevent ionic charge transfer within the crystal lattice, thus stabilizing its absorption and emission wavelengths and making the time fade versus temperature response more accurate and repeatable. The silicon dioxide may be doped with at least one of Ce, Cr, Dy, Er, Eu, Gd, Ho, Mn, Nd, Pr, Sm, Tb, Ti, and Yb to further improve the fluorescent efficiency.

[0106] [Table 2]

[0107] The method for producing polycrystalline nanocomposite fluorescent sensor elements is as follows. a) A phosphor powder of uniform particle size is first produced. b) The powdered filler material is uniformly mixed with the phosphor powder. c) The mixture is compressed under high pressure (at least about 5 tons / in) to near solid density. 2 ) to produce a polycrystalline nanocomposite green body. d) This green body is sintered at high temperature in a controlled atmosphere to produce a sintered polycrystalline nanocomposite object. e) Optionally, the sintered polycrystalline nanocomposite object is then annealed at a slightly reduced temperature in a normal atmosphere for a period of time to produce an annealed sintered polycrystalline nanocomposite object. f) Multiple sensor elements are fabricated from annealed and sintered polycrystalline nanocomposite pieces. g) Optionally, the nanocomposite crystalline object is ground into a powder of substantially uniform particle size, and steps a) through f) are repeated to produce a more uniform polycrystalline nanocomposite object. A preferred particle size is about 1 to about 25 μm. This nanocomposite powder can also be used to fabricate a fluorescent sensor using other methods known in the art.

[0108] In some embodiments, the sensor element 14 is a translucent polycrystalline solid. Without being bound by theory, an advantage of a polycrystalline solid over a single crystal solid is that the grain boundaries in the polycrystalline structure help trap light within the sensor, which increases the intensity of absorption and emission. Multiple grain boundaries can also help distribute internal stresses, reduce ionic charge transfer, and create a more stable sensor element with less hysteresis. A method for creating a polycrystalline sensor element is as follows. a) A phosphor powder of uniform particle size is first produced. b) The powder is compressed under high pressure (at least about 5 tons / in) to nearly solid density. 2) to produce a green body. c) This green body is sintered at high temperature in a controlled atmosphere to produce a sintered polycrystalline solid (note that sintering for extended periods of time will result in a single crystal solid, as the individual grains grow larger over time). d) Optionally, the sintered polycrystalline solid is then annealed at a slightly reduced temperature in a normal atmosphere to produce an annealed sintered polycrystalline solid. e) Many sensor elements are fabricated from annealed and sintered polycrystalline solids.

[0109] 10 shows the fluorescent sensor element 14 encapsulated with a glass coating 90 to protect it from the outside atmosphere. The glass coating 90 can be, for example, fused silica, borosilicate glass, or any glass containing silicates. Such a coating is applied to prevent chemical attack, oxidation, and moisture from affecting the fluorescent sensor element 14, and is particularly important when the sensor element is more porous and less dense.

[0110] In alternative embodiments, the fluorescent sensor element 14 may be used in any application where fluorescence time decay is measured to sense, for example but not limited to, pressure, oxygen, pH, or moisture.

[0111] How to make multiple devices The present technology is directed to a method for fine tuning the time decay versus temperature response in a batch of fluorescent sensor elements to create multiple devices, comprising the following steps: a) mixing a batch of fluorescent materials (e.g., host crystals, dopants, and fillers); b) obtaining a sample from the batch; c) allowing these samples to clot; d) testing the samples to determine if a majority of the samples fall within the parameters for a given accuracy bin value; e) adjusting the batch material based on the results of the initial test by adding and mixing additional material into the batch; f) obtaining a new sample from this batch; g) allowing these new samples to clot; h) testing new samples to determine if a majority of the samples fall within the parameters for a given accuracy bin value; i) repeating the above steps until a majority of the test samples fall within the parameters at the bin values ​​of a given accuracy; j) solidifying the entire batch; Through.

[0112] The goal of this method is to maximize the number of generated sensor elements that fall within a given accuracy bin value.

