Reflectance adjustment film, laminate, and method for manufacturing reflectance adjustment film
The laminated reflectance adjustment film with silicon dioxide and yttrium oxide, enhanced by group 4A element substitution, addresses hardness and contamination issues, providing a robust and efficient manufacturing solution.
Patent Information
- Application Number
- JP2023075063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing reflectance adjustment films have low hardness, leading to susceptibility to scratches and potential contamination when a hard coat layer is provided separately, increasing the number of manufacturing steps.
A reflectance adjustment film is formed by laminating low and high refractive index films, with the low refractive index film composed of silicon dioxide and yttrium oxide where some yttrium atoms are replaced with group 4A elements, and optionally oxygen atoms are replaced with nitrogen atoms, enhancing hardness without a separate hard coat layer.
The film achieves high hardness and scratch resistance while minimizing contamination risks, with improved manufacturing efficiency by integrating the hard coat properties directly into the film structure.
Smart Images

Figure 2024159216000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a reflectance adjusting film, a laminate, and a method for manufacturing a reflectance adjusting film. [Background technology]
[0002] A reflectance adjusting film for adjusting the reflectance of light may be laminated on the surface of a glass substrate or the like. For example, Patent Document 1 describes an antireflection film for preventing the reflection of light as a reflectance adjusting film. The antireflection film of Patent Document 1 can be formed, for example, by alternately laminating a low refractive index film and a high refractive index film on a glass substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2019-151321 Summary of the Invention [Problem to be solved by the invention]
[0004] The reflectance adjustment film having the configuration as described in Patent Document 1 has a low hardness (softness) and may be scratched during use, etc. For this reason, in order to increase the hardness of the reflectance adjustment film and improve the scratch resistance, etc., a hard coat layer can be provided on the substrate as a layer separate from the reflectance adjustment film.
[0005] However, when a hard coat layer is provided as a film separate from the reflectance adjusting film, the number of steps increases accordingly, and when the reflectance adjusting film is formed on the hard coat layer, there is a risk of foreign matter being mixed into the reflectance adjusting film.
[0006] Therefore, an object of at least one embodiment of the present disclosure is to provide a reflectance adjusting film having high hardness, a laminate including the reflectance adjusting film, and a method for manufacturing the reflectance adjusting film. [Means for solving the problem]
[0007] In order to achieve this objective, the reflectance adjusting film according to at least one embodiment of the present disclosure has: A reflectance adjusting film for adjusting the reflectance of light, Multiple films are laminated, the plurality of films include a low refractive index film and a high refractive index film having a refractive index higher than that of the low refractive index film, The low refractive index film is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), provided that the yttrium oxide (Y 2 O 3 ) some of the yttrium (Y) atoms are replaced by atoms of group 4A elements, The refractive index of at least one of the films adjacent to the high refractive index film is smaller than the refractive index of the high refractive index film. This is a reflectance adjusting film.
[0008] The laminate according to at least one embodiment of the present disclosure is a laminate in which a reflectance adjusting film according to at least one embodiment of the present disclosure is formed on at least one surface of a substrate.
[0009] A method for manufacturing a reflectance adjusting film according to at least one embodiment of the present disclosure includes a low refractive index film formation process for forming the low refractive index film and a high refractive index film formation process for forming the high refractive index film, in which the low refractive index film is formed by a sputtering method in the low refractive index film formation process, and the high refractive index film is formed by a sputtering method in the high refractive index film formation process. Effect of the Invention
[0010] According to the present disclosure, it is possible to provide a reflectance adjusting film having high hardness, a laminate including the reflectance adjusting film, and a method for manufacturing the reflectance adjusting film. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a reflectance adjustment film according to an embodiment of the present disclosure and a laminate according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a laminate having a hard coat layer and a reflectance adjusting film according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In the present disclosure, "on" or "on the surface" may refer to a state in which the material is in direct contact with the surface, or may refer to a state in which another layer or the like is interposed therebetween.
[0013] In this disclosure, unless otherwise specified, the term "suppression" of any phenomenon is not limited to minimizing the occurrence of such phenomenon, but also includes eliminating the occurrence of such phenomenon.
[0014] In this disclosure, unless otherwise specified, the term "reflectance adjusting film" refers to a film-like structure that can adjust the reflectance of incident light by changing the film thickness, refractive index, etc.
[0015] In the present disclosure, unless otherwise specified, the term "film thickness" may refer to either the "physical film thickness" or the "optical film thickness".
