Cleaning blade and method for manufacturing the same, process cartridge, and image forming apparatus
The cleaning blade with a sloped coating layer of incompatible fluororesins addresses curling and friction issues, enhancing cleaning performance and stability in electrophotographic image forming apparatuses.
Patent Information
- Application Number
- JP2023075485
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
AI Technical Summary
Existing cleaning blades in electrophotographic image forming apparatuses face issues with curling and uneven frictional resistance, leading to toner slipping and rotation stopping, despite efforts to apply lubricants to reduce friction.
A cleaning blade design with a coating layer that increases in average thickness away from the tip ridgeline, using a sloped structure or steps, composed of incompatible fluororesins to maintain uniform contact and reduce friction.
The design achieves excellent cleaning performance by preventing curling and toner slipping while maintaining low frictional resistance, ensuring stable operation and reduced wear.
Smart Images

Figure 2024160468000002 
Figure 2024160468000003 
Figure 2024160468000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a cleaning blade and a manufacturing method thereof, a process cartridge, and an image forming apparatus. [Background technology]
[0002] Conventionally, in electrophotographic image forming apparatuses, residual toner adhering to the surface of an image carrier (sometimes called a member to be cleaned) after a toner image is transferred to a recording medium or an intermediate transfer body is removed by a cleaning means. As the cleaning means, a cleaning blade is widely used because of its simple structure and excellent cleaning performance. A cleaning blade is usually composed of an elastic member made of polyurethane rubber or the like and a support member. The base end of the elastic member is supported by the support member, and the contact portion (tip ridge portion) of the elastic member is pressed against the surface of the image carrier to intercept and scrape off the toner remaining on the surface of the image carrier.
[0003] As the cleaning blade, a cleaning blade in which a powder lubricant is applied to the area where the cleaning blade is in pressure contact with the image carrier has been proposed (see, for example, Patent Document 1). The elastic blade has a Martens hardness of 50 N / mm at least near the tip edge of the lower surface of the blade and at least near the tip edge of the tip surface. 2 More than 600N / mm 2 A surface layer made of the following resin material was formed, and the Martens hardness measured from the surface at a position 20 μm away from the tip edge of the underside of the blade, and the Martens hardness measured from the surface at a position 20 μm away from the tip edge of the blade tip, were 1.8 N / mm 2 More than 12N / mm 2 The following cleaning blade has been proposed (see, for example, Patent Document 2). Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a cleaning blade which has excellent cleaning properties and can suppress curling. [Means for solving the problem]
[0005] The cleaning blade of the present invention as a means for solving the above problems is as follows: A cleaning blade having an elastic member and a coating layer, The cleaning blade is a cleaning blade that removes residue by contacting a tip edge portion of the cleaning blade with a surface of a member to be cleaned, the coating layer is provided on a cleaning blade tip surface which includes the tip ridge portion and is parallel to a thickness direction of the elastic member, and on a cleaning blade underside which includes the tip ridge portion and faces the member to be cleaned, The average thickness of the coating layer on the tip surface of the cleaning blade increases with increasing distance from the tip ridge line. Effect of the Invention
[0006] According to the present invention, it is possible to provide a cleaning blade which has excellent cleaning properties and is capable of suppressing curling. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic perspective view of one embodiment of a cleaning blade of the present invention, and an enlarged view of the vicinity of the tip edge line. [Diagram 2] FIG. 2 is an enlarged cross-sectional view showing an example of the vicinity of the leading edge line of the cleaning blade of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the measurement position for the average thickness of the coating layer in the cleaning blade of the present invention. [Figure 4A] FIG. 4A is an explanatory diagram showing an example of the immersion step when the immersion angle is 0° (θ=0). [Figure 4B] FIG. 4B is an explanatory diagram showing an example of the immersion step when the immersion angle is 30° (θ=30). [Figure 4C] FIG. 4C is an explanatory diagram showing an example of the immersion step when the immersion angle is 50° (θ=50). [Diagram 5] FIG. 5 is a schematic diagram of a dipping device according to an embodiment of the present invention. [Figure 6] FIG. 6 is a schematic diagram of an imaging unit according to an embodiment of the present invention. [Figure 7] FIG. 7 is a schematic diagram of a printer according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In cleaning means using a cleaning blade, there is concern that friction between the cleaning blade and the image carrier increases the torque, which is the force required to rotate the image carrier, causing the image carrier to stop rotating. There is also concern that frictional resistance at the contact portion (edge portion) caused by the rubbing between the cleaning blade and the image carrier may cause the contact portion to curl up, allowing toner to slip through the curled up portion, resulting in poor cleaning.
[0009] In order to eliminate these problems, methods have been proposed, such as the invention described in Patent Document 1, in which a lubricant is applied to the contact portion of the cleaning blade, or the contact portion of the cleaning blade is modified with a curable composition, etc. Also known is a method of preventing the above problems by performing a step (touch-up) of applying toner or a metal soap such as zinc stearate to the contact portion of the cleaning blade when assembling an image forming apparatus or replacing the cleaning blade.
[0010] In order to keep the frictional resistance between the cleaning blade and the member to be cleaned low and prevent the cleaning blade from rolling up, the lubricant coating applied to the cleaning blade needs to have an appropriate thickness. However, in the conventional techniques including the inventions described in Patent Documents 1 and 2, an excessively thick lubricant coating may be formed near the edge of the cleaning blade. This may result in uneven contact between the cleaning blade and the member to be cleaned, which may cause the toner to slip through.
[0011] As a result of extensive research, the inventors have discovered that by configuring the average thickness of the coating layer on the tip surface of the cleaning blade so that it increases with increasing distance from the tip ridge, it is possible to achieve both excellent cleaning performance and the ability to prevent curling. Usually, as the image forming apparatus operates, toner and malus gradually remain between the cleaning blade and the image carrier, and function as a lubricant. Therefore, the cleaning blade only needs to be provided with a coating layer having a thickness that exhibits lubricating properties during the short period from when the image forming apparatus starts operating until the behavior of the cleaning blade becomes stable. On the other hand, from the viewpoint of cleaning performance, it is preferable that the coating layer is thin in order to make the contact state of the tip edge of the cleaning blade uniform. The present invention configures the thickness of the coating layer formed on the elastic member to be inclined depending on the distance from the tip ridge, thereby maintaining a uniform contact state at the tip ridge and preventing toner from slipping through, while keeping low the frictional resistance between the cleaning blade and the surface of the member being cleaned until toner and mars are sufficiently supplied to the contact portion, thereby preventing curling.
[0012] The present invention will now be described in detail.
[0013] (cleaning blade) The cleaning blade of the present invention is a cleaning blade having an elastic member and a coating layer, the cleaning blade is a cleaning blade that removes residues by contacting a leading edge portion of the cleaning blade with the surface of a member to be cleaned, the coating layer is provided on a cleaning blade leading surface that includes the leading edge portion and is parallel to the thickness direction of the elastic member, and on a cleaning blade underside that includes the leading edge portion and faces the member to be cleaned, the average thickness of the coating layer on the cleaning blade leading surface increases with increasing distance from the leading edge portion. The cleaning blade may have other members as necessary. In this specification, the "cleaning blade" may be referred to as a "blade", the "cleaning blade tip surface" may be referred to as the "blade tip surface", the "cleaning blade undersurface" may be referred to as the "blade undersurface", and the "tip ridge portion" may be referred to as the "edge portion".
[0014] The structure and size of the member to be cleaned are not particularly limited and can be appropriately selected depending on the purpose. The material of the member to be cleaned is not particularly limited and can be appropriately selected depending on the purpose. Examples of the material include metal, plastic, and ceramic. The member to be cleaned may be in the form of, for example, a drum, a belt, a plate, a sheet, or the like. The member to be cleaned is not particularly limited and can be appropriately selected depending on the purpose. When the cleaning blade is applied to an image forming apparatus, for example, the member to be cleaned can be an image carrier.
[0015] The residue is not particularly limited as long as it is attached to the surface of the member to be cleaned and is a target for removal by the cleaning blade, and examples thereof include toner, lubricant, inorganic fine particles, organic fine particles, dirt, dust, and mixtures thereof.
[0016] Here, one embodiment and another embodiment of the cleaning blade of the present invention will be described with reference to the drawings, however, the use of the cleaning blade of the present invention is not limited to these embodiments. In addition, in each drawing, the same components are denoted by the same reference numerals, and duplicated explanations may be omitted. Furthermore, the number, position, shape, etc. of the following components are not limited to the present embodiment, and may be any number, position, shape, etc. that is preferable for implementing the present invention.
[0017] [Figure 1] FIG. 1 is a schematic perspective view of one embodiment of a cleaning blade of the present invention, and an enlarged view of the vicinity of the tip edge line. The cleaning blade 62 is composed of a rectangular holder 621 serving as a support member and made of a rigid material such as metal or hard plastic, and a rectangular elastic blade 622 serving as an elastic member. The cleaning blade 62 is disposed so that the leading edge portion 62c comes into contact with the surface of the member to be cleaned along the longitudinal direction.
[0018] The elastic blade 622 has a cleaning blade tip surface 62a, a cleaning blade lower surface 62b, a tip ridge portion 62c which is one end on the free end side of the elastic blade 622, and a cleaning blade side surface 62d, and has a coating layer 623 which includes the tip ridge portion 62c. The coating layer 623 is provided on a cleaning blade tip surface 62a which includes the tip ridge portion 62c and is parallel to the thickness direction of the elastic blade 622, and on a cleaning blade lower surface 62b which includes the tip ridge portion 62c and faces the member to be cleaned. The elastic blade 622 is fixed to one end of the holder 621 by adhesive or the like, and the other end of the holder 621 is supported in a cantilever manner by a case of the cleaning device or the like.
