Resin composition for etching mask pattern formation and method for manufacturing etching mask pattern

A resin composition with a block copolymer having specific block structures addresses the challenge of forming vertically aligned phase-separated structures with fine patterns and high-temperature annealing, achieving defect-free etching mask patterns for semiconductor manufacturing.

JP2024158543APending Publication Date: 2024-11-08TOKYO OHKA KOGYO CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023073814
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods struggle to form phase-separated structures with vertical alignment and fine patterns using block copolymers, especially when the period (L0) is less than 20 nm and high-temperature annealing is required, leading to defects such as adhesion of foreign matter and uneven patterns.

Method used

A resin composition containing a block copolymer with specific block structures, including a first block composed of a polymer with general formula (b1) and a second block composed of block 2M and block 2G, which allows for phase separation and vertical alignment even at high temperatures, forming an etching mask pattern with a period less than 20 nm.

Benefits of technology

The method achieves excellent vertical alignment and suppresses defects in the phase-separated structure, enabling the formation of a high-quality etching mask pattern suitable for fine features in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158543000001_ABST
    Figure 2024158543000001_ABST
Patent Text Reader

Abstract

To provide a resin composition for etching mask pattern formation and a method for manufacturing an etching mask pattern which can obtain a phase separation structure that has a period (L0) of less than 20 nm and is excellent in vertical orientation even when being subjected to high temperature annealing.SOLUTION: A method for manufacturing an etching mask pattern includes the steps of: coating a resin composition for etching mask pattern formation onto a support, and forming a block copolymer layer having film thickness of 25 nm or more; and phase-separating the block copolymer layer. A resin composition for etching mask pattern formation contains a block copolymer having a first block and a second block, the first block is composed of a structure of general formula (b1), and the second block is composed of a block 2M of a structure of general formula (b2m), and a block 2G of a structure of general formula (b2g).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for forming an etching mask pattern, and a method for producing an etching mask pattern. [Background technology]

[0002] In recent years, with the further miniaturization of large-scale integrated circuits (LSIs), there is a demand for technology to process more delicate structures. In response to such demands, technology is being developed to form finer patterns by utilizing a phase-separated structure formed by the self-organization of a block copolymer in which mutually incompatible blocks are bonded together (see, for example, Patent Document 1). In order to utilize the phase separation structure of a block copolymer, it is essential to form the self-organized nanostructure formed by microphase separation only in a specific region and to align it in a desired direction. To achieve this position control and orientation control, processes such as graphoepitaxy, which controls the phase separation pattern by a guide pattern, and chemical epitaxy, which controls the phase separation pattern by differences in the chemical state of the substrate, have been proposed (see, for example, Non-Patent Document 1).

[0003] Block copolymers form structures with regular periodic structures through phase separation. The "period of the structure" refers to the period of the phase structure observed when a phase-separated structure is formed, and refers to the sum of the lengths of each phase that is incompatible with each other. When the phase-separated structure forms a cylindrical structure perpendicular to the substrate surface, the period (L0) of the structure is the center-to-center distance (pitch) between two adjacent cylindrical structures.

[0004] It is known that the period of the structure (L0) is determined by the degree of polymerization N and the intrinsic polymerization properties such as the Flory-Huggins interaction parameter χ. In other words, the larger the product of χ and N, χ·N, the greater the mutual repulsion between different blocks in the block copolymer. Therefore, when χ·N>10.5 (hereinafter referred to as the "strength separation limit"), the repulsion between different types of blocks in the block copolymer is large, and phase separation is more likely to occur. At the strength separation limit, the period of the structure is approximately N 2 / 3 χ 1 / 6 Thus, the relationship of the following formula (1) is established. In other words, the period of the structure is proportional to the degree of polymerization N, which correlates with the molecular weight and the molecular weight ratio between different blocks.

[0005] L0 ∝ a N 2 / 3 χ 1 / 6 (1) [In the formula, L0 represents the period of the structure, a represents a parameter indicating the size of the monomer, N represents the degree of polymerization, and χ represents an interaction parameter, and the larger this value is, the higher the phase separation performance is.]

[0006] Therefore, the period (L0) of the structure can be adjusted by adjusting the composition and total molecular weight of the block copolymer. It is known that the periodic structure formed by block copolymers changes from cylinders (columnar), lamellae (plates), to spheres (spherical) depending on the volume ratio of the polymer components, and the period depends on the molecular weight. Therefore, in order to form a structure with a relatively large period (L0) by utilizing the phase-separated structure formed by the self-organization of block copolymers, a method of increasing the molecular weight of the block copolymer can be considered.

[0007] In addition, a method using a block copolymer having a larger interaction parameter (χ) than a block copolymer having a styrene block and a methyl methacrylate block, which is a general-purpose block copolymer, is also considered. For example, Patent Document 2 proposes a block copolymer in which a substituent is introduced into a part of the methyl methacrylate block. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2008-36491 A [Patent Document 2] Patent Publication No. 2022-020519 [Non-patent literature]

[0009] [Non-Patent Document 1] Proceedings of SPIE, Vol. 7637, No. 76370G-1 (2010). Summary of the Invention [Problem to be solved by the invention]

[0010] The phase-separated structure formed by the self-organization of the block copolymer can be used to form an etching mask pattern. In this case, it is preferable to vertically align the phase-separated structure with a relatively large film thickness (for example, a film thickness of 25 nm or more).

[0011] In order to form a phase-separated structure having a finer pattern, it is preferable that the period (L0) of the phase-separated structure is smaller and that the phase-separated structure has a vertical alignment. However, when the period (L0) of the block copolymer described in Patent Document 2 is small (for example, less than 20 nm), it becomes difficult to form a phase-separated structure having a vertical alignment.

[0012] In order to obtain a highly accurate structure, it is necessary to suppress the occurrence of defects (surface defects). The term "defect" refers to all defects that are detected when observing a phase separation pattern from directly above using a scanning electron microscope or the like. The defects include, for example, defects caused by adhesion of foreign matter or precipitates to the surface of a phase separation pattern, such as scum (resin composition residue), bubbles, and dust, after the formation of a phase separation pattern, defects related to the pattern shape, such as bridges between line patterns and filling of holes in a contact hole pattern, and color unevenness of the pattern.

[0013] The above-mentioned phase-separated structure can be obtained by annealing the block copolymer applied to a substrate or the like. In general, in order to suppress the occurrence of defects in the phase-separated pattern, it is preferable to set the annealing temperature high. However, when the annealing temperature is high (e.g., 290°C) for the block copolymer described in Patent Document 2, it becomes difficult to form a phase-separated structure having vertical alignment.

[0014] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a resin composition for forming an etching mask pattern, which has a period (L0) of less than 20 nm and can give a phase-separated structure with excellent vertical alignment even when subjected to high-temperature annealing, and a method for producing an etching mask pattern using the same. [Means for solving the problem]

[0015] A first aspect of the present invention is a method for producing an etching mask pattern, comprising the steps of: applying a resin composition for forming an etching mask pattern onto a support to form a layer containing a block copolymer having a thickness of 25 nm or more; and phase-separating the layer containing the block copolymer, wherein the resin composition for forming an etching mask pattern contains a block copolymer having a first block and a second block, the first block being composed of a polymer consisting of a repeating structure of a structural unit represented by the following general formula (b1), and the second block being composed of a block 2M consisting of a polymer consisting of a repeating structure of a structural unit represented by the following general formula (b2m), and a block 2G consisting of a polymer consisting of a repeating structure of a structural unit represented by the following general formula (b2g).

[0016] [ka] [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. R b1 is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. x, y, and z represent molar ratios. x+y+z=100 mol %. y / (y+z) is 0.01 or more and 0.11 or less. x is 20 to 80 mol %.]

[0017] A second aspect of the present invention is a resin composition for forming an etching mask pattern, which contains a block copolymer having a first block and a second block, wherein the first block is composed of a polymer consisting of a repeating structure of a structural unit represented by the following general formula (b1), and the second block is composed of a block 2M consisting of a polymer consisting of a repeating structure of a structural unit represented by the following general formula (b2m), and a block 2G consisting of a polymer consisting of a repeating structure of a structural unit represented by the following general formula (b2g).

