Negative electrode mixture, manufacturing method of the negative electrode mixture, and secondary battery

The use of a composite material with silicon particles bound by a polymer with specific bending strain properties and a sulfide solid electrolyte enhances the cycle characteristics of secondary batteries by maintaining contact and ion conduction paths.

JP2024159051AActive Publication Date: 2024-11-08TOYOTA JIDOSHA KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023074789
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Secondary batteries containing Si as a negative electrode active material face challenges in cycle characteristics.

Method used

A negative electrode composite material comprising active material secondary particles made of silicon particles bound by a polymer with specific bending strain properties and a sulfide solid electrolyte, enhancing the bonding and deformability between these components.

Benefits of technology

Improves the cycle characteristics of secondary batteries by maintaining contact and ion conduction paths despite volume changes during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159051000001_ABST
    Figure 2024159051000001_ABST
Patent Text Reader

Abstract

To disclose a negative electrode mixture capable of improving a cycle characteristic of a secondary battery.SOLUTION: A negative electrode mixture of the present disclosure, contains: an active material secondary particle; and a sulfide solid electrolyte. The active material secondary particle contains: a plurality of silicon particles; and a polymer for binding the silicon particles to each other. The polymer has a characteristic of 0.37≤εA / εB (here, εA is a bending distortion of a compact A, and the compact A is formed by the polymer and the sulfide solid electrolyte, and includes 20 vol.% of the polymer, and has a filling factor of 90%. εB is a bending distortion of a compact B, and the compact B is formed by the sulfide solid electrolyte, and is a compact having a filling factor of 90%).SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a negative electrode mixture, a method for producing the negative electrode mixture, and a secondary battery. [Background technology]

[0002] Patent Document 1 discloses a negative electrode layer for use in an all-solid-state battery, which has secondary particles of an active material and a sulfide solid electrolyte, the secondary particles of the active material including a plurality of particles containing Si element or Sn element and a binder, and the porosity of the negative electrode layer is 15% or less. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-121557 A Summary of the Invention [Problem to be solved by the invention]

[0004] Secondary batteries having Si as the negative electrode active material still have room for improvement in terms of cycle characteristics. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A negative electrode mixture comprising: active material secondary particles; and a sulfide solid electrolyte; the secondary particles of the active material include a plurality of silicon particles and a polymer that bonds the silicon particles together, The polymer has the following characteristics: Characteristics: 0.37≦ε A / ε B ε A : Bending strain of molded body A Molded body A: A molded body made of the polymer and the sulfide solid electrolyte, containing 20% ​​by volume of the polymer and having a filling rate of 90%. ε B : Bending strain of molded body B Molded body B: Molded body made of the sulfide solid electrolyte and having a packing rate of 90% having Negative electrode composite material. <Aspect 2> The negative electrode mixture of aspect 1, The polymer is a fluorine-based polymer. Negative electrode composite material. <Aspect 3> The negative electrode mixture of Aspect 1 or 2, The polymer is a polyvinylidene fluoride polymer. Negative electrode composite material. <Aspect 4> A method for producing a negative electrode mixture, comprising: Mixing at least a plurality of silicon particles and a polymer to obtain active material secondary particles; and At least, the active material secondary particles and a sulfide solid electrolyte are mixed to obtain a negative electrode mixture, The polymer has the following characteristics: Characteristics: 0.37≦ε A / ε B ε A : Bending strain of molded body A Molded body A: A molded body made of the polymer and the sulfide solid electrolyte, containing 20% ​​by volume of the polymer and having a filling rate of 90%. ε B : Bending strain of molded body B Molded body B: Molded body made of the sulfide solid electrolyte and having a packing rate of 90% Using one having Manufacturing method. <Aspect 5> A secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The negative electrode active material layer has the negative electrode mixture according to any one of aspects 1 to 3. Secondary battery. Effect of the Invention

[0006] The negative electrode mixture of the present disclosure can improve the cycle characteristics of a secondary battery. [Brief description of the drawings]

[0007] [Figure 1] 2A and 2B are schematic diagrams illustrating an example of secondary particles of active material and a sulfide solid electrolyte contained in a negative electrode mixture. [Diagram 2] 1 illustrates an example of the configuration of a secondary battery. [Diagram 3] 4 shows the relationship between εA / εB and the capacity retention rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1.Negative electrode composite material FIG. 1 shows a schematic configuration of a negative electrode composite 1 according to one embodiment. As shown in FIG. 1, the negative electrode composite 1 includes active material secondary particles 1a and a sulfide solid electrolyte 1b. The active material secondary particles 1a include a plurality of silicon particles 1ax and a polymer 1ay that bonds the silicon particles 1ax together. The polymer 1ay has a molecular weight of 0.37≦ε A / ε B Here, the ε A is the bending strain of the molded body A, the molded body A is made of the polymer 1ay and the sulfide solid electrolyte 1b, contains the polymer 1ay at 20 volume % and has a filling rate of 90%, and the ε B is the bending strain of the molded body B, which is made of the sulfide solid electrolyte 1b and has a packing rate of 90%.

