Lithium ion secondary battery
The lithium-ion secondary battery addresses cobalt depletion concerns by using a high Ni content lithium-transition metal composite oxide with specific particle structure and a Si-containing negative electrode material, achieving reduced initial resistance and storage stability.
Patent Information
- Application Number
- JP2023075673
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2043-05-01
AI Technical Summary
The increasing demand for lithium-ion secondary batteries has raised concerns about the depletion of cobalt (Co) and the resulting increase in initial resistance and resistance during storage when the Co content in the positive electrode active material is reduced.
A lithium-ion secondary battery design that includes a positive electrode with a high Ni content lithium-transition metal composite oxide (75% Ni based on total metal elements excluding Li) and secondary particles with an aspect ratio of 1.9 or more primary particles, combined with a negative electrode containing a carbon material and a Si-containing material, to suppress initial resistance and resistance increase during storage.
The design effectively reduces cobalt content while maintaining low initial resistance and preventing resistance increase during storage, enhancing the battery's performance and stability.
Smart Images

Figure 2024160551000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to lithium-ion secondary batteries. [Background technology]
[0002] Lithium ion secondary batteries are suitable for use as driving power sources mounted on vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and electric vehicles (BEVs), and the demand for lithium ion secondary batteries is rapidly expanding. As a positive electrode active material used in lithium ion secondary batteries, lithium transition metal composite oxides are used, and among them, lithium nickel cobalt manganese composite oxides containing Ni, Co, and Mn as shown in Patent Document 1 are exemplified. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-191662 A Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, in recent years, as the demand for lithium ion secondary batteries increases, there is concern about the depletion of cobalt (Co) used in lithium ion secondary batteries. As a countermeasure, it is considered to reduce the content of Co in the positive electrode active material. However, as a result of intensive research by the present inventors, it has been found that when the content of Co in the positive electrode active material is reduced, the initial resistance and the resistance during storage of the lithium ion secondary battery increase significantly.
[0005] The technology disclosed herein has been made in consideration of the above circumstances, and aims to provide a lithium-ion secondary battery in which the cobalt content in the positive electrode active material is reduced while suppressing the initial resistance and the increase in resistance during storage. [Means for solving the problem]
[0006] The technology disclosed herein relates to a lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, the positive electrode comprising a positive electrode active material layer containing a positive electrode active material, the positive electrode active material comprising a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, the lithium transition metal composite oxide having a content of Ni of 75 mol % or more with respect to a total of metal elements other than Li, the lithium transition metal composite oxide being secondary particles formed by aggregation of primary particles, the primary particles having an aspect ratio of 1.9 or more, the negative electrode comprising a negative electrode active material layer containing a negative electrode active material, the negative electrode active material comprising a carbon material and a Si-containing material, and a content ratio of Si element in the negative electrode active material being 5 mass % or more and 10 mass % or less when a total amount of the negative electrode active material is taken as 100 mass %.
[0007] According to this configuration, the composition of the positive electrode active material, specifically the content of Ni in the lithium transition metal composite oxide, is set to a predetermined range. The lithium transition metal composite oxide is a secondary particle, and the aspect ratio of the primary particle of the lithium transition metal composite oxide is 1.9 or more. Furthermore, the negative electrode active material contains a predetermined amount of Si-containing material in addition to the carbon material. This makes it possible to provide a lithium ion secondary battery that reduces the cobalt content in the positive electrode active material while suppressing the initial resistance and the increase in resistance during storage. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic internal structure of a lithium-ion secondary battery according to one embodiment. [Diagram 2] FIG. 2 is a schematic exploded view showing the configuration of an electrode body of a lithium ion secondary battery according to one embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing the configuration of a positive electrode active material according to one embodiment. [Figure 4] FIG. 4 is a schematic diagram showing the configuration of a negative electrode sheet (negative electrode) according to one embodiment. [Diagram 5]FIG. 5 is a view corresponding to FIG. 4 and showing the configuration of a negative electrode sheet (negative electrode) according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, some preferred embodiments of the lithium ion secondary battery disclosed herein will be described with reference to the drawings as appropriate. Matters other than those specifically mentioned in this specification and necessary for implementing the present disclosure (for example, the general configuration and manufacturing process of a lithium ion secondary battery that does not characterize the present disclosure) can be understood as design matters of a person skilled in the art based on the prior art in the field. The lithium ion secondary battery disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field.
[0010] In the following drawings, the same reference numerals are used for components and parts that perform the same function, and duplicated explanations may be omitted or simplified. In this specification, the notation "A to B" indicating a range includes not only the meaning of A or more and B or less, but also the meanings of "preferably larger than A" and "preferably smaller than B." In this specification, a "lithium ion secondary battery" (hereinafter sometimes simply referred to as a "battery") refers to a general electricity storage device that uses lithium ions as a charge carrier and can be repeatedly charged and discharged by the transfer of charge associated with the lithium ions between the positive and negative electrodes.
[0011] Hereinafter, the present disclosure will be described in detail using as an example a flat prismatic lithium ion secondary battery having a flat electrode body and a flat battery case, but it is not intended that the present disclosure be limited to the embodiment described therein.
[0012] FIG. 1 is a cross-sectional view showing a schematic internal structure of a lithium ion secondary battery according to an embodiment. The lithium ion secondary battery 100 shown in FIG. 1 is a sealed battery constructed by housing a flat electrode body 20 and a non-aqueous electrolyte 80 in a flat rectangular battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The battery case 30 is also provided with an injection port (not shown) for injecting the non-aqueous electrolyte 80. The positive electrode terminal 42 is electrically connected to the positive electrode current collector plate 42a. The negative electrode terminal 44 is electrically connected to the negative electrode current collector plate 44a. The material of the battery case 30 is, for example, a lightweight metal material with good thermal conductivity, such as aluminum.
[0013] Fig. 2 is a schematic exploded view showing the configuration of an electrode body of a lithium ion secondary battery according to one embodiment. As shown in Figs. 1 and 2, the electrode body 20 has a configuration in which a strip-shaped positive electrode sheet 50 and a strip-shaped negative electrode sheet 60 are overlapped with two strip-shaped separators 70 interposed therebetween and wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long-sized positive electrode collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long-sized negative electrode collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are respectively joined to the positive electrode current collector 42a and the negative electrode current collector 44a. The positive electrode sheet 50 is an example of the "positive electrode" disclosed herein, and the negative electrode sheet 60 is an example of the "negative electrode" disclosed herein.
[0014] <Positive electrode> The positive electrode (positive electrode sheet 50) disclosed herein includes a positive electrode active material layer 54. As shown in Fig. 2, the positive electrode (positive electrode sheet 50) here includes a positive electrode current collector 52 and a positive electrode active material layer 54 supported by the positive electrode current collector 52. Note that, although the positive electrode active material layer 54 is illustrated only on one surface of the positive electrode current collector 52 in this embodiment, the positive electrode active material layer 54 may be provided on both surfaces of the positive electrode current collector 52.
[0015] 3 is a schematic diagram showing a configuration of a positive electrode active material 56 according to one embodiment. The positive electrode active material layer 54 contains a positive electrode active material 56 capable of reversibly absorbing and releasing charge carriers. The positive electrode active material 56 according to this embodiment includes a lithium transition metal composite oxide 56a serving as a base material, and a coating portion 56c disposed on at least a portion of the surface of the lithium transition metal composite oxide 56a. The coating portion 56c is typically disposed on the lithium transition metal composite oxide 56a by physical and / or chemical bonding.
[0016] The lithium transition metal composite oxide 56a according to this embodiment has a layered structure and contains lithium (Li), nickel (Ni), and manganese (Mn) as essential elements. The lithium transition metal composite oxide 56a according to this embodiment is a so-called high Ni content lithium transition metal composite oxide in which the content of Ni relative to the total of metal elements other than Li is 75 mol % or more. The high Ni content lithium transition metal composite oxide is an example of the "lithium transition metal composite oxide in which the content of Ni relative to the total of metal elements other than Li is 75 mol % or more" disclosed herein.
[0017] The positive electrode active material may contain a positive electrode active material other than the lithium transition metal composite oxide 56a within a range that does not impair the effects of the present disclosure (for example, less than 10 mass % relative to the total mass of the positive electrode active material, preferably 5 mass % or less). Also, the positive electrode active material may be composed only of the lithium transition metal composite oxide 56a.
[0018] From the viewpoint of high volumetric energy density of the lithium ion secondary battery, the content of Ni in the total of metal elements other than Li in the lithium transition metal composite oxide 56a is preferably 80 mol % or more, more preferably 90 mol % or more. On the other hand, from the viewpoint of high stability, the content of Ni in the total of metal elements other than Li is preferably 95 mol % or less, more preferably 90 mol % or less.
