Exterior component formed of ceramic material including protective layer and method for manufacturing such exterior component
A transparent inorganic coating with controlled refractive index and thickness protects ceramic components from mechanical and chemical damage while maintaining their aesthetic appearance.
Patent Information
- Application Number
- JP2024026492
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-02-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-02-26
AI Technical Summary
Existing protective layers for ceramic exterior components in watchmaking and jewelry are not transparent, do not absorb optical radiation, and lack resistance to chemical and mechanical attacks, making them unsuitable for decorative applications.
A transparent inorganic protective coating with a thickness between 300 nm and 5 μm is applied to ceramic substrates, matching the substrate's refractive index to minimize optical interference and provide mechanical and chemical protection.
The coating maintains the substrate's appearance while offering excellent resistance to abrasion and chemical attacks, ensuring the substrate's unique color is preserved.
Smart Images

Figure 2024159500000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to ornamentation in the field of watchmaking, jewellery or clothing, and more particularly to an exterior part made of a ceramic material comprising a protective coating and to a method for manufacturing such an exterior part.
[0002] In this specification, the term "exterior part" is commonly used in the above mentioned fields to refer to parts that are visible to the user, in particular parts that have a decorative function.
[0003] Apparel accessories also include articles or accessories for clothing such as belts, shoes, clothing, and further include writing instruments, eyeglasses, leather goods, telephones, or any decorative item. [Background technology]
[0004] In the field of watchmaking, many solutions have been developed to protect ceramic exterior parts such as dials, flanges, bezels, middles, crowns, push-pieces, links, etc. from chemical and / or mechanical attacks that could alter their appearance or color.
[0005] By way of example, the exterior component may include a thin protective layer deposited by a vacuum deposition process such as PVD (physical vapor deposition), CVD (chemical vapor deposition) or ALD (atomic layer deposition) deposition processes.
[0006] However, the prior art solutions are not entirely satisfactory: in fact, prior art protective layers are not completely transparent and yet have a small thickness, for example less than 5 μm, i.e. do not absorb a portion of the incident light radiation in the visible region of the light spectrum, do not produce interference colors and do not have adequate resistance to chemical and mechanical attack.
[0007] It should be noted that thin layers deposited by ALD deposition have advantages over thin layers deposited by PVD and CVD deposition: in fact, these ALD thin layers are very effective in protecting the substrate from chemical attack and, due to their small thickness, are invisible to the naked eye and do not affect the appearance of the substrate they cover.
[0008] However, these layers are very thin and therefore very sensitive to mechanical stresses such as friction and shocks, and therefore cannot be used to cover exterior parts that may come into contact with external elements, such as the bezel or middle of a watch.
[0009] Layers with thicknesses greater than those of ALD thin layers, typically in the micron range, offer greater resistance to mechanical stress, but are visible on the substrate and therefore do not meet the requirements, especially if the appearance of the substrate needs to be maintained for decorative reasons. Summary of the Invention [Problem to be solved by the invention]
[0010] There is therefore a need for protective solutions that are effective against chemical and mechanical attack and that are suitable for preserving the appearance of the substrates thus protected. [Means for solving the problem]
[0011] The present invention overcomes the above-mentioned drawbacks and for this purpose relates to an exterior part, preferably for a watch, comprising a substrate made of a ceramic material, on whose surface a transparent inorganic protective coating extends, the coating being configured, at least at its interface with the substrate, to have a refractive index substantially equal to that of the substrate for wavelengths in the visible range of the light spectrum, so that no or only very few interference phenomena occur, i.e. are substantially invisible to the naked eye, and the exterior part has a color substantially identical to the intrinsic color of the substrate.
[0012] The coating also has a relatively small thickness, which saves deposition time and manufacturing costs of the exterior parts, while being thick enough to provide good mechanical resistance to abrasion and good protection against chemical attack. In particular, the coating has a thickness of 300 nm to 5 μm. The coating can advantageously have a high hardness, typically a Vickers hardness of the order of 25 GPa.
[0013] Thus, the present invention allows for the protection of exterior components while allowing the native color of the substrate to be preserved.
