Method for producing composition containing polytetrafluoroethylene, and composition containing polytetrafluoroethylene

By polymerizing tetrafluoroethylene with polymer (I) in an aqueous medium and using solvent-coagulant coagulation, the method addresses high residual polymer content issues, resulting in efficient and high-yield polytetrafluoroethylene compositions with reduced polymer (I).

JP2024159739APending Publication Date: 2024-11-08DAIKIN INDUSTRIES LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024073898
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for producing polytetrafluoroethylene compositions result in high residual content of polymer (I), leading to inefficiencies and challenges in obtaining compositions with reduced polymer (I) content.

Method used

A method involving the polymerization of tetrafluoroethylene in an aqueous medium with polymer (I), followed by coagulation and washing with an organic solvent and coagulant, to efficiently remove polymer (I) from the polytetrafluoroethylene composition.

Benefits of technology

The method effectively reduces the polymer (I) content in the polytetrafluoroethylene composition, achieving higher yields and improved purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159739000001
    Figure 2024159739000001
  • Figure 2024159739000002
    Figure 2024159739000002
  • Figure 2024159739000003
    Figure 2024159739000003
Patent Text Reader

Abstract

To provide a method for producing a composition containing polytetrafluoroethylene by polymerizing tetrafluoroethylene in the presence of a polymer containing a specific polymerization unit, where this method enables the production of a composition where the content of a polymer containing a specific polymerization unit is reduced compared to the composition obtained by the conventional production method.SOLUTION: A method for producing a composition containing polytetrafluoroethylene includes polymerizing tetrafluoroethylene in an aqueous medium in the presence of a polymer (I) containing a polymerization unit (I) based on a monomer (I) represented by the general formula (I), to obtain a polymerized dispersion liquid containing polytetrafluoroethylene. The polytetrafluoroethylene in the polymerized dispersion liquid, an organic solvent, and a coagulation agent are brought into contact with each other, to coagulate the polytetrafluoroethylene in the polymerized dispersion liquid, thereby obtaining a composition containing the polytetrafluoroethylene. CX1X3=CX2R(-CZ1Z2-A0)m (I) (each symbol in the formula is as defined in the specifications).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for making a composition containing polytetrafluoroethylene and to a composition containing polytetrafluoroethylene. [Background technology]

[0002] Patent Document 1 describes a method for producing a fluoropolymer, which includes a step of obtaining a fluoropolymer by polymerizing a fluoromonomer in an aqueous medium in the presence of a polymer (1) containing polymerized units (1) based on a monomer represented by the following general formula (1). CX2=CY(-CZ2-O-Rf-A) (1) (In the formula, X may be the same or different and is -H or -F; Y is -H, -F, an alkyl group or a fluorine-containing alkyl group; Z may be the same or different and is -H, -F, an alkyl group or a fluoroalkyl group; Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms or a fluorine-containing alkylene group having 2 to 100 carbon atoms and having an ether bond; A is -COOM, -SO3M or -OSO3M (M is -H, a metal atom, -NR 7 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7 is H or an organic group, provided that at least one of X, Y, and Z contains a fluorine atom.

[0003] Patent Document 2 describes a method for producing a fluoropolymer composition, in which a fluoropolymer raw material obtained by polymerizing a fluoromonomer in an aqueous medium in the presence of a polymer (I) containing a polymerization unit (I) based on a monomer (I) represented by general formula (I) is contacted with an oxidizing agent. CX 1 X 3 =CX 2 R(-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X3 are each independently F, Cl, H or CF; X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2019 / 168183 [Patent Document 2] International Publication No. 2023 / 277139 Summary of the Invention [Problem to be solved by the invention]

[0005] The present disclosure has an object to provide a production method for producing a composition containing polytetrafluoroethylene by polymerizing tetrafluoroethylene in the presence of a polymer containing specific polymerization units, which is capable of producing a composition in which the content of the polymer containing specific polymerization units is reduced compared to compositions obtained by conventional production methods. [Means for solving the problem]

[0006] According to the present disclosure, there is provided a method for producing a composition containing polytetrafluoroethylene, comprising: polymerizing tetrafluoroethylene in an aqueous medium in the presence of a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I) to obtain a polymerization dispersion containing polytetrafluoroethylene; and contacting the polytetrafluoroethylene in the polymerization dispersion with an organic solvent and a coagulant to coagulate the polytetrafluoroethylene in the polymerization dispersion to obtain a composition containing polytetrafluoroethylene. CX 1 X 3 =CX 2 R(-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF; X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a production method for producing a composition containing polytetrafluoroethylene by polymerizing tetrafluoroethylene in the presence of a polymer containing specific polymerization units, which can produce a composition in which the content of the polymer containing specific polymerization units is reduced compared to compositions obtained by conventional production methods. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Before specifically describing the present disclosure, some terms used in the present disclosure will be defined or explained.

[0009] In the present disclosure, fluororesins are partially crystalline fluoropolymers, or fluoroplastics. Fluororesins have a melting point and are thermoplastic, but may be melt-processable or non-melt-processable.

[0010] In the present disclosure, melt processability means that the polymer can be melted and processed using conventional processing equipment such as an extruder, an injection molding machine, etc. Therefore, melt processable polytetrafluoroethylene usually has a melt flow rate of 0.01 to 500 g / 10 min, as measured by the measurement method described below.

[0011] In the present disclosure, polytetrafluoroethylene [PTFE] is preferably a fluoropolymer having a content of tetrafluoroethylene units relative to all polymerized units of 99 mol % or more.

[0012] In the present disclosure, any fluororesin (excluding polytetrafluoroethylene) is preferably a fluoropolymer having a tetrafluoroethylene unit content of less than 99 mol % relative to all polymerized units.

[0013] In the present disclosure, the content of each monomer constituting the fluoropolymer can be calculated by an appropriate combination of NMR, FT-IR, elemental analysis, and X-ray fluorescence analysis depending on the type of monomer.

[0014] In this disclosure, "organic group" means a group containing one or more carbon atoms or a group formed by removing a hydrogen atom from an organic compound. Examples of the "organic group" are: an alkyl group which may have one or more substituents; an alkenyl group optionally having one or more substituents; an alkynyl group optionally having one or more substituents; a cycloalkyl group optionally having one or more substituents, a cycloalkenyl group optionally having one or more substituents, a cycloalkadienyl group optionally having one or more substituents, an aryl group which may have one or more substituents; an aralkyl group optionally having one or more substituents; a non-aromatic heterocyclic group optionally having one or more substituents, a heteroaryl group optionally having one or more substituents, Cyano group, Formyl group, RaO-, RaCO-, RaSO2-, RaCOO-, RaNRaCO-, RaCONRa-, RaOCO-, RaOSO2-, and RaNRbSO2- (In these formulas, Ra is independently an alkyl group which may have one or more substituents; an alkenyl group optionally having one or more substituents; an alkynyl group optionally having one or more substituents; a cycloalkyl group optionally having one or more substituents, a cycloalkenyl group optionally having one or more substituents, a cycloalkadienyl group optionally having one or more substituents, an aryl group which may have one or more substituents; an aralkyl group optionally having one or more substituents; a non-aromatic heterocyclic group optionally having one or more substituents, or a heteroaryl group optionally having one or more substituents, Rb is independently H or an alkyl group which may have one or more substituents. Includes: The organic group is preferably an alkyl group which may have one or more substituents.

[0015] In the present disclosure, a "substituent" means a substitutable group. Examples of the "substituent" include an aliphatic group, an aromatic group, a heterocyclic group, an acyl group, an acyloxy group, an acylamino group, an aliphatic oxy group, an aromatic oxy group, a heterocyclic oxy group, an aliphatic oxycarbonyl group, an aromatic oxycarbonyl group, a heterocyclic oxycarbonyl group, a carbamoyl group, an aliphatic sulfonyl group, an aromatic sulfonyl group, a heterocyclic sulfonyl group, an aliphatic sulfonyloxy group, an aromatic sulfonyloxy group, a heterocyclic sulfonyloxy group, a sulfamoyl group, an aliphatic sulfonamide group, an aromatic sulfonamide group, a heterocyclic sulfonamide group, an amino group, an aliphatic amino These include an aromatic amino group, an aromatic amino group, a heterocyclic amino group, an aliphatic oxycarbonylamino group, an aromatic oxycarbonylamino group, a heterocyclic oxycarbonylamino group, an aliphatic sulfinyl group, an aromatic sulfinyl group, an aliphatic thio group, an aromatic thio group, a hydroxy group, a cyano group, a sulfo group, a carboxy group, an aliphatic oxyamino group, an aromatic oxyamino group, a carbamoylamino group, a sulfamoylamino group, a halogen atom, a sulfamoylcarbamoyl group, a carbamoylsulfamoyl group, a dialiphatic oxyphosphinyl group, and a diaromatic oxyphosphinyl group.

[0016] The aliphatic group may be saturated or unsaturated, and may have a hydroxy group, an aliphatic oxy group, a carbamoyl group, an aliphatic oxycarbonyl group, an aliphatic thio group, an amino group, an aliphatic amino group, an acylamino group, a carbamoylamino group, etc. Examples of the aliphatic group include alkyl groups having a total of 1 to 8 carbon atoms, preferably 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a vinyl group, a cyclohexyl group, and a carbamoylmethyl group.

[0017] The aromatic group may have, for example, a nitro group, a halogen atom, an aliphatic oxy group, a carbamoyl group, an aliphatic oxycarbonyl group, an aliphatic thio group, an amino group, an aliphatic amino group, an acylamino group, a carbamoylamino group, etc. Examples of the aromatic group include aryl groups having 6 to 12 carbon atoms, preferably 6 to 10 carbon atoms in total, such as a phenyl group, a 4-nitrophenyl group, a 4-acetylaminophenyl group, and a 4-methanesulfonylphenyl group.

[0018] The heterocyclic group may have a halogen atom, a hydroxy group, an aliphatic oxy group, a carbamoyl group, an aliphatic oxycarbonyl group, an aliphatic thio group, an amino group, an aliphatic amino group, an acylamino group, a carbamoylamino group, etc. Examples of the heterocyclic group include a 5- or 6-membered heterocycle having a total of 2 to 12, preferably 2 to 10, carbon atoms, such as a 2-tetrahydrofuryl group and a 2-pyrimidyl group.

[0019] The acyl group may have an aliphatic carbonyl group, an arylcarbonyl group, a heterocyclic carbonyl group, a hydroxy group, a halogen atom, an aromatic group, an aliphatic oxy group, a carbamoyl group, an aliphatic oxycarbonyl group, an aliphatic thio group, an amino group, an aliphatic amino group, an acylamino group, a carbamoylamino group, etc. Examples of the acyl group include acyl groups having a total of 2 to 8 carbon atoms, preferably 2 to 4 carbon atoms, such as an acetyl group, a propanoyl group, a benzoyl group, and a 3-pyridinecarbonyl group.

[0020] The acylamino group may have an aliphatic group, an aromatic group, a heterocyclic group, etc., such as an acetylamino group, a benzoylamino group, a 2-pyridinecarbonylamino group, a propanoylamino group, etc. Examples of the acylamino group include an acylamino group having a total of 2 to 12 carbon atoms, preferably 2 to 8 carbon atoms, and an alkylcarbonylamino group having a total of 2 to 8 carbon atoms, such as an acetylamino group, a benzoylamino group, a 2-pyridinecarbonylamino group, a propanoylamino group, etc.

[0021] The aliphatic oxycarbonyl group may be saturated or unsaturated, and may have a hydroxy group, an aliphatic oxy group, a carbamoyl group, an aliphatic oxycarbonyl group, an aliphatic thio group, an amino group, an aliphatic amino group, an acylamino group, a carbamoylamino group, etc. Examples of the aliphatic oxycarbonyl group include alkoxycarbonyl groups having a total of 2 to 8 carbon atoms, preferably 2 to 4 carbon atoms, such as a methoxycarbonyl group, an ethoxycarbonyl group, and a (t)-butoxycarbonyl group.

[0022] The carbamoyl group may have an aliphatic group, an aromatic group, a heterocyclic group, etc. Examples of the carbamoyl group include an unsubstituted carbamoyl group, an alkylcarbamoyl group having a total of 2 to 9 carbon atoms, preferably an unsubstituted carbamoyl group, an alkylcarbamoyl group having a total of 2 to 5 carbon atoms, such as an N-methylcarbamoyl group, an N,N-dimethylcarbamoyl group, and an N-phenylcarbamoyl group.

[0023] The aliphatic sulfonyl group may be saturated or unsaturated, and may have a hydroxy group, an aromatic group, an aliphatic oxy group, a carbamoyl group, an aliphatic oxycarbonyl group, an aliphatic thio group, an amino group, an aliphatic amino group, an acylamino group, a carbamoylamino group, etc. Examples of the aliphatic sulfonyl group include alkylsulfonyl groups having a total of 1 to 6 carbon atoms, preferably a total of 1 to 4 carbon atoms, such as a methanesulfonyl group.

[0024] The aromatic sulfonyl group may have a hydroxy group, an aliphatic group, an aliphatic oxy group, a carbamoyl group, an aliphatic oxycarbonyl group, an aliphatic thio group, an amino group, an aliphatic amino group, an acylamino group, a carbamoylamino group, etc. Examples of the aromatic sulfonyl group include arylsulfonyl groups having a total of 6 to 10 carbon atoms, such as a benzenesulfonyl group.

[0025] The amino group may have an aliphatic group, an aromatic group, a heterocyclic group, or the like.

[0026] The acylamino group may have, for example, an acetylamino group, a benzoylamino group, a 2-pyridinecarbonylamino group, a propanoylamino group, etc. Examples of the acylamino group include an acylamino group having a total of 2 to 12 carbon atoms, preferably a total of 2 to 8 carbon atoms, and more preferably an alkylcarbonylamino group having a total of 2 to 8 carbon atoms, such as an acetylamino group, a benzoylamino group, a 2-pyridinecarbonylamino group, a propanoylamino group, etc.

[0027] The aliphatic sulfonamide group, aromatic sulfonamide group, and heterocyclic sulfonamide group may be, for example, a methanesulfonamide group, a benzenesulfonamide group, or a 2-pyridinesulfonamide group.

[0028] The sulfamoyl group may have an aliphatic group, an aromatic group, a heterocyclic group, etc. Examples of the sulfamoyl group include a sulfamoyl group, an alkylsulfamoyl group having a total of 1 to 9 carbon atoms, a dialkylsulfamoyl group having a total of 2 to 10 carbon atoms, an arylsulfamoyl group having a total of 7 to 13 carbon atoms, and a heterocyclic sulfamoyl group having a total of 2 to 12 carbon atoms, more preferably a sulfamoyl group, an alkylsulfamoyl group having a total of 1 to 7 carbon atoms, a dialkylsulfamoyl group having a total of 3 to 6 carbon atoms, an arylsulfamoyl group having a total of 6 to 11 carbon atoms, and a heterocyclic sulfamoyl group having a total of 2 to 10 carbon atoms, such as a sulfamoyl group, a methylsulfamoyl group, an N,N-dimethylsulfamoyl group, a phenylsulfamoyl group, and a 4-pyridine sulfamoyl group.

[0029] The aliphatic oxy group may be saturated or unsaturated and may have a methoxy group, an ethoxy group, an i-propyloxy group, a cyclohexyloxy group, a methoxyethoxy group, etc. Examples of the aliphatic oxy group include alkoxy groups having a total of 1 to 8 carbon atoms, preferably 1 to 6 carbon atoms, such as a methoxy group, an ethoxy group, an i-propyloxy group, a cyclohexyloxy group, a methoxyethoxy group, etc.

[0030] The aromatic amino group and heterocyclic amino group may have an aliphatic group, an aliphatic oxy group, a halogen atom, a carbamoyl group, a heterocyclic group condensed with the aryl group, or an aliphatic oxycarbonyl group, preferably an aliphatic group having 1 to 4 carbon atoms in total, an aliphatic oxy group having 1 to 4 carbon atoms in total, a halogen atom, a carbamoyl group having 1 to 4 carbon atoms in total, a nitro group, or an aliphatic oxycarbonyl group having 2 to 4 carbon atoms in total.

[0031] The aliphatic thio group may be saturated or unsaturated and is an alkylthio group having a total of 1 to 8 carbon atoms, more preferably 1 to 6 carbon atoms, such as a methylthio group, an ethylthio group, a carbamoylmethylthio group, or a t-butylthio group.

[0032] The carbamoylamino group may have an aliphatic group, an aryl group, a heterocyclic group, etc. Examples of the carbamoylamino group include a carbamoylamino group, an alkylcarbamoylamino group having a total of 2 to 9 carbon atoms, a dialkylcarbamoylamino group having a total of 3 to 10 carbon atoms, an arylcarbamoylamino group having a total of 7 to 13 carbon atoms, and a heterocyclic carbamoylamino group having a total of 3 to 12 carbon atoms, preferably a carbamoylamino group, an alkylcarbamoylamino group having a total of 2 to 7 carbon atoms, a dialkylcarbamoylamino group having a total of 3 to 6 carbon atoms, an arylcarbamoylamino group having a total of 7 to 11 carbon atoms, and a heterocyclic carbamoylamino group having a total of 3 to 10 carbon atoms, such as a carbamoylamino group, a methylcarbamoylamino group, an N,N-dimethylcarbamoylamino group, a phenylcarbamoylamino group, and a 4-pyridinecarbamoylamino group.

[0033] In this disclosure, ranges expressed by endpoints include all numbers subsumed within that range (eg, 1 to 10 includes 1.4, 1.9, 2.33, 5.75, 9.98, etc.).

[0034] In this disclosure, the term "at least 1" includes all numbers greater than or equal to 1 (e.g., at least 2, at least 4, at least 6, at least 8, at least 10, at least 25, at least 50, at least 100, etc.).

[0035] Specific embodiments of the present disclosure will be described in detail below, but the present disclosure is not limited to the following embodiments.

[0036] The polymer (I) used in the production method of the present disclosure contains polymerization units (I) based on the monomer (I) represented by general formula (I). CX 1 X 3 =CX 2 R(-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF; X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more.

[0037] The presence of polymer (I) during polymerization allows the polymerization of tetrafluoroethylene (TFE) to proceed smoothly, resulting in a polymerization dispersion containing polytetrafluoroethylene. However, there is a problem that polymer (I) remains in the resulting polymerization dispersion and in the polytetrafluoroethylene recovered from the polymerization dispersion by the conventional method. For example, Patent Document 1 describes a method in which the polymerization dispersion is stirred at high speed to coagulate the fluororesin in the polymerization dispersion, and the coagulated wet powder is dried, but this method results in a relatively large amount of polymer (I) remaining in the resulting polytetrafluoroethylene.

[0038] The applicant has already found a means for solving this problem, and has proposed, in an application already submitted, a production method for obtaining a composition containing a fluororesin (fluororesin composition).

[0039] In the above-mentioned production method already proposed, tetrafluoroethylene (TFE) is polymerized in an aqueous medium in the presence of polymer (I) to obtain a polymerization dispersion containing a fluororesin containing TFE units, the fluororesin in the obtained polymerization dispersion is coagulated to obtain a coagulate, and the obtained coagulate is washed to obtain a composition containing a fluororesin (fluororesin composition), and the coagulation and washing are carried out by either one or both of the following methods (1) and (2): (1) Coagulation is carried out by contacting the fluororesin in the polymer dispersion with an organic solvent. (2) Washing is carried out by contacting the coagulate with an organic solvent.

[0040] In the above-mentioned production method, at least one of washing and coagulation is carried out using an organic solvent, so that the polymer (I) remaining in the fluororesin obtained by polymerization can be removed from the fluororesin with high efficiency. As a result, a fluororesin composition with a reduced content of polymer (I) can be obtained, even though the fluororesin composition is obtained using polymer (I).

[0041] On the other hand, when polytetrafluoroethylene (PTFE) in the polymer dispersion is coagulated by the above-mentioned production method, there is a problem that a part of the PTFE in the polymer dispersion does not coagulate and remains in the polymer dispersion.

[0042] The first production method of the present disclosure is proposed as a production method for solving this problem, and although the composition containing PTFE is obtained by using polymer (I), a composition having a reduced content of polymer (I) can be obtained, and further, the composition containing PTFE can be produced in a high yield.

[0043] That is, the first production method of the present disclosure is a production method for a composition containing PTFE, which comprises polymerizing TFE in an aqueous medium in the presence of a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I) to obtain a polymerization dispersion containing PTFE, and coagulating the PTFE in the polymerization dispersion by contacting the PTFE in the polymerization dispersion with an organic solvent and a coagulant to obtain a composition containing PTFE.

[0044] Thus, in the first manufacturing method of the present disclosure, when PTFE is coagulated, the PTFE in the polymerization dispersion is contacted with an organic solvent and a coagulant.By using an organic solvent and a coagulant in combination, the PTFE in the polymerization dispersion can be coagulated surprisingly smoothly, and after recovering the coagulant from the polymerization dispersion, a dispersion (wastewater) with almost no PTFE remaining can be obtained.

[0045] The reason why the first manufacturing method of the present disclosure has the above-mentioned effect is presumed to be as follows. The polymerization dispersion contains PTFE and polymer (I). In the polymerization dispersion, the PTFE particles are stably dispersed in the aqueous medium due to the electrostatic repulsion between the PTFE particles and the stabilizing effect of the polymer (I) on the PTFE particles. When the organic solvent and the coagulant come into contact with the PTFE in the polymerization dispersion, the electrostatic repulsion between the PTFE particles is reduced mainly by the action of the coagulant, and at the same time, the polymer (I) is transferred into the organic solvent by the action of the organic solvent and separated from the PTFE particles. It is presumed that the PTFE particles are coagulated with high efficiency due to the synergistic action of the organic solvent and the coagulant.

[0046] There is also a demand for a technique capable of removing the polymer (I) remaining in the fluororesin obtained by polymerization from the fluororesin with even higher efficiency.

[0047] The second production method of the present disclosure is proposed as a production method to meet such demands, and although it is a PTFE-containing composition obtained by using polymer (I), it is possible to obtain a composition with a reduced content of polymer (I).

[0048] That is, the second manufacturing method of the present disclosure is a manufacturing method for a composition containing PTFE, which comprises polymerizing TFE in an aqueous medium in the presence of a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I) to obtain a polymerization dispersion containing PTFE, contacting the PTFE in the polymerization dispersion with an organic solvent to coagulate the PTFE in the polymerization dispersion to obtain a coagulate, and then washing the coagulate at 20°C or higher to obtain a composition containing PTFE.

[0049] Thus, in the second manufacturing method of the present disclosure, the PTFE in the polymer dispersion is brought into contact with an organic solvent to coagulate the PTFE, and the obtained coagulated material is washed at a relatively high temperature. By carrying out the coagulation using an organic solvent and washing the coagulated material at a relatively high temperature, a composition with a reduced content of polymer (I) can be obtained.

[0050] Next, the organic solvent and the coagulant used in the production method of the present disclosure will be described in more detail.

[0051] (Organic solvent) The organic solvent used in the first and second manufacturing methods of the present disclosure is preferably an organic solvent (excluding nitrogen-containing compounds). The nitrogen-containing compound may be urea. The organic solvent used in the manufacturing method of the present disclosure may be an organic solvent (excluding coagulants).

[0052] In the first manufacturing method of the present disclosure, as described above, the organic solvent and the coagulant act synergistically to coagulate PTFE particles with high efficiency. It is assumed that the organic solvent mainly functions to reduce the dispersion stabilization effect of the polymer (I) on the PTFE particles. Therefore, it is preferable that the organic solvent has a higher solubility in water than that of the polymer (I).

[0053] As the organic solvent, an organic solvent that does not ionize at least in an acidic aqueous solution is preferable, and a non-electrolyte is more preferable.

[0054] Examples of organic solvents include: alcohol; Carboxylic acids such as acetic acid, propionic acid, ethoxyacetic acid, and valeric acid; Esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, and dimethyl carbonate; Ketones such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, diacetone alcohol, 3-methyl-2-cyclopentenone; Aromatic hydrocarbons such as benzene, toluene, and xylene; Ethers such as diethyl ether, tetrahydrofuran, dioxane, diethylene glycol diethyl ether, 1,2-dimethoxyethane; etc.

[0055] As the organic solvent, alcohol is preferable. The alcohol may be any of monohydric alcohol, dihydric alcohol and trihydric alcohol. As the alcohol, monohydric alcohol is preferable because the efficiency of removing the polymer (I) is further improved.

[0056] Alcohol, for example, one-carbon alcohols, such as methanol; Alcohols with two carbon atoms, such as ethanol and ethylene glycol; Alcohols with 3 carbon atoms, such as 1-propanol, 2-propanol, propylene glycol, and glycerin Alcohols with four carbon atoms, such as 1-butanol, 2-butanol, 2-methyl-1-propanol, and 2-methyl-2-propanol; Alcohols with 5 carbon atoms, such as 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, and 2-methyl-2-butanol; Alcohols with 6 carbon atoms, such as 1-hexanol, 2-hexanol, 3-hexanol, 2-methyl-1-pentanol, 3-methyl-1-pentanol, 4-methyl-1-pentanol, 2-methyl-2-pentanol, 3-methyl-2-pentanol, 4-methyl-2-pentanol, 2-methyl-3-pentanol, 3-methyl-3-pentanol, 2,2-dimethyl-1-butanol, 2,3-dimethyl-1-butanol, 3,3-dimethyl-1-butanol, 2,3-dimethyl-2-butanol, 3,3-dimethyl-2-butanol, and 2-ethyl-1-butanol; Alcohols with seven carbon atoms, such as 1-heptanol, 2-heptanol, and 2-methyl-1-hexanol; Fluorinated alcohols such as 5-fluoropropanol, 1H,1H,5H-octafluoropentanol; etc.

[0057] The alcohol is preferably one having a MolLogP in the range of 0.3 to 1.6, since this further improves the efficiency of removing the polymer (I).The MolLogP is more preferably 1.2 or less.

[0058] Examples of alcohols having a MolLogP within the range of 0.3 to 1.6 include 2-methyl-1-propanol, 2-butanol, and 1-pentanol.

[0059] MolLogP is the octanol / water partition coefficient of a compound calculated using the open source library RDKit.

[0060] The number of carbon atoms in the alcohol is preferably 1 to 7, more preferably 2 or more, further preferably 3 or more, and more preferably 5 or less, since the efficiency of removing the polymer (I) is further improved.

[0061] As the organic solvent, at least one selected from the group consisting of 1-propanol, 2-propanol, 2-butanol and 2-pentanol is preferred, since the efficiency of removing the polymer (I) is further improved and the PTFE in the polymerization dispersion can be coagulated more smoothly, and at least one selected from the group consisting of 2-propanol, 2-butanol and 2-pentanol is more preferred.

[0062] (Coagulant) The coagulant used in the first production method of the present disclosure is preferably a coagulant (excluding alcohol). In the second production method, a coagulant can be used in the same manner as in the first production method.

