Positive electrode active material and sodium ion secondary battery

By employing Na-containing oxide particles with controlled size, aspect ratio, and composition, the gravimetric energy density of positive electrode active materials is significantly improved, addressing the limitations of conventional P2 type structures in sodium ion secondary batteries.

JP2024158367AActive Publication Date: 2024-11-08TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023073516
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

Conventional positive electrode active materials with a P2 type structure have limitations in terms of gravimetric energy density.

Method used

The development of a positive electrode active material comprising Na-containing oxide particles with a P2 type structure, containing elements such as Mn, Ni, and Co, with specific average particle diameter and aspect ratio, and a predetermined chemical composition, which are produced through a controlled manufacturing process.

Benefits of technology

The resulting positive electrode active material exhibits enhanced gravimetric energy density due to optimized particle size and composition, leading to improved performance in sodium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158367000001_ABST
    Figure 2024158367000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode active material which has a P2-type structure and a large energy density.SOLUTION: The positive electrode active material of the present disclosure includes Na-containing oxide. The Na-containing oxide particles have a P2-type structure. The Na-containing oxide particles include at least one of Mn, Ni, and Co and includes Na and O as constituent elements. The Na-containing oxide particles have an average particle diameter of at least 2.0 μm. The Na-containing oxide particles have an average aspect ratio of at least 1.0 and 3.0 at largest.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a positive electrode active material and a sodium ion secondary battery. [Background technology]

[0002] Patent Documents 1 and 2 disclose Na-containing oxides having a P2 type structure and a specific chemical composition. The Na-containing oxides having a P2 type structure are used as positive electrode active materials for sodium ion secondary batteries. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-201588 A [Patent Document 2] JP 2017-045600 A Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional positive electrode active materials having a P2 type structure have room for improvement in terms of gravimetric energy density. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A positive electrode active material comprising Na-containing oxide particles, The Na-containing oxide particles have a P2 type structure, The Na-containing oxide particles contain, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O, The Na-containing oxide particles have an average particle size of 2.0 μm or more, The Na-containing oxide particles have an average aspect ratio of 1.0 or more and 3.0 or less. Cathode active material. <Aspect 2> The positive electrode active material of Aspect 1, wherein the Na-containing oxide particles contain more than 0.35 moles of Na per 1 mole of O as a constituent element, Positive electrode active material. <Aspect 3> The positive electrode active material of Aspect 1 or 2, wherein the Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W).) having a chemical composition represented by, Positive electrode active material. <Aspect 4> The positive electrode active material of any one of Aspects 1 to 3, wherein the Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0 < a ≤ 1.00, 0 < x < 1.00, 0 < y < 0.50, 0 < z < 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W).) having a chemical composition represented by, Positive electrode active material. <Aspect 5> The positive electrode active material of any one of Aspects 1 to 4, wherein the Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+rO2 (where 0.70 < a ≤ 1.00, 0.30 < x < 0.60, 0.10 < y < 0.40, 0.10 < z < 0.50, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) having a chemical composition represented by a positive electrode active material. <Aspect 6> A positive electrode active material containing Na-containing oxide particles, wherein the Na-containing oxide particles have a P2-type structure, the Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0.70 < a ≤ 1.00, 0 < x < 1.00, 0 < y < 0.50, 0 < z < 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) having a chemical composition represented by a positive electrode active material. <Aspect 7> The positive electrode active material of Aspect 6, wherein the Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0.70 < a ≤ 1.00, 0.30 < x < 0.60, 0.10 < y < 0.40, 0.10 < z < 0.50, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) having a chemical composition represented by a positive electrode active material. <Aspect 8> A positive electrode active material according to any one of Aspects 1 to 7, wherein the P2-type structure has a c-axis length of 11.10 Å or less. Cathode active material. <Aspect 9> A sodium ion secondary battery, A positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer includes the positive electrode active material according to any one of aspects 1 to 8. Sodium ion secondary battery. Effect of the Invention

[0006] The positive electrode active material of the present disclosure has excellent gravimetric energy density. [Brief description of the drawings]

[0007] [Figure 1] 1 shows an example of a flow of a method for producing a Na-containing oxide having a P2 type structure. [Diagram 2] 1 illustrates an example of the configuration of a sodium ion secondary battery. [Diagram 3] 1 shows X-ray diffraction patterns of the positive electrode active materials according to Examples 1 to 3. [Figure 4] 1 shows an X-ray diffraction pattern of the positive electrode active material according to Comparative Example 1. [Diagram 5] 2 shows a cross-sectional SEM image of the positive electrode active material according to Example 1. [Figure 6] 2 shows an external SEM image of the positive electrode active material according to Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1.Cathode active material 1.1 First form The positive electrode active material according to the first embodiment includes Na-containing oxide particles. The Na-containing oxide particles have a P2 type structure. The Na-containing oxide particles include, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O. The Na-containing oxide particles have an average particle size of 2.0 μm or more. The Na-containing oxide particles have an average aspect ratio of 1.0 or more and 3.0 or less.

[0009] 1.1.1 Crystal structure The Na-containing oxide particles according to the first embodiment have at least a P2 type structure (belonging to space group P63mc) as a crystal structure. The Na-containing oxide particles may have a crystal structure other than the P2 type structure in addition to the P2 type structure. Examples of the crystal structure other than the P2 type structure include various crystal structures (P3 type structure, etc.) formed when Na is desorbed from the P2 type structure. The Na-containing oxide particles may have a P2 type structure as a main phase. The crystal structure of the Na-containing oxide particles as a main phase may change depending on the charge / discharge state.

[0010] The Na-containing oxide particle according to the first embodiment may be a single crystal consisting of one crystallite, or may be a polycrystal having a plurality of crystallites. The end faces of the crystallites of the Na-containing oxide particles are considered to be the entrance and exit of intercalation. That is, when the crystallites of the Na-containing oxide particles are small, the effect of increasing the number of entrances and exits of intercalation and decreasing the reaction resistance, the effect of shortening the distance of movement of sodium ions and decreasing the diffusion resistance, the effect of reducing the absolute amount of expansion and contraction during charging and discharging and making it difficult for cracks to occur, etc. can be expected. For example, the diameter of the crystallites constituting the Na-containing oxide particles may be 0.1 μm or more and 5.0 μm or less, 0.5 μm or more and 4.0 μm or less, or 1.0 μm or more and 3.0 μm or less. The "crystallite" or "diameter of the crystallite" can be obtained by observing the Na-containing oxide particles with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when a closed region surrounded by a grain boundary is observed by observing the Na-containing oxide particles, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is determined, and this is regarded as the "diameter of the crystallite". In addition, when the Na-containing oxide particle is composed of a single crystal, the particle itself can be said to be one crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can be determined by EBSD or XRD. For example, the diameter of the crystallite can be determined based on the Scherrer formula from the half-width of the diffraction line of the XRD pattern. When the diameter of the crystallite specified by any method is within the above range, the Na-containing oxide particle is likely to exhibit higher performance. The crystallite constituting the Na-containing oxide particle may have a first surface exposed on the surface of the oxide, and the first surface may be planar.

