Anode active material particles, anode active material layer, solid-state battery, and method for manufacturing anode active material particles

By incorporating a metal and oxide portion with controlled crystallite sizes in negative electrode active material particles, the cycle performance of solid-state batteries is improved, addressing the need for enhanced durability.

JP2024160785APending Publication Date: 2024-11-15TOYOTA JIDOSHA KK +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023076141
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Solid-state batteries require improved cycle characteristics to enhance their performance and durability.

Method used

The development of negative electrode active material particles comprising a metal portion and an oxide portion, with specific crystallite sizes, produced through mechanochemical treatment, which alleviates expansion and contraction, thereby reducing mechanical deterioration.

Benefits of technology

The solution provides negative electrode active material particles with high cycle characteristics, enhancing the stability and longevity of solid batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160785000001_ABST
    Figure 2024160785000001_ABST
Patent Text Reader

Abstract

To provide negative electrode active material particles capable of realizing high cycle characteristics, a solid-state battery having such negative electrode active material particles, and a method for manufacturing such negative electrode active material particles.SOLUTION: Negative electrode active material particles according to the present disclosure include a metal portion and an oxide portion of this metal in the particles, and in particular, the metal portion has an average crystallite size of 50 to 200 nm, and the metal oxide portion has an average crystallite size of 30 nm or less. A solid-state battery according to the present disclosure has a negative electrode active material layer according to the present disclosure. The negative electrode active material layer according to the present disclosure includes the negative electrode active material particles according to the present disclosure and a solid electrolyte. A method for manufacturing the negative electrode active material particles according to the present disclosure includes mechanochemically treating metal suboxide particles to obtain the metal portion and the oxide portion of this metal.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to negative electrode active material particles, a negative electrode active material layer, a solid-state battery, and a method for producing negative electrode active material particles. [Background technology]

[0002] Patent Document 1 discloses a negative electrode composite material including a sulfide-based solid electrolyte containing lithium, phosphorus, and sulfur, and a negative electrode active material made of a metal powder containing at least one element selected from Groups 13 and 14 of the periodic table. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-003679 A Summary of the Invention [Problem to be solved by the invention]

[0004] There is a demand for solid-state batteries to have high cycle characteristics.

[0005] An object of the present disclosure is to provide negative electrode active material particles capable of realizing high cycle characteristics, a solid-state battery having such negative electrode active material particles, and a method for producing such negative electrode active material particles. [Means for solving the problem]

[0006] The present inventors have discovered that the above problems can be solved by the following means.

[0007] <Embodiment 1> Negative electrode active material particles including a metal portion and an oxide portion of the metal. <Aspect 2> The negative electrode active material particles according to aspect 1, wherein the metal portion has an average crystallite size of 50 to 200 nm, and the metal oxide portion has an average crystallite size of 30 nm or less. <Aspect 3> 3. The negative electrode active material particle according to claim 1 or 2, wherein the metal portion is a tin metal portion and the metal oxide portion is a tin dioxide portion. <Aspect 4> A negative electrode active material layer comprising the negative electrode active material particles according to any one of aspects 1 to 3 and a solid electrolyte. <Aspect 5> A solid-state battery having the negative electrode active material layer according to embodiment 4. Aspect 6 3. A method for producing anode active material particles according to aspect 1 or 2, comprising mechanochemically treating metal suboxide particles to obtain a metal portion and an oxide portion of the metal. Aspect 7 7. The method of embodiment 6, wherein the mechanochemical treatment is carried out by ball milling. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide negative electrode active material particles that can achieve high cycle characteristics. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a graph showing X-ray diffraction (XRD) patterns of the negative electrode active material particles (SnO(MC)), tin monoxide (SnO), tin (Sn), and tin dioxide (SnO 2 ) of the present disclosure. [Diagram 2] FIG. 2 is an image showing a high-resolution transmission electron microscope (TEM) image of the negative electrode active material particles of the present disclosure and a fast Fourier transform (FFT) pattern of each region. [Diagram 3] FIG. 3 is a graph showing (a) an electron beam diffraction pattern and (b) an intensity profile for the negative electrode active material particles of the present disclosure. [Figure 4] FIG. 4 is a graph showing (a) a dark field image of the Sn region and (b) the crystallite size distribution quantified by image analysis for negative electrode active material particles of the present disclosure. [Diagram 5]FIG. 5 is a graph showing (a) a dark field image of the SnO 2 region and (b) the crystallite size distribution quantified by image analysis for a negative electrode active material particle of the present disclosure. [Figure 6] FIG. 6 is a graph showing charge / discharge curves when Sn is used as the negative electrode active material particles. [Figure 7] FIG. 7 is a graph showing charge / discharge curves when untreated SnO was used as the negative electrode active material particles. [Figure 8] FIG. 8 is a graph showing charge / discharge curves when mechanochemically treated SnO is used as the negative electrode active material particles. [Figure 9] FIG. 9 is a graph showing the changes in charge / discharge capacity and Coulombic efficiency over cycles when Sn was used as the negative electrode active material particles. [Figure 10] FIG. 10 is a graph showing the changes in charge / discharge capacity and Coulombic efficiency with cycling when untreated SnO was used as the negative electrode active material particles. [Figure 11] FIG. 11 is a graph showing the changes in charge / discharge capacity and Coulombic efficiency with cycling when mechanochemically treated SnO was used as the negative electrode active material particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0011] 《Negative electrode active material particles》 The negative electrode active material particles of the present disclosure contain a metal portion and an oxide portion of this metal within the particles, particularly within the primary particles.

