Coating liquid, method for producing thermal recording medium, and thermal recording medium

A coating liquid with a solvent content of 1% to 5% by mass improves the transparency of heat-sensitive recording materials, addressing the issue of obscured container contents and eliminating the need for explosion-proof equipment.

JP2024157787AInactive Publication Date: 2024-11-08OSAKA SEALING PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023072365
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Heat-sensitive recording materials used as labels or packaging films for containers can obscure the contents, making it difficult for consumers to identify the contents of opaque containers.

Method used

A coating liquid for forming an intermediate layer in heat-sensitive recording materials containing a binder and a solvent in the range of 1% to 5% by mass, which improves the leveling property and smoothness of the intermediate layer, enhancing transparency and reducing the need for explosion-proof equipment.

Benefits of technology

The solution enhances the transparency of heat-sensitive recording materials, allowing consumers to easily identify the contents of opaque containers while avoiding the need for specialized safety equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157787000001_ABST
    Figure 2024157787000001_ABST
Patent Text Reader

Abstract

To provide a coating liquid that can improve transparency of an intermediate layer 4 of a thermal recording medium 1, a method for producing a thermal recording medium using the same, and a thermal recording medium.SOLUTION: The present invention provides coating liquid for forming an intermediate layer of a thermal recording medium, which has a thermal recording layer 3 as well as the intermediate layer 4 on a substrate 2. The coating liquid contains a binder and also contains 1 mass% or more and 5 mass% or less of a solvent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating liquid suitable for forming an intermediate layer of a thermosensitive recording medium, a method for producing a thermosensitive recording medium using the same, and a thermosensitive recording medium. [Background technology]

[0002] A thermal recording medium develops color when heated by a thermal head or the like, and a recorded image is obtained. Thermal recording media are used in a wide range of applications, such as printers for output of facsimiles, automatic ticket vending machines, scientific measuring instruments, and CRT medical measuring instruments (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-362027 A Summary of the Invention [Problem to be solved by the invention]

[0004] When such a thermal recording medium is used, for example, as a label or packaging film for containers containing various foods, if the thermal recording medium is opaque, the contents of the container will be hidden by the label or packaging film, making it difficult for consumers to see the contents.

[0005] For this reason, it is desirable to improve the transparency of the thermosensitive recording medium so that the contents of the container can be confirmed.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and focuses on the transparency of the intermediate layer formed on the thermosensitive recording layer, with the object of providing a coating liquid for forming an intermediate layer that is effective in improving the transparency of a thermosensitive recording material, a method for manufacturing a thermosensitive recording material using the same, and a thermosensitive recording material. [Means for solving the problem]

[0007] In order to achieve the above object, the present invention is configured as follows.

[0008] (1) The coating liquid of the present invention is a coating liquid for forming an intermediate layer of a thermosensitive recording material having a thermosensitive recording layer and an intermediate layer on a substrate, and contains a binder and 1% by mass or more and 5% by mass or less of a solvent.

[0009] According to the coating liquid for forming the intermediate layer of the present invention, by containing a solvent in an amount of 1% by mass or more and 5% by mass or less, the leveling property of the coating liquid is improved, and the smoothness of the intermediate layer is improved. This makes it possible to increase the transparency of the intermediate layer of the thermosensitive recording medium. As a result, this contributes to improving the transparency of the entire thermosensitive recording medium.

[0010] In addition, since the coating liquid only needs to contain a solvent in an amount of 5 mass % or less, there is no need for explosion-proof equipment when using the coating liquid.

[0011] (2) In a preferred embodiment of the present invention, the solvent is at least one of 2-propanol, propylene glycol, and 1,3 propanediol.

[0012] According to this embodiment, the transparency of the intermediate layer of the thermosensitive recording medium can be improved by preparing the coating liquid by adding at least one solvent selected from the group consisting of 2-propanol, propylene glycol, and 1,3-propanediol, which contributes to improving the transparency of the entire thermosensitive recording medium.

[0013] (3) In another embodiment of the present invention, a crosslinking agent is included.

[0014] According to this embodiment, crosslinking is promoted by the solvent and crosslinking agent contained in the coating liquid, and crosslinking is completed earlier and the state of the intermediate layer is stabilized compared to the case where only the crosslinking agent is used without a solvent.

[0015] (4) In still another embodiment of the present invention, the binder contains a core-shell resin and a core resin that does not have a shell portion of the core-shell resin.

[0016] According to this embodiment, since the intermediate layer contains a core-shell type resin having a hydrophilic shell portion, a smooth intermediate layer with good film-forming properties is formed, while since the intermediate layer contains a core type resin having no hydrophilic shell portion, deterioration of water resistance can be prevented. In this way, by preventing deterioration of the water resistance of the intermediate layer, deterioration of the water resistance of the entire thermal recording medium can also be prevented.

[0017] (5) A method for producing a thermal recording medium according to the present invention is a method for producing a thermal recording medium having a thermal recording layer and an intermediate layer on a substrate, comprising the steps of: The method includes a step of forming an intermediate layer using a coating liquid for forming the intermediate layer, the coating liquid containing a binder and 1% by mass or more and 5% by mass or less of a solvent.

[0018] According to the method for producing a thermosensitive recording medium of the present invention, the coating liquid for forming the intermediate layer contains a solvent in an amount of 1% by mass or more and 5% by mass or less, so that the leveling property is good and the smoothness of the intermediate layer is improved. This makes it possible to increase the transparency of the intermediate layer of the thermosensitive recording medium. As a result, this contributes to improving the transparency of the entire thermosensitive recording medium.

[0019] In addition, since the coating liquid only needs to contain a solvent in an amount of 5 mass % or less, there is no need for explosion-proof equipment when using the coating liquid.

[0020] (6) In another embodiment of the present invention, the coating liquid contains at least one of 2-propanol, propylene glycol, and 1,3 propanediol as the solvent.

[0021] According to this embodiment, the transparency of the intermediate layer of the thermosensitive recording medium can be improved by preparing the coating liquid by adding at least one solvent selected from the group consisting of 2-propanol, propylene glycol, and 1,3-propanediol, which contributes to improving the transparency of the entire thermosensitive recording medium.

[0022] (7) In still another embodiment of the present invention, the method further comprises a step of forming a topcoat layer on the intermediate layer, and the coating liquid contains a crosslinking agent.

[0023] According to this embodiment, crosslinking is promoted by the solvent and crosslinking agent contained in the coating liquid for forming the intermediate layer, and crosslinking is completed earlier and the state of the intermediate layer is stabilized compared to the case where only the crosslinking agent without the solvent is used, so that the time required for aging from the step of forming the intermediate layer to the step of forming the top coat layer can be shortened.

