Lithium ion secondary battery
A lithium ion secondary battery with a high nickel content and controlled Co:Mn ratio in the positive electrode, combined with a Si-containing negative electrode material, addresses cobalt depletion concerns by reducing resistance and enhancing storage stability.
Patent Information
- Application Number
- JP2023072404
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-26
AI Technical Summary
The increasing demand for lithium ion secondary batteries has raised concerns about the depletion of cobalt (Co) used in their positive electrode active materials, leading to a significant increase in resistance during storage when the Co content is reduced.
A lithium ion secondary battery design that includes a positive electrode active material with a high nickel-containing lithium transition metal composite oxide, a layered structure with a Ni content of 75 mol% and a controlled Co to Mn ratio (0≦Co/Mn≦0.43), and a negative electrode containing a carbon material and a Si-containing material to suppress resistance increase.
The battery effectively reduces cobalt content while maintaining low resistance during storage by minimizing Mn precipitation on the negative electrode surface, thereby enhancing durability and stability.
Smart Images

Figure 2024157813000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to lithium-ion secondary batteries. [Background technology]
[0002] Lithium ion secondary batteries are suitable for use as driving power sources mounted on vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and electric vehicles (BEVs), and the demand for lithium ion secondary batteries is rapidly expanding. As a positive electrode active material used in lithium ion secondary batteries, lithium transition metal composite oxides are used, and among them, lithium nickel cobalt manganese composite oxides containing Ni, Co, and Mn as shown in Patent Document 1 are exemplified. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-191662 A Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, in recent years, as the demand for lithium ion secondary batteries increases, there is concern about the depletion of cobalt (Co) used in lithium ion secondary batteries. As a countermeasure, it is considered to reduce the content of Co in the positive electrode active material. However, as a result of intensive research by the present inventors, it has been found that when the content of Co in the positive electrode active material is reduced, the resistance of the lithium ion secondary battery increases significantly during storage.
[0005] The technology disclosed herein has been made in consideration of the above circumstances, and aims to provide a lithium-ion secondary battery in which the cobalt content in the positive electrode active material is reduced while suppressing an increase in resistance during storage. [Means for solving the problem]
[0006] The technology disclosed herein relates to a lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, the positive electrode comprising a positive electrode active material layer containing a positive electrode active material, the positive electrode active material being a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, the lithium transition metal composite oxide having a Ni content of 75 mol % or more relative to a total of metal elements other than Li, the negative electrode comprising a negative electrode active material layer containing a negative electrode active material, the negative electrode active material including a carbon material and a Si-containing material, and the positive electrode active material having a Co element content (mol) and a Mn element content (mol) satisfy the following relationship: 0≦Co / Mn≦0.43.
[0007] According to this configuration, the composition of the positive electrode active material, specifically the Ni content and the ratio of the Co content to the Mn content, are each set within a predetermined range. Furthermore, the negative electrode active material contains a Si-containing material in addition to a carbon material. This makes it possible to provide a lithium-ion secondary battery that reduces the cobalt content in the positive electrode active material while suppressing an increase in resistance during storage. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic internal structure of a lithium-ion secondary battery according to one embodiment. [Diagram 2] FIG. 2 is a schematic exploded view showing the configuration of an electrode body of a lithium ion secondary battery according to one embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing the configuration of a negative electrode sheet (negative electrode) according to one embodiment. [Figure 4] FIG. 4 is a view corresponding to FIG. 3 and showing the configuration of a negative electrode sheet (negative electrode) according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, some preferred embodiments of the lithium ion secondary battery disclosed herein will be described with reference to the drawings as appropriate. Matters other than those specifically mentioned in this specification and necessary for implementing the present disclosure (for example, the general configuration and manufacturing process of a lithium ion secondary battery that does not characterize the present disclosure) can be understood as design matters of a person skilled in the art based on the prior art in the field. The lithium ion secondary battery disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field.
[0010] In the following drawings, the same reference numerals are used for components and parts that perform the same function, and duplicated explanations may be omitted or simplified. In this specification, the notation "A to B" indicating a range includes not only the meaning of A or more and B or less, but also the meanings of "preferably larger than A" and "preferably smaller than B." In this specification, a "lithium ion secondary battery" (hereinafter sometimes simply referred to as a "battery") refers to a general electricity storage device that uses lithium ions as a charge carrier and can be repeatedly charged and discharged by the transfer of charge associated with the lithium ions between the positive and negative electrodes.
[0011] Hereinafter, the present disclosure will be described in detail using as an example a flat prismatic lithium ion secondary battery having a flat electrode body and a flat battery case, but it is not intended that the present disclosure be limited to the embodiment described therein.
[0012] FIG. 1 is a cross-sectional view showing a schematic internal structure of a lithium ion secondary battery according to an embodiment. The lithium ion secondary battery 100 shown in FIG. 1 is a sealed battery constructed by housing a flat electrode body 20 and a non-aqueous electrolyte 80 in a flat rectangular battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The battery case 30 is also provided with an injection port (not shown) for injecting the non-aqueous electrolyte 80. The positive electrode terminal 42 is electrically connected to the positive electrode current collector plate 42a. The negative electrode terminal 44 is electrically connected to the negative electrode current collector plate 44a. The material of the battery case 30 is, for example, a lightweight metal material with good thermal conductivity, such as aluminum.
[0013] Fig. 2 is a schematic exploded view showing the configuration of an electrode body of a lithium ion secondary battery according to one embodiment. As shown in Figs. 1 and 2, the electrode body 20 has a configuration in which a strip-shaped positive electrode sheet 50 and a strip-shaped negative electrode sheet 60 are overlapped with two strip-shaped separators 70 interposed therebetween and wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long-sized positive electrode collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long-sized negative electrode collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are respectively joined to the positive electrode current collector 42a and the negative electrode current collector 44a. The positive electrode sheet 50 is an example of the "positive electrode" disclosed herein, and the negative electrode sheet 60 is an example of the "negative electrode" disclosed herein.
