Device and method for manufacturing alloy target material
The apparatus and method for manufacturing alloy target materials address the challenge of producing large, irregularly shaped materials with non-fixed compositions by using a nozzle, laser, and substrate to achieve uniformity and density, meeting specialized coating demands.
Patent Information
- Application Number
- JP2023099865
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-06-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-19
AI Technical Summary
Existing methods struggle to produce large, irregularly shaped alloy target materials with non-fixed compositions, particularly for applications requiring varying film compositions or doping at specific positions, as conventional methods like casting and powder metallurgy fail to achieve uniformity and density.
An apparatus and method utilizing a material nozzle, high-energy laser, and target material support substrate to spray and fuse micron-sized or nano-sized material powder, adjusting nozzle positions and angles, and controlling the laser beam to form alloy target materials with adjustable compositions and shapes, enabling layer-by-layer manufacturing.
The method produces alloy target materials with uniform composition and density, accommodating varying coating requirements, such as periodic doping, by ensuring precise control over the coating process and material distribution.
Smart Images

Figure 2024159377000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of target material technology, and in particular to an apparatus and method for producing alloy target materials. [Background technology]
[0002] For vacuum deposition processes such as magnetron sputtering and pulsed laser deposition, the material of the thin film is transferred from the surface of the target material, and the target material is one of its most important components. In recent years, the development and iteration of vacuum deposition technology has greatly promoted the progress of target material manufacturing technology. Based on the chemical composition and geometric shape of the target material, the target material has different classification methods. Distinguished by the chemical composition, the target material can be divided into oxide targets, ceramic targets, alloy targets, single metal targets, etc. Distinguished by the geometric shape, the target material can be divided into planar targets, irregular targets, etc. For each type of target material, the target material with simple chemical composition and geometric shape has a relatively simple manufacturing method, while the target material with complex composition or geometric shape is still difficult to manufacture.
[0003] Taking alloy target material with complex components as an example, currently, the manufacturing methods of alloy target material with complex components are mainly divided into two kinds: casting method and powder metallurgy method. The casting method is used to manufacture alloy target material, which has relatively high purity, but the alloy uniformity is relatively poor, especially when there is a large difference in melting point or density of the components, it is difficult to obtain alloy target material with uniform components. The powder metallurgy method is used to manufacture alloy target material, which can obtain target material with relatively uniform components, but the density is easily non-uniform, and it is difficult to manufacture target material with large size and irregular shape.
[0004] Meanwhile, some special coating scenarios impose new requirements on target materials, for example, in some applications, the composition of the thin film needs to be gradually and uniformly changed, or doped at some specific positions in the film layer, which requires the composition of the alloy target material to be not fixed but changed. The conventional target material manufacturing method cannot meet this need. Therefore, it is a problem to be solved in the prior art to provide a method for producing large, irregularly shaped alloy target materials with non-fixed composition. Summary of the Invention [Means for solving the problem]
[0005] The objective of the present invention is to provide an apparatus and method for manufacturing alloy target material, which can be used to produce alloy target material with large size, irregular shape, and non-fixed composition, and different coating scenes can meet the special requirements of the target material.
[0006] In order to achieve the above objectives, the present invention provides the following technical solutions: The present invention provides an apparatus for producing alloy target material, which includes a material nozzle, a high energy laser, and a target material support substrate. The material nozzle is disposed above the target material support substrate and is used to inject material powder required for manufacturing the alloy target material. The high energy laser is positioned above the target material support substrate and is used to generate a high energy laser beam. The target material support substrate supports a target material coating formed from the material powder and controls the size and shape of the target material coating. Preferably, the number of the material nozzles is three to five. Preferably, the apparatus for producing alloy target material further comprises a controller, the controller being connected to the material nozzle, the high energy laser and the target material support substrate.
[0007] The present invention further provides a method for producing an alloy target material, comprising the steps of: (1) Prepare the required material powder based on the chemical element composition of the alloy target material to be produced. (2) Dispensing the material powder in step (1) into the material nozzle of the manufacturing apparatus described in the technical solution, and then individually adjusting the spatial position and angle of the material nozzle to match the position and area sprayed by the material nozzle on the target material support substrate, thereby obtaining a focus surface of the same position and size.