[0016] Hereinafter, specific embodiments of the present disclosure will be described with reference to drawings, etc., as necessary. For the sake of convenience, each drawing is drawn in a schematic manner with appropriate omissions, exaggeration, etc. In addition, when mechanisms and principles are mentioned in the following embodiments and examples, the described mechanisms and principles are merely presumed and are not limited to the described mechanisms and principles.
[0017] [1. Reflectance control film and laminate] First, the reflectance adjusting film and the laminate according to some embodiments of the present disclosure will be described with reference to examples.
[0018] [1-1. Structure of reflectance adjustment film and laminate] The cross-sectional view of FIG. 1 shows a schematic configuration of an example of a reflectance adjustment film according to an embodiment of the present disclosure and a laminate according to an embodiment of the present disclosure using the same. As shown in the figure, the laminate 100 according to an embodiment of the present disclosure has a reflectance adjustment film 10 according to an embodiment of the present disclosure formed on one surface of a substrate 20. The reflectance adjustment film 10 is a film formed by laminating a plurality of films (low refractive index layers 11 and high refractive index layers 12 described later) into which light is incident. The reflectance adjustment film 10 is formed by alternately laminating low refractive index films 11 and high refractive index films 12. In the figure, the film adjacent to the substrate 20 and the film furthest from the substrate 20 are low refractive index films 11, respectively.
[0019] The order in which the low refractive index film 11 and the high refractive index film 12 are stacked is not particularly limited, but when the reflectance adjusting film 10 is used as an anti-reflection film, the film farthest from the substrate 20 is the low refractive index film 11 .
[0020] In FIG. 1, the number of low refractive index films 11 is three, and the number of high refractive index films 12 is two. However, in the reflectance adjustment film according to the embodiment of the present disclosure, the number of low refractive index films and high refractive index films is not limited, and at least one layer of each film may be sufficient. In the reflectance adjustment film according to the embodiment of the present disclosure, the total number of low refractive index films and high refractive index films is preferably three or more, more preferably five or more, and the upper limit is not particularly limited, but may be, for example, 30 or less, 20 or less, 15 or less, or 10 or less. The smaller the total number of low refractive index films and high refractive index films (i.e., the smaller the total number of layers of the low refractive index films and high refractive index films), the shorter the time required for production of the reflectance adjustment film according to the embodiment of the present disclosure, or the lower the cost required for production, which is preferable. In addition, the larger the total number of low refractive index films and high refractive index films (i.e., the larger the total number of layers of the low refractive index films and high refractive index films), the easier it is to obtain the target reflectance of the reflectance adjustment film according to the embodiment of the present disclosure, which is preferable.
[0021] The substrate 20 is not particularly limited, but may be, for example, a plate-shaped substrate. The material of the substrate 20 may be glass, resin, or the like. Examples of glass include glass plates and glass lenses. Examples of resin include resin plates and resin lenses. The material of the resin is not particularly limited, and may be, for example, polyolefin, polyester, PC (polycarbonate), acrylic resin, or the like. Examples of the polyolefin include, for example, PP (polypropylene), PE (polyethylene), COP (cycloolefin polymer), or the like. Examples of the polyester include, for example, PET (polyethylene terephthalate), or the like. Examples of the acrylic resin include, for example, PMMA (polymethyl methacrylate), or the like. In FIG. 1, the substrate 20 is a single layer, but is not limited thereto, and may be a laminate of multiple layers, in which case each layer may be the same or different. The laminate 100 may be, for example, a lens having a reflectance adjustment film 10, window glass, or the like.
[0022] The reflectance adjustment film 10 in FIG. 1 includes only a low refractive index film 11 and a high refractive index film 12. However, the reflectance adjustment film according to the embodiment of the present disclosure is not limited to this, and may include layers other than the low refractive index film and the high refractive index film. In addition, the number of low refractive index films 11 is three, and the number of high refractive index films 12 is two. In the reflectance adjustment film 10 in FIG. 1, the low refractive index film 11 and the high refractive index film 12 are laminated in direct contact with each other, but the configuration according to the embodiment of the present disclosure is not limited to this configuration, and may be laminated, for example, via a layer other than the low refractive index film and the high refractive index film. Furthermore, in FIG. 1, the reflectance adjustment film 10 is laminated on the substrate 20 in direct contact with each other. However, the present disclosure is not limited to this, and may be laminated, for example, via a layer other than the low refractive index film 11 and the high refractive index film 12 on the substrate 20. However, from the viewpoint of preventing foreign matter originating from the other layers, etc. from being mixed into the reflectance adjusting film, it is preferable that the reflectance adjusting film according to an embodiment of the present disclosure and the laminate according to an embodiment of the present disclosure do not include any layers other than the low refractive index film and the high refractive index film.
