Aqueous flexographic ink, printed material, and laminate
A specialized water-based flexographic ink formulation with specific urethane resins and additives addresses plate entanglement and blocking issues, enhancing lamination strength and print quality on non-permeable substrates.
Patent Information
- Application Number
- JP2023071390
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Water-based flexographic inks face issues with plate entanglement, blocking, and poor lamination strength during high-speed printing and lamination, particularly on non-permeable substrates like film, leading to defects such as mixed color bleeding and reduced laminate strength.
A water-based flexographic ink formulation using a combination of aqueous urethane resins with specific molecular weights and structural units derived from polyester and polyether polyols, along with additives, to enhance solubility, adhesion, and lamination strength.
The ink achieves improved plate entanglement resistance, blocking resistance, and lamination strength, ensuring high-quality printed matter and laminates even under high-speed printing conditions.
Smart Images

Figure 2024157197000001 
Figure 2024157197000002 
Figure 2024157197000003
Abstract
Description
[Technical field]
[0001] The present invention relates to water-based flexographic inks, prints and laminates. [Background technology]
[0002] In recent years, the printing ink industry has been calling for the use of water-based inks due to the increasing demand for reducing the environmental impact and safety during printing. Flexographic printing is useful for printing with water-based inks. Flexographic printing is a type of letterpress printing in which ink is applied to a resin relief plate via an anilox roll, and the ink is transferred from the relief plate to a plastic substrate or the like. Flexographic printing excels in high-speed printing, and can reproduce fine characters and sharp expressions even with a small amount of ink transferred.
[0003] When water-based ink is printed on a non-permeable substrate such as a film substrate, the ink cannot be permeated and dried as when printed on a paper substrate, resulting in problems such as color bleeding, uneven coloring, poor adhesion, poor drying, and blocking (the phenomenon in which the ink is transferred to the back) due to the tack derived from the resin contained in the water-based ink. In particular, when printing at high speed, the drying property is further reduced, and blocking often occurs. In addition, when lamination processing is performed, the laminate after processing may not have sufficient lamination strength. In flexographic printing, from the viewpoint of productivity of printed matter, unless blocking resistance when printed at high speed and lamination strength when made into a laminate are both achieved, it is not sufficient for printing suitability.
[0004] In addition, printing with water-based flexographic inks is prone to printing defects such as plate entanglement due to printing conditions such as long printing times and environments where the ink dries easily, such as low humidity. Plate entanglement is a phenomenon in which ink penetrates not only into the convex parts of the plate, but also into the sides of the convex parts and other parts (concave parts), and the ink that accumulates in the concave parts transfers ink to parts of the printed matter that are not originally printed. In halftone printing of highlight parts where the area of the convex parts of the flexographic plate is small, a phenomenon occurs in which the convex parts of the plate are immersed in the cells of the anilox roll (called dot dipping), and this influence particularly promotes plate entanglement, resulting in excessively large halftone dots that deviate from the range of appropriate halftone dot sizes that should be obtained for the halftone dot size originally designed for the flexographic plate (called dot gain), which causes a problem of reduced design quality of the printed matter.
[0005] Patent Document 1 discloses an invention of a water-based gravure or flexographic ink that is excellent in hue reproducibility such as density reproducibility and halftone dot reproducibility, as well as in adhesion to substrates and blocking resistance. However, there is room for improvement in the selection of urethane resin, and there is concern that printing defects such as plate tangling may occur during printing, and that the laminate strength may decrease when packaging bags are made using the ink and retorted.
[0006] Patent Document 2 discloses a rotary printing ink excellent in water resistance, laminate strength, and blocking resistance, and a rotary printing ink set, a plastic film print, and a laminated product using the ink. However, since only an aqueous urethane resin with a large mass average molecular weight is used, the ink has low resolubility, and in environments such as low humidity, plate tangling and dot gain may occur, resulting in printing defects. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2021-031572 [Patent Document 2] JP 2018-184512 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a water-based flexographic ink that can provide a printed matter having good resistance to plate entanglement and blocking during printing, and a laminate having good lamination strength after retorting. [Means for solving the problem]
[0009] As a result of intensive research, the present inventors have found that the above problems can be solved by using the water-based flexographic ink described below, and have completed the present invention. Effect of the Invention
[0010] According to the present invention, it is possible to provide a water-based flexographic ink which can give a printed matter having good resistance to plate entanglement and blocking during printing, and a laminate having good lamination strength after retort. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following describes in detail an embodiment of the present invention. However, the following description is an example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention.
[0012] In this specification, the above-mentioned "water-based flexographic ink" may be simply referred to as "water-based ink" or "ink", but these terms have the same meaning.
[0013] <Water-based flexographic ink> The water-based ink of the present invention is a water-based flexographic ink containing a water-based urethane resin (X) having a mass average molecular weight of 20000 or more and 100000 or less, and a water-based urethane resin (Y) having a mass average molecular weight of 3000 or more and less than 20000, the water-based urethane resin (X) containing a constituent unit derived from a polyester polyol and / or a polyether polyol. The water-based flexographic ink preferably contains a pigment, an additive, a liquid medium, etc., as necessary.
[0014] The ink of the present invention uses the above-mentioned water-based urethane resin (X) and the above-mentioned water-based urethane resin (Y) in combination, and the two work together to suppress tackiness derived from the resin and improve the resolubility of the ink. As a result, even when printing at high speed for a long period of time, the ink has high blocking resistance and can prevent the occurrence of plate tangling, resulting in an excellent ink that achieves both laminate strength and printability. The above discussion of the mechanism is merely an example and is not intended to limit the present invention.
[0015] From the viewpoint of achieving both laminate strength and printability, the mass ratio of the aqueous urethane resin (X) to the aqueous urethane resin (Y) contained in the aqueous ink is preferably from 90:10 to 55:45, more preferably from 90:10 to 60:40, even more preferably from 88:12 to 65:35, and particularly preferably from 85:15 to 70:30.
[0016] <Water-based urethane resin (X)> The aqueous urethane resin (X) has a mass average molecular weight of 20,000 or more and 100,000 or less, and contains a constituent unit derived from a polyester polyol and / or a polyether polyol. The aqueous urethane resin (X) is preferably one having a hydroxyl group at a terminal, which is obtained by a condensation reaction between a polyol and a polyisocyanate, and the constituent unit derived from the polyester polyol and / or the polyether polyol is preferably derived from the polyol. The aqueous urethane resin (X) is preferably an aqueous urethane urea resin (X) obtained by reacting a urethane prepolymer having an isocyanate group at its terminal, which is a condensation reaction product of a polyol and a polyisocyanate, with a chain extender.