[0014] <Positive electrode> The positive electrode (positive electrode sheet 50) disclosed herein includes a positive electrode active material layer 54. As shown in Fig. 2, the positive electrode (positive electrode sheet 50) here includes a positive electrode current collector 52 and a positive electrode active material layer 54 supported by the positive electrode current collector 52. Note that, although the positive electrode active material layer 54 is illustrated only on one surface of the positive electrode current collector 52 in this embodiment, the positive electrode active material layer 54 may be provided on both surfaces of the positive electrode current collector 52.
[0015] The positive electrode active material layer 54 contains a positive electrode active material capable of reversibly absorbing and releasing charge carriers. The positive electrode active material according to this embodiment essentially contains a high Ni content lithium transition metal composite oxide having a layered structure and containing lithium (Li), nickel (Ni), and manganese (Mn) as essential elements. The high Ni content lithium transition metal composite oxide is an example of the "lithium transition metal composite oxide in which the content of Ni relative to the total of metal elements other than Li is 75 mol % or more" disclosed herein.
[0016] The positive electrode active material may contain a positive electrode active material other than the high Ni-containing lithium transition metal composite oxide within a range that does not impair the effects of the present disclosure (for example, less than 10 mass % relative to the total mass of the positive electrode active material, preferably 5 mass % or less). In addition, the positive electrode active material may be composed only of the high Ni-containing lithium transition metal composite oxide.
[0017] In the high Ni-containing lithium transition metal composite oxide according to this embodiment, the Ni content relative to the total metal elements other than Li is 75 mol% or more. From the viewpoint of high volumetric energy density of the lithium ion secondary battery, the Ni content relative to the total metal elements other than Li is preferably 80 mol% or more, more preferably 90 mol% or more. On the other hand, from the viewpoint of high stability, the Ni content relative to the total metal elements other than Li is preferably 95 mol% or less, more preferably 93 mol% or less.
[0018] Examples of the high Ni-containing lithium transition metal composite oxide having a layered structure include lithium nickel manganese composite oxide, lithium nickel cobalt manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide. These may be used alone or in combination of two or more. It can be confirmed by a known method (e.g., X-ray diffraction method) that the particles of the high Ni-containing lithium transition metal composite oxide have a layered structure (i.e., a layered crystal structure).
[0019] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. This also applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0020] In some preferred embodiments, the high Ni lithium transition metal composite oxide preferably has a composition represented by the following general formula (i): Li α Ni x Mn y M z O2...Equation (i) In the above formula (i), x, y, z, and α respectively satisfy the following: 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, and x+y+z=1. M in the formula (i) is at least one element selected from the group consisting of Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
[0021] In the above formula (i), α preferably satisfies 0.9 ≦ α ≦ 1.2, more preferably satisfies 1.0 ≦ α ≦ 1.1. From the viewpoint of battery characteristics (for example, energy density, cycle characteristics, thermal stability), x preferably satisfies 0.8 ≦ x ≦ 0.95, more preferably satisfies 0.8 ≦ x ≦ 0.9. From the viewpoints of, for example, energy density, thermal stability, and cost, y preferably satisfies 0.1 ≦ y ≦ 0.25, more preferably satisfies 0.17 ≦ y ≦ 0.25. z preferably satisfies 0 ≦ z ≦ 0.1, more preferably satisfies 0 ≦ z ≦ 0.03, and still more preferably is 0. In the above formula (i), "x + y + z = 1" includes not only the case where x + y + z is 1, but also the case where it is regarded as substantially 1 as long as the effects of the technology disclosed herein can be realized. Typically, x + y + z can be 0.95 to 1.1, preferably x + y + z can be 0.99 to 1.05.
[0022] Further, when 0 < z in the formula (i), M more preferably contains W from the viewpoints of a lower initial resistance and a more stabilized layered crystal structure of the lithium transition metal composite oxide.
[0023] The cathode active material has the following relationship between the content (mol) of Co element and the content (mol) of Mn element: 0 ≦ Co / Mn ≦ 0.43 That is. Thereby, the content ratios of Co element and Mn element in the cathode active material are controlled. In the above relationship, the smaller the value of Co / Mn, the more preferably the cobalt content in the cathode active material can be reduced while suppressing the increase in resistance during storage. Therefore, it is preferably 0 ≦ Co / Mn ≦ 0.32, and more preferably 0 ≦ Co / Mn ≦ 0.21.
[0024] In the positive electrode active material used in the conventional lithium ion battery, the content ratio of Co element to the metal elements other than Li is typically about 10 mol% to 40 mol%. However, since the Co resource is limited, it is preferable to reduce the content of Co in the positive electrode active material compared to the conventional one. Therefore, in some preferred embodiments, the content ratio of Co to the total of the metal elements other than Li is, for example, preferably 5 mol% or less, more preferably 3 mol% or less, and even more preferably 0 mol% (i.e., Co-free).
[0025] The average particle diameter (D50) of the lithium transition metal composite oxide is not particularly limited. From the viewpoint of improving the energy density and output characteristics of the positive electrode active material layer, the average particle diameter (D50) of the lithium transition metal composite oxide is preferably 5 μm to 30 μm, more preferably 10 μm to 20 μm. In this specification, the term "average particle diameter (D50)" refers to the median diameter (D50) and also means a particle diameter corresponding to a cumulative frequency of 50 volume % from the smaller particle diameter side (fine particle side) in a volume-based particle size distribution based on a laser diffraction / scattering method. Therefore, the average particle diameter (D50) can be determined using a laser diffraction / scattering type particle size distribution measuring device or the like.
[0026] Although not particularly limited, the lithium transition metal composite oxide is preferably substantially spherical. However, it may be of an indefinite shape. In this specification, the term "substantially spherical" refers to a shape that can be generally regarded as a sphere as a whole, and an average aspect ratio (major axis / minor axis ratio) based on a cross-sectional observation image of an electron microscope is, for example, 1 to 1.5. The lithium transition metal composite oxide is typically in the form of secondary particles formed by agglomeration of multiple primary particles by physical or chemical bonding forces. In other words, the lithium transition metal composite oxide (i.e., secondary particles) is an aggregate of primary particles in which a large number of primary particles are aggregated to form one particle.
