Positive electrode material, manufacturing method thereof, and zinc negative electrode secondary battery
A carbon material with a tailored interlayer distance in the positive electrode of zinc negative electrode secondary batteries addresses the challenges of dendrite formation and capacity limitations, achieving high energy density and stable cycling through interlayer ion storage.
Patent Information
- Application Number
- JP2023074723
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing zinc negative electrode secondary batteries face challenges in suppressing zinc dendrite formation and achieving high capacity and cycle characteristics due to the limitations of current positive electrode materials, particularly when using aqueous or organic electrolytes.
A positive electrode material with a carbon material having a layered structure and specific interlayer distance, combined with an aqueous electrolyte, facilitates ion storage through interlayer insertion and surface adsorption, enhancing energy density and cycle stability.
The proposed electrode material enables a zinc negative electrode secondary battery with high capacity, high energy density, and improved cycle characteristics by allowing smooth ion insertion and desorption, effectively suppressing zinc dendrite formation.
Smart Images

Figure 2024159011000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode material for a zinc negative electrode secondary battery, a method for producing the same, and a zinc negative electrode secondary battery using the positive electrode material. [Background technology]
[0002] Zinc negative electrode secondary batteries, which use zinc (theoretical capacity 820 mAh / g), an abundant and easily available resource, as the negative electrode, are low-cost, have a relatively high energy density, and are also excellent in safety. One of the issues with zinc negative electrode secondary batteries is how to suppress the formation of zinc dendrites at the negative electrode during charging. As electrolytes for suppressing the formation of dendrites while proceeding with charging and discharging, the use of aqueous electrolytes such as concentrated zinc chloride aqueous solutions and concentrated alkaline aqueous solutions, and organic electrolytes such as an acetonitrile solution of zinc bis(trifluoromethylsulfonyl)imide (Zn(TFSI)2) has been considered (see Patent Documents 1 and 2, and Non-Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-173005 [Patent Document 2] Special Publication No. 2016-513354 [Non-patent literature]
[0004] [Non-Patent Document 1] Y. Zeng et al., Advanced Materials, 29, 1700274 (2017) [Non-Patent Document 2] N. Zhang et al., ACS Appl. Mater. Interfaces, 11, 32978-32986 (2019) Summary of the Invention [Problem to be solved by the invention]
[0005] When using an aqueous electrolyte, the positive electrode active material is, for example, Ni(OH)2, MnO2, Ag2O, etc., but there are problems such as a not very large capacity and poor cycle characteristics.
[0006] In addition, although Patent Document 1 uses activated carbon as the positive electrode material, the capacity and cycle characteristics are not confirmed. Furthermore, Patent Document 2 uses a nanocarbon material as the positive electrode material, but the reported capacity exceeding 1000 mAh / g is C, which exceeds LiC6. 4.4 This corresponds to the composition of Zn. The energy density is too high in this result, and it is considered that the effect of other factors such as the reaction of the current collector is actually influenced, and the reliability is lacking. In addition, Patent Document 2 does not show any specific results regarding the cycle characteristics.
[0007] In Non-Patent Document 2, which uses an organic electrolyte, graphite is used as the positive electrode material, and cycle stability has been confirmed, but the capacity is still small at present.
[0008] Therefore, an object of the present disclosure is to provide a positive electrode material for a zinc negative electrode secondary battery that has high capacity and high cycle characteristics and can be stably charged and discharged at a high energy density, a manufacturing method thereof, and a zinc negative electrode secondary battery using the positive electrode material. [Means for solving the problem]
[0009] In order to solve the above problems, one embodiment of the positive electrode material disclosed herein is a positive electrode material for a zinc negative electrode secondary battery, which contains a carbon material having a layered structure as a positive electrode active material, and the interlayer distance of the carbon material is greater than the interlayer distance of graphite, which is 0.335 nm, and less than 0.66 nm.
[0010] For example, in Patent Document 1, activated carbon is used as the positive electrode active material and a concentrated zinc chloride aqueous solution is used as the electrolyte. In this battery system, the reaction 2ZnCl2 → ZnCl4 - +Zn 2+The complex formation proceeds by the reaction of ZnCl x - Ions such as , , and , are generated. It is believed that the ions are then adsorbed onto the surface of the activated carbon, which is how electricity storage progresses. However, since activated carbon only stores ions by surface adsorption, a large capacity cannot be expected.
[0011] In contrast, in the positive electrode material of the present invention, ions are stored between the layers of the carbon material by interlayer insertion in addition to surface adsorption, and thus electricity storage progresses.
[0012] In particular, if the interlayer distance of the carbon material is too large, ions may not remain between the layers, making it difficult for the charging reaction to proceed, whereas if the interlayer distance of the carbon material is too small, it becomes difficult for ions to be inserted between the layers, making it difficult for the charging reaction to proceed.
[0013] In this regard, the carbon material of this configuration has an interlayer distance that is greater than the interlayer distance of graphite, which is 0.335 nm (J. Inamoto, et al., J. Electrochem. Soc., 2021, 168, 010528), and is less than 0.66 nm, so that the insertion and desorption of ions proceed smoothly. As a result, a zinc negative electrode secondary battery with high capacity and high cycle characteristics that can be stably charged and discharged at high energy density can be obtained.