[0017] The weight average molecular weight of the aqueous urethane resin (X) is 20,000 or more and 100,000 or less, preferably 20,000 or more and 50,000 or less, more preferably 20,000 or more and less than 40,000, even more preferably 21,000 or more and 39,000 or less, and particularly preferably 22,000 or more and 38,000 or less, or 23,000 or more and 37,000 or less.
[0018] The acid value of the aqueous urethane resin (X) is preferably 10 to 60 mgKOH / g, more preferably 15 to 55 mgKOH / g, and even more preferably 20 to 45 mgKOH / g. If the acid value of the aqueous urethane resin (X) is within the above range, the dispersibility and solubility in water are sufficient, and the ink is stable, and the plate entanglement resistance, blocking resistance, and lamination strength are also excellent. The acid value is the amount of acid in 1 g of resin calculated by titrating the acid with an alkali, converted into mg of potassium hydroxide, and is measured according to JIS K0070.
[0019] The hydroxyl value of the aqueous urethane resin (X) is preferably 1 to 50 mgKOH / g, more preferably 10 to 45 mgKOH / g, and more preferably 15 to 40 mgKOH / g. This is because the aqueous urethane resin (X) has good solubility in water, resulting in good plate entanglement resistance, blocking resistance, and laminate strength. The hydroxyl value is a value measured according to JIS K0070, which is calculated by esterifying or acetylating the hydroxyl groups in the resin and back titrating the remaining acid with an alkali to convert the amount of hydroxyl groups in 1 g of resin into mg of potassium hydroxide.
[0020] The glass transition temperature of the aqueous urethane resin (X) is preferably −70 to 0° C., more preferably −65 to −5° C., and further preferably −60 to −10° C. Here, the glass transition temperature refers to the maximum value of tan δ in dynamic viscoelasticity measurement.
[0021] The content of the aqueous urethane resin (X) in the total mass of the ink is preferably 1 to 20 mass%, more preferably 3 to 18 mass%, even more preferably 5 to 15 mass%, and particularly preferably 13 mass% or less or 11 mass% or less.
[0022] (Polyol) The aqueous urethane resin (X) contains a structural unit derived from a polyester polyol and / or a polyether polyol, more preferably a structural unit derived from a polyester polyol, further preferably a structural unit derived from a polyester polyol and a polyether polyol, and particularly preferably a structural unit derived from a polyol having a carboxyl group. It may also contain a structural unit derived from another polyol.
[0023] From the viewpoint of achieving both laminate strength and printability, it is preferable that the aqueous urethane resin (X) contains a structural unit derived from a polyester polyol, and the aqueous urethane resin (Y) described below contains a structural unit derived from a polyether polyol.
[0024] From the viewpoints of plate entanglement resistance, blocking resistance, and laminate strength, the content of the polyol-derived structural units is preferably 45 to 85 mass%, more preferably 50 to 80 mass%, and even more preferably 55 to 75 mass%, of the total mass of the aqueous urethane resin (X).
[0025] (Polyester polyol) The polyester polyol is preferably, for example, a condensation product of a dibasic acid and a diol. From the viewpoints of plate entanglement resistance, blocking resistance, and laminate strength, it is preferable that the dibasic acid contains at least one selected from the group consisting of adipic acid, succinic acid, sebacic acid, azelaic acid, and dimer acid.
[0026] The diol preferably includes a branched diol, and also preferably includes both a branched diol and a linear diol. Here, the linear diol is a diol having a linear structure with two or more carbon atoms, and refers to alkylene glycol, dialkylene glycol, trialkylene glycol, and other diols. In addition, the branched diol refers to a diol in which at least one hydrogen atom of the hydrocarbon group of alkylene glycol is replaced with a non-hydrogen atom.
[0027] Examples of the branched diol include 2-butyl-2-ethyl-1,3-propanediol (hereinafter also referred to as BEPG), 2-methyl-1,3-propanediol (hereinafter also referred to as MPO), 3-methyl-1,5-pentanediol (hereinafter also referred to as MPD), neopentyl glycol (hereinafter also referred to as NPG), 1,2-propylene glycol (hereinafter also referred to as PG), 2,4-diethyl-1,5-pentanediol, 1,3-butanediol, dipropylene glycol, etc. Among these, MPD and NPG are preferable.
[0028] The linear diol is preferably an alkylene glycol, and examples of such compounds include ethylene glycol (also written as EG), diethylene glycol, 1,3-propanediol (also written as 1,3-PD), 1,4-butanediol (also written as 1,4-BD), 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,4-butynediol, 1,4-butylenediol, diethylene glycol, and triethylene glycol. Among these, linear diols having 8 or less carbon atoms, preferably 6 or less carbon atoms, are preferred, and EG, 1,3-PD, 1,4-BD, 1,5-pentanediol, 1,6-hexanediol, and 1,8-octanediol are more preferred.
[0029] The mass ratio of the branched diol and linear diol (branched diol: linear diol) in the diol contained in the polyester polyol is preferably 10:90 to 90:10, more preferably 20:80 to 80:20, and further preferably 30:70 to 70:30.
[0030] The branched diol and the linear diol may each be present in one polyester polyol, or a polyester polyol containing only a branched diol and a polyester polyol containing only a linear diol may be used as a mixture raw material to produce the aqueous urethane resin (X).
[0031] The content of the polyester polyol-derived structural unit in the total mass of the aqueous urethane resin (X) is preferably 20 to 80 mass%, more preferably 30 to 70 mass%, and even more preferably 40 to 60 mass%. The above range is preferable because it provides excellent plate entanglement resistance, blocking resistance, and laminate strength.
[0032] (Polyether polyol) From the viewpoints of plate entanglement resistance, blocking resistance, and lamination strength, the polyether polyol preferably contains at least one selected from the group consisting of polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, and more preferably contains polyethylene glycol. The polyether polyol can be used alone or in a mixture of two or more kinds, and may be a copolymerized polyether polyol or may be used in combination with a single polyether polyol. It is also possible to use polyether polyols other than the above in combination. For example, polymers or copolymers of methylene oxide, 1,3-propanediol, 1,5-pentanediol, 1,6-hexanediol, etc. can be mentioned.