[0024] (8) In one embodiment of the present invention, the coating liquid contains, as the binder, a core-shell resin and a core resin that does not have a shell portion of the core-shell resin.

[0025] According to this embodiment, since the intermediate layer contains a core-shell type resin having a hydrophilic shell portion, a smooth intermediate layer with good film-forming properties is formed, while since the intermediate layer contains a core type resin having no hydrophilic shell portion, deterioration of water resistance can be prevented. In this way, deterioration of water resistance of the intermediate layer can be prevented, and thus deterioration of water resistance of the entire thermal recording medium can also be prevented.

[0026] (9) The thermosensitive recording medium of the present invention is a thermosensitive recording medium comprising a thermosensitive recording layer and an intermediate layer on a substrate, The intermediate layer is formed from a coating liquid for forming the intermediate layer, which contains a binder and 1% by mass or more and 5% by mass or less of a solvent.

[0027] According to the thermosensitive recording medium of the present invention, the intermediate layer is formed from a coating liquid containing 1% by mass or more and 5% by mass or less of a solvent, so that the smoothness of the intermediate layer is improved. This can increase the transparency of the intermediate layer of the thermosensitive recording medium. As a result, this contributes to improving the transparency of the entire thermosensitive recording medium.

[0028] In addition, since the coating liquid only needs to contain a solvent in an amount of 5 mass % or less, there is no need for explosion-proof equipment when using the coating liquid. Effect of the Invention

[0029] Thus, according to the present invention, the coating liquid for forming the intermediate layer contains a solvent in an amount of 1% by mass or more and 5% by mass or less, thereby improving the leveling property and smoothness of the intermediate layer. This can increase the transparency of the intermediate layer of the thermosensitive recording medium. As a result, this contributes to improving the transparency of the entire thermosensitive recording medium.

[0030] In addition, since the coating liquid only needs to contain a solvent in an amount of 5 mass % or less, there is no need for explosion-proof equipment when using the coating liquid. [Brief description of the drawings]

[0031] [Figure 1] FIG. 1 is a schematic cross-sectional view of a thermosensitive recording medium according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings.

[0033] 1 is a schematic cross-sectional view of a thermosensitive recording medium according to one embodiment of the present invention. The thermosensitive recording medium 1 of this embodiment is formed by laminating a thermosensitive recording layer 3 that develops color when heated, an intermediate layer 4, and a topcoat layer 5 on the upper surface of a substrate 2.

[0034] In order to increase the adhesion between the substrate 2 and the thermosensitive recording layer 3, an anchor layer may be provided.

[0035] The structure of each layer will be described below.

[0036] [Base material] A transparent synthetic resin film, such as a polypropylene film, a polyethylene terephthalate film, a polystyrene film, or a polycarbonate film, can be used as the substrate 2. There are no particular limitations on the thickness of such a film, but a thickness of, for example, about 10 μm to 100 μm is preferable since it provides excellent coatability to the substrate 2 and transparency of the substrate 2. In order to reduce the amount of resin material used and to eliminate the use of plastics, the thickness of the substrate 2 is preferably 50 μm or less, and more preferably 40 μm or less.

[0037] [Thermal recording layer] Materials for forming the thermosensitive recording layer 3 include a color former that changes color when heated, a color developer, a filler, a binder, a lubricant, and the like.

[0038] It is preferable to use each of the above materials with a fine particle size in order to increase the transparency of the intermediate layer and thereby improve the transparency of the thermal recording medium 1. Such materials with a fine particle size suppress diffuse reflection of the particles.

[0039] Specifically, the leuco dyes that are color formers include 3-(N-isobutyl-N-ethyl)amino-6-methyl-7-anilinofluoran, 3-(N-isopentyl-N-ethyl)amino-6-methyl-7-o-chloroanilinofluoran, 3-(N-ethyl-Np-toluidino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isopentyl)amino-6-methyl-7-anilinofluoran, 3-(N-ethoxypropyl-N-ethyl)amino-6-methyl-7-anilinofluoran, 3-(N-cyclohexyl-N-methyl)amino-6-methyl-7-anilinofluoran, 3-(N-methyl-Nn-propyl)amino-6-methyl-7-anilinofluoran, 3-dibutylamino-6-methyl-7-anilinofluoran, 3 -diethylamino-6-methyl-7-p-toluidinofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-8-methylfluoran, 3-diethylamino-7-(m-trifluoromethylanilino)fluoran, 3-diethylamino-7-(o-chloroanilino)fluoran, 3-diethylamino-7-chlorofluoran, 3-dibutylamino-6-methyl-7-bromofluoran, 3-dibutylamino-7-(o-chloroanilino)fluoran, 3-dipentylamino-6-methyl-7-anilinofluoran, 3-dimethylamino-5-methyl-7-methylfluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, crystal violet lactone, and the like can be used.

[0040] The particle size of the color former is preferably 0.1 μm to 1.0 μm. Here, the particle size refers to the 50% average particle size measured by a microtrack laser analysis / scattering type particle size analyzer. Hereinafter, "particle size" refers to the 50% average particle size measured by this microtrack laser analysis / scattering type particle size analyzer.

[0041] Examples of the developer include 1,1-bis(p-hydroxyphenyl)cyclohexane, 1,1-bis(p-hydroxyphenyl)propane, 2,2-bis(p-hydroxyphenyl)propane, 2,2-bis(p-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2'-methylenebis(4-chlorophenol), 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,4'-dihydroxydiphenylsulfone, 4,4'-dihydroxydiphenylsulfone, 4-hydroxy-4'-n-propoxydiphenylsulfone, 4-hydroxy-4'-isopropoxydiphenylsulfone, 4-hydroxy-4'-methyldiphenylsulfone, 4-hydroxyfur ... phenyl-4'-benzyloxyphenyl sulfone, 4-hydroxy-4'-allyloxydiphenyl sulfone, bis(3-allyl-4-hydroxyphenyl)sulfone, poly(4-hydroxybenzoic acid), benzyl 4-hydroxybenzoate, 2,4-bis(phenylsulfonyl)phenol, α-{4-[(4-hydroxyphenyl)sulfonyl]phenyl}-ω-hydroxypoly(degree of polymerization n=1-7)(oxyethyleneoxyethyleneoxy-p-phenylenesulfonyl-p-phenylene)2,2-bis[(4-methyl-3-phenoxycarbonylaminophenyl)urea]diphenyl sulfone, 3,5-bis(α-methylbenzyl)salicylic acid, bis[4-(n-octyloxycarbonylamino)salicylic acid zinc], 4,4'-bis(p-tolylsulfonylaminocarbonylamino)diphenylmethane, 4-hydroxybenzenesulfonanilide, 2'-(3-phenylureido)benzenesulfonanilide, N-(2-hydroxyphenyl)-2-[(4-hydroxyphenyl)thio]acetamide, N-(4-hydroxyphenyl)-2-[(4-hydroxyphenyl)thio]acetamide, 4-[[4-[4-[[4-(1-methylethoxy)phenyl]sulfonylphenoxy]butoxy]phenyl]sulfonyl]phenol, 4-tert-butylphenol-formaldehyde polycondensate, N-(p-toluenesulfonyl)N'-(3-p-toluenesulfonyloxyphenyl)urea, 1-phenyl-3-(4-methylphenylsulfonyl)urea, etc. can be used, and the particle size thereof is preferably 0.1 μm or more and 1.0 μm or less.

