Method of manufacturing non-aqueous electrolyte secondary battery
The method of pressurizing and depressurizing the battery case during the manufacturing process addresses the challenge of electrolyte impregnation in high-capacity wound electrode bodies, ensuring efficient electrolyte distribution and improved battery characteristics.
Patent Information
- Application Number
- JP2023071323
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Existing methods for manufacturing non-aqueous electrolyte secondary batteries with high-capacity wound electrode bodies face challenges in efficiently impregnating the electrolyte, particularly in the central parts, leading to potential battery characteristic deterioration due to insufficient impregnation.
A manufacturing method involving constructing a battery assembly with a wound electrode body and non-aqueous electrolyte, then pressurizing the battery case to 0.4 MPa or more for 20 minutes or more, followed by depressurization, to promote electrolyte impregnation into the electrode body.
This method ensures efficient impregnation of the non-aqueous electrolyte into the wound electrode body, reducing the risk of battery characteristic deterioration and enhancing manufacturing efficiency.
Smart Images

Figure 2024157157000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a non-aqueous electrolyte secondary battery. [Background technology]
[0002] Conventionally, in manufacturing a nonaqueous electrolyte secondary battery including an electrode assembly, a nonaqueous electrolyte, and a battery case that contains the electrode assembly and the nonaqueous electrolyte, studies have been made on how to efficiently inject the nonaqueous electrolyte into the battery case and how to quickly permeate the nonaqueous electrolyte into the electrode assembly. Related prior art documents include Patent Documents 1 to 3.
[0003] For example, Patent Document 1 describes that in a liquid injection step of injecting a nonaqueous electrolyte into a battery case, the pressure inside the battery case is reduced to a low pressure state and maintained for a certain period of time, and then the pressure is gradually increased to a high pressure state, thereby enabling the nonaqueous electrolyte to be filled in a short period of time. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-033114 A [Patent Document 2] JP 2007-165170 A [Patent Document 3] Patent No. 5683938 Summary of the Invention [Problem to be solved by the invention]
[0005] However, according to the study by the present inventors, when applying the above technology to a non-aqueous electrolyte secondary battery equipped with a recent high-capacity electrode body, particularly a wound electrode body, there is still room for improvement. That is, since only both ends in the winding axis direction of the wound electrode body are opened, the non-aqueous electrolyte is supplied to the inside only from the both ends. In addition, in recent high-capacity wound electrode bodies, the length (width) in the winding axis direction is, for example, 20 cm or more, which is significantly longer than conventional ones. For this reason, the central part of the winding axis direction of the wound electrode body is particularly difficult to impregnate with the non-aqueous electrolyte, which causes a problem that the time required for impregnation during manufacturing becomes excessively long or the impregnation is insufficient, resulting in a deterioration of the battery characteristics.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a method for manufacturing a nonaqueous electrolyte secondary battery that can promote impregnation of a nonaqueous electrolyte into a wound electrode body. [Means for solving the problem]
[0007] According to the present invention, there is provided a method for producing a non-aqueous electrolyte secondary battery comprising: a wound electrode assembly including a positive electrode and a negative electrode; a non-aqueous electrolyte; and a battery case that contains the wound electrode assembly and the non-aqueous electrolyte, the positive electrode comprising a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, the negative electrode comprising a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector, the negative electrode comprising a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector, the width of the negative electrode active material layer in the winding axis direction being 20 cm or more. This production method includes a construction step of constructing a battery assembly by containing the wound electrode assembly and the non-aqueous electrolyte in the battery case, and a pressurization step of, after the construction step, disposing the battery assembly in a chamber whose internal pressure is adjustable with the battery case open, pressurizing the pressure in the chamber until the pressure in the battery case becomes 0.4 MPa or more, and maintaining the state in which the pressure in the battery case is 0.4 MPa or more for 20 minutes or more.
[0008] By including the pressurizing step, the impregnation of the nonaqueous electrolyte into the wound electrode body can be promoted. Therefore, even in the case of a wound electrode body with a high capacity in recent years, the nonaqueous electrolyte can be permeated to the center in the winding axis direction in a relatively short time compared to a case where the pressurizing step is not included. Therefore, the battery can be manufactured efficiently, and the deterioration of the battery characteristics due to insufficient impregnation of the nonaqueous electrolyte can be suppressed. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view that illustrates a nonaqueous electrolyte secondary battery according to one embodiment. [Diagram 2] FIG. 2 is a schematic vertical cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a schematic cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 4 is a perspective view that illustrates a schematic view of an electrode assembly attached to a sealing plate. [Diagram 5] FIG. 5 is a perspective view that illustrates a schematic diagram of a wound electrode body. [Figure 6] FIG. 6 is a schematic diagram showing the configuration of a wound electrode body. [Figure 7] FIG. 7 is a flow chart of a manufacturing method according to one embodiment. [Figure 8] FIG. 8 is a schematic diagram of a pressure adjusting device according to one embodiment. [Figure 9] FIG. 9 is a graph showing the progress of pressure in the pressurizing step according to one embodiment. [Figure 10] FIG. 10 is a graph showing the relationship between the impregnation rate and the applied pressure in Test Example I. [Figure 11] FIG. 11 is a graph showing the relationship between the impregnation rate and the pressure retention time in Test Example I. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, some preferred embodiments of the technology disclosed herein will be described with reference to the drawings. It should be noted that matters other than those specifically mentioned in this specification and necessary for carrying out the present invention (for example, the general configuration and manufacturing process of a non-aqueous electrolyte secondary battery that does not characterize the present invention) can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the field. In this specification, the expression "A to B" indicating a range includes the meaning of "greater than A" and "smaller than B" as well as the meaning of A or more and B or less. In addition, in this specification, "pressure" refers to a gauge pressure based on atmospheric pressure (i.e., the difference obtained by subtracting atmospheric pressure from absolute pressure).
[0011] In this specification, the term "nonaqueous electrolyte secondary battery" refers to a general electricity storage device that can be repeatedly charged and discharged by the movement of charge carriers between a positive electrode and a negative electrode via a nonaqueous electrolyte. The concept of nonaqueous electrolyte secondary battery includes storage batteries such as lithium ion secondary batteries and capacitors such as lithium ion capacitors and electric double layer capacitors.
[0012] <Battery 100> First, the configuration of a nonaqueous electrolyte secondary battery manufactured by the technology disclosed herein will be described. FIG. 1 is a perspective view of a nonaqueous electrolyte secondary battery (hereinafter, simply referred to as a battery) 100. FIG. 2 is a schematic longitudinal sectional view taken along line II-II in FIG. 1. FIG. 3 is a schematic transverse sectional view taken along line III-III in FIG. 1. In the following description, the symbols L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom, and the symbols X, Y, and Z in the drawings represent the short side direction, the long side direction perpendicular to the short side direction, and the height direction perpendicular to the short side direction and the long side direction, respectively, of the battery 100. However, these directions are merely for the convenience of description, and do not limit the installation form of the battery 100 in any way.
[0013] 2, the battery 100 includes a battery case 10, an electrode assembly 20, a positive electrode terminal 30, a negative electrode terminal 40, and a non-aqueous electrolyte (not shown). The battery 100 here is a lithium ion secondary battery. The battery 100 is preferably a lithium ion secondary battery.
[0014] The battery case 10 is a housing that contains the electrode assembly 20 and the nonaqueous electrolyte. As shown in FIG. 1, the battery case 10 has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. The material of the battery case 10 may be the same as that used conventionally, and is not particularly limited. The battery case 10 is preferably made of a metal, and more preferably made of, for example, aluminum, an aluminum alloy, iron, an iron alloy, or the like. As shown in FIG. 2, the battery case 10 has an exterior body 12 having an opening 12h, and a sealing plate (lid) 14 that closes the opening 12h. The battery case 10 preferably has an exterior body 12 and a sealing plate 14.
