Positive electrode active material and lithium secondary battery comprising the same
A bimodal lithium composite oxide active material with optimized peak intensity ratios and a surface coating stabilizes High-Ni positive electrodes, addressing structural instability and improving the performance and stability of lithium secondary batteries.
Patent Information
- Application Number
- JP2024139382
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-14
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-08-10
AI Technical Summary
High-Ni positive electrode active materials used in lithium secondary batteries face structural instability and rapid degradation due to Li/Ni cation mixing, leading to poor high-temperature and room-temperature performance, and issues such as cell swelling and reduced cycle life.
A bimodal positive electrode active material comprising lithium composite oxides with small and large particles, optimized to achieve specific peak intensity ratios and voltage ratios during charging and discharging, and a coating layer to stabilize the surface, reducing grain boundaries and enhancing structural stability.
The solution improves the structural stability and high-temperature performance of lithium secondary batteries, maintaining high capacity characteristics while reducing side reactions and cell swelling, thereby enhancing the battery's overall stability and life characteristics.
Smart Images

Figure 2024159862000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode active material and a lithium secondary battery containing the same, and more specifically, to a positive electrode active material and a lithium secondary battery containing the same, which, when charged and discharged under specified conditions, have a voltage V and a battery capacity Q in the third cycle, and show a specified peak intensity ratio and voltage ratio in a graph in which the X-axis is the voltage V and the Y-axis is the value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V. [Background technology]
[0002] Batteries store electricity by using materials capable of electrochemical reactions at the positive and negative electrodes. A representative example of such batteries is the lithium secondary battery, which stores electrical energy by the difference in chemical potential when lithium ions are intercalated / deintercalated at the positive and negative electrodes.
[0003] The lithium secondary battery is manufactured by using a material capable of reversible intercalation / deintercalation of lithium ions as a positive electrode and a negative electrode active material, and filling an organic electrolyte or a polymer electrolyte between the positive electrode and the negative electrode.
[0004] Lithium composite oxides are used as the positive electrode active material of lithium secondary batteries, and composite oxides such as LiCoO2, LiMn2O4, LiNiO2, and LiMnO2 are examples of the oxides that have been researched.
[0005] Among the positive electrode active materials, LiCoO2 is the most widely used because of its excellent life characteristics and charge / discharge efficiency. However, it has a drawback in that it is expensive due to the limited availability of cobalt as a raw material, and therefore has limited price competitiveness.
[0006] Lithium manganese oxides such as LiMnO2 and LiMn2O4 have the advantages of being thermally safe and inexpensive, but have problems with small capacity and poor high-temperature characteristics. In addition, LiNiO2-based positive electrode active materials show high discharge capacity battery characteristics, but are difficult to synthesize due to the problem of cation mixing between Li and transition metals, which causes major problems with rate characteristics.
[0007] In addition, a large amount of Li by-products is generated depending on the depth of this cation mixing, and most of these Li by-products are composed of compounds of LiOH and Li2CO3, which causes gelation during the manufacture of the positive electrode paste and gas generation during charge and discharge after the electrode is manufactured. The remaining Li2CO3 increases the swelling phenomenon of the cell, reducing the cycle and causing the battery to swell.
[0008] To make up for these shortcomings, the demand for high-Ni positive electrode active materials with Ni content of 50% or more as the positive electrode active material for secondary batteries has increased. However, although such high-Ni positive electrode active materials exhibit high capacity characteristics, there is a problem in that structural instability due to Li / Ni cation mixing occurs as the Ni content in the positive electrode active material increases. Due to the structural instability of such positive electrode active materials, lithium secondary batteries can rapidly deteriorate not only at high temperatures but also at room temperature.
[0009] Therefore, it is necessary to develop a positive electrode active material that can overcome these problems of high-Ni positive electrode active materials. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Korean Patent Publication No. 10-2010-0131921 Summary of the Invention [Problem to be solved by the invention]
[0011] In the lithium secondary battery market, the growth of lithium secondary batteries for electric vehicles is driving the market, while the demand for positive electrode materials used in lithium secondary batteries is also continuously changing.
[0012] For example, lithium secondary batteries using LFP have traditionally been used primarily from the standpoint of ensuring safety, but recently there has been a trend toward expanding the use of nickel-based lithium composite oxides, which have a larger energy capacity per weight than LFP.
[0013] In accordance with such trends in positive electrode materials, the present invention aims to provide a positive electrode active material having improved electrochemical properties and stability by reducing the structural instability of a high-Ni positive electrode active material.
[0014] In particular, the applicant has found that in a high-Ni positive electrode active material having a Ni content of 50% or more, preferably 80% or more, when the positive electrode active material is charged and discharged under predetermined conditions, if the positive electrode active material satisfies a predetermined peak intensity ratio and voltage ratio in a graph having a voltage V and a battery capacity Q at the third cycle, with the X-axis being the voltage V and the Y-axis being the value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V, then the electrochemical characteristics and stability of the positive electrode active material can be further improved.
[0015] Thus, the present invention aims to provide a positive electrode active material that, when charged and discharged under specified conditions, has a voltage V and a battery capacity Q in the third cycle, and shows a specified peak intensity ratio and voltage ratio, which will be described later, in a graph in which the X-axis is the voltage V and the Y-axis is a value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V.
[0016] Another object of the present invention is to provide a positive electrode comprising the positive electrode active material defined herein.
[0017] Yet another object of the present invention is to provide a lithium secondary battery using the positive electrode defined herein. [Means for solving the problem]
[0018] According to one aspect of the present invention, there is provided a positive electrode active material including a lithium composite oxide capable of intercalating / deintercalating lithium.
[0019] The lithium composite oxide included in the positive electrode active material may contain at least Ni and Co. In addition to Ni and Co, the lithium composite oxide may further contain Mn and / or Al.
[0020] In one embodiment, the positive electrode active material has a property that, when a lithium secondary battery having the positive electrode active material as a positive electrode and a lithium foil as a negative electrode is charged and discharged under the following charge and discharge conditions,
[0021] [Charge / discharge conditions] 1 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 2 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 3 cycle: -Cut off voltage 3.0V~4.4V -Charge: 1C (CCCV) / Discharge: 1C (CC)
[0022] In a graph having a voltage V and a battery capacity Q at the third cycle, with the X-axis representing the voltage V and the Y-axis representing the value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V, the peak intensity ratio (A) defined by the following formula 1 can be satisfied.
