Delamination container, and preform for delamination container

The laminated container design with a high-crystallinity whitening line portion and preform process addresses the issue of inner container distortion, ensuring easy peeling and reducing remaining contents by maintaining structural integrity and air introduction.

JP2024158996AInactive Publication Date: 2024-11-08YOSHINO KOGYOSHO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023074692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing laminated containers face issues with the inner container distorting as contents decrease, leading to an increase in the remaining amount of contents.

Method used

A laminated container design with a whitening line portion having higher crystallinity than other parts, which acts as a pillar to prevent distortion during volume reduction, and a preform process to ensure the whitening line does not stick to the outer container, allowing easy peeling and securing an air introduction space.

Benefits of technology

The design effectively suppresses the increase in remaining contents by preventing distortion and facilitating easy peeling of the inner container from the outer container, while maintaining structural integrity and air introduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158996000001_ABST
    Figure 2024158996000001_ABST
Patent Text Reader

Abstract

To suppress an increase in the residual amount of contents.SOLUTION: A delamination container according to the present invention has an inner container 12, the volume of which is reduced and deformed as the contained content decreases, and an outer container 11 in which the inner container is stacked, wherein a cylindrical mouth portion 13, a cylindrical shoulder portion 15, a cylindrical body portion 16, and a cup-shaped bottom portion 17 are arranged in this order from top to bottom along the container axis O direction. In the inner container, the portion of the inner container located below the mouth portion is provided with a whitening line 23A that has a circumferential width and extends in the axial direction of the container, and the maximum value of crystallinity at the whitening line is higher than the maximum value of crystallinity at the portions other than the whitening line in the shoulder and body portions of the inner container, respectively.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a delaminating container and a preform for a delaminating container. [Background technology]

[0002] Conventionally, as shown in Patent Document 1 below, for example, there has been known a peelable laminated container which includes an inner container that undergoes a volumetric deformation as the contained contents decrease, and an outer container in which the inner container is placed in a stacked state, with a cylindrical mouth, a cylindrical shoulder, a cylindrical body, and a cup-shaped bottom arranged in this order from top to bottom along the axial direction of the container. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-142186 A Summary of the Invention [Problem to be solved by the invention]

[0004] There was room for improvement in preventing the container from becoming distorted in volume as the contents decrease, resulting in an increase in the amount of remaining contents.

[0005] The present invention provides a delaminating container and a preform for a delaminating container that can prevent the amount of content remaining from increasing. [Means for solving the problem]

[0006] A laminated peelable container according to one embodiment of the present invention comprises an inner container that undergoes volumetric deformation as the contents contained therein decrease, and an outer container in which the inner container is housed in a stacked state, and has a cylindrical mouth, a cylindrical shoulder, a cylindrical body, and a cup-shaped bottom arranged in this order from top to bottom along the container axial direction, and a whitening line portion having a circumferential width and extending in the container axial direction is provided in a portion of the inner container located below the mouth, and the maximum crystallinity of the whitening line portion is higher than the maximum crystallinity of the portions of the inner container, excluding the whitening line portion, in each of the shoulder and body portions.

[0007] Since the maximum crystallinity at the whitening line is higher than the maximum crystallinity at the shoulder and body of the inner container in each case, the stiffness of the whitening line is higher than the stiffness of the other parts of the inner container located below the mouth. As a result, when the inner container is deformed in a reduced volume due to a decrease in the contents, the other parts contract with the whitening line acting as a pillar, which makes it possible to prevent the inner container from being deformed in a distorted manner in volume reduction, and it becomes easier to secure a space for introducing outside air extending in the container axial direction between the outer surface of the inner container and the inner surface of the outer container, making it possible to prevent the remaining amount of contents from increasing.

[0008] The degree of crystallinity of the whitened line portion may decrease from the outer surface to the inner surface of the inner container.