[0018] [ka] [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. R b1 is a hydrogen atom or a methyl group. 2 R is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphate group. 3 is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. b2 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. x, y, and z represent a molar ratio. x+y+z=100 mol %. y / (y+z) is 0.01 or more and 0.11 or less. x is 20 to 80 mol %.] Effect of the Invention

[0019] According to the present invention, it is possible to provide a resin composition for forming an etching mask pattern, which has excellent vertical alignment even in a thick film, and a method for producing an etching mask pattern using the same. [Brief description of the drawings]

[0020] [Figure 1]1A to 1C are schematic process diagrams illustrating an embodiment of a method for producing an etching mask pattern. [Diagram 2] FIG. 13 is a diagram illustrating an embodiment of an optional step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] In this specification and claims, the term "aliphatic" is a relative concept to aromaticity and is defined as meaning a group, compound, etc. that does not have aromaticity. Unless otherwise specified, the term "alkyl group" includes linear, branched and cyclic monovalent saturated hydrocarbon groups. The same applies to the alkyl group in an alkoxy group. Unless otherwise specified, the term "alkylene group" includes linear, branched and cyclic divalent saturated hydrocarbon groups. The term "halogenated alkyl group" refers to an alkyl group in which some or all of the hydrogen atoms have been substituted with halogen atoms, and examples of the halogen atoms include fluorine, chlorine, bromine and iodine atoms. The term "fluorinated alkyl group" or "fluorinated alkylene group" refers to an alkyl group or alkylene group in which some or all of the hydrogen atoms have been substituted with fluorine atoms. The term "structural unit" refers to a monomer unit that constitutes a polymeric compound (resin, polymer, copolymer). The phrase "optionally has a substituent" includes both the case where a hydrogen atom (-H) is replaced with a monovalent group and the case where a methylene group (-CH2-) is replaced with a divalent group. The term "exposure" is intended to include any concept including irradiation with radiation. Unless otherwise specified, the "α-position (carbon atom at the α-position)" refers to the carbon atom to which the side chain of the block copolymer is bonded. The "α-position carbon atom" of a methyl methacrylate unit refers to the carbon atom to which the carbonyl group of methacrylic acid is bonded. The "α-position carbon atom" of a styrene unit refers to the carbon atom to which a benzene ring is bonded. "Number average molecular weight" (Mn) is the number average molecular weight measured by size exclusion chromatography in terms of standard polystyrene unless otherwise specified. "Weight average molecular weight" (Mw) is the weight average molecular weight measured by size exclusion chromatography in terms of standard polystyrene unless otherwise specified. The value of Mn or Mw is expressed in units (gmol - ) indicates the molar mass. In the present specification and claims, some structures represented by chemical formulas may have asymmetric carbons and may have enantiomers or diastereomers, in which case a single formula represents all the isomers. These isomers may be used alone or as a mixture.

[0022] (Method of manufacturing an etching mask pattern) The method for producing an etching mask pattern of the present embodiment includes a step of applying the resin composition for forming an etching mask pattern of the above-described embodiment onto a support to form a layer containing a block copolymer (hereinafter referred to as "step (i)"); a step of phase-separating the layer containing the block copolymer (hereinafter referred to as "step (ii)"); and a step of selectively removing, from the BCP layer 3, a phase consisting of at least one type of block of the first block and the second block constituting the (BCP) component (hereinafter referred to as "step (iii)"). Hereinafter, such a method for producing an etching mask pattern will be specifically described with reference to Fig. 1. However, the present invention is not limited to this.

[0023] FIG. 1 shows an embodiment of a method for producing an etching mask pattern. In the embodiment shown in FIG. 1, first, a primer is applied onto a support 1 to form a primer layer 2 (FIG. 1(I)). Next, the resin composition for forming an etching mask pattern of the above-mentioned embodiment is applied onto the undercoat agent layer 2 to form a layer containing a block copolymer (BCP layer) 3 (FIG. 1(II); this is step (i)). Next, an annealing treatment is performed by heating, so that the BCP layer 3 is separated into a phase 3a and a phase 3b (FIG. 1(III); step (ii)). As a result, a structure 3' including a phase-separated structure is produced on the support 1 on which the undercoat agent layer 2 has been formed. The structure 3' including a phase-separated structure can be used to produce an etching mask pattern. In addition, the "first block" and the "second block" in the resin composition for forming an etching mask pattern described below may be referred to as "block (b1)" and "block (b2)", respectively.

[0024] [Process (i)] In the step (i), a resin composition for forming an etching mask pattern is applied onto a support 1 to form a BCP layer 3 having a thickness of 25 nm or more. In the embodiment shown in FIG. 1, first, a base agent is applied onto a support 1 to form a base agent layer 2 . By providing the undercoat agent layer 2 on the support 1, a balance of hydrophilicity and hydrophobicity between the surface of the support 1 and the layer (BCP layer) 3 containing a block copolymer can be achieved. That is, when the primer layer 2 contains a resin component having the structural units constituting the block (b1), the adhesion between the phase of the BCP layer 3 consisting of the block (b1) and the support 1 is enhanced. When the primer layer 2 contains a resin component having the structural units constituting the block (b2), the adhesion between the phase of the BCP layer 3 consisting of the block (b2) and the support 1 is enhanced. As a result, due to phase separation of the BCP layer 3, cylindrical structures and lamellar structures oriented in the direction perpendicular to the surface of the support 1 are easily formed.

[0025] [Step (ii)] In step (ii), the BCP layer 3 formed on the support 1 is subjected to phase separation. By heating the support 1 after step (i) and performing an annealing treatment, the block copolymer is selectively removed to form a phase-separated structure that exposes at least a part of the surface of the support 1. That is, a structure 3' including a phase-separated structure separated into a phase 3a and a phase 3b is produced on the support 1. The temperature condition of the annealing treatment is preferably equal to or higher than the glass transition temperature of the (BCP) component used and lower than the thermal decomposition temperature, and when the block copolymer is, for example, a polystyrene-polymethyl methacrylate (PS-PMMA) block copolymer (mass average molecular weight 5000 to 100000), the temperature is preferably 250 to 300° C., more preferably 260 to 295° C., and particularly preferably 270 to 290° C. The heating time is preferably 30 to 3600 seconds. Moreover, the annealing process is preferably carried out in a gas with low reactivity, such as nitrogen.

[0026] [Step (iii)] In the step (iii), a phase of at least one of the first and second blocks constituting the (BCP) component in the structure 3' is selectively removed, thereby forming an etching mask pattern.

[0027] As a method for selectively removing a phase consisting of any one of the blocks, a method for subjecting the BCP layer to an oxygen plasma treatment, a method for subjecting the BCP layer to a hydrogen plasma treatment, or the like can be mentioned. For example, after phase separation of a BCP layer containing the (BCP) component, the BCP layer is subjected to oxygen plasma treatment, hydrogen plasma treatment, or the like, whereby the phase consisting of the first block is not selectively removed, but the phase consisting of the second block is selectively removed.

[0028] FIG. 2 shows an example embodiment of step (iii). In the embodiment shown in Figure 2, the structure 3' produced on the support 1 in step (ii) is subjected to an oxygen plasma treatment to selectively remove the phase 3a and form an etching mask pattern consisting of spaced apart phases 3b, where phase 3b is the phase consisting of the first block and phase 3a is the phase consisting of the second block.

[0029] The etching mask pattern obtained as described above can be used as is for etching a support, but by further heating it, the shape of the etching mask pattern on the support 1 can also be changed. The heating temperature is preferably equal to or higher than the glass transition temperature of the block copolymer used and lower than its thermal decomposition temperature, and is preferably carried out in a gas with low reactivity such as nitrogen.

[0030] In the method for producing an etching mask pattern of this embodiment, a phase-separated structure having a period (L0) of less than 20 nm and excellent vertical alignment even after high-temperature annealing can be obtained by using the following resin composition for forming an etching mask pattern. Hereinafter, this resin composition for forming an etching mask pattern will be described in detail.

[0031] [Resin composition for forming etching mask pattern] The resin composition for forming an etching mask pattern of this embodiment contains a block copolymer having a first block and a second block. The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1). The second block is composed of a block 2M composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b2m), and a block 2G composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b2g).

[0032] [ka] [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. R b1 is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. x, y, and z represent molar ratios. x+y+z=100 mol %. y / (y+z) is 0.01 or more and 0.11 or less. x is 20 to 80 mol %.]

[0033] <Block copolymer (BCP) component> A block copolymer is a polymer in which multiple types of blocks (partial constituent components in which the same type of structural unit is repeatedly bonded) are bonded together. The blocks constituting a block copolymer may be of two types, or three or more types. The block copolymer in this embodiment (hereinafter also referred to as "(BCP) component") has a first block and a second block.

[0034] <First Block> The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1) (hereinafter, also referred to as structural unit (b1)).

[0035] [ka] [In the formula, R 1 R is an alkyl group which may have an oxygen atom or a silicon atom. b1 is a hydrogen atom or a methyl group. n is an integer of 0 to 5. When n is an integer of 2 or more, multiple R 1 may be the same or different.

[0036] In the formula (b1), R 1R is an alkyl group which may have an oxygen atom or a silicon atom. The alkyl group preferably has 1 to 5 carbon atoms, more preferably has 1 to 4 carbon atoms, even more preferably has 1 to 3 carbon atoms, and is further preferably an ethyl group or a methyl group. 1 is particularly preferably a methyl group.

[0037] In the formula (b1), R b1 is a hydrogen atom or a methyl group. In the formula (b1), n ​​is preferably an integer of 0 to 3, more preferably an integer of 0 to 2, and further preferably 0 or 1.

[0038] <Second Block> The second block is composed of block 2M and block 2G. Block 2M is composed of a polymer composed of a repeating structure of a structural unit represented by the following general formula (b2m) (hereinafter also referred to as structural unit (b2m)). Block 2G is composed of a polymer composed of a repeating structure of a structural unit represented by the following general formula (b2g) (hereinafter also referred to as structural unit (b2g)).

