Lithium ion secondary battery
The lithium ion battery with a magnesium-doped lithium cobalt oxide and fluorinated electrolyte, combined with a protective film from vinylene carbonate, addresses discharge capacity and reliability issues, enabling operation from sub-zero to high temperatures.
Patent Information
- Application Number
- JP2023076161
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-11-15
AI Technical Summary
Lithium ion secondary batteries face challenges in discharge capacity, cycle characteristics, reliability, safety, and cost, with a need for improved performance across a wide temperature range, including sub-zero to high temperatures.
A lithium ion battery design incorporating a positive electrode active material with lithium cobalt oxide containing magnesium, a fluorinated cyclic or chain carbonate electrolyte, and vinylene carbonate as an additive to form a protective film, preventing magnesium elution and enhancing stability.
The design suppresses capacity degradation, improves safety, and allows charging and discharging over a wide temperature range, reducing deterioration and enhancing reliability.
Smart Images

Figure 2024160794000001_ABST
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to a lithium-ion secondary battery.
[0002] One embodiment of the present invention is not limited to the above fields, and relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, a vehicle, and a manufacturing method thereof. The above-mentioned semiconductor device, display device, light-emitting device, power storage device, lighting device, electronic device, and vehicle can use the lithium-ion secondary battery of one embodiment of the present invention as a necessary power source. For example, the above-mentioned electronic device includes an information terminal device equipped with a lithium-ion secondary battery. Furthermore, the above-mentioned power storage device includes a stationary power storage device.
[0003] A lithium-ion secondary battery (sometimes written as lithium-ion battery) is a battery that uses lithium ions as the carrier ion. Lithium-ion batteries are secondary batteries that can be used repeatedly by charging and discharging. [Background technology]
[0004] In recent years, various types of power storage devices have been actively developed, such as lithium-ion secondary batteries, lithium-ion capacitors, air batteries, all-solid-state batteries, etc. In particular, the demand for high-output, high-capacity lithium-ion secondary batteries has rapidly expanded in line with the development of the semiconductor industry, and they have become indispensable in the modern information society as a rechargeable energy source.
[0005] In particular, there is a high demand for secondary batteries with large discharge capacity per weight and excellent cycle characteristics for mobile electronic devices, etc. In order to meet this demand, active improvements have been actively made to the positive electrode active material of the positive electrode of secondary batteries (e.g., Patent Documents 1 to 3).
[0006] In addition, it is desired that lithium-ion batteries can be charged and discharged over a wide temperature range depending on the application. Therefore, research and development to enable charging and discharging of lithium-ion batteries at high or low temperatures is actively conducted. In addition, Non-Patent Document 1 proposes an electrolyte containing 3,3,3-methyl trifluoropropionate (MTFP):fluoroethylene carbonate (FEC) mixed at a ratio of 9:1 to improve output characteristics below freezing point. In addition, Non-Patent Document 2 reports the crystal structure of the positive electrode active material. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-179758 A [Patent Document 2] WO2020 / 026078 Brochure [Patent Document 3] Patent Publication No. 2022-070247 [Non-patent literature]
[0008] [Non-Patent Document 1] John, H. et al, “An All-Fluorinated Ester Electrolyte for Stable High-Voltage Li Metal Batteries Capable of Ultra-Low-Temperature Operation”, ACE Energy LETTERS, 2020, 5, 1438-1447 [Non-Patent Document 2] Zhaohui Chen et al, “Staging Phase Transitions in LixCoO2”, Journal of The Electrochemical Society, 2002, 149(12) A1604-A1609 Summary of the Invention [Problem to be solved by the invention]
[0009] Lithium ion secondary batteries have room for improvement in various aspects, such as discharge capacity, cycle characteristics, reliability, safety, and cost.
[0010] An object of one embodiment of the present invention is to provide a secondary battery in which a decrease in charge / discharge capacity during charge / discharge cycles is suppressed.Another object is to provide a secondary battery that has a large charge / discharge capacity and is safe or highly reliable.Another object is to provide a positive electrode active material or composite oxide that can be used in a lithium ion secondary battery and in which a decrease in discharge capacity during charge / discharge cycles is suppressed.Another object is to provide a positive electrode active material or composite oxide whose crystal structure is not easily destroyed even after repeated charge / discharge.Another object is to provide a positive electrode active material or composite oxide that has a large charge / discharge capacity.
[0011] Another object of one embodiment of the present invention is to provide a positive electrode active material, a composite oxide, a power storage device, or a manufacturing method thereof.
[0012] Another object of one embodiment of the present invention is to provide a lithium-ion battery including a new electrolyte and a new positive electrode active material so that the battery can be charged and discharged in a wide temperature range including from below freezing to high temperatures. [Means for solving the problem]
[0013] One embodiment of the present invention is a lithium ion secondary battery including a positive electrode having a positive electrode active material, an electrolyte, and a negative electrode having graphite, in which the positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in a surface layer portion of the positive electrode active material is higher than the magnesium concentration inside the positive electrode active material, and the electrolyte includes a fluorinated cyclic carbonate or a fluorinated chain carbonate, and vinylene carbonate (VC) is added to the electrolyte.
[0014] In the above configuration, the positive electrode active material is lithium cobalt oxide further containing aluminum, nickel, and fluorine. The electrolyte contains a fluorinated cyclic carbonate or a fluorinated chain carbonate, so that the fluorine contained in the electrolyte repels the fluorine on the outermost surface of the positive electrode active material, and the fluorine can be retained on the outermost surface of the positive electrode active material. Therefore, the fluorine on the surface of the positive electrode active material can be suppressed, and the elution of magnesium can be prevented.
[0015] When vinylene carbonate is used as an additive and charging and discharging are performed, a coating (Solid Electrolyte Interphase: SEI film) is formed on at least a part of the interface between the negative electrode (graphite) and the electrolyte. In addition, when vinylene carbonate is used as an additive and charging and discharging are performed, a coating (also called a protective layer or coating layer) is also formed on the surface of the positive electrode active material. At least a part of the interface between the positive electrode active material and the electrolyte has a coating. The coating of the positive electrode active material formed can prevent magnesium from eluting. The coating of the positive electrode active material includes a deposit of decomposition products of the electrolyte (including lithium salt). Therefore, an electrolyte containing a fluorinated cyclic carbonate or a fluorinated chain carbonate and to which vinylene carbonate (VC) is added can obtain a synergistic effect with lithium cobalt oxide containing magnesium. The amount of vinylene carbonate added is 0.1% by weight or more and 5% by weight or less based on the total weight of the electrolyte. In addition, the graphite coating or the coating of the positive electrode active material can be analyzed by LCMS, GC-MS, NMR (e.g. 1 1 H NMR) can be used to characterize the compound.
[0016] <Analytical methods for electrolytes> The composition of the electrolyte can be confirmed using X-ray Photoelectron Spectroscopy (XPS), Gas Chromatography-Mass Spectrometry (GC-MS), Liquid Chromatography Mass Spectrometry (LC-MS), Ion Chromatography (IC), Inductively Coupled Plasma Atomic Emission Spectroscopy (ICP-AES), Atomic Absorption Spectrometry (AAS), Glow Discharge Mass Spectrometry (GD-MS), Nuclear Magnetic Resonance (NMR), Fourier Transform Infrared Spectroscopy (FT-IR), etc.
[0017] <Analysis by GC-MS> When using GC-MS, the structural formula of the compounds contained in the electrolyte can be specified. The electrolyte may be recovered from a secondary battery. When recovering the electrolyte, it is preferable to disassemble the secondary battery in a glove box under an argon atmosphere to take out the electrolyte. Further, when the amount of the electrolyte contained in the secondary battery is small, a solvent that does not affect the GC-MS analysis may be poured into the secondary battery, and a liquid in which the solvent and the electrolyte are mixed may be taken out. It is preferable to use deuterated acetonitrile as the solvent. The apparatus used for the analysis is not particularly limited, but for example, it can be the following apparatus. Also, when the following apparatus is used, a structural formula with a degree of coincidence (Hit%) with reference data of 80% or more, preferably 90% or more, and more preferably 93% or more can be adopted as the structural formula of the compounds contained in the electrolyte. Apparatus name: Agilent Technologies 7890A GC System Agilent Technologies 5975C inert MSD
[0018] <Analysis by LC-MS> When using LC-MS, the structural formula of the compounds contained in the electrolyte can be identified. The electrolyte may be recovered from a secondary battery. When recovering the electrolyte, it is preferable to disassemble the secondary battery in a glove box under an argon atmosphere to take out the electrolyte. Further, when the amount of the electrolyte contained in the secondary battery is small, a solvent that does not affect the LC-MS analysis may be poured into the secondary battery, and a liquid in which the solvent and the electrolyte are mixed may be taken out. It is preferable to use deuterated acetonitrile as the solvent. The apparatus and conditions used for the analysis are not particularly limited, but for example, the following apparatus and conditions can be adopted. Also, when using the following apparatus, a structural formula with a degree of coincidence with the reference data of 80% or more, preferably 90% or more, more preferably 93% or more can be adopted as the structural formula of the compound contained in the electrolyte. Name of LC apparatus: Waters Acquity UPLC Name of MS apparatus: Waters Xevo QTof MS
[0019] In this specification and the like, "below the freezing point" refers to 0°C or lower, "high temperature" refers to 25°C or higher, and "room temperature" refers to higher than 0°C and lower than 25°C. In this specification and the like, the "temperature range including from below the freezing point to high temperature" includes the above room temperature.
[0020] In this specification and the like, the "particles" used for active material particles and the like are not limited to referring only to spherical (circular cross-sectional shape). For example, the particles include those with an elliptical cross-sectional shape, an asymmetric shape, etc., and further, the individual particles do not have to be aligned and may be amorphous to each other.
[0021] The term "non-aqueous electrolyte" refers to an organic solvent that exhibits carrier ion conductivity, and generally refers to a liquid electrolyte, but is not limited to a liquid electrolyte in the present invention. Therefore, in the present specification and the like, the concept of a non-aqueous electrolyte is described as "electrolyte". That is, the electrolyte, which is one embodiment of the present invention, is not limited in its state, and includes, for example, an electrolyte whose viscosity has been increased from a liquid state as a result of adjusting the viscosity. Furthermore, the electrolyte also includes a solid state or a semi-solid state. The semi-solid state refers to an intermediate state between a liquid state and a solid state. Specific examples of semi-solid states include flexible solid states, and typically include gel-like electrolytes. Semi-solid electrolytes are generally referred to as semi-solid electrolytes, and the electrolyte, which is one embodiment of the present invention, also includes a semi-solid electrolyte. The above-mentioned liquid, solid, or semi-solid state, or viscosity, is confirmed when the lithium ion battery is placed at 25°C.
[0022] In this specification and the like, a value that indicates the magnitude of viscosity is called viscosity, and "appropriate viscosity" refers to having a viscosity that is appropriate for a lithium ion battery.
[0023] In this specification and the like, segregation of a certain element refers to a state in which a certain element (for example, A) is distributed non-uniformly in a solid composed of multiple elements (for example, A, B, C).
[0024] In this specification, the distribution of a certain element refers to the continuous presence of the element when the element is detected in a range that is not noise by any analytical method. The continuous change in the concentration of the element may be called a concentration gradient. The maximum value in the distribution may be called a peak. When identifying the peak, a distribution limited to a certain region may be targeted. The above-mentioned distribution is not limited to a normal distribution. When the distribution corresponds to a normal distribution, the half-width of the distribution may also be determined.
[0025] In this specification, uneven distribution means that the concentration of an element in a certain region is different from that in other regions. It is synonymous with uneven distribution or the mixture of high concentration areas and low concentration areas. The uneven distribution of an element through solid solution is called segregation. Effect of the Invention
[0026] According to one embodiment of the present invention, the fluorine contained in the electrolyte repels the fluorine on the outermost surface of the positive electrode active material, preventing the elution of magnesium from the positive electrode active material. In addition, by using vinylene carbonate (VC), a coating is also formed on the surface of the positive electrode active material, preventing the elution of magnesium from the positive electrode active material and suppressing the deterioration of the positive electrode active material. Furthermore, the formation of the coating can also suppress the decomposition of the electrolyte after the coating is formed. The combination of these factors produces a synergistic effect that can significantly reduce the deterioration of the secondary battery.
[0027] One aspect of the present invention allows charging and discharging over a wide temperature range, including from freezing to high temperatures.
[0028] According to one embodiment of the present invention, deterioration of a secondary battery can be suppressed and the reliability can be improved.
[0029] In addition, the aging treatment for forming a coating on the positive electrode active material can be shortened or omitted. The aging treatment is sometimes called initial charge / discharge or conditioning.
[0030] Note that the above-mentioned effects do not preclude the existence of other effects. In addition, the above-mentioned effects are considered to be independent of each other, and one embodiment of the present invention does not necessarily have to achieve all of the above-mentioned effects. Furthermore, effects other than those described above can be extracted from the description of this specification and the like. [Brief description of the drawings]
[0031] [Figure 1] 1(A) and 1(B) are diagrams illustrating a lithium-ion battery of one embodiment of the present invention. [Diagram 2] 2A to 2C illustrate a method for manufacturing a positive electrode of one embodiment of the present invention. [Diagram 3] 3A to 3F illustrate a positive electrode active material of one embodiment of the present invention. [Figure 4] FIG. 4 illustrates a crystal structure of a positive electrode active material of one embodiment of the present invention. [Diagram 5] FIG. 5 is a diagram illustrating the crystal structure of the positive electrode active material. [Figure 6] FIG. 6 is a diagram illustrating the diffraction peaks of the positive electrode active material. [Figure 7] FIG. 7 is a diagram illustrating the diffraction peaks of the positive electrode active material. [Figure 8] 8(A) and 8(B) are diagrams illustrating the diffraction peaks of the positive electrode active material. [Figure 9] 9A to 9D illustrate a positive electrode of one embodiment of the present invention. [Figure 10] 10A and 10B are diagrams illustrating a lithium-ion battery of one embodiment of the present invention. [Figure 11] 11A to 11C illustrate a lithium-ion battery of one embodiment of the present invention. [Figure 12] 12A to 12D illustrate a lithium-ion battery and a power storage system of one embodiment of the present invention. [Figure 13] 13A to 13C illustrate a lithium-ion battery of one embodiment of the present invention. [Figure 14] 14A to 14C illustrate a lithium-ion battery of one embodiment of the present invention. [Figure 15] 15A to 15C are diagrams illustrating an electric vehicle of one embodiment of the present invention. [Figure 16] 16(A) to 16(D) are diagrams illustrating a transportation vehicle according to one embodiment of the present invention. [Figure 17] 17A to 17C are diagrams illustrating a two-wheeled vehicle and the like according to one embodiment of the present invention. [Figure 18] 18A to 18D illustrate electronic devices or the like according to one embodiment of the present invention. [Figure 19] 19(A) to 19(D) are diagrams showing an example of space equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be easily understood by those skilled in the art that the form and details of the present invention can be modified in various ways. Furthermore, the present invention is not to be interpreted as being limited to the description of the embodiments shown below.
[0033] (Embodiment 1) In this embodiment, a lithium-ion battery which is one embodiment of the present invention will be described with reference to the drawings.
[0034] <Lithium-ion battery> A lithium ion battery according to one embodiment of the present invention has an electrolyte that allows charging and discharging in a wide temperature range including at least below freezing and even up to high temperatures. In addition to the electrolyte described above, the lithium ion battery has a negative electrode, a positive electrode, a separator between the negative electrode and the positive electrode, and an exterior body that covers the periphery of the negative electrode and the positive electrode. Depending on the form of the exterior body, the battery is called a laminated lithium ion battery, a coin cell lithium ion battery, or a cylindrical lithium ion battery, but the present invention is not limited to the form of the exterior body. The separator can be omitted when the electrolyte is solid or semi-solid.
[0035] 1A illustrates an example of the configuration of a lithium ion battery 100. In a cross-sectional view, the lithium ion battery 100 has a negative electrode 106, a separator 108, and a positive electrode 107. In the lithium ion battery 100, an electrolyte 109 is liquid, and the electrolyte 109 is present throughout the negative electrode 106, the separator 108, and the positive electrode 107. As described above, the electrolyte 109 is not limited to being liquid.
[0036] The negative electrode 106 includes a negative electrode current collector 101 and a negative electrode active material layer 102. The negative electrode active material layer 102 includes at least an active material and may include a conductive material and / or a binder. A known material can be used for the negative electrode active material, and details of the material will be described later. The positive electrode 107 includes a positive electrode current collector 105 and a positive electrode active material layer 104. The positive electrode active material layer 104 includes at least an active material and may include a conductive material and / or a binder. A known material may be used for the positive electrode active material, but the use of a positive electrode active material of one embodiment of the present invention can withstand high-voltage charging and increase the discharge capacity of a lithium-ion battery. The positive electrode active material of one embodiment of the present invention will be described later.
[0037] The conductive material has a function of supporting a current path between active materials and / or between the active material and the current collector. Any known material can be used as the conductive material, and details will be described later. The binder is also called a binding agent, and has a function of supporting adhesion between active materials and / or between the active material and the current collector. Any known material can be used as the binder, and details will be described later.