[0008] The injection efficiency of the material nozzle is individually adjusted based on the stoichiometric ratio of each element at a specific position of the alloy target material to be manufactured, a high-energy laser is turned on, and the high-energy laser generates a high-energy laser beam to synchronously heat the material powder injected by the material nozzle onto the target material support substrate, so as to fuse the material powder to form a target material coating layer.
[0009] During the injection of the material powder, the target material support substrate is moved and sprayed to form a target material coating of a desired size and shape.
[0010] After the spraying of the previous target material coating layer is completed, the target material support substrate is moved, and the target material coating layer of the previous layer is successively sprayed on the upper surface of the target material coating layer to form a target material coating layer of the required size and shape for the next layer. By cyclically spraying one layer at a time, an alloy target material is obtained.
[0011] Preferably, in step (1), the material powder is an element or an alloy, and the material powder is micron-sized particles and / or nano-sized particles.
[0012] Preferably, the area of the focus surface in step (2) is 1 to 100 mm 2 The overlap rate between the material ejection nozzle and the focus plane is >95%.
[0013] Preferably, when the alloy target material is a periodically doped alloy target material, the material nozzle in step (2) obtains different focus planes on the target material support substrate, and sets the injection modes of the material nozzle in different focus planes, and adjusts the operation times of the different injection modes to realize periodic doping.
[0014] Preferably, the injection efficiency of the material nozzle in the above step (2) is 0 to 100 mm. 3 / s.
[0015] Preferably, in step (2), the target material support substrate or the material nozzle and the high-energy laser move in a three-dimensional space, and the relative speed of the movements is 1 to 100 mm / s.
[0016] Preferably, after the cyclical layer-by-layer thermal spraying in the step (2) is completed, the method further includes separating the alloy target material coating layer obtained by the cyclical layer-by-layer thermal spraying from the target material support substrate to obtain the alloy target material.
[0017] The present invention provides an apparatus for producing alloy target material, which includes a material nozzle, a high-energy laser and a target material support substrate. The material nozzle and the high-energy laser are respectively disposed above the target material support substrate. The present invention uses the material nozzle to inject the material powder required for the alloy target material to be produced, and the number of the material nozzles is set according to the type of material powder required for the alloy target material to be produced. The injection efficiency of the material nozzle is individually adjusted and set according to the stoichiometric ratio of each element at a specific position of the alloy target material to be produced, so as to meet the requirement of doping a specific position in the film layer in the coating scene, and to realize the purpose of the composition non-fixing of the alloy target material. And the thickness of the single-layer target material coating layer is controlled by adjusting the injection efficiency of the material nozzle. The spatial position and angle of the material nozzle are individually adjusted to ensure that the composition and density of the target material are uniform. The high-energy laser generates a high-energy laser beam to heat the target material support substrate, and heat the material powder sprayed on the surface of the target material support substrate and / or the target material coating layer formed after the material powder is fused, i.e., the spraying area is heated, and the material powder in the spraying area has sufficient ability to shape and diffuse, reach alloying, and form a target material coating layer with required composition. The present invention uses the target material support substrate to support the target material coating layer formed by the material powder. The target material support substrate is moved to realize the control of the size and shape of the target material coating layer. The target material coating layer is sprayed one layer at a time to produce a large-sized and irregular-shaped alloy target material. The manufacturing apparatus provided by the present invention can obtain an alloy target material with non-fixed composition, irregular shape, and large size, while overcoming the non-uniformity of composition and density in the manufacturing process of the conventional target material, and meeting the special requirements for the target material with different coating scenes. [Brief description of the drawings]
[0018] [Figure 1]FIG. 1 is a schematic diagram showing the structure of an apparatus for producing an alloy target material according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a focus plane in the present invention. [Diagram 3] FIG. 3 is a diagram showing the positional relationship between a target material coating layer and a target material support substrate in the present invention. [Figure 4] FIG. 4 is a schematic diagram of the microstructure of the BaHf-doped superconducting alloy target material YBa2Cu3 produced in Example 2 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention provides an apparatus for producing alloy target material, which includes a material nozzle 1, a high energy laser 2 and a target material support substrate 3.
[0020] The material nozzle 1 is provided above the target material support substrate 3 and is used to inject material powder required for the alloy target material to be prepared.
[0021] The high energy laser 2 is disposed above the target material supporting substrate 3 and is used to generate a high energy laser beam.
[0022] The target material supporting substrate 3 supports a target material coating layer formed from the material powder, and controls the size and shape of the target material coating layer.