[0019] Examples of the lithium transition metal composite oxide 56a having a layered structure include lithium nickel manganese composite oxide, lithium nickel cobalt manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide. These may be used alone or in combination of two or more. It can be confirmed by a known method (e.g., X-ray diffraction method) that the particles of the high Ni-containing lithium transition metal composite oxide have a layered structure (i.e., a layered crystal structure).
[0020] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. This also applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0021] In some preferred embodiments, the lithium transition metal composite oxide 56a preferably has a composition represented by the following general formula (i): Li α Ni xMn y M z O2...Equation (i) In the above formula (i), x, y, z, and α respectively satisfy the following: 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, and x+y+z=1. M in the formula (i) is at least one element selected from the group consisting of Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
[0022] In the above formula (i), α preferably satisfies 0.9≦α≦1.2, and more preferably satisfies 1.0≦α≦1.1. From the viewpoint of battery characteristics (e.g., energy density, cycle characteristics, and thermal stability), x preferably satisfies 0.8≦x≦0.95, and more preferably satisfies 0.8≦x≦0.9. From the viewpoint of, for example, energy density, thermal stability, and cost, y preferably satisfies 0.1≦y≦0.25, and more preferably satisfies 0.17≦y≦0.25. Z preferably satisfies 0≦z≦0.1, and more preferably satisfies 0≦z≦0.03, and further preferably is 0. In addition, in the above formula (i), "x+y+z=1" includes the case where x+y+z is 1, and is substantially regarded as 1 as long as the effect of the technology disclosed herein can be realized, and typically, x+y+z=0.95 to 1.1, and preferably x+y+z=0.99 to 1.05.
[0023] In some preferred embodiments, the lithium transition metal composite oxide 56a preferably contains W. In other words, the lithium transition metal composite oxide 56a is preferably doped with W as an additive element. This stabilizes the layered structure of the lithium transition metal composite oxide 56a, and thus improves the initial resistance more preferably, and suppresses the elution of Mn into the non-aqueous electrolyte, thereby more preferably suppressing the increase in resistance during storage. When the lithium transition metal composite oxide 56a is doped with W as an additive element (solid solution), it is preferably doped at 0.1 to 0.5 mol %, and more preferably doped at 0.1 to 0.3 mol %, based on the total of the transition metal elements of the lithium transition metal composite oxide 56a other than W.
[0024] The lithium transition metal composite oxide 56a has the following relationship between the Co element content (mol) and the Mn element content (mol): 0≦Co / Mn≦0.42 It is preferable that the ratio be 0≦Co / Mn≦0.25, and it is even more preferable that the ratio be 0≦Co / Mn≦0.21. This allows the content ratio of Co and Mn in the positive electrode active material to be appropriately controlled. In the above-mentioned relationship, the smaller the value of Co / Mn, the more preferably the cobalt content in the lithium transition metal composite oxide 56a can be reduced while suppressing an increase in resistance during storage.
[0025] In lithium transition metal composite oxides used in conventional lithium ion secondary batteries, the content ratio of Co element to metal elements other than Li is typically about 10 mol % to 40 mol %. However, since cobalt resources are limited, in this embodiment, it is preferable to reduce the Co content of the lithium transition metal composite oxide 56a compared to the conventional case. Therefore, in some preferred embodiments, the content ratio of Co to the total of metal elements other than Li is, for example, preferably 5 mol % or less, more preferably 3 mol % or less, and even more preferably 0 mol % (i.e., Co-free).
[0026] As shown in FIG. 3, the lithium transition metal composite oxide 56a is in the form of secondary particles in which a plurality of primary particles 56p are typically aggregated by physical or chemical bonding forces. The number of primary particles 56p of the lithium transition metal composite oxide 56a constituting the secondary particles of the lithium transition metal composite oxide 56a is not particularly limited, but is, for example, approximately 10 or more, preferably approximately 30 or more, and more preferably approximately 50 or more. The number of primary particles 56p is not particularly limited, but may be, for example, approximately 120 or less. In this specification, the term "primary particle" refers to the smallest unit of particles constituting the positive electrode active material, and more specifically, refers to the smallest unit determined from the geometric shape of the appearance observed under an electron microscope. In this specification, an aggregate formed by aggregation of 10 or more such primary particles 56p is called a "secondary particle".
[0027] In this embodiment, the primary particles 56p have a so-called elongated shape with an aspect ratio (major axis / minor axis ratio) of 1.9 or more. This allows the initial resistance to be suitably improved. The major axis of the primary particles 56p according to this embodiment typically extends substantially parallel to the direction (a-axis) perpendicular to the stacking direction (c-axis) of the layered lithium transition metal composite oxide. The minor axis of the primary particles 56p according to this embodiment typically extends substantially parallel to the stacking direction (c-axis). The upper limit of the aspect ratio of the primary particles 56p is not particularly limited, but is preferably 2.5 or less, more preferably 2.2 or less, for example.
[0028] In this specification, the "aspect ratio of primary particles" refers to the long axis / short axis ratio of primary particles 56p constituting the lithium transition metal composite oxide 56a. The aspect ratio of primary particles refers to the average value of the long axis / short axis ratio of a plurality of primary particles 56p that are arbitrarily selected from a cross-sectional electron microscope image of the lithium transition metal composite oxide 56a. The plurality of primary particles 56p may be, for example, 20 or more. Specifically, the average particle diameter of the primary particles 56p is obtained by, for example, preparing a cross-sectional observation sample of the lithium transition metal composite oxide 56a by cross-section polisher processing. Next, an SEM image of the cross-sectional observation sample of the lithium transition metal composite oxide 56a is obtained using a scanning electron microscope (SEM). Then, the aspect ratio (ratio of long axis to short axis) is calculated based on the long axis and short axis of a plurality of primary particles 56p arbitrarily selected from the SEM image using image analysis type particle size distribution measurement software (for example, "Mac-View"), and the arithmetic average value is obtained.
[0029] The average particle diameter of the primary particles 56p of the lithium transition metal composite oxide 56a is not particularly limited. For example, from the viewpoint of high output characteristics and cycle characteristics of the positive electrode active material 56, the average particle diameter of the primary particles 56p of the lithium transition metal composite oxide 56a may be, for example, 0.1 μm to 2.5 μm, preferably 1.0 μm or more, more preferably 1.3 μm or more, and even more preferably 1.9 μm or more. On the other hand, from the viewpoint of higher output characteristics and cycle characteristics of the positive electrode active material 56, the average particle diameter of the primary particles 56p of the lithium transition metal composite oxide 56a is preferably 2.2 μm or less, more preferably 2.1 μm or less. Note that the "average particle diameter of the primary particles of the lithium transition metal composite oxide" refers to the average particle diameter of the major axis of the primary particles 56p of the lithium transition metal composite oxide 56a. It can be obtained by determining the major axis of each of a plurality of primary particles 56p arbitrarily selected from an SEM image and calculating the average value by the same method as the aspect ratio of the primary particles described above.
[0030] 3, the primary particles 56p according to this embodiment are typically arranged in the lithium transition metal composite oxide 56a (secondary particle) so as to extend (so as to be radially oriented) from the center C toward the outer diameter OL. One end of the long side of the primary particle 56p is arranged on the outer diameter OL side, and the other end is arranged on the center C side. In other words, the a-axis of the primary particle 56p is arranged so as to extend from the center C toward the outer diameter OL.
[0031] The primary particles 56p and secondary particles according to this embodiment can be produced by a conventionally known method (for example, a crystallization method, etc.). Although not particularly limited, the method for forming the primary particles 56p and secondary particles as described above can be produced by, for example, a conventionally known crystallization method. First, a hydroxide is prepared as a precursor of a lithium transition metal composite oxide in which primary particles are radially oriented. This hydroxide usually contains metal elements other than lithium among the metal elements contained in the lithium transition metal composite oxide. When producing such a hydroxide, a compound containing ammonium ions (for example, ammonia) is used as an alkaline compound. At this time, the aspect ratio (long diameter and short diameter of the primary particles 56p) and the arrangement of the primary particles 56p can be controlled by adjusting the pH, NH3 concentration, and reaction time. The NH3 concentration in the reaction solution is preferably 2 wt% or less, for example, 1 to 2 wt%. The pH of the reaction solution is preferably about 10.5 to 12. The reaction time is preferably about 20 to 40 hours. The obtained hydroxide is then mixed with a lithium source compound (e.g., lithium hydroxide, etc.) and calcined. At this time, the calcination temperature and calcination time during calcination can be adjusted to suitably control the shape of the secondary particles of the lithium transition metal composite oxide 56a. The calcination temperature is not particularly limited, but may be, for example, 700°C to 800°C. The calcination time is not particularly limited, but may be, for example, 10 hours to 20 hours. This makes it possible to obtain secondary particles of the lithium transition metal composite oxide 56a according to this embodiment in which elongated primary particles 56p are radially oriented, as illustrated in FIG. 3.
