Method of manufacturing optical member, and optical member
By forming a fine uneven structure on PMMA surfaces through ion irradiation and applying a protective silicon oxide film, the method addresses thermal expansion issues and maintains antireflection efficacy in high-temperature conditions.
Patent Information
- Application Number
- JP2023075695
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2043-05-01
AI Technical Summary
Optical components made of polymethyl methacrylate (PMMA) face issues with crack formation in anti-reflection films due to thermal expansion mismatch and increased surface reflection when multiple lenses are used, particularly in high-temperature environments such as automotive lighting systems.
A method involving ion irradiation to form a fine uneven structure on the PMMA surface, followed by depositing a protective film with a lower refractive index material like silicon oxide to maintain the structure's integrity and reduce reflection.
The method ensures high antireflection effectiveness and maintains spectral properties even in high-temperature environments, preventing film collapse and ensuring consistent performance.
Smart Images

Figure 2024160561000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing optical components, which can be applied, for example, to a method for manufacturing optical components with high anti-reflection effect in a high-temperature environment by forming a protective film on a fine uneven structure formed on the surface of a plastic (synthetic resin) substrate. [Background technology]
[0002] Plastics with excellent light transmission are lightweight, have excellent mechanical strength, are easy to process, and can be designed freely, so they are used as an alternative material to glass. Plastics are particularly used in the optical field, and in recent years, plastics have been used in a wide range of parts such as automobile headlights.
[0003] Transparent plastics that are widely used today include thermoplastic polyvinyl chloride (PVC), polystyrene (PS), polycarbonate (PC), polymethyl methacrylate (PMMA), and thermosetting polyethylene glycol bisallyl carbonate (CR39).
[0004] Among these plastics, PMMA excels in transparency, light weight, ease of processing, and impact resistance as an optical component, and in particular, its light transmittance is the best compared to other resins. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-15826 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when forming an anti-reflection film for suppressing surface reflection on the surface of a PMMA base material in order to improve the transmittance of optical components that use polymethyl methacrylate resin (PMMA), the following problems arise.
[0007] For example, in the optical field, such as in consumer device projectors, a reliability condition of around 70°C is required, so an anti-reflective film can be formed on the surface of a PMMA substrate by vacuum deposition. On the other hand, in the lighting systems in the automotive field, a reliability condition is that they must be able to withstand high temperatures of 90-100°C (hereinafter, high temperature environments refer to environments of around 90-100°C), so there is an issue that the difference between the linear expansion coefficient of the substrate and that of the anti-reflective film can cause cracks in the formed anti-reflective film.
[0008] In addition, while automobile headlights initially used a single lens, there is now a demand for more precise headlights using multiple lenses. When multiple lenses are used, aberration correction is required, which increases the number of lenses, and this also creates the problem of increased surface reflection.
[0009] In view of the above-mentioned problems, the present disclosure aims to provide a method for manufacturing an optical component having high anti-reflection effect in a high-temperature environment by forming a protective film on a fine uneven structure formed on the surface of a substrate made of a synthetic resin such as polymethyl methacrylate resin, with the aim of having heat resistance in the desired high-temperature environment and preventing loss of light. [Means for solving the problem]
[0010] In order to solve such problems, the manufacturing method for optical components according to the present disclosure is characterized by comprising: (1) a fine concave-convex structure forming process in which a surface of a substrate is changed by ion irradiation to form a fine concave-convex structure on the surface of the substrate; and (2) a protective film forming process in which a deposition material is evaporated and deposited on the surface of the substrate to form a protective film on the fine concave-convex structure formed on the surface of the substrate. Effect of the Invention
[0011] According to the present disclosure, a protective film can be formed on a fine uneven structure formed on the surface of a synthetic resin substrate, making it possible to manufacture optical components that have a high anti-reflection effect even in high-temperature environments. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing the conditions for forming a fine uneven structure in step A and the spectral characteristics of a substrate having a fine uneven structure. [Diagram 2] FIG. 13 is a diagram showing the conditions for forming a fine uneven structure in step C and the spectral characteristics of a substrate having a fine uneven structure. [Diagram 3] FIG. 2 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 1. [Figure 4] FIG. 13 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the process of Example 2. [Diagram 5] FIG. 13 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 3. [Figure 6] FIG. 13 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 4. [Figure 7] FIG. 13 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 5. [Figure 8] The results show the spectral characteristics of a substrate having a fine uneven structure formed in process A before a high-temperature test and the spectral characteristics of the substrate in a high-temperature environment. [Figure 9] 1 shows the results of the spectral characteristics before a high-temperature test and the spectral characteristics under a high-temperature environment using the substrate of Example 1. [Figure 10] 13 shows the results of the spectral characteristics before a high-temperature test and the spectral characteristics under a high-temperature environment using the substrate of Example 3. [Figure 11] 1 shows the results of a comparison of the antireflection effect between Example 1 and other antireflection coatings. [Figure 12] FIG. 1 is a diagram showing the spectral characteristics of Example 1 and other antireflection coatings. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (A) Embodiment Hereinafter, an embodiment of the optical thin film manufacturing method of the present disclosure will be described in detail with reference to the drawings.