[0015] As shown in Fig. 1, the exterior body 12 includes a substantially rectangular bottom wall 12a, a pair of long side walls 12b extending from the long side of the bottom wall 12a and facing each other, and a pair of short side walls 12c extending from the short side of the bottom wall 12a and facing each other. The long side walls 12b and the short side walls 12c are examples of side walls extending from the edge of the bottom wall toward the opening. The area of the long side walls 12b is larger than the area of the short side walls 12c. In this specification, the term "substantially rectangular" includes not only a perfect rectangular shape (rectangular shape), but also a shape in which the corners connecting the long and short sides of the rectangle are rounded or a shape with a notch at the corner.
[0016] As shown in Fig. 1, the sealing plate 14 has a substantially rectangular shape in a plan view. As shown in Fig. 2, the sealing plate 14 is attached to the exterior body 12 so as to close the opening 12h of the exterior body 12. The sealing plate 14 faces the bottom wall 12a of the exterior body 12. The battery case 10 is integrated by joining (e.g., welding) the sealing plate 14 to the periphery of the opening 12h of the exterior body 12. The battery case 10 is hermetically sealed (sealed).
[0017] As shown in FIG. 2, the sealing plate 14 is provided with a liquid injection hole 15, a gas exhaust valve 17, and two terminal extraction holes 18 and 19. The liquid injection hole 15 is a through hole penetrating the sealing plate 14 in the thickness direction (height direction Z). The liquid injection hole 15 is for injecting a non-aqueous electrolyte after the sealing plate 14 is assembled to the exterior body 12. The sealing plate 14 is preferably provided with the liquid injection hole 15. The liquid injection hole 15 is sealed with a sealing member 16 after the non-aqueous electrolyte is injected. The gas exhaust valve 17 is configured to break when the pressure inside the battery case 10 reaches or exceeds a predetermined value, thereby discharging the gas inside the battery case 10 to the outside. The terminal extraction holes 18 and 19 are formed at both ends of the sealing plate 14 in the long side direction Y (the left end and the right end in FIG. 2). The terminal extraction holes 18 and 19 penetrate the sealing plate 14 in the thickness direction (height direction Z). The terminal withdrawal holes 18, 19 each have an inner diameter large enough to allow the positive electrode terminal 30 and the negative electrode terminal 40 to be inserted therethrough before being attached to the sealing plate 14 (before being crimped).
[0018] The positive electrode terminal 30 and the negative electrode terminal 40 are each fixed to the sealing plate 14 of the battery case 10. The positive electrode terminal 30 is disposed on one side of the sealing plate 14 in the long side direction Y (the left side in Figs. 1 and 2). The negative electrode terminal 40 is disposed on the other side of the sealing plate 14 in the long side direction Y (the right side in Figs. 1 and 2). As shown in Fig. 2, the positive electrode terminal 30 extends from the inside to the outside of the sealing plate 14 through the terminal pull-out hole 18. The negative electrode terminal 40 extends from the inside to the outside of the sealing plate 14 through the terminal pull-out hole 19. The positive electrode terminal 30 and the negative electrode terminal 40 are preferably attached to the sealing plate 14. Here, the positive electrode terminal 30 and the negative electrode terminal 40 are crimped to the peripheral portion surrounding the terminal pull-out holes 18 and 19 of the sealing plate 14 by crimping. The positive electrode terminal 30 and the negative electrode terminal 40 have crimping portions 30c, 40c formed at their ends on the exterior body 12 side (the lower ends in FIG. 2).
[0019] 2, the positive electrode terminal 30 is electrically connected to the positive electrode 22 (see FIG. 6, specifically, the positive electrode tab group 23) of the electrode body group 20 via the positive electrode current collecting portion 50 inside the battery case 10. The positive electrode terminal 30 is insulated from the sealing plate 14 by an insulating member 80 and a gasket 90. The positive electrode terminal 30 is preferably made of metal, and more preferably made of, for example, aluminum or an aluminum alloy.
[0020] The negative electrode terminal 40 is electrically connected to the negative electrode 24 (see FIG. 6, specifically, the negative electrode tab group 25) of the electrode body group 20 through the negative electrode current collector 60 inside the battery case 10. The negative electrode terminal 40 is insulated from the sealing plate 14 by an insulating member 80 and a gasket 90. The negative electrode terminal 40 is preferably made of a metal, and more preferably made of, for example, copper or a copper alloy. The negative electrode terminal 40 may be configured by joining two conductive members together. For example, the portion of the negative electrode terminal 40 connected to the negative electrode current collector 60 may be made of copper or a copper alloy, and the portion exposed on the outer surface of the sealing plate 14 may be made of aluminum or an aluminum alloy.
[0021] A plate-shaped positive electrode external conductive member 32 and a plate-shaped negative electrode external conductive member 42 are attached to the outer surface of the sealing plate 14. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are members to which bus bars are attached when electrically connecting a plurality of batteries 100 to each other. The positive electrode external conductive member 32 is electrically connected to the positive electrode terminal 30. The negative electrode external conductive member 42 is electrically connected to the negative electrode terminal 40. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are insulated from the sealing plate 14 by an external resin member 92. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are preferably made of metal, and more preferably made of aluminum or an aluminum alloy, for example. However, the positive electrode external conductive member 32 and the negative electrode external conductive member 42 are not essential and may be omitted in other embodiments.
[0022] As shown in FIG. 2, the electrode assembly group 20 is accommodated inside the battery case 10 (more specifically, inside the exterior body 12). FIG. 4 is a perspective view that shows a schematic view of the electrode assembly group 20 attached to the sealing plate 14. The electrode assembly group 20 has three wound electrode bodies 20a, 20b, and 20c here. When a plurality of wound electrode bodies 20a, 20b, and 20c are arranged inside one battery case 10, the wound electrode body 20b located in the center of the short side direction X may be difficult to be impregnated with the nonaqueous electrolyte. Therefore, it is particularly effective to apply the technology disclosed herein. However, the number of wound electrode bodies arranged inside one battery case 10 is not particularly limited, and may be two or more (plural), or may be one. The electrode assembly group 20 may be arranged inside the battery case 10 in a state where it is covered with an insulating electrode body holder. In other words, an electrode assembly holder may be interposed between the electrode assembly group 20 and the battery case 10 (specifically, the exterior body 12). The electrode assembly holder is preferably made of resin.
[0023] FIG. 5 is a perspective view showing the wound electrode body 20a. FIG. 6 is a schematic diagram showing the configuration of the wound electrode body 20a. In the following, the wound electrode body 20a will be described in detail as an example, but the wound electrode bodies 20b and 20c can also be configured in a similar manner. The wound electrode body 20a includes a positive electrode 22 and a negative electrode 24. As shown in FIG. 6, the wound electrode body 20a is preferably configured by stacking a strip-shaped positive electrode 22 and a strip-shaped negative electrode 24 with a strip-shaped separator 26 interposed therebetween and winding the strip-shaped positive electrode 22 and the strip-shaped negative electrode 24 around the winding axis WL. Although not particularly limited, the number of windings (number of turns) of the wound electrode body 20a is preferably 20 turns or more, more preferably 30 turns or more, and even more preferably 50 turns or more, and may be, for example, 150 turns or less, 100 turns or less. As the number of windings increases, it becomes more difficult for the nonaqueous electrolyte to permeate the central portion of the wound electrode body 20a (the central portion in the short side direction X and the central portion in the long side direction Y). Therefore, it is particularly effective to apply the technology disclosed herein.
[0024] As can be seen from FIG. 2 and FIG. 6, the wound electrode body 20a is disposed inside the battery case 10 with the winding axis WL oriented along the bottom wall 12a (in other words, oriented substantially parallel to the long side direction Y). The winding axis WL direction coincides with the long side direction Y. The wound electrode body 20a is disposed inside the battery case 10 with the winding axis WL oriented perpendicular to the short side wall 12c. A pair of end faces (opening ends) of the wound electrode body 20a in the winding axis WL direction face a pair of short side walls 12c of the exterior body 12, respectively. Both end faces of the wound electrode body 20a in the winding axis WL direction serve as inlets through which the nonaqueous electrolyte flows in. In such a case, it is particularly effective to apply the technology disclosed herein.