[0063] In the first manufacturing method of the present disclosure, as described above, the PTFE particles are coagulated with high efficiency by the action of the organic solvent and the coagulant. It is assumed that the coagulant mainly has the function of reducing the electrostatic repulsion between the PTFE particles. Therefore, the coagulant is preferably an electrolyte, and is preferably an electrolyte that has high solubility in water and high ionization degree under acidic conditions. In addition, the coagulant is preferably an electrolyte that ionizes at least in an acidic aqueous solution.

[0064] The coagulant is preferably a strong acid, a weak alkali, or one exhibiting strong alkalinity, and more preferably a strong acid or a weak alkalinity.

[0065] The coagulant is preferably one that is easily decomposed and removed in the drying process.

[0066] The coagulant is: Inorganic salts such as potassium nitrate, ammonium carbonate, and ammonium bicarbonate; Inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, etc.; Nitrogen-containing compounds such as ammonia and urea; etc.

[0067] As the coagulant, at least one selected from the group consisting of ammonium carbonate, ammonium hydrogen carbonate, ammonia and urea is preferred, since this allows the PTFE in the polymerization dispersion to be coagulated more smoothly, and at least one selected from the group consisting of ammonium carbonate and ammonium hydrogen carbonate is more preferred.

[0068] In one embodiment of the present disclosure, the above-mentioned alcohol can be used as the organic solvent, and at least one selected from the group consisting of ammonium carbonate, ammonium bicarbonate, ammonia, and urea can be used as the coagulant.

[0069] Next, the coagulation method used in the production method of the present disclosure will be described in more detail.

[0070] (Coagulation method) In the first production method of the present disclosure, when coagulating PTFE in the polymer dispersion, PTFE, an organic solvent, and a coagulant are brought into contact with each other.

[0071] In the first manufacturing method, the method of contacting PTFE, the organic solvent, and the coagulant is not particularly limited, and examples thereof include a method of adding the polymerization dispersion and the coagulant to the organic solvent, and a method of adding the organic solvent and the coagulant to the polymerization dispersion. The mixture containing the polymerization dispersion, the organic solvent, and the coagulant may be stirred to sufficiently contact PTFE, the organic solvent, and the coagulant, and coagulate the PTFE in the polymerization dispersion. The coagulation of PTFE may be performed in a batch manner or a continuous manner. The timing of adding the organic solvent and the coagulant to the polymerization dispersion may be before coagulation or during coagulation.

[0072] In the second manufacturing method of the present disclosure, when coagulating PTFE in the polymerization dispersion, PTFE is brought into contact with an organic solvent. In the second manufacturing method, a coagulant can be used in addition to an organic solvent during coagulation. In one embodiment of the second manufacturing method, coagulation is performed without using a coagulant.

[0073] In the second manufacturing method, the method of contacting PTFE with an organic solvent is not particularly limited, and examples thereof include a method of adding a polymerization dispersion to an organic solvent, and a method of adding an organic solvent to a polymerization dispersion. The mixture containing the polymerization dispersion and the organic solvent may be stirred to sufficiently contact PTFE with the organic solvent, thereby coagulating the PTFE in the polymerization dispersion. The coagulation of PTFE may be performed in a batch manner or a continuous manner.

[0074] Before coagulation, the PTFE content in the polymerization dispersion obtained by polymerization may be adjusted using water. The PTFE content in the polymerization dispersion used for coagulation may be 5 to 40% by mass, or 5 to 20% by mass, based on the polymerization dispersion.

[0075] The PTFE content in the polymer dispersion is a value obtained by drying 1 g of the polymer dispersion in a blower dryer at 150°C for 60 minutes, measuring the mass of the heating residue, and calculating the ratio of the mass of the heating residue to the mass (1 g) of the polymer dispersion as a percentage.

[0076] In the first and second manufacturing methods, the amount of organic solvent used for coagulation is preferably 1.0% by mass or more relative to the weight (dry weight) of PTFE in the polymerization dispersion, since the removal efficiency of the polymer (I) is further improved and the PTFE in the polymerization dispersion can be coagulated more smoothly. The amount of organic solvent used for coagulation is more preferably 5.0% by mass or more, more preferably 10% by mass or more, and particularly preferably 20% by mass or more. The upper limit of the amount of organic solvent used for coagulation is not particularly limited. For example, the organic solvent can be used in an amount of 50 times or less, more preferably 10 times or less, even more preferably 5 times or less, and particularly preferably 3 times or less, relative to the weight of PTFE in the polymerization dispersion.

[0077] In addition, in the first manufacturing method of the present disclosure, since a coagulant is used in addition to the organic solvent during coagulation, it is also possible to reduce the amount of organic solvent used. By reducing the amount of organic solvent used, the amount of organic solvent remaining in the coagulation product can be reduced. The amount of organic solvent used for coagulation is preferably 150% by mass or less, more preferably 100% by mass or less, and even more preferably 50% by mass or less, based on the weight (dry weight) of PTFE in the polymerization dispersion.

[0078] In addition, in the second manufacturing method of the present disclosure, from the viewpoint of reducing the weight of PTFE remaining in the polymerization dispersion without coagulation, the amount of the organic solvent used for coagulation is preferably 50 mass% or more, more preferably 80 mass% or more, and even more preferably 100 mass% or more, based on the weight of PTFE in the polymerization dispersion.

[0079] In the first production method, the amount of the coagulant used for coagulation is preferably 0.01 mass% or more, more preferably 0.10 mass% or more, even more preferably 0.30 mass% or more, and preferably 5.0 mass% or less, more preferably 3.0 mass% or less, and even more preferably 1.0 mass% or less, based on the weight (dry weight) of PTFE in the polymerization dispersion, so that the PTFE in the polymerization dispersion can be coagulated more smoothly.

[0080] In the first production method, the temperature at which the PTFE in the polymerization dispersion is contacted with the organic solvent and the coagulant for coagulation is preferably 5 to 80°C, more preferably 10°C or higher, even more preferably 15°C or higher, more preferably 70°C or lower, and even more preferably 60°C or lower, since this further improves the efficiency of removing the polymer (I) and further allows the PTFE in the polymerization dispersion to be coagulated more smoothly.

[0081] In the second production method, the temperature when the PTFE in the polymerization dispersion is contacted with the organic solvent for coagulation is preferably 5 to 80°C, more preferably 10°C or more, even more preferably 15°C or more, even more preferably 20°C or more, particularly preferably 25°C or more, more preferably 70°C or less, and even more preferably 60°C or less, since the removal efficiency of the polymer (I) is further improved and the PTFE in the polymerization dispersion can be coagulated more smoothly.

[0082] In the first and second manufacturing methods, the pH of the polymerization dispersion obtained by polymerization may be adjusted before coagulation. For coagulation, the pH of the polymerization dispersion when the PTFE in the polymerization dispersion is contacted with the organic solvent and the coagulant is preferably within the range of 3 to 12, more preferably 4 or more, even more preferably 6 or more, still more preferably 8 or more, more preferably 11 or less, and even more preferably 10 or less, since the removal efficiency of the polymer (I) is further improved and the PTFE in the polymerization dispersion can be coagulated more smoothly.

[0083] The pH can be adjusted by adding an acid or alkali to the polymer dispersion. For example, if the pH of the polymer dispersion is too low, an alkali such as ammonia can be added to the polymer dispersion to adjust the pH of the polymer dispersion to within the above range.

[0084] In the first manufacturing method, after the PTFE in the polymerization dispersion is coagulated, the composition containing PTFE can be collected as the coagulated product.The polymer (I) is removed from the coagulated product obtained by contacting the PTFE in the polymerization dispersion with the organic solvent and the coagulating agent, but it is preferable to further wash the obtained coagulated product, since this further improves the efficiency of removing the polymer (I).

[0085] In the first manufacturing method, the coagulated material (PTFE) obtained by contacting the PTFE in the polymer dispersion with the organic solvent and the coagulant can be washed using an organic solvent or water. As a method for washing the coagulated material, a method of washing the coagulated material with at least water is preferable. As a method for washing the coagulated material, a method of washing the coagulated material with only water, and a method of washing the coagulated material with an organic solvent and then washing the coagulated material with water can be mentioned.

[0086] In the second manufacturing method, the PTFE in the polymerization dispersion is coagulated to obtain a coagulated product, and then the coagulated product is washed at 20° C. or higher. By washing the coagulated product at a relatively high temperature, the efficiency of removing the polymer (I) is improved. In the first manufacturing method, the coagulated product may be washed at a relatively high temperature, as in the second manufacturing method.

[0087] The temperature during washing in the second production method may be 25°C or more, 30°C or more, 35°C or more, or 40°C or more, and may be less than 100°C, 90°C or less, 80°C or less, 70°C or less, 60°C or less, or 50°C or less.

[0088] In the second manufacturing method, the coagulated material (PTFE) can be washed using an organic solvent or water. As a method for washing the coagulated material, a method of washing the coagulated material with at least water is preferable. As a method for washing the coagulated material, a method of washing the coagulated material with water only, and a method of washing the coagulated material with an organic solvent and then washing the coagulated material with water can be mentioned.

[0089] In one embodiment of the second production method, the organic solvent or water used for washing is adjusted to 20° C. or higher. The temperature of the organic solvent or water used for washing may be 25° C. or higher, 30° C. or higher, 35° C. or higher, or 40° C. or higher, and may be less than 100° C., 90° C. or lower, 80° C. or lower, 70° C. or lower, 60° C. or lower, or 50° C. or lower.

[0090] The washing of the coagulated material (PTFE) with an organic solvent or water is carried out by a conventionally known method. The washing with an organic solvent or water may be carried out once or twice or more. The washing of the coagulated material (PTFE) may be carried out in a batch manner or in a continuous manner. The time required for washing may be 1 minute or more, 3 minutes or more, or 30 minutes or less.

[0091] After the PTFE has been washed, it may be dried, details of which are described below.

[0092] Next, the method for preparing the polymer dispersion to be subjected to coagulation will be described in more detail.

[0093] (Preparation of Polymer Dispersion) The polymerization dispersion used in the manufacturing method of the present disclosure is produced by polymerizing TFE in an aqueous medium in the presence of polymer (I).By polymerizing a fluoromonomer containing at least TFE in an aqueous medium in the presence of polymer (I), so-called emulsion polymerization reaction proceeds, and usually, a polymerization dispersion in which PTFE particles are dispersed in an aqueous medium is obtained.Then, the PTFE particles are coagulated, and the PTFE in the polymerization dispersion can be recovered.

[0094] (Polymer (I)) The polymer (I) used in the production method of the present disclosure contains polymerization units (I) based on the monomer (I) represented by general formula (I). CX 1 X 3 =CX 2 R(-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF; X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more.

[0095] In the present disclosure, the anionic group includes functional groups that provide an anionic group, such as a sulfate group, a carboxylate group, an acid group such as -COOH, an acid salt group such as -COONH4, etc. The anionic group includes a sulfate group, a carboxylate group, a phosphate group, a phosphonate group, a sulfonate group, or a -C(CF3)2OM (wherein M is -H, a metal atom, -NR 7 4. An optionally substituted imidazolium, an optionally substituted pyridinium, or an optionally substituted phosphonium, wherein R 7 is H or an organic group.

[0096] In the production method of the present disclosure, one or more types of monomers can be used as the monomer (I) represented by general formula (I).

[0097] R is a linking group. In the present disclosure, the "linking group" is a (m+1)-valent linking group, and when m is 1, it is a divalent linking group. The linking group may be a single bond, and preferably contains at least one carbon atom, and the number of carbon atoms may be 2 or more, 4 or more, 8 or more, 10 or more, or 20 or more. There is no upper limit, but it may be, for example, 100 or less, or 50 or less.

[0098] The linking group may be linear or branched, cyclic or acyclic in structure, saturated or unsaturated, substituted or unsubstituted, and may optionally contain one or more heteroatoms selected from the group consisting of sulfur, oxygen, and nitrogen, and may optionally contain one or more functional groups selected from the group consisting of esters, amides, sulfonamides, carbonyls, carbonates, urethanes, ureas, and carbamates. The linking group may not contain carbon atoms, but may be a catenary heteroatom such as oxygen, sulfur, or nitrogen.

[0099] m is an integer of 1 or more, preferably 1 or 2, and more preferably 1. When m is an integer of 2 or more, Z 1 , Z 2 and A 0 may be the same or different. Next, a preferred structure when m is 1 in general formula (I) will be described.

[0100] R is preferably a catenary heteroatom such as oxygen, sulfur, or nitrogen, or a divalent organic group.

[0101] When R is a divalent organic group, the hydrogen atom bonded to the carbon atom may be replaced with a halogen other than fluorine, such as chlorine, and may or may not contain a double bond. R may be either linear or branched, and may be either cyclic or acyclic. R may also contain a functional group (e.g., ester, ether, ketone (keto group), amine, halide, etc.).

[0102] R may also be a non-fluorinated divalent organic group, or a partially fluorinated or perfluorinated divalent organic group.

[0103] R may be, for example, a hydrocarbon group in which no fluorine atoms are bonded to the carbon atom, a hydrocarbon group in which some of the hydrogen atoms bonded to the carbon atom are substituted with fluorine atoms, or a hydrocarbon group in which all of the hydrogen atoms bonded to the carbon atom are substituted with fluorine atoms, and these may contain an oxygen atom, a double bond, or a functional group.

[0104] R is preferably a hydrocarbon group having 1 to 100 carbon atoms which may contain an ether bond or a keto group, and in the hydrocarbon group, some or all of the hydrogen atoms bonded to the carbon atoms may be substituted with fluorine.

[0105] R is preferably -(CH2) a -, -(CF2) a -, -(CF2) a -O-, -O-(CF2) a -, -(CF2) a -O-(CF2) b -, -O(CF2) a -O-(CF2) b -, -(CF2) a -[O-(CF2) b ] c -, -O(CF2) a -[O-(CF2) b ] c -,-[(CF2) a -O] b -[(CF2) c -O] d -, -O[(CF2) a -O] b -, -O[(CF2) a -O] b -[(CF2) c -O] d -, -O-[CF2CF(CF3)O] a -(CF2) b -, -O-(CF2) a -O-[CF(CF3)CF2O]b -, -O-[CF2CF(CF3)O] a -(CF2) b -O-, -O-[CF2CF(CF3)O] a -(CF2) b -O-[CF(CF3)CF2O] c -, -[CF2CF(CF3)O] a -, -[CF(CF3)CF2O] a -, -(CF2) a -O-[CF(CF3)CF2O] a -, -(CF2) a -O-[CF(CF3)CF2O] a -(CF2) b -, -[CF2CF(CF3)] a -CO-(CF2) b - and at least one selected from combinations thereof. In the formula, a, b, c, and d are independently at least 1. a, b, c, and d may be independently 2 or more, 3 or more, 4 or more, 10 or more, or 20 or more. The upper limit of a, b, c, and d is, for example, 100.

[0106] R is more preferably at least one selected from -O-CF2-, -O-CF2CF2-, -O-CF2CF2-O-, -O-CF2CF2CF2-, -O-CF2CF2CF2-O-, -O-CF2CF(CF3)-O-, -O-CF2CF2-O-CF(CF3)CF2-O-, -O-CF2CF(CF3)-O-CF2CF2-O-, and -O-CF2CF(CF3)-O-CF2-.

[0107] R is represented by the general formula (r1): -CF2-O-(CX 6 2) e -{O-CF(CF3)} f -(O) g - (r1) (In the formula, X 6are each independently H, F or CF3, e is an integer of 0 to 3, f is an integer of 0 to 3, and g is 0 or 1), and a divalent group represented by the general formula (r2): -CF2-O-(CX 7 2) e -(O) g - (r2) (In the formula, X 7 are each independently H, F or CF3, e is an integer of 0 to 3, and g is 0 or 1), and a divalent group represented by the following formula is more preferable.

[0108] Specific examples suitable for R include -CF2-O-, -CF2-O-CF2-, -CF2-O-CH2-, -CF2-O-CH2CF2-, -O-CF2-, -O-CF2CF 2-, -O-CF2CF2CF2-, -O-CF2CF2CF2CF2-, -O-CF2CF(CF3)-O-CF2-, -O-CF2CF(CF3)-O-CF2CF2- , -CF2-O-CF2CF2-, -CF2-O-CF2CH2-, -CF2-O-CF2CF2CH2-, -CF2-O-CF(CF3)-, -CF2-O-CF(CF3 )CF2-, -CF2-O-CF(CF3)CF2-O-, -CF2-O-CF(CF3)CF2-O-CF2-, -CF2-O-CF(CF3)CH2-, and the like. Among these, R is preferably a perfluoroalkylene group which may contain an oxygen atom, specifically, -CF2-O-, -CF2-O-CF2-, -O-CF2-, -O-CF2CF2-, -O-CF2CF(CF3)-O-CF2-, -O-CF2CF(CF3)-O-CF2CF2-, -CF2-O-CF2CF2-, -CF2-O-CF(CF3)-, -CF2-O-CF(CF3)CF2-, or -CF2-O-CF(CF3)CF2-O- is preferred.

[0109] -R-CZ of general formula (I) 1 Z 2 - is represented by the general formula (s1): -CF2-O-(CX 6 2) e -{O-CF(CF3)} f -(O) g -CZ1 Z 2 - (s1) (In the formula, X 6 are each independently H, F or CF3, e is an integer of 0 to 3, f is an integer of 0 to 3, g is 0 or 1, and Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group), and in formula (s1), Z 1 and Z 2 More preferably, each is F or CF3, and even more preferably, one is F and the other is CF3.

[0110] In addition, in the general formula (I), -R-CZ 1 Z 2 - is represented by the general formula (s2): -CF2-O-(CX 7 2) e -(O) g -CZ 1 Z 2 - (s2) (In the formula, X 7 are each independently H, F or CF3, e is an integer of 0 to 3, g is 0 or 1, and Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group), and in formula (s2), Z 1 and Z 2 More preferably, each is F or CF3, and even more preferably, one is F and the other is CF3.

[0111] -R-CZ of general formula (I) 1 Z 2- as -CF2-O-CF2-, -O-CF2CF2-, -O-CF2CF2CF2-, -O-CF2CF2CF2CF2-, -O-CF2CF(CF3)-O-CF2-, -O-CF2CF(CF3)-O-CF 2CF2-, -O-CF2CF(CF3)-O-CF2CF2CF2-, -CF2-O-CF(CF3)-, -CF2-OC(CF3)2-, -CF2-O-CF2-CF2-, -CF2-O-CF2-CF(CF3)-, -CF2-O-CF2-C(CF3)2-, -CF2-O-CF2CF2-CF2-, -CF2-O-CF2CF2-CF(CF3)-, -CF2-O-CF2CF2-C(CF3)2-, -CF2-O-CF(CF3)- CF2-, -CF2-O-CF(CF3)-CF(CF3)-, -CF2-O-CF(CF3)-C(CF3)2-, -CF2-O-CF(CF3)CF2-CF2-, -CF2-O-CF(CF3)CF2-CF(CF3 )-, -CF2-O-CF(CF3)CF2-C(CF3)2-, -CF2-O-CF(CF3)CF2-O-CF2-, -CF2-O-CF(CF3)CF2-O-CF(CF3)-, or -CF2-O-CF(CF 3) CF2-OC(CF3)2- is preferred, -O-CF2CF2-, -O-CF2CF2CF2-, -O-CF2CF2CF2CF2-, -O-CF2CF(CF3)-O-CF2-, -O-CF2CF(CF3)-O- CF2CF2-, -CF2-O-CF(CF3)-, -CF2-O-CF2-CF(CF3)-, -CF2-O-CF2CF2-CF(CF3)-, -CF2-O-CF(CF3)-CF(CF3)-, -CF2-O-CF(CF3)CF2-CF(CF3)- or -CF2-O-CF(CF3)CF2-O-CF(CF3)- are more preferred, with -O-CF2CF2- and -O-CF2CF(CF3)-O-CF2CF2- being even more preferred.

[0112] It is also preferred that the polymer (I) is highly fluorinated. For example, the polymer (I) may contain anionic groups (A) such as phosphate moieties (e.g., CH2OP(O)(OM)2) and sulfate moieties (e.g., CH2OS(O)2OM). 0), it is preferred that 80% or more, 90% or more, 95% or more, or 100% of the C-H bonds in the polymer (I) are substituted with C-F bonds.

[0113] The monomer (I) and the polymer (I) each have an anionic group (A 0 ), it is also preferable that the compound has a C-F bond and does not have a C-H bond. That is, in the general formula (I), 1 , X 2 , and X 3 are all F, and R is preferably a perfluoroalkylene group having 1 or more carbon atoms, and the perfluoroalkylene group may be either linear or branched, may be either cyclic or noncyclic, and may contain at least one catenary heteroatom. The number of carbon atoms in the perfluoroalkylene group may be 2 to 20, or may be 4 to 18.

[0114] The monomer (I) and the polymer (I) may be partially fluorinated. That is, the monomer (I) and the polymer (I) may have an anionic group (A 0 ), it is also preferred that the alkyl group has at least one hydrogen atom bonded to a carbon atom and at least one fluorine atom bonded to a carbon atom.

[0115] Anionic group (A 0) may be -SO2M, -SO3M, -OSO3M, -COOM, -SO2NR'CH2COOM, -CH2OP(O)(OM)2, [-CH2O]2P(O)(OM), -CH2CH2OP(O)(OM)2, [-CH2CH2O]2P(O)(OM), -CH2CH2OSO3M, -P(O)(OM)2, -SO2NR'CH2CH2OP(O)(OM)2, [-SO2NR'CH2CH2O]2P(O)(OM), -CH2OSO3M, -SO2NR'CH2CH2OSO3M, or -C(CF3)2OM. Among these, -SO3M, -OSO3M, -COOM, -P(O)(OM)2 or -C(CF3)2OM are preferred, -COOM, -SO3M, -OSO3M, -P(O)(OM)2 or -C(CF3)2OM are more preferred, -SO3M, -COOM or -P(O)(OM)2 are even more preferred, and -SO3M or -COOM is particularly preferred.

[0116] M is H, a metal atom, or NR 7 4. An optionally substituted imidazolium, an optionally substituted pyridinium, or an optionally substituted phosphonium, wherein R 7 is H or an organic group.

[0117] The metal atom includes alkali metals (Group 1), alkaline earth metals (Group 2), etc., and is preferably Na, K or Li.

[0118] M is -H, a metal atom, or NR 7 4 is preferred, and -H, an alkali metal (Group 1), an alkaline earth metal (Group 2) or NR 7 4 is more preferred, -H, -Na, -K, -Li or NH4 is even more preferred, -H, -Na, -K or NH4 is even more preferred, -H, -Na or NH4 is especially preferred, and -H or -NH4 is most preferred.

[0119] In the polymer (I), each polymer unit (I) may have a different anionic group or may have the same anionic group.

[0120] The monomer (I) is also preferably a monomer represented by the general formula (Ia). The polymer (I) is also preferably a polymer containing a polymer unit (Ia) based on a monomer represented by the general formula (Ia). CF2=CF-O-Rf 0 -A 0 (Ia) (In the formula, A 0 is an anionic group, and Rf 0 is a perfluorinated divalent linking group which may be linear or branched, cyclic or acyclic in structure, saturated or unsaturated, substituted or unsubstituted, and which optionally contains one or more heteroatoms selected from the group consisting of sulfur, oxygen, and nitrogen.

[0121] The monomer (I) is also preferably a monomer represented by the general formula (Ib). The polymer (I) is also preferably a polymer containing polymerized units (Ib) based on a monomer represented by the general formula (Ib). CH2=CH-O-Rf 0 -A 0 (Ib) (In the formula, A 0 is an anionic group, and Rf 0 is a perfluorinated divalent linking group defined by formula Ia.

[0122] In the general formula (I), A 0 is a sulfate group. 0 is, for example, -CH2OSO3M, -CH2CH2OSO3M, or -SO2NR'CH2CH2OSO3M, where R' is H or an alkyl group having 1 to 4 carbon atoms, and M is the same as above.

[0123] A 0is a sulfate group, examples of the monomer represented by general formula (I) include CF2=CF(OCF2CF2CH2OSO3M), CF2=CF(O(CF2)4CH2OSO3M), CF2=CF(OCF2CF(CF3)CH2OSO3M), CF2=CF(OCF2CF(CF3)OCF2CF2CH2OSO3M), CH2=CH(O(CF2)4CH2OSO3M), CF2=CF(OCF2CF2SO2N(CH3)CH2CH2OSO3M), CH2=CH(OCF2CF2CH2OSO3M), CF2=CF(OCF2CF2CF2CF2SO2N(CH3)CH2CH2OSO3M), CH2=CH(OCF2CF2CF2CH2OSO3M), etc. In the above formula, M is the same as above.

[0124] In the general formula (I), A 0 In one preferred embodiment, A is a sulfonate group. 0 An example is -SO3M, where M is the same as above.

[0125] A 0 When is a sulfonate group, examples of the monomer represented by general formula (I) include CF2=CF(OCF2CF2SO3M), CF2=CF(O(CF2)3SO3M), CF2=CF(O(CF2)4SO3M), CF2=CF(OCF2CF(CF3)SO3M), CF2=CF(OCF2CF(CF3)OCF2CF2SO3M), CH2=CH(OCF2CF2SO3M), CF2=CF(OCF2CF(CF3)OCF2CF2CF2CF2SO3M), CH2=CH(O(CF2)4SO3M), CH2=CH(O(CF2)3SO3M), etc. In the above formula, M is the same as above.

[0126] In the general formula (I), A 0 In one preferred embodiment, A is a carboxylate group. 0 Examples of the alkyl group include COOM and SO2NR'CH2COOM, where R' is H or an alkyl group having 1 to 4 carbon atoms, and M is the same as above. 0is a carboxylate group, examples of the monomer represented by general formula (I) include CF2=CF(OCF2CF2COOM), CF2=CF(O(CF2)3COOM), CF2=CF(O(CF2)4COOM), CF2=CF(O(CF2)5COOM), CF2=CF(OCF2CF(CF3)COOM), CF2=CF(OCF2CF(CF3)O(CF2) n COOM) (n is greater than 1), CH2=CH(OCF2CF2COOM), CH2=CH(O(CF2)4COOM), CH2=CH(O(CF2)3COOM), CF2=CF(OCF2CF2SO2NR'CH2COOM), CF2=CF(O(CF2)4SO2NR'CH2COOM), CF2=CF(OCF2CF(CF3)SO2NR'CH2COOM), CF2=CF(OCF2CF(CF3)OCF2CF2SO2NR'CH2COOM), CH2=CH(OCF2CF2SO2NR'CH2COOM), CF2=CF(OCF2CF(CF3)OCF2CF2CF2CF2SO2NR'CH2COOM), CH2=CH(O(CF2)4SO2NR'CH2COOM), CH2=CH(O(CF2)3SO2NR'CH2COOM). In the above formula, R' is H or an alkyl group having 1 to 4 carbon atoms, and M is the same as above.

