Styrene-based elastomer composition, uncured resin film, cured resin film, adhesive film, sealing material and substrate
A styrenic elastomer composition with styrene-based copolymers and maleimide compounds addresses the issue of insufficient dielectric properties and adhesion in high-frequency adhesives, ensuring stable performance and compatibility for 5G substrate applications.
Patent Information
- Application Number
- JP2023075920
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing adhesives used in substrate applications for high-frequency 5G communication do not exhibit sufficient dielectric properties in the millimeter wave range and often separate or fail to adhere properly to materials like LCP and MPI, leading to unsuitable performance for flexible printed circuits.
A styrenic elastomer composition comprising styrene-based copolymers, maleimide compounds with dimer acid skeletons, and organic peroxides, which are mixed to form a varnish-like solution that maintains adhesion and dielectric properties, preventing separation and enhancing compatibility with organic resins and copper.
The styrenic elastomer composition provides excellent dielectric properties and strong adhesion to both organic resins and copper, suitable for high-frequency applications without turbidity or separation, making it useful for substrate materials in flexible printed circuits.
Smart Images

Figure 2024160719000001 
Figure 2024160719000002 
Figure 2024160719000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a styrenic elastomer composition, uncured and cured resin films containing the composition, adhesive films, adhesives, sealants, and substrates comprising the styrenic elastomer composition. [Background technology]
[0002] In recent years, the next-generation mobile communication system known as 5G has become popular, aiming to realize high-speed, large-capacity, low-latency communications. To realize this, materials for high-frequency bands are required, and since reducing transmission loss is essential as a noise countermeasure, there is a demand for the development of insulating materials with excellent dielectric properties (low dielectric constant and low dielectric tangent).
[0003] Among these, insulating materials with excellent dielectric properties are in demand for circuit board applications. Insulating materials with excellent dielectric properties are required for circuit boards such as rigid and flexible circuit boards, and reactive polyphenylene ether resins (PPE) are being used for rigid circuit boards, while liquid crystal polymers (LCPs) and modified polyimides (MPIs) with improved properties are being used for flexible printed circuit boards (FPCs).
[0004] When manufacturing the above FPC, an adhesive is required to attach the base film and coverlay film to the surface having the wiring portion by using a heat press, etc. Traditionally, adhesives that mainly use epoxy resins have been used, but recently there has been a demand for adhesives with excellent dielectric properties.
[0005] In light of this background, adhesives with excellent dielectric properties have been reported (for example, Patent Documents 1 to 4), but most of them are combinations of epoxy resins, other thermosetting resins, and thermoplastic resins. These compositions have excellent dielectric properties in the frequency range of 10 GHz or less, but 5G requires them to have dielectric properties in the frequency range of 28 GHz or more, known as millimeter waves, and many of the adhesives that were previously said to have excellent dielectric properties do not currently have sufficient dielectric properties.
[0006] In addition, a resin composition containing a special maleimide compound and a thermoplastic resin has been disclosed as a composition that has excellent high-frequency characteristics and also has a high level of adhesion to conductors (Patent Document 5). However, it has been found that the resin composition described in Patent Document 5 is in a varnish state and the resins are not compatible with each other, resulting in separation of the varnish, making it impossible to obtain a resin film, or even if a resin film is obtained, it does not exhibit adhesiveness, making it unsuitable for substrate applications. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-248141 A [Patent Document 2] JP 2011-68713 A [Patent Document 3] International Publication No. 2016 / 17473 [Patent Document 4] JP 2016-79354 A [Patent Document 5] International Publication No. 2018 / 16489 Summary of the Invention [Problem to be solved by the invention]
[0008] Accordingly, an object of the present invention is to provide a styrene-based elastomer composition which is in a varnish form and free of turbidity or separation, has excellent dielectric properties, and has strong adhesive strength to organic resins such as LCP and MPI, and to copper, as well as an uncured resin film, a cured resin film, an adhesive, a sealant, and a substrate comprising the styrene-based elastomer composition. [Means for solving the problem]
[0009] Means of Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the following styrene-based elastomer composition can achieve the above object, thereby completing the present invention.