[0023] 2 shows an example of a laminate having a hard coat layer and a reflectance adjustment film according to an embodiment of the present disclosure. As shown in the figure, in this laminate 100a, a hard coat layer 30 is formed on one surface of a substrate 20, and a reflectance adjustment film 10a is formed on the surface of the hard coat layer 30 opposite to the substrate 20. The reflectance adjustment film 10a is formed by alternately laminating low refractive index films 11a and high refractive index films 12a. In the figure, the film adjacent to the hard coat layer 30 (closest to the substrate 20) and the film furthest from the substrate 20 are low refractive index films 11a, respectively.
[0024] When a hard coat layer is used as a layer separate from the reflectance adjustment film as shown in FIG. 2, for example, the hardness of the reflectance adjustment film can be increased to improve scratch resistance. However, as described above, the number of steps required to provide the hard coat layer increases. Also, when forming the reflectance adjustment film on the hard coat layer, there is a risk of foreign matter being mixed into the reflectance adjustment film. In contrast, the reflectance adjustment film 10 according to the embodiment of FIG. 1 has a high hardness even without a hard coat layer, and therefore can solve such problems.
[0025] As described above, in the reflectance adjustment film according to the embodiment of the present disclosure, the low refractive index film is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), except that yttrium oxide (Y 2 O 3 In the case of yttrium oxide (Y), some of the yttrium (Y) atoms are replaced by atoms of group 4A elements. 2 O 3 In the case of yttrium oxide (Y), some of the oxygen (O) atoms may be replaced with nitrogen (N) atoms. 2 O 3By replacing some of the oxygen (O) atoms in the reflectance control film with nitrogen (N) atoms, it is expected that the film will have low adhesion to basic substances and anti-fouling properties with respect to certain substances. The principle by which adhesion and anti-fouling properties are imparted is thought to be that, for example, the hydroxyl groups, which are active groups on the reflectance control film surface, are inactivated when some of the oxygen (O) atoms are replaced with nitrogen (N) atoms.
[0026] In addition, yttrium oxide (Y 2 O 3 ) is silicon dioxide (SiO 2 ) is harder than yttrium oxide (Y 2 O 3 ) and silicon dioxide (SiO 2 The film formed by the mixture containing silicon dioxide (SiO 2 It is believed that the hardness will be higher than that of a low refractive index film composed only of yttrium oxide (Y 2 O 3 For example, by substituting some of the yttrium (Y) atoms in the low refractive index film with atoms of a Group 4A element, the bonds of the crystals that make up the low refractive index film become stronger. According to this, it is believed that when some of the yttrium (Y) atoms in the low refractive index film are substituted with atoms of a Group 4A element, the film has a higher hardness than when it is not substituted.
[0027] The hardness of the reflectance adjustment film according to the embodiment of the present disclosure is not particularly limited. However, when the substrate is glass, the hardness of the reflectance adjustment film is preferably 6.0 GPa or more, more preferably 6.1 GPa or more. The upper limit is, for example, 11 GPa or less.
[0028] In the present disclosure, the hardness is a numerical value measured by a method described in the Examples below. However, in the present disclosure, the hardness may be measured by a method other than the measurement method described below.
[0029] The reflectance adjustment film according to the embodiment of the present disclosure may be, but is not limited to, an anti-reflection film. For example, the reflectance adjustment film according to the embodiment of the present disclosure may have a light transmittance of approximately 0%. Such a reflectance adjustment film may be, for example, a mirror with a light reflectance of approximately 100%. In the reflectance adjustment film according to the embodiment of the present disclosure, the reflectance, transmittance, etc. of light can be adjusted, for example, by appropriately setting the number, film thickness, refractive index, stacking order, etc. of the low refractive index films and the high refractive index films. In addition, in the reflectance adjustment film according to the embodiment of the present disclosure, the reflectance, transmittance, etc. of light can also be adjusted to be different depending on the wavelength of light, for example.
