Dual-coated high nickel lithium ion cathode material and manufacturing method and use thereof

The double-coated high nickel lithium ion cathode material addresses gas generation issues in high-nickel batteries by combining wet and dry coating techniques, achieving enhanced stability and safety with reduced gas emissions and lower cobalt content.

JP2024160213AActive Publication Date: 2024-11-13GUIZHOU ZHENHUA E CHEM INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024071597
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-25
Publication Date
2024-11-13
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

High-nickel lithium ion batteries suffer from significant gas generation due to their instability and high nickel content, which limits their large-scale use and safety performance.

Method used

A double-coated high nickel lithium ion cathode material is developed through a combination of wet and dry coating processes, where a first coating layer of a metal oxide is applied via wet coating, followed by a second coating layer of a boron-containing compound via dry coating, to stabilize the structure and reduce gas generation.

Benefits of technology

The process enhances the stability and safety of high nickel lithium ion batteries by reducing gas generation, allowing for easier mass production with improved cycle performance and lower cobalt content, thus reducing raw material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160213000015
    Figure 2024160213000015
  • Figure 2024160213000001
    Figure 2024160213000001
  • Figure 2024160213000002
    Figure 2024160213000002
Patent Text Reader

Abstract

To provide a high-nickel cathode material for lithium ion batteries, which has a stable structure and interface, is relatively stable in air, is easy to mass-produce, generates little gas in the manufactured battery, and is highly safe.SOLUTION: The present invention relates to a dual-coated high nickel lithium ion cathode material and a manufacturing method and use thereof. The dual-coated high nickel lithium ion cathode material includes a cathode material substrate, a first coating layer coated on a surface of the cathode material substrate, and a second coating layer coated on a surface of the first coating layer, and the first coating layer and the second coating layer are manufactured by a method including the steps of sequentially coating the cathode material substrate with a metal oxide and coating the cathode material substrate with a boron-containing compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of lithium ion batteries, and in particular to a dual-coated high nickel lithium ion cathode material and its method of manufacture and use, and to low gassing high nickel lithium ion batteries manufactured with said dual-coated high nickel lithium ion cathode material. [Background technology]

[0002] As consumers' requirements for driving range for new energy vehicles continue to grow, high-nickel ternary lithium batteries are becoming more and more popular. In 2022, the proportion of high-nickel ternary lithium batteries installed in vehicles will gradually surpass that of low-nickel ternary lithium batteries. High-nickel lithium-ion batteries (Ni mole fraction ≧ 0.6) have become one of the important development directions in the future. On the one hand, the current high-nickel positive electrode material is mainly in the form of secondary spherical particles, which has a relatively high capacity compared with the single-crystal particle form, but the sintering temperature is relatively low, so the gas generation is also relatively serious. On the other hand, high-nickel positive electrode materials have a high nickel content, so they are unstable in air and are prone to relatively serious gas generation after battery formation.

[0003] Patent Document 1 discloses a double-coated modified lithium-ion battery cathode material including a cathode material substrate, a first coating layer coated on the surface of the substrate, and a second coating layer coated on the surface of the first coating layer. The first coating layer is a nanosheet-like high-speed ion conductor layer, and the second coating layer is an Al compound layer. The patent involves a two-step sintering process. In the coating process, the high-speed ion conductor coating method is to add the cathode material substrate to water and stir to form a uniform slurry A, add ammonium tungstate, ammonium molybdate or ammonium vanadate to water and stir to form a uniform solution B, add solution B and a citric acid solution to slurry A and stir uniformly, heat the mixture until a viscous gel appears, evaporate the moisture, and further dry and dehydrate the gel slurry to obtain a cathode material coated with a nanosheet-like high-speed ion conductor. This coating method is too complicated, requires strict control of process parameters, needs to be heated to dry the moisture, is difficult to industrialize, and also needs to improve the gas generation performance. The substrate material is in a secondary spherical form.

[0004] Patent Document 2 discloses a double-coated cathode material in which the cathode material includes a first coating layer and a second coating layer sequentially coated on the cathode material. The cathode material is Li a Ni x Co y Mn 1-x-y O2, where 0.3 < x < 0.9, 0.1 < y < 0.35, and 0.95 < a < 1.03. The first coating layer and the second coating layer are different. The first coating layer is an LATP layer or an LNTO layer, and the second coating layer is an LNTO layer or an LATP layer. The patent process targets only high-nickel materials of system 9 or below, and the coating material is a high-speed ion conductor. It employs two dry coating steps and two sintering processes. The substrate material is also in a secondary spherical form. The invention alleviates the problems of rapid capacity decay and excessive side reactions existing in the cycle process compared to single coating, but the gas generation performance still needs to be improved.

[0005] Patent Document 3 discloses a Co / B co-coated nickel-cobalt-manganese lithium ion positive electrode material and its manufacturing method. The present invention relates to doping an appropriate amount of F / W in the manufacturing process of the lithium ion positive electrode material, and doping a small amount of F-ions, W 6+ ion doping to improve cycle performance and safety performance. F ions have a very strong electronegativity, so O 2- It suppresses the overflow of ions, stabilizes the structural stability of the material, and plays the role of a framework. 6+ The ions can improve the high-temperature cycle performance of the material, and the Co / B double coating is performed during the two sintering steps of the present invention. The positive electrode material coated with Co / B under high voltage is effective in improving the cycle performance and electronic conductivity of the battery, reducing residual alkali, reducing gas swelling, and reducing the occurrence of side reactions of the positive electrode material when it comes into contact with the electrolyte, but the gas generation performance still needs to be improved.

[0006] In addition, to solve the problem of gas generation performance, most of the prior art adopts the process of cleaning with inorganic or organic solvents, coating after cleaning, and low-temperature sintering. Although the process is relatively simple, the performance is also limited, so there are not many companies with high nickel mass production, and especially when the mole fraction of Ni is ≧0.9, the free lithium is relatively high, and it is difficult to produce products with good performance with the above simple process. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] China Patent Application Publication No. 112349905 [Patent Document 2] China Patent Application Publication No. 111628158 [Patent Document 3] China Patent Application Publication No. 108807926 Summary of the Invention [Problem to be solved by the invention]

[0008] The technical problem that the present invention aims to solve is to provide a dual-coated high-nickel lithium ion positive electrode material, improve the stability of the positive electrode material, reduce the gas generation of high-nickel lithium ion batteries, and improve the safety performance of high-nickel lithium ion batteries.

[0009] Through research, the inventors have found that for high-nickel positive electrode materials with a nickel mole fraction of more than 0.8, a process of wet and dry coating can be adopted, in which strong acid is added in the wet process to etch the surface, followed by wet coating, and then dry coating with a boron-containing fast ion conductor, which can significantly improve the stability of the material and reduce the gas generation performance of the battery. In addition, the sintering temperature after wet coating is relatively high, which is effective in stabilizing the structure and interface, and the sintering temperature after dry coating is relatively low, which is effective in suppressing side reactions between the material and the electrolyte. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention proposes the following technical solutions.

[0011] The present invention provides a dual-coated high nickel lithium ion battery cathode material, comprising a cathode material substrate, a first coating layer coated on the surface of the cathode material substrate, and a second coating layer coated on the surface of the first coating layer; Here, the first coating layer and the second coating layer are produced by a method including the steps of coating a positive electrode material substrate with a metal oxide and then with a boron-containing compound.

[0012] In some embodiments of the present invention, the general chemical formula of the positive electrode material is Li a Ni x Co y Mn z M bIt is O2·cA·dB, where 1.00 ≦ a ≦ 1.20, 0.00 < b ≦ 0.01, 0.00 < c ≦ 0.01, 0.00 < d ≦ 0.05, 0.80 ≦ x < 1.00, 0.00 ≦ y < 0.12, 0.00 ≦ z < 0.2, and x + y + z = 1. M is a doping element, and the M is one or more selected from the group consisting of Mg, Ti, Al, Zr, Ba, and rare earth elements. A is the first coating layer, and B is the second coating layer.

[0013] In some embodiments of the present invention, in the above double-coated high nickel lithium ion battery cathode material, 1.00 ≦ a ≦ 1.20, 0.001 ≦ b ≦ 0.01, 0.80 ≦ x < 1.00, 0.00 ≦ y < 0.12, 0.00 ≦ z < 0.2, 0.0005 < c ≦ 0.01, 0.001 < d ≦ 0.05, and x + y + z = 1. Preferably, 1.02 ≦ a ≦ 1.20, 0.0015 ≦ b ≦ 0.005, 0.80 ≦ x < 1.00, 0.00 ≦ y < 0.12, 0.00 ≦ z < 0.2, 0.0005 < c ≦ 0.01, 0.001 < d ≦ 0.03, and x + y + z = 1.

[0014] Preferably, in the above double-coated high nickel lithium ion battery cathode material, the rare earth element is one or more selected from the group consisting of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, yttrium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, or europium, and preferably yttrium.

[0015] In some embodiments of the present invention, in the above double-coated high nickel lithium ion battery cathode material, the first coating layer is a coating layer formed by wet coating a metal oxide. Preferably, the metal oxide is one or more selected from the group consisting of Al2O3, TiO2, ZrO2, MgO, and rare earth element oxides.