[0023] [Formula 1] I1 / I2≧1.4
[0024] (In Equation 1, I1 is the y-axis value dQ / dV of the peak that appears between 3.0V and 3.8V in the charging region, and I2 is the y-axis value dQ / dV of the peak that appears between 3.8V and 4.1V in the charging region.)
[0025] In addition, the positive electrode active material may include a lithium composite oxide represented by the following Chemical Formula 1.
[0026] [Chemical formula 1] Li a Ni 1-(b+c+d+e) Co b M1 c M2 d M3 e O f
[0027] (where: M1 is at least one selected from Mn and Al; M2 and M3 are each independently selected from Al, Ba, B, Ce, Cr, Mg, Mn, Mo, Na, K, P, Sr, Ti, W, Nb, and Zr; M1 to M3 are different from each other. 0.90≦a≦1.05, 0≦b≦0.10, 0≦c≦0.10, 0≦d≦0.025, 0≦e≦0.025, 1.0≦f≦2.0)
[0028] According to another aspect of the present invention, there is provided a positive electrode comprising the positive electrode active material defined herein.
[0029] Yet, according to yet another aspect of the present invention, there is provided a lithium secondary battery using the positive electrode defined herein. Effect of the Invention
[0030] The positive electrode active material according to the present invention, when charged and discharged under predetermined conditions, has a voltage V and a battery capacity Q at the third cycle, and exhibits a predetermined peak intensity ratio and voltage ratio in a graph in which the X-axis is the voltage V and the Y-axis is a value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V. In this case, the positive electrode active material can maintain the high capacity characteristics of a high-Ni positive electrode active material having a Ni content of 50% or more, preferably 80% or more, while improving the structural instability that has been pointed out as a drawback of high-Ni positive electrode active materials.
[0031] In addition, the positive electrode active material according to the present invention is a bimodal positive electrode active material including a first lithium composite oxide as small particles and a second lithium composite oxide as large particles having different average particle diameters, and since the gaps between the large particles can be filled with small particles having a relatively small average particle diameter, the integration density of the lithium composite oxide within a unit volume can be improved, thereby increasing the energy density per unit volume.
[0032] Moreover, the cathode active material according to the present invention can reduce the density of the crystal grain boundaries of the lithium composite oxide constituting the cathode active material, thereby reducing the surface area and grain boundary of the lithium composite oxide, thereby reducing the possibility of a side reaction between the cathode active material and an electrolyte, and improving not only the high temperature stability but also the storage stability of the cathode active material. [Brief description of the drawings]
[0033] [Figure 1] This is a graph showing the voltage V and battery capacity Q at the third cycle when a lithium secondary battery having a positive electrode active material as a positive electrode and a lithium foil as a negative electrode is charged and discharged under predetermined charge and discharge conditions, with the X-axis representing the voltage V and the Y-axis representing the value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V. [Diagram 2] FIG. 2 is a diagram illustrating a schematic cross section of a lithium composite oxide for calculating the density of crystal grain boundaries defined in the present application. [Diagram 3] FIG. 2 is a diagram illustrating a schematic cross section of a lithium composite oxide for calculating the density of crystal grain boundaries defined in the present application. [Figure 4] 1 is a graph showing the voltage V and battery capacity Q at the third cycle when a lithium secondary battery having the positive electrode active material according to Example 1 as a positive electrode and a lithium foil as a negative electrode is charged and discharged under predetermined charge and discharge conditions, with the X-axis representing the voltage V and the Y-axis representing the value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V. [Diagram 5] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 2. [Figure 6] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 3. [Figure 7] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 4. [Figure 8] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 5. [Figure 9] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 6. [Figure 10] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 7. [Figure 11] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 8. [Figure 12] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Example 9. [Figure 13] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Comparative Example 1. [Figure 14] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Comparative Example 2. [Figure 15] 1 is a graph in which the X-axis represents voltage (V) and the Y-axis represents dQ / dV for the positive electrode active material according to Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Certain terms are defined herein for the convenience of making the present invention easier to understand. Unless otherwise defined herein, scientific and technical terms used in the present invention shall have the meanings commonly understood by those of ordinary skill in the art. Furthermore, unless otherwise specified by the context, singular terms shall be understood to include their plural forms, and plural terms shall be understood to include their singular forms.
[0035] Hereinafter, the positive electrode active material according to the present invention and the lithium secondary battery including the positive electrode active material will be described in more detail.
[0036] positive electrode active material According to one aspect of the present invention, there is provided a positive electrode active material including a lithium composite oxide capable of intercalating / deintercalating lithium.
[0037] The lithium composite oxide included in the positive electrode active material may contain at least Ni and Co. In addition to Ni and Co, the lithium composite oxide may further contain Mn and / or Al.
[0038] In one embodiment, the positive electrode active material may be a bimodal positive electrode active material including a first lithium composite oxide having small particles and a second lithium composite oxide having large particles.
[0039] In this case, the gaps between the large particles can be filled with small particles having a relatively small average particle size, thereby improving the integration density of the lithium composite oxide in a unit volume, and increasing the energy density per unit volume.
[0040] In the present application, the range of the average particle diameter D50 of small particles and large particles is not particularly limited, but in order to distinguish whether any lithium composite oxide is small particles or large particles, the following reference range of the average particle diameter D50 of small particles and large particles may be determined.
[0041] The small particles refer to lithium composite oxides having an average particle size D50 of 8 μm or less, and the large particles refer to lithium composite oxides having an average particle size D50 of 8.5 μm or more. There is no upper limit to the average particle size D50 of the large particles, but for example, the large particles may have an average particle size of 8.5 to 23.0 μm.
[0042] In the bimodal cathode active materials according to various embodiments of the present invention, the first lithium composite oxide and the second lithium composite oxide having the average particle size D50 defined above may be present in a mixed state in a weight ratio of 5:95 to 50:50.
[0043] In this case, the first lithium composite oxide may be present in a form in which it fills the gaps between the second lithium composite oxide, or it may be attached to the surface of the second lithium composite oxide, or it may be present in a form in which the first lithium composite oxide aggregates with each other.
[0044] In the positive electrode active material, the first lithium composite oxide and the second lithium composite oxide are preferably present in a weight ratio of 5:95 to 50:50.
[0045] If the ratio of the first lithium composite oxide to the second lithium composite oxide in the positive electrode active material is too high or too low, the press density of the positive electrode active material may decrease, and the effect of improving the energy density per unit volume of the positive electrode active material may become small.