[0019] [Figure 2] FIG. 2 is an example of an enlarged cross-sectional view of the vicinity of the tip edge line of the cleaning blade of the present invention. The elastic blade 622 has a blade tip surface 62a, a blade undersurface 62b, a tip ridge portion 62c which is one end of the free end side of the elastic blade 622, and a coating layer 623 on the blade tip surface 62a including the tip ridge portion 62c, and on the blade undersurface 62b including the tip ridge portion 62c. D in FIG. 2 indicates the distance from the tip edge portion 62c of the cleaning blade tip surface 62a.
[0020] <Elastic material> The shape of the elastic member may be selected appropriately depending on the purpose as long as it has a structure that can remove the residue on the member to be cleaned, but it is preferable that the contact side at the contact point between the elastic member and the member to be cleaned is straight, and it is more preferable that it is plate-shaped or rectangular.
[0021] The material of the elastic member is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the material has a high resilience modulus so that it can follow the eccentricity of the member to be cleaned and minute undulations on the surface of the member to be cleaned. More specifically, the resilience of the elastic member in accordance with JIS K6255 standard is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10% to 80% at 23°C. Having the coefficient of resilience within the desired range is advantageous in that it can eliminate problems such as poor cleaning caused by the elastic member as a whole losing its flexibility and being unable to follow the vibrations or roughness of the image carrier, or blade squeal (abnormal noise) caused by excessively strong repulsion.
[0022] The method for measuring the resilience of the elastic member is not particularly limited, and for example, it can be measured at 23° C. using a No. 221 resilience tester (manufactured by Toyo Seiki Seisakusho Co., Ltd.) in accordance with JIS K6255 standard.
[0023] Specific examples of the elastic material include polyurethane rubber, silicone rubber, fluororubber, nitrile rubber (NBR), ethylene propylene diene rubber (EPDM), etc. Among these, polyurethane rubber is preferable from the viewpoints of durability and non-staining properties.
[0024] When the material of the elastic member is urethane rubber, the Martens hardness of the urethane rubber is 0.6 N / mm 2 Excess 1.5N / mm 2 It is preferable that: The Martens hardness of the urethane rubber is 0.6N / mm 2 If the contact pressure exceeds the limit, it is preferable to suppress warping of the cleaning blade 62 when the contact pressure is set high to improve the cleaning performance for polymerized toner. Specifically, when the cleaning blade 62 warps, the blade lower surface 62b comes into contact with the member to be cleaned, which is called the belly contact phenomenon, and the contact area between the cleaning blade 62 and the surface of the member to be cleaned increases rapidly, resulting in a decrease in the contact pressure and a decrease in cleaning performance. In particular, in the configuration of the present invention in which the cleaning tip has a coating layer on its ridgeline, the above phenomenon may occur significantly, so it is preferable that the Martens hardness of the urethane rubber is in the above numerical range.
[0025] The method for measuring the Martens hardness is not particularly limited and can be appropriately selected depending on the purpose. For example, based on ISO14577, a nanoindenter (ENT-3100, manufactured by Elionix) can be used to measure the Martens hardness by pressing a Berkovich indenter with a load of 1,000 μN for 10 seconds, holding the indenter at this load for 5 seconds, and then pulling the indenter out at the same load rate for 10 seconds. The location for measuring the Martens hardness is not particularly limited, but may be, for example, a location 20 μm away from the tip edge of the bladed sheet after molding. Note that the "Martens hardness" in this specification is the average value of the values obtained by measuring the Martens hardness at 4 to 6 points at each measurement location.
[0026] The structure of the elastic member is not particularly limited and may be appropriately selected depending on the purpose, and may be, for example, a single-layer structure, a laminated structure, a laminated structure in which a plurality of members are combined, etc. Among these, the single-layer structure and the laminated structure in which a plurality of members are laminated are preferred from the viewpoint of ease of processing into a cleaning blade. When the elastic member has a two-layer structure in which layers made of different materials are laminated together, the materials of the layer that abuts against the member to be cleaned (contact layer) and the layer that does not abut against the member to be cleaned (anti-contact layer) are not particularly limited and can be selected appropriately depending on the purpose, but it is preferable that the material of the contact layer is urethane rubber, as described above. The Martens hardness of the contact layer and the anti-contact layer is 0.6 N / mm 2 Excess 1.5N / mm 2 It is preferable that:
[0027] The size of the elastic member is not particularly limited and can be appropriately selected depending on the size of the member to be cleaned.
[0028] [Method of manufacturing elastic member] The method for producing the elastic member is not particularly limited and can be appropriately selected depending on the purpose. For example, a polyurethane prepolymer is prepared using a polyol compound and a polyisocyanate compound, a curing agent and, if necessary, a curing catalyst are added to the polyurethane prepolymer, the polyurethane prepolymer is centrifugal molded in a specified mold, and the resulting product is left at room temperature to mature (cure), and then cut into a plate of specified dimensions to obtain the elastic member.
[0029] -Polyol compounds- The polyol compound is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyol compound include high molecular weight polyols and low molecular weight polyols.
[0030] Examples of the high molecular weight polyol include polyester polyols which are condensates of alkylene glycols and aliphatic dibasic acids; polyester polyols such as polyester polyols of alkylene glycols and adipic acid, such as ethylene adipate ester polyol, butylene adipate ester polyol, hexylene adipate ester polyol, ethylene propylene adipate ester polyol, ethylene butylene adipate ester polyol, and ethylene neopentylene adipate ester polyol; polycaprolactone polyols such as polycaprolactone ester polyol obtained by ring-opening polymerization of caprolactone; and polyether polyols such as poly(oxytetramethylene) glycol and poly(oxypropylene) glycol. These may be used alone or in combination of two or more.
[0031] Examples of the low molecular weight polyols include dihydric alcohols such as 1,4-butanediol, ethylene glycol, neopentyl glycol, hydroquinone-bis(2-hydroxyethyl)ether, 3,3'-dichloro-4,4'-diaminodiphenylmethane, and 4,4'-diaminodiphenylmethane; and trihydric or higher polyhydric alcohols such as 1,1,1-trimethylolpropane, glycerin, 1,2,6-hexanetriol, 1,2,4-butanetriol, trimethylolethane, 1,1,1-tris(hydroxyethoxymethyl)propane, diglycerin, and pentaerythritol. These may be used alone or in combination of two or more.
[0032] -Polyisocyanate compounds- The polyisocyanate compound is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate compound include methylene diphenyl diisocyanate (MDI), tolylene diisocyanate (TDI), xylylene diisocyanate (XDI), naphthylene 1,5-diisocyanate (NDI), tetramethyl xylene diisocyanate (TMXDI), isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate (H6XDI), dicyclohexylmethane diisocyanate (H12MDI), hexamethylene diisocyanate (HDI), dimer acid diisocyanate (DDI), norbornene diisocyanate (NBDI), and trimethylhexamethylene diisocyanate (TMDI). These may be used alone or in combination of two or more.
[0033] - Hardener - The curing agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the curing agent include amines and alcohols. These may be used alone or in combination of two or more. The hardener can be used, for example, to adjust the hardness of the elastic member.
[0034] -Curing catalyst- The curing catalyst is not particularly limited and can be appropriately selected depending on the purpose. Examples of the curing catalyst include 2-methylimidazole and 1,2-dimethylimidazole. The content of the curing catalyst is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 0.01% by mass to 0.5% by mass, and more preferably from 0.05% by mass to 0.3% by mass, based on the total mass of the prepolymer and the curing agent.
[0035] <Coating layer> The coating layer contains a first fluororesin and a second fluororesin that is incompatible with the first fluororesin, and may further contain other components as necessary. The coating layer refers to a layer provided on the cleaning blade tip surface which includes the tip ridge portion and is parallel to the thickness direction of the elastic member, and on the underside of the cleaning blade which includes the tip ridge portion and faces the member to be cleaned. The coating layer may be formed on at least a portion of the elastic member including the contact edge where the blade and the member to be cleaned come into contact, may be formed on the entire contact edge, or may be formed on the entire surface of the elastic member.
[0036] The coating layer in the cleaning blade preferably has the following characteristics (1) to (3). (1) The average thickness of the coating layer on the tip surface of the cleaning blade at a distance of 0.02 mm from the tip ridge is 0.5 μm or more and 3 μm or less. (2) The average thickness of the coating layer on the tip surface of the cleaning blade at a distance of 0.1 mm from the tip ridge is 1 μm or more and 7 μm or less. (3) The average thickness of the coating layer on the tip surface of the cleaning blade at a distance of 0.3 mm from the tip ridge is 3 μm or more and 10 μm or less. In other words, the cleaning blade of the present invention is preferably configured such that the average thickness of the coating layer on the blade tip surface is thin at the tip ridge of the cleaning blade and thickens with increasing distance from the tip ridge. Specifically, the coating layer may have a gradient structure in which the average thickness of the coating layer increases continuously with increasing distance from the tip ridge, or a step structure in which the average thickness of the coating layer increases stepwise with increasing distance from the tip ridge, but a gradient structure is preferred. Note that, as will be described in detail later, the average thickness of the coating layer can be adjusted, for example, by changing the angle between the blade tip surface and the coating liquid surface and the lifting speed when lifting the blade from the coating liquid. In this specification, "the distance from the ridge of the tip surface of the cleaning blade" may be referred to as "D." For example, "the average thickness of the coating layer when D is 0.02 mm" can be read as "the average thickness of the coating layer at a distance of 0.02 m from the ridge of the tip surface of the cleaning blade."
