Silicon clathrate electrode active material, negative electrode mixture, negative electrode active material layer, solid-state lithium-ion battery, and method for manufacturing negative electrode active material layer

A silicon clathrate electrode active material with a controlled sodium compound ratio and clathrate type II structure, combined with a solid electrolyte, effectively minimizes expansion during charging, enhancing battery performance.

JP2024160567APending Publication Date: 2024-11-14TOYOTA JIDOSHA KK +1

Patent Information

Application Number
JP2023075707
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Silicon clathrate electrode active materials, while suppressing expansion during charging, still require further reduction in expansion to enhance battery performance.

Method used

A silicon clathrate electrode active material containing a specific ratio of a sodium compound, within the range of 0.1% to 5.0% by mass, and optionally having a clathrate type II structure, is used in conjunction with a solid electrolyte to form a negative electrode composite material, which is then processed to minimize expansion during charging.

Benefits of technology

The solution results in a silicon clathrate electrode active material that exhibits minimal expansion during charging, contributing to improved battery performance by reducing confining pressure fluctuations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160567000001_ABST
    Figure 2024160567000001_ABST
Patent Text Reader

Abstract

To provide a silicon clathrate electrode active material that exhibits low expansion during charging, and a solid-state lithium-ion battery having such a silicon clathrate electrode active material.SOLUTION: A silicon clathrate electrode active material according to the present disclosure includes a sodium compound. In addition, in the silicon clathrate electrode active material according to the present disclosure, the ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound is 0.1 mass% or more and 5.0 mass% or less. A solid-state lithium-ion battery according to the present disclosure has a negative electrode active material layer according to the present disclosure. The negative electrode active material layer according to the present disclosure contains a negative electrode mixture according to the present disclosure. The negative electrode mixture according to the present disclosure includes the silicon clathrate electrode active material according to the present disclosure and a solid electrolyte.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a silicon class rate electrode active material, a negative electrode composite material, a negative electrode active material layer, a solid lithium ion battery, and a method for manufacturing a negative electrode active material layer.

Background Art

[0002] In recent years, battery development has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles has been promoted. Also, silicon is known as an electrode active material used in batteries, particularly lithium ion batteries.

[0003] The silicon electrode active material has a large theoretical capacity and is effective for increasing the energy density of the battery. On the other hand, the silicon electrode active material has a problem of large expansion during charging. In contrast, it is known that by using a silicon class rate electrode active material as the silicon electrode active material, the expansion during charging can be suppressed.

[0004] For example, Patent Document 1 discloses a silicon class rate electrode active material having a silicon class rate type II crystal phase and having a composition of Na x Si 136 (1.98 < x < 2.54).

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0006] Although the silicon class rate electrode active material can suppress the expansion during charging as compared with the ordinary silicon electrode active material, it is required to further suppress the expansion during charging of the silicon class rate electrode active material.

[0007] An object of the present disclosure is to provide a silicon clathrate electrode active material that exhibits small expansion during charging, and a solid-state lithium-ion battery having such a silicon clathrate electrode active material. [Means for solving the problem]

[0008] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A silicon clathrate electrode active material containing a sodium compound, The ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound is 0.1 mass% or more and 5.0 mass% or less. Silicon clathrate electrode active material. <Aspect 2> 2. The silicon clathrate electrode active material according to embodiment 1, wherein the ratio is 0.5% by mass or more and 3.0% by mass or less. <Aspect 3> 3. The silicon clathrate electrode active material of claim 1 or 2, wherein the sodium compound is sodium oxide and / or sodium silicate. <Aspect 4> 4. The silicon clathrate electrode active material according to any one of aspects 1 to 3, having at least a partial clathrate II structure. <Aspect 5> A negative electrode mixture comprising the silicon clathrate electrode active material according to any one of aspects 1 to 4 and a solid electrolyte. Aspect 6 6. The anode composite of claim 5, wherein the solid electrolyte is a sulfide solid electrolyte. Aspect 7 A negative electrode active material layer comprising the negative electrode mixture according to aspect 5 or 6. <Aspect 8> A solid-state lithium ion battery having the anode active material layer of embodiment 7. <Aspect 9> Mixing the silicon clathrate electrode active material according to any one of aspects 1 to 4, a solid electrolyte, and an organic solvent; and Drying the slurry obtained by the mixing. 8. A method for producing a negative electrode active material layer according to claim 7, comprising: Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a silicon clathrate electrode active material that exhibits small expansion during charging, and a solid-state lithium ion battery having such a silicon clathrate electrode active material. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a graph showing the results of measuring the bond energy by X-ray photoelectron spectroscopy (XPS) in Examples 1 to 3 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0012] Silicon clathrate electrode active material The silicon clathrate electrode active material of the present disclosure includes a sodium compound. In addition, in the silicon clathrate electrode active material of the present disclosure, the ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound is 0.1 mass% or more and 5.0 mass% or less.