[0010] <1> (A) styrene-based elastomer: 100 parts by mass, (B) 1 to 50 parts by mass of a maleimide compound having at least one dimer acid skeleton in one molecule, which is represented by the following formula (1): [ka] (In formula (1), A is independently a tetravalent organic group having a cyclic structure, B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms, Q is independently represented by the following formula (2): [ka] (In formula (2), R 1 are independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and x1 and x2 are each independently a number from 0 to 10. is a divalent alicyclic hydrocarbon group having 6 to 60 carbon atoms and a cyclohexane skeleton represented by W is B or Q; n is 0 to 100, and m is 0 to 200, but n and m are not 0 at the same time; The order of the repeating units bracketed by n and m is not limited, and the bonding pattern may be alternating, block, or random. (C) Organic peroxide: 0.01~10 parts by mass A styrene-based elastomer composition comprising: <2> The styrene-based elastomer of component (A) is a copolymer of styrene and a compound having a carbon-carbon double bond. <1> The styrene-based elastomer composition according to claim 1. <3> In formula (1), A is any of the tetravalent organic groups represented by the following structural formulas: <1> The styrene-based elastomer composition according to claim 1. [ka] (The bond not bonded to a substituent in the above structural formula is bonded to the carbonyl carbon that forms a cyclic imide structure in formula (1).) <4> Further, the adhesive agent (D) is contained. <1> ~ <3> 13. The styrene-based elastomer composition according to claim 12. <5> <1> ~ <4> 2. An uncured resin film comprising the styrene-based elastomer composition according to claim 1. <6> <1> ~ <4> 13. A cured resin film comprising the cured product of the styrenic elastomer composition according to any one of claims 1 to 12. <7> <1> ~ <4> 13. An adhesive film comprising the styrene-based elastomer composition according to claim 12. <8> <1> ~ <4> 13. An adhesive comprising the styrene-based elastomer composition according to claim 12. <9> <1> ~ <4> 13. An encapsulant comprising the styrene-based elastomer composition according to claim 12. <10> <1> ~ <4> 13. A substrate having a cured product of the styrenic elastomer composition according to claim 12. Effect of the Invention
[0011] The styrene-based elastomer composition of the present invention is in a varnish form, does not become cloudy or separate, has excellent dielectric properties, and has strong adhesive strength to organic resins such as LCP and MPI, and to copper. Therefore, the styrene-based elastomer composition of the present invention is particularly useful as a bonding sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will now be described in more detail.
[0013] (A) Styrene-based elastomer The styrene-based elastomer of component (A) mainly contributes to low dielectric properties at high frequencies, improved heat resistance and adhesiveness of the cured product of the composition, and improved flexibility when the composition is made into a film, and is not particularly limited as long as it has a structural unit derived from a styrene-based compound and is an elastomer, and may be a thermoplastic elastomer having a structural unit derived from styrene. In addition, it may be a thermoplastic elastomer that has been modified with a reactive functional group or may not be modified.
[0014] In the present invention, the styrene-based elastomer is preferably a copolymer of styrene and a compound having a carbon-carbon double bond (a compound other than styrene having a carbon-carbon double bond), which is partially or completely hydrogenated. That is, it is preferably a block copolymer and / or random copolymer in which styrene is the hard segment and a compound having a carbon-carbon double bond (a compound other than styrene having a carbon-carbon double bond) is the soft segment. Examples of styrene-based elastomers include styrene / butadiene / styrene block / random copolymer, styrene / isoprene / styrene block / random copolymer, styrene / ethylene / butylene / styrene block / random copolymer, styrene / ethylene / propylene / styrene block / random copolymer, and styrene / butadiene block / random copolymer. Block copolymers are preferred from the viewpoint of quality stability.