[0046] The lithium composite oxide included in the positive electrode active material may be represented by the following Chemical Formula 1. If the positive electrode active material includes a first lithium composite oxide of small particles and a second lithium composite oxide of large particles, the first lithium composite oxide and the second lithium composite oxide may also be represented by the following Chemical Formula 1.
[0047] [Chemical formula 1] Li a Ni 1-(b+c+d+e) Co bM1 c M2 d M3 e O f
[0048] (where: M1 is at least one selected from Mn and Al; M2 and M3 are each independently selected from Al, Ba, B, Ce, Cr, Mg, Mn, Mo, Na, K, P, Sr, Ti, W, Nb, and Zr; M1 to M3 are different from each other, 0.90≦a≦1.05, 0≦b≦0.10, 0≦c≦0.10, 0≦d≦0.025, 0≦e≦0.025, 1.0≦f≦2.0)
[0049] In addition, the first lithium composite oxide and the second lithium composite oxide may be lithium composite oxides having the same composition represented by Chemical Formula 1, but are not necessarily limited thereto. For example, the first lithium composite oxide and the second lithium composite oxide may be synthesized by calcining precursors having the same composition and different average particle sizes, or the first lithium composite oxide and the second lithium composite oxide may be synthesized by calcining precursors having different compositions and different average particle sizes.
[0050] The lithium composite oxide represented by Formula 1 may be a high-Ni type lithium composite oxide having a Ni content (molar ratio) of 80% or more. In this case, the Ni content in the lithium composite oxide may be determined by the values of b+c+d+e in Formula 1 as follows:
[0051] Ni(mol%) / (Ni+Co+M1+M2+M3)(mol%)≧80
[0052] The positive electrode active material according to the present invention, when charged and discharged under predetermined conditions, has a voltage V and a battery capacity Q at the third cycle, and exhibits a predetermined peak intensity ratio and voltage ratio in a graph in which the X-axis is the voltage V and the Y-axis is a value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V. In this case, the positive electrode active material can maintain the high capacity characteristics of a high-Ni positive electrode active material having a Ni content of 50% or more, preferably 80% or more, while improving the structural instability that has been pointed out as a drawback of high-Ni positive electrode active materials.
[0053] Specifically, when a lithium secondary battery having the positive electrode active material as a positive electrode and a lithium foil as a negative electrode is charged and discharged under the following charge and discharge conditions,
[0054] [Charge / discharge conditions] 1 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 2 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 3 cycle: -Cut off voltage 3.0V~4.4V -Charge: 1C (CCCV) / Discharge: 1C (CC)
[0055] In a graph (see FIG. 1) having a voltage V and a battery capacity Q at the third cycle, with the X-axis representing the voltage V and the Y-axis representing a value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V, the positive electrode active material can satisfy a peak intensity ratio (A) defined by the following formula 1.
[0056] [Formula 1] I1 / I2≧1.4
[0057] (In Equation 1, I1 is the y-axis value dQ / dV of the peak that appears between 3.0V and 3.8V in the charging region, and I2 is the y-axis value dQ / dV of the peak that appears between 3.8V and 4.1V in the charging region.)
[0058] The positive electrode active material may undergo a change in crystal structure (phase transformation) during charging, where I1 is the y-axis value dQ / dV of a peak that appears in a phase transformation region (H→M) from H1 (hexagonal 1) to M (monoclinic), and I2 is the y-axis value dQ / dV of a peak that appears in a phase transformation region (M→H2) from M (monoclinic) to H2 (hexagonal 2).
[0059] In this case, damage to the positive active material due to a change in the crystal structure in the M→H2 phase transformation region may be relatively greater than that in the H1→M phase transformation region, which may cause the crystal structure of the positive active material to collapse. Therefore, when I1 / I2 is 1.4 or more, preferably 1.4 to 1.92, it may be advantageous to improve the stability of the positive active material.
[0060] In addition, the positive electrode active material may satisfy the peak intensity ratio (B) defined by the following formula 2.
[0061] [Formula 2] I1 / I3≧0.7
[0062] (In Equation 2, I1 is the y-axis value dQ / dV of the peak that appears between 3.0V and 3.8V in the charging region, and I3 is the y-axis value dQ / dV of the peak that appears between 4.1V and 4.4V in the charging region.)
[0063] Similarly, I3 is the y-axis value dQ / dV of the peak appearing in the phase transformation region (H2→H3) from H2 (hexagonal 2) to H3 (hexagonal 3), and similarly to Equation 1, damage to the positive electrode active material due to changes in crystal structure may be relatively greater in the H2→H3 phase transformation region than in the H1→M phase transformation region. Therefore, when I1 / I3 is 0.7 or more, preferably 0.7 to 1.41, it may be advantageous to improve the stability of the positive electrode active material.
[0064] In addition, the positive electrode active material may satisfy the peak intensity ratio (C) defined by the following formula 3:
[0065] [Formula 3] I2 / I3≧0.5
[0066] (In Equation 3, I2 is the y-axis value dQ / dV of the peak that appears between 3.8V and 4.1V in the charging region, and I3 is the y-axis value dQ / dV of the peak that appears between 4.1V and 4.4V in the charging region.)
[0067] In this case, damage to the positive active material due to a change in crystal structure in the H2→H3 phase transformation region may be relatively greater than that in the M→H2 phase transformation region, and therefore, when I3 is relatively smaller than I2, and I2 / I3 is 0.5 or more, this can contribute to improving the stability of the positive active material.
[0068] In addition, the positive electrode active material may satisfy the peak intensity ratio (D) defined by the following formula 4.
[0069] [Formula 4] DI1 / DI2≧1.25
[0070] (In Equation 4, DI1 is the y-axis value dQ / dV of the peak that appears between 3.0V and 3.8V in the discharge region, and DI2 is the y-axis value dQ / dV of the peak that appears between 3.8V and 4.1V in the discharge region.)
[0071] The positive electrode active material may undergo a change in crystal structure during discharge, similar to the charge reaction, and the change in crystal structure may occur in the reverse order to the charge reaction.
[0072] Specifically, DI1 is the y-axis value dQ / dV of a peak that appears in the phase transformation region (M → H1) from M (monoclinic) to H1 (hexagonal 1), and DI2 is the y-axis value dQ / dV of a peak that appears in the phase transformation region (H2 → M) from H2 (hexagonal 2) to M (monoclinic).
[0073] In this case, damage to the positive active material due to changes in the crystal structure in the H2→M phase transformation region may be relatively greater than that in the M→H1 phase transformation region, which may cause the crystal structure of the positive active material to collapse. Therefore, when DI1 / DI2 is 1.25 or more, preferably 1.25 to 1.46, it may be advantageous to improve the stability of the positive active material.