[0032] As shown in FIG. 3, in some preferred embodiments, a coating portion 56c may be disposed on at least a portion of the surface of the lithium transition metal composite oxide 56a. However, the coating portion 56c is not essential and may be omitted in some embodiments. The coating portion 56c preferably contains a boron compound. By disposing a boron compound as the coating portion 56c on the surface of the lithium transition metal composite oxide 56a, Mn elution from the lithium transition metal composite oxide 56a into the non-aqueous electrolyte 80 can be suppressed, and an increase in resistance during storage can be suppressed. In addition, in the positive electrode active material 56, by providing the coating portion 56c, the bonding force between the primary particles 56p is increased. This can alleviate stress during expansion and contraction and suppress particle cracking of the lithium transition metal composite oxide 56a. From this viewpoint, an increase in resistance during storage can be suitably suppressed. As the boron compound, for example, a boron-containing oxide or an oxide containing boron and lithium is preferable, and a lithium borate salt is particularly preferable. Specific examples of the boron compound include LiBO2, LiB(OH)4, Li3BO3, and B2O3, and LiBO2 is particularly preferred. The proportion of the boron compound as the coating portion 56c may be, for example, 0.5 to 2.0 mol %, and preferably 0.7 to 1.5 mol %, calculated as boron (B) when the total amount of metal elements other than Li in the positive electrode active material is taken as 100 mol %.
[0033] In some preferred embodiments, the coating portion 56c may further contain aluminum oxide (Al2O3) in addition to the boron compound. More specifically, the aluminum oxide has a function of trapping hydrogen fluoride gas (hydrofluoric acid) generated by decomposition of the non-aqueous electrolyte 80. This can suppress the elution of Mn into the non-aqueous electrolyte 80 caused by the reaction between the positive electrode active material 56 (lithium transition metal composite oxide 56a) and hydrogen fluoride gas. Therefore, by disposing the coating portion 56c containing aluminum oxide in addition to the boron compound on the surface, it is possible to more suitably suppress the increase in resistance during storage. The proportion of aluminum oxide as the coating portion 56c may be, for example, 0.1 to 0.5 mol %, and is preferably 0.3 to 0.5 mol %, in terms of aluminum (Al) when the total amount of metal elements other than Li in the lithium transition metal composite oxide 56a is taken as 100 mol %.
[0034] The coating portion 56c is preferably disposed at least on the surface of the secondary particle of the lithium transition metal composite oxide 56a. In this case, the coverage of the positive electrode active material 56 by the coating portion 56c may be 60% or more. The fact that the coating portion 56c is disposed on the surface of the secondary particle and the ratio (coverage) of the portion covered by the coating portion 56c can be confirmed by, for example, XPS (X-ray Photoelectron Spectroscopy) analysis of the positive electrode active material 56.
[0035] When the lithium transition metal composite oxide 56a has voids, the coating portion 56c is preferably present inside the secondary particles in addition to or instead of the surface of the secondary particles. Specifically, the coating portion 56c is preferably present on the surface of the primary particles 56p inside the secondary particles. The amount of the coating portion 56c present inside the secondary particles may be greater or less than the amount of the coating portion 56c present on the surface of the secondary particles. This allows the effect of the technology disclosed herein to be exerted at a higher level. The presence of the coating portion 56c inside the secondary particles can be confirmed by LA-ICP-MS (Laser Ablation Inductively Coupled Plasma Mass Spectrometry) analysis.
[0036] The average particle diameter (D50) of the lithium transition metal composite oxide 56a (secondary particles) is not particularly limited. From the viewpoint of particularly high filling property of the positive electrode active material layer 54 and high volumetric energy density of the lithium ion secondary battery 100, the average particle diameter (D50) of the lithium transition metal composite oxide 56a (secondary particles) is preferably 5 μm to 30 μm, and more preferably 10 μm to 20 μm.
[0037] In this specification, the "average particle diameter (D50) of the lithium transition metal composite oxide (secondary particles)" refers to the median diameter (D50) and means the particle diameter corresponding to a cumulative frequency of 50 volume % from the fine particle side with a small particle diameter in the volume-based particle size distribution based on the laser diffraction / scattering method. Therefore, the average particle diameter (D50) of the lithium transition metal composite oxide (secondary particles) can be determined using a laser diffraction / scattering type particle size distribution measuring device or the like.
[0038] In this embodiment, the lithium transition metal composite oxide 56a may have a so-called solid structure in which the primary particles 56p are simply aggregated to form secondary particles. However, the lithium transition metal composite oxide 56a is not limited to this, and may have voids derived from gaps between the primary particles 56p aggregated inside the secondary particles. The voids may or may not be open. When the voids are open, one void may have two or more openings. The voids are located inside the virtual outer diameter OL of the secondary particles in a cross-sectional view, and are typically spaces surrounded by a plurality of primary particles 56p.
[0039] When the lithium transition metal composite oxide 56a (secondary particles) has voids, the porosity is preferably 2% or more and 10% or less. The porosity of the secondary particles is, for example, 2% or more, and may be 3% or more, or 5% or more. By setting the porosity of the secondary particles to a predetermined value or more, the initial resistance of the lithium ion secondary battery 100 can be reduced. In addition, appropriate voids can be secured inside the secondary particles of the lithium transition metal composite oxide 56a. In addition, when the lithium transition metal composite oxide 56a has the coating portion 56c, the coating portion 56c can be evenly arranged up to the center C of the secondary particles. On the other hand, if the porosity of the secondary particles is excessive (typically, the porosity exceeds 10%), the resistance increase during storage increases. Therefore, the porosity of the secondary particles is, for example, 10% or less, and may be 9% or less, or 8% or less. In this specification, the "average porosity of the lithium transition metal composite oxide" is understood from a cross-sectional electron microscope image of the lithium transition metal composite oxide, and the average value can be calculated by measuring the porosity of a plurality of secondary particles selected at random. The plurality of secondary particles can be, for example, 20 or more. First, a cross-sectional observation sample of the lithium transition metal composite oxide 56a is prepared by cross-section polisher processing or the like. Next, a SEM image of the cross-sectional observation sample is obtained using a scanning electron microscope (SEM). From the obtained SEM image, the area of the entire secondary particles and the total area of all voids inside the secondary particles are calculated using image analysis software (e.g., "ImageJ"). Then, the following formula (ii): Porosity (%) = (total area of all voids / total area of secondary particles) x 100...(ii) The porosity is calculated using the formula below, and the average value is calculated.
[0040] The porosity of the lithium transition metal composite oxide 56a can be adjusted, for example, by changing the synthesis conditions when a hydroxide, which is a precursor of the lithium transition metal composite oxide 56a, is synthesized by a crystallization method. Specifically, in the crystallization method, a raw material aqueous solution containing metal elements other than lithium and a pH adjusting solution are added to a reaction solution to synthesize the hydroxide. The porosity of the hydroxide can be adjusted by changing the pH value of the reaction solution and the stirring speed at this time. The hydroxide is mixed with a lithium source compound (e.g., lithium hydroxide, etc.) and baked to obtain the lithium transition metal composite oxide 56a in the form of secondary particles and with an adjusted porosity.
[0041] The BET specific surface area of the lithium transition metal composite oxide 56a is not particularly limited. Since this can impart excellent output characteristics to the lithium ion secondary battery 100, the BET specific surface area of the lithium transition metal composite oxide 56a is preferably 0.50 m 2 / g~0.85m 2 / g, more preferably 0.55m 2 / g~0.80m 2 The BET specific surface area of the lithium transition metal composite oxide 56a can be measured by a nitrogen adsorption method using a commercially available specific surface area measuring device.
[0042] The content of the positive electrode active material 56 in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material 56 relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is, for example, 80 mass% or more, preferably 87 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and most preferably 97 mass% or more.
[0043] The positive electrode current collector 52 may be a known material used in the lithium ion secondary battery 100, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). Aluminum foil is preferable as the positive electrode current collector 52 according to this embodiment.
[0044] The dimensions of the positive electrode current collector 52 are not particularly limited and can be appropriately determined according to the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness of the positive electrode current collector 52 is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0045] <Negative electrode> The negative electrode (negative electrode sheet 60) disclosed herein includes a negative electrode active material layer 64. As shown in Fig. 2, the negative electrode (negative electrode sheet 60) includes a negative electrode current collector 62 and a negative electrode active material layer 64 supported on the negative electrode current collector 62. Note that, although the negative electrode active material layer 64 is illustrated only on one surface of the negative electrode current collector 62 in this embodiment, the negative electrode active material layer 64 may be provided on both surfaces of the negative electrode current collector 62.