[0009] 1.1 Active material secondary particles The secondary particles of the active material 1a include a plurality of silicon particles 1ax and a polymer 1ay that bonds the silicon particles 1ax to each other. The polymer 1ay has a molecular weight of 0.37≦ε A / ε B It has the following characteristics.

[0010] 1.1.1 Silicon particles The chemical composition of the silicon particles 1ax is not particularly limited. The ratio of the Si element to all elements contained in the silicon particles 1ax may be, for example, 50 mol% to 100 mol%, 70 mol% to 100 mol%, or 90 mol% to 100 mol%. The silicon particles 1ax may contain other elements in addition to the Si element. The other elements may be at least one of Li, Sn, Fe, Co, Ni, Ti, Cr, Al, B, and P. When the silicon particles 1ax are obtained by removing Li from Li-Si alloy particles, the silicon particles 1ax may contain Si and Li. The silicon particles 1ax may also contain impurities such as oxides. The silicon particles 1ax may be amorphous or crystalline.

[0011] The silicon particles 1ax may be porous. When the silicon particles 1ax are porous and have voids, the voids can absorb the expansion of silicon, and the increase in the restraining pressure of the secondary battery can be reduced, and it is considered possible to further improve the cycle characteristics of the secondary battery. The silicon particles 1ax may be, for example, particles containing nanoporous silicon. Nanoporous silicon refers to silicon having a plurality of pores with a pore diameter of the nanometer order (less than 1000 nm, preferably 100 nm or less). The silicon particles 1ax may be porous silicon particles containing pores with a diameter of 55 nm or less. Pores with a diameter of 55 nm or less are difficult to crush even by pressing. In other words, porous silicon particles containing pores with a diameter of 55 nm or less tend to maintain a porous state even after pressing. For example, pores with a diameter of 55 nm or less may be contained in an amount of 0.21 cc / g or more and 0.30 cc / g or less per gram of the silicon particles 1ax. The lower limit may be 0.22 cc / g or more, or 0.23 cc / g or more, and the upper limit may be 0.28 cc / g or less, or 0.26 cc / g or less. The amount of pores with a diameter of 55 nm or less contained in the silicon particles 1ax can be determined from the pore size distribution by, for example, a nitrogen gas adsorption method or a DFT method.

[0012] The porosity of the silicon particles 1ax is not particularly limited. The porosity of the silicon particles 1ax may be, for example, 0% or more and 80% or less. The lower limit may be 1% or more, 5% or more, 10% or more, or 20% or more, and the upper limit may be 70% or less, 60% or less, 50% or less, 40% or less, or 30% or less. The porosity of the silicon particles 1ax can be determined, for example, by observation using a scanning electron microscope (SEM). It is preferable that the number of samples is large, for example, 100 or more. The porosity can be an average value determined from these samples.

[0013] The size of the silicon particles 1ax is not particularly limited. The particle diameter D1 of the silicon particles 1ax may be, for example, 10 nm or more and 10 μm or less. The lower limit may be 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and the upper limit may be 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The particle diameter D1 of the silicon particles 1ax can be obtained by observation with an electron microscope such as an SEM, and is obtained as the number average value of the maximum Feret diameter of each of a plurality of particles. The number of samples is preferably large, for example, 20 or more, 50 or more, or 100 or more. The particle diameter D1 of the silicon particles 1ax can be appropriately adjusted, for example, by changing the manufacturing conditions of the silicon particles or performing a classification process.

[0014] The shape of the silicon particles 1ax is not particularly limited. For example, the silicon particles 1ax may be spherical or non-spherical.

[0015] The number of silicon particles 1ax contained in one active material secondary particle 1a is not particularly limited. The number of silicon particles 1ax contained in one active material secondary particle 1a may be 2 or more and 10000 or less. The lower limit may be 5 or more, 10 or more, 50 or more, or 100 or more, and the upper limit may be 5000 or less, 1000 or less, or 500 or less.

[0016] 1.1.2 Polymers The polymer 1ay has a function of binding silicon particles 1ax together. The location of the polymer in the active material secondary particle 1a is not particularly limited. The polymer 1ay may be present on the surface layer side of the active material secondary particle 1a, may be present on the center side, or may be present on both sides. The polymer 1ay may be exposed on the surface of the active material secondary particle 1a.