[0014] In particular embodiments, the invention may further include one or more of the following features, taken alone or in any technically possible combination:
[0015] In certain embodiments, the protective coating is configured such that the protective coating imparts a color to the exterior component that is characterized by a difference from the intrinsic color of the substrate of Delta E≦10 in L*a*b* color space.
[0016] In certain embodiments, the protective coating is configured such that the protective coating imparts a color to the exterior component that is characterized by a difference from the native color of the substrate of delta E≦5 in L*a*b* color space.
[0017] In certain embodiments, the protective coating has a thickness of from 300 nm to 1 μm.
[0018] In certain embodiments, the protective coating is formed from at least two compounds having refractive indices greater and less than that of the substrate for wavelengths in the visible region of the light spectrum, respectively. By controlling the proportion of each compound in the protective coating composition, the refractive index of the protective coating can be precisely controlled to be substantially equal to that of the substrate, thereby eliminating interference phenomena.
[0019] In a particular embodiment, the protective coating is Tix Al y O z The at least one layer is made of
[0020] In a particular embodiment, the protective coating is Si x O y N z The at least one layer is made of
[0021] In a particular embodiment, the substrate may be made of an oxide, a nitride, a carbide, a carbonitride or a boride, in particular alumina Al2O3, zirconia ZrO2 or an alumina-zirconia composite.
[0022] According to another aspect, the invention further relates to a method for producing an exterior part, such as that described above, comprising the steps of preparing a surface of a substrate and depositing a transparent inorganic protective coating on said surface by a vacuum deposition method in a reactive or non-reactive atmosphere.
[0023] The depositing step is performed from at least one source of at least one material selected such that the protective coating has a refractive index substantially equal to the refractive index of the substrate in the visible region of the light spectrum, said step also being performed such that the protective coating has a thickness of 300 nm to 5 μm such that the protective coating is resistant to mechanical and chemical attack.
[0024] In a particular implementation, the step of depositing the protective coating is performed by cathodic sputtering.
[0025] In a particular implementation, the protective coating is deposited from at least two sources of different materials selected such that during the deposition step, each of the materials forms a compound having a refractive index in the visible region of the light spectrum greater than and less than that of the substrate, respectively, and the sputtering power of each source is controlled such that the proportion of each compound in the protective coating is such that the coating has substantially the same refractive index as that of the substrate.
[0026] In a particular implementation, the protective coating is deposited from at least one source of a mixture of at least two materials, said materials being selected such that during the deposition step, said materials each form a compound having a refractive index in the visible region of the light spectrum that is greater than and less than the refractive index of the substrate, respectively, and the source is prepared to contain predetermined proportions of said materials such that at the end of the deposition step, the protective coating has a refractive index that is substantially the same as the refractive index of the substrate.
[0027] In a particular implementation, the materials selected are Al and Ti, and the deposition step is performed such that at the end of the deposition step, a protective coating is applied to the Ti x Al y O z The method is carried out using O2 as a reactive gas to form a mixture of TiO2 and Al2O3 to form a compound of the type.
[0028] In a particular implementation, the protective coating is deposited from at least one source of a single material selected to form several compounds of the single material by reacting with several reactive gases present during the deposition step, the compounds having refractive indices greater than and less than the refractive index of the substrate, respectively, in the visible region of the light spectrum, the reactive gases being present in a predetermined ratio such that at the end of the deposition step, the protective coating has a refractive index substantially identical to that of the substrate.
[0029] In a particular implementation, the deposition step comprises depositing a protective coating of Si at the end of the deposition step. x O y N z The deposition was carried out from a source made of Si, using O2 and N2 as reactive gases, to form compounds of the type containing a mixture of SiO2 and Si3N4. [Brief description of the drawings]
[0030] Other characteristics and advantages of the invention will become apparent from the following detailed description, given by way of non-limiting example with reference to FIG. [Figure 1] 1 shows a schematic cross-sectional view of an exterior part according to a preferred embodiment of the present invention;
[0031] Please note that the figures are not necessarily drawn to scale for clarity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The present invention relates to an external part 10, as shown diagrammatically in figure 1. The external part 10 according to the invention is suitable for the fields of watchmaking, jewellery, clothing etc. Preferably, the external part 10 is intended to form a watch dial, a middle, a bezel, a bracelet or any other watch part visible to the user.