[0127] In the general formula (I), A 0 In one preferred embodiment, A is a phosphate group. 0 Examples of such a group include -CH2OP(O)(OM)2, [-CH2O]2P(O)(OM), -CH2CH2OP(O)(OM)2, [-CH2CH2O]2P(O)(OM), [-SO2NR'CH2CH2O]2P(O)(OM) or SO2NR'CH2CH2OP(O)(OM), where R' is an alkyl group having 1 to 4 carbon atoms, and M is the same as above.

[0128] A 0is a phosphate, examples of the monomer represented by general formula (I) include CF2=CF(OCF2CF2CH2OP(O)(OM)2), CF2=CF(O(CF2)4CH2OP(O)(OM)2), CF2=CF(OCF2CF(CF3)CH2OP(O)(OM)2), CF2=CF(OCF2CF(CF3)OCF2CF2CH2OP(O)(OM)2), CF2=CF(OC F2CF2SO2N(CH3)CH2CH2OP(O)(OM)2), CF2=CF(OCF2CF2CF2CF2SO2N(CH3)CH2CH2OP(O)(OM)2), CH2=CH(OCF2CF2CH2OP(O)(OM)2), CH2=CH(O(CF2)4CH2OP(O)(OM)2), CH2=CH(O(CF2)3CH2OP(O)(OM)2), etc. In the above formula, M is the same as above.

[0129] In the general formula (I), A 0 In one preferred embodiment, A is a phosphonate group. 0 is a phosphonate group, examples of the monomer represented by general formula (I) include CF2=CF(OCF2CF2P(O)(OM)2), CF2=CF(O(CF2)4P(O)(OM)2), CF2=CF(OCF2CF(CF3)P(O)(OM)2), CF2=CF(OCF2CF(CF3)OCF2CF2P(O)(OM)2), CH2=CH(OCF2CF2P(O)(OM)2), CH2=CH(O(CF2)4P(O)(OM)2), CH2=CH(O(CF2)3P(O)(OM)2), where M is the same as above.

[0130] The monomer (I) is preferably a monomer (1) represented by general formula (1). The polymer (I) is preferably a polymer (1) containing polymerization units (1) based on a monomer represented by general formula (1). CX2=CY(-CZ2-O-Rf-A) (1) (In the formula, X may be the same or different and is -H or F; Y is -H, -F, an alkyl group or a fluorine-containing alkyl group; Z may be the same or different and is -H, -F, an alkyl group or a fluoroalkyl group; Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms or a fluorine-containing alkylene group having 2 to 100 carbon atoms and having an ether bond; A is -COOM, -SO3M, -OSO3M or -C(CF3)2OM (M is -H, a metal atom, -NR 7 4. An optionally substituted imidazolium, an optionally substituted pyridinium, or an optionally substituted phosphonium, wherein R 7 is H or an organic group.) With the proviso that at least one of X, Y and Z contains a fluorine atom.)

[0131] In the production method of the present disclosure, the monomer (1) represented by general formula (1) may be copolymerized with other monomers. The polymer (1) may be a homopolymer of the monomer (1) represented by the general formula (1) or a copolymer with other monomers.

[0132] The above-mentioned fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond is an alkylene group that does not contain a structure in which an oxygen atom is at the terminal and contains an ether bond between carbon atoms.

[0133] In general formula (1), X is -H or F. Both X's may be -F, or at least one X may be -H. For example, one X may be -F and the other -H, or both X's may be -H.

[0134] In the general formula (1), Y is -H, -F, an alkyl group or a fluorine-containing alkyl group. The alkyl group is an alkyl group that does not contain a fluorine atom, and may have one or more carbon atoms. The alkyl group preferably has six or less carbon atoms, more preferably four or less, and even more preferably three or less. The fluorine-containing alkyl group is an alkyl group that contains at least one fluorine atom, and may have one or more carbon atoms. The fluorine-containing alkyl group preferably has six or less carbon atoms, more preferably four or less, and even more preferably three or less. The Y is preferably -H, -F or CF3, and more preferably -F.

[0135] In the general formula (1), Z is the same or different and is -H, -F, an alkyl group or a fluoroalkyl group. The alkyl group is an alkyl group that does not contain a fluorine atom, and may have one or more carbon atoms. The alkyl group preferably has six or less carbon atoms, more preferably four or less, and even more preferably three or less. The fluorine-containing alkyl group is an alkyl group that contains at least one fluorine atom, and may have one or more carbon atoms. The fluorine-containing alkyl group preferably has six or less carbon atoms, more preferably four or less, and even more preferably three or less. The Z is preferably -H, -F or CF3, and more preferably -F.

[0136] In the general formula (1), at least one of X, Y and Z contains a fluorine atom. For example, X may be -H, and Y and Z may be -F.

[0137] In the general formula (1), the above Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms, or a fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond.

[0138] The number of carbon atoms in the fluorine-containing alkylene group is preferably 2 or more. The number of carbon atoms in the fluorine-containing alkylene group is preferably 30 or less, more preferably 20 or less, even more preferably 10 or less, particularly preferably 6 or less, and most preferably 3 or less. Examples of the fluorine-containing alkylene group include -CF2-, -CH2CF2-, -CF2CF2-, -CF2CH2-, -CF2CF2CF2-, -CF2CF2CH2-, -CF(CF3)-, -CF(CF3)CF2-, -CF(CF3)CH2-, and the like. The fluorine-containing alkylene group is preferably a perfluoroalkylene group.

[0139] The number of carbon atoms in the fluorine-containing alkylene group having an ether bond is preferably 3 or more. The number of carbon atoms in the fluorine-containing alkylene group having an ether bond is preferably 60 or less, more preferably 30 or less, even more preferably 12 or less, particularly preferably 9 or less, and most preferably 6 or less. The fluorine-containing alkylene group having an ether bond is, for example, a group represented by the general formula: [ka] (In the formula, Z 1 is F or CF3;Z 2 and Z 3 are H or F;Z respectively 4 is H, F, or CF3; p1+q1+r1 is an integer of 1 to 10; s1 is 0 or 1; and t1 is an integer of 0 to 5).

[0140] Specific examples of the fluorine-containing alkylene group having an ether bond include -CF2CF(CF3)OCF2-, -CF(CF3)CF2-O-CF(CF3)-, -(CF(CF3)CF2-O) n -CF(CF3)- (wherein n is an integer of 1 to 10), -CF(CF3)CF2-O-CF(CF3)CH2-, -(CF(CF3)CF2-O) nExamples include -CF(CF3)CH2- (wherein n is an integer of 1 to 10), -CH2CF2CF2O-CH2CF2CH2-, -CF2CF2CF2O-CF2-, -CF2CF2CF2O-CF2CF2-, -CF2CF2CF2O-CF2CF2CF2-, -CF2CF2CF2O-CF2CF2CH2-, -CF2CF2O-CF2-, -CF2CF2O-CF2CH2-, etc. The fluorine-containing alkylene group having an ether bond is preferably a perfluoroalkylene group.

[0141] In the general formula (1), A is -COOM, -SO3M, -OSO3M, or -C(CF3)2OM (M is H, a metal atom, NR 7 4. An optionally substituted imidazolium, an optionally substituted pyridinium, or an optionally substituted phosphonium, wherein R 7 is H or an organic group).

[0142] R 7 As for the 1-10 is preferably an organic group represented by the formula: 1-4 More preferred is an organic group of H or C 1-4 More preferred are alkyl groups of the formula:

[0143] The metal atom includes alkali metals (Group 1), alkaline earth metals (Group 2), etc., and is preferably Na, K or Li.

[0144] M is H, a metal atom, or NR 7 4 is preferred, H, an alkali metal (group 1), an alkaline earth metal (group 2) or NR 7 4 is more preferred, H, Na, K, Li or NH4 is even more preferred, H, Na, K or NH4 is even more preferred, H, Na or NH4 is especially preferred, and H or NH4 is most preferred.

[0145] A is preferably -COOM or -SO3M.

[0146] The monomer represented by the general formula (1) may, for example, be a monomer represented by the general formula (1a): CX2 = CFCF2-O-(CF(CF3)CF2O) n5 -CF(CF3)-A (1a) (wherein each X is the same and represents F or H, n5 represents 0 or an integer of 1 to 10, and A is as defined above) is exemplified.

[0147] In general formula (1a), n5 is preferably 0 or an integer from 1 to 5, more preferably 0, 1 or 2, and even more preferably 0 or 1, because particles having a small primary particle size can be obtained.

[0148] In the production method of the present disclosure, the monomer represented by general formula (1a) may be copolymerized with other monomers. The polymer (1) may be a homopolymer of the monomer represented by the general formula (1a) or a copolymer with other monomers.

[0149] The monomer (1) is preferably a monomer represented by the general formula (1A). The polymerized units (1) are preferably polymerized units (1A) based on a monomer represented by general formula (1A). CH2=CF(-CF2-O-Rf-A) (1A) (In the formula, Rf and A are the same as above.)

[0150] In the production method of the present disclosure, the monomer represented by general formula (1A) may be copolymerized with other monomers. The polymer (1) may be a homopolymer of the monomer represented by the general formula (1A) or a copolymer with other monomers.

[0151] Specific examples of the monomer represented by formula (1A) include those represented by the general formula:

[0152] [ka]

[0153] (In the formula, Z 1 is F or CF3;Z 2 and Z 3 are H or F;Z respectively 4 is H, F or CF3; p1+q1+r1 are integers from 0 to 10; s1 is 0 or 1; t1 is an integer from 0 to 5, except for Z 3 and Z 4 are both H, then p1+q1+r1+s1 is not 0; A is as defined above). More specifically,

[0154] [ka]

[0155] The following are preferred:

[0156] [ka]

[0157] It is preferable that:

[0158] As the monomer represented by general formula (1A), it is preferable that A in formula (1A) is -COOM, and in particular, at least one selected from the group consisting of CH2=CFCF2OCF(CF3)COOM and CH2=CFCF2OCF(CF3)CF2OCF(CF3)COOM (wherein M is as defined above) is preferable, and CH2=CFCF2OCF(CF3)COOM is more preferable.

[0159] Further, examples of the monomer represented by the general formula (1) include the monomer represented by the following formula: CF2=CFCF2-O-Rf-A (wherein Rf and A are the same as above)

[0160] More specifically, [ka] etc.

[0161] The monomer (I) is also preferably a monomer (2) represented by the general formula (2). The polymer (I) is also preferably a polymer (2) containing polymerized units (2) based on a monomer represented by general formula (2). CX2=CY(-O-Rf-A) (2) (In the formula, X is the same or different and is -H or F; Y is -H, -F, an alkyl group or a fluorine-containing alkyl group; Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms or a fluorine-containing alkylene group having an ether bond or a keto group having 2 to 100 carbon atoms; and A is the same as defined above.)

[0162] In the production method of the present disclosure, the monomer (2) represented by general formula (2) may be copolymerized with another monomer. The polymer (2) may be a homopolymer of the monomer represented by the general formula (2) or a copolymer with other monomers.

[0163] In general formula (2), X is -H or F. Both X's may be -F, or at least one X may be -H. For example, one X may be -F and the other -H, or both X's may be -H.

[0164] In the general formula (2), Y is -H, -F, an alkyl group or a fluorine-containing alkyl group. The alkyl group is an alkyl group that does not contain a fluorine atom, and may have one or more carbon atoms. The alkyl group preferably has six or less carbon atoms, more preferably four or less, and even more preferably three or less. The fluorine-containing alkyl group is an alkyl group that contains at least one fluorine atom, and may have one or more carbon atoms. The fluorine-containing alkyl group preferably has six or less carbon atoms, more preferably four or less, and even more preferably three or less. Y is preferably -H, -F or -CF3, and more preferably -F.

[0165] In the general formula (2), it is preferable that at least one of X and Y contains a fluorine atom. For example, X may be -H, and Y and Z may be -F.

[0166] In general formula (2), Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms, a fluorine-containing alkylene group having an ether bond having 2 to 100 carbon atoms, or a fluorine-containing alkylene group having a keto group having 2 to 100 carbon atoms. The fluorine-containing alkylene group having an ether bond having 2 to 100 carbon atoms is an alkylene group that does not include a structure in which an oxygen atom is at the terminal and contains an ether bond between carbon atoms.

[0167] The carbon number of the fluorine-containing alkylene group of Rf is preferably 2 or more. Also, it is preferably 30 or less, more preferably 20 or less, even more preferably 10 or less, and particularly preferably 5 or less. Examples of the fluorine-containing alkylene group include -CF2-, -CH2CF2-, -CF2CF2-, -CF2CH2-, -CF2CF2CH2-, -CF(CF3)-, -CF(CF3)CF2-, -CF(CF3)CH2-, -CF2CF2CF2-, and CF2CF2CF2CF2-. The fluorine-containing alkylene group is preferably a perfluoroalkylene group, and more preferably an unbranched linear perfluoroalkylene group.

[0168] The number of carbon atoms in the fluorine-containing alkylene group having an ether bond is preferably 3 or more. The number of carbon atoms in the fluorine-containing alkylene group having an ether bond is preferably 60 or less, more preferably 30 or less, even more preferably 12 or less, and particularly preferably 5 or less. The fluorine-containing alkylene group having an ether bond is, for example, a group represented by the general formula: [ka] (In the formula, Z 1 is F or CF3;Z 2 and Z 3 are H or F;Z respectively 4is H, F, or CF3; p1+q1+r1 is an integer of 1 to 10; s1 is 0 or 1; and t1 is an integer of 0 to 5).

[0169] Specific examples of the fluorine-containing alkylene group having an ether bond include, -CF2CF(CF3)OCF2-, -CF2CF(CF3)OCF2CF2-, -CF2CF(CF3)OCF2CF2CF2-, -CF(CF3)CF2-O-CF(CF3)-, -(CF(CF3)CF2-O) n -CF(CF3)- (wherein n is an integer of 1 to 10), -CF(CF3)CF2-O-CF(CF3)CH2-, -(CF(CF3)CF2-O) n Examples include -CF(CF3)CH2- (wherein n is an integer of 1 to 10), -CH2CF2CF2O-CH2CF2CH2-, -CF2CF2CF2O-CF2-, -CF2CF2CF2O-CF2CF2-, -CF2CF2CF2O-CF2CF2CF2-, -CF2CF2CF2O-CF2CF2CH2-, -CF2CF2O-CF2-, -CF2CF2O-CF2CH2-, etc. The fluorine-containing alkylene group having an ether bond is preferably a perfluoroalkylene group.

[0170] The carbon number of the fluorine-containing alkylene group having a keto group is preferably 3 or more. The carbon number of the fluorine-containing alkylene group having a keto group is preferably 60 or less, more preferably 30 or less, even more preferably 12 or less, and particularly preferably 5 or less.

[0171] Specific examples of the fluorine-containing alkylene group having a keto group include -CF2CF(CF3)CO-CF2-, -CF2CF(CF3)CO-CF2CF2-, -CF2CF(CF3)CO-CF2CF2CF2-, -CF2CF(CF3)CO-CF2CF2CF2-, etc. The fluorine-containing alkylene group having a keto group is preferably a perfluoroalkylene group.

[0172] Water may be added to the keto group in the fluorine-containing alkylene group. Therefore, the monomer (2) may be a hydrate. Examples of the fluorine-containing alkylene group having water added to the keto group include -CF2CF(CF3)C(OH)2-CF2-, -CF2CF(CF3)C(OH)2-CF2CF2-, -CF2CF(CF3)C(OH)2-CF2CF2CF2-, -CF2CF(CF3)C(OH)2-CF2CF2CF2CF2-, and the like.

[0173] The monomer represented by general formula (2) is preferably at least one selected from the group consisting of monomers represented by general formulae (2a), (2b), (2c), (2d), (2e), (2f) and (2g). CF2=CF-O-(CF2) n1 -A (2a) (In the formula, n1 represents an integer of 1 to 10, and A is the same as defined above.) CF2=CF-O-(CF2C(CF3)F) n2 -A (2b) (In the formula, n2 represents an integer of 1 to 5, and A is as defined above.) CF2=CF-O-(CFX 1 ) n3 -A (2c) (In the formula, X 1 represents F or CF3, n3 represents an integer of 1 to 10, and A is as defined above. CF2=CF-O-(CF2CFX 1 O) n4 -(CF2) n6 -A (2d) (In the formula, n4 represents an integer of 1 to 10, n6 represents an integer of 1 to 3, and A and X 1 is the same as the above definition.) CF2=CF-O-(CF2CF2CFX 1 O) n5 -CF2CF2CF2-A (2e) (In the formula, n5 represents an integer of 0 to 10; A and X 1 is the same as the above definition.) CF2=CF-O-(CF2) n7 -O-(CF2) n8 -A (2f) (In the formula, n7 represents an integer of 1 to 10, n8 represents an integer of 1 to 3, and A is as defined above.) CF2=CF[OCF2CF(CF3)] n9 O(CF2) n10 O[CF(CF3)CF2O] n11 CF(CF3)-A (2g) (In the formula, n9 represents an integer of 0 to 5, n10 represents an integer of 1 to 8, and n11 represents an integer of 0 to 5. A is as defined above.)

[0174] In the general formula (2a), the above n1 is preferably an integer of 5 or less, and more preferably an integer of 2 or less.

[0175] Examples of the monomer represented by general formula (2a) include CF2=CF-O-CF2COOM, CF2=CF(OCF2CF2COOM), CF2=CF(O(CF2)3COOM), CF2=CF(OCF2CF2SO3M), CF2=CFOCF2SO3M, and CF2=CFOCF2CF2CF2SO3M (wherein M is as defined above).

[0176] In general formula (2b), n2 is preferably an integer of 3 or less, from the viewpoint of the dispersion stability of the resulting composition.

[0177] In the general formula (2c), n3 is preferably an integer of 5 or less from the viewpoint of water solubility, the above A is preferably -COOM, and the above M is preferably H, Na or NH4.

[0178] In the general formula (2d), X 1 is preferably -CF3 from the viewpoint of dispersion stability of the composition, n4 is preferably an integer of 5 or less from the viewpoint of water solubility, A is preferably -COOM, and M is preferably H, Na or NH4.

[0179] Examples of the monomer represented by general formula (2d) include CF2=CFOCF2CF(CF3)OCF2CF2COOM, CF2=CFOCF2CF(CF3)OCF2COOM, CF2=CFOCF2CF(CF3)OCF2CF2CF2COOM, CF2=CFOCF2CF(CF3)OCF2CF2CF2COOM, CF2=CFOCF2CF(CF3)OCF2SO3M, CF2=CFOCF2CF(CF3)OCF2CF2SO3M, CF2=CFOCF2CF(CF3)OCF2CF2CF2SO3M (wherein M represents H, NH4 or an alkali metal).

[0180] In general formula (2e), n5 is preferably an integer of 5 or less from the viewpoint of water solubility, A is preferably -COOM, and M is preferably H or NH4.

[0181] An example of the monomer represented by the general formula (2e) is CF2=CFOCF2CF2CF2COOM (wherein M represents H, Na, NH4 or an alkali metal).

[0182] In the general formula (2f), n7 is preferably an integer of 5 or less from the viewpoint of water solubility, A is preferably -COOM or -SO3M, and more preferably -COOM, and M is preferably H, Na, K, or NH4.

[0183] An example of the monomer represented by the general formula (2f) is CF2=CF-O-(CF2)3-O-CF2-COOM (wherein M represents H, NH4 or an alkali metal).

[0184] In the general formula (2g), n9 is preferably an integer of 3 or less from the viewpoint of water solubility, n10 is preferably an integer of 3 or less, n11 is preferably an integer of 3 or less, A is preferably -COOM or -SO3M, and more preferably -COOM. M is preferably H, Na, K, or NH4.

[0185] Examples of the monomer represented by general formula (2g) include CF2=CFO(CF2)2OCF(CF3)COOM, CF2=CFOCF2CF2OCF(CF3)CF2OCF(CF3)COOM, CF2=CFOCF2CF(CF3)OCF2CF2OCF(CF3)COOM, CF2=CF[OCF2CF(CF3)]2O(CF2)2O[CF(CF3)CF2O]CF(CF3)COOM, and CF2=CF[OCF2CF(CF3)]3O(CF2)2O[CF(CF3)CF2O]3CF(CF3)COOM (wherein M represents H, NH4 or an alkali metal).

[0186] The monomer (I) is also preferably a monomer (3) represented by the general formula (3). The polymer (I) is also preferably a polymer (3) containing polymerization units (3) based on a monomer represented by general formula (3). CX2=CY(-Rf-A) (3) (In the formula, X is the same or different and is -H or F; Y is -H, -F, an alkyl group or a fluorine-containing alkyl group; Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms or a fluorine-containing alkylene group having an ether bond having 2 to 100 carbon atoms; and A is the same as defined above.)

[0187] In the production method of the present disclosure, the monomer (3) represented by general formula (3) may be copolymerized with other monomers. The polymer (3) may be a homopolymer of the monomer represented by the general formula (3) or a copolymer with other monomers.

[0188] The fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond is an alkylene group that does not include a structure in which an oxygen atom is at the terminal and that contains an ether bond between carbon atoms.

[0189] In general formula (3), Rf is preferably a fluorine-containing alkylene group having a carbon number of 1 to 40. In general formula (3), at least one of X and Y preferably contains a fluorine atom.

[0190] The monomer represented by the general formula (3) is represented by the general formula (3a): CF2=CF-(CF2) n1 -A (3a) (wherein n1 represents an integer of 1 to 10, and A is as defined above), and a monomer represented by general formula (3b): CF2=CF-(CF2C(CF3)F) n2 -A (3b) (wherein n2 represents an integer of 1 to 5, and A is as defined above), is preferable.

[0191] In the general formula (3a) and the general formula (3b), A is preferably -SO3M or COOM, and M is H, a metal atom, NR 7 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent is preferable. 7 represents H or an organic group.

[0192] In general formula (3a), n1 is preferably an integer of 5 or less, and more preferably an integer of 2 or less. A is preferably -COOM, and M is preferably H or NH4.

[0193] An example of the monomer represented by the general formula (3a) is CF2=CFCF2COOM (wherein M is as defined above).

[0194] In general formula (3b), n2 is preferably an integer of 3 or less from the viewpoint of dispersion stability of the resulting composition, A is preferably -COOM, and M is preferably H or NH4.

[0195] Next, a preferred configuration in which m in general formula (I) is an integer of 2 or more will be described.

[0196] It is also preferable that the monomer (I) is at least one selected from the group consisting of monomers represented by general formula (4a) and general formula (4b). It is also preferable that the polymer (I) is a polymer (4) containing polymerization units (4) based on at least one monomer selected from the group consisting of monomers represented by general formula (4a) and general formula (4b). CF2=CF-CF2-OQ F1 -CF(-Q F2 -CZ 1 Z 2 -A)2(4a) (In the formula, Z 1 , Z 2 and A is the same as above, Q F1 and Q F2 are the same or different and each is a single bond, a fluorine-containing alkylene group which may contain an ether bond between carbon atoms, or a fluorine-containing oxyalkylene group which may contain an ether bond between carbon atoms. CF2=CF-OQ F1 -CF(-Q F2 -CZ 1 Z 2 -A)2(4b) (In the formula, Z 1 , Z 2 , A, Q F1 and Q F2 is the same as above)

[0197] As the monomers represented by the general formula (4a) and the general formula (4b), [ka] etc.

[0198] As the monomer (I), at least one selected from the group consisting of the monomer (1), the monomer (2) and the monomer (3) is preferable, the monomer (1) is more preferable, and the monomer (1A) is further preferable. The polymer (I) is preferably at least one selected from the group consisting of the polymer (1), the polymer (2) and the polymer (3), and more preferably the polymer (1).

[0199] In the production method of the present disclosure, the monomer (I) may be copolymerized with other monomers. The polymer (I) may be a homopolymer consisting of only the polymerization unit (I), or may be a copolymer containing the polymerization unit (I) and a polymerization unit based on another monomer copolymerizable with the monomer represented by the general formula (I). From the viewpoint of solubility in an aqueous medium, a homopolymer consisting of only the polymerization unit (I) is preferred. The polymerization unit (I) may be the same or different in each occurrence, and the polymer (I) may contain polymerization units (I) based on two or more different monomers represented by the general formula (I).

[0200] The other monomer is preferably a monomer represented by the general formula CFR=CR2 (wherein R is independently H, F or a perfluoroalkyl group having 1 to 4 carbon atoms). In addition, the other monomer is preferably a fluorine-containing ethylenic monomer having 2 or 3 carbon atoms. Examples of the other monomer include CF2=CF2, CF2=CFCl, CH2=CF2, CFH=CH2, CFH=CF2, CF2=CFCF3, CH2=CFCF3, CH2=CHCF3, CHF=CHCF3 (E form), CHF=CHCF3 (Z form), etc. Among them, in terms of good copolymerizability, at least one selected from the group consisting of tetrafluoroethylene (CF2=CF2), chlorotrifluoroethylene (CF2=CFCl) and vinylidene fluoride (CH2=CF2) is preferred, and at least one selected from the group consisting of tetrafluoroethylene and vinylidene fluoride is more preferred. Therefore, the polymerization units based on the other monomer are preferably polymerization units based on tetrafluoroethylene. The polymerization units based on the other monomer may be the same or different in each occurrence, and the polymer (I) may contain polymerization units based on two or more different other monomers.

[0201] The other monomers include those represented by the general formula (n1-2):

[0202] [ka]

[0203] (In the formula, X 1 , X 2 are the same or different H or F;X 3 is H, F, Cl, CH3 or CF3;X 4 , X 5 are the same or different and are H or F; a and c are the same or different and are 0 or 1. Rf 3 is a fluorine-containing alkyl group having 1 to 40 carbon atoms or a fluorine-containing alkyl group having ether bonds having 2 to 100 carbon atoms).

[0204] Specifically, CH2=CFCF2-O-Rf 3 , CF2=CF-O-Rf 3 , CF2=CFCF2-O-Rf 3 , CF2=CF-Rf 3 , CH2=CH-Rf 3 , CH2=CH-O-Rf 3 (In the formula, Rf 3 is the same as the above formula (n1-2)).

[0205] As the other monomer, there may be mentioned a monomer represented by the formula (n2-1):

[0206] [ka]

[0207] (In the formula, X 9 is H, F or CH3; Rf 4 Also included are fluorine-containing acrylate monomers represented by Rf (a fluorine-containing alkyl group having 1 to 40 carbon atoms or a fluorine-containing alkyl group having 2 to 100 carbon atoms and an ether bond). 4 The base is

[0208] [ka]

[0209] (wherein d3 is an integer of 1 to 4; e3 is an integer of 1 to 10), etc. can be mentioned.

[0210] As the other monomer, there may be mentioned a monomer represented by the formula (n2-2): CH2=CHO-Rf 5 (n2-2) (In the formula, Rf 5 Also included are fluorine-containing vinyl ethers represented by the formula (I) (a fluorine-containing alkyl group having 1 to 40 carbon atoms or a fluorine-containing alkyl group having 2 to 100 carbon atoms and having an ether bond).

[0211] Specific examples of the monomer of general formula (n2-2) include:

[0212] [ka]

[0213] (wherein e6 is an integer of 1 to 10) are preferred.

[0214] More specifically,

[0215] [ka]

[0216] etc.