[0074] In addition, the positive electrode active material may satisfy the peak intensity ratio (E) defined by the following formula 5:
[0075] [Formula 5] DI1 / DI3≧0.41
[0076] (In Equation 5, DI1 is the y-axis value dQ / dV of the peak that appears between 3.0V and 3.8V in the discharge region, and DI3 is the y-axis value dQ / dV of the peak that appears between 4.1V and 4.4V in the discharge region.)
[0077] Similarly, DI3 is the y-axis value dQ / dV of a peak that appears in the phase transformation region (H3→H2) from H3 (hexagonal 3) to H2 (hexagonal 2). As with Equation 4, damage to the positive electrode active material due to changes in crystal structure may be relatively greater in the H3→H2 phase transformation region than in the H2→M phase transformation region. Therefore, it is preferable from the viewpoint of stability of the positive electrode active material that the peak intensity of DI3 has a smaller value than that of DI1, and thus DI1 / DI3 has a value of 0.41 or more.
[0078] In addition, the positive electrode active material may satisfy the peak intensity ratio (F) defined by the following formula 6:
[0079] [Formula 6] DI2 / DI3≧0.34
[0080] (In Equation 6, DI2 is the y-axis value dQ / dV of the peak that appears between 3.8V and 4.1V in the discharge region, and DI3 is the y-axis value dQ / dV of the peak that appears between 4.1V and 4.4V in the discharge region.)
[0081] In this case, damage to the positive active material due to a change in crystal structure in the H3→H2 phase transformation region may be relatively greater than that in the H2→M phase transformation region, and therefore, when DI2 / DI3 is 0.34 or more, preferably 0.34 to 0.58, it may be advantageous to improve the stability of the positive active material.
[0082] Moreover, the positive electrode active material can satisfy the voltage ratio (G) defined by the following formula 7.
[0083] [Formula 7] |ΔV1=(V1-DV1)|≦0.05
[0084] (In Equation 7, V1 is the x-axis value V of the peak that appears between 3.0V and 3.8V in the charging region, and DV1 is the x-axis value V of the peak that appears between 3.0V and 3.8V in the discharging region.)
[0085] V1 is the voltage value of the I1 peak during charging, and DV1 is the voltage value corresponding to the DI1 peak during discharging. Ideally, the voltage value of the I1 peak and the voltage value of the DI1 peak should be the same, but due to resistance or kinetic problems, there is no choice but to generate a difference between the voltage values of the I1 peak and the DI1 peak. However, in the case of a positive electrode active material that satisfies at least formulas 1 to 6, it is possible for ΔV1 shown in formula 7 to have a value of 0.05 or less, preferably 0.022 or less, by exhibiting excellent resistance characteristics.
[0086] In the case of lithium composite oxides containing Ni, residual lithium, i.e., Li impurities such as LiOH and Li2CO3, may be formed on the surface of the lithium composite oxide due to cation mixing of Li and Ni. Such Li impurities may cause gelation during the preparation of paste for preparing a positive electrode or may act as a cause of cell swelling.
[0087] Such Li impurities may be formed in larger amounts in a high-Ni type positive electrode active material, but as described below, the positive electrode active material according to the present invention has an advantage in that Li impurities present on the surface of the lithium composite oxide can be removed during the process of forming a coating layer including a metal oxide that covers at least a portion of the surface of the lithium composite oxide.
[0088] More specifically, the positive electrode active material may include a coating layer including a metal oxide, covering at least a portion of the surface of the lithium composite oxide.
[0089] In addition, the metal oxide included in the coating layer may be represented by the following Chemical Formula 2. In this case, the coating layer may be defined as a region on the surface of the lithium composite oxide where the metal oxide represented by the following Chemical Formula 2 is present.
[0090] [Chemical formula 2] Li x M4 y O z
[0091] (wherein M4 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Ce, Gd, and Nd, and 0≦x≦10, 0≦y≦8, and 2≦z≦13.)
[0092] In addition, the coating layer may be in a form in which different metal oxides are simultaneously present within one layer, or different metal oxides represented by Formula 2 above are present in separate layers.
[0093] The metal oxide represented by the above Chemical Formula 2 may be in a state of being physically and / or chemically bonded to the primary particles represented by the above Chemical Formula 1. In addition, the metal oxide may exist in a state of forming a solid solution with the primary particles represented by the above Chemical Formula 1.
[0094] The positive electrode active material according to the present embodiment includes a coating layer that covers at least a portion of the surface of the first lithium composite oxide and the second lithium composite oxide, and thus the structural stability can be improved. In addition, when such a positive electrode active material is used in a lithium secondary battery, the high-temperature storage stability and life characteristics of the positive electrode active material can be improved. In addition, the metal oxide reduces residual lithium on the surfaces of the first lithium composite oxide and the second lithium composite oxide, and at the same time, acts as a pathway for lithium ions, thereby improving the efficiency characteristics of the lithium secondary battery.
[0095] The metal oxide is a composite oxide of lithium and an element represented by A, or an oxide of A. The metal oxide is, for example, Li a W b O c , Li a Zr b O c , Li a Ti b O c , Li a Ni b O c , Li a B b O c , Li a Co b O c , Li a Al b O c , Co b O c, Al b O c , W b O c , Zr b O c , Ti b O c Or B b O c However, the above-mentioned examples are merely given for the sake of convenience to facilitate understanding, and the metal oxide defined in the present application is not limited to the above-mentioned examples.
[0096] In another embodiment, the metal oxide may be an oxide in which lithium and at least two elements represented by A are combined, or may further include a metal oxide in which lithium and at least two elements represented by A are combined. The metal oxide in which lithium and at least two elements represented by A are combined may be, for example, Li a (W / Ti) b O c , Li a (W / Zr) b O c , Li a (W / Ti / Zr) b O c , Li a (W / Ti / B) b O c etc., but are not necessarily limited to these.
[0097] Here, the metal oxide may exhibit a concentration gradient that decreases from the surface portion of the secondary particle toward the center portion of the secondary particle, whereby the concentration of the metal oxide may decrease from the outermost surface of the secondary particle toward the center portion of the secondary particle.