[0042] Examples of the filler that can be used include aluminum hydroxide, magnesium hydroxide, aluminum oxide, magnesium oxide, aluminum silicate, calcium carbonate, magnesium carbonate, titanium oxide, barium sulfate, silica gel, activated clay, talc, clay, kaolin, calcined kaolin, diatomaceous earth, white carbon, zinc oxide, silicon oxide, colloidal silica, polystyrene resin particles, urea-formalin resin particles, polyolefin resin particles, and the like, and the particle size thereof is preferably 1.0 μm or less.

[0043] Examples of the binder that can be used include polyvinyl alcohol, modified polyvinyl alcohol, starch, casein, gelatin, polyamide, polyacrylamide, modified polyacrylamide, hydroxyethyl cellulose, methyl cellulose, carboxymethyl cellulose, hydroxypropyl cellulose, polyvinyl acetate, polyacrylic acid esters, styrene-maleic anhydride copolymers, isobutylene-maleic anhydride copolymers, diisobutylene-maleic anhydride copolymers, vinyl acetate-maleic anhydride copolymers, methyl vinyl-maleic anhydride copolymers, isopropylene-maleic anhydride copolymers, styrene-butadiene copolymers, polyvinyl chloride, polyvinylidene chloride, vinyl chloride-vinyl acetate copolymers, polyurethane, polystyrene, polyvinylpyrrolidone, acrylic acid esters, acrylonitrile, and methyl vinyl ether.

[0044] Examples of the sensitizer that can be used include stearic acid, stearic acid amide, stearic acid anilide, methylol stearic acid amide, methylene bis stearic acid amide, ethylene bis stearic acid amide, 1-benzyloxynaphthalene, 2-benzyloxynaphthalene, 2,6-diisopropylnaphthalene, 1,2-diphenoxyethane, 1,2-diphenoxymethylbenzene, 1,2-bis(3,4-dimethylphenol)ethane, 1,2-bis(3-methylphenoxy)ethane, 1,2-bis(4-methylphenoxy)ethane, di(p-chlorobenzyl)oxalate, di(p-methylbenzyl)oxalate, dibenzyl oxalate, p-benzylbiphenyl, m-terphenyl, diphenyl sulfone, benzyl p-benzyloxybenzoate, dibenzyl terephthalate, and p-toluenesulfonamide.

[0045] As the lubricant, for example, paraffin wax, fatty acids such as oleic acid, polyolefin waxes such as polyethylene wax, metal soaps such as zinc stearate, ester waxes such as carnauba wax, silicone oil, whale oil, and other oils can be used, and the particle size thereof is preferably 0.5 μm or less.

[0046] It is known that it is particularly effective to incorporate paraffin wax into the thermosensitive recording layer 3 in order to improve the transparency of the thermosensitive recording medium 1. This paraffin has a low melting point below the color-developing temperature of the thermosensitive recording layer 3, preferably below 80°C, and more preferably below 50°C.

[0047] The particle size of the low melting point paraffin is preferably 0.5 μm or less as described above. The content of the paraffin is, for example, 0.1 g / m 2 ~1.0g / m 2 It is preferable that:

[0048] By incorporating low-melting point paraffin in this manner, when the coating liquid for forming the thermosensitive recording layer 3 is applied onto the substrate 2 and the coating liquid dries, the low-melting point paraffin melts and penetrates into and fills gaps in the unevenness of the surfaces of the particles that make up the thermosensitive recording layer 3. This suppresses diffuse reflection from the surfaces of the particles in the thermosensitive recording layer 3, and the transparency of the thermosensitive recording medium 1 can be improved.

[0049] [Middle layer] The intermediate layer 4 has a barrier property against water and oil, and improves the water resistance, chemical resistance, and the like of the thermosensitive recording layer 3 .

[0050] The intermediate layer 4 is mainly formed of a binder. Examples of the binder for the intermediate layer 4 include an emulsion of an acrylic resin, a resin having a water-soluble portion, and an SBR resin.

[0051] In order to improve the transparency of the thermal recording medium 1, the binder of the intermediate layer 4 can be a resin having a water-soluble portion, for example, polyvinyl alcohol (PVA), which is a resin having a hydroxyl group as a hydrophilic structural unit. Alternatively, a core-shell type resin, for example, a core-shell type acrylic resin, in which hydrophobic core particles are coated with a water-soluble shell polymer can be used. Furthermore, a core type resin consisting of a core portion having no shell portion of the core-shell type resin can also be used. The core portion of the core-shell type resin and the core portion of the core type resin may be the same or different.

[0052] Water-soluble polyvinyl alcohol and core-shell type acrylic resin have good film-forming properties. When the coating liquid for forming the intermediate layer is applied onto the thermosensitive recording layer 3 and dried, the resin having a water-soluble portion permeates into the thermosensitive recording layer 3 to form a smooth intermediate layer 4. This suppresses diffuse reflection in the thermosensitive recording layer 3 and improves the transparency of the thermosensitive recording layer 3.

[0053] The coating liquid for forming the intermediate layer 4 in this embodiment contains the above-mentioned binder and also contains 1% by mass or more and 5% by mass or less of a solvent based on the entire coating liquid.

[0054] As this solvent, for example, an alcohol-based solvent such as 2-propanol, which is a secondary alcohol, or propylene glycol and 1-3 propanediol, which are dihydric alcohols, is preferable.

[0055] By adding such a solvent to the coating solution, the leveling property during coating is improved, and the smoothness of the intermediate layer is improved, resulting in an increase in transparency, as will be shown in the examples below.

[0056] The coating liquid for forming the intermediate layer in this embodiment contains a crosslinking agent, the main component of which is preferably, for example, a carbodiimide compound, a polyamide epichlorohydrin resin, an oxazoline-based compound, or ammonium zirconium carbonate.

[0057] In order to enhance transparency, the crosslinking agent preferably contains, as its main component, a carbodiimide compound or a polyamide epichlorohydrin resin.