[0015] From the viewpoint of heat resistance, it is preferable to use styrene / ethylene / butylene / styrene block / random copolymer, styrene / ethylene / propylene / styrene block / random copolymer, styrene / butadiene block / random copolymer, etc., in which the double bonds of compounds having carbon-carbon double bonds (compounds other than styrene having carbon-carbon double bonds) have been eliminated by hydrogenation reaction (hydrogenation). Hydrogenation may be partial or complete, but complete hydrogenation or one with a high hydrogenation rate is more preferable from the viewpoint of heat resistance.
[0016] The mass ratio of styrene / compound having a carbon-carbon double bond (compound other than styrene having a carbon-carbon double bond) and the part in which the double bond is hydrogenated in the styrene copolymer is preferably 10 / 90 to 70 / 30, more preferably 20 / 80 to 67 / 33. If the mass ratio is within this range, a composition having excellent compatibility and dispersibility and stable quality can be obtained. That is, the styrene content by mass in the styrene-based elastomer is preferably 10 to 70 mass%, more preferably 20 to 67 mass%.
[0017] The styrene elastomer may be modified with a carboxyl group or an amino group. The styrene elastomer may be modified, for example, by copolymerizing an unsaturated carboxylic acid during polymerization of the styrene elastomer. The styrene elastomer may also be modified by heating and kneading the styrene elastomer and the unsaturated carboxylic acid in the presence of an organic peroxide. Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, maleic anhydride, itaconic anhydride, and fumaric anhydride.
[0018] The number average molecular weight (Mn) of the styrene-based elastomer (A) is preferably 10,000 to 300,000, and more preferably 10,000 to 200,000. When the number average molecular weight is within the specified range, the resulting composition has excellent film properties, excellent compatibility and dispersibility with other components such as components (B) and (C), and exhibits good adhesion. The number average molecular weight referred to in the present invention refers to the number average molecular weight measured by gel permeation chromatography (GPC) under the following conditions using polystyrene as a standard substance.
[0019] [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-L TSKgel SuperHZ4000(4.6mmI.D.×15cm×1) TSKgel SuperHZ3000(4.6mmI.D.×15cm×1) TSKgel SuperHZ2000 (4.6mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 5 μL (0.2% by mass in THF solution)
[0020] The styrene-based elastomer (A) may be a commercially available product. Specific examples include the Tuftec series manufactured by Asahi Kasei Corporation and the FG series manufactured by Kraton. The composition of the present invention may contain one type of styrene-based elastomer alone or a mixture of two or more types.
[0021] (B) Specific Maleimide Compound The component (B) used in the present invention is a specific maleimide compound, which contains at least one dimer acid skeleton, at least one linear alkylene group having 6 or more carbon atoms, and at least two cyclic imide groups in one molecule. The component (B) is a thermosetting resin, and by adding it, the heat resistance, mechanical properties, and adhesiveness are improved, resulting in a highly reliable composition. In addition, the component (B) has good dielectric properties because it has a dimer acid skeleton. Therefore, the composition exhibits excellent dielectric properties.
[0022] The dimer acid referred to here is a liquid fatty acid mainly composed of a dicarboxylic acid with 36 carbon atoms, produced by dimerization of unsaturated fatty acids with 18 carbon atoms, which are derived from natural products such as vegetable oils. Dimer acids do not have a single skeleton, but rather have multiple structures, and there are several types of isomers. Representative dimer acids are classified as linear (a), monocyclic (b), aromatic (c), and polycyclic (d). In this specification, the dimer acid skeleton refers to a group derived from a dimer diamine having a structure in which the carboxy group of such a dimer acid is substituted with a primary aminomethyl group. Examples of the divalent hydrocarbon group derived from the dimer acid skeleton include, but are not limited to, the following structures. Furthermore, from the viewpoint of the heat resistance and reliability of the cured product, it is more preferable that the divalent hydrocarbon group derived from the dimer acid skeleton of component (B) has a structure in which the carbon-carbon double bond in the hydrocarbon group derived from the dimer acid skeleton is reduced by a hydrogenation reaction. [ka]
[0023] The maleimide compound of the component (B) is preferably a maleimide compound having at least one dimer acid skeleton in one molecule, as represented by the following formula (1). When the compound of formula (1) is used as component (B), it has good compatibility with component (A) and is unlikely to become cloudy or separate when made into a varnish, so there is little risk of unevenness occurring in the composition and variations in the properties of the composition.