[0016] In some embodiments of the present invention, in the dual-coated high nickel lithium ion battery cathode material, the rare earth oxide is one or more selected from lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, promethium oxide, samarium oxide, yttrium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, lutetium oxide, scandium oxide, or europium oxide, and is preferably yttrium oxide.

[0017] In some embodiments of the present invention, in the above dual-coated high nickel lithium ion battery positive electrode material, the second coating layer is a coating layer formed by dry coating with a boron-containing compound, and preferably, the boron-containing compound is one or more selected from boric acid, lithium borate, lithium metaborate, and lithium tetraborate.

[0018] In some embodiments of the present invention, in the dual-coated high nickel lithium ion battery cathode material, the cathode material is in the form of primary particles or a small amount of primary particles aggregated together.

[0019] In some embodiments of the present invention, in the dual-coated high nickel lithium ion battery cathode material, the cathode material contains <2000 ppm total free lithium, based on the cathode material weight.

[0020] In some embodiments of the present invention, in the dual-coated high nickel lithium ion battery cathode material, the specific surface area of ​​the cathode material is 0.4 to 1.5 m 2 / g, and preferably, the average particle size of the positive electrode material is 2 to 5 μm.

[0021] In some embodiments of the present invention, in the dual-coated high nickel lithium ion battery cathode material, the wet coating comprises mixing a wet coating reagent with a cathode material substrate and then sintering; Preferably, the wet coating reagent comprises a metal oxide and water, and preferably further comprises a strong acid.

[0022] The present invention further provides a method for preparing the above-mentioned dual-coated high nickel lithium ion battery positive electrode material, (1) mixing a lithium source compound, a positive electrode material precursor, and an M source compound to obtain a mixture; Step (2) of subjecting the mixture of step (1) to a first sintering to obtain a positive electrode material substrate; (3) wet-coating the cathode material substrate produced in (2) to obtain a cathode material coated with a first coating layer; and (4) dry-coating the cathode material coated with the first coating layer produced in step (3) to obtain a dual-coated high nickel lithium ion battery cathode material.

[0023] In some embodiments of the present invention, in the above-mentioned production method, the lithium source compound, the positive electrode material precursor and the M source compound have an element molar ratio of Li:(Ni+Co+Mn):M of (1.0-1.2):1.0:(0.00-0.01).

[0024] In some embodiments of the present invention, in the above manufacturing method, the wet coating includes a step of mixing a positive electrode material substrate, water, a strong acid, and a metal oxide, followed by a second sintering step; Preferably, the mass ratio of the positive electrode material substrate to the metal oxide is 1.0:(0.0005 to 0.005), preferably the mass ratio of the positive electrode material substrate to the water is 1:(1.0 to 2.0), and more preferably the mass ratio of the positive electrode material substrate to the strong acid is 1:(0.001 to 0.01); More preferably, the temperature of the second sintering is 600 to 800° C., the sintering time is preferably 6 to 20 hours, and further preferably, the method further includes the steps of filtering and drying after the mixing.

[0025] In some embodiments of the present invention, in the above manufacturing method, the dry coating includes a step of mixing the positive electrode material coated with the first coating layer produced in step (3) and the boron-containing compound, followed by a third sintering step; Preferably, the mass ratio of the positive electrode material coated with the first coating layer to the boron-containing compound is 1.0:(0.002 to 0.02), More preferably, the temperature of the third sintering is 250 to 450° C., and the sintering time is preferably 3 to 15 hours.

[0026] The present invention further provides a low-gassing high-nickel lithium ion battery, which contains the above-mentioned dual-coated high-nickel lithium ion battery positive electrode material or the dual-coated high-nickel lithium ion battery positive electrode material prepared by the above-mentioned preparation method.

[0027] In some embodiments of the present invention, the low gas generation high nickel lithium ion battery has an initial discharge capacity of 190-210 mAh / g under a charge / discharge condition of 4.2 V, 1 C.

[0028] In some embodiments of the present invention, the low gassing high nickel lithium ion battery has a thickness expansion rate of 32% or less when stored at 4.25 V and 70° C. for 30 days.

[0029] The present invention further provides the use of the above-mentioned dual-coated high nickel lithium ion battery cathode material or the dual-coated high nickel lithium ion battery cathode material prepared by the above-mentioned preparation method or the above-mentioned low gassing high nickel lithium ion battery in digital products, electric vehicles or energy storage fields. Effect of the Invention

[0030] The beneficial effects of the present invention include the following: The high nickel positive electrode material for lithium ion batteries of the present invention has a stable structure and interface, is relatively stable in air, is easy to mass-produce, and the produced battery generates little gas and has high safety. The high nickel positive electrode material for lithium ion batteries of the present invention has the form of primary particles and secondary particles formed by agglomeration of a small amount of primary particles, has a high specific capacity, and is excellent in cycle performance. The high nickel positive electrode material for lithium ion batteries of the present invention has a low cobalt content, which significantly reduces raw material costs. [Brief description of the drawings]

[0031] [Figure 1] 1 is a scanning electron microscope photograph of the positive electrode material prepared in Example 1 of the present invention, magnified at 3000 times. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] In the present invention, unless otherwise specified in a particular case, the numerical ranges described herein include upper and lower limits, and "greater than" and "less than" are not limited to the specific values ​​described in defining the range, but include the endpoints and all integers and fractions within the range. In this case, "and / or" is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0033] High-nickel lithium ion positive electrode materials have a high nickel content and are relatively unstable in air, so batteries manufactured using the high-nickel lithium ion positive electrode materials have high gassing and significant safety concerns, limiting the large-scale use of high-nickel lithium ion positive electrode materials. The present invention provides a dual-coated high-nickel lithium ion battery positive electrode material and a low-gassing high-nickel lithium ion secondary battery manufactured using the positive electrode material.

[0034] According to the first aspect, in one specific embodiment of the present invention, the present invention provides a double-coated high-nickel lithium-ion battery cathode material, which includes a cathode material substrate, a first coating layer coated on the surface of the cathode material substrate, and a second coating layer coated on the surface of the first coating layer. Here, the double-coated high-nickel lithium-ion battery cathode material is manufactured by a method including the steps of sequentially wet-coating and dry-coating the cathode material substrate.

[0035] In some embodiments of the present invention, the chemical general formula of the double-coated high-nickel lithium-ion battery cathode material is Li a Ni x Co y Mn z M b O2·cA·dB, where 1.00 ≦ a ≦ 1.20, 0.00 < b ≦ 0.01, 0.00 < c ≦ 0.01, 0.00 < d ≦ 0.05, 0.80 ≦ x < 1.00, 0.00 ≦ y < 0.12, 0.00 ≦ z < 0.2, and x + y + z = 1. M is a doping element, and M is one or more selected from the group consisting of Mg, Ti, Al, Zr, Ba, and rare earth elements. A is the first coating layer, and B is the second coating layer.

[0036] In some embodiments of the present invention, the chemical general formula of the double-coated high-nickel lithium-ion battery cathode material is Li a Ni x Co y Mn z M bIt is O2·cA·dB, where 1.00 ≦ a ≦ 1.20, 0.001 ≦ b ≦ 0.01, 0.80 ≦ x < 1.00, 0.00 ≦ y < 0.12, 0.00 ≦ z < 0.2, 0.0005 < c ≦ 0.01, 0.001 < d ≦ 0.05, x + y + z = 1, M is a doping element, and the M is one or more selected from the group consisting of Mg, Ti, Al, Zr, Ba, and rare earth elements. A is the first coating layer, B is the second coating layer. Preferably, 1.02 ≦ a ≦ 1.20, more preferably 1.10 ≦ a ≦ 1.20, more preferably 0.83 ≦ x ≦ 0.92, preferably 0.03 ≦ y ≦ 0.07, more preferably 0.03 ≦ z ≦ 0.1, still more preferably 0.0015 ≦ b ≦ 0.005, and even more preferably 0.002 ≦ b ≦ 0.003.

[0037] Hereinafter, the types of elements, compounds of the coating layer, and contents in the positive electrode material of the present invention will be described.

[0038] The inventors of the present invention have found that in the chemical general formula of the positive electrode material of the present invention, the doping element of the present invention is one or more selected from the group consisting of Mg, Ti, Al, Zr, Ba, and rare earth elements. Here, the rare earth element is one or more selected from lanthanum, cerium, praseodymium, neodymium, promethium, samarium, yttrium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, or europium. By selecting a chemical element close to the matrix element instead of the vacancies of some matrix elements, the skeletal structure of the material can be stabilized.

[0039] In some embodiments of the present invention, the first coating layer is a coating layer formed of a metal oxide, and the metal oxide is one or more selected from the group consisting of Al2O3, TiO2, ZrO2, MgO, and rare earth element oxides. Here, the rare earth element oxides are one or more selected from lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, promethium oxide, samarium oxide, yttrium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, lutetium oxide, scandium oxide, or europium oxide. By selecting chemical elements close to the substrate element and performing a shallow coating, the shallow interface can be stabilized and side reactions with the electrolyte can be suppressed.

[0040] In some preferred embodiments of the present invention, the second coating layer is a coating layer formed of a boron-containing compound. Preferably, the boron-containing compound is one or more selected from boric acid, lithium borate, lithium metaborate, or lithium tetraborate.