[0014] (A-1) Overview In recent years, there has been an increasing demand for plastic optical components as an alternative to glass-based optical components. For example, a method for preventing surface reflection on an optical lens by forming a fine uneven structure on the surface of a substrate is known.
[0015] One such fine uneven structure is called a moth-eye structure (so-called because it imitates the minute protrusions on the surface of a moth's eye). In the present disclosure, the moth-eye structure is exemplified as an example of a fine uneven structure, but the present disclosure is not limited to the moth-eye structure.
[0016] Conventionally, as a method for forming a moth-eye structure on the surface of a plastic substrate, for example, there is a method for forming a fine uneven structure by injection molding using a mold.
[0017] However, with this method, there is a risk that the resin will stick to the mold when the molded product is removed from the mold, destroying the fine uneven structure, making it difficult to adopt this method as a product production method.
[0018] Another method is to use ion sputtering. Ion sputtering is a phenomenon that occurs due to ion irradiation, and there is a method in which the surface of a PMMA substrate is irradiated with ions to modify the surface and change the surface shape. Conventionally, for example, a plasma gun is installed in a vacuum deposition device, and ions are irradiated during film formation to activate evaporated molecules and improve film strength.
[0019] The inventors of the present application confirmed that a moth-eye shape (a shape having a fine uneven structure) is formed on the surface of a PMMA substrate by irradiating the PMMA substrate with ions without forming (laminating) a multilayer film on the substrate surface, and confirmed the anti-reflection effect and spectroscopic characteristics of a PMMA substrate having a moth-eye shape.
[0020] PMMA has a chain structure, and the CO portion of C-OOCH3 is broken by plasma, forming a moth-eye shape. In fact, using this method as a reference, a moth-eye shape could be formed on the substrate surface using a plasma gun and changing conditions such as adjusting the argon gas flow rate, oxygen flow rate, and ion irradiation power. Moth-eyes could also be formed using another method, a CVD (chemical vapor deposition) device, by plasma discharge adjusting the argon gas flow rate, oxygen flow rate, and high-frequency power. The formation of a fine uneven structure on the substrate surface confirmed the anti-reflection effect or the spectral characteristic effect of enhancing transparency.
[0021] However, when testing was performed in the high-temperature environments required for the automotive industry, the spectral characteristics changed and the lens reverted to its original surface reflection, making it impossible to achieve the intended purpose. This is believed to be because the moth-eye shape, which is a fine uneven structure, collapses in the high-temperature environment.
[0022] Therefore, after extensive research, the inventors of the present application have proposed forming a thin protective film that does not generate stress in the film (protective film) on the fine uneven structure (e.g., moth-eye shape) on the surface of a synthetic resin substrate, rather than depositing (laminating) a conventional multilayer anti-reflection film on a substrate.
[0023] As a result, it was possible to maintain the fine uneven structure shape even in a high-temperature environment, improve the heat resistance of the optical components, and confirm the surface anti-reflection function and spectral characteristics.
[0024] The protective film maintains its fine uneven structure and has improved heat resistance. The material for the protective film is preferably silicon oxide, which has a lower refractive index than the synthetic resin of the base material. Since a high refractive index increases reflection due to optical interference, a material with an intermediate refractive index is preferable. For example, a material with a refractive index of 1.6 or less is preferable, and 1.65 or less is even more preferable. The optical thickness of the protective film when irradiated with light having a wavelength of 550 nm is preferably λ / 50 to λ / 16.
[0025] The protective film functions as an anti-reflection film that suppresses reflection on the substrate surface, and in addition has a spectral characteristic that separates the wavelengths of light. Furthermore, the protective film functions as a film that maintains the shape of the fine uneven structure even in a high-temperature environment. In the present disclosure, the protective film is exemplified as a silicon oxide (SiO2) film or a silicon oxide mixed (SiOx) film, but is not limited thereto.