[0039] [ka] [In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms.]

[0040] (B2M) The structural unit (b2m) is a structural unit represented by the above general formula (b2m). In the above formula (b2m), R b2R is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 The alkyl group having 1 to 5 carbon atoms is preferably a linear or branched alkyl group having 1 to 5 carbon atoms, and specific examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, an isopentyl group, and a neopentyl group. The halogenated alkyl group having 1 to 5 carbon atoms is a group in which some or all of the hydrogen atoms of the alkyl group having 1 to 5 carbon atoms are substituted with halogen atoms. As the halogen atom, a fluorine atom is particularly preferable. R b2 is preferably a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a fluorinated alkyl group having 1 to 5 carbon atoms, and from the viewpoint of industrial availability, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.

[0041] (B2G) The structural unit (b2g) is a structural unit represented by the above general formula (b2g).

[0042] In the above formula (b2g), R b2 R is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 is R in the above formula (b2m). b2 is the same as:

[0043] In the above formula (b2g), R 2is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. The alkyl group is preferably a linear or branched alkyl group, more preferably a linear alkyl group. When the alkyl group is linear, the number of carbon atoms may be 1 or more, but the number of carbon atoms is preferably 2 or more. The upper limit of the number of carbon atoms of the linear alkylene group is not particularly limited, but from the viewpoint of phase separation performance, the number of carbon atoms is preferably 15 or less, more preferably 10 or less, even more preferably 8 or less, even more preferably 6 or less, and particularly preferably 5 or less. When the alkyl group is branched, the number of carbon atoms may be 3 or more. The upper limit of the number of carbon atoms of the branched alkyl group is not particularly limited, but from the viewpoint of phase separation performance, the number of carbon atoms is preferably 15 or less, more preferably 10 or less, even more preferably 8 or less, even more preferably 6 or less, and particularly preferably 5 or less. The alkyl group preferably has 2 to 15 carbon atoms, more preferably 2 to 10 carbon atoms, even more preferably 2 to 8 carbon atoms, still more preferably 2 to 6 carbon atoms, and particularly preferably 2 to 5 carbon atoms. R 2 The alkyl group is preferably a linear alkyl group having 2 to 5 carbon atoms.

[0044] R 2 The alkyl group of R may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphoric acid group. 2 When the alkyl group has a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphoric acid group, the fluorine atom, the carboxy group, the amino group, the cyano group, the hydroxy group, or the phosphoric acid group may be a substituent that replaces a hydrogen atom of the alkyl group. The number of hydrogen atoms replaced by the group is not particularly limited, but is preferably 1 to 3. R 2When the alkyl group has a silicon atom, the silicon atom may be a substituent that replaces a methylene group (-CH2-) in the alkyl group. The number of methylene groups substituted with silicon atoms is not particularly limited, but is preferably 1. R 2 is preferably an alkyl group which may be substituted with an alkylsilyl group, a fluoromethyl group, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphate group. The alkyl group in the alkylsilyl group preferably has 1 to 3 carbon atoms, more preferably has 1 or 2 carbon atoms. The alkylsilyl group is preferably a trialkylsilyl group, more preferably a triethylsilyl group or a trimethylsilyl group, and even more preferably a trimethylsilyl group. The fluoromethyl group is preferably a trifluoromethyl group.

[0045] R 2 Preferred examples are shown below, but are not limited to these: In the following formula, * represents a bond bonded to the sulfur atom (S) in the above formula (b2g).

[0046] [ka] [In the formula, Y 2 is a linear or branched alkylene group having 1 to 15 carbon atoms.]

[0047] In the above formulas (r2-1) to (r2-8), Y 2 is a linear or branched alkylene group having 1 to 15 carbon atoms. When the alkylene group is linear, it more preferably has 1 to 10 carbon atoms, even more preferably has 1 to 8 carbon atoms, and particularly preferably has 1 to 5 carbon atoms. When the alkylene group is branched, it more preferably has 2 to 10 carbon atoms, even more preferably has 2 to 8 carbon atoms, and particularly preferably has 2 to 5 carbon atoms. Y 2 The alkylene group is preferably a linear alkylene group having 1 to 5 carbon atoms.

[0048] R 2Specific examples of are shown below, but are not limited to these. In the following formula, * represents a bond bonded to the sulfur atom (S) in the above formula (b2g). [ka] [In the formula, q is an integer of 1 to 15.]

[0049] In the above formula, q is preferably an integer of 1 to 10, more preferably an integer of 1 to 8, further preferably an integer of 1 to 6, and particularly preferably an integer of 1 to 5.

[0050] In the above formula (b2g), R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms, which may have a hydroxyl group. When the alkylene group is linear, the number of carbon atoms may be 1 or more, but preferably 3 or more. The upper limit of the number of carbon atoms of the linear alkylene group is preferably 8 or less, more preferably 5 or less, and even more preferably 4 or less, from the viewpoint of phase separation performance. The number of carbon atoms of the linear alkylene group is particularly preferably 3. When the alkylene group is branched, the number of carbon atoms may be 3 or more, but preferably 4 or more. The upper limit of the number of carbon atoms of the branched alkylene group is preferably 8 or less, more preferably 5 or less, from the viewpoint of phase separation performance. The number of carbon atoms of the alkyl group is preferably 3 to 10, more preferably 3 to 8, even more preferably 3 to 5, even more preferably 3 to 4, and especially preferably 3. R 3 The alkylene group is preferably a linear alkylene group having 3 carbon atoms.

[0051] R 3 The alkylene group may have a hydroxy group. The hydroxy group may be a substituent that replaces a hydrogen atom of the alkylene group. The number of hydrogen atoms replaced by the hydroxy group is not particularly limited, but is preferably 1 to 3, more preferably 1 or 2, and even more preferably 1.

[0052] The structural unit (b2g) is preferably a structural unit represented by general formula (b2g-1) shown below.

[0053] [ka] [In the formula, R 4 is a hydrogen atom or a hydroxyl group. 1 and k 2 R is each independently an integer of 1 to 5. b2 and R 2 is R in the above formula (b2g). b2 and R 2 is the same as:

[0054] In the above formula (b2g-1), R b2 and R 2 is R in the above formula (b2g). b2 and R 2 Same as R 2 is preferably one represented by the above formulas (r2-1) to (r2-8), and more preferably one represented by (r2-9) to (r2-16).

[0055] In the above formula (b2g-1), R 4 is a hydrogen atom or a hydroxy group.

[0056] In the formula (b2g-1), k1 and k2 each independently represent an integer of 1 to 5. k1 and k2 each preferably represent an integer of 1 to 3, more preferably 1 or 2, and further preferably 1.

[0057] Specific examples of the structural unit (b2g) are shown below, but are not limited to these. In the following formula, R represents a methyl group or a hydrogen atom, and a methyl group is preferable.

[0058] [ka]

[0059] [ka]

[0060] In the formula (b1), (b2g) and (b2m), x, y and z represent a molar ratio, where x+y+z=100 mol %, and y / (y+z) is 0.01 or more and 0.11 or less.

[0061] x is preferably 20 to 80 mol %, more preferably 25 to 75 mol %, and even more preferably 30 to 70 mol %. When x is within the above range, a phase-separated structure having a period (L0) of less than 20 nm and excellent vertical alignment even when high-temperature annealing is performed is easily obtained.

[0062] y is preferably 0.5 to 8 mol%, more preferably 1 to 7 mol%, and even more preferably 1.5 to 6 mol%. When y is within the above range, a phase-separated structure having a period (L0) of less than 20 nm and excellent vertical alignment even when high-temperature annealing is performed is easily obtained.

[0063] z is preferably 10 to 70 mol %, more preferably 15 to 65 mol %, and even more preferably 20 to 60 mol %. When z is within the above range, a phase-separated structure having a period (L0) of less than 20 nm and excellent vertical alignment even when high-temperature annealing is performed is easily obtained.

[0064] y / (y+z) is preferably 0.02 or more, more preferably 0.03 or more, even more preferably 0.04 or more, particularly preferably 0.05 or more, and most preferably 0.06 or more. y / (y+z) is preferably 0.109 or less, more preferably 0.105 or less, even more preferably 0.103 or less, and particularly preferably 0.100 or less. When y / (y+z) is within the above range, the period (L0) is less than 20 nm, and a phase-separated structure that is excellent in vertical alignment even when high-temperature annealing is performed is easily obtained.

[0065] The (BCP) component may have other blocks in addition to the first block and the second block. In a preferred embodiment, the (BCP) component is a block copolymer composed of a first block and a second block.

[0066] The number average molecular weight (Mn) of the (BCP) component (based on polystyrene conversion by size exclusion chromatography) is not particularly limited, but is preferably 5,000 to 100,000, more preferably 10,000 to 80,000, still more preferably 15,000 to 70,000, particularly preferably 15,000 to 5,000, and most preferably 20,000 to 35,000. The molecular weight dispersity (Mw / Mn) of each block constituting the (BCP) component is preferably from 1.0 to 1.5, more preferably from 1.0 to 1.4, and even more preferably from 1.0 to 1.3.