[0217] Others, general formula (n2-3): CH2=CHCH2O-Rf 6 (n2-3) (In the formula, Rf 6 is a fluorine-containing alkyl group having 1 to 40 carbon atoms or a fluorine-containing alkyl group having an ether bond having 2 to 100 carbon atoms), a fluorine-containing allyl ether represented by the general formula (n2-4): CH2=CH-Rf 7 (n2-4) (In the formula, Rf 7Also included are fluorine-containing vinyl monomers represented by the formula (I) being a fluorine-containing alkyl group having 1 to 40 carbon atoms or a fluorine-containing alkyl group having 2 to 100 carbon atoms and having an ether bond.

[0218] Specific examples of the monomers represented by the general formulas (n2-3) and (n2-4) include:

[0219] [ka]

[0220] and the like monomers.

[0221] The polymer (I) usually has a terminal group. The terminal group is a terminal group generated during polymerization, and representative terminal groups are independently selected from hydrogen, iodine, bromine, linear or branched alkyl groups, and linear or branched fluoroalkyl groups, and may optionally contain at least one catenary heteroatom. The alkyl group or fluoroalkyl group preferably has 1 to 20 carbon atoms. These terminal groups are generally generated from the initiator or chain transfer agent used in the formation of the polymer (I), or are generated during the chain transfer reaction.

[0222] In the polymer (I), the content of the polymerized units (I) is, in order of preference, 1.0 mol% or more, 3.0 mol% or more, 5.0 mol% or more, 10 mol% or more, 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, and 90 mol% or more relative to the total polymerized units. The content of the polymerized units (I) is particularly preferably substantially 100 mol%, and the polymer (I) is most preferably composed only of the polymerized units (I).

[0223] In the polymer (I), the content of the polymerization units based on other monomers copolymerizable with the monomer represented by the general formula (I) is, in order of preference, 99.0 mol% or less, 97.0 mol% or less, 95.0 mol% or less, 90 mol% or less, 80 mol% or less, 70 mol% or less, 60 mol% or less, 50 mol% or less, 40 mol% or less, 30 mol% or less, 20 mol% or less, and 10 mol% or less, based on the total polymerization units. It is particularly preferable that the content of the polymerization units based on other monomers copolymerizable with the monomer represented by the general formula (I) is substantially 0 mol%, and it is most preferable that the polymer (I) does not contain any polymerization units based on other monomers.

[0224] The number average molecular weight of the polymer (I) is 0.1×10 4 More than 0.2×10 is preferable. 4 More preferably, 0.3×10 4 More preferably, 0.4×10 4 More preferably, 0.5×10 4 More preferably, 1.0×10 4 More than 3.0×10 is particularly preferable. 4 More particularly, 3.1×10 4 More than 75.0×10 is most preferable. 4 Less than 50.0×10 is preferable. 4 Less than 40.0×10 is more preferable. 4 More preferably, 30.0×10 4 The following is particularly preferred: 20.0×10 4 The following is particularly preferred. The number average molecular weight and weight average molecular weight are values ​​calculated by gel permeation chromatography (GPC) using monodisperse polystyrene as a standard. In addition, when measurement by GPC is not possible, the number average molecular weight of the polymer (I) can be determined from the correlation between the number average molecular weight calculated from the number of terminal groups obtained by NMR, FT-IR, etc. and the melt flow rate. The melt flow rate can be measured in accordance with JIS K 7210.

[0225] The lower limit of the weight average molecular weight of the polymer (I) is preferably 0.2×104 Above, 0.4×10 4 Above, 0.6×10 4 Above, 0.8 x 10 4 That's it, 1.0 x 10 4 That's it, 2.0 x 10 4 That's it, 5.0 x 10 4 That's it, 10.0 x 10 4 That's it, 15.0 x 10 4 That's it, 20.0 x 10 4 That's it, 25.0 x 10 4 The upper limit of the weight average molecular weight of the polymer (I) is preferably 150.0×10 4 Below, 100.0 x 10 4 Below, 60.0 x 10 4 Below, 50.0 x 10 4 Below, 40.0 x 10 4 The following is the result.

[0226] The polymer (I) preferably has an ion exchange ratio (IXR) of 53 or less, where IXR is defined as the number of carbon atoms in the polymer backbone relative to the ionic group. Precursor groups that become ionic upon hydrolysis (e.g., -SO2F) are not considered ionic groups for purposes of determining IXR.

[0227] IXR is preferably 0.5 or more, more preferably 1 or more, even more preferably 3 or more, even more preferably 4 or more, particularly preferably 5 or more, and particularly preferably 8 or more. IXR is more preferably 43 or less, more preferably 33 or less, and particularly preferably 23 or less.

[0228] The ion exchange capacity of the polymer (I) is, in order of preference, 0.80 meq / g or more, 1.50 meq / g or more, 1.75 meq / g or more, 2.00 meq / g or more, 2.20 meq / g or more, more than 2.20 meq / g, 2.50 meq / g or more, 2.60 meq / g or more, 3.00 meq / g or more, and 3.50 meq / g or more. The ion exchange capacity is the content of ionic groups (anionic groups) in the polymer (I) and is calculated from the composition of the polymer (I).

[0229] In the polymer (I), the ionic (anionic) groups are typically distributed along the polymer backbone. The polymer (I) comprises a polymer backbone with recurring side chains attached to the backbone, which side chains preferably carry ionic groups.

[0230] The polymer (I) preferably comprises an ionic group having a pKa of less than 10, more preferably less than 7. The ionic group of the polymer (I) is preferably selected from the group consisting of sulfonate, carboxylate, phosphonate and phosphate.

[0231] The terms "sulfonate, carboxylate, phosphonate, and phosphate" are intended to refer to the respective salts or to the respective acids capable of forming salts. When salts are used, preferably the salts are alkali metal or ammonium salts. Preferred ionic groups are carboxylate and sulfonate groups.

[0232] The polymer (I) is preferably water-soluble. Water-soluble means the property of being easily dissolved or dispersed in an aqueous medium. The polymer (I) having water-solubility has a particle size that cannot be measured by dynamic light scattering (DLS), for example, or has a particle size of 10 nm or less.

[0233] The viscosity of an aqueous solution of polymer (I) is preferably 5.0 mPa.s or more, more preferably 8.0 mPa.s or more, even more preferably 10.0 mPa.s or more, particularly preferably 12.0 mPa.s or more, and most preferably 14.0 mPa.s or more, preferably 100.0 mPa.s or less, more preferably 50.0 mPa.s or less, even more preferably 25.0 mPa.s or less, and especially preferably 20.0 mPa.s or less.

[0234] The viscosity of the aqueous solution of polymer (I) can be determined by adjusting the content of polymer (I) in the aqueous solution to 33 mass % relative to the aqueous solution, and measuring the viscosity of the obtained aqueous solution at 20°C using a tuning fork vibro viscometer (model: SV-10) manufactured by A&D Corporation.

[0235] The critical micelle concentration (CMC) of the polymer (I) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less.

[0236] The critical micelle concentration of the polymer (I) can be determined by measuring the surface tension. The surface tension can be measured, for example, by a surface tensiometer CBVP-A3 manufactured by Kyowa Interface Science Co., Ltd.

[0237] The acid value of the polymer (I) is preferably 60 or more, more preferably 90 or more, even more preferably 120 or more, particularly preferably 150 or more, and most preferably 180 or more. The upper limit is not particularly limited, but is preferably 300 or less.

[0238] The acid value of the polymer (I) is determined by the presence of an anionic group other than an acid functional group, such as -COOM, -SO3M, -OSO3M, or -C(CF3)2OM (where M is a metal atom, NR 7 4. An optionally substituted imidazolium, an optionally substituted pyridinium, or an optionally substituted phosphonium, wherein R 7 If the compound has an aryl group (H or an organic group), these groups can be converted to acid forms and then measured by acid-base titration.

[0239] The content of polymer (I) in the polymerization dispersion is preferably more than 0.23 mass% relative to PTFE, and is preferably 10.0 mass% or less, 5.0 mass% or less, more preferably 2.0 mass% or less, even more preferably 1.0 mass% or less, and particularly preferably 0.50 mass% or less.

[0240] The content of the polymer (I) in the polymer dispersion can be determined by solid-state NMR measurement or melting NMR measurement. When the polymer (I) contains a carbonyl group, it can also be determined by a Fourier transform infrared spectrometer. Further, WO 2014 / 099453, WO 2010 / 075497, WO 2010 / 075496, WO 2011 / 008381, WO 2009 / 055521, WO 1987 / 007619, JP 61-293476 A, WO 2010 / 075494, WO 2010 / 075359, WO 2012 / 082454, WO 2006 / 119224, WO 2013 / 085864, WO 2014 / 09225, WO 2015 / 09226, WO 2016 / 09228, WO 2017 / 09229, WO 2019 / 09229, WO 2018 / 09229, WO 2019 ... Measurement methods for each polymer are described in Publication No. 2012 / 082707, International Publication No. 2012 / 082703, International Publication No. 2012 / 082451, International Publication No. 2006 / 135825, International Publication No. 2004 / 067588, International Publication No. 2009 / 068528, JP 2004-075978, JP 2001-226436, International Publication No. 1992 / 017635, International Publication No. 2014 / 069165, JP 11-181009, etc. As a method for measuring the content of the polymer (I), the measurement methods for each polymer described therein can be used.

[0241] (Polymerization of Tetrafluoroethylene (TFE)) In the manufacturing method of the present disclosure, at least tetrafluoroethylene (TFE) is polymerized as a fluoromonomer in an aqueous medium. This allows a polymerization dispersion containing polytetrafluoroethylene (PTFE) to be obtained. The PTFE obtained by polymerization of TFE in an aqueous medium is usually obtained in the form of primary particles dispersed in the polymerization dispersion.

[0242] The amount of polymer (I) added in the above polymerization is preferably more than 0.02% by mass and not more than 10% by mass, more preferably not more than 1% by mass, based on the aqueous medium. By setting the amount of polymer (I) added within the above range, the polymerization of the fluoromonomer in the aqueous medium can proceed smoothly. The amount of polymer (I) added is the total amount of polymer (I) added in the above polymerization.

[0243] In the above polymerization, the polymer (I) may be added all at once, or the polymer (I) may be added continuously. The continuous addition of the polymer (I) means, for example, that the polymer (I) is not added all at once, but is added over time, without interruption, or in portions. In the above polymerization, an aqueous solution containing the polymer (I) and water may be prepared, and the aqueous solution may be added.

[0244] In the above polymerization, it is preferable to start adding the polymer (I) before the solid content of the PTFE formed in the aqueous medium reaches 0.5% by mass, and to continue adding the polymer (I) thereafter. The timing of starting the addition of the polymer (I) is preferably before the solid content of the PTFE reaches 0.3% by mass, more preferably before it reaches 0.2% by mass, even more preferably before it reaches 0.1% by mass, and particularly preferably at the same time as the start of polymerization. The above solid content is the content of PTFE relative to the total of the aqueous medium and PTFE.

[0245] In the above polymerization, if at least one polymer (I) is used, PTFE can be produced efficiently. In addition, two or more compounds included in the polymer (I) may be used simultaneously, and a compound having surface activity other than the polymer (I) may be used simultaneously as long as it is volatile or may remain in a molded product made of PTFE.

[0246] In the above polymerization, a nucleating agent may be used. The amount of the nucleating agent added can be appropriately selected depending on the type of the nucleating agent. The amount of the nucleating agent added may be 5000 ppm by mass or less, preferably 1000 ppm by mass or less, more preferably 500 ppm by mass or less, even more preferably 100 ppm by mass or less, particularly preferably 50 ppm by mass or less, and most preferably 10 ppm by mass or less, based on the aqueous medium.

[0247] In the above polymerization, it is preferable to add a nucleating agent to the aqueous medium before the start of polymerization or before the solid content of PTFE formed in the aqueous medium reaches 5.0 mass %. By adding the nucleating agent at the beginning of polymerization, an aqueous dispersion having a small average primary particle size and excellent stability can be obtained.

[0248] The amount of the nucleating agent added at the beginning of polymerization is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, still more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more, based on the PTFE obtained. The upper limit of the amount of the nucleating agent added at the beginning of polymerization is not limited, but is, for example, 2000% by mass.

[0249] The use of a nucleating agent results in PTFE having a smaller primary particle size compared to polymerization carried out in the absence of said nucleating agent.

[0250] Examples of the nucleating agent include dicarboxylic acids, perfluoropolyether (PFPE) acids or salts thereof, hydrocarbon-containing surfactants, etc. The nucleating agent preferably does not contain an aromatic ring and is preferably an aliphatic compound.

[0251] The nucleating agent is preferably added before or simultaneously with the addition of the polymerization initiator, but by adding it during the polymerization, the particle size distribution can also be adjusted.

[0252] The amount of the dicarboxylic acid is preferably 1000 ppm by mass or less, more preferably 500 ppm by mass or less, and even more preferably 100 ppm by mass or less, relative to the aqueous medium.

[0253] The perfluoropolyether (PFPE) acid or salt thereof may have any chain structure in which oxygen atoms in the backbone of the molecule are separated by saturated fluorocarbon groups having 1 to 3 carbon atoms. Also, two or more types of fluorocarbon groups may be present in the molecule. A representative structure has a repeat unit represented by the following formula: (-CFCF3-CF2-O-) n (VII) (-CF2-CF2-CF2-O-) n (VIII) (-CF2-CF2-O-) n -(-CF2-O-) m (IX) (-CF2-CFCF3-O-)n-(-CF2-O-) m (X)

[0254] These structures are described by Kasai in J. Appl. Polymer Sci. 57, 797 (1995). As disclosed therein, the PFPE acid or its salt may have a carboxylic acid group or its salt at one or both ends. The PFPE acid or its salt may also have a sulfonic acid, phosphonic acid group or their salt at one or both ends. The PFPE acid or its salt may also have a different group at each end. For monofunctional PFPEs, the other end of the molecule is usually perfluorinated, but may contain hydrogen or chlorine atoms. The PFPE acid or its salt has at least two ether oxygens, preferably at least four ether oxygens, and even more preferably at least six ether oxygens. Preferably, at least one of the fluorocarbon groups separating the ether oxygens, and more preferably at least two of such fluorocarbon groups, has two or three carbon atoms. Even more preferably, at least 50% of the fluorocarbon groups separating the ether oxygens have two or three carbon atoms. Also, preferably, the PFPE acid or salt thereof has a total of at least 15 carbon atoms, for example, the preferred minimum value of n or n+m in the repeating unit structure above is at least 5. Two or more of the PFPE acids or salts thereof having an acid group at one or both termini may be used in the manufacturing method of the present disclosure. The PFPE acid or salt thereof preferably has a number average molecular weight of less than 6000 g / mol.

[0255] The amount of the hydrocarbon-containing surfactant added is preferably 40 ppm by mass or less, more preferably 30 ppm by mass or less, and even more preferably 20 ppm by mass or less, based on the aqueous medium. It is presumed that the ppm amount of lipophilic nucleation sites present in the aqueous medium is less than the amount added. Therefore, the amount of the lipophilic nucleation sites is less than the above 40 ppm by mass, 30 ppm by mass, and 20 ppm by mass. Since the lipophilic nucleation sites are considered to exist as molecules, even a small amount of the hydrocarbon-containing surfactant can generate a large amount of lipophilic nucleation sites. Therefore, even if the hydrocarbon-containing surfactant is added to the aqueous medium at about 1 ppm by mass, a beneficial effect can be obtained. The preferred lower limit is 0.01 ppm by mass.

[0256] The hydrocarbon-containing surfactants include nonionic and cationic surfactants, including siloxane surfactants such as those disclosed in U.S. Pat. No. 7,897,682 (Brothers et al.) and U.S. Pat. No. 7,977,438 (Brothers et al.).

[0257] The hydrocarbon-containing surfactant is preferably a non-ionic surfactant (e.g., a non-ionic hydrocarbon surfactant). That is, the nucleating agent is preferably a non-ionic surfactant. The non-ionic surfactant preferably does not contain an aromatic moiety.

[0258] Nonionic surfactants usually do not contain charged groups and have a hydrophobic portion that is a long chain hydrocarbon. The hydrophilic portion of the nonionic surfactant contains water-soluble functional groups such as ethylene ether chains derived from polymerization with ethylene oxide.

[0259] Examples of nonionic surfactants include the following. Polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene alkyl esters, sorbitan alkyl esters, polyoxyethylene sorbitan alkyl esters, glycerol esters, and derivatives thereof.

[0260] Specific examples of polyoxyethylene alkyl ethers include polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, and polyoxyethylene behenyl ether.

[0261] Specific examples of polyoxyethylene alkylphenyl ethers include polyoxyethylene nonylphenyl ether and polyoxyethylene octylphenyl ether.

[0262] Specific examples of polyoxyethylene alkyl esters include polyethylene glycol monolaurate, polyethylene glycol monooleate, and polyethylene glycol monostearate.

[0263] Specific examples of sorbitan alkyl esters include polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, and polyoxyethylene sorbitan monooleate.

[0264] Specific examples of polyoxyethylene sorbitan alkyl esters include polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, and polyoxyethylene sorbitan monostearate.

[0265] Examples of glycerol esters include glycerol monomyristate, glycerol monostearate, glycerol monooleate, etc.

[0266] Specific examples of the above derivatives include polyoxyethylene alkylamines, polyoxyethylene alkylphenyl-formaldehyde condensates, polyoxyethylene alkyl ether phosphates, and the like.

[0267] The ethers and esters may have an HLB value of 10-18.

[0268] Examples of nonionic surfactants include the Triton (registered trademark) X series (X15, X45, X100, etc.), the Tergitol (registered trademark) 15-S series, the Tergitol (registered trademark) TMN series (TMN-6, TMN-10, TMN-100, etc.), and the Tergitol (registered trademark) L series, all manufactured by The Dow Chemical Company; the Pluronic (registered trademark) R series (31R1, 17R2, 10R5, 25R4 (m-22, n-23), and the Iconol (registered trademark) TDA series (TDA-6, TDA-9, TDA-10), all manufactured by BASF Corporation.

[0269] The nonionic surfactant is preferably a nonionic surfactant that does not contain fluorine. For example, ether-type nonionic surfactants such as polyoxyethylene alkylphenyl ether, polyoxyethylene alkyl ether, polyoxyethylene alkylene alkyl ether, etc.; polyoxyethylene derivatives such as ethylene oxide / propylene oxide block copolymers; ester-type nonionic surfactants such as sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene sorbitol fatty acid ester, glycerin fatty acid ester, polyoxyethylene fatty acid ester, etc.; amine-based nonionic surfactants such as polyoxyethylene alkylamine, alkyl alkanolamide, etc. may be mentioned.

[0270] In the above nonionic surfactants, the hydrophobic group may be any one of an alkylphenol group, a linear alkyl group, and a branched alkyl group.

[0271] The nonionic surfactant is preferably a nonionic surfactant represented by the general formula (i). R 6 -OA 1 -H(i) (In the formula, R 6 is a linear or branched primary or secondary alkyl group having 8 to 18 carbon atoms; A 1 is a polyoxyalkylene chain.

[0272] In the general formula (i), R 6 The number of carbon atoms in R is preferably 10 to 16, and more preferably 12 to 16. 6 When the carbon number of R is 18 or less, the composition tends to have excellent sedimentation stability. 6 If the carbon number of R exceeds 18, the flow temperature is high and it is difficult to handle. 6 If the number of carbon atoms is less than 8, the surface tension of the composition increases, and the permeability and wettability tend to decrease.

[0273] A 1 The polyoxyalkylene chain of may be composed of oxyethylene and oxypropylene. It is a polyoxyalkylene chain having an average repeat number of oxyethylene groups of 5 to 20 and an average repeat number of oxypropylene groups of 0 to 2, and is a hydrophilic group. The number of oxyethylene units may include either a broad or narrow unimodal distribution as is usually provided, or a broader or bimodal distribution obtained by blending. When the average repeat number of oxypropylene groups is more than 0, the oxyethylene groups and oxypropylene groups in the polyoxyalkylene chain may be arranged in a block form or random form. From the viewpoint of the viscosity and sedimentation stability of the composition, a polyoxyalkylene chain composed of an average repeat number of oxyethylene groups of 7 to 12 and an average repeat number of oxypropylene groups of 0 to 2 is preferred. In particular, A 1 It is preferable that the oxypropylene group has an average of 0.5 to 1.5, since this results in good low foaming properties.

[0274] More preferably, R 6 is (R')(R'')HC-, where R' and R'' are the same or different linear, branched, or cyclic alkyl groups having a total of at least 5, preferably 7 to 17 carbon atoms. Preferably, at least one of R' or R'' is a branched or cyclic hydrocarbon group.

[0275] Specific examples of the polyoxyethylene alkyl ether include C 13 H 27 -O-(C2H4O) n -H, C 12 H25 -O-(C2H4O) n -H, C 10 H 21 CH(CH3)CH2-O-(C2H4O) n -H, C 13 H 27 -O-(C2H4O) n -(CH(CH3)CH2O)-H, C 16 H 33 -O-(C2H4O) n -H, HC(C5H 11 )(C7H 15 )-O-(C2H4O) n -H (wherein n is an integer of 1 or more). Commercially available polyoxyethylene alkyl ethers include, for example, the Genapol X series (manufactured by Clariant) such as Genapol X080 (trade name), the Noigen TDS series (manufactured by Daiichi Kogyo Seiyaku) such as Noigen TDS-80 (trade name), the Leocol TD series (manufactured by Lion) such as Leocol TD-90 (trade name), the Lionol (registered trademark) TD series (manufactured by Lion), the T-Det A series (manufactured by Harcros Chemicals) such as T-Det A138 (trade name), and the Tergitol (registered trademark) 15-S series (manufactured by Dow Chemical).

[0276] The nonionic surfactant is preferably an ethoxylate of 2,6,8-trimethyl-4-nonanol having an average of about 4 to about 18 ethylene oxide units, an ethoxylate of 2,6,8-trimethyl-4-nonanol having an average of about 6 to about 12 ethylene oxide units, or a mixture thereof. Nonionic surfactants of this type are also commercially available, for example, under the trade names TERGITOL TMN-6, TERGITOL TMN-10, and TERGITOL TMN-100X (all trade names, manufactured by The Dow Chemical Company).

[0277] The hydrophobic group of the nonionic surfactant may be any one of an alkylphenol group, a linear alkyl group, and a branched alkyl group. For example, the nonionic surfactant may be a group represented by the general formula (ii): R 7 -C6H4-OA 2 -H (ii) (In the formula, R 7 is a linear or branched alkyl group having 4 to 12 carbon atoms; A 2 is a polyoxyalkylene chain. Specific examples of the nonionic surfactant include Triton (registered trademark) X-100 (trade name, manufactured by Dow Chemical Company).

[0278] A 2 The polyoxyalkylene chain of may be composed of oxyethylene and oxypropylene. It is a polyoxyalkylene chain having an average repeat number of oxyethylene groups of 5 to 20 and an average repeat number of oxypropylene groups of 0 to 2, and is a hydrophilic group. The number of oxyethylene units may include either a broad or narrow unimodal distribution as is usually provided, or a broader or bimodal distribution obtained by blending. When the average repeat number of oxypropylene groups is more than 0, the oxyethylene groups and oxypropylene groups in the polyoxyalkylene chain may be arranged in a block form or random form. From the viewpoint of the viscosity and sedimentation stability of the composition, a polyoxyalkylene chain composed of an average repeat number of oxyethylene groups of 7 to 12 and an average repeat number of oxypropylene groups of 0 to 2 is preferred. In particular, A 2 It is preferable that the oxypropylene group has an average of 0.5 to 1.5, since this results in good low foaming properties.

[0279] More preferably, R 7 is a primary or secondary alkyl group, more preferably (R')(R'')HC-, where R' and R'' are the same or different linear, branched, or cyclic alkyl groups having a total of at least 5 carbon atoms, preferably 7 to 17. Preferably, at least one of R' or R'' is a branched or cyclic hydrocarbon group.

[0280] The nonionic surfactant also includes polyol compounds. Specific examples include those described in International Publication No. 2011 / 014715. Typical examples of polyol compounds include compounds having one or more sugar units as polyol units. The sugar units may be modified to contain at least one long chain. Suitable polyol compounds containing at least one long chain moiety include, for example, alkyl glycosides, modified alkyl glycosides, sugar esters, and combinations thereof. Sugars include, but are not limited to, monosaccharides, oligosaccharides, and sorbitan. Monosaccharides include pentoses and hexoses. Typical examples of monosaccharides include ribose, glucose, galactose, mannose, fructose, arabinose, and xylose. Oligosaccharides include oligomers of 2 to 10 identical or different monosaccharides. Examples of oligosaccharides include, but are not limited to, saccharose, maltose, lactose, raffinose, and isomaltose.

[0281] Typically, suitable sugars for use as polyol compounds include cyclic compounds containing a five-membered ring with four carbon atoms and one heteroatom (typically oxygen or sulfur, but preferably an oxygen atom), or a six-membered ring with five carbon atoms and one heteroatom, preferably an oxygen atom, as described above. These further contain at least two or at least three hydroxyl groups (-OH groups) attached to the carbon ring atoms. Typically, the sugars are modified in that one or more of the hydrogen atoms of the hydroxyl groups (and / or hydroxyalkyl groups) attached to the carbon ring atoms are replaced by a long-chain residue, such that an ether or ester bond is created between the long-chain residue and the sugar moiety. The sugar-based polyol may contain one sugar unit or multiple sugar units. The sugar unit or multiple sugar units may be modified with a long-chain moiety as described above. Specific examples of sugar-based polyol compounds include glycosides, sugar esters, sorbitan esters, and mixtures and combinations thereof.

[0282] A preferred class of polyol compounds are the alkyl or modified alkyl glucosides. These classes of surfactants contain at least one glucose moiety. [ka] (In the formula, x represents 0, 1, 2, 3, 4, or 5; R 1 and R 2 independently represent H or a long chain unit containing at least 6 carbon atoms, with the proviso that R 1 and R 2 At least one of R is not H. 1 and R 2 Exemplary examples include fatty alcohol residues. Examples of fatty alcohols include hexanol, heptanol, octanol, nonanol, decanol, undecanol, dodecanol (lauryl alcohol), tetradecanol, hexadecanol (cetyl alcohol), heptadecanol, octadecanol (stearyl alcohol), eicosanoic acid, and combinations thereof. The above formula represents a specific example of an alkyl polyglucoside showing glucose in the pyranose form, but it is understood that other sugars or sugars of the same sugar but in different enantiomeric or diastereomeric forms may be used. Alkyl glucosides can be obtained, for example, by acid-catalyzed reaction of glucose, starch, or n-butyl glucoside with fatty alcohols, which typically results in a mixture of various alkyl glucosides (Alkylpolygylcoside, Rompp, Lexikon Chemie, Version 2.0, Stuttgart / New York, Georg Thieme Verlag, 1999). Examples of fatty alcohols include hexanol, heptanol, octanol, nonanol, decanol, undecanol, dodecanol (lauryl alcohol), tetradecanol, hexadecanol (cetyl alcohol), heptadecanol, octadecanol (stearyl alcohol), eicosanoic acid, and combinations thereof. Alkyl glucosides are also commercially available from Cognis GmbH, Dusseldorf, Germany under the trade name GLUCOPON or DISPONIL.