[0025] Here, the battery 100 has a so-called horizontal tab structure in which the positive electrode tab group 23 and the negative electrode tab group 25 are located at both ends of the wound electrode body 20a in the winding axis WL direction (left and right in Figs. 2 and 4). However, in other embodiments, the battery 100 may have a so-called upper tab structure in which the positive electrode tab group 23 and the negative electrode tab group 25 are located at one end of the wound electrode body 20a in the winding axis WL direction (for example, the upper end in Figs. 2 and 4). In this case, the winding axis WL direction may be the same as the height direction Z.
[0026] The wound electrode body 20a preferably has a flat outer shape as shown in Fig. 5. The wound electrode body 20a has a pair of flat portions 20f extending along the long side direction Y (winding axis WL direction) and a pair of curved portions (R portions) 20r connecting the pair of flat portions 20f. The flat portions 20f have a flat outer surface (YZ plane in Fig. 5). The curved portions 20r have a curved outer surface. In this specification, the term "flat outer surface" is not limited to a completely flat surface, and includes cases where there are slight steps, curves, recesses, protrusions, etc. when viewed microscopically.
[0027] 2 and 5, the pair of flat portions 20f face the pair of long side walls 12b of the exterior body 12. The flat portions 20f extend along the long side walls 12b. The pair of curved portions 20r face the bottom wall 12a and the sealing plate 14 of the exterior body 12. As in this embodiment, the wound electrode body 20a is preferably disposed inside the battery case 10 such that the stacking direction (thickness direction) of the positive electrode 22 (see FIG. 6) and the negative electrode 24 (see FIG. 6) in the flat portions 20f coincides with the short side direction X (direction perpendicular to the long side walls 12b).
[0028] Although not particularly limited, in a high-capacity battery 100 used for in-vehicle applications, etc., as shown in FIG. 5, the height Ta of the wound electrode body 20a (the length from the lower end of the curved portion 20r on the bottom wall 12a side to the upper end of the curved portion 20r on the sealing plate 14 side) is preferably 12 cm or less, more preferably 6 to 12 cm, even more preferably 8 to 11 cm, and particularly preferably 9 to 10 cm.
[0029] The positive electrode 22 may be the same as a conventional one, and is not particularly limited. As shown in FIG. 6, the positive electrode 22 has a positive electrode collector 22c, and a positive electrode active material layer 22a and a positive electrode protective layer 22p fixed on at least one surface of the positive electrode collector 22c. However, the positive electrode protective layer 22p is not essential and can be omitted in other embodiments. The positive electrode collector 22c is strip-shaped. The positive electrode collector 22c is made of a conductive metal such as aluminum, an aluminum alloy, nickel, or stainless steel. Here, the positive electrode collector 22c is a metal foil, specifically an aluminum foil.
[0030] A plurality of positive electrode tabs 22t are provided at one end (left end in FIG. 6) in the long side direction Y of the positive electrode collector 22c. The plurality of positive electrode tabs 22t each protrude toward one side (left side in FIG. 6) in the long side direction Y. The plurality of positive electrode tabs 22t protrude in the long side direction Y beyond the separator 26. The plurality of positive electrode tabs 22t are provided at intervals (intermittently) along the longitudinal direction of the positive electrode 22. By providing the plurality of positive electrode tabs 22t, the resistance of the battery 100 can be reduced. Here, the positive electrode tab 22t is a part of the positive electrode collector 22c and is made of metal foil (aluminum foil). It is preferable that the positive electrode tab 22t is a collector exposed portion where the positive electrode active material layer 22a and the positive electrode protective layer 22p are not formed at least in a part and the positive electrode collector 22c is exposed.
[0031] As shown in FIG. 3, the positive electrode tabs 22t are stacked at one end (the left end in FIG. 3) in the long side direction Y to form a positive electrode tab group 23. The positive electrode tabs 22t are stacked and bent so that the outer ends are aligned and curved. This improves the accommodation in the battery case 10 and allows the battery 100 to be made smaller. In addition, the volumetric energy density of the battery 100 can be improved. A positive electrode current collector 50 is attached (more specifically, joined) to the positive electrode tab group 23. The positive electrode tab group 23 is electrically connected to the positive electrode terminal 30 via the positive electrode current collector 50. The positive electrode current collector 50 may be made of the same metal type as the positive electrode current collector 22c, for example, a conductive metal such as aluminum, an aluminum alloy, nickel, or stainless steel. The positive electrode current collector 50 has a joint J with the positive electrode tab group 23 formed therein. The joint J is, for example, a welded joint formed by welding such as ultrasonic welding, resistance welding, or laser welding in a state where a plurality of positive electrode tabs 22t are overlapped.
[0032] As shown in Fig. 6, the positive electrode active material layer 22a is provided in a strip shape along the longitudinal direction of the strip-shaped positive electrode current collector 22c. The positive electrode active material layer 22a contains a positive electrode active material (e.g., lithium transition metal composite oxide) capable of reversibly absorbing and releasing charge carriers. The positive electrode active material layer 22a may further contain any component other than the positive electrode active material, such as a conductive material, a binder, various additive components, and the like. As the conductive material, for example, a carbon material such as acetylene black (AB) can be used. As the binder, for example, polyvinylidene fluoride (PVdF) can be used.
[0033] Although not particularly limited, in a high-capacity battery 100 used for in-vehicle applications, etc., the width of the positive electrode active material layer 22a in the direction of the winding axis WL (average value, excluding the portion formed in the positive electrode tab 22t), in other words, the length Lc in the long side direction Y, is preferably 15 cm or more, more preferably 20 cm or more, and even more preferably 25 cm or more.
[0034] As shown in FIG. 6, the positive electrode protective layer 22p is provided between the positive electrode collector 22c and the positive electrode active material layer 22a in the long side direction Y. Here, the positive electrode protective layer 22p is provided at one end (the left end in FIG. 6) of the positive electrode collector 22c in the long side direction Y. The positive electrode protective layer 22p is provided in a strip shape along the positive electrode active material layer 22a. The positive electrode protective layer 22p contains an inorganic filler (e.g., alumina). The positive electrode protective layer 22p may contain any component other than the inorganic filler, such as a conductive material, a binder, various additive components, and the like. The conductive material and the binder may be the same as those exemplified as those that may be contained in the positive electrode active material layer 22a.
[0035] The negative electrode 24 may be the same as a conventional one, and is not particularly limited. As shown in FIG. 6, the negative electrode 24 has a negative electrode collector 24c and a negative electrode active material layer 24a fixed on at least one surface of the negative electrode collector 24c. The negative electrode collector 24c is strip-shaped. The negative electrode collector 24c is made of a conductive metal such as copper, a copper alloy, nickel, or stainless steel. Here, the negative electrode collector 24c is a metal foil, specifically a copper foil.
[0036] A plurality of negative electrode tabs 24t are provided at one end of the negative electrode current collector 24c in the long side direction Y (the right end in FIG. 6). The plurality of negative electrode tabs 24t each protrude toward one side of the long side direction Y (the right side in FIG. 6). The plurality of negative electrode tabs 24t protrude in the long side direction Y beyond the separator 26. The plurality of negative electrode tabs 24t are provided at intervals (intermittently) along the longitudinal direction of the negative electrode 24. By providing the plurality of negative electrode tabs 24t, the resistance of the battery 100 can be reduced. Here, the negative electrode tab 24t is a part of the negative electrode current collector 24c and is made of metal foil (copper foil). It is preferable that the negative electrode tab 24t is a collector exposed portion where the negative electrode active material layer 24a is not formed at least in a part and the negative electrode current collector 24c is exposed.
[0037] As shown in FIG. 3, the negative electrode tabs 24t are stacked at one end (the right end in FIG. 3) in the long side direction Y to form a negative electrode tab group 25. The negative electrode tabs 24t are stacked and bent so that the outer ends are aligned and curved. This improves the accommodation in the battery case 10 and allows the battery 100 to be made smaller. In addition, the volumetric energy density of the battery 100 can be improved. A negative electrode current collector 60 is attached (more specifically, joined) to the negative electrode tab group 25. The negative electrode tab group 25 is electrically connected to the negative electrode terminal 40 via the negative electrode current collector 60. The negative electrode current collector 60 may be made of the same metal type as the negative electrode current collector 24c, for example, a conductive metal such as copper, a copper alloy, nickel, or stainless steel. A joint J with the negative electrode tab group 25 is formed in the negative electrode current collector 60. The joint J is a welded joint formed by welding such as ultrasonic welding, resistance welding, or laser welding in a state where a plurality of negative electrode tabs 24t are overlapped, similarly to the positive electrode side.