[0067] <Organic solvent components> The above-mentioned resin composition for forming an etching mask pattern can be prepared by dissolving the above-mentioned (BCP) component in an organic solvent component. The organic solvent component may be any solvent capable of dissolving each component used to form a homogeneous solution, and any solvent known in the art as a solvent for film compositions mainly composed of resins may be used.

[0068] Examples of the organic solvent component include lactones such as γ-butyrolactone; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl-n-pentyl ketone, methyl isopentyl ketone, and 2-heptanone; polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol; compounds having an ester bond such as ethylene glycol monoacetate, diethylene glycol monoacetate, propylene glycol monoacetate, and dipropylene glycol monoacetate; and ether bonds such as monoalkyl ethers, monomethyl ether, monoethyl ether, monopropyl ether, and monobutyl ether of the polyhydric alcohols or the compounds having an ester bond, or monophenyl ether. derivatives of polyhydric alcohols such as compounds having a bond [among which, propylene glycol monomethyl ether acetate (PGMEA) and propylene glycol monomethyl ether (PGME) are preferred]; cyclic ethers such as dioxane, esters such as methyl lactate, ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, and ethyl ethoxypropionate; and aromatic organic solvents such as anisole, ethyl benzyl ether, cresyl methyl ether, diphenyl ether, dibenzyl ether, phenetole, butyl phenyl ether, ethylbenzene, diethylbenzene, pentylbenzene, isopropylbenzene, toluene, xylene, cymene, and mesitylene. The organic solvent component may be used alone or in a mixture of two or more kinds. Among them, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone, and EL are preferred.

[0069] A mixed solvent obtained by mixing PGMEA and a polar solvent is also preferred. The mixing ratio (mass ratio) may be appropriately determined in consideration of the compatibility between PGMEA and the polar solvent, and is preferably within a range of 1:9 to 9:1, and more preferably 2:8 to 8:2. For example, when EL is blended as the polar solvent, the mass ratio of PGMEA:EL is preferably 1:9 to 9:1, more preferably 2:8 to 8:2. When PGME is blended as the polar solvent, the mass ratio of PGMEA:PGME is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3. When PGME and cyclohexanone are blended as the polar solvent, the mass ratio of PGMEA:(PGME+cyclohexanone) is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3.

[0070] As the organic solvent component in the resin composition for forming an etching mask pattern, a mixed solvent of PGMEA or EL, or a mixed solvent of the PGMEA and a polar solvent, and γ-butyrolactone is also preferred. In this case, the mass ratio of the former to the latter is preferably 70:30 to 95:5. The organic solvent component contained in the resin composition for forming an etching mask pattern is not particularly limited, and is appropriately set at a coatable concentration according to the coating film thickness, and is generally used so that the solid content concentration is within the range of 0.2 to 70 mass %, preferably 0.2 to 50 mass %.

[0071] <Optional ingredients> In addition to the (BCP) component and organic solvent component, the above-mentioned resin composition for forming an etching mask pattern may further contain, as desired, miscible additives such as an additional resin for improving the performance of the layer, a surfactant for improving coatability, a dissolution inhibitor, a plasticizer, a stabilizer, a colorant, an antihalation agent, a dye, a sensitizer, a base amplifier, a basic compound, and the like.

[0072] Primer: As the undercoat agent, a resin composition containing a resin component can be used. The resin component for the undercoat agent can be appropriately selected from among conventionally known resin components used for thin film formation, depending on the type of block constituting the (BCP) component. The resin component for the undercoat agent may be, for example, a thermally polymerizable resin, or may be a photosensitive resin contained in a positive resist composition or a negative resist composition. In addition, a compound may be used as a surface treatment agent, and a non-polymerizable film formed by applying the compound may be used as the undercoat agent layer. For example, a siloxane-based organic monomolecular film formed using phenethyltrichlorosilane, octadecyltrichlorosilane, hexamethyldisilazane, or the like as a surface treatment agent may also be suitably used as the undercoat agent layer.

[0073] Examples of such a resin component include a resin containing a resin having both of the structural units constituting each of the blocks (b1) and (b2), and a resin having both of the structural units having high affinity with each of the blocks constituting the (BCP) component.

[0074] As the resin component for the primer, it is preferable to use, for example, a compound or resin that contains both a portion that has a high affinity for styrene, such as an aromatic ring, and a portion that has a high affinity for methyl methacrylate (such as a highly polar functional group). An example of a resin component that includes both a site with high affinity for styrene and a site with high affinity for methyl methacrylate is a resin obtained by polymerizing at least a monomer having an aromatic ring and a monomer having a highly polar functional group. Examples of monomers having an aromatic ring include monomers having aryl groups in which one hydrogen atom has been removed from an aromatic hydrocarbon ring, such as a phenyl group, a biphenyl group, a fluorenyl group, a naphthyl group, an anthryl group, or a phenanthryl group, or monomers having heteroaryl groups in which a part of the carbon atoms constituting the ring of these groups is substituted with a heteroatom such as an oxygen atom, a sulfur atom, or a nitrogen atom. Examples of monomers having a highly polar functional group include monomers having a trimethoxysilyl group, a trichlorosilyl group, an epoxy group, a glycidyl group, a carboxy group, a hydroxyl group, a cyano group, or a hydroxyalkyl group in which a part of the hydrogen atoms of an alkyl group is substituted with a hydroxyl group. Other examples of compounds that contain both a moiety with high affinity for styrene and a moiety with high affinity for methyl methacrylate include compounds that contain both an aryl group and a highly polar functional group, such as phenethyltrichlorosilane, and compounds that contain both an alkyl group and a highly polar functional group, such as alkylsilane compounds.

[0075] Examples of the resin component for the base agent include a resin having both styrene and methyl methacrylate as structural units, and a resin having all of styrene, methyl methacrylate, and (hydroxyethyl) methacrylate as structural units.

[0076] When the resin composition for the base agent has two or more different types of constituent units, examples of the resin include a random copolymer, an alternating polymer of styrene and methyl methacrylate (in which each monomer is copolymerized alternately), and the like.

[0077] The primer can be prepared by dissolving the above-mentioned resin components in a solvent. Such a solvent may be any solvent capable of dissolving each component used to form a homogeneous solution, and examples thereof include the same organic solvent components as those exemplified in the description of the resin composition for forming an etching mask pattern of the above embodiment.

[0078] The type of the support 1 is not particularly limited as long as the resin composition can be applied to the surface thereof. For example, substrates made of inorganic substances such as metals (silicon, copper, chromium, iron, aluminum, etc.), glass, titanium oxide, silica, and mica; substrates made of oxides such as SiO2; substrates made of nitrides such as SiN; substrates made of oxynitrides such as SiON; and substrates made of organic substances such as acrylic, polystyrene, cellulose, cellulose acetate, and phenolic resin. Among these, metal substrates are preferred, and for example, silicon substrates (Si substrates) or copper substrates (Cu substrates) are likely to form structures with vertically oriented cylinder structures and lamellar structures. Among these, Si substrates are particularly preferred. The size and shape of the support 1 are not particularly limited. The support 1 does not necessarily have to have a smooth surface, and substrates of various shapes can be appropriately selected. For example, substrates having a curved surface, flat plates with an uneven surface, and substrates having a flaky shape can be mentioned.

[0079] The surface of the support 1 may be provided with an inorganic and / or organic film. Examples of inorganic films include inorganic anti-reflective coatings (inorganic BARCs). Examples of organic films include organic anti-reflective coatings (organic BARCs). The inorganic film can be formed, for example, by applying an inorganic anti-reflective coating composition, such as a silicon-based material, onto a support and baking the composition. The organic film can be formed, for example, by applying an organic film-forming material, which is a resin component that constitutes the film, dissolved in an organic solvent, onto a substrate using a spinner or the like, and baking the material at a temperature of preferably 200 to 300° C., preferably for 30 to 300 seconds, more preferably for 60 to 180 seconds. This organic film-forming material does not necessarily need to be sensitive to light or electron beams, as in the case of a resist film, and may or may not be sensitive. Specifically, resists and resins that are commonly used in the manufacture of semiconductor elements and liquid crystal display elements can be used. In addition, the organic film forming material is preferably a material capable of forming an organic film that can be etched, particularly dry etched, so that the organic film pattern can be formed by etching the organic film using a pattern made of block copolymer formed by processing the BCP layer 3. Among them, it is preferable that the material be a material capable of forming an organic film that can be etched by oxygen plasma etching or the like. Such an organic film forming material may be a material that has been used to form an organic film such as organic BARC. For example, the ARC series manufactured by Nissan Chemical Industries, Ltd., the AR series manufactured by Rohm and Haas, and the SWK series manufactured by Tokyo Ohka Kogyo Co., Ltd. can be mentioned.