[0014] The interlayer distance of the carbon material is preferably 0.345 nm or more and 0.50 nm or less.
[0015] When the interlayer distance of the carbon material satisfies the above range, the insertion and desorption of ions proceeds more smoothly, which is further advantageous in obtaining a zinc negative electrode secondary battery with high capacity and high cycle characteristics.
[0016] The carbon material preferably contains, as its constituent elements, a carbon atom and an oxygen atom covalently bonded to the carbon atom.
[0017] Carbon materials are not easily oxidized, so a high voltage is usually required to insert ions into them.
[0018] In contrast, the carbon material of the present invention is a partially oxidized carbon material, and therefore has a lower ion insertion potential than, for example, graphite, which is made only of carbon atoms. In addition, the carbon material of the present invention contains covalent oxygen atoms, and therefore has a larger interlayer distance than graphite, etc. Thus, ion insertion and desorption become easier, and the charge / discharge reaction of the carbon material is facilitated.
[0019] The content of the oxygen atoms contained in the carbon material is preferably less than 38 atomic %.
[0020] If the oxygen atom content is 38 atomic % or more, the interlayer distance of the carbon material becomes too large, making it difficult to store ions, and the charging reaction may not proceed. By keeping the oxygen atom content within the above range, a zinc negative electrode secondary battery with high capacity and high cycle characteristics can be obtained.
[0021] The content of the oxygen atoms contained in the carbon material is more preferably 2 atomic % or more and 30 atomic % or less.
[0022] If the oxygen atom content is less than 2 atomic %, the ion insertion potential is high and the interlayer distance is small, which may make it difficult for the charging reaction to proceed. By keeping the oxygen atom content within the above range, it is further advantageous to obtain a zinc negative electrode secondary battery with high capacity and high cycle characteristics.
[0023] One embodiment of the method for producing the positive electrode material disclosed herein is a method for producing the above-mentioned positive electrode material, in which graphite powder is oxidized and then heat-treated at a temperature of 200° C. or higher and 800° C. or lower to obtain the carbon material.
[0024] Graphite oxide is obtained by oxidizing graphite powder. When graphite oxide is subjected to heat treatment, some of the oxygen atoms in the graphite oxide are removed, and nanometer-order holes are formed in the layers. In the layered compound obtained in this way, some of the carbon atoms are oxidized, and the layers have holes, so that the ion insertion potential is lower than that of graphite, making it easier to insert ions. This makes it easier for the charging reaction of the carbon material to proceed.
[0025] One embodiment of the zinc negative electrode secondary battery disclosed herein comprises a positive electrode, a negative electrode, and an electrolyte disposed between the positive electrode and the negative electrode, the positive electrode including the positive electrode material described above.
[0026] According to this configuration, a zinc negative electrode secondary battery having higher capacity and higher cycle characteristics than conventional zinc negative electrode secondary batteries can be obtained.
[0027] The electrolytic solution is preferably an aqueous electrolytic solution.
[0028] According to this configuration, it is possible to effectively suppress the formation of zinc dendrites, thereby providing a zinc negative electrode secondary battery with high capacity and high cycle characteristics. Effect of the Invention
[0029] As described above, in the positive electrode material of the present disclosure, ions are stored between the layers of the carbon material by intercalation in addition to surface adsorption, and thus charging proceeds. This allows for a zinc negative electrode secondary battery with high capacity and high cycle characteristics that can be stably charged and discharged at a high energy density. [Brief description of the drawings]
[0030] [Figure 1] FIG. 1 is a diagram showing the configuration of a zinc negative electrode secondary battery according to one embodiment. [Diagram 2] FIG. 1 is a diagram showing an example of the molecular structure of graphene-like graphite. [Diagram 3] 4 is a graph showing charge / discharge curves of a battery cell in Experimental Example 1. [Figure 4]13 is a graph showing charge / discharge curves of a battery cell in Experimental Example 2. [Diagram 5] 13 is a graph showing charge / discharge curves of a battery cell in Experimental Example 3. [Figure 6] 13 is a graph showing charge / discharge curves of a battery cell in Experimental Example 4. [Figure 7] 13 is a graph showing charge / discharge curves of a battery cell in Experimental Example 5. [Figure 8] 13 is a graph showing charge / discharge curves of a battery cell in Experimental Example 6. [Figure 9] 13 is a graph showing charge / discharge curves of a battery cell in Experimental Example 8. [Figure 10] 4 is a graph showing a charge / discharge curve of the battery cell of Reference Example 1. [Figure 11] 6 is a graph showing charge / discharge curves of a battery cell of Reference Example 2. [Figure 12] 13 is a graph showing a charge / discharge curve of a battery cell of Reference Example 3. [Figure 13] 13 is a graph showing a charge / discharge curve of a battery cell of Reference Example 4. [Figure 14] 13 is a graph showing charge / discharge curves of a battery cell of Reference Example 5. [Figure 15] 1 is a graph showing the relationship between the interlayer distance and the oxygen content of the carbon materials used in the Experimental Examples and the Reference Examples. [Figure 16] 1 is a graph showing a charging curve of a battery cell of a test example. [Figure 17] 16 is a graph showing the results of X-ray diffraction measurement of GLG300 before charging (P0) and at points P1 to P4 in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings. The following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present disclosure, its application, or its uses.