[0038] As shown in Fig. 6, the negative electrode active material layer 24a is provided in a strip shape along the longitudinal direction of the strip-shaped negative electrode current collector 24c. The negative electrode active material layer 24a contains a negative electrode active material (e.g., a carbon material such as graphite, or a silicon-containing material) capable of reversibly absorbing and releasing charge carriers. The negative electrode active material layer 24a may further contain any component other than the negative electrode active material, such as a binder, various additive components, and the like. As the binder, for example, rubbers such as styrene butadiene rubber (SBR) or celluloses such as carboxymethyl cellulose (CMC) can be used.
[0039] The width of the negative electrode active material layer 24a in the winding axis WL direction (average value, excluding the portion formed in the negative electrode tab 24t), in other words, the length La in the long side direction Y, is typically the same as or longer than the length Lc in the long side direction Y of the positive electrode active material layer 22a. The length La is 20 cm or more here from the viewpoint of increasing capacity, etc. The length La is more preferably 25 cm or more. In the wound electrode body 20a, the nonaqueous electrolyte is supplied only from both ends in the long side direction Y (winding axis WL direction). Therefore, the longer the length La, the more difficult it is for the nonaqueous electrolyte to penetrate into the center part in the long side direction Y. Therefore, it is particularly effective to apply the technology disclosed herein. The length La may be, for example, 100 cm or less, 50 cm or less. This allows the effect of the technology disclosed herein to be exerted at a high level.
[0040] As shown in FIG. 6, the separator 26 is a member that insulates the positive electrode active material layer 22a of the positive electrode 22 from the negative electrode active material layer 24a of the negative electrode 24. The width of the separator 26 in the winding axis WL direction, in other words, the length Ls in the long side direction Y, is typically equal to or longer than the length La in the long side direction Y of the negative electrode active material layer 24a. The separator 26 is preferably a resin porous sheet made of a polyolefin resin such as polyethylene (PE) or polypropylene (PP). The separator 26 may have a functional layer such as an adhesive layer or a heat-resistant layer (Heat Resistance Layer: HRL) on the surface of the substrate part made of a resin porous sheet. The configuration of the adhesive layer or the heat-resistant layer may be the same as that of a conventional one. The adhesive layer is a layer containing a binder. The heat-resistant layer is a layer containing an inorganic filler such as alumina, silica, boehmite, magnesia, titania, or the like, and a binder such as PVdF. The heat-resistant layer may also serve as an adhesive layer.
[0041] The nonaqueous electrolyte typically contains a nonaqueous solvent and a supporting salt (electrolyte salt). As the nonaqueous solvent, one or more of those that are known to be usable in nonaqueous electrolyte secondary batteries can be used. Examples of the nonaqueous solvent include organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones. The nonaqueous solvent preferably contains a carbonate. Examples of the carbonate include chain carbonates such as ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), and cyclic carbonates such as propylene carbonate (PC).
[0042] The supporting salt is not particularly limited as long as it contains a charge carrier (typically lithium ion), and one or more of those known to be usable in non-aqueous electrolyte secondary batteries can be used. Examples of the supporting salt include fluorine-containing lithium salts such as LiPF6 and LiBF4. The supporting salt preferably contains LiPF6. The non-aqueous electrolyte may further contain additional components (additives).
[0043] <Manufacturing method of battery 100> FIG. 7 is a flow chart of a manufacturing method according to one embodiment. As shown in FIG. 7, the manufacturing method according to this embodiment includes the following steps: a construction step (step S10); a pressurizing step (step S20); a depressurizing step (step S30); an initial charging step (step S40); and a sealing step (step S50), in this order. However, the depressurizing step (step S30) is optional and may be omitted in other embodiments. Also, the order of the initial charging step (step S40) and the sealing step (step S50) may be reversed. Also, other steps may be included at any stage.
[0044] The construction step (step S10) is a step of constructing a battery assembly 100A by housing an electrode body group 20 (wound electrode bodies 20a, 20b, 20c) and a non-aqueous electrolyte in a battery case 10. This step is typically performed in a glove box under atmospheric pressure and room temperature (for example, about 25°C ± 10°C, 25°C ± 5°C). In addition, in this specification, the term "battery assembly" refers to an intermediate product that has been assembled to a state before the initial charging step (step S40) is performed in the manufacturing process of the battery 100. The order in which the electrode body group 20 and the non-aqueous electrolyte are housed in the battery case 10 is not particularly limited. Here, this step includes an arrangement step (step S11) and an injection step (step S12) in this order.
[0045] The arrangement step (step S11) is a step of arranging the electrode body group 20 (wound electrode bodies 20a, 20b, 20c) inside the battery case 10. In this step, for example, first, as shown in FIG. 4, an assembly is produced in which the sealing plate 14 and the electrode body group 20 are integrated. Next, the electrode body group 20 is accommodated inside the exterior body 12 by fitting the sealing plate 14 into the opening 12h of the exterior body 12. As a result, the wound electrode bodies 20a, 20b, 20c are accommodated inside the exterior body 12 with the winding axis WL oriented along the bottom wall 12a, as shown in FIG. 2. Next, the sealing plate 14 is welded to the periphery of the opening 12h of the exterior body 12 to integrate the exterior body 12 and the sealing plate 14.
[0046] Incidentally, before or after the exterior body 12 and the sealing plate 14 are integrated, moisture within the exterior body 12 (particularly within the electrode assembly 20) may be removed using a heating and drying device, a vacuum drying device, or the like, with the liquid injection hole 15 open. In this case, the heating temperature is preferably set to about 200°C or less, for example, within the range of 50 to 200°C.
[0047] The liquid injection step (step S12) is a step of injecting a nonaqueous electrolyte from the liquid injection hole 15 provided in the sealing plate 14 after the arrangement step (step S11). In this step, for example, a nonaqueous electrolyte is first prepared. Then, a predetermined amount of the nonaqueous electrolyte is injected from the liquid injection hole 15 into the inside of the battery case 10 in which the electrode body group 20 (wound electrode bodies 20a, 20b, 20c) is accommodated. The predetermined amount of the nonaqueous electrolyte may be injected in one go, or may be injected in multiple steps, divided into two or more steps (for example, two or three times). When dispensing in multiple steps, it is preferable to provide a certain period of time between the first injection and the second injection. By providing a period of time of time of leaving, the nonaqueous electrolyte can be suitably impregnated into the inside of the wound electrode bodies 20a, 20b, 20c, so that the liquid level of the nonaqueous electrolyte drops, and a larger amount of the nonaqueous electrolyte can be injected in the injection (second injection) after leaving. This step may be carried out under atmospheric pressure, or may be carried out under a pressure reduced below atmospheric pressure within the battery case 10, for example for the purpose of improving the impregnation of the electrode assembly 20 with the non-aqueous electrolyte.
[0048] The amount of nonaqueous electrolyte injected is preferably an amount that ensures excess electrolyte between the battery case 10 and the wound electrode bodies 20a, 20b, and 20c. It is more preferable that the amount of nonaqueous electrolyte injected is an amount that, when performing the pressurizing step (step S20) described later, the liquid level of the excess electrolyte is in an area A1 (see FIG. 2) that satisfies the following: when the height (length in the direction from the bottom wall 12a toward the sealing plate 14) of the wound electrode bodies 20a, 20b, and 20c is Ta, the liquid level of the excess electrolyte is between a height of 1 / 8Ta from the end of the wound electrode bodies 20a, 20b, and 20c on the bottom wall 12a side to a height of 7 / 8Ta from the end of the wound electrode bodies 20a, 20b, and 20c on the bottom wall 12a side.