[0009] Since the crystallinity of the whitened line portion decreases from the outer surface to the inner surface of the inner container, in the state of the laminated peelable container obtained by blow molding the preform, the space between the inner surface of the outer container and the outer surface of the inner container is narrow, and it is clear that the whitened line portion cannot be formed on the inner container. The only way to form the whitened line portion is to insert the inner preform used to mold the inner container into the outer preform used to mold the outer container. Then, when the inner preform provided with the whitened line portion is inserted into the outer preform to obtain a preform, and then the preform is blow molded, the whitened line portion of the inner preform becomes difficult to stretch. This makes it possible to make the whitened line portion of the inner container less likely to stick to the inner surface of the outer container; for example, even if the inner container and the outer container are made of the same material, the inner container can be easily peeled off from the inner surface of the outer container as the contents are reduced; and because the whitened line portion of the inner container becomes thicker, when the inner container reduces in volume as the contents are reduced, other parts of the inner container contract using the whitened line portion as a pillar, preventing the inner container from reducing in volume in a distorted manner. It also makes it easier to secure a space for introducing outside air extending in the axial direction of the container between the outer surface of the inner container and the inner surface of the outer container, preventing the amount of contents remaining from increasing.

[0010] A preform for a delaminating container according to one embodiment of the present invention is a preform for molding a delaminating container comprising an inner container which undergoes volume reduction and deformation as the contained contents decrease, and an outer container in which the inner container is internally laminated, and which has a cylindrical mouth, a cylindrical shoulder, a cylindrical body, and a cup-shaped bottom arranged in this order from top to bottom along the container axial direction, the preform comprising a bottomed cylindrical inner preform for molding the inner container, and a bottomed cylindrical outer preform for molding the outer container, the inner preform being inserted into the outer preform, a portion of the inner preform located below the portion that will become the mouth of the inner container is provided with a whitening line portion which has a width in the circumferential direction and extends in the container axial direction, and the maximum crystallinity value in the whitening line portion is higher than the maximum crystallinity value of the portions of the inner preform that will become the shoulder and body of the inner container, excluding the whitening line portion.

[0011] Since the maximum crystallinity value in the white line portion is higher than the maximum crystallinity value in the portion of the inner preform that will become the shoulder and body portion of the inner container, excluding the white line portion, the white line portion of the inner preform is less likely to stretch during blow molding. This makes it possible to make the whitened line portion of the inner container less likely to stick to the inner surface of the outer container; for example, even if the inner container and outer container are made of the same material, the inner container can be easily peeled off from the inner surface of the outer container as the contents are reduced; and because the whitened line portion of the inner container becomes thicker, when the inner container reduces in volume as the contents are reduced, other parts of the inner container contract using the whitened line portion as a pillar, preventing the inner container from reducing in volume in a distorted manner. It also makes it easier to secure a space for introducing outside air extending in the axial direction of the container between the outer surface of the inner container and the inner surface of the outer container, preventing the amount of contents remaining from increasing.

[0012] The crystallinity of the whitened line portion may decrease from one of the inner and outer surfaces of the inner preform to the other, and the haze value of the whitened line portion may be 10% or more and 84% or less.

[0013] Since the crystallinity of the whitened line portion decreases from one of the inner and outer surfaces of the inner preform to the other, the whitened line portion can be formed by heat treating the inner preform from one of the surfaces to thermally crystallize it in a short period of time without thermally deteriorating the inner preform. Since the haze value of the whitened line portion is 10% or more and 84% or less, it is possible to reliably obtain a peelable laminated container that prevents the inner container from becoming difficult to peel off from the inner surface of the outer container as the contents decrease, and prevents the amount of contents remaining from increasing. If the haze value of the whitened line portion is less than 10%, the crystallinity in the whitened line portion will be too low, making it difficult to prevent the whitened line portion from stretching during blow molding. If the haze value of the whitened line portion is more than 84%, the crystallinity in the whitened line portion will be too high, making it possible that the whitened line portion will not stretch and may tear during blow molding.

[0014] The ratio of the thickness of the thermally crystallized portion to the thickness of the whitened line portion may be less than 35%.

[0015] Since the ratio of the thickness of the thermally crystallized portion to the thickness of the whitened line portion is less than 35%, it is possible to reliably prevent the whitened line portion from breaking due to lack of stretching during blow molding. Effect of the Invention

[0016] According to the above aspect of the present invention, it is possible to prevent the amount of content remaining from increasing. [Brief description of the drawings]

[0017] [Figure 1] 1 is a side view including a partial vertical cross section of a delaminating container shown as one embodiment of the present invention. [Diagram 2] 1 is a side view including a partial vertical cross section of a preform for a delaminating container shown as one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. 1, the peelable laminate container 1 of this embodiment includes an inner container 12 that undergoes volume reduction deformation as the contained contents decrease, and an outer container 11 in which the inner container 12 is placed in a stacked state. The inner container 12 is highly flexible, and is stacked on the inner surface of the outer container 11 in a peelable manner.