[0098] As described above, the metal oxide exhibits a concentration gradient that decreases from the surface portion of the secondary particle toward the center portion of the secondary particle, thereby effectively reducing the residual lithium present on the surface of the positive electrode active material, and thus preventing side reactions due to unreacted residual lithium. In addition, the metal oxide can prevent the crystallinity of the inner region of the surface of the positive electrode active material from decreasing. In addition, the metal oxide can prevent the overall structure of the positive electrode active material from collapsing during an electrochemical reaction.
[0099] Moreover, the coating layer may include a first oxide layer including at least one metal oxide represented by the above chemical formula 2, and a second oxide layer including at least one metal oxide represented by the above chemical formula 2 and including a metal oxide different from the metal oxide included in the first oxide layer.
[0100] For example, the first oxide layer may be present to cover at least a portion of the exposed surfaces of the primary particles present at the outermost portion of the secondary particles, and the second oxide layer may be present to cover at least a portion of the exposed surfaces of the primary particles not covered by the first oxide layer and the surface of the first oxide layer.
[0101] When the first lithium composite oxide and the second lithium composite oxide are defined as composite particles including at least one primary particle, the coating layer not only covers at least a portion of the surface of the composite particle (e.g., secondary particle), but also can be present at the interface between a plurality of primary particles constituting the composite particle.
[0102] In addition, the coating layer may exist as a layer that continuously or discontinuously coats the surfaces of the primary particles and / or the secondary particles. When the coating layer exists discontinuously, the coating layer may exist in the form of islands. In other cases, the coating layer may exist in the form of a solid solution that does not form a boundary with the primary particles and / or the secondary particles formed by agglomeration of the primary particles.
[0103] The coating layer can be obtained by mixing the precursor of the lithium composite oxide with the raw material of the metal oxide represented by Chemical Formula 2 and then performing a primary firing, or by primary firing the precursor of the lithium composite oxide, mixing the raw material of the metal oxide represented by Chemical Formula 2, and then performing a secondary firing.
[0104] In addition, the lithium composite oxide capable of lithium intercalation / deintercalation may be a composite particle including at least one primary particle. If the lithium composite oxide includes a plurality of primary particles, the plurality of primary particles may be present as secondary particles that are aggregates of each other.
[0105] The primary particle means one grain or crystallite, and the secondary particle means an aggregate formed by agglomeration of a plurality of primary particles. There may be voids and / or grain boundaries between the primary particles constituting the secondary particle.
[0106] In particular, according to the present invention, the density of the crystal grain boundaries of the lithium composite oxide can be reduced to reduce the surface area and grain boundaries of the lithium composite oxide, thereby reducing the possibility of side reactions between the positive electrode active material and the electrolyte, and improving the high temperature stability as well as the storage stability of the positive electrode active material.
[0107] Specifically, the lithium composite oxide may have a grain boundary density of 0.90 or less, calculated by the following Equation 8, for primary particles P arranged on a virtual line L crossing the center of the lithium composite oxide in a cross-sectional SEM image.
[0108] [Formula 8] Grain boundary density = (number of boundaries B between primary particles arranged on the imaginary straight line L / number of primary particles P arranged on the imaginary straight line)
[0109] 2 and 3 are schematic diagrams showing the cross section of a lithium composite oxide for calculating the density of the crystal grain boundary defined in the present application. The density of the crystal grain boundary of the lithium composite oxide calculated with reference to FIG. 2 and FIG. 3 is shown in Table 1 below.
[0110] [Table 1]
[0111] In this case, the lithium composite oxide may have a structure in which the number of interfaces (grain boundaries) between primary particles arranged on an imaginary line is one, and the number of primary particles arranged on the imaginary line is two, resulting in a grain boundary density of 0.5, as shown in Figure 2. Although not shown separately, the lithium composite oxide may be a lithium composite oxide having a single crystal structure composed of a single primary particle.
[0112] When the grain boundary density represented by Formula 8 has a value of 0.90 or less, the surface area and grain boundary surface of the lithium composite oxide can be reduced, thereby reducing the possibility of a side reaction between the positive electrode active material and an electrolyte, and improving the high temperature stability as well as the storage stability of the positive electrode active material.
[0113] In addition, when the positive electrode active material is a bimodal positive electrode active material including a first lithium composite oxide having small particles and a second lithium composite oxide having large particles, the grain boundary densities of the first lithium composite oxide and the second lithium composite oxide may both be 0.90 or less, preferably 0.75 or less.
[0114] Lithium secondary battery According to yet another aspect of the present invention, a positive electrode may be provided, the positive electrode including a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. Here, the positive electrode active material layer may include a positive electrode active material according to various embodiments of the present invention. Therefore, since the positive electrode active material is the same as that described above, detailed description will be omitted for convenience, and only the remaining components not described above will be described below.
[0115] The positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, or the like. The positive electrode current collector may usually have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0116] The positive electrode active material layer may be prepared by coating a positive electrode slurry composition containing the positive electrode active material, a conductive material, and optionally a binder, on the positive electrode current collector.
[0117] In this case, the positive electrode active material may be included in an amount of 80 to 99 wt%, more specifically, 85 to 98.5 wt%, based on the total weight of the positive electrode active material layer. When included in the above content range, excellent capacity characteristics can be exhibited, but the amount is not necessarily limited thereto.
[0118] The conductive material is used to impart conductivity to the electrode, and can be used without any particular restrictions as long as it does not cause a chemical change in the battery and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One or a mixture of two or more of these can be used. The conductive material can be contained in an amount of 0.1 to 15 wt% based on the total weight of the positive electrode active material layer.
[0119] The binder serves to improve adhesion between positive electrode active material particles and adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 0.1 to 15 wt% based on the total weight of the positive electrode active material layer.
[0120] The positive electrode may be manufactured by a conventional method for manufacturing a positive electrode, except for using the positive electrode active material described above. Specifically, the positive electrode may be manufactured by coating a positive electrode slurry composition prepared by dissolving or dispersing the positive electrode active material described above and, optionally, a binder and a conductive material in a solvent, on a positive electrode current collector, followed by drying and rolling.
[0121] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder in consideration of the coating thickness of the slurry and the production yield, and to have a viscosity that allows excellent thickness uniformity to be exhibited when the slurry is applied to produce a positive electrode.
[0122] In another embodiment, the positive electrode can be manufactured by casting the positive electrode slurry composition on a separate support, peeling the composition from the support, and laminating the resulting film on a positive electrode current collector.
[0123] According to yet another aspect of the present invention, there is provided an electrochemical device including the above-described positive electrode. The electrochemical device may be, specifically, a battery, a capacitor, or the like, and more specifically, may be a lithium secondary battery.