[0037] The method for measuring the average thickness of the coating layer is not particularly limited, but for example, a part of the coating layer is scraped off using a spatula, a cotton swab, or the like, and the shape is measured using a three-dimensional measuring device such as a contact surface roughness meter (Surftest SJ-500: manufactured by Mitutoyo) or a laser microscope (LEXT OLS4100: manufactured by Olympus). As a more specific measuring method, for example, as shown in FIG. 3, the cleaning blade tip surface 62a is measured at five positions, namely, positions 41 mm, 110 mm, 178 mm, 247 mm, and 315 mm away from the cleaning blade side surface 62d in the longitudinal direction at positions 0.02 mm, 0.1 mm, and 0.3 mm away from the tip ridge portion 62c, and the obtained values are averaged. Note that the coating layer 623 is omitted in FIG. 3.
[0038] <<Daiichi Fluorine Resin>> In this specification, the term "fluororesin" refers to a resin containing fluorine in the molecule. The fluororesin is preferably a fluorine-containing olefin polymer, and more preferably a fluorine-containing olefin polymer in which hydrogen atoms are substituted with fluorine atoms. In one aspect of the present invention, the first fluororesin is preferably a domain in the sea-island structure of the coating layer. It is preferable to select the type and amount of resin between the first fluororesin and the second fluororesin described later so that the first fluororesin forms a domain.
[0039] In this specification, the term "incompatible" refers to the property of multiple mixed substances being mixed without an interface between them and not completely mixed, and the term "compatible" refers to the property of multiple mixed substances being mixed without an interface between them. In this specification, the term "incompatible state" refers to a state in which an interface exists between the first fluororesin and the second fluororesin, and may also refer to a state in which they are partially compatible with each other. As one embodiment of the immiscible state, the coating layer preferably has a sea-island structure, which means a structure in which, when a continuous phase of one component contained in the coating layer formed on the cleaning blade is expressed as a "sea (hereinafter sometimes referred to as a matrix)", the other component is in the form of "islands (hereinafter sometimes referred to as domains)" in the "sea". The term "sea-island structure" as used herein refers to a state in which the first fluororesin, which is a domain, and the second fluororesin, which is a matrix, are incompatible with each other and do not have any compatible portions. When the coating layer has a sea-island structure, the domains in the sea-island structure are preferably particles.
[0040] The shape of the domain is not particularly limited and may be appropriately selected depending on the purpose, and may be either a regular shape or an irregular shape. Among these, a regular shape is preferable. When the domain has a fixed shape, it is preferably spherical. When the domain has a spherical shape, it is preferably particulate. The domains having such a shape are preferable because it is possible to prevent problems such as the first fluororesin detached from the coating layer damaging the member to be cleaned or the elastic member of the cleaning blade.
[0041] The volume average particle diameter (50% volume diameter, median diameter) of the first fluororesin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 μm or more and 1 μm or less, more preferably 0.5 μm or less, and even more preferably 0.3 μm or less. If the first fluororesin has a volume average particle size of 1 μm or less, it is possible to prevent the problem that the first fluororesin is prone to settling in the solvent, making it difficult to stably disperse the first fluororesin, and this is preferable. If the first fluororesin has a volume average particle size of 0.5 μm or less, it can be more stably dispersed in the non-aqueous solvent, which is preferable.
[0042] The method for measuring the volume average particle size (50% volume diameter, median diameter) is not particularly limited and may be appropriately selected depending on the purpose, and may be measured, for example, by a laser diffraction / scattering method, a dynamic light scattering method, an image imaging method, etc. Specific examples of the method for measuring the volume average particle size include a method in which particles collected from the coating layer of the cleaning blade are measured by a laser diffraction / scattering method using a Microtrac (manufactured by Nikkiso Co., Ltd.), and a method in which fine particles on the cleaning blade are directly observed and measured using a scanning electron microscope (SEM). The volume average particle size of the particles hardly changes between when they are added to the dispersion liquid to be applied to the cleaning blade and when they are present in the coating layer.
[0043] The first fluororesin is not particularly limited and can be selected according to the purpose, and examples thereof include polytetrafluoroethylene (PTFE), fluorinated ethylene-propylene copolymer (FEP), perfluoroalkoxy polymer (PFA), chlorotrifluoroethylene copolymer (CTFE), tetrafluoroethylene-chlorotrifluoroethylene copolymer (TFE / CTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polychlorotrifluoroethylene (PCTFE), etc. Among these, polytetrafluoroethylene (PTFE) is preferred in terms of further improving the sliding properties of the cleaning blade.
[0044] The polytetrafluoroethylene (PTFE) may be appropriately synthesized or may be a commercially available product, such as Dyneon TF Micropowder TF-9201Z, Dyneon TF Micropowder TF-9207Z (both manufactured by 3M), Nano FLON119N, FLUORO E (both manufactured by Shamrock), TLP10F-1 (manufactured by Mitsui-DuPont Fluorochemicals), KTL-500F (manufactured by Kitamura Co., Ltd.), and Algoflon L203F (manufactured by SOLVAY).
[0045] <<Secondary fluororesin>> When the coating layer contains the second fluororesin, the adhesion of the first fluororesin to the elastic member is improved, and detachment of the coating layer can be prevented, thereby preventing curling of the cleaning blade and an increase in torque. In one aspect of the present invention, the second fluororesin is preferably a matrix in the sea-island structure of the coating layer. It is preferable to select the type and amount of the second fluororesin to be added between the first fluororesin and the second fluororesin so that the second fluororesin forms a matrix.
[0046] The second fluororesin is not particularly limited as long as it can disperse the first fluororesin uniformly and stably, and may be appropriately selected depending on the purpose, and examples thereof include vinylidene fluoride (VdF), hexafluoropropylene (HFP), tetrafluoroethylene (TFE), etc. Among these, a ternary copolymer of VdF-HFP-TFE is preferred from the viewpoints of lubricity and adhesion to elastic members.
[0047] The composition of VdF / HFP / TFE in the terpolymer is preferably 30 mol% to 80 mol% / 10 mol% to 35 mol% / 5 mol% to 35 mol% in terms of imparting flexibility and solubility in a solvent to the blade, respectively.
[0048] A fluorine-based oil may be added to the second fluorine resin, which not only functions as a binder but also further improves the sliding function. Examples of the fluorine-based oil include those having a tetrafluoroethylene (TFE) oligomer or perfluoroether as the main skeleton. The fluorine-based oil having a perfluoroether in the main skeleton is not particularly limited and can be appropriately selected depending on the purpose as long as it has sliding properties and does not inhibit the dispersion of the fluororesin. From the viewpoint of kinetic viscosity, however, it is preferable that the average molecular weight is 2,000 to 3,500.
[0049] When a mixture of the second fluororesin and the fluoro-based oil is used, the content of the second fluororesin is preferably 90% by mass or more and 99% by mass or less, and more preferably 95% by mass or more and 98% by mass or less, based on the total mass of the mixture, in order to prevent contamination of the photoconductor, etc. due to bleed-out of the fluoro-based oil.
[0050] The first fluororesin and the second fluororesin in the present invention may be the same material or different materials. When the same material is used, the coating layer can be produced by devising a manufacturing method so that the first fluororesin and the second fluororesin are in an incompatible state. For example, by adding a second fluororesin to a first fluororesin that has been cured in advance and curing it, an interface is formed between the first fluororesin and the second fluororesin, and the coating layer that is partially incompatible can be produced. In addition, the coating layer can also be produced by adding a hydrophilic substituent to the first fluororesin and mixing the second fluororesin to which a hydrophobic substituent has been added.
[0051] <<Other ingredients>> The other components are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include resin particles other than the fluororesin. In this specification, the "non-fluororesin resin particles" may be referred to as "other resin particles." The other resin particles are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other resin particles include fine particles of inorganic compounds, acrylic resins, styrene resins, and vinyl resins. Examples of the inorganic compound particles include silica, alumina, and zirconia. These may be used alone or in combination of two or more.
[0052] The shape of the other resin particles is not particularly limited and can be appropriately selected according to the purpose, but is preferably spherical. By making the other resin particles have such a shape, it is preferable to prevent the other resin particles detached from the coating layer from damaging the member to be cleaned or the elastic member of the cleaning blade.
[0053] The volume average particle size (50% volume diameter, median diameter) of the other resin particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 μm or more and 1 μm or less, more preferably 0.5 μm or less, and even more preferably 0.3 μm or less. If the volume average particle size of the other resin particles is 1 μm or less, the particles tend to settle in the solvent, which makes it difficult to stably disperse the particles, and this is advantageous in that such a problem can be prevented. If the volume average particle size of the other resin particles is 0.5 μm or less, it is possible to disperse the particles more stably in the non-aqueous solvent, which is preferable.
[0054] <Other materials> The other members are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other members include a support member.
[0055] - Supporting member - The shape of the support member is not particularly limited and can be appropriately selected depending on the purpose. For example, the shape may be a plate or a strip. The structure of the support member is not particularly limited and can be appropriately selected depending on the purpose. The size of the support member is not particularly limited and can be appropriately selected depending on the size of the member to be cleaned. The material of the support member is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include metal, plastic, ceramic, etc. Among these, metal is preferable from the viewpoint of strength, and steel such as stainless steel, aluminum, and phosphor bronze are more preferable.
[0056] (Manufacturing method of cleaning blade) The method for producing a cleaning blade of the present invention includes an immersion step and a removal step, and may also include a measurement step and other steps as necessary. The manufacturing apparatus for the cleaning blade according to the present invention includes an immersion means and a lifting means, and may also include a measuring means and other means as necessary.
[0057] <Soaking process> The immersion step is a step of immersing the elastic member in the coating liquid. The immersion means is a means for immersing the elastic member in the coating liquid. The immersion step can be suitably carried out by the immersion means. It should be noted that the "elastic member" is the same as that described in the <elastic member> section above, and therefore a description thereof will be omitted.