[0049] More specifically, in one embodiment, the amount of non-aqueous electrolyte injected is preferably about 300 to 400 ml (e.g., 315 ml) per battery assembly 100 A. Alternatively, in another embodiment, the ratio (Vl / Va) of the volume Vl of the injected amount (total amount) of non-aqueous electrolyte to the internal volume Va of the battery case 10 at 25° C. and 1 atmospheric pressure is preferably about 0.2 to 0.4, more preferably 0.27 to 0.3, and in one example, 0.28.
[0050] In one embodiment, it is preferable to perform the pressurizing step (step S20) after the entire amount of the predetermined amount of nonaqueous electrolyte is injected. In other words, it is preferable not to inject nonaqueous electrolyte after the pressurizing step (step S20). The presence of a sufficient amount of nonaqueous electrolyte in the battery case 10 from the beginning of the pressurizing step allows the effects of the technology disclosed herein to be exhibited favorably.
[0051] In the above manner, a battery assembly 100A (see FIG. 8) is constructed in which the electrode body group 20 and the nonaqueous electrolyte are housed in the battery case 10. In one embodiment, after the construction step (step S10), typically after the liquid injection step (step S12), it is preferable to start the pressurization step (step S20) without reducing the pressure in the battery case 10 to 0 MPa or less (atmospheric pressure or less). More specifically, it is preferable to start the pressurization step (step S20) without reducing the pressure in the battery case 10 to preferably −0.05 MPa or less, more preferably −0.01 MPa or less, and even more preferably −0.02 MPa or less. This makes it possible to ensure a relatively long retention time in the pressurization step (step S20), and more effectively promote the impregnation of the nonaqueous electrolyte.
[0052] The battery assembly 100A is placed in a chamber 210 of the pressure adjustment device 200 (see FIG. 8) in the subsequent pressurization step (step S20) and depressurization step (step S30). FIG. 8 is a schematic diagram of the pressure adjustment device 200. The pressure adjustment device 200 of this embodiment includes a chamber 210 that houses the battery assembly 100A and a pressure adjustment unit 220 that adjusts the pressure in the chamber 210. The chamber 210 here has a cylindrical shape and is sized to accommodate one or more battery assemblies 100A as is. Here, three battery assemblies 100A are housed in the chamber 210, but the number can of course be changed as appropriate. The chamber 210 is configured so that the internal pressure can be adjusted by the pressure adjustment unit 220. The chamber 210 is provided with an exhaust passage 211. An exhaust valve 212 is attached to the exhaust passage 211. The exhaust valve 212 is electrically connected to a control device (not shown), and is configured to be switchable between an open state and a closed state by the control device.
[0053] Here, the pressure adjusting unit 220 includes a gas flow path 230, a three-way valve 240, a gas supply source 250, a vacuum source 260, and a control device (not shown). The pressure adjusting unit 220 is configured such that the gas supply source 250 is connected to one of the branched gas flow paths 230, the vacuum source 260 is connected to the other, and the three-way valve 240 is disposed at the branch point.
[0054] The gas flow path 230 includes a first flow path 231, a second flow path 232, and a third flow path 233. One end of the first flow path 231 is connected to the chamber 210, and the other end is connected to the three-way valve 240. One end of the second flow path 232 is connected to the three-way valve 240, and the other end is connected to a gas supply source 250. One end of the third flow path 233 is connected to the three-way valve 240, and the other end is connected to a vacuum source 260. The three-way valve 240 is electrically connected to a control device, and is configured to be switchable between a state in which the first flow path 231 is connected to the second flow path 232 and a state in which the first flow path 231 is connected to the third flow path 233 by the control device.
[0055] Here, the gas supply source 250 is an air compressor that generates compressed air. However, the gas supply source 250 may be, for example, a gas cylinder filled with an inert gas or the like. The vacuum source 260 is a vacuum pump. The pressure adjustment unit 220 is configured to be able to pressurize the inside of the chamber 210 by switching the three-way valve 240 to a state in which the first flow path 231 and the second flow path 232 are connected so that the chamber 210 and the gas supply source 250 communicate with each other. The pressure adjustment unit 220 is configured to be able to depressurize the inside of the chamber 210 by switching the three-way valve 240 to a state in which the first flow path 231 and the third flow path 233 are connected so that the chamber 210 and the vacuum source 260 communicate with each other.
[0056] The pressurizing step (step S20) is a step of pressurizing the inside of the battery case 10 until it reaches a predetermined first pressure after the construction step (step S10) and maintaining the pressure for a predetermined time or more. This step is typically performed in a room temperature environment (e.g., about 25°C±10°C, 25°C±5°C). In this step, for example, as shown in FIG. 8, the battery assembly 100A is first accommodated in the chamber 210 of the pressure adjustment device 200 with the battery case 10 in an open state (here, the liquid injection hole 15 is in an open state). Then, the pressure in the chamber 210 is changed in a state where there is no pressure difference between the inside and outside of the battery case 10 (in other words, a state where the battery case 10 is not bulging or denting). Specifically, the control device closes exhaust valve 212, switches three-way valve 240 to connect chamber 210 to gas supply source 250, supplies gas from gas supply source 250 into chamber 210, and pressurizes chamber 210 to a predetermined first pressure. This effectively promotes the impregnation of the nonaqueous electrolyte.
[0057] Fig. 9 is a graph showing the transition of pressure in this step according to one embodiment. In this step, as shown in Fig. 9, it is preferable to continuously supply gas from the gas supply source 250 to perform pressurization until a predetermined first pressure is reached. That is, it is preferable to pressurize from a state of, for example, 0 MPa (atmospheric pressure) to the predetermined first pressure in one pressurization. Although not particularly limited, it is preferable that the speed at which the pressure inside the chamber 210 is increased (typically to the predetermined first pressure) (pressure increase speed) is 0.0013 to 0.0133 MPa / sec.
[0058] In the case where the battery assembly 100A includes the large-sized wound electrode bodies 20a, 20b, and 20c (specifically, the wound electrode bodies 20a, 20b, and 20c in which the length La in the long side direction Y of the negative electrode active material layer 24a is 20 cm or more) as in the present embodiment, it is necessary to pressurize the inside of the chamber 210 until the pressure inside the battery case 10 becomes 0.4 MPa or more. From the viewpoint of further improving the working efficiency and productivity, it is preferable to pressurize the inside of the battery case 10 until the pressure inside the battery case 10 becomes 0.5 MPa or more, more preferably until the pressure inside the battery case 10 becomes 0.6 MPa or more, and further preferably until the pressure inside the battery case 10 becomes 0.7 MPa or more. On the other hand, when the pressure becomes high to a certain extent, the impregnation promotion effect reaches a plateau and it takes time to increase the pressure, so that the pressure inside the battery case 10 is preferably, for example, 1 MPa or less, 0.9 MPa or less.
[0059] In this embodiment, the chamber 210 is maintained for a predetermined time in a pressurized state where the pressure inside the battery case 10 is 0.4 MPa or more. The time for which the inside of the battery case 10 is maintained in such a pressurized state (pressurized holding time) is longer than that of the conventional techniques disclosed in, for example, Patent Documents 1-3, and is required to be 20 minutes or more. This promotes impregnation of the nonaqueous electrolyte, and the nonaqueous electrolyte can be thoroughly impregnated into the inside of the large-sized wound electrode bodies 20a, 20b, and 20c, particularly the central portion in the long side direction Y. The pressurized holding time is preferably 30 minutes or more, more preferably 40 minutes or more, and even more preferably 45 minutes or more, and 50 minutes or more. From the viewpoint of improving the work efficiency and productivity, the pressurized holding time is preferably, for example, 300 minutes (5 hours) or less, more preferably 250 minutes or less, and even more preferably, for example, 120 minutes (2 hours) or less, and 60 minutes (1 hour) or less. Note that the "pressurized holding time" here typically means a time for continuous holding. That is, in this step, it is preferable to maintain the pressurized state continuously for 20 minutes or more, although it is also acceptable to reduce the pressure to less than 0.4 MPa for a very short period of time (for example, within a few seconds to a minute).