[0017] The type of polymer 1ay is not particularly limited as long as it has the characteristics described below. Whether polymer 1ay has the characteristics described below depends on the type of monomer unit constituting polymer 1ay and the molecular weight of polymer 1ay. In this embodiment, a known polymer having the characteristics described below may be selected and used as polymer 1ay. Polymer 1ay may be at least one selected from butadiene rubber (BR)-based polymers, butylene rubber (IIR)-based polymers, acrylate butadiene rubber (ABR)-based polymers, styrene butadiene rubber (SBR)-based polymers, polyvinylidene fluoride (PVdF)-based polymers, polytetrafluoroethylene (PTFE)-based polymers, polyacrylic acid-based polymers, polyacrylic acid ester-based polymers, and the like. In particular, when polymer 1ay is a fluorine-based polymer, particularly a polyvinylidene fluoride (PVdF)-based polymer, high performance is likely to be exhibited. Fluorine-based polymers have low reactivity with the sulfide solid electrolyte 1b described below. Therefore, it is possible to suppress deterioration of the sulfide solid electrolyte 1b due to a reaction between the polymer 1ay and the sulfide solid electrolyte 1b. In addition, from the viewpoint of ion conductivity, etc., a fluorine-based polymer is advantageous. The polymer 1ay may be a copolymer. For example, a polyvinylidene fluoride (PVdF)-based polymer may have a unit derived from a monomer other than VdF in addition to a unit derived from VdF. Only one type of the polymer 1ay may be used alone, or two or more types may be used in combination.

[0018] The polymer 1ay has the following characteristics. When the active material secondary particles 1a contain the polymer 1ay having such characteristics, the active material secondary particles 1a and the sulfide solid electrolyte 1b are easily contacted with each other, the binding force between the active material secondary particles 1a and the sulfide solid electrolyte 1b is improved, and further, since the polymer 1ay itself has a deformable property, it is considered that the active material secondary particles 1a and the sulfide solid electrolyte 1b are unlikely to peel off from each other. That is, even if the volume of the active material secondary particles 1a (particularly the silicon particles 1ax) in the negative electrode mixture 1 changes with charging and discharging, it is considered that the active material secondary particles 1a and the sulfide solid electrolyte 1b are unlikely to peel off from each other, and the ion conduction path and the like are maintained. As a result, the cycle characteristics (capacity retention rate) are improved when the secondary battery is used.

[0019] Characteristics: 0.37≦ε A / ε B ε A : Bending strain of molded body A Molded body A: A molded body made of the polymer and the sulfide solid electrolyte, containing 20% ​​by volume of the polymer and having a filling rate of 90%. ε B : Bending strain of molded body B Molded body B: Molded body made of the sulfide solid electrolyte and having a packing rate of 90%

[0020] In this application, three molded bodies with different packing ratios (= true density / bulk density) are prepared, the bending strain of each molded body is measured, and from the relationship between the measured three bending strains and the packing ratios, an approximation curve is used to specify the bending strain at a packing ratio of 90%, which is regarded as "the bending strain of molded body A" and "the bending strain of molded body B." Specifically, it is as follows.

[0021] The "bending strain of molded body A" is specified as follows. First, polymer 1ay is dissolved in butyl butyrate to prepare a polymer solution. After weighing the polymer solution so that the sulfide solid electrolyte 1b and polymer 1ay are in a volume ratio of 80:20, butyl butyrate is added so that the solid content weight is 28%, and about 1.5 cc of the solution is adjusted. This solution is mixed with a shaker for 9 minutes and an ultrasonic homogenizer for 1 minute and 30 seconds to obtain a slurry. The slurry is cast on a glass petri dish, dried on a hot plate at 120 ° C., and then crushed to obtain a mixed powder of polymer 1ay and sulfide solid electrolyte 1b. The mixed powder is press molded to obtain a molded body for bending test. Here, three types of molded bodies with different filling rates are prepared by adjusting the weighing value of the mixed powder and the press pressure. Specifically, three molded bodies are prepared: a molded body with a filling rate of 70%, length of 20 mm, width of 2 mm, and thickness of 1 mm; a molded body with a filling rate of 77%, length of 20 mm, width of 2 mm, and thickness of 1 mm; and a molded body with a filling rate of 82%, length of 20 mm, width of 2 mm, and thickness of 1 mm. A three-point bending test is performed on each molded body to identify each bending strain. The relationship between these three bending strains and the filling rate is plotted on a graph, and an approximation curve is drawn by linear approximation to identify the bending strain at a filling rate of 90%, which is regarded as the "bending strain of molded body A."

[0022] The "bending strain of molded body B" is specified as follows. First, a molded body for bending test is obtained by press molding the sulfide solid electrolyte 1b. Here, three types of molded bodies with different filling rates are prepared by adjusting the weighing value of the sulfide solid electrolyte 1b and the pressing pressure. Specifically, three molded bodies are prepared: a molded body with a filling rate of 60%, a length of 20 mm, a width of 2 mm, and a thickness of 1 mm, a molded body with a filling rate of 73%, a length of 20 mm, a width of 2 mm, and a thickness of 1 mm, and a molded body with a filling rate of 78%, a length of 20 mm, a width of 2 mm, and a thickness of 1 mm. A three-point bending test described below is performed on each molded body to specify each bending strain. The relationship between these three bending strains and the filling rate is plotted on a graph, and an approximation curve is drawn by linear approximation to specify the bending strain at a filling rate of 90%, which is regarded as the "bending strain of molded body B".