[0058] <<Coating liquid>> The coating liquid is not particularly limited as long as it can form a coating layer that has excellent cleaning properties and suppresses the occurrence of curling on the elastic member, and can be appropriately selected depending on the purpose. It is preferable that the coating liquid contains a first fluororesin, a second fluororesin, and a fluorine-based inactive liquid. Incidentally, the "first fluororesin" and the "second fluororesin" are the same as those described in the above section (cleaning blade), and therefore a description thereof will be omitted.
[0059] - Fluorine-based inert liquid - The fluorine-based inactive liquid is not particularly limited as long as it is an organic solvent containing fluorine and can be appropriately selected depending on the purpose. Examples of the fluorine-based inactive liquid include hydrofluoroether (HFE), perfluorocarbon (PFC), and perfluoroether (PFE). These may be used alone or in combination of two or more.
[0060] When the coating liquid contains the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid, the total content of the first fluororesin and the second fluororesin is preferably 5 mass% or more and 10 mass% or less with respect to the total amount of the coating liquid, and the content of the fluorine-based inactive liquid is preferably 90 mass% or more and 95 mass% or less with respect to the total amount of the coating liquid. By setting the content of each component in the coating liquid within the above-mentioned numerical range, the viscosity of the coating liquid can be appropriately adjusted, and a coating layer having a desired average thickness can be formed, which is preferable.
[0061] The viscosity of the coating liquid is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of obtaining a coating layer having an appropriate average thickness, the viscosity is preferably 1.75 mPa·s or more and 1.95 mPa·s or less. The method for measuring the viscosity is not particularly limited, but for example, the viscosity can be measured using a vibration viscometer (manufactured by Sekonic Corporation).
[0062] The method for manufacturing a cleaning blade of the present invention is characterized in that the angle between the coating liquid surface and the cleaning blade tip surface in the immersion step is 5° to 45°. In this specification, the "angle between the coating liquid surface and the cleaning blade tip surface" is sometimes referred to as the "immersion angle." More specifically, the immersion angle indicates the angle (θ) between the liquid surface of the coating liquid 600 and the cleaning blade tip surface 62a, as shown in Figures 4A to 4C. Note that Figure 4A is an explanatory diagram showing an example of an immersion process when the immersion angle is 0° (θ=0), Figure 4B is an explanatory diagram showing an example of an immersion process when the immersion angle is 30° (θ=30), and Figure 4C is an explanatory diagram showing an example of an immersion process when the immersion angle is 50° (θ=50).
[0063] From the viewpoint of obtaining a cleaning blade that has excellent cleaning properties and is capable of preventing curling, the immersion angle is preferably from 5° to 45°, and more preferably 30°.
[0064] <Pulling process> The pulling up step is a step of pulling up the elastic member from the coating liquid. The lifting means is a means for lifting the elastic member from the coating liquid. The pulling step can be suitably carried out by the pulling means. It should be noted that the “elastic member” is the same as that described in the above-mentioned <elastic member> section, and the “coating liquid” is the same as that described in the above-mentioned <<coating liquid>> section, so explanations thereof will be omitted.
[0065] In the pulling-up step, the speed at which the elastic member is pulled up from the coating liquid is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of obtaining a cleaning blade that has excellent cleaning properties and is capable of preventing curling, the speed is preferably 5 mm / s or more and 45 mm / s or less. In this specification, the "speed at which the elastic member is pulled up from the coating liquid" may be referred to as the "pulling up speed."
[0066] <Measurement process> The measuring step is a step of measuring the contents of the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid in the coating liquid. The measuring means is a means for measuring the contents of the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid in the coating liquid. The measuring step can be suitably carried out by the measuring means. The "coating liquid", the "first fluororesin", the "second fluororesin", and the "fluorine-based inactive liquid" are the same as those described above in the (cleaning blade) and <<coating liquid>> sections, and therefore their explanation will be omitted.
[0067] The measurement method is not particularly limited as long as it can measure the content of each component in the coating liquid, and can be appropriately selected depending on the purpose. For example, a measurement method based on heating residue described in Section 2 of JIS K 5601-1-2 can be used.
[0068] Based on the results obtained by the measurement process, the fluorine-based inactive liquid can be replenished to the coating liquid, and the contents of the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid in the coating liquid can be adjusted. Furthermore, the speed at which the elastic member is pulled up in the pulling step can be adjusted based on the results obtained in the measuring step. Since the fluorine-based inert liquid contained in the coating liquid is volatile, the content (ratio) of each component in the coating liquid varies over time. When the fluorine-based inert liquid volatilizes and the contents (ratios) of the first fluororesin and the second fluororesin in the coating liquid increase, the viscosity of the coating liquid may increase. Therefore, by replenishing the coating liquid with the fluorine-based inactive liquid, the coating liquid can be kept at an appropriate viscosity, and by adjusting the pulling speed in accordance with the viscosity of the coating liquid, a coating layer can be formed with higher accuracy and stability.
[0069] Here, an example of the method for producing a cleaning blade of the present invention will be described with reference to the drawings.
[0070] [Figure 5] FIG. 5 is a schematic diagram of a dipping device according to an embodiment of the present invention. The dipping apparatus includes a storage tank 201, a coating liquid 600, a lubrication pump 203, a coating tank 204, a stirrer 205, a viscometer 206, a fluorine-based inert liquid 207, a filter 208, a cooling jacket 209, a hood 210, a steam tank 211, an elevator 213, and the like. A coating liquid 600 is stored in a storage tank 201, and the coating liquid 600 is sent to a coating tank 204 by a circulation pump 203. The coating liquid 600 that overflows from the coating tank 204 is circulated by being returned to the storage tank 201 again. A filter 208 is provided on the circulation path to remove foreign matter in the coating liquid 600. The storage tank 201 is provided with a stirrer 205, which stirs the coating liquid 600 to prevent settling of the first fluororesin and the second fluororesin. The storage tank 201 is provided with a viscometer 206, which measures the viscosity of the coating liquid 600 to indirectly measure the ratio of each component contained in the coating liquid 600. Depending on the measurement result, a fluorine-based inert liquid 207 is added to the coating liquid 600 as needed, thereby making it possible to keep the ratio of each component constant. A cooling jacket 209 is provided around the storage tank 201, and the temperature is kept constant by installing cold water. A hood 210 is installed around the coating tank 204, and a steam tank 211 is formed to suppress the evaporation of the fluorine-based inactive liquid. The elastic member 622 is held by an elevator 213, and is immersed in the coating liquid 600 in the coating tank 204 and then pulled up to perform dip coating.
[0071] (Image forming apparatus and image forming method) The image forming apparatus of the present invention has a cleaning blade as cleaning means, and may, as necessary, have an image carrier, a charging means for charging the surface of the image carrier, an exposure means for exposing the charged image carrier to light to form an electrostatic latent image, a developing means for developing the electrostatic latent image with toner to form a visible image, a transfer means for transferring the visible image to a recording medium, a fixing means for fixing the transferred image transferred to the recording medium, and other means. The image forming method according to the present invention may include a charging step, an exposure step, a development step, a transfer step, a fixing step, a cleaning step, and other steps. The charging step and the exposure step may be collectively referred to as an electrostatic latent image forming step. It should be noted that the "cleaning blade" is the same as that described in the above (cleaning blade) section, and therefore a description thereof will be omitted. The image forming method can be suitably carried out by the image forming apparatus, the charging step can be suitably carried out by the charging means, the exposure step can be suitably carried out by the exposure means, the developing step can be suitably carried out by the developing means, the transfer step can be suitably carried out by the transfer means, the fixing step can be suitably carried out by the fixing means, the cleaning step can be suitably carried out by the cleaning means, and the other steps can be suitably carried out by the other means.
[0072] <Image carrier> The image bearing member is not particularly limited in terms of material, shape, structure, size, etc., and can be appropriately selected from known ones. A preferred shape is a drum shape, and examples of the material include inorganic photoreceptors such as amorphous silicon and selenium, and organic photoreceptors such as polysilane and phthalopolymethine. Examples of the organic photoreceptor include a laminated photoreceptor having a laminated structure in which a layer (charge generation layer) in which a charge generation material such as metal-free phthalocyanine or titanyl phthalocyanine is dispersed in a binder resin and a layer (charge transport layer) in which a charge transport material is dispersed in a binder resin are stacked on a support such as an aluminum drum, and a single-layered photoreceptor having a single-layered photosensitive layer in which both a charge generation material and a charge transport material are dispersed in a binder resin on a support. In the single-layered photoreceptor, a hole transport material and an electron transport material can also be added to the photosensitive layer as charge transport materials. In addition, an undercoat layer may be provided between the support and the laminated charge generation layer or the single-layered photosensitive layer.
[0073] <Charging process and charging means> The charging step is a step of charging the surface of the image bearing member by the charging unit. The charging means is not particularly limited as long as it can charge the surface of the image bearing member, and can be appropriately selected depending on the purpose. Examples of the charging means include a contact charger known per se having a conductive or semiconductive roller, brush, film, rubber blade, etc., and a non-contact charger that utilizes corona discharge such as a corotron or scorotron. The charging means may have any shape, such as a roller, a magnetic brush, a fur brush, etc., and can be selected according to the specifications and shape of an electrophotographic image forming apparatus. When a magnetic brush is used as the charging means, the magnetic brush uses various ferrite particles, such as Zn-Cu ferrite, as the charging means, and is composed of a non-magnetic conductive sleeve for supporting the charging means, and a magnet roll contained within the conductive sleeve. When a brush is used as the charging means, for example, fur that has been treated to be conductive with carbon, copper sulfide, metal or metal oxide can be used as the material for the fur brush, and the fur can be wrapped around or attached to a metal or other conductive core to form a charger.