[0011] The Na-containing oxide particles according to the first embodiment have a predetermined average particle size (D50) and a predetermined average aspect ratio. In order to achieve such an average particle size and average aspect ratio, in this embodiment, a specific process described below is adopted when producing the Na-containing oxide particles. According to the knowledge of the present inventor, the Na-containing oxide particles obtained through such a specific process tend to have a c-axis length of the P2 type structure smaller than that of conventional ones. For example, the P2 type structure in the Na-containing oxide particles according to the first embodiment may have a c-axis length of 11.10 Å or less. The P2 type structure may have a c-axis length of 11.05 Å or more and 11.10 Å or less. The lattice constants (a-axis length, b-axis length, and c-axis length) of the P2 type structure can be determined by full pattern fitting from the X-ray diffraction pattern of the Na-containing oxide particles. The software used is PDXL2 from Rigaku Corporation. Here, the "X-ray diffraction pattern of the Na-containing oxide particles" refers to one obtained under the following conditions. That is, an X-ray diffraction pattern is obtained for the Na-containing oxide particles using an X-ray diffraction device (Rigaku, fully automatic multipurpose X-ray diffraction device SmartLab) with CuKα as the radiation source, a tube voltage of 45 kV, a tube current of 200 mA, a step width of 0.02°, and a 2θ / θ scan at a scan speed of 1° / min.

[0012] 1.1.2 Chemical composition The Na-containing oxide particles according to the first embodiment contain, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O. The Na-containing oxide particles are particularly likely to obtain higher performance when they contain, as constituent elements, at least Na, Mn, one or both of Ni and Co, and O, and among these, when they contain, as constituent elements, at least Na, Mn, Ni, Co, and O. Alternatively, the Na-containing oxide particles are also likely to obtain higher performance when they contain, as constituent elements, at least Na, Mn, Fe, and O. The Na-containing oxide particles according to the first embodiment may contain, as a constituent element, more than 0.35 mol of Na per mol of O. The upper limit of the amount of Na per mol of O is not particularly limited. The Na-containing oxide particles according to the first embodiment may contain, as a constituent element, more than 0.35 mol and not more than 0.50 mol of Na per mol of O, or 0.38 mol or more and not more than 0.45 mol of Na. Thus, Na-containing oxide particles containing more than 0.35 mol of Na per mol of O tend to have an excellent weight energy density as a positive electrode active material.

[0013] The Na-containing oxide particles according to the first embodiment include Na a Mn x-p Ni y-q Co z-r M p+q+rIt may have a chemical composition represented by O2 (where 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). When the Na-containing oxide particles have such a chemical composition, the P2-type structure is likely to be maintained. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, 0.60 or more, or 0.70 or more, and is ≤ 1.00, and may be ≤ 0.90. Also, x is ≥ 0, and may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is ≤ 1.00, and may be < 1.00, ≤ 0.90, ≤ 0.80, ≤ 0.70, ≤ 0.60, ≤ 0.50, or < 0.50. Also, y is ≥ 0, and may be greater than 0, 0.10 or more, or 0.20 or more, and is ≤ 1.00, and may be < 1.00, ≤ 0.90, ≤ 0.80, ≤ 0.70, ≤ 0.60, ≤ 0.50, ≤ 0.40, ≤ 0.30, or ≤ 0.20. Also, z is ≥ 0, and may be greater than 0, 0.10 or more, 0.20 or more, or 0.30 or more, and is ≤ 1.00, and may be < 1.00, ≤ 0.90, ≤ 0.80, ≤ 0.70, ≤ 0.60, ≤ 0.50, ≤ 0.40, or ≤ 0.30. The element M has a small contribution to charge and discharge. In this regard, in the above chemical composition, since p + q + r < 0.17, a high charge and discharge capacity is likely to be ensured. p + q + r may be ≤ 0.16, ≤ 0.15, ≤ 0.14, ≤ 0.13, ≤ 0.12, ≤ 0.11, or ≤ 0.10. On the other hand, when the element M is included, the P2-type structure is likely to be stabilized. In the above chemical composition, p + q + r is ≥ 0, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.

[0014] The Na-containing oxide particles according to the first embodiment contain Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0 < a ≤ 1.00, 0 < x < 1.00, 0 < y < 0.50, 0 < z < 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). Further, the Na-containing oxide particles according to the first embodiment contain Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0.70 < a ≤ 1.00, 0.30 < x < 0.60, 0.10 < y < 0.40, 0.10 < z < 0.50, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). Conventionally, it has been difficult to produce Na-containing oxide particles having a P2-type structure and such a chemical composition. However, in the present embodiment, by adopting specific conditions described later as the production conditions for Na-containing oxide particles having a P2-type structure, Na-containing oxide particles having a P2-type structure and such a chemical composition can be obtained. The Na-containing oxide particles having such a chemical composition have excellent weight energy density as a positive electrode active material.

[0015] 1.1.3 Shape The Na-containing oxide particles according to the first embodiment may be solid particles, hollow particles, or particles having voids. The Na-containing oxide particles according to the first embodiment have excellent weight energy density as a positive electrode active material by having the following average aspect ratio and average particle diameter.

[0016] 1.1.3.1 Aspect ratio The P2 type structure is a hexagonal crystal system, has a large diffusion coefficient of Na ions, and is prone to crystal growth in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2 type structure, the crystal is prone to grow in a plate-like shape in a specific direction. Therefore, the Na-containing oxide particles having the P2 type structure are usually plate-like particles with a large aspect ratio in which the crystal growth direction is biased in a specific direction. Specifically, the Na-containing oxide particles having the P2 type structure are usually plate-like particles with an average aspect ratio that is significantly greater than 3.0. Here, the end of the plate-like particle becomes the entrance and exit of intercalation. As far as the present inventors have confirmed, plate-like particles with a large aspect ratio tend to have a smaller proportion of the part that contributes to intercalation in the entire particle, and the weight energy density is likely to decrease.