[0019] The material of the inner container 12 and the outer container 11 is a synthetic resin material, and may be the same material or different materials. Examples of synthetic resin materials include PET (polyethylene terephthalate), PP (polypropylene), PE (polyethylene), nylon (polyamide), and EVOH (ethylene-vinyl alcohol copolymer). In the illustrated example, the material of the inner container 12 and the outer container 11 is PET.

[0020] The delaminating container 1 has a cylindrical mouth 13, a cylindrical shoulder 15, a cylindrical body 16, and a cup-shaped bottom 17. The mouth 13, the shoulder 15, the body 16, and the bottom 17 are arranged in this order coaxially with a common axis. Hereinafter, this common axis will be referred to as the container axis O, the mouth 13 side along the container axis O will be referred to as the upper side, and the bottom 17 side along the container axis O will be referred to as the lower side. The direction intersecting the container axis O as viewed from the container axis O direction will be referred to as the radial direction, and the direction going around the container axis O as viewed from the container axis O direction will be referred to as the circumferential direction.

[0021] The mouth 13 of the laminated peelable container 1 is formed by stacking the mouth of the inner container 12 and the mouth of the outer container 11, the shoulder 15 of the laminated peelable container 1 is formed by stacking the shoulder of the inner container 12 and the shoulder of the outer container 11, the body 16 of the laminated peelable container 1 is formed by stacking the body of the inner container 12 and the body of the outer container 11, and the bottom 17 of the laminated peelable container 1 is formed by stacking the bottom of the inner container 12 and the bottom of the outer container 11. In the following description, unless otherwise specified, it is assumed that both the inner container 12 and the outer container 11 have the same shape.

[0022] The size of the delaminating delaminating container 1 in the container axis O direction is, for example, 150 mm or more and 250 mm or less. The content volume of the delaminating delaminating container 1 is, for example, 200 ml or more and 800 ml or less. The maximum outer diameter of the body 16 is, for example, 58 mm or more and 80 mm or less. In the illustrated example, the size of the delaminating delaminating container 1 in the container axis O direction is about 230 mm, and the delaminating delaminating container 1 is for a content volume of 720 ml.

[0023] The mouth portion 13 of the delaminating container 1 is formed in a cylindrical shape extending straight upward from the upper end portion of the shoulder portion 15 . A flange portion that protrudes radially outward and extends continuously over the entire circumferential length is formed at the upper end of the mouth of the inner container 12. The flange portion is placed on the upper opening edge of the mouth of the outer container 11.

[0024] A male threaded portion 18 to which a cap (not shown) is screwed, and a sealed protrusion 19 to which a peripheral wall portion of the cap (not shown) is fitted are formed from top to bottom on the outer peripheral surface of the mouth of the outer container 11. The sealed protrusion 19 protrudes radially outward from the mouth of the outer container 11 and extends continuously over the entire circumferential length. An airtight seal is formed between the outer peripheral surface of the sealed protrusion 19 and the inner peripheral surface of the peripheral wall portion of the cap (not shown). The cap may be fitted to the mouth of the outer container 11 by undercut fitting.

[0025] An outside air introduction hole 14 is formed at the mouth of the outer container 11 to introduce outside air between the outer container 11 and the inner container 12 as the content decreases. The outside air introduction hole 14 is located at the radially outermost part of the sealed protrusion 19, and is located above the sealing surface that extends continuously over the entire circumferential length. The position where the outside air introduction hole 14 is formed is not limited to the mouth of the outer container 11, but may be, for example, the body, shoulder, or bottom of the outer container 11 other than the mouth, or may be between the upper opening edge of the mouth of the outer container 11 and the underside of the flange portion of the mouth of the inner container 12, etc.