[0013] Silicon clathrates can be obtained in any manner. Generally, silicon clathrates can be formed by removing sodium from a sodium silicon (NaSi) alloy.

[0014] For example, in the manufacture of silicon clathrate, first, silicon and sodium hydride are reacted to prepare a NaSi alloy. Then, the NaSi alloy thus prepared is heated to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a silicon clathrate. Alternatively, the NaSi alloy thus prepared is reacted with aluminum fluoride as a sodium trapping agent to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a silicon clathrate.

[0015] At this time, in addition to the silicon clathrate, sodium compounds are also produced, but these sodium compounds can be removed by a subsequent treatment.

[0016] In contrast, the present inventors have unexpectedly discovered that a silicon clathrate electrode active material containing a small amount of sodium derived from a sodium compound exhibits small expansion during charging.

[0017] The reason for this is presumed to be as follows, without intending to be bound by any theory: That is, a small amount of sodium derived from the sodium compound can suppress the oxidation reaction of the silicon clathrate electrode active material and the reduction reaction of the solid electrolyte that proceed at the interface between the silicon clathrate electrode active material and the solid electrolyte, and this is thought to suppress the decrease in the silicon clathrate electrode active material used for charging, and the charging reaction proceeds uniformly to suppress expansion during charging.

[0018] In the present disclosure, the "electrode active material" can be used as either a "positive electrode active material" or a "negative electrode active material", and is particularly used as a "negative electrode active material".

[0019] The silicon clathrate electrode active material of the present disclosure includes a sodium compound.

[0020] In the present disclosure, the ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound is 0.1 mass% or more and less than 5.0 mass%. This ratio within the above range is preferable in order to sufficiently suppress expansion during charging.

[0021] This ratio may be 0.2% by mass or more, 0.3% by mass or more, 0.4% by mass or more, 0.5% by mass or more, 0.6% by mass or more, 0.7% by mass or more, or 0.8% by mass or more, and may be 4.5% by mass or less, 4.0% by mass or less, 3.5% by mass or less, 3.3% by mass or less, 3.2% by mass or less, 3.1% by mass or less, 3.0% by mass or less, 2.9% by mass or less, or 2.8% by mass or less.

[0022] This ratio can be calculated as the ratio of the area in the range of 1072 eV to 1076 eV to the area in the range of 1070 eV to 1076 eV in the results of X-ray photoelectron spectroscopy (XPS) measurement of the silicon clathrate electrode active material. As an apparatus for XPS measurement, VersaProbe II manufactured by ULVAC-PHI Corporation can be used.

[0023] The sodium compound in this disclosure may be sodium oxide and / or sodium silicate.

[0024] The silicon clathrate electrode active material of the present disclosure may at least partially have a clathrate II structure, which can further reduce expansion during charging.

[0025] In order to adjust the ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound in the silicon clathrate electrode active material, a treatment for removing oxides on the surface of the silicon clathrate electrode active material can be performed.