[0041] In some embodiments of the present invention, in the above chemical general formula, 0.0005 < c ≤ 0.01 and 0.001 < d ≤ 0.03. If the coating layer is too thick, it will affect the performance of the capacity. Preferably, 0.00075 ≤ c ≤ 0.003, more preferably, 0.002 ≤ c ≤ 0.003, still more preferably, 0.002 < d ≤ 0.01, and even more preferably, 0.0025 ≤ d ≤ 0.01.

[0042] In some embodiments of the present invention, the positive electrode material powder includes primary particles and secondary particles formed by aggregation of a small amount of primary particles as observed by a scanning electron microscope (SEM).

[0043] When the positive electrode material of the present invention is in the form of primary particles, it means that the positive electrode material is in the form of primary particles and secondary particles formed by aggregation of a small amount of primary particles.

[0044] The term "secondary particles formed by agglomeration of a small amount of primary particles" refers to a situation in which the percentage of secondary particles formed by agglomeration of primary particles in the positive electrode material is less than 10%.

[0045] The term "single crystal" or "single crystal-like" as used herein refers to the positive electrode material having a primary particle morphology characteristic.

[0046] In some embodiments of the present invention, the positive electrode material contains <2000 ppm total free lithium, based on the weight of the positive electrode material.

[0047] In some embodiments of the present invention, the specific surface area of ​​the positive electrode material is 0.4 to 1.5 m 2 / g, and preferably the average particle size of the positive electrode material is 2 to 5 μm.

[0048] According to a second aspect, the present invention further provides a method for producing the above dual-coated high nickel lithium ion battery cathode material, (1) mixing a lithium source compound, a positive electrode material precursor, and an M source compound to obtain a mixture; Step (2) of subjecting the mixture of step (1) to a first sintering to obtain a positive electrode material substrate; (3) wet-coating the cathode material substrate produced in (2) to obtain a cathode material coated with a first coating layer; and (4) dry-coating the cathode material coated with the first coating layer produced in step (3) to obtain a dual-coated high nickel lithium ion battery cathode material.

[0049] It should be understood that the above-mentioned positive electrode material precursor includes one or more of nickel-cobalt-manganese precursor, nickel-cobalt precursor, or nickel-manganese precursor. For example, the nickel-cobalt-manganese precursor is one or more of hydroxide, carboxyl oxide, or oxide containing nickel, cobalt, and manganese elements, and has a particle size of 3 μm to 20 μm.

[0050] In some embodiments of the present invention, the lithium source compound, the positive electrode material precursor, and the M source compound have an elemental molar ratio of Li:(Ni+Co+Mn):M of (1.0-1.2):1.0:(0.00-0.01), and preferably the lithium source compound, the positive electrode material precursor, and the M source compound have an elemental molar ratio of Li:(Ni+Co+Mn):M of (1.0-1.2):1.0:(0.0013-0.005).

[0051] In some embodiments of the present invention, the wet coating includes a step of mixing the positive electrode material substrate and a wet coating reagent followed by a second sintering step, where the wet coating reagent includes a metal oxide, a strong acid, and water.

[0052] In some embodiments of the present invention, the mass ratio of the positive electrode material substrate to a metal oxide is 1.0:(0.0005 to 0.005), preferably 1.0:(0.0016 to 0.003), the mass ratio of the positive electrode material substrate to water is 1.0:(1.0 to 2.0), preferably 1.0:(1.2 to 2), the mass ratio of the positive electrode material substrate to a strong acid is 1.0:(0.001 to 0.01), preferably 1.0:(0.001 to 0.006), more preferably 1.0:(0.005 to 0.006), In some embodiments of the present invention, the temperature of the second sintering is 600-800°C, preferably 700-780°C, and the sintering time is preferably 6-20h, preferably 8-10h, and more preferably further includes a step of filtering and drying after the mixing.

[0053] In the present invention, the strong acid is not particularly limited and may be any commercially available common strong acid, for example, one or more of sulfuric acid, hydrochloric acid, and nitric acid.

[0054] In some embodiments of the present invention, the dry coating includes mixing the positive electrode material coated with the first coating layer produced in step (3) and the boron-containing compound, followed by a third sintering step; In some embodiments of the present invention, the mass ratio of the positive electrode material coated with the first coating layer to the boron-containing compound is 1.0:(0.002 to 0.02), preferably 1.0:(0.004 to 0.006), the sintering temperature is 250 to 450°C, preferably 250 to 300°C, and the sintering time is more preferably 3 to 15 hours, preferably 8 to 12 hours.

[0055] It should be understood that the sintering in the wet coating step is a second sintering, and the sintering in the dry coating step is a third sintering.

[0056] In some embodiments of the present invention, the first sintering, the second sintering and the third sintering are followed by a step of crushing selected from airflow crushing and classification, and the first sintering, the second sintering and the third sintering are all protected by an oxygen atmosphere.

[0057] In some embodiments of the present invention, the lithium source compound includes one or more of a lithium-containing oxide, hydroxide, carbonate, sulfate, or nitrate, including, but not limited to, for example, lithium hydroxide monohydrate.

[0058] In some embodiments of the present invention, the M source compound includes one or more of an oxide, hydroxide, carbonate, sulfate, or nitrate containing an M element, and is preferably an oxide or nitrate, for example, including, but not limited to, one or more of aluminum oxide, titanium oxide, magnesium oxide, yttrium oxide, barium oxide, or zirconium oxide.

[0059] In some embodiments of the present invention, the metal oxide is one or more selected from the group consisting of Al2O3, TiO2, ZrO2, MgO, and rare earth element oxides, and the rare earth element oxide is one or more selected from lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, promethium oxide, samarium oxide, yttrium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, lutetium oxide, scandium oxide, or europium oxide.

[0060] In some embodiments of the present invention, the second coating layer is a coating layer formed of a boron-containing compound, and preferably, the boron-containing compound is one or more selected from boric acid, lithium borate, lithium metaborate, and lithium tetraborate.

[0061] According to a third aspect, the present invention further provides a low gassing high nickel lithium ion battery, the low gassing high nickel lithium ion battery comprising the above-mentioned duplex coated high nickel positive electrode material or the duplex coated high nickel positive electrode material produced by the above-mentioned production method.

[0062] In some embodiments of the present invention, the low gas generation high nickel lithium ion battery has an initial discharge capacity of 190-210 mAh / g under a charge / discharge condition of 4.2 V, 1 C.

[0063] In some preferred embodiments of the present invention, the low gassing high nickel lithium ion battery has a thickness expansion rate of 32% or less, preferably less than 30%, after storage at 70° C. for 30 days.

[0064] It should be understood that the low gassing high nickel lithium ion battery of the present invention includes electrodes, a non-aqueous electrolyte, a separator, and a container, where the electrodes include a positive electrode and a negative electrode, and the positive electrode includes a positive electrode current collector and a positive electrode coating material applied to the positive electrode current collector. The current collector may be various current collectors well known to those skilled in the art, such as aluminum foil, copper foil followed by nickel-plated steel strip, etc., and the positive electrode coating material includes a positive electrode active material, a binder, and a conductive agent, where the positive electrode active material is the dual-coated high nickel lithium ion positive electrode material of the present invention, the positive electrode conductive agent includes, but is not limited to, one or more of carbon black conductive agent, carbon nanotubes (CNT), SP-Li, flake graphite, Ketjen black, VGCF, and CNF, and the binder includes, but is not limited to, one or more of polyvinylidene fluoride (PVDF), vinylidene fluoride (VF2) homopolymer and polyvinylidene fluoride copolymer, and vinylidene fluoride (VF2) / hexafluoropropylene (HFP) copolymer.

[0065] The negative electrode includes a current collector and a negative electrode coating material applied to the current collector. The current collector may be various current collectors well known to those skilled in the art, such as aluminum foil, copper foil followed by nickel-plated steel strip, etc. The negative electrode coating material includes a negative electrode active material, a binder, and a conductive agent. The negative electrode active material includes, but is not limited to, artificial graphite (C) or mesocarbon microbeads. The conductive agent includes, but is not limited to, one or more of carbon black conductive agent, carbon nanotubes (CNT), SP-Li, conductive graphite, flake graphite, Ketjen black, VGCF, and CNF. The binder includes, but is not limited to, one or more of polyvinylidene fluoride (PVDF), styrene butadiene rubber emulsion (SBR), and sodium carboxymethyl cellulose (CMC).

[0066] It should be understood that the separator is a PP / PE film conventionally used in the industry to separate positive and negative electrodes from each other, and the container is an enclosure for the positive electrode, negative electrode, separator, and electrolyte.

[0067] According to a fourth aspect, the present invention further provides the use of said duplex-coated high-nickel cathode material or said duplex-coated high-nickel cathode material produced by said production method, or said low-gassing high-nickel lithium ion battery in the fields of digital products, electric vehicles or energy storage.

[0068] The material of the present invention and its manufacturing method and use will be described below with reference to specific examples. However, any reagents or equipment not described in the specification of the present application are within the ordinary skill of the art.

[0069] The reagents used in the following examples are shown in Table 1.