[0026] In this embodiment, the inner container 12 is provided with a whitened line portion 23A that has a width in the circumferential direction and extends in the container axis O direction in a portion located below the mouth portion. The number of whitened lines 23A may be one or more, preferably two to four. The range of whitened lines 23A in the direction of the container axis O may be changed as appropriate, for example, the whitened lines 23A may be provided only in the body portion. The whitened lines 23A are preferably provided in at least half of the squeezed region of the body portion in the direction of the container axis O. The circumferential width of the whitened line portion 23A is 5% or less of the circumferential length of the outer circumferential surface at the maximum outer diameter part of the body of the inner container 12. In the inner container 12, the whitened line portion 23A extends from the middle part of the shoulder portion in the container axis O direction, through the body portion, to the radial center part of the bottom wall of the bottom portion.

[0027] The crystallinity of the whitened line portion 23A at the same position along the wall thickness direction is uniform over the entire length in the direction of the container axis O. The maximum value of the crystallinity in the whitened line portion 23A is higher than the maximum value of the crystallinity in the shoulder and body portions of the inner container 12 excluding the whitened line portion 23A. In this application, the degree of crystallinity refers to the degree of both thermal crystallization and oriented crystallization. The crystallinity of the whitened line portion 23A may be different at different positions in the container axis O direction, even if the position along the wall thickness direction is the same.

[0028] The crystallinity of the whitened line portion 23A decreases from one of the inner and outer surfaces to the other of the inner and outer surfaces of the inner container 12. The proportion of the thickness of the thermally crystallized portion in the whitened line portion 23A is less than 35%. In the present application, the thermally crystallized portion means a portion having a haze value, which indicates the degree of cloudiness, of 10% or more. In the illustrated example, the crystallinity of the whitened line portion 23A decreases from the outer surface to the inner surface of the inner container 12. The thermally crystallized portion of the whitened line portion 23A is located between the outer surface of the inner container 12 and a depth position that is 35% of the wall thickness of the inner container 12.

[0029] The haze value of the whitened line portion 23A is 10% or more and 84% or less. This haze value is a numerical value including both the thermally crystallized portion located on the outer surface side of the inner container 12 and the portion other than the thermally crystallized portion located on the inner surface side of the inner container 12. The inner container 12 and the outer container 11 are made of a synthetic resin material that has a haze value of less than 10% when not thermally crystallized. The haze value can be measured using a color difference meter (SZ-Σ80-OS manufactured by Nippon Denshoku Industries Co., Ltd.). Note that the haze value is 90% or more at the mouth portion of a so-called PET bottle that is thermally crystallized (whitened).

[0030] The thickness of the thermally crystallized portion in the whitened line portion 23A is obtained by scraping off a fixed thickness of the inner or outer surface of the inner container 12, measuring the haze value each time by irradiating the exposed scraped-off surface with a light beam, and identifying the position in the thickness direction of the boundary where the haze value changes from 10% or more to less than 10%.

[0031] 2, the delaminating container 1 is formed by blow molding a preform 10 for a delaminating container, in which an inner preform 22 for forming an inner container 12 is inserted into an outer preform 21 for forming an outer container 11. The outer preform 21 and the inner preform 22 are each formed into a cylindrical shape with a bottom. The mouths of the outer preform 21 and the inner preform 22 do not stretch during blow molding, and the mouth of the outer preform 21 has a male threaded portion 18, a sealed protrusion 19, and an outside air introduction hole 14, similar to the mouth of the outer container 11.

[0032] The inner preform 22 has a whitened line portion 23B that has a width in the circumferential direction and extends in the direction of the container axis O in a portion located below the portion that will become the mouth of the inner container 12. The whitened line portion 23B is provided in a portion of the inner preform 22 that will stretch during blow molding. The circumferential width of the whitened line portion 23B is preferably 5% or less of the circumferential length of the outer circumferential surface of the body of the inner preform 22. The whitened line portion 23B extends downward from a portion of the inner preform 22 that will become the shoulder of the inner container 12, and extends radially inward from a portion that will become the bottom wall of the bottom of the inner container 12.

[0033] The crystallinity of the whitened line portion 23B at the same position along the wall thickness direction is uniform over the entire length in the direction of the container axis O. The maximum value of the crystallinity of the whitened line portion 23B is higher than the maximum value of the crystallinity of the portion of the inner preform 22 that will become the shoulder and body of the inner container 12, excluding the whitened line portion 23B. The crystallinity of the whitened line portion 23B may be different at different positions in the container axis O direction, even if the position along the wall thickness direction is the same.