[0058] By adding the above-mentioned solvent to the coating liquid for forming the intermediate layer containing such a crosslinking agent, crosslinking is promoted and completed earlier than in the case of a coating liquid containing only a crosslinking agent, resulting in a stable state of the intermediate layer.

[0059] This makes it possible to shorten the time required for aging after the process of applying a coating liquid for forming an intermediate layer onto the thermal recording layer 3 to form the intermediate layer 4, until the process of applying a coating liquid for forming a topcoat layer onto the intermediate layer 4 to form a topcoat layer, and thus makes it possible to omit the aging process.

[0060] The coating liquid for forming the intermediate layer in this embodiment contains a filler in addition to the above-mentioned binder, solvent, and crosslinking agent, and also contains a wetting agent, etc., as necessary.

[0061] Examples of the filler include colloidal silica, calcium carbonate, polymethyl methacrylate (PMMA), and polystyrene (PS).

[0062] The particle size of these fillers is preferably 1.0 μm or less. In order to improve transparency, colloidal silica having a small particle size is preferred as the filler.

[0063] [Topcoat layer] The top coat layer 5 improves the matching of the thermosensitive recording layer 3 with the thermal head, allowing the thermosensitive recording layer 3 to develop color appropriately.

[0064] The topcoat layer 5 is made of a binder to which a filler, a lubricant, a crosslinking agent, etc. are added.

[0065] Examples of the resin that serves as the binder include acrylic resin. The lubricant may, for example, be polyethylene or zinc stearate.

[0066] The cross-linking agent may, for example, be zirconium carbonate.

[0067] Examples of the filler include colloidal silica, calcium carbonate, polymethyl methacrylate (PMMA), and polystyrene (PS).

[0068] The particle size of these fillers is preferably 1.0 μm or less. In order to improve transparency, colloidal silica having a small particle size is preferred as the filler.

[0069] The manufacturing method of the thermosensitive recording medium of this embodiment includes a step of applying a coating liquid for forming a thermosensitive recording layer onto the substrate 2 and drying it to form the thermosensitive recording layer 3, a step of applying a coating liquid for forming an intermediate layer onto the thermosensitive recording layer 3 and drying it to form the intermediate layer 4, and a step of applying a coating liquid for forming a topcoat layer onto the intermediate layer 4 and drying it to form the topcoat layer 5. EXAMPLES

[0070] Next, the present invention will be described in more detail based on specific examples, but the following examples are not intended to limit the present invention in any way.

[0071] The present inventors prepared a number of types of coating liquids with different solvent contents in order to evaluate the effect on transparency of the addition of a solvent to a coating liquid for forming an intermediate layer.

[0072] In these coating solutions, a carboxyl-containing acrylic resin was used as a binder. Specifically, Resin 1, which is a core-shell type acrylic resin having a hydrophobic acrylic core and a hydrophilic acrylic shell, and Resin 2, which is a core type resin consisting of a core part of the core-shell type acrylic resin without a shell part, were used as the binder.

[0073] This carboxyl group-containing acrylic resin is an acrylic resin that does not contain a SiOH group (silanol group), that is, an acrylic resin that is not modified with silane.

[0074] Resin 1, a core-shell type resin, has a solids concentration of 24.8%, a viscosity of 248 mPa·s at a rotation speed of 60 rpm, and a pH of 7.7.

[0075] Resin 2, which is a core-type resin, has a solids concentration of 20.2%, a viscosity of 940 mPa·s at a rotation speed of 60 rpm, and a pH of 8.

[0076] The binder was prepared by mixing the above-mentioned resin 1 and resin 2 in a mass ratio of "50:50."

[0077] As a crosslinking agent, Carbodilite V-10 (manufactured by Nisshinbo Chemical Co., Ltd.), whose main component is a carbodiimide compound, was used.

[0078] The crosslinking agent was added in an amount of "6" per "100" of binder in terms of mass ratio when dry.

[0079] 2-propanol was used as a solvent, and each coating liquid was prepared so that the content of 2-propanol relative to the entire coating liquid was 0.5 mass %, 1 mass %, 3 mass %, 4 mass %, 5 mass %, and 7 mass %.

[0080] Each of the prepared coating solutions for forming the intermediate layer was applied onto the thermosensitive recording layer 3 on the substrate 2 and dried to form an intermediate layer, and a number of samples were prepared. In each sample, no topcoat layer was formed, and the transparency up to the intermediate layer was evaluated.

[0081] Next, the configurations of the substrate 2 and the thermosensitive recording layer 3 of the embodiment will be specifically described, and this configuration is the same as that of the above-mentioned Patent Document 1 (Japanese Patent No. 6202599) previously proposed by the present applicant.

[0082] As the substrate 2, a 40 μm-thick OPP (biaxially oriented polypropylene) film was used.

[0083] The thermosensitive recording layer 3 used 3,3'-diallyl-4,4'-dihydroxydiphenylsulfone with a particle size of 0.4 μm as the developer, and kaolin with a particle size of 0.4 μm as the filler. The binder used was SBR with a glass transition temperature Tg of -3°C. The lubricant used was paraffin with a melting point of 46°C and a particle size of 0.2 μm. The dye used was 2-aniline-3-methyl-6-(N-methyl-p-toluidino)fluoran with a particle size of 0.5 μm.

[0084] The mass ratios of the developer, kaolin, SBR, paraffin, and dye when dry were 25, 10, 20, 4, and 12, respectively, for a total of 74.

[0085] A coating solution for forming a thermal recording layer having this composition was prepared, and applied to the OPP film in a coating amount of 4.5 g / m2 in terms of dry mass. 2 After coating, the coating was dried to form a thermosensitive recording layer 3.

[0086] On this thermal recording layer 3, a plurality of types of intermediate layer forming coating solutions having different solvent contents were applied in a coating amount of 2.0 g / m2 in terms of dry mass. 2 After coating so as to obtain the above, the coating was dried to form the intermediate layer 4, and a plurality of samples were prepared.

[0087] In this manner, the present inventors prepared a number of samples each having the intermediate layer 4 of the thermosensitive recording medium 1 shown in FIG. 1 formed thereon, and evaluated the transparency of each sample.

[0088] The transparency was evaluated by measuring the haze in accordance with JIS K 7136.

[0089] The haze value is calculated by the following formula.

[0090] HAZE(%)=DIF / TT×100 =(TT-PT) / TT×100 TT: Total light transmittance PT: Parallel transmittance DIF: Diffuse (scattered) light component The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 1 below.