[0074] The charger is not limited to the contact type charger described above, but is preferred in that an image forming apparatus in which ozone generated from the charger is reduced can be obtained. It is preferable that the charger is disposed in contact with or without contact with the image bearing member, and charges the surface of the image bearing member by applying DC and AC voltages in a superimposed manner. It is also preferable that the charger is a charging roller having a gap tape on the image carrier and arranged in close proximity to the image carrier without contacting the image carrier, and that the surface of the image carrier is charged by applying DC and AC voltages in a superimposed manner to the charging roller.
[0075] <Exposure Step and Exposure Means> The exposure step is a step of exposing the charged surface of the image carrier to light, and is performed by the exposure unit. The exposure step can be performed, for example, by exposing the surface of the image carrier to light in an imagewise manner using the exposure unit. Optical systems for exposure are roughly divided into analog optical systems and digital optical systems. The analog optical system is an optical system that projects an original directly onto the surface of an image carrier by an optical system. The digital optical system is an optical system that receives image information as an electrical signal, converts the electrical signal into an optical signal, and exposes the image carrier to form an image. The exposure means is not particularly limited and can be appropriately selected depending on the purpose as long as it can expose the charged image carrier to light to form an electrostatic latent image. Examples of the exposure means include various exposure devices such as a copying optical system, a rod lens array system, a laser optical system, a liquid crystal shutter optical system, and an LED optical system. In the present invention, a backlight system in which exposure is performed imagewise from the back side of the image carrier may be adopted.
[0076] <Developing step and developing means> The developing step is a step of developing the electrostatic latent image into the toner image by the developing unit. The developing means is not particularly limited as long as it can develop the electrostatic latent image into a toner image and can be appropriately selected depending on the purpose. For example, the developing means may include a developing unit that contains the toner and is capable of applying the toner to the electrostatic latent image in a contact or non-contact manner. The developing device may be of a dry developing type or a wet developing type, and may be a single-color developing device or a multi-color developing device, and may, for example, be one having an agitator that charges the toner by friction agitation, and a rotatable magnetic roller. In the developing unit, for example, the toner and, if necessary, a carrier are mixed and stirred, and the toner becomes charged by friction during this process and is held in a standing state on the surface of the rotating magnet roller, forming a magnetic brush. Since the magnet roller is disposed in the vicinity of the image carrier, a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the image carrier by the electrical attraction of the electrostatic latent image, and as a result, the electrostatic latent image is developed by the toner to form the toner image on the surface of the image carrier. The toner contained in the developing device may be a developer containing the toner, and the developer may be a one-component developer or a two-component developer. The toner can be used as a one-component magnetic toner that does not use a carrier, or as a non-magnetic toner.
[0077] <Transfer process and transfer means> The transfer step is a step of transferring the toner image onto a recording medium by the transfer unit. The transfer step preferably includes, for example, a primary transfer step in which an intermediate transfer body is used and the toner image is transferred to the surface of the intermediate transfer body to form a composite transfer image, and a secondary transfer step in which the composite transfer image is transferred to a recording medium. The transfer means is not particularly limited as long as it is capable of transferring the toner image onto a recording medium and can be appropriately selected depending on the purpose. A preferred embodiment has a primary transfer means that transfers the toner image onto the surface of the intermediate transfer body to form a composite transfer image, and a secondary transfer means that transfers the composite transfer image onto a recording medium. The primary transfer means and the secondary transfer means preferably include, for example, at least a transfer device that peels and charges the toner image formed on the surface of the image carrier onto a recording medium. The transfer device is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a corona transfer device using corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, an adhesive transfer device, etc. The number of the transfer devices may be one or more.
[0078] The recording medium is not particularly limited as long as it is capable of transferring the unfixed toner image after development, and can be appropriately selected depending on the purpose. A typical example is plain paper, but for example, a PET base for an OHP can also be used.
[0079] <Fixing process and fixing means> The fixing step is a step of fixing the toner image transferred onto the recording medium by the fixing unit. When toners of two or more colors are used, the toners of each color may be fixed as they are transferred onto the recording medium, or the toners of all colors may be fixed in a laminated state after being transferred onto the recording medium. The fixing means is not particularly limited as long as it can fix the toner image transferred to the recording medium, and can be appropriately selected depending on the purpose. A thermal fixing method using a known heating and pressurizing means can be adopted. The heating and pressurizing means is not particularly limited and can be appropriately selected depending on the purpose. For example, a combination of a heating roller and a pressure roller, or a combination of a heating roller, a pressure roller and an endless belt can be mentioned. The heating temperature is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 80° C. to 200° C. If necessary, for example, a known optical fixing device may be used together with the fixing means.
[0080] <Cleaning process and cleaning means> The cleaning step is a step of removing the toner remaining on the surface of the image bearing member by the cleaning means. As the cleaning means, the cleaning blade of the present invention fixed to a supporting member is used.
[0081] The line pressure applied by the cleaning blade of the present invention to the surface of the image bearing member is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 N / m or more and 100 N / m or less, and more preferably 10 N / m or more and 50 N / m or less. When the linear pressure is 10 N / m or more and 100 N / m or less, cleaning defects caused by the toner slipping through between the edge portion and the member to be cleaned are unlikely to occur, and curling of the cleaning blade can be suppressed, which is preferable. The linear pressure can be measured, for example, by using a measuring device incorporating a small compression load cell manufactured by Kyowa Electric Industry Co., Ltd.
[0082] The angle between the tangent to the image carrier and the tip surface of the blade at the position where the tip ridge portion of the cleaning blade of the present invention abuts (hereinafter, sometimes referred to as the "cleaning angle") is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 65° or more and 85° or less. If the cleaning angle is 65° or more and 85° or less, the occurrence of curling of the blade can be easily suppressed, and the occurrence of cleaning defects can be suppressed, which is preferable.
[0083] <Other steps and other means> Examples of the other steps include a static elimination step, a recycling step, and a control step. Examples of the other means include a static elimination means, a recycling means, and a control means.
[0084] <<Static charge removal process and static charge removal means>> The charge removing step is a step of removing electricity by applying a charge removing bias voltage to the image bearing member, and is performed by the charge removing unit. The charge removing means is not particularly limited as long as it can apply a charge removing bias voltage to the image bearing member and can be appropriately selected depending on the purpose. For example, a charge removing lamp can be used.
[0085] <<Recycling process and recycling methods>> The recycling step is a step of recycling the toner removed in the cleaning step to the developing means, and is performed by the recycling means. The recycling means is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include known transport means.
[0086] <<Control process and control means>> The control step is a step of controlling each of the steps, and is carried out by a control means. The control means is not particularly limited as long as it can control the movement of each of the means, and can be appropriately selected depending on the purpose. Examples of the control means include devices such as a sequencer and a computer.
[0087] Here, an example of an image forming apparatus according to the present invention will be described with reference to the drawings.
[0088] [Figure 6] FIG. 6 is a schematic diagram of a printer (image forming apparatus) according to an embodiment of the present invention. Printer 500 is equipped with four imaging units 1Y for yellow, magenta, cyan, and black (hereinafter sometimes referred to as Y, C, M, and K, respectively), imaging unit 1C, imaging unit 1M, and imaging unit 1K (hereinafter sometimes referred to collectively as "imaging units 1"). These use different colors of Y, M, C, and K toner as image forming substances to form images, but are otherwise configured similarly.
[0089] A transfer unit 60 equipped with an intermediate transfer belt 14 as an intermediate transfer body is disposed above each of the four image creating units 1. The toner images of each color formed on the surfaces of the photoconductors 3Y, 3C, 3M, and 3K (which may be collectively referred to as "photoconductors 3") of each image creating unit 1 are transferred onto the surface of the intermediate transfer belt 14 in a superimposed manner.
[0090] An optical writing unit 40 is disposed below each of the four imaging units 1. The optical writing unit 40, which serves as a latent image forming means, irradiates each photoconductor 3 of each imaging unit 1 with laser light L emitted based on image information. This forms electrostatic latent images for Y, C, M, and K on each photoconductor 3. The optical writing unit 40 irradiates each photoconductor 3 with laser light L emitted from a light source via a plurality of optical lenses and mirrors while deflecting the laser light L by a polygon mirror 41 that is driven to rotate by a motor. Instead of such a configuration, a unit that performs optical scanning using an LDE array may also be employed.
[0091] A first paper feed cassette 151 and a second paper feed cassette 152 are disposed vertically stacked below the optical writing unit 40. Each of these paper feed cassettes contains a stack of transfer paper P, which is a recording medium, and a first paper feed roller 151a and a second paper feed roller 152a contact the topmost transfer paper P, respectively. 6 by a drive means not shown, the top transfer sheet P in the first paper feed cassette 151 is discharged toward the paper feed path 153 disposed to extend vertically on the right side of the cassette in FIG 6. When the second paper feed roller 152a is driven to rotate counterclockwise in FIG 6 by a drive means not shown, the top transfer sheet P in the second paper feed cassette 152 is discharged toward the paper feed path 153.
[0092] A plurality of conveying roller pairs 154 are disposed in the paper feed path 153. The transfer paper P sent into the paper feed path 153 is sandwiched between the rollers of the conveying roller pairs 154 and conveyed within the paper feed path 153 from the bottom to the top in FIG. A pair of registration rollers 55 is disposed at the downstream end in the transport direction of the paper feed path 153. As soon as the pair of registration rollers 55 pinches the transfer paper P sent from the pair of transport rollers 154 between the rollers, the pair of registration rollers 55 temporarily stops the rotation of both rollers. Then, the pair of registration rollers 55 sends the transfer paper P toward the secondary transfer nip, which will be described later, at an appropriate timing.