[0038] 1(B) illustrates a lithium ion battery 100 that does not have the negative electrode active material layer 102, unlike the lithium ion battery 100 in FIG. 1(A). The negative electrode active material layer 102 can be eliminated depending on the material of the negative electrode current collector 101. Other configurations of the lithium ion battery 100 in FIG. 1(B) are similar to those of the lithium ion battery 100 in FIG. 1(A), and therefore descriptions thereof will be omitted.
[0039] In this embodiment, a lithium ion battery having excellent discharge characteristics and / or excellent charge characteristics in a wide temperature range including temperatures from below freezing to high temperatures can be realized. The following description focuses on the configuration of the lithium ion battery required for this purpose. Specifically, the following description focuses on the positive electrode active material and the electrolyte. The details of the configuration of the lithium ion battery other than the positive electrode active material and the electrolyte will be described in the third embodiment and onwards.
[0040] <Cathode active material> The positive electrode active material has a function of taking in and / or releasing lithium ions, which are carrier ions, during charging and discharging. The positive electrode active material used in one embodiment of the present invention can be charged and discharged even at a high charging voltage (hereinafter also referred to as "high charging voltage") in a wide temperature range from below freezing to high temperatures, and can be made of a material that is less likely to deteriorate (or has less increase in resistance) during charging and discharging. Unless otherwise specified in this specification, the "charging voltage" is expressed based on the potential of lithium metal. In this specification, the "high charging voltage" refers to a charging voltage of, for example, 4.5V or more, preferably 4.6V or more, and more preferably 4.65V or more.
[0041] The positive electrode active material is not limited to one type, and two or more materials with different median diameters (D50) may be mixed, or two or more materials with different compositions may be mixed, as long as the materials are little deteriorated during charging and discharging even at high charging voltages over a wide temperature range including below freezing to high temperatures. In this specification, "different compositions" includes not only cases where the composition of elements contained in the materials is different, but also cases where the ratio of elements contained in the materials is different even if the composition of elements contained in the materials is the same.
[0042] As described above, in this specification, the "high charging voltage" is defined as 4.5 V or more based on the potential when the negative electrode is lithium metal, but when the potential when the negative electrode is a carbon material (e.g., graphite) is used as the reference, 4.4 V or more is called the "high charging voltage." In short, in the case of a half cell in which lithium metal is used as the negative electrode, a charging voltage of 4.5 V or more is called the high charging voltage, and in the case of a full cell in which a carbon material (e.g., graphite) is used as the negative electrode, a charging voltage of 4.4 V or more is called the high charging voltage.
[0043] The temperature during charging or discharging described in this specification refers to the temperature of the environment in which the lithium-ion battery is placed (hereinafter, sometimes referred to as "environmental temperature" in this specification). In measuring battery characteristics, a thermostatic bath that is stable at a desired temperature is used, so the environmental temperature is equal to the temperature of the thermostatic bath. After placing a test cell (e.g., a full cell or a half cell) to be measured in the thermostatic bath, measurement can be started after a sufficient time (e.g., one hour or more) has elapsed until the test cell reaches the same temperature as the thermostatic bath, but the measurement of battery characteristics is not necessarily limited to this method.
[0044] <Electrolytes> As the electrolyte used in one embodiment of the present invention, a material having excellent lithium ion conductivity in a wide temperature range including from below freezing to high temperatures can be used.
[0045] The electrolyte has an organic solvent, but the organic solvent of the electrolyte according to one embodiment of the present invention is not limited to being liquid at 25° C., and may be solid at 25° C. or semi-solid at room temperature. The organic solvent of the electrolyte according to one embodiment of the present invention is preferably liquid in a wide temperature range including below freezing to high temperatures, but is not limited thereto. The organic solvent may be liquid, solid, or semi-solid in a wide temperature range including below freezing to high temperatures.
[0046] <Organic solvent> The organic solvent described in this embodiment may contain a fluorinated cyclic carbonate (sometimes referred to as a fluorinated cyclic carbonate) or a fluorinated chain carbonate (sometimes referred to as a fluorinated chain carbonate). Furthermore, the organic solvent preferably contains both a fluorinated cyclic carbonate and a fluorinated chain carbonate. Both the fluorinated cyclic carbonate and the fluorinated chain carbonate have a substituent that exhibits electron-withdrawing properties, and have a lower solvation energy of lithium ions than an organic compound that does not have a substituent that exhibits electron-withdrawing properties. Therefore, both the fluorinated cyclic carbonate and the fluorinated chain carbonate are suitable as organic solvents.
[0047] As the fluorinated cyclic carbonate, fluoroethylene carbonate (fluorinated ethylene carbonate, fluoroethylene carbonate, FEC, F1EC), difluoroethylene carbonate (DFEC, F2EC), trifluoroethylene carbonate (F3EC), or tetrafluoroethylene carbonate (F4EC) can be used. DFEC has isomers such as cis-4,5 and trans-4,5. Since all of the fluorinated cyclic carbonates have electron-withdrawing substituents, it is believed that the solvation energy of lithium ions is low.
[0048] The following structural formula (H10) is the structural formula of FEC, in which the electron-withdrawing substituent is an F group.
[0049] [ka]
[0050] Methyl 3,3,3-trifluoropropionate is an example of a fluorinated chain carbonate. The following structural formula (H22) is the structural formula of methyl 3,3,3-trifluoropropionate. The abbreviation for methyl 3,3,3-trifluoropropionate is "MTFP." In MTFP, the electron-withdrawing substituent is a CF3 group.
[0051] [ka]
[0052] An example of a fluorinated chain carbonate is trifluoromethyl 3,3,3-trifluoropropionate. The following structural formula (H23) is the structural formula of trifluoromethyl 3,3,3-trifluoropropionate. The electron-withdrawing substituent is a CF3 group.
[0053] [ka]
[0054] As a fluorinated chain carbonate, there is trifluoromethyl propionate. The following structural formula (H24) is the structural formula of trifluoromethyl propionate. The electron-withdrawing substituent is the CF3 group.
[0055] [Chemical formula]
[0056] As a fluorinated chain carbonate, there is methyl 2,2-difluoropropionate. The following structural formula (H25) is the structural formula of methyl 2,2-difluoropropionate. The electron-withdrawing substituent is the CF2 group.
[0057] [Chemical formula]
[0058] As the organic solvent of the electrolyte which is one aspect of the present invention, it is preferable to contain one or more selected from the above-mentioned fluorinated cyclic carbonates and fluorinated chain carbonates. For example, the organic solvent described in this embodiment may contain FEC or MTFP. The reason will be explained.
[0059] <FEC and MTFP> FEC is a cyclic carbonate and has a high relative dielectric constant, so when it is used as an organic solvent for an electrolyte, it has the effect of promoting dissociation of lithium salts. Furthermore, since FEC has a substituent that exhibits electron-withdrawing properties, it is easy to bind with lithium ions by Coulomb force or the like. Specifically, since FEC has a smaller solvation energy than ethylene carbonate (abbreviated as "EC") that does not have a substituent that exhibits electron-withdrawing properties, it can be said that FEC is easy to form solvation with lithium ions. Furthermore, FEC is considered to have a deep HOMO, and when the HOMO is deep, it is difficult to oxidize and oxidation resistance is improved. In addition, as one embodiment of the present invention, MTFP may be used as the organic solvent. MTFP is a chain carbonate and has the effect of reducing or maintaining the viscosity of the entire electrolyte. Of course, MTFP also has a smaller solvation energy than methyl propionate (abbreviated as "MP") that does not have a substituent that exhibits electron-withdrawing properties, so it may form solvation with lithium ions.
[0060] When FEC and MTFP are mixed, FEC and MTFP having such physical properties are preferably mixed in a volume ratio of x:100-x (where 5≦x≦30, preferably 10≦x≦20) with the total content of these two organic solvents being 100 vol%. The organic solvents are preferably mixed so that MTFP is greater than FEC. The volume ratio may be the volume ratio measured before mixing the organic solvents, and the outside air when mixing the organic solvents may be room temperature (typically 25° C.). An organic solvent mixed with FEC and MTFP is preferable because it exhibits a viscosity that allows operation as a lithium ion battery and maintains an appropriate viscosity over a wide temperature range including below freezing to high temperatures.
[0061] Since typical organic solvents used in lithium ion batteries freeze at about -20°C, it is difficult to fabricate a lithium ion battery that can be charged and discharged at -40°C, preferably -50°C. The organic solvent described as an example in this embodiment allows the freezing point to be -40°C or lower, preferably -50°C or lower, and a lithium ion battery that can be charged and discharged even in a sub-freezing environment of -40°C or lower can be realized. As a result, a lithium ion battery that can be charged and discharged over a wide temperature range including at least sub-freezing points can be realized.
[0062] If the electrolyte according to one embodiment of the present invention contains a fluorinated cyclic carbonate or a fluorinated chain carbonate, a lithium ion battery capable of being charged and discharged in a wide temperature range including at least freezing point can be provided. In addition, by containing a fluorinated cyclic carbonate or a fluorinated chain carbonate, the fluorine contained in the electrolyte repels the fluorine on the outermost surface of the positive electrode active material, and the fluorine can be retained on the outermost surface of the positive electrode active material. Therefore, the fluorine on the surface of the positive electrode active material can be suppressed, and the elution of magnesium can be prevented.
[0063] The organic solvent described above is preferably highly purified with a low content of particulate waste or molecules other than the organic solvent's constituent molecules (hereinafter, also referred to simply as "impurities", including oxygen (O2), water (H2O) or moisture). Specifically, the amount of the above impurities contained in the organic solvent is 100 ppm or less, preferably 50 ppm or less, and more preferably less than 10 ppm.
[0064] In order to reduce the amount of impurities contained in the organic solvent to less than 10 ppm, it is preferable to heat the organic solvent under reduced pressure before use in a secondary battery to remove the above-mentioned impurities. When the organic solvent is used in a secondary battery, the secondary battery is manufactured by injecting the organic solvent in a dry room where moisture is sufficiently reduced.
[0065] For example, moisture can be detected by Karl Fischer titration, and moisture with different binding strength (e.g., crystal water, combined water, or attached water) can be quantified by changing the heating conditions. For example, under heating conditions of 120°C for 30 minutes, moisture generated around 100°C can be mainly detected. In this specification, the unit ppm for the amount of impurities contained in the organic solvent refers to mass fraction, i.e. ppm (mass / mass).
[0066] When a secondary battery is charged and discharged, a part of the organic solvent is decomposed, which reduces the reliability of the secondary battery. Therefore, since impurities such as oxygen (O2), water (H2O) or moisture contained in the organic solvent may cause the organic solvent to decompose, the less impurities there are in the organic solvent, the less the decomposition of the organic solvent can be suppressed, as described above. In addition, if fluorine is present at a site that is likely to be the starting point of decomposition in the molecules used in the organic solvent, decomposition is less likely to occur, so it is preferable to use such a material.
[0067] <Lithium salt> The lithium salt dissolved in the organic solvent is, for example, LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, Li2B 10 Cl 10 , Li2B 12 Cl 12 At least one of LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), LiN(C2F5SO2)2, and lithium bis(oxalate)borate (LiBOB) can be used, and the above-mentioned lithium salts may be used in any combination and in any ratio. The lithium salt is one of the components of the electrolyte of one embodiment of the present invention, but is not necessarily required.
[0068] <Additives> In addition, for the purpose of improving safety, an additive may be mixed into the organic solvent to form a coating at the interface between the active material and the electrolyte. The additive may be one or more selected from vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), SUN (suberonitrile), or dinitrile compounds such as succinonitrile or adiponitrile. The concentration of the additive may be, for example, 0.1% by weight (wt%) or more and 5% by weight (wt%) or less with respect to the entire organic solvent. In particular, vinylene carbonate (VC) has the effect of suppressing the diffusion of fluorine on the outermost surface of the positive electrode active material and preventing the elution of magnesium into the electrolyte. In addition, it is preferable to select a material different from the organic solvent as the additive.
[0069] The lithium-ion battery of one embodiment of the present invention contains at least the above-described positive electrode active material and an electrolyte, and thus can maintain the state of the outermost surface of the positive electrode active material, prevent magnesium from eluting into the electrolyte, and realize a lithium-ion battery that can be charged and discharged over a wide temperature range including from below freezing to high temperatures.
[0070] (Embodiment 2) In this embodiment, a positive electrode active material that can be used in a lithium-ion battery according to one embodiment of the present invention (hereinafter also referred to as a "positive electrode active material that can be used as one embodiment of the present invention") and a manufacturing method thereof will be described with reference to FIGS.
[0071] As described above in the first embodiment, the positive electrode active material usable in the lithium ion battery according to one aspect of the present invention can be any material that is less prone to deterioration during charging and discharging at a high charging voltage. Therefore, the positive electrode active material usable in the lithium ion battery disclosed in this specification and the like does not need to be interpreted as being limited to the specific materials described in the present embodiment and the like, and materials that are known at the time of filing the present application as being less prone to deterioration during charging and discharging even at a high charging voltage (e.g., 4.5 V or higher) can also be used.
[0072] An example of a method for producing a positive electrode active material that can be used as one embodiment of the present invention will be described below. In this embodiment, a case where a positive electrode active material is produced using a solid phase method will be described, but a positive electrode active material produced using a co-precipitation method, a hydrothermal method, or the like other than the solid phase method can be applied to the lithium ion battery of the present invention. Note that the flow used to explain the production method and the like in this embodiment shows the order of elements connected by lines, and does not show the order of elements not connected by lines.
[0073] [Method of producing positive electrode active material] An example of a manufacturing flow of the positive electrode active material 10 will be described with reference to FIGS.
[0074] In step S11 shown in FIG. 2(A), a lithium source (Li source) and a transition metal M source (M source) are prepared as starting materials for lithium and transition metal M, respectively.
[0075] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, lithium fluoride, etc. It is preferable that the lithium source has high purity, and for example, it is preferable to use a material with a purity of 99.99% or more.
[0076] The transition metal M may be, for example, one or more of manganese, cobalt, and nickel. When lithium cobalt oxide (LCO) is prepared as the positive electrode active material, cobalt is used as the transition metal M. When nickel-cobalt-manganese composite oxide (NCM) is prepared as the positive electrode active material, cobalt, manganese, and nickel are used as the transition metal M. Aluminum may be used in addition to the transition metal M.
[0077] As the transition metal M source, it is preferable to use a compound having the transition metal M, and for example, an oxide of a metal exemplified as the transition metal M, or a hydroxide of the metal exemplified as the transition metal M, can be used. As a cobalt source, cobalt oxide, cobalt hydroxide, etc. can be used. As a manganese source, manganese oxide, manganese hydroxide, etc. can be used. As a nickel source, nickel oxide, nickel hydroxide, etc. can be used. As an aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used. In addition, when two or more transition metal M sources are used, it is preferable to prepare them in a ratio (mixing ratio) that allows the two or more transition metal M sources to have a layered rock salt type crystal structure.
[0078] <Step S12> Next, in step S12 shown in FIG. 2(A), the lithium source and the cobalt source are pulverized and mixed to prepare a mixed material. The pulverization and mixing can be performed in a dry or wet manner. The wet method is preferable because it can disintegrate the material into smaller pieces. When performing the wet method, a solvent is prepared. As the solvent, a ketone such as acetone, an alcohol such as ethanol and isopropanol, ether, dioxane, acetonitrile, N-methyl-2-pyrrolidone (NMP), etc. can be used. It is more preferable to use an aprotic solvent that does not easily react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or more is used. It is preferable to mix the lithium source and the cobalt source with dehydrated acetone with a purity of 99.5% or more, in which the moisture content is suppressed to 10 ppm or less, and then pulverize and mix the material. By using dehydrated acetone with the above-mentioned purity, it is possible to reduce impurities that may be mixed in.
[0079] A ball mill, a bead mill, or the like can be used as a means for pulverization and mixing. When using a ball mill, aluminum oxide balls or zirconium oxide balls are preferably used as pulverization media. Zirconium oxide balls are preferred because they emit less impurities. When using a ball mill, a bead mill, or the like, the peripheral speed is preferably set to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media. In this embodiment, the peripheral speed is set to 838 mm / s (rotation speed 400 rpm, ball mill diameter 40 mm).
[0080] <Step S13> Next, in step S13 shown in FIG. 2(A), the mixed material is heated. The heating is preferably performed at 800° C. or more and 1100° C. or less, more preferably at 900° C. or more and 1000° C. or less, and even more preferably at about 950° C. If the temperature is too low, the decomposition and melting of the Li source and M source may be insufficient. On the other hand, if the temperature is too high, lithium may sublime from the Li source and / or the transition metal used as the M source may be excessively reduced. If the heating time is too short, a composite oxide having lithium and the transition metal M may not be synthesized, but if it is too long, the productivity decreases. Therefore, the heating time is preferably 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating rate depends on the heating temperature reached, but is preferably 80° C. / h or more and 250° C. / h or less, more preferably 100° C. / h or more and 250° C. / h or less.
[0081] It is preferable that the heating atmosphere is an atmosphere with little water. The atmosphere with little water can be defined by the dew point, and for example, the heating atmosphere is an atmosphere with a dew point of -50°C or less, more preferably an atmosphere with a dew point of -80°C or less. Furthermore, the heating atmosphere is preferably an atmosphere containing oxygen such as dry air. For example, there is a method of continuously introducing oxygen into the reaction chamber. In this case, the flow rate of oxygen is preferably 5 L / min or more and 15 L / min or less. The state in which oxygen is continuously introduced into the reaction chamber and flows through the reaction chamber is called "flow".