[0023] "Bending strain" refers to bending strain measured by a three-point bending test in accordance with JIS K7171:2016. Specifically, a molded body (length 20 mm, width 2 mm, thickness 1 mm) is prepared using the above-mentioned procedure, and the molded body is set in a bending tester so that the distance between the supports is 18.5 mm, and a three-point bending test is performed. The span of the bending test is 1 mm. The test speed of the bending test is 0.05 mm / min.

[0024] As described above, the polymer 1ay has a molecular weight of 0.37≦ε A / ε B It has the following characteristics: ε A / ε B The upper limit is not particularly limited, and may be, for example, 1.00 or less, 0.95 or less, 0.90 or less, 0.85 or less, 0.80 or less, 0.75 or less, 0.70 or less, or 0.65 or less.

[0025] 1.1.3 Other ingredients The active material secondary particles 1a may contain other components in addition to the silicon particles 1ax and polymer 1ay. The active material secondary particles 1a may contain silicon particles 1ax and polymer 1ay in a total amount of more than 50% by mass and 100% by mass or less, 70% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, or 95% by mass or more and 100% by mass or less. The active material secondary particles 1a may contain silicon particles 1ax in an amount of 50% by mass or more and 99% by mass or less, 70% by mass or more and 99% by mass or less, or 90% by mass or more and 99% by mass or less, and may contain polymer 1ay in an amount of 1% by mass or more and 50% by mass or less, 1% by mass or more and 30% by mass or less, or 1% by mass or more and 10% by mass or less.

[0026] 1.1.4 Size of secondary particles of active material The active material secondary particles 1a can be said to be agglomerated by a plurality of silicon particles 1ax via a polymer 1ay. The average particle diameter of the active material secondary particles 1a is not particularly limited. The average particle diameter of the active material secondary particles 1a may be 100 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and may be 100 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The average particle diameter of the active material secondary particles 1a can be obtained by observation with an electron microscope such as SEM, and is obtained, for example, as the average value of the maximum Feret diameters of a plurality of secondary particles. The number of samples is preferably large, and may be, for example, 20 or more, 50 or more, or 100 or more. Alternatively, the average particle diameter (D50) of the active material secondary particles 1a measured by extracting only the active material secondary particles 1a from the negative electrode mixture 1 may be 100 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, or may be 100 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. Note that the average particle diameter D50 referred to in this application is the particle diameter (median diameter) at an integrated value of 50% in a volume-based particle size distribution determined by a laser diffraction / scattering method.

[0027] 1.1.5 Manufacturing method of secondary particles of active material The active material secondary particles 1a can be produced, for example, by mixing silicon particles 1ax, polymer 1ay, and optional components. There is no particular limit to the mixing method, and it may be wet mixing using a solvent or dry mixing without using a solvent. There is also no particular limit to the mixing means, and it may be mechanically mixed using various mixing devices or may be mixed manually.

[0028] 1.2 Sulfide solid electrolyte The sulfide solid electrolyte 1b may be a glass-based sulfide solid electrolyte (sulfide glass), a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. The sulfide glass is amorphous. The sulfide glass may have a glass transition temperature (Tg). In addition, when the sulfide solid electrolyte 1b has a crystalline phase, examples of the crystalline phase include a Thio-LISICON type crystalline phase, a LGPS type crystalline phase, and an Argyrodite type crystalline phase. The sulfide solid electrolyte 1b may contain, for example, a Li element, an X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and an S element. In addition, the sulfide solid electrolyte 1b may further contain at least one of an O element and a halogen element. In addition, the sulfide solid electrolyte 1b may contain an S element as a main component of an anion element. The sulfide solid electrolyte 1b may be, for example, Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-GeS2, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-LiI-LiBr, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-ZmSn (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers, and M is any of P, Si, Ge, B, Al, Ga, and In). The composition of the sulfide solid electrolyte 1b is not particularly limited, and examples thereof include xLi2S·(100-x)P2S5 (70≦x≦80), yLiI·zLiBr·(100-yz)(xLi2S·(1-x)P2S5) (0.7≦x≦0.8, 0≦y≦30, 0≦z≦30), and the like. Alternatively, the sulfide solid electrolyte 1b may be represented by the general formula: Li 4-x Ge 1-x P xIt may have a composition represented by S4(0 < x < 1). In the above general formula, at least a part of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a part of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, a part of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, a part of S may be substituted with a halogen (at least one of F, Cl, Br, and I). Alternatively, the sulfide solid electrolyte 1b is Li 7-a PS 6-a X a (X is at least one of Cl, Br, and I, and a is a number of 0 or more and 2 or less). a may be 0, or may be greater than 0. In the latter case, a may be 0.1 or more, may be 0.5 or more, or may be 1 or more. Also, a may be 1.8 or less, or may be 1.5 or less. The sulfide solid electrolyte 1b may be, for example, in a particulate form. The average particle diameter (D50) of the sulfide solid electrolyte 1b may be, for example, 10 nm or more and 10 μm or less.