[0027] The BET specific surface area of the lithium transition metal composite oxide is not particularly limited. Since this can impart excellent output characteristics to a lithium ion secondary battery, the BET specific surface area of the lithium transition metal composite oxide is preferably 0.50 m 2 / g~0.85m 2 / g, more preferably 0.55m 2 / g~0.80m 2 The BET specific surface area of the lithium transition metal composite oxide can be measured by a nitrogen adsorption method using a commercially available specific surface area measuring device.
[0028] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is, for example, 80 mass% or more, preferably 87 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and most preferably 97 mass% or more.
[0029] A known positive electrode current collector used in lithium ion secondary batteries may be used as the positive electrode current collector 52, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). As the positive electrode current collector 52, aluminum foil is preferred.
[0030] The dimensions of the positive electrode current collector 52 are not particularly limited and can be appropriately determined according to the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness of the positive electrode current collector 52 is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0031] <Negative electrode> The negative electrode (negative electrode sheet 60) disclosed herein includes a negative electrode active material layer 64. As shown in Fig. 2, the negative electrode (negative electrode sheet 60) includes a negative electrode current collector 62 and a negative electrode active material layer 64 supported on the negative electrode current collector 62. Note that, although the negative electrode active material layer 64 is illustrated only on one surface of the negative electrode current collector 62 in this embodiment, the negative electrode active material layer 64 may be provided on both surfaces of the negative electrode current collector 62.
[0032] The negative electrode active material layer 64 contains a negative electrode active material 66 that can reversibly occlude and release charge carriers. FIG. 3 is a schematic diagram showing the configuration of a negative electrode sheet 60 (negative electrode) according to an embodiment. The negative electrode active material 66 according to this embodiment essentially includes a carbon material 66c and a Si-containing material 66s. However, the negative electrode active material 66 may further contain other negative electrode active materials in addition to the carbon material 66c and the Si-containing material 66s. Also, for convenience of explanation, although not shown here, the negative electrode active material layer 64 may contain a conductive material, a binder, a thickener, etc. in addition to the negative electrode active material 66.
[0033] As the carbon material 66c, for example, graphite, hard carbon, soft carbon, etc. are used, and among them, graphite is preferably used. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in a form where the graphite is coated with an amorphous carbon material.
[0034] The average particle diameter of the carbon material 66c is not particularly limited, but for example, it is 0.1 μm or more and 50 μm or less, preferably 1 μm or more and 25 μm or less, and more preferably 5 μm or more and 20 μm or less. The average particle diameter (D50) of the carbon material can be obtained, for example, by the laser diffraction scattering method.
[0035] The Si-containing material 66s is, for example, silicon (Si), SiO x (0.05 < x < 1.95), silicon oxide represented by, a Si-C composite containing Si particles in carbon particles, lithium silicate (Li x Si y O z) and the like. As the Si-containing material 66s, silicon, silicon oxide, and Si-C composites can be suitably used. As the Si-containing material 66s, an alloy consisting of Si and an element other than Si can be used. Examples of elements other than Si include Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, and Ti. By including the Si-containing material 66s in the negative electrode active material 66, it is possible to suppress the formation of a coating layer originating from Mn eluted from the positive electrode active material on the surface of the negative electrode active material layer 64. Therefore, it is possible to suitably suppress the increase in resistance during storage.
[0036] The average particle size of the Si-containing material 66s is not particularly limited, but is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. The average particle size (D50) of the carbon material can be determined, for example, by a laser diffraction scattering method.
[0037] Although not particularly limited, when the total amount of the negative electrode active material 66 is taken as 100 mass%, if the content ratio of the Si element in the negative electrode active material 66 is 2 mass% or more, the effect of suppressing the formation of a coating layer originating from Mn dissolved from the positive electrode active material on the surface of the negative electrode active material layer 64 can be obtained, and therefore the effect of suppressing the storage resistance can be exhibited. The higher the content ratio of the Si element, the better the effect of suppressing the resistance increase during storage, but the lower the content ratio of the Si element, the better the capacity maintenance rate during storage. Therefore, from the viewpoint of achieving both the effect of suppressing the resistance increase during storage and the capacity maintenance rate, the content ratio of the Si element in the negative electrode active material 66 is preferably 2 mass% or more and 13 mass% or less, more preferably 5 mass% or more and 10 mass% or less.
[0038] The distribution of the Si-containing material 66s in the negative electrode active material layer 64 is not particularly limited, and the Si-containing material may be dispersed throughout the entire negative electrode active material layer 64, may be concentrated and dispersed in the upper layer (the surface layer side of the negative electrode active material layer 64) of the negative electrode active material layer 64, or may be concentrated and dispersed in the lower layer (the negative electrode current collector 62 side) of the negative electrode active material layer 64. In some preferred embodiments, the Si-containing material 66s is preferably concentrated and dispersed in the upper layer (corresponding to the negative electrode upper layer 164u in FIG. 4) of the negative electrode active material layer 64, as shown in the second embodiment (FIG. 4) described later. As shown in FIG. 3, in this embodiment, the Si-containing material 66s is dispersed almost uniformly throughout the entire negative electrode active material layer 64. Note that "concentrated and dispersed in the upper layer of the negative electrode active material layer 64" is an example of "the content ratio of the Si element in the negative electrode upper layer is 90 mass% or more when the Si element in the entire negative electrode active material is 100 mass%" disclosed herein.
[0039] The negative electrode active material layer 64 may contain components other than the negative electrode active material 66, such as a conductive material, a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc., which have been used conventionally in lithium secondary batteries, may be used without any particular limitation. As the thickener, for example, carboxymethyl cellulose (CMC) may be used.
[0040] The negative electrode active material layer 64 preferably further contains a conductive material. As the conductive material, for example, carbon black (CB) such as acetylene black (AB) or Ketjen black, carbon nanotubes (CNT), carbon fibers such as vapor grown carbon fiber (VGCF), activated carbon, graphite, and other carbon materials can be suitably used, and among them, it is preferable to contain CNT. By containing CNT as the conductive material, the capacity retention rate can be suitably maintained. As the CNT, any one of single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT) may be used, and these may be used alone or in combination of two or more. When CNT is used as the conductive material of the negative electrode active material layer 64, it is preferable to use SWCNT. When CNT is used as the conductive material of the negative electrode active material layer 64, it is preferable to contain 0.5 mass % or less of CNT with respect to the entire negative electrode active material layer.