[0030] The reflectance adjustment film according to the embodiment of the present disclosure has its reflectance adjusted by, for example, the following method. As described above, the reflectance adjustment film according to the embodiment of the present disclosure is configured by stacking a plurality of films. The refractive indexes of the adjacent films are different from each other. Here, when light is incident from one film to the other film, if the refractive indexes of the two adjacent films are different, a part of the incident light is reflected at the boundary between the two adjacent films. The greater the difference in refractive index between the two adjacent layers, the greater the intensity of the reflected light. In addition, the film thickness of the stacked films affects the phase of the reflected light that occurs at the boundary between the two adjacent films. In the reflectance adjustment film according to the embodiment of the present disclosure, light is reflected at the boundary between each of the stacked films. Therefore, by adjusting the refractive index and film thickness of the stacked films, the reflectance of the reflectance adjustment film according to the embodiment of the present disclosure can be adjusted.
[0031] When the reflectance adjusting film according to the embodiment of the present disclosure is an anti-reflection film, the upper limit of the reflectance of light is not particularly limited, but the average reflectance in visible light (380 nm to 780 nm) is preferably 2.5% or less, more preferably 2.0% or less, 1.5% or less, or 1.0% or less. The lower limit of the reflectance is not particularly limited, but is, for example, 0 or a value exceeding 0.
[0032] In the present disclosure, the reflectance of light may be measured using a device capable of measuring the reflectance of light. An example of a device capable of measuring the reflectance of light is a reflection spectroscopic film thickness meter (product name: FE-3000) manufactured by Otsuka Electronics Co., Ltd. The reflectance of light may be a numerical value measured from the wavelength of incident light, the film thickness of the low refractive index film and the high refractive index film, the optical constants of these films, and the optical constants of the substrate. However, in the present disclosure, the reflectance of light may be measured by a method other than the above-mentioned measurement method. In the present disclosure, the reflectance of light may be an actual value measured using a device, or may be a simulated value calculated by optical simulation software or the like.
[0033] [1-2. Low refractive index film] Hereinafter, the low refractive index film in the reflectance adjustment film according to the embodiment of the present disclosure will be described with reference to an example.
[0034] The refractive index of the low refractive index film is not particularly limited, but for example, the refractive index for light with a wavelength of 500 nm is in the range of 1.47 to 1.58.
[0035] In the present disclosure, the refractive index may be a value measured using, for example, an apparatus capable of measuring the refractive index. An example of an apparatus capable of measuring the refractive index is a reflection spectroscopic film thickness meter (product name: FE-3000) manufactured by Otsuka Electronics Co., Ltd. However, in the present disclosure, the refractive index may be measured using a method other than the following measurement method.
[0036] As described above, the low refractive index film in the reflectance adjustment film according to the embodiment of the present disclosure is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), except that yttrium oxide (Y 2 O 3 In the case of yttrium oxide (Y), some of the yttrium (Y) atoms are replaced by atoms of group 4A elements. 2 O 3) may further have some oxygen (O) atoms substituted with nitrogen (N) atoms. The content of yttrium oxide in the low refractive index film is not particularly limited, but for example, the lower limit is preferably 1.0 mol% or more, more preferably 1.1 mol% or more, and the upper limit is preferably less than 10 mol%, more preferably less than 6 mol%, from the viewpoint of improving antireflection performance.
[0037] In the present disclosure, the atomic content in the film may be a value measured by, for example, an X-ray photoelectron spectrometer. An example of the X-ray photoelectron spectrometer is an X-ray photoelectron spectrometer (product name: PHI5000 VersaProbe2) manufactured by ULVAC-PHI, Inc. According to the X-ray photoelectron spectrometer, a sample is irradiated with X-rays and the energy of photoelectrons emitted from the sample surface is measured, thereby obtaining information on the composition and chemical bond state of the surface, and thus the atomic content in the film can be measured. In the present disclosure, the atomic content in the film may be measured by a method other than the following measurement method.
[0038] In addition, the low refractive index film in the reflectance adjustment film according to the embodiment of the present disclosure is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ) may or may not contain other components. Examples of other components include magnesium fluoride (MgF 2 ) etc.
[0039] In the reflectance adjusting film according to the embodiment of the present disclosure, the yttrium oxide (Y 2 O 3In the case of ), some of the yttrium (Y) atoms are replaced by atoms of a Group 4A element. The atoms of the Group 4A element are not particularly limited, but may be, for example, at least one selected from the group consisting of titanium (Ti), zirconium (Zr) and hafnium (Hf), preferably at least one of zirconium (Zr) and hafnium (Hf), and particularly preferably zirconium (Zr). These atoms or materials forming them may be used alone, or a combination of two or more of these atoms and materials forming them may be used.