[0032] <Zinc negative electrode secondary battery> As shown in Fig. 1, a zinc negative electrode secondary battery 100 (hereinafter also simply referred to as "battery 100") according to the present disclosure includes a positive electrode 110, a negative electrode 120, and an electrolyte 130 disposed between the positive electrode 110 and the negative electrode 120 so as to be in contact with both of them. The positive electrode 110 has a positive electrode active material layer 111 (positive electrode material) and a positive electrode current collector 112 that collects current from the positive electrode active material layer 111. The negative electrode 120 has a negative electrode active material layer 121 (negative electrode material) and a negative electrode current collector 122 that collects current from the negative electrode active material layer 121.
[0033] The constituent material of the positive electrode current collector 112 and the negative electrode current collector 122 (both may be collectively referred to as "current collectors" in this specification) is not particularly limited as long as it is a conductive material. Specific examples of the current collector that can be used include aluminum (Al), other metal current collectors used in known secondary batteries, and resin current collectors having a conductive resin layer. Examples of the shape of the current collector include foil, mesh, and porous shapes.
[0034] 1, the battery 100 may have a battery case that houses the positive electrode 110, the negative electrode 120, and the electrolyte 130, and a separator disposed between the positive electrode 110 and the negative electrode 120. The material, shape, and other configurations of the battery case are not particularly limited, and may be of a known configuration that is generally adopted in secondary batteries. The separator is not particularly limited, and may be of a known configuration such as a porous resin film or ceramics.
[0035] The shape of the battery 100 in the present disclosure is not particularly limited, and any known shape such as a coin type, a laminate type, a cylindrical type, or a rectangular type can be used.
[0036] Battery 100 in the present disclosure is a secondary battery that can be repeatedly charged and discharged, and is useful, for example, as an in-vehicle battery, a stationary battery, a medical battery, a consumer battery, and the like.
[0037] [Negative electrode active material layer] The negative electrode active material layer 121 includes a negative electrode active material. The negative electrode active material includes at least one of zinc and a zinc alloy. The negative electrode active material can be, for example, at least one of zinc powder and zinc alloy powder. In addition, a foil-shaped, mesh-shaped, or porous pure metal zinc or zinc alloy may be used as the negative electrode 120, serving as both the negative electrode active material layer 121 and the negative electrode current collector 122.
[0038] The negative electrode active material layer 121 may further contain at least one of a conductive assistant and a binder, as necessary. The conductive assistant is not particularly limited as long as it is a material having electronic conductivity, and may be, for example, a material generally known in zinc negative electrode secondary batteries, such as acetylene black, carbon black, graphene, etc. The binder is not particularly limited, and may be a material generally known in zinc negative electrode secondary batteries, such as a fluorine-based binder, such as polyvinylidene fluoride or polytetrafluoroethylene.
[0039] The contents of the negative electrode active material and the conductive assistant in the negative electrode active material layer 121 are not particularly limited and may be amounts generally known in zinc negative electrode secondary batteries. Specifically, for example, the content of the negative electrode active material may be 10% by mass or more and 90% by mass or less, and the content of the conductive assistant may be 20% by mass or less.
[0040] The method for forming the negative electrode active material layer 121 is not particularly limited, and the layer can be manufactured by a known method.
[0041] [Electrolyte] The electrolyte solution 130 is disposed between the positive electrode active material layer 111 and the negative electrode active material layer 121 so as to be in contact with both of them. The electrolyte solution 130 contains an electrolyte and a solvent, and may be an aqueous electrolyte solution or an organic electrolyte solution.
[0042] The electrolyte is not particularly limited, and may be any known material generally used in zinc negative electrode secondary batteries.Specific examples of the electrolyte include zinc halides such as zinc chloride and zinc bromide, alkaline agents such as potassium hydroxide and sodium hydroxide, and salts such as zinc bis(trifluoromethylsulfonyl)imide (Zn(TFSI)2).
[0043] The solvent may be either water or an organic solvent, and the organic solvent may be a known material that is generally used in zinc negative electrode secondary batteries, such as acetonitrile.
[0044] The electrolyte 130 is preferably an aqueous electrolyte, and more preferably at least one of a concentrated zinc halide aqueous solution and a concentrated alkaline aqueous solution. This makes it possible to effectively suppress the formation of zinc dendrites at the negative electrode during charging. In the case of a concentrated zinc halide aqueous solution, the concentration can be, for example, ZnCl2:H2O in terms of substance ratio of 2:8 to 2:3. In the case of a concentrated alkaline aqueous solution, the concentration can be, for example, 6 mol / dm 3 ~10mol / dm 3 It can be said that:
[0045] The electrolyte 130 may be in liquid form or in other forms, such as a gel.