[0026] The oxide removal treatment is carried out by immersing the silicon clathrate electrode active material in a solution capable of dissolving and removing silicon oxide, for example, a hydrogen fluoride (HF) aqueous solution, to dissolve and remove silicon oxide, thereby removing sodium compounds present on the surface of the silicon clathrate electrode active material. In addition, the silicon clathrate electrode active material may contain sodium silicate (Na 2 SiO 3 ), sodium silicate can be converted to soluble silicic acid (H 2 SiO 3 ), and the silicic acid can be removed to reduce the sodium atoms in the silicon clathrate electrode active material (Na 2 SiO 3 +2HCl→2NaCl(dissolved)+H 2 SiO 3 (dissolution)).

[0027] The oxide removal process can be accelerated by performing an oxidation process before the oxide removal process. As a specific oxidation process, the silicon clathrate electrode active material can be placed in an oxidizing atmosphere and optionally heated. As a method for placing the material in an oxidizing atmosphere, for example, the material is placed in an apparatus capable of reducing pressure and replacing gas, and the pressure in the apparatus is reduced to room temperature, and then the air is introduced.

[0028] On the other hand, when oxidation treatment is performed, silicon oxide (SiO 2 When the oxidation process is performed with HF, an oxide film of SiO 2 When the oxidation treatment is not performed, the amount of sodium compound produced is small, so the ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound is small.

[0029] In the present disclosure, it is preferable not to carry out an oxidation treatment, or, if an oxidation treatment is carried out, to appropriately adjust the amount of air introduced.

[0030] 《Negative electrode mixture》 The negative electrode mixture of the present disclosure includes a silicon clathrate electrode active material as a negative electrode active material, a solid electrolyte, and optionally a conductive additive and a binder.

[0031] In the present disclosure, the term "negative electrode mixture" refers to a composition that can form a negative active material layer as it is or by further containing other components. In the present disclosure, the term "negative electrode mixture slurry" refers to a slurry that contains a dispersion medium in addition to the "negative electrode mixture" and can be applied and dried to form a negative electrode active material layer.

[0032] <Silicon clathrate electrode active material> For the silicon clathrate electrode active material, reference may be made to the above description of the silicon clathrate electrode active material of the present disclosure.

[0033] <Solid electrolyte> The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte, an oxide solid electrolyte, a polymer electrolyte, or the like, and is preferably a sulfide solid electrolyte.

[0034] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li 2 SP 2 S 5 System (Li 7 P 3 S 11 , Li 3 P.S. 4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2, LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -GeS 2 (Li 13 GeP 3 S 16 , Li 10 GeP 2 S 12 etc.), LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.

[0035] An example of an oxide solid electrolyte is Li 7 La 3 Zr 2 O 12 , Li 7-x La 3 Zr 1-x Nb x O 12 , Li 7-3x La 3 Zr 2 Al x O 12 , Li 3x La 2 / 3-x TiO 3 , Li 1+x Al x Ti 2-x (PO 4 ) 3 , Li 1+x Al x Ge 2-x (PO 4 ) 3 , Li 3 PO 4 , or Li 3+x PO 4-x N x(LiPON), but is not limited to these.

[0036] The sulfide solid electrolyte and the oxide solid electrolyte may be glass or crystallized glass (glass ceramic).

[0037] Examples of the polymer electrolyte include, but are not limited to, polyethylene oxide (PEO), polypropylene oxide (PPO), and copolymers thereof.

[0038] The mass ratio of the silicon clathrate electrode active material to the solid electrolyte in the negative electrode mixture (mass of silicon clathrate electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0039] <Conductive assistant> The conductive assistant is not particularly limited. For example, the conductive assistant may be, but is not limited to, VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), or other carbon material, metal material, or the like.

[0040] <binder> The binder is not particularly limited. For example, the binder may be, but is not limited to, a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), or styrene butadiene rubber (SBR), or a combination thereof.

[0041] 《Negative electrode active material layer》 The negative electrode active material layer of the present disclosure contains the negative electrode mixture of the present disclosure. For the negative electrode mixture, the above description of the negative electrode mixture of the present disclosure can be referenced.

[0042] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.