[0017] In contrast, the Na-containing oxide particles according to the first embodiment have a certain aspect ratio or less, with the crystal growth direction being suppressed from being biased. Specifically, the Na-containing oxide particles according to the first embodiment have an average aspect ratio of 1.0 to 3.0. When the average aspect ratio of the Na-containing oxide particles having a P2 structure is 3.0 or less, the weight energy density and the like as a positive electrode active material are likely to increase. The average aspect ratio of the Na-containing oxide particles according to the first embodiment may be 1.0 to 2.9, 1.0 to 2.8, 1.0 to 2.7, 1.0 to 2.6, 1.0 to 2.5, or 1.0 to 2.4.

[0018] The "average aspect ratio" of the Na-containing oxide particles is measured as follows. That is, the cross section of the Na-containing oxide particles (when the Na-containing oxide particles are contained in the positive electrode active material layer described later, the cross section of the positive electrode active material layer) is observed with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) to identify the shape of the Na-containing oxide particles. In the shape, the maximum Feret diameter is identified and regarded as the "major axis". In addition, in the shape, the largest diameter perpendicular to the "major axis" is regarded as the "minor axis". The ratio of the "major axis" to the "minor axis" (major axis / minor axis) is regarded as the "aspect ratio" of the Na-containing oxide particles. The "aspect ratio" is calculated for each Na-containing oxide particle, and the number average value is regarded as the "average aspect ratio".

[0019] 1.1.3.2 Average particle size As described above, in the conventional technology, the Na-containing oxide particles having a P2 type structure are plate-like particles with a large aspect ratio in which the crystal growth direction is biased to a specific direction. In the conventional technology, when the growth of the P2 phase is suppressed, the average particle size of the Na-containing oxide particles becomes extremely small, and there is a concern that excessive aggregation between particles may occur, and there is also a risk that a sufficient amount of the P2 phase may not be obtained. As a result, it is difficult to ensure a sufficient weight energy density for the Na-containing oxide particles according to the conventional technology. In contrast, the Na-containing oxide particles according to the first embodiment can solve such problems by having a certain or larger size while having the above-mentioned average aspect ratio. Specifically, the Na-containing oxide particles according to the first embodiment have an average particle size of 2.0 μm or more. The average particle size of the Na-containing oxide particles according to the first embodiment may be 2.0 μm or more and 5.0 μm or less, 2.0 μm or more and 4.0 μm or less, or 2.0 μm or more and 3.0 μm or less.

[0020] The "average particle size" of the Na-containing oxide particles is the particle size at an integrated value of 50% in the volume-based particle size distribution determined by a laser diffraction / scattering method (D50, median size).

[0021] 1.1.4 Other As described above, the positive electrode active material according to the first embodiment includes Na-containing oxide particles having the above-specified average particle diameter and average aspect ratio, and thus has excellent weight energy density. The positive electrode active material according to the first embodiment may consist only of the above Na-containing oxide particles, or may include, together with the above Na-containing oxide particles, other positive electrode active materials (other positive electrode active materials). From the viewpoint of further enhancing the above effects, the proportion of other positive electrode active materials in the entire positive electrode active material may be small. For example, assuming the total amount of the positive electrode active material is 100% by mass, the content of the above Na-containing oxide particles may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.

[0022] 1.2 Second Embodiment The positive electrode active material according to the second embodiment includes Na-containing oxide particles. The Na-containing oxide particles have a P2-type structure. The Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0.70 < a ≤ 1.00, 0 < x < 1.00, 0 < y < 0.50, 0 < z < 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W).) has a chemical composition represented by

[0023] 1.2.1 Crystal Structure The Na-containing oxide particles according to the second embodiment have at least a P2 type structure (belonging to space group P63mc) as a crystal structure, similar to the Na-containing oxide particles according to the first embodiment. The Na-containing oxide particles may have a crystal structure other than the P2 type structure in addition to the P2 type structure. Examples of the crystal structure other than the P2 type structure include various crystal structures (P3 type structure, etc.) formed when Na is desorbed from the P2 type structure. The Na-containing oxide particles may have a P2 type structure as a main phase. The crystal structure of the Na-containing oxide particles as a main phase may change depending on the charge / discharge state.

[0024] The Na-containing oxide particles according to the second embodiment may be a single crystal consisting of one crystallite, or may be a polycrystal having a plurality of crystallites, similar to the Na-containing oxide particles according to the first embodiment. As described above, the end faces of the crystallites of the Na-containing oxide particles are considered to be the inlets and outlets of intercalation. That is, when the crystallites of the Na-containing oxide particles are small, the effect of increasing the number of inlets and outlets of intercalation and decreasing the reaction resistance, the effect of shortening the distance of movement of sodium ions and decreasing the diffusion resistance, the effect of reducing the absolute amount of expansion and contraction during charging and discharging and making it difficult for cracks to occur, etc. can be expected. For example, the diameter of the crystallites constituting the Na-containing oxide particles may be 0.1 μm or more and 5.0 μm or less, 0.5 μm or more and 4.0 μm or less, or 1.0 μm or more and 3.0 μm or less. The crystallites constituting the Na-containing oxide particles may have a first surface exposed on the surface of the oxide, and the first surface may be planar.

[0025] The Na-containing oxide particles according to the second embodiment have a P2-type structure and a predetermined chemical composition. In order to achieve such a crystal structure and chemical composition, in this embodiment, a specific process described later is adopted during the production of the Na-containing oxide particles. According to the findings of the present inventors, the c-axis length of the P2-type structure of the Na-containing oxide particles obtained through such a specific process is likely to be smaller than that of the prior art. For example, the P2-type structure in the Na-containing oxide particles according to the second embodiment may have a c-axis length of 11.10 Å or less. The P2-type structure may have a c-axis length of 11.05 Å or more and 11.10 Å or less. The method for measuring lattice constants such as the c-axis length is as described above.

[0026] 1.2.2 Chemical Composition The Na-containing oxide particles according to the second embodiment contain Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0.70 < a ≤ 1.00, 0 < x < 1.00, 0 < y < 0.50, 0 < z < 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). The Na-containing oxide particles according to the second embodiment contain Na a Mn x-p Ni y-q Co z-r M p+q+rO2 (where 0.70 < a ≤ 1.00, 0.30 < x < 0.60, 0.10 < y < 0.40, 0.10 < z < 0.50, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). It may have a chemical composition represented by this. Conventionally, it has been difficult to produce Na-containing oxide particles having a P2-type structure and such a chemical composition. However, in the present embodiment, as the production conditions of the Na-containing oxide particles having a P2-type structure, by adopting specific conditions, it is possible to obtain Na-containing oxide particles having a P2-type structure and such a chemical composition. The Na-containing oxide particles having such a chemical composition have a high weight energy density as a positive electrode active material. a is more than 0.70, and may be 0.75 or more, or 0.80 or more, and is at most 1.00, and may be 0.90 or less, or less than 0.90. Further, x is more than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, more than 0.30, 0.40 or more, or 0.50 or more, and is less than 1.00, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, less than 0.60, 0.50 or less, or less than 0.50. Further, y is more than 0, and may be 0.10 or more, more than 0.10, or 0.20 or more, and is less than 0.50, 0.45 or less, or 0.40 or less. Further, z is more than 0, and may be 0.10 or more, more than 0.10, 0.20 or more, or 0.30 or more, and is less than 1.00, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, less than 0.50, 0.40 or less, or 0.30 or less. p + q + r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more, and is at most 0.17, 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.