[0091] [Table 1] As described above, the substrate of each of Samples No. 1 to No. 7 is an OPP film. In addition, the coating liquid for forming the intermediate layer used in producing each sample contains the above-mentioned resin 1 and resin 2 as the binder, Carbodilite V-10, the main component of which is a carbodiimide compound, as the crosslinking agent, and 2-propanol as the solvent.

[0092] In sample No. 1, the coating liquid for forming the intermediate layer does not contain 2-propanol as a solvent.

[0093] In each of Samples No. 2 to No. 7, the content of 2-propanol in the coating fluid for forming the intermediate layer was 0.5 mass %, 1 mass %, 3 mass %, 4 mass %, 5 mass %, and 7 mass % relative to the entire coating fluid.

[0094] The haze value up to the intermediate layer of Sample No. 1, which was formed using the coating liquid for forming the intermediate layer that did not contain 2-propanol, was 16.70.

[0095] The haze value up to the intermediate layer of Sample No. 2, which was formed using a coating liquid for forming an intermediate layer containing 0.5% by mass of 2-propanol, was 17.80.

[0096] The haze value up to the intermediate layer of Sample No. 3, which was formed using a coating liquid for forming an intermediate layer containing 1% by mass of 2-propanol, was 15.55.

[0097] The haze value up to the intermediate layer of Sample No. 4, which was formed using a coating liquid for forming an intermediate layer containing 3% by mass of 2-propanol, was 14.81.

[0098] The haze value up to the intermediate layer of Sample No. 5, which was formed using a coating liquid for forming an intermediate layer containing 4% by mass of 2-propanol, was 16.01.

[0099] The haze value up to the intermediate layer of Sample No. 6, which was formed using a coating liquid for forming an intermediate layer containing 5% by mass of 2-propanol, was 15.14.

[0100] The haze value up to the intermediate layer of Sample No. 7, which was formed using a coating liquid for forming an intermediate layer containing 7% by mass of 2-propanol, was 19.61.

[0101] Thus, the haze values ​​up to the intermediate layer formed by the coating liquid for forming the intermediate layer of Samples 3, 4, 5 and 6, which have 2-propanol contents of 1 mass%, 3 mass%, 4 mass% and 5 mass%, are all lower than the haze value of 16.70 up to the intermediate layer of Sample No. 1, which does not contain 2-propanol, indicating improved transparency.

[0102] In particular, sample No. 4, which contains 3 mass % of 2-propanol, has the lowest haze value of 14.81, and thus exhibits the greatest improvement in transparency.

[0103] On the other hand, in sample No. 2, in which the 2-propanol content is 0.5% by mass, which is less than 1% by mass, the effect of containing 2-propanol is not obtained, and the haze value of the intermediate layer is higher than the haze value of 16.70 of sample No. 1.

[0104] In addition, sample No. 7, in which the 2-propanol content is 7% by mass, which is greater than 5% by mass, has a haze value that is higher than the haze value of 16.70 of sample No. 1, and no improvement in transparency due to the addition of a solvent is observed.

[0105] Therefore, in order to improve the transparency, the content of 2-propanol is preferably from 1% by mass to 5% by mass.

[0106] If the solvent content exceeds 5% by mass, explosion-proof equipment is required as stipulated in the Ordinance for Prevention of Organic Solvent Poisoning. In contrast, the content of the 2-propanol solvent in this coating fluid for forming the intermediate layer is 5% by mass or less, so explosion-proof equipment is not required when using the coating fluid for forming the intermediate layer.

[0107] As described above, adding 2-propanol as a solvent to the coating liquid for forming the intermediate layer in an amount of 1% by mass or more and 5% by mass or less is effective in improving transparency.

[0108] The present inventors evaluated the effect of the type of crosslinking agent on the improvement in transparency due to the addition of the solvent. Specifically, for multiple types of crosslinking agents, samples were prepared in which the intermediate layer was formed using a coating liquid that did not contain the solvent 2-propanol, and samples in which the intermediate layer was formed using a coating liquid that contained 3% by mass of 2-propanol, and the haze value of the thermal recording medium up to the intermediate layer was measured in the same manner as above.

[0109] The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 2 below.

[0110] [Table 2] As shown in Table 2, the base material, binder, and solvent of each sample are the same as those in Table 1 above.

[0111] Sample No. 1 and Sample No. 4 are samples that use the above-mentioned Carbodilite V-10 as a crosslinking agent. These samples are a sample that does not contain 2-propanol as a solvent, and a sample that contains 3 mass% of 2-propanol, which has the highest transparency, and are Sample No. 1 and Sample No. 4 in Table 1 above.

[0112] Samples No. 8 and No. 9 are samples that use, as a crosslinking agent, Carbodilite E-05 (manufactured by Nisshinbo Chemical Inc.), which is a carbodiimide compound having the same main component as Carbodilite V-10.

[0113] Samples No. 10 and No. 11 are samples that use, as a crosslinking agent, Barrierstar C (manufactured by Mitsui Chemicals, Inc.), whose main component is a polyamide epichlorohydrin resin.

[0114] Samples No. 12 and No. 13 are samples that use EPOCROS WS700 (manufactured by Nippon Shokubai Co., Ltd.), a water-soluble polymer containing an oxazoline group as the main component, as a crosslinking agent.

[0115] Samples No. 14 and No. 15 are samples that use, as a crosslinking agent, Oxazoline AC-7 (manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.), whose main component is ammonium zirconium carbonate.

[0116] In samples No. 8 and No. 9, which used Carbodilite E-05, a carbodiimide compound as the main component, as the crosslinking agent, the haze value up to the intermediate layer of sample No. 8, which did not contain the solvent 2-propanol, was 15.77.In contrast, the haze value up to the intermediate layer of sample No. 9, which contained 3 mass% 2-propanol, was 15.97, which was an increase compared to the haze value of sample No. 8, and no improvement in transparency was observed.

[0117] In samples No. 10 and No. 11, which used Barrier Star C, whose main component is polyamide epichlorohydrin, as the crosslinking agent, the haze value up to the intermediate layer of sample No. 10, which did not contain the solvent 2-propanol, was 31.96. In contrast, the haze value up to the intermediate layer of sample No. 11, which contained 3 mass% 2-propanol, was 31.70, a lower value than the haze value of sample No. 10, indicating improved transparency.

[0118] In samples No. 12 and No. 13, which used EPOCROSS WS700, a water-soluble polymer containing oxazoline groups, as the main component as the crosslinking agent, the haze value up to the intermediate layer of sample No. 12, which did not contain the solvent 2-propanol, was 14.63. In contrast, the haze value up to the intermediate layer of sample No. 13, which contained 3 mass% 2-propanol, was 14.82, an increase compared to the haze value of sample No. 12, and no improvement in transparency was observed.