[0283] Other nonionic surfactants include difunctional block copolymers supplied by BASF as part of its Pluronic® R series, and tridecyl alcohol alkoxylates supplied by BASF as part of its Iconol® TDA series.

[0284] The nonionic surfactant is preferably at least one selected from the group consisting of nonionic surfactants represented by general formula (i) and nonionic surfactants represented by general formula (ii), and more preferably a nonionic surfactant represented by general formula (i).

[0285] The non-ionic surfactant preferably does not contain an aromatic moiety.

[0286] In the above polymerization, a compound having a functional group capable of reacting by radical polymerization and a hydrophilic group may be used together with the polymer (I). As the compound having a functional group capable of reacting by radical polymerization and a hydrophilic group, the same compound as the modified monomer (A) described later can be used.

[0287] In the above polymerization, in addition to the polymer (I) and other surface active compounds used as desired, additives for stabilizing each compound can be used, such as a buffer, a pH adjuster, a stabilizing aid, and a dispersion stabilizer.

[0288] As the stabilizing aid, paraffin wax, fluorine-based oil, fluorine-based solvent, silicone oil, etc. are preferable. The stabilizing aid may be used alone or in combination of two or more. As the stabilizing aid, paraffin wax is more preferable. The paraffin wax may be liquid, semi-solid, or solid at room temperature, but is preferably a saturated hydrocarbon having 12 or more carbon atoms. The melting point of the paraffin wax is usually preferably 40 to 65°C, more preferably 50 to 65°C.

[0289] The amount of the stabilizing aid used is preferably 0.1 to 12 mass %, more preferably 0.1 to 8 mass %, based on the mass of the aqueous medium used. It is desirable that the stabilizing aid is sufficiently hydrophobic and completely separated from the aqueous dispersion after polymerization so as not to become a contaminating component.

[0290] The above polymerization is preferably carried out by polymerizing TFE substantially in the absence of a fluorine-containing surfactant (excluding compounds having a functional group and a hydrophilic group capable of reacting in radical polymerization). Conventionally, a fluorine-containing surfactant has been used for the polymerization of TFE in an aqueous medium, but according to the production method of the present disclosure, PTFE can be obtained even without using a fluorine-containing surfactant.

[0291] In the present disclosure, "substantially in the absence of a fluorine-containing surfactant" means that the amount of the fluorine-containing surfactant relative to the aqueous medium is 10 ppm by mass or less. The amount of the fluorine-containing surfactant relative to the aqueous medium is preferably 1 ppm by mass or less, more preferably 100 ppb by mass or less, even more preferably 10 ppb by mass or less, and even more preferably 1 ppb by mass or less.

[0292] The fluorine-containing surfactant may be an anionic fluorine-containing surfactant, etc. The anionic fluorine-containing surfactant may be, for example, a surfactant containing fluorine atoms having a total carbon number of 20 or less excluding the anionic group.

[0293] The above-mentioned fluorine-containing surfactant may also be a surfactant containing fluorine in the anionic moiety having a molecular weight of 1,000 or less. The above-mentioned "anionic portion" refers to the portion of the above-mentioned fluorine-containing surfactant excluding the cation. For example, F(CF2) represented by the formula (I) described below n1 In the case of COOM, "F(CF2) n1 The "COO" part.

[0294] The above-mentioned fluorosurfactant also includes a fluorosurfactant having a LogPOW of 3.5 or less. The LogPOW is a partition coefficient between 1-octanol and water, and is expressed as LogP [wherein P represents the ratio of the fluorosurfactant concentration in octanol to the fluorosurfactant concentration in water when a 1:1 octanol / water mixture containing the fluorosurfactant undergoes phase separation]. The LogPOW is calculated from the HPLC elution time of the sample solution using a calibration curve of each elution time and the known octanol / water partition coefficient, which is prepared by performing HPLC on standard substances (heptanoic acid, octanoic acid, nonanoic acid, and decanoic acid) having known octanol / water partition coefficients under the following conditions: column: TOSOH ODS-120T column (φ4.6 mm×250 mm, manufactured by Tosoh Corporation), eluent: acetonitrile / 0.6% by mass HClO4 water=1 / 1 (vol / vol%), flow rate: 1.0 ml / min, sample amount: 300 μL, column temperature: 40° C., and detection light: UV 210 nm.

[0295] Specific examples of the fluorine-containing surfactant include those described in U.S. Patent Application Publication No. 2007 / 0015864, U.S. Patent Application Publication No. 2007 / 0015865, U.S. Patent Application Publication No. 2007 / 0015866, U.S. Patent Application Publication No. 2007 / 0276103, U.S. Patent Application Publication No. 2007 / 0117914, U.S. Patent Application Publication No. 2007 / 142541, U.S. Patent Application Publication No. 2008 / 0015319, U.S. Patent No. 3,250,808, and the like. No. 3,271,341, JP 2003-119204 A, WO 2005 / 042593 A, WO 2008 / 060461 A, WO 2007 / 046377 A, JP 2007-119526 A, WO 2007 / 046482 A, WO 2007 / 046345 A, U.S. Patent Application Publication No. 2014 / 0228531 A, WO 2013 / 189824 A, and WO 2013 / 189826 A can be mentioned.

[0296] The anionic fluorine-containing surfactant may be a surfactant represented by the following general formula (N 0 ): X n0 -Rf n0 -Y 0 (N 0 ) (In the formula, X n0 is H, Cl or F. n0 Y is a linear, branched or cyclic alkylene group having 3 to 20 carbon atoms, in which some or all of the H's are substituted with F, and the alkylene group may contain one or more ether bonds, and some of the H's may be substituted with Cl. 0 is an anionic group. Y 0 The anionic group may be -COOM, -SO2M, or -SO3M, and may be -COOM or -SO3M. M is H, a metal atom, or NR 7 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7is H or an organic group. The metal atom includes alkali metals (Group 1), alkaline earth metals (Group 2), etc., such as Na, K, or Li. R 7 As the 1-10 may be an organic group of H or C 1-4 may be an organic group of H or C 1-4 The alkyl group may be: M is H, a metal atom or NR 7 4, H, an alkali metal (group 1), an alkaline earth metal (group 2) or NR 7 4, which may be H, Na, K, Li or NH4. Above Rf n0 may be one in which 50% or more of H is substituted with fluorine.

[0297] The above general formula (N 0 ) is represented by the following: The following general formula (N 1 ): X n0 -(CF2) m1 -Y 0 (N 1 ) (In the formula, X n0 is H, Cl, or F; m1 is an integer of 3 to 15; Y 0 is as defined above, a compound represented by the following general formula (N 2 ): Rf n1 -O-(CF(CF3)CF2O) m2 CFX n1 -Y 0 (N 2 ) (In the formula, Rf n1 is a perfluoroalkyl group having 1 to 5 carbon atoms, m2 is an integer of 0 to 3, and X n1 is F or CF3, and Y 0 is as defined above, a compound represented by the following general formula (N 3 ): Rf n2 (CH2) m3 -(Rfn3 ) q -Y 0 (N 3 ) (In the formula, Rf n2 is a partially or fully fluorinated alkyl group having 1 to 13 carbon atoms which may contain an ether bond, m3 is an integer of 1 to 3, Rf n3 is a linear or branched perfluoroalkylene group having 1 to 3 carbon atoms, q is 0 or 1, and Y 0 is as defined above, a compound represented by the following general formula (N 4 ): Rf n4 -O-(CY n1 Y n2 ) p CF2-Y 0 (N 4 ) (In the formula, Rf n4 is a linear or branched partially or fully fluorinated alkyl group having 1 to 12 carbon atoms, which may contain an ether bond and / or a chlorine atom; Y n1 and Y n2 are the same or different and are H or F, p is 0 or 1, and Y 0 is as defined above.) and a compound represented by the general formula (N 5 ): [ka] (In the formula, X n2 , X n3 and X n4 Rf may be the same or different and are H, F, or a linear or branched partially or completely fluorinated alkyl group having 1 to 6 carbon atoms, which may contain an ether bond. n5 is a linear or branched, partially or completely fluorinated alkylene group having 1 to 3 carbon atoms, which may contain an ether bond; L is a linking group; Y 0 is as defined above, where X n2 , X n3 , X n4 and Rf n5 The total number of carbon atoms is 18 or less.

[0298] The above general formula (N 0 More specifically, the compound represented by the formula (I) is a perfluorocarboxylic acid (I), a ω-H perfluorocarboxylic acid (II), a perfluoroether carboxylic acid (III), a perfluoroalkyl alkylene carboxylic acid (IV), a perfluoroalkoxy fluorocarboxylic acid (V), a perfluoroalkyl sulfonic acid (VI), a ω-H perfluoro sulfonic acid (VII), a perfluoroalkyl alkylene sulfonic acid (VIII), a perfluoroalkyl alkylene sulfonic acid (IX), a fluorocarboxylic acid (X), a fluorocarboxylic acid (X), a alkoxy fluoro sulfonic acid (XI), a compound (XII), a compound (XIII), and the like.

[0299] The perfluorocarboxylic acid (I) is represented by the following general formula (I): F(CF2) n1 COOM (I) (In the formula, n1 is an integer of 3 to 14, and M is H, a metal atom, or NR 7 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7 is H or an organic group.

[0300] The ω-H perfluorocarboxylic acid (II) is represented by the following general formula (II): H(CF2) n2 COOM (II) (wherein n2 is an integer of 4 to 15, and M is as defined above).

[0301] The perfluoroether carboxylic acid (III) is represented by the following general formula (III): Rf 1 -O-(CF(CF3)CF2O) n3 CF(CF3)COOM (III) (In the formula, Rf 1 is a perfluoroalkyl group having 1 to 5 carbon atoms, n3 is an integer of 0 to 3, and M is as defined above.

[0302] The perfluoroalkyl alkylene carboxylic acid (IV) is represented by the following general formula (IV): Rf 2 (CH2) n4 Rf 3 COOM (IV) (In the formula, Rf 2 is a perfluoroalkyl group having 1 to 5 carbon atoms, and Rf 3 is a linear or branched perfluoroalkylene group having 1 to 3 carbon atoms, n4 is an integer of 1 to 3, and M is as defined above.

[0303] The alkoxyfluorocarboxylic acid (V) is represented by the following general formula (V): Rf 4 -O-CY 1 Y 2 CF2-COOM (V) (In the formula, Rf 4 is a linear or branched partially or fully fluorinated alkyl group having 1 to 12 carbon atoms, which may contain an ether bond and / or a chlorine atom; Y 1 and Y 2 are the same or different and are H or F, and M is as defined above.

[0304] The perfluoroalkylsulfonic acid (VI) is represented by the following general formula (VI): F(CF2) n5 SO3M (VI) (wherein n5 is an integer of 3 to 14, and M is as defined above).

[0305] The above ω-H perfluorosulfonic acid (VII) is represented by the following general formula (VII): H(CF2) n6 SO3M (VII) (wherein n6 is an integer of 4 to 14, and M is as defined above).

[0306] The perfluoroalkyl alkylene sulfonic acid (VIII) is represented by the following general formula (VIII): Rf 5 (CH2) n7 SO3M (VIII) (In the formula, Rf 5 is a perfluoroalkyl group having 1 to 13 carbon atoms, n7 is an integer of 1 to 3, and M is as defined above.

[0307] The alkyl alkylene carboxylic acid (IX) is represented by the following general formula (IX): Rf 6 (CH2) n8 COOM (IX) (In the formula, Rf 6 is a linear or branched partially or completely fluorinated alkyl group having 1 to 13 carbon atoms which may contain an ether bond, n8 is an integer from 1 to 3, and M is as defined above.

[0308] The fluorocarboxylic acid (X) is represented by the following general formula (X): Rf 7 -O-Rf 8 -O-CF2-COOM (X) (In the formula, Rf 7 is a linear or branched partially or fully fluorinated alkyl group having 1 to 6 carbon atoms, which may contain an ether bond and / or a chlorine atom; Rf 8 is a linear or branched, partially or fully fluorinated alkyl group having 1 to 6 carbon atoms, and M is as defined above.

[0309] The alkoxyfluorosulfonic acid (XI) is represented by the following general formula (XI): Rf 9 -O-CY 1 Y 2 CF2-SO3M (XI) (In the formula, Rf 9 is a linear or branched alkyl group having 1 to 12 carbon atoms, which may contain an ether bond, and which may contain chlorine, and which is partially or completely fluorinated; Y 1 and Y 2 are the same or different and are H or F, and M is as defined above.

[0310] The compound (XII) is represented by the following general formula (XII): [ka] (In the formula, X 1 , X 2 and X 3 Rf may be the same or different and are H, F and linear or branched partially or completely fluorinated alkyl groups having 1 to 6 carbon atoms, which may contain ether bonds; 10 is a perfluoroalkylene group having 1 to 3 carbon atoms, L is a linking group, and Y 0 is an anionic group. Y 0 may be -COOM, -SO2M, or -SO3M, or may be -SO3M or COOM, where M is as defined above. Examples of L include a single bond and a partially or completely fluorinated alkylene group having 1 to 10 carbon atoms which may contain an ether bond.

[0311] The compound (XIII) is represented by the following general formula (XIII): Rf 11 -O-(CF2CF(CF3)O) n9 (CF2O) n10 CF2COOM (XIII) (In the formula, Rf 11is a fluoroalkyl group containing chlorine and having 1 to 5 carbon atoms, n9 is an integer of 0 to 3, n10 is an integer of 0 to 3, and M is as defined above.) Compound (XIII) is represented by CF2ClO(CF2CF(CF3)O) n9 (CF2O) n10 CF2COONH4 (a mixture having an average molecular weight of 750, where n9 and n10 are defined above).

[0312] As described above, examples of the anionic fluorine-containing surfactant include carboxylic acid surfactants and sulfonic acid surfactants.

[0313] The fluorine-containing surfactant may be one type of fluorine-containing surfactant or a mixture containing two or more types of fluorine-containing surfactants.

[0314] The fluorine-containing surfactant may be a compound represented by the following formula: The fluorine-containing surfactant may be a mixture of these compounds. In one embodiment of the above polymerization, TFE is polymerized substantially in the absence of a compound represented by the following formula: F(CF2)7COOM, F(CF2)5COOM, H(CF2)6COOM, H(CF2)7COOM, CF3O(CF2)3OCHFCF2COOM, C3F7OCF(CF3)CF2OCF(CF3)COOM, CF3CF2CF2OCF(CF3)COOM, CF3CF2OCF2CF2OCF2COOM, C2F5OCF(CF3)CF2OCF(CF3)COOM, CF3OCF(CF3)CF2OCF(CF3)COOM, CF2ClCF2CF2OCF(CF3)CF2OCF2COOM, CF2ClCF2CF2OCF2CF(CF3)OCF2COOM, CF2ClCF(CF3)OCF(CF3)CF2OCF2COOM, CF2ClCF(CF3)OCF2CF(CF3)OCF2COOM, [ka] (In each formula, M is H, metal atom, NR 7 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7 is H or an organic group.

[0315] (aqueous medium) The aqueous medium used in the production method of the present disclosure means a liquid containing water. The aqueous medium is not particularly limited as long as it contains water, and may contain water and, for example, a fluorine-free organic solvent such as alcohol, ether, or ketone, and / or a fluorine-containing organic solvent having a boiling point of 40° C. or less, and is preferably water alone.

[0316] In the manufacturing method of the present disclosure, it is also preferable to polymerize TFE and modified monomer. That is, PTFE may be homo-PTFE that contains only TFE unit, or modified PTFE that contains TFE unit and modified monomer unit based on modified monomer that can be copolymerized with TFE.

[0317] The amount of the modifying monomer added when polymerizing TFE is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.03% by mass or more, particularly preferably 0.05% by mass or more, preferably 1.0% by mass or less, more preferably 0.8% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0.3% by mass or less, based on the amount of the resulting PTFE.

[0318] The above-mentioned modified monomer is not particularly limited as long as it is copolymerizable with TFE, and includes fluoromonomers and non-fluoromonomers. The modified monomer used may be one type or multiple types.

[0319] The non-fluoromonomer is not particularly limited and may be represented by the general formula: CH2=CR Q1 -LR Q2 (In the formula, R Q1 represents a hydrogen atom or an alkyl group. L represents a single bond, -CO-O-*, -O-CO-* or -O-. * represents R Q2 R represents the bond position. Q2 represents a hydrogen atom, an alkyl group or a nitrile group.

[0320] Examples of non-fluoromonomers include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, hexyl methacrylate, cyclohexyl methacrylate, vinyl methacrylate, vinyl acetate, acrylic acid, methacrylic acid, acrylonitrile, methacrylonitrile, ethyl vinyl ether, cyclohexyl vinyl ether, etc. Of these, butyl methacrylate, vinyl acetate, and acrylic acid are preferred as non-fluoromonomers.

[0321] Examples of fluoromonomers include perfluoroolefins such as hexafluoropropylene (HFP); hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride (VDF); perhaloolefins such as chlorotrifluoroethylene; perfluorovinyl ethers; (perfluoroalkyl)ethylenes; and perfluoroallyl ethers.

[0322] The perfluorovinyl ether is not particularly limited, and may be, for example, a perfluorovinyl ether represented by the general formula (A): CF2=CF-ORf (A) (wherein Rf represents a perfluoro organic group). In the present disclosure, the "perfluoro organic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms. The perfluoro organic group may have an ether oxygen.

[0323] An example of the perfluorovinyl ether is perfluoro(alkyl vinyl ether) [PAVE] represented by the general formula (A), in which Rf is a perfluoroalkyl group having 1 to 10 carbon atoms. The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5.

[0324] Examples of the perfluoroalkyl group in the PAVE include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group.

[0325] The perfluorovinyl ether further includes those in which Rf in the general formula (A) is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms, and those in which Rf is the following formula:

[0326] [ka]

[0327] (wherein m represents 0 or an integer of 1 to 4), Rf is a group represented by the following formula:

[0328] CF3CF2CF2-(O-CF(CF3)-CF2) n - (wherein n represents an integer of 1 to 4).

[0329] Examples of hydrogen-containing fluoroolefins include CH2=CF2, CFH=CH2, CFH=CF2, CH2=CFCF3, CH2=CHCF3, CHF=CHCF3 (E-form), and CHF=CHCF3 (Z-form).

[0330] The (perfluoroalkyl)ethylene (PFAE) is not particularly limited, and examples thereof include (perfluorobutyl)ethylene (PFBE) and (perfluorohexyl)ethylene.

[0331] Examples of perfluoroallyl ethers include General formula: CF2=CF-CF2-ORf (wherein Rf represents a perfluoro organic group).

[0332] Rf in the above general formula is the same as Rf in general formula (A). Rf is preferably a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoroalkoxyalkyl group having 1 to 10 carbon atoms. As the perfluoroallyl ether, at least one selected from the group consisting of CF2=CF-CF2-O-CF3, CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9 is preferable, at least one selected from the group consisting of CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9 is more preferable, and CF2=CF-CF2-O-CF2CF2CF3 is even more preferable.

[0333] A preferred example of the modifying monomer is the modifying monomer (3) having a monomer reactivity ratio of 0.1 to 8. By allowing the modifying monomer (3) to exist, PTFE particles having a small particle size can be obtained, and an aqueous dispersion with high dispersion stability can be obtained.

[0334] Here, the monomer reactivity ratio in copolymerization with TFE is the value obtained by dividing the rate constant of the reaction of the growing radical with TFE by the rate constant of the reaction of the growing radical with the modified monomer when the growing radical is less than the repeating unit based on TFE. The lower this value, the higher the reactivity of the modified monomer with TFE. The monomer reactivity ratio can be calculated by the composition in the polymer produced immediately after the start of copolymerization of TFE with the modified monomer and using the Feynman-Ross equation.

[0335] The copolymerization is carried out in a 6.0L stainless steel autoclave using 3600g of deionized degassed water, 1000 mass ppm of ammonium perfluorooctanoate relative to the water, and 100g of paraffin wax at a pressure of 0.78 MPaG and a temperature of 70°C. 0.05g, 0.1g, 0.2g, 0.5g, and 1.0g of modified monomer are added to the reactor, respectively, and 0.072g of ammonium persulfate (20 mass ppm relative to water) is added, and TFE is continuously fed to maintain the polymerization pressure of 0.78 MPaG. When the amount of TFE charged reaches 1000g, stirring is stopped and the reactor is depressurized until atmospheric pressure is reached. After cooling, the paraffin wax is separated to obtain an aqueous dispersion containing the produced polymer. The aqueous dispersion is stirred to coagulate the produced polymer, and then dried at 150°C. The composition of the resulting polymer is calculated by an appropriate combination of NMR, FT-IR, elemental analysis, and X-ray fluorescence analysis depending on the type of monomer.

[0336] The modifying monomer (3) having a monomer reactivity ratio of 0.1 to 8 is preferably at least one selected from the group consisting of the modifying monomers represented by the formulas (3a) to (3d). CH2=CH-Rf 1 (3a) (In the formula, Rf 1 is a perfluoroalkyl group having 1 to 10 carbon atoms. CF2=CF-O-Rf 2 (3b) (In the formula, Rf 2 is a perfluoroalkyl group having 1 to 2 carbon atoms. CF2=CF-O-(CF2) n CF=CF2(3c) (In the formula, n is 1 or 2.)

[0337] [ka] (In the formula, X 3 and X 4 is F, Cl or a methoxy group, and Y is of formula Y1 or Y2.

[0338] [ka] (In formula Y2, Z and Z' are F or a fluorinated alkyl group having 1 to 3 carbon atoms.)

[0339] The content of the modified monomer (3) unit is preferably in the range of 0.00001 to 1.0% by mass based on the total polymerized units of PTFE. The lower limit is more preferably 0.0001% by mass, more preferably 0.0005% by mass, even more preferably 0.001% by mass, and even more preferably 0.005% by mass. The upper limit is, in order of preference, 0.90% by mass, 0.50% by mass, 0.40% by mass, 0.30% by mass, 0.20% by mass, 0.15% by mass, 0.10% by mass, 0.08% by mass, 0.05% by mass, and 0.01% by mass.

[0340] The modified monomer is preferably at least one selected from the group consisting of hexafluoropropylene, chlorotrifluoroethylene, vinylidene fluoride, perfluoro(alkyl vinyl ether), (perfluoroalkyl)ethylene, ethylene, and modified monomers having a functional group capable of reacting by radical polymerization and a hydrophilic group, because it can obtain an aqueous dispersion with a small average primary particle size, a small aspect ratio of primary particles, and excellent stability.By using the modified monomer, it is possible to obtain an aqueous dispersion of PTFE with a smaller average primary particle size, a smaller aspect ratio of primary particles, and excellent dispersion stability.In addition, it is possible to obtain an aqueous dispersion with less uncoagulated polymer.

[0341] From the viewpoint of reactivity with TFE, the modifying monomer preferably contains at least one selected from the group consisting of hexafluoropropylene, perfluoro(alkyl vinyl ether) and (perfluoroalkyl)ethylene. More preferably, it contains at least one selected from the group consisting of hexafluoropropylene, perfluoro(methyl vinyl ether), perfluoro(propyl vinyl ether), (perfluorobutyl)ethylene, (perfluorohexyl)ethylene, and (perfluorooctyl)ethylene. The total amount of the hexafluoropropylene unit, the perfluoro(alkyl vinyl ether) unit and the (perfluoroalkyl)ethylene unit is preferably in the range of 0.00001 to 1% by mass based on the total polymerized units of PTFE. The lower limit of the total amount is more preferably 0.0001% by mass, more preferably 0.0005% by mass, even more preferably 0.001% by mass, and even more preferably 0.005% by mass. The upper limit is, in order of preference, 0.80% by mass, 0.70% by mass, 0.50% by mass, 0.40% by mass, 0.30% by mass, 0.20% by mass, 0.15% by mass, 0.10% by mass, 0.08% by mass, 0.05% by mass, and 0.01% by mass.

[0342] The above-mentioned modified monomer preferably includes a modified monomer having a functional group capable of reacting by radical polymerization and a hydrophilic group (hereinafter referred to as "modified monomer (A)").

[0343] By making the above-mentioned modified monomer (A) exist, it is possible to obtain PTFE particles with small primary particle size, and obtain an aqueous dispersion with high dispersion stability. It is also possible to reduce the amount of uncoagulated polymer. Furthermore, it is possible to reduce the aspect ratio of primary particles.

[0344] The amount of the modified monomer (A) used is preferably more than an amount equivalent to 0.1 ppm by mass of the aqueous medium, more preferably more than 0.5 ppm by mass, even more preferably more than 1.0 ppm by mass, even more preferably 5 ppm by mass or more, and particularly preferably 10 ppm by mass or more. If the amount of the modified monomer (A) used is too small, the average primary particle size of the obtained PTFE may not be reduced. The amount of the modified monomer (A) used may be within the above range, but the upper limit may be, for example, 5000 mass ppm. In the above production method, the modified monomer (A) may be added to the system during the reaction in order to improve the stability of the aqueous dispersion during or after the reaction.

[0345] Since the above-mentioned modifying monomer (A) is highly water-soluble, even if unreacted modifying monomer (A) remains in the aqueous dispersion, it can be easily removed in the concentration step or the coagulation and washing steps.

[0346] The above-mentioned modifying monomer (A) is incorporated into the produced polymer during the polymerization process. However, since the concentration of the modifying monomer (A) itself in the polymerization system is low and the amount incorporated into the polymer is small, there is no problem of a decrease in the heat resistance of PTFE or coloration after baking.

[0347] Examples of the hydrophilic group in the modified monomer (A) include -NH2, -PO3M, -OPO3M, -SO3M, -OSO3M, and -COOM (in each formula, M is H, a metal atom, or NR 7y 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7y are H or organic groups and may be the same or different. Any two of them may be bonded to each other to form a ring. Of these, -SO3M or -COOM is preferred as the hydrophilic group. R 7y The organic group in R is preferably an alkyl group. 7y As the 1-10 is preferably an organic group represented by the formula:1-4 More preferred is an organic group represented by the formula: 1-4 More preferred are alkyl groups of the formula: The metal atom may be a monovalent or divalent metal atom, such as an alkali metal (group 1) or an alkaline earth metal (group 2), with Na, K or Li being preferred.