[0043] <<Method for producing negative electrode active material layer>> The disclosed method of producing an anode active material layer includes mixing a silicon clathrate electrode active material of the disclosed invention, a solid electrolyte, and an organic solvent, and drying the resulting slurry.

[0044] For the solid electrolyte, reference may be made to the above description regarding the negative electrode mixture of the present disclosure.

[0045] Examples of the organic solvent include non-polar solvents such as heptane, xylene, and toluene, and polar solvents such as ester solvents, tertiary amine solvents, ether solvents, thiol solvents, and ketone solvents. The organic solvent is preferably a polar solvent, and more preferably a ketone solvent.

[0046] Solid-state lithium-ion battery The solid-state lithium ion battery of the present disclosure has the negative electrode active material layer of the present disclosure. The solid-state lithium ion battery of the present disclosure may have, in this order, a negative electrode current collector layer, a negative electrode active material layer of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer. Furthermore, the lithium ion battery of the present disclosure may be restrained by restraining members such as end plates from both sides in the stacking direction of each of the layers.

[0047] In the present disclosure, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. Also, the solid-state battery of the present disclosure may be an all-solid-state battery, i.e., a battery that uses only a solid electrolyte as an electrolyte.

[0048] In the lithium ion battery of the present disclosure, the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure, and therefore expansion due to charging is reduced, thereby suppressing an increase in confining pressure due to charging.

[0049] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, the material may be stainless steel (SUS), aluminum, copper, nickel, iron, titanium, carbon, a resin current collector, or the like, but is not limited to these.

[0050] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0051] <Negative electrode active material layer> For the negative electrode active material layer, reference can be made to the above description regarding the negative electrode active material layer of the present disclosure.

[0052] <Solid electrolyte layer> The solid electrolyte layer includes at least a solid electrolyte. In addition to the solid electrolyte, the solid electrolyte layer may include a binder, etc., as necessary. For the solid electrolyte and the binder, the above description regarding the negative electrode mixture of the present disclosure can be referred to.

[0053] The solid electrolyte layer may be impregnated with an electrolyte solution having lithium ion conductivity.

[0054] The electrolyte preferably contains an electrolyte supporting salt and a solvent. Examples of the electrolyte supporting salt (lithium salt) having lithium ion conductivity include LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 Inorganic lithium salts such as LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiC(CF 3 SO 2 ) 3Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.

[0055] The thickness of the solid electrolyte layer is, for example, 0.1 to 1000 μm. The thickness of the solid electrolyte layer is preferably 0.1 to 300 μm, and particularly preferably 0.1 to 100 μm.

[0056] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally a solid electrolyte, a conductive assistant, a binder, and the like.

[0057] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganate (LiMn 2 O 4 ), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li 1+x Mn 2-x-y MyO 4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), or the like, but is not limited thereto.

[0058] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials that constitute the coating layer include LiNbO 3 In addition, Li 4Ti 5 O 12 , Li 3 PO 4 These include, but are not limited to, the following.

[0059] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0060] For the solid electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode mixture of the present disclosure.

[0061] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0062] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0063] <Positive electrode current collector layer> The material and shape of the positive electrode current collector layer are not particularly limited, and the above description of the negative electrode active material layer of the present disclosure can be referred to. In particular, the material of the positive electrode current collector layer is preferably aluminum. The shape is preferably a foil. EXAMPLES

[0064] 《Synthesis of silicon clathrate electrode active material》 <Alloying> Comparative Example 1 As a silicon (Si) source, Si powder (Kojundo Kagaku, SIEPB32) was prepared. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon alloy. The obtained lithium silicon alloy was reacted with ethanol in an argon atmosphere, and further treated with hydrogen fluoride (HF) to obtain a powder having voids inside the primary particles, i.e., a Si powder having a porous structure.