[0024] [ka] (In formula (1), A is independently a tetravalent organic group having a cyclic structure, B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms, Q is independently represented by the following formula (2): [ka] (In formula (2), R 1 are independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and x1 and x2 are each independently a number from 0 to 10. is a divalent alicyclic hydrocarbon group having 6 to 60 carbon atoms and a cyclohexane skeleton represented by W is B or Q; n is 0 to 100, and m is 0 to 200, but n and m are not 0 at the same time; The order of the repeating units bracketed by n and m is not limited, and the bonding pattern may be alternating, block, or random.
[0025] In the formula (1), A independently represents a tetravalent organic group having a cyclic structure, and among these, any of the tetravalent organic groups represented by the following structural formulas is preferable. [ka] (The bond not bonded to a substituent in the above structural formula is bonded to the carbonyl carbon that forms a cyclic imide structure in formula (1).)
[0026] In addition, in the formula (1), B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms, preferably 8 to 100, and more preferably 10 to 50. Among them, it is preferable that the divalent hydrocarbon group is a branched divalent hydrocarbon group in which one or more hydrogen atoms are substituted with an alkyl or alkenyl group having 6 to 200 carbon atoms, preferably 8 to 100, and more preferably 10 to 50 carbon atoms. The branched divalent hydrocarbon group may be either a saturated aliphatic hydrocarbon group or an unsaturated hydrocarbon group, and may have an alicyclic structure or an aromatic ring structure in the middle of the molecular chain. Specific examples of the branched divalent hydrocarbon group include divalent hydrocarbon groups derived from diamines at both ends, called dimer diamines. Note that dimer diamines are compounds derived from dimers (dimer acids) of unsaturated fatty acids such as oleic acid, and therefore B is particularly preferably a group obtained by removing two carboxy groups from the dimer acids shown in (a) to (d) above.
[0027] In addition, in the formula (1), Q independently represents the following formula (2): [ka] (In formula (2), R 1 are independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and x1 and x2 are each independently a number from 0 to 10. It is a divalent alicyclic hydrocarbon group having a cyclohexane skeleton and having 6 to 60 carbon atoms, preferably 8 to 30 carbon atoms, and more preferably 10 to 20 carbon atoms, represented by the following formula:
[0028] Here, R 1 Specific examples of R include a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a t-butyl group. Among these, a hydrogen atom and a methyl group are preferable. 1 may be the same or different. Moreover, the above x1 and x2 each independently represent a number from 0 to 10, preferably a number from 0 to 8, and more preferably a number from 0 to 6. Note that x1 and x2 may be the same or different.
[0029] Specific examples of Q include divalent alicyclic hydrocarbon groups represented by the following structural formulas. [ka] (The bond not bonded to a substituent in the above structural formula is bonded to the nitrogen atom forming a cyclic imide structure in formula (1).)
[0030] In the formula (1), W is B or Q. Regarding W, the structural unit having B or Q is determined depending on the production method.
[0031] In the formula (1), n is 0 to 100, preferably 2 to 60, and more preferably 5 to 50, and m is 0 to 200, preferably 1 to 50, and more preferably 3 to 40, but n and m are not simultaneously 0. If n or m is too large, the fluidity may decrease, and moldability may be poor.