[0113] A large batch can be produced and thoroughly mixed. Small samples from this batch are then processed and tested, and the batch is adjusted in the manner described above until the majority of the test samples fall within the parameters in a particular accuracy bin.

[0114] The sensor elements can be manufactured in a variety of ways. Figure 11 shows a disk-shaped sensor element 14 stamped from a sheet 80 or cut from a rod 81 of sintered material. The sheets can have any desired thickness, for example from about 50 to about 1000 microns. The rod 81 can have any desired diameter, for example from about 200 to about 1000 microns.

[0115] In embodiments, the step of solidifying the sample may be performed, for example, by baking, hardening, drying or sintering.

[0116] The fluorescent sensor elements are sorted and binned according to their time decay response to temperature, as shown in Figure 12. To increase yield and minimize scrap material costs, it is desirable to be able to sort and bin the resulting sensor elements 14 before they are fully assembled with the optical light guides.

[0117] In another embodiment, a final batch of fluorescent material is deposited into the sensor cap or onto a target substrate and then solidified, thereby forming the sensor element 14 within the sensor cap.

[0118] Correction for batch-to-batch variation In an embodiment, the method produces sensor elements after the original batch that have the same calibration accuracy as the original batch of sensor elements.

[0119] Due to process variations during manufacturing, each batch of bulk phosphor powder will inevitably have a slightly different time fade vs. temperature characteristic. This is undesirable because it means that the fluorescent sensor element produced with each new batch will behave differently. For example, at a given temperature, it may have a different time fade than the previous batch, and therefore must be calibrated differently. Calibrating each individual sensor is inefficient and impractical. Thus, a method is required to tune each new batch of bulk fluorescent material to match performance characteristics from the previously produced batch.

[0120] In an embodiment, the method described below for fine tuning batches of phosphor material is used to compensate for batch-to-batch variations in producing large quantities of phosphor powder. By producing two or more batches of phosphor powder with different particle sizes and dopant concentrations, and by sampling and adjusting the batches, new batches can be fine-tuned to behave with the same fluorescence time decay vs. temperature characteristics as the previously produced batch. In this way, sensor elements are produced over time with the same calibration accuracy as the original batch.

[0121] Example method Referring to FIG. 12, in an embodiment, with the goal of maximizing the number of sensor elements produced that fit within bin D, the sensor elements are manufactured by repeating the following steps: Providing and mixing a batch of phosphor material; and Selecting bin values ​​of a given precision that represent a desired time decay for the temperature response, with a predefined tolerance. Sample Test 1 obtaining a first sample from the batch; allowing the first sample to coagulate to produce a first set of sensor elements; testing a first set of sensor elements to form a first test result; recording a statistical distribution of the first test results; comparing the first test result to a bin value of a predetermined precision; and Adjusting the batch of fluorescent material based on the results of the pre-test by adding and mixing additional material into the batch. Sample Test 2 obtaining a (second) sample from the adjusted batch; allowing the sample to coagulate to produce a second set of sensor elements; testing a second set of sensor elements to form second test results; recording the statistical distribution of the test results; comparing the second test result to a predetermined precision bin value; determining whether a majority of the sensor elements fall into a desired bin (e.g., bin D in FIG. 12); and If the majority of the sensor elements fall within the desired bin, solidifying the entire batch of fluorescent material.

[0122] Batch adjustments are made to correct for both offset and gradient errors. Offset adjustments occur when the time decay versus time response needs to be corrected in one direction and is a uniform offset applied across the entire temperature sensing range.

[0123] The slope error is necessary to correct for changes in the time decay versus temperature behavior over the temperature range, with the offset at low temperatures being different than the offset at high temperatures.

[0124] Performing a batch offset adjustment Batch adjustment to correct for offset errors may be accomplished by any combination of the following methods: adding more phosphor powder with the same chemical composition but larger particle size to shift the temperature response down; adding more phosphor powder with the same chemical composition but smaller particle size to shift the temperature response up; Adding less filler material to shift the temperature response down; and Add more filler material and shift to higher temperature response.