[0027] 1.2.3 Shape The Na-containing oxide particles according to the second embodiment may be solid particles, hollow particles, or particles having voids. The Na-containing oxide particles according to the second embodiment may have the following average aspect ratio and average particle size.

[0028] 1.2.3.1 Aspect Ratio The Na-containing oxide particles according to the second embodiment may have a certain aspect ratio or less, with the crystal growth direction being suppressed from being biased. Specifically, the Na-containing oxide particles according to the second embodiment may have an average aspect ratio of 1.0 to 3.0. When the average aspect ratio of the Na-containing oxide particles having a P2 structure is 3.0 or less, the weight energy density and the like as a positive electrode active material are more likely to be increased. The average aspect ratio of the Na-containing oxide particles according to the second embodiment may be 1.0 to 2.9, 1.0 to 2.8, 1.0 to 2.7, 1.0 to 2.6, 1.0 to 2.5, or 1.0 to 2.4. The method for measuring the "average aspect ratio" is as described above.

[0029] 1.2.3.2 Average particle size The Na-containing oxide particles according to the second embodiment may have an average particle diameter of 2.0 μm or more. The average particle diameter of the Na-containing oxide particles according to the second embodiment may be 2.0 μm or more and 5.0 μm or less, 2.0 μm or more and 4.0 μm or less, or 2.0 μm or more and 3.0 μm or less. The method for measuring the "average particle diameter" of the Na-containing oxide particles is as described above.

[0030] 1.2.4 Other As described above, the positive electrode active material according to the second embodiment has an excellent weight energy density by including the Na-containing oxide particles having the specific chemical composition. The positive electrode active material according to the second embodiment may be composed of only the Na-containing oxide particles, or may include other positive electrode active materials (other positive electrode active materials) together with the Na-containing oxide particles. From the viewpoint of further enhancing the above effect, the ratio of other positive electrode active materials in the entire positive electrode active material may be small. For example, the content of the Na-containing oxide particles may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less, based on the entire positive electrode active material being 100% by mass.

[0031] 2. Manufacturing method of positive electrode active material The Na-containing oxide particles according to the first and second embodiments can be produced, for example, by the following method. As shown in FIG. 1, the method for producing Na-containing oxide particles having a P2 type structure according to one embodiment includes the following steps: S1: Obtaining a precursor comprising at least one element of Mn, Ni and Co; S2: Coating the surface of the precursor with a Na source to obtain a composite; S3: sintering the composite to obtain a Na-containing oxide having a P2 type structure. S3-1: Pre-firing the composite at a temperature of 300° C. or more and less than 700° C. for 2 hours or more and 10 hours or less; S3-2: Following the preliminary firing, the composite is subjected to a main firing at a temperature of 700° C. or more and 1100° C. or less for a period of 30 minutes to 48 hours or less; and S3-3: Following the main sintering, the composite is allowed to cool in the atmosphere from a temperature T1 of 200° C. or higher to a temperature T2 of 100° C. or lower.

[0032] 2.1 S1 In S1, a precursor containing at least one element of Mn, Ni, and Co is obtained. The precursor may contain at least Mn, one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor may be a salt containing at least one element of Mn, Ni, and Co. For example, the precursor may be at least one of carbonate, sulfate, nitrate, and acetate. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple types of compounds. The precursor may have various shapes. For example, the precursor may be particulate, or may be spherical particles as described later. The particle size of the particles made of the precursor is not particularly limited. The composition of the precursor may be appropriately determined so as to correspond to the composition of the Na-containing oxide, which is the final product.

[0033] In S1, a precipitate as the precursor may be obtained by a coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. This makes it easier to obtain spherical particles as the precursor. The "ion source capable of forming a precipitate in an aqueous solution with transition metal ions" may be at least one selected from, for example, sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above salt or hydroxide containing at least one element selected from Mn, Ni, and Co. Specifically, in S1, the ion source and the transition metal compound may be prepared as solutions, and the solutions may be dropped and mixed to obtain a precipitate as the precursor. In this case, for example, water is used as the solvent. In this case, various sodium compounds may be used as the base, and an aqueous ammonia solution or the like may be added to adjust the basicity. In the case of the coprecipitation method, for example, an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate are prepared, and the aqueous solutions are dropped and mixed to obtain a precipitate as the precursor. Alternatively, the precursor can be obtained by a sol-gel method, and in particular, by a coprecipitation method, spherical particles can be easily obtained as the precursor.

[0034] In S1, the precursor may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. These elements M have, for example, a function of stabilizing the P2 type structure. The method of obtaining a precursor containing element M is not particularly limited. When the precursor is obtained by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dropped and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped when Na-doping baking is performed in S2 and S3 described later.

[0035] 2.2 S2 In S2, the surface of the precursor obtained in S1 is coated with a Na source to obtain a composite. The Na source may be a salt containing Na, such as a carbonate or a nitrate, or may be a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor may be determined taking into account the amount of Na lost during the subsequent calcination.

[0036] In S2, the coverage of the Na source on the surface of the precursor is not particularly limited. For example, in S2, the above-mentioned composite may be obtained by covering 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the above-mentioned precursor with a Na source. Alternatively, in S2, the above-mentioned composite may be obtained by covering less than 40 area%, 35 area% or less, or 30 area% or less of the surface of the above-mentioned precursor with a Na source. If the coverage of the Na source is small, when the composite is fired, P2 type crystals tend to grow on the surface of the composite. On the other hand, if the coverage of the Na source is large, when the composite is fired, the crystallites of the P2 type crystals tend to become small, and the growth of the P2 type crystals tends to be suppressed.

[0037] In S2, the method for coating the surface of the precursor with the Na source is not particularly limited. For example, the precursor and the Na source can be mixed in a dry or wet manner to coat the surface of the precursor with the Na source. Alternatively, the surface of the precursor may be coated with the Na source by a tumbling fluidized coating method or a spray drying method. That is, a coating solution in which the Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor, and dried at the same time or after the contact. The coverage rate of the Na source on the surface of the precursor can be controlled by adjusting the coating conditions (temperature, time, number of times, etc.).