[0032] In the maleimide compound represented by formula (1), the order of the repeating units bracketed by n and m in the formula is not limited, and the bonding mode may be alternate, block, or random, but is preferably a block bond.
[0033] The maleimide compound of the component (B) is further preferably a maleimide compound represented by the following formula (3) having at least one dimer acid skeleton in one molecule.
[0034] [ka] (In formula (3), A is independently a tetravalent organic group having a cyclic structure, B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms, at least one of which is a hydrocarbon group derived from a dimer acid skeleton, m is 1 to 200.
[0035] Specific examples of A and B in formula (3) include the same as those exemplified for A and B in formula (1), and m is 1 to 200, preferably 1 to 50, and more preferably 3 to 40.
[0036] There are no particular limitations on the number average molecular weight of the maleimide compound of component (B), but from the standpoint of the handleability of the composition, it is preferably from 2,000 to 50,000, and more preferably from 5,000 to 40,000. The component (B) may be used alone or in combination of two or more.
[0037] The amount of (B) is preferably 1 to 50 parts by mass, more preferably 3 to 40 parts by mass, per 100 parts by mass of (A). If this ratio is more than 50 parts by mass, the varnish may become cloudy or the film properties may be impaired. On the other hand, if it is less than 1 part by mass, the thermosetting component may be reduced, resulting in a decrease in mechanical properties and adhesiveness.
[0038] (C)Organic peroxide The organic peroxide, component (C), is added primarily to initiate the crosslinking reaction of the maleimide compound, component (B), or, if there is a radically polymerizable functional group in the styrene-based elastomer, component (A), to promote the reaction between the functional group and the maleimide compound, component (B). Examples of organic peroxides include dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, tert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.
[0039] The amount of the (C) component is preferably 0.01 to 5.0 parts by mass, and more preferably 0.1 to 3.0 parts by mass, per 100 parts by mass of the total amount of the (A) and (B) components. If the amount of the (C) component exceeds 5.0 parts by mass, the adhesive strength may decrease, and the dielectric properties may deteriorate due to the residual (C) component. If the amount of the (C) component is less than 0.01 part by mass, the curability may decrease, resulting in deterioration of the dielectric properties and deterioration of the adhesiveness.
[0040] <Other additives> The styrene-based elastomer composition of the present invention may further contain various additives, if necessary, within the range that does not impair the effects of the present invention.
[0041] (D) Adhesive assistant As the adhesion promoter, a coupling agent such as a silane coupling agent or a titanate coupling agent, or a monomer having a (meth)acrylic group can be blended.
[0042] Examples of the silane coupling agent include epoxy-functional alkoxysilanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercapto-functional alkoxysilanes such as γ-mercaptopropyltrimethoxysilane; amine-functional alkoxysilanes such as γ-aminopropyltrimethoxysilane and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane; and methacryl-functional alkoxysilanes such as 3-methacryloxypropyltrimethoxysilane.
[0043] Titanium coupling agents include isopropyl triisostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, bis(dioctyl pyrophosphate) oxyacetate titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, and isopropyl tri(N-aminoethyl aminoethyl) titanate.
[0044] Examples of monomers having a (meth)acrylic group include 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, dipropylene glycol diacrylate, tricyclodecane dimethanol diacrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene diacrylate, bisphenol A diacrylate, trimethylolpropane triacrylate, tris(2-acryloxymethyl)isocyanurate, ditrimethylolpropane tetraacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol methacrylate, dipropylene glycol methacrylate, tricyclodecane dimethanol methacrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene methacrylate, bisphenol A dimethacrylate, trimethylolpropane trimethacrylate, tris(2-methacryloxymethyl)isocyanurate, and ditrimethylolpropane tetramethacrylate.
[0045] When the (D) component is blended, the blending amount of the (D) component is preferably 0.01 to 5.0 parts by mass, and more preferably 0.1 to 3.0 parts by mass, per 100 parts by mass of the (A) component. If the blending amount of the (D) component is in the range of 0.01 to 5.0 parts by mass per 100 parts by mass of the (A) component, the adhesiveness is improved.