[0119] In samples No. 14 and No. 15, which used oxazoline AC-7, whose main component is ammonium zirconium carbonate, as the crosslinking agent, the haze value of sample No. 14, which did not contain the solvent 2-propanol, was 14.90. In contrast, the haze value up to the intermediate layer of sample No. 15, which contained 3 mass% 2-propanol, was 15.10, which was an increase compared to the haze value of sample No. 14, and no improvement in transparency was observed.

[0120] In the case of samples No. 8, No. 12, and No. 14, which had relatively high transparency with a haze value up to the middle layer below 16 even without containing the solvent 2-propanol, and which used the crosslinking agents Carbodilite E-05, Epocross WS700, and Oxazoline AC-7, no improvement in transparency was observed by adding a solvent.

[0121] When Carbodilite V-10 or Barrierstar C is used as the crosslinking agent, the transparency can be improved by adding a solvent to the coating liquid for forming the intermediate layer.

[0122] The present inventors evaluated the effect of the type of solvent on the improvement of transparency by the addition of a solvent. Specifically, for each of a number of types of solvent, samples were prepared in which each intermediate layer was formed using each coating liquid containing 3% by mass of the solvent, and the haze value of the thermal recording medium up to the intermediate layer was measured.

[0123] In addition to the above-mentioned 2-propanol, propylene glycol and 1-3 propanediol were used as the solvent.

[0124] The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 3 below.

[0125] [Table 3] As shown in Table 3, the base material, binder, and crosslinking agent of each sample are the same as those in Table 1. Sample No. 1 is a sample to which no solvent is added, and corresponds to Sample No. 1 in Table 1. Sample No. 4 is a sample containing 3 mass% of 2-propanol, and corresponds to Sample No. 4 in Table 1.

[0126] The haze value up to the intermediate layer of Sample No. 1, in which no solvent was added, was 16.70.

[0127] The haze value up to the intermediate layer of sample No. 4, which contains 3 mass % of 2-propanol as a solvent, is 14.81.

[0128] Sample No. 16, which contains 3% by mass of propylene glycol as a solvent, has a haze value up to the intermediate layer of 14.50, which is lower than the haze value of 16.70 for Sample No. 1, which does not contain solvent, indicating improved transparency.

[0129] Sample No. 17, which contains 3% by mass of 1-3 propanediol as a solvent, has a haze value up to the intermediate layer of 14.98, which is lower than the haze value of 16.70 for Sample No. 1, which does not contain solvent, indicating improved transparency.

[0130] Thus, samples No. 4, No. 16, and No. 17, which contain 3 mass % of 2-propanol, propylene glycol, and 1,3-propanediol as the solvent, all have improved transparency compared to samples containing no solvent.

[0131] The present inventors evaluated the influence of the substrate on the improvement of transparency by the addition of a solvent. Specifically, the substrate was changed from the above-mentioned OPP film having a thickness of 40 μm to a PET (polyethylene terephthalate) film having a thickness of 50 μm, and 2-propanol, a solvent, was added to each of the coating liquids for forming the intermediate layer in amounts of 1 mass %, 3 mass %, and 5 mass %, as in Table 1 above, to prepare each of the coating liquids for forming the intermediate layer. A plurality of samples were prepared by forming the intermediate layer 4 with each of the prepared coating liquids. The haze value of each of the prepared samples was measured in the same manner as above.

[0132] The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 4 below.

[0133] [Table 4] As shown in Table 4, the binder, crosslinking agent and solvent of each sample are the same as those in Table 1 above, except that the base material is PET.

[0134] Sample No. 18, to which the solvent 2-propanol was not added, had a haze value of 15.18 up to the intermediate layer.

[0135] The haze value up to the intermediate layer of sample No. 19, which contains 1% by mass of 2-propanol, is 14.42, which is lower than the haze value of 15.18 of sample No. 18, which does not contain 2-propanol, indicating improved transparency.

[0136] The haze value up to the intermediate layer of sample No. 20, which contains 3 mass% 2-propanol, is 14.21, which is lower than the haze value of 15.18 of sample No. 18, which does not contain 2-propanol, indicating improved transparency.

[0137] The haze value up to the intermediate layer of sample No. 21, which contains 5% by mass of 2-propanol, is 14.50, which is lower than the haze value of 15.18 of sample No. 18, which does not contain 2-propanol, indicating improved transparency.

[0138] Thus, even when the substrate is PET, as in the case where the substrate is OPP, samples No. 19, No. 20, and No. 21, which were produced using a coating fluid for forming an intermediate layer containing 1 mass%, 3 mass%, and 5 mass% 2-propanol, had lower haze values ​​up to the intermediate layer compared to sample No. 18, which did not contain 2-propanol, and all showed improved transparency.

[0139] In particular, sample No. 20, which was prepared using a coating liquid for forming an intermediate layer containing 3% by mass of 2-propanol, had the lowest haze value and the most improved transparency.

[0140] The present inventors evaluated the influence of the binder on transparency. Specifically, the above-mentioned resins 1 and 2 were changed to resins 3 and 4, and the haze values ​​of a sample prepared using a coating liquid for forming an intermediate layer to which 2-propanol was not added and a sample prepared using a coating liquid containing 3% by mass of 2-propanol were measured in the same manner as above.

[0141] Resin 3 is a core-shell type resin with a solid content of 25.7%, a viscosity of 541 mPa·s at a rotation speed of 60 rpm, and a pH of 6.2.

[0142] Resin 4 is a core-type resin with a solid content of 20%, a viscosity of 1036 mPa·s at a rotation speed of 60 rpm, and a pH of 7.9.

[0143] The mass ratio of resin 3 to resin 4 was set to "50":"50" as above.

[0144] The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 5 below.

[0145] [Table 5] As shown in Table 5, the binders of the samples are resins 3 and 4, but the base material, crosslinking agent, and solvent are the same as those in Table 1 above.

[0146] Sample No. 22, to which no 2-propanol solvent was added, had a haze value of 61.04% up to the intermediate layer.

[0147] In contrast, sample No. 23 containing 3 mass % of 2-propanol had a haze value up to the intermediate layer of 51.83, which is a lower value than the haze value of sample No. 22, and thus the transparency was improved.

[0148] For the above Tables 1 to 5, samples were prepared in which an intermediate layer was formed using a coating liquid for forming the intermediate layer, and the transparency up to the intermediate layer was evaluated.

[0149] The present inventors prepared a sample in which a coating liquid for forming a topcoat layer was applied onto this intermediate layer and dried to form a topcoat layer, and evaluated the transparency up to the topcoat layer.