[0124] The lithium secondary battery may specifically include a positive electrode, a negative electrode facing the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Here, since the positive electrode is the same as that described above, a detailed description thereof will be omitted for the sake of brevity, and only the remaining components not described above will be described in detail below.
[0125] The lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0126] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0127] The negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or the like, or an aluminum-cadmium alloy. The negative electrode current collector may generally have a thickness of 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.
[0128] The negative electrode active material layer may be prepared by coating a negative electrode slurry composition containing the negative electrode active material, a conductive material, and optionally a binder, on the negative electrode current collector.
[0129] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. Also, a thin film of metallic lithium may be used as the negative electrode active material. Also, both low crystalline carbon and high crystalline carbon may be used as the carbon material. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.
[0130] The negative electrode active material may be included in an amount of 80 to 99 wt % based on the total weight of the negative electrode active material layer.
[0131] The binder is a component that aids in bonding between the conductive material, the active material, and the current collector, and may be added in an amount of 0.1 to 10 wt% based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0132] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 wt% or less, preferably 5 wt% or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and may be, for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black; conductive fibers such as carbon fiber or metal fiber; metal powder such as carbon fluoride, aluminum, nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc.
[0133] In one embodiment, the negative electrode active material layer may be prepared by coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent on a negative electrode current collector and drying the coating. Alternatively, the negative electrode slurry composition may be cast on a separate support, and then peeled off from the support to obtain a film, which may be laminated on the negative electrode current collector.
[0134] In the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator that is generally used in lithium secondary batteries can be used without any particular restrictions. In particular, it is preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte impregnation ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single layer or multilayer structure.
[0135] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, and the like that can be used in the production of lithium secondary batteries, but are not limited to these.
[0136] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0137] The organic solvent may be used without any particular limitation as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; an ether solvent such as dibutyl ether or tetrahydrofuran, etc.; a ketone solvent such as cyclohexanone, etc.; an aromatic hydrocarbon solvent such as benzene or fluorobenzene, etc.; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), propylene carbonate (propylene carbonate), etc. Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a hydrocarbon group having a linear, branched or cyclic structure with 2 to 20 carbon atoms, which may contain an aromatic ring or an ether bond with a double bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the performance of the electrolyte can be excellent.
[0138] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0139] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, improving the discharge capacity of the battery, etc. In this case, the additives may be contained in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.
[0140] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs), etc.
[0141] The external shape of the lithium secondary battery according to the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, etc. Furthermore, the lithium secondary battery may be used as a battery cell used as a power source for a small device, and may also be preferably used as a unit battery for a medium- to large-sized battery module including a number of battery cells.
[0142] According to yet another aspect of the present invention, there can be provided a battery module including the lithium secondary battery as a unit cell and / or a battery pack including the same.
[0143] The battery module or the battery pack is used as a power source for one or more medium- to large-sized devices including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0144] The present invention will be described in more detail with reference to the following examples. However, these examples are merely for the purpose of illustrating the present invention, and the scope of the present invention is not limited to these examples.
[0145] Production Example 1. Production of positive electrode active material (1) Example 1 A small-particle first lithium composite oxide and a large-particle NiCoMn(OH)2 hydroxide precursor (Ni:Co:Mn=91:8:1 (at%)) of a second lithium composite oxide were synthesized by a known co-precipitation method using nickel sulfate, cobalt sulfate, and manganese sulfate. The hydroxide precursor of the first lithium composite oxide (first hydroxide precursor) had an average particle size D50 of 3.0 μm, and the hydroxide precursor of the second lithium composite oxide (second hydroxide precursor) had an average particle size D50 of 18.0 μm.
[0146] Next, the first hydroxide precursor and the second hydroxide precursor were mixed in a weight ratio of 30:70, LiOH (Li / (Ni+Co+Mn) molar ratio=1.05±0.05) was added, and the mixture was heated to 780° C. at a rate of 2° C. per minute while maintaining an O2 atmosphere in a calcination furnace, and heat-treated for 12 hours (primary calcination) to obtain a mixture of the first lithium composite oxide and the second lithium composite oxide.
[0147] Next, distilled water was poured into the mixture of the first lithium composite oxide and the second lithium composite oxide, the mixture was washed with water for 1 hour, and then dried in a vacuum dryer at 120° C. for 12 hours.
[0148] Next, while maintaining an O2 atmosphere in a sintering furnace, the temperature was increased to 700°C at a rate of 2°C per minute and heat-treated for 12 hours (secondary sintering) to obtain a bimodal cathode active material in which the first lithium composite oxide having small particles and the second lithium composite oxide having large particles are mixed in a predetermined ratio.
[0149] (2) Example 2 A positive electrode active material was prepared in the same manner as in Example 1, except that 0.5 mol % of NaNO3 was added to the mixture of the first hydroxide precursor and the second hydroxide precursor before the primary firing, and then the mixture was heat-treated.
[0150] (3) Example 3 A positive electrode active material was prepared in the same manner as in Example 1, except that 0.3 mol % of Ba(OH)2 was added to the mixture of the first hydroxide precursor and the second hydroxide precursor before the primary firing, and then the mixture was heat-treated.
[0151] (4) Example 4 A positive electrode active material was prepared in the same manner as in Example 1, except that the temperature was increased to 820° C. at a rate of 2° C. per minute and heat-treated (primary baking) for 12 hours.
[0152] (5) Example 5 A positive electrode active material was prepared in the same manner as in Example 4, except that 0.5 mol % of NaNO3 was added to the mixture of the first hydroxide precursor and the second hydroxide precursor before the primary firing, and then the mixture was heat-treated.
[0153] (6) Example 6 A positive electrode active material was prepared in the same manner as in Example 4, except that 0.3 mol % of Ba(OH)2 was added to the mixture of the first hydroxide precursor and the second hydroxide precursor before the primary firing, and then heat-treated.
[0154] (7) Example 7 A positive electrode active material was prepared in the same manner as in Example 1, except that the temperature was increased to 850° C. at a rate of 2° C. per minute and heat-treated for 12 hours (primary baking).
[0155] (8) Example 8 A positive electrode active material was prepared in the same manner as in Example 7, except that 0.5 mol % of NaNO3 was added to the mixture of the first hydroxide precursor and the second hydroxide precursor before the primary firing, and then the mixture was heat-treated.
[0156] (9) Example 9 A positive electrode active material was prepared in the same manner as in Example 7, except that 0.3 mol % of Ba(OH)2 was added to the mixture of the first hydroxide precursor and the second hydroxide precursor before the primary firing, and then heat-treated.