[0034] The crystallinity of the whitened line portion 23B decreases from one of the inner and outer surfaces of the inner preform 22 to the other. The thermally crystallized portion accounts for less than 35% of the thickness of the whitened line portion 23B. The thermally crystallized portion has a haze value of 10% or more. In the illustrated example, the crystallinity of the whitened line portion 23B decreases from the outer surface to the inner surface of the inner preform 22. The thermally crystallized portion of the whitened line portion 23B is located between the outer surface of the inner preform 22 and a depth position that is 35% of the wall thickness of the inner preform 22. The haze value of the whitened line portion 23B is equal to or greater than 10% and equal to or less than 84%.

[0035] As described above, the inner preform 22 and the inner container 12 have substantially the same ratio of the thickness of the thermally crystallized portion in the thickness direction and substantially the same haze value in the whitened line portions 23A, 23B.

[0036] As described above, according to the peelable laminate container 1 of this embodiment, the maximum value of crystallinity in the whitened line portion 23A is higher than the maximum value of crystallinity in the shoulder and body portions of the inner container 12 excluding the whitened line portion 23A, so that the stiffness of the whitened line portion 23A is higher than the stiffness of the other portions of the inner container 12 located below the mouth portion. As a result, when the inner container 12 is reduced in volume due to a decrease in the contents, the other portions contract with the whitened line portion 23A of the inner container 12 acting as a pillar, so that it is possible to prevent the inner container 12 from being distorted in volume, and it is easy to secure an introduction space for outside air extending in the direction of the container axis O between the outer surface of the inner container 12 and the inner surface of the outer container 11, and it is possible to prevent the remaining amount of the contents from increasing.

[0037] Since the crystallinity of the whitened line portion 23A decreases from the outer surface toward the inner surface of the inner container 12, in the state of the peelable laminated container 1 obtained by blow molding the preform 10, the space between the inner surface of the outer container 11 and the outer surface of the inner container 12 is narrow, and it is clear that the whitened line portion 23A cannot be provided in the inner container 12. The only option is to provide the whitened line portion 23B, which will become the whitened line portion 23A, in the inner preform 22 for molding the inner container 12 before inserting it into the outer preform 21 for molding the outer container 11. The maximum crystallinity value in the whitened line portion 23B is higher than the maximum crystallinity value in the portion of the inner preform 22 that will become the shoulder and body of the inner container 12 excluding the whitened line portion 23B.

[0038] Then, when the inner preform 22 provided with the whitened line portion 23B is inserted into the outer preform 21 to obtain the preform 10, and then the preform 10 is blow molded, the whitened line portion 23B of the inner preform 22 becomes difficult to stretch. This makes it possible to make the whitened line portion 23A of the inner container 12 less likely to stick to the inner surface of the outer container 11; for example, even if the inner container 12 and the outer container 11 are made of the same material, the inner container 12 can be easily peeled off from the inner surface of the outer container 11 as the contents decrease; and because the whitened line portion 23A of the inner container 12 becomes thicker, when the inner container 12 reduces in volume as the contents decrease, other parts of the inner container 12 contract using the whitened line portion 23A of the inner container 12 as a pillar, preventing the inner container 12 from reducing in volume in an irregular manner. This makes it easier to secure a space for introducing outside air extending in the direction of the container axis O between the outer surface of the inner container 12 and the inner surface of the outer container 11, preventing the amount of remaining contents from increasing.

[0039] Since the crystallinity of the whitened line portion 23B decreases from one of the inner and outer surfaces of the inner preform 22 toward the other surface, the whitened line portion 23B can be formed by heat-treating the inner preform 22 from the one surface thereof to thermally crystallize it in a short time without thermally deteriorating the inner preform 22. Since the haze value of the whitened line portion 23B is 10% or more and 84% or less, it is possible to reliably obtain a peelable laminated container 1 that can prevent the inner container 12 from becoming difficult to peel from the inner surface of the outer container 11 as the contents decrease and prevents the amount of remaining contents from increasing. If the haze value of the whitened line portion 23B is less than 10%, the crystallinity in the whitened line portion 23B will be too low, making it difficult to suppress the stretching of the whitened line portion 23B during blow molding. If the haze value of the whitened line portion 23B exceeds 84%, the crystallinity in the whitened line portion 23B will be too high, and there is a risk that the whitened line portion 23B will not stretch and will tear during blow molding.