[0033] From the viewpoints of plate entanglement resistance, blocking resistance, and laminate strength, the content of the structural units derived from polyether polyol is preferably 1 to 20 mass%, more preferably 2 to 15 mass%, and even more preferably 3 to 10 mass%, of the total mass of the aqueous urethane resin (X).
[0034] (Polyol having a carboxyl group) In order to dissolve or disperse the aqueous urethane resin (X) in an aqueous medium, the aqueous urethane resin (X) must be hydrophilic. The polyether polyols and polyester polyols listed above are also hydrophilic, but it is preferable to use a polyol having a carboxyl group in combination. That is, it is preferable that the aqueous urethane resin (X) further contains a structural unit derived from a polyol having a carboxyl group. The carboxyl group is preferably neutralized with a basic compound.
[0035] Examples of polyols having a carboxyl group include dimethylolalkanoic acids such as dimethylolacetic acid, dimethylolpropionic acid, dimethylolbutanoic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolpentanoic acid, dihydroxysuccinic acid, dihydroxypropionic acid, and dihydroxybenzoic acid. These carboxyl group-containing polyols can be used alone or in combination. Among these, dimethylolpropionic acid and dimethylolbutanoic acid are preferable.
[0036] When the aqueous urethane resin (X) contains a structural unit derived from a polyol having a carboxyl group, the content of the structural unit derived from a polyol having a carboxyl group is, from the viewpoints of plate entanglement resistance, blocking resistance, and laminate strength, preferably 1 to 50 mass %, more preferably 2 to 30 mass %, and even more preferably 3 to 15 mass %, of the total mass of the aqueous urethane resin (X).
[0037] (Other polyols) Other suitable polyols include polycarbonate polyols. Examples of polycarbonate polyols include those obtained by reacting polyols with carbonate compounds such as dialkyl carbonates, alkylene carbonates, and diaryl carbonates. The polyols constituting the polycarbonate polyols can be the polyols listed above as examples of the components of the polyester polyols. Examples of dialkyl carbonates include dimethyl carbonate and diethyl carbonate, examples of alkylene carbonates include ethylene carbonate, and examples of diaryl carbonates include diphenyl carbonate.
[0038] (Polyisocyanate) As the polyisocyanate, a diisocyanate is preferable, and as such a compound, various known aromatic, aliphatic or alicyclic diisocyanates can be used. For example, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylsilyl diisocyanate, 1,3,4-trimethylsilyl diisocyanate, 1,4 ... Representative examples include methylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, and dimer diisocyanate in which the carboxyl group of a dimer acid is converted to an isocyanate group. These can be used alone or in a mixture of two or more kinds. Among them, isophorone diisocyanate, tolylene diisocyanate, and 4,4'-diphenylmethane diisocyanate are preferred, and isophorone diisocyanate is more preferred from the viewpoint of solubility.
[0039] (Chain extension reaction with chain extender) In the synthesis of the aqueous urethane resin (X), it is preferable to carry out a chain extension reaction using a chain extender as necessary. The chain extension reaction is carried out by synthesizing an isocyanate group-excessive urethane prepolymer, and then reacting it with a diamine or other polyamine as a chain extender. From the viewpoint of a significant increase in viscosity of the resin solution, this reaction is preferably carried out when neutralizing the resin to make it aqueous. The chain extension makes it possible to further increase the molecular weight of the aqueous urethane resin (X). In addition, when a polyamine is used as a chain extender, a urea bond is introduced, and thus a further improvement in the cohesive force of the aqueous urethane resin (X) can be expected.
[0040] Examples of chain extenders include diamines such as hydrazine, ethylenediamine, propylenediamine, 1,4-tetramethylenediamine, 2-methyl-1,5-pentanediamine, hexamethylenediamine, nonamethylenediamine, xylylenediamine, isophoronediamine, piperazine and its derivatives, phenylenediamine, tolylenediamine, xylylenediamine, adipic acid dihydrazide, and isophthalic acid dihydrazide; Diamines having a hydroxyl group, such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine; Triamines such as diethylenetriamine; Diols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,4-bis(β-hydroxyethoxy)benzene, 1,4-cyclohexanediol, bis(β-hydroxyethyl)terephthalate, and xylylene glycol; Triols such as trimethylolpropane; Pentaols such as pentaerythritol; Amino alcohols such as N-(β-aminoethyl)ethanolamine Known chain extenders such as the above can be used. By using a monofunctional monoamine or monool in combination, it is also possible to control the molecular weight by terminating the chain extension. Among these, isophoronediamine and 2-hydroxyethylethylenediamine are preferable.
[0041] <Water-based urethane resin (Y)> The water-based ink of the present invention contains an aqueous urethane resin (Y) having a mass average molecular weight of 3000 or more and less than 20000. The aqueous urethane resin (Y) is preferably one having a hydroxyl group at a terminal, which is obtained by a condensation reaction between a polyol and a polyisocyanate. The aqueous urethane resin (Y) is also preferably one obtained by reacting a urethane prepolymer having an isocyanate group at its terminal, which is a condensation reaction product of a polyol and a polyisocyanate, with a chain extender. The aqueous urethane resin (Y) can be, for example, the same as the aqueous urethane resin (X) exemplified above, except for the mass average molecular weight. However, when the aqueous urethane resin (X) is a urethane urea resin, it is preferable that the aqueous urethane resin (Y) is not a urethane urea resin.
[0042] The weight average molecular weight of the aqueous urethane resin (Y) is 3,000 or more and less than 20,000, preferably 4,000 or more and 19,000 or less, preferably 5,000 or more and 18,000 or less, and more preferably 10,000 or more and 17,000 or less.
[0043] The acid value of the aqueous urethane resin (Y) is preferably from 5 to 50 mgKOH / g, more preferably from 8 to 40 mgKOH / g, and further preferably from 10 to 30 mgKOH / g.
[0044] The hydroxyl value of the aqueous urethane resin (Y) is preferably from 1 to 50 mgKOH / g, more preferably from 10 to 45 mgKOH / g, and even more preferably from 15 to 40 mgKOH / g.
[0045] The glass transition temperature of the aqueous urethane resin (Y) is preferably −60 to 0° C., more preferably −55 to −5° C., and further preferably −50 to −10° C. Here, the glass transition temperature refers to the maximum value of Tan δ in dynamic viscoelasticity measurement.