[0125] The filler material is typically an inorganic, transparent powder such as a glass or crystalline material of similar particle size to the phosphor powder, or smaller.

[0126] Performing batch gradient set adjustment Batch adjustments to correct gradient errors require the addition of more material with different dopant concentrations. For example: Shifting the slope to be more positive, reading higher at higher temperatures, by adding more phosphor powder with the same amount but a higher dopant concentration; and By adding more phosphor powder with the same chemical composition but lower dopant concentration, the slope is shifted to be more negative, reading lower at higher temperatures.

[0127] In this manner, by adjusting the batch ratio, both the offset and slope can be corrected to match the time decay of the current batch to the temperature characteristic to the time decay of the initial batch to the temperature characteristic.

[0128] The goal of the method is to maximize the number of sensor elements 14 manufactured that fall into bin D. For example, after sample test 1, the first test results are compared to a given accuracy bin value and the majority of the sensor elements may fall into bins B and C. After conditioning and sample test 2, the majority of the sensor elements may fall into bins C and D. After final conditioning and sample test 3, the majority of the sensor elements will fall into bin D.

[0129] In an embodiment, the sensor elements are disks.During a testing step, a number of disks are selected from the batch and tested to determine the statistical distribution of the batch.

[0130] In an embodiment, the method includes testing the samples to determine if the majority of the samples fall within the parameters at a bin value of a predetermined precision. For example, the precise bin value may be 49.95 degrees Celsius to 50.05 degrees Celsius. The samples may be tested by placing them in a precision dry well calibrator and setting the reference temperature at 50.00 degrees Celsius. A fiber optic light guide is placed in contact with each sample and its temperature is measured and recorded in a spreadsheet. A statistically significant number of samples, for example 20 sensor elements, are tested. A histogram is generated in the spreadsheet showing the temperature distribution of the samples. This distribution is typically Gaussian in nature and has a peak around which most of the samples are read. The peak value is then compared to a calibration reference temperature of 50.00 degrees Celsius. By subtracting the reference temperature from the peak of the Gaussian distribution, an offset error value is determined. This offset error value is the offset that needs to be corrected via a batch adjustment process.

[0131] The following examples show examples of batch adjustment via offset adjustment and batch adjustment via gradient adjustment.

[0132] Offset Example: For example, in an embodiment where the reference temperature is 50.00 degrees Celsius, if the time decay of the Gaussian peak corresponds to a temperature of 49.50 degrees Celsius, then the batch needs to be adjusted to shift to a higher temperature of 0.5 degrees Celsius. This adjustment can be achieved in a variety of ways, such as by adding more phosphor material of the same type but smaller particle size distribution, or by adding a filler material. If more phosphor powder of a different particle size is added, the amount of material to be added next is determined in proportion to the difference in temperature response in the two batches. If a filler material is added, the amount is determined through iteration and experience. Two or more iterations can be performed to adjust the batch to obtain the Gaussian peak temperature to match the reference temperature.

[0133] Gradient Example: For example, in an embodiment where the reference temperature is 50.00 degrees Celsius, a second calibration point may be similarly tested at a higher temperature, such as 200.00 degrees Celsius, to correct for the gradient error. If the Gaussian peak near 200.00 degrees Celsius indicates a different offset error than that determined at 50.00 degrees Celsius, a gradient adjustment must also be made. This may be accomplished by adding phosphor powder of the same type but different dopant concentration. The amount of material to add is determined in proportion to the difference in gradient characteristics in the two batches.

[0134] Each bin of sorted sensor elements will have the same accuracy characteristics. The method produces multiple sensor elements from the same bin. In embodiments, the sensor elements can be mass produced with repeatable fluorescence time decay characteristics and maximum yield within the bin of the desired accuracy. This allows for mass production of temperature probes with the desired accuracy.

[0135] Figure 12 shows a histogram of the grouped bins. If a high accuracy probe is desired, sensor elements from bin D are selected. If lower accuracy is acceptable, sensor elements from other bins may be selected.