[0046] Other examples of additives include inorganic fillers such as silica, alumina, and boron nitride, resin powders such as PTFE powder, metal particles such as silver, organopolysiloxanes having reactive functional groups, non-functional silicone oils, thermoplastic resins, thermoplastic elastomers other than styrene-based, organic synthetic rubbers, photosensitizers, light stabilizers, polymerization inhibitors, flame retardants, pigments, dyes, etc. In order to improve the electrical properties of the cured product of the thermosetting maleimide resin composition, an ion trapping agent or the like may be blended as other additives.
[0047] The styrene-based elastomer composition of the present invention can be produced by mixing the components (A), (B) and (C) and other additives which are added as required. The styrene-based elastomer composition of the present invention can be dissolved in an organic solvent and treated as a varnish. The styrene-based elastomer composition can be easily molded into a sheet or film by forming it into a varnish. Any organic solvent can be used without limitation as long as it dissolves the (A) component and the (B) component. As the organic solvent, for example, toluene, xylene, anisole, cyclohexanone, cyclopentanone, etc. can be suitably used. The above organic solvents may be used alone or in combination of two or more kinds. The concentration of the styrene-based elastomer composition of the present invention in the varnish is preferably 5 to 80% by mass, more preferably 10 to 75% by mass.
[0048] This styrene-based elastomer composition can be suitably used mainly as an adhesive, a primer, a bonding film or sheet material for a substrate, a sealing material, an adhesive layer for a coverlay film for an FPC, or a flexible flat cable. There are no limitations on the method or form of use. For example, it can be used as an uncured resin film or a cured resin film, or as an adhesive. Examples of use are shown below, but are not limited thereto.
[0049] For example, a styrene-based elastomer composition (varnish) dissolved in an organic solvent is applied to a support sheet, and then the organic solvent is removed by heating at a temperature of usually 80° C. or higher, preferably 100° C. or higher, for 0.5 to 5 hours, to obtain an uncured film-like or sheet-like composition (uncured resin film). As the support sheet, a commonly used one may be used, for example, polyolefin resins such as polyethylene (PE) resin, polypropylene (PP) resin, and polystyrene (PS) resin, and polyester resins such as polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, and polycarbonate (PC) resin, and the surface of these support sheets may be subjected to a release treatment. In addition, the coating method is not particularly limited, and examples thereof include a gap coater, a curtain coater, a roll coater, and a laminator. In addition, the thickness of the coating layer is not particularly limited, but the thickness after distillation of the solvent is in the range of 1 to 100 μm, preferably 3 to 80 μm. Furthermore, a cover film may be used on the coating layer.
[0050] Moreover, a copper foil can be attached onto the coating layer to use it as a substrate material.
[0051] Furthermore, the organic solvent is removed by applying a varnish to the substrate and heating it at a temperature of usually 80°C or higher, preferably 100°C or higher, for 0.5 to 5 hours, and the material to be bonded to the substrate is pressed while being heated, and then heated at a temperature of 130°C or higher, preferably 150°C or higher, for 0.5 to 10 hours to bond the material.
[0052] Examples of methods for applying the styrene-based elastomer composition solution (varnish) include ordinary coating methods and printing methods. Specifically, coating methods such as air doctor coating, bar coating, blade coating, knife coating, reverse coating, transfer roll coating, gravure roll coating, kiss coating, cast coating, spray coating, slot orifice coating, calendar coating, dam coating, dip coating, and die coating, as well as printing methods such as intaglio printing such as gravure printing, and stencil printing such as screen printing, can be used. EXAMPLES
[0053] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0054] The components used in the examples and comparative examples are shown below.