[0082] In addition to the above flow, the heating atmosphere may be made to contain oxygen by, for example, depressurizing the reaction chamber, introducing oxygen, and then controlling the oxygen so that it does not enter or leave the reaction chamber. This is called "purging." For example, the reaction chamber may be depressurized to -970 hPa, and then oxygen may be introduced to 50 hPa, and the oxygen entry or exit may be stopped. This state may be described as filling the reaction chamber with oxygen.
[0083] After heating, the material may be naturally cooled, but it is preferable that the time required for the temperature to drop from the specified temperature to room temperature is within 10 to 50 hours, for example, 80° C. / h to 250° C. / h, and more preferably 180° C. / h to 210° C. / h. However, cooling to room temperature is not always necessary, and it is sufficient to cool the material to a temperature that is acceptable for the next step.
[0084] The heating in this step may be performed using a rotary kiln or a roller hearth kiln. Heating using a rotary kiln may be performed while stirring in either a continuous or batch type.
[0085] The crucible used for heating is preferably an aluminum oxide crucible. The aluminum oxide crucible is a material that does not easily release impurities. In this embodiment, an aluminum oxide crucible with a purity of 99.9% is used. It is preferable to place a lid on the crucible before heating. This can prevent the material from volatilizing or sublimating. Placing a lid on the crucible means that it is possible to prevent the material from volatilizing or sublimating during the temperature increase and decrease in this step, and it is not necessary to seal the crucible with a lid. For example, as described above, by filling the reaction chamber with oxygen, this step can be performed without sealing the crucible.
[0086] In addition, it is preferable to use a used crucible rather than a new one. In this specification, a new crucible refers to one that has undergone the process of putting in and heating materials containing lithium, transition metal M, and / or additive elements two or less times. In addition, a used crucible refers to one that has undergone the process of putting in and heating materials containing lithium, transition metal M, and / or additive elements three or more times. This is because when a new crucible is used, there is a risk that some of the materials, including lithium fluoride, may be absorbed, diffused, moved, and / or attached to the sheath during heating. If some of the materials are lost due to these reasons, there is a growing concern that the distribution of elements in the surface layer of the positive electrode active material will not be within a preferred range. On the other hand, with a used crucible, this risk is less likely.
[0087] After the heating is completed, the material may be crushed and sieved as necessary. When recovering the heated material, the material may be transferred from the crucible to a mortar and then recovered. The mortar is preferably made of aluminum oxide or zirconium oxide. The aluminum oxide mortar is made of a material that does not easily release impurities. Specifically, an aluminum oxide mortar with a purity of 90% or more, preferably 99% or more, is used. The same heating conditions as those in step S13 can be applied to the heating steps described below other than step S13.
[0088] <Step S14> Through the above steps, a composite oxide (LiMO2) containing lithium and a transition metal M can be obtained in step S14 of Fig. 2(A). The composite oxide is expressed as LiMO2, but the composition is not strictly limited to Li:M:O = 1:1:2. When cobalt is used as the transition metal M, it is called a composite oxide containing cobalt and expressed as LiCoO2, but the composition is not strictly limited to Li:Co:O = 1:1:2.
[0089] Although the composite oxide is produced by the solid phase method as in steps S11 to S14, the composite oxide may be produced by a coprecipitation method or a hydrothermal method.
[0090] <Step S15> Next, in step S15 shown in FIG. 2(A), the composite oxide is heated. Since this is the first heating of the composite oxide, the heating in step S15 may be called initial heating. Alternatively, since the heating is performed before step S20 described below, it may be called preheating or pretreatment. The crucible and / or lid used in this step are the same as those used in step S13. Although the following effects are expected from the initial heating, the initial heating is not essential to obtain the positive electrode active material which is one embodiment of the present invention.
[0091] The initial heating may cause lithium to be released from a part of the composite oxide. It is also expected to have the effect of increasing the crystallinity of the composite oxide. In addition, the Li source and / or the metal M source prepared in step S11 may contain impurities, but the initial heating can reduce the impurities from the composite oxide.
[0092] Furthermore, the initial heating has the effect of smoothing the surface of the composite oxide. A smooth surface of a composite oxide means that there are few irregularities, the surface of the composite oxide is generally rounded, and the corners are also rounded. A surface with little foreign matter adhering to it is sometimes called smooth.
[0093] For this initial heating, it is not necessary to prepare a raw material such as a Li source, or a material that functions as a flux (a material added to facilitate melting).
[0094] If the heating time of this step is too short, sufficient effect is not obtained, but if it is too long, productivity decreases. For example, the heating conditions can be selected from those described in step S13. Regarding the heating conditions, the heating temperature of this step should be lower than the temperature of step S13 in order to maintain the crystal structure of the complex oxide. Furthermore, the heating time of this step should be shorter than the time of step S13 in order to maintain the crystal structure of the complex oxide. For example, heating at a temperature of 700°C to 1000°C for 2 hours to 20 hours is recommended.
[0095] The effect of enhancing the crystallinity of the complex oxide includes, for example, the effect of relieving distortion resulting from a shrinkage difference caused by heating the complex oxide, and the effect of relieving deviation resulting from the shrinkage difference.
[0096] The heating in step S13 may cause a temperature difference between the surface and the inside of the composite oxide. The temperature difference may induce a contraction difference. It is also considered that the temperature difference causes the contraction difference because the fluidity of the surface and the inside is different. The energy related to the contraction difference gives the composite oxide a difference in internal stress, which causes distortion. The above energy may be called strain energy. The internal stress is removed by the initial heating in step S15, or in other words, the strain energy is thought to be reduced by the initial heating in step S15. When the strain energy is reduced, the distortion of the composite oxide is relaxed. Therefore, the surface of the composite oxide may become smooth after step S15. In other words, it is thought that the contraction difference caused in the composite oxide is relaxed after step S15, and the surface of the composite oxide becomes smooth. Step S15 may be called tempering or annealing of the composite oxide.
[0097] Furthermore, the shrinkage difference may cause microscopic deviations in the composite oxide, for example deviations in the crystal plane. In order to reduce such deviations, it is advisable to carry out this step. By passing through this step, it is possible to reduce the deviations in the composite oxide. If the deviations are made uniform, the surface of the composite oxide may become smooth. This is also referred to as the alignment of crystal grains. In other words, it is believed that, by passing through step S15, deviations of crystals and the like that have occurred in the composite oxide are alleviated, and the surface of the composite oxide becomes smooth.
[0098] A smooth surface of a complex oxide can be said to have a surface roughness of at least 10 nm or less when surface irregularity information is quantified from measurement data on a cross section of the complex oxide. The cross section is, for example, a cross section obtained when observing with a scanning transmission electron microscope (referred to as STEM).
[0099] When a composite oxide with a smooth surface is used as a positive electrode active material, deterioration during charging and discharging in a lithium ion battery is reduced and cracking of the positive electrode active material can be prevented.
[0100] In step S14, a composite oxide containing lithium and a transition metal M that has been synthesized in advance may be used. In this case, steps S11 to S13 can be omitted. By carrying out step S15 on a composite oxide that has been synthesized in advance, a composite oxide with a smooth surface can be obtained.
[0101] It is possible that the lithium in the composite oxide is reduced by the initial heating. The reduction in lithium may facilitate the incorporation of the additive element, which will be described in the next step S20_1, into the composite oxide. In addition, if the additive element is added to a composite oxide with a smooth surface, the additive element can be added evenly, so it is preferable to add the additive element after the initial heating. The step of adding the additive element will be described with reference to FIG. 2(B).
[0102] <Step S20_1> and <Step S21_1> Step S20_1 shown in Fig. 2(A) is shown in detail in Fig. 2(B). In step S21_1 in Fig. 2(B), an additive element A1 source (A1 source) to be added to the composite oxide is prepared. In order to compensate for the lithium lost by the initial heating, a lithium source may be prepared together with the additive element A1 source.
[0103] The additive element A1 can be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.
[0104] When magnesium is selected as the additive element A1, the source of the additive element A1 can be called a magnesium source (Mg source). As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used. In addition, a plurality of the above-mentioned magnesium sources may be used.
[0105] When fluorine is selected as the additive element A1, the source of the additive element A1 can be called a fluorine source (F source). As the fluorine source, for example, lithium fluoride, magnesium fluoride, aluminum fluoride, titanium fluoride, cobalt fluoride, nickel fluoride, zirconium fluoride, vanadium fluoride, manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride, calcium fluoride, sodium fluoride, potassium fluoride, barium fluoride, cerium fluoride, lanthanum fluoride, or sodium aluminum hexafluoride can be used. Among them, lithium fluoride is preferable because it has a relatively low melting point of 848°C and is easily melted in the heating process described below. Note that FIG. 2(B) shows an example in which a Mg source and a F source are used as the additive element A1 source.
[0106] Magnesium fluoride can be used as both the fluorine source and the magnesium source, and lithium fluoride can be used as the lithium source. Another lithium source that can be used in step S21_1 is lithium carbonate.
[0107] In this embodiment, lithium fluoride is prepared as the fluorine source, and magnesium fluoride is prepared as the fluorine source and magnesium source. When lithium fluoride and magnesium fluoride are mixed at a molar ratio of about LiF:MgF2=65:35, the effect of lowering the melting point is maximized. On the other hand, if the amount of lithium fluoride is large, there is a concern that the lithium becomes excessive and the cycle characteristics deteriorate. Therefore, in this embodiment, the molar ratio of lithium fluoride and magnesium fluoride is preferably LiF:MgF2=x:1 (0≦x≦1.9), more preferably LiF:MgF2=x:1 (0.1≦x≦0.5), and even more preferably LiF:MgF2=x:1 (x=0.33 or nearby). Note that "nearby" refers to a value that is greater than 0.9 times and less than 1.1 times the value.
[0108] At the same time, the amount of magnesium added is preferably more than 0.1 atomic % and less than 3 atomic % relative to the number of Co atoms in LiMO2, typically LiCoO2, in step S14, more preferably 0.5 atomic % to 2 atomic %, and even more preferably 0.5 atomic % to 1 atomic %. If the amount of magnesium added is 0.1 atomic % or less, the initial discharge capacity is high, but the discharge capacity may drop rapidly by repeating high-voltage charging. If the amount of magnesium added is more than 0.1 atomic %, that is, more than 0.1 atomic % to 3 atomic %, both the initial discharge characteristics and the charge-discharge cycle characteristics are good even if the high-voltage charging is repeated. On the other hand, if the amount of magnesium added is more than 3 atomic %, the initial discharge capacity is low, and the charge-discharge cycle characteristics also tend to gradually deteriorate.
[0109] <Step S22_1> Next, in step S22_1 shown in Fig. 2(B), the magnesium source and the fluorine source are mixed while being pulverized. This step can be performed under the pulverization conditions and the mixing conditions selected from those described in step S12.
[0110] If necessary, a heating step may be performed after step S22_1. The heating step in this case can be performed under the heating conditions selected from those described in step S13. The heating time is preferably 2 hours or more, and the heating temperature is preferably 800° C. or more and 1100° C. or less.
[0111] <Step S23_1> Next, in step S23_1 shown in Fig. 2(B), the material crushed and mixed above can be collected to obtain the additive element A1 source (A1 source). Note that the additive element A1 source shown in step S23_1 may have multiple raw materials such as a Mg source and a F source, and in this case, the A1 source can be called a mixture.
[0112] <Step S31> Next, in step S31 shown in FIG. 2A, the composite oxide and the source of the additive element A1 (A1 source) are mixed. The number of atoms A of the transition metal M in the composite oxide having lithium and the transition metal M is M and the number of magnesium atoms A of the additive element A1. Mg The ratio of A M :A Mg = 100:y (0.1 ≦ y ≦ 6), and A M :A Mg It is more preferable that y=100:y (0.3≦y≦3).
[0113] In order not to destroy the composite oxide, the mixing in step S31 is preferably performed under milder conditions than the conditions for pulverization and mixing in step S12. For example, the mixing conditions are preferably set at a lower rotation speed or shorter time than in step S12. In addition, a dry method is more suitable than a wet method because the conditions are milder.
[0114] The mixing is preferably carried out in an atmosphere having a dew point of −100° C. or higher and −10° C. or lower. For example, the mixing can be carried out in a dry room. The atmosphere of the dry room may contain dry air.
[0115] <Step S32> Next, in step S32 of Fig. 2(A), the mixed materials are collected to obtain a mixture 903. When collected, the mixture 903 may be crushed to break up any agglomerated materials. Furthermore, the mixture 903 may be sieved to break up any agglomerated materials. Sieving may be performed after crushing, or sieving may be performed while crushing, or only sieving may be performed instead of crushing.
[0116] In this embodiment, the method of adding lithium fluoride as a fluorine source and magnesium fluoride as a magnesium source to the composite oxide that has been initially heated has been described, but the present invention is not limited to the above method. In step S11, that is, in the stage of the starting materials for the composite oxide, a magnesium source, a fluorine source, etc. can be prepared together with a Li source and an M source, and the process can proceed to step S12. After that, heating is performed in step S13 to obtain LiMO2 to which magnesium and fluorine have been added. In this case, there is no need to separate the steps from step S11 to step S14 from the steps from step S21_1 to step S23_1. It can be said that this is a simple and highly productive method.
[0117] Alternatively, a composite oxide to which magnesium and fluorine have been added in advance may be used. If a composite oxide to which magnesium and fluorine have been added is used, the steps S11 to S32 and S20_1 can be omitted. This method is simple and has high productivity.
[0118] Alternatively, a magnesium source and a fluorine source may be further added to a composite oxide to which magnesium and fluorine have been added in advance in accordance with step S20_1. Instead of the magnesium source and the fluorine source, or in addition to the magnesium source and the fluorine source, a nickel source and an aluminum source may be added.
[0119] <Step S33> 2(A), the mixture 903 is heated. The heating conditions can be selected from those described in step S13. The heating time is preferably 2 hours or more.
[0120] Here, a supplementary note on the heating temperature will be provided. The lower limit of the heating temperature in step S33 must be equal to or higher than the temperature at which the reaction between the composite oxide (LiMO2) and the additive element A1 source proceeds. The temperature at which the reaction proceeds may be any temperature at which the elements contained in the composite oxide and the additive element A1 source can diffuse into each other, and may be lower than the melting temperatures of these materials. An oxide will be used as an example to explain the Tammann temperature T d (Melting point of oxide T m It is known that solid-phase diffusion occurs at a temperature above which the temperature is calculated as 0.757 times the temperature at which the solid phase diffusion occurs. Therefore, the heating temperature in step S33 may be 500° C. or higher.
[0121] Of course, the reaction proceeds more easily if the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts. For example, when LiF and MgF2 are used as the source of the additive element A1, the eutectic point of LiF and MgF2 is around 742°C, so that the lower limit of the heating temperature in step S33 is preferably set to 742°C or higher.
[0122] In addition, the mixture 903 obtained by mixing LiCoO2:LiF:MgF2=100:0.33:1 (molar ratio) shows an endothermic peak at about 830° C. in differential scanning calorimetry (DSC). Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.
[0123] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and the productivity is high.
[0124] The upper limit of the heating temperature is below the decomposition temperature of the composite oxide. For example, in the case of LiCoO2, the upper limit is below the decomposition temperature of 1130°C. At temperatures close to the decomposition temperature, there is concern that LiMO2 may decompose, although only in small amounts. If LiMO2 decomposes, it is undesirable because it may produce unnecessary reaction products in the composite oxide, typically Co3O4 in the case of lithium cobalt oxide. Therefore, it is more preferable that the temperature is 1000°C or lower, even more preferable that the temperature is 950°C or lower, and even more preferable that the temperature is 920°C or lower.
[0125] In consideration of these, the heating temperature in step S33 is preferably 500°C or more and less than 1130°C, more preferably 500°C or more and less than 1000°C, even more preferably 500°C or more and less than 950°C, even more preferably 500°C or more and less than 920°C, and even more preferably 500°C or more and less than 900°C. Also, it is preferably 742°C or more and less than 1130°C, more preferably 742°C or more and less than 1000°C, even more preferably 742°C or more and less than 950°C, even more preferably 742°C or more and less than 920°C, and even more preferably 742°C or more and less than 900°C. Also, it is preferably 800°C or more and less than 1130°C, more preferably 800°C or more and less than 1000°C, even more preferably 800°C or more and less than 950°C, even more preferably 800°C or more and less than 920°C, and even more preferably 800°C or more and less than 900°C. Furthermore, the temperature is preferably 830°C or higher and lower than 1130°C, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, even more preferably 830°C or higher and 920°C or lower, and even more preferably 830°C or higher and 900°C or lower.
[0126] The heating temperature in step S33 is preferably lower than that in step S13 in order to prevent the composite oxide (LiMO2) from decomposing. The heating temperature in step S33 is preferably higher than that in step S15.