[0041] The content of the negative electrode active material 66 in the negative electrode active material layer 64 is preferably 90% by mass or more, and more preferably 95% by mass or more and 99% by mass or less. The content of the binder in the negative electrode active material layer 64 is preferably 0.1% by mass or more and 8% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less. The content of the thickener in the negative electrode active material layer 64 is preferably 0.3% by mass or more and 3% by mass or less, and more preferably 0.5% by mass or more and 2% by mass or less.
[0042] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, 10 μm to 200 μm, and preferably 20 μm to 100 μm, when the negative electrode active material layer 64 is provided only on one surface of the negative electrode current collector 62. When the negative electrode active material layer 64 is provided on both surfaces of the negative electrode current collector 62, the thickness of each surface (each of the thicknesses of one surface and the other surface) is, for example, 10 μm to 200 μm, and preferably 20 μm to 100 μm.
[0043] A known negative electrode current collector used in lithium ion secondary batteries may be used as the negative electrode current collector 62, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.). Copper foil is preferable as the negative electrode current collector 62.
[0044] The dimensions of the negative electrode current collector 62 are not particularly limited and can be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness of the negative electrode current collector 62 is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0045] As the separator 70, various porous sheets similar to those conventionally used in lithium ion secondary batteries can be used, and examples thereof include porous resin sheets made of resins such as polyethylene (PE) and polypropylene (PP). Such porous resin sheets may have a single-layer structure or a multi-layer structure of two or more layers (for example, a three-layer structure in which PP layers are laminated on both sides of a PE layer). The separator 70 may be provided with a heat-resistant layer (HRL).
[0046] The non-aqueous electrolyte 80 can be the same as that used in conventional lithium ion secondary batteries, and typically can be an organic solvent (nonaqueous solvent) containing a supporting salt. As the non-aqueous solvent, aprotic solvents such as carbonates, esters, and ethers can be used. Among them, carbonates are preferred because they have a particularly high effect of reducing low-temperature resistance due to the positive electrode material. Examples of carbonates include ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such non-aqueous solvents can be used alone or in appropriate combination of two or more. As the supporting salt, for example, lithium salts such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI) can be suitably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.
[0047] In addition, the nonaqueous electrolyte 80 may contain various additives such as gas generating agents, film forming agents, dispersants, and thickeners, other than the nonaqueous solvent and supporting salt described above, as long as the effects of the present disclosure are not significantly impaired. Examples of additives used in the nonaqueous electrolyte 80 include positive and negative electrode film forming agents such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), and 1,3-propane sultone (PS); overcharge inhibitors such as biphenyl (BP), cyclohexylbenzene (CHB), t-butylbenzene, and t-amylbenzene. Among them, it is preferable to contain FEC. When FEC is contained as an additive in the nonaqueous electrolyte 80, it is preferable to contain FEC at a ratio of 20 vol% or less with respect to the nonaqueous electrolyte 80.
[0048] The lithium ion secondary battery 100 configured as above uses a high Ni-containing lithium transition metal composite oxide as the positive electrode active material, and in the positive electrode active material, the content (mol) of Co element and the content (mol) of Mn element satisfy the following relationship: 0≦Co / Mn≦0.43. The negative electrode active material contains a carbon material and a Si-containing material. This makes it possible to reduce the cobalt content in the positive electrode active material while suppressing an increase in resistance during storage.
[0049] In detail, when a lithium transition metal composite oxide having a layered structure containing Mn is used as a positive electrode active material, if the Co content in the positive electrode active material is reduced, the stability of the positive electrode active material is reduced, and Mn dissolution from the positive electrode active material layer during storage becomes significant. The dissolved Mn precipitates on the surface of the negative electrode active material layer (typically the graphite surface), and a film grows starting from the precipitated Mn. This film causes the durability of the lithium ion battery to deteriorate. Therefore, in the past, a lithium ion secondary battery using a lithium transition metal composite oxide having a layered structure containing Mn and a reduced Co content as a positive electrode active material had a problem of a large increase in resistance during storage.
[0050] In contrast, the lithium ion secondary battery 100 according to this embodiment contains a high Ni-containing lithium transition metal composite oxide as the positive electrode active material. In other words, since the content of Ni relative to the total of metal elements other than Li in the lithium transition metal composite oxide is 75 mol % or more, the Mn ratio in the lithium transition metal composite oxide can be suppressed. In addition, the content ratio of Co element and Mn element in the positive electrode active material is controlled by making the content ratio of Co element (mol) and the content ratio of Mn element (mol) in the positive electrode active material 0≦Co / Mn≦0.43. Furthermore, the Si-containing material contained in the negative electrode active material suppresses the precipitation of Mn on the negative electrode surface. This makes it possible to suppress the formation of a Mn coating on the negative electrode surface. Therefore, it is possible to provide a lithium ion secondary battery 100 in which the increase in resistance during storage is suppressed.
[0051] The lithium ion secondary battery 100 can be used for various applications. Suitable applications include a driving power source mounted on vehicles such as an electric vehicle (BEV; Battery Electric Vehicle), a hybrid electric vehicle (HEV; Hybrid Electric Vehicle), and a plug-in hybrid electric vehicle (PHEV; Plug-in Hybrid Electric Vehicle). The lithium ion secondary battery 100 can also be used as a storage battery for a small power storage device or the like. The lithium ion secondary battery 100 can also be used in the form of a battery pack in which a plurality of lithium ion secondary batteries 100 are typically connected in series and / or parallel.