[0080] The method for applying the primer onto the support 1 to form the primer layer 2 is not particularly limited, and may be any of the conventionally known methods. For example, the undercoat layer 2 can be formed by applying the undercoat agent onto the support 1 by a conventionally known method such as spin coating or using a spinner to form a coating film, and then drying the coating film. The method for drying the coating film may be any method capable of volatilizing the solvent contained in the undercoat agent, such as baking. In this case, the baking temperature is preferably 80 to 300° C., more preferably 180 to 270° C., and further preferably 220 to 270° C. The baking time is preferably 30 to 500 seconds, and more preferably 60 to 400 seconds. The thickness of the undercoat agent layer 2 after the coating film has dried is preferably about 10 to 100 nm, and more preferably about 20 to 50 nm.

[0081] The surface of the support 1 may be washed before forming the primer layer 2 on the support 1. Washing the surface of the support 1 improves the coatability of the primer. The cleaning treatment may be carried out by any of the conventional methods known in the art, including, for example, oxygen plasma treatment, ozone oxidation treatment, acid-alkali treatment, and chemical modification treatment.

[0082] After forming the primer layer 2, the primer layer 2 may be rinsed with a rinsing liquid such as a solvent, if necessary. The rinsing removes uncrosslinked portions and the like in the primer layer 2, improving the affinity with at least one block constituting the block copolymer, and facilitating the formation of a phase-separated structure consisting of a cylindrical structure and a lamellar structure oriented in a direction perpendicular to the surface of the support 1. The rinse liquid may be any liquid capable of dissolving the uncrosslinked portions, and solvents such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethyl lactate (EL), or commercially available thinners may be used. After the cleaning, post-baking may be performed to volatilize the rinsing liquid. The temperature condition for this post-baking is preferably 80 to 250°C, more preferably 80 to 200°C, and further preferably 80 to 150°C. The baking time is preferably 30 to 500 seconds, and more preferably 60 to 240 seconds. The thickness of the undercoat agent layer 2 after such post-baking is preferably about 1 to 10 nm, and more preferably about 2 to 7 nm.

[0083] Next, on the undercoat agent layer 2, a layer (BCP layer) 3 containing a (BCP) component is formed. The method for forming the BCP layer 3 on the undercoat layer 2 is not particularly limited, and examples thereof include a method in which the resin composition for forming an etching mask pattern of the above-mentioned embodiment is applied onto the undercoat layer 2 by a conventionally known method such as using spin coating or a spinner to form a coating film, and then drying.

[0084] The thickness of the BCP layer 3 need only be sufficient so that it can be used as an etching mask and so that phase separation occurs. The film thickness of the BCP layer 3 is equal to or greater than 25 nm. When the film thickness is equal to or greater than the lower limit, the phase-separated structure formed from the BCP layer 3 tends to remain during etching and tends to function as a mask. The thickness of the BCP layer 3 may be 100 nm or less, 75 nm or less, 50 nm or less, 40 nm or less, or 35 nm or less. When the thickness is equal to or less than the upper limit, a phase-separated structure having a desired periodic size can be easily obtained, and the uniformity of the nanostructure can be easily improved. The thickness of the BCP layer 3 is preferably 25 to 100 nm. For example, when the support 1 is a Si substrate, the thickness of the BCP layer 3 is preferably adjusted to 25 to 100 nm, more preferably 25 to 75 nm.

[0085] In the method for producing an etching mask pattern according to the present embodiment described above, by using the above-mentioned resin composition for forming an etching mask pattern, a phase-separated structure having a period (L0) of less than 20 nm and excellent vertical alignment even when subjected to high-temperature annealing can be obtained. The film thickness of the obtained phase-separated structure is 25 nm or more, and this phase-separated structure can be used for producing an etching mask pattern. In addition, according to the method for producing an etching mask pattern of this embodiment, it is possible to produce a support having nanostructures on the support surface, the positions and orientations of which can be more freely designed. For example, the structure formed has high adhesion to the support and is likely to have a phase-separated structure consisting of cylindrical structures and lamellar structures oriented perpendicular to the support surface.

[0086] [Optional process] Guide pattern formation process The method for producing an etching mask pattern according to this embodiment may include a step of providing a guide pattern on the undercoat agent layer (guide pattern forming step) before the above-mentioned steps (i) and (ii), which makes it possible to control the arrangement structure of the phase separation structure. For example, even in the case of a block copolymer that forms a random fingerprint-like phase separation structure when no guide pattern is provided, by providing a groove structure of the resist film on the surface of the undercoat layer, a phase separation structure oriented along the groove can be obtained. Based on this principle, a guide pattern may be provided on the undercoat layer 2. In addition, if the surface of the guide pattern has affinity with any of the blocks constituting the (BCP) component, a phase separation structure oriented perpendicular to the support surface is easily formed.

[0087] The guide pattern can be formed using, for example, a resist composition. The resist composition for forming the guide pattern can be appropriately selected from resist compositions generally used for forming resist patterns and their modifications, and can be used by selecting one having affinity with any of the blocks constituting the (BCP) component. The resist composition may be either a positive resist composition for forming a positive pattern in which the exposed portion of the resist film is dissolved and removed, or a negative resist composition for forming a negative pattern in which the unexposed portion of the resist film is dissolved and removed, but is preferably a negative resist composition. As the negative resist composition, for example, a resist composition containing an acid generator and a base component whose solubility in a developer containing an organic solvent is reduced by the action of an acid, and the base component contains a resin component having a structural unit that is decomposed by the action of an acid to increase polarity, is preferable. After the resin composition for forming an etching pattern is poured onto the undercoat layer on which the guide pattern is formed, an annealing treatment is performed to cause phase separation. Therefore, it is preferable that the resist composition for forming the guide pattern is one capable of forming a resist film having excellent solvent resistance and heat resistance.

[0088] (Resin composition for forming etching mask pattern) The resin composition for forming an etching mask pattern of this embodiment may be any of those described above in the previous embodiment. The block copolymer ((BCP) component) in the resin composition for forming an etching mask pattern may be produced, for example, by a production method having the steps shown below.

[0089] <Production method of block copolymer (BCP) component> Step (p1): A step of obtaining a block copolymer having a first block and a precursor of a second block (hereinafter, also referred to as a "BCP precursor"). Step (p2): Adding R to the precursor of the second block in the BCP precursor 2 Compounds represented by -SH (R 2 is R in the above formula (b2g). 2) to obtain a block copolymer (component (BCP)) containing a first block and a second block.

[0090] Process (p1): The precursor of the second block is composed of block 2M and block 2GP. Block 2M is composed of a polymer composed of a structural unit (b2m). Block 2GP is composed of a polymer composed of a structural unit (b2gp), which is a precursor of the structural unit (b2g).

[0091] The structural unit (b2gp) is a structural unit containing an epoxy group or a vinyl group, and examples of the structural unit include those represented by the following general formula (b2gp).

[0092] [ka] [In the formula, Rp 2 represents an epoxy group or a vinyl group. 2 R represents a linear or branched alkylene group having 1 to 8 carbon atoms. b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms.]

[0093] The BCP precursor can be obtained, for example, by the following procedure: First, a monomer (e.g., styrene or a derivative thereof, hereinafter also referred to as monomer (b1)) from which the structural unit (b1) is derived is polymerized to synthesize a precursor of the first block. Next, a monomer that derives the structural unit (b2gp) (for example, glycidyl methacrylate, acrylic methacrylate, etc., hereinafter also referred to as monomer (b2gp)) is added to the obtained polymerization reaction liquid, and a further polymerization reaction is carried out. Next, a monomer that derives the structural unit (b2m) (e.g., methyl methacrylate, hereinafter also referred to as monomer (b2m)) is added to the obtained polymerization reaction liquid, and a polymerization reaction is further carried out to obtain a BCP precursor.

[0094] Alternatively, after carrying out the polymerization reaction of the monomer (b1), the monomer (b2m) is added to the polymerization reaction liquid to carry out the polymerization reaction, and then the monomer (b2gp) is added to the obtained polymerization reaction liquid to carry out the polymerization reaction, thereby obtaining the BCP precursor.

[0095] Alternatively, after carrying out a polymerization reaction of the monomer (b2m), the monomer (b2gp) is added to the polymerization reaction liquid and a polymerization reaction is carried out. Next, the monomer (b1) is added to the obtained polymerization reaction liquid and a polymerization reaction is carried out, thereby obtaining a BCP precursor.

[0096] Alternatively, after carrying out a polymerization reaction of the monomer (b2gp), the monomer (b2m) is added to the polymerization reaction liquid and a polymerization reaction is carried out. Next, the monomer (b1) is added to the obtained polymerization reaction liquid and a polymerization reaction is carried out, thereby obtaining a BCP precursor.

[0097] The polymerization reaction is preferably living polymerization because it is narrowly dispersed and easy to synthesize. Preferred living polymerization methods include living anionic polymerization and living radical polymerization, and living anionic polymerization is particularly preferred because it can more narrowly dispersed.