[0070] [Table 1-1]

[0071] [Table 1-2]

[0072] Example 1 A double planetary ball mill was milled with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Ti=1.2:1:0.005. 0.92 Co 0.03 Mn 0.05(OH)2) and nano titanium dioxide powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, and then the material (i.e., the mixed material) was discharged. The mixed material was placed in a muffle furnace, and heated to 800 ° C at a heating rate of 5 ° C / min in an oxygen atmosphere and sintered for 25 hours (first sintering), cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material 1 for a positive electrode material (i.e., a positive electrode material substrate). Then, the mass ratio of water: main material 1: sulfuric acid: alumina was weighed to be 1.5: 1.0: 0.006: 0.0012, and the total was 1 kg. Water, main material, and sulfuric acid (98 wt%) were added to the reaction kettle in order, mixed and stirred for 10 minutes, and alumina was added, stirring was continued for 10 minutes, suction filtration was performed, and drying was performed at 120 ° C. The dried sample was heated to 600°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 18 hours (second sintering), and cooled to room temperature. The sample after the second sintering was further pulverized by an airflow pulverizer at a pulverization pressure of 0.65MPa to obtain the main material 2 for the positive electrode material (i.e., the positive electrode material coated with the first coating layer), and then weighed so that the mass ratio of the main material 2:boric acid was 1.0:0.004, totaling 1 kg. The weighed boric acid was added to the main material 2, ball milled at a rotation speed of 40Hz for 10 minutes, and the uniformly mixed material was placed in a muffle furnace, heated to 450°C at a heating rate of 5°C / min in an air atmosphere, sintered for 6 hours, cooled to room temperature, and sieved through a 300-mesh wire screen to obtain a double-coated high-nickel lithium-ion battery positive electrode material 1.

[0073] The elemental composition analysis was carried out on the dual-coated high nickel lithium ion battery positive electrode material 1 using the following test method, and the results are shown in Table 2. The chemical formula of the final positive electrode material is Li 1.2 Ni 0.92 Co 0.03 Mn 0.05 Ti 0.005 O2·0.0012Al2O3·0.006 Li3BO3.

[0074] 0.2000 g (accurate to 0.0001 g) of sample was accurately weighed into a clean 100 mL glass beaker. 10 mL (1:1) of aqua regia solution was added to the beaker (also a blank test was performed), the surface dish was placed on the beaker, and the solution was heated and evaporated to near dryness by placing it on a hot plate, after which the heating was stopped, the beaker was removed, and the solution was cooled to room temperature. The surface dish and the side walls of the beaker were rinsed with deionized water and washed at least three times, and all the solution was transferred to a 50 mL measuring bottle, made to volume with deionized water, and shaken. 1 mL of sample was transferred to a 100 mL measuring bottle, made to volume, and shaken. The above solution was tested using an inductively coupled plasma optical emission spectrometer (Thermo Fisher Scientific Inc., USA / icap7400) with reference to the first part of YS / T 1006.2-2014.

[0075] [Table 2]

[0076] The physical parameters of the dual-coated high nickel lithium ion battery positive electrode material were tested according to the following methods. 1) Test of average particle size: Tested using MS3000 laser particle sizer, the method is as follows, and the test results are shown in Table 12. An appropriate amount of sample was taken in a 100 ml beaker, and the inner wall of the beaker was washed once with a washing bottle, and the sample attached to the bottom of the beaker was washed with a washing bottle. The amount of pure water added to the beaker was controlled to 20-30 mL, and the ultrasonic time was set to 5 min (stirring for 10 s each before, during, and after ultrasonic, and the stirring speed was about 2 r / s). 100 ± 10 ml of pure water was added to the sampler of the MS3000 laser particle sizer, the rotation speed was adjusted to 3000 r / min, and start was clicked, and the instrument automatically waited for the presentation against the light and measurement background to operate. The sample after the ultrasonic wave was finished was transferred to the stirring tank, and the beaker was further washed with a washing bottle to ensure that all the sample was transferred. After the sample was completely added, the software automatically started the measurement. When the measurement was completed, the data was automatically saved. 2) Specific surface area test: The analysis test was performed using a fully automatic specific surface area and porosity analyzer (TriStar II 3020, Micromeritics, Inc., USA), and the test results are shown in Table 12. 3) The test method for free lithium is as follows, and the test results are shown in Table 12. Accurately weigh out an appropriate amount of sample (approximately 30 g), accurate to 0.01 g. Place the sample in a 250 mL Erlenmeyer flask, add a magnetic stirring bar, add 100 mL of deionized water, place the Erlenmeyer flask on a magnetic stirrer, start the stirrer and stir for 30 minutes, filter the mixed solution through filter paper and a funnel, transfer 50 mL of the filtrate with a 50 mL pipette, place in a 100 mL beaker, add a magnetic stirring bar, place the beaker on a magnetic stirrer, add 2 drops of phenolphthalein indicator, and titrate with 0.05 mol / L hydrochloric acid standard titration solution until the color of the solution changes from red to colorless. Record the volume V1 (end point 1) of the 0.05 mol / L hydrochloric acid standard titration solution, add 2 drops of methyl red indicator, the color changes from colorless to yellow, titrate with 0.05 mol / L hydrochloric acid standard titration solution until the color of the solution changes from yellow to orange, place the beaker in a heating furnace and heat until the solution boils (until the color of the solution changes from orange to yellow), remove the 100 mL beaker, cool to room temperature, place the beaker on a magnetic stirrer again, titrate with 0.05 mol / L hydrochloric acid standard titration solution until the color of the solution changes from yellow to light red, record the volume V2 (end point 2) of the 0.05 mol / L hydrochloric acid standard titration solution, Lithium hydroxide: LiOH (wt%) = [V2-2 x (V2-V1)] x 0.05 x 23.946 x 2 x 100 / (m x 1000) Lithium carbonate: Li2CO3 (wt%) = (V2-V1) x 0.05 x 73.886 x 2 x 100 / (m x 1000) Total free lithium: Li + (wt%)=V2×0.05×6.94×2×100 / (m×1000) m - mass of sample in g, V1 is the first titration endpoint, and V2 is the second titration endpoint. 4) Morphological test of positive electrode material: The positive electrode material 1 of Example 1 was subjected to SEM testing, and the test parameters were selected as follows: acceleration voltage EHT=15.00 kV, working distance WD=7.0 mm, and probe Signal A=InLens. As shown in FIG. 1, it can be seen from FIG. 1 that the material is in the form of primary particles, that is, primary particles and a small amount of secondary particles formed by agglomeration of the primary particles.

[0077] Example 2 The double planetary ball mill was charged with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Zr=1.08:1:0.002, and a molar ratio of Ni:Co:Mn=92:03:05. 0.92 Co 0.03 Mn 0.05 Add (OH)2) and nano-zirconia powder in a total of 1 kg, ball mill at 40Hz for 10 minutes to mix uniformly, then discharge the material (i.e., mixed material). The mixed material is placed in a muffle furnace, heated to 830℃ at a heating rate of 5℃ / min under oxygen atmosphere, and sintered for 20 hours (first sintering), cooled to room temperature, ball milled at 40Hz for 10 minutes to obtain main material 1 for positive electrode material. Then, weigh out the water:main material 1:sulfuric acid:titanium dioxide mass ratio to be 2.0:1.0:0.005:0.0016, totaling 1 kg. Add water, main material, and sulfuric acid (98wt%) in the reaction vessel in order, mix and stir for 10 minutes, add titanium dioxide, continue stirring for 10 minutes, suction filter, and dry at 120℃. The dried sample was heated to 700°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 8 hours (second sintering), and cooled to room temperature. The sample after the second sintering was further crushed by an airflow crusher at a crushing pressure of 0.65 MPa to obtain a main material 2 for a positive electrode material. The main material 2 and lithium borate were weighed so that the mass ratio of the main material 2 to lithium borate was 1.0:0.006, totaling 1 kg. The lithium borate was added to the main material 2, ball milled at a rotation speed of 40 Hz for 10 minutes, and the uniformly mixed material was placed in a muffle furnace, heated to 250°C at a heating rate of 5°C / min in an air atmosphere, sintered for 12 hours, cooled to room temperature, and sieved through a 300-mesh wire screen to obtain a double-coated high-nickel lithium-ion battery positive electrode material 2.

[0078] According to the method of Example 1, the primary particle size, specific surface area and total free lithium content of the dual-coated high nickel lithium ion battery positive electrode material are tested, and the results are shown in Table 12.

[0079] Using the test method in Example 1, the dual-coated high nickel lithium ion battery positive electrode material 2 was subjected to elemental composition analysis. The results are shown in Table 3. The chemical formula of the final positive electrode material is Li 1.08 Ni 0.92 Co 0.03 Mn 0.05 Zr 0.002 O2·0.002TiO2·0.008Li3BO3.