[0052] As an example, a rectangular lithium ion secondary battery 100 including an electrode body 20 having a flat wound structure has been described. However, the lithium ion secondary battery disclosed herein can also be configured as a lithium ion secondary battery including a laminated electrode body (i.e., an electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated). The laminated electrode body may include a plurality of separators such that one separator is interposed between each of the positive electrodes and the negative electrodes, and may be one in which the positive electrodes and the negative electrodes are alternately laminated while one separator is folded. The lithium ion secondary battery according to this embodiment can also be constructed in the form of a cylindrical lithium ion secondary battery, a coin-type lithium ion secondary battery, a laminated lithium ion secondary battery, or the like. Furthermore, an all-solid-state secondary battery using a solid electrolyte as the electrolyte can also be constructed.
[0053] <Second embodiment> Fig. 4 is a view of a negative electrode sheet 160 (negative electrode) according to the second embodiment, corresponding to Fig. 3. In Fig. 4, the negative electrode sheet 160 may be similar to the above-mentioned lithium ion secondary battery 100, except that a negative electrode active material layer 164 is provided instead of the negative electrode active material layer 64. As shown in Fig. 4, the negative electrode active material layer 164 has a so-called multi-layer structure including a negative electrode upper layer 164u and a negative electrode lower layer 164d.
[0054] In some preferred embodiments, the negative electrode active material layer 164 may include a negative electrode lower layer 164d in contact with the negative electrode current collector 62, and a negative electrode upper layer 164u that is farther from the negative electrode current collector 62 than the negative electrode lower layer 164d is, as viewed in the thickness direction. However, the negative electrode active material layer 164 may have a multi-layer structure of three or more layers. For example, a layer having a composition different from those of the negative electrode upper layer 164u and the negative electrode lower layer 164d may be formed between the negative electrode upper layer 164u and the negative electrode lower layer 164d.
[0055] The negative electrode upper layer 164u is a layer located closer to the surface than the negative electrode lower layer 164d when viewed in the thickness direction of the negative electrode active material layer 164. The negative electrode upper layer 164u is located farther from the negative electrode current collector 62 than the negative electrode lower layer 164d. Here, the negative electrode upper layer 164u constitutes the outermost layer of the negative electrode active material layer 164. In other words, the negative electrode upper layer 164u is located closer to the positive electrode (positive electrode sheet 50) than the negative electrode lower layer 164d.
[0056] The negative electrode active material 66 of the negative electrode upper layer 164u essentially contains a Si-containing material 66s. When the amount of Si element in the entire negative electrode active material layer 164 is taken as 100 mass%, the content ratio of the Si element contained in the negative electrode upper layer 164u is preferably 90 mass% or more, more preferably 95 mass% or more, and further preferably 98 mass% or more. Typically, the content of the Si element contained in the negative electrode upper layer 164u is greater than the content of the Si element contained in the negative electrode lower layer 164d. In other words, in the negative electrode active material layer 164, the Si element is concentrated and dispersed on the positive electrode (positive electrode sheet 50) side.
[0057] As described above, Mn dissolved from the positive electrode active material layer 54 precipitates on the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 64, in other words, on the surface layer of the negative electrode active material layer 164, to form a coating. By concentrating and dispersing the Si-containing material on the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 164, i.e., on the negative electrode upper layer 164u side, the effect of suppressing the formation of a coating by Mn on the surface of the negative electrode active material layer 164 is more efficiently exhibited. Therefore, an increase in resistance during storage can be suitably suppressed.
[0058] In this specification, the "content ratio (mass%) of the Si element contained in the negative electrode upper layer when the amount of Si element in the entire negative electrode active material layer is taken as 100%" can be calculated as follows. First, the thickness of the negative electrode upper layer is obtained by observing a cross-sectional SEM image of the negative electrode active material layer 164. Next, for a predetermined area of the negative electrode active material layer, a sample is collected by scraping off the negative electrode active material layer by the thickness of the obtained negative electrode upper layer, and an ICP (Inductively Coupled Plasma) analysis is performed to calculate the amount of Si element in the negative electrode upper layer. Similarly, for the negative electrode lower layer, a sample is collected by scraping off a predetermined area of the negative electrode active material layer, and the amount of Si element in the negative electrode lower layer is calculated by ICP analysis. Then, the content ratio of the Si element in the negative electrode upper layer to the amount of Si element in the entire negative electrode active material layer can be obtained from the values of the Si element amounts of the negative electrode upper layer and the negative electrode lower layer obtained respectively.
[0059] The content of Si element contained in the negative electrode upper layer 164u is preferably 2 mass % or more, and more preferably 5 mass % or more, when the total amount of the negative electrode active material 66 in the negative electrode upper layer 164u is taken as 100 mass %.
[0060] The negative electrode lower layer 164d is a layer located closer to the negative electrode current collector 62 than the negative electrode upper layer 164u when viewed in the thickness direction of the negative electrode active material layer 64. Here, the negative electrode lower layer 164d is in contact with the negative electrode current collector 62.
[0061] The negative electrode active material 66 of the negative electrode lower layer 164d essentially contains a carbon material 66c. The negative electrode lower layer 164d may contain a Si-containing material 66s, or may not contain a Si-containing material 66s. The content of the Si element contained in the negative electrode lower layer 164d is not particularly limited, but may be, for example, 2% by mass or less, and preferably 1% by mass or less, when the negative electrode active material of the negative electrode lower layer 164d is taken as 100% by mass. The content of the C element contained in the negative electrode lower layer 164d is not particularly limited, but is preferably 98% by mass or more, and more preferably 99% by mass or more, when the negative electrode active material of the negative electrode lower layer 164d is taken as 100% by mass.
[0062] The ratio (Tu / Ta) of the thickness Tu of the negative electrode upper layer 164u to the total thickness Ta of the negative electrode active material layer 164 is, for example, 0.8 or less, and preferably 0.7 or less. This allows the Si-containing material 66s (in other words, Si element) in the negative electrode active material layer 164 to be dispersed on the positive electrode (positive electrode sheet 50) side, and thus the effect of suppressing the formation of a coating by Mn is more efficiently exhibited. Therefore, the increase in resistance during storage can be suitably suppressed. In addition, from the viewpoint of packing property, the ratio of the thickness Tu of the negative electrode upper layer 164u to the total thickness Ta of the negative electrode active material layer 164 is, for example, 0.4 or more, and preferably 0.5 or more. Note that the "ratio of the thickness of the negative electrode upper layer to the total thickness of the negative electrode active material layer" in the specification is measured in a cross-sectional SEM image of the negative electrode active material layer 164.