[0046] [Cathode active material layer] The positive electrode active material layer 111 contains a carbon material having a layered structure as a positive electrode active material. The carbon material having a layered structure has a predetermined interlayer distance as described later. The carbon material functions as a host material for ions.
[0047] The only reported use of activated carbon with a high specific surface area that mainly utilizes the adsorption reaction of ions is that of Patent Document 1. In the example using activated carbon, ions are only stored by surface adsorption, and large capacity cannot be expected.
[0048] In this regard, it is known that various ions are inserted between adjacent carbon layers of carbon materials having a layered structure, which may contribute to high capacity. However, in a battery system using zinc as the negative electrode and, particularly, an aqueous electrolyte, the decomposition reaction of the electrolyte proceeds at a lower potential than the insertion reaction of ions into the carbon material. For this reason, there are virtually no reports of using a carbon material having a layered structure as a positive electrode active material in such a battery system.
[0049] In contrast, in the positive electrode material of the present invention, ions are stored on the surface and between the layers of the carbon material by surface adsorption and intercalation at a potential lower than the potential at which the decomposition reaction of the electrolyte proceeds, and thus electricity storage proceeds. Thus, a zinc negative electrode secondary battery with high capacity and high cycle characteristics that can be stably charged and discharged at a high energy density can be obtained.
[0050] Specific examples of the carbon material include graphene-like graphite (also referred to as "GLG" in this specification) described below, carbon materials containing GLG, soft carbon heat-treated at low to medium temperatures, hard carbon, Ketjen black, carbon black, etc., and preferably GLG or carbon materials containing GLG.
[0051] Specific examples of carbon materials containing GLG include mixtures of GLG and other carbon materials, and layered compounds having an outer layer made of GLG and an inner layer made of graphite.
[0052] An example of the molecular structure of GLG is shown in Figure 2. As shown in Figure 2, GLG, designated by the reference numeral 20, is a layered compound whose constituent elements are carbon atom 21 and oxygen atom 22 bonded to the carbon atom 21 by a covalent bond, and has nanometer-order holes 23 formed in the layer. GLG can be prepared by subjecting graphite oxide (GO) to a heat treatment. It is believed that some of the carbon atoms in the graphite are replaced by oxygen atoms by the oxidation of the graphite, and some of the oxygen atoms are removed by the heat treatment to form the holes 23.
[0053] Carbon materials are not easily oxidized, so a high voltage is usually required to insert ions. In contrast, GLG has a layered structure similar to graphite, but since it is a partially oxidized carbon material, the ion insertion potential is lower than that of carbon materials such as graphite, which is made up of only carbon atoms. This makes it easier for ions to be inserted, and the charging reaction of the carbon material progresses more easily.
[0054] The interlayer distance of the carbon material is larger than that of graphite. As mentioned above, the interlayer distance of graphite is generally known to be 0.335 nm. Since the interlayer distance is larger than that of graphite, ions can be easily inserted and removed, which is advantageous in obtaining a zinc negative electrode secondary battery with high capacity and high cycle characteristics. For example, since GLG contains covalent oxygen atoms derived from graphite oxide, the interlayer distance tends to be larger than that of graphite, and both cations and anions are easily inserted. Therefore, it is desirable to use GLG or a carbon material containing GLG as the positive electrode active material from the viewpoint of having a larger interlayer distance than graphite.
[0055] Specifically, the interlayer distance of the carbon material is more than 0.335 nm and less than 0.66 nm, preferably 0.345 nm or more and 0.50 nm or less, and more preferably 0.37 nm or more and 0.45 nm or less.
[0056] If the interlayer distance of the carbon material is too large, ions do not remain between the layers, and the charging reaction may not proceed easily. If the interlayer distance of the carbon material is too small, it is difficult for ions to be inserted between the layers, and the charging reaction may not proceed easily. If the interlayer distance of the carbon material satisfies the above range, ions can be easily inserted and removed, which is advantageous in obtaining a zinc negative electrode secondary battery with high capacity and high cycle characteristics.
[0057] The content of oxygen atoms in GLG is preferably more than 0 atomic % and less than 38 atomic %, more preferably from 2 atomic % to 30 atomic %, even more preferably from 6 atomic % to 15 atomic %, and particularly preferably from 8 atomic % to 13 atomic %.
[0058] In GLG, if the content of oxygen atoms is too high, the interlayer distance of GLG becomes too large, making it difficult to store ions and preventing the charging reaction from proceeding. In addition, if the content of oxygen atoms is insufficient in GLG, the interlayer distance becomes small and the ion insertion potential becomes high, making it difficult to proceed with the charging and discharging reaction. By having the content of oxygen atoms in the above range, the carbon material is more advantageous in obtaining a zinc negative electrode secondary battery with high capacity and high cycle characteristics.
[0059] The positive electrode active material layer 111 may further contain at least one of a conductive assistant and a binder, if necessary. As the conductive assistant, binder, etc., the same materials as those in the negative electrode active material layer 121 can be used. When the conductive assistant, binder, etc. are blended in the positive electrode active material layer 111, the contents thereof can be the same as those in the negative electrode active material layer 121.