[0023] As shown in FIG. 1, in an embodiment of the present invention, the manufacturing apparatus for the alloy target material includes a material nozzle 1. In the present invention, the material nozzle 1 is preferably a Laval nozzle. In the present invention, the number of the material nozzles 1 is preferably set according to the type of material powder required for the alloy target material waiting to be manufactured, and more preferably 3 to 5. In the present invention, the injection efficiency of the material nozzle 1 is preferably adjusted individually. In the present invention, the injection efficiency of the material nozzle 1 is preferably set according to the stoichiometric ratio of each element at a specific position of the alloy target material waiting to be manufactured. In the present invention, the spatial position and angle of the material nozzle 1 are preferably adjusted individually.
[0024] The present invention sets the injection efficiency of different material nozzles 1 by individually adjusting the spatial position and angle of the material nozzle 1, and based on the stoichiometric ratio of each element at a specific position of the alloy target material to be produced, thereby meeting the requirement of doping a certain position in the film layer in the coating scene, and realizing the purpose of non-fixing the components of the alloy target material.
[0025] As shown in Fig. 1, in an embodiment of the present invention, the apparatus for manufacturing the alloy target material includes a high-energy laser 2. The present invention uses a high-energy laser beam generated by the high-energy laser 2 to heat the target material support substrate, and heat the material powder sprayed on the surface of the target material support substrate 3 and / or the target material coating layer formed after the material powder is fused, i.e., heat the sprayed area, so that the material powder in the sprayed area has sufficient ability to be shaped and diffused to reach alloying, and form a target material coating layer of required composition.
[0026] As shown in Fig. 1, in an embodiment of the present invention, the apparatus for producing the alloy target material includes a target material supporting substrate 3. The present invention uses the target material supporting substrate 3 to support a target material coating layer formed by the material powder, and by moving the target material supporting substrate 3, it is possible to control the size and shape of the target material coating layer, and to spray the target material coating layer one by one, so as to finally produce alloy target materials with large sizes and irregular shapes, and different coating scenes can meet the special requirements for target materials.
[0027] In the present invention, the alloy target material manufacturing apparatus preferably further comprises a controller, which is connected to the material nozzle 1, the high-energy laser 2 and the target material support substrate 3. In the present invention, it is preferable that the material nozzle 1, the high-energy laser 2, and the target material support substrate 3 are each individually installed in a vacuum chamber containing an inert gas.
[0028] The present invention further provides a method for manufacturing an alloy target, comprising the steps of: (1) Prepare the required material powder according to the chemical element composition of the alloy target material to be manufactured. (2) Dispense the material powder in step (1) into the material nozzle 1 of the manufacturing apparatus of the technical solution, and then individually adjust the spatial position and angle of the material nozzle 1 to match the position and area sprayed by the material nozzle 1 on the target material support substrate 3, and obtain a focus surface of the same position and size.
[0029] The injection efficiency of the material nozzle 1 is individually adjusted according to the stoichiometric ratio of each element at a specific position of the alloy target material to be produced. A high-energy laser 2 is turned on, and the high-energy laser beam generated by the high-energy laser 2 is used to synchronously heat the material powder injected by the material nozzle 1 onto the target material support substrate 3, so as to fuse the material powder to form a target material coating layer.
[0030] During the spraying process of the material powder, the target material supporting substrate 3 is moved and sprayed to form a target material coating layer of a desired size and shape.
[0031] After the spraying of the previous layer of target material coating layer is completed, the target material support substrate 3 is moved, and the spraying is continued on the upper surface of the previous layer of target material coating layer to form a target material coating layer of the required size and shape of the next layer, and the spraying is cyclically performed layer by layer to obtain an alloy target material.
[0032] The present invention prepares the necessary material powders based on the chemical element composition of the alloy target material to be produced.
[0033] In the present invention, the material powder is preferably an element or an alloy. In the present invention, the material powder is preferably micron-sized particles and / or nano-sized particles. The present invention adopts micron-sized particles and / or nano-sized particles as material powder, which has the advantage of short element diffusion path, and at the same time, sufficient energy diffusion is obtained by the action of the auxiliary high-energy laser beam, so that the final target material coating layer obtained by injection has high uniformity of composition and density.