[0033] The exterior component 10 comprises a dielectric substrate 11 made of a ceramic material, such as alumina Al2O3, zirconia ZrO2, or an alumina-zirconia composite, with or without a pigment to color said substrate. The exterior component 10 further comprises a transparent inorganic protective coating 12 extending over the surface of the substrate 11 that is intended to be visible to the user.
[0034] It should be noted that the term "transparent" in this specification refers to the ability of a material to not absorb light in a manner visible to the human eye.
[0035] The protective coating 12 may be formed of a single thin layer or multiple thin layers.
[0036] Advantageously, the protective coating 12 is capable of protecting the substrate 11 from chemical attack, especially caused by humidity, sulfur gases, oxygen and acidic environments, and is further dimensioned to withstand mechanical stresses, especially caused by friction or impact.
[0037] For this purpose, the protective coating 12 extends over a thickness chosen for example between 300 nm and 5 μm, more particularly between 300 nm and 1 μm. Preferably, the thickness of the protective coating 12 is equal to 1 μm.
[0038] Protective coating 12 is configured to have a refractive index in the visible region of the light spectrum substantially equal to that of substrate 11, at least at its interface with said substrate 11. As used herein, the refractive index of protective coating 12 is substantially equal to that of substrate 11 to within plus or minus 5 percent of the value of substrate 11.
[0039] Advantageously, these characteristics allow protective coating 12 to produce little or no optical interference, thus allowing exterior component 10 protected by layer 12 to have the native color of substrate 11. It should be noted that any interference that does occur is so slight as to be invisible to the user and therefore negligible.
[0040] The concept of "intrinsic color" refers herein to the color of the uncoated substrate 11, as perceived by a user when illuminated with white light, due to the material that constitutes the substrate 11. Thus, the protective coating 12 is invisible to the naked eye in the sense that the exterior part 10 has substantially the same color with or without the protective coating 12 deposited on the substrate 11.
[0041] More specifically, protective coating 12 is configured such that protective coating 12 imparts a color to exterior component 10 that is characterized by a difference from the native color of substrate 11 in L*a*b* color space of Delta E≦10, and more specifically Delta E≦5.
[0042] In summary, thanks to the features of the present invention, exterior component 10 includes chemical protection for substrate 11 while maintaining the aesthetic appearance and mechanical strength of the substrate.
[0043] Preferably, the protective coating is formed from at least two compounds having a higher and lower refractive index than substrate 11, respectively, for wavelengths in the visible region of the light spectrum.
[0044] For example, protective coating 12 may include a mixture of TiO2, which has a high refractive index, and Al2O3, which has a low refractive index. It should be noted that this example of protective coating 12 is not compatible with substrates 11 made of materials whose refractive index is lower than that of a coating of Al2O3 alone or higher than that of a coating of TiO2 alone.
[0045] Alternatively, the protective coating 12 may include a mixture of Si3Ni4, which has a high refractive index, and SiO2, which has a low refractive index.
[0046] More generally, in summary, the protective coating 12 may be Ti x Al y O z or Si x O y N z The at least one thin layer may be made of
[0047] The present invention also relates to a method for manufacturing an exterior part 10, such as the aforementioned exterior part 10. The method comprises the steps of preparing a surface of a substrate 11 intended to be visible to a user and depositing a protective coating 12 on said surface by a vacuum deposition method.
[0048] The preparation step may include polishing, sandblasting, brushing, satin finishing, or performing any other surface treatment operation on the substrate 11.
[0049] The deposition step is carried out using one or more sources of material, the composition of which is selected to form a protective coating 12 having a refractive index substantially equal to that of the substrate 11 in the visible region of the light spectrum.
[0050] This deposition step is also performed so as to deposit the protective coating 12 in such a way that it has a thickness such that it is resistant to mechanical attack, in particular abrasion and chemical attack, as described above.
[0051] Furthermore, the method can include a preliminary step of preparing at least one material source to be used during the deposition step. The step of preparing the source makes it possible, for example, to adapt the appropriate type of source depending on the vacuum deposition method to be used during the deposition step and to adapt the proportions of materials in the source when the source comprises several materials in order to obtain the desired protective coating 12. The type of material source differs depending on the vacuum deposition method used in that the source is a target in solid form if the deposition method used is a physical vapor deposition PVD method and the source is a gas phase precursor if the deposition method used is a chemical vapor deposition CVD method or an atomic layer deposition ALD method.