[0046] The content of the aqueous urethane resin (Y) in the total mass of the ink is preferably 0.5 to 15 mass%, more preferably 0.8 to 10 mass%, even more preferably 1 to 8 mass%, and particularly preferably 1.5 to 5 mass%.
[0047] (Polyol) The aqueous urethane resin (Y) preferably contains structural units derived from a polyester polyol and / or a polyether polyol, more preferably contains structural units derived from a polyether polyol, and further preferably contains structural units derived from a polyol having a carboxyl group.
[0048] From the viewpoints of plate entanglement resistance, blocking resistance, and laminate strength, the polyether polyol preferably contains at least one selected from the group consisting of polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, and more preferably contains polyethylene glycol and / or polytetramethylene glycol.
[0049] From the viewpoints of plate entanglement resistance, blocking resistance, and laminate strength, the content of the polyether polyol is preferably 20 to 80 mass %, more preferably 30 to 70 mass %, and even more preferably 40 to 60 mass %, of the total mass of the aqueous urethane resin (Y).
[0050] When the polyether polyol contains polyethylene glycol, the content of the constitutional units derived from polyethylene glycol is preferably 20 to 60 mass%, more preferably 25 to 55 mass%, and even more preferably 30 to 50 mass%, of the total mass of the aqueous urethane resin (Y), from the viewpoints of plate entanglement resistance and blocking resistance.
[0051] <Method for producing aqueous urethane resin (X) and aqueous urethane resin (Y)> The method for producing the aqueous urethane resin (X) and the aqueous urethane resin (Y) is not particularly limited, and they are produced by known methods. For example, as described in Japanese Patent No. 4900136, a method of polymerizing polyol and polyisocyanate without using an organic solvent can be mentioned. More specifically, for example, after charging polyol and polyisocyanate, the atmosphere is replaced with dry nitrogen, and the reaction is carried out at 90°C to 220°C for 10 minutes to 5 hours. Then, a neutralizing agent is added while cooling to obtain the product.
[0052] <Basic compounds> When the aqueous urethane resin (X) and / or the aqueous urethane resin (Y) have an acid group, the acid group is preferably neutralized with a basic compound. The neutralization may be carried out before producing an ink using the aqueous urethane resin (X) and the aqueous urethane resin (Y), or may be carried out by adding a basic compound as a neutralizing agent to the ink after producing an ink containing a binder resin, or may be both.
[0053] Examples of the basic compound used for the neutralization include organic amines, ammonia, metal salts, etc. Among these, ammonia and organic amines are preferred.
[0054] (Organic amine) The basic compound used for neutralization is preferably an organic amine, and more preferably an alkylamine such as trimethylamine, triethylamine, or butylamine, 2-dimethylaminoethanol, 2-diethylaminoethanol, diethanolamine, triethanolamine, aminomethylpropanol, or morpholine, and even more preferably triethylamine or dimethylethanolamine.
[0055] The neutralization rate in the above neutralization is preferably 100 to 150% in the ink, and more preferably 110 to 140%. When it is in the above range, the printing stability and drying property of the printed matter are excellent. In this specification, the neutralization rate is a value calculated by [(base equivalent of the basic compound) / (acid equivalent of the binder resin)]×100.
[0056] <Liquid medium> The aqueous ink of the present invention preferably contains water as a liquid solvent, and from the viewpoint of suppressing plate entanglement, it preferably further contains an organic solvent, and among these, it is more preferable that it contains a glycol-based solvent and / or a glycol ether-based solvent. When the water-based ink contains a glycol-based solvent and / or a glycol ether-based solvent, the resolubility of the ink is improved, so that when the ink is transferred to the substrate to form the halftone dots, the halftone dots can be prevented from becoming deformed due to drying, etc., and plate tangling can be suppressed.
[0057] Examples of glycol solvents include ethylene glycol, 1,3-propanediol, propylene glycol, 1,2-butanediol, 1,4-butanediol, pentylene glycol, 1,2-hexanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol. Of these, propylene glycol is preferred.
[0058] Examples of glycol ether-based solvents include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monoethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, diethylene glycol monoisopropyl ether, triethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, triethylene glycol monoisobutyl ether, ethylene glycol monohexyl ether, diethylene glycol monohexyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, and tripropylene glycol monomethyl ether.
[0059] The content of the glycol solvent and / or glycol ether solvent is preferably from 1 to 20 mass %, more preferably from 2 to 18 mass %, and even more preferably from 3 to 15 mass %, of the total mass of the ink.
[0060] In order to control the wettability of the ink to the substrate and the drying property of the ink, the water-based ink of the present invention preferably further contains a hydrophilic solvent in addition to the above-mentioned solvents. From the viewpoint of the leveling property and drying property of the ink, the content of the hydrophilic solvent is preferably 0.5 to 10 mass % and more preferably 1 to 5 mass % in 100 mass % of the water-based ink.
[0061] Examples of hydrophilic solvents include monohydric alcohol solvents such as ethanol, 1-propanol, 2-propanol, 1-butanol, 2-methyl-1-propanol, 2-butanol, and 2-methyl-2-propanol, which can be used alone or in combination of two or more. Among these, 1-propanol and 2-propanol are preferred.
[0062] <Pigments> The water-based ink of the present invention preferably further contains a pigment. As the pigment, for example, achromatic pigments such as carbon black, titanium oxide, calcium carbonate, etc. or chromatic organic pigments can be used. Organic pigments such as yellow, magenta, cyan, and black are preferably blended in a ratio of 5 to 30% by mass in 100% by mass of the water-based ink. In the case of white titanium oxide, it is preferably blended in a ratio of 10 to 60% by mass in 100% by mass of the water-based ink.
[0063] Examples of organic pigments include insoluble azo pigments such as toluidine red, toluidine maroon, Hansa yellow, benzidine yellow, and pyrazolone red; soluble azo pigments such as lithol red, heliobordeaux, pigment scarlet, and permanent red 2B; derivatives of vat dyes such as alizarin, indanthrone, and thioindigo maroon; phthalocyanine organic pigments such as phthalocyanine blue and phthalocyanine green; quinacridone organic pigments such as quinacridone red and quinacridone magenta; perylene organic pigments such as perylene red and perylene scarlet; and isoindolinone. Examples of suitable pigments include isoindolinone-based organic pigments such as pyranthrone yellow and isoindolinone orange, pyranthrone-based organic pigments such as pyranthrone red and pyranthrone orange, thioindigo-based organic pigments, condensed azo-based organic pigments, benzimidazolone-based organic pigments, quinophthalone-based organic pigments such as quinophthalone yellow, and isoindoline-based organic pigments such as isoindoline yellow. Other pigments include flavanthrone yellow, acylamide yellow, nickel azo yellow, copper azomethine yellow, perinone orange, anthrone orange, dianthraquinonyl red, and dioxazine violet.