[0040] The reflectance adjusting film according to the embodiment of the present disclosure is a low refractive index film containing yttrium oxide (Y 2 O 3 For example, by substituting some of the yttrium (Y) atoms with atoms of a Group 4A element, it is possible to obtain high hardness (scratch resistance, etc.). The reason for this is that, for example, when some of the yttrium (Y) atoms are substituted with atoms of a Group 4A element (e.g., zirconium (Zr)), the hardness of yttrium oxide (Y 2 O 3 ) is thought to be due to its higher hardness.
[0041] In addition, the low refractive index film in the reflectance adjustment film according to the embodiment of the present disclosure may be, for example, crystalline. The fact that the low refractive index film is crystalline can be confirmed by a general crystallinity evaluation method such as, for example, X-ray diffraction, electron beam diffraction, Raman spectroscopy, etc. In addition, the fact that the low refractive index film contains yttrium oxide containing nitrogen and a Group 4A element can be identified by, for example, secondary ion mass spectrometry (SIMS).
[0042] In the low refractive index film, yttrium oxide (Y 2 O 3 The substitution rate of yttrium (Y) atoms in the above-mentioned alloy with atoms of a Group 4A element (content of atoms of the Group 4A element) is not particularly limited as long as it exceeds 0, but the upper limit may be, for example, 20 mol%, 15 mol%, 10 mol%, or 5 mol%.
[0043] In the low refractive index film, yttrium oxide (Y 2 O 3 ), when some of the oxygen (O) atoms are replaced by nitrogen (N) atoms, yttrium oxide (Y 2 O 3 The substitution rate of oxygen (O) atoms in the above-mentioned copolymer (X) with nitrogen (N) atoms (nitrogen atom content) is not particularly limited as long as it exceeds 0, and may be 1 atomic% or more, and the upper limit may be, for example, 10 atomic%, 5 atomic%, 3 atomic%, or 2 atomic%.
[0044] Furthermore, the low refractive index film does not need to contain metal elements that are allergy-inducing components or harmful metals, such as Hg, Ni, Cr, Co, Cu, Sn, Au, Pt, Pd, Sb, Ag, Fe, or Zn.
[0045] The physical thickness of the low refractive index film is not particularly limited and can be appropriately selected depending on the desired optical properties.
[0046] In the present disclosure, the physical film thickness may be a value measured by a spectroscopic film thickness meter. With a spectroscopic film thickness meter, a sample is irradiated with light, and an optical interference phenomenon caused by a phase shift based on the optical path difference between the irradiated light and the reflected light is measured, whereby the film thickness can be measured from the obtained reflection spectrum and refractive index. An example of a spectroscopic film thickness meter is a reflection spectroscopic film thickness meter (product name: FE-3000) manufactured by Otsuka Electronics Co., Ltd. However, in the present disclosure, the physical film thickness may be measured by a method other than the above.
[0047] [1-3. High refractive index film] Hereinafter, the high refractive index film in the reflectance adjustment film according to the embodiment of the present disclosure will be described with reference to an example.
[0048] The refractive index of the high refractive index film is not particularly limited as long as it is higher than the refractive index of the low refractive index film. For example, the refractive index for light with a wavelength of 500 nm is preferably such that the lower limit is 1.9 or more and the upper limit is 2.75 or less, 2.5 or less, or 2.3 or less.
[0049] In the reflectance adjusting film according to the embodiment of the present disclosure, the material for forming the high refractive index film is not particularly limited, but may be, for example, tantalum pentoxide (Ta 2 O 5 ), niobium pentoxide (Nb 2 O 5 ), titanium dioxide (TiO 2 ), zirconium oxide (ZrO 2 ), and cerium oxide (CeO 2 ), or may be formed of other materials. From the viewpoint of achieving both hardness and refractive index, the high refractive index film is preferably formed of tantalum pentoxide. Furthermore, when the high refractive index film is formed of tantalum pentoxide, it may or may not contain other materials. These atoms or materials forming them may be used alone, or a combination of two or more of these atoms and materials forming them may be used.
[0050] The physical thickness of the high refractive index film is not particularly limited and can be appropriately selected depending on the desired optical properties.