[0034] After obtaining the material powder, the present invention dispenses the material powder into the material nozzle 1 of the manufacturing apparatus of the technical solution, and then individually adjusts the spatial position and angle of the material nozzle 1 to match the position and area of the material nozzle 1 spraying on the target material support substrate 3, and obtains a focus surface of the same position and size.
[0035] In the present invention, the area of the focus surface is 1 to 100 mm 2It is preferable that the material nozzle 1 is 100% or less. In the present invention, the overlap rate between the material nozzle 1 and the focus surface is >95%. The present invention controls the overlap rate between the material nozzle 1 and the focus surface within the above range, and ensures that the material powders discharged from different material nozzles 1 are sprayed at the same position on the focus surface, and can be diffused to form an alloy with uniform composition, avoiding the reduction in the target material outline resolution and composition uniformity caused by an excessively large focus surface, and at the same time avoiding the low efficiency of target material production caused by an excessively small focus surface. The present invention individually adjusts the spatial position and angle of the material nozzle 1 to match the position and area of the material nozzle 1 sprayed on the target material support substrate 3, obtain the same position and size of the focus surface, and ensure the uniform composition and density of the target material.
[0036] In the present invention, when the alloy target material is a periodically doped alloy target material, the material nozzle preferably obtains different focus planes on the target material support substrate, and sets the injection modes of the material nozzle at the different focus planes, and adjusts the operation times of the different injection modes to realize the manufacture of the periodically doped alloy target material.
[0037] In the present invention, the operating times of the different injection modes are preferably adjusted based on the superlattice structure of the target thin film produced by depositing the periodically doped alloy target material.
[0038] In the present invention, the material nozzle 1 is preferably a Laval nozzle. The present invention adjusts the injection efficiency of the material nozzle 1 by controlling the speed of the working gas of the Laval nozzle. The present invention adjusts the injection efficiency of the material nozzle 1 individually according to the stoichiometric ratio of each element at a specific position of the alloy target material to be produced, so that the chemical element composition metric ratio of the material powder injected from different material nozzles 1 and the alloy target material to be produced in the spraying area are consistent, and finally a target target material coating layer with no fixed components is obtained.
[0039] In the present invention, the ejection efficiency of the material nozzle 1 is preferably 0 to 100 mm. 3 / s. The present invention controls the injection efficiency within the above range, and guarantees the uniformity of the composition of the target material while ensuring the target manufacturing efficiency. It avoids the dynamic process that too high injection efficiency limits the element diffusion process, which is not suitable for manufacturing a target material with uniform composition, and at the same time, it is possible to manufacture a target material with uniformly changing composition or periodically doped composition by adjusting the change in the injection efficiency of different material nozzles 1.
[0040] The present invention utilizes the high energy laser beam generated by the high energy laser 2 to synchronously heat the material powder sprayed by the material nozzle 1 onto the target material support substrate 3, thereby fusing the material powder to form a target material coating layer.
[0041] In the present invention, it is preferable that the target material support substrate 3 or the material nozzle 1 and the high energy laser 2 move in a three-dimensional space. In the present invention, it is preferable that the relative speed of the movement is 1 to 100 mm / s. The present invention controls the relative speed of the movement within the above range, achieving both efficiency and accuracy in the production of the target material, and avoids a too high movement speed from reducing the accuracy of the outer shape of the target material, while at the same time avoiding a too low movement speed from reducing the efficiency in the production of the target material.
[0042] In the present invention, during the moving process, the focus plane is preferably kept on the plane of the target material supporting substrate 3 to ensure the uniformity of the composition of the target material coating layer.
[0043] After the cyclical layer-by-layer thermal spraying is completed, the present invention separates the alloy target material coating layer obtained by the cyclical layer-by-layer thermal spraying from the target material support substrate 3 to obtain the alloy target material.
[0044] The manufacturing method of the alloy target material provided by the present invention uses laser assisted spraying and adopts additive manufacturing to spray the target material coating layer by layer, which can form an alloy target material with non-fixed composition, irregular shape and large size, while overcoming the non-uniformity of composition and density in the manufacturing process of traditional target materials, and meeting the special requirements for target materials with different coating scenes.