[0136] Batch material adjustment The method includes adjusting the composition of the batch materials to adjust the behavior of the phosphor matrix, adjusting and correcting the time fade readings from batch to batch (e.g., from sample test 1 to sample test 2) in two optional ways. The first option is by adding a filler material to the phosphor powder to change the density and concentration of the phosphor powder. The second option is by introducing a second phosphor powder of a different batch but of similar chemical composition and adjusting its mix ratio to the first phosphor powder.

[0137] First option: Add filler material to the phosphor powder

[0138] In an embodiment, the composition of the batch material is adjusted by modifying the density and concentration of the powder, for example by introducing inorganic filler materials of similar or smaller particle size than the phosphor powder.

[0139] This option shifts the time fade characteristics of the bulk matrix material. Generally, higher density results in longer time fade and lower temperature readings. Adding, for example, 10% filler material can shift the temperature response by 0.2 degrees Celsius to 2.0 degrees Celsius higher depending on the phosphor powder.

[0140] In embodiments, the inorganic filler may be a glass powder or a crystalline powder. Glass powder is acceptable for low temperature operation, while crystalline powder is preferred for high temperature operation. Examples of such materials are borosilicate glass, fused silica, diamond, YAG, and others.

[0141] Second option: Add a second batch of phosphor powder with a different dopant concentration or particle size than the original phosphor powder.

[0142] In an embodiment, the composition of the batch material is adjusted by introducing a second phosphor powder of a different batch but of similar chemical composition and adjusting its mix ratio relative to the phosphor powder of the first batch.

[0143] The second batch of material can be made with a larger or smaller average particle size than the first batch. Larger particle sizes generally result in brighter, more efficient fluorescence, as well as longer time decay values ​​and lower temperature readings.

[0144] The second material can also be doped with different dopant concentrations, for example if the fluorescent material is YAG-Er, the concentration of Er can be adjusted from 0.1 to 20% by weight to shift the time fade response.

[0145] Clot samples and batches

[0146] In an embodiment, the method solidifies the sample and substantially all of the batch by sintering the compacted powdered batch material in a controlled atmospheric environment for a predetermined period of time and within a predetermined temperature range.

[0147] Compressed and sintered phosphor solids have the following advantages: It is a solid structure that can be processed into any desired shape; High density for increased stability against degraded gases in high temperature environments; The cut individual sensor disks have a more consistent time decay response due to a more uniform and controlled density throughout the bulk solid; and By mixing powder batches in different ratios of bulk powder materials with different particle size distributions or different dopant concentrations, the time decay to temperature response can be finely tuned.

[0148] In an embodiment, the fluorescent sensor element is a phosphor powder-based sensor element, which is sintered without the addition of fillers.

[0149] In another embodiment, a filler is added to the phosphor powder and mixed to provide a phosphor material that is then compressed under high pressure into a green object having a solid, rigid shape. The green object is then sintered at high temperature. The compressed phosphor material can be sintered in a controlled atmosphere environment. For example, sintering of doped YAG can be performed in an inert nitrogen environment or in vacuum. Alternatively, firing in air with oxygen present maximizes oxygen diffusion into the crystal and reduces the time required for annealing.

[0150] For example, a fluorescent sensor object made from doped YAG may be sintered at a temperature ranging from about 1500 degrees Celsius to about 1900 degrees Celsius for about 2 to about 24 hours, and then annealed at a lower temperature ranging from about 800 degrees Celsius to about 1400 degrees Celsius for about 2 to about 48 hours. If the sensor is to operate in an atmospheric environment, annealing is ideally performed in air with oxygen present. In the case of doped YAG, annealing by cycling at about 800 degrees Celsius to about 1400 degrees Celsius for many hours or many days improves oxygen saturation and helps stabilize ionic charge transfer, which reduces the effects of time-fading hysteresis.

[0151] When an oxygen-containing filler, such as silicon dioxide, is added and sintering is carried out in air, the sintering time can be completed in as little as about 2 hours without the need for further annealing. Thus, the addition of filler also reduces manufacturing process time.

[0152] The final pressed and sintered product ideally has greater than 90% of the full single crystal solid density.