[0065] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0066] <Clathrate formation> The obtained NaSi alloy and aluminum fluoride (AlF 3 ) were weighed out so that the molar ratio was 1:0.35, and the weighed NaSi alloy and AlF 3 The powdered reaction raw materials were mixed in a cutter mill to obtain reaction raw materials. The obtained powdered reaction raw materials were placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 310°C for 60 hours to obtain a reaction product containing silicon clathrate. The obtained reaction product was placed in a device capable of reducing pressure and replacing gases, and the pressure inside the device was reduced to room temperature, after which the air was introduced and oxidized. The oxidized reaction product was then oxidized with HNO 3 and H 2The reaction product was washed with an acid using a mixed solvent in which O was mixed with 10:90 by volume to remove by-products in the reaction product. After washing, the mixture was filtered, and the filtered solid was dried at 120°C for 3 hours or more to obtain a powdered silicon clathrate electrode active material. The obtained material was further washed with a 3 wt% HF solution, filtered, and then dried at 120°C for 3 hours or more to obtain a silicon clathrate electrode active material of Comparative Example 1.

[0067] Example 1 A silicon clathrate electrode active material of Example 1 was obtained in the same manner as in Comparative Example 1, except that the heating time in the clathrate formation was 20 hours and oxidation was not carried out.

[0068] Example 2 A silicon clathrate electrode active material of Example 2 was obtained in the same manner as in Comparative Example 1, except that oxidation in the clathrate formation was not carried out.

[0069] Example 3 A silicon clathrate electrode active material of Example 3 was obtained in the same manner as in Comparative Example 1, except that in the clathrate formation, air was introduced to oxidize the material so that the amount of air inflow was 1 / 100 of that in Comparative Example 1.

[0070] The silicon clathrate electrode active material in each example had a clathrate II type crystal phase.

[0071] <<Making a lithium-ion battery>> Using the silicon clathrate electrode active material of each example, a lithium ion battery of each example was produced as follows.

[0072] <Preparation of negative electrode mixture> A polypropylene container was filled with a ketone-based solvent, a 5 wt% ketone-based solution of polyvinylidene fluoride (PVDF)-based binder, vapor grown carbon fiber (VGCF) as a conductive additive, a synthesized silicon clathrate electrode active material, and Li as a sulfide solid electrolyte. 2 SP 2 S 5The glass ceramic was added and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.). Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a slurry-like negative electrode mixture (negative electrode mixture slurry).

[0073] <Formation of negative electrode active material layer> The obtained negative electrode composite slurry was applied onto a copper (Cu) foil serving as a negative electrode current collector layer by the blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C to form a negative electrode active material layer on the negative electrode current collector layer.

[0074] <Formation of solid electrolyte layer> A polypropylene container was filled with heptane, a 5 wt% heptane solution of butylene rubber (BR)-based binder, and Li as a sulfide solid electrolyte. 2 SP 2 S 5 The glass ceramic was added and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.) Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry.

[0075] The obtained solid electrolyte slurry was applied onto an aluminum (Al) foil as a release sheet by a blade method using an applicator, and dried for 30 minutes on a hot plate heated to 100°C to form a solid electrolyte layer. Three solid electrolyte layers were produced.

[0076] Preparation of Positive Electrode Mixture A polypropylene container is filled with a ketone-based solvent, a 5 wt% ketone-based solution of a PVDF-based binder, and LiNi with an average particle size of 6 μm as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 , Li as sulfide solid electrolyte 2 SP 2 S 5 The glass ceramic and VGCF as a conductive additive were added to the container, and the mixture was stirred for 30 seconds using an ultrasonic disperser (UH-50 manufactured by SMT). Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.), further stirred with an ultrasonic dispersing device for 30 seconds, and then shaken for 3 minutes with the shaker to obtain a positive electrode composite slurry.

[0077] <Formation of Positive Electrode Active Material Layer> The obtained positive electrode mixture slurry was applied onto an Al foil serving as a positive electrode current collector layer by a blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C, thereby forming a positive electrode active material layer on the positive electrode current collector layer.

[0078] <Battery Assembly> The positive electrode current collector layer, the positive electrode active material layer, and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. to obtain a positive electrode laminate.

[0079] The negative electrode current collector layer, the negative electrode active material layer, and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. to obtain a negative electrode laminate.