[0060] This step is preferably performed in a state where the liquid level of the excess electrolyte injected in the injection step (step S12) is lower than the upper end of the wound electrode bodies 20a, 20b, and 20c, more preferably lower than the upper end of the positive electrode tab group 23 and the upper end of the negative electrode tab group 25. This makes it easier for the air replaced with the nonaqueous electrolyte to be degassed, and the impregnation of the nonaqueous electrolyte can be promoted at a higher level. In addition, this step is preferably performed in a state where the liquid level of the excess electrolyte is higher than the lower end of the wound electrode bodies 20a, 20b, and 20c, more preferably higher than the lower end of the flat portion 20f. This makes it easier for the nonaqueous electrolyte to flow into the inside of the wound electrode bodies 20a, 20b, and 20c, and the impregnation of the nonaqueous electrolyte can be promoted at a higher level. In particular, this step is preferably carried out in a state in which the liquid level of the excess electrolyte is in the above-mentioned region A1 (see FIG. 2), and it is particularly preferable that the liquid level of the excess electrolyte is maintained in the above-mentioned region A1 from the start to the end of this step.
[0061] The depressurization step (step S30) is a step of depressurizing the inside of the battery case 10 to a predetermined second pressure after the pressurization step (step S20). This step is typically performed in a room temperature (for example, about 25°C ± 10°C, 25°C ± 5°C) environment. In this step, for example, the battery assembly 100A continues to be accommodated in the chamber 210 of the pressure adjustment device 200, and the inside of the chamber 210 is depressurized to a predetermined second pressure. Specifically, the control device switches the three-way valve 240 to communicate the chamber 210 with the vacuum source 260, and the gas in the chamber 210 is discharged by the vacuum source 260, and the inside of the chamber 210 is depressurized to the predetermined second pressure. By depressurizing the inside of the chamber 210, for example, residual air remaining inside the wound electrode bodies 20a, 20b, and 20c can be degassed, and the impregnation of the nonaqueous electrolyte can be effectively promoted.
[0062] In this step, it is preferable to continuously drive the vacuum source 260 to reduce the pressure until the predetermined second pressure is reached. That is, it is preferable to reduce the pressure from the first pressure state adjusted in the previous pressurization step, for example, to the predetermined second pressure in one depressurization. Although not particularly limited, it is preferable that the speed at which the pressure inside the chamber 210 is increased (typically to the predetermined second pressure) (pressure reduction speed) is 0.3 to 3 kPa / sec.
[0063] In the case where the battery assembly 100A includes the large-sized wound electrode bodies 20a, 20b, 20c (specifically, the wound electrode bodies 20a, 20b, 20c in which the length La in the long side direction Y of the negative electrode active material layer 24a is 20 cm or more) as in the present embodiment, it is preferable to reduce the pressure in the chamber 210 until the pressure in the battery case 10 becomes -55 kPa or less. This can effectively promote the impregnation of the nonaqueous electrolyte. From the viewpoint of further improving the work efficiency and productivity, it is preferable to reduce the pressure in the battery case 10 until it becomes -60 kPa or less, and more preferably until it becomes -80 kPa or less. On the other hand, when the pressure is lowered to a certain extent, the impregnation promotion effect reaches a plateau and it takes time to reduce the pressure, so that the pressure in the battery case 10 is preferably -95 kPa or more, for example.
[0064] In this step, it is further preferable to hold the chamber 210 in a reduced pressure state where the pressure inside the battery case 10 is -55 kPa or less for a predetermined time. The time for holding the inside of the battery case 10 in such a reduced pressure state (reduced pressure holding time) is preferably 1 minute or more, more preferably 4 minutes or more, and more preferably 5 minutes or more when the battery assembly 100A includes the wound electrode bodies 20a, 20b, 20c having a large size (specifically, the wound electrode bodies 20a, 20b, 20c having a length La in the long side direction Y of the negative electrode active material layer 24a of 20 cm or more). The reduced pressure holding time may typically be shorter than the pressurized holding time in the previous pressurizing step (step S20). From the viewpoint of improving the work efficiency and productivity, the reduced pressure holding time is more preferably 150 minutes or less, more preferably 125 minutes or less, and particularly preferably 120 minutes (2 hours) or less, 60 minutes (1 hour) or less, and 30 minutes or less.
[0065] In one embodiment, when the pressurized holding time in the previous pressurizing step (step S20) (i.e., the time during which the battery case 10 is held in a state of 0.4 MPa or more) is T1 and the reduced pressure holding time in this step (i.e., the time during which the battery case 10 is held in a state of -55 kPa or less) is T2, the ratio (T1 / T2) of the pressurized holding time T1 to the reduced pressure holding time T2 is preferably 2 to 40, and more preferably 3 to 8. By setting the ratio within the above range, impregnation of the electrolyte can be effectively promoted.
[0066] This step is preferably performed when there is still excess electrolyte between the battery case 10 and the wound electrode bodies 20a, 20b, and 20c, and more preferably when the liquid level of the excess electrolyte is above the lower ends of the wound electrode bodies 20a, 20b, and 20c, and even above the lower end of the flat portion 20f, and particularly in the above-mentioned region A1 (see Figure 2).
[0067] After the depressurization step (step S30), for example after a predetermined depressurization holding time has elapsed, the inside of the chamber 210 is typically returned to atmospheric pressure. Specifically, for example, the control device opens the exhaust valve 212 and exhausts the gas in the chamber 210 from the exhaust passage 211, thereby returning the inside of the chamber 210 to atmospheric pressure. As a result, the pressure in the battery case 10 also returns to near atmospheric pressure (for example, to -0.02 to 0.02 MPa).
[0068] In one embodiment, after the depressurization step (step S30), it is preferable to once return the pressure inside the battery case 10 to close to atmospheric pressure (for example, to -0.02 to 0.02 MPa), and then perform the initial charging step (step S40) without pressurizing or depressurizing the chamber 210 again. More specifically, after the depressurization step (step S30), it is preferable to perform the initial charging step (step S40) without bringing the pressure inside the battery case 10 into a depressurized state of -0.05 MPa or less, or into a pressurized state of 0.1 MPa or more. This allows the battery 100 to be manufactured more efficiently than when large pressurization and depressurization are repeated.
[0069] In the initial charging step (step S40), after the depressurization step (step S30), the battery assembly 100A is removed from the chamber 210 and charged at least once. The initial charging causes electrolysis of the nonaqueous electrolyte, and a coating (SEI film) containing decomposition products may be formed on the surface of the negative electrode active material layer 24a. This step may be performed in a room temperature environment (e.g., about 25°C±10°C, 25°C±5°C) or in a high temperature environment, for example, about 45°C. By performing the step in a high temperature environment, the formation of the coating can be promoted.
[0070] The battery assembly 100A can be charged in the same manner as in the past. Typically, an external power source is connected between the positive and negative terminals of the battery assembly 100A, and charging is performed until a predetermined final voltage is reached between the positive and negative terminals. The battery assembly 100A is preferably charged until the state of charge (SOC) is 5% or more, more preferably 10% or more. The state of charge (SOC) of the battery assembly 100A in this step is preferably 50% or less, more preferably 40% or less, and more preferably 30% or less. For example, when the negative electrode active material is a carbon material, the final voltage may be set to about 3V or more, typically 3.5V or more, for example 4V or more. The charging rate may be set to, for example, about 0.1C to 2C. Charging may be performed once, or may be repeated two or more times with discharging in between.
[0071] In this step, gas may be generated due to decomposition of the nonaqueous electrolyte solution. Therefore, after charging the battery assembly 100A at least once, the pressure inside the battery case 10 may be reduced again to a pressure equal to or lower than atmospheric pressure for the purpose of discharging the generated gas to the outside of the battery case 10.
[0072] In the sealing step (step S50), after the initial charging step (step S40), the liquid injection hole 15 is sealed with the sealing member 16 while the inside of the battery case 10 is kept at atmospheric pressure or is reduced below atmospheric pressure. This causes the battery case 10 to be airtightly sealed (hermetically sealed). In this manner, the battery 100 can be suitably manufactured.