[0153] The compressed powder object is sintered at a predetermined temperature range and duration, which may vary depending on the powder material. By increasing the sintering time, the grain structure will eventually form a single crystal solid. In some embodiments, this is desirable because solid crystals are very stable mechanically. However, for materials such as rare earth doped YAG, sintering to the point of an optically transparent single crystal solid reduces the fluorescence efficiency. Only a small fraction of the excitation light is absorbed by the crystal lattice and tends to travel through the crystalline material. Sintering to the point of only a polycrystalline grain structure improves the fluorescence efficiency by providing better diffusion and absorption of the excitation light, resulting in a thinner sensor element structure.

[0154] In an embodiment, a filler material is added to the phosphor powder prior to pressing and sintering to produce the following beneficial characteristics: a. Improved densification of bulk materials at the overall lower sintering temperatures required to bond the materials. This is important because many fluorescent materials degrade irreversibly when exposed to high temperatures. There are also cost and processing time advantages to this. b. A stronger resulting material matrix is ​​formed that is essentially ceramic. Thus, the stronger material is less likely to crack and is easier to machine, polish, and work with after dicing. c. Improved chemical inertness, as the filler material coats and isolates the fluorescent material from its chemical environment. d. Improved ability to fuse and splice the ends of optical fibers. For example, YAG phosphor powder with SiO2 additive can be plasma fused to the end of a fused silica optical fiber. e. By adjusting the percentage of additive, the time fade response can be shifted, allowing fine tuning of the response from batch to batch as described above (or a second inert additive such as diamond powder may also be present to aid in this effort). f. The time decay behavior of some solid crystal structures is not repeatable with temperature due to ionic charge transfer (and reversible color center evolution) that affects the fluorescence mode, while the presence of additives helps stabilize the fluorescence response. g. Finally, additional additives may be readily fused and bonded onto the surface of the sintered and shaped sensor element to provide further protection from the surrounding chemical environment and / or aid in bonding to a substrate or optical fiber, as in FIG. 10.

[0155] In an embodiment, rare earth doped YAG phosphor powder (without filler) can be sintered into a solid structure and diced into a disk shape.

[0156] The pressed shape of the solid structure may be a plate or rod. Sintering can result in a partially polycrystalline or fully single crystalline composition in the solid structure. The solid structure is then machined or diced into the desired sensor element shape (e.g., a disk).

[0157] In an embodiment, the glass phosphor powder matrix is ​​mixed to provide the phosphor material, which is pressurized under high pressure (at least 5 tons / inch 2 ) and deposited and / or pressed into the cap or onto the target substrate. A high temperature sintering and annealing process is then performed on the cap or target assembly. Thus, the sintered material also forms a mechanical bond with the cap or target substrate. In an embodiment, a filler material is added to lower the sintering temperature of the mixture. For example, a low melting temperature glass powder, with a melting point of about 700° C., can be used with a magnesium fluorogermanate based phosphor to produce a fluorescent sensor element with an operating temperature of up to 600° C.

[0158] In embodiments, the particle size of the filler powder is similar to or smaller than the phosphor particle size. Nanoparticulate fillers or nanoparticulate phosphors may be used.

[0159] 13, the fluorescent temperature sensor 10 is part of a phosphor temperature measurement apparatus generally designated 100. The apparatus 100 includes a light source 102, a light detector 104, such as, but not limited to, a photodetector, an analog to digital converter 106, a microprocessor 110, and a printed circuit board 108 having a memory 112. The memory 112 has instructions for instructing the processor to determine a temperature based on the optical signal from the fluorescent sensor element, which is then transmitted from the printed circuit board 108 as an electronic digital signal.

[0160] While example embodiments have been described with what are presently believed to be examples of the most practical and / or preferred embodiments possible, it should be understood that the description is not limited to the disclosed embodiments, but on the contrary, is intended to cover various modifications and equivalent arrangements falling within the spirit and scope of the example embodiments. Those skilled in the art will recognize, or be able to ascertain using no more than routine experimentation, many equivalents to the specific example embodiments described in detail herein. Such equivalents are intended to be encompassed by the claims appended hereto or as later filed.