[0026] (A-2) Optical thin film manufacturing method The optical thin film manufacturing method according to this embodiment will be described below.
[0027] In the optical thin film manufacturing method according to this embodiment, a fine uneven structure is formed on the surface of a substrate by ion irradiation, and a protective film is formed on the fine uneven structure on the substrate surface.
[0028] (1) Base material The substrate is a plastic substrate (transparent substrate) made of a highly transparent plastic (synthetic resin). The transparent substrate plastic is a chain-bonded polymethyl methacrylate resin (PMMA) with excellent transparency.
[0029] This disclosure utilizes the property of PMMA that the surface of the substrate is changed by ion irradiation to form a moth-eye shape on the substrate surface. Therefore, the present disclosure is not limited to PMMA, and other synthetic resins can be widely used as long as they have a fine uneven structure formed on the surface by ion irradiation.
[0030] In addition, polycarbonate (PC) containing a benzene ring and cycloolefin polymer (COP: Cyclo Olefin Polymer), a cyclic compound, do not form a fine uneven structure on the substrate surface when irradiated with ions, making it difficult to use these as substrates.
[0031] (2) Material (evaporation material) It is preferable that the material has a lower refractive index than the plastic (synthetic resin) used in the base material. If the base material synthetic resin has a high refractive index, there is a risk that light interference will increase reflection.
[0032] In this embodiment, the material (evaporation material) is silicon oxide. Note that the material (evaporation material) is not limited to silicon oxide, and may be, for example, aluminum oxide, titanium oxide, tantalum oxide, zirconium oxide, or the like.
[0033] (3) Formation method Generally, there are two methods for forming a protective film on the surface of a substrate: (a) depositing the silicon oxide material directly, and (b) forming a Si+SiO2+SiO composite film material (hereinafter referred to as "SiOx") by plasma discharge (polymerization) of hexamethyldisiloxane (HMDS).
[0034] (3-1) Pre-process First, when forming a fine uneven structure on a substrate, there may be stains such as burns, fingerprints, oil, etc. on the surface of the substrate, so pure and neutral detergents are added to an ultrasonic cleaner, the substrate is placed in it, and ultrasonic cleaning is performed. In addition, since PMMA has a high water absorption rate, it is also desirable to pre-dry the substrate.
[0035] (3-2) Place the substrate in a vacuum device. After the above-mentioned pre-processing is completed, the substrate is placed in a vacuum device. The exhaust system of the vacuum device is not particularly limited, and for example, a vacuum pump such as a diffusion pump or a turbo molecular pump can be used.
[0036] The apparatus used in the optical thin film formation method is, for example, a vacuum deposition apparatus equipped with a plasma gun, a chemical vapor deposition apparatus, or both.
[0037] When using a vacuum deposition device equipped with a plasma gun, two steps can be considered: "Process A" for forming a fine uneven structure on the substrate surface, and "Process B" for forming a protective film on the fine uneven structure on the substrate surface.
[0038] Similarly, when a chemical vapor deposition apparatus is used, a "step C" of forming a moth-eye shape on the surface of the substrate and a "step D" of forming a protective film on the moth-eye shape on the surface of the substrate can be considered.
[0039] In the following examples (Examples 1 to 5), any effective steps among "Step A" to "Step D" can be combined.
[0040] Although details will be described later, depending on the combination of steps, there is a method in which the "moth-eye shape" and the "protective film" are formed using both a vacuum deposition apparatus and a chemical vapor deposition apparatus, and there is also a method in which the "moth-eye shape" and the "protective film" are formed using either a vacuum deposition apparatus or a chemical vapor deposition apparatus.
[0041] In other words, the former method (that is, the method using two devices) can be said to be a method for forming a "moth-eye shape" and a "protective film" in two stages.
[0042] Conversely, the latter method (i.e., the method using one device) can be said to be a method of forming the "moth-eye shape" and the "protective film" in one step. In other words, since the process can be carried out continuously using one device, it is expected to improve the productivity of optical components and make manufacturing more efficient.
[0043] (3-3) Vacuum deposition equipment equipped with a plasma gun A vacuum deposition apparatus equipped with a plasma gun generally comprises a vacuum chamber, a substrate setting section (rack) for setting the substrate within the vacuum chamber, a deposition source provided with a crucible for setting the deposition material, an electron gun, a plasma gun, a heater for heating the substrate, and a vacuum pump as an exhaust system.