[0029] 1.3 Other Components The negative electrode mixture 1 includes at least the active material secondary particles 1a and the sulfide solid electrolyte 1b. The negative electrode mixture 1 may also include other components as desired. Examples of the other components include various solid components and liquid components. For example, the negative electrode mixture 1 may include other active materials in addition to the active material secondary particles 1a and the sulfide solid electrolyte 1b. The ratio of the silicon particles 1ax to all active materials included in the negative electrode mixture 1 may be more than 50% by mass and 100% by mass or less, 70% by mass or more and 100% by mass or less, or 90% by mass or more and 100% by mass or less. The other active materials that may be included in the negative electrode mixture 1 may be, for example, at least one selected from graphite, lithium, and the like. The negative electrode mixture 1 may also include other electrolytes in addition to the active material secondary particles 1a and the sulfide solid electrolyte 1b. The other electrolytes may be solid electrolytes other than the sulfide solid electrolyte 1b. The ratio of the sulfide solid electrolyte 1b to all electrolytes contained in the negative electrode mixture 1 may be more than 50% by mass and 100% by mass or less, 70% by mass or more and 100% by mass or less, or 90% by mass or more and 100% by mass or less. The other electrolytes that may be contained in the negative electrode mixture 1 may be, for example, an oxide solid electrolyte or an ion-bonded solid electrolyte (for example, one containing Li, Y, and a halogen element as constituent elements). The negative electrode mixture 1 may also contain a conductive assistant together with the active material secondary particles 1a and the sulfide solid electrolyte 1b. Any conductive assistant known as a conductive material for batteries may be used as the conductive assistant. The negative electrode mixture 1 may also contain a binder together with the active material secondary particles 1a and the sulfide solid electrolyte 1b. Any binder known as a binder for batteries may be used as the binder. The amount of other components that may be contained in the negative electrode mixture 1 is not particularly limited, and may be appropriately determined according to the intended battery performance, etc.

[0030] 2. Manufacturing method of negative electrode mixture The technology of the present disclosure also has an aspect as a method for producing a negative electrode composite. That is, a method for producing a negative electrode composite 1 according to one embodiment includes (1) mixing at least a plurality of silicon particles 1ax and a polymer 1ay to obtain active material secondary particles 1a, and (2) mixing at least the active material secondary particles 1a and a sulfide solid electrolyte 1b to obtain the negative electrode composite 1. Here, in this embodiment, the polymer 1ay is a silicon particle having a molecular weight of 0.37≦ε A / ε B That is, in this embodiment, before the active material secondary particles 1a are produced, a combination of the polymer 1ay having the above-mentioned characteristics and the sulfide solid electrolyte 1b is selected. For example, the sulfide solid electrolyte 1b to be combined with the active material secondary particles 1a is prepared, and the bending strain ε of the molded body B is measured as described above. B " is specified, multiple types of polymers are prepared, and for each polymer, "the bending strain ε A " and the identified ε B and multiple ε A Based on each of and, ε A / ε B Calculate the calculated ε A / ε B A combination of the sulfide solid electrolyte 1b and the polymer 1ay such that the value of the active material secondary particles 1a is 0.37 or more is selected, the selected polymer 1ay is used to prepare active material secondary particles 1a, and the selected sulfide solid electrolyte 1b and the active material secondary particles 1a are used to prepare a negative electrode composite material 1.

[0031] 3. Secondary battery FIG. 2 shows a schematic configuration of a secondary battery 100 according to an embodiment. As shown in FIG. 2, the secondary battery 100 has a positive electrode active material layer 20, an electrolyte layer 30, and a negative electrode active material layer 40. In the battery 100 according to an embodiment, the negative electrode active material layer 40 contains the above-mentioned negative electrode composite material 1. Problems related to cycle characteristics are likely to become apparent when the secondary battery contains a solid electrolyte. In contrast, in the secondary battery 100, the negative electrode active material layer 40 contains a predetermined active material secondary particle 1a together with a sulfide solid electrolyte 1b, so that the cycle characteristics can be improved as described above. In the secondary battery 100, in addition to the negative electrode active material layer 40 containing a sulfide solid electrolyte, one or both of the positive electrode active material layer 20 and the electrolyte layer 30 may contain a sulfide solid electrolyte. In addition, in the secondary battery 100, all of the positive electrode active material layer 20, the electrolyte layer 30, and the negative electrode active material layer 40 may contain a sulfide solid electrolyte. Furthermore, the secondary battery 100 may be a solid-state battery. A solid-state battery refers to a battery in which an electrolyte having carrier ion conductivity is mainly composed of a solid electrolyte. However, a liquid component may be included in part. Alternatively, the secondary battery 100 may be an all-solid-state battery that does not substantially contain a liquid component. The secondary battery 100 may have a general configuration as a battery. For example, as shown in FIG. 2, the secondary battery 100 may have a positive electrode current collector 10 in contact with the positive electrode active material layer 20 and a negative electrode current collector 50 in contact with the negative electrode active material layer 40 in addition to the positive electrode active material layer 20, the electrolyte layer 30, and the negative electrode active material layer 40. In the secondary battery 100, the configuration other than the negative electrode active material layer 40 is the same as that of the conventional battery, and may have a configuration such as that described in Patent Document 1 (JP Patent Publication 2019-121557 A), for example. The manufacturing method of the secondary battery 100 may also be the same as that of the conventional battery, except that the negative electrode mixture 1 is used. EXAMPLES