[0157] (10) Comparative Example 1 A positive electrode active material was prepared in the same manner as in Example 1, except that the temperature was increased to 700° C. at a rate of 2° C. per minute and heat-treated for 8 hours (primary baking).
[0158] (11) Comparative Example 2 A positive electrode active material was prepared in the same manner as in Example 1, except that the temperature was increased to 705° C. at a rate of 2° C. per minute and heat-treated for 8 hours (primary baking).
[0159] (12) Comparative Example 3 A positive electrode active material was prepared in the same manner as in Example 1, except that the temperature was increased to 710° C. at a rate of 2° C. per minute and heat-treated for 8 hours (primary baking).
[0160] Manufacturing Example 2. Manufacturing of lithium secondary batteries A positive electrode slurry was prepared by dispersing 92 wt% of the positive electrode active material prepared in Preparation Example 1, 4 wt% of artificial graphite (super-P), and 4 wt% of PVDF binder in 30 g of N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was uniformly applied to a thin aluminum film having a thickness of 15 μm and dried in a vacuum at 135° C. to prepare a positive electrode for a lithium secondary battery.
[0161] A coin battery was fabricated using a lithium foil as a counter electrode for the positive electrode, a porous polyethylene film (Celgard 2300, thickness: 25 μm) as a separator, and an electrolyte of LiPF6 at a concentration of 1.15 M in a solvent of ethylene carbonate and ethyl methyl carbonate mixed in a volume ratio of 3:7.
[0162] Experimental Example 1: Structural analysis of positive electrode active material Cross-sectional SEM images were obtained using FE-SEM (Bruker) for each of the first lithium composite oxide small particles and the second lithium composite oxide large particles contained in the positive electrode active material prepared according to Preparation Example 1, and then the average grain boundary density was calculated from the cross-sectional SEM images according to the following Equation 8.
[0163] [Formula 8] Grain boundary density = (the number of boundaries between primary particles arranged on a virtual line that crosses the center of the lithium composite oxide in a cross-sectional SEM image of the lithium composite oxide / the number of primary particles arranged on the virtual line)
[0164] The results of the measurement of the grain boundary density are shown in Table 2 below.
[0165] [Table 2]
[0166] Experimental Example 2: Evaluation of the electrochemical properties of the positive electrode active material (1) Measurement results of peak intensity ratio and voltage ratio of lithium secondary battery When the lithium secondary battery produced in Production Example 2 was charged and discharged at 25° C. under the following charge and discharge conditions, the voltage V and battery capacity Q in the third cycle were measured using an electrochemical analyzer (Toyo, Toscat-3100), and a graph was created in which the X-axis represents the voltage V and the Y-axis represents the value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V. From the graph, the peak intensity ratios defined by Equations 1 to 6 and the voltage ratios defined by Equation 7 were determined. The peak intensity ratios defined by Equations 1 to 6 and the voltage ratios defined by Equation 7 are shown in Tables 3 to 6 below.
[0167] [Charge / discharge conditions] 1 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 2 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 3 cycle: -Cut off voltage 3.0V~4.4V -Charge: 1C (CCCV) / Discharge: 1C (CC)
[0168] [Table 3]
[0169] [Table 4]
[0170] [Table 5]
[0171] [Table 6]
[0172] (2) Evaluation of the battery capacity and life characteristics of lithium secondary batteries The lithium secondary battery manufactured according to Manufacturing Example 2 was charged and discharged 50 times at 1C / 1C within a driving voltage range of 3.0V to 4.4V at a temperature of 25°C using an electrochemical analyzer (Toyo, Toscat-3100), and the ratio of the discharge capacity at the 50th cycle to the initial capacity (cycle capacity retention) was measured.
[0173] The evaluation results of the life characteristics of the lithium secondary batteries measured by the above method are shown in Table 7 below.
[0174] [Table 7]
[0175] Referring to the results of Table 7, it can be seen that the lithium secondary batteries using the positive electrode active materials according to Examples 1 to 9 have improved life characteristics compared to the lithium secondary batteries using the positive electrode active materials according to Comparative Examples 1 to 3.
[0176] Experimental Example 3. Evaluation of the stability of positive electrode active materials and lithium secondary batteries (1) Evaluation of thermal stability of positive electrode active material The weight loss was measured at a heating rate of 10°C / min from 25°C to 350°C under Ar atmosphere at normal pressure using a thermogravimetric analyzer (TA Instruments, Q20) to evaluate the thermal stability of the positive electrode active material prepared in Preparation Example 1. The onset temperature (op-set) at which the weight loss (thermal decomposition) peak appeared for each positive electrode active material is shown in Table 8 below.
[0177] [Table 8]
[0178] Referring to the results in Table 8, it was found that the on-set temperature at which the weight loss (thermal decomposition) peak appears in the positive electrode active materials according to Examples 1 to 9 is higher than that of the positive electrode active materials according to Comparative Examples 1 to 3. That is, it can be seen that the thermal stability of the positive electrode active materials according to Examples 1 to 9 is superior to that of the positive electrode active materials according to Comparative Examples 1 to 3.
[0179] (2) Measurement of gas generation rate of lithium secondary batteries The lithium secondary battery prepared according to Preparation Example 2 was charged to 4.25 V at a constant current of 0.2 C and then stored at 60° C. for 14 days to measure the volume change of the lithium secondary battery due to gas generation in the lithium secondary battery. The measurement results of the volume change are shown in Table 9 below.
[0180] [Table 9]
[0181] Referring to the results in Table 9, it can be seen that the volume change of the lithium secondary batteries using the positive electrode active materials according to Examples 1 to 9 is smaller than the volume change of the lithium secondary batteries using the positive electrode active materials according to Comparative Examples 1 to 3.
[0182] Although the embodiments of the present invention have been described above, a person having ordinary knowledge in the art may modify and change the present invention in various ways by adding, changing, deleting or adding components, etc., without departing from the spirit of the present invention described in the claims, and this can also be said to be included in the scope of the present invention.