[0044] [Process A] The substrate is placed on a rack with its surface facing the deposition source, and the deposition material is placed in a crucible. Next, the vacuum chamber is depressurized with a vacuum pump, and the substrate is heated by a heater as necessary. The material (deposition material) that has evaporated and sublimated in the vacuum chamber is then irradiated with ions using a plasma gun, changing the shape of the substrate surface and forming a fine uneven structure on the substrate surface. In other words, a moth-eye shape is formed on the substrate surface. This process is called "Process A." According to Process A, the substance is activated by ion irradiation, improving the film strength.
[0045] It should be noted that evaporation and sublimation of the deposition material are not essential, and in the following Examples 1 to 5 given as examples of this embodiment, cases in which evaporation and sublimation of the deposition material were not carried out are illustrated.
[0046] [Process B] The substrate is placed on a rack so that its surface faces the deposition source, and the deposition material is placed in a crucible. Next, the vacuum chamber is depressurized with a vacuum pump, and the substrate is heated by a heater as necessary. Up to this point, part of the process overlaps with process A.
[0047] Then, in the vacuum chamber, the deposition material is dissolved and evaporated by an electron gun, and the evaporated deposition material is deposited on the surface of the substrate to form a protective film on the surface of the substrate. This process is called "Process B".
[0048] (3-4)Chemical vapor deposition equipment (CVD) A chemical vapor deposition apparatus generally comprises a reaction chamber, a substrate mounting section for mounting a substrate within the reaction chamber, a high-frequency power source, a material supply section for supplying gasified material to the reaction chamber by generating plasma discharge using high-frequency waves, a supply section for supplying a gas (carrier gas) to the reaction chamber, and a vacuum pump as an exhaust system for evacuating the inside of the reaction chamber.
[0049] [Process C] The substrate is placed in the substrate placement section, and the material is placed in the material supply section. The reaction chamber is then evacuated by the vacuum pump, and the gas is supplied by the supply section so that the gas flows from the supply section to the vacuum pump in the reaction chamber. Then, plasma is generated at high frequency (e.g., 36.56 MHz), and the material supply section supplies the evaporated material into the reaction chamber, forming a fine uneven structure on the substrate surface. This process is called "Process C."
[0050] Here, the type of gas supplied by the supply unit into the reaction chamber may be argon gas, oxygen gas, nitrogen gas, or the like.
[0051] [Process D] The substrate is placed in the substrate placement section, and the material is placed in the material supply section. Next, the reaction chamber is evacuated by the vacuum pump, and the gas is supplied by the supply section so that the gas flows from the supply section to the vacuum pump in the reaction chamber. Up to this point, there is a part of the same process as in process C.
[0052] Then, in the material supply unit, plasma discharge is generated by high frequency to gasify organic silicon such as hexamethyldisiloxane (HMDS), tetraethoxysilane (TEOS), and triethoxysilane (TRIES), and the gasified material is polymerized by high frequency to form SiOx. The material supply unit then supplies SiOx into the reaction chamber to form a protective film on the surface of the substrate. This process is called "Process D."
[0053] (3-5) Conditions for forming a fine uneven structure on the substrate surface The conditions for forming the fine uneven structure shape on the surface of the substrate in "Step A" and "Step C" will be described with reference to Figs. 1 and 2.
[0054] FIG. 1(A) shows the conditions for forming a fine uneven structure by step A, and FIG. 1(B) shows the results of confirming the transmission characteristics of a substrate having a fine uneven structure under each condition.
[0055] In FIG. 1(B), the horizontal axis indicates wavelength [nm] and the vertical axis indicates transmittance [%]. The transmittance of each wavelength was confirmed by transmitting light through the substrate while changing the wavelength (λ) from 400 nm to 750 nm.
[0056] 1(B), the results for condition number 102 were good, maintaining a transmittance of about 95% to 97% at each wavelength from 400 nm to 750 nm. Therefore, in the following examples and comparative examples, when a fine uneven structure is formed on the surface of a substrate in step A, it is formed under the condition of condition number 102.
[0057] FIG. 2(A) shows the conditions for forming a fine uneven structure by step C, and FIG. 1(B) shows the results of confirming the transmission characteristics of a substrate having a fine uneven structure under each condition.
[0058] 2B, it can be seen that the result of condition number 111 maintains high transmittance at each wavelength from 400 nm to 750 nm, and in particular maintains transmittance of about 90% to 97% for light with wavelengths of 470 nm to 750 nm. Therefore, in the following examples and comparative examples, a fine uneven structure is formed on the surface of a substrate under the condition of condition number 111.