[0045] The following will refer to the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only some of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0046] Example 1 Using the alloy target material manufacturing equipment shown in Figure 1, a disk-shaped superconducting alloy target material YBa2Cu3 with a diameter of 15 cm and a thickness of 1 cm is manufactured. The manufacturing method is as follows: (1) Three types of material powders, namely, elemental Y powder, elemental Ba powder, and elemental Cu powder, are prepared based on the disk-shaped superconducting alloy target material YBa2Cu3. (2) The three kinds of material powders in step (1) are dispensed into three material nozzles 1 of the manufacturing equipment for the alloy target material, and then the spatial positions and angles of the three material nozzles 1 are individually adjusted to match the positions and areas sprayed by the three material nozzles 1 on the target material support substrate 3, and obtain focus surfaces at the same position and size.
[0047] The injection efficiency of the above three material nozzles 1, which inject simple Y powder, simple Ba powder, and simple Cu powder based on the stoichiometric ratio of each element of the disk-shaped superconducting alloy target material YBa2Cu3 (i.e., the alloy target material to be manufactured), is set to 19 mm 3 / s, 78mm 3 / s and 21.5mm 3 / s. The high-energy laser 2 is turned on, and the high-energy laser beam generated by the high-energy laser 2 is used to synchronously heat the material powders sprayed onto the target material support substrate 3 by the three material nozzles 1, so that the material powders are fused together to form a target material coating layer, and the target material coating layer has good uniformity with sufficient energy. During the spraying process of the material powder, the target material supporting substrate 3 is moved and sprayed to form a circular target material coating layer with a required diameter of 15 cm.
[0048] The alloy target material manufacturing apparatus further includes a controller, which is connected to the material nozzle 1, the high energy laser 2 and the target material support substrate 3.
[0049] The material nozzle 1, the high energy laser 2, and the target material support substrate 3 are individually positioned within a vacuum chamber containing an inert gas. After the spraying of the coating layer of the target material of the previous layer is completed, the target material support substrate 3 is moved, and spraying continues on the upper surface of the coating layer of the target material of the previous layer to form a circular coating layer of target material with a diameter of 15 cm required for the next layer, and spraying is continued cyclically layer by layer to obtain a disk-shaped superconducting alloy target material YBa2Cu3 with a thickness of 1 cm. The relative speed at which the target material support substrate 3 moves with respect to the material nozzle 1 is 1 mm / s.
[0050] Example 2 The alloy target material manufacturing apparatus shown in FIG. 1 is used to manufacture a BaHf-doped disk-shaped superconducting alloy target material YBa2Cu3 with a diameter of 15 cm and a thickness of 1 cm, which is used to deposit a YBa2Cu3O7+BaHfO3 superlattice thin film. The manufacturing method is as follows: (1) Based on the disk-shaped superconducting alloy target material YBa2Cu3 doped with BaHf, elemental Y powder, elemental Ba powder, elemental Cu powder and elemental Hf powder were prepared, which were made into four types of material powder and divided into five parts of material powder, of which the elemental Ba powder accounted for two parts. (2) The five portions of material powder in step (1) are dispensed into five material nozzles 1 of the manufacturing device for the alloy target material, and then the spatial positions and angles of the three material nozzles 1 to which the elemental Y powder, elemental Ba powder and elemental Cu powder are attached are individually adjusted to match the positions and areas sprayed by the three material nozzles 1 on the target material support substrate 3, and obtain focus surfaces at the same position and size. The spatial positions and angles of the remaining two material nozzles 1 to which the elemental Ba powder and elemental Hf powder are attached are individually adjusted to match the positions and areas sprayed by the two material nozzles 1 on the target material support substrate 3, and obtain other focus surfaces at the same position and size.
[0051] In order to obtain the same focal plane, the injection efficiencies of the three material nozzles 1 for injecting the above-mentioned simple Y powder, simple Ba powder, and simple Cu powder were set to 19 mm 3 / s, 78mm 3 / s and 21.5mm 3 The injection efficiency of the remaining two material nozzles 1 for injecting elemental Ba powder and elemental Hf powder to obtain the other focus planes was adjusted to 3.9 mm / s according to the stoichiometric ratio of each element of YBa2Cu3 in the disk-shaped superconducting alloy target material YBa2Cu3 doped with BaHf (i.e., the alloy target material waiting to be manufactured), and this injection mode was designated as Mode A. 3 / s and 3.9mm 3The injection mode is individually adjusted according to the stoichiometric ratio of each element of BaHf in the BaHf-doped disk-shaped superconducting alloy target material YBa2Cu3 (i.e., the alloy target material to be manufactured) so that the injection speed is 1s / s, and the injection mode is Mode B. During operation, the operation times of Mode A and Mode B are adjusted to 1s and 1s, respectively, according to the superlattice structure required for the target thin film, and are operated cyclically. The high-energy laser 2 is turned on, and the high-energy laser beam generated by the high-energy laser 2 is used to synchronously heat the material powder injected by the five material nozzles 1 onto the target material support substrate 3, and the material powder injected by operating in different modes is respectively fused to form a target material coating layer with a changing component period, and has good uniformity with sufficient energy. The microstructure schematic diagram of the BaHf-doped superconducting alloy target material YBa2Cu3 is shown in FIG. 4.