[0032] The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0033] 1. Polymer characterization by bending tests 1.1 Preparation of bending test specimens 1.1.1 PVdF-based polymer 1 PVdF-based polymer 1 was dissolved in butyl butyrate to obtain a polymer solution. The sulfide electrolyte after atomization described below and the polymer solution were weighed so that the volume ratio of the sulfide solid electrolyte to the polymer after drying was 80:20, and butyl butyrate was further added as a solvent to adjust the solid content weight to 28%, and about 1.5 cc of the solution was prepared. This was mixed for 9 minutes with a shaker and for 1 minute and 30 seconds with an ultrasonic dispersion device to obtain a slurry. The slurry was cast on a glass petri dish, dried on a hot plate at 120 ° C., and then crushed in a mortar to obtain a mixed powder of PVdF-based polymer 1 and a sulfide solid electrolyte. The mixed powder was weighed and press molded in a jig to obtain a molded body (length 20 mm, width 2 mm, thickness 1 mm) for bending test. Here, the weighed value of the mixed powder was changed, and the pressing pressure was changed from 0.5 to 3.5t to obtain three molded bodies with different filling rates. Of these, one molded body had a filling rate of 70%, one molded body had a filling rate of 77%, and one molded body had a filling rate of 82%.

[0034] 1.1.2 PVdF-based polymers 2-5 PVdF-based polymers 2 to 5 were prepared, each having a different copolymerization component amount and molecular weight from the above-mentioned PVdF-based polymer 1. For each of polymers 2 to 5, three molded articles with different filling rates were obtained in the same manner as above.

[0035] 1.1.3 BR polymers Using a BR polymer, three molded articles with different filling rates were obtained in the same manner as above.

[0036] Hereinafter, the above-mentioned molded article containing a PVdF-based polymer or a BR-based polymer will be referred to as a "polymer molded article."

[0037] 1.1.4 Sulfide solid electrolyte 0.550g of Li2S (Furuuchi Chemical), 0.887g of P2S5 (Aldrich), 0.285g of LiI (Nippo Chemical), and 0.277g of LiBr (Kojundo Chemical) were mixed in an agate mortar for 5 minutes. 4g of n-heptane (dehydrated grade, Kanto Chemical) was added to the resulting mixture, and mechanical milling was performed for 40 hours using a planetary ball mill to obtain a sulfide solid electrolyte. The obtained sulfide solid electrolyte was further mechanically milled for 20 hours to obtain a powder. After the powdering, the particles were weighed and pressed in a jig to obtain a molded body (length 20mm, width 2mm, thickness 1mm) for bending test. Here, the weighed value of the sulfide solid electrolyte was changed, and the pressing pressure was changed from 50 to 400MPa to obtain three molded bodies with different filling rates. One molded body had a filling rate of 60%, one molded body had a filling rate of 73%, and one molded body had a filling rate of 78%.

[0038] Hereinafter, the molded body made of the sulfide solid electrolyte will be referred to as a "solid electrolyte molded body."

[0039] 1.2 Bending test For each polymer, three polymer molded bodies with different filling rates were prepared as described above, and a three-point bending test was performed on each of them to determine the bending strain. The measured values ​​were plotted with the filling rate on the horizontal axis and the bending strain on the vertical axis, and an approximate curve was drawn from the three-point plot by linear approximation to obtain the bending strain ε at a filling rate of 90%. A (90% bending strain ε A On the other hand, the bending strain ε B (90% bending strain ε B ) was identified.

[0040] 1.3 ε A / ε B Calculation of 90% bending strain ε of each polymer molding A and the 90% bending strain ε of the solid electrolyte compact B Relative to ε A / ε BThe results are shown in Table 1 below.

[0041] [Table 1]

[0042] 2. Evaluation of battery cycle characteristics Each of the above polymers was used to prepare active material secondary particles, the active material secondary particles were used to prepare a negative electrode mixture, the negative electrode mixture was used to prepare a secondary battery, and the cycle characteristics of the secondary battery were evaluated.