[0073] <Uses of Battery 100> The battery 100 can be used for various purposes, but for example, since it includes the large-sized wound electrode bodies 20a, 20b, 20c (specifically, the wound electrode bodies 20a, 20b, 20c in which the length La in the long side direction Y of the negative electrode active material layer 24a is 20 cm or more) and has a high capacity, it can be suitably used as a power source (driving power source) for a motor mounted on a vehicle such as a passenger car or truck. The type of vehicle is not particularly limited, but examples include a plug-in hybrid electric vehicle (PHEV), a hybrid electric vehicle (HEV), and an electric vehicle (BEV; Battery Electric Vehicle). The battery 100 can also be suitably used as a battery pack in which a plurality of batteries 100 are arranged in a predetermined arrangement direction and a load is applied from the arrangement direction by a restraining mechanism.
[0074] Several examples of the present invention will be described below, but it is not intended that the present invention be limited to these examples.
[0075] <Test Example I: Examination of the pressurization process> In this test example, the impregnation rate was compared by changing the conditions of the pressurizing step (pressure and pressurized holding time). Specifically, first, a plurality of battery assemblies having the same configuration were constructed. In detail, first, in the arrangement step, a flat-shaped wound electrode body (total height Ta including curved parts is 9.4 cm, and length La in the long side direction of the negative electrode active material layer is 28.6 cm) was housed inside the exterior body. Next, a sealing plate was welded to the periphery of the opening of the exterior body to integrate the exterior body and the sealing plate. Next, in the liquid injection step, a predetermined amount of nonaqueous electrolyte was injected into the inside of the battery case from the liquid injection hole provided in the sealing plate. In this manner, a plurality of battery assemblies having the same configuration (Examples 1 to 4, Comparative Examples 1 and 2) were constructed.
[0076] Next, after the electrolyte injection step, the battery assembly was moved into the chamber of the pressure adjustment device. Then, in the pressurization step, without reducing the pressure inside the battery case below atmospheric pressure, the chamber was pressurized from atmospheric pressure under the conditions (pressurizing force and pressure holding time) shown in Table 1 while the electrolyte injection hole was left open.
[0077] After the pressurization step, the battery assembly was disassembled in an atmosphere of dry air (for example, with a dew point of about -50°C) without performing the depressurization step, and the wound electrode body was taken out of the battery case. Next, when the wound electrode body was unwound, the part not impregnated with the non-aqueous electrolyte (non-impregnated part) was observed to have color unevenness. Therefore, the width Ln of the non-impregnated part in the winding axis direction was measured visually, and the ratio of the impregnated part to the width of the positive electrode active material layer, that is, the impregnation rate (%) of the non-aqueous electrolyte was calculated from the following formula (1). The results are shown in Table 1. Impregnation rate (%) = (Lc - Ln) / Lc × 100 Formula (1) (wherein Lc is the width of the positive electrode active material layer in the winding axis direction, and Ln is the width of the unimpregnated portion in the winding axis direction.)
[0078] [Table 1]
[0079] FIG. 10 is a graph showing the relationship between the impregnation rate and the pressure applied in Examples 1 to 3 and Comparative Example 2. As shown in FIG. 10 and Table 1, when the width in the winding axis direction of the negative electrode active material layer is 20 cm or more, it is found that the pressure in the pressurizing step needs to be 0.4 MPa or more in order to achieve an impregnation rate of 75% or more, or even 80% or more. Also, FIG. 11 is a graph showing the relationship between the impregnation rate and the pressure holding time in Examples 3 and 4 and Comparative Examples 1 and 2. As shown in FIG. 11 and Table 1, when the pressure holding time exceeded 15 minutes, the approximation curve rose sharply around 20 minutes, and the impregnation rate changed sharply. Therefore, when the width in the winding axis direction of the negative electrode active material layer is 20 cm or more, it is effective to set the pressure holding time to 20 minutes or more, and it was found that the impregnation rate can be achieved by setting the pressure holding time to 20 minutes or more. It was also found that a more remarkable effect can be achieved by setting the pressure holding time to 30 minutes or more.
[0080] <Test Example II: Examination of the decompression process> In this test example, the time required for the nonaqueous electrolyte to be completely impregnated into the wound electrode body was compared with and without the depressurization step. Specifically, first, a plurality of battery assemblies (Examples 5 and 6) having the same configuration were constructed in the same manner as in Test Example I. Next, as in Test Example I, the battery assemblies were moved into a chamber, and the inside of the chamber was pressurized under the conditions (pressurizing force and pressurized holding time) shown in Table 2. Next, for the battery assembly of Example 6, after the pressurization step, the inside of the chamber was subsequently depressurized under the conditions (depressurizing force and depressurized holding time) shown in Table 2. On the other hand, for the battery assembly of Example 5, the depressurization step was not performed.
[0081] Next, for each example, the battery assemblies were disassembled one by one at regular intervals after injection, and visually checked to see if there was an unimpregnated portion in the center of the separator in the winding axis direction. Then, the time until the unimpregnated portion could no longer be confirmed (the complete impregnation time required for complete impregnation) was measured. The results are shown in Table 2. The complete impregnation time is expressed as a relative value with the result of Example 5 as the standard (100).
[0082] [Table 2]
[0083] As shown in Table 2, it was found that by further including a depressurization step after the pressurization step, the gas remaining in the wound electrode body can be efficiently degassed, thereby shortening the time required for complete impregnation and further improving the impregnation of the nonaqueous electrolyte.
[0084] <Test Example III: Examination of the decompression process> In this test example, the time required for the nonaqueous electrolyte to be completely impregnated into the wound electrode body was compared by changing the reduced pressure holding time in the reduced pressure step. Specifically, first, a plurality of battery assemblies (Examples 7 to 10) having the same configuration were constructed in the same manner as in Test Example II. Next, as in Test Example II, the battery assemblies were moved into a chamber, and the chamber was pressurized under the conditions (pressurizing force and pressurized holding time) shown in Table 3. Next, for the battery assemblies of Examples 8 to 10, after the pressurizing step, the chamber was subsequently depressurized under the conditions (depressurizing force and reduced pressure holding time) shown in Table 3. Here, the total of the pressurized holding time and reduced pressure holding time was unified to 40.5 minutes for Examples 8 to 10. That is, when the reduced pressure holding time was extended, the pressurized holding time was shortened accordingly. On the other hand, the battery assembly of Example 7 was not subjected to the reduced pressure step.
[0085] Next, in the same manner as in Test Example II, for each example, the battery assemblies were disassembled one by one at regular intervals after injection, and visually checked for the presence of unimpregnated areas in the center of the winding axis direction of the separator. Then, the time until the unimpregnated areas could no longer be confirmed (the complete impregnation time required for complete impregnation) was measured. The results are shown in Table 3. The complete impregnation time is expressed as a relative value with the result of Example 7 as the standard (100).
[0086] [Table 3]
[0087] As shown in Table 3, it was found that by setting the reduced pressure holding time in the reduced pressure step to 1 minute or more, the time required for complete impregnation could be shortened by about 20%, and the impregnation of the nonaqueous electrolyte could be improved. In particular, it was found that by setting the reduced pressure holding time to about 5 minutes (for example, about 3 to 7 minutes), the impregnation of the nonaqueous electrolyte could be improved to an even higher level.
[0088] Although several embodiments of the present invention have been described above, the above embodiments are merely examples. The present invention can be implemented in various other forms. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes of the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. Furthermore, if a technical feature is not described as essential, it can be appropriately deleted.
[0089] For example, in the embodiment of FIG. 7 described above, the liquid injection step (step S12) is performed after the arrangement step (step S11), but this is not limited thereto. In other embodiments, for example, the liquid injection step (step S12) may be followed by the arrangement step (step S11). Furthermore, when the nonaqueous electrolyte is injected into the battery case 10 before the sealing plate 14 is welded to the periphery of the opening 12h of the exterior body 12, in other words, when the electrode body group 20 (wound electrode bodies 20a, 20b, 20c) and the nonaqueous electrolyte are accommodated inside the battery case 10 and then the exterior body 12 and the sealing plate 14 are integrated, the liquid injection hole 15 may not be provided in the sealing plate 14.