[0080] Furthermore, the Al foil as a release sheet was peeled off from the surfaces of the solid electrolyte layers of the positive electrode laminate and the negative electrode laminate, and then the Al foil as a release sheet was peeled off from the third solid electrolyte layer.

[0081] The positive electrode laminate and the negative electrode laminate were laminated on top of each other so that the solid electrolyte layer of each laminate faced the third solid electrolyte layer, and the laminate was set in a flat uniaxial press and pre-pressed at 100 MPa and 25° C. for 10 seconds, and finally the laminate was set in a flat uniaxial press and pressed at a pressure of 200 MPa and a press temperature of 120° C. for 1 minute, thereby obtaining an all-solid-state battery.

[0082] "evaluation> <Proportion of mass of sodium compound to total mass of silicon clathrate electrode active material and sodium compound> The silicon clathrate electrode active materials obtained in Comparative Example 1 and Examples 1 to 3 were subjected to XPS measurement using an X-ray photoelectron spectrometer (ULVAC-PHI, VersaProbe II). The ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound was calculated as the ratio of the area in the range of 1072 eV to 1076 eV to the area in the range of 1070 eV to 1076 eV in the XPS measurement results. In addition, from the obtained peaks, it was estimated that the sodium compound was at least one of sodium oxide and sodium silicate.

[0083] <Expansion amount> The all-solid-state battery of each example was restrained at a predetermined restraining pressure using a restraining jig, and the amount of restraining pressure fluctuation was measured when constant current / constant voltage charging was performed up to 4.55 V at a 10-hour rate (1 / 10C). This amount of restraining pressure fluctuation was taken as the amount of expansion in this disclosure. The amount of restraining pressure fluctuation is the difference between the maximum and minimum values ​​of the restraining pressure, and the values ​​of the examples are shown as relative values ​​when the value of Comparative Example 1 is taken as 100.

[0084] "result" Table 1 shows the ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound (mass fraction of the sodium compound) and the amount of expansion of the silicon clathrate electrode active material for each example.

[0085] [Table 1]

[0086] As shown in Table 1, the batteries of Examples 1 to 3, in which the ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound was within the range of the present disclosure, had a smaller amount of expansion than the battery of Comparative Example 1.

Claims

1. A silicon clathrate electrode active material containing a sodium compound, The ratio of the mass of the sodium compound to the total mass of the silicon clathrate electrode active material and the sodium compound is 0.1 mass% or more and 5.0 mass% or less; Silicon clathrate electrode active material.

2. The silicon clathrate electrode active material according to claim 1 , wherein the ratio is 0.5% by mass or more and 3.0% by mass or less.

3. The silicon clathrate electrode active material according to claim 1 , wherein the sodium compound is sodium oxide and / or sodium silicate.

4. 2. The silicon clathrate electrode active material of claim 1 having at least partially a clathrate II type structure.

5. A negative electrode mixture comprising the silicon clathrate electrode active material according to claim 1 and a solid electrolyte.

6. 6. The negative electrode mixture of claim 5, wherein the solid electrolyte is a sulfide solid electrolyte.

7. A negative electrode active material layer comprising the negative electrode mixture according to claim 5 .

8. A solid-state lithium ion battery comprising the negative electrode active material layer according to claim 7.

9. Mixing the silicon clathrate electrode active material according to claim 1, a solid electrolyte, and an organic solvent; and Drying the slurry obtained by the mixing. The method for producing a negative electrode active material layer according to claim 7 , comprising:

Citation Information

Patent Citations

  • Negative electrode active material including silicon clathrate ii

    JP2021034279A

  • Rapid reduction of sodium occupancy in type ii silicon clathrate by chemical etching

    US20150376016A1

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158003A

Cited By

  • Method for manufacturing silicon clathrate electrode active material, and method for manufacturing lithium-ion battery

    JP2024165116A

  • Method for manufacturing silicon clathrate electrode active material and method for manufacturing lithium ion battery

    JP7782511B2