[0052] In one variant implementation of the method, the protective coating 12 is deposited from at least two sources of different materials, for example different metallic materials. The materials are selected such that during the deposition step, each of the materials forms a compound, for example an oxide, nitride or carbide, which has a refractive index in the visible region of the light spectrum that is greater than and less than that of the substrate 11, respectively. During the deposition step, by controlling the sputtering power of each source, the proportion of each compound deposited to form the protective coating 12 is controlled so that the protective coating 12 has a desired refractive index. This desired refractive index of the protective coating 12 is substantially the same as the refractive index of the substrate 11, as described above.
[0053] For example, one of the materials can be Al and the other Ti. A preparatory step is performed to obtain two sources, one made of Ti and the other made of Al, and the deposition step is performed with O2 as reactive gas. In this example, at the end of the deposition step, the protective coating 12 is formed from a mixture of TiO2 and Al2O3. These two metal oxides have higher and lower refractive indices than the refractive index of the substrate 11, respectively, so that by controlling their proportions in the protective coating 12, the refractive index of the coating 12 can be controlled.
[0054] In another variant implementation of the method, the protective coating 12 is deposited from at least one source of a mixture of at least two materials, said materials also being selected such that during the deposition step, each of said materials forms a compound, for example an oxide, a nitride, a boride or a carbide, said compounds having a refractive index in the visible region of the light spectrum that is greater and less than that of the substrate 11, respectively. During a preliminary step, the sources are prepared containing predetermined proportions of said materials in order to control the composition of the deposited protective coating 12, so that the protective coating 12 has the desired refractive index at the end of the deposition step.
[0055] For example, a preparatory step can be performed to obtain a source of a mixture of Ti and Al, and a deposition step can be performed with O2 as reactive gas. In this example, at the end of the deposition step, the protective coating 12 consists of a mixture of TiO2 and Al2O3. As in the previous variant implementation, these two metal oxides have higher and lower refractive indices than the refractive index of the substrate 11, respectively, so that by controlling their proportions in the protective coating 12, the refractive index of the coating 12 can be controlled to be substantially equal to that of the substrate 11. Since the sources are prepared upstream with a predetermined proportion of each material, this variant is more suitable for industrially implementing the method in a simple, fast and stable manner.
[0056] In yet another variant implementation of the method, the protective coating 12 can be deposited from at least one source of a single material selected such that during the deposition step, the single material forms various compounds depending on the reactive gas used, such as O2 or N2. In the visible region of the light spectrum, the compounds have refractive indices lower and higher than that of the substrate 11, respectively. Thus, by controlling the amount of each gas present during the deposition step, the stoichiometric composition of the compounds constituting the protective coating 12 can be controlled to obtain the desired refractive index of the protective coating 12.
[0057] For example, a pre-preparation step can be performed to obtain a Si source and the deposition step can be performed with N2 and O2 as reactive gases. In this example, at the end of the deposition step, the protective coating 12 consists of a mixture of SiO2 and Si3N4. Thus, by mixing metal oxides with nitrides of the same metals in controlled proportions, the refractive index of the coating 12 can be controlled to be substantially the same as that of the substrate 11.
[0058] These different variants advantageously make it possible to obtain, with high flexibility and in a relatively simple manner, a protective coating 12 having an effective refractive index that corresponds as accurately as possible to the refractive index of the substrate 11 by adjusting the proportions between the different compounds that make up the protective coating 12.
[0059] The step of depositing the protective coating 12 is preferably carried out in a reactive or non-reactive atmosphere by a physical vapor deposition (PVD) method, for example by arc evaporation, laser ablation, ion beam sputtering or electron beam or Joule effect deposition, preferably by cathodic sputtering. Alternatively, the deposition step can be carried out by any chemical vapor deposition (CVD) or atomic layer deposition (ALD) method.
[0060] More generally, it should be noted that the above implementations and embodiments are described as non-limiting examples, and therefore other variations are possible.
[0061] In particular, materials other than those described in the variant implementations of the method described above can be used, and in particular, although the use of metallic material sources has been described, it is also possible to use non-metallic material sources.