[0064] Examples of organic pigments by Color Index (CI) number are CI Pigment Yellow 12, 13, 14, 17, 20, 24, 74, 83, 86, 93, 109, 110, 117, 120, 125, 128, 129, 137, 138, 139, 147, 148, 150, 151, 153, 154, 155, 166, 168, 180, 185, CI Pigment Orange 16, 36, 43, 51, 55, 59, 61, CI Pigment Red 9, 48, 49, 52, 5 3, 57, 97, 122, 123, 149, 168, 177, 180, 192, 202, 206, 215, 216, 217, 220, 223, 224, 226, 227, 228, 238, 240, CI Pigment Violet 19, 23, 29, 30, 37, 40, 50, CI Pigment Blue 15, 15:1, 15:3, 15:4, 15:6, 22, 60, 64, CI Pigment Green 7, 36, CI Pigment Brown 23, 25, 26, etc.
[0065] Specific examples of carbon black include Degussa's Special Black 350, 250, 100, 550, 5, 4, 4A, 6, Printex U, V, 140U, 140V, 95, 90, 85, 80, 75, 55, 45, 40, P, 60, L6, L, 300, 30, 3, 35, 25, A, G, and Cabot's REGAL 400R, 660R, 330R, 250R, and MOGUL Examples include "MA7, 8, 11, 77, 100, 100R, 100S, 220, 230" and "#2700, #2650, #2600, #200, #2350, #2300, #2200, #1000, #990, #980, #970, #960, #950, #900, #850, #750, #650, #52, #50, #47, #45, #45L, #44, #40, #33, #332, #30, #25, #20, #10, #5, CF9, #95, #260" manufactured by Mitsubishi Chemical Corporation.
[0066] Specific examples of titanium oxide include "Tipaque CR-50, 50-2, 57, 80, 90, 93, 95, 953, 97, 60, 60-2, 63, 67, 58, 58-2, 85", "Tipaque R-820, 830, 930, 550, 630, 680, 670, 580, 780, 780-2, 850, 855", "Tipaque A-100, 220", "Tipaque W-10", "Tipaque PF-740, 744", and "TTO-55(A ), 55(B), 55(C), 55(D), 55(S), 55(N), 51(A, 51(C)", "TTO-S-1, 2", "TTO-M-1, 2", Teika's "Titanix JR-301, 403, 405, 600A, 605, 600E, 603, 805, 806, 701, 800, 808", "Titanix JA-1, C, 3, 4, 5", DuPont's "Tipure R-900, 902, 960, 706, 931", etc.
[0067] <Extender pigment> The water-based ink of the present invention preferably contains a body pigment. Examples of body pigments preferably used in water-based inks include calcium carbonate, magnesium carbonate, barium sulfate, white carbon, talc, aluminum hydroxide, magnesium hydroxide, alumina white, silica powder, diatomaceous earth, silica, calcium silicate, attapulgite, sericite, mica, hydrotalcite, bentonite, zeolite, kaolin clay, and pyrophyllite. These may be used alone or in combination. Among them, it is preferable to contain barium sulfate and / or silica, and it is even more preferable to contain barium sulfate.
[0068] The content of the extender pigment is preferably from 0.1 to 10 mass %, more preferably from 0.5 to 8 mass %, and even more preferably from 1 to 5 mass %, of the total mass of the water-based ink.
[0069] <Additives> Suitable additives that can be used in the water-based ink include a hardener, an antiblocking agent, a thickener, a rheology modifier, an antifoaming agent, a leveling agent, a preservative, a surface tension modifier, polyolefin particles, and the like.
[0070] (Polyolefin particles) The water-based ink of the present invention preferably further contains polyolefin particles for the purposes of improving the rub resistance of the ink film and improving the drying properties of the water-based ink.
[0071] The melting point of the polyolefin particles is preferably 90 to 140° C., more preferably 95 to 135° C., and even more preferably 95 to 125° C. The average particle size of the polyolefin particles is preferably 0.5 to 10 μm, more preferably 0.5 to 8 μm, and even more preferably 0.5 to 5 μm. The average particle size is a value measured by the Coulter Counter method. Polyolefin particles having the above particle size and melting point form a strong ink coating that is compatible with the water-based urethane resin, and promote improvement of water-rub resistance.
[0072] The content of polyolefin particles is preferably 0.5 to 5 mass % in terms of solid content in the total mass of the water-based ink. When it is 0.5 mass % or more, water friction resistance is improved, and when it is used at 5 mass % or less, the water-based ink has good stability over time.
[0073] As the polyolefin particles, commercially available polyolefin particles can be used, for example, Chemipearl W100, W200, W300, W310, W306, W400, W401, W4005, W410, W500, WF640, W700, W800, W900, W950, WH201, and WP100 manufactured by Mitsui Chemicals, Inc.
[0074] (Hydrazide additives) The water-based ink of the present invention may contain a hydrazide additive for the purpose of improving adhesion to a substrate, room temperature crosslinking of the resin (when the resin contains a keto group), etc. An example of the hydrazide additive is adipic acid hydrazide.
[0075] <Water-based ink manufacturing method> The water-based ink can be produced by dissolving and / or dispersing (pigment dispersion) a resin and a color pigment in water and a specified amount of a solvent, as described in, for example, JP 2020-186344 A. Thereafter, the obtained dispersion can be mixed with additives, a liquid medium, etc. as necessary to produce the water-based ink. As a dispersing machine used for dispersing the pigment, a commonly used machine such as a roller mill, a ball mill, a pebble mill, an attritor, a sand mill, etc. can be used. Among them, it is preferable to disperse the pigment using a sand mill, a gamma mill, or other bead mill.