[0098] In the step (p1), the proportion of the number of moles of monomer (b1) used in the production of the BCP precursor is preferably 20 to 80 mol %, more preferably 30 to 75 mol %, and even more preferably 35 to 70 mol %, relative to the total number of moles (100 mol %) of monomer (b1), monomer (b2gp) and monomer (b2m). In the step (p1), the proportion of the number of moles of the monomer (b2gp) used in the production of the BCP precursor is preferably 0.5 to 8 mol %, more preferably 1 to 7 mol %, and even more preferably 1.5 to 6 mol %, relative to the total number of moles (100 mol %) of the monomer (b1), the monomer (b2gp) and the monomer (b2m). In the step (p1), the proportion of the number of moles of monomer (b2m) used in the production of the BCP precursor is preferably 10 to 70 mol%, more preferably 15 to 65 mol%, and even more preferably 20 to 60 mol%, relative to the total number of moles (100 mol%) of monomer (b1), monomer (b2gp) and monomer (b2m).

[0099] Process (p2): R 2 A compound represented by the formula (hereinafter referred to as "compound (R 2 The compound (b2gp) reacts with the epoxy group or vinyl group of the structural unit (b2gp) to convert the structural unit (b2gp) into the structural unit (b2g). When the building block (b2gp) contains an epoxy group, the BCP precursor and the compound (R 2 The reaction of R2gp with the compound (R-SH) can be carried out in an organic solvent such as tetrahydrofuran in the presence of a catalyst such as lithium hydroxide. The reaction temperature can be set, for example, at 20 to 60°C, preferably 30 to 50°C, and more preferably 35 to 45°C. The reaction time can be appropriately set depending on the amount of BCP precursor used, and may be a time sufficient for all of the structural units (b2gp) in the precursor of the second block to be converted to structural units (b2g). The reaction time can be set, for example, for 1 to 10 hours. When the structural unit (b2gp) contains a vinyl group, the reaction of the BCP precursor with the compound (R2gp with 2 The reaction of -SH) can be carried out by a thiol-ene reaction. The thiol-ene reaction can be carried out in an organic solvent such as tetrahydrofuran in the presence of a catalyst such as azobisisobutyronitrile (AIBN). The reaction temperature can be, for example, 60 to 90°C, preferably 70 to 90°C, and more preferably 75 to 85°C. The reaction time can be appropriately set depending on the amount of the BCP precursor used, and may be a time sufficient for all of the structural units (b2gp) in the precursor of the second block to be converted to structural units (b2g). The reaction time can be, for example, 1 to 10 hours.

[0100] [ka] [In the formula, R 1 , R b1 and n is R in the formula (b1). 1 , R b1 and n. R 2 and R 3 is R in the formula (b2g). 2 and R 3 is the same as R b2 , y and z are R in the formula (b2g) and the formula (b2m). b2 , y and z. 2 Rp represents a linear or branched alkyl group having 1 to 8 carbon atoms. 2 represents an epoxy group or a vinyl group.

[0101] <Organic solvent components> The resin composition for forming an etching mask pattern of the present embodiment can be prepared by dissolving the above-mentioned (BCP) component in an organic solvent component. The organic solvent component may be any solvent capable of dissolving each component used to form a homogeneous solution, and any solvent known in the art as a solvent for film compositions mainly composed of resins may be used.

[0102] Examples of the organic solvent component include lactones such as γ-butyrolactone; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl-n-pentyl ketone, methyl isopentyl ketone, and 2-heptanone; polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol; compounds having an ester bond such as ethylene glycol monoacetate, diethylene glycol monoacetate, propylene glycol monoacetate, and dipropylene glycol monoacetate; and ether bonds such as monoalkyl ethers, monomethyl ether, monoethyl ether, monopropyl ether, and monobutyl ether of the polyhydric alcohols or the compounds having an ester bond, or monophenyl ether. derivatives of polyhydric alcohols such as compounds having a bond [among which, propylene glycol monomethyl ether acetate (PGMEA) and propylene glycol monomethyl ether (PGME) are preferred]; cyclic ethers such as dioxane, esters such as methyl lactate, ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, and ethyl ethoxypropionate; and aromatic organic solvents such as anisole, ethyl benzyl ether, cresyl methyl ether, diphenyl ether, dibenzyl ether, phenetole, butyl phenyl ether, ethylbenzene, diethylbenzene, pentylbenzene, isopropylbenzene, toluene, xylene, cymene, and mesitylene. The organic solvent component may be used alone or in a mixture of two or more kinds. Among them, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone, and EL are preferred.

[0103] A mixed solvent obtained by mixing PGMEA and a polar solvent is also preferred. The mixing ratio (mass ratio) may be appropriately determined in consideration of the compatibility between PGMEA and the polar solvent, and is preferably within a range of 1:9 to 9:1, and more preferably 2:8 to 8:2. For example, when EL is blended as the polar solvent, the mass ratio of PGMEA:EL is preferably 1:9 to 9:1, more preferably 2:8 to 8:2. When PGME is blended as the polar solvent, the mass ratio of PGMEA:PGME is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3. When PGME and cyclohexanone are blended as the polar solvent, the mass ratio of PGMEA:(PGME+cyclohexanone) is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3.

[0104] As the organic solvent component in the resin composition for forming an etching mask pattern, a mixed solvent of PGMEA or EL, or a mixed solvent of the PGMEA and a polar solvent, and γ-butyrolactone is also preferred. In this case, the mass ratio of the former to the latter is preferably 70:30 to 95:5. The organic solvent component contained in the resin composition for forming an etching mask pattern is not particularly limited, and is appropriately set at a coatable concentration according to the coating film thickness, and is generally used so that the solid content concentration is within the range of 0.2 to 70 mass %, preferably 0.2 to 50 mass %.

[0105] <Optional ingredients> In addition to the above-mentioned (BCP) component and organic solvent component, the resin composition for forming an etching mask pattern may further contain, as desired, compatible additives such as additional resins for improving the performance of the layer, surfactants for improving coatability, dissolution inhibitors, plasticizers, stabilizers, colorants, antihalation agents, dyes, sensitizers, base amplifiers, basic compounds, and the like.

[0106] According to the resin composition for forming an etching mask pattern of the present embodiment described above, it is possible to form a phase-separated structure having a period (L0) of less than 20 nm and excellent vertical alignment even when subjected to high-temperature annealing. Therefore, the phase-separated structure can be used as an etching mask.

[0107] (The (BCP) component can increase the value of χ compared to a block copolymer (PS-b-PMMA) having a styrene block and a methyl methacrylate block because the second block has a structural unit (b2g). Thereby, a fine phase separation structure with a shorter period can be formed using a block copolymer with a lower degree of polymerization (N). However, when the value of χ is high, the vertical alignment tends to decrease. In particular, at a film thickness applicable to an etching mask pattern (for example, a film thickness of 25 nm or more, preferably 30 nm or more), the (BCP) component becomes less likely to form a vertically aligned phase separation structure.) The resin composition for forming an etching mask pattern of the present embodiment has a second block composed of block 2M and block 2G, and y / (y + z) is 0.01 or more and 0.11 or less, so that the vertical alignment is improved, and a vertically aligned phase separation structure can be formed at a film thickness applicable to an etching mask pattern.)

Examples

[0108] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.)

[0109] (Synthesis of BCP precursor) The BCP precursors (1) to (8) were synthesized according to the following procedure.)

[0110] (Synthesis of BCP precursor (1)) All anionic polymerizations were carried out under an argon atmosphere. 30 mL of tetrahydrofuran (THF) and lithium chloride (LiCl) (21.2 mg, 0.500 mmol) were transferred to a 50 mL Schlenk tube and cooled to -78 °C in a CoolNexus bath. sec-Butyllithium (Sec-BuLi) (1.05 M hexane / cyclohexane solution) was added to the Schlenk tube until the color of the solution turned yellow. The Schlenk tube was removed from the CoolNexus bath and warmed to room temperature until the solution became colorless. The Schlenk tube was cooled again to -78 °C in the CoolNexus bath, and sec-BuLi (0.095 mL, 0.100 mmol) was added as an initiator. Styrene (1.19 mL, 10.4 mmol) was added and stirred for 30 minutes. As a result, a bright orange solution was obtained. 1,1-Diphenylethylene (DPE) (0.088 mL, 0.50 mmol) was added, and the color of the solution changed to dark red. After stirring for 30 minutes, glycidyl methacrylate (GMA) (0.157 mL, 1.31 mmol) was added and stirred for 120 minutes. The color of the solution changed from red to transparent. Then, methyl methacrylate (MMA) (1.41 mL, 13.3 mmol) was added and stirred for 30 minutes. As a terminator, 3 mL of degassed methanol (MeOH) was added to the Schlenk tube to terminate the polymerization. The Schlenk tube was lifted out of the CoolNexus bath, and the solution was poured into MeOH for reprecipitation. After filtering the solid precipitate, it was dried under reduced pressure at 40 °C to obtain a white powder of BCP precursor (1) (2.57 g, 86% yield).