[0127] Furthermore, when heating the mixture 903, it is preferable to control the partial pressure of fluorine or fluoride resulting from a fluorine source or the like in the processing chamber or crucible within an appropriate range. In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, may function as a flux. This function allows the heating temperature to be lowered below the decomposition temperature of the complex oxide (LiMO2), for example, to 742°C or higher and 950°C or lower, and the additive element A1 including magnesium is distributed in the surface layer, making it possible to manufacture a positive electrode active material with good characteristics.
[0128] However, LiF may sublime when heated, and since LiF has a lower specific gravity in a gaseous state than oxygen, it is conceivable that the amount of LiF in the mixture 903 may decrease. This weakens its function as a flux. Therefore, it is necessary to heat the mixture while suppressing the sublimation of LiF. Even if LiF is not used as the fluorine source, etc., Li on the LiMO2 surface may react with F as the fluorine source, producing LiF, which may then sublime. Therefore, even if a fluoride with a higher melting point than LiF is used, it is necessary to suppress sublimation in the same way.
[0129] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF in the processing chamber is high. Such heating can suppress the sublimation of LiF in the mixture 903. In addition, by placing a lid on the container as described above, the sublimation of LiF in the mixture 903 can also be suppressed.
[0130] The heating in this step is preferably performed so as not to stick the mixture 903 together. If the mixture 903 sticks together during heating, the contact area with oxygen in the atmosphere decreases, and the route along which the additive element A1 (e.g., magnesium and / or fluorine) diffuses is blocked, which may make it difficult for the additive element A1 (e.g., magnesium and / or fluorine) to diffuse.
[0131] It is also believed that if the additive element A1 (e.g., fluorine) is uniformly distributed in the surface layer, a smooth positive electrode active material with few irregularities can be obtained. Therefore, in order to maintain the smooth surface or to make it even smoother after the heating in step S15 in this process, it is better that the mixture 903 does not stick to each other.
[0132] A supplementary note on the heating time: The heating time varies depending on conditions such as the heating temperature, the size of LiMO2 in step S14, and the composition. When the median diameter (D50) of LiMO2 is small, a lower temperature or a shorter heating time may be more preferable than when the median diameter (D50) is large. The median diameter (D50) can be determined using a laser diffraction particle size distribution analyzer.
[0133] In the case where lithium cobalt oxide is used as LiMO2 in step S14 in FIG. 2(A), when the median diameter (D50) of lithium cobalt oxide is about 12 μm, such as 10 μm to 14 μm, the heating temperature in step S33 is, for example, preferably 800° C. to 920° C., more preferably 850° C. to 920° C. The heating time in step S33 is, for example, more preferably 10 hours or more, more preferably 20 hours or more, and may be 60 hours or more. If the median diameter (D50) is large, the volume of the complex oxide (LiMO2) becomes large, and the internal stress is relaxed or removed in the bulk layer of the complex oxide, so that a heating time may be required. If the median diameter (D50) is large, it takes time for the additive element A1, including magnesium, to be uniformly distributed in the surface layer, so that the heating time may be long as described above. Although the median diameter (D50) of lithium cobalt oxide may increase after heat treatment, it is preferable that the median diameter (D50) after heat treatment is 10 μm or more and 14 μm or less. In other words, it is preferable that the median diameter (D50) of the positive electrode active material is 10 μm or more and 14 μm or less.
[0134] In the case where lithium cobalt oxide is used as LiMO2 in step S14, when the median diameter (D50) of lithium cobalt oxide is about 7 μm, such as 5 μm to 9 μm, the heating temperature in step S33 is preferably in the same range as the heating temperature when the median diameter (D50) is about 12 μm. On the other hand, the heating time in step S33 can be shorter than the heating time when the median diameter (D50) is about 12 μm. For example, 1 hour to 10 hours is preferable, and 5 hours to 10 hours is more preferable. If the median diameter (D50) is small, the time for the additive element A1, including magnesium, to be distributed in the surface layer is shortened, so that the heating time can be shortened as described above. If the median diameter (D50) is small, the volume of the composite oxide (LiMO2) is small, so that the time for tempering or annealing the bulk layer of the composite oxide is short. Although the median diameter (D50) of lithium cobalt oxide may increase after heat treatment, it is preferable that the median diameter (D50) is 5 μm or more and 9 μm or less even after heat treatment. In other words, it is preferable that the median diameter (D50) of the positive electrode active material is 5 μm or more and 9 μm or less.
[0135] After step S33, a step of further adding an additional element different from the additional element A1 described above may be provided. This step will be described with reference to FIG.
[0136] <Step S20_2> and <Step S21_2> The details of step S20_2 shown in Fig. 2(A) are shown in Fig. 2(C). In step S21_2 in Fig. 2(C), a source of an additive element A2 (A2 source) to be added to the composite oxide is prepared. A lithium source may be prepared together with the additive element A2 source.
[0137] The additive element A2 may be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. The additive element A2 may be at least an element not selected as the additive element A1, but may contain an element selected as the additive element A1. Note that FIG. 2(C) shows an example in which a Ni source and an Al source are used as the additive element A2 source.
[0138] In this embodiment, nickel hydroxide is prepared as the nickel source, and aluminum hydroxide is prepared as the aluminum source. Nickel oxide or nickel carbonate may be used instead of nickel hydroxide. Aluminum oxide or aluminum carbonate may be used instead of aluminum hydroxide.
[0139] <Step S22_2> Next, in step S22_2 shown in Fig. 2(C), the nickel source is mixed while being pulverized, and further the aluminum source is mixed while being pulverized. This step can be carried out by selecting from the pulverization conditions and mixing conditions described in step S12. Note that this step may be carried out by mixing the nickel source and the aluminum source while being pulverized after combining them as in step S22_1 in Fig. 2(B).
[0140] If necessary, a heating step may be performed after step S22_2. The heating step in this case can be performed under the heating conditions selected from those described in step S13.
[0141] <Step S23_2> Next, in step S23_2 shown in FIG. 2(C), the material crushed or mixed as described above can be recovered to obtain a source of the additional element A2 (A2 source).
[0142] <Step S34> Next, in step S34 shown in FIG. 2(A), the composite oxide heated in step S33 is mixed with the additive element A2 source (A2 source). As described above, a plurality of additive element A2 sources (A2 sources) may be prepared. The number of atoms A of the transition metal M in the composite oxide is M and the number of nickel atoms in the additive element A2, A Ni The ratio of A M :A Ni = 100:y (0.1 ≦ y ≦ 3), and A M :A Ni It is more preferable that the number of atoms of the transition metal M in the composite oxide is 100:y (0.3≦y≦1). M and the number of aluminum atoms A of the additive element A2. Al The ratio of A M :A Al = 100:y (0.1 ≦ y ≦ 3), and A M :A Al It is more preferable that y=100:y (0.3≦y≦1).
[0143] The mixing conditions in step S34 can be selected from the mixing conditions described in step S31.
[0144] <Step S35> Next, in step S35 of Fig. 2(A), the mixed materials are collected to obtain a mixture 904. When collected, the mixture 904 may be crushed to break up any aggregates. The mixture 904 may be sieved to further break up any aggregates. Sieving may be performed after crushing, sieving may be performed while crushing, or only sieving may be performed instead of crushing.
[0145] <Step S36> 2(A), the mixture 904 is heated. This can be performed under heating conditions selected from those described in step S33. The heating time is preferably 2 hours or more.
[0146] The heating temperature in step S36 is preferably 500°C to 1130°C, more preferably 500°C to 1000°C, even more preferably 500°C to 950°C, and even more preferably 500°C to 900°C, as in step S33. Also, it is preferably 742°C to 1130°C, more preferably 742°C to 1000°C, even more preferably 742°C to 950°C, and even more preferably 742°C to 900°C. Also, it is preferably 800°C to 1100°C, more preferably 830°C to 1130°C, more preferably 830°C to 1000°C, even more preferably 830°C to 950°C, and even more preferably 830°C to 900°C. The heating temperature in step S36 is preferably lower than that in step S13. The heating temperature in step S36 is preferably lower than that in step S33.
[0147] The heating in this step is preferably performed so as not to stick the mixture 904 together. If the mixture 904 sticks together during heating, the contact area with oxygen in the atmosphere decreases and the route along which the additive element A2 diffuses is blocked, which may result in poor distribution of the additive element A2.
[0148] <Step S37> Next, in step S37 shown in FIG. 2(A), the heated material is recovered and crushed as necessary to obtain the positive electrode active material 10. At this time, it is preferable to further sieve the recovered positive electrode active material 10. By the above steps, the positive electrode active material 10 according to one embodiment of the present invention can be produced. The positive electrode active material according to one embodiment of the present invention has a smooth surface. The above is an example of a method for producing a positive electrode active material.
[0149] [Cathode active material] A cross section of a positive electrode active material 10 that can be obtained by the above-mentioned manufacturing method will be described with reference to FIG. 3(A). FIG. 3(B) shows a cross section of a positive electrode active material 10 in which, unlike FIG. 3(A), grain boundaries 15 are clearly indicated by dashed lines. The positive electrode active material 10 shown in FIG. 3(A) and FIG. 3(B) both have a surface layer portion 10a and an interior portion (the interior portion is referred to as a "bulk portion") 10b, and the boundary between them is indicated by a dashed line. It is more preferable that the surface layer portion 10a covers 90% or more of the bulk portion 10b. The dashed lines in FIG. 3(A) and FIG. 3(B) are examples, the dashed lines in FIG. 3(B) are examples, and the proportion of the surface layer portion that is covered is also an example.
[0150] The surface layer portion 10a does not have to cover the entire bulk portion 10b. Figures 3(A) and 3(B) show a positive electrode active material 10 in which the surface layer portion 10a covers 50% or more, specifically 65% or more and 75% or less, of the outer periphery of the bulk portion 10b. For example, as shown in Figure 3B, the positive electrode active material 10 may have a region in which the bulk portion 10b is exposed.
[0151] The grain boundary 15 shown in FIG. 3(B) refers to, for example, a portion where the positive electrode active material 10 is fixed to itself, a portion where the crystal orientation changes inside the positive electrode active material 10, that is, a portion where the repetition of bright and dark lines in a STEM image or the like becomes discontinuous, a portion containing many crystal defects, or a portion where the crystal structure is disordered. The crystal defect refers to a defect that can be observed in a cross-sectional TEM (transmission electron microscope) image, a cross-sectional STEM image, or the like, and the defect can also be called a structure in which other elements have entered between the lattices, or a cavity, or the like. In other words, the grain boundary 15 can be said to be one of the plane defects. The vicinity of the grain boundary 15 refers to a region within 20 nm, preferably within 10 nm, of the grain boundary 15, and the vicinity of the grain boundary exists both inside and outside the particle. These can be distinguished by indicating the vicinity of the grain boundary inside the particle or the vicinity of the grain boundary outside the particle.
[0152] Since the positive electrode active material 10 has a composite oxide containing oxygen and a transition metal capable of inserting and extracting lithium, the interface between a region containing a transition metal M (e.g., Co, Ni, Mn, Fe, etc.) that is oxidized and reduced with the insertion and extraction of lithium and a region containing no transition metal M can be regarded as the "surface" of the positive electrode active material. An additive element may be present in the region containing no transition metal M. Surfaces newly generated by slips, cracks, and / or cracks may also be regarded as the surface of the positive electrode active material.
[0153] Again, in this specification, the surface layer portion 10a is, for example, a region within 50 nm, more preferably within 35 nm, even more preferably within 20 nm, and most preferably within 10 nm from the surface toward the inside. Alternatively, the surface layer portion may be referred to as the vicinity of the surface, the surface vicinity region, or the shell. The region within 50 nm, more preferably within 35 nm, even more preferably within 20 nm, and most preferably within 10 nm from the surface toward the inside refers to the distance in the depth direction along a perpendicular or approximately perpendicular direction from the surface. The perpendicular or approximately perpendicular direction at the surface refers to a direction in which the angle with the tangent at the surface is 80° or more and 100° or less. The bulk portion 10b refers to a region deeper than the surface layer portion 10a. The bulk portion 10b may be referred to as the inside, and may also be referred to as the core. The bulk portion 10b may include the center of the positive electrode active material.
[0154] In the positive electrode active material 10, the region where lithium is inserted and removed may be referred to as the "surface." Therefore, the "surface" can be considered to be a region of the positive electrode active material 10 that is in contact with the electrolyte. For example, the surface of the positive electrode active material 10 includes the surface of the surface layer portion 10a, and in a region where the bulk portion 10b is exposed, the bulk portion 10b may be the surface.
[0155] Carbonate groups, hydroxyl groups, and the like that are chemically adsorbed after preparation of the positive electrode active material 10 are considered to be regions into which lithium cannot be inserted or removed, and these do not constitute the surface of the positive electrode active material 10. Similarly, the electrolyte, binder, conductive material, or compounds derived therefrom that are attached to the positive electrode active material 10 do not constitute the surface of the positive electrode active material 10 either.
[0156] The "surface" of the positive electrode active material 10 in a cross-sectional STEM (scanning transmission electron microscope) image or the like is the boundary between an area where an electron beam bond image is observed and an area where it is not observed, and can be the outermost part of an area where bright spots originating from atomic nuclei of metal elements having atomic numbers larger than that of lithium are confirmed. The surface in a cross-sectional STEM image or the like may be determined in conjunction with the results of an analysis with higher spatial resolution, such as electron energy loss spectroscopy (EELS) or the like.
[0157] The positive electrode active material needs to have a transition metal capable of oxidation and reduction in order to maintain charge neutrality even when lithium ions are inserted and removed. The positive electrode active material 10 of one embodiment of the present invention mainly uses cobalt as the transition metal M responsible for the oxidation and reduction reaction, but in addition to cobalt, at least one or more selected from nickel and manganese may be used. If the transition metal M contained in the positive electrode active material 10 is 75 atomic % or more, preferably 90 atomic % or more, and more preferably 95 atomic % or more, cobalt is preferable because it has many advantages such as being relatively easy to synthesize, being easy to handle, and having excellent cycle characteristics.
[0158] When nickel is used as the transition metal M in the positive electrode active material 10 at 33 atomic % or more, preferably at 60 atomic % or more, and more preferably at 80 atomic % or more, the raw material may be cheaper than when a large amount of cobalt is used, and the discharge capacity per weight may be increased, which is preferable.
[0159] The additive element A (additive element A1 and additive element A2) contained in the positive electrode active material 10 is listed again, and it is preferable to use one or more elements selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.
[0160] In other words, the positive electrode active material 10 can be called lithium cobalt oxide to which the additive element A has been added. As will be described later, the additive element A can further stabilize the crystal structure of the positive electrode active material 10.
[0161] The additive element A does not necessarily have to include one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.
[0162] For example, if the positive electrode active material 10 does not substantially contain manganese as the additive element A, the above-mentioned advantages of being relatively easy to synthesize and easy to handle, and having excellent cycle characteristics, become even greater. The weight of manganese contained in the positive electrode active material 10 is preferably, for example, 600 ppm or less, more preferably 100 ppm or less. The weight of manganese can be analyzed, for example, using a glow discharge mass spectrometer (GD-MS).
[0163] <Crystal structure> The change in crystal structure accompanying the change in x in LixCoO2 will be described with reference to Figs. 4 to 8, while comparing a cathode active material 10 that can be used as one embodiment of the present invention with a conventional cathode active material. Fig. 4 shows the crystal structure of a cathode active material 10 that can be used as one embodiment of the present invention, and Fig. 5 shows the crystal structure of a conventional cathode active material. The conventional cathode active material shown in Fig. 5 is lithium cobalt oxide (LiCoO2) that does not have any added elements. In this specification, etc., "does not have any added elements" refers to the case where the amount of the added elements is below the lower limit of detection when measured using an analytical means, or, if the amount of the added elements is close to the lower limit of detection, the added elements are included within a range that does not affect the presence or absence of the action or effect.
[0164] <Li x When x in CoO2 is 1≫ The positive electrode active material 10 that can be used as one embodiment of the present invention is Li xWhen x=1 in CoO2, that is, in the discharged state, it is preferable for the material to have a layered rock-salt type crystal structure belonging to the space group R-3m. In this crystal structure, lithium occupies an octahedral site, and there are three CoO2 layers in the unit cell. For this reason, this crystal structure is sometimes called an O3 type crystal structure. Note that a CoO2 layer is defined as a structure in which an octahedral structure in which oxygen is coordinated to cobalt six times is continuous on a plane with edge sharing. The CoO2 layer is sometimes referred to as a layer consisting of an octahedron of cobalt and oxygen. In Figure 4, Li x The crystal structure when x in CoO2 is 1 is labeled R-3m(O3). x The crystal structure when x in CoO2 is 1 is the same as the crystal structure shown in Figure 4, and is similarly denoted as R-3m(O3).
[0165] The layered rock-salt complex oxide has a high discharge capacity, has a two-dimensional lithium ion diffusion path, is suitable for lithium ion insertion / extraction reactions, and is excellent as a positive electrode active material for lithium ion batteries. Therefore, it is preferable that the bulk portion 10b, which occupies the majority of the positive electrode active material 10, has a layered rock-salt crystal structure.