[0046] The negative electrode active material layer 64 contains a negative electrode active material 66 capable of reversibly absorbing and releasing charge carriers. FIG. 4 is a schematic diagram showing the configuration of a negative electrode sheet 60 (negative electrode) according to one embodiment. The negative electrode active material 66 according to this embodiment essentially contains a carbon material 66c and a Si-containing material 66s. However, the negative electrode active material 66 may further contain other negative electrode active materials in addition to the carbon material 66c and the Si-containing material 66s. Although not shown here for convenience of explanation, the negative electrode active material layer 64 may contain a conductive material, a binder, a thickener, and the like in addition to the negative electrode active material 66.
[0047] As the carbon material 66c, for example, graphite, hard carbon, soft carbon, etc. are used, and among them, graphite is preferably used. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.
[0048] The average particle diameter of the carbon material 66c is not particularly limited, but for example, it is 0.1 μm or more and 50 μm or less, preferably 1 μm or more and 25 μm or less, and more preferably 5 μm or more and 20 μm or less. The average particle diameter (D50) of the carbon material can be determined by, for example, the laser diffraction scattering method.
[0049] The Si-containing material 66s is, for example, silicon (Si), SiO x (0.05 < x < 1.95), silicon oxide represented by, a Si-C composite containing Si particles in carbon particles, lithium silicate (Li x Si y O z ) and the like. As the Si-containing material 66s, silicon, silicon oxide, and Si-C composites can be preferably used. In addition, as the Si-containing material 66s, an alloy composed of Si and an element other than Si can be used. Examples of the element other than Si include Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, Ti, and the like. By including the Si-containing material 66s in the negative electrode active material 66, the formation of a coating layer starting from Mn eluted from the positive electrode active material on the surface of the negative electrode active material layer 64 can be suppressed. Therefore, an increase in resistance during storage can be preferably suppressed.
[0050] The average particle diameter of the Si-containing material 66s is not particularly limited, but for example, it is 0.1 μm or more and 50 μm or less, preferably 1 μm or more and 25 μm or less, and more preferably 5 μm or more and 20 μm or less. The average particle diameter (D50) of the carbon material can be determined by, for example, the laser diffraction scattering method.
[0051] In this embodiment, the content of the Si element in the negative electrode active material 66 when the total amount of the negative electrode active material 66 is 100 mass %, is 5 mass % or more and 10 mass % or less, from the viewpoint of both the effect of suppressing the resistance increase during storage and the capacity maintenance rate. If the content of the Si element is low (typically, less than 5 mass %), the effect of suppressing the formation of a coating layer originating from Mn eluted from the positive electrode active material on the surface of the negative electrode active material layer 64 cannot be suitably obtained, and the effect of suppressing the storage resistance cannot be obtained well. On the other hand, if the content of the Si element is too high (typically, more than 10 mass %), the capacity maintenance rate during storage decreases, which is not preferable.
[0052] The distribution of the Si-containing material 66s in the negative electrode active material layer 64 is not particularly limited, and the Si-containing material may be dispersed throughout the entire negative electrode active material layer 64, may be concentrated and dispersed in the upper layer (the surface layer side of the negative electrode active material layer 64) of the negative electrode active material layer 64, or may be concentrated and dispersed in the lower layer (the negative electrode current collector 62 side) of the negative electrode active material layer 64. In some preferred embodiments, the Si-containing material 66s is preferably concentrated and dispersed in the upper layer (corresponding to the negative electrode upper layer 164u in FIG. 5) of the negative electrode active material layer 64, as shown in the second embodiment (FIG. 5) described later. As shown in FIG. 4, in this embodiment, the Si-containing material 66s is dispersed almost uniformly throughout the entire negative electrode active material layer 64. Note that "concentrated and dispersed in the upper layer of the negative electrode active material layer 64" is an example of "the content ratio of the Si element in the negative electrode upper layer is 90 mass% or more when the Si element in the entire negative electrode active material is 100 mass%" disclosed herein.
[0053] The negative electrode active material layer 64 may contain components other than the negative electrode active material 66, such as a conductive material, a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc., which have been used conventionally in lithium secondary batteries, may be used without any particular limitation. As the thickener, for example, carboxymethyl cellulose (CMC) may be used.
[0054] The negative electrode active material layer 64 preferably further contains a conductive material. As the conductive material, for example, carbon black (CB) such as acetylene black (AB) or Ketjen black, carbon nanotubes (CNT), carbon fibers such as vapor grown carbon fiber (VGCF), activated carbon, graphite, and other carbon materials can be suitably used, and among them, it is preferable to contain CNT. By containing CNT as the conductive material, the capacity retention rate can be suitably maintained. As the CNT, any one of single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT) may be used, and these may be used alone or in combination of two or more. When CNT is used as the conductive material of the negative electrode active material layer 64, it is preferable to use SWCNT. When CNT is used as the conductive material of the negative electrode active material layer 64, it is preferable to contain 0.5 mass % or less of CNT with respect to the entire negative electrode active material layer.
[0055] The content of the negative electrode active material 66 in the negative electrode active material layer 64 is preferably 90% by mass or more, and more preferably 95% by mass or more and 99% by mass or less. The content of the binder in the negative electrode active material layer 64 is preferably 0.1% by mass or more and 8% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less. The content of the thickener in the negative electrode active material layer 64 is preferably 0.3% by mass or more and 3% by mass or less, and more preferably 0.5% by mass or more and 2% by mass or less.
[0056] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, 10 μm to 200 μm, and preferably 20 μm to 100 μm, when the negative electrode active material layer 64 is provided only on one surface of the negative electrode current collector 62. When the negative electrode active material layer 64 is provided on both surfaces of the negative electrode current collector 62, the thickness of each surface (each of the thicknesses of one surface and the other surface) is, for example, 10 μm to 200 μm, and preferably 20 μm to 100 μm.
[0057] A known negative electrode current collector used in lithium ion secondary batteries may be used as the negative electrode current collector 62, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.). Copper foil is preferable as the negative electrode current collector 62.
[0058] The dimensions of the negative electrode current collector 62 are not particularly limited and can be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness of the negative electrode current collector 62 is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0059] As the separator 70, various porous sheets similar to those conventionally used in lithium ion secondary batteries can be used, and examples thereof include porous resin sheets made of resins such as polyethylene (PE) and polypropylene (PP). Such porous resin sheets may have a single-layer structure or a multi-layer structure of two or more layers (for example, a three-layer structure in which PP layers are laminated on both sides of a PE layer). The separator 70 may be provided with a heat-resistant layer (HRL).
[0060] The non-aqueous electrolyte 80 can be the same as that used in conventional lithium ion secondary batteries, and typically can be an organic solvent (nonaqueous solvent) containing a supporting salt. As the non-aqueous solvent, aprotic solvents such as carbonates, esters, and ethers can be used. Among them, carbonates are preferred because they have a particularly high effect of reducing low-temperature resistance due to the positive electrode material. Examples of carbonates include ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such non-aqueous solvents can be used alone or in appropriate combination of two or more. As the supporting salt, for example, lithium salts such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI) can be suitably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.
[0061] In addition, the nonaqueous electrolyte 80 may contain various additives such as gas generating agents, film forming agents, dispersants, and thickeners, other than the above-mentioned nonaqueous solvent and supporting salt, as long as the effect of the present disclosure is not significantly impaired. Examples of additives used in the nonaqueous electrolyte 80 include positive and negative electrode film forming agents such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), and 1,3-propane sultone (PS); overcharge inhibitors such as biphenyl (BP), cyclohexylbenzene (CHB), t-butylbenzene, and t-amylbenzene. Among them, the nonaqueous electrolyte 80 preferably contains FEC. When the nonaqueous electrolyte 80 contains FEC as an additive, it is preferable that the nonaqueous electrolyte 80 contains FEC at a ratio of 20 vol% or less.
[0062] The positive electrode active material of the lithium ion secondary battery 100 configured as above includes a lithium transition metal composite oxide that is a high Ni lithium transition metal composite oxide, and the lithium transition metal composite oxide has a primary particle aspect ratio of 1.9 or more. The negative electrode active material of the lithium ion secondary battery 100 includes a carbon material and a Si-containing material, and includes a negative electrode active material in which the content ratio of Si element in the negative electrode active material is 5 mass% or more and 10 mass% or less when the total amount of the negative electrode active material is 100 mass%. This makes it possible to reduce the cobalt content in the positive electrode active material while suppressing an increase in initial resistance and suppress an increase in resistance during storage.