[0052] During the spraying process of the material powder, the target material supporting substrate 3 is moved and sprayed to form a circular target material coating layer with a required diameter of 15 cm. The alloy target material manufacturing apparatus further includes a controller, which is connected to the material nozzle 1, the high energy laser 2 and the target material support substrate 3. The material nozzle 1, the high energy laser 2, and the target material support substrate 3 are individually positioned within a vacuum chamber containing an inert gas. After the spraying of the previous layer of target material coating layer is completed, the target material support substrate 3 is moved, and the spraying continues on the upper surface of the previous layer of target material coating layer to form a circular target material coating layer with the required diameter of 15 cm for the next layer, and the spraying is cyclically performed layer by layer to obtain a disk-shaped superconducting alloy target material YBa2Cu3 doped with BaHf and having a thickness of 1 cm. The relative speed at which the target material support substrate 3 moves with respect to the material nozzle 1 is 1 mm / s. The prepared target material is applied to a pulsed laser deposition process, and the target material rotates uniformly during the deposition process, so that a superlattice nanostructure of YBa2Cu3O7 periodically doped with BaHfO3, i.e., YBa2Cu3O7+BaHfO3 superlattice thin film can be obtained.
[0053] Example 3 The alloy target material manufacturing apparatus shown in FIG. 1 is used to manufacture a circular superconducting alloy target material YBa2Cu3 with an outer diameter of 15 cm and an inner diameter of 13 cm, and the utilization rate of the target material in the pulsed laser deposition process is improved. The manufacturing method is as follows: (1) Three types of material powders, namely, elemental Y powder, elemental Ba powder, and elemental Cu powder, are prepared based on the disk-shaped superconducting alloy target material YBa2Cu3. (2) The three kinds of material powders in step (1) are dispensed into three material nozzles 1 of the manufacturing equipment for the alloy target material, and then the spatial positions and angles of the three material nozzles 1 are individually adjusted to match the positions and areas sprayed by the three material nozzles 1 on the target material support substrate 3, and obtain focus surfaces at the same position and size.
[0054] The injection efficiency of the above three material nozzles 1, which inject simple Y powder, simple Ba powder, and simple Cu powder according to the stoichiometric ratio of each element of the disk-shaped superconducting alloy target material YBa2Cu3 (i.e., the alloy target material waiting to be manufactured), was set to 19 mm 3 / s, 78mm 3 / s and 21.5mm 3 / s. The high-energy laser 2 is turned on, and the high-energy laser beam generated by the high-energy laser 2 is used to synchronously heat the material powders sprayed onto the target material support substrate 3 by the three material nozzles 1, so that the material powders are fused together to form a target material coating layer, and the target material coating layer has good uniformity with sufficient energy.
[0055] During the spraying process of the material powder, the target material supporting substrate 3 is moved and sprayed to form a ring-shaped target material coating layer with a required diameter of 15 cm and an inner diameter of 13 cm. The alloy target material manufacturing apparatus further includes a controller, which is connected to the material nozzle 1, the high energy laser 2 and the target material support substrate 3. The material nozzle 1, high energy laser 2, and target material support substrate 3 are individually positioned within a vacuum chamber containing an inert gas. After the spraying of the previous target material coating layer is completed, the target material support substrate 3 is moved, and the spraying continues on the upper surface of the previous target material coating layer to form a circular target material coating layer with a diameter of 15 cm and an inner diameter of 13 cm required for the next layer. By spraying cyclically layer by layer, a circular ring-shaped superconducting alloy target material YBa2Cu3 with a thickness of 1 cm is obtained. The relative speed at which the target support substrate 3 moves with respect to the material nozzle 1 is 1 mm / s.