[0038] In S2, the precursor may be coated with an M source together with a Na source. For example, in S2, the precursor obtained in S1, a Na source, and an M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W may be mixed to obtain a composite. The M source may be, for example, a salt containing the element M, such as a carbonate or sulfate, or a compound other than a salt, such as an oxide or hydroxide. The amount of the M source relative to the precursor may be determined depending on the chemical composition of the Na-containing oxide after firing.

[0039] 2.3 S3 In S3, the composite obtained in S2 is calcined to obtain a Na-containing oxide having a P2 type structure. S3 includes the above S3-1, S3-2, and S3-3.

[0040] 2.3.1 S3-1 In S3-1, the composite is pre-fired at a temperature of 300°C or more and less than 700°C for 2 hours or more and 10 hours or less. In S3-1, the composite may be arbitrarily shaped and then pre-fired. The pre-fire is performed at a temperature lower than that of the main firing. If the pre-fire is insufficient, the main firing must be performed at a high temperature and for a long time in order to generate a sufficient amount of P2 phase in S3-2, and the P2 phase may grow abnormally. If the pre-fire is insufficient in S3-1, it may be difficult to dope a sufficient amount of Na, and it may be difficult to obtain the P2 phase while having a specific chemical composition. By performing the pre-fire sufficiently, the P2 phase can be properly generated in the main firing, the generation of crystal phases other than the P2 phase can be suppressed, and the shape of the P2-type Na-containing oxide particles can be easily controlled appropriately. That is, in S3-1, the pre-firing temperature is 300°C or more and less than 700°C, and the pre-firing time is 2 hours or more and 10 hours or less, so that the composite can be subjected to sufficient pre-firing, and the Na-containing oxide particles having a P2 type structure obtained through S3-2 and S3-3 described later have a predetermined average aspect ratio and average particle size. In addition, by subjecting the composite to sufficient pre-firing, the P2 type structure can be appropriately generated in S3-2 and S3-3 while having a predetermined chemical composition. The pre-firing temperature may be 400°C or more and less than 700°C, 450°C or more and less than 700°C, 500°C or more and less than 700°C, 550°C or more and less than 700°C, or 550°C or more and less than 650°C. In addition, the pre-firing time may be 2 hours or more and less than 8 hours, 3 hours or more and less than 8 hours, 4 hours or more and less than 8 hours, 5 hours or more and less than 8 hours, or 5 hours or more and less than 7 hours. The pre-firing atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere.

[0041] 2.3.2 S3-2 In S3-2, following the above pre-firing, the composite is subjected to main firing at a temperature of 700°C to 1100°C for 30 minutes to 48 hours. In S3-2, the main firing temperature of the composite is 700°C to 1100°C, preferably 800°C to 1000°C. If the main firing temperature is too low, the P2 phase is not generated, and if the main firing temperature is too high, the O3 phase and the like are likely to be generated instead of the P2 phase. The temperature rise condition from the pre-firing temperature to the main firing temperature is not particularly limited. As described above, the main firing time is 30 minutes to 48 hours. However, the shape of the Na-containing oxide can be controlled by the main firing time. As described above, in the method of the present disclosure, when the coverage rate of the Na source in the composite is 40 area % or more, when the composite is fired, P2 type crystals with small crystallites are likely to be formed on the surface. In the method of the present disclosure, abnormal growth of P2 type crystals is suppressed by growing the P2 type crystals along the surface of the composite. As a result, the shape of the Na-containing oxide particles has a predetermined average aspect ratio and average particle size. If the firing time is too short, the generation of the P2 phase is insufficient. On the other hand, if the firing time is too long, the P2 type crystals grow excessively, and the predetermined average aspect ratio and average particle size cannot be achieved. As far as the present inventors have confirmed, when the firing time is 30 minutes or more and 3 hours or less, the Na-containing oxide particles are likely to have the predetermined average aspect ratio and average particle size.

[0042] 2.3.3 S3-3 In step S3-3, following the main firing, the composite is rapidly cooled (cooled at a temperature drop rate of 20°C / min or more) from a temperature T1 of 200°C or more to a temperature T2 of 100°C or less. The preliminary firing and main firing are performed, for example, in a heating furnace. In step S3-3, for example, the composite is main fired in a heating furnace, then cooled to an arbitrary temperature T1 of 200°C or more in the heating furnace, and after the temperature T1 is reached, the fired product is removed from the heating furnace and rapidly cooled outside the furnace to an arbitrary temperature T2 of 100°C or less. The temperature T1 may be any temperature of 200°C or more, or any temperature of 250°C or more. The temperature T2 may be any temperature of 100°C or less, or any temperature of 50°C or less, or may be the cooling end temperature. In a certain temperature range between the temperature T1 and the temperature T2, moisture is likely to penetrate between the layers of the P2 type structure due to atomic vibration, molecular motion, etc. When cooling the composite (Na-containing oxide having a P2 type structure) after the main firing, it is considered that the amount of moisture that penetrates between the layers of the P2 type structure is reduced by shortening the time in which the temperature range in which moisture easily penetrates (i.e., by cooling quickly). In this regard, when cooling the composite after the main firing in step S3-3, by allowing it to cool in a dry atmosphere outside the furnace from an arbitrary temperature T1 of 200°C or higher to an arbitrary temperature T2 of 100°C or lower, the cooling rate from temperature T1 to temperature T2 is high (e.g., 20°C / min or higher), moisture is less likely to penetrate between the layers of the P2 type structure, and the collapse of the P2 type structure can be suppressed. As a result, Na-containing oxide particles having a P2 type structure and a predetermined chemical composition can be obtained.

[0043] By the above-mentioned method, the Na-containing oxide particles according to the first embodiment and the Na-containing oxide particles according to the second embodiment can be produced.

[0044] 3. Sodium-ion secondary battery The positive electrode active material according to the embodiment includes the specific Na-containing oxide. The positive electrode active material can be used, for example, as a positive electrode active material of a sodium ion secondary battery. FIG. 2 shows a schematic configuration of a sodium ion secondary battery according to an embodiment. As shown in FIG. 2, a sodium ion secondary battery 100 according to an embodiment has a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30. Here, the positive electrode active material layer 10 includes the positive electrode active material according to the embodiment.