[0150] That is, an intermediate layer was formed using the same coating liquid for forming the intermediate layer as in Tables 1 to 5 above, a coating liquid for forming a topcoat layer was applied onto this intermediate layer, and dried to form a topcoat layer, and the haze value up to this topcoat layer was measured.

[0151] The coating liquid for forming the top coat layer contained an acrylic resin as a base resin, ammonium zirconium carbonate as a crosslinking agent, and further contained a wetting agent and an antifoaming agent.

[0152] This coating solution for forming the topcoat layer is applied onto the intermediate layer 4 in a coating amount of 1.5 g / m2 in terms of dry mass. 2 The coating was then dried so as to form a top coat layer 5.

[0153] As in Table 1 above, each coating liquid for forming an intermediate layer was prepared so that the amount of 2-propanol added as a solvent was 0.5 mass%, 1 mass%, 3 mass%, 4 mass%, 5 mass%, and 7 mass%, and each intermediate layer was formed using each coating liquid.

[0154] Furthermore, the above-mentioned coating liquid for forming a topcoat layer was applied onto each intermediate layer, and dried to form a topcoat layer, thereby preparing each sample, and the haze value up to the topcoat layer was measured for each sample.

[0155] The composition of the coating liquid for forming the intermediate layer used in producing each sample and the measurement results are shown in Table 6 below.

[0156] [Table 6] As shown in Table 6, the substrate and the composition of the coating liquid for forming the intermediate layer (binder, crosslinking agent, solvent, and amount of solvent added) are the same as those in Table 1 above, and the haze value up to the topcoat layer was measured instead of the haze value up to the intermediate layer.

[0157] In sample No. 24, in which an intermediate layer was formed using a coating liquid for forming an intermediate layer that did not contain 2-propanol and a topcoat layer was then formed thereon, the haze value up to the topcoat layer was 20.67.

[0158] On the other hand, 2-propanol was added at 0.5 mass%, 1 mass%, 3 mass%, The haze values ​​up to the topcoat layer of samples No. 25, No. 26, No. 27, No. 28, No. 29, and No. 30, in which intermediate layers were formed using coating fluids containing 4 mass%, 5 mass%, and 7 mass%, respectively, and then topcoat layers were formed thereon, were 26.25, 21.80, 21.48, 21.63, 21.25, and 22.60, respectively.

[0159] The haze values ​​up to the top coat layer of these samples No. 25, No. 26, No. 27, No. 28, No. 29, and No. 30 are all higher than the haze value of 20.67 up to the top coat layer of sample No. 24, in which an intermediate layer was formed using a coating liquid for forming an intermediate layer to which 2-propanol was not added, and a top coat layer was then formed on top of that. Thus, no improvement in transparency was observed.

[0160] However, as will be explained below, in samples in which an intermediate layer was formed using a coating liquid for intermediate layer formation that contained Carbodilite E-05, Barrierstar C, Epocross WS700, and Oxazoline AC-7 as crosslinking agents, and then a topcoat layer was formed on this intermediate layer, all of which showed improved transparency up to the topcoat layer.

[0161] That is, as in Table 2 above, for multiple types of crosslinking agents, the haze values ​​up to the topcoat layer were measured for a sample in which an intermediate layer was formed using a coating liquid for forming an intermediate layer that did not contain the solvent 2-propanol and a topcoat layer was formed thereon, and for a sample in which an intermediate layer was formed using a coating liquid for forming an intermediate layer that contained 3% by mass of 2-propanol and a topcoat layer was formed thereon.

[0162] The composition of the coating liquid for forming the intermediate layer used in producing each sample and the measurement results are shown in Table 7 below.

[0163] [Table 7] As shown in Table 7, the composition of the substrate and the coating liquid for forming the intermediate layer (amounts of binder, solvent, crosslinker, and solvent added) are the same as those in Table 2 above, and the haze value up to the topcoat layer was measured instead of the haze value up to the intermediate layer.

[0164] Samples No. 24 and No. 27 are samples in which an intermediate layer was formed using a coating liquid for forming an intermediate layer that used Carbodilite V-10 as a crosslinking agent, and then a topcoat layer was formed on top of the intermediate layer. These are samples No. 24 and No. 27 in Table 6 above.

[0165] As described above, the haze value up to the top coat layer of sample No. 27, which was prepared using a coating liquid for forming an intermediate layer containing 3 mass% 2-propanol, was 21.48, which is a higher value than the haze value up to the top coat layer of sample No. 24, which was prepared using a coating liquid for forming an intermediate layer that did not contain 2-propanol, of 20.67, and no improvement in transparency was observed.

[0166] In samples No. 31 and No. 32, which use Carbodilite E-05, a carbodiimide compound as the main component, as the crosslinking agent, the haze value up to the top coat layer of sample No. 31, which does not contain the solvent 2-propanol, is 22.35. In contrast, the haze value up to the top coat layer of sample No. 32, which contains 3 mass% 2-propanol, is 22.15, which is a lower haze value than sample No. 31 and improves transparency.

[0167] In samples No. 33 and No. 34, which use Barrier Star C, whose main component is polyamide epichlorohydrin, as the crosslinking agent, the haze up to the top coat layer of sample No. 33, which does not contain the solvent 2-propanol, is 28.49. In contrast, the haze value up to the top coat layer of sample No. 34, which contains 3 mass% 2-propanol, is 28.41, a lower haze value than sample No. 33, and transparency is improved.

[0168] In samples No. 35 and No. 36, which use EPOCROS WS700, an oxazoline group-containing water-soluble polymer, as the main component as the crosslinking agent, the haze value up to the top coat layer of sample No. 35, which does not contain the solvent 2-propanol, is 22.11. In contrast, the haze value up to the top coat layer of sample No. 36, which contains 3 mass% 2-propanol, is 21.58, a lower haze value than sample No. 35, and transparency is improved.

[0169] In samples No. 37 and No. 38, which use oxazoline AC-7, whose main component is ammonium zirconium carbonate, as the crosslinking agent, the haze value up to the top coat layer of sample No. 37, which does not contain the solvent 2-propanol, is 23.84. In contrast, the haze value up to the top coat layer of sample No. 38, which contains 3 mass% 2-propanol, is 23.46, which is a lower haze value than sample No. 37, and transparency is improved.

[0170] Thus, when the crosslinking agents were Carbodilite E-05, Barrierstar C, Epocross WS700, and Oxazoline AC-7, the samples using a coating liquid for forming an intermediate layer containing 3% by mass of solvent all had lower haze values ​​up to the top coat layer and improved transparency compared to samples that did not contain solvent.