[0093] [Figure 7] FIG. 7 is a schematic diagram of an imaging unit according to an embodiment of the present invention. As shown in Fig. 7, the imaging unit 1 includes a drum-shaped photoconductor 3 serving as an image carrier. In Fig. 7, the photoconductor 3 is shown as being drum-shaped, but it may be in the form of a sheet or an endless belt. Around the photoconductor 3, there are arranged a charging roller 4, a developing device 5, a primary transfer roller 7, a cleaning device 6, a lubricant application device 10, a static elimination lamp (not shown), and the like. The charging roller 4 is a charging member provided in a charging device as a charging means, and the developing device 5 is a developing means for converting the latent image formed on the surface of the photoconductor 3 into a toner image. The primary transfer roller 7 is a primary transfer member provided in a primary transfer device as a primary transfer means for transferring the toner image on the surface of the photoconductor 3 onto the intermediate transfer belt 14. The cleaning device 6 is a cleaning means for cleaning the toner remaining on the photoreceptor 3 after the toner image is transferred onto the intermediate transfer belt 14 . The lubricant applicator 10 is a lubricant applicator that applies a lubricant onto the surface of the photoreceptor 3 after the cleaning device 6 has cleaned it. The charge removing lamp (not shown) is a charge removing unit that removes the surface potential of the photoconductor 3 after cleaning.
[0094] The charging roller 4 is disposed at a predetermined distance from the photoconductor 3 in a non-contact manner, and charges the photoconductor 3 to a predetermined polarity and a predetermined potential. The surface of the photoconductor 3 uniformly charged by the charging roller 4 is irradiated with laser light L from an optical writing unit 40, which is a latent image forming means, based on image information, and an electrostatic latent image is formed.
[0095] The developing device 5 has a developing roller 51 as a developer carrier. A developing bias is applied to the developing roller 51 from a power source (not shown). A supply screw 52 and an agitating screw 53 are provided in a casing of the developing device 5 to agitate the developer contained in the casing while transporting the developer in opposite directions. A doctor 54 is also provided to regulate the developer carried by the developing roller 51. The toner in the developer stirred and transported by the twin screws of the supply screw 52 and the stirring screw 53 is charged to a predetermined polarity. The developer is then pumped up onto the surface of the developing roller 51, and the pumped up developer is regulated by the doctor 54, and the toner adheres to the latent image on the photoconductor 3 in the development area facing the photoconductor 3.
[0096] The cleaning device 6 includes a fur brush 101, a cleaning blade 62, and the like. The cleaning blade 62 contacts the photoconductor 3 in a counter direction to the direction in which the surface of the photoconductor 3 moves.
[0097] The lubricant applicator 10 includes a solid lubricant 103, a lubricant pressure spring 103a, etc., and uses a fur brush 101 as an applicator brush for applying the solid lubricant 103 onto the photoconductor 3. The solid lubricant 103 is held by a bracket 103b, and is pressed toward the fur brush 101 by the lubricant pressure spring 103a. The solid lubricant 103 is scraped off by the fur brush 101, which rotates in the same direction as the rotation direction of the photoconductor 3, and the lubricant is applied onto the photoconductor 3. By applying the lubricant to the photoconductor 3, the friction coefficient of the surface of the photoconductor 3 is maintained at 0.2 or less during non-image formation. The lubricant applicator 10 may be omitted.
[0098] The charging device in this embodiment is a non-contact close-by arrangement type in which the charging roller 4 is placed close to the photoconductor 3, but the charging device may be a known type such as a corotron, scorotron, solid-state charger, etc. Of these charging methods, the contact charging method or the non-contact close-by arrangement method is more preferable, and has the advantages of high charging efficiency, low ozone generation, and the ability to miniaturize the device.
[0099] Any light-emitting material can be used as the light source of the laser light L of the optical writing unit 40, the charge removal lamp, etc. Specifically, a fluorescent lamp, a tungsten lamp, a halogen lamp, a mercury lamp, a sodium lamp, a light-emitting diode (LED), a semiconductor laser (LD), an electroluminescence (EL), etc. can be used. In order to irradiate only light in a desired wavelength range, various filters such as a sharp cut filter, a band pass filter, a near infrared cut filter, a dichroic filter, an interference filter, and a color temperature conversion filter can be used. Of these light sources, light emitting diodes and semiconductor lasers are preferably used since they have high irradiation energy and emit light with a long wavelength of 600 to 800 nm.
[0100] The transfer unit 60 as a transfer means includes, in addition to the intermediate transfer belt 14, a belt cleaning unit 162, a belt cleaning blade 162a, a first bracket 63, a second bracket 64, etc. It also includes four primary transfer rollers 7 (primary transfer roller 7Y, primary transfer roller 7C, primary transfer roller 7M, and primary transfer roller 7K), a secondary transfer backup roller 66, a drive roller 67, an auxiliary roller 68, a tension roller 69, etc. The intermediate transfer belt 14 is endlessly moved counterclockwise in FIG. 6 by the rotational drive of the drive roller 67 while being stretched around these eight roller members. The four primary transfer rollers 7 (primary transfer roller 7Y, primary transfer roller 7C, primary transfer roller 7M, and primary transfer roller 7K) sandwich the intermediate transfer belt 14 thus endlessly moved between each of the photoconductors 3 to form a primary transfer nip. A transfer bias of the opposite polarity (e.g., positive) to that of the toner is applied to the back surface (inner peripheral surface of the loop) of the intermediate transfer belt 14. As the intermediate transfer belt 14 passes through the primary transfer nips for Y, C, M, and K in sequence with its endless movement, the Y, C, M, and K toner images on each of the photoconductors 3 are primarily transferred onto the front surface of the intermediate transfer belt 14 in a superimposed manner. As a result, a four-color superimposed toner image (hereinafter referred to as a four-color toner image) is formed on the intermediate transfer belt 14.
[0101] The secondary transfer backup roller 66 sandwiches the intermediate transfer belt 14 between itself and a secondary transfer roller 70 disposed outside the loop of the intermediate transfer belt 14 to form a secondary transfer nip. The pair of registration rollers 55 sends the transfer paper P sandwiched between the rollers toward the secondary transfer nip at a timing that allows synchronization with the four-color toner image on the intermediate transfer belt 14. The four-color toner image on the intermediate transfer belt 14 is collectively secondarily transferred to the transfer paper P in the secondary transfer nip by the influence of the secondary transfer electric field formed between the secondary transfer roller 70 to which a secondary transfer bias is applied and the secondary transfer backup roller 66, and the nip pressure. Then, combined with the white color of the transfer paper P, it becomes a full-color toner image.
[0102] Residual toner that has not been transferred to the transfer paper P and remains on the intermediate transfer belt 14 after passing through the secondary transfer nip is cleaned by a belt cleaning unit 162. The belt cleaning unit 162 brings a belt cleaning blade 162a into contact with the front surface of the intermediate transfer belt 14, thereby scraping off and removing the residual toner on the intermediate transfer belt 14.
[0103] The first bracket 63 of the transfer unit 60 is adapted to swing around the axis of rotation of the auxiliary roller 68 at a predetermined rotation angle as the driving of a solenoid (not shown) is turned on and off. When forming a monochrome image, the printer 500 rotates the first bracket 63 slightly counterclockwise in FIG. 6 by driving the solenoid described above. This rotation causes the primary transfer rollers 7Y, 7C, and 7M for Y, C, and M to revolve counterclockwise in FIG. 6 around the rotation axis of the auxiliary roller 68, thereby separating the intermediate transfer belt 14 from the photoconductors 3Y, 3C, and 3M for Y, C, and M. Then, of the imaging units 1, only the imaging unit 1K for K is driven to form a monochrome image. This makes it possible to suppress wear of the members constituting the imaging unit 1 caused by unnecessary driving of the imaging units for Y, C, and M during monochrome image formation.
[0104] A fixing unit 80 is disposed above the secondary transfer nip in FIG. 6. The fixing unit 80 includes a pressure heating roller 81 containing a heat source such as a halogen lamp, and a fixing belt unit 82. The fixing belt unit 82 includes a fixing belt 84 as a fixing member, a heating roller 83 containing a heat source such as a halogen lamp, a tension roller 85, a driving roller 86, a temperature sensor (not shown), and the like. The endless fixing belt 84 is stretched by the heating roller 83, the tension roller 85, and the driving roller 86 and moves endlessly in the counterclockwise direction in FIG. 6. During this endless movement, the fixing belt 84 is heated from the back side by the heating roller 83. The pressure heating roller 81, which is driven to rotate in the clockwise direction in FIG. 6, abuts on the front side of the heated fixing belt 84 at the portion where the fixing belt 84 is wrapped around the heating roller 83. This forms a fixing nip where the pressure heating roller 81 and the fixing belt 84 abut on each other.
[0105] A temperature sensor (not shown) is disposed outside the loop of the fixing belt 84 so as to face the front surface of the fixing belt 84 with a predetermined gap therebetween, and detects the surface temperature of the fixing belt 84 immediately before it enters the fixing nip and transmits the detection result to a fixing power circuit (not shown). The fixing power circuit controls the on / off supply of power to the heat source contained in the heating roller 83 and the heat source contained in the pressure heating roller 81 based on the detection result by the temperature sensor.
[0106] After passing through the secondary transfer nip described above, the transfer paper P is separated from the intermediate transfer belt 14 and then sent into the fixing unit 80. Then, in the process of being conveyed from the bottom to the top in FIG. 6 while being sandwiched in the fixing nip inside the fixing unit 80, the full-color toner image is fixed onto the transfer paper P by being heated and pressed by the fixing belt 84. The transfer paper P that has been subjected to the fixing process is discharged outside the machine after passing between the rollers of the discharge roller pair 87. A stack section 88 is formed on the upper surface of the housing of the printer 500 main body, and the transfer paper P discharged outside the machine by the discharge roller pair 87 is stacked in this stack section 88 in order.