[0060] [Charge / discharge characteristics] In order to suppress the decomposition reaction of the electrolyte and promote the charging reaction, the initial (first cycle) charging potential is set to Zn 2+ The potential versus Hg / Zn is preferably 1.95 V or less, more preferably 1.8 V or less, and particularly preferably 1.7 V or less. When the electrolyte is an aqueous potassium hydroxide solution, the potential versus Hg / HgO is preferably 0.3 V or less, and more preferably 0 V or less.
[0061] The initial charge capacity is preferably 5 mAh / g or more, more preferably 30 mAh / g or more, and particularly preferably 100 mAh / g or more.
[0062] The initial discharge capacity is not limited, but is preferably 10 mAh / g or more, and more preferably 20 mAh / g or more.
[0063] The charge capacity at the fifth cycle is preferably 5 mAh / g or more, more preferably 30 mAh / g or more, and particularly preferably 100 mAh / g or more.
[0064] The discharge capacity at the fifth cycle is preferably 4 mAh / g or more, more preferably 30 mAh / g or more, and particularly preferably 100 mAh / g or more.
[0065] In addition, when the capacity is extremely large beyond the theoretical capacity, there is a possibility that reactions other than the insertion and desorption of ions into and from the carbon material, specifically, other reactions such as the decomposition reaction of the electrolyte and the decomposition reaction of the carbon material, are proceeding. Such reactions cause deterioration of the battery and lead to a decrease in cycle stability. Although there is no upper limit for the capacity, it is preferable that it is, for example, less than 1000 mAh / g from the viewpoint of suppressing the progress of such other reactions.
[0066] The initial coulomb efficiency is preferably 5% or more, more preferably 15% or more, and particularly preferably 20% or more.
[0067] The coulomb efficiency in the fifth cycle is preferably 10% or more, more preferably 20% or more, further preferably 40% or more, and particularly preferably 60% or more.
[0068] Although the Coulombic efficiency may exceed 100%, if the Coulombic efficiency is extremely high, other reactions such as the above-mentioned decomposition reaction of the electrolyte and the decomposition reaction of the carbon material may be proceeding. The upper limit of the Coulombic efficiency is not limited, but from the viewpoint of suppressing the proceeding of such other reactions, it may be set to, for example, 110% or less.
[0069] <Manufacturing method of zinc negative electrode secondary battery> The manufacturing method of a zinc negative electrode secondary battery, with respect to the steps other than the manufacturing method of the GLG described below, is not particularly limited as long as the above-mentioned positive electrode 110, negative electrode 120, and electrolyte 130 are used, and any known method can be used.
[0070] In addition, when the active material layer, i.e., the positive electrode active material layer 111 and the negative electrode active material layer 121, contains other components such as a conductive assistant and a binder, the active material layer is obtained by mixing these and forming a layer on a current collector. The method of mixing the components is not particularly limited, and known methods such as manual mixing using a mortar or the like, or a mixer, can be used. The method of forming the layer is also not particularly limited, and a layer formation method by a wet method or a dry method usually used in zinc negative electrode secondary batteries can be used.
[0071] [GLG Manufacturing Method] GLG can be obtained, for example, by oxidizing graphite powder to obtain graphite oxide, and then subjecting the graphite oxide to a heat treatment.
[0072] First, graphite powder is oxidized to obtain graphite oxide (GO). The method of oxidizing graphite is not particularly limited, and any known method can be used. Examples of known methods include the Brodie method using fuming nitric acid and KClO3, the Hummers method using H2SO4, NaNO3, and KMnO4, and the Staudenmeier method using H2SO4, HNO3, and KClO3. The graphite oxidation method affects the oxygen content and interlayer distance of GLG.
[0073] Next, the graphite oxide is subjected to a heat treatment. This removes some of the oxygen atoms in the graphite oxide, and nanometer-order holes are formed in the layers. The heat treatment temperature of the graphite oxide also affects the oxygen content and interlayer distance of the GLG. The heat treatment temperature is 200°C or higher and 800°C or lower, more preferably 220°C or higher and 450°C or lower, and particularly preferably 250°C or higher and 400°C or lower.
[0074] The heat treatment time for the graphite oxide is not intended to be limited, but may be, for example, 2 hours or more, preferably 3 hours or more and 10 hours or less, and more preferably 4 hours or more and 8 hours or less.
[0075] The heat treatment of the graphite oxide is preferably carried out in a vacuum or in an inert gas atmosphere in order to prevent further oxidation.
[0076] <Experimental and Reference Examples> Next, specific experimental examples and reference examples will be described.
[0077] Table 1 shows the configurations of the carbon materials and electrolyte solutions in Experimental Examples 1 to 12 and Reference Examples 1 to 6, as well as the results of charge / discharge measurements.
[0078] [Table 1]
[0079] [Preparation of GLG] 10 g of graphite powder (Z-5F, average particle size 5 μm, manufactured by Ito Graphite Industries Co., Ltd.) was placed in a 500 mL beaker, 200 mL of fuming nitric acid was added, and the mixture was heated to 60 ° C. Then, 80 g of potassium chlorate was slowly added while stirring, and the mixture was kept for 3 hours. The reaction solution was then transferred to 2 L of water, suction filtered, and washed with pure water until the pH was 5 or higher to obtain graphite oxide (GO) (Brodie method).