Claims

1. 1. A fluorescent sensor device for measuring a parameter of an object, comprising: a phosphor powder in a doped host, the doped host comprising a host doped with a dopant, the phosphor powder absorbing excitation light and emitting radiation light to produce a fluorescent response, the fluorescent response having a time decay response indicative of a parameter of the object; an inorganic filler powder, the inorganic filler powder being substantially optically transparent to the excitation light and the emitted light and capable of stabilizing the fluorescent response; The fluorescent sensor element is formed by mixing the phosphor powder and the inorganic filler powder to form a mixture, then depositing and / or pressing the mixture to form a green body, and further solidifying the green body to form the fluorescent sensor element.

2. 2. The fluorescent sensor element of claim 1 having a predetermined time decay response, said time decay response being adjusted according to the concentration of said inorganic filler powder.

3. The inorganic filler powder is silicon dioxide (SiO 2 ), glass, borosilicate glass, diamond, yttrium orthosilicate (YSO), yttria stabilized zirconia (YSZ), yttrium oxide (Y 2 O 3 ), yttrium orthovanadate (YVO 4 ), yttrium aluminum garnet (YAG), yttrium aluminum perovskite (YAP), yttrium aluminum monoclinic (YAM), yttrium gallium garnet (YGG), aluminum oxide (Al 2 O 3 ), lanthanum oxysulfide (La 2 O 2 S), gadolinium sulfide (Gd 2 O 2 S), magnesium oxide (MgO), germanium oxide (GeO 2 ), titanium oxide (TiO 2 ), and magnesium fluoride (MgF 2 2. The fluorescent sensor element according to claim 1, wherein the fluorescent sensor element is at least one of:

4. The base material may be yttrium orthosilicate (YSO), yttria-stabilized zirconia (YSZ), yttrium oxide (Y 2 O 3 ), yttrium orthovanadate (YVO 4 ), yttrium aluminum garnet (YAG), yttrium aluminum perovskite (YAP), yttrium aluminum monoclinic (YAM), yttrium gallium garnet (YGG), aluminum oxide (Al 2 O 3 ), lanthanum oxysulfide (La 2 O 2 S), gadolinium sulfide (Gd 2 O 2 S), magnesium titanate (Mg 2 TiO 4 ), magnesium oxide (3.5MgO), magnesium fluorogermanate (0.5MgF 2 GeO 2 ), magnesium fluorogermanate (Mg 4 FGeO 6 ), and potassium silicofluoride (K 2 SiF 6 4. The fluorescent sensor element according to claim 1, wherein the fluorescent sensor element is at least one of the following:

5. 5. The fluorescent sensor element according to claim 1, 3 or 4, wherein the dopant is at least one of cerium (Ce), chromium (Cr), dysprosium (Dy), erbium (Er), europium (Eu), gadolinium (Gd), holmium (Ho), manganese (Mn), neodymium (Nd), praseodymium (Pr), samarium (Sm), terbium (Tb), titanium (Ti), thulium (Tm), and ytterbium (Yb).

6. 2. The fluorescent sensor element of claim 1, wherein the inorganic filler powder is an oxygen-containing filler powder.

7. 7. The fluorescent sensor element according to claim 6, wherein the oxygen-containing filler powder is one of a glass powder and a borosilicate glass powder.

8. The glass powder is Special glass powders tailored to closely match the melting temperature, transparency, and thermal expansion coefficient of the doped host; or 8. The fluorescent sensor element according to claim 7, which is any special glass powder having a melting temperature lower than that of the doped host.