Claims
1. A positive electrode active material containing a lithium composite oxide capable of lithium intercalation / deintercalation, The positive electrode active material has a bimodal structure including a first lithium composite oxide that is a small particle and a second lithium composite oxide that is a large particle, a molar ratio of Ni to all metal elements excluding lithium in each of the first lithium composite oxide and the second lithium composite oxide is 50% or more; an average value of the grain boundary density calculated by the following formula 8 for primary particles located on a virtual line crossing the center of the first lithium composite oxide in a cross-sectional SEM image of the first lithium composite oxide, and an average value of the grain boundary density calculated by the following formula 8 for primary particles located on a virtual line crossing the center of the second lithium composite oxide in a cross-sectional SEM image of the second lithium composite oxide are 0.90 or less. Cathode active material. [Formula 8] Grain boundary density=(number of boundaries between primary particles arranged on the imaginary line / number of primary particles arranged on the imaginary line)
2. 2. The positive electrode active material according to claim 1, wherein an average value of a grain boundary density calculated by the following formula 8 for primary particles located on a virtual line crossing a center of the first lithium composite oxide in a cross-sectional SEM image of the first lithium composite oxide is not more than an average value of a grain boundary density calculated by the following formula 8 for primary particles located on a virtual line crossing a center of the second lithium composite oxide in a cross-sectional SEM image of the second lithium composite oxide. [Formula 8] Grain boundary density=(number of boundaries between primary particles arranged on the imaginary line / number of primary particles arranged on the imaginary line)
3. 2. The positive electrode active material according to claim 1, wherein an average value of a grain boundary density calculated by the following formula 8 for primary particles on a virtual line crossing a center of the first lithium composite oxide in a cross-sectional SEM image of the first lithium composite oxide is 0.50 to 0.88: [Formula 8] Grain boundary density=(number of boundaries between primary particles arranged on the imaginary line / number of primary particles arranged on the imaginary line)
4. 2. The positive electrode active material according to claim 1, wherein an average value of the grain boundary density calculated by the following formula 8 for primary particles on a virtual line crossing a center of the second lithium composite oxide in a cross-sectional SEM image of the second lithium composite oxide is 0.67 to 0.90: [Formula 8] Grain boundary density=(number of boundaries between primary particles arranged on the imaginary line / number of primary particles arranged on the imaginary line)
5. When a lithium secondary battery having the positive electrode active material as a positive electrode and a lithium foil as a negative electrode is charged and discharged under the following charge and discharge conditions, [Charge / discharge conditions] 1 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 2 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 3 cycles: -Cut off voltage 3.0V~4.4V -Charge: 1C (CCCV) / Discharge: 1C (CC) In a graph showing a voltage V and a battery capacity Q at the third cycle, the X-axis is the voltage V and the Y-axis is a value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V, The positive electrode active material according to claim 1 , which satisfies a peak intensity ratio (A) defined by the following formula 1: [Formula 1] I1 / I2≧1.4 (In Equation 1, I1 is the y-axis value dQ / dV of the peak that appears in the phase transformation region from hexagonal to monoclinic between 3.0 V and 3.8 V in the charging region, I2 is the y-axis value dQ / dV of the peak that appears in the phase transformation region from monoclinic to hexagonal between 3.8V and 4.1V in the charging region.
6. The positive electrode active material according to claim 5 , wherein the peak intensity ratio (A) defined by the formula 1 is 1.4 or more and 1.92 or less.
7. The positive electrode active material according to claim 1 , wherein the lithium composite oxide is represented by the following chemical formula 1: [Chemical formula 1] Li a Ni 1-(b+c+d+e) Co b M1 c M2 d M3 e O f (where: M1 is at least one selected from Mn and Al; M2 and M3 are each independently selected from Al, Ba, B, Ce, Cr, Mg, Mn, Mo, Na, K, P, Sr, Ti, W, Nb, and Zr; M1 to M3 are different from each other, 0.90≦a≦1.05, 0≦b≦0.10, 0≦c≦0.10, 0≦d≦0.025, 0≦e≦0.025, 1.0≦f≦2.0)
8. The positive electrode active material according to claim 1 , wherein the first lithium composite oxide has an average particle size D50 of 8 μm or less.
9. The positive electrode active material according to claim 1 , wherein the second lithium composite oxide has an average particle size D50 of 8.5 μm or more.
10. A positive electrode active material containing a lithium composite oxide capable of lithium intercalation / deintercalation, The molar ratio of Ni to all metal elements excluding lithium in the lithium composite oxide is 50% or more; When a lithium secondary battery having the positive electrode active material as a positive electrode and a lithium foil as a negative electrode is charged and discharged under the following charge and discharge conditions, [Charge / discharge conditions] 1 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 2 cycle: -Cut off voltage 3.0V~4.3V -Charge: 0.1C (CCCV) / Discharge: 0.1C (CC) 3 cycles: -Cut off voltage 3.0V~4.4V -Charge: 1C (CCCV) / Discharge: 1C (CC) In a graph showing a voltage V and a battery capacity Q at the third cycle, the X-axis is the voltage V and the Y-axis is a value dQ / dV obtained by differentiating the battery capacity Q with respect to the voltage V, The peak intensity ratio (A) defined by the following formula 1 is satisfied, [Formula 1] I1 / I2≧1.4 (In Equation 1, I1 is the y-axis value dQ / dV of the peak that appears in the phase transformation region from hexagonal to monoclinic between 3.0 V and 3.8 V in the charging region, I2 is the y-axis value dQ / dV of the peak that appears in the phase transformation region from monoclinic to hexagonal between 3.8V and 4.1V in the charging region. A positive electrode active material, wherein a grain boundary density calculated by the following Equation 8 for primary particles arranged on a virtual line crossing a center of the lithium composite oxide in a cross-sectional SEM image of the lithium composite oxide is 0.90 or less: [Formula 8] Grain boundary density=(number of boundaries between primary particles arranged on the imaginary line / number of primary particles arranged on the imaginary line)
11. The positive electrode active material according to claim 10 , wherein the peak intensity ratio (A) defined by the formula 1 is 1.4 or more and 1.92 or less.
12. The positive electrode active material according to claim 10 , comprising a coating layer covering at least a portion of the surface of the lithium composite oxide and comprising a metal oxide represented by the following Chemical Formula 2: [Chemical formula 2] Li x M4 y O z (wherein M4 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Ce, Gd, and Nd, and 0≦x≦10, 0≦y≦8, and 2≦z≦13.)
Citation Information
Patent Citations
Method for producing graphite material having high thermal expansion coefficient and the graphite material
JP2021130580A
Positive electrode active material and lithium secondary battery comprising the same
JP2022064841A
Positive electrode active material and lithium secondary battery containing the same
JP2023027385A
Industrial furnace and combustion control method for industrial furnace
KR1020200059128A
Cathode active material, and cathode, lithium secondary battery comprising the same
KR1020100131921A