[0059] (A-3) Description of the Examples (A-3-1) Example 1 (Process A + Process B) 3 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the steps of Example 1. Example 1 is a combination of Steps A and B.
[0060] In process A, the substrate is placed on the rack of the vacuum deposition equipment, and the air pressure in the vacuum chamber is reduced to 5×10 by using a vacuum pump. -3 Ion irradiation was performed after evacuating to (5E-3) Pa. The vacuum deposition apparatus used was a dome type with an apparatus diameter (diameter of the vacuum chamber) of 1600φ.
[0061] In process B, the vacuum deposition apparatus of process A was used. In other words, the vacuum chamber was not opened, and SiO2 as a material was evaporated by an electron gun to form a SiO2 film on the surface of the substrate.
[0062] In Example 1, the optical thickness of the SiO2 film formed on the surface of the substrate was changed, and the transmission characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0063] The SiO2 film conditions were such that the optical film thicknesses were λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, and λ / 2 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These six substrates and one without a SiO2 film (uncoated) were used as samples.
[0064] The results in FIG. 3 show that at each wavelength from 400 nm to 750 nm, all of the substrates with optical film thicknesses of λ / 32 to λ / 2 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, λ / 2) had a transmittance of approximately 90% or more, and all of the substrates maintained high transmittance.
[0065] In FIG. 3, among the six substrates, each of the substrates from λ / 32 to λ / 3 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3) maintains a transmittance of approximately 92% or more for light with wavelengths of 470 nm to 750 nm, demonstrating good anti-reflection effects, and furthermore, each of the substrates from λ / 32 to λ / 4 (λ / 32, λ / 16, λ / 8, λ / 4) maintains a transmittance of approximately 95% to 99%, demonstrating high anti-reflection effects.
[0066] Moreover, it can be seen that among the six base materials, the λ / 3 and λ / 2 base materials tend to have higher transmittance as the wavelength value increases.
[0067] Furthermore, among the six base materials, the base materials with wavelengths from λ / 32 to λ / 3 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3) all have high transmittance for light with wavelengths from 470 nm to 750 nm, but tend to have high transmittance for wavelengths shorter than 550 nm.
[0068] (A-3-2) Example 2 (Process A + Process D) 4 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the steps of Example 2. Example 2 is a combination of Steps A and D.
[0069] In process A, the substrate is placed on the rack of a vacuum deposition device (dome-shaped 1600φ) and the air pressure in the vacuum chamber is reduced to 5×10 -3 The chamber was evacuated to (5E-3) Pa and ion irradiation was performed.
[0070] In process D, the substrate was reinstalled in the substrate installation section of the chemical vapor deposition apparatus, the pressure in the reaction chamber was evacuated to 0.2 Pa, and a SiOx film was formed on the substrate surface by polymerizing hexamethyldisiloxane (HMDS) through plasma discharge. In order to move to process D, the vacuum chamber of the vacuum deposition apparatus was opened to remove the substrate, and the substrate was then reset in the chemical vapor deposition apparatus.
[0071] In Example 2, the optical thickness of the SiOx film formed on the surface of the substrate was changed, and the transmission characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0072] The SiOx film conditions were set so that the optical film thickness was λ / 32, λ / 16, λ / 8, and λ / 4 when the wavelength λ of the light irradiated to the substrate was 550 nm. These four substrates and one without SiO2 film (uncoated) were used as samples.
[0073] The results in FIG. 4 show that at each wavelength from 400 nm to 750 nm, the substrates with optical film thicknesses of λ / 32 to λ / 4 (λ / 32, λ / 16, λ / 8, λ / 4) all had a transmittance of approximately 92% or more, and all substrates maintained high transmittance.
[0074] Furthermore, among the four substrates, the λ / 32 to λ / 8 (λ / 32, λ / 16, λ / 8) substrates maintain a transmittance of approximately 94% to 97% for light with wavelengths of 470 nm to 750 nm, and the λ / 32 and λ / 16 substrates maintain a transmittance of approximately 95% or more for light with wavelengths of 470 nm to 750 nm, demonstrating a high anti-reflection effect.
[0075] Furthermore, among the four base materials, the λ / 32 and λ / 16 base materials each have high transmittance for light with wavelengths of 470 nm to 750 nm, but tend to have high transmittance for wavelengths shorter than 550 nm.