Claims
1. 1. An exterior part (10), comprising a substrate (11) made of a ceramic material, on the surface of which extends a transparent inorganic protective coating (12), the protective coating (12) being configured to have a refractive index substantially equal to that of the substrate (11) in the visible region of the light spectrum, such that the exterior part (10) has a color substantially identical to the intrinsic color of the substrate (11), the coating (12) extending over a thickness selected between 300 nm and 5 μm.
2. 2. The exterior part (10) of claim 1, wherein the protective coating (12) is configured such that it imparts to the exterior part (10) a color that differs from the intrinsic color of the substrate (11) by a delta E≦10 in L*a*b* color space.
3. 3. The exterior part (10) of claim 2, wherein the protective coating (12) is configured such that it imparts to the exterior part (10) a color whose difference from the intrinsic color of the substrate (11) is characterized by a delta E≦5 in L*a*b* color space.
4. The exterior part (10) of claim 1, wherein the protective coating (12) has a thickness of from 300 nm to 1 μm.
5. 2. The exterior part (10) of claim 1, wherein the protective coating (12) is formed from at least two compounds having refractive indices greater than and less than the refractive index of the substrate, respectively, for wavelengths in the visible region of the light spectrum.
6. The protective coating (12) is Ti x A y O z The exterior part (10) according to claim 1, comprising at least one layer made of
7. The protective coating (12) is Si x O y N z The exterior part (10) according to claim 1, comprising at least one layer made of
8. The substrate (11) is made of alumina Al 2 O 3 , Zirconia ZrO 2 or an alumina-zirconia composite.
9. A method for manufacturing an exterior part (10), comprising the steps of: - preparing the surface of the substrate (11); depositing a transparent inorganic protective coating (12) on said surface by vacuum deposition; Including, The method of claim 1, wherein the depositing step is performed from at least one source of at least one material selected such that the protective coating (12) has a refractive index substantially equal to the refractive index of the substrate (11) in the visible region of the light spectrum, and the step is also performed such that the protective coating (12) has a thickness of 300 nm to 5 μm.
10. The method of claim 9, wherein the step of depositing a protective coating (12) is performed by cathodic sputtering.
11. 10. The method of claim 9, wherein the protective coating (12) is deposited from at least two sources of different materials, the materials being selected so as to form during the deposition step, each of the compounds having a refractive index in the visible region of the light spectrum greater than and less than the refractive index of the substrate (11), respectively, and the sputtering power of each source being controlled such that the proportion of each compound in the protective coating (12) is such that the coating has substantially the same refractive index as the refractive index of the substrate (11).
12. 10. The method of claim 9, wherein the protective coating (12) is deposited from at least one source of a mixture of materials, the materials being selected so as to form, during the deposition step, a compound each having a refractive index in the visible region of the light spectrum greater than and less than the refractive index of the substrate (11), the sources being prepared to contain predetermined proportions of the materials, such that the protective coating (12) has, at the end of the deposition step, substantially the same refractive index as that of the substrate (11).
13. The materials selected are Al and Ti, and the deposition step is carried out such that at the end of the deposition step, the protective coating (12) is x A y O z To form compounds of the type TiO 2 and Al 2 O 3 The reaction gas contains a mixture of O 2 The method according to claim 11 or 12, which is carried out using
14. 10. The method of claim 9, wherein the protective coating (12) is deposited from at least one source of a single material selected such that during the deposition step it forms several compounds by reacting with several reactive gases present, the compounds having refractive indices in the visible region of the light spectrum greater and smaller than the refractive index of the substrate (11), respectively, the reactive gases being present in a predetermined ratio such that at the end of the deposition step the protective coating (12) has a refractive index substantially identical to that of the substrate (11).
15. The deposition step is carried out such that at the end of the deposition step, the protective coating (12) is Si x O y N z To form compounds of the type SiO 2 and Si 3 N 4 The reactive gas is O from a source made of Si, so as to contain a mixture of 2 and N 2 The method according to claim 14, wherein the method is carried out using
Citation Information
Patent Citations
Coated articles with protective coatings and cathode targets for making coated articles
JP2005523832A
Titanium oxide transparent coating containing at least one of aluminum and aluminum oxide and having a rutile structure
JP2006518809A
Substrate with antibacterial properties
JP2009541189A