[0040] Since the ratio of the thickness of the thermally crystallized portion to the thickness of the whitened line portion 23B is less than 35%, it is possible to reliably prevent the whitened line portion 23B from breaking without being stretched during blow molding.

[0041] When an inner preform 22 in which the thickness ratio of the thermally crystallized portion of the whitened line portion 23B was 31.0% and the haze value of the whitened line portion 23B was 79.5% was used and blow molded together with an outer preform 21, a peelable laminate container 1 was obtained without tearing. However, when an inner preform in which the thickness ratio of the thermally crystallized portion of the whitened line portion 23B was 35.0% and the haze value of the whitened line portion 23B was 85.0%, it was confirmed that the inner container broke and no peelable laminate container was obtained.

[0042] The technical scope of the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention.

[0043] The crystallinity of the whitened line portion 23A may decrease from the inner surface of the inner container 12 toward the outer surface, and the crystallinity of the whitened line portion 23B may decrease from the inner surface of the inner preform 22 toward the outer surface. The crystallinity of the whitened line portions 23A and 23B may be the same throughout the entire area in the thickness direction. The haze value of the whitened line portions 23A and 23B and the ratio of the thickness of the thermally crystallized portion to the whitened line portions 23A and 23B are not limited to those in the above embodiment and may be appropriately changed.

[0044] In addition, within the scope of the invention, the components in the above-described embodiments may be replaced with well-known components, and the above-described embodiments and the above-described variations may be combined as appropriate. [Explanation of symbols]

[0045] 1. Delaminated container 10. Preform for delaminating container 11 Outer container 12 Inner container 13 Mouth 15 Shoulder 16 Torso 17 Bottom 21 Outer preform 22 Preform inside 23A, 23B Whitening line O Container axis

Claims

1. The container has an inner container which undergoes volume reduction deformation as the amount of content contained therein decreases, and an outer container in which the inner container is placed in a stacked state, the container having a cylindrical mouth, a cylindrical shoulder, a cylindrical body, and a cup-shaped bottom, which are arranged in this order from top to bottom along the container axial direction, The inner container has a whitened line portion that has a width in the circumferential direction and extends in the container axial direction in a portion located below the mouth portion, A peelable laminated container, in which the maximum crystallinity value in the whitened line portion is higher than the maximum crystallinity value in the portions excluding the whitened line portion in each of the shoulder portion and the body portion of the inner container.

2. 2. The delamination container according to claim 1, wherein the degree of crystallinity of the whitened line portion decreases from the outer surface toward the inner surface of the inner container.

3. A preform for molding a delaminating container, comprising an inner container which undergoes volumetric deformation as the amount of content contained therein decreases, and an outer container in which the inner container is placed in a stacked state, the preform having a cylindrical mouth, a cylindrical shoulder, a cylindrical body, and a cup-shaped bottom, which are arranged in this order from top to bottom along the container axial direction, a bottomed cylindrical inner preform for molding the inner container; A bottomed cylindrical outer preform for molding the outer container, The inner preform is inserted into the outer preform, In the inner preform, a whitening line portion having a width in a circumferential direction and extending in an axial direction of the container is provided in a portion located below a portion that will become a mouth portion of the inner container, A preform for a peelable laminated container, in which the maximum crystallinity value in the whitened line portion is higher than the maximum crystallinity value in the portion of the inner preform that will become the shoulder and body portion of the inner container, excluding the whitened line portion.

4. the crystallinity of the whitened line portion decreases from one of the inner surface and the outer surface of the inner preform to the other surface, The delaminating container preform according to claim 3, wherein the haze value of the whitened line portion is 10% or more and 84% or less.

5. 5. The delaminating container preform according to claim 4, wherein the ratio of the thickness of the thermally crystallized portion to the thickness of the whitened line portion is less than 35%.

Citation Information

Patent Citations

  • Double structure vessel having excellent regular contractility of inner bag vessel

    JP2019142186A