[0090] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A method for producing a non-aqueous electrolyte secondary battery comprising: a wound electrode assembly including a positive electrode and a negative electrode; a non-aqueous electrolyte; and a battery case accommodating the wound electrode assembly and the non-aqueous electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector; the negative electrode comprises a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector; and the width of the negative electrode active material layer in the winding axis direction is 20 cm or more; a pressurizing step of, after the assembly step, placing the battery assembly in a chamber whose internal pressure is adjustable with the battery case in an open state, changing the pressure in the chamber to increase the pressure in the battery case to 0.4 MPa or more, and maintaining the state in which the pressure in the battery case is 0.4 MPa or more for 20 minutes or more. Item 2: The method for producing a nonaqueous electrolyte secondary battery according to item 1, further comprising, after the pressurizing step, a depressurizing step of reducing the pressure inside the battery case until the pressure therein becomes −55 kPa or less. Item 3: The method for producing a nonaqueous electrolyte secondary battery according to Item 2, wherein in the pressure reducing step, the pressure inside the battery case is maintained at -55 kPa or less for one minute or more. Item 4: The method for producing a nonaqueous electrolyte secondary battery according to Item 3, wherein, in the pressurizing step, a pressurized holding time T1 during which the pressure inside the battery case is held at 0.4 MPa or more and a reduced pressure holding time T2 during which the pressure inside the battery case is held at -55 kPa or less in the depressurizing step are both defined as a pressure holding time T1 and a reduced pressure holding time T2, respectively, and a ratio (T1 / T2) of the pressurized holding time T1 to the reduced pressure holding time T2 is 2 or more and 40 or less. Item 5: The method for producing a nonaqueous electrolyte secondary battery according to any one of Items 2 to 4, further comprising an initial charging step of charging the battery assembly for the first time after the depressurizing step, wherein the initial charging step is started without adjusting the pressure in the battery case to -0.05 MPa or less to 0.1 MPa or more again once the pressure in the battery case has been adjusted to -0.02 MPa or more and 0.02 MPa or less after the depressurizing step. Item 6: The method for producing a nonaqueous electrolyte secondary battery according to any one of Items 1 to 5, wherein after the assembly step, the pressurizing step is started without lowering the pressure inside the battery case to -0.05 MPa or less. Item 7: The method for producing a nonaqueous electrolyte secondary battery according to any one of items 1 to 6, wherein the battery case has an injection hole, the construction step includes an arrangement step of arranging the wound electrode body inside the battery case, and an injection step of injecting the nonaqueous electrolyte through the injection hole after the arrangement step, and the pressure in the chamber is changed in the pressurizing step with the injection hole open. Item 8: The method for producing a nonaqueous electrolyte secondary battery according to any one of items 1 to 7, wherein the battery case has an exterior body having an opening, a bottom wall, and a side wall extending from an edge of the bottom wall toward the opening, and a sealing plate that seals the opening, and in the construction step, the wound electrode body is housed in the battery case with a winding axis oriented along the bottom wall. Item 9: The method for producing a nonaqueous electrolyte secondary battery according to item 8, wherein in the construction step, the nonaqueous electrolyte is injected between the battery case and the wound electrode body so as to contain excess electrolyte, and the pressurization step is performed in a state in which a liquid level of the excess electrolyte is in an area A1 that satisfies the following: between a height of 1 / 8 Ta from an end of the wound electrode body on the bottom wall side to a height of 7 / 8 Ta from an end of the wound electrode body on the bottom wall side, where Ta is the length of the wound electrode body in a direction from the bottom wall toward the sealing plate. Item 10: The method for producing a nonaqueous electrolyte secondary battery according to any one of items 1 to 9, wherein in the pressurizing step, the pressure inside the battery case is maintained at 0.4 MPa or more for 30 minutes or more. [Explanation of symbols]
[0091] 10 Battery case 15 Liquid injection hole 20 Electrode group 20a, 20b, 20c wound electrode body 22 Positive electrode 22a Cathode active material layer 22c Positive electrode current collector 24 Negative electrode 24a Negative electrode active material layer 24c Negative electrode current collector 26 Separator 100 batteries 200 Pressure Regulator 210 Chamber 220 Pressure Regulator S10 construction process S11 Placement process S12 Liquid injection process S20 Pressurization process S30 Decompression process S40 First Charging Process
Claims
1. The battery comprises a wound electrode body including a positive electrode and a negative electrode, a non-aqueous electrolyte, and a battery case that accommodates the wound electrode body and the non-aqueous electrolyte, The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector, The width of the negative electrode active material layer in the winding axis direction is 20 cm or more. A method for producing a non-aqueous electrolyte secondary battery, comprising: a construction step of housing the wound electrode body and the nonaqueous electrolyte in the battery case to construct a battery assembly; a pressurizing step of placing the battery assembly in a chamber capable of adjusting an internal pressure while the battery case is in an open state after the construction step, pressurizing the battery case until the pressure in the battery case becomes 0.4 MPa or more by changing the pressure in the chamber, and maintaining the state in which the pressure in the battery case is 0.4 MPa or more for 20 minutes or more; The method for producing a non-aqueous electrolyte secondary battery includes the steps of:
2. The pressure reduction step further comprises reducing the pressure inside the battery case to −55 kPa or less after the pressurizing step. The method for producing the nonaqueous electrolyte secondary battery according to claim 1 .
3. In the decompression step, the pressure inside the battery case is maintained at −55 kPa or less for 1 minute or more. The method for producing the nonaqueous electrolyte secondary battery according to claim 2 .
4. a ratio (T1 / T2) of the pressurized holding time T1 to the reduced pressure holding time T2 is 2 or more and 40 or less, where T1 is a pressurized holding time during which the pressure in the battery case is held at 0.4 MPa or more in the pressurizing step and T2 is a reduced pressure holding time during which the pressure in the battery case is held at -55 kPa or less in the depressurizing step; The method for producing the nonaqueous electrolyte secondary battery according to claim 3 .
5. The method further includes a first charging step of charging the battery assembly for the first time after the depressurization step, The initial charging step is started after the pressure reduction step, once the pressure in the battery case is adjusted to -0.02 MPa or more and 0.02 MPa or less, without adjusting the pressure in the battery case to -0.05 MPa or less or 0.1 MPa or more again. The method for producing the nonaqueous electrolyte secondary battery according to any one of claims 2 to 4.
6. After the construction step, the pressurization step is started without lowering the pressure inside the battery case to −0.05 MPa or less. The method for producing the nonaqueous electrolyte secondary battery according to claim 1 .
7. the battery case has a liquid injection hole, The construction step includes: a placement step of placing the wound electrode body inside the battery case; and a liquid injection step of injecting the nonaqueous electrolyte through the liquid injection hole after the placing step, In the pressurizing step, the pressure in the chamber is changed in a state in which the liquid injection hole is opened. The method for producing the nonaqueous electrolyte secondary battery according to claim 1 .
8. The battery case is an exterior body having an opening, a bottom wall, and a side wall extending from an edge of the bottom wall toward the opening; a sealing plate that seals the opening, In the construction step, the wound electrode body is accommodated in the battery case with a winding axis oriented along the bottom wall. The method for producing the nonaqueous electrolyte secondary battery according to claim 1 .
9. In the construction step, the nonaqueous electrolyte is injected between the battery case and the wound electrode body so as to contain excess electrolyte, The pressurizing step is performed in such a manner that the liquid level of the excess electrolyte is in an area A1 that satisfies the following: When the length of the wound electrode body in the direction from the bottom wall to the sealing plate is Ta, Between a height of 1 / 8 Ta from the end of the wound electrode body on the bottom wall side to a height of 7 / 8 Ta from the end of the wound electrode body on the bottom wall side; In the state where The method for producing the nonaqueous electrolyte secondary battery according to claim 8 .
10. In the pressurizing step, the pressure inside the battery case is maintained at 0.4 MPa or more for 30 minutes or more. The method for producing the nonaqueous electrolyte secondary battery according to claim 1 .
Citation Information
Patent Citations
Manufacture of nonaqueous electrolyte secondary battery
JP1999111339A
Nonaqueous electrolyte secondary battery
JP2000058067A
Nonaqueous electrolyte secondary battery
JP2001176482A
Square lithium ion secondary battery
JP2018147574A
Method for manufacturing non-aqueous electrolyte secondary battery
JP2022079233A