[0348] Examples of the "functional group capable of reacting by radical polymerization" in the modifying monomer (A) include groups having an ethylenically unsaturated bond, such as a vinyl group and an allyl group. The group having an ethylenically unsaturated bond is represented by the following formula: CX e X g =CX f R- (In the formula, X e , X f and X g are each independently F, Cl, H, CF3, CF2H, CFH2, or CH3; and R is a linking group. The linking group of R can be represented by the formula: a Preferred are -CH=CH2 and -CF=CH 2、 -CH=CF 2、 Examples of groups having unsaturated bonds include -CF=CF2, -CH2-CH=CH2, -CF2-CF=CH2, -CF2-CF=CF2, -(C=O)-CH=CH2, -(C=O)-CF=CH2, -(C=O)-CF=CH2, -(C=O)-CF=CF2, -(C=O)-CF=CF2, -(C=O)-C(CH3)=CH2, -(C=O)-C(CF3)=CH2, -(C=O)-C(CH3)=CF2, -(C=O)-C(CF3)=CF2, -O-CH2-CH=CH2, -O-CF2-CF=CH2, -O-CH2-CH=CF2, and -O-CF2-CF=CF2.

[0349] The modified monomer (A) has a functional group that can react by radical polymerization, so it is assumed that when used in the polymerization, it reacts with the fluorine-containing monomer at the initial stage of the polymerization reaction, and forms highly stable particles that have hydrophilic groups derived from the modified monomer (A).Therefore, it is considered that the number of particles increases when polymerization is carried out in the presence of the modified monomer (A).

[0350] The above polymerization may be carried out in the presence of one type of the modifying monomer (A), or in the presence of two or more types thereof.

[0351] In the above polymerization, a compound having an unsaturated bond can be used as the modifying monomer (A).

[0352] The modifying monomer (A) is represented by the general formula (4): CX i X k =CX j R a -(CZ 1 Z 2 ) k -Y 3 (4) (In the formula, X i , X j and X k are each independently F, Cl, H, or CF; Y 3 is a hydrophilic group; R a is a linking group; Z 1 and Z 2 are each independently H, F or CF3, and k is 0 or 1). Examples of the hydrophilic group include -NH2, -PO3M, -OPO3M, -SO3M, -OSO3M, and -COOM (in each formula, M is H, a metal atom, or NR 7y 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7y are H or organic groups and may be the same or different. Any two of them may be bonded to each other to form a ring. Of these, -SO3M or -COOM is preferred as the hydrophilic group. R 7y The organic group in R is preferably an alkyl group. 7y As the 1-10 is preferably an organic group represented by the formula: 1-4 More preferred is an organic group represented by the formula: 1-4The above metal atom is preferably a monovalent or divalent metal atom, such as an alkali metal (group 1) or an alkaline earth metal (group 2), with Na, K or Li being preferred. By using the modifying monomer (A), it is possible to obtain an aqueous dispersion having a smaller average primary particle size and excellent stability, and also to reduce the aspect ratio of the primary particles.

[0353] Above R a is a linking group. In the present disclosure, the "linking group" refers to a divalent linking group. The linking group may be a single bond, and preferably contains at least one carbon atom, and the number of carbon atoms may be 2 or more, 4 or more, 8 or more, 10 or more, or 20 or more. There is no upper limit, but it may be, for example, 100 or less, or 50 or less. The linking group may be linear or branched, cyclic or acyclic in structure, saturated or unsaturated, substituted or unsubstituted, and may optionally contain one or more heteroatoms selected from the group consisting of sulfur, oxygen, and nitrogen, and may optionally contain one or more functional groups selected from the group consisting of esters, amides, sulfonamides, carbonyls, carbonates, urethanes, ureas, and carbamates. The linking group may not contain carbon atoms, but may be a catenary heteroatom such as oxygen, sulfur, or nitrogen.

[0354] Above R a is preferably, for example, a catenary heteroatom such as oxygen, sulfur, or nitrogen, or a divalent organic group. R a When R is a divalent organic group, the hydrogen atom bonded to the carbon atom may be replaced with a halogen atom other than fluorine, such as chlorine, and may or may not contain a double bond. a may be either linear or branched, and may be either cyclic or noncyclic. a may contain functional groups (eg, esters, ethers, ketones, amines, halides, etc.). R amay also be a non-fluorinated divalent organic group, or a partially fluorinated or perfluorinated divalent organic group. R a Examples of the hydrocarbon group include a hydrocarbon group having no fluorine atoms bonded to a carbon atom, a hydrocarbon group in which some of the hydrogen atoms bonded to a carbon atom are substituted with fluorine atoms, a hydrocarbon group in which all of the hydrogen atoms bonded to a carbon atom are substituted with fluorine atoms, -(C=O)-, -(C=O)-O-, or a hydrocarbon group containing an ether bond, which may contain an oxygen atom, a double bond, or a functional group.

[0355] R a is preferably -(C=O)-, -(C=O)-O-, or a hydrocarbon group having 1 to 100 carbon atoms which may contain an ether bond and may contain a carbonyl group, and in the hydrocarbon group, some or all of the hydrogen atoms bonded to the carbon atoms may be substituted with fluorine. R a Preferably, -(CH2) a -, -(CF2) a -, -O-(CF2) a -, -(CF2) a -O-(CF2) b -, -O(CF2) a -O-(CF2) b -, -(CF2) a -[O-(CF2) b ] c -, -O(CF2) a -[O-(CF2) b ] c -,-[(CF2) a -O] b -[(CF2) c -O] d -, -O[(CF2) a -O] b -[(CF2) c -O] d -, -O-[CF2CF(CF3)O] a -(CF2) b -, -(C=O)-, -(C=O)-O-, -(C=O)-(CH2) a-, -(C=O)-(CF2) a -, -(C=O)-O-(CH2) a -, -(C=O)-O-(CF2) a -, -(C=O)-[(CH2) a -O] b -, -(C=O)-[(CF2) a -O] b -, -(C=O)-O[(CH2) a -O] b -, -(C=O)-O[(CF2) a -O] b -, -(C=O)-O[(CH2) a -O] b -(CH2) c -, -(C=O)-O[(CF2) a -O] b -(CF2) c -, -(C=O)-(CH2) a -O-(CH2) b -, -(C=O)-(CF2) a -O-(CF2) b -, -(C=O)-O-(CH2) a -O-(CH2) b -, -(C=O)-O-(CF2) a -O-(CF2) b At least one selected from the group consisting of -, -(C=O)-O-C6H4-, and combinations thereof. In the formula, a, b, c, and d are independently at least 1. a, b, c, and d may be independently 2 or more, 3 or more, 4 or more, 10 or more, or 20 or more. The upper limit of a, b, c, and d is, for example, 100.

[0356] R aSpecific examples suitable as -CF2-O-, -CF2-O-CF2-, -CF2-O-CH2-, -CF2-O-CH2CF2-, -CF2-O-CF2CF2-, -CF2-O-CF2CH2-, -CF2-O-CF2CF2CH2-, -CF2-O-CF(CF3)-, -CF2-O-CF(CF3) CF2-, -CF2-O-CF(CF3)CF2-O-, -CF2-O-CF(CF3)CH2-, -(C=O)-, -(C=O)-O-, -(C=O)- (CH2)-, -(C=O)-(CF2)-, -(C=O)-O-(CH2)-, -(C=O)-O-(CF2)-, -(C=O)-[(CH2)2-O] n -, -(C=O)-[(CF2)2-O] n -, -(C=O)-O[(CH2)2-O] n -, -(C=O)-O[(CF2)2-O] n -, -(C=O)-O[(CH2)2-O] n -(CH2)-, -(C=O)-O[(CF2)2-O] n -(CF2)-, -(C=O)-(CH2)2-O-(CH2)-, -(C=O)-(CF2)2-O-(CF2)-, -(C=O)-O-(CH2)2-O-(CH2)-, -(C=O)-O-(CF2)2-O-(CH2)-, -(C=O)-O-(CF2)2-O-(CF2)-, -(C=O)-O-C6H4- and the like. a Specifically, -CF2-O-, -CF2-O-CF2-, -CF2-O-CF2CF2-, -CF2-O-CF(CF3)-, -CF2-O-CF(CF3)CF2-, -CF2 -O-CF(CF3)CF2-O-, -(C=O)-, -(C=O)-O-, -(C=O)-(CH2)-, -(C=O)-O-(CH2)-, -(C=O)-O[(CH2)2-O] n -, -(C=O)-O[(CH2)2-O] n Preferred are -(CH2)-, -(C=O)-(CH2)2-O-(CH2)-, or -(C=O)-O-C6H4-. In the above formula, n is an integer of 1-10.

[0357] -R in general formula (4) a -(CZ 1 Z 2 )k -としては、-CF2-O-CF2-、-CF2-O-CF(CF3)-、-CF2-OC(CF3)2-、-CF2-O-CF2-CF2-、-CF2-O-CF2-CF(CF3)-、-CF2-O-CF2-C(CF3)2-、-CF2-O-CF2CF2-CF2-、-CF2-O-CF2CF2-CF(CF3)-、-CF2-O-CF2CF2-C(CF3)2-、-CF2-O-CF(CF3)-CF2-、-CF2-O-CF(CF3)-CF(CF3)-、-CF2-O-CF(CF3)-CF(CF3)-、-CF2-O-CF(CF3)-C(CF3)2-、-CF2-O-C F(CF3)CF2-CF2-、-CF2-O-CF(CF3)CF2-CF(CF3)-、-CF2-O-CF(CF3)CF2-C(CF3)2-、-CF2-O-CF(CF3)CF2-O-CF2-、-CF2-O-CF(CF3)CF2-O-CF(CF3)-、 -CF2-O-CF(CF3)CF2-OC(CF3)2-、-(C=O)-、-(C=O)-O-、-(C=O)-(CH2)-、- (C=O)-(CF2)-、-(C=O)-O-(CH2)-、-(C=O)-O-(CF2)-、-(C=O)-[(CH2)2-O] n -(CH2)-、-(C=O)-[(CF2)2-O] n -(CF2)-、-(C=O)-[(CH2)2-O] n -(CH2)-(CH2)-、-(C=O)-[(CF2)2-O] n -(CF2)-(CF2)-、-(C=O)-O[(CH2)2-O] n -(CF2)-、-(C=O)-O[(CH2)2-O] n -(CH2)-(CH2)-、-(C=O)-O[(CF2)2-O] n -(CF2)-、-(C=O)-O[(CF2)2-O] n-(CF2)-(CF2)-, -(C=O)-(CH2)2-O-(CH2)-(CH2)-, -(C=O)-(CF2)2-O-(CF2)-(CF2)-, -(C=O)-O-(CH2)2-O-(CH2)-(CH2)-, -(C=O )-O-(CF2)2-O-(CF2)-(CF2)-, -(C=O)-O-(CH2)2-O-(CH2)-C(CF3)2-, -(C=O)-O-(CF2)2-O-(CF2)-C(CF3)2-, or -(C=O)-O-C6H4- C(CF3)2- is preferred, -CF2-O-CF(CF3)-, -CF2-O-CF2-CF(CF3)-, -CF2-O-CF2CF2-CF(CF3)-, -CF2-O-CF(CF3)-CF(CF3)-, -CF2-O-CF(C F3)CF2-CF(CF3)-, -CF2-O-CF(CF3)CF2-O-CF(CF3)-, -(C=O)-, -(C=O)-O-(CH2)-, -(C=O)-O-(CH2)-(CH2)-, -(C=O)-O[(CH2)2-O] n -(CH2)-(CH2)-, -(C=O)-O-(CH2)2-O-(CH2)-C(CF3)2- or -(C=O)-O-C6H4-C(CF3)2- are more preferred. In the above formula, n is an integer of 1-10.

[0358] Specific examples of the compound represented by formula (4) include: [ka] (In the formula, X j and Y 3 is the same as above. n is an integer of 1 to 10.

[0359] R a As the general formula (r1): -(C=O) h -(O) i -CF2-O-(CX 6 2) e -{O-CF(CF3)} f -(O) g - (r1) (In the formula, X 6are each independently H, F or CF3, e is an integer of 0 to 3, f is an integer of 0 to 3, g is 0 or 1, h is 0 or 1, and i is 0 or 1), and a divalent group represented by the general formula (r2): -(C=O) h -(O) i -CF2-O-(CX 7 2) e -(O) g - (r2) (In the formula, X 7 are each independently H, F or CF3, e is an integer of 0 to 3, g is 0 or 1, h is 0 or 1, and i is 0 or 1.) is also preferred.

[0360] -R in general formula (4) a -(CZ 1 Z 2 ) k - may also be represented by the following formula (t1): -(C=O) h -(O) i -CF2-O-(CX 6 2) e -{O-CF(CF3)} f -(O) g -CZ 1 Z 2 - (t1) (In the formula, X 6 are each independently H, F, or CF3, e is an integer of 0 to 3, f is an integer of 0 to 3, g is 0 or 1, h is 0 or 1, i is 0 or 1, and Z 1 and Z 2 are each independently F or CF3), and in formula (t1), Z 1 and Z 2 More preferably, one is F and the other is CF3. In addition, in the general formula (4), -R a -(CZ 1 Z 2 ) k - is represented by the following formula (t2): -(C=O) h -(O) i-CF2-O-(CX 7 2) e -(O) g -CZ 1 Z 2 - (t2) (In the formula, X 7 are each independently H, F, or CF3, e is an integer of 0 to 3, g is 0 or 1, h is 0 or 1, i is 0 or 1, and Z 1 and Z 2 are each independently F or CF3), and in the formula (t2), Z 1 and Z 2 More preferably, one is F and the other is CF3.

[0361] The compound represented by the general formula (4) is a hydrophilic group (Y 3 ), it is also preferable that the compound has a C—F bond and does not have a C—H bond. That is, in the general formula (4), i , X j , and X k All of the are F and R a is preferably a perfluoroalkylene group having 1 or more carbon atoms, and the perfluoroalkylene group may be either linear or branched, may be either cyclic or noncyclic, and may contain at least one catenary heteroatom. The number of carbon atoms in the perfluoroalkylene group may be 2 to 20, or may be 4 to 18.

[0362] The compound represented by the general formula (4) may be partially fluorinated. That is, the compound represented by the general formula (4) may have a hydrophilic group (Y 3 ), it is also preferred that the alkyl group has at least one hydrogen atom bonded to a carbon atom and at least one fluorine atom bonded to a carbon atom.

[0363] The compound represented by the general formula (4) is also preferably a compound represented by the following formula (4a): CF2=CF-O-Rf 0 -Y 3 (4a) (In the formula, Y3 is a hydrophilic group, and Rf 0 is a perfluorinated divalent linking group which may be linear or branched, cyclic or acyclic in structure, saturated or unsaturated, substituted or unsubstituted, and which optionally contains one or more heteroatoms selected from the group consisting of sulfur, oxygen, and nitrogen.

[0364] The compound represented by the general formula (4) is also preferably a compound represented by the following formula (4b). CH2=CH-O-Rf 0 -Y 3 (4b) (In the formula, Y 3 is a hydrophilic group, and Rf 0 is a perfluorinated divalent linking group defined by formula (4a).

[0365] In the general formula (4), Y 3 In one preferred embodiment, Y is -OSO3M. 3 is -OSO3M, examples of the compound represented by general formula (4) include CF2=CF(OCF2CF2CH2OSO3M), CH2=CH(O(CF2)4CH2OSO3M), CF2=CF(O(CF2)4CH2OSO3M), CF2=CF(OCF2CF(CF3)CH2OSO3M), CF2=CF(OCF2CF(CF3)OCF2CF2CH2OSO3M), CH2=CH(O(CF2)4CH2OSO3M), CF2=CF(OCF2CF2SO2N(CH3)CH2CH2OSO3M), CH2=CH(OCF2CF2CH2OSO3M), CF2=CF(OCF2CF2CF2CF2SO2N(CH3)CH2CH2OSO3M), etc. In the above formula, M is the same as above.

[0366] In the general formula (4), Y 3 Another preferred form is -SO3M. 3When is -SO3M, examples of the compound represented by general formula (4) include CF2=CF(OCF2CF2SO3M), CF2=CF(O(CF2)4SO3M), CF2=CF(OCF2CF(CF3)SO3M), CF2=CF(OCF2CF(CF3)OCF2CF2SO3M), CH2=CH(OCF2CF2SO3M), CF2=CF(OCF2CF(CF3)OCF2CF2CF2CF2SO3M), CH2=CH(O(CF2)4SO3M), CH2=CH(O(CF2)3SO3M), etc. In the above formula, M is the same as above.

[0367] In the general formula (4), Y 3 It is also a preferred form for Y to be -COOM. 3 is -COOM, the compound represented by the general formula (4) is, for example, CF2=CF(OCF2CF2COOM), CF2=CF(OCF2CF2CF2COOM), CF2=CF(O(CF2)5COOM), CF2=CF(OCF2CF(CF3)COOM), CF2=CF(OCF2CF(CF3)O(CF2) n COOM) (n is greater than 1), CH2=CH(OCF2CF2COOM), CH2=CH(O(CF2)4COOM), CH2=CH(O(CF2)3COOM), CF2=CF(OCF2CF2SO2NR'CH2COOM), CF2=CF(O(CF2)4SO2NR'CH2COOM), CF2=CF(OCF2CF(CF3)SO2NR'CH2COOM), CF2=CF(OCF2CF(CF3)OCF2CF2SO2NR'CH2COOM), CH2=CH(OCF2CF2SO2NR'CH2COOM), CF2=CF(OCF2CF(CF3)OCF2CF2CF2CF2SO2NR'CH2COOM), CH2=CH(O(CF2)4SO2NR'CH2COOM), CH2=CH(O(CF2)3SO2NR'CH2COOM). In the above formula, R' is H or C 1-4 is an alkyl group, and M is the same as above.

[0368] In the general formula (4), Y 3 In another preferred embodiment, Y is -OPO3M or -OP(O)(OM)2.3 is -OPO3M or -OP(O)(OM)2, examples of the compound represented by general formula (4) include CF2=CF(OCF2CF2CH2OP(O)(OM)2), CF2=CF(O(CF2)4CH2OP(O)(OM)2), CF2=CF(OCF2CF(CF3)CH2OP(O)(OM)2), CF2=CF(OCF2CF(CF3)OCF2CF2CH2OP(O)(OM)2), CF2=CF(OCF 2CF2SO2N(CH3)CH2CH2OP(O)(OM)2), CF2=CF(OCF2CF2CF2CF2SO2N(CH3)CH2CH2OP(O)(OM)2), CH2=CH(OCF2CF2CH2OP(O)(OM)2, CH2=CH(O(CF2)4CH2OP(O)(OM)2), CH2=CH(O(CF2)3CH2OP(O)(OM)2), etc. In the above formula, M is the same as above.

[0369] In the general formula (4), Y 3 In another preferred embodiment, Y is -PO3M or -P(O)(OM)2. 3 is -PO3M or -P(O)(OM)2, examples of the compound represented by general formula (4) include CF2=CF(OCF2CF2P(O)(OM)2), CF2=CF(O(CF2)4P(O)(OM)2), CF2=CF(OCF2CF(CF3)P(O)(OM)2), CF2=CF(OCF2CF(CF3)OCF2CF2P(O)(OM)2), CH2=CH(OCF2CF2P(O)(OM)2), CH2=CH(O(CF2)4P(O)(OM)2), CH2=CH(O(CF2)3P(O)(OM)2), and the like, where M is the same as above.

[0370] The compound represented by the general formula (4) includes the compound represented by the general formula (5): CX2=CY(-CZ2-O-Rf-Y 3 ) (5) (In the formula, X may be the same or different and is -H or -F; Y is -H, -F, an alkyl group or a fluorine-containing alkyl group; Z may be the same or different and is -H, -F, an alkyl group or a fluorine-containing alkyl group. Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms or a fluorine-containing alkylene group having an ether bond having 2 to 100 carbon atoms. Y 3 is the same as above.) A compound represented by general formula (6): CX2=CY(-O-Rf-Y 3 ) (6) (In the formula, X is the same or different and is -H or -F; Y is -H, -F, an alkyl group or a fluorine-containing alkyl group; Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms or a fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond. Y 3 is the same as above.) and a compound represented by general formula (7): CX2=CY(-Rf-Y 3 ) (7) (In the formula, X is the same or different and is -H or -F; Y is -H, -F, an alkyl group or a fluorine-containing alkyl group; Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms or a fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond. Y 3 is the same as above. The above-mentioned fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond is an alkylene group that does not contain a structure in which an oxygen atom is at the terminal and contains an ether bond between carbon atoms.

[0371] In general formula (5), X is -H or -F. Both X's may be -F, or at least one X may be -H. For example, one X may be -F and the other may be -H, or both X's may be -H.

[0372] In formula (5), Y is -H, -F, an alkyl group or a fluorine-containing alkyl group. The alkyl group is an alkyl group containing no fluorine atom, and may have a carbon number of at least 1. The alkyl group preferably has a carbon number of at most 6, more preferably at most 4, and even more preferably at most 3. The above-mentioned fluorine-containing alkyl group is an alkyl group containing at least one fluorine atom, and the carbon number may be at least 1. The above-mentioned fluorine-containing alkyl group preferably has 6 or less carbon atoms, more preferably 4 or less, and even more preferably 3 or less carbon atoms. The above Y is preferably -H, -F or -CF3, and more preferably -F.

[0373] In formula (5), Z may be the same or different and is -H, -F, an alkyl group or a fluoroalkyl group. The alkyl group is an alkyl group containing no fluorine atom, and may have a carbon number of at least 1. The alkyl group preferably has a carbon number of at most 6, more preferably at most 4, and even more preferably at most 3. The above-mentioned fluorine-containing alkyl group is an alkyl group containing at least one fluorine atom, and the carbon number may be at least 1. The above-mentioned fluorine-containing alkyl group preferably has 6 or less carbon atoms, more preferably 4 or less, and even more preferably 3 or less carbon atoms. The above Z is preferably -H, -F or -CF3, and more preferably -F.

[0374] In the general formula (5), it is preferable that at least one of X, Y, and Z contains a fluorine atom. For example, X may be -H, and Y and Z may be -F.

[0375] In the general formula (5), the above Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms, or a fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond. The number of carbon atoms in the fluorine-containing alkylene group is preferably 2 or more. Also, the number is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less. Examples of the fluorine-containing alkylene group include -CF2-, -CH2CF2-, -CF2CF2-, -CF2CH2-, -CF2CF2CH2-, -CF(CF3)-, -CF(CF3)CF2-, and -CF(CF3)CH2-. The fluorine-containing alkylene group is preferably a perfluoroalkylene group.

[0376] The carbon number of the fluorine-containing alkylene group having an ether bond is preferably 3 or more. The carbon number of the fluorine-containing alkylene group having an ether bond is preferably 60 or less, more preferably 30 or less, and even more preferably 12 or less. Examples of the fluorine-containing alkylene group having an ether bond include a group represented by the following formula: [ka] (In the formula, Z 1 is F or CF3;Z 2 and Z 3 are H or F;Z respectively 4 is H, F, or CF3; p1+q1+r1 is an integer of 1 to 10; s1 is 0 or 1; and t1 is an integer of 0 to 5). Specific examples of the fluorine-containing alkylene group having an ether bond include -CF(CF3)CF2-O-CF(CF3)-, -(CF(CF3)CF2-O) n -CF(CF3)- (wherein n is an integer of 1 to 10), -CF(CF3)CF2-O-CF(CF3)CH2-, -(CF(CF3)CF2-O) n Examples include -CF(CF3)CH2- (wherein n is an integer of 1 to 10), -CH2CF2CF2O-CH2CF2CH2-, -CF2CF2CF2O-CF2CF2-, -CF2CF2CF2O-CF2CF2CH2-, -CF2CF2O-CF2-, -CF2CF2O-CF2CH2-, etc. The fluorine-containing alkylene group having an ether bond is preferably a perfluoroalkylene group.

[0377] In the general formula (5), Y 3 is -COOM, -SO3M or -OSO3M (M is H, a metal atom, NR 7y 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7y are H or an organic group and may be the same or different. Any two of them may be bonded to each other to form a ring. R 7y The organic group in is preferably an alkyl group. R 7y As the 1-10 is preferably an organic group represented by the formula: 1-4 More preferred is an organic group represented by the formula: 1-4 More preferred are alkyl groups of the formula: The metal atom includes alkali metals (Group 1) and alkaline earth metals (Group 2), and is preferably Na, K or Li. M is -H, a metal atom, or NR 7 4 is preferred, and -H, an alkali metal (Group 1), an alkaline earth metal (Group 2) or NR 7 4 is more preferred, -H, -Na, -K, -Li or NH4 is even more preferred, -H, -Na, -K or NH4 is even more preferred, -H, -Na or NH4 is especially preferred, and -H or -NH4 is most preferred. Above Y 3 As the alkyl group, -COOM or -SO3M is preferable, and -COOM is more preferable.

[0378] The compound represented by the general formula (5) is preferably a compound (5a) represented by the general formula (5a). CH2=CF(-CF2-O-Rf-Y 3 ) (5a) (Wherein, Rf and Y 3 is the same as above.)

[0379] Specific examples of the compound represented by the general formula (5a) include compounds represented by the following formula:

[0380] [ka]

[0381] (In the formula, Z 1 is F or CF3;Z 2 and Z 3 are H or F;Z respectively 4 is H, F or CF3; p1+q1+r1 are integers between 0 and 10; s1 is 0 or 1; t1 is an integer between 0 and 5; Y 3 is the same as above, except for Z 3 and Z 4 are both H, then p1+q1+r1+s1 is not 0). More specifically,

[0382] [ka]

[0383] The following are preferred, among which:

[0384] [ka]

[0385] It is preferable that:

[0386] The compound represented by the general formula (5a) is, for example, 3 is preferably -COOM, and particularly preferably at least one selected from the group consisting of CH2=CFCF2OCF(CF3)COOM and CH2=CFCF2OCF(CF3)CF2OCF(CF3)COOM (wherein M is as defined above), and more preferably CH2=CFCF2OCF(CF3)COOM.

[0387] The compound represented by the general formula (5) is preferably a compound (5b) represented by the general formula (5b). CX 2 2 = CFCF2-O-(CF(CF3)CF2O) n5 -CF(CF3)-Y3 (5b) (In the formula, each 2 are the same and represent F or H. n5 represents 0 or an integer of 1 to 10, Y 3 is the same as the above definition.)

[0388] In the above formula (5b), n5 is preferably 0 or an integer of 1 to 5, more preferably 0, 1 or 2, and even more preferably 0 or 1, in terms of the stability of the resulting aqueous dispersion. 3 is preferably -COOM in that it provides suitable water solubility and stability of the aqueous dispersion, and the above M is preferably H or NH4 in that it is less likely to remain as an impurity and improves the heat resistance of the obtained molded article.

[0389] Examples of the compound represented by the above formula (5b) include CH2=CFCF2OCF(CF3)COOM and CH2=CFCF2OCF(CF3)CF2OCF(CF3)COOM (wherein M is as defined above).

[0390] Further, examples of the compound represented by the general formula (5) include a compound represented by the general formula (5c).

[0391] CF2=CFCF2-O-Rf-Y 3 (5c) (Wherein, Rf and Y 3 is the same as above)

[0392] More specifically, [ka] etc.

[0393] In general formula (6), X is -H or -F. Both X's may be -F, or at least one X may be -H. For example, one X may be -F and the other may be -H, or both X's may be -H.