[0171] As in Table 3 above, an intermediate layer was formed using a coating liquid for intermediate layer formation prepared so that the solvent content was 3 mass% for three types of solvent, namely 2-propanol, propylene glycol, and 1,3-propanediol, and a topcoat layer was formed on the intermediate layer, and the haze values ​​up to the topcoat layer of the sample were measured.

[0172] The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 8 below.

[0173] [Table 8] As shown in Table 8, the composition of the substrate and the coating liquid for forming the intermediate layer (binder, crosslinking agent, solvent, and amount of solvent added) are the same as those in Table 3 above, and the haze value up to the topcoat layer was measured instead of the haze value up to the intermediate layer.

[0174] Samples No. 24 and 27 are samples in which an intermediate layer was formed using a coating liquid for forming an intermediate layer that used Carbodilite V-10 as a crosslinking agent, and then a topcoat layer was formed on top of the intermediate layer, and these are Samples No. 24 and 27 in Table 6 above.

[0175] As described above, the haze value up to the top coat layer of sample No. 27, which was prepared using a coating fluid for forming an intermediate layer containing 3 mass% 2-propanol, was 21.48, which was higher than the haze value up to the top coat layer of sample No. 24, which was prepared using a coating fluid for forming an intermediate layer that did not contain a solvent, being 20.67, and no improvement in transparency was observed.

[0176] The haze value up to the top coat layer of sample No. 39, which contained 3 mass% propylene glycol as a solvent, was 21.27, which was higher than the haze value up to the top coat layer of sample No. 24, which was prepared using a coating liquid for forming an intermediate layer that did not contain a solvent, of 20.67, and no improvement in transparency was observed.

[0177] Sample No. 40, which contains 3% by mass of 1-3 propanediol as a solvent, has a haze value up to the top coat layer of 21.29, which is higher than the haze value of 20.67 for sample No. 24, which does not contain a solvent, and no improvement in transparency is observed.

[0178] As in Table 4 above, the substrate was changed to a 50 μm thick PET (polyethylene terephthalate) film, and an intermediate layer was formed using a coating liquid for forming an intermediate layer to which the solvent 2-propanol was added at contents of 1 mass %, 3 mass %, and 5 mass %. Samples were then produced in which a topcoat layer was formed on top of the intermediate layer, and the haze value up to the topcoat layer of each of the samples produced was measured.

[0179] The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 9 below.

[0180] [Table 9] As shown in Table 9, the composition of the substrate and the coating liquid for forming the intermediate layer (binder, crosslinking agent, solvent, and amount of solvent added) are the same as those in Table 4 above, and the haze value up to the topcoat layer was measured instead of the haze value up to the intermediate layer.

[0181] Sample No. 41, which does not contain the solvent 2-propanol, has a haze value up to the top coat layer of 21.46%.

[0182] The haze value up to the top coat layer of sample No. 42, which contains 1 mass% 2-propanol, is 20.50, which is a lower value than the haze value up to the top coat layer of sample No. 41, which does not contain 2-propanol, of 21.46, indicating improved transparency.

[0183] The haze value up to the top coat layer of sample No. 43, which contains 3 mass% 2-propanol, is 20.90, which is a lower value than the haze value up to the top coat layer of sample No. 41, which does not contain 2-propanol, of 21.46, indicating improved transparency.

[0184] The haze value up to the top coat layer of sample No. 44, which contains 5% by mass of 2-propanol, is 20.55, which is a lower value than the haze value of 21.46 of sample No. 41, which does not contain 2-propanol, and thus the transparency is improved.

[0185] Thus, even though the base material is PET, samples No. 42, No. 43, and No. 44, which were produced using coating fluids for forming an intermediate layer containing 1 mass%, 3 mass%, and 5 mass% 2-propanol, respectively, had lower haze values ​​up to the top coat layer than sample No. 41, which did not contain 2-propanol, and all of them had improved transparency.

[0186] As in Table 5 above, the binder was changed from resin 1 and 2 to resin 3 and 4, and the haze value up to the top coat layer was measured for a sample prepared using a coating liquid for forming an intermediate layer that did not contain 2-propanol and a sample prepared using a coating liquid containing 3% by mass of 2-propanol.

[0187] The composition of the coating liquid used to prepare each sample and the measurement results are shown in Table 10 below.

[0188] [Table 10] As shown in Table 10, the composition of the substrate and the coating liquid for forming the intermediate layer (binder, crosslinking agent, solvent, and amount of solvent added) are the same as those in Table 5 above, and the haze value up to the topcoat layer was measured instead of the haze value up to the intermediate layer.

[0189] Sample No. 45, to which no 2-propanol solvent was added, had a haze value up to the top coat layer of 33.34%.

[0190] In contrast, sample No. 46, which contains 3% by mass of 2-propanol, has a haze value up to the top coat layer of 31.72, which is a lower value than the haze value of sample No. 45, 33.34, and therefore has improved transparency. [Explanation of symbols]

[0191] 1 Thermal recording medium 2 Base material 3. Thermal recording layer 4. Middle Tier 5 Topcoat layer

Claims

1. A coating liquid for forming an intermediate layer of a thermosensitive recording medium having a thermosensitive recording layer and an intermediate layer on a substrate, comprising: Contains a binder and a solvent in an amount of 1% by mass or more and 5% by mass or less. Coating fluid.

2. The solvent is at least one of 2-propanol, propylene glycol, and 1-3 propanediol. The coating fluid according to claim 1.

3. Contains a crosslinking agent, The coating fluid according to claim 1.

4. The binder contains a core-shell type resin and a core type resin that does not have a shell portion of the core-shell type resin. The coating fluid according to claim 1 .

5. A method for producing a thermal recording medium having a thermal recording layer and an intermediate layer on a substrate, comprising the steps of: forming the intermediate layer using a coating liquid for forming the intermediate layer, The coating liquid contains a binder and a solvent in an amount of 1% by mass or more and 5% by mass or less. A method for producing a thermal recording medium.

6. The coating liquid contains at least one of 2-propanol, propylene glycol, and 1-3 propanediol as the solvent. A method for producing the thermosensitive recording medium according to claim 5.

7. forming a topcoat layer on the intermediate layer; The coating liquid contains a crosslinking agent. A method for producing the thermosensitive recording medium according to claim 5.

8. The coating liquid contains, as the binder, a core-shell resin and a core resin having no shell portion of the core-shell resin. A method for producing the thermosensitive recording medium according to any one of claims 5 to 7.

9. A thermal recording medium comprising a thermal recording layer and an intermediate layer on a substrate, The intermediate layer is formed from a coating liquid for forming an intermediate layer containing a binder and containing 1% by mass or more and 5% by mass or less of a solvent. Thermal recording medium.

Citation Information

Patent Citations

  • Thermal recording label

    JP2002362027A