[0076] The viscosity of the water-based ink produced by the above method is preferably in the range of 10 mPa s or more from the viewpoint of preventing sedimentation of the pigment and adequately dispersing it, and 1000 mPa s or less from the viewpoint of workability during ink production and printing. The above viscosity is measured at 25°C using a B-type viscometer. The viscometer may be one manufactured by Tokimec Co., Ltd.
[0077] <Printed material> The printed matter in this embodiment has a printed layer made of the water-based flexographic ink according to claim 1 or 2 on a substrate 1. The printed matter has a printed layer formed, for example, on the surface of a substrate by printing with the water-based ink by a flexographic printing method.
[0078] (Flexographic printing method) In flexographic printing, ink is supplied from an ink container directly or via an ink supply pump or the like to an anilox roller, which has an uneven surface. The ink supplied to the anilox roller is transferred to the plate surface through contact with the raised parts of the plate, and then finally transferred to the substrate through contact between the plate surface and the substrate, forming an image and / or letters.
[0079] <Base material> The substrate is wound up and is in the form of a roll with a set width. Therefore, it is different from sheets of paper that are cut into individual pieces in advance. The width of the substrate is appropriately selected based on the plate width of the printing press to be used and the width of the image (picture) part of the gravure plate. When printing by overlapping multiple colors of ink, there is no particular restriction on the order in which the inks are printed.
[0080] (Base material 1) The type and thickness of the substrate 1 are not particularly limited, but it is preferably a plastic substrate. Specific examples of substrates used for printed matter include polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate, polyethylene naphthalate, polycarbonate, and polylactic acid; polyamide resins such as nylon 6 and nylon 12; polystyrene resins such as polystyrene, AS resin, and ABS resin, chlorine-containing resins such as polyvinyl chloride and polyvinylidene chloride; ethylene-vinyl alcohol copolymer resins; cellophane; paper; metal foils such as aluminum, stainless steel, and iron; or film or sheet-like materials made of composite materials thereof. Among these, polyolefin resins and / or polyester resins are preferred.
[0081] The substrate 1 is preferably subjected to an easy-adhesion treatment on the surface to be printed (the surface in contact with the printing layer), and examples of the easy-adhesion treatment include corona discharge treatment, ultraviolet / ozone treatment, plasma treatment, oxygen plasma treatment, and primer treatment. For example, corona discharge treatment produces hydroxyl groups, carboxyl groups, carbonyl groups, and the like on the substrate. When the resin in the ink has a functional group such as a hydroxyl group, these functional groups can form hydrogen bonds with the resin.
[0082] <Laminate> The laminate in this embodiment has a substrate 1, a printed layer made of the water-based flexographic ink according to claim 1 or 2, and a substrate 2 in this order. The laminate can be obtained, for example, by further laminating the printed layer of the printed matter. The laminate can be obtained by applying an anchor coat or adhesive or the like onto the printed layer, drying it, and then bonding it to the substrate 2. The substrate 2 may be the same as or different from the substrate 1, and preferably has thermoplasticity (heat sealability). For example, an unstretched polyolefin substrate can be used. In this laminate, the printed layer made of water-based ink is positioned as an intermediate layer (for example, substrate 1 / printed layer / adhesive layer / substrate 2).
[0083] The lamination method is preferably a non-solvent lamination method, a dry lamination method, an extrusion lamination method, etc. Among them, the non-solvent lamination method is preferable.
[0084] (Non-sol lamination method) The non-solvent lamination method is a method in which a solvent-free adhesive is applied to the printed layer of the obtained printed matter, and then laminated by pressing with a sealant base material. The most common adhesive is a two-part type of polyol / isocyanate, and specific examples include Toyo-Morton's EA-N373A / EA-N373B.
[0085] (Dry lamination method) The dry lamination method involves diluting the adhesive to an appropriate viscosity with an organic solvent, applying it to the printed layer of the resulting printed matter, drying it, and then laminating it by pressing it onto the sealant base material. The most common adhesive is a two-part polyol / isocyanate type, and specific examples include Toyo-Morton's TM-250HV / CAT-RT86L-60, TM-550 / CAT-RT37, and TM-314 / CAT-14B.
[0086] (Extrusion lamination method) The extrusion lamination method is a method in which a thermoplastic resin is melted and extruded into a film form from a slit-shaped die called a T-die onto the printed layer side of the obtained printed matter, and then laminated onto a substrate. An anchor coating agent is often applied to the printed layer side of the printed matter before lamination. It is also possible to extrude molten resin onto the printed layer of the printed matter, and then attach a sealant substrate from a separate unwinder. Anchor coating agents include imine-based, butadiene-based, Isocyanate-based anchor coating agents can be used. Specific examples of suitable agents include EL-420 (imine-based), EL-452 (butadiene-based), EL-530A / B (isocyanate-based), and EL-540 / CAT-RT32 (isocyanate-based) manufactured by Toyo-Morton Co., Ltd. As the molten resin, low-density polyethylene, polypropylene, ethylene-vinyl acetate copolymer, and the like can be used. Specific examples of suitable agents include Novatec LD LC600A (low-density polyethylene) manufactured by Japan Polyethylene Corporation. EXAMPLES
[0087] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the invention. In the examples, "parts" means "parts by mass" and "%" means "% by mass".
[0088] <Mass average molecular weight, number average molecular weight> The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by gel permeation chromatography (GPC) and calculated as molecular weights using polystyrene as a standard substance under the following measurement conditions. GPC equipment: Showa Denko Shodex GPC-104 Columns: The following columns were used in series connection: Showa Denko Shodex LF-404 x 2 Showa Denko Shodex LF-G Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 0.3mL / min
[0089] <Glass transition temperature> The glass transition temperature was measured at the maximum value of tan δ using a dynamic viscoelasticity measuring device (DVA-200 manufactured by IT Measurement & Control Co., Ltd.) The measurement conditions are shown below. Measurement sample: Dried resin film with a thickness of 150 μm Measurement temperature range: -70~200℃ Temperature rise: 5℃ / min Measurement frequency: 10Hz
[0090] <Hydroxyl value and acid value> It was determined according to the method described in JIS K0070.