[0063] Specifically, the lithium transition metal composite oxide having a layered structure typically has a layered structure in which a lithium layer, an oxygen layer, a transition metal layer, and an oxygen layer are repeatedly stacked. The lithium transition metal composite oxide absorbs and releases Li ions from the direction (a-axis) perpendicular to the stacking direction (c-axis). When a lithium transition metal composite oxide having a layered structure containing Mn is used as a positive electrode active material, the stability of the lithium transition metal composite oxide decreases when the Co content in the lithium transition metal composite oxide is reduced. Typically, the interlayer space of the lithium transition metal composite oxide becomes narrow, and the conductivity of Li ions decreases, thereby increasing the initial resistance. In addition, the stability of the lithium transition metal composite oxide decreases, and Mn elution from the positive electrode active material layer (specifically, the lithium transition metal composite oxide) becomes significant during storage. For example, Mn eluted from the positive electrode active material layer precipitates on the surface (typically the graphite surface) of the negative electrode active material layer, and further, a coating growth occurs starting from the precipitated Mn. This coating causes durability deterioration of the lithium ion secondary battery. Therefore, conventional lithium-ion secondary batteries that use a lithium transition metal composite oxide with a layered structure containing Mn and with a reduced Co content as a positive electrode active material have had problems such as a deterioration in initial resistance and a large increase in resistance during storage.
[0064] In contrast, in the lithium ion secondary battery 100 according to this embodiment, the content of Ni in the lithium transition metal composite oxide 56a relative to the total of the metal elements other than Li is 75 mol % or more, so that the Mn ratio in the lithium transition metal composite oxide 56a can be suppressed. The primary particles 56p according to this embodiment have an elongated shape with an aspect ratio of 1.9 or more. According to the primary particles 56p having such a configuration, the primary particles 56p are arranged in the lithium transition metal composite oxide 56a so that the major axis extends from the outer diameter OL toward the center C, thereby forming secondary particles. An efficient diffusion path of Li ions from the surface (outer diameter OL side) of the lithium transition metal composite oxide 56a to the center C is formed, and the diffusion path length is reduced. This improves the Li ion diffusibility of the lithium transition metal composite oxide 56a. Therefore, the initial resistance can be reduced. Furthermore, according to the Si-containing material 66s contained in the negative electrode active material 66, the precipitation of Mn on the surface of the negative electrode active material layer 64 is suppressed. This makes it possible to suppress the formation of a Mn coating on the surface of the negative electrode active material layer 64. Therefore, even when the Co content in the lithium transition metal composite oxide is reduced, it is possible to provide a lithium ion secondary battery 100 in which an increase in initial resistance is suppressed and an increase in resistance during storage is suppressed.
[0065] The lithium ion secondary battery 100 can be used for various applications. Suitable applications include a driving power source mounted on vehicles such as an electric vehicle (BEV; Battery Electric Vehicle), a hybrid electric vehicle (HEV; Hybrid Electric Vehicle), and a plug-in hybrid electric vehicle (PHEV; Plug-in Hybrid Electric Vehicle). The lithium ion secondary battery 100 can also be used as a storage battery for a small power storage device or the like. The lithium ion secondary battery 100 can also be used in the form of a battery pack in which a plurality of lithium ion secondary batteries 100 are typically connected in series and / or parallel.
[0066] As an example, a rectangular lithium ion secondary battery 100 including an electrode body 20 having a flat wound structure has been described. However, the lithium ion secondary battery disclosed herein can also be configured as a lithium ion secondary battery including a laminated electrode body (i.e., an electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated). The laminated electrode body may include a plurality of separators such that one separator is interposed between each of the positive electrodes and the negative electrodes, and may be one in which the positive electrodes and the negative electrodes are alternately laminated while one separator is folded. The lithium ion secondary battery according to this embodiment can also be constructed in the form of a cylindrical lithium ion secondary battery, a coin-type lithium ion secondary battery, a laminated lithium ion secondary battery, or the like. Furthermore, an all-solid-state secondary battery using a solid electrolyte as the electrolyte can also be constructed.
[0067] <Second embodiment> Fig. 5 is a view of a negative electrode sheet 160 (negative electrode) according to the second embodiment, corresponding to Fig. 4. In Fig. 5, the negative electrode sheet 160 may be similar to the above-mentioned lithium ion secondary battery 100, except that a negative electrode active material layer 164 is provided instead of the negative electrode active material layer 64. As shown in Fig. 5, the negative electrode active material layer 164 has a so-called multi-layer structure including a negative electrode upper layer 164u and a negative electrode lower layer 164d.
[0068] In some preferred embodiments, the negative electrode active material layer 164 may include a negative electrode lower layer 164d in contact with the negative electrode current collector 62, and a negative electrode upper layer 164u that is farther from the negative electrode current collector 62 than the negative electrode lower layer 164d is, as viewed in the thickness direction. However, the negative electrode active material layer 164 may have a multi-layer structure of three or more layers. For example, a layer having a composition different from those of the negative electrode upper layer 164u and the negative electrode lower layer 164d may be formed between the negative electrode upper layer 164u and the negative electrode lower layer 164d.
[0069] The negative electrode upper layer 164u is a layer located closer to the surface than the negative electrode lower layer 164d when viewed in the thickness direction of the negative electrode active material layer 164. The negative electrode upper layer 164u is located farther from the negative electrode current collector 62 than the negative electrode lower layer 164d. Here, the negative electrode upper layer 164u constitutes the outermost layer of the negative electrode active material layer 164. In other words, the negative electrode upper layer 164u is located closer to the positive electrode (positive electrode sheet 50) than the negative electrode lower layer 164d.
[0070] The negative electrode active material 66 of the negative electrode upper layer 164u essentially contains a Si-containing material 66s. When the amount of Si element in the entire negative electrode active material layer 164 is taken as 100 mass%, the content ratio of the Si element contained in the negative electrode upper layer 164u is preferably 90 mass% or more, more preferably 95 mass% or more, and further preferably 98 mass% or more. Typically, the content of the Si element contained in the negative electrode upper layer 164u is greater than the content of the Si element contained in the negative electrode lower layer 164d. In other words, in the negative electrode active material layer 164, the Si element is concentrated and dispersed on the positive electrode (positive electrode sheet 50) side.
[0071] As described above, Mn dissolved from the positive electrode active material layer 54 (typically, the lithium transition metal composite oxide 56a) precipitates on the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 64, in other words, on the surface layer of the negative electrode active material layer 164, to form a coating. Here, by adopting a configuration in which the Si-containing material is concentrated and dispersed on the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 164, i.e., on the negative electrode upper layer 164u side, the effect of suppressing the formation of a coating by Mn on the surface of the negative electrode active material layer 164 is more efficiently exhibited. Therefore, an increase in resistance during storage can be suitably suppressed.
[0072] In this specification, the "content ratio (mass%) of the Si element contained in the negative electrode upper layer when the amount of Si element in the entire negative electrode active material layer is taken as 100%" can be calculated as follows. First, the thickness of the negative electrode upper layer is obtained by observing a cross-sectional SEM image of the negative electrode active material layer 164. Next, for a predetermined area of the negative electrode active material layer, a sample is collected by scraping off the negative electrode active material layer by the thickness of the obtained negative electrode upper layer, and an ICP (Inductively Coupled Plasma) analysis is performed to calculate the amount of Si element in the negative electrode upper layer. Similarly, for the negative electrode lower layer, a sample is collected by scraping off a predetermined area of the negative electrode active material layer, and the amount of Si element in the negative electrode lower layer is calculated by ICP analysis. Then, the content ratio of the Si element in the negative electrode upper layer to the amount of Si element in the entire negative electrode active material layer can be obtained from the values of the Si element amounts of the negative electrode upper layer and the negative electrode lower layer obtained respectively.
[0073] The content of Si element contained in the negative electrode upper layer 164u is preferably 2 mass % or more, and more preferably 5 mass % or more, when the total amount of the negative electrode active material 66 in the negative electrode upper layer 164u is taken as 100 mass %.
[0074] The negative electrode lower layer 164d is a layer located closer to the negative electrode current collector 62 than the negative electrode upper layer 164u when viewed in the thickness direction of the negative electrode active material layer 64. Here, the negative electrode lower layer 164d is in contact with the negative electrode current collector 62.
[0075] The negative electrode active material 66 of the negative electrode lower layer 164d essentially contains a carbon material 66c. The negative electrode lower layer 164d may contain a Si-containing material 66s, or may not contain a Si-containing material 66s. The content of the Si element contained in the negative electrode lower layer 164d is not particularly limited, but may be, for example, 2% by mass or less, and preferably 1% by mass or less, when the negative electrode active material of the negative electrode lower layer 164d is taken as 100% by mass. The content of the C element contained in the negative electrode lower layer 164d is not particularly limited, but is preferably 98% by mass or more, and more preferably 99% by mass or more, when the negative electrode active material of the negative electrode lower layer 164d is taken as 100% by mass.