[0055] (A) Styrene-based elastomer (A-1) Amine-modified styrene / ethylene / butylene / styrene block copolymer, hydrogenated, styrene content 30% (Tuftec MP10: Asahi Kasei Corporation) (A-2) Carboxylic acid modified styrene / ethylene / butylene / styrene block copolymer, styrene content 30% (Tuftec M1913: Asahi Kasei Corporation) (A-3) Styrene / ethylene / butylene / styrene block copolymer, styrene content 30% (Tuftec H1041: manufactured by Asahi Kasei Corporation)
[0056] (B) Maleimide Compound (B-1): A bismaleimide compound represented by the following formula (SLK-1500, manufactured by Shin-Etsu Chemical Co., Ltd.) [ka] m≒2 (average value) (B-2): Bismaleimide compound represented by the following formula (SLK-3000, manufactured by Shin-Etsu Chemical Co., Ltd.) [ka] m≒5 (average value) (B-3): 4,4'-diphenylmethane bismaleimide (BMI-1000: manufactured by Daiwa Chemical Industry Co., Ltd., for comparison)
[0057] (C)Organic peroxide (C-1): Dicumyl peroxide (Percumyl D: manufactured by NOF Corp.)
[0058] (D) Adhesive assistant (D-1): 3-methacryloxypropyltrimethoxysilane (KBM-503: manufactured by Shin-Etsu Chemical Co., Ltd.)
[0059] <Preparation of varnish, appearance and stability of varnish> The components according to the formulations in Tables 1 and 2 were placed in a 500 mL four-neck flask equipped with a Dimroth condenser and a stirrer, and stirred at 50° C. for 2 hours to obtain a varnish-like resin composition.
[0060] [Table 1]
[0061] [Table 2]
[0062] <Appearance of varnish> Regarding the varnish before being made into a film, when there was no visible residue or turbidity, and a 30 mass% xylene solution of the resin composition was placed in a quartz cell, and the direct light transmittance at 740 nm with an optical path length of 1 mm was measured at 25°C using a spectrophotometer U-4100 (manufactured by Hitachi High-Tech Science Corp.), those with a direct light transmittance of 50% or more were marked with an O, and those with visible residue or turbidity and a direct light transmittance of less than 50% were marked with an X.
[0063] From the results of Tables 1 and 2, it was confirmed that the varnish compositions of Examples 1 to 11 were stable with no separation or turbidity in terms of varnish appearance. The stability of the varnish compositions was also confirmed in Comparative Examples 1 and 3. On the other hand, the varnishes of Comparative Examples 2 and 4 were turbid.
[0064] <Preparation of uncured resin film> The varnish-like styrene-based elastomer composition was applied to a 38 μm-thick PET film using a roller coater so that the thickness after drying would be 50 μm, and then dried at 120° C. for 10 minutes to obtain an uncured resin film.
[0065] <Handling of uncured resin film> The uncured resin film was visually inspected for cracks or breakage when it was bent 90 degrees at 25° C. When no cracks, breaks, tacks, etc. were observed, it was marked with an ◯, and when even a small amount of cracks, breaks, tacks, etc. were observed, it was marked with an ×.
[0066] From the results of Tables 1 and 2, it was confirmed that there were no cracks or breaks in the uncured resin film properties of Examples 1 to 11. Similarly to the Examples, no cracks or the like were confirmed in Comparative Examples 1 and 3. On the other hand, the occurrence of cracks and tack was observed in Comparative Examples 2 and 4. Further evaluation of Comparative Examples 2 and 4 was discontinued.
[0067] <Dielectric constant, dielectric loss tangent> The uncured resin film was cured at 180° C. for 2 hours, and the resulting resin film was cut to prepare a 60 mm×60 mm test piece. The dielectric constant and dielectric loss tangent of the obtained test piece were measured at 10 GHz and 28 GHz at 25° C. using an SPDR dielectric resonator (MS46122B, manufactured by Anritsu Corporation).