[0394] In formula (6), Y is -H, -F, an alkyl group or a fluorine-containing alkyl group. The alkyl group is an alkyl group containing no fluorine atom, and may have a carbon number of at least 1. The alkyl group preferably has a carbon number of at most 6, more preferably at most 4, and even more preferably at most 3. The above-mentioned fluorine-containing alkyl group is an alkyl group containing at least one fluorine atom, and the carbon number may be at least 1. The above-mentioned fluorine-containing alkyl group preferably has 6 or less carbon atoms, more preferably 4 or less, and even more preferably 3 or less carbon atoms. The above Y is preferably -H, -F or -CF3, and more preferably -F.

[0395] In the general formula (6), it is preferable that at least one of X and Y contains a fluorine atom. For example, X may be -H, and Y and Z may be -F.

[0396] In the general formula (6), the above Rf is a fluorine-containing alkylene group having 1 to 40 carbon atoms, or a fluorine-containing alkylene group having 2 to 100 carbon atoms and an ether bond. The number of carbon atoms in the fluorine-containing alkylene group is preferably 2 or more. The number of carbon atoms in the fluorine-containing alkylene group is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less. Examples of the fluorine-containing alkylene group include -CF2-, -CH2CF2-, -CF2CF2-, -CF2CH2-, -CF2CF2CH2-, -CF(CF3)-, -CF(CF3)CF2-, and -CF(CF3)CH2-. The fluorine-containing alkylene group is preferably a perfluoroalkylene group.

[0397] In the above general formula (6), Y 3 is -COOM, -SO3M or -OSO3M (M is H, a metal atom, NR 7y 4. An imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent, R 7yare H or an organic group and may be the same or different. Any two of them may be bonded to each other to form a ring. R 7y The organic group of R is preferably an alkyl group. 7y As the 1-10 is preferably an organic group represented by the formula: 1-4 More preferred is an organic group represented by the formula: 1-4 More preferred are alkyl groups of the formula: The metal atom includes alkali metals (Group 1) and alkaline earth metals (Group 2), and is preferably Na, K or Li. M is -H, a metal atom, or NR 7 4 is preferred, and -H, an alkali metal (Group 1), an alkaline earth metal (Group 2) or NR 7 4 is more preferred, -H, -Na, -K, -Li or NH4 is even more preferred, -H, -Na, -K or NH4 is even more preferred, -H, -Na or NH4 is especially preferred, and -H or -NH4 is most preferred. Above Y 3 As the alkyl group, -COOM or -SO3M is preferable, and -COOM is more preferable.

[0398] The compound represented by general formula (6) is preferably at least one selected from the group consisting of compounds represented by general formulae (6a), (6b), (6c), (6d) and (6e). CF2=CF-O-(CF2) n1 -Y 3 (6a) (In the formula, n1 represents an integer of 1 to 10, and Y 3 is the same as the above definition.) CF2=CF-O-(CF2C(CF3)F) n2 -Y 3 (6b) (In the formula, n2 represents an integer of 1 to 5; Y 3 is the same as the above definition.) CF2=CF-O-(CFX 1 ) n3 -Y 3 (6c) (In the formula, X 1represents F or CF3, n3 represents an integer of 1 to 10, Y 3 is the same as the above definition.) CF2=CF-O-(CF2CFX 1 O) n4 -(CF2) n6 -Y 3 (6d) (In the formula, n4 represents an integer of 1 to 10, n6 represents an integer of 1 to 3, and Y 3 and X 1 is the same as the above definition.) CF2=CF-O-(CF2CF2CFX 1 O) n5 -CF2CF2CF2-Y 3 (6e) (In the formula, n5 represents an integer of 0 to 10, and Y 3 and X 1 is the same as the above definition.)

[0399] In the formula (6a), n1 is preferably an integer of 5 or less, and more preferably an integer of 2 or less. 3 is preferably -COOM in that it provides suitable water solubility and stability of the aqueous dispersion, and M is preferably H or NH4 in that it is less likely to remain as an impurity and improves the heat resistance of the resulting molded article.

[0400] Examples of the compound represented by the above formula (6a) include CF2=CF-O-CF2COOM, CF2=CF(OCF2CF2COOM), and CF2=CF(OCF2CF2CF2COOM) (wherein M is as defined above).

[0401] In the above formula (6b), n2 is preferably an integer of 3 or less from the viewpoint of the stability of the resulting aqueous dispersion, and Y 3 is preferably -COOM in that it provides suitable water solubility and stability of the aqueous dispersion, and M is preferably H or NH4 in that it is less likely to remain as an impurity and improves the heat resistance of the resulting molded article.

[0402] In the above formula (6c), n3 is preferably an integer of 5 or less in terms of water solubility, and Y 3 is preferably -COOM in terms of obtaining suitable water solubility and stability of the aqueous dispersion, and the above M is preferably H or NH4 in terms of improving dispersion stability.

[0403] In the above formula (6d), the above X 1 is preferably -CF3 from the viewpoint of stability of the aqueous dispersion, n4 is preferably an integer of 5 or less from the viewpoint of water solubility, and Y 3 is preferably -COOM in that it provides suitable water solubility and stability of the aqueous dispersion, and the above M is preferably H or NH4.

[0404] Examples of the compound represented by the above formula (6d) include CF2=CFOCF2CF(CF3)OCF2CF2COOM, CF2=CFOCF2CF(CF3)OCF2COOM, and CF2=CFOCF2CF(CF3)OCF2CF2CF2COOM (wherein M represents H, NH4, or an alkali metal).

[0405] In the general formula (6e), the n5 is preferably an integer of 5 or less in terms of water solubility, and the Y 3 is preferably -COOM in that it provides suitable water solubility and stability of the aqueous dispersion, and the above M is preferably H or NH4.

[0406] An example of the compound represented by general formula (6e) is CF2=CFOCF2CF2CF2COOM (wherein M represents H, NH4 or an alkali metal).

[0407] In general formula (7), Rf is preferably a fluorine-containing alkylene group having a carbon number of 1 to 40. In general formula (7), at least one of X and Y preferably contains a fluorine atom.

[0408] The compound represented by general formula (7) is represented by general formula (7a): CF2=CF-(CF2) n1 -Y 3 (7a) (In the formula, n1 represents an integer of 1 to 10, and Y 3 is as defined above.) and a compound represented by general formula (7b): CF2=CF-(CF2C(CF3)F) n2 -Y 3 (7b) (In the formula, n2 represents an integer of 1 to 5; Y 3 is as defined above. Preferably, at least one compound selected from the group consisting of compounds represented by Above Y 3 is preferably -SO3M or -COOM, where M is H, a metal atom, NR 7y 4. It is preferable that the R is an imidazolium which may have a substituent, a pyridinium which may have a substituent, or a phosphonium which may have a substituent. 7y represents H or an organic group.

[0409] In the formula (7a), n1 is preferably an integer of 5 or less, and more preferably an integer of 2 or less. 3 is preferably -COOM in that it provides suitable water solubility and stability of the aqueous dispersion, and M is preferably H or NH4 in that it is less likely to remain as an impurity and improves the heat resistance of the resulting molded article. An example of the compound represented by the above formula (7a) is CF2=CFCF2COOM (wherein M is as defined above).

[0410] In the above formula (7b), n2 is preferably an integer of 3 or less from the viewpoint of the stability of the resulting aqueous dispersion, and Y 3 is preferably -COOM in that it provides suitable water solubility and stability of the aqueous dispersion, and M is preferably H or NH4 in that it is less likely to remain as an impurity and improves the heat resistance of the resulting molded article.

[0411] The above-mentioned modified monomer preferably includes modified monomer (A), and preferably includes at least one selected from the group consisting of compounds represented by general formula (5a), general formula (5c), general formula (6a), general formula (6b), general formula (6c), and general formula (6d), and more preferably includes a compound represented by general formula (5a) or general formula (5c).

[0412] When the modified monomer (A) is used as the modified monomer, the content of the modified monomer (A) unit is preferably in the range of 0.00001 to 1.0 mass% based on the total polymerized units of PTFE. The lower limit is more preferably 0.0001 mass%, more preferably 0.0005 mass%, even more preferably 0.001 mass%, and even more preferably 0.005 mass%. The upper limit is, in order of preference, 0.90 mass%, 0.50 mass%, 0.40 mass%, 0.30 mass%, 0.20 mass%, 0.15 mass%, 0.10 mass%, 0.08 mass%, 0.05 mass%, and 0.01 mass%.

[0413] In the production method of the present disclosure, the polymerization of TFE is usually carried out at a polymerization temperature of 10 to 150°C and a polymerization pressure of 0.05 to 5 MPaG. For example, the polymerization temperature is more preferably 30°C or higher, and even more preferably 50°C or higher. Also, it is more preferably 120°C or lower, and even more preferably 100°C or lower. Also, the polymerization pressure is more preferably 0.3 MPaG or higher, and even more preferably 0.5 MPaG or higher, and even more preferably 5.0 MPaG or lower, and even more preferably 3.0 MPaG or lower. In particular, from the viewpoint of improving the yield of PTFE, it is preferably 1.0 MPaG or higher, more preferably 1.2 MPaG or higher, even more preferably 1.5 MPaG or higher, and even more preferably 2.0 MPaG or higher.

[0414] In one embodiment, the polymerization is carried out by charging pure water into a pressure-resistant reaction vessel equipped with a stirrer, deoxidizing, charging TFE, adjusting the temperature to a predetermined temperature, and adding a polymerization initiator to start the reaction. If the pressure decreases as the reaction proceeds, additional TFE is continuously or intermittently supplied to maintain the initial pressure. When a predetermined amount of TFE has been supplied, the supply is stopped, the TFE in the reaction vessel is purged, and the temperature is returned to room temperature to terminate the reaction. Additional TFE may be continuously or intermittently supplied to prevent the pressure from decreasing.

[0415] In the production of PTFE, the polymer (I) can be used within the range of use in the production method of the present disclosure described above. The concentration of the polymer (I) is not particularly limited as long as it is within the above range. If the amount added is too large, needle-shaped particles with a large aspect ratio are generated, and the aqueous dispersion becomes gel-like and loses stability. The lower limit of the amount of the polymer (I) used is preferably 0.0001% by mass, more preferably 0.001% by mass, even more preferably 0.01% by mass, and particularly preferably 0.02% by mass, based on the aqueous medium. The upper limit of the amount of the polymer (I) used is preferably 10% by mass, more preferably 5% by mass, based on the aqueous medium.

[0416] The polymer (I) may be added to a reaction vessel all at once before the initiation of polymerization, may be added all at once after the initiation of polymerization, may be added in several divided portions during polymerization, or may be added continuously during polymerization.

[0417] In the production of PTFE, as the polymerization initiator, persulfates (e.g., ammonium persulfate), and organic peroxides such as disuccinic acid peroxide and diglutaric acid peroxide can be used alone or in the form of a mixture thereof. They may also be used in combination with a reducing agent such as sodium sulfite to form a redox system. Furthermore, during polymerization, a radical scavenger such as hydroquinone or catechol, or a peroxide decomposer such as ammonium sulfite, can be added to adjust the radical concentration in the system.

[0418] As the redox polymerization initiator, it is preferable to use a redox initiator that combines an oxidizing agent and a reducing agent. Examples of the oxidizing agent include persulfates, organic peroxides, potassium permanganate, manganese triacetate, and cerium ammonium nitrate. Examples of the reducing agent include sulfites, bisulfites, bromates, diimines, and oxalic acid. Examples of the persulfates include ammonium persulfate and potassium persulfate. Examples of the sulfites include sodium sulfite and ammonium sulfite. In order to increase the decomposition rate of the initiator, it is also preferable to add a copper salt or an iron salt to the combination of the redox initiator. Examples of the copper salt include copper(II) sulfate, and examples of the iron salt include iron(II) sulfate.

[0419] Examples of the redox initiator include potassium permanganate / oxalic acid, potassium permanganate / ammonium oxalate, ammonium persulfate / bisulfite / iron sulfate, manganese triacetate / oxalic acid, cerium ammonium nitrate / oxalic acid, bromate / bisulfite, and the like, with potassium permanganate / oxalic acid being preferred. When using a redox initiator, either an oxidizing agent or a reducing agent may be charged in advance into a polymerization tank, and then the other may be added continuously or intermittently to initiate polymerization. For example, when potassium permanganate / oxalic acid is used, it is preferred to charge oxalic acid into a polymerization tank and continuously add potassium permanganate thereto.

[0420] In the production of PTFE, known chain transfer agents can be used, for example, saturated hydrocarbons such as methane, ethane, propane, butane, etc.; halogenated hydrocarbons such as chloromethane, dichloromethane, difluoroethane, etc.; alcohols such as methanol, ethanol, isopropanol, etc.; and hydrogen, etc., but those that are in a gaseous state at normal temperature and pressure are preferred.

[0421] The amount of the chain transfer agent used is usually 1 to 10,000 ppm by mass, and preferably 1 to 5,000 ppm by mass, based on the total amount of TFE supplied.

[0422] In the production of PTFE, a saturated hydrocarbon having 12 or more carbon atoms, which is substantially inert to the reaction and becomes liquid under the above reaction conditions, may be used as a dispersion stabilizer for the reaction system in an amount of 2 to 10 parts by mass per 100 parts by mass of the aqueous medium. In addition, ammonium carbonate, ammonium phosphate, etc. may be added as a buffer for adjusting the pH during the reaction.

[0423] When the polymerization of TFE is completed, a polymer dispersion having a solid content of 1.0 to 50% by mass and an average primary particle size of 50 to 500 nm can be obtained.

[0424] The lower limit of the solid content concentration is preferably 5% by mass, more preferably 8% by mass, and the upper limit is not particularly limited, but may be 40% by mass or 35% by mass.

[0425] The lower limit of the average primary particle size is preferably 100 nm, more preferably 150 nm, and the upper limit is preferably 400 nm, more preferably 350 nm.

[0426] The average primary particle size can be measured by dynamic light scattering. The average primary particle size can be measured by preparing an aqueous dispersion adjusted to a solid content concentration of about 1.0 mass%, using dynamic light scattering at 25°C, with a refractive index of the solvent (water) of 1.3328 and a viscosity of the solvent (water) of 0.8878 mPa·s, and accumulating 70 times. For the dynamic light scattering, for example, ELSZ-1000S (manufactured by Otsuka Electronics Co., Ltd.) can be used.

[0427] The average primary particle diameter can also be measured by the following method. The dispersion is diluted with water until the solid content becomes 0.15% by mass, and the transmittance of 550 nm projected light per unit length of the diluted latex obtained and the number-based average particle diameter determined by measuring the unidirectional diameter using a transmission electron microscope photograph are measured to create a calibration curve. Using this calibration curve, the average particle diameter can be calculated from the measured transmittance of 550 nm projected light for each sample.

[0428] (Polytetrafluoroethylene (PTFE) In the first manufacturing method, the PTFE in the polymer dispersion obtained as described above is brought into contact with an organic solvent and a coagulant to coagulate the PTFE, and the coagulated material obtained is washed and dried as desired to obtain a PTFE powder. In the second manufacturing method, the PTFE in the polymer dispersion obtained as described above is brought into contact with an organic solvent to coagulate the PTFE, and the coagulated material is washed and dried to obtain a PTFE powder. The PTFE powder may be what is called a "fine powder".

[0429] According to the manufacturing method of the present disclosure, it is possible to manufacture PTFE powder having a relatively large average secondary particle size. The average secondary particle size of PTFE is 200 to 1000 μm, more preferably 250 μm or more, more preferably 900 μm or less, even more preferably 800 μm or less, and even more preferably 700 μm or less. The average secondary particle size of PTFE is the mass-based average particle size (50% cumulative particle size) d50, and can be determined by measurement in accordance with JIS K6891.

[0430] By using the manufacturing method of the present disclosure, it is possible to obtain PTFE with an appropriately adjusted secondary particle size. The mechanism by which the secondary particle size is adjusted is not clear, but is thought to be as follows.

[0431] In the first manufacturing method, the polymer (I) can be removed by using an organic solvent during coagulation, but the presence of the organic solvent on the particle surface allows the aggregated particles formed by the aggregation of primary particles to exist stably in water. In addition, the aggregated particles formed by the aggregation of primary particles during the coagulation process have a weak coagulation force, and the secondary particle size obtained by coagulation and washing is small. Therefore, by adding a coagulant, the coagulation force of the aggregated particles formed by the aggregation of primary particles can be strengthened, and a PTFE powder having the desired secondary particle size can be obtained.

[0432] In the second manufacturing method, the organic solvent is added to the primary particles obtained in the aggregating step, and the aggregated particles have the organic solvent unevenly distributed on the surface of the aggregated particles. The organic solvent can be easily removed by increasing the temperature in the washing step. At this time, a high temperature increases the speed at which the organic solvent is removed from the aggregated particles, and the aggregated particles can further aggregate with each other to form larger particles than when the particle surfaces are wetted with washing water to stabilize them, and a PTFE powder with the desired secondary particle size can be obtained.

[0433] The PTFE preferably has an ion exchange ratio (IXR) greater than 53. Preferred PTFE has no ionizable groups or a limited number of ionizable groups resulting in an ion exchange ratio greater than about 100. The ion exchange ratio of the preferred PTFE is preferably 1000 or greater, more preferably 2000 or greater, and even more preferably 5000 or greater.

[0434] PTFE may have a core-shell structure. For example, modified PTFE having a core of high molecular weight PTFE and a shell of lower molecular weight PTFE or modified PTFE in a particle can be mentioned. For example, modified PTFE described in JP-A-2005-527652 can be mentioned.

[0435] The above core-shell structure may have the following structure. Core: TFE homopolymer Shell: TFE homopolymer Core: Modified PTFE Shell: TFE homopolymer Core: Modified PTFE Shell: Modified PTFE Core: TFE homopolymer Shell: Modified PTFE Core: Low molecular weight PTFE Shell: High molecular weight PTFE Core: High molecular weight PTFE Shell: Low molecular weight PTFE

[0436] In the PTFE having the core-shell structure, the lower limit of the core ratio is preferably 0.5% by mass, more preferably 1.0% by mass, even more preferably 2.0% by mass, even more preferably 3.0% by mass, particularly preferably 5.0% by mass, and most preferably 10.0% by mass. The upper limit of the core ratio is preferably 99.5% by mass, more preferably 99.0% by mass, even more preferably 98.0% by mass, even more preferably 97.0% by mass, particularly preferably 95.0% by mass, and most preferably 90.0% by mass.

[0437] In the PTFE having the core-shell structure, the lower limit of the shell ratio is preferably 0.5% by mass, more preferably 1.0% by mass, even more preferably 2.0% by mass, even more preferably 3.0% by mass, particularly preferably 5.0% by mass, and most preferably 10.0% by mass. The upper limit of the shell ratio is preferably 99.5% by mass, more preferably 99.0% by mass, even more preferably 98.0% by mass, even more preferably 97.0% by mass, particularly preferably 95.0% by mass, and most preferably 90.0% by mass.

[0438] In the PTFE having the core-shell structure, the core or the shell may be configured to have two or more layers. For example, the PTFE may have a three-layer structure having a core center portion of modified PTFE, a core outer layer portion of TFE homopolymer, and a shell of modified PTFE.

[0439] The PTFE having the core-shell structure also includes PTFE particles each having multiple cores.

[0440] By adding pigments for coloring or various fillers for improving mechanical properties before or during the coagulation, it is possible to obtain a pigmented or filled PTFE fine powder in which the pigments and fillers are uniformly mixed.

[0441] The drying of the coagulated material obtained by coagulating the aqueous dispersion of PTFE is usually carried out by using means such as vacuum, high frequency, hot air, etc., while keeping the coagulated material in a state where it is not very fluid, preferably in a state where it is left stationary. The friction between powders, especially at high temperatures, generally has an undesirable effect on fine powder-type PTFE. This is because the particles made of this type of PTFE have the property of easily fibrillating even with small shearing force, and losing the original stable particle structure state.

[0442] The drying is carried out at a drying temperature of 10 to 300°C, preferably 100 to 300°C.

[0443] The obtained PTFE fine powder is preferable for molding, and suitable applications include hydraulic and fuel system tubes for aircraft and automobiles, flexible hoses for chemical solutions, steam, etc., and wire coating applications.

[0444] The PTFE fine powder is also preferably used as a processing aid. When used as a processing aid, the fine powder can be mixed with a host polymer or the like to improve the melt strength during melt processing of the host polymer, and the mechanical strength, electrical properties, flame retardancy, drip prevention during combustion, and sliding properties of the resulting polymer.

[0445] The PTFE fine powder is also preferably used as a binder for batteries and for dust prevention purposes.

[0446] It is also preferable to use the PTFE fine powder as a processing aid after compounding it with a resin other than PTFE. The fine powder is suitable as a raw material for PTFE, for example, as described in JP-A-11-49912, U.S. Pat. No. 5,804,654, JP-A-11-29679, and JP-A-2003-2980. The processing aid using the fine powder is in no way inferior to the processing aids described in the above publications.

[0447] The high molecular weight PTFE powder obtained by polymerization has extensibility and non-melt processability, and is also useful as a raw material for extensible bodies (porous bodies). When this stretched body is a membrane (PTFE stretched membrane or PTFE porous membrane), it can be stretched by a known PTFE stretching method. By stretching, the high molecular weight PTFE is easily fibrillated, and becomes a PTFE porous body (membrane) consisting of nodes and fibers. Preferably, a sheet-like or rod-like paste extrudate is roll-stretched in the extrusion direction to obtain a uniaxially stretched membrane. Furthermore, a biaxially stretched film can also be obtained by stretching the film in the width direction using a tenter or the like. It is also preferable to carry out a semi-baking treatment before stretching.

[0448] This expanded PTFE body is a porous body having a high porosity, and can be suitably used as a filter medium for various precision filters such as air filters and chemical filters, a support material for polymer electrolyte membranes, and the like. They are also useful as materials for products used in the fields of textiles, medicine, electrochemicals, sealing materials, air filtration, ventilation / internal pressure regulation, liquid filtration, and general consumer goods. Specific applications are given below as examples.

[0449] Electrochemical Field Dielectric material prepreg, EMI shielding material, heat transfer material, etc. More specifically, printed wiring board, electromagnetic shielding material, insulating heat transfer material, insulating material, etc. Sealing materials field Gaskets, packing, pump diaphragms, pump tubes, aircraft sealing materials, etc.

[0450] Air Filtration Field ULPA filters (for semiconductor manufacturing), HEPA filters (for hospitals and semiconductor manufacturing), cylindrical cartridge filters (for industrial use), bag filters (for industrial use), heat-resistant bag filters (for exhaust gas treatment), heat-resistant pleated filters (for exhaust gas treatment), SINBRAN filters (for industrial use), catalyst filters (for exhaust gas treatment), adsorbent filters (for HDD installation), adsorbent vent filters (for HDD installation), vent filters (for HDD installation and others), vacuum cleaner filters (for vacuum cleaners), general-purpose multi-layer felt material, GT cartridge filters (for GT compatible products), cooling filters (for electronic device housings), etc.

[0451] Ventilation / internal pressure regulation field Freeze-drying materials such as freeze-drying containers, automotive ventilation materials for electronic circuits and lamps, container applications such as container caps, protective ventilation applications for electronic devices including small terminals such as tablet terminals and mobile phones, medical ventilation applications, etc.

[0452] Liquid Filtration Semiconductor liquid filtration filters (for semiconductor manufacturing), hydrophilic PTFE filters (for semiconductor manufacturing), chemical filters (for chemical liquid treatment), pure water production line filters (for pure water production), backwash type liquid filtration filters (for industrial wastewater treatment), etc.

[0453] General consumer goods field Clothing, cable guides (movable wires for motorcycles), motorcycle clothing, cast liners (medical supporters), vacuum cleaner filters, bagpipes (musical instruments), cables (signal cables for guitars, etc.), strings (for stringed instruments), etc.

[0454] Textiles PTFE fiber (textile material), sewing thread (textile), weaving thread (textile), rope, etc.

[0455] Medical field Internal implants (extended products), artificial blood vessels, catheters, general surgery (tissue reinforcement materials), head and neck products (dura substitutes), oral health (tissue regenerative medicine), orthopedics (bandages), etc.

[0456] The manufacturing method of the present disclosure also allows the production of low molecular weight PTFE. The low molecular weight PTFE may be produced by polymerization, or it may be produced by lowering the molecular weight of the high molecular weight PTFE obtained by polymerization by a known method (thermal decomposition, decomposition by irradiation, etc.).

[0457] Low-molecular-weight PTFE (also called PTFE micropowder) having a molecular weight of 600,000 or less has excellent chemical stability, extremely low surface energy, and is not prone to fibrillation. Therefore, it is suitable as an additive for improving the slipperiness and texture of coating surfaces in the production of plastics, inks, cosmetics, paints, greases, office automation equipment components, toners, and the like (see, for example, JP-A-10-147617).

[0458] Further, in the presence of a chain transfer agent, a polymerization initiator and a polymer (I) may be dispersed in an aqueous medium, and TFE or a monomer copolymerizable with TFE and TFE may be polymerized to obtain a low molecular weight PTFE. In this case, the chain transfer agent is preferably at least one selected from the group consisting of alkanes having 2 to 4 carbon atoms. Specifically, methane, ethane, propane, butane, and isobutane are more preferable, and ethane and propane are even more preferable. In this case, the amount of the chain transfer agent is preferably 10 mass ppm or more or more than 10 mass ppm relative to the aqueous medium.

[0459] When the low-molecular-weight PTFE obtained by the above polymerization is used as a powder, the above aqueous dispersion can be coagulated to form powder particles.

[0460] In the present disclosure, high molecular weight PTFE refers to non-melt processable and fibrillating PTFE, whereas low molecular weight PTFE refers to melt processable and non-fibrillating PTFE.

[0461] The term "non-melt processable" means that the melt flow rate cannot be measured at a temperature higher than the crystallization melting point according to ASTM D 1238 and D 2116.

[0462] The presence or absence of fibrillation properties can be judged by "paste extrusion," a typical method for molding "high molecular weight PTFE powder," a powder made from a TFE polymer. Paste extrusion is usually possible because high molecular weight PTFE has fibrillation properties. If the unsintered molded product obtained by paste extrusion has no substantial strength or elongation, for example, if it breaks when pulled with an elongation of 0%, it can be considered to have no fibrillation properties.

[0463] The high molecular weight PTFE preferably has a standard specific gravity (SSG) of 2.130 to 2.280. The standard specific gravity is measured by a water displacement method in accordance with ASTM D 792 using a sample molded in accordance with ASTM D4895-89. In the present disclosure, "high molecular weight" means that the standard specific gravity is within the above range.

[0464] The above low molecular weight PTFE has a melt viscosity of 1×10 at 380°C. 2 ~7×10 5 In the present disclosure, "low molecular weight" means that the melt viscosity is within the above range. The melt viscosity is measured in accordance with ASTM D 1238 using a flow tester (manufactured by Shimadzu Corporation) and a 2φ-8L die, with a 2g sample preheated at 380°C for 5 minutes, and maintained at the above temperature under a load of 0.7 MPa.