[0091] [Synthesis Example 1-1] (Synthesis of Water-Based Urethane Resin (X) UX01) In a reactor equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen gas inlet tube, 150.0 parts of poly(3-methyl-1,5-pentane adipate)diol having a number average molecular weight of 2000, 15.0 parts of polyethylene glycol having a number average molecular weight of 2000, 30.0 parts of 2,2-dimethylolbutanoic acid and 90.0 parts of isophorone diisocyanate were reacted at the boiling point in 200 parts of methyl ethyl ketone for 6 hours while introducing nitrogen gas to obtain a terminal isocyanate prepolymer, and then cooled to 40°C and 100 parts of acetone were added to obtain a solvent solution of the terminal isocyanate prepolymer. Next, the obtained terminal isocyanate prepolymer solution was gradually added at room temperature to a mixture of 15.0 parts of 2-hydroxyethylethylenediamine and 400 parts of acetone, and reacted at 50°C for 3 hours to obtain a solvent-based polyurethane resin solution. Next, 18.0 parts of triethylamine and 700 parts of deionized water were gradually added to the above solvent-based polyurethane resin solution to neutralize and make it water-soluble, and then all of the methyl ethyl ketone and acetone were distilled off under azeotropic conditions, and water was added to adjust the viscosity, thereby obtaining an aqueous urethane resin (X)UX01 having an acid value of 38 mgKOH / g, a solid content of 25% and a mass average molecular weight of 25,000.
[0092] [Synthesis Examples 1-2 to 1-10, Comparative Synthesis Examples 1-1 and 1-2] (Synthesis of Water-Based Urethane Resins (X) UX02 to UX10, Water-Based Urethane Resins PU01 and PU02) Aqueous urethane resins (X) UX02 to UX10 and comparative aqueous urethane resins PU01 and PU02 of Synthesis Example were synthesized in the same manner as in Synthesis Example 1-1, except that the raw materials and charging ratios shown in Table 1 were used. The mass average molecular weight was measured by GPC during the process of obtaining a solvent-based polyurethane resin solution and the process of distilling off all of the methyl ethyl ketone and acetone under azeotropic conditions, while adjusting the reaction time as appropriate, and the mass average molecular weight shown in Table 1 was determined. The following raw materials were used in the synthesis. PMPA2000: Poly(3-methyl-1,5-pentane adipate)diol (number average molecular weight 2000) NPG2000: Poly(neopentyl adipate)diol (number average molecular weight 2000) PEG2000: Polyethylene glycol (number average molecular weight 2000) PTMG2000: Polytetramethylene glycol (number average molecular weight 2000) C-2090: Kuraray MPD / HD / PC polycarbonate polyol (number average molecular weight 2000) DMBA: 2,2-dimethylolbutanoic acid IPDI: Isophorone diisocyanate AEA: 2-hydroxyethylethylenediamine
[0093] [Table 1]
[0094] [Synthesis Example 2-1] (Synthesis of Water-Based Urethane Resin (Y) UY01) While introducing nitrogen gas into a reaction vessel equipped with a thermometer, a stirrer, a reflux condenser, a stirring device, and a reflux condenser, 60.0 parts of polyethylene glycol having a number average molecular weight of 400, 75.0 parts of polyethylene glycol having a number average molecular weight of 1000, 30.0 parts of polytetramethylene glycol having a number average molecular weight of 2000, 15.0 parts of 2,2-dimethylolbutanoic acid, 24.0 parts of N,N-bis(2-hydroxypropyl)aniline, and 6.0 parts of 1,4-cyclohexanedimethanol were charged and reacted at 90°C for 3 hours. Under stirring, 90.0 parts of isophorone diisocyanate was added dropwise over 20 minutes and the temperature was raised to 140°C. After cooling, the resulting water-soluble resin was neutralized by gradually adding a mixed solution of 6.5 parts of 28% ammonia water and ion-exchanged water dropwise to make it water-soluble, and an aqueous urethane resin (Y)UY01 with a solid content of 20% was obtained. The resulting aqueous urethane resin (Y) UY01 had an acid value of 19.0 mgKOH / g and a mass average molecular weight (Mw) of 15000. The acid value and mass average molecular weight (Mw) were measured by the methods described above.
[0095] [Synthesis Examples 2-2 to 2-7, Comparative Synthesis Example 2-1] (Synthesis of Water-Based Urethane Resins (Y) UY02 to UY07, Water-Based Urethane Resin PU03) Water-based urethane resins (Y) UY02 to UY07 and water-based urethane resin PU03 were synthesized in the same manner as in Synthesis Example 2-1, except that the raw materials and charging ratios shown in Table 2 were used. The following raw materials were used in the synthesis. PEG200: Polyethylene glycol with a number average molecular weight of 200 PEG600: Polyethylene glycol with a number average molecular weight of 600 PEG1000: Polyethylene glycol with a number average molecular weight of 1000 PTMG2000: Polytetramethylene glycol with a number average molecular weight of 2000 PMPA2000: Poly(3-methyl-1,5-pentane adipate)diol (number average molecular weight 400) C-2090: Kuraray MPD / HD / PC polycarbonate polyol (number average molecular weight 2000) DMBA: 2,2-dimethylolbutanoic acid PDIA: N,N-bis(2-hydroxypropyl)aniline CHDM: 1,4-cyclohexanedimethanol IPDI: Isophorone diisocyanate
[0096] [Table 2]
[0097] (Example 1) Preparation of water-based flexographic ink (INK1) and creation of printed matter 25.0 parts of pigment [Toyo Color Co., Ltd. indigo pigment CI Pigment Blue 15:3], 3.0 parts of barium sulfate, 35.0 parts of water-based urethane resin (X) UX01 of synthesis example 1, 10.0 parts of water-based urethane resin (Y) UY01, 16.0 parts of ion-exchanged water, 0.5 parts of acetylene glycol surfactant [Surfynol 420, Nissin Chemical Industry Co., Ltd.], 0.3 parts of adipic acid hydrazide, and 2.0 parts of isopropanol were added, and the mixture was stirred for 10 minutes with a stirrer, and then dispersed for 10 minutes using a bead mill dispersing machine, Eiger Mill (Eiger Co., Ltd. bead mill), to obtain a pigment dispersion. 3.0 parts of Mitsui Chemical Co., Ltd. Chemipearl W500 (solid content 40.0%), 5.0 parts of propylene glycol, and 0.2 parts of triethylamine were added to the pigment dispersion, and the mixture was kneaded to obtain the target water-based ink (INK1).