[0045] 3.1 Cathode active material layer The positive electrode active material layer 10 includes at least the positive electrode active material according to the above embodiment, and may further include an electrolyte, a conductive assistant, a binder, and the like. Furthermore, the positive electrode active material layer 10 may further include various additives. The content of each of the positive electrode active material, electrolyte, conductive assistant, binder, and the like in the positive electrode active material layer 10 may be appropriately determined according to the intended battery performance. For example, the content of the positive electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire positive electrode active material layer 10 (total solid content) being 100 mass%. The shape of the positive electrode active material layer 10 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer 10 having a substantially flat surface. The thickness of the positive electrode active material layer 10 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0046] 3.1.1 Cathode active material The positive electrode active material is as described above. That is, the positive electrode active material includes the Na-containing oxide particles according to the first embodiment and / or the Na-containing oxide particles according to the second embodiment. As described above, the positive electrode active material may be composed of only the Na-containing oxide particles, or may include other positive electrode active materials (other positive electrode active materials) together with the Na-containing oxide particles. From the viewpoint of further enhancing the effect of the technology of the present disclosure, the ratio of other positive electrode active materials in the entire positive electrode active material may be small. For example, the content of the Na-containing oxide particles may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.

[0047] 3.1.2 Electrolytes The electrolyte that can be contained in the positive electrode active material layer 10 may be a solid electrolyte, a liquid electrolyte (electrolytic solution), or a combination of these. The solid electrolyte may be any known solid electrolyte for sodium ion secondary batteries. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes are excellent in ion conductivity and heat resistance. Examples of inorganic solid electrolytes include Na3Zr2PSi2O 12 and oxides such as Na2O-11Al2O3; NaBH4, NaB 10 H 10 , NaCB9H 10 , NaCB 11 H 12 , NaB 12 Cl 12 Hydrides and borides such as Na3PS4, Na3SbS4, Na 2.88 Sb 0.88 W 0.12Examples of the solid electrolyte include at least one selected from sulfides such as S4 and fluorides such as NaPF6 and NaBF4. The solid electrolyte may be, for example, particulate. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination. The electrolytic solution may contain, for example, sodium ions as carrier ions. The electrolytic solution may be an aqueous electrolytic solution or a non-aqueous electrolytic solution. The composition of the electrolytic solution may be the same as that of the electrolytic solution of a sodium ion secondary battery known in the art. For example, the electrolytic solution may be a carbonate-based solvent in which a sodium salt is dissolved at a predetermined concentration. Examples of the carbonate-based solvent include fluoroethylene carbonate (FEC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), and the like. Examples of the sodium salt include NaPF6 and the like.

[0048] 3.1.3 Conductive additives Examples of the conductive assistant that may be included in the positive electrode active material layer 10 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0049] 3.1.4 Binders Examples of binders that can be included in the positive electrode active material layer 10 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0050] 3.2 Electrolyte layer The electrolyte layer 20 contains at least an electrolyte. When the sodium ion secondary battery 100 is a solid-state battery (a battery containing a solid electrolyte, which may be a battery partially using a liquid electrolyte in combination, or an all-solid-state battery not containing a liquid electrolyte), the electrolyte layer 20 contains a solid electrolyte and may further contain a binder or the like. In this case, the content of the solid electrolyte and the binder or the like in the electrolyte layer 20 is not particularly limited. On the other hand, when the sodium ion secondary battery 100 is an electrolyte battery, the electrolyte layer 20 contains an electrolyte solution and may further have a separator or the like for holding the electrolyte solution and preventing contact between the positive electrode active material layer 10 and the negative electrode active material layer 30. The thickness of the electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0051] The electrolyte contained in the electrolyte layer 20 may be appropriately selected from those exemplified as electrolytes that may be contained in the positive electrode active material layer 10. The binder that may be contained in the electrolyte layer 20 may also be appropriately selected from those exemplified as binders that may be contained in the positive electrode active material layer 10. Each of the electrolytes and binders may be used alone or in combination of two or more. The separator may be any separator that is normally used in sodium ion secondary batteries, and examples of the separator include those made of resins such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multi-layer structure. Examples of the multi-layer separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.

[0052] 3.3 Negative electrode active material layer The negative electrode active material layer 30 includes at least a negative electrode active material, and may further include an electrolyte, a conductive assistant, a binder, and the like. Furthermore, the negative electrode active material layer 30 may further include various additives. The contents of the negative electrode active material, electrolyte, conductive assistant, binder, and the like in the negative electrode active material layer 30 may be appropriately determined according to the intended battery performance. For example, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire negative electrode active material layer 30 (total solid content) being 100 mass%. The shape of the negative electrode active material layer 30 is not particularly limited, and may be, for example, a sheet-like negative electrode active material layer having a substantially flat surface. The thickness of the negative electrode active material layer 30 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0053] As the negative electrode active material, various substances having a potential (charge / discharge potential) for absorbing and releasing sodium ions that is lower than that of the positive electrode active material of the present disclosure can be adopted. The negative electrode active material may be, for example, an inorganic negative electrode active material such as metallic sodium, an organic compound negative electrode active material, or a combination of these. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be a general shape as a negative electrode active material for a battery. For example, the negative electrode active material may be in a particulate form. The negative electrode active material particles may be primary particles, or may be secondary particles in which a plurality of primary particles are aggregated. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material may be in a sheet form (foil form, film form) such as sodium foil. That is, the negative electrode active material layer 30 may be made of a sheet of negative electrode active material.

[0054] Examples of the electrolyte that may be contained in the negative electrode active material layer 30 include the above-mentioned solid electrolyte, electrolytic solution, or a combination thereof. Examples of the conductive assistant that may be contained in the negative electrode active material layer 30 include the above-mentioned carbon material and metal material. The binder that may be contained in the negative electrode active material layer 30 may be appropriately selected from, for example, those exemplified as the binder that may be contained in the above-mentioned positive electrode active material layer 10. The electrolyte and the binder may each be used alone, or two or more types may be used in combination.

[0055] 3.4 Positive electrode current collector As shown in FIG. 2, the sodium ion secondary battery 100 may include a positive electrode collector 40 in contact with the positive electrode active material layer 10. The positive electrode collector 40 may be any of those generally used as a positive electrode collector for a battery. The positive electrode collector 40 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The positive electrode collector 40 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 40 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 40 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 40 may contain Al. The positive electrode collector 40 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. The positive electrode current collector 40 may be a metal foil or a substrate plated or vapor-deposited with the above metal. When the positive electrode current collector 40 is made of a plurality of metal foils, some layer may be present between the plurality of metal foils. The thickness of the positive electrode current collector 40 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0056] 3.5 Negative electrode current collector As shown in FIG. 2, the sodium ion secondary battery 100 may include a negative electrode current collector 50 in contact with the negative electrode active material layer 30. The negative electrode current collector 50 may be any of those commonly used as a negative electrode current collector for a battery. The negative electrode current collector 50 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The negative electrode current collector 50 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, the metal foil is excellent in terms of ease of handling. The negative electrode current collector 50 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 50 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring reduction resistance, the negative electrode current collector 50 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 50 may have some kind of coating layer on its surface for the purpose of adjusting the resistance, etc. Also, the negative electrode current collector 50 may be a metal foil or a base material on which the above-mentioned metal is plated or vapor-deposited. Also, when the negative electrode current collector 50 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 50 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0057] 3.6 Other matters In addition to the above configuration, the sodium ion secondary battery 100 may have obvious configurations as a secondary battery, such as tabs and terminals. The sodium ion secondary battery 100 may have each of the above configurations housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. In addition, a plurality of batteries 100 may be electrically connected in any way and stacked in any way to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The sodium ion secondary battery 100 may also have obvious configurations such as necessary terminals. The shape of the sodium ion secondary battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, or the like.