[0080] The obtained GO was dried overnight at 60°C. The GO powder was placed in an alumina container, and the temperature was raised to a predetermined heat treatment temperature T (°C) at 1°C / min under vacuum, and then held for 5 hours to obtain GLG. In this specification, GLG obtained by treatment at heat treatment temperature T (°C) may be referred to as "GLGT" (for example, GLG obtained at a heat treatment temperature of 300°C may be referred to as "GLG300").
[0081] The identification of GLG and the measurement of the interlayer distance were performed by X-ray diffraction (D2 Phaser, CuKα, manufactured by Bruker).
[0082] The oxygen content in GLG was determined by elemental analysis (Flash Smart, ThermoFischer Scientific).
[0083] [Preparation of electrolyte] The zinc chloride aqueous solution was prepared by dissolving zinc chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 99.9%) in water so that the ratio of substances was ZnCl2:H2O = 3:7. The alkaline aqueous solution was prepared by dissolving potassium hydroxide (manufactured by Nacalai Tesque, 99%) in water so that the concentration was 8 mol / dm 3 The zinc chloride and zinc bromide aqueous solution was prepared in the same manner as the zinc chloride aqueous solution, except that zinc chloride and zinc bromide (Fujifilm Wako Pure Chemical Industries, Ltd., 99.9%) were mixed in a ratio of 1:0.09 instead of zinc chloride.
[0084] [Battery manufacturing] GLG, acetylene black (AB, Denka Co., Ltd.), and polyvinylidene fluoride (PVdF, Kureha Co., Ltd.) were mixed in a mortar in a mass ratio of 18:1:1, and pressed against a titanium mesh at 118 MPa for 15 minutes to prepare a working electrode (positive electrode). When an aqueous zinc chloride solution was used as the electrolyte, zinc metal was used for the counter electrode (negative electrode) and reference electrode. When an alkaline aqueous solution was used as the electrolyte, a mixture of AB and PVdF mixed in a mortar in a mass ratio of 8:2 was pressed against a nickel mesh at 118 MPa for 15 minutes to prepare a counter electrode, and a reference electrode was prepared by pressing a mixture of 1 mol / dm 3 A mercury / mercury oxide electrode using a KOH solution of 10000g was used. These electrodes were attached to a cell (homemade) and filled with a zinc chloride solution or an alkaline solution to construct a three-electrode cell.
[0085] [Charge / discharge measurement] Charge and discharge measurements were performed using a potentiostat / galvanostat (manufactured by Hokuto Denko). In the case of zinc chloride aqueous solution, the current density was 20mAh / g, the cutoff voltage was 0.5V at the lower limit and 2.4V at the upper limit. In the case of alkaline aqueous solution, the current density was 100mAh / g, the cutoff voltage was -1.2V at the lower limit and 0.4V at the upper limit. The measurement temperature was 30℃.
[0086] [X-ray diffraction measurement] The identification of GLG and the measurement of the interlayer distance were performed by X-ray diffraction (D2 Phaser, CuKα, manufactured by Bruker).
[0087] [Elemental analysis measurement] The oxygen content in GLG was determined by elemental analysis (Flash Smart manufactured by ThermoFischer Scientific). In Table 1, the oxygen content values of GLG250, GLG400, GLG500, and GLG800 are estimated values based on the relationship between the interlayer distance and the oxygen content of GO and various GLGs obtained by X-ray diffraction measurement and elemental analysis measurement.
[0088] [Experimental Examples 1-6] As shown in Table 1, the batteries of Experimental Examples 1 to 6 were manufactured using GLG prepared as the carbon material of the positive electrode active material at heat treatment temperatures T of 250°C, 300°C, 400°C, 500°C, 700°C, and 800°C, respectively, and an aqueous zinc chloride solution as the electrolyte, and charge / discharge measurements were performed. The charge / discharge curves of the batteries are shown in Figs. 3 to 8.
[0089] [Experimental Examples 7-11] As shown in Table 1, the batteries of Experimental Examples 7 to 11 were manufactured using GLG prepared at heat treatment temperatures T of 250°C, 300°C, 400°C, 500°C, and 700°C as the carbon material of the positive electrode active material, and an aqueous potassium hydroxide solution as the electrolyte, and charge / discharge measurements were performed. The charge / discharge curve of the battery of Experimental Example 8 is shown in FIG.
[0090] [Experimental Example 12] A battery was manufactured using GLG prepared at a heat treatment temperature of 300°C as the carbon material for the positive electrode active material, and an aqueous solution of zinc chloride and zinc bromide as the electrolyte, and charge / discharge measurements were performed.
[0091] [Reference examples 1 and 2] The batteries of Reference Examples 1 and 2 were manufactured using commercially available acetylene black (manufactured by Denka Co., Ltd.) as the carbon material and an aqueous zinc chloride solution and an aqueous potassium hydroxide solution as the electrolyte, respectively, and charge / discharge measurements were performed. The charge / discharge curves of Reference Examples 1 and 2 are shown in Figs. 10 and 11.