[0166] The crystal structure of the surface layer 10a of the positive electrode active material 10 that can be used as one embodiment of the present invention does not have to be a layered rock salt type. The surface layer 10a preferably has a function of reinforcing the layered structure of the bulk portion 10b, which is made up of octahedra of cobalt and oxygen, so that it is not broken even if lithium is removed from the positive electrode active material 10 by charging. Alternatively, the surface layer 10a preferably functions as a barrier film for the positive electrode active material 10. Alternatively, the surface layer 10a, which is the outer periphery of the positive electrode active material 10, preferably reinforces the positive electrode active material 10. The reinforcement referred to here means suppressing structural changes in the surface layer 10a and bulk portion 10b of the positive electrode active material 10, including oxygen desorption, and / or suppressing oxidative decomposition of the electrolyte on the surface of the positive electrode active material 10.
[0167] The surface layer 10a is the region from which lithium ions are first desorbed during charging, and is the region where the lithium concentration is likely to be lower than that of the bulk portion 10b. When lithium ions are desorbed from the surface atoms of the positive electrode active material 10 in the surface layer 10a, some of the bonds are broken. Therefore, the surface layer 10a is likely to become unstable, and is the region where the crystal structure is likely to change, that is, where deterioration is likely to begin. On the other hand, if the surface layer 10a can be made sufficiently stable, Li x When x in CoO2 is small, for example, even if x is 0.24 or less, the layered structure of the CoO2 layer in the bulk portion 10b can be made hard to break. Furthermore, displacement of the CoO2 layer in the bulk portion 10b can be suppressed.
[0168] In order to make the surface layer portion 10a have a stable composition and crystal structure, it is preferable that the surface layer portion 10a has an additive element A, and more preferably has a plurality of additive elements A. It is also preferable that the surface layer portion 10a has a higher concentration of one or more selected from the additive elements A than the bulk portion 10b. It is also preferable that the one or more selected from the additive elements A contained in the positive electrode active material 10 have a concentration gradient. It is also more preferable that the distribution of the positive electrode active material 10 differs depending on the additive element A. For example, it is more preferable that the depth from the surface of the concentration peak differs depending on the additive element A. The concentration peak here refers to the maximum value of the concentration in the surface layer portion 10a or at a depth of 50 nm or less from the surface.
[0169] Here, the above-mentioned concentration gradient and concentration peak will be explained with reference to the conceptual diagrams of FIG. 3(C) to FIG. 3(F).
[0170] 3(C) and 3(D) show enlarged views of the vicinity of AB in FIG. 3(A). FIG. 3(C) and 3(D) show cross sections of the surface layer having the (001) plane (hereinafter, referred to as the (001) plane, and may also be referred to as the c-plane or basal plane), that is, cross sections of the region oriented in (001). In the layered rock salt type crystal structure, cations are arranged parallel to the (001) plane. This can be said to be a structure in which the CoO2 layer and the lithium layer are alternately stacked parallel to the (001) plane. Therefore, the diffusion path of lithium ions exists parallel to the (001) plane. Since the CoO2 layer is relatively stable, the (001) plane on which the CoO2 layer exists on the surface is relatively stable, and the main diffusion path of lithium ions during charging and discharging is not exposed to the (001) plane.
[0171] FIG. 3(C) showing such a (001) plane shows the distribution of magnesium and the like as an example of the additive element A. The shading in FIG. 3(C) corresponds to the change in the concentration of magnesium. Since the CoO2 layer is relatively stable on the (001) plane, the additive element A may not be detected. When it is detected, FIG. 3(C) shows an example of the distribution of the additive element A, in which the additive element A is present at the highest concentration on or near the surface of the surface layer portion 10a, and the concentration of the additive element A decreases toward the bulk portion 10b. It can be said that there is a concentration peak of magnesium and the like at the position showing the highest concentration. The decrease in concentration may be referred to as a concentration gradient. In this specification, the additive element A that shows the distribution as shown in FIG. 3(C) on the (001) plane will be referred to as the additive element X.
[0172] FIG. 3(D) shows the distribution of aluminum as another example of the additive element A. The shading in FIG. 3(D) corresponds to the change in the concentration of aluminum. Since the CoO2 layer is relatively stable on the (001) plane, the additive element A may not be detected. When it is detected, FIG. 3(D) shows an example of the distribution of the additive element A, in which the additive element A is present at the highest concentration at a position deeper than the surface or near the surface in the surface layer portion 10a, and the concentration of the additive element A decreases toward the surface and bulk portion 10b. Although the aluminum concentration peak is at the position showing the highest concentration, the aluminum concentration peak position may be located slightly deeper than the concentration peak position of the magnesium and the like. The decrease in concentration may be referred to as a concentration gradient. In this specification, the additive element A that shows a distribution as shown in FIG. 3(D) on the (001) plane will be referred to as the additive element Y.
[0173] Depending on the element of the additive element A, a distribution like that of the additive element X or a distribution like that of the additive element Y may be shown, and the distributions may differ from each other. Also, depending on the element of the additive element A, a concentration peak position like that of the additive element X or a concentration peak position like that of the additive element Y may be shown, and the concentration peak positions may differ from each other.
[0174] Figures 3(E) and 3(F) show enlarged views of the vicinity of CD in Figure 3(A). Figures 3(E) and 3(F) can be said to be cross-sectional views of the surface layer having faces other than the (001) face (hereinafter, sometimes referred to as ab faces or edge faces), and faces other than the (001) face are faces where diffusion paths for lithium ions exist in a layered rock-salt crystal structure.
[0175] In FIG. 3(E), which shows a plane other than the (001) plane, the distribution of magnesium, etc., is shown as an example of the additive element X. Compared to the (001) plane in FIG. 3(C), the concentration of the additive element X may be higher in the plane other than the (001) plane in FIG. 3(E). The concentration peak of magnesium, etc. may be located on or near the surface of the surface layer 10a, and may show a higher intensity than the concentration peak in the (001) plane in FIG. 3(C). Furthermore, the additive element X may be distributed over a wide range in the plane other than the (001) plane in FIG. 3(E).
[0176] Figure 3(F) shows the distribution of aluminum as an example of an added element Y. It is preferable that the aluminum concentration peak is located in a region of 5 nm to 50 nm from the surface toward the inside, whether it is the (001) plane in Figure 3(D) or a plane other than the (001) plane in Figure 3(F). Depending on the heat treatment conditions, the aluminum concentration peak may be deeper in a plane other than the (001) plane in Figure 3(F) than in the (001) plane in Figure 3D.
[0177] In this manner, the distribution of the additive element may differ depending on the planar direction of the positive electrode active material.
[0178] Again, the diffusion path of lithium ions exists on the surface corresponding to a plane other than the (001) plane, and the diffusion path of lithium ions is exposed on the surface corresponding to a plane other than the (001) plane. Therefore, as shown in FIG. 3E and FIG. 3F, the surface layer portion 10a corresponding to the plane other than the (001) plane is an important region for maintaining the diffusion path of lithium ions, and at the same time, it is likely to become unstable because it is the region from which lithium ions are first desorbed. Therefore, in order to maintain the crystal structure of the entire positive electrode active material 10, it is preferable to preferentially reinforce the surface other than the (001) plane and the surface layer portion 10a corresponding thereto. In other words, it is preferable that the additive element A is preferentially present on the surface other than the (001) plane and the surface layer portion 10a corresponding thereto.
[0179] As described in the above manufacturing method, if the additive element is mixed into LiCoO2 formed through initial heating and then heated, the additive element spreads through the diffusion path of lithium ions. Therefore, it is easy to make the distribution of the additive element in the surface layer portion 10a corresponding to the surface other than (001) as shown in Figures 3(C) and 3(D) a preferable range.
[0180] Also, although it has been stated that the surface of the positive electrode active material 10 is preferably smooth and has few irregularities, the positive electrode active material 10 does not necessarily have to be entirely smooth. For example, the positive electrode active material 10 may have irregularities due to slip occurring on a surface parallel to the (001) plane, for example, on a surface where lithium is arranged. Slip is also called stacking fault. For example, pressing is performed when making a positive electrode, and the LiCoO2 may be deformed along the lattice fringe direction (ab-plane direction) by the pressing, and this deformation is also included in slip. Deformation includes the shifting of the lattice fringes back and forth. When the lattice fringes shift back and forth, a step occurs on the surface in the direction perpendicular to the lattice fringes (c-axis direction).
[0181] Furthermore, the surface resulting from the slip and its surface layer 10a are often (001) faces, and the surface layer 10a corresponding to the (001) face may not have any added elements or may have elements below the detection limit. As mentioned above, the (001) face does not expose the diffusion path of lithium ions and is relatively stable, so there is almost no problem even if the added elements do not exist or are below the detection limit.
[0182] In a composite oxide with a composition of LiCoO2 and a layered rock-salt type crystal structure of R-3m, cobalt is arranged parallel to the (001) plane. In addition, in a High-Angle Annular Dark Field Scanning TEM (HAADF-STEM) image, cobalt, which has the highest atomic number in LiCoO2, has the highest brightness. Therefore, in a HAADF-STEM image, the arrangement of atoms with high brightness can be considered to be the arrangement of cobalt. The repetition of this arrangement of high brightness is synonymous with crystal fringes or lattice fringes.
[0183] Next, the additive elements will be described. Magnesium, which is one of the additive elements X, is divalent, and since magnesium ions are more stable at the lithium site than at the cobalt site in the layered rock-salt crystal structure, they are more likely to enter the lithium site. The presence of magnesium at an appropriate concentration at the lithium site of the surface layer portion 10a makes it easier to reinforce the layered rock-salt crystal structure of the bulk portion 10b, etc. This is presumably because the magnesium present at the lithium site functions as a pillar supporting the CoO2 layers. In addition, the presence of magnesium enhances the Li x When x in CoO2 is, for example, 0.24 or less, the detachment of oxygen from around magnesium can be suppressed. In addition, the presence of magnesium is expected to increase the density of the positive electrode active material 10. In addition, if the magnesium concentration in the surface layer portion 10a is high, it is expected that the corrosion resistance against hydrofluoric acid generated by decomposition of the organic solvent will be improved.
[0184] If magnesium is present at an appropriate concentration, it does not adversely affect the insertion and desorption of lithium during charging and discharging, and the above-mentioned benefits can be enjoyed. However, if there is an excess of magnesium, it may adversely affect the insertion and desorption of lithium. Furthermore, the effect of stabilizing the crystal structure may be reduced. This is thought to be because magnesium enters the cobalt site in addition to the lithium site. In addition, unnecessary magnesium compounds (oxides, fluorides, etc.) that do not substitute for either the lithium site or the cobalt site may segregate on the surface of the positive electrode active material, and may become resistance components of the lithium-ion battery. In addition, as the magnesium concentration of the positive electrode active material increases, the discharge capacity of the positive electrode active material may decrease. This is thought to be because too much magnesium enters the lithium site, reducing the amount of lithium that contributes to charging and discharging.
[0185] Therefore, it is preferable that the amount of magnesium contained in the entire positive electrode active material 10 is appropriate. For example, the number of magnesium atoms is preferably 0.001 times or more and 0.1 times or less than the number of cobalt atoms, more preferably more than 0.01 times and less than 0.04 times, and even more preferably about 0.02 times. The amount of magnesium contained in the entire positive electrode active material 10 may be a value obtained by performing an elemental analysis of the entire positive electrode active material 10 using, for example, GD-MS (glow discharge mass spectrometry) or ICP-MS (inductively coupled plasma mass spectrometry), or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material 10.
[0186] Nickel, which is one of the additive elements X, can exist on either the cobalt site or the lithium site. When nickel exists on the cobalt site, it has a lower redox potential than cobalt, which leads to an increase in discharge capacity, which is preferable.
[0187] In addition, when nickel is present at the lithium site, it can suppress the shift of the layered structure consisting of octahedra of cobalt and oxygen. It also suppresses the change in volume caused by charging and discharging. It also increases the elastic modulus, i.e., makes the battery harder. This is presumably because the nickel present at the lithium site also functions as a pillar supporting the CoO2 layers.
[0188] On the other hand, an excess of nickel is undesirable because it increases the influence of distortion due to the Jahn-Teller effect, and may also adversely affect the insertion and extraction of lithium.
[0189] Therefore, the amount of nickel contained in the entire positive electrode active material 10 is preferably an appropriate amount. For example, the number of nickel atoms contained in the positive electrode active material 10 is preferably higher than 0% and less than 7.5% of the number of cobalt atoms, preferably 0.05% to 4%, preferably 0.1% to 2%, and more preferably 0.2% to 1%. Alternatively, it is preferably higher than 0% and less than 4%. Alternatively, it is preferably higher than 0% and less than 2%. Alternatively, it is preferably 0.05% to less than 7.5%. Alternatively, it is preferably 0.05% to less than 2%. Alternatively, it is preferably 0.1% to less than 7.5%. Alternatively, it is preferably 0.1% to less than 4%. The amount of nickel shown here may be a value obtained by performing an elemental analysis of the entire positive electrode active material using, for example, GD-MS, ICP-MS, or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.
[0190] In addition, aluminum, which is one of the additive elements Y, can be present at the cobalt site in the layered rock salt crystal structure. Since aluminum is a typical trivalent element and its valence does not change, lithium around the aluminum is unlikely to move even during charging and discharging. Therefore, aluminum and the lithium around it function as columns and can suppress changes in the crystal structure. Aluminum also has the effect of suppressing the elution of surrounding cobalt and improving continuous charging resistance. In addition, since the Al-O bond is stronger than the Co-O bond, it is possible to suppress the detachment of oxygen around the aluminum. These effects improve the thermal stability. Therefore, the safety can be improved when the positive electrode active material having aluminum as an additive element is used in a lithium ion battery. In addition, it is possible to obtain a positive electrode active material 10 whose crystal structure is unlikely to collapse even when repeatedly charged and discharged.
[0191] Furthermore, it is preferable that aluminum, which is one of the additive elements Y, exists at a position slightly deeper than the surface (specifically, the aluminum concentration peak is in a region deeper than the concentration peak of the additive element X). Alternatively, it is preferable that the presence of aluminum, which is one of the additive elements Y, is confirmed in a region deeper than the deepest position where the presence of the additive element X is confirmed. This is because, since lithium existing near the aluminum substituted for the lithium site is fixed, if aluminum is substituted for the lithium site on the surface, there is a risk of blocking the diffusion path of lithium.
[0192] On the other hand, if aluminum is excessive, it may adversely affect the insertion and desorption of lithium. Therefore, it is preferable that the aluminum contained in the entire positive electrode active material 10 is an appropriate amount. For example, the number of aluminum atoms contained in the entire positive electrode active material 10 is preferably 0.05% to 4% of the number of cobalt atoms, preferably 0.1% to 2% and more preferably 0.3% to 1.5%. Alternatively, 0.05% to 2% is preferable. Alternatively, 0.1% to 4% is preferable. The amount contained in the entire positive electrode active material 10 may be, for example, a value obtained by performing elemental analysis of the entire positive electrode active material 10 using GD-MS, ICP-MS, etc., or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material 10.
[0193] In addition, fluorine, which is one of the additive elements X, is a monovalent anion, and when part of the oxygen is replaced by fluorine in the surface layer portion 10a, the lithium desorption energy is reduced. This is because the valence of the cobalt ion accompanying lithium desorption is changed from trivalent to tetravalent in the absence of fluorine, and from divalent to trivalent in the presence of fluorine, resulting in different oxidation-reduction potentials. Therefore, when part of the oxygen is replaced by fluorine in the surface layer portion 10a of the positive electrode active material 10, it can be said that desorption and insertion of lithium ions near the fluorine can occur smoothly. Therefore, when used in a lithium ion battery, it is possible to improve the charge / discharge characteristics, large current characteristics, etc. In addition, the presence of fluorine in the surface layer portion 10a having the surface that is in contact with the electrolyte can effectively improve the corrosion resistance against hydrofluoric acid. In addition, as described in a later embodiment, when the melting point of a fluoride such as lithium fluoride is lower than the melting point of another additive element source, it can function as a flux (also called a flux agent) that lowers the melting point of the other additive element source.
[0194] In addition, when the surface layer 10a contains both magnesium and nickel, there is a possibility that the divalent magnesium can exist more stably near the divalent nickel. x Even when x in CoO2 is small, the elution of magnesium can be suppressed, which can contribute to the stabilization of the surface layer portion 10a.
[0195] In addition, it is preferable to have additive elements with different distributions, such as additive element X and additive element Y, in order to stabilize the crystal structure in a wider region. For example, when the positive electrode active material 10 has both magnesium and nickel as additive element X and aluminum as additive element Y, it is possible to stabilize the crystal structure in a wider region than when it has only one of additive element X and additive element Y. In this way, when the positive electrode active material 10 has both additive element X and additive element Y, the additive element Y, such as aluminum, is not essential for the surface, since the additive element X, such as magnesium, can sufficiently stabilize the surface. Rather, it is preferable for aluminum to be distributed widely in a deep region, for example, in a region with a depth from the surface of 5 nm to 50 nm, in order to stabilize the crystal structure in a wider region.
[0196] When a plurality of additive elements are contained as described above, the effects of the respective additive elements are synergistic and can contribute to further stabilization of the surface layer portion 10a. In particular, when magnesium, nickel and aluminum are contained, the effect of providing a stable composition and crystal structure is high and it is preferable.