[0107] Four toner cartridges 100Y, 100C, 100M, and 100K (collectively referred to as "toner cartridges 100") containing Y, C, M, and K toners are disposed above the transfer unit 60. The Y, C, M, and K toners in each toner cartridge 100 are appropriately supplied to the developing devices 5 (developing device 5Y, developing device 5C, developing device 5M, and developing device 5K) of each image creating unit 1. Each toner cartridge 100 is detachable from the printer body independently of each image creating unit 1.
[0108] Next, the image forming operation in the printer 500 will be described. When a print execution signal is received from an operation unit (not shown) or the like, a predetermined voltage or current is applied sequentially and at a predetermined timing to the charging roller 4 and the developing roller 51. Similarly, a predetermined voltage or current is applied sequentially and at a predetermined timing to the optical writing unit 40 and a light source such as a static electricity removal lamp, etc. In synchronization with this, the photoconductor 3 is rotated in the direction of the arrow in FIG. 6 by a photoconductor drive motor (not shown) serving as a drive means. When the photoconductor 3 rotates in the direction of the arrow in FIG. 6, the surface of the photoconductor 3 is uniformly charged to a predetermined potential by the charging roller 4. Then, the optical writing unit 40 irradiates the photoconductor 3 with a laser beam L corresponding to image information, and the portion of the photoconductor 3 surface irradiated with the laser beam L is discharged to form an electrostatic latent image. The surface of the photoconductor 3 on which the electrostatic latent image has been formed is rubbed by a magnetic brush of developer formed on the developing roller 51 at the portion facing the developing device 5. At this time, the negatively charged toner on the developing roller 51 moves to the electrostatic latent image side by a predetermined developing bias applied to the developing roller 51, and is turned into a toner image (developed). In each imaging unit 1, a similar imaging process is performed, and a toner image of each color is formed on the surface of each photoconductor 3 of each imaging unit 1. In this way, in the printer 500, the electrostatic latent image formed on the photoconductor 3 is reverse-developed by the developing device 5 using negatively charged toner. In this embodiment, an example using an N / P (negative / positive: toner adheres to areas with low potential) non-contact charging roller method has been described, but the present invention is not limited to this.
[0109] The toner images of each color formed on the surface of each photoconductor 3 are sequentially transferred to the intermediate transfer belt 14 so as to be superimposed on the surface of the intermediate transfer belt 14. As a result, a four-color toner image is formed on the intermediate transfer belt 14. The four-color toner image formed on the intermediate transfer belt 14 is transferred to the transfer paper P fed from the first paper feed cassette 151 or the second paper feed cassette 152, passed between the rollers of the registration roller pair 55, and fed to the secondary transfer nip. At this time, the transfer paper P is stopped once while being sandwiched between the registration roller pair 55, and is fed to the secondary transfer nip in synchronization with the leading edge of the image on the intermediate transfer belt 14. The transfer paper P to which the toner image has been transferred is separated from the intermediate transfer belt 14 and conveyed to the fixing unit 80. Then, the transfer paper P to which the toner image has been transferred passes through the fixing unit 80, whereby the toner image is fixed to the transfer paper P by the action of heat and pressure, and then discharged outside the printer 500 and stacked in the stack section 88.
[0110] Meanwhile, residual toner remaining on the surface of the intermediate transfer belt 14, from which the toner image has been transferred to the transfer paper P at the secondary transfer nip, is removed by a belt cleaning unit 162. Furthermore, residual toner remaining on the surface of the photoconductor 3, from which the toner images of each color have been transferred to the intermediate transfer belt 14 at the primary transfer nip, is removed by a cleaning device 6, a lubricant is applied by a lubricant application device 10, and then the surface is neutralized by a neutralization lamp. As shown in Fig. 7, each imaging unit 1 of the printer 500 includes a photoconductor 3, a charging roller 4, a developing device 5, a cleaning device 6, a lubricant applicator 10, etc. housed in a frame 2. The imaging unit 1 is detachable from the main body of the printer 500 as a process cartridge. In the printer 500, the imaging unit 1 is configured so that the photoconductor 3 and the process means as a process cartridge are replaced as a whole. Alternatively, the photoconductor 3, the charging roller 4, the developing device 5, the cleaning device 6, and the lubricant applicator 10 may be replaced as a unit with new ones.
[0111] The printer may also be configured to be capable of forming a single color image, and may also be configured to perform copying based on image data read by an image reading unit (not shown).
[0112] (Process cartridge) The process cartridge of the present invention has a cleaning blade as a cleaning blade means, and may have an image bearing member, a charging means, an exposure means, a developing means, a transfer means, a discharging means, and a lubricant application means, if necessary. Incidentally, each configuration of the process cartridge is the same as that described in the above section (Image forming apparatus and image forming method), and therefore description thereof will be omitted. The process cartridge is a device (component) that is detachably mountable to an image forming apparatus. EXAMPLES
[0113] Examples and comparative examples of the present invention will be described below, but the present invention is not limited to these examples and comparative examples. However, "parts" refers to "parts by mass" unless otherwise specified.
[0114] Example 1 <Cleaning Blade Production> <<Elastic member and supporting member>> The elastic member was a polyurethane elastomer sheet obtained by centrifugal molding, curing and post-crosslinking. The average thickness, Martens hardness (HM) and dimensions of the polyurethane elastomer sheet were as follows: Average thickness: 2.0mm Martens hardness (HM): 1.0N / mm 2 Dimensions: 356mm x 13.5mm The polyurethane elastomer sheet was attached at its end to a metal plate having the following material and dimensions: Material: Stainless steel plate Dimensions: 354mm x 15.6mm
[0115] <<Preparation of coating solution>> --Preparation of particle dispersion A-- Five parts of polytetrafluoroethylene (PTFE) micropowder (TF9201Z, manufactured by 3M, volume average particle size 200 nm) as a first fluororesin, two parts of a VdF-HFP-TFE ternary copolymer consisting of vinylidene fluoride (VdF), hexafluoropropylene (HFP), and tetrafluoroethylene (TFE) as a second fluororesin, and 93 parts of 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether (HFE-347, manufactured by Tokyo Chemical Industry Co., Ltd.) as a fluorine-based inert liquid were placed in a screw tube and stirred with a stirrer or the like to prepare particle dispersion A. The viscosity of the particle dispersion A was 1.85 mPa·s, which was measured using a vibration viscometer (manufactured by Sekonic Corporation).
[0116] <<Dipping>> One end surface (cleaning blade tip surface) used as the tip of the cleaning blade on the peripheral side surface was immersed to a depth of 2 mm in the particle dispersion A and then pulled up. At this time, the immersion angle was set to 30° and the pulling speed was set to 5 mm / s. Thereafter, the cleaning blade of Example 1 was produced by drying for 30 minutes at room temperature (25°C).
[0117] <Assembly of image forming device> The cleaning blade of Example 1 was attached to a process cartridge of a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.) (the printer section has a similar configuration to the printer 500 shown in FIG. 6) to assemble an image forming apparatus. The cleaning blade was attached to the image forming apparatus so that the linear pressure was 20 g / cm and the cleaning angle was 79°.
[0118] (Examples 2 to 5 and Comparative Examples 1 to 4) Cleaning blades of Examples 2 to 5 and Comparative Examples 1 to 4 were produced in the same manner as in Example 1, except that the immersion angle and the lifting speed were changed as shown in Table 1.
[0119] (Measurement of the average thickness of the coating layer) The average thickness of the coating layer was measured by observing the cross section of the cleaning blade using a laser microscope OLS-4100 (manufactured by Olympus Corporation). Specifically, using a trimming razor for preparing SEM samples (manufactured by Nisshin EM), the coating layer on the surface of the cleaning blade was partially scraped off until the elastic material was exposed, and the average thickness of the coating layer was calculated by measuring the height difference between the surface where the coating layer was scraped off (the upper surface of the elastic material) and the surface where the coating layer was not scraped off (the upper surface of the coating layer). The average thickness of the coating layer was determined as the average value of the values obtained by measuring five positions, namely, positions 41 mm, 110 mm, 178 mm, 247 mm, and 315 mm away from the cleaning blade side surface 62d in the longitudinal direction at positions 0.02 mm, 0.1 mm, and 0.3 mm away from the tip ridge portion 62c of the cleaning blade tip surface 62a.
[0120] (torque rating) Thermocouples were attached to the cleaning blade holders of Examples 1 to 5 and Comparative Examples 1 to 4 to measure their temperatures, and the cleaning blades were then installed in a Ricoh ProC9200 color multifunction printer. Laboratory environment: 29°C and 60% RH, paper feed conditions: a free run was performed, and after the cleaning blade holder temperature rose and became constant, paper feed was continued for one hour. The condition of the cleaning blade after paper feed was visually observed and evaluated according to the following evaluation criteria. --Evaluation criteria-- ○: No curling was observed ×: Occurrence of curling was confirmed.