[0111] <Synthesis of BCP precursor (2)> BCP precursor (2) was synthesized in the same manner as the synthesis of BCP precursor (1) above, except that the amount of St used was 1.07 mL (9.29 mmol), the amount of GMA used was 0.117 mL (0.976 mmol), and the amount of MMA used was 0.936 mL (8.78 mmol).

[0112] <Synthesis of BCP precursor (3)> The BCP precursor (3) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of St used was 1.27 mL (11.0 mmol), the amount of GMA used was 0.0988 mL (0.828 mmol), and the amount of MMA used was 0.891 mL (8.37 mmol).

[0113] <Synthesis of BCP Precursor (4)> The BCP precursor (4) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of St used was 1.63 mL (14.1 mmol), the amount of GMA used was 0.0475 mL (0.398 mmol), and the amount of MMA used was 0.664 mL (6.23 mmol).

[0114] <Synthesis of BCP Precursor (5)> The BCP precursor (5) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of St used was 1.20 mL (10.4 mmol), the amount of GMA used was 0.257 mL (2.15 mmol), and the amount of MMA used was 0.916 mL (8.60 mmol).

[0115] <Synthesis of BCP Precursor (6)> The BCP precursor (6) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of St used was 1.83 mL (15.9 mmol), the amount of GMA used was 0.108 mL (0.905 mmol), and the amount of MMA used was 0.645 mL (6.06 mmol).

[0116] <Synthesis of BCP Precursor (7)> The BCP precursor (7) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of St used was 1.72 mL (15.0 mmol), the amount of GMA used was 0.105 mL (0.882 mmol), and the amount of MMA used was 0.760 mL (7.13 mmol).

[0117] <Synthesis of BCP Precursor (8)> The BCP precursor (8) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of St used was 1.38 mL (12.0 mmol), the amount of GMA used was 0 mL (0 mmol), and the amount of MMA used was 1.33 mL (12.5 mmol).

[0118]

Chemical formula

[0119] The BCP precursors (9) to (15) were synthesized according to the following procedure.

[0120] <Synthesis of BCP precursor (9)> All anionic polymerizations were carried out under an argon atmosphere. 30 mL of tetrahydrofuran (THF) and lithium chloride (LiCl) (21.2 mg, 0.500 mmol) were transferred to a 50 mL Schlenk tube and cooled to -78 °C in a CoolNexus bath. sec-Butyllithium (Sec-BuLi) (1.05 M hexane / cyclohexane solution) was added to the Schlenk tube until the color of the solution turned yellow. The Schlenk tube was removed from the CoolNexus bath and warmed to room temperature until the solution became colorless. The Schlenk tube was cooled again to -78 °C in the CoolNexus bath, and sec-BuLi (0.095 mL, 0.100 mmol) was added as an initiator. Styrene (1.36 mL, 11.8 mmol) was added and stirred for 30 minutes. As a result, a bright orange solution was obtained. 1,1-Diphenylethylene (DPE) (0.088 mL, 0.50 mmol) was added, and the color of the solution changed to dark red. After stirring for 30 minutes, methyl methacrylate (MMA) (1.29 mL, 12.1 mmol) was added and stirred for 30 minutes. The color of the solution changed from red to transparent. Then, glycidyl methacrylate (GMA) (0.143 mL, 1.20 mmol) was added and stirred for 120 minutes. As a terminator, 3 mL of degassed methanol (MeOH) was added to the Schlenk tube to terminate the polymerization. The Schlenk tube was lifted out of the CoolNexus bath, and the solution was poured into MeOH for reprecipitation. After filtering the solid precipitate, it was dried under reduced pressure at 40 °C to obtain a white powder of BCP precursor (9) (2.54 g, 84% yield).

[0121] <Synthesis of BCP precursor (10)> BCP precursor (10) was synthesized in the same manner as the synthesis of the above BCP precursor (9), except that the amount of St used was 1.11 mL (9.70 mmol), the amount of MMA used was 0.901 mL (8.46 mmol), and the amount of GMA used was 0.112 mL (0.940 mmol).

[0122] <Synthesis of BCP precursor (11)> The BCP precursor (11) was synthesized in the same manner as the synthesis of the above BCP precursor (9), except that the amount of St used was 1.27 mL (11.1 mmol), the amount of MMA used was 0.933 mL (8.76 mmol), and the amount of GMA used was 0.0787 mL (0.659 mmol).

[0123] <Synthesis of BCP Precursor (12)> The BCP precursor (12) was synthesized in the same manner as the synthesis of the above BCP precursor (9), except that the amount of St used was 1.65 mL (14.4 mmol), the amount of MMA used was 0.643 mL (6.04 mmol), and the amount of GMA used was 0.0460 mL (0.385 mmol).

[0124] <Synthesis of BCP Precursor (13)> The BCP precursor (13) was synthesized in the same manner as the synthesis of the above BCP precursor (9), except that the amount of St used was 1.28 mL (11.1 mmol), the amount of MMA used was 0.888 mL (8.34 mmol), and the amount of GMA used was 0.234 mL (1.96 mmol).

[0125] <Synthesis of BCP Precursor (14)> The BCP precursor (14) was synthesized in the same manner as the synthesis of the above BCP precursor (9), except that the amount of St used was 1.89 mL (16.4 mmol), the amount of MMA used was 0.591 mL (5.55 mmol), and the amount of GMA used was 0.108 mL (0.903 mmol).

[0126] <Synthesis of BCP Precursor (15)> The BCP precursor (15) was synthesized in the same manner as the synthesis of the above BCP precursor (9), except that the amount of St used was 1.94 mL (16.9 mmol), the amount of MMA used was 0.600 mL (5.63 mmol), and the amount of GMA used was 0.0831 mL (0.696 mmol).

[0127]

Chemical Structure

[0128] The BCP precursor (16) was synthesized according to the following procedure.

[0129] <Synthesis of BCP Precursor (16)> All anionic polymerizations were carried out under an argon atmosphere. 30 mL of tetrahydrofuran (THF) and lithium chloride (LiCl) (21.2 mg, 0.500 mmol) were transferred to a 50 mL Schlenk tube and cooled to -78 °C in a Cool Nex bath. Sec-butyllithium (Sec-BuLi) (1.05 M hexane / cyclohexane solution) was added to the Schlenk tube until the color of the solution turned yellow. The Schlenk tube was removed from the Cool Nex bath and warmed to room temperature until the solution became colorless. The Schlenk tube was cooled again to -78 °C in the Cool Nex bath, and sec-BuLi (0.095 mL, 0.100 mmol) was added as an initiator. Styrene (1.03 mL, 9.04 mmol) was added and stirred for 30 minutes. As a result, a bright orange solution was obtained. 1,1-Diphenylethylene (DPE) (0.088 mL, 0.50 mmol) was added, and the color of the solution changed to dark red. After stirring for 30 minutes, a monomer mixture of methyl methacrylate (MMA) (1.11 mL, 10.5 mmol) and glycidyl methacrylate (GMA) (0.139 mL, 1.16 mmol) was added and stirred for 30 minutes. The color of the solution changed from red to transparent. As a terminator, 3 mL of degassed methanol (MeOH) was added to the Schlenk tube to terminate the polymerization. The Schlenk tube was lifted out of the Cool Nex bath, and the solution was poured into MeOH for reprecipitation. After filtering the solid of the precipitate, vacuum drying was carried out at 40 °C to obtain a white powder of the BCP precursor (16) (2.41 g, 88% yield).

[0130]

Chemical formula

[0131] The BCP precursors (1) to (15) consist of block 2M in which the precursor of the second block is composed of a polymer having a repeating structure of a structural unit derived from methyl methacrylate, and block 2G in which the precursor of the second block is composed of a polymer having a repeating structure of a structural unit derived from glycidyl methacrylate. The BCP precursor (16) is a random copolymer in which the precursors of the second block have a structure in which the structural units derived from methyl methacrylate and the structural units derived from glycidyl methacrylate are randomly arranged.

[0132] (Synthesis of block copolymer) (Synthesis of BCP(1)) (Synthesis of block copolymer: BCP(1)) 0.2 g of the BCP precursor (1) and THF (20 wt% solution) were placed in a 10 mL glass tube and immersed in an ice water bath. A 1 wt% aqueous lithium hydroxide (LiOH) solution (LiOH 0.05 molar equivalent / GMA unit) and 2,2,2-trifluoroethanethiol (2 molar equivalents / GMA unit) were added to the glass tube. After stirring at room temperature for 20 minutes, the reactor was set to 40 °C and stirred for 3 hours to synthesize BCP(1). Depending on the Mn and PHFMA fraction of the synthesized BCP(1), precipitation was repeated several times with methanol or water / methanol to remove residual reagents. The product was dried under reduced pressure at room temperature overnight to obtain a white powder of BCP(1). The Mn of BCP(1) measured by size exclusion chromatography (SEC) was measured The NMR analysis values of BCP(1) were as follows. 11H NMR (400 MHz, Acetone-d6, δ, ppm): 0.84 (s, α-CH3, PMMA), 0.87 (s, α-CH3, PMMA), 1.00 (s, α-CH3, PMMA), 1.03 (s, α-CH3, PHFMA), 1.23 - 1.73 (br, backbone, -CH2-CH-, PS), 1.75 - 2.23 (br, backbone, -CH2-CH-, PS, br, backbone, -CH2-C(CH3)-, PHFMA and PMMA), 2.78 - 3.00 (d, CH(OH)-CH2-S-, PHFMA), 3.40 - 3.77 (s, -S-CH2-CF3, PHFMA), 3.54 - 3.75 (s, -OCH3, PMMA), 3.92 - 4.07 (d, -(C=O)O-CH2-, PHFMA), 4.07 - 4.18 (m, -CH(OH)-, PHFMA) 4.50 - 4.72 (br, -CH(OH)-, PHFMA), 6.36 - 6.84 (m, o-aromatic, PS), 6.85 - 7.35 (m, m-, p-aromatic, PS).