[0063] The above-mentioned negative electrode upper layer 164u and negative electrode lower layer 164d can be produced by a conventionally known method. For example, but not limited to, the negative electrode upper layer 164u and negative electrode lower layer 164d can be formed by preparing a negative electrode active material layer forming slurry using two or more types of negative electrode active materials 66 having different compositions (typically, the content ratio of the Si-containing material) and applying the negative electrode active material layer forming slurry.
[0064] Hereinafter, examples of the technology disclosed herein will be described, but it is not intended that the technology disclosed herein be limited to those shown in these examples.
[0065] <Test Example 1: Examination of the presence or absence of Si in the negative electrode active material> (Example 1) [Preparation of positive electrode sheet] A layered lithium transition metal composite oxide having a composition (molar ratio) of Ni, Co, and Mn of Ni:Co:Mn=83:0:17 (corresponding to 83 / 0 / 17 in the "Ni / Co / Mn" column in Table 1) was prepared as the positive electrode active material according to Example 1. The molar ratio of Li to the total of the transition metal elements (Ni+Co+Mn) of the lithium transition metal composite oxide (Li / (Ni+Co+Mn)) was 1.0 mol%. The positive electrode active material prepared above, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in a solid mass ratio of positive electrode active material:AB:PVDF=100:1:1. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to the obtained mixture and kneaded to prepare a slurry for forming a positive electrode active material layer. The obtained positive electrode active material layer forming slurry was applied to both sides of a positive electrode current collector made of aluminum foil with a thickness of 15 μm and dried to form a positive electrode active material layer. The obtained positive electrode active material layer was roll-pressed using a rolling roller and then cut to a predetermined size to prepare a positive electrode sheet.
[0066] [Preparation of negative electrode sheet] First, graphite as a carbon material and a Si-C composite as a Si-containing material were mixed so that the content ratio of Si element was 10 mass% and the content ratio of C element was 90 mass% when the total amount of the negative electrode active material was 100 mass%, to prepare a negative electrode active material. Styrene butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and single-walled carbon nanotubes (SWCNT) as a conductive material were mixed in ion-exchanged water at a solid content mass ratio of negative electrode active material:SBR:CMC:SWCNT=100:1:1:0.5 to prepare a slurry for forming a negative electrode active material layer. The obtained slurry for forming a negative electrode active material layer was applied on a negative electrode current collector made of copper foil with a thickness of 10 μm and dried to form a negative electrode active material layer. The obtained negative electrode active material layer was roll-pressed using a rolling roller and then cut to a predetermined size. In this way, a negative electrode sheet according to Example 1 was produced in which the Si-containing material was dispersed almost uniformly throughout the entire negative electrode active material.
[0067] [Preparing the separator] As a separator, a porous polyolefin sheet having a thickness of 20 μm and a three-layer structure of PP / PE / PE was prepared.
[0068] [Preparation of non-aqueous electrolyte] A non-aqueous electrolyte was prepared by dissolving LiPF6 as a supporting electrolyte at a concentration of 1 mol / L in a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC) in a volume ratio of EC:EMC:DMC:FEC=25:40:30:5.
[0069] [Preparation of lithium-ion secondary batteries for evaluation] The positive electrode sheet and the negative electrode sheet were stacked with a separator interposed therebetween to obtain a laminate. The laminate was then wound to obtain a wound body, which was then pressed to obtain a flattened electrode body. A current collector terminal was attached to the electrode body, which was then inserted into a battery case and welded, after which a non-aqueous electrolyte was poured in. The battery case was then sealed to produce a lithium ion secondary battery for evaluation.
[0070] [Initial charging process] The obtained lithium ion secondary battery for evaluation according to Example 1 was subjected to a constant current charge at a current value of 0.1 C to a voltage of 4.2 V as an initial charge process in a temperature environment of 25° C., and then constant voltage charge was performed until the current value became 1 / 20 C. Thereafter, the battery was discharged at a constant current value of 0.1 C to 3.0 V.
[0071] (Examples 2 to 4) Lithium ion secondary batteries for evaluation according to Examples 2 to 4 were produced in the same manner as in Example 1, except that the composition (molar ratio) of Ni, Co, and Mn in the positive electrode active material was changed as shown in the "Ni / Co / Mn" column in Table 1, and an initial charging process was performed.
[0072] (Examples 5 to 8) Lithium ion secondary batteries for evaluation according to Examples 5 to 8 were produced in the same manner as in Example 1, except that the composition (molar ratio) of Ni, Co, and Mn in the positive electrode active material was changed as shown in the "Ni / Co / Mn" column in Table 1, and the negative electrode active material was changed to only graphite (i.e., did not contain a Si-containing material), and an initial charging process was performed.
[0073] (Reference example) In addition, as a reference example, a lithium-ion secondary battery for evaluation was produced in the same manner as in Example 1, except that the composition (molar ratio) of Ni, Co, and Mn in the positive electrode active material was 83:5:12, and the negative electrode active material was graphite alone (i.e., did not contain a Si-containing material), and an initial charging process was performed.
[0074] [Evaluation of storage resistance increase rate] First, the lithium ion secondary batteries for evaluation according to Examples 1 to 8 and Reference Example were charged at a constant current and constant voltage (CCCV) at a current value of 0.3 C in a thermostatic chamber at 25° C., and the SOC (State of Charge) was adjusted to 50%. Then, pulse discharge was performed at a current value of 5 C for 10 seconds. The voltage change (ΔV) during the pulse discharge was obtained and calculated using the following formula (I): Resistance value = voltage change (ΔV) / current value (5C)…(I) The resistance value before storage (initial resistance value) was calculated using the above formula. Then, the SOC was adjusted to 100% in a temperature environment of 25°C. Each of the lithium ion secondary batteries for evaluation was placed in a thermostatic chamber at 60°C and stored for 14 days. The resistance value after storage was calculated in the same manner as for the initial resistance. Then, the resistance value after storage was calculated using the following formula (II): Resistance increase rate (%) = (resistance value after storage / resistance value before storage) x 100...(II) The resistance increase rate (%) was calculated from the above data, and the results are shown in Table 1.