[0051] [1-4. Other membranes] The reflectance adjusting film according to the embodiment of the present disclosure may include, for example, other films. Examples of other films include a medium refractive index film. The medium refractive index film is not particularly limited as long as it has a refractive index higher than that of the low refractive index film and lower than that of the high refractive index film. The material for forming the medium refractive index film is not particularly limited, but may be, for example, aluminum oxide (Al 2 O 3 ) or may be formed of other materials.
[0052] [2. Method for manufacturing reflectance control film and method for manufacturing laminate] The method for producing the reflectance adjustment film according to the embodiment of the present disclosure and the laminate according to the embodiment of the present disclosure is not particularly limited, but for example, the low refractive index film and the high refractive index film may be formed sequentially on the substrate.
[0053] The method of forming the low refractive index film and the high refractive index film in the reflectance adjustment film according to the embodiment of the present disclosure is not particularly limited, but is preferably performed by, for example, a vacuum deposition method, a sputtering method, an ion plating method, or an ion beam deposition method, which are classified as physical vapor deposition, or an atomic layer deposition method or a plasma CVD method, which are classified as chemical vapor deposition. The deposition method has a tendency to form a film with a high film formation rate but low hardness (soft). The sputtering method has a tendency to form a film with a low film formation rate but high hardness (hard). In terms of hardness, the reflectance adjustment film according to the embodiment of the present disclosure is preferably formed by sputtering each of the low refractive index film and the high refractive index film. In the manufacturing method of the reflectance adjustment film according to the embodiment of the present disclosure and the manufacturing method of the laminate according to the embodiment of the present disclosure, as described above, in the low refractive index film forming step, the low refractive index film is formed by sputtering, and in the high refractive index film forming step, the high refractive index film is formed by sputtering.
[0054] The low refractive index film is made of yttrium oxide (Y 2 O 3 ), in order to replace some of the oxygen (O) atoms with nitrogen (N) atoms, for example, argon (Ar) can be replaced with nitrogen (N 2 Alternatively, the film may be formed by sputtering in an atmosphere containing 1,2-dichloroethane (reactive sputtering).
[0055] In the low refractive index film formation step and the high refractive index film formation step in the manufacturing method for a reflectance adjustment film according to an embodiment of the present disclosure and the manufacturing method for a laminate according to an embodiment of the present disclosure, the method of performing sputtering is not particularly limited, and may be, for example, similar to or equivalent to a general sputtering method.
[0056] In the low refractive index film formation process and the high refractive index film formation process, from the viewpoint of production efficiency, it is preferable that the film formation rate by the sputtering method is not too slow, and from the viewpoint of film hardness, it is preferable that the film formation rate by the sputtering method is not too fast. EXAMPLES
[0057] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.
[0058] <Materials used> Silicon dioxide (SiO 2 ), yttrium oxide (Y 2 O 3 ), and zirconium oxide (ZrO 2 Tantalum pentoxide (Ta 2 O 5 ) was used. Glass was used as the substrate.
[0059] <Production of Laminate Having Reflectance Adjustment Film Formed> A laminate having a reflectance adjusting film of each of Examples 1 to 3 and Comparative Example 1 was manufactured by a sputtering method. The sputtering of the low refractive index film and the high refractive index film described below was all performed using a nitrogen (N 2 First, the target for forming the low refractive index film was selected from the group consisting of yttrium oxide (Y 2 O 3 A low refractive index film was formed on one surface of the substrate by sputtering so that the composition of the first low refractive index film was as shown in Table 1 below (first layer, physical film thickness 250 nm). Next, a target for forming the high refractive index film was sputtered on the surface of the first low refractive index film to form a high refractive index film (second layer, physical film thickness 15 nm). Next, the target for forming the low refractive index film was sputtered using yttrium oxide (Y 2 O 3A low refractive index film was formed by sputtering the second high refractive index film so that the composition of the second high refractive index film was as shown in Table 1 below (third layer, physical thickness 30 nm). Next, a target for forming the high refractive index film was sputtered on the third low refractive index film to form a high refractive index film (fourth layer, physical thickness 115 nm). Finally, the target for forming the low refractive index film was changed to yttrium oxide (Y 2 O 3 A low refractive index film was formed by sputtering on the surface of the high refractive index film of the fourth layer so that the composition of yttrium oxide (Y) was as shown in Table 1 below (fifth layer, physical film thickness 86 nm). The laminate thus obtained, in which a reflectance control film was formed on a glass substrate, was evaluated. The low refractive index film formed by the above method was 2 O 3 ) in which some of the yttrium (Y) atoms are replaced by zirconium (Zr) atoms, and yttrium oxide (Y 2 O 3 ) in which some of the oxygen (O) atoms have been replaced by nitrogen (N) atoms.