[0080] [Table 3]

[0081] Example 3 The double planetary ball mill was charged with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Al=1.1:1:0.003, and a molar ratio of Ni:Co:Mn=87:05:08. 0.87 Co 0.05 Mn 0.08(OH)2) and nano-alumina powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, after which the material (i.e., the mixed material) was discharged, and the mixed material was placed in a muffle furnace, heated to 860 ° C at a heating rate of 5 ° C / min in an oxygen atmosphere, and sintered for 20 hours (first sintering), cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material 1 for a positive electrode material. Then, water, main material 1, sulfuric acid, and zirconia were weighed in a total of 1 kg so that the mass ratio of water: main material 1: sulfuric acid: zirconia was 1.2: 1.0: 0.005: 0.003, and water, main material, and sulfuric acid were added in sequence to a reaction kettle, mixed and stirred for 10 minutes, and zirconia was added, stirring was continued for 10 minutes, suction filtration was performed, and drying was performed at 120 ° C. The dried sample was heated to 750°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 10 hours (second sintering), and cooled to room temperature. The sample after the second sintering was further crushed by an airflow crusher at a crushing pressure of 0.65 MPa to obtain a main material 2 for a positive electrode material. Then, the main material 2 and lithium metaborate were weighed out in total to 1 kg so that the mass ratio of the main material 2 to lithium metaborate was 1.0:0.005, lithium metaborate was added to the main material 2, and ball milled at a rotation speed of 40 Hz for 10 minutes. The uniformly mixed material was placed in a muffle furnace, heated to 300°C at a heating rate of 5°C / min in an air atmosphere, sintered for 8 hours, cooled to room temperature, and sieved through a 300-mesh wire screen to obtain a double-coated high-nickel lithium-ion battery positive electrode material 3.

[0082] According to the method of Example 1, the primary particle size, specific surface area and total free lithium content of the dual-coated high nickel lithium ion battery positive electrode material 3 are tested, and the results are shown in Table 12.

[0083] Using the test method in Example 1, the dual-coated high nickel lithium ion battery positive electrode material 3 was subjected to elemental composition analysis. The results are shown in Table 4. The final chemical formula of the positive electrode material is Li 1.1 Ni 0.87 Co 0.05 Mn 0.08 Al 0.003 O2·0.0025ZrO2·0.01LiBO2.

[0084] [Table 4]

[0085] Example 4 The double planetary ball mill was charged with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Zr=1.12:1:0.002, and a molar ratio of Ni:Co:Mn=83:07:10. 0.83 Co 0.07 Mn 0.1 (OH)2) and nano-zirconia powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, after which the material (i.e., the mixed material) was discharged, and the mixed material was placed in a muffle furnace, heated to 880 ° C at a heating rate of 5 ° C / min in an oxygen atmosphere, sintered for 24 hours, cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material 1 for a positive electrode material. Then, water, main material 1, sulfuric acid, and alumina were weighed in a total of 1 kg so that the mass ratio of water: main material 1: sulfuric acid: alumina was 1.5: 1.0: 0.005: 0.003 in the reaction kettle, and water, main material, and sulfuric acid (98 wt%) were added in sequence to the reaction kettle, mixed and stirred for 10 minutes, further alumina was added, stirring was continued for 10 minutes, suction filtration was performed, and dried at 120 ° C. The dried sample was heated to 780°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 10 hours (second sintering), and cooled to room temperature. The sample after the second sintering was further crushed by an airflow crusher at a crushing pressure of 0.65 MPa to obtain a main material 2 for a positive electrode material. Then, the main material 2 and lithium tetraborate were weighed out in total to 1 kg so that the mass ratio of the main material 2 to lithium tetraborate was 1.0:0.004, and the lithium tetraborate was added to the main material 2, and ball milled at a rotation speed of 40 Hz for 10 minutes. The uniformly mixed material was placed in a muffle furnace, heated to 280°C at a heating rate of 5°C / min in an air atmosphere, sintered for 8 hours, cooled to room temperature, and sieved through a 300-mesh wire screen to obtain a double-coated high-nickel lithium-ion battery positive electrode material 4.

[0086] According to the method of Example 1, the primary particle size, specific surface area and total free lithium content of the dual-coated high nickel lithium ion battery positive electrode material 4 are tested, and the results are shown in Table 12.

[0087] Using the test method in Example 1, the dual-coated high nickel lithium ion battery positive electrode material 4 was subjected to elemental composition analysis. The results are shown in Table 5. The final chemical formula of the positive electrode material is Li 1.12 Ni 0.83 Co 0.07 Mn 0.10 Zr 0.002 O2·0.003Al2O3·0.0025Li2B4O7.

[0088] [Table 5]

[0089] Example 5 The double planetary ball mill was charged with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Zr=1.1:1:0.0013, and a molar ratio of Ni:Co:Mn=87:05:08. 0.87 Co 0.05 Mn 0.08(OH)2) and nano-zirconia powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, after which the material (i.e., the mixed material) was discharged, and the mixed material was placed in a muffle furnace, heated to 810 ° C at a heating rate of 5 ° C / min in an oxygen atmosphere, sintered for 30 hours, cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material 1 for a positive electrode material. Then, water, main material 1, sulfuric acid, and alumina were weighed in a total of 1 kg so that the mass ratio of water: main material 1: sulfuric acid: alumina was 1.2: 1.0: 0.005: 0.0024, and water, main material, and sulfuric acid (98 wt%) were added in sequence to the reaction kettle, mixed and stirred for 10 minutes, and alumina was further added, stirring was continued for 10 minutes, suction filtration, and drying at 120 ° C. The dried sample was heated to 760°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 12 hours (second sintering), and cooled to room temperature. The sample after the second sintering was further crushed by an airflow crusher at a crushing pressure of 0.65 MPa to obtain a main material 2 for a positive electrode material. Then, the main material 2 and boric acid were weighed out in total at 1 kg so that the mass ratio of the main material 2 to boric acid was 1.0:0.004, and boric acid was added to the main material 2, and ball milled at a rotation speed of 40 Hz for 10 minutes. The uniformly mixed material was placed in a muffle furnace, heated to 320°C at a heating rate of 5°C / min in an air atmosphere, sintered for 6 hours, cooled to room temperature, and sieved through a 300-mesh wire screen to obtain a double-coated high-nickel lithium-ion battery positive electrode material 5.

[0090] According to the method of Example 1, the primary particle size, specific surface area and total free lithium content of the dual-coated high nickel lithium ion battery positive electrode material 5 are tested, and the results are shown in Table 12.

[0091] Using the test method in Example 1, the dual-coated high nickel lithium ion battery positive electrode material 5 was subjected to elemental composition analysis. The results are shown in Table 6. The chemical formula of the final positive electrode material is Li 1.1 Ni 0.87 Co 0.05 Mn 0.08 Zr 0.0016 O2·0.0024Al2O3·0.0065Li3BO3.

[0092] [Table 6]

[0093] Example 6 A double planetary ball mill was milled with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Y=1.02:1:0.002, and a molar ratio of Ni:Co:Mn=92:05:03. 0.92 Co 0.05 Mn 0.03 (OH)2) and yttrium oxide powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, after which the material (i.e., the mixed material) was discharged, and the mixed material was placed in a muffle furnace, heated to 850 ° C. at a heating rate of 5 ° C. / min in an oxygen atmosphere, and sintered for 8 hours (first sintering), cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material 1 for a positive electrode material. Then, water, main material 1, nitric acid, and niobium oxide were weighed in a total of 1 kg so that the mass ratio of water: main material 1: nitric acid: niobium oxide was 1.0: 1.0: 0.001: 0.002, and water, main material, and nitric acid (65 wt%) were added in sequence to the reaction kettle, mixed and stirred for 10 minutes, and niobium oxide was further added, stirring was continued for 10 minutes, suction filtration was performed, and drying was performed at 120 ° C. The dried sample was heated to 720°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 20 hours (second sintering), and cooled to room temperature. The sample after the second sintering was further crushed by an airflow crusher at a crushing pressure of 0.65 MPa to obtain a main material 2 for a positive electrode material. Then, the main material 2 and lithium borate were weighed out in total at 1 kg so that the mass ratio of the main material 2 to lithium borate was 1.0:0.02, the lithium borate was added to the main material 2, and ball milled at a rotation speed of 40 Hz for 10 minutes. The uniformly mixed material was placed in a muffle furnace, heated to 350°C at a heating rate of 5°C / min in an air atmosphere, sintered for 3 hours, cooled to room temperature, and sieved through a 300-mesh wire screen to obtain a double-coated high-nickel lithium-ion battery positive electrode material 6.

[0094] According to the method of Example 1, the primary particle size, specific surface area and total free lithium content of the dual-coated high nickel lithium ion battery positive electrode material 6 are tested, and the results are shown in Table 12.

[0095] Using the test method in Example 1, the dual-coated high nickel lithium ion battery positive electrode material 6 was subjected to elemental composition analysis. The results are shown in Table 7. The final chemical formula of the positive electrode material is Li 1.02 Ni 0.92 Co 0.05 Mn 0.03 Y 0.002 O2·0.00075Nb2O5·0.03Li3BO3.