[0058] The sodium ion secondary battery 100 can be manufactured by applying a known method, except for using the above-mentioned specific positive electrode active material. For example, it can be manufactured as follows. However, the manufacturing method of the sodium ion secondary battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding or the like. (1) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The positive electrode layer slurry is applied to the surface of a positive electrode current collector using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector, thereby forming a positive electrode. (2) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The negative electrode layer slurry is applied to the surface of the negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, thereby forming a negative electrode. (3) The layers are laminated so that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order. Other members such as terminals are attached to the laminate as necessary. (4) The laminate is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to form a secondary battery. In the case of an electrolyte battery, the electrolyte may be impregnated in the negative electrode active material layer, the separator, and the positive electrode active material layer at the above step (3).

[0059] 4. Method for increasing the gravimetric energy density of sodium-ion secondary batteries The technology of the present disclosure also has an aspect of being a method for increasing the weight energy density of a sodium ion secondary battery. That is, the method of increasing the weight energy density of a sodium ion secondary battery of the present disclosure is characterized by using the above-mentioned positive electrode active material of the present disclosure in a positive electrode active material layer of the sodium ion secondary battery.

[0060] 5. Vehicles equipped with sodium-ion secondary batteries As described above, the positive electrode active material of the present disclosure has an excellent weight energy density and is suitable as a positive electrode active material for a sodium ion secondary battery. A sodium ion secondary battery having such a large weight energy density can be suitably used in at least one vehicle selected from, for example, a hybrid vehicle (HEV), a plug-in hybrid vehicle (PHEV) and an electric vehicle (BEV). That is, the technology of the present disclosure also has an aspect of a vehicle having a sodium ion secondary battery, the sodium ion secondary battery having a positive electrode active material layer, an electrolyte layer and a negative electrode active material layer, and the positive electrode active material layer containing the positive electrode active material of the present disclosure. EXAMPLES

[0061] As described above, one embodiment of the positive electrode active material and the sodium ion secondary battery has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0062] 1. Preparation of Positive Electrode Active Material 1.1 Example 1 1.1.1 Preparation of precursor (1) MnSO4·5H2O, NiSO4·6H2O, and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to obtain a concentration of 1.2 mol / L to obtain a first solution. In a separate container, Na2CO3 was dissolved in distilled water to obtain a concentration of 1.2 mol / L to obtain a second solution. (2) 1000 mL of pure water was placed in a reaction vessel (with a baffle plate), and 500 mL of the first solution and 500 mL of the second solution were each added dropwise at a rate of about 4 mL / min. (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and fine particles were removed by air classification to obtain precursor particles. The precursor particles were a composite salt containing Mn, Ni, and Co. The molar ratio of Mn, Ni, and Co in the precursor particles was Mn:Ni:Co=4:3:3.

[0063] 1.1.2 Preparation of the complex The precursor particles and Na2CO3 were mixed with Na 0.9 Mn 0.4 Ni 0.3 Co 0.3 The precursor and Na2CO3 were weighed out so as to obtain a composition for the O2 feed. The weighed precursor and Na2CO3 were mixed in a mortar to obtain a composite.

[0064] 1.1.3 Firing of the composite The composite was placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 900°C in 100 minutes. (5) The temperature in the heating furnace is kept at 900°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 900°C to 250°C in 120 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in a dry atmosphere outside the furnace until it reaches 25°C in 10 minutes.

[0065] The fired product after cooling in the air was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles having a P2 type structure.

[0066] 1.2 Example 2 The composition of the precursor particles and the ratio of the precursor particles to Na2CO3 were changed, and the other factors were the same as in Example 1. In Example 2, the molar ratio of Mn, Ni, and Co in the precursor particles was set to Mn:Ni:Co=5:3:2. In addition, the precursor particles and Na2CO3 were mixed in a mixture of Na 0.8 Mn 0.5 Ni 0.3 Co 0.2 It was weighed out so as to obtain the O2 charge composition.

[0067] 1.3 Example 3 The composition of the precursor particles and the ratio of the precursor particles to Na2CO3 were changed, and the other factors were the same as in Example 1. In Example 3, the molar ratio of Mn, Ni, and Co in the precursor particles was set to Mn:Ni:Co=4:2:4. In addition, the precursor particles and Na2CO3 were mixed in a mixture of Na 0.8 Mn 0.4 Ni 0.2 Co 0.4 It was weighed out so as to obtain the O2 charge composition.

[0068] 1.4 Comparative Example 1 The composition of the precursor particles and the ratio of the precursor particles to Na2CO3 were changed, and fine particles after air flow classification were used as the precursor particles. In Comparative Example 1, the molar ratio of Mn, Ni, and Co in the precursor particles was set to Mn:Ni:Co=5:2:3. The precursor particles and Na2CO3 were mixed with Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 It was weighed out so as to obtain the O2 charge composition.

[0069] 2. Evaluation of positive electrode active material 2.1 Elemental analysis Elemental analysis was carried out to identify the chemical composition of each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1. The results are shown in Table 1 below.

[0070] 2.2 Identification of crystal structure by X-ray diffraction measurement For each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1, X-ray diffraction measurements were performed using CuKα as a radiation source to obtain X-ray diffraction patterns. FIG. 3 shows the X-ray diffraction patterns of each of Examples 1 to 3. FIG. 4 shows the X-ray diffraction pattern of Comparative Example 1. As shown in FIGS. 3 and 4, it can be seen that all of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1 have a P2 type structure belonging to the space group P63mc. In addition, the lattice constants (a-axis length, b-axis length, c-axis length) of the P2 type structure of each of Examples 1 to 3 and Comparative Example 1 were obtained from each X-ray diffraction pattern. The results are shown in Table 1 below.

[0071] 2.3 Measurement of average particle size The average particle size (D50) was measured for each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1. The results are shown in Table 1 below.