[0012] Preferably, in the negative electrode active material particles of the present disclosure, the average crystallite size of the metal portion is 50 to 200 nm, and the average crystallite size of the metal oxide portion is 30 nm or less. In the measurement of the average crystallite size of the present disclosure, an XRD pattern of the negative electrode active material particles is measured using an X-ray diffraction device, the crystalline phase in the negative electrode active material particles is identified, and a high-resolution image is obtained using a transmission electron microscope (TEM), and a dark-field image is obtained by selecting the Debye rings of the metal and the oxide of this metal, and the crystallite size of each crystal image can be estimated from the dark-field image.

[0013] The present inventors have found that high cycle characteristics can be achieved by using particles containing a metal portion and an oxide portion of this metal as negative electrode active material particles. Without intending to be bound by any theory, the reason for this is believed to be that in the negative electrode active material particles of the present disclosure, the combination of a metal portion and an oxide portion of this metal alleviates the expansion and contraction caused by the insertion and removal of lithium ions inside the particles, and mechanical deterioration such as peeling and cracking that occurs in the negative electrode active material layer is suppressed.

[0014] The negative electrode active material particles of the present disclosure contain a metal portion and an oxide portion of this metal within the particle, particularly within the primary particle.

[0015] (Metal parts) In the present disclosure, the metal portion refers to a region made of a metal in the negative electrode active material particle. Examples of the metal include tin (Sn), silicon (Si), and silver (Ag), and the metal is preferably tin.

[0016] The average crystallite size of the metal portion is preferably 50 to 200 nm, and may be 60 nm or more, 70 nm or more, 80 nm or more, 90 nm or more, 100 nm or more, 110 nm or more, 120 nm or more, or 130 nm or more, and may be 190 nm or less, 180 nm or less, 170 nm or less, 160 nm or less, 150 nm or less, or 140 nm or less.

[0017] (metal oxide part) In the present disclosure, the metal oxide portion refers to a region made of the same metal oxide as the metal portion in the negative electrode active material particle. Examples of the metal oxide include tin dioxide (SnO2), silicon dioxide (SiO2), and silver(III) oxide (Ag2O3), and the metal oxide is preferably tin dioxide.

[0018] The average crystallite size of the metal oxide portion is preferably 30 nm or less. This average crystallite size may be 1 nm or more, 3 nm or more, 5 nm or more, 7 nm or more, 9 nm or more, 10 nm or more, 11 nm or more, 12 nm or more, or 13 nm or more, and may be 25 nm or less, 20 nm or less, 18 nm or less, 16 nm or less, 15 nm or less, or 14 nm or less.

[0019] <<Method for producing negative electrode active material particles>> The disclosed method of making negative electrode active material particles includes mechanochemically treating metal suboxide particles to obtain a metal portion and an oxide portion of the metal.

[0020] In the present disclosure, the metal suboxide particles refer to particles having an intermediate degree of oxidation between the metal portion and the oxide portion of this metal. Examples of the metal suboxide particles include tin monoxide (SnO), silicon monoxide (SiO), and silver (I) oxide (Ag20), and preferably tin monoxide.

[0021] The mechanochemical treatment can be carried out by a ball mill. When the mechanochemical treatment is carried out by a ball mill, the rotation speed of the ball mill can be 100 rpm or more, 200 rpm or more, or 300 rpm or more. The treatment time can be 1 hour or more, 10 hours or more, or 30 hours or more.