[0096] [Table 7]

[0097] Example 7 The difference from Example 6 is that nitric acid is not added to the wet coating, and the specific method is as follows:

[0098] A double planetary ball mill was milled with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Y=1.02:1:0.002, and a molar ratio of Ni:Co:Mn=92:05:03. 0.92 Co 0.05 Mn 0.03(OH)2) and yttrium oxide powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, after which the material (i.e., the mixed material) was discharged, and the mixed material was placed in a muffle furnace, and in an oxygen atmosphere, the temperature was raised to 850 ° C. at a heating rate of 5 ° C. / min, and sintered for 8 hours (first sintering), cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material 1 for a positive electrode material. Then, water, main material 1, and niobium oxide were weighed in a total of 1 kg so that the mass ratio of water: main material 1: niobium oxide was 1.0:1.0:0.002, and water and main material were added in sequence to the reaction kettle, mixed and stirred for 10 minutes, further niobium oxide was added, stirring was continued for 10 minutes, suction filtration was performed, and the mixture was dried at 120 ° C. The dried sample was heated to 720 ° C. at a heating rate of 10 ° C. / min, and sintered for 20 hours (second sintering) in an oxygen atmosphere, and cooled to room temperature. Furthermore, the sample after the second sintering was pulverized by an airflow pulverizer at a pulverization pressure of 0.65 MPa to obtain a main material 2 for a positive electrode material. Then, the main material 2 and lithium borate were weighed out in a total of 1 kg so that the mass ratio of the main material 2 to lithium borate was 1.0:0.02, the lithium borate was added to the main material 2, and the mixture was ball milled at a rotation speed of 40 Hz for 10 minutes. The uniformly mixed material was placed in a muffle furnace, heated to 350°C at a heating rate of 5°C / min in an air atmosphere, sintered for 3 hours, cooled to room temperature, and sieved through a 300-mesh wire screen to obtain a double-coated high-nickel lithium-ion battery positive electrode material 7.

[0099] According to the method of Example 1, the primary particle size, specific surface area and total free lithium content of the dual-coated high nickel lithium ion battery positive electrode material 7 are tested, and the results are shown in Table 12.

[0100] Using the test method in Example 1, the dual-coated high nickel lithium ion battery positive electrode material 7 was subjected to elemental composition analysis. The results are shown in Table 8. The final chemical formula of the positive electrode material is Li 1.02 Ni 0.92 Co 0.05 Mn 0.03 Y 0.002 O2·0.00075Nb2O5·0.03Li3BO3.

[0101] [Table 8]

[0102] Comparative Example 1 The double planetary ball mill was charged with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Zr=1.12:1:0.002, and a molar ratio of Ni:Co:Mn=83:07:10. 0.83 Co 0.07 Mn 0.1 (OH)2) and nano-zirconia powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, after which the material (i.e., the mixed material) was discharged, and the mixed material was placed in a muffle furnace, heated to 880 ° C at a heating rate of 5 ° C / min under an oxygen atmosphere, sintered for 24 hours, cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material 1 for a positive electrode material. Then, water, main material 1, sulfuric acid, and alumina were weighed in a total of 1 kg so that the mass ratio of water: main material 1: sulfuric acid: alumina was 1.5: 1.0: 0.005: 0.003, and water, main material, and sulfuric acid were added in sequence, mixed and stirred for 10 minutes, alumina was further added, stirring was continued for 10 minutes, suction filtration was performed, and the mixture was dried at 120 ° C. The dried sample was heated to 780 ° C at a heating rate of 10 ° C / min under an oxygen atmosphere, sintered for 10 hours (second sintering), and cooled to room temperature. Furthermore, the sample after the second sintering was air-flow crushed and sieved through a 300-mesh wire screen to obtain a positive electrode material D1.

[0103] The primary particle size, specific surface area and total free lithium content of the positive electrode material D1 were tested according to the methods described in Example 1, and the results are shown in Table 12.

[0104] The elemental composition analysis of the positive electrode material D1 was carried out using the test method in Example 1. The results are shown in Table 9. The chemical formula of the finally obtained positive electrode material D1 is Li 1.12 Ni 0.83 Co 0.07 Mn 0.10 Zr 0.002 O2·0.003Al2O3.

[0105] [Table 9]

[0106] Comparative Example 2 The molar ratio of Li:(Ni+Co+Mn):Zr=1.12:1:0.002 was added to a ball mill, and lithium hydroxide monohydrate and a precursor (chemical formula: Ni 0.83 Co 0.07 Mn 0.1 (OH)2) and nano-zirconia powder were added in a total of 1 kg, and the mixture was uniformly mixed by ball milling at a rotation speed of 40 Hz for 10 minutes, and then the material (i.e., the mixed material) was discharged. The mixed material was placed in a muffle furnace, heated to 880 ° C. at a heating rate of 5 ° C. / min in an oxygen atmosphere, sintered for 24 hours, cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain a main material for a positive electrode material 1. Then, lithium tetraborate was weighed out in a total of 1 kg so that the mass ratio of main material 1:lithium tetraborate was 1.0:0.004, lithium tetraborate was added to main material 1, and ball milled at a rotation speed of 40 Hz for 10 minutes. The uniformly mixed material was placed in a muffle furnace, heated to 280 ° C. at a heating rate of 5 ° C. / min in an air atmosphere, sintered for 8 hours, cooled to room temperature, and sieved through a 300-mesh wire net to obtain a positive electrode material D2.

[0107] The primary particle size, specific surface area and total free lithium content of the positive electrode material D2 were tested according to the method of Example 1, and the results are shown in Table 12.

[0108] The elemental composition analysis of the positive electrode material D2 was carried out using the test method in Example 1. The results are shown in Table 10. The chemical formula of the finally obtained positive electrode material D2 is Li 1.12 Ni 0.83 Co 0.07 Mn 0.10 Zr 0.002 O2·0.0025Li2B4O7.

[0109] [Table 10]

[0110] Comparative Example 3 The difference from Example 4 is that the first coating is performed using dry coating, followed by water washing, and then the second dry coating is performed. The specific method is as follows:

[0111] The double planetary ball mill was charged with lithium hydroxide monohydrate and a precursor (chemical formula: Ni) with a molar ratio of Li:(Ni+Co+Mn):Zr=1.12:1:0.002, and a molar ratio of Ni:Co:Mn=83:07:10. 0.83 Co 0.07 Mn 0.1 A total of 1 kg of (OH)2) and nano-zirconia powder was added, and the mixture was mixed uniformly by ball milling at a rotation speed of 40 Hz for 10 minutes. The mixture was then discharged and placed in a muffle furnace, heated to 880°C at a heating rate of 5°C / min in an oxygen atmosphere, sintered for 24 hours, cooled to room temperature, and ball milled at a rotation speed of 40 Hz for 10 minutes to obtain the main material 1 for the positive electrode material.

[0112] The obtained main material 1 and alumina were added to a ball mill in a mass ratio of 1.0:0.003, totaling 400 g, and ball milled for 10 minutes at a rotation speed of 40 Hz to mix uniformly. The materials were then discharged and the mixed material was placed in a muffle furnace and heated to 780°C at a heating rate of 10°C / min in an oxygen atmosphere, sintered for 10 hours (second sintering), and cooled to room temperature to obtain an intermediate product.

[0113] Then, water and the intermediate product were added in a total of 1 kg to the reaction vessel so that the mass ratio of water:intermediate product was 1.5:1.0, mixed and stirred for 10 minutes, suction filtered, and dried at 120°C. The main material 2 for the positive electrode material was obtained from the dried sample. Then, the main material 2 and lithium tetraborate were weighed out in a total of 1 kg so that the mass ratio of main material 2:lithium tetraborate was 1.0:0.004, lithium tetraborate was added to the main material 2, and ball milled at a rotation speed of 40 Hz for 10 minutes. The uniformly mixed material was placed in a muffle furnace, heated to 280°C at a heating rate of 5°C / min in an air atmosphere, sintered for 8 hours, cooled to room temperature, and sieved through a 300-mesh wire net to obtain a positive electrode material D3.

[0114] The primary particle size, specific surface area and total free lithium content of the positive electrode material D3 were tested according to the methods described in Example 1, and the results are shown in Table 12.

[0115] The elemental composition analysis was carried out on the positive electrode material D3 using the test method in Example 1. The results are shown in Table 11. The chemical formula of the final positive electrode material is Li 1.12 Ni 0.83 Co 0.07 Mn 0.10 Zr 0.002 O2·0.003Al2O3·0.0025Li2B4O7.

[0116] [Table 11]

[0117] [Table 12]

[0118] (Experimental Example) Manufacturing and performance evaluation of lithium-ion batteries.

[0119] Different battery systems have a great impact on the cycle retention rate of materials. The battery system used in this experiment is the most common evaluation system, that is, 1mol / L lithium hexafluorophosphate solution is used as the electrolyte, the solvent in the lithium hexafluorophosphate solution is a mixed solvent with a mass ratio of dimethyl carbonate (DMC): ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1:1, the mixture of artificial graphite, conductive carbon black, carboxymethyl cellulose, and adhesive with a weight ratio of 95:1:1:3 is used as the negative electrode material, and the cell model is 454261, so as to expose the actual defects of the positive electrode material as soon as possible and determine the performance of the positive electrode material.

[0120] A whole battery (cell model 454261) was fabricated according to the following method.

[0121] Positive electrode preparation: The positive electrode materials prepared in the above examples and comparative examples, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) as a binder were added to N-methylpyrrolidone (NMP) in a weight ratio of 94:3:3 (the weight ratio of the positive electrode material to NMP was 2.1:1), mixed thoroughly, and stirred to form a uniform slurry, which was then applied to an aluminum foil current collector, dried, and pressed into an electrode piece.

[0122] Negative electrode manufacturing: Negative electrode artificial graphite, conductive carbon black (SP), carboxymethyl cellulose (CMC), and adhesive (SBR) were mixed in a weight ratio of 95:1:1:3 with sufficient amount of pure water, stirred to form a uniform slurry, applied to a copper foil current collector, dried, and pressed into a pole piece.