[0060] <Evaluation method> For the low refractive index film formed as described above, (1) the refractive index was measured according to the following procedure. In addition, for the laminates formed with the reflectance adjusting films of Examples 1 to 3 and Comparative Example 1, (2) the hardness and (3) the average reflectance were measured according to the following procedure.
[0061] (1) Refractive index The refractive index of the low refractive index film was measured at a light wavelength of 500 nm using a reflection spectroscopic film thickness meter (manufactured by Otsuka Electronics Co., Ltd., product name: FE-3000). The results are shown in Table 1 below.
[0062] (2)Hardness The hardness of the reflectance adjustment film in the manufactured laminate was measured using a nanoindenter (manufactured by ELIONIX Co., Ltd., product name: ENT-1100a). A Berkovich indenter was used as the indenter, and the nanoindentation hardness (hardness) was measured when the reflectance adjustment film was pressed with a maximum load of 1.5 mN. Specifically, the indenter was first pressed into the sample at a constant rate until the maximum load was reached. Next, the load was removed at a constant rate until the load became 0, and the indenter was removed from the sample. The displacement of the indenter during loading and unloading was recorded to determine the maximum load. Next, the contact projected area (base area of the pyramid) of the contact portion when the indenter was pressed in was determined. The determined maximum load was divided by the contact projected area to determine the nanoindentation hardness. The results are shown in Table 1 below.
[0063] (3) Average reflectance Using optical simulation software (manufactured by TOHO TSUSHO INC., product name: ThinFilmView), simulation values of average reflectance in the visible light region (380 nm to 780 nm) were calculated. The results are shown in Table 1 below.
[0064] [Table 1]
[0065] As shown in Table 1, the hardness of Examples 1 to 3 was higher than that of Comparative Example 1. In addition, the hardness of the yttrium oxide (Y 2 O 3 The hardness increased by increasing the proportion of yttrium oxide (Y 2 O 3 By changing the ratio of , the average reflectance was calculated to change.
[0066] Moreover, the laminates of Examples 1 to 3 all had a total light transmittance of 95% as measured by an ultraviolet-visible-near infrared spectrophotometer (manufactured by Shimadzu Corporation, product name: SolidSpec-3700), which resulted in excellent transparency (not shown in Table 1). Furthermore, the laminates of Examples 1 to 3 all had a pencil hardness (based on the old JIS K5400) of 9H or more, which was high hardness (not shown in Table 1). In addition, the low refractive index film formed by the method of this example contains yttrium oxide (Y 2 O 3 ) in which some of the oxygen (O) atoms have been replaced with nitrogen (N) atoms, but yttrium oxide (Y 2 O 3 Even in low refractive index films in which the oxygen (O) atoms of yttrium oxide (Y 2 O 3 The hardness increased by increasing the proportion of (not shown in Table 1).
[0067] Furthermore, the present invention is not limited to the above-described embodiments, and can be arbitrarily and appropriately combined, modified, or selected and adopted as needed within the scope that does not deviate from the spirit of the present invention.