[0197] However, if the surface layer 10a is occupied only by a compound of the additive element and oxygen, it is not preferable because it makes it difficult to insert and remove lithium. For example, it is not preferable that the surface layer 10a is occupied only by MgO, a structure in which MgO and NiO(II) are solid-solved, and / or a structure in which MgO and CoO(II) are solid-solved. Therefore, it is preferable that the surface layer 10a contains at least cobalt and also contains lithium in a discharged state, so that a path for insertion and removal of lithium is secured.
[0198] In order to ensure sufficient paths for lithium insertion and desorption, the surface layer 10a preferably has a higher cobalt concentration than magnesium. The surface layer 10a preferably has a higher cobalt concentration than nickel. The surface layer 10a preferably has a higher cobalt concentration than aluminum. The surface layer 10a preferably has a higher cobalt concentration than fluorine.
[0199] Furthermore, since there is a concern that an excessive amount of nickel may hinder the diffusion of lithium, it is preferable that the surface layer portion 10a has a higher concentration of magnesium than nickel.
[0200] In addition, it is preferable that some of the additive elements, especially magnesium and nickel, are present at a higher concentration in the surface layer portion 10a than in the bulk portion 10b, and that they are also present randomly and dilutely in the bulk portion 10b. It is also preferable that aluminum, which is one of the additive elements, is also present randomly and dilutely in the bulk portion 10b. When magnesium and aluminum are present at an appropriate concentration in the lithium site of the bulk portion 10b, it has the effect of making it easier to maintain the layered rock salt type crystal structure as described above. When nickel is present at an appropriate concentration in the bulk portion 10b, it is possible to suppress the deviation of the layered structure consisting of octahedra of cobalt and oxygen as described above. When magnesium and nickel are present together, a synergistic effect of suppressing the elution of magnesium can be expected as described above.
[0201] In addition, it is preferable that the crystal structure of lithium cobalt oxide changes continuously from the bulk portion 10b toward the surface portion 10a due to the concentration gradient of the added element. In this case, it is preferable that the surface portion 10a has a composition and crystal structure that are more stable at room temperature (25°C) than the bulk portion 10b. For example, it is preferable that at least a part of the surface portion 10a of the positive electrode active material 10 that can be used as one embodiment of the present invention has a rock salt type crystal structure. Alternatively, it is preferable that the surface portion 10a has both a layered rock salt type crystal structure and a rock salt type crystal structure. Alternatively, it is preferable that the surface portion 10a has the characteristics of both a layered rock salt type crystal structure and a rock salt type crystal structure.
[0202] In addition, it is preferable that the crystal orientation of the surface layer portion 10a and the bulk portion 10b is approximately the same due to the concentration gradient of the added element, or that the surface layer portion 10a and the bulk portion 10b are topotaxy.
[0203] In this specification, topotaxis refers to a three-dimensional structural similarity in which the crystal orientations roughly match, or to a crystallographically identical orientation, whereas epitaxy refers to a structural similarity of a two-dimensional interface.
[0204] The topotaxis between the surface layer portion 10a and the bulk portion 10b can reduce the distortion of the crystal structure and / or the deviation of the atomic arrangement. This can suppress the cause of pits. In this specification, the term "pit" refers to a hole formed by the progression of defects in the positive electrode active material.
[0205] <Li x When x in CoO2 is small≫ The positive electrode active material 10 that can be used as one embodiment of the present invention has the above-mentioned distribution of the added elements and / or crystal structure, and therefore, in the charged state, that is, Li x The crystal structure when x in CoO2 is small is different from that of conventional positive electrode active materials. <x≦0.24をいうこととする。
[0206] First, conventional Li x Lithium cobalt oxide with x=0.5, which corresponds to a slightly smaller value for CoO2, has a crystal structure that has high lithium symmetry and belongs to the monoclinic space group P2 / m, as shown in Figure 5. This structure has one CoO2 layer in the unit cell. Therefore, it is sometimes called monoclinic O1 type, or O1 type. In Figure 5, the crystal structure with x=0.5 is labeled P2 / m (monoclinic O1).
[0207] In addition, conventional Li x In CoO2, lithium cobalt oxide when x=0 has a crystal structure of trigonal space group P-3m1 as shown in Figure 5, with one CoO2 layer in the unit cell. Therefore, this crystal structure is sometimes called trigonal O1 type, or O1 type. In addition, the trigonal crystal is sometimes converted to a composite hexagonal lattice and called hexagonal O1 type. In Figure 5, the crystal structure when x=0 is labeled P-3m1 (trigonal O1).
[0208] In addition, conventional Li xLithium cobalt oxide when x=0.12, which corresponds to a small value in CoO2, has a crystal structure of space group R-3m as shown in FIG. 5. This structure can be said to be a structure in which a trigonal O1 type CoO2 structure and an R-3m(O3) LiCoO2 structure are alternately stacked. Therefore, this crystal structure is sometimes called an H1-3 type crystal structure. In reality, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is twice that of other structures. However, in FIG. 5 and other documents, the c-axis of the H1-3 type crystal structure is shown as 1 / 2 of the unit cell in order to make it easier to compare with other crystal structures. In FIG. 5, the crystal structure with x=0.12 is labeled R-3m1(H1-3).
[0209] The H1-3 type crystal structure can be expressed by the coordinates of cobalt and oxygen in the unit cell as Co(0,0,0.42150±0.00016), O1(0,0,0.27671±0.00045), and O2(0,0,0.11535±0.00045). O1 and O2 are oxygen atoms. Which unit cell should be used to express a certain crystal structure can be determined, for example, by Rietveld analysis of X-ray diffraction (XRD). In the Rietveld analysis, the unit cell with the smallest GOF (goodness of fit) value can be adopted.
[0210] Li that applies when x is small x When charging and discharging are repeated so that x in CoO2 becomes 0.12 or less, conventional lithium cobalt oxide repeatedly undergoes changes in crystal structure (i.e., non-equilibrium phase change) between the H1-3 type crystal structure and the R-3m(O3) structure in the discharged state, as shown in Figure 5.
[0211] However, these two crystal structures have a large deviation in the CoO2 layer. As shown by the dotted line and arrow in the crystal structure labeled R-3m1 (H1-3) in Figure 5, in the H1-3 type crystal structure, the CoO2 layer is significantly deviated from R-3m (O3) in the discharged state. Such dynamic structural changes can adversely affect the stability of the crystal structure.
[0212] Furthermore, the two crystal structures that cause dynamic structural changes also have a large difference in volume. When compared per the same number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the R-3m(O3) crystal structure in the discharged state is higher than 3.5%, typically 3.9% or more.
[0213] In addition, the H1-3 crystal structure, which has continuous CoO2 layers like the trigonal O1 type, is likely to be unstable.
[0214] Therefore, when charging and discharging are repeated so that x is 0.12 or less, the crystal structure of conventional lithium cobalt oxide collapses. The collapse of the crystal structure causes deterioration of cycle characteristics. This is because the collapse of the crystal structure reduces the number of sites where lithium can exist stably and makes it difficult to insert and remove lithium. Note that not only when charging and discharging are repeated so that x is 0.12 or less, but also when x is 0.24 or less, the collapse of the crystal structure often occurs, causing deterioration of cycle characteristics. For this reason, in practical use, conventional lithium cobalt oxide is repeatedly charged and discharged in lithium-ion batteries while controlling x to a value greater than 0.24.
[0215] On the other hand, the positive electrode active material 10 shown in FIG. 4 and usable as one embodiment of the present invention is Li x The change in the crystal structure between the discharge state where x in CoO2 is 1 and the state where x is 0.24 or less, or the state where x is 0.15, is smaller than that of conventional positive electrode active materials. Specifically, the positive electrode active material 10 can reduce the shift of the CoO2 layer between the state where x is 1 and the state where x is 0.24 or less. The positive electrode active material 10 can also reduce the change in volume compared per cobalt atom. Therefore, the positive electrode active material 10 is less likely to lose its crystal structure even when repeated charging and discharging such that x is 0.24 or less is performed, and excellent cycle characteristics can be achieved. The positive electrode active material 10 also has a low resistance to Li x When x in CoO2 is 0.24 or less, the positive electrode active material 10 can have a more stable crystal structure than the conventional positive electrode active material.x When the state where x in CoO₂ is 0.24 or less is maintained, short circuits are less likely to occur, thus improving the safety of the lithium-ion battery.
[0216] FIG. 4 shows the crystal structures of the positive electrode active material 10 when 0.1 < x ≦ 0.24, x = 0.2, and x = 0.15. The positive electrode active material 10 has a crystal structure different from the H1-3 type crystal structure of conventional lithium cobaltate when x = 0.2 and x = 0.15.
[0217] Specifically, the positive electrode active material 10 when x = 0.2 has a crystal structure belonging to the trigonal space group R-3m. This is because the symmetry of the CoO₂ layer is the same as that of O3. Therefore, in this specification and the like, this crystal structure will be referred to as the "O3' type crystal structure". In FIG. 4, R-3m(O3)' is attached to the crystal structure of x = 0.2. Although the O3' type crystal structure of the positive electrode active material 10 has been described as the case of x = 0.2, if x is about 0.2, it can be an O3' type crystal structure. That x is about 0.2 can be expressed as, for example, 0.18 ≦ x ≦ 0.24, typically 0.18 ≦ x ≦ 0.22.
[0218] The O3' type crystal structure can show the coordinates of cobalt and oxygen in the unit cell within the range of Co(0,0,0.5), O(0,0,x), 0.20 ≦ x ≦ 0.25. Also, the lattice constant a of the unit cell is preferably 0.2797 ≦ a ≦ 0.2837 (nm), more preferably 0.2807 ≦ a ≦ 0.2827 (nm), and typically a = 0.2817 (nm). Also, the lattice constant c is preferably 1.368 ≦ c ≦ 1.388 (nm), more preferably 1.375 ≦ c ≦ 1.381 (nm), and typically c = 1.378 (nm).
[0219] Further, as an example of 0.1 < x ≤ 0.24, when x = 0.15, the positive electrode active material 10 has a crystal structure belonging to the monoclinic space group P2 / m. This means that there is one CoO2 layer in the unit cell. Therefore, in this specification and the like, this crystal structure shall be referred to as the "monoclinic O1(15)-type crystal structure". In Fig. 4, P2 / m (monoclinic O1(15)) is attached to the crystal structure with x = 0.15. Although the monoclinic O1(15)-type crystal structure of the positive electrode active material 10 has been described for the case of x = 0.15, if x is about 0.15, it can be a monoclinic O1(15)-type crystal structure. That x is about 0.15 can be expressed as, for example, 0.13 ≤ x ≤ 0.24, typically 0.13 ≤ x ≤ 0.18.
[0220] The monoclinic O1(15)-type crystal structure shows the coordinates of cobalt and oxygen in the unit cell as Co1(0.5, 0, 0.5), Co2(0, 0.5, 0.5), O1(X O1 , 0, Z O1 ), 0.23 ≤ X O1 ≤ 0.24, 0.61 ≤ Z O1 ≤ 0.65, O2(X O2 , 0.5, Z O2 ), 0.75 ≤ X O2 ≤ 0.78, 0.68 ≤ Z O2 ≤ 0.71, within the range. Also, the lattice constant a of the unit cell is a = 0.488 ± 0.001 (nm), the lattice constant b is b = 0.282 ± 0.001 (nm), and c = 0.484 ± 0.001 (nm). The angles indicating the monoclinic crystal are α = 90°, β = 109.58 ± 0.01°, and γ = 90°.
[0221] Note that this crystal structure can also be fitted with the space group R-3m with a certain degree of error allowed. In this case, the coordinates of cobalt and oxygen in the unit cell can be shown within the range of Co(0, 0, 0.5), O(0, 0, Z O ), 0.21 ≤ Z O ≤ 0.23. Also, the lattice constant a of the unit cell is a = 0.2817 ± 0.002 (nm), and the lattice constant c is c = 1.368 ± 0.002 (nm).
[0222] In both the O3' and monoclinic O1(15) crystal structures, ions of cobalt, nickel, magnesium, etc. occupy six oxygen coordination positions, although light elements such as lithium may occupy four oxygen coordination positions.
[0223] As shown by the dotted line along the edge of the CoO2 layer in Figure 4, there is almost no deviation of the CoO2 layer between R-3m(O3) in the discharged state and the O3'-type crystal structure and the monoclinic O1(15)-type crystal structure. The difference in volume per the same number of cobalt atoms between R-3m(O3) in the discharged state and the O3'-type crystal structure is 2.5% or less, more specifically 2.2% or less, typically 1.8%. The difference in volume per the same number of cobalt atoms between R-3m(O3) in the discharged state and the monoclinic O1(15)-type crystal structure is 3.3% or less, more specifically 3.0% or less, typically 2.5%.
[0224] The positive electrode active material 10 is Li x It can be seen that when x in CoO2 is small, that is, when a large amount of lithium is released, the change in the crystal structure is suppressed more than in conventional positive electrode active materials. In addition, the change in volume is also suppressed when compared per the same number of cobalt atoms. Therefore, it can be seen that the crystal structure of the positive electrode active material 10 is not easily broken even when charging and discharging are repeated such that x is 0.24 or less, and the decrease in the charge and discharge capacity during the charge and discharge cycle is suppressed. In addition, since more lithium can be stably used than in conventional positive electrode active materials, the positive electrode active material 10 has a large discharge capacity per weight and per volume. Therefore, by using the positive electrode active material 10, a lithium ion battery with a high discharge capacity per weight and per volume can be produced.
[0225] The positive electrode active material 10 is Li x It has been confirmed that when x in CoO2 is 0.15 or more and 0.24 or less, it may have an O3' type crystal structure, and it is presumed that even when x is more than 0.24 and 0.27 or less, it has an O3' type crystal structure. xIt has been confirmed that when x in CoO2 is greater than 0.1 and less than 0.2, typically between 0.13 and 0.18, it may have a monoclinic O1(15) type crystal structure. However, the crystal structure is similar to that of Li x Since it is affected by not only x in CoO2 but also the number of charge / discharge cycles, charge / discharge current, temperature, electrolyte, etc., it is not necessarily limited to the above range of x.
[0226] For this reason, the positive electrode active material 10 is Li x When x in CoO2 is greater than 0.1 and equal to or less than 0.24, it may have only the O3' type crystal structure, may have only the monoclinic O1(15) type, or may have both crystal structures. The bulk portion 10b of the positive electrode active material 10 does not have to have the O3' type and / or the monoclinic O1(15) type crystal structure entirely. It may contain other crystal structures, or may be partially amorphous.
[0227] Also, Li x In order to make the x in CoO2 small, it is generally necessary to charge at a high charging voltage. x The state where x in CoO2 is small can be said to be a state where the material is charged at a high charging voltage. In other words, the positive electrode active material 10 is preferable because it can maintain the R-3m(O3) crystal structure even when it is charged at a high charging voltage, for example, a voltage of 4.6V or more at 25°C. In other words, the positive electrode active material 10 is preferable because it can take an O3' type crystal structure when it is charged at a higher charging voltage, for example, a voltage of 4.65V or more and 4.7V or less at 25°C. In other words, the positive electrode active material 10 is preferable because it can take a monoclinic O1(15) type crystal structure when it is charged at an even higher charging voltage, for example, a voltage of more than 4.7V and 4.8V or less at 25°C.
[0228] When the charging voltage is further increased, the H1-3 type crystal may be observed in the positive electrode active material 10. As described above, the crystal structure is affected by the number of charge / discharge cycles, the charge / discharge current, the electrolyte, etc., so that the positive electrode active material 10 usable as one embodiment of the present invention may have an O3' type crystal structure even when the charging voltage is lower, for example, at 4.5 V or more and less than 4.6 V at 25° C. Similarly, when the positive electrode active material 10 is charged at a voltage of 4.65 V or more and 4.7 V or less at 25° C., the positive electrode active material 10 may have a monoclinic O1(15) type crystal structure.
[0229] In addition, when graphite is used as the negative electrode active material in a lithium ion battery, the voltage of the lithium ion battery is lower than the above by the potential of the graphite. The potential of graphite is about 0.01 V to 0.7 V based on the potential of lithium metal. Therefore, in the case of a lithium ion battery using graphite as the negative electrode active material, the same crystal structure is obtained at a voltage obtained by subtracting the potential of graphite from the above voltage.
[0230] In addition, in the O3' type crystal structure and the monoclinic O1(15) type crystal structure in Figure 4, lithium is shown to exist at all lithium sites with equal probability, but this is not limited to this. Lithium may exist biasedly at some of the lithium sites. The distribution of lithium can be analyzed, for example, by neutron diffraction.
[0231] It can also be said that the O3' type crystal structure and the monoclinic O1(15) type crystal structure have random lithium between the layers, but are similar to the CdCl2 type crystal structure. This CdCl2 type-like crystal structure is similar to the CdCl2 type crystal structure, but the lithium nickel oxide is Li 0.06 Although the crystal structure is close to that when charged to NiO2, it is known that pure lithium cobalt oxide or layered rock salt type positive electrode active materials containing a large amount of cobalt do not usually adopt a CdCl2 type crystal structure.