[0076] The ratio (Tu / Ta) of the thickness Tu of the negative electrode upper layer 164u to the total thickness Ta of the negative electrode active material layer 164 is, for example, 0.8 or less, and preferably 0.7 or less. This allows the Si-containing material 66s (in other words, Si element) in the negative electrode active material layer 164 to be dispersed on the positive electrode (positive electrode sheet 50) side, and thus the effect of suppressing the formation of a coating by Mn is more efficiently exhibited. Therefore, the increase in resistance during storage can be suitably suppressed. In addition, from the viewpoint of packing property, the ratio of the thickness Tu of the negative electrode upper layer 164u to the total thickness Ta of the negative electrode active material layer 164 is, for example, 0.4 or more, and preferably 0.5 or more. Note that the "ratio of the thickness of the negative electrode upper layer to the total thickness of the negative electrode active material layer" in the specification is measured in a cross-sectional SEM image of the negative electrode active material layer 164.
[0077] The above-mentioned negative electrode upper layer 164u and negative electrode lower layer 164d can be produced by a conventionally known method. For example, but not limited to, the negative electrode upper layer 164u and negative electrode lower layer 164d can be formed by preparing a negative electrode active material layer forming slurry using two or more types of negative electrode active materials 66 having different compositions (typically, the content ratio of the Si-containing material) and applying the negative electrode active material layer forming slurry.
[0078] Hereinafter, examples of the technology disclosed herein will be described, but it is not intended that the technology disclosed herein be limited to those shown in these examples.
[0079] <Test Example 1: Examination of the structure of the positive electrode active material and the presence or absence of Si in the negative electrode active material> (Example 1) [Preparation of positive electrode sheet] First, the positive electrode active material according to Example 1 was prepared. Specifically, a hydroxide precursor was produced by a crystallization method. In this case, a compound containing ammonium ions was used as an alkaline compound, and the hydroxide was produced by setting the pH of the reaction solution to 11, the NH3 concentration to 1.0 to 1.5 wt%, and the reaction time to 40 hours. Then, when the obtained hydroxide was mixed with a lithium source and fired, the firing temperature was set to 770°C and the firing time was set to 15 hours. As a result, a lithium transition metal composite oxide (Li1Ni 0.83 Mn 0.17 O2) (corresponding to 83 / 0 / 17 in the "Ni / Co / Mn" column in Table 1). The aspect ratio of the primary particles was measured by the method described above.
[0080] The positive electrode active material prepared above, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in a solid mass ratio of positive electrode active material:AB:PVDF=100:1:1. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to the obtained mixture and kneaded to prepare a slurry for forming a positive electrode active material layer. The obtained slurry for forming a positive electrode active material layer was applied to both sides of a positive electrode current collector made of aluminum foil with a thickness of 15 μm and dried to form a positive electrode active material layer. The obtained positive electrode active material layer was roll-pressed using a rolling roller, and then cut to a predetermined size to prepare a positive electrode sheet according to Example 1.
[0081] [Preparation of negative electrode sheet] First, graphite as a carbon material and a Si-C composite as a Si-containing material were mixed so that the content ratio of Si element was 10 mass% and the content ratio of C element was 90 mass% when the total amount of the negative electrode active material was 100 mass%, to prepare the negative electrode active material of Example 1.
[0082] The negative electrode active material prepared above, styrene butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and single-walled carbon nanotubes (SWCNT) as a conductive material were mixed in ion-exchanged water at a solid content mass ratio of negative electrode active material:SBR:CMC:SWCNT=100:1:1:0.5 to prepare a slurry for forming a negative electrode active material layer. The obtained slurry for forming a negative electrode active material layer was applied onto a negative electrode current collector made of copper foil with a thickness of 10 μm and dried to form a negative electrode active material layer. The obtained negative electrode active material layer was roll-pressed using a rolling roller and then cut to a predetermined size. As a result, a negative electrode sheet according to Example 1 in which the Si-containing material was almost uniformly dispersed throughout the entire negative electrode active material was produced.
[0083] [Preparing the separator] As a separator, a porous polyolefin sheet having a thickness of 20 μm and a three-layer structure of PP / PE / PE was prepared.
[0084] [Preparation of non-aqueous electrolyte] A non-aqueous electrolyte was prepared by dissolving LiPF6 as a supporting electrolyte at a concentration of 1 mol / L in a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC) in a volume ratio of EC:EMC:DMC:FEC=25:40:30:5.
[0085] [Preparation of lithium-ion secondary batteries for evaluation] The positive electrode sheet and the negative electrode sheet were stacked with a separator interposed therebetween to obtain a laminate. The laminate was then wound to obtain a wound body, which was then pressed to obtain a flattened electrode body. A current collector terminal was attached to the electrode body, which was then inserted into a battery case and welded, after which a non-aqueous electrolyte was poured in. The battery case was then sealed to produce a lithium ion secondary battery for evaluation.
[0086] [Initial charging process] The obtained lithium ion secondary battery for evaluation according to Example 1 was subjected to a constant current charge at a current value of 0.1 C to a voltage of 4.2 V as an initial charge process in a temperature environment of 25° C., and then constant voltage charge was performed until the current value became 1 / 20 C. Thereafter, the battery was discharged at a constant current value of 0.1 C to 3.0 V.
[0087] (Example 2) Li1Ni 0.83 Mn 0.17 A lithium-ion secondary battery for evaluation according to Example 2 was produced in the same manner as in Example 1, except that a lithium transition metal composite oxide in which W (tungsten) was doped at 0.3 mol % as an additive element in O2 was used, and an initial charging process was performed.
[0088] (Example 3) A lithium ion secondary battery for evaluation according to Example 3 was produced and subjected to an initial charging process in the same manner as in Example 1, except that the aspect ratio of the primary particles of the lithium transition metal composite oxide was 1.5. The aspect ratio of the primary particles was adjusted by controlling the pH of the reaction solution during the production of the precursor, the NH3 concentration, and the reaction time.
[0089] (Example 4) A lithium ion secondary battery for evaluation according to Example 4 was produced in the same manner as in Example 1, except that the negative electrode active material was graphite alone (that is, no Si-containing material was included), and an initial charging process was performed.
[0090] (Example 5) A lithium ion secondary battery for evaluation according to Example 5 was produced in the same manner as in Example 1, except that the aspect ratio of the primary particles of the lithium transition metal composite oxide was 1.5 and the negative electrode active material was graphite alone (i.e., no Si-containing material was included), and an initial charging process was performed.
[0091] [Evaluation of initial resistance] First, the lithium ion secondary batteries for evaluation according to Examples 1 to 5 were charged at a constant current and constant voltage (CCCV) at a current value of 0.3 C in a thermostatic chamber at 25° C., and the SOC (State of Charge) was adjusted to 50%. Then, pulse discharge was performed at a current value of 5 C for 10 seconds. The voltage change (ΔV) during the pulse discharge was obtained and calculated using the following formula (I): Resistance value = voltage change (ΔV) / current value (5C)…(I) The resistance value before storage (initial resistance value) was calculated using the above formula. The results are shown in Table 1.
[0092] [Evaluation of storage resistance increase rate] After measuring the initial resistance, the evaluation lithium ion secondary batteries according to Examples 1 to 5 were adjusted to SOC 100% in a temperature environment of 25°C. Each evaluation lithium ion secondary battery was placed in a thermostatic chamber at 60°C and stored for 14 days. The resistance after storage was calculated in the same manner as for the initial resistance. Then, the resistance was calculated using the following formula (II): Resistance increase rate (%) = (resistance value after storage / resistance value before storage) x 100...(II) The resistance increase rate (%) was calculated from the above data, and the results are shown in Table 1.
[0093] [Capacity maintenance rate] In parallel with the evaluation of the storage resistance increase rate, the capacity retention rate was evaluated. Specifically, the discharge capacity measured during the resistance increase rate evaluation for the evaluation lithium ion secondary batteries according to Examples 1 to 5 was taken as the initial capacity. Thereafter, the discharge capacity of the evaluation lithium ion secondary batteries stored in the above-mentioned storage resistance increase rate evaluation (i.e., after storage at 60°C for 14 days) was determined in the same manner as the initial capacity. Then, the following formula (III): Capacity retention rate (%) = discharge capacity after 14 days storage / initial capacity × 100…(III) The capacity retention rate (%) for each example was calculated using the following formula: The results are shown in Table 1.
[0094] [Table 1]
[0095] From the results of Examples 1 and 5, in Example 1, in which the aspect ratio of the primary particles of the lithium transition metal composite oxide was 1.9 and the negative electrode active material containing the carbon material and the Si-containing material was used, both the reduction in initial resistance and the increase in resistance during storage were favorably observed compared to Example 5. On the other hand, in Example 3, in which the aspect ratio of the primary particles of the lithium transition metal composite oxide was 1.5 and the positive electrode active material was used, the reduction in initial resistance was not observed compared to Example 1. From this, it is considered that the effect of reducing the initial resistance can be obtained by using a lithium transition metal composite oxide whose primary particles have an aspect ratio of 1.9 or more. Furthermore, in Example 4, in which the negative electrode active material was only graphite (i.e., did not contain a Si-containing material), the reduction in the rate of increase in resistance during storage was not observed compared to Example 1. It was found that the effect of suppressing the increase in resistance during storage can be favorably obtained by satisfying both the aspect ratio of the primary particles of the lithium transition metal composite oxide being 1.9 or more and the use of a negative electrode active material containing a carbon material and a Si-containing material.