[0092] [Reference examples 3 and 4] The batteries of Reference Examples 3 and 4 were manufactured using the above-mentioned graphite powder, which is the raw material of GLG, as the carbon material and an aqueous zinc chloride solution and an aqueous potassium hydroxide solution as the electrolyte, respectively, and were subjected to charge / discharge measurements. The charge / discharge curves of Reference Examples 3 and 4 are shown in FIG. 12 and FIG. 13.
[0093] [Reference examples 5 and 6] The batteries of Reference Examples 5 and 6 were manufactured using the above-mentioned graphite oxide (GO) powder as the carbon material and an aqueous zinc chloride solution and an aqueous potassium hydroxide solution as the electrolyte, respectively, and were subjected to charge / discharge measurements. The charge / discharge curve of Reference Example 5 is shown in FIG.
[0094] <Charge / discharge characteristics> 3 to 9 and Table 1, it was found that the battery cells of Experimental Examples 1 to 12 exhibited charge / discharge behavior with large capacity and excellent cycle characteristics. In particular, in the systems in which GLG250, GLG300, and GLG400 of Experimental Examples 1 to 3 were used as the positive electrode active material and an aqueous zinc chloride solution was used as the electrolyte, the capacity at the 5th cycle was 100 mAh / g or more and the Coulombic efficiency at the 5th cycle was 90% or more, indicating that the batteries could function as zinc negative electrode secondary batteries with high capacity, high cycle characteristics, and high Coulombic efficiency.
[0095] Specifically, in the battery cell (GLG300, zinc chloride aqueous solution) of Experimental Example 2 shown in FIG. 4, the potential began to rise from about 1.45 V in the first cycle of charging, and rose gradually from about 1.6 V, and the initial charging capacity reached 430 mAh / g. During discharging, the potential gradually dropped from about 1.3 V, and the initial discharging capacity was 180 mAh / g. In the second cycle of charging, the reaction initiation potential dropped to 0.53 V, and the capacity was 181 mAh / g. The discharging reaction in the second cycle started at 1.3 V, which was almost the same as in the first cycle. The discharging capacity was 130 mAh / g, and the coulombic efficiency was 72%. In the fifth cycle, the discharging potential dropped to 1.2 V, but the coulombic efficiency rose and reached 87%.
[0096] In addition, the battery cell of Experimental Example 8 (GLG300, potassium hydroxide aqueous solution) shown in FIG. 9 had a smaller capacity than the battery cell of Experimental Example 2 using a zinc chloride aqueous solution, but it was found to show similar charge / discharge behavior.
[0097] On the other hand, in the system of Reference Example 1 in which acetylene black was used as the positive electrode active material and an aqueous zinc chloride solution was used as the electrolyte, as shown in FIG. 10, the potential rose rapidly to 2.0 V during charging, but thereafter the potential did not rise, remaining at around 2.05 V. This is thought to be due to the progress of the decomposition reaction of the electrolyte. When the capacity reached 865 mAh / g, charging was stopped and discharging was started, but the obtained discharge capacity was as small as 25 mAh / g. In addition, neither charging nor discharging was possible after the second cycle.
[0098] In the system of Reference Example 2 in which acetylene black was used as the positive electrode active material and potassium hydroxide aqueous solution was used as the electrolyte, almost no capacity was obtained in the first cycle of charging, as shown in FIG. 11. During discharge, the potential dropped sharply from 0.1 V, and after a potential plateau appeared at -0.38 V, it dropped again. The obtained discharge capacity was very small, at 2.25 mAh / g. After the second cycle, neither charging nor discharging was possible.
[0099] Furthermore, in the system of Reference Example 3 in which graphite was used as the positive electrode active material and an aqueous zinc chloride solution was used as the electrolyte, the initial charging potential was as high as 1.92 V, which is considered to be due to the progress of the decomposition reaction of the electrolyte, as shown in Fig. 12. When the initial capacity reached 2816 mAh / g, charging was stopped and discharging was started, but the obtained discharge capacity was as small as 42.6 mAh / g.
[0100] In the system of Reference Example 4 in which graphite was used as the positive electrode active material and an aqueous potassium hydroxide solution was used as the electrolyte, it is believed that the decomposition reaction of the electrolyte proceeded during the initial charging, as shown in Fig. 13. When the initial capacity reached 2327 mAh / g, charging was stopped and discharging was started, but the obtained discharge capacity was as small as 14.5 mAh / g.
[0101] In addition, in the system of Reference Example 5 in which graphite oxide was used as the positive electrode active material and zinc chloride aqueous solution was used as the electrolyte, charging in the first cycle was not possible, as shown in FIG. 14. When discharging in the first cycle was performed, the decomposition reaction of GO probably proceeded, and a large capacity was observed. In the subsequent charging reaction, the decomposition reaction of the electrolyte proceeded. Moreover, charging and discharging became impossible after the third cycle.