[0022] 《Negative electrode active material layer》 In the present disclosure, the negative electrode active material layer includes negative electrode active material particles and a solid electrolyte, and optionally a conductive assistant and a binder.

[0023] <Negative electrode active material particles> For the negative electrode active material particles, reference can be made to the above description of the negative electrode active material particles of the present disclosure.

[0024] <Solid electrolyte> Examples of solid electrolytes include sulfide amorphous solid electrolytes, such as Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, and Li2S-P2S5; sulfide crystalline solid electrolytes, such as Li7P3S 11 , Li3PS4, and Li 3.25 P 0.75 S4, etc.; as well as combinations thereof.

[0025] <Conductive assistant> Examples of the conductive assistant include carbon materials such as VGCF (Vapor Grown Carbon Fiber), carbon black, acetylene black (AB), Ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF), as well as metal materials, and combinations thereof.

[0026] <binder> Binders can include, but are not limited to, polymer resins such as polyvinylidene fluoride (PVDF), acrylonitrile butadiene rubber (ABR), and styrene butadiene rubber (SBR), as well as combinations thereof.

[0027] 《Solid-state battery》 In the present disclosure, the solid-state battery has the negative electrode active material layer of the present disclosure. The solid-state battery of the present disclosure may have a negative electrode current collector layer, a negative electrode active material layer, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer in this order. Each layer constituting the solid-state battery of the present disclosure will be described below.

[0028] In the present disclosure, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. Also, the solid-state battery of the present disclosure may be an all-solid-state battery, i.e., a battery that uses only a solid electrolyte as an electrolyte.

[0029] <Negative electrode current collector layer> Examples of the negative electrode current collector layer include, but are not limited to, various metals such as silver, copper, gold, aluminum, nickel, iron, stainless steel, and titanium, as well as alloys thereof.

[0030] <Negative electrode active material layer> For the negative electrode active material layer, reference can be made to the above description regarding the negative electrode active material layer of the present disclosure.

[0031] <Solid electrolyte layer> The solid electrolyte layer contains a solid electrolyte and, optionally, a binder. For the solid electrolyte and binder of the solid electrolyte layer, reference can be made to the above description of the negative electrode active material layer of the present disclosure.

[0032] <Cathode active material layer> The positive electrode active material layer contains positive electrode active material particles and a solid electrolyte, and optionally a conductive assistant and a binder.

[0033] Examples of the positive electrode active material particles include lithium metal oxide particles containing at least one transition metal selected from manganese, cobalt, nickel, and titanium and lithium, such as lithium cobalt oxide (Li x CoO2) particles, lithium nickel oxide (LiNO2) particles, lithium manganese oxide (LiMn2O4) particles, Li 1+x M y Mn 2-x-y Lithium manganese oxide and lithium titanate (LiO4 (M=Al, Mg, Fe, Cr, Co, Ni, Zn)) are spinel-type materials substituted with different elements. x TiO y), lithium metal phosphate (LiMPO4: M = Fe, Mn, Co, Ni), and lithium nickel cobalt manganese oxide (Li 1+x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2) particles, etc., as well as combinations thereof.

[0034] For the solid electrolyte, conductive assistant, and binder of the positive electrode active material layer, the above descriptions regarding the negative electrode active material layer of the present disclosure can be referred to.

[0035] <Positive electrode current collector layer> For the positive electrode current collector layer, reference may be made to the above description regarding the negative electrode current collector layer of the present disclosure. EXAMPLES

[0036] <<Preparation of sample>> <Preparation of negative electrode active material particles> The SnO powder was placed in a zirconium oxide (ZrO2) pot together with balls made of ZrO2, and subjected to mechanochemical (MC) treatment using a planetary ball mill at 370 rpm for 40 hours to produce negative electrode active material particles.

[0037] (Preparation of sulfide solid electrolyte) Lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) were weighed out in a ratio of 75 mol%:25 mol%, and a sulfide solid electrolyte was produced by mechanochemical treatment.

[0038] <Preparation of negative electrode mixture> The negative electrode active material particles, the sulfide solid electrolyte, and acetylene black were weighed out to a weight ratio of 8:10:1 and mixed in a mortar to prepare a negative electrode composite. For comparison, negative electrode composites using simple Sn and SnO that had not been subjected to mechanical treatment were also prepared in the same manner.