[0133] <Synthesis of BCP(2) - (16)> BCP(2) - (16) were synthesized in the same manner as the synthesis of BCP(1) above, except that BCP precursors (2) - (16) were used instead of BCP precursor (1).

[0134] The Mn of BCP(1) - (16) was measured by size exclusion chromatography (SEC). The number average molecular weight (Mn) of each block copolymer synthesized above, x, y, and z in the above reaction formula, and the value of y / (y + z) in the above reaction formula were summarized in Table 1. x, y, and z are the mol% in the obtained BCP(1) - (16). The value of y / (y + z) is the value with the fourth decimal place rounded down.

[0135]

Table 1

[0136]

Table 2

[0137] The components shown in Tables 1 and 2 were mixed and dissolved in an organic solvent component to prepare respective examples of resin compositions for forming etching mask patterns (solid content concentration: 1% by mass).

[0138] [Table 3]

[0139] [Table 4]

[0140] In Tables 3 and 4, the abbreviations have the following meanings: The numbers in brackets [ ] are the blend amounts (parts by mass). BCP-1: BCP(1). BCP-2: BCP(2). BCP-3: BCP(3). BCP-4: BCP(4). BCP-5: BCP(5). BCP-6: BCP(6). BCP-7: BCP(7). BCP-8: BCP(8). BCP-9: BCP(9). BCP-10: BCP(10). BCP-11: BCP(11). BCP-12: BCP(12). BCP-13: BCP(13). BCP-14: BCP(14). BCP-15: BCP(15). BCP-16: BCP(16). (S)-1: PGMEA (polyethylene glycol monomethyl ether acetate)

[0141] Using the resin composition for forming an etching mask pattern of each of the above examples, a structure including a phase-separated structure was obtained by a production method including the steps (i) and (ii) described below.

[0142] (Rating 1) <Production of Structure Including Phase Separation Structure> (Preparation of primer) To prepare the primer, we prepared a primer resin NL-(1), which is a random copolymer of styrene, methyl methacrylate, and (hydroxyethyl) methacrylate.

[0143] The composition ratio of NL-(1) (proportion (molar ratio) of each structural unit in the structural formula) styrene / methyl methacrylate / (hydroxyethyl) methacrylate was 49 / 46 / 5, and the number average molecular weight (Mn) was 28,000.

[0144] The primer resin NL-(1) was mixed and dissolved in PGMEA to prepare the primer NL-1.

[0145] Process (i): A 12-inch silicon wafer was prepared as a support.

[0146] The undercoat agent NL-1 was spin-coated onto a silicon substrate, and then heated in air at 250° C. for 5 minutes, forming a 30 nm-thick undercoat agent layer made of undercoat agent resin NL-(1) on the substrate surface. The undercoat layer was then rinsed with a rinse solution (PGME / PGMEA=7 / 3) consisting of propylene glycol monomethyl ether (PGME) and propylene glycol monomethyl ether acetate (PGMEA), and then heated at 100° C. for 1 minute to volatilize the rinse solution.

[0147] Next, the resin composition of each example was spin-coated onto the substrate so as to have a film thickness of 25 nm, thereby forming a resin composition layer (a layer containing a block copolymer).

[0148] Step (ii): The resin composition layer formed on the substrate was prebaked at 90° C. for 60 seconds in a nitrogen atmosphere, and then annealed at 290° C. for 5 minutes in a nitrogen atmosphere to form a phase-separated structure.

[0149] [Resolution evaluation] The phase separation structure on the surface of the obtained substrate was analyzed by SEM image at 100,000x magnification using Hitachi High-Technologies' "CG6300". Next, the pattern period was analyzed from the SEM image using Hitachi High-Technologies' "Terminal PC Software". The resolution was evaluated based on the following evaluation criteria. The evaluation results are shown in Tables 5 to 6 as "resolution".

[0150] Judgment criteria: A: The period was less than 20 nm. B: The period was 20 nm or more. When the resin compositions of Comparative Examples 1 to 7 were used, a phase separation structure was not formed, and therefore the period could not be calculated. These are indicated by "-".

[0151] [Evaluation of vertical alignment] The surface (phase separation state) of the obtained substrate was observed with a length measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation). As a result of such observation, the vertical alignment was evaluated based on the following evaluation criteria. The results are shown in Tables 5 to 6 as "vertical alignment".

[0152] Judgment criteria: A: A vertically oriented phase-separated structure is formed over the entire surface of the substrate. B: A perpendicularly oriented phase-separated structure is not formed in a part of the substrate. C: A vertically oriented phase-separated structure is not formed over the entire surface of the substrate.

[0153] [Table 5]

[0154] [Table 6]

[0155] In Examples 1 to 8, in which y / (y+z) in the second block was 0.01 or more and 0.11 or less, a vertically oriented phase-separated structure was formed over the entire surface of the substrate, and the resolution was less than 20 nm. In Comparative Examples 1 to 8, in which y / (y+z) in the second block was less than 0.01 or more than 0.11, a vertically oriented phase-separated structure was not formed over the entire surface of the substrate, and the resolution could not be measured. In Reference Example 1 in which the second block was a random copolymer, the resolution was less than 20 nm, but a vertically oriented phase-separated structure was not formed in a part of the substrate.

Claims

1. A step of applying a resin composition for forming an etching mask pattern onto a support to form a layer containing a block copolymer and having a thickness of 25 nm or more; allowing the layer containing the block copolymer to phase separate; having The resin composition for forming an etching mask pattern contains a block copolymer having a first block and a second block, The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1): A method for producing an etching mask pattern, wherein the second block comprises a block 2M composed of a polymer composed of a repeating structure of a structural unit represented by the following general formula (b2m), and a block 2G composed of a polymer composed of a repeating structure of a structural unit represented by the following general formula (b2g). 【Chemistry 1】 [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. b1 is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. x, y, and z each represent a molar ratio. x+y+z=100 mol %. y / (y+z) is 0.01 or more and 0.11 or less. x is 20 to 80 mol %.

2. The method for producing an etching mask pattern according to claim 1 , wherein the block copolymer is a polymer represented by the following general formula (BCP1) or the following general formula (BCP2): 【Chemistry 2】 [In formula (BCP1) and formula (BCP2), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. b1 is a hydrogen atom or a methyl group. In formula (BCP1) and formula (BCP2), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. In formula (BCP1) and formula (BCP2), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. x, y, and z each represent a molar ratio. x+y+z=100 mol %. y / (y+z) is 0.01 or more and 0.11 or less. x is 20 to 80 mol %.

3. 3. The method for producing an etching mask pattern according to claim 1, wherein the block copolymer has a number average molecular weight of 15,000 to 35,000.

4. A resin composition for forming an etching mask pattern, comprising a block copolymer having a first block and a second block, The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1): The second block is a resin composition for forming an etching mask pattern, which comprises a block 2M composed of a polymer composed of a repeating structure of a structural unit represented by the following general formula (b2m), and a block 2G composed of a polymer composed of a repeating structure of a structural unit represented by the following general formula (b2g): 【Chemistry 3】 [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. b1 is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. x, y, and z each represent a molar ratio. x+y+z=100 mol %. y / (y+z) is 0.01 or more and 0.11 or less. x is 20 to 80 mol %.

5. The resin composition for forming an etching mask pattern according to claim 4 , wherein the block copolymer is a polymer represented by the following general formula (BCP1) or the following general formula (BCP2): 【Chemistry 4】 [In formula (BCP1) and formula (BCP2), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. b1 is a hydrogen atom or a methyl group. In formula (BCP1) and formula (BCP2), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 2 to 10 carbon atoms, which may have a hydroxy group. In formula (BCP1) and formula (BCP2), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. x, y, and z represent molar ratios. x+y+z=100 mol %. y / (y+z) is 0.01 or more and 0.11 or less. x is 20 to 80 mol %.

6. 6. The resin composition for forming an etching mask pattern according to claim 4, wherein the block copolymer has a number average molecular weight of 15,000 to 35,000.

Citation Information

Patent Citations

  • Pattern formation method and mold

    JP2008036491A

  • Resin composition for forming phase separation structure, method for producing structure body including phase separation structure, and block copolymer

    JP2022020519A