[0072] 2.4 Measurement of average aspect ratio by SEM observation The positive electrode active materials of Examples 1 to 3 and Comparative Example 1 were each formed into a pellet, subjected to CP processing, and then cross-sections were observed by FE-SEM to measure the average aspect ratio. The results are shown in Table 1 below. For reference, FIG. 5 shows an SEM image of a cross-section of the positive electrode active material of Example 1 formed into a pellet. FIG. 6 shows the external appearance of the positive electrode active material of Example 1.

[0073] 3. Preparation of evaluation cells Coin cells were produced using the positive electrode active materials of each of Examples 1 to 3 and Comparative Example 1. The coin cells were produced as follows. (1) The positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were weighed out so that the mass ratio of the positive electrode active material:AB:PVdF=85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied onto an aluminum foil and vacuum dried overnight at 120°C to obtain a positive electrode, which is a laminate of a positive electrode active material layer and a positive electrode current collector. (2) The electrolyte used was a 1:1 volumetric mixture of EC and DEC in which NaPF6 was dissolved to a concentration of 1M. (3) Metallic sodium foil was prepared as the negative electrode. (4) A coin cell (CR2032) was prepared using the positive electrode, electrolyte, and negative electrode.

[0074] 4.Charge / Discharge Characteristics Evaluation The capacity of each of the coin cells of Examples 1 to 3 and Comparative Example 1 was measured by charging and discharging at 0.1 C (1 C = 160 mA / g) in a voltage range of 1.0 to 4.8 V in a thermostatic chamber maintained at 25° C. The results are shown in Table 1 below. (2) Each of the coin cells of Example 4 and Comparative Example 2 was charged and discharged at 0.1 C (1 C = 190 mA / g) in a voltage range of 1.0-4.3 V in a thermostatic chamber maintained at 25° C., and the initial discharge capacity, average discharge potential, and weight energy density were measured. The results are shown in Table 2 below.

[0075] 5. Evaluation Results For each of Examples 1 to 3 and Comparative Example 1, the chemical composition, average particle size (D50), average aspect ratio, and lattice constant of the positive electrode active material, as well as the initial discharge capacity, average discharge potential, and weight energy density of the evaluation cells are shown.

[0076] [Table 1]

[0077] [Table 2]

[0078] As is clear from the results shown in Tables 1 and 2, the positive electrode active materials according to Examples 1 to 3, which have a relatively large D50 of 2.0 μm or more and a relatively small average aspect ratio of 3.0 or less, have a superior weight energy density to the positive electrode active material according to Comparative Example 1, which has a relatively small D50 of less than 2.0 μm and a relatively large average aspect ratio of more than 3.0. In addition, the initial discharge capacity and average discharge potential of the positive electrode active materials according to Examples 1 to 3 are equal to or higher than those of Comparative Example 1.

[0079] Furthermore, as is clear from the results shown in Tables 1 and 2, the positive electrode active materials of Examples 1 to 3 having a predetermined chemical composition have a superior weight energy density to the positive electrode active material of Comparative Example 1 having a chemical composition different from that of Examples 1 to 3.

[0080] 6. Supplementary Information In the above examples, the precursor is obtained by coprecipitation, but the precursor can be obtained by other methods. In the above examples, the surface of the precursor is coated with a Na source by spray drying to obtain a composite, but the composite can be obtained by other methods. In the above examples, the Na-containing oxide having a P2 type structure is exemplified as having a predetermined chemical composition, but the chemical composition of the Na-containing oxide is not limited to this. The Na-containing oxide may be doped with an element M other than Mn, Ni, and Co. The element M is as described in the embodiment.

[0081] 7. Summary As described above, in a positive electrode active material containing a Na-containing oxide, if the Na-containing oxide satisfies the following requirements (1-1) to (1-4), it can be said that the energy density of the positive electrode active material is increased. (1-1) The Na-containing oxide particles have a P2 type structure. (1-2) The Na-containing oxide particles contain at least one element selected from the group consisting of Mn, Ni, and Co, Na, and O as constituent elements. (1-3) The Na-containing oxide particles have an average particle diameter of 2.0 μm or more. (1-4) The Na-containing oxide particles have an average aspect ratio of 1.0 or more and 3.0 or less.

[0082] Also, in the positive electrode active material containing the Na-containing oxide, when the Na-containing oxide satisfies the following requirements (2-1) and (2-2), it can be said that the energy density of the positive electrode active material increases. (2-1) The Na-containing oxide particles have a P2-type structure. (2-2) The Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0.70 < a ≤ 1.00, 0 < x < 1.00, 0 < y < 0.50, 0 < z < 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). It has a chemical composition represented by.

Explanation of symbols

[0083] 100 Sodium ion secondary battery 10 Positive electrode active material layer 20 Electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector

Claims

1. A positive electrode active material comprising Na-containing oxide particles, The Na-containing oxide particles have a P2 type structure, The Na-containing oxide particles contain, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O, The Na-containing oxide particles have an average particle size of 2.0 μm or more, The Na-containing oxide particles have an average aspect ratio of 1.0 or more and 3.0 or less. Cathode active material.

2. The positive electrode active material according to claim 1 , The Na-containing oxide particles contain, as a constituent element, more than 0.35 moles of Na per mole of O. Cathode active material.

3. The positive electrode active material according to claim 1 , The Na-containing oxide particles are a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Cathode active material.

4. The positive electrode active material according to claim 1 , The Na-containing oxide particles are a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Cathode active material.

5. The positive electrode active material according to claim 1 , The Na-containing oxide particles are a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0.70<a≦1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). Cathode active material.

6. A positive electrode active material comprising Na-containing oxide particles, The Na-containing oxide particles have a P2 type structure, The Na-containing oxide particles are a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0.70<a≦1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Cathode active material.

7. The positive electrode active material according to claim 6, The Na-containing oxide particles are a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0.70<a≦1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). Cathode active material.

8. The positive electrode active material according to any one of claims 1 to 7, The P2 type structure has a c-axis length of 11.10 Å or less. Cathode active material.

9. A sodium ion secondary battery, A positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 7. Sodium ion secondary battery.

Citation Information

Patent Citations

  • Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery

    CN108565457A

  • Spherical-like sodium ion battery positive electrode material, preparation method thereof and sodium ion battery

    CN115000399A

  • Complex metal oxide, positive electrode active material for sodium secondary battery, positive electrode for sodium secondary battery, and the sodium secondary battery

    JP2012201588A

  • Control method of sodium ion secondary battery, controller for sodium ion secondary battery, and sodium ion secondary battery for use in control method or controller for sodium ion secondary battery

    JP2017045600A

  • Positive electrode active material for sodium ion secondary battery and manufacturing method of the same, and sodium ion secondary battery

    JP2018137122A