[0039] <Preparation of Evaluation Cell> 9.5 mg of the negative electrode composite and 80 mg of the sulfide solid electrolyte were placed in a cylindrical container of 10 mmΦ and stacked, and the stack was uniaxially pressurized, after which lithium foil and indium foil were attached to prepare an evaluation cell (Example). For comparison, cells using negative electrode composites made of simple Sn (Comparative Example 1) and SnO without mechanical treatment (Comparative Example 2) were also prepared in the same manner.

[0040] "evaluation" Evaluation of negative electrode active material particles The XRD patterns of the negative electrode active material particles were measured using an X-ray diffractometer, and the crystalline phases in the negative electrode active material particles were identified. In addition, high-resolution images were obtained using a transmission electron microscope (TEM), and dark-field images were obtained by selecting the Debye rings of Sn and SnO2, and the crystallite sizes of each crystal were estimated from the dark-field images.

[0041] <Cycle characteristic evaluation> The evaluation cell thus fabricated had a current density of 0.13 mA / cm at 25°C and in the potential range of -0.62 to 1.38 V vs. Li-In. 2 Constant current charge / discharge measurements were performed under the following conditions.

[0042] "result" <Confirmation of the presence of Sn and SnO2 in particles> The XRD patterns of the prepared negative electrode active material particles (SnO(MC)), SnO, Sn, and SnO2 are shown in Figure 1. As shown in Figure 1, the negative electrode active material particles obtained by the mechanochemical treatment contained two phases, Sn and SnO2.

[0043] <Confirmation of the state of Sn and SnO2 in particles> A high-resolution TEM image of the produced negative electrode active material particles and the fast Fourier transform (FFT) patterns of each region are shown in Figure 2. As shown in Figure 2, Sn and SnO2 within the particles were highly dispersed at the nano level.

[0044] Average crystallite size of Sn and SnO2 The average crystallite sizes of Sn and SnO2 were estimated from the dark-field images. The electron beam diffraction pattern and its intensity profile obtained from the prepared negative electrode active material particles are shown in Figure 3. The peaks in this intensity profile correspond to the diffraction from each crystalline phase. Based on these peaks, Debye rings consisting of diffraction from only Sn and only SnO2 were selected and dark-field images were obtained. The distribution of crystallite sizes quantified by dark-field images and image analysis is shown in Figures 4 and 5. As shown in Figures 4 and 5, Sn had an average crystallite size of about 130 nm, and SnO2 had an average crystallite size of about 13 nm.

[0045] <Cycle characteristics> Charge / discharge curves of evaluation cells using mechanochemically treated SnO (negative electrode active material particles of the present disclosure), as well as simple Sn and SnO without mechanochemical treatment for comparison, are shown in Figures 6 to 8. Changes in charge / discharge capacity and Coulombic efficiency with cycling are shown in Figures 9 to 11. As shown in Figures 6 to 8 and 9 to 11, when mechanochemically treated SnO (negative electrode active material particles of the present disclosure) was used, the decrease in charge capacity with cycling was suppressed compared to when simple Sn and SnO without mechanochemical treatment were used.

[0046] The initial charge capacity, the charge capacity after 20 cycles, and the capacity retention rate after 20 cycles for the cells of the Example and Comparative Example are shown in Table 1. As shown in Table 1, the cycle characteristics of the cell of the Example were higher than that of the cell of the Comparative Example.

[0047] [Table 1]

Claims

1. A negative electrode active material particle comprising a metal portion and an oxide portion of the metal.

2. 2. The negative electrode active material particle according to claim 1, wherein the metal portion has an average crystallite size of 50 to 200 nm, and the metal oxide portion has an average crystallite size of 30 nm or less.

3. 3. The negative electrode active material particle according to claim 1, wherein the metal portion is a metallic tin portion, and the metal oxide portion is a tin dioxide portion.

4. An anode active material layer comprising the anode active material particles according to claim 1 and a solid electrolyte.

5. A solid-state battery comprising the negative electrode active material layer according to claim 4.

6. The method for producing anode active material particles according to claim 1 or 2, comprising mechanochemically treating metal suboxide particles to obtain the metal portion and the metal oxide portion.

7. The method according to claim 6, wherein the mechanochemical treatment is carried out by ball milling.

Citation Information

Patent Citations

  • Negative electrode active material for lithium ion secondary battery and production method therefor and lithium ion secondary battery

    JP2013093259A

  • Composite negative electrode active material body, negative electrode for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery

    JP2015125817A

  • Positive electrode active material for all-solid-state lithium ion batteries, electrode and all-solid-state lithium ion battery

    WO2021145444A1