[0076] (A-3-3) Example 3 (Step C + Step D) 5 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the steps of Example 3. Example 3 is a combination of Steps C and D.
[0077] In step C, a substrate was placed on the substrate placement section of the chemical vapor deposition apparatus, the pressure in the reaction chamber was evacuated to 0.2 Pa, and plasma discharge was performed.
[0078] In process D, the chemical vapor deposition apparatus of process C was used as it was, and the reaction chamber was not opened, and a SiOx film was formed on the surface of the substrate by polymerizing hexamethyldisiloxane (HMDS) through plasma discharge.
[0079] In Example 3, the optical thickness of the SiOx film formed on the surface of the substrate was changed, and the transmission characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0080] The SiOx film conditions were set so that the optical film thickness was λ / 32, λ / 16, λ / 8, and λ / 4 when the wavelength λ of the light irradiated to the substrate was 550 nm. These four substrates and one without SiO2 film (uncoated) were used as samples.
[0081] The results in FIG. 5 show that, at wavelengths of 480 nm to 750 nm used in the measurements, the substrates with optical film thicknesses of λ / 32 to λ / 4 (λ / 32, λ / 16, λ / 8, λ / 4) all had a transmittance of approximately 90% or more, and all substrates maintained high transmittance.
[0082] Furthermore, among the four base materials, the base materials with wavelengths from λ / 32 to λ / 8 (λ / 32, λ / 16, λ / 8) have a transmittance of approximately 93% or more at wavelengths of approximately 520 nm or more, and are therefore found to have a high anti-reflection effect.
[0083] (A-3-4) Example 4 (Step C + Step B) 6 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the steps of Example 4. Example 4 is a combination of Steps C and B.
[0084] In step C, a substrate was placed on the substrate placement section of the chemical vapor deposition apparatus, the pressure in the reaction chamber was evacuated to 0.2 Pa, and plasma discharge was performed.
[0085] In process B, the substrate is placed on the rack of a vacuum deposition device (dome type, 1600φ) and the air pressure in the vacuum chamber is increased to 2×10 -3 The chamber was evacuated to (2E-3) Pa, and the SiO2 material was evaporated with an electron gun to form a SiO2 film on the surface of the substrate. In order to move to step B, the reaction chamber of the chemical vapor deposition apparatus was opened, the substrate was removed, and the substrate was reset in the vacuum deposition apparatus.
[0086] In Example 4, the optical thickness of the SiO2 film formed on the surface of the substrate was changed, and the transmission characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0087] The SiO2 film conditions were such that the optical film thicknesses were λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, and λ / 2 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These six substrates and one without a SiO2 film (uncoated) were used as samples.
[0088] The results in FIG. 6 show that at wavelengths of approximately 470 nm to 750 nm used in the measurements, the substrates with optical film thicknesses of λ / 32 to λ / 2 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, λ / 2) all had a transmittance of approximately 90% or more, and all substrates maintained high transmittance.
[0089] Furthermore, among the four base materials, the base materials with wavelengths from λ / 32 to λ / 3 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3) have a transmittance of approximately 93% or more at wavelengths of approximately 500 nm or more, and are therefore found to have a high anti-reflection effect.
[0090] (A-3-5) Example 5 (Process A + Process B) FIG. 7 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the process of Example 5.
[0091] Example 5 is a combination of process A and process B, and aluminum oxide was used as the material (evaporation material) of the protective film.
[0092] In process A, the substrate is placed on the rack of the vacuum deposition equipment, and the air pressure in the vacuum chamber is reduced to 5×10 by using a vacuum pump. -3 Ion irradiation was performed after evacuating to (5E-3) Pa. The vacuum deposition apparatus used was a dome type with an apparatus diameter (diameter of the vacuum chamber) of 1600φ.
[0093] In process B, the vacuum deposition apparatus used in process A was used. In other words, the vacuum chamber was not opened, and the Al2O3 material was evaporated by an electron gun to form an Al2O3 film on the surface of the substrate.
[0094] In Example 5, the optical thickness of the Al2O3 on the substrate surface was changed, and the transmission characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0095] The Al2O3 film conditions were such that the optical film thicknesses were λ / 32, λ / 16, and λ / 8 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These six substrates and one without an Al2O3 film (uncoated) were used as samples.
[0096] 7, it can be seen that, among the three substrates, the λ / 32 to λ / 16 (λ / 32, λ / 16) substrates have a transmittance of about 91% or more for light with wavelengths of 400 nm to 750 nm, and maintain a high transmittance. In particular, among the three substrates, the λ / 32 substrate has a transmittance of about 94% or more for light with wavelengths of 400 nm to 750 nm, and maintains a high transmittance.