[0098] The above water-based ink (INK1) was applied to a flexographic plate (photopolymer plate, KODAK FLEXCEL NXH digital flexographic plate, plate thickness 1.14 mm, screen ruling 175 lpi) and an anilox roll (1200 lpi, 3 cc / m 2 Using a flexographic printing machine (MIRAFLEX CM) equipped with a printer, 30,000 m of printing was performed on substrate 1 (polyethylene terephthalate substrate (PET) E5100, 12 μm thick) at a speed of 300 m / min under an environment of 30°C temperature and 10% humidity, to obtain a printed matter. The drying conditions for the ink layer were drying temperature: intercolor dryer 100°C, tunnel dryer 100°C.
[0099] (Examples 2 to 23 and Comparative Examples 1 to 5) Production of Water-Based Inks (INK2 to 28) and Creation of Printed Matter Inks INK2 to INK28 of Examples 2 to 23 and Comparative Examples 1 to 5 were prepared in the same manner as in Example 1 above, except that the raw materials and ratios shown in Tables 3 and 4 were used. Printing was performed in the same manner as above to obtain printed matter.
[0100] (Examples 1 to 23 and Comparative Examples 1 to 5) Preparation of packaging bags using laminates A polyisocyanate adhesive [EA-N373A / EA-N373B] (manufactured by Toyo-Morton) was applied onto the printed layer of the obtained print, and a CPP (manufactured by Japan Polychem Corporation) was attached as a sealant onto the applied surface using a non-sul laminating machine at a line speed of 50 m / min, and lamination processing was performed. The laminate was aged at 40 degrees for 48 hours. The edges of the CPP surfaces of this laminate were heat-sealed at 190° C. to form a bag, thereby obtaining a packaging bag. The content was water. A retort resistance test was carried out using this packaging bag.
[0101] The above printed matter and laminate were used to evaluate the plate entanglement resistance, blocking resistance, and lamination strength by the methods described below.
[0102] [Plate tangling resistance] For the prints obtained in the above Examples and Comparative Examples, the plate entanglement resistance of the 1% dot area was evaluated for the printed area after printing 30,000 m at a printing speed of 300 m / min. This is an evaluation of the low dot % area during high-speed printing, which is a very severe condition. A: No thickening of the 1% halftone dots is observed and a clear image is formed. (Excellent) B: Slight thickening is observed in the 1% dot area, and the dots are not connected. (Good) C: 1% dots are slightly thickened and the dots are not connected. (Usable) D: 1% The shape of the dots is distorted and dot bridging is observed (poor). The practical level is rated A to C.
[0103] [Blocking resistance] The printed matter obtained in the above examples and comparative examples was rewound from the outside of the roll to the core in the state in which the printed matter was produced and wound, and the degree of ink peeling and peeling resistance were evaluated. Note that the conditions for evaluating blocking resistance during winding were stricter than those for evaluation by simple press load and pressure, and the evaluation criteria were as follows. A: No ink loss and no peeling resistance when rewound (Excellent) B: No ink is removed and there is slight peeling resistance when rewound (good) C: No ink loss and weak peel resistance when rewound (usable) D: Ink is removed and there is strong resistance to peeling when rewound (defective) The practical level is rated A to C.
[0104] [Laminate strength] The packaging bags using the laminates obtained in the above Examples and Comparative Examples were subjected to a retort test at 120°C for 80 minutes, and the laminate strength immediately after retort was compared with the laminate strength before the retort test. Regarding the laminate strength, the laminate was cut to a width of 15 mm, and the printed layer and the substrate 2 were peeled off from each other, and the peel strength was evaluated using an Intesco 201 universal tensile tester. Note that the laminate strength after retort resistance is likely to decrease, and the conditions are excessively stricter than the conditions for measuring laminate strength that are usually performed, and the evaluation criteria are as follows. A: No decrease in peel strength was observed before and after retort, and the peel strength after retort was 2.0N / 15mm or more (excellent) B: A decrease in peel strength of less than 1.0 N / 15 mm was observed before and after retort, and the peel strength after retort was 2.0 N / 15 mm or more (good). C: A decrease in peel strength of 1.0N / 15mm or more was observed before and after retort, and the peel strength after retort was 1.0N / 15mm or more and less than 2.0N / 15mm (usable). D: A decrease in peel strength of 1.0 N / 15 mm or more was observed before and after retort, and the peel strength after retort was less than 1.0 N / 15 mm (defective). The practical level is rated A to C.
[0105] [Table 3]
[0106] [Table 3]
[0107] [Table 4]
[0108] <Evaluation Results> As shown in Table 3, the examples provided water-based inks that were all at practical levels in terms of plate tangling resistance, blocking resistance, and lamination strength, while the comparative examples provided water-based inks that were not at practical levels in terms of at least one of plate tangling resistance, blocking resistance, and lamination strength, as shown in Table 4.
Claims
1. An aqueous flexographic ink comprising an aqueous urethane resin (X) having a mass average molecular weight of 20,000 or more and 100,000 or less, and an aqueous urethane resin (Y) having a mass average molecular weight of 3,000 or more and less than 20,000, The aqueous flexographic ink, wherein the aqueous urethane resin (X) contains a structural unit derived from a polyester polyol and / or a polyether polyol.
2. 3. The water-based flexographic ink according to claim 1, wherein the water-based urethane resin (Y) contains a constituent unit derived from a polyester polyol and / or a polyether polyol.
3. 3. The water-based flexographic ink according to claim 1, wherein the mass ratio of the water-based urethane resin (X) to the water-based urethane resin (Y) is 90:10 to 55:
45.
4. The water-based flexographic ink according to claim 1 or 2, wherein the acid value of the water-based urethane resin (X) is 10 to 60 mgKOH / g.
5. The water-based flexographic ink according to claim 1 or 2, further comprising a glycol-based solvent and / or a glycol ether-based solvent.
6. The water-based flexographic ink according to claim 1 or 2, further comprising an organic amine.
7. A printed matter having a printing layer formed on a substrate 1 and comprising the aqueous flexographic ink according to claim 1 or 2.
8. A laminate comprising a substrate 1, a printing layer made of the aqueous flexographic ink according to claim 1 or 2, and a substrate 2 in this order.
Citation Information
Patent Citations
Rotary printing ink and use thereof
JP2018184512A
Aqueous gravure or flexographic ink
JP2021031572A
Water-based ink for soft packaging
JP2022188799A
Cited By
Aqueous ink composition, ink-coated film, method for manufacturing the same, laminate film, and packaging material
JP7916589B1