[0232] In addition, it is preferable that the concentration gradient of the additive element is the same in multiple locations of the surface layer 10a of the positive electrode active material 10. In other words, it is preferable that the reinforcement derived from the additive element is present homogeneously in the surface layer 10a. Even if a part of the surface layer 10a is reinforced, if there is a part without reinforcement, stress may be concentrated in the part without reinforcement. If stress is concentrated in a part of the positive electrode active material 10, defects such as cracks may occur there, which may lead to cracking of the positive electrode active material and a decrease in discharge capacity. However, it is not necessary that the additive element has the same concentration gradient in all of the surface layer 10a of the positive electrode active material 10.
[0233] <Grain Boundaries> The additive element contained in the positive electrode active material 10 that can be used as one embodiment of the present invention is preferably distributed as described above, and at least a part of the additive element is unevenly distributed in and near the crystal grain boundaries 15 as shown in FIG. 3(B).
[0234] For example, the magnesium concentration at and near the crystal grain boundaries 15 of the positive electrode active material 10 is preferably higher than that in other regions of the bulk portion 10b. The fluorine concentration at and near the crystal grain boundaries 15 is preferably higher than that in other regions of the bulk portion 10b. The nickel concentration at and near the crystal grain boundaries 15 is preferably higher than that in other regions of the bulk portion 10b. The aluminum concentration at and near the crystal grain boundaries 15 is preferably higher than that in other regions of the bulk portion 10b.
[0235] Since the grain boundaries 15 are one type of planar defect, they tend to become unstable like the surface, and changes in the crystal structure are likely to begin. By increasing the concentration of the additive element at and near the grain boundaries 15, such changes in the crystal structure can be more effectively suppressed.
[0236] Furthermore, when the magnesium concentration and fluorine concentration are high at and near the grain boundaries 15, even if cracks occur along the grain boundaries 15 of the positive electrode active material 10 usable as one embodiment of the present invention, the magnesium concentration and fluorine concentration become high near the surface caused by the cracks. Therefore, the corrosion resistance to hydrofluoric acid can be improved even in the positive electrode active material after the cracks occur.
[0237] <Analysis method> In a certain positive electrode active material, Li x When x in CoO2 is small, whether or not the positive electrode active material 10 that can be used as one embodiment of the present invention has an O3' type and / or monoclinic O1(15) type crystal structure is determined by Li x This can be determined by analyzing a positive electrode having a positive electrode active material in a charged state where x in CoO2 is small, using XRD, electron beam diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc.
[0238] In particular, XRD is preferred in that it can analyze the symmetry of transition metals such as cobalt contained in the positive electrode active material with high resolution, can compare the degree of crystallinity and the orientation of the crystals, can analyze the periodic distortion of the lattice and the crystallite size, can obtain sufficient accuracy even when the positive electrode obtained by disassembling the lithium ion battery is measured as it is, etc. Among XRD, powder XRD can obtain diffraction peaks that reflect the crystal structure of the bulk part 10b of the positive electrode active material 10, which occupies most of the volume of the positive electrode active material 10.
[0239] When the measurement sample is a powder, this is sometimes called the powder XRD measurement, and the powder can be set by placing it in a glass sample holder, sprinkling the sample on a greased silicone anti-reflective plate, etc. When the measurement sample is a positive electrode, the positive electrode can be attached to a substrate with double-sided tape, and the positive electrode active material layer can be set to match the measurement surface required by the device.
[0240] Furthermore, even in the case of a cathode active material 10 that can be used as an embodiment of the present invention, if x is too small, such as 0.1 or less, or under conditions where the charging voltage exceeds 4.9 V, an H1-3 type or trigonal O1 type crystal structure may be generated. Therefore, in order to determine whether or not a cathode active material 10 can be used as an embodiment of the present invention, analysis of the crystal structure, such as XRD, and information on the charging capacity or charging voltage, etc. are required.
[0241] In addition, when the positive electrode active material has a small x, the crystal structure may change when it is exposed to air. For example, the crystal structure may change from O3' type or monoclinic O1(15) type to H1-3 type. Therefore, it is preferable to handle all samples used for analyzing the crystal structure in an inert atmosphere such as an argon atmosphere.
[0242] In addition, whether or not the distribution of an additive element in a certain positive electrode active material is in the state described above can be determined by analyzing it using, for example, XPS, energy dispersive X-ray spectroscopy (EDX), electron probe micro analysis (EPMA), or the like.
[0243] The crystal structure of surface layer 10a, crystal grain boundaries 15, etc. can be analyzed by electron beam diffraction of a cross section of positive electrode active material 10, or the like.
[0244] <Evaluation conditions> An example of an evaluation condition for determining whether a certain composite oxide is a positive electrode active material 10 that can be used as an embodiment of the present invention is to prepare a coin cell (e.g., CR2032 type, diameter 20 mm, height 3.2 mm) having lithium metal as a counter electrode and charge it under predetermined conditions. Also, an example of an evaluation condition for determining whether a certain electrolyte is an electrolyte that can be used as an embodiment of the present invention is to prepare a coin cell (e.g., CR2032 type, diameter 20 mm, height 3.2 mm) having lithium metal as a counter electrode and charge it under predetermined conditions.
[0245] The procedure 1 described below is an example for confirming the physical properties of the positive electrode active material 10 that can be used as one embodiment of the present invention. Therefore, the electrolyte has a different configuration from that of the lithium ion battery that is one embodiment of the present invention.
[0246] <Evaluation Procedure 1> A lithium ion battery is disassembled, the electrolyte-impregnated positive electrode is removed, and the positive electrode is punched out to a size that fits into a prepared coin cell. The positive electrode contains a conductive material and a binder in addition to the positive electrode active material. The electrolyte and the like are removed before punching out the positive electrode. For example, after removing the positive electrode, the positive electrode may be washed using an organic solvent or the like.
[0247] The coin cell has lithium metal as a counter electrode. However, the counter electrode may be made of a material other than lithium metal. Unless otherwise specified, the potential in this specification is the potential of the positive electrode when the counter electrode is lithium metal.
[0248] The coin cell has a 25 μm thick porous polypropylene film as a separator.
[0249] The coin cell uses stainless steel (SUS) for the positive electrode can and stainless steel (SUS) for the negative electrode can.
[0250] In this manner, a coin cell A for evaluation is prepared.
[0251] The coin cell A for evaluation prepared under the above conditions is charged at a constant current (also called CC charging) of 10 mA / g (equivalent to 0.05 C when 1 C is 200 mA / g of positive electrode active material weight) to an arbitrary voltage (for example, 4.5 V, 4.55 V, 4.6 V, or 4.65 V, 4.7 V, 4.75 V, 4.8 V). In order to observe the phase change of the positive electrode active material, it is desirable to charge at such a small current value.
[0252] The temperature during charging of the evaluation coin cell A may be 25° C. The temperature during charging may be the temperature of the thermostatic bath in which the coin cell A is placed.
[0253] After charging under such conditions, the coin cell A is disassembled in a glove box in an argon atmosphere to remove the positive electrode, thereby obtaining a positive electrode active material with an arbitrary charging capacity. When various analyses are performed thereafter, it is preferable to seal the cell in an argon atmosphere in order to suppress reactions with external components. For example, XRD can be performed by sealing the cell in a sealed container in an argon atmosphere. In addition, it is preferable to remove and analyze the positive electrode promptly after charging is completed. Specifically, it is preferable to do so within 1 hour after charging is completed, and more preferably within 30 minutes.
[0254] <Evaluation Procedure 2> A lithium-ion battery is disassembled, the positive electrode impregnated with electrolyte is taken out, and the electrolyte is analyzed by nuclear magnetic resonance (e.g. 1 Measurements using 1H NMR are carried out to identify at least the organic solvent. Using the nuclear magnetic resonance method, the mixing ratio (volume ratio) of the organic solvent can also be identified. In addition, it is possible to identify the lithium salt and additives contained in the electrolyte. The additive forms a film on the positive electrode active material. If the amount of additive is small, it may be consumed completely during charging and discharging, become a film, and no longer exist in the electrolyte.
[0255] Then, the positive electrode is punched out to a size that fits into a coin cell. The positive electrode contains a conductive material and a binder in addition to the positive electrode active material. The electrolyte and the like are removed after the measurement by the nuclear magnetic resonance method and before the positive electrode is punched out. For example, after the positive electrode is taken out, the positive electrode may be washed with an organic solvent or the like.
[0256] The coin cell has lithium metal as the counter electrode, although materials other than lithium metal may also be used for the counter electrode.
[0257] The coin cell is prepared with an electrolyte that has been identified using a nuclear magnetic resonance method. The electrolyte is an electrolyte according to one embodiment of the present invention.
[0258] The coin cell has a 25 μm thick porous polypropylene film as a separator.
[0259] The coin cell uses stainless steel (SUS) for the positive electrode can and stainless steel (SUS) for the negative electrode can.
[0260] In this manner, a coin cell B for evaluation is prepared.
[0261] The coin cell B for evaluation prepared under the above conditions is charged to an arbitrary voltage (for example, 4.5V, 4.55V, 4.6V, or 4.65V, 4.7V, 4.75V, 4.8V) and then discharged. For the charging conditions, see the following examples. For the discharging conditions, see the following examples.
[0262] The charging temperature of the evaluation coin cell B can be set to 25°C and below freezing, and it can be confirmed how the charge / discharge capacity at below freezing corresponds to the charge / discharge capacity at 25°C.
[0263] <XRD> The XRD measurement of the coin cell A and the like can be performed using the following apparatus and conditions. Note that the XRD measurement apparatus and conditions are not limited to those described below. XRD equipment: Bruker AXS, D8 ADVANCE X-ray source: CuKα1 ray Output: 40KV, 40mA
[0264] <Powder XRD pattern> The ideal XRD patterns calculated from the O3' type crystal structure, the monoclinic O1(15) type crystal structure, and the H1-3 type crystal structure model are shown in Figures 6, 7, 8(A), and 8(B) using CuKα1 radiation. xThe ideal XRD patterns calculated from the crystal structure of LiCoO2 O3 with x=1 in CoO2 and trigonal O1 with x=0 are also shown. Figures 8(A) and 8(B) show the XRD patterns of O3' type, monoclinic O1(15) type, and H1-3 type. Figure 8(A) shows the XRD patterns of the region with 2θ ranging from 18° to 21°, and Figure 8(B) shows the XRD patterns of the region with 2θ ranging from 42° to 46°. The patterns of LiCoO2(O3) and CoO2(O1) were created using Reflex Powder Diffraction, one of the modules of Materials Studio (BIOVIA), from crystal structure information obtained from ICSD (Inorganic Crystal Structure Database). The range of 2θ was 15° to 75°, Step=0.01°, and wavelength λ1=1.540562×10 -10 m, and monochromator was single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 2. The patterns of the O3' type and monoclinic O1(15) type crystal structures were estimated from the XRD patterns of the positive electrode active material usable as one embodiment of the present invention, and fitted using TOPAS ver.3 (crystal structure analysis software manufactured by Bruker) to create XRD patterns in the same manner as the others.
[0265] As shown in Figures 6, 8(A), and 8(B), when the O3' type crystal structure is analyzed by X-ray diffraction, diffraction peaks appear at 2θ = 19.25 ± 0.12° (19.13° or more and less than 19.37°) and 2θ = 45.47 ± 0.10° (45.37° or more and less than 45.57°).
[0266] In addition, in the monoclinic O1(15) crystal structure, X-ray diffraction analysis reveals diffraction peaks at 2θ = 19.47 ± 0.10° (19.37° to 19.57°) and 2θ = 45.62 ± 0.05° (45.57° to 45.67°).
[0267] On the other hand, as shown in Figures 7, 8(A) and 8(B), no peaks appear at these positions in the H1-3 type crystal structure and trigonal O1. x The appearance of peaks at 19.13 or more and less than 19.37° and / or 19.37° or more and 19.57° or less, and at 45.37° or more and less than 45.57° and / or 45.57° or more and 45.67° or less when x in CoO2 is small can be said to be a characteristic of the positive electrode active material 10 that can be used as one embodiment of the present invention.
[0268] It can also be said that the positions at which XRD diffraction peaks appear are close between the crystal structures with x=1 and x≦0.24. More specifically, for the main diffraction peaks of the crystal structures with x=1 and x≦0.24 that appear at 2θ values between 42° and 46°, the difference in 2θ is 0.7° or less, more preferably 0.5° or less.
[0269] The positive electrode active material 10 that can be used in one embodiment of the present invention is Li x When x in CoO2 is small, it has O3'-type and / or monoclinic O1(15)-type crystal structure, but not all of it may be O3'-type and / or monoclinic O1(15)-type crystal structure. It may contain other crystal structures, or may be partially amorphous. However, when Rietveld analysis is performed on the XRD pattern, it is preferable that the O3'-type and / or monoclinic O1(15)-type crystal structure is 50% or more, more preferably 60% or more, and even more preferably 66% or more. If the O3'-type and / or monoclinic O1(15)-type crystal structure is 50% or more, more preferably 60% or more, and even more preferably 66% or more, it can be a positive electrode active material with sufficiently excellent cycle characteristics.
[0270] Furthermore, even after 100 or more charge / discharge cycles from the start of measurement, when Rietveld analysis is performed, the O3' type and / or monoclinic O1(15) type crystal structure is preferably 35% or more, more preferably 40% or more, and even more preferably 43% or more.
[0271] In addition, the sharpness of the diffraction peaks in the XRD pattern indicates the high crystallinity. Therefore, it is preferable that each diffraction peak after charging is sharp, that is, the half-width is narrow. The half-width varies depending on the XRD measurement conditions or the value of 2θ, even for peaks generated from the same crystal phase. In the case of the above-mentioned measurement conditions, in peaks observed at 2θ=43° or more and 46° or less, the half-width is preferably 0.2° or less, more preferably 0.15° or less, and even more preferably 0.12° or less. It is not necessary that all peaks meet this requirement. If some peaks meet this requirement, it can be said that the crystallinity of the crystal phase is high. Therefore, it contributes to stabilizing the crystal structure after charging sufficiently.
[0272] In addition, the crystallite size of the O3' type and monoclinic O1(15) crystal structures of the positive electrode active material 10 is reduced to only about 1 / 20 of that of LiCoO2(O3) in the discharged state. Therefore, even if the XRD measurement conditions are the same as those of the positive electrode before and after charging and discharging, the Li x When x in CoO2 is small, a clear peak of the O3' type crystal structure can be confirmed. On the other hand, in conventional LiCoO2, even if a part of it can have a structure similar to the O3' type crystal structure, the crystallite size becomes small and the peak becomes broad and small. The crystallite size can be calculated from the half-width of the XRD peak.
[0273] This embodiment mode can be freely combined with other embodiment modes.
[0274] (Embodiment 3) In this embodiment, a configuration other than the positive electrode active material and the electrolyte contained in the lithium ion battery will be described.
[0275] [Positive electrode] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and may further include at least one of a conductive additive and a binder. The positive electrode active material may be the same as that described in the first embodiment.
[0276] FIG. 9(A) shows an example of a schematic cross-sectional view of a positive electrode.
[0277] The current collector 550 can be, for example, a metal foil. The positive electrode can be formed by applying a slurry onto a metal foil and drying it. Note that pressing may be performed after drying. The positive electrode is formed by forming an active material layer on the current collector 550.
[0278] The slurry is a material liquid used for forming an active material layer on the current collector 550, and contains an active material, a binder, and a solvent, and preferably further contains a conductive assistant. The slurry is also called an electrode slurry or an active material slurry, and a positive electrode slurry is used when a positive electrode active material layer is formed, and a negative electrode slurry is also used when a negative electrode active material layer is formed.
[0279] The positive electrode active material 561 has a function of taking in and / or releasing lithium ions with charging and discharging. The positive electrode active material 561 used as one embodiment of the present invention can be a material that does not deteriorate much with charging and discharging even at high charging voltages. In this specification and the like, unless otherwise specified, the charging voltage is expressed based on the potential of lithium metal. In this specification and the like, a high charging voltage is, for example, a charging voltage of 4.6V or more, preferably 4.65V or more, more preferably 4.7V or more, even more preferably 4.75V or more, and most preferably 4.8V or more.
[0280] The positive electrode active material 561 used in one embodiment of the present invention can be any material that does not deteriorate much due to charging and discharging even at a high charging voltage, and can be any material described in embodiment 1 or embodiment 2. Note that the positive electrode active material 561 can be two or more materials with different particle sizes as long as the material does not deteriorate much due to charging and discharging even at a high charging voltage.
[0281] The conductive assistant is also called a conductive agent or conductive material, and may be a carbon material. By attaching the conductive assistant between a plurality of active materials, the plurality of active materials are electrically connected to each other, and the conductivity is increased. In this specification, the term "attachment" does not only refer to the physical adhesion between the active material and the conductive assistant, but also includes the case where a covalent bond is formed, the case where the conductive assistant is bonded by van der Waals forces, the case where the conductive assistant covers a part of the surface of the active material, the case where the conductive assistant is embedded in the surface irregularities of the active material, and the case where the conductive assistant is electrically connected even if they are not in contact with each other.
[0282] Specific examples of carbon materials that can be used as the conductive assistant include carbon black (furnace black, acetylene black, graphite, etc.).
[0283] FIG. 9(A) illustrates carbon black 553 as a conductive additive.