[0096] Furthermore, in Example 2, in which the lithium transition metal composite oxide was doped with W as an additive element in addition to the configuration of Example 1, even better results were obtained in terms of the initial resistance and suppression of resistance increase during storage. This is believed to be because the layered structure of the lithium transition metal composite oxide was stabilized by doping with W, which further improved the conductivity of Li ions and suppressed the dissolution of Mn into the non-aqueous electrolyte.
[0097] <Test Example 2: Examination of Si ratio> (Examples 6 to 8) Lithium ion secondary batteries for evaluation according to Examples 6 to 8 were produced and subjected to an initial charging process in the same manner as in Example 1, except that the content ratio of Si element when the total amount of the negative electrode active material, that is, graphite as the carbon material and the Si-C composite as the Si-containing material, was taken as 100 mass %, was changed as shown in the "Si content ratio" column in Table 2. The lithium ion secondary batteries for evaluation according to Examples 6 to 8 were evaluated in the same manner as in Test Example 1 by the above-mentioned method. The results are shown in Table 2.
[0098] [Table 2]
[0099] As shown in the results of Table 2, in Example 7 and Example 1, in which the content ratio of the Si element in the negative electrode active material was 5 mass% or 10 mass%, the resistance increase during storage was suitably suppressed, and no decrease in the capacity retention rate was observed. In Example 6, in which the content ratio of the Si element was 2 mass%, the effect of suppressing the resistance increase during storage was not obtained very well. The reason for this is considered to be that in Example 6, the negative electrode did not contain enough Si-containing material to sufficiently suppress the precipitation of Mn on the surface of the negative electrode active material. In addition, the higher the content ratio of the Si element, the better the effect of suppressing the increase in the battery resistance, while in Example 8, in which the content ratio of the Si element was 13 mass%, the capacity retention rate was lower than in other examples. Therefore, from the viewpoint of achieving both the effect of suppressing the resistance increase during storage and the capacity retention rate, the content ratio of the Si element in the negative electrode active material is considered to be in the more suitable range of 5 to 10 mass%.
[0100] <Test Example 3: Study on the aspect ratio of primary particles> (Examples 9-10) Lithium ion secondary batteries for evaluation according to Examples 9 to 10 were produced in the same manner as in Example 1, except that the aspect ratio of the primary particles of the lithium transition metal composite oxide was set as shown in "primary particle aspect ratio" in Table 3, and an initial charging process was performed. The aspect ratio of the primary particles was adjusted by controlling the pH of the reaction solution during the production of the precursor, the NH3 concentration, and the reaction time. The aspect ratio of the primary particles was measured by the method described above. The lithium ion secondary batteries for evaluation according to Examples 9 to 10 were evaluated in the same manner as in Test Example 1 by the method described above. The results are shown in Table 3.
[0101] [Table 3]
[0102] From the results in Table 3, compared to Example 3 in which the aspect ratio of the primary particles of the lithium transition metal composite oxide was 1.5, Examples 1, 9, and 10 in which the aspect ratio of the primary particles was 1.9 or more all showed good results in terms of initial resistance. This is presumably because, by setting the aspect ratio to 1.9 or more, an efficient diffusion path for Li ions was formed in the secondary particle form, and the length of the diffusion path was reduced, thereby improving the Li ion diffusibility of the lithium transition metal composite oxide 56a. Also, from the results of Examples 1, 9, and 10, it was observed that the larger the aspect ratio of the primary particles, the better the initial resistance tended to be.
[0103] <Test Example 4: Examination of Covering Part> (Example 11) The configuration of the lithium transition metal composite oxide was the same as in Example 1, and a positive electrode active material was used in which 1 mol % of LiBO2, calculated as boron, was disposed on the surface of the lithium transition metal composite oxide, relative to 100 mol % of the total amount of metal elements other than Li in the lithium transition metal composite oxide. A lithium ion secondary battery for evaluation according to Example 11 was produced and subjected to an initial charging process in the same manner as in Example 1.
[0104] (Example 12) A lithium ion secondary battery for evaluation according to Example 14 was produced and subjected to an initial charging process in the same manner as in Example 1, except that a positive electrode active material in which Al2O3 was disposed on the surface of a lithium transition metal composite oxide in addition to LiBO2 as a coating portion was used. The ratios of LiBO2 and Al2O3 were, in terms of Li and Al, respectively, and the molar ratio of LiBO2:Al2O3=1:0.5 relative to 100 mol % of the total amount of metal elements other than Li in the lithium transition metal composite oxide.
[0105] The evaluation lithium ion secondary batteries according to Examples 11 and 12 were evaluated in the same manner as in Test Example 1 by the above-mentioned method. The results are shown in Table 4.
[0106] [Table 4]
[0107] As shown in the results of Table 4, in Example 11, in which LiBO2 was arranged on the surface of the lithium transition metal composite oxide as a coating portion, better results were obtained in terms of suppressing the increase in resistance during storage. In addition, in Example 12, in which Al2O3 was contained in addition to LiBO2 as a coating portion, even better results were obtained in terms of suppressing the increase in resistance during storage. The reason for this is that the boron compound, when arranged on the surface of the lithium transition metal composite oxide, serves to suppress the reaction area between the non-aqueous electrolyte and the lithium transition metal composite oxide, thereby suppressing the elution of Mn. In addition, aluminum oxide serves to trap hydrogen fluoride gas generated by the decomposition of the non-aqueous electrolyte. Therefore, it is considered that better results were obtained in Examples 11 and 12 in terms of suppressing the increase in resistance during storage.
[0108] <Test Example 5: Examination of Ni compounding ratio in positive electrode active material> (Examples 13-19) Lithium ion secondary batteries for evaluation according to Examples 13 to 19 were produced in the same manner as in Example 1, except that the composition (molar ratio) of Ni, Co, and Mn in the lithium transition metal composite oxide was changed as shown in the "Ni / Co / Mn" column in Table 5, and an initial charging process was performed. The molar ratio of Li (Li / (Ni+Co+Mn)) to the total of the transition metal elements (Ni+Co+Mn) in the lithium transition metal composite oxides according to Examples 13 to 19 was all 1.0 mol %. The lithium ion secondary batteries for evaluation according to Examples 13 to 19 were evaluated in the same manner as in Test Example 1 by the above-mentioned method. The results are shown in Table 5.
[0109] [Table 5]
[0110] As shown in the results of Table 5, in Example 1 and Examples 13 to 15 in which the Ni content of the lithium transition metal composite oxide is 83 mol%, the resistance suppression effect during storage and the capacity retention rate were stably achieved together, even when the Co content of the lithium transition metal composite oxide was reduced. Similarly, in Examples 16 to 17 in which the Ni content of the lithium transition metal composite oxide is 95 mol%, and Examples 18 to 19 in which the Ni content of the lithium transition metal composite oxide is 75 mol%, both the resistance suppression effect during storage and the capacity retention rate were achieved. In addition, in terms of the Co / Mn ratio of the lithium transition metal composite oxide, Example 15 in which the Co / Mn ratio is 0.42 also achieved both the resistance suppression effect during storage and the capacity retention rate.
[0111] <Test Example 6: Examination of the distribution of Si-containing material in the negative electrode active material layer> (Examples 20-21) A first negative electrode active material layer-forming slurry was prepared in the same manner as in Example 1, except that the negative electrode active material was graphite alone (i.e., the content ratio of Si element was 0 mass% and the content ratio of C element was 100 mass% when the total amount of the negative electrode active material was 100 mass%). Similarly, a second negative electrode active material layer forming slurry was prepared in the same manner as in Example 1, except that the graphite and the Si-C composite were mixed so that the content ratio of Si element was 20 mass% and the content ratio of C element was 80 mass% when the total amount of the negative electrode active material was 100 mass%.