[0043] 2.1 Comparative Example 1 2.1.1 Preparation of the positive electrode A positive electrode slurry was prepared by stirring the NCM-based positive electrode active material, sulfide-based solid electrolyte, vapor-grown carbon fiber, PVdF-based binder, and butyl butyrate with an ultrasonic disperser. The mass ratio of the NCM-based positive electrode active material, sulfide-based solid electrolyte, vapor-grown carbon fiber, and PVdF-based binder was 100:16:2:0.75. The positive electrode slurry was applied to an Al foil as a positive electrode current collector by a blade method, and the resulting coating was dried on a hot plate at 100°C for 30 minutes to obtain a positive electrode having a positive electrode active material layer on the surface of the Al foil.

[0044] 2.1.2 Preparation of the negative electrode The PVDF-based polymer 1 was dissolved in butyl butyrate to obtain a polymer solution. The polymer solution and Si particles (particle size 0.5 μm, manufactured by Kojundo Chemical Co., Ltd.) were weighed so that the mass ratio of Si particles:polymer was 100:8, and the mixture was stirred with an ultrasonic dispersion device and a shaker to obtain a negative electrode slurry. The negative electrode slurry was cast on a glass petri dish, dried on a hot plate, and crushed in a mortar to obtain active material secondary particles. The obtained active material secondary particles are secondary particles (aggregated particles) consisting of a plurality of Si particles and a polymer that binds the Si particles together. The active material secondary particles, sulfide-based solid electrolyte, vapor-grown carbon fiber, BR-based binder, mesitylene, and dibutyl ether were stirred and mixed using an ultrasonic dispersion device and a stirrer to obtain a negative electrode slurry in which the negative electrode mixture was dispersed in a solvent. Here, the mass ratio of Si particles:polymer:sulfide-based solid electrolyte:vapor-grown carbon fiber:BR-based binder was 100:8:77.6:8.4:1.5. This negative electrode slurry was applied onto Ni foil as a negative electrode current collector by a blade method, and dried on a hot plate at 100°C for 30 minutes to obtain a negative electrode having a negative electrode active material layer on the surface of the Ni foil.

[0045] 2.1.3 Preparation of solid electrolyte layer A solid electrolyte slurry was obtained by stirring the sulfide-based solid electrolyte, PVdF-based binder, and butyl butyrate with an ultrasonic dispersing device. The mass ratio of the sulfide-based solid electrolyte to the PVdF-based binder was 99.6:0.4. This solid electrolyte slurry was applied onto an Al foil by a blade method, and dried on a hot plate at 100°C for 30 minutes to form a solid electrolyte layer on the Al foil.

[0046] 2.1.4 Preparation of the positive electrode laminate The positive electrode active material layer and the solid electrolyte layer were laminated and pressed with a roll press at a pressure of 50 kN / cm and a temperature of 160°C. The Al foil was then peeled off from the solid electrolyte layer and a 1 cm 2 By punching out the laminate into a size of 100 mm, a positive electrode laminate having a structure of Al foil / positive electrode active material layer / solid electrolyte layer was obtained.

[0047] 2.1.5 Preparation of negative electrode laminate The negative electrode active material layer and the solid electrolyte layer were laminated and pressed with a roll press at a pressure of 50 kN / cm, and then the Al foil of the solid electrolyte layer was peeled off to obtain a first laminate having a configuration of Ni foil / negative electrode active material layer / solid electrolyte layer. Further, an additional solid electrolyte layer was laminated on the solid electrolyte layer side of the first laminate, and pre-pressed with a flat uniaxial press at a pressure of 100 MPa and a temperature of 25°C, after which the Al foil was peeled off from the solid electrolyte layer and pressed to a thickness of 1.08 cm. 2 A second laminate having a structure of Ni foil / negative electrode active material layer / solid electrolyte layer / solid electrolyte layer was obtained by punching out the resulting laminate into a size of 100 mm. This second laminate was used as the negative electrode laminate.

[0048] 2.1.6 Fabrication of the battery stack The above positive electrode laminate and negative electrode laminate were laminated and pressed with a flat uniaxial press at a pressure of 200 MPa and a temperature of 135°C to obtain a battery laminate having a configuration of Ni foil / negative electrode active material layer / solid electrolyte layer / solid electrolyte layer / solid electrolyte layer / cathode active material layer / Al foil.

[0049] 2.1.7 Battery Stack Constraints and Initial Charge / Discharge The battery stack was sandwiched between two restraining plates, and these two restraining plates were fastened with a fastener at a restraining pressure of 1 MPa to fix the distance between the two restraining plates. (1) 1 / 10C, ​​constant current charging up to 4.55V (2) Then, charge to 4.55V with a constant voltage of 1 / 100C. (3) Then, discharge at a constant current of 1C down to 3V. (4) After that, discharge at a constant voltage of 3V until the final current is 1 / 100C. (5) Then, charge at a constant current of 1 / 3C up to 4.35V. Furthermore, after that, (6) Constant voltage charging up to 4.35V, final current 1 / 100C (7) Then, discharge at a constant current of 1 / 3C to 3V. (8) After that, discharge at a constant voltage of 3V until the final current is 1 / 100C. I did this twice.