[0056] As can be seen from the above, the manufacturing method of alloy target material provided by the present invention uses laser assisted spraying, adopts additive manufacturing to spray target material coating layer by layer, and can form alloy target material with non-fixed composition, irregular shape and large size, while overcoming the non-uniformity of composition and density in the manufacturing process of traditional target material, and meeting the special requirements of target material with different coating scenes. The above is merely a preferred embodiment of the present invention. Furthermore, those skilled in the art may make some improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered as within the scope of protection of the present invention. [Explanation of symbols]
[0057] 1 material nozzle, 2 high energy laser, 3 target material support substrate, 4 material powder, 5 target material coating layer, 6 focus plane, x x-axis in three-dimensional space, y y-axis in three-dimensional space, z z-axis in three-dimensional space
Claims
1. a material nozzle, a high energy laser, and a target material support substrate; The material nozzle is provided above the target material support substrate and is used to inject material powder required for the alloy target material to be manufactured; the high energy laser is disposed above the target material support substrate and is used to generate a high energy laser beam; The target material support substrate supports a target material coating layer formed from the material powder, and controls a size and shape of the target material coating layer. The present invention relates to an apparatus for manufacturing an alloy target material.
2. 2. The manufacturing apparatus according to claim 1, wherein the number of the material nozzles is 3 to 5.
3. The apparatus for producing an alloy target material further includes a controller. the controller is connected to the material nozzle, the high energy laser, and the target material support substrate; 2. The manufacturing apparatus according to claim 1.
4. 1. A method for producing an alloy target material, comprising the steps of: (1) preparing a required material powder according to the chemical element composition of an alloy target material to be produced; The material powder in the step (1) is dispensed into a material nozzle of the manufacturing apparatus according to any one of claims 1 to 3, and then the spatial position and angle of the material nozzle are individually adjusted to match the position and area of the material nozzle sprayed onto the target material support substrate, thereby obtaining a focus surface of the same position and size. adjust the injection efficiency of the material nozzle individually according to the stoichiometric ratio of each element at a specific position of the alloy target material to be manufactured, turn on a high-energy laser, and use a high-energy laser beam generated by the high-energy laser to synchronously heat the material powder injected by the material nozzle onto the target material support substrate, so as to fuse the material powder to form a target material coating layer; During the injection of the material powder, the target material support substrate is moved and sprayed to form a target material coating layer of a desired size and shape; After the spraying of the previous target material coating layer is completed, the target material support substrate is moved, and the previous target material coating layer is successively sprayed on the upper surface thereof to form a target material coating layer of a required size and shape for the next layer, and the spraying is cyclically performed layer by layer to obtain an alloy target material. A method for producing an alloy target material.
5. The method according to claim 4, wherein in step (1), the material powder is an element or an alloy, and the material powder is micron-sized particles and / or nano-sized particles.
6. The area of the focus surface in step (2) is 1 to 100 mm 2 5. The method of claim 4, wherein an overlap rate between the material ejection nozzle and the focus plane is >95%.
7. When the alloy target material is a periodically doped alloy target material, the material nozzle in step (2) obtains different focus planes on the target material support substrate; Setting the injection modes of the material nozzles in different focus planes, adjusting the operation times of the different injection modes, and realizing periodic doping; The method according to claim 4 .
8. The injection efficiency of the material nozzle in the step (2) is 0 to 100 mm 3 The method according to claim 4, wherein the formula (I) is a formula (I) / s.
9. The injection efficiency of the material nozzle in the step (2) is 0 to 100 mm 3 The method according to claim 7, wherein the formula (I) is a formula (I) / s.
10. 5. The manufacturing method according to claim 4, wherein in step (2), the target material support substrate or the material nozzle and the high-energy laser move in a three-dimensional space, and the relative speed of the movement is 1 to 100 mm / s.
11. 5. The method according to claim 4, further comprising, after the cyclical layer-by-layer thermal spraying is completed in step (2), separating the alloy target material coating layer obtained by the cyclical layer-by-layer thermal spraying from the target material support substrate to obtain an alloy target material.
Citation Information
Patent Citations
Sputtering target assembly with graded interlayer and method of making - Patent Application 20070122997
JP2019518865A
Method for producing three-dimensional molding, and device for producing three-dimensional molding
JP2021085041A
Processing nozzle, processing head, processing device
WO2016151781A1