[0068] <Peel strength> A slide glass having a length of 75 mm, a width of 25 mm, and a thickness of 1.0 mm was prepared, and the resin composition side of the uncured film with the PET film, on one surface of the slide glass, without the PET substrate attached, was placed, and lamination was performed under the conditions of a temperature of 120°C, a pressure of 0.3 MPa, and a time of 60 seconds. After lamination, the PET substrate was peeled off, and a copper foil having a thickness of 18 μm (manufactured by Mitsui Kinzoku Co., Ltd., Ra 0.6 μm), an LCP having a thickness of 50 μm (manufactured by Chiyoda Integre Co., Ltd.) or an MPI (PIXEO SR, manufactured by Kaneka Corporation) was placed on the resin composition surface, and lamination was performed under the conditions of a temperature of 120°C, a pressure of 0.3 MPa, and a time of 60 seconds. After lamination, an adhesion test piece was prepared by curing at a temperature of 180°C for 2 hours.
[0069] To evaluate the adhesion, the 90° peel strength (kN / m) was measured when peeling the copper foil, LCP, or MPI of each adhesive test piece from the slide glass at a temperature of 23°C and a tensile speed of 50 mm / min in accordance with JIS-C-6481 "Test methods for copper-clad laminates for printed wiring boards."
[0070] The above evaluation results are shown in Tables 3 and 4.
[0071] [Table 3]
[0072] [Table 4]
[0073] From the above results, the styrene-based elastomer composition of the present invention is free from separation or turbidity of the varnish, has excellent dielectric properties after curing, and exhibits high adhesive strength to metals and organic resins, and therefore, it has been confirmed that the composition is useful as an insulating material suitable for circuit board applications.
Claims
1. (A) styrene-based elastomer: 100 parts by mass, (B) 1 to 50 parts by mass of a maleimide compound having at least one dimer acid skeleton in one molecule, which is represented by the following formula (1): [Formula 1] (In formula (1), A is independently a tetravalent organic group having a cyclic structure, B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms; Q is independently represented by the following formula (2): [chemical 2] (In formula (2), R 1 are independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and x1 and x2 are each independently a number from 0 to 10. is a divalent alicyclic hydrocarbon group having 6 to 60 carbon atoms and a cyclohexane skeleton represented by W is B or Q; n is 0 to 100, m is 0 to 200, but n and m are not 0 at the same time; The order of the repeating units bracketed by n and m is not limited, and the bonding pattern may be alternating, block, or random. (C) Organic peroxide: 0.01 to 10 parts by mass A styrene-based elastomer composition comprising:
2. 2. The styrene-based elastomer composition according to claim 1, wherein the styrene-based elastomer of component (A) is a copolymer of styrene and a compound having a carbon-carbon double bond.
3. 2. The styrene-based elastomer composition according to claim 1, wherein A in formula (1) is any one of tetravalent organic groups represented by the following structural formulas: [C3] (The bond not bonded to a substituent in the above structural formula is bonded to the carbonyl carbon that forms a cyclic imide structure in formula (1).)
4. The styrene-based elastomer composition according to claim 1, further comprising an adhesion promoter as component (D).
5. An uncured resin film comprising the styrene-based elastomer composition according to claim 1.
6. A cured resin film comprising the cured product of the styrenic elastomer composition according to claim 1.
7. An adhesive film comprising the styrene-based elastomer composition according to claim 1.
8. An adhesive comprising the styrene-based elastomer composition according to claim 1.
9. A sealing material comprising the styrene-based elastomer composition according to claim 1.
10. A substrate having the cured product of the styrenic elastomer composition according to claim 1.
Citation Information
Patent Citations
Thermosetting cyclic imide resin composition
JP2022111423A
Curable resin laminate, dry film, cured product, and electronic component
JP2022157695A
Fluororesin substrate laminate and method for manufacturing fluororesin substrate laminate
JP2022170140A
Heat-curable maleimide resin composition, film, prepreg, laminate and printed-wiring board
JP2023067340A