[0102] <Relationship between interlayer distance and oxygen content of carbon materials> FIG. 15 is a graph showing the relationship between the interlayer distance and the oxygen content of graphite (G), graphite oxide (GO), GLG250, GLG300, GLG400, GLG500, GLG700, and GLG800.
[0103] As shown in FIG. 15, there is a roughly proportional correlation between the interlayer distance and the oxygen content of the carbon material.
[0104] <Test Example> A test battery cell was fabricated and charged, and the structural change of GLG during charging was verified using X-ray diffraction measurement.
[0105] The method for fabricating the battery cell of the test example is as follows. First, GO, the raw material of GLG, was peeled and dispersed in dilute ammonia water, and this dispersion was cast onto a substrate and dried to form a sheet. The sheet GO was then heat-treated under the same conditions as those for obtaining GLG300 to obtain a sheet electrode of GLG300. Using this sheet electrode as the working electrode, a battery cell was fabricated in the same manner as in Experimental Example 2.
[0106] Fig. 16 shows the charging curve of the battery cell of the test example. At points P1 to P4 in Fig. 16, the sheet electrodes of GLG300 were removed from the battery cell, washed with water, dried, and then subjected to X-ray diffraction measurement. Fig. 17 is a graph showing the results of X-ray diffraction measurement of the sheet electrodes of GLG300 before charging (P0) and at points P1 to P4 in Fig. 16.
[0107] According to the Carbon glossary, the stage structure of a graphite intercalation compound is defined as "a structure in which the inserted chemical species (intercalates) are regularly distributed in the c-axis direction according to their concentration, and is expressed by the number of stages n," and "n represents the number of carbon layers sandwiched between the intercalate layers."
[0108] That is, a "stage 1 graphite intercalation compound" refers to a graphite intercalation compound in which an intercalated layer is included between every layer of graphite, while a "stage 2 graphite intercalation compound" refers to a graphite intercalation compound in which an intercalated layer is included between every other layer.
[0109] As shown in Figures 16 and 17, when charging started, the intensity of the 002 peak that appeared in the XRD pattern of GLG300 (P0 in Figure 17) decreased, and the 003 peak and 004 peak derived from the stage 2 type structure appeared (point P1). Then, as charging progressed from point P2 to point P4, the 002 peak and 003 peak derived from the stage 1 type structure appeared. This result indicates that as charging progresses, ions are inserted between the layers of GLG300, forming an ion intercalated layer. It is considered that ions are stored between the layers of GLG300, and the structure changes from stage 2 to stage 1.
[0110] From the results of FIG. 17, the interlayer distance between adjacent carbon layers in GLG300 is 0.410 nm, and the interlayer distance between adjacent carbon layers in the stage 1 structure is calculated to be 0.975 nm. In other words, ions with a diameter of about 0.565 nm, i.e., ZnC x - It is suggested that ions such as these are inserted. [Industrial Applicability]
[0111] The present disclosure is extremely useful because it can provide a positive electrode material for a zinc negative electrode secondary battery that has high capacity and high cycle characteristics and can be stably charged and discharged at a high energy density, a manufacturing method thereof, and a zinc negative electrode secondary battery using the positive electrode material. [Explanation of symbols]
[0112] 100 Zinc negative electrode secondary battery 110 Positive electrode 111 Cathode active material (cathode material) 112 Positive electrode current collector 120 negative electrode 121 Negative electrode active material (negative electrode material) 122 Negative electrode current collector 130 Electrolyte 20 Graphene-like graphite (layered compound) 21 Carbon atoms 22 Oxygen Atoms 23 holes
Claims
1. A positive electrode material for a zinc negative electrode secondary battery, comprising: The positive electrode active material contains a carbon material having a layered structure, A positive electrode material, wherein the interlayer distance of the carbon material is greater than the interlayer distance of graphite, which is 0.335 nm, and less than 0.66 nm.
2. The positive electrode material according to claim 1 , wherein the interlayer distance of the carbon material is 0.345 nm or more and 0.50 nm or less.
3. The positive electrode material according to claim 1 , wherein the carbon material has carbon atoms and oxygen atoms covalently bonded to the carbon atoms as constituent elements.
4. 4. The cathode material according to claim 3, wherein the content of the oxygen atoms contained in the carbon material is less than 38 atomic %.
5. 5. The positive electrode material according to claim 4, wherein the content of the oxygen atoms contained in the carbon material is 2 atomic % or more and 30 atomic % or less.
6. A method for producing the positive electrode material according to any one of claims 3 to 5, comprising the steps of: A method for producing a positive electrode material, comprising oxidizing graphite powder and then heat-treating it at a temperature of 200° C. or higher and 800° C. or lower to obtain the carbon material.
7. The battery includes a positive electrode, a negative electrode, and an electrolyte solution. A zinc negative electrode secondary battery, wherein the positive electrode comprises the positive electrode material according to any one of claims 1 to 5.
8. The zinc negative electrode secondary battery according to claim 7 , wherein the electrolyte is an aqueous electrolyte.
Citation Information
Patent Citations
rechargeable zinc ion battery
JP2016513354A
Zinc chloride battery
JP2022173005A