[0050] 2.1.8 Cycle characteristics evaluation through durability tests The battery stack after the above charge and discharge was subjected to a durability test, and the cycle characteristics were evaluated by calculating the capacity retention rate. Specifically, 150 charge and discharge cycles were performed under the following conditions, and the ratio of the discharge capacity C2 after 150 cycles to the discharge capacity C1 at the first cycle was calculated and defined as the capacity retention rate. Charging: 2C, constant current charging up to 4.17V Discharge: 2C, constant current discharge up to 3.14V Capacity retention rate (%): [Discharge capacity C2 / Discharge capacity C1] × 100

[0051] 2.2 Examples 1 to 5 A battery was produced in the same manner as in Comparative Example 1, except that the above-mentioned PVdF-based polymers 2 to 5 or BR-based polymer were used instead of PVdF-based polymer 1 as the polymer constituting the active material secondary particles, and the cycle characteristics were evaluated.

[0052] 2.3 Evaluation results Figure 3 shows the characteristic ε of the polymer that constitutes the secondary particles of the active material. A / ε B As shown in FIG. 3, the relationship between the capacity retention rate and the polymer constituting the secondary particles of the active material is 0.37≦ε A / ε BIt can be seen that when the secondary battery has such a characteristic, the capacity retention rate of the secondary battery is improved and the secondary battery has excellent cycle characteristics. When the secondary active material particles contain a polymer having such a characteristic, the secondary active material particles and the sulfide solid electrolyte are easily contacted with each other, the binding force between the secondary active material particles and the sulfide solid electrolyte is improved, and further, since the polymer itself has a deformable property, it is considered that the secondary active material particles and the sulfide solid electrolyte are less likely to peel off. That is, even if the volume of the secondary active material particles (especially Si particles) in the negative electrode composite changes with charging and discharging, it is considered that the secondary active material particles and the sulfide solid electrolyte are less likely to peel off, and the ion conduction path and the like are maintained. As a result, it is considered that the cycle characteristics (capacity retention rate) of the secondary battery are improved. From the above results, it can be said that the cycle characteristics of the secondary battery are improved by constructing a secondary battery using a negative electrode composite that satisfies the following. (1) The negative electrode mixture contains secondary particles of an active material and a sulfide solid electrolyte. (2) The secondary particles of the active material include a plurality of silicon particles and a polymer that bonds the silicon particles together. (3) The polymer has a ε of 0.37≦ε A / ε B Here, ε A is the bending strain of the molded body A, the molded body A being made of the polymer and the sulfide solid electrolyte, containing the polymer at 20 volume % and having a filling rate of 90%, and ε B is the bending strain of compact B, which is made of the sulfide solid electrolyte and has a packing rate of 90%. [Explanation of symbols]

[0053] 1 Negative electrode composite material 1a Active material secondary particles 1ax silicon particles 1ay Polymer 1b Sulfide solid electrolyte 100 Secondary battery 10 Positive electrode current collector 20 Cathode active material layer 30 Electrolyte layer 40 Negative electrode active material layer 50 Negative electrode current collector

Claims

1. A negative electrode mixture comprising: active material secondary particles; and a sulfide solid electrolyte; the secondary particles of the active material include a plurality of silicon particles and a polymer that bonds the silicon particles together, The polymer has the following characteristics: Characteristics: 0.37≦ε A / ε B ε A : bending strain of molded body A Molded body A: A molded body made of the polymer and the sulfide solid electrolyte, containing 20% ​​by volume of the polymer and having a filling rate of 90%. ε B : bending strain of molded body B Molded body B: Molded body made of the sulfide solid electrolyte and having a filling rate of 90% having Negative electrode composite material.

2. The negative electrode mixture according to claim 1 , The polymer is a fluorine-based polymer. Negative electrode composite material.

3. The negative electrode mixture according to claim 1 , The polymer is a polyvinylidene fluoride polymer. Negative electrode composite material.

4. A method for producing a negative electrode mixture, comprising: Mixing at least a plurality of silicon particles and a polymer to obtain active material secondary particles; and At least, the active material secondary particles and a sulfide solid electrolyte are mixed to obtain a negative electrode mixture, The polymer has the following characteristics: Characteristics: 0.37≦ε A / ε B ε A : bending strain of molded body A Molded body A: A molded body made of the polymer and the sulfide solid electrolyte, containing 20% ​​by volume of the polymer and having a filling rate of 90%. ε B : bending strain of molded body B Molded body B: Molded body made of the sulfide solid electrolyte and having a filling rate of 90% Using one having Manufacturing method.

5. A secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The negative electrode active material layer comprises the negative electrode mixture according to any one of claims 1 to 3. Secondary battery.

Citation Information

Patent Citations

  • All-solid battery

    JP2020087882A

  • All-solid battery

    JP2022079934A

  • Anode active substance, anode material and battery

    WO2023002758A1

  • Negative electrode layer

    JP2019121557A