[0068] A part or all of the above-described embodiments may be described as follows, but is not limited to the following. (Appendix 1) A reflectance adjusting film for adjusting the reflectance of light, Multiple films are laminated, the plurality of films include a low refractive index film and a high refractive index film having a refractive index higher than that of the low refractive index film, The low refractive index film is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), provided that the yttrium oxide (Y 2 O 3 ) some of the yttrium (Y) atoms are replaced by atoms of group 4A elements, The refractive index of at least one of the films adjacent to the high refractive index film is smaller than the refractive index of the high refractive index film. Reflectance adjustment film. (Appendix 2) The yttrium oxide (Y 2 O 3 ) The reflectance adjusting film according to appendix 1, further comprising a part of oxygen (O) atoms substituted with nitrogen (N) atoms. (Appendix 3) The yttrium oxide (Y 2 O 3 3. The reflectance adjusting film according to claim 1 or 2, wherein the content of (Appendix 4) 4. The reflectance adjusting film according to claim 1, wherein the atom of the Group 4A element in the low refractive index film is a zirconium (Zr) atom. (Appendix 5) A reflectance adjusting film for adjusting the reflectance of light, It is a laminated film of multiple films, the plurality of films include a low refractive index film and a high refractive index film having a refractive index higher than that of the low refractive index film, The refractive index of at least one of the films adjacent to the high refractive index film is smaller than the refractive index of the high refractive index film; The hardness of the reflectance adjusting film is 6.0 GPa or more. Reflectance adjustment film. (Appendix 6) 6. The reflectance adjusting film according to any one of claims 1 to 5, wherein the refractive index of the low refractive index film for light with a wavelength of 500 nm is in the range of 1.47 to 1.58. (Appendix 7) 7. The reflectance adjusting film according to any one of claims 1 to 6, wherein the number of the plurality of films is three or more. (Appendix 8) The high refractive index film is made of tantalum pentoxide (Ta 2 O 5 ), niobium pentoxide (Nb 2 O 5 ), titanium dioxide (TiO 2 ), zirconium oxide (ZrO 2 ), and cerium oxide (CeO 28. The reflectance adjusting film according to claim 1, which is formed of at least one selected from the following: (Appendix 9) 9. The reflectance adjusting film according to any one of claims 1 to 8, which is an anti-reflection film for preventing reflection of light. (Appendix 10) A laminate comprising a reflectance control film according to any one of claims 1 to 9 formed on at least one surface of a substrate. (Appendix 11) 11. The laminate according to claim 10, wherein among the plurality of films in the reflectance adjustment film, the film farthest from the substrate is the low refractive index film. (Appendix 12) 12. The laminate according to claim 10 or 11, wherein the substrate is at least one of glass and resin. (Appendix 13) The method includes a low refractive index film forming step of forming the low refractive index film, and a high refractive index film forming step of forming the high refractive index film, In the low refractive index film forming step, the low refractive index film is formed by a sputtering method, and in the high refractive index film forming step, the high refractive index film is formed by a sputtering method. A method for producing a reflectance adjusting film according to any one of claims 1 to 9. (Appendix 14) A method for producing a laminate according to any one of claims 10 to 12, comprising the step of producing the reflectance control film on the substrate by the production method according to claim 13. [Explanation of symbols]
[0069] 10, 10a Reflectance adjustment film 11, 11a Low refractive index film 12, 12a High refractive index film 20 Base material 30 Hard coat layer 100, 100a laminate
Claims
1. A reflectance adjusting film for adjusting the reflectance of light, Multiple films are laminated, the plurality of films include a low refractive index film and a high refractive index film having a refractive index larger than that of the low refractive index film, The low refractive index film is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), provided that the yttrium oxide (Y 2 O 3 ) some of the yttrium (Y) atoms are replaced by atoms of a Group 4A element, The refractive index of at least one of the films adjacent to the high refractive index film is smaller than the refractive index of the high refractive index film. Reflectance adjustment film.
2. The yttrium oxide (Y 2 O 3 2. The reflectance adjusting film according to claim 1, wherein a part of oxygen (O) atoms is further substituted with nitrogen (N) atoms.
3. 3. The reflectance adjusting film according to claim 1, wherein the content of said yttrium oxide in said low refractive index film is 1.0 mol % or more.
4. 4. The reflectance adjusting film according to claim 1, wherein the atoms of the Group 4A element in the low refractive index film are zirconium (Zr) atoms.
5. 5. The reflectance adjusting film according to claim 1, wherein the refractive index of the low refractive index film for light having a wavelength of 500 nm is in the range of 1.47 to 1.
58.
6. The high refractive index film is tantalum pentoxide (Ta 2 O 5 The reflectance adjusting film according to claim 1 , which is formed of
7. The reflectance adjusting film according to claim 1 , which is an anti-reflection film for preventing reflection of light.
8. A laminate comprising the reflectance control film according to claim 1 formed on at least one surface of a substrate.
9. The laminate according to claim 8 , wherein the low refractive index film is the film farthest from the substrate among the plurality of films in the reflectance adjustment film.
10. The method includes a low refractive index film forming step of forming the low refractive index film, and a high refractive index film forming step of forming the high refractive index film, In the low refractive index film forming step, the low refractive index film is formed by a sputtering method, and in the high refractive index film forming step, the high refractive index film is formed by a sputtering method. A method for producing the reflectance adjustment film according to claim 1 .
Citation Information
Patent Citations
Lens with antireflection film
JP1991162943A
Optical member having antireflection film
JP1993011101A
Optical member with antireflection film
JP1993034502A
Optical article and manufacturing method
JP2006215081A
Method of suppressing splash and method for manufacturing plastic lens
JP2006284778A