[0112] The first negative electrode active material layer forming slurry was applied onto the negative electrode current collector made of the same copper foil as that used in Example 1, dried, and roll-pressed using a rolling roller to obtain a predetermined density. Next, the second negative electrode active material layer forming slurry was applied onto the dried coating film of the first negative electrode active material layer forming slurry, dried, and roll-pressed using a rolling roller to obtain a predetermined density. At this time, the thickness of the second negative electrode active material layer forming slurry was set to 0.5 with respect to the thickness of the entire negative electrode active material layer. As a result, a negative electrode sheet of Example 20 was obtained in which the negative electrode lower layer formed by the first negative electrode active material layer forming slurry and the negative electrode upper layer formed by the second negative electrode active material layer forming slurry were supported on the negative electrode current collector. In addition, in the negative electrode sheet of Example 20, the content ratio of the Si element in the negative electrode upper layer was 99 mass% when the Si element in the entire negative electrode active material was 100 mass%. Similarly, the second negative electrode active material layer forming slurry was applied onto the same copper foil negative electrode current collector as used in Example 1, dried, and roll-pressed using a rolling roller to obtain a predetermined density. Next, the first negative electrode active material layer forming slurry was applied onto the dried coating film of the second negative electrode active material layer forming slurry, dried, and roll-pressed using a rolling roller to obtain a predetermined density. At this time, the thickness of the first negative electrode active material layer forming slurry was set to 0.5 with respect to the thickness of the entire negative electrode active material layer. As a result, a negative electrode sheet of Example 21 was obtained in which a negative electrode lower layer formed by the second negative electrode active material layer forming slurry and a negative electrode upper layer formed by the first negative electrode active material layer forming slurry were supported on a negative electrode current collector. In addition, in the negative electrode sheet of Example 21, the content ratio of the Si element in the negative electrode upper layer was 1 mass% when the Si element in the entire negative electrode active material was 100 mass%.
[0113] Except for using the above-mentioned negative electrode sheet, evaluation batteries according to Examples 20 and 21 were produced in the same manner as in Example 1, and an initial charging process was performed. Evaluations were performed in the same manner as in Test Example 1 for the evaluation lithium ion secondary batteries according to Examples 20 and 21, using the above-mentioned method. The results are shown in Table 6.
[0114] [Table 6]
[0115] As shown in the results of Table 6, in all of Examples 1, 20, and 21, the effect of suppressing the resistance increase during storage was observed compared to Example 4, in which only graphite was used as the negative electrode active material. In Examples 1, 20, and 21, in which the Si blending ratio was 10 mass%, almost no difference was observed in the capacity maintenance rate during storage due to the distribution of the Si-containing material. In addition, when comparing Examples 1, 20, and 21, in Example 1, in which the Si-C composite was uniformly dispersed throughout the negative electrode active material layer, the effect of suppressing the resistance increase rate during storage was good, and in Example 20, in which the Si-containing material was concentrated and arranged in the upper layer, even better results were obtained in suppressing the resistance increase rate during storage. This is thought to be because the effect of suppressing the precipitation of Mn by the Si-containing material was more efficiently expressed on the surface of the negative electrode active material by concentrating and arranging the Si-containing material in the upper layer of the negative electrode active material.
[0116] Although the preferred embodiment of the present disclosure has been described above, the above embodiment is merely an example. The present disclosure can be implemented in various other forms. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. In addition, if the technical feature is not described as essential, it is also possible to delete it as appropriate.
[0117] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, wherein the positive electrode comprises a positive electrode active material layer containing a positive electrode active material, the positive electrode active material comprising a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, the lithium transition metal composite oxide having a Ni content of 75 mol % or more with respect to a total of metal elements other than Li, the lithium transition metal composite oxide being secondary particles formed by aggregation of primary particles, the primary particles having an aspect ratio of 1.9 or more, the negative electrode comprises a negative electrode active material layer containing a negative electrode active material, the negative electrode active material comprising a carbon material and a Si-containing material, and a content ratio of Si element in the negative electrode active material being 5 mass % or more and 10 mass % or less when a total amount of the negative electrode active material is taken as 100 mass %. Item 2: The lithium transition metal composite oxide has the following general formula: Li α Ni x Mn y M z Item 2. The lithium ion secondary battery according to item 1, wherein α is 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, and x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W. Item 3: The lithium ion secondary battery according to item 1 or 2, wherein in the lithium transition metal composite oxide, the content (moles) of Co element and the content (moles) of Mn element satisfy the following relationship: 0≦Co / Mn≦0.42. Item 4: The lithium ion secondary battery according to any one of Items 1 to 3, wherein the lithium transition metal composite oxide contains W. Item 5: The lithium ion secondary battery according to any one of Items 1 to 4, wherein the primary particles have an aspect ratio of 2.5 or less. Item 6: The lithium ion secondary battery according to any one of Items 1 to 5, further comprising a coating portion disposed on at least a part of a surface of the lithium transition metal composite oxide, the coating portion including a boron compound. Item 7: The lithium ion secondary battery according to item 6, wherein the coating portion further contains aluminum oxide. Item 8: The lithium ion secondary battery according to any one of items 1 to 7, wherein the negative electrode further includes a negative electrode current collector, the negative electrode active material layer includes a negative electrode lower layer in contact with the negative electrode current collector, and a negative electrode upper layer further from the negative electrode current collector than the negative electrode lower layer, when viewed in a thickness direction, and a content ratio of Si element in the negative electrode upper layer is 90 mass % or more when Si element in the entire negative electrode active material is taken as 100 mass %. Item 9: The lithium ion secondary battery according to item 8, wherein a ratio of a thickness of the negative electrode upper layer to a total thickness of the negative electrode active material layer is 0.4 or more and 0.8 or less. Item 10: The lithium ion secondary battery according to any one of Items 1 to 9, wherein the Si-containing material includes at least one selected from the group consisting of Si, silicon oxide, and a Si-C composite. [Explanation of symbols]
[0118] 20 Electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 56 Cathode active material 56a Lithium transition metal complex oxide 56c Covering part 56p primary particle 60, 160 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64, 164 Negative electrode active material layer 164u negative electrode upper layer 164d Negative electrode lower layer 66 Negative electrode active material 66c Carbon Materials 66s Si-containing material 70 Separator 80 Non-aqueous electrolytes 100 Lithium-ion secondary battery
Claims
1. A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, The positive electrode includes a positive electrode active material layer containing a positive electrode active material, The positive electrode active material includes a lithium transition metal composite oxide having a layered structure including Li, Ni, and Mn, The lithium transition metal composite oxide is The content of Ni relative to the total of metal elements other than Li is 75 mol% or more, These are secondary particles formed by agglomeration of primary particles, The aspect ratio of the primary particles is 1.9 or more, the negative electrode includes a negative electrode active material layer containing a negative electrode active material, The negative electrode active material includes a carbon material and a Si-containing material, When the total amount of the negative electrode active material is taken as 100 mass%, the content ratio of Si element in the negative electrode active material is 5 mass% or more and 10 mass% or less. Lithium-ion secondary battery.
2. The lithium transition metal composite oxide has the following general formula: Li α Ni x Mn y M z O 2 (wherein 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.) The lithium ion secondary battery according to claim 1 .
3. In the lithium transition metal composite oxide, the content (mol) of Co element and the content (mol) of Mn element have the following relationship: 0≦Co / Mn≦0.42 Fulfilling The lithium ion secondary battery according to claim 1 or 2.
4. The lithium transition metal composite oxide contains W. The lithium ion secondary battery according to claim 1 or 2.
5. The aspect ratio of the primary particles is 2.5 or less. The lithium ion secondary battery according to claim 1 or 2.
6. The lithium transition metal composite oxide further includes a coating portion disposed on at least a portion of a surface of the lithium transition metal composite oxide. The coating portion contains a boron compound. The lithium ion secondary battery according to claim 1 or 2.
7. The coating portion further includes aluminum oxide. The lithium ion secondary battery according to claim 6.
8. The negative electrode further includes a negative electrode current collector, the negative electrode active material layer includes a negative electrode lower layer in contact with the negative electrode current collector and a negative electrode upper layer located farther from the negative electrode current collector than the negative electrode lower layer when viewed in a thickness direction, The content ratio of the Si element in the negative electrode upper layer is 90 mass% or more when the Si element in the entire negative electrode active material is 100 mass%. The lithium ion secondary battery according to claim 1 or 2.
9. a ratio of a thickness of the negative electrode upper layer to a total thickness of the negative electrode active material layer is 0.4 or more and 0.8 or less; The lithium ion secondary battery according to claim 8.
10. The Si-containing material includes at least one selected from the group consisting of Si, silicon oxide, and Si-C composites; The lithium ion secondary battery according to claim 1 or 2.
Citation Information
Patent Citations
Positive electrode active material, method for producing positive electrode active material, positive electrode containing positive electrode active material, and lithium secondary battery
JP2022514966A
Positive electrode active material and method for producing same
JP2024505836A
Lithium secondary battery
US20220416241A1
Secondary battery, battery pack, electric vehicle, power storage system, electric power tool and electronic device
JP2017191662A
Cited By
Positive electrode active material for non-aqueous electrolyte secondary batteries, and non-aqueous electrolyte secondary battery
WO2026140728A1