[0465] The high molecular weight PTFE has a melt viscosity much higher than that of the low molecular weight PTFE, and it is difficult to measure the melt viscosity accurately. On the other hand, although the melt viscosity of the low molecular weight PTFE can be measured, it is difficult to obtain a molded product that can be used to measure the standard specific gravity from the low molecular weight PTFE, and it is difficult to measure the standard specific gravity accurately. Therefore, in this disclosure, the standard specific gravity is adopted as an index of the molecular weight of the high molecular weight PTFE, and the melt viscosity is adopted as an index of the molecular weight of the low molecular weight PTFE. Note that there is no known measurement method that can directly specify the molecular weight of either the high molecular weight PTFE or the low molecular weight PTFE.

[0466] The high molecular weight PTFE preferably has a peak temperature of 333 to 347° C., more preferably 335 to 345° C. The low molecular weight PTFE preferably has a peak temperature of 322 to 333° C., more preferably 324 to 332° C. The peak temperature can be specified as the temperature corresponding to the maximum value appearing on a differential thermal (DTA) curve obtained by heating PTFE that has no history of being heated to a temperature of 300° C. or higher at a rate of 10° C. / min using a TG / DTA (thermogravimetric / differential thermal analyzer).

[0467] The peak temperature of the PTFE may be from 322 to 347°C. When the PTFE is a high molecular weight PTFE, the upper limit of the peak temperature of the PTFE may be 347°C or less, 346°C or less, 345°C or less, 344°C or less, 343°C or less, 342°C or less, 341°C or less, or 340°C or less. When the PTFE is a high molecular weight PTFE, the lower limit of the peak temperature of the PTFE may be 333° C. or higher, or 335° C. or higher. When the PTFE is a low molecular weight PTFE, the upper limit of the peak temperature of the PTFE may be 333° C. or less, or 332° C. or less. When the PTFE is a low-molecular-weight PTFE, the lower limit of the peak temperature of the PTFE may be 322° C. or higher, or 324° C. or higher.

[0468] The average primary particle diameter of the low-molecular-weight PTFE primary particles is preferably 10 to 300 nm, more preferably 50 nm or more, more preferably 100 nm or more, further preferably 150 nm or more, and more preferably 250 nm or less. A relatively small average primary particle diameter of the primary particles can be obtained, for example, by adding a modified monomer to the polymerization system at the initial stage of TFE polymerization.

[0469] The average primary particle size of the primary particles of low molecular weight PTFE can be measured by dynamic light scattering. First, a low molecular weight PTFE aqueous dispersion with a polymer solid concentration adjusted to about 1.0 mass% is prepared, and the average primary particle size can be measured using dynamic light scattering at a measurement temperature of 25°C, a refractive index of the solvent (water) of 1.3328, a viscosity of the solvent (water) of 0.8878 mPa·s, and an accumulation number of 70 times. For example, an ELSZ-1000S (manufactured by Otsuka Electronics Co., Ltd.) can be used for the dynamic light scattering method.

[0470] The high molecular weight PTFE preferably has at least one endothermic peak in the range of 333 to 347°C in a heat of fusion curve obtained by heating PTFE that has not been heated to a temperature of 300°C or higher at a rate of 10°C / min using a differential scanning calorimeter (DSC), and has a heat of fusion of 52mJ / mg or more at 290 to 350°C calculated from the heat of fusion curve. The heat of fusion of PTFE is more preferably 55mJ / mg or more, and even more preferably 58mJ / mg or more.

[0471] An unsintered tape (green tape) can also be obtained from the PTFE fine powder obtained above.

[0472] In the manufacturing method of the present disclosure, when PTFE is coagulated, washed, dried, etc., wastewater and off-gas are generated. The polymer (I), decomposition products and by-products of the polymer (I) produced as by-products from the polymer (I), residual monomers, etc. may be recovered and purified from the wastewater generated by the coagulation or washing and / or the off-gas generated by drying, thereby reusing the polymer (I), decomposition products and by-products of the polymer (I) produced as by-products from the polymer (I), residual monomers, etc. The method for the recovery and purification is not particularly limited, but can be performed by a known method. For example, the method described in JP-T-2011-520020, the method described in U.S. Patent Application Publication No. 2007 / 15937, U.S. Patent Application Publication No. 2007 / 25902, and U.S. Patent Application Publication No. 2007 / 27251, and specifically, the following method may be used.

[0473] Examples of a method for recovering the polymer (I), decomposition products and by-products of the polymer (I), residual monomers, etc., from the wastewater include a method in which the wastewater is contacted with adsorption particles such as ion exchange resin, activated carbon, silica gel, clay, zeolite, etc., to adsorb the polymer (I), etc., and then the wastewater is separated from the adsorption particles. If the adsorption particles having the polymer (I) etc. adsorbed thereon are incinerated, the release of the polymer (I) etc. into the environment can be prevented.

[0474] The polymer (I) and the like can also be recovered by desorbing and eluting the polymer (I) and the like from ion exchange resin particles adsorbing the polymer (I) and the like by a known method. For example, when the ion exchange resin particles are anion exchange resin particles, the polymer (I) and the like can be eluted by contacting a mineral acid with the anion exchange resin. When a water-soluble organic solvent is subsequently added to the resulting eluate, the mixture is usually separated into two phases, and the lower phase containing the polymer (I) and the like is recovered and neutralized to recover the polymer (I) and the like. Examples of the water-soluble organic solvent include polar solvents such as alcohols, ketones, and ethers.

[0475] Other methods for recovering the polymer (I) from the ion-exchange resin particles include a method using an ammonium salt and a water-soluble organic solvent, and a method using an alcohol and, if desired, an acid. In the latter method, an ester derivative of the polymer (I) is produced, which can be easily separated from the alcohol by distillation.

[0476] When the wastewater contains PTFE particles and other solids, it is preferable to remove them before contacting the wastewater with the adsorption particles. Methods for removing PTFE particles and other solids include a method of precipitating them by adding aluminum salts or the like, and then separating the wastewater from the precipitate, and an electrocoagulation method. Mechanical methods may also be used for removal, such as cross-flow filtration, deep bed filtration, and precoat filtration. The concentration of unaggregated PTFE in the wastewater is preferably low from the viewpoint of productivity, more preferably less than 0.4 mass %, particularly preferably less than 0.3 mass %.

[0477] As a method for recovering the polymer (I) and the like from the off-gas, there is a method using a scrubber to contact the off-gas with deionized water, an aqueous alkali solution, an organic solvent such as a glycol ether solvent, etc., to obtain a scrubber solution containing the polymer (I) and the like. When a high-concentration aqueous alkali solution is used as the aqueous alkali solution, the scrubber solution can be recovered in a state in which the polymer (I) and the like are phase-separated, so that recovery and reuse of the polymer (I) and the like can be easily achieved. Examples of the alkaline compound include alkali metal hydroxides and quaternary ammonium salts.

[0478] The scrubber solution containing the polymer (I) and the like may be concentrated using a reverse osmosis membrane or the like. The concentrated scrubber solution usually contains fluorine ions, but by further adding alumina after concentration to remove the fluorine ions, it is possible to facilitate the reuse of the polymer (I) and the like. Alternatively, the scrubber solution may be brought into contact with adsorbent particles to adsorb the polymer (I) and the like, and the polymer (I) and the like may be recovered by the above-mentioned method.

[0479] The polymer (I) and the like recovered by any of the above methods can be reused.

[0480] (Polytetrafluoroethylene (PTFE)-containing composition) According to the present disclosure, there is provided a composition comprising a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I) and PTFE, in which the content of the polymer (I) is 0.23 mass% or less based on the PTFE, and the average secondary particle size of the PTFE is 200 to 1000 μm. CX 1 X 3 =CX 2 R(-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF; X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more.

[0481] Since the composition of the present disclosure has a reduced content of polymer (I), the properties of a molded article obtained using the composition are not affected by the presence of polymer (I). Therefore, a molded article having excellent properties can be obtained from the composition.

[0482] The PTFE contained in the composition is preferably a non-melt-processible PTFE, as described above.

[0483] The standard specific gravity of the PTFE contained in the composition is preferably 2.210 or less, more preferably 2.200 or less, and even more preferably 2.190 or less.

[0484] The content of the polymer (I) in the composition is 0.23% by mass or less, preferably 0.20% by mass or less, more preferably 0.15% by mass or less, based on PTFE. The content of the polymer (I) in the composition is preferably 0.0001% by mass or more, more preferably 0.001% by mass or more, and even more preferably 0.01% by mass or more, based on PTFE.

[0485] The content of polymer (I) in the composition can be determined by the same method as that for the content of polymer (I) in the polymer dispersion.

[0486] Furthermore, the composition of the present disclosure is characterized in that it contains PTFE having an average secondary particle diameter of 200 to 1000 μm. When the average secondary particle diameter of PTFE is within the above range, the handleability of the composition is improved.

[0487] The average secondary particle diameter of PTFE is preferably 250 μm or more, preferably 900 μm, more preferably 800 μm or less, and even more preferably 700 μm or less. The larger the average secondary particle diameter, the lower the fluctuation rate of the extrusion pressure when extruding PTFE from an extruder using a paste extrusion molding method. The average secondary particle diameter of PTFE may be 350 μm or more, 400 μm or more, more than 400 μm, 430 μm or more, or 450 μm or more. A relatively large average secondary particle diameter is particularly suitable as the average secondary particle diameter of non-melt-processable PTFE (high molecular weight PTFE).

[0488] The average secondary particle size is different from the average particle size of the primary particles dispersed in the aqueous dispersion (average primary particle size), and is the average particle size of the secondary particles formed by aggregation of the primary particles. The composition of the present disclosure may be an aggregate (powder) of the secondary particles formed by aggregation of the primary particles.

[0489] The average secondary particle diameter of PTFE is the mass-based average particle diameter (50% cumulative particle diameter) d50, and can be determined by measurement in accordance with JIS K6891.

[0490] The average secondary particle size of PTFE can be adjusted, for example, by adjusting the amount of organic solvent used to coagulate PTFE, by adjusting the amount of coagulant used to coagulate PTFE, by adjusting the timing of adding organic solvent and coagulant to the polymerization dispersion when coagulating PTFE, and by adjusting the washing temperature when washing the coagulated product.For example, the composition of the present disclosure can be produced by the production method of the present disclosure.

[0491] In one embodiment of the composition of the present disclosure, a fluorine-containing surfactant is contained. The composition containing a fluorine-containing surfactant has an advantage that it can be produced stably with high productivity using the fluorine-containing surfactant.

[0492] In one embodiment of the composition of the present disclosure, it is substantially free of a fluorine-containing surfactant.

[0493] In the present disclosure, "substantially free of fluorinated surfactant" means that the content of fluorinated surfactant in the composition is 10 ppm by mass or less, preferably 1 ppm by mass or less, more preferably 100 ppb by mass or less, even more preferably 10 ppb by mass or less, still more preferably 1 ppb by mass or less, and particularly preferably below the detection limit of the fluorinated surfactant as measured by liquid chromatography-mass spectrometry (LC / MS).

[0494] The content of the fluorine-containing surfactant can be quantified by a known method, for example, by LC / MS analysis. First, methanol is added to the composition to perform extraction, and the resulting extract is analyzed by LC / MS. To further increase the extraction efficiency, treatments such as Soxhlet extraction and ultrasonic treatment may be performed. Molecular weight information is extracted from the obtained LC / MS spectrum, and a match with the structural formula of the candidate fluorine-containing surfactant is confirmed. Then, aqueous solutions containing five or more levels of the confirmed fluorine-containing surfactant are prepared, and LC / MS analysis is performed on the aqueous solutions containing each level. The relationship between the content and the area for each content is plotted, and a calibration curve is drawn. Then, using the calibration curve, the area of ​​the LC / MS chromatogram of the fluorine-containing surfactant in the extract can be converted into the content of the fluorine-containing surfactant.

[0495] The form of the composition of the present disclosure is not particularly limited, and may be, for example, an aqueous dispersion, a coagulant, a dried product, a gum, a crumb, a powder, a pellet, or the like. The form of the composition of the present disclosure is preferably a powder. The aqueous dispersion is a dispersion system in which an aqueous medium is a dispersion medium and PTFE is a dispersoid. The aqueous medium is not particularly limited as long as it is a liquid containing water, and may contain, in addition to water, an organic solvent such as alcohol, ether, ketone, or paraffin wax.

[0496] The aqueous dispersion may be one in which a powder made of PTFE is dispersed in an aqueous medium. The composition of the present disclosure is preferably a powder.

[0497] The composition of the present disclosure may contain known compounding agents such as pigments, thickeners, dispersants, defoamers, antifreeze agents, film-forming assistants, and other polymer compounds.

[0498] The composition of the present disclosure can be suitably produced by the production method of the present disclosure.

[0499] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims.

[0500] <1> According to a first aspect of the present disclosure, A method for producing a composition containing polytetrafluoroethylene, comprising the steps of: A polymerization dispersion containing polytetrafluoroethylene is obtained by polymerizing tetrafluoroethylene in an aqueous medium in the presence of a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I), The polytetrafluoroethylene in the polymerization dispersion is coagulated by contacting the polytetrafluoroethylene in the polymerization dispersion with an organic solvent and a coagulant to obtain a composition containing polytetrafluoroethylene. A manufacturing method is provided. (In the present disclosure, this may be referred to as a first manufacturing method.) CX 1 X 3 =CX 2 R(-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF; X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more. <2> According to a second aspect of the present disclosure, In the first aspect, there is provided a process wherein the organic solvent is an alcohol having 1 to 7 carbon atoms. <3> According to a third aspect of the present disclosure, The process according to the first or second aspect provides a process in which the organic solvent is an alcohol having 2 to 7 carbon atoms. <4> According to a fourth aspect of the present disclosure, There is provided a production method according to any one of the first to third aspects, wherein the amount of the organic solvent used for coagulation is 1.0 mass % or more and 150 mass % or less based on the polytetrafluoroethylene in the polymerization dispersion. <5> According to a fifth aspect of the present disclosure, There is provided a production method according to any one of the first to fourth aspects, wherein the coagulant is at least one selected from the group consisting of ammonium carbonate, ammonium hydrogen carbonate, ammonia and urea. <6> According to a sixth aspect of the present disclosure, There is provided a production method according to any one of the first to fifth aspects, wherein the amount of the coagulant used for coagulation is 0.01% by mass or more and 5.0% by mass or less with respect to the polytetrafluoroethylene in the polymer dispersion. <7> According to a seventh aspect of the present disclosure, There is provided a production method according to any one of the first to sixth aspects, wherein the temperature when the polytetrafluoroethylene in the polymer dispersion, the organic solvent and the coagulant are brought into contact with each other is 5 to 80°C. <8> According to an eighth aspect of the present disclosure, There is provided a production method according to any one of the first to seventh aspects, in which the polytetrafluoroethylene in the polymer dispersion is coagulated to obtain a coagulate, and then the coagulate is washed to obtain the composition. <9> According to a ninth aspect of the present disclosure, A composition is provided which contains a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I) and polytetrafluoroethylene, in which the content of polymer (I) is 0.23 mass% or less based on the polytetrafluoroethylene, and the average secondary particle size of the polytetrafluoroethylene is 200 to 1000 μm. CX 1 X 3 =CX 2 R(-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF; X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more. <10> According to a tenth aspect of the present disclosure, There is provided a composition according to a ninth aspect which is substantially free of a fluorine-containing surfactant. <11> According to an eleventh aspect of the present disclosure, A method for producing a composition containing polytetrafluoroethylene, comprising the steps of: A polymerization dispersion containing polytetrafluoroethylene is obtained by polymerizing tetrafluoroethylene in an aqueous medium in the presence of a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I), The polytetrafluoroethylene in the polymerization dispersion is coagulated by contacting the polytetrafluoroethylene in the polymerization dispersion with an organic solvent to obtain a coagulated product, and then the coagulated product is washed at 20° C. or higher to obtain a composition containing polytetrafluoroethylene. A manufacturing method is provided. (In the present disclosure, this may be referred to as a second manufacturing method.) CX 1X 3 = CX 2 R( - CZ 1 Z 2 - A 0 ) m (I) (wherein X 1 and X 3 are each independently F, Cl, H or CF3; X 2 is H, F, an alkyl group or a fluorinated alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorinated alkyl group; m is an integer of 1 or more.)

Example

[0501] Next, experimental examples will be given to explain the embodiments of the present disclosure, but the present disclosure is not limited to such experimental examples only.

[0502] Each numerical value in the experimental examples was measured by the following method.

[0503] <Solid content concentration of PTFE polymerization dispersion liquid> 1 g of the polymerization dispersion liquid was dried in a blower dryer at 150 °C for 60 minutes, and the value representing the ratio of the mass of the heat residue to the mass of the polymerization dispersion liquid (1 g) as a percentage was adopted.

[0504] <Content of polymer D in PTFE powder> The content of polymer D contained in the PTFE powder was determined by obtaining the correlation between solid 19 F - MAS NMR measurement and Fourier transform infrared spectroscopic analysis, and was determined by a Fourier transform infrared spectroscopic analyzer.

[0505] <Solid content concentration in condensate drainage> After condensing PTFE in the polymerization dispersion liquid, the condensate (wet powder) was recovered from the polymerization dispersion liquid by filtration. 10 g of the filtrated condensate drainage was dried in a hot air dryer at 120 °C for 60 minutes, and the value obtained by expressing the ratio of the mass of the heat residue to the mass of the condensate drainage (10 g) as a percentage was adopted as the solid content concentration (mass%) in the condensate drainage. The lower the solid content concentration (mass%), the higher the proportion of PTFE recovered in the polymerization dispersion liquid.

[0506] <Average secondary particle diameter of PTFE> Measured in accordance with JIS K6891, and the mass-based average particle diameter (50% integrated particle diameter) was taken as the average secondary particle diameter.

[0507] The polymer (I) used in the experimental example is as follows.

[0508] Polymer D: Homopolymer of monomer D represented by the formula: CH2=CF(CF2OCFCF3COOH) (number average molecular weight 8.6×10 4 , weight average molecular weight 18.0×10 4 ) The number average molecular weight and the weight average molecular weight were measured by gel permeation chromatography (GPC) using GPC HLC-8020 manufactured by Tosoh Corporation, and columns manufactured by Shodex (one GPC KF-801, one GPC KF-802, and two GPC KF-806M connected in series) were used. Tetrahydrofuran (THF) was used as the solvent and flowed at a flow rate of 1 ml / min for measurement, and the molecular weight was calculated using monodisperse polystyrene as a standard.

[0509] Preparation Example 1 A PTFE polymerization dispersion liquid was obtained by the method described in Synthesis Example 2 of International Publication No. 2021 / 045227. Various physical properties of the obtained PTFE polymerization dispersion liquid are shown below. Solid content concentration of PTFE polymerization dispersion liquid: 29.1 mass% pH of PTFE polymerization dispersion liquid: 4.1 Content of polymer D in PTFE polymerization dispersion liquid: 0.37 mass%

[0510] Comparative Example 1 The temperature of the PTFE polymer dispersion (pH 6.2) obtained in Preparation Example 1, which was diluted with deionized water to a solid concentration of 13%, was adjusted to 21°C, and 2-butanol in an amount equivalent to 40% by mass relative to the PTFE in the polymer dispersion was added to the diluted polymer dispersion, and then coagulated under stirring conditions. The wet powder obtained after filtration was added with water in an amount equivalent to 400% by mass relative to the PTFE, adjusted to 15°C, washed three times, and then dried at 120°C for 12 hours to obtain a PTFE powder.

[0511] Experimental Example 1 A PTFE powder was obtained in the same manner as in Comparative Example 1, except that in addition to 2-butanol in an amount equivalent to 40 mass %, ammonium carbonate in an amount equivalent to 0.66 mass % based on the PTFE in the polymerization dispersion was added.

[0512] Experimental Example 2 A PTFE powder was obtained in the same manner as in Experimental Example 1, except that 2-propanol was added instead of 2-butanol.

[0513] Experimental Example 3 A PTFE powder was obtained in the same manner as in Experimental Example 1, except that 2-pentanol was added instead of 2-butanol.

[0514] Experimental Example 4 A PTFE powder was obtained in the same manner as in Experimental Example 1, except that the amount of 2-butanol added was changed to an amount equivalent to 16% by mass based on the PTFE in the polymerization dispersion.

[0515] Experimental Example 5 A PTFE powder was obtained in the same manner as in Experimental Example 1, except that nitric acid was added instead of ammonium carbonate, and the amount of 2-butanol added was changed to an amount equivalent to 133 mass % relative to the PTFE in the polymer dispersion.

[0516] The above results are shown in Table 1. [Table 1]

[0517] Next, an example of a production method for obtaining a composition containing PTFE by contacting the PTFE in the polymer dispersion with an organic solvent to coagulate the PTFE and washing the obtained coagulate at a relatively high temperature will be described.

[0518] Experimental Example 6 The temperature of the PTFE polymer dispersion obtained in Preparation Example 1, which was diluted with deionized water to a solid content concentration of 13%, was adjusted to 40°C, and 2-butanol was added in an amount equivalent to 130% by mass of PTFE in the polymer dispersion, and then coagulated under stirring conditions. The mixture was filtered to obtain a wet powder. Water equivalent to 700% by mass of PTFE was added to the obtained wet powder, the temperature was adjusted to 40°C, and the mixture was washed three times and then filtered to obtain a wet washed powder. The obtained wet washed powder was dried at 120°C for 12 hours to obtain a PTFE powder.

[0519] Experimental Example 7 A PTFE powder was obtained in the same manner as in Experimental Example 6, except that the washing temperature was changed from 40°C to 30°C.

[0520] Experimental Example 8 A PTFE powder was obtained in the same manner as in Experimental Example 6, except that the washing temperature was changed from 40°C to 25°C.

[0521] The wet washed powder was dried at 240°C for 18 hours to obtain a PTFE powder. The SSG of the obtained PTFE powder was 2.168, the TII was 32, the extrusion pressure was 19.2MPa, and the variation rate of the extrusion pressure was 5.3%. The SSG, TII, extrusion pressure, and variation rate were measured by the following methods.

[0522] Standard specific gravity (SSG) The measurement was performed by the water displacement method according to ASTM D 792 using samples molded according to ASTM D4895-89.

[0523] Thermal instability index (TII) Measured in accordance with ASTM D 4895-89.

[0524] Extrusion Pressure 100 g of PTFE powder is left at room temperature for at least 2 hours, and then 21.7 g of a lubricant (Isopar H, ExxonMobil) is added as an extrusion aid, and mixed for 3 minutes to obtain a PTFE powder mixture. The resulting PTFE powder mixture is left in a 25°C thermostatic bath for 2 hours, and then paste extrusion molding is performed at 25°C under conditions of a reduction ratio of 100 (RR100, cylinder diameter 25 mm, orifice diameter 2.5 mm, orifice land length 1.1 mm, introduction angle 30°) and an extrusion speed of 51 cm / min to obtain a PTFE extrusion bead containing a lubricant. The extrusion pressure is determined by measuring the load when the extrusion load reaches an equilibrium state during paste extrusion and dividing the load by the cross-sectional area of ​​the cylinder used for paste extrusion.

[0525] Fluctuation rate of extrusion pressure In the measurement of the extrusion pressure, the difference between the maximum load and the minimum load when the extrusion load reached an equilibrium state was determined, and the rate of change was calculated using the following formula. (Fluctuation rate (%)) = [(Maximum load value) - (Minimum load value)] / (Cylinder cross-sectional area) / (Extrusion pressure) x 100

[0526] Experimental Example 9 A PTFE powder was obtained in the same manner as in Experimental Example 6, except that the temperature during washing was changed from 40° C. to 20° C. The solid content concentration in the coagulation wastewater was less than 0.1 mass %.

[0527] The above results are shown in Table 2. [Table 2]

Claims

1. A method for producing a composition containing polytetrafluoroethylene, comprising the steps of: A polymerization dispersion containing polytetrafluoroethylene is obtained by polymerizing tetrafluoroethylene in an aqueous medium in the presence of a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I), The polytetrafluoroethylene in the polymerization dispersion is coagulated by contacting the polytetrafluoroethylene in the polymerization dispersion with an organic solvent and a coagulant to obtain a composition containing polytetrafluoroethylene. Manufacturing method. C.X. 1 X 3 = C.X. 2 R (-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF 3 and X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more.

2. 2. The method according to claim 1, wherein the organic solvent is an alcohol having 1 to 7 carbon atoms.

3. 3. The method according to claim 1, wherein the organic solvent is an alcohol having 2 to 7 carbon atoms.

4. 3. The method according to claim 1, wherein the amount of the organic solvent used for coagulation is 1.0% by mass or more and 150% by mass or less based on the polytetrafluoroethylene in the polymerization dispersion.

5. 3. The method according to claim 1, wherein the coagulant is at least one selected from the group consisting of ammonium carbonate, ammonium hydrogen carbonate, ammonia and urea.

6. 3. The method according to claim 1, wherein the amount of the coagulant used for coagulation is 0.01% by mass or more and 5.0% by mass or less based on the polytetrafluoroethylene in the polymer dispersion.

7. 3. The method according to claim 1, wherein the temperature when the polytetrafluoroethylene in the polymer dispersion, the organic solvent and the coagulant are brought into contact with each other is 5 to 80°C.

8. 3. The method according to claim 1, wherein the composition is obtained by coagulating the polytetrafluoroethylene in the polymer dispersion to obtain a coagulate, and then washing the coagulate.

9. A composition comprising a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I) and polytetrafluoroethylene, wherein the content of the polymer (I) is 0.23 mass% or less based on the polytetrafluoroethylene, and the average secondary particle size of the polytetrafluoroethylene is 200 to 1000 μm. C.X. 1 X 3 = C.X. 2 R (-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF 3 and X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more.

10. The composition according to claim 9, which is substantially free of a fluorine-containing surfactant.

11. A method for producing a composition containing polytetrafluoroethylene, comprising the steps of: A polymerization dispersion containing polytetrafluoroethylene is obtained by polymerizing tetrafluoroethylene in an aqueous medium in the presence of a polymer (I) containing polymerization units (I) based on a monomer (I) represented by general formula (I), The polytetrafluoroethylene in the polymerization dispersion is coagulated by contacting the polytetrafluoroethylene in the polymerization dispersion with an organic solvent to obtain a coagulated product, and then the coagulated product is washed at 20° C. or higher to obtain a composition containing polytetrafluoroethylene. Manufacturing method. C.X. 1 X 3 = C.X. 2 R (-CZ 1 Z 2 -A 0 ) m (I) (In the formula, X 1 and X 3 are each independently F, Cl, H or CF 3 and X 2 is H, F, an alkyl group or a fluorine-containing alkyl group; A 0 is an anionic group; R is a linking group; Z 1 and Z 2 are each independently H, F, an alkyl group or a fluorine-containing alkyl group; and m is an integer of 1 or more.

Citation Information

Patent Citations

  • Method for manufacturing fluoropolymer

    WO2019168183A1

  • Method for producing fluoropolymer composition, and fluoropolymer composition

    WO2023277139A1