[0123] The separator is a PP / PE / PP three-layer composite film material.

[0124] After pressing, the positive and negative electrode pieces were spot-welded with tabs, a separator was inserted, the electrode was wound on a winder, and then placed in a wrapping jig, the top and sides were sealed, and the electrode was baked in an oven. After that, 9 g of electrolyte was poured in an environment of less than 1.5% relative humidity, and the electrolyte was formed for 48 hours (Zhejiang Hangzhou KE LIP-3AHB06 high temperature chemical formation system), and the electrode was sealed by vacuum drawing. Here, the electrolyte was 1 mol / L lithium hexafluorophosphate, and the solvent in the lithium hexafluorophosphate solution was a mixed solvent with a mass ratio of dimethyl carbonate (DMC):ethylene carbonate (EC):diethyl carbonate (DEC) = 1:1:1.

[0125] A Dongguan Keyserui Mechanical and Electrical KPBAK-03E-02 high-efficiency vacuum drying box was used for sample drying and high-temperature battery testing.

[0126] The charge-discharge test of the lithium ion battery prepared according to the present invention was carried out by Wuhan LAND battery tester, the method is as follows, and the results are shown in Table 13.

[0127] 1) Capacity test method The lithium-ion battery thus manufactured was connected to the test stand, and the test procedure was started. Setting steps: set the test temperature to 25°C, leave it for 4 hours, charge it to 4.2V at a constant current of 1C, transfer to a constant voltage of 4.2V for 0.5h, leave it for 5 minutes, and then discharge it to 3.0V at a constant current of 1C, and obtain the capacity at the current and voltage. 2) Capacity retention test method The battery that has undergone the above capacity test is connected to the test stand, the test procedure is started, and the set steps are: set the test temperature to 45°C, leave it for 4 hours, charge to 4.2V at a constant current of 1C, transfer to charging at a constant voltage of 4.2V for 0.5h, leave it for 5 minutes, and then discharge to a cut-off voltage of 3.0V at a constant current of 1C, leave it for 5 minutes, and repeat the previous constant current charging start steps to perform a cycle test, so that the capacity retention rate of different cycles can be obtained. 3) Measurement of battery thickness expansion rate using a PPG battery thickness gauge The battery was fully charged to a specified voltage of 4.25 V, and the thickness of the battery was measured using a PPG battery thickness meter. The battery was then left in a constant temperature bath at 70°C for 30 days, after which the battery was removed and the thickness of the battery was measured using the PPG battery thickness meter. The battery thickness expansion rate was calculated using the formula: Battery thickness expansion rate = (battery thickness after constant temperature - battery thickness before constant temperature) / battery thickness before constant temperature.

[0128] [Table 13]

[0129] The positive electrode materials prepared according to the above examples of the present invention are all in the form of primary particles. As can be seen from Table 12, the positive electrode materials prepared according to the above examples of the present invention have a total free lithium content of <2000 ppm and a specific surface area of ​​0.8 to 1.2 m 2 / g and the particle size is between 2.5 and 4 μm.

[0130] As can be seen from Table 13, the lithium ion battery was manufactured using the double-coated high nickel lithium ion battery positive electrode material, and the thickness expansion rate of the battery after 30 days in a thermostatic chamber at 70 ° C was less than 90%. Compared with Example 4, Comparative Example 1 used wet coating only once, and the thickness expansion rate of the battery after 30 days in a thermostatic chamber at 70 ° C was 120%, which is much higher than that of Example 4; Comparative Example 2 used dry coating only once, and the thickness expansion rate of the battery after 30 days in a thermostatic chamber at 70 ° C was 105%, which is much higher than that of Example 4; Comparative Example 3 used a process of first dry coating, followed by water washing and then a second dry coating, and the thickness expansion rate of the battery after 30 days in a thermostatic chamber at 70 ° C was 152%, which is much higher than that of Example 4 and other examples of the present invention. Furthermore, in Examples 1 to 6 of the present invention, the surface was etched by adding a strong acid in a wet process, and the produced positive electrode material was used to manufacture a lithium ion battery. After being left in a constant temperature bath at 70°C for 30 days, the battery had a thickness expansion rate of 23 to 32%. Compared to Example 6, in Example 7, the surface was not etched by adding a strong acid in a wet process, and the produced positive electrode material was used to manufacture a lithium ion battery. After being left in a constant temperature bath at 70°C for 30 days, the battery had a thickness expansion rate of 87%, which is an improvement of nearly 172% over Example 6.

[0131] From the above, in Comparative Example 1 and Comparative Example 2, the thickness expansion rate of the positive electrode material produced using one coating was high and the gas generation performance was poor. In Comparative Example 3, the positive electrode material produced using a process in which the first dry coating was followed by water washing and then a second dry coating was performed, the content of free lithium was significantly reduced by water washing, but conversely the thickness expansion rate was high and the gas generation performance was reduced. The present invention is excellent in both cycle performance and gas generation performance while maintaining a high capacity compared to high nickel positive electrode materials by the process of combined wet coating and dry coating. Therefore, the positive electrode material of the present invention can maintain good cycle performance and gas generation performance while having a high capacity, and is excellent in overall performance.

[0132] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Modifications, equivalent substitutions, and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

[0133] (Appendix) (Appendix 1) A double-coated high-nickel lithium-ion battery cathode material, comprising a cathode material substrate, a first coating layer coated on the surface of the cathode material substrate, and a second coating layer coated on the surface of the first coating layer. Here, the first coating layer and the second coating layer are manufactured by a method including the steps of sequentially coating the cathode material substrate with a metal oxide and then coating it with a boron-containing compound. A double-coated high-nickel lithium-ion battery cathode material, characterized by the above.

[0134] (Appendix 2) The chemical general formula of the cathode material is Li a Ni x Co y Mn z M b O2·cA·dB, where 1.00 ≦ a ≦ 1.20, 0.00 < b ≦ 0.01, 0.00 < c ≦ 0.01, 0.00 < d ≦ 0.05, 0.80 ≦ x < 1.00, 0.00 ≦ y < 0.12, 0.00 ≦ z < 0.2, and x + y + z = 1. M is a doping element, and M is one or more selected from the group consisting of Mg, Ti, Al, Zr, Ba, and rare earth elements. A is the first coating layer, and B is the second coating layer. The double-coated high-nickel lithium-ion battery cathode material according to Appendix 1, characterized by the above.

[0135] (Appendix 3) 1.00 ≤ a ≤ 1.20, 0.001 ≤ b ≤ 0.01, 0.80 ≤ x < 1.00, 0.00 ≤ y < 0.12, 0.00 ≤ z < 0.2, 0.0005 < c ≤ 0.01, 0.001 < d ≤ 0.05, and x + y + z = 1. Preferably, 1.02 ≤ a ≤ 1.20, 0.0015 ≤ b ≤ 0.005, 0.80 ≤ x < 1.00, 0.00 ≤ y < 0.12, 0.00 ≤ z < 0.2, 0.0005 < c ≤ 0.01, 0.001 < d ≤ 0.03, and x + y + z = 1. The double-coated high-nickel lithium-ion battery cathode material according to Supplementary Note 2.

[0136] (Supplementary Note 4) The rare earth element is one or more selected from lanthanum, cerium, praseodymium, neodymium, promethium, samarium, yttrium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, or europium, and preferably yttrium. The double-coated high-nickel lithium-ion battery cathode material according to Supplementary Note 2.

[0137] (Supplementary Note 5) The first coating layer is a coating layer formed by a metal oxide. Preferably, the metal oxide is one or more selected from the group consisting of Al2O3, TiO2, ZrO2, MgO, and rare earth element oxides. More preferably, the first coating layer is a coating layer formed by wet-coating a metal oxide. The double-coated high-nickel lithium-ion battery cathode material according to Supplementary Note 1.

[0138] (Supplementary Note 6) The rare earth element oxide is one or more selected from lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, promethium oxide, samarium oxide, yttrium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, lutetium oxide, scandium oxide, or europium oxide, and preferably yttrium oxide. 6. The dual-coated high nickel lithium ion battery cathode material according to claim 5.

[0139] (Appendix 7) The second coating layer is a coating layer formed by a boron-containing compound, and preferably, the boron-containing compound is one or more selected from boric acid, lithium borate, lithium metaborate, and lithium tetraborate, and more preferably, the second coating layer is a coating layer formed by dry coating the boron-containing compound. 2. The dual-coated high nickel lithium ion battery cathode material according to claim 1.

[0140] (Appendix 8) The positive electrode material is in the form of primary particles; 8. The dual-coated high nickel lithium ion battery positive electrode material according to any one of claims 1 to 7.

[0141] (Appendix 9) and / or, based on the weight of the positive electrode material, the positive electrode material contains <2000 ppm total free lithium; and / or The specific surface area of ​​the positive electrode material is 0.4 to 1.5 m 2 / g, and preferably, the average particle size of the positive electrode material is 2 to 5 μm. 8. The dual-coated high nickel lithium ion battery positive electrode material according to any one of claims 1 to 7.