[0075] [Table 1]
[0076] As shown in the results in Table 1, a comparison of the Reference Example and Examples 5 to 8 shows that the resistance characteristics deteriorate as the Co content in the positive electrode active material decreases, since the resistance increase rate during storage increases. However, in Examples 1 to 4, by including a Si-C composite in addition to graphite as the negative electrode active material, the resistance increase during storage was suppressed compared to Examples 5 to 8, and the resistance increase rate was close to that of the Reference Example.
[0077] <Test Example 2: Examination of Ni compounding ratio in positive electrode active material> (Examples 9-16) Lithium ion secondary batteries for evaluation according to Examples 9 to 16 were produced and subjected to an initial charging process in the same manner as in Example 1, except that the composition (molar ratio) of Ni, Co, and Mn in the positive electrode active material was changed as shown in the "Ni / Co / Mn" column in Table 2. The resistance increase rate during storage of the lithium ion secondary batteries for evaluation according to Examples 9 to 16 was evaluated in the same manner as described above. The results are shown in Table 2.
[0078] [Table 2]
[0079] As shown in the results in Table 2, the resistance suppressing effect during storage was observed in Examples 9 to 12 in which the Ni blending ratio in the positive electrode active material was 90 mol %, and in Examples 13 to 16 in which the Ni blending ratio in the positive electrode active material was 75 mol %.
[0080] <Test Example 3: Examination of Si ratio> (Examples 17-19) Lithium ion secondary batteries for evaluation according to Examples 17 to 19 were produced in the same manner as in Example 1, except that the content ratio of Si element when the total amount of the negative electrode active material, that is, graphite as the carbon material and the Si-C composite as the Si-containing material, was taken as 100 mass %, was changed as shown in the "Si content ratio" column in Table 3, and an initial charging process was performed. The lithium ion secondary batteries for evaluation according to Examples 17 to 19 were evaluated for the resistance increase rate during storage in the same manner as described above. The results are shown in Table 3.
[0081] [Capacity maintenance rate] Furthermore, in this test example, the evaluation of the resistance increase rate during storage was performed in parallel with the evaluation of the capacity retention rate. First, for the evaluation lithium ion secondary batteries according to Examples 1, 5, and 17 to 19, the discharge capacity measured during the evaluation of the resistance increase rate during storage was taken as the initial capacity. Thereafter, the discharge capacity of the evaluation lithium ion secondary batteries stored in the above-mentioned evaluation of the resistance increase rate during storage (i.e., after storage at 60°C for 14 days) was determined in the same manner as the initial capacity. Then, the discharge capacity was calculated using the following formula (III): Capacity retention rate (%) = discharge capacity after 14 days storage / initial capacity × 100…(III) was used to determine the capacity retention rates (%) for Examples 1, 5, and 17 to 19. The results are shown in Table 3.
[0082] [Table 3]
[0083] As shown in the results of Table 3, even in Example 18, in which the content ratio of the Si element was 2 mass%, the effect of suppressing the increase in resistance during storage was observed, compared to Example 5, in which only graphite was used as the negative electrode active material. In addition, the higher the content ratio of the Si element, the better the effect of suppressing the increase in battery resistance, while the lower the content ratio of the Si element, the better the capacity retention rate. Therefore, from the viewpoint of achieving both the effect of suppressing the increase in resistance during storage and the capacity retention rate, it is considered that the content ratio of the Si element in the negative electrode active material is more preferably in the range of 5 to 10 mass%.
[0084] <Test Example 4: Examination of the distribution of Si-containing material in the negative electrode active material layer> (Examples 20-21) A first negative electrode active material layer-forming slurry was prepared in the same manner as in Example 1, except that the negative electrode active material was graphite alone (i.e., the content ratio of Si element was 0 mass% and the content ratio of C element was 100 mass% when the total amount of the negative electrode active material was 100 mass%). Similarly, a second negative electrode active material layer forming slurry was prepared in the same manner as in Example 1, except that the graphite and the Si-C composite were mixed so that the content ratio of Si element was 20 mass% and the content ratio of C element was 80 mass% when the total amount of the negative electrode active material was 100 mass%.
[0085] The first negative electrode active material layer forming slurry was applied onto the negative electrode current collector made of the same copper foil as that used in Example 1, dried, and roll-pressed using a rolling roller to obtain a predetermined density. Next, the second negative electrode active material layer forming slurry was applied onto the dried coating film of the first negative electrode active material layer forming slurry, dried, and roll-pressed using a rolling roller to obtain a predetermined density. At this time, the thickness of the second negative electrode active material layer forming slurry was set to 0.5 with respect to the thickness of the entire negative electrode active material layer. As a result, a negative electrode sheet of Example 20 was obtained in which the negative electrode lower layer formed by the first negative electrode active material layer forming slurry and the negative electrode upper layer formed by the second negative electrode active material layer forming slurry were supported on the negative electrode current collector. In addition, in the negative electrode sheet of Example 20, the content ratio of the Si element in the negative electrode upper layer was 99 mass% when the Si element in the entire negative electrode active material was 100 mass%. Similarly, the second negative electrode active material layer forming slurry was applied onto the same copper foil negative electrode current collector as used in Example 1, dried, and roll-pressed using a rolling roller to obtain a predetermined density. Next, the first negative electrode active material layer forming slurry was applied onto the dried coating film of the second negative electrode active material layer forming slurry, dried, and roll-pressed using a rolling roller to obtain a predetermined density. At this time, the thickness of the first negative electrode active material layer forming slurry was set to 0.5 with respect to the thickness of the entire negative electrode active material layer. As a result, a negative electrode sheet of Example 21 was obtained in which a negative electrode lower layer formed by the second negative electrode active material layer forming slurry and a negative electrode upper layer formed by the first negative electrode active material layer forming slurry were supported on a negative electrode current collector. In addition, in the negative electrode sheet of Example 21, the content ratio of the Si element in the negative electrode upper layer was 1 mass% when the Si element in the entire negative electrode active material was 100 mass%.