[0097] (A-3-6) Comparative example 1 (process A) FIG. 8 shows the results of using a substrate on which a fine uneven structure was formed in step A, showing the spectral characteristics of the substrate before a high-temperature test and the spectral characteristics of the substrate in a high-temperature environment.
[0098] In Comparative Example 1, a fine uneven structure was formed on the surface of the substrate in step A, and the transmittance characteristics of the substrate were measured and confirmed in a high-temperature environment.
[0099] In step A, the substrate was placed on a rack in a vacuum deposition apparatus, the pressure in the vacuum chamber was evacuated to 5×10 −3 (5E-3) Pa using a vacuum pump, and ion irradiation was performed.
[0100] In FIG. 8, the dotted line indicates the result of the spectral characteristics of the substrate before the high-temperature test, and the solid line indicates the result of the spectral characteristics of the substrate after the high-temperature test.
[0101] 8, the transmittance of the substrate that underwent the high-temperature test was lower than that of the substrate before the high-temperature test at each wavelength from 400 nm to 750 nm. In other words, it is understood that the transmittance (spectral characteristics) of the fine uneven structure formed on the substrate surface was reduced by being placed in a high-temperature environment.
[0102] (A-3-7) High temperature test results for Example 1 (Process A + Process B) 9 shows the results of the spectral characteristics before the high-temperature test and in a high-temperature environment using the base material of Example 1. Here, a SiO2 film with a thickness of λ / 8 was used.
[0103] 9, it can be seen that in a high-temperature environment, the transmittance of the substrate after the high-temperature test is almost the same as that of the substrate before the high-temperature test at each wavelength of 400 nm to 750 nm. In other words, it can be seen that even in a high-temperature environment, the transmittance (spectral characteristics) does not decrease, and a high anti-reflection effect is achieved.
[0104] Conventionally, when exposed to high temperatures, the fine uneven structure on the surface of the substrate collapses, resulting in a decrease in the anti-reflection effect and spectral characteristics (see Comparative Example 1).
[0105] In contrast, as in Example 1, the antireflection effect and the spectral characteristics can be maintained even at high temperatures by forming a SiO2 film as a protective film on the fine uneven structure on the substrate surface in step B. In other words, even in the intended high-temperature environment, the protective film suppresses the collapse of the fine uneven structure, thereby maintaining the antireflection effect and the spectral characteristics.
[0106] Furthermore, in Example 1, since the steps A and B can be carried out consecutively using the same vacuum deposition apparatus, the efficiency of manufacturing optical components can be improved.
[0107] (A-3-8) High temperature test results of Example 3 (Process C + Process D) 10 shows the results of the spectral characteristics before the high-temperature test and in a high-temperature environment using the base material of Example 3. Here, a SiOx film with a thickness of λ / 16 was used.
[0108] 10, it can be seen that in a high-temperature environment, the transmittance of the substrate after the high-temperature test is almost the same as that of the substrate before the high-temperature test at each wavelength of about 480 nm to 750 nm. In other words, it can be seen that even in a high-temperature environment, the transmittance (spectral characteristics) does not decrease, and a high anti-reflection effect is achieved.
[0109] In the case of Example 3, similarly to the case of (A-3-7), the anti-reflection effect and the spectral characteristics can be maintained even at high temperatures by forming a SiOx film as a protective film on the fine uneven structure on the substrate surface in step D. This is because the protective film suppresses the collapse of the fine uneven structure even in the intended high-temperature environment, thereby maintaining the anti-reflection effect and the spectral characteristics.
[0110] Also in the third embodiment, since the steps C and D can be carried out consecutively using the same chemical vapor deposition apparatus, the efficiency of manufacturing optical components can be improved.
[0111] (A-3-9) Comparison with other anti-reflective coatings Fig. 11 shows the results of comparing the antireflection effect between Example 1 and other antireflection films, and Fig. 12 shows the spectral characteristics between Example 1 and other antireflection films.
[0112] As shown in FIG. 11, two other examples of anti-reflection films are a "four-layer anti-reflection film formed by vacuum deposition" and a "single-layer anti-reflection film formed by vacuum deposition."
[0113] As shown in Fig. 11, the test contents included the spectral characteristics showing the average transmittance from 450 nm to 650 nm, a high temperature test (90°C), and a high temperature test (100°C). The spectral characteristics were based on the results of the spectral characteristics in Fig. 12.