[0121] (Cleaning rating) The cleaning blades of Examples 1 to 5 and Comparative Examples 1 to 4 were installed in a Ricoh color multifunction printer Ricoh ProC9200, and 3,600 sheets (A4 landscape) were printed using a color stability chart under laboratory conditions of 29°C and 60% RH. The presence or absence of adhesions on the image carrier, fur brush, and printed paper was visually confirmed. Evaluation was made according to the following criteria. --Evaluation criteria-- 〇: No adhesions were found ×: Adhesion was observed
[0122] [Table 1]
[0123] In Examples 1 to 5, no curling occurred, and no deposits were found on the image carrier, the fur brush, or the printed paper, and good results were obtained in all respects. In Comparative Example 1, the lifting speed was increased compared to Example 3, so the thickness of the coating layer was increased, and although no curling occurred, deposits occurred on the image carrier, fur brush, and printed paper. In Comparative Example 2, the immersion angle was set to 0° compared to Example 3, so dripping from the tip surface of the blade was suppressed. As a result, the thickness of the coating layer near the tip ridge increased, and although no curling occurred, deposits occurred on the image carrier, fur brush, and printed paper. In Comparative Example 3, the immersion angle was set to 50° compared to Example 3, which promoted dripping from the tip surface of the blade. As a result, the thickness of the coating layer increased as the distance from the tip ridge increased, and although no curling occurred, deposits were formed on the image carrier, fur brush, and printed paper. In Comparative Example 4, the lifting speed was slower than in Example 1, so the thickness of the coating layer was reduced, and although no adhesion occurred on the image carrier, fur brush, or printed paper, curling did occur.
[0124] For example, aspects of the present invention are as follows. <1> A cleaning blade having an elastic member and a coating layer, The cleaning blade is a cleaning blade that removes residue by contacting a tip edge portion of the cleaning blade with a surface of a member to be cleaned, the coating layer is provided on a cleaning blade tip surface which includes the tip ridge portion and is parallel to a thickness direction of the elastic member, and on a cleaning blade underside which includes the tip ridge portion and faces the member to be cleaned, The cleaning blade is characterized in that the average thickness of the coating layer on the tip surface of the cleaning blade increases with increasing distance from the tip ridge line. <2> the average thickness of the coating layer at a distance of 0.02 mm from the edge of the tip of the cleaning blade is 0.5 μm or more and 3 μm or less; the average thickness of the coating layer at a distance of 0.1 mm from the edge of the tip of the cleaning blade is 1 μm or more and 7 μm or less; The average thickness of the coating layer at a distance of 0.3 mm from the edge of the tip of the cleaning blade is 3 μm or more and 10 μm or less. <1> 2. The cleaning blade according to claim 1 . <3> The coating layer includes a first fluororesin and a second fluororesin that is incompatible with the first fluororesin. <1> or the above <2> 2. The cleaning blade according to claim 1, <4> The above <1> From the above <3> A method for producing a cleaning blade according to any one of the above, an immersion step of immersing the elastic member in a coating liquid; a lifting step of lifting the elastic member from the coating liquid, The method for producing a cleaning blade is characterized in that in the immersion step, the angle between the coating liquid surface and the tip surface of the cleaning blade is 5° or more and 45° or less. <5> The coating liquid includes a first fluororesin, a second fluororesin incompatible with the first fluororesin, and a fluorine-based inactive liquid. <4> 2. A method for producing the cleaning blade according to claim 1. <6> a total content of the first fluororesin and the second fluororesin is 5% by mass or more and 10% by mass or less with respect to a total amount of the coating liquid, The content of the fluorine-based inactive liquid is 90% by mass or more and 95% by mass or less with respect to the total amount of the coating liquid. <5> 2. A method for producing the cleaning blade according to claim 1. <7> A measuring step of measuring the contents of the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid in the coating liquid, adjusting a lifting speed of the elastic member in the lifting step based on the results obtained in the measuring step; <5> or the above <6> 2. A method for producing the cleaning blade according to claim 1. <8> A measuring step of measuring the contents of the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid in the coating liquid, Based on the results obtained in the measuring step, the fluorine-based inert liquid is replenished, and the contents of the first fluorine resin, the second fluorine resin, and the fluorine-based inert liquid in the coating liquid are adjusted. <5> From the above <7> 13. A method for producing the cleaning blade according to claim 12. <9> The above <1> From the above <3> 2. A process cartridge comprising the cleaning blade according to claim 1. <10> The above <1> From the above <3> 2. An image forming apparatus comprising the cleaning blade according to claim 1.
[0125] The above <1> From the above <3> The cleaning blade according to any one of the preceding claims. <4> From the above <8> The method for producing a cleaning blade according to any one of the <9> The process cartridge according to the <10> According to the image forming apparatus described in the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0126] 1 Imaging unit 1Y Imaging unit (for yellow) 1C Imaging unit (for cyan) 1M Imaging unit (for magenta) 1K Imaging unit (for black) 10 Lubricant application device 100Y toner cartridge (for yellow) 100C Toner Cartridge (for Cyan) 100M Toner Cartridge (Magenta) 100K toner cartridge (for black) 101 Fur Brush 103 Solid lubricants 103a Lubricant pressure spring 103b Bracket 14 Intermediate transfer belt 151 First paper feed cassette 151a First paper feed roller 152 Second paper feed cassette 152a Second feed roller 153 Paper feed path 154 Transport roller pair 162 Belt cleaning unit 162a Belt cleaning blade 201 Storage Tank 203 Lubrication Pump 204 Coating tank 205 Mixer 206 Viscometer 207 Fluorine-based activated liquid 208 Filters 209 Cooling jacket 210 Food 211 Steam Tank 213 Elevator 2 frame 3 Photoreceptor 3Y Photoconductor (for yellow) 3C Photoconductor (for cyan) 3M Photoconductor (for magenta) 3K photoconductor (for black) 4. Charging roller 40 Optical writing unit 41 Polygon Mirror 5. Developing device 5Y developing unit (for yellow) 5C Developer (for cyan) 5M Developing Unit (for Magenta) 5K Developing Unit (Black) 51 Developing roller 52 Supply screw 53 Mixing screw 54 Doctor 55 Registration roller pair 6 Cleaning device 60 Transcription Unit 600 Coating Liquid 62 Cleaning blade 62a Cleaning blade tip surface 62b Underside of cleaning blade 62c Tip ridge 62d Cleaning blade side 621 Holder 622 Elastic Blade 623 Covering layer 63 First Bracket 64 Second bracket 66 Secondary transfer backup roller 67 Drive roller 68 Auxiliary roller 69 Tension roller 7 Primary transfer roller 7Y Primary transfer roller (for yellow) 7C Primary transfer roller (for cyan) 7M Primary Transfer Roller (for Magenta) 7K Primary transfer roller (for black) 70 Secondary transfer roller 8. Charge roller cleaner 80 Fuser unit 81 Pressure and heating roller 82 Fixing belt unit 83 Heating Roller 84 Fixing belt 85 Tension roller 86 Drive roller 87 Paper ejection roller pair 88 Stack Section 500 Printers L Laser light P Transfer paper D Distance from the edge of the cleaning blade [Prior art documents] [Patent documents]
[0127] [Patent Document 1] Japanese Patent Application Publication No. 2-82283 [Patent Document 2] JP 2014-178441 A
Claims
1. A cleaning blade having an elastic member and a coating layer, The cleaning blade is a cleaning blade that removes residue by contacting a tip edge portion of the cleaning blade with a surface of a member to be cleaned, the coating layer is provided on a cleaning blade tip surface which includes the tip ridge portion and is parallel to a thickness direction of the elastic member, and on a cleaning blade underside which includes the tip ridge portion and faces the member to be cleaned, A cleaning blade, characterized in that an average thickness of the coating layer on the tip surface of the cleaning blade increases with increasing distance from the tip ridge line.
2. the average thickness of the coating layer at a distance of 0.02 mm from the edge of the tip of the cleaning blade is 0.5 μm or more and 3 μm or less; the average thickness of the coating layer at a distance of 0.1 mm from the edge of the tip of the cleaning blade is 1 μm or more and 7 μm or less; 2. The cleaning blade according to claim 1, wherein an average thickness of the coating layer at a distance of 0.3 mm from the edge line of the tip surface of the cleaning blade is 3 μm or more and 10 μm or less.
3. The cleaning blade according to claim 1 , wherein the coating layer comprises a first fluororesin and a second fluororesin that is incompatible with the first fluororesin.
4. A method for producing the cleaning blade according to claim 1, comprising the steps of: an immersion step of immersing the elastic member in a coating liquid; a lifting step of lifting the elastic member from the coating liquid, a cleaning blade manufacturing method comprising the steps of: immersing the cleaning blade in a liquid covering the cleaning blade and forming an angle between the liquid surface and the tip surface of the cleaning blade in the immersion step;
5. The method for producing a cleaning blade according to claim 4 , wherein the coating liquid contains a first fluororesin, a second fluororesin incompatible with the first fluororesin, and a fluorine-based inactive liquid.
6. a total content of the first fluororesin and the second fluororesin is 5% by mass or more and 10% by mass or less with respect to a total amount of the coating liquid, The method for producing a cleaning blade according to claim 5 , wherein the content of the fluorine-based inactive liquid is from 90% by mass to 95% by mass based on the total amount of the coating liquid.
7. A measuring step of measuring the contents of the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid in the coating liquid, The method for producing a cleaning blade according to claim 6 , further comprising adjusting a lifting speed of the elastic member in the lifting step based on the result obtained in the measuring step.
8. A measuring step of measuring the contents of the first fluororesin, the second fluororesin, and the fluorine-based inactive liquid in the coating liquid, 7. The method for producing a cleaning blade according to claim 6, further comprising the steps of: replenishing the fluorine-based inactive liquid based on the results obtained in the measurement step, and adjusting the contents of the first fluorine-based resin, the second fluorine-based inactive liquid in the coating liquid.
9. 4. A process cartridge comprising the cleaning blade according to claim 1.
10. 4. An image forming apparatus comprising the cleaning blade according to claim 1.
Citation Information
Patent Citations
Method for coating lubricant on cleaning blade of cleaning device for image forming device