[0086] Except for using the above-mentioned negative electrode sheet, evaluation batteries according to Examples 20 and 21 were produced in the same manner as in Example 1, and an initial charging process was performed. The evaluation lithium ion secondary batteries according to Examples 20 and 21 were evaluated for the storage resistance increase rate in the same manner as described above. The results are shown in Table 4.
[0087] [Table 4]
[0088] As shown in the results of Table 4, in all of Examples 1, 20, and 21, the effect of suppressing the resistance increase during storage was observed compared to Example 5, in which only graphite was used as the negative electrode active material. Looking at Examples 1, 20, and 21, all of which have a Si blending ratio of 10 mass%, Example 1, in which the Si-containing material (Si-C composite) was uniformly dispersed throughout the negative electrode active material layer, showed a good effect of suppressing the resistance increase rate during storage, and Example 20, in which the Si-containing material (Si-C composite) was concentrated and arranged in the upper layer, showed even better results in suppressing the resistance increase rate during storage. This is thought to be because the Si-containing material was concentrated and arranged in the upper layer of the negative electrode active material, which more efficiently expressed the effect of suppressing the precipitation of Mn by the Si-containing material on the surface of the negative electrode active material.
[0089] Although the preferred embodiment of the present disclosure has been described above, the above embodiment is merely an example. The present disclosure can be implemented in various other forms. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. In addition, if the technical feature is not described as essential, it is also possible to delete it as appropriate.
[0090] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, wherein the positive electrode comprises a positive electrode active material layer containing a positive electrode active material, the positive electrode active material being a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, and wherein in the lithium transition metal composite oxide, a content of Ni relative to a total of metal elements other than Li is 75 mol % or more, the negative electrode comprises a negative electrode active material layer containing a negative electrode active material, the negative electrode active material including a carbon material and a Si-containing material, and in the positive electrode active material, a content (mol) of Co element and a content (mol) of Mn element satisfy the following relationship: 0≦Co / Mn≦0.43. Item 2: The lithium ion secondary battery according to item 1, wherein in the positive electrode active material, the content (mol) of Co element and the content (mol) of Mn element satisfy the following relationship: 0≦Co / Mn≦0.32. Item 3: The positive electrode active material has the following general formula: Li α Ni x Mn y M z Item 3. The lithium ion secondary battery according to item 1 or 2, wherein α is 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, and x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W. Item 4: The lithium ion secondary battery according to any one of Items 1 to 3, wherein a content ratio of Si element in the negative electrode active material is 5 mass % or more and 10 mass % or less when a total amount of the negative electrode active material is taken as 100 mass %. Item 5: The lithium ion secondary battery according to any one of Items 1 to 4, wherein the negative electrode further includes a negative electrode current collector, the negative electrode active material layer includes a negative electrode lower layer in contact with the current collector, and a negative electrode upper layer further from the negative electrode current collector than the negative electrode lower layer, when viewed in a thickness direction, and a content ratio of Si element in the negative electrode upper layer is 90 mass % or more when Si element in the entire negative electrode active material is taken as 100 mass %. Item 6: The lithium ion secondary battery according to item 5, wherein a ratio of a thickness of the negative electrode upper layer to a total thickness of the negative electrode active material layer is 0.4 or more and 0.8 or less. Item 7: The lithium ion secondary battery according to any one of Items 1 to 6, wherein the Si-containing material includes at least one selected from the group consisting of Si, silicon oxide, and a Si-C composite. [Explanation of symbols]
[0091] 20 Electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 60, 160 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64, 164 Negative electrode active material layer 164u negative electrode upper layer 164d Negative electrode lower layer 66 Negative electrode active material 66c Carbon Materials 66s Si-containing material 70 Separator 100 Lithium-ion secondary battery
Claims
1. A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, The positive electrode includes a positive electrode active material layer containing a positive electrode active material, The positive electrode active material is a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, In the lithium transition metal composite oxide, the content of Ni relative to the total of metal elements other than Li is 75 mol % or more, the negative electrode includes a negative electrode active material layer containing a negative electrode active material, The negative electrode active material includes a carbon material and a Si-containing material, In the positive electrode active material, the content (mol) of Co element and the content (mol) of Mn element have the following relationship: 0≦Co / Mn≦0.43 Fulfilling Lithium-ion secondary battery.
2. In the positive electrode active material, the content (mol) of Co element and the content (mol) of Mn element have the following relationship: 0≦Co / Mn≦0.32 Fulfilling The lithium ion secondary battery according to claim 1 .
3. The positive electrode active material has the following general formula: Li α Ni x Mn y M z O 2 (wherein 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.) The lithium ion secondary battery according to claim 1 or 2.
4. When the total amount of the negative electrode active material is taken as 100 mass%, the content ratio of Si element in the negative electrode active material is 5 mass% or more and 10 mass% or less. The lithium ion secondary battery according to claim 1 or 2.
5. The negative electrode further includes a negative electrode current collector, the negative electrode active material layer includes a negative electrode lower layer in contact with the negative electrode current collector and a negative electrode upper layer located farther from the negative electrode current collector than the negative electrode lower layer when viewed in a thickness direction, The content ratio of the Si element in the negative electrode upper layer is 90 mass% or more when the Si element in the entire negative electrode active material is 100 mass%. The lithium ion secondary battery according to claim 1 or 2.
6. a ratio of a thickness of the negative electrode upper layer to a total thickness of the negative electrode active material layer is 0.4 or more and 0.8 or less; The lithium ion secondary battery according to claim 5 .
7. The Si-containing material includes at least one selected from the group consisting of Si, silicon oxide, and Si-C composites; The lithium ion secondary battery according to claim 1 or 2.
Citation Information
Patent Citations
Negative electrode for lithium ion secondary battery
JP2018125077A
Nonaqueous-electrolyte secondary-battery negative electrode
WO2015115051A1
Lithium ion secondary battery
WO2016152861A1
Positive electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
WO2021241078A1
Negative electrode for lithium-ion secondary battery
WO2022080995A1