[0114] The four-layer anti-reflection coating, made by vacuum deposition, has an average transmittance of approximately 98% from 450nm to 650nm, and has excellent spectral characteristics. In the high temperature tests (90℃) and (100℃) required for the optical field in the automotive field, microcracks occurred, making the appearance unacceptable, so it was rated "X".
[0115] The single-layer film made by the vacuum deposition method showed no problems in the high-temperature test (90°C), but cracks occurred in the high-temperature test (100°C), resulting in an "X" rating.
[0116] As shown in FIG. 9, Example 1 had an average transmittance of about 98% or more from 450 nm to 650 nm. It also showed excellent results with no change in the high temperature test and high temperature and high humidity test. Since Example 1 is manufactured using the same equipment, continuous production is possible, and mass production is also expected.
[0117] (A-4) Effects of the embodiment As described above, according to this embodiment, a protective film is formed on the fine uneven structure formed on the surface of a synthetic resin base material, and optical components having a high anti-reflection effect in a high temperature environment can be manufactured.
Claims
1. a microrelief structure forming step of changing a surface of a substrate by ion irradiation to form a microrelief structure on the surface of the substrate; a protective film forming step of evaporating a deposition material and depositing it on the surface of the base material to form a protective film on the fine uneven structure formed on the surface of the substrate; A method for producing an optical member, comprising:
2. The fine unevenness forming step includes discharging plasma in a reduced pressure vessel and irradiating the surface of the base with ions in the plasma atmosphere to form the fine unevenness on the surface of the base, The protective film forming step is performed in the same vessel as the fine unevenness structure forming step, by using silicon oxide as the deposition material and attaching silicon oxide to the surface of the base material by vacuum deposition to form a silicon oxide film on the fine unevenness structure on the surface of the base material. The method for producing an optical member according to claim 1 .
3. The fine unevenness forming step includes discharging plasma in a reduced pressure vessel and irradiating the surface of the base with ions in the plasma atmosphere to form the fine unevenness on the surface of the base, The protective film forming step is performed in the same vessel as the fine unevenness forming step, by gasifying an organosilicon compound by chemical vapor deposition using an organosilicon compound as the deposition material, and forming a silicon oxide mixed film on the fine unevenness on the surface of the base material. The method for manufacturing an optical component according to claim 1 .
4. The fine unevenness forming step includes discharging plasma in a reduced pressure vessel and irradiating the surface of the base with ions in the plasma atmosphere to form the fine unevenness on the surface of the base, The protective film forming step is performed in a container different from that in the fine unevenness structure forming step, in which an organosilicon compound is used as the deposition material, and the organosilicon compound is gasified by chemical vapor deposition to form a silicon oxide mixed film on the fine unevenness structure on the surface of the base material. The method for manufacturing an optical component according to claim 1 .
5. The fine unevenness forming step includes discharging plasma in a reduced pressure vessel and irradiating the surface of the base with ions in the plasma atmosphere to form the fine unevenness on the surface of the base, The protective film forming step is performed in a container different from that in the fine unevenness forming step, in which silicon oxide is used as the deposition material, and silicon oxide is attached to the surface of the base material by vacuum deposition to form a silicon oxide film on the fine unevenness on the surface of the base material. The method for manufacturing an optical component according to claim 1 .
6. 2. The method for manufacturing an optical component according to claim 1, wherein the evaporation material has a refractive index of 1.6 or less, and the protective film has an optical thickness of λ / 50 to λ / 16 when irradiated with light having a wavelength of 550 nm.
7. 6. The method for manufacturing an optical component according to claim 2, wherein in the protective film forming step, the silicon oxide film has an optical thickness of λ / 50 to λ / 3 when irradiated with light having a wavelength of 550 nm.
8. 5. The method for manufacturing an optical component according to claim 3, wherein in the protective film forming step, the silicon oxide mixed film has an optical film thickness of λ / 50 to λ / 8 when irradiated with light having a wavelength of 550 nm.
Citation Information
Patent Citations
Anti-fog coated lens
CN218298561U
Antireflection treatment of transparent substrate
JP1987143846A
Reflection preventing plate
JP1989239501A
Optical functional membrane, optical functional film, antiglare- antireflection film, manufacturing method therefor, polarizing plate, and liquid crystal display device
JP2004341541A
Antireflection method, antireflection structure, antireflection structural body having the antireflection structure and method for manufacturing the same
JP2006343758A