[0142] (Appendix 10) The wet coating includes a step of mixing a wet coating reagent with a positive electrode material substrate and then sintering, and preferably, the wet coating reagent includes a metal oxide and water, and preferably further includes a strong acid; 8. The dual-coated high nickel lithium ion battery positive electrode material according to any one of claims 1 to 7.

[0143] (Appendix 11) (1) mixing a lithium source compound, a positive electrode material precursor, and an M source compound to obtain a mixture; Step (2) of subjecting the mixture of step (1) to a first sintering to obtain a positive electrode material substrate; (3) wet-coating the cathode material substrate produced in (2) to obtain a cathode material coated with a first coating layer; and (4) dry-coating the cathode material coated with the first coating layer produced in step (3) to obtain a dual-coated high nickel lithium ion battery cathode material. 8. A method for producing a dual-coated high nickel lithium ion battery positive electrode material according to any one of claims 1 to 7.

[0144] (Appendix 12) The lithium source compound, the positive electrode material precursor, and the M source compound have an element molar ratio of Li:(Ni+Co+Mn):M of (1.0 to 1.2):1.0:(0.00 to 0.01). The manufacturing method described in Appendix 11.

[0145] (Appendix 13) The wet coating includes a step of mixing a positive electrode material substrate, water, a strong acid, and a metal oxide, followed by a second sintering step; Preferably, the mass ratio of the positive electrode material substrate to the metal oxide is 1.0:(0.0005 to 0.005), preferably the mass ratio of the positive electrode material substrate to the water is 1:(1.0 to 2.0), and more preferably the mass ratio of the positive electrode material substrate to the strong acid is 1:(0.001 to 0.01); More preferably, the second sintering temperature is 600 to 800° C., the sintering time is preferably 6 to 20 h, and further preferably, the mixing step is followed by filtering and drying. The manufacturing method described in Appendix 11.

[0146] (Appendix 14) The dry coating includes mixing the positive electrode material coated with the first coating layer produced in step (3) and the boron-containing compound, followed by a third sintering step; Preferably, the mass ratio of the positive electrode material coated with the first coating layer to the boron-containing compound is 1.0:(0.002 to 0.02), More preferably, the temperature of the third sintering is 250 to 450°C, and the sintering time is preferably 3 to 15 hours. The manufacturing method described in Appendix 11.

[0147] (Appendix 15) Contains the positive electrode material according to any one of appendix 1 to 7, Low gassing high nickel lithium ion battery.

[0148] (Appendix 16) The low gas generation high nickel lithium ion battery has an initial discharge capacity of 190 to 210 mAh / g under a charge / discharge condition of 4.2 V and 1 C, and / or The low gas generation high nickel lithium ion battery has a thickness expansion rate of 32% or less when stored at 70°C for 30 days. 16. The low gassing high nickel lithium ion battery of claim 15.

[0149] (Appendix 17) Use of the positive electrode material according to any one of claims 1 to 7 in the field of digital products, electric vehicles or energy storage.

Claims

1. A dual-coated high nickel lithium ion battery cathode material, comprising: a cathode material substrate; a first coating layer coated on a surface of the cathode material substrate; and a second coating layer coated on a surface of the first coating layer; wherein the first coating layer and the second coating layer are produced by a method including the steps of successively coating a positive electrode material substrate with a metal oxide and a boron-containing compound. The dual-coated high nickel lithium ion battery positive electrode material is characterized by the above.

2. The general chemical formula of the positive electrode material is Li a Ni x Co y Mn z M b O 2 ·cA·dB, where 1.00≦a≦1.20, 0.00<b≦0.01, 0.00<c≦0.01, 0.00<d≦0.05, 0.80≦x<1.00, 0.00≦y<0.12, 0.00≦z<0.2, x+y+z=1, M is a doping element, and M is one or more selected from the group consisting of Mg, Ti, Al, Zr, Ba, and rare earth elements, A is a first coating layer, and B is a second coating layer, The dual-coated high nickel lithium ion battery positive electrode material according to claim 1.

3. 1.00≦a≦1.20, 0.001≦b≦0.01, 0.80≦x<1.00, 0.00≦y<0.12, 0.00≦z<0.2, 0.0005<c≦0.01, 0.001<d≦0.05, and x+y+z=1, and preferably 1.02≦a≦1.20, 0.0015≦b≦0.005, 0.80≦x<1.00, 0.00≦y<0.12, 0.00≦z<0.2, 0.0005<c≦0.01, 0.001<d≦0.03, and x+y+z=1. The dual-coated high nickel lithium ion battery cathode material of claim 2.

4. The rare earth element is one or more selected from lanthanum, cerium, praseodymium, neodymium, promethium, samarium, yttrium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and europium, and is preferably yttrium. The dual-coated high nickel lithium ion battery cathode material of claim 2.

5. The first coating layer is a coating layer formed of a metal oxide, and preferably, the metal oxide is Al. 2 O 3 , TiO 2 , ZrO 2 , MgO, and rare earth element oxides, and more preferably, the first coating layer is a coating layer formed by wet coating a metal oxide.

2. The dual-coated high nickel lithium ion battery cathode material of claim 1.

6. The rare earth element oxide is one or more selected from lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, promethium oxide, samarium oxide, yttrium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, lutetium oxide, scandium oxide, and europium oxide, and is preferably yttrium oxide. The dual-coated high nickel lithium ion battery cathode material of claim 5.

7. The second coating layer is a coating layer formed by a boron-containing compound, and preferably, the boron-containing compound is one or more selected from boric acid, lithium borate, lithium metaborate, and lithium tetraborate, and more preferably, the second coating layer is a coating layer formed by dry coating the boron-containing compound.

2. The dual-coated high nickel lithium ion battery cathode material of claim 1.

8. The positive electrode material is in the form of primary particles; The dual-coated high nickel lithium ion battery cathode material according to any one of claims 1 to 7.

9. and / or, based on the weight of the cathode material, the cathode material contains <2000 ppm total free lithium; and / or The specific surface area of ​​the positive electrode material is 0.4 to 1.5 m 2 / g, and preferably the average particle size of the positive electrode material is 2 to 5 μm. The dual-coated high nickel lithium ion battery cathode material according to any one of claims 1 to 7.

10. The wet coating includes a step of mixing a wet coating reagent with a positive electrode material substrate and then sintering, and preferably, the wet coating reagent includes a metal oxide and water, and preferably further includes a strong acid; The dual-coated high nickel lithium ion battery cathode material according to any one of claims 1 to 7.

11. (1) mixing a lithium source compound, a positive electrode material precursor, and an M source compound to obtain a mixture; Step (2) of subjecting the mixture of step (1) to a first sintering to obtain a positive electrode material substrate; (3) wet-coating the cathode material substrate prepared in step (2) to obtain a cathode material coated with a first coating layer; and (4) dry-coating the cathode material coated with the first coating layer produced in step (3) to obtain a dual-coated high nickel lithium ion battery cathode material. A method for producing the dual-coated high nickel lithium ion battery cathode material according to any one of claims 1 to 7.

12. The lithium source compound, the positive electrode material precursor, and the M source compound have an element molar ratio of Li:(Ni+Co+Mn):M of (1.0 to 1.2):1.0:(0.00 to 0.01). The method of claim 11.

13. The wet coating includes a step of mixing a positive electrode material substrate, water, a strong acid, and a metal oxide, followed by a second sintering step; Preferably, the mass ratio of the positive electrode material substrate to the metal oxide is 1.0: (0.0005 to 0.005), preferably the mass ratio of the positive electrode material substrate to the water is 1: (1.0 to 2.0), and more preferably the mass ratio of the positive electrode material substrate to the strong acid is 1: (0.001 to 0.01); More preferably, the temperature of the second sintering is 600-800° C., the sintering time is preferably 6-20 h, and more preferably, the mixing step further includes a filtering and drying step. The method of claim 11.

14. The dry coating includes mixing the positive electrode material coated with the first coating layer produced in step (3) and a boron-containing compound, followed by a third sintering step; Preferably, the mass ratio of the positive electrode material coated with the first coating layer to the boron-containing compound is 1.0:(0.002 to 0.02); More preferably, the temperature of the third sintering is 250 to 450°C, and the sintering time is preferably 3 to 15 h. The method of claim 11.

15. A cathode material comprising the cathode material according to any one of claims 1 to 7. Low gassing high nickel lithium ion battery.

16. The low gassing high nickel lithium ion battery has an initial discharge capacity of 190-210 mAh / g under a charge / discharge condition of 4.2 V, 1 C; and / or The low gas generation high nickel lithium ion battery has a thickness expansion rate of 32% or less when stored at 70°C for 30 days.

16. The low gassing high nickel lithium ion battery of claim 15.

17. Use of the cathode material according to any one of claims 1 to 7 in the field of digital products, electric vehicles or energy storage.

Citation Information

Patent Citations

  • Positive electrode active material, nonaqueous secondary battery, and method for manufacturing positive electrode active material

    JP2019003786A

  • Positive electrode active material, manufacturing method thereof, secondary battery, battery module, battery pack and device

    JP2023513558A

  • High nickel positive electrode material, its preparation method and lithium ion battery

    JP2024515954A

  • Non-aqueous electrolyte secondary battery

    WO2020202745A1

  • Co / B co-cladded nickel cobalt manganese lithium ion cathode material, and preparation method thereof

    CN108807926A