9. The oxygen-containing filler powder may be yttrium orthosilicate (YSO), yttria-stabilized zirconia (YSZ), yttrium oxide (Y 2 O 3 ), yttrium orthovanadate (YVO 4 ), yttrium aluminum garnet (YAG), yttrium aluminum perovskite (YAP), yttrium aluminum monoclinic (YAM), yttrium gallium garnet (YGG), aluminum oxide (Al 2 O 3 ), lanthanum oxysulfide (La 2 O 2 S), gadolinium sulfide (Gd 2 O 2 S), magnesium oxide (MgO), germanium oxide (GeO 2 ), and titanium oxide (TiO 2 7. The fluorescent sensor element according to claim 6, wherein the fluorescent sensor element is at least one of the following:

10. 2. The fluorescent sensor element of claim 1, wherein the inorganic filler powder is silicon dioxide powder.

11. 2. The fluorescent sensor element according to claim 1, wherein the inorganic filler powder is diamond powder.

12. The fluorescent sensor element according to claim 1 , wherein the inorganic filler powder is a matrix powder.

13. The fluorescent sensor element according to claim 1 , wherein the solidification is any one of sintering, curing, drying and baking.

14. 10. The fluorescent sensor element of claim 1 having a density greater than about 90% of the solid phase density.

15. The mixture is at least about 5 tons / in 2 Preferably at a pressure of about 100 tons / inch 2 2. The fluorescent sensor element according to claim 1, wherein the fluorescent sensor element is pressed under a pressure of 0.1 to 1.

0.

16. 10. The fluorescent sensor element of claim 1, wherein the green body is solidified by firing in a controlled atmospheric environment, the controlled atmospheric environment being one of an inert gas atmosphere, an oxygen atmosphere, or a vacuum.

17. The fluorescent sensor element of claim 1 , wherein the parameter of the object is one of temperature, pressure, oxygen concentration, pH, and humidity.

18. 1. A fluorescent sensor for measuring a parameter of an object, comprising: an optical light guide having a distal end; a fluorescent sensor element formed on the distal end or on the object; the optical light guide is operatively coupled to a light source that transmits excitation light along the optical light guide toward the fluorescent sensor element when the distal end is in proximity to or in contact with the object to generate a fluorescent response of the fluorescent sensor element by absorbing the excitation light and emitting emission light, the fluorescent response being characterized by a time decay response indicative of a parameter of the object; The fluorescent sensor element comprises: a doped host phosphor powder, the doped host comprising a host doped with a dopant, the phosphor powder being capable of absorbing the excitation light and emitting radiation light; an inorganic filler powder, the inorganic filler powder being substantially optically transparent to the excitation light and the emitted light and capable of stabilizing the fluorescent response; The fluorescent sensor element is formed by mixing the phosphor powder and the inorganic filler powder to form a mixture, then depositing and / or pressing the mixture to form a green body, and further solidifying the green body to form the fluorescent sensor element.

19. 1. A fluorescent sensor apparatus for measuring a parameter of an object, comprising: an optical light guide having a distal end; a fluorescent sensor element formed on the distal end or on the object; a light source operatively coupled to the optical light guide to transmit excitation light along the optical light guide toward the fluorescent sensor element when the distal end is in proximity to or in contact with the object, the fluorescent sensor element absorbing the excitation light and emitting emitted light to generate a fluorescent response of the fluorescent sensor element, the fluorescent response being characterized by a time decay response indicative of a parameter of the object; a detector operatively coupled to the optical light guide for measuring the time decay response; The fluorescent sensor element comprises: a doped host phosphor powder, the doped host comprising a host doped with a dopant, the phosphor powder capable of absorbing the excitation light and emitting the emission light; an inorganic filler powder, the inorganic filler powder being substantially optically transparent to the excitation light and the emitted light and capable of stabilizing the fluorescent response; a fluorescent sensor device, the fluorescent sensor element being formed by mixing the phosphor powder and the inorganic filler powder to form a mixture, then depositing and / or pressing the mixture to form a green body, and further solidifying the green body to form the fluorescent sensor element.

Citation Information

Patent Citations

  • Optical measuring techniques

    JP1987501448A

  • Temperature sensor probe and its manufacturing method

    JP2009128144A

  • Fluorescence thermometer and temperature measuring method

    JP2012211848A

  • Fluorescence temperature sensor

    JP2016080457A

  • Thermographic temperature sensor