[0284] A binder (resin) may be mixed to bond a current collector 550 such as a metal foil and an active material to form a positive electrode of a lithium ion battery. The binder is also called a binding agent. The binder is a polymer material, and if a large amount of the binder is contained, the ratio of the active material in the positive electrode decreases, and the discharge capacity of the lithium ion battery decreases. Therefore, it is preferable to mix the binder in a minimum amount. In FIG. 9(A), the regions not filled with the positive electrode active material 561, the second active material 562, and the carbon black 553 indicate voids or binders.
[0285] 9A shows an example in which the positive electrode active material 561 is illustrated as a sphere, but is not particularly limited thereto. For example, the cross-sectional shape of the positive electrode active material 561 may be an ellipse, a rectangle, a trapezoid, a pyramid, a polygon with rounded corners, or an asymmetric shape. For example, FIG. 9B shows an example in which the positive electrode active material 561 has a polygonal shape with rounded corners.
[0286] 9B, graphene 554 is used as a carbon material used as a conductive additive. In FIG. 9B, a positive electrode active material layer including a positive electrode active material 561, graphene 554, and carbon black 553 is formed over a current collector 550.
[0287] In the step of mixing the graphene 554 and the carbon black 553 to obtain an electrode slurry, the weight of the carbon black to be mixed is preferably 1.5 to 20 times, more preferably 2 to 9.5 times, that of the graphene.
[0288] In addition, when the mixture of graphene 554 and carbon black 553 is within the above range, the dispersion stability of carbon black 553 is excellent during slurry preparation, and agglomeration is unlikely to occur. In addition, when the mixture of graphene 554 and carbon black 553 is within the above range, a higher electrode density can be achieved than a positive electrode using only carbon black 553 as a conductive additive. By increasing the electrode density, the capacity per unit weight can be increased. Specifically, the density of the positive electrode active material layer measured by weight can be 3.5 g / cc or more.
[0289] Although the electrode density is lower than that of a positive electrode using only graphene as a conductive additive, by mixing the first carbon material (graphene) and the second carbon material (acetylene black) within the above range, it can be used for rapid charging. Therefore, it is particularly effective when used as an in-vehicle lithium-ion battery.
[0290] Fig. 9C illustrates an example of a positive electrode using carbon fiber 555 instead of graphene. Fig. 9C illustrates an example different from Fig. 9B. When carbon fiber 555 is used, aggregation of carbon black 553 can be prevented and dispersibility can be improved.
[0291] In FIG. 9C, the regions not filled with the positive electrode active material 561, the carbon fibers 555, and the carbon black 553 indicate voids or binders.
[0292] Another example of the positive electrode is shown in Fig. 9(D). Fig. 9(C) shows an example in which carbon fiber 555 is used in addition to graphene 554. When both graphene 554 and carbon fiber 555 are used, aggregation of carbon black such as carbon black 553 can be prevented and dispersibility can be further improved.
[0293] Note that in FIG. 9D, regions that are not filled with the positive electrode active material 561, the carbon fibers 555, the graphene 554, and the carbon black 553 indicate voids or binders.
[0294] A lithium ion battery can be produced by using any one of the positive electrodes shown in Figures 9(A) to 9(D), stacking a separator on the positive electrode, placing the stack of the negative electrode on the separator in a container (outer packaging, metal can, etc.) that houses the stack, and filling the container with a liquid electrolyte.
[0295] <Binder> As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Also, as the binder, fluororubber can be used.
[0296] <Positive electrode current collector> As the current collector, a material having high electrical conductivity, such as metals such as stainless steel, gold, platinum, aluminum, and titanium, and alloys thereof, can be used. In addition, it is preferable that the material used for the positive electrode current collector does not dissolve at the potential of the positive electrode. In addition, an aluminum alloy to which an element that improves heat resistance, such as silicon, titanium, neodymium, scandium, or molybdenum, is added can be used. In addition, it may be formed of a metal element that reacts with silicon to form a silicide. Examples of the metal element that reacts with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector can be appropriately used in the form of a foil, plate, sheet, net, punched metal, or expanded metal. It is preferable to use a current collector having a thickness of 5 μm or more and 30 μm or less.
[0297] [Negative electrode] The negative electrode includes a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, and may further include a conductive assistant and a binder.
[0298] <Negative electrode active material> As the negative electrode active material, for example, an alloy material and / or a carbon material can be used.
[0299] The carbon material used for the negative electrode active material may be one or more selected from graphite, graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon fiber (carbon nanotube), graphene, carbon black, and the like.
[0300] Examples of the graphite include artificial graphite and natural graphite. Examples of the artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, as the artificial graphite, spherical graphite having a spherical shape can be used. For example, MCMB may have a spherical shape, which is preferable. In addition, it is relatively easy to reduce the surface area of MCMB, which may be preferable. Examples of the natural graphite include flake graphite and spheroidized natural graphite.
[0301] When lithium ions are inserted into graphite (when lithium-graphite intercalation compounds are formed), graphite exhibits a low potential similar to that of lithium metal (0.05 V to 0.3 V vs. Li / Li + ) This allows lithium-ion batteries using graphite to exhibit high operating voltages. In addition, graphite is preferred because it has the advantages of relatively high capacity per unit volume, relatively small volume expansion, low cost, and greater safety than lithium metal.
[0302] In addition, the negative electrode active material can be an element capable of carrying out a charge / discharge reaction by alloying / dealloying reaction with lithium. For example, one or more materials selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. Such elements have a larger capacity than carbon, and silicon in particular has a high theoretical capacity of 4200mAh / g. Compounds containing these elements may also be used. For example, SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb, SbSn, etc. Here, elements capable of carrying out charge / discharge reactions through alloying / dealloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloying materials.
[0303] In this specification, "SiO" refers to, for example, silicon monoxide. Alternatively, SiO may be SiO x Here, x preferably has a value of 1 or close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.
[0304] In addition, titanium dioxide (TiO2), lithium titanium oxide (Li4Ti5O 12 ), lithium-graphite intercalation compound (Li xC6), niobium pentoxide (Nb2O5), tungsten oxide (WO2), molybdenum oxide (MoO2), and the like can be used.
[0305] In addition, the negative electrode active material is Li3N-type Li, a complex nitride of lithium and transition metals. 3-x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N3 has a large discharge capacity (900mAh / g, 1890mAh / cm 3 ) and is preferred.
[0306] When a composite nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, and therefore it is preferable to combine it with a material that does not contain lithium ions, such as V2O5 or Cr3O8, as the positive electrode active material. Even when a material that contains lithium ions is used as the positive electrode active material, the composite nitride of lithium and a transition metal can be used as the negative electrode active material by first removing the lithium ions contained in the positive electrode active material.
[0307] In addition, materials that undergo a conversion reaction can also be used as the negative electrode active material. For example, transition metal oxides that do not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include oxides such as Fe2O3, CuO, Cu2O, RuO2, and Cr2O3, and CoS 0.89 It also occurs in sulfides such as NiS and CuS, nitrides such as Zn3N2, Cu3N and Ge3N4, phosphides such as NiP2, FeP2 and CoP3, and fluorides such as FeF3 and BiF3.
[0308] In addition, a combination of a plurality of the above-mentioned negative electrode active materials may be used, for example, a negative electrode active material in which graphite and silicon particles are mixed may be used. Silicon particles are silicon powder as a material for the negative electrode active material of a lithium ion secondary battery, and refer to those having an average particle size in the particle size distribution, i.e., an average particle size of about 100 nm, and may be called nanosilicon particles. The silicon particles used are preferably adjusted to a uniform particle size by crushing a silicon raw material. The silicon particles may contain at least one of silicon, silicon oxide, and silicon alloy. The particle size can be measured by a representative laser diffraction particle size distribution measurement, but is not limited to the laser diffraction particle size distribution measurement, and the major axis of the particle cross section may be measured by analysis such as SEM (scanning electron microscope) or TEM (transmission electron microscope).
[0309] The conductive additive and binder that the negative electrode active material layer can have can be the same materials as the conductive additive and binder that the positive electrode active material layer can have.
[0310] <Negative electrode current collector> The negative electrode current collector may be made of the same material as the positive electrode current collector, or may be made of copper, etc. Note that it is preferable to use a material that does not form an alloy with carrier ions such as lithium for the negative electrode current collector.
[0311] [Electrolyte] The electrolyte used can be the same as that described in the first embodiment.
[0312] [Separator] When the electrolyte contains a liquid electrolyte (also called an electrolyte solution), a separator is disposed between the positive electrode and the negative electrode. As the separator, for example, a separator formed of fibers having cellulose such as paper, nonwoven fabric, glass fiber, ceramics, or synthetic fibers using nylon (polyamide), vinylon (polyvinyl alcohol fiber), polypropylene (referred to as PP), polyimide (referred to as PI), polyester, acrylic, polyolefin, polyurethane, etc. can be used. The porosity of the separator in the thickness can be 35% to 90%, preferably 60% to 85%. The porosity of the separator using polypropylene can be 35% to 45%. The porosity of the separator using polyimide can be 75% to 85%. The thickness of the separator is preferably 10 μm to 80 μm, more preferably 20 μm to 60 μm. A separator using polyimide is preferable because it can have a high porosity and can be made thick (typically, the thickness is 50 μm or more and 60 μm or less).
[0313] The separator is preferably formed into a bag shape and disposed so as to encase either the positive electrode or the negative electrode.
[0314] The separator may have a multi-layer structure. For example, an organic material film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine material, a polyamide material, or a mixture of these. As the ceramic material, for example, aluminum oxide particles or silicon oxide particles may be used. As the fluorine material, for example, PVDF or polytetrafluoroethylene may be used. As the polyamide material, for example, nylon or aramid (meta-aramid or para-aramid) may be used.
[0315] By using a separator with a multi-layer structure, the safety of the lithium-ion battery can be maintained even if the overall thickness of the separator is thin, so the capacity per volume of the lithium-ion battery can be increased.
[0316] [Exterior body] The exterior body of the lithium ion battery can be made of a metal material such as aluminum or a resin material. A film-shaped exterior body can also be used. As the film, a three-layer structure film can be used in which a thin metal film having excellent flexibility such as aluminum, stainless steel, copper, nickel, etc. is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, polyamide, etc., and an insulating synthetic resin film such as a polyamide-based resin or polyester-based resin is further provided on the thin metal film as the outer surface of the exterior body.
[0317] This embodiment mode can be used in combination with other embodiment modes.
[0318] (Embodiment 4) In this embodiment, a lithium ion battery will be described as an example.
[0319] [Laminated lithium-ion battery] An example of a laminated lithium ion battery 100 is shown in Fig. 10(A) and Fig. 10(B). Fig. 10(A) and Fig. 10(B) are external views, and the lithium ion battery 100 has the electrolyte and separator (not shown in Fig. 10) described in the above embodiment, the negative electrode 106, and the positive electrode 107. In the lithium ion battery 100, the negative electrode 106 may have a larger area than the positive electrode 107. The lithium ion battery 100 further has a negative electrode lead electrode 510 electrically connected to the negative electrode 106, and a positive electrode lead electrode 511 electrically connected to the positive electrode 107. The electrolyte layer, the negative electrode 106, and the positive electrode 107 are housed in an exterior body 509, and a part of the negative electrode lead electrode 510 and a part of the positive electrode lead electrode 511 protrude from the exterior body 509. A bonding area 508 is provided on a part of the outer periphery of the exterior body 509. Fig. 10(A) shows an example in which the negative lead electrode 510 and the positive lead electrode 511 protrude from the same side of the exterior body 509, and the adhesive region 508 is located at least on the side from which each lead electrode protrudes and two sides adjacent to the side. Fig. 10(B) shows an example in which the side from which the negative lead electrode 510 protrudes from the exterior body 509 and the side from which the positive lead electrode 511 protrudes from the exterior body 509 face each other, and the adhesive region 508 is located at least on the two sides from which each lead electrode protrudes and one side sandwiched between the two sides. In Figs. 10(A) and 10(B), the side on which the adhesive region 508 is not located may correspond to the side on which the exterior body 509 is folded.
[0320] When the electrolyte and positive electrode active material of the present invention are used in the laminated lithium ion battery 100, excellent charge and discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.
[0321] [Coin-type lithium-ion battery] An example of a coin-type lithium ion battery will be described. FIG. 11(A) is an exploded perspective view of a coin-type (single-layer flat) lithium ion battery, FIG. 11(B) is an external view, and FIG. 11(C) is a cross-sectional view thereof. Coin-type lithium ion batteries are mainly used in small electronic devices. In this specification and the like, coin-type lithium ion batteries include button-type lithium ion batteries.
[0322] In order to make it easier to understand, Fig. 11(A) is a schematic diagram showing the overlapping of components (upper and lower relationships and positional relationships). Therefore, Fig. 11(A) and Fig. 11(B) are not completely corresponding views.
[0323] 11(A) shows a state in which the positive electrode 304, the negative electrode 307, the spacer 342, and the washer 332 are overlapped and sealed with the negative electrode can 302 and the positive electrode can 301. Note that the electrolyte and the separator described in the above embodiment are not shown in FIG. 11(A). The spacer 342 and the washer 332 are used to protect the inside or to fix the position inside the can when the positive electrode can 301 and the negative electrode can 302 are crimped together. The spacer 342 or the washer 332 is made of stainless steel or an insulating material.
[0324] A laminated structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 is used as a positive electrode 304 .
[0325] FIG. 11(B) is a perspective view of the completed coin-type lithium-ion battery 100.
[0326] In the coin-type lithium-ion battery 100, a positive electrode can 301 also serving as a positive electrode terminal and a negative electrode can 302 also serving as a negative electrode terminal may be insulated and sealed with a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed of a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.
[0327] In addition, the positive electrode 304 and the negative electrode 307 used in the coin-type lithium ion battery 100 each need only have an active material layer formed on one side.
[0328] As shown in FIG. 11(C), positive electrode can 301 is placed at the bottom, and positive electrode 304, negative electrode 307, and negative electrode can 302 are stacked in this order, and positive electrode can 301 and negative electrode can 302 are crimped together via gasket 303 to produce coin-shaped lithium ion battery 100.
[0329] When the electrolyte and positive electrode active material of the present invention are used in the coin-type lithium ion battery 100, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.
[0330] [Cylindrical lithium-ion battery] An example of a cylindrical lithium ion battery will be described with reference to Fig. 12(A). As shown in Fig. 12(A), a cylindrical lithium ion battery 616 has a positive electrode cap (battery lid) 601 on the top surface, and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap 601 and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0331] Fig. 12(B) is a schematic diagram showing a cross section of a cylindrical lithium ion battery. The cylindrical lithium ion battery shown in Fig. 12(B) has a positive electrode cap (battery lid) 601 on the top surface, and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0332] A battery element is provided inside a hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with an electrolyte layer 605 sandwiched therebetween. Although not shown, the battery element is wound around a central axis. One end of the battery can 602 is closed and the other end is open. Inside the battery can 602, the battery element in which the positive electrode, the negative electrode, and the separator are wound is sandwiched between a pair of opposing insulating plates 608 and 609. An electrolyte (not shown) according to one embodiment of the present invention is injected into the inside of the battery can 602 in which the battery element is provided.
[0333] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form active materials on both sides of the current collector. Although the lithium ion battery 616 in which the height of the cylinder is greater than the diameter of the cylinder is illustrated in Figures 12(A) to 12(D), this is not limited to this. A lithium ion battery in which the diameter of the cylinder is greater than the height of the cylinder may also be used. With such a configuration, for example, the lithium ion battery can be made smaller.
[0334] A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of a metal material such as aluminum. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 613, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cap 601 via a PTC element (Positive Temperature Coefficient) 611. The safety valve mechanism 613 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the increase in the internal pressure of the battery exceeds a predetermined threshold value. The PTC element 611 is a thermosensitive resistor element whose resistance increases when the temperature increases, and the increase in resistance limits the amount of current to prevent abnormal heat generation. The PTC element can be made of barium titanate (BaTiO3)-based ceramic material or the like.
[0335] 12C shows an example of a power storage system 615. The power storage system 615 has a plurality of lithium ion batteries 616 and may be called a battery pack. A positive electrode of each lithium ion battery is in contact with and electrically connected to a conductor 624 separated by an insulator 625. The conductor 624 is electrically connected to a control circuit 620 via a wiring 623. A negative electrode of each lithium ion battery is electrically connected to the control circuit 620 via a wiring 626. A protection circuit that prevents overcharging or overdischarging, or the like, can be used as the control circuit 620.
[0336] 12(D) shows an example of a power storage system 615. The power storage system 615 has a plurality of lithium ion batteries 616, and the plurality of lithium ion batteries 616 are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of lithium ion batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 by wiring 627. The plurality of lithium ion batteries 616 may be connected in parallel, may be connected in series, or may be connected in parallel and then further connected in series. By configuring the power storage system 615 having a plurality of lithium ion batteries 616, it is possible to extract a large amount of power.
[0337] A number of lithium ion batteries 616 may be connected in parallel and then further connected in series.
[0338] A temperature control device may be provided between the multiple lithium ion batteries 616. When the lithium ion batteries 616 are overheated, they can be cooled by the temperature control device, and when the lithium ion batteries 616 are too cold, they can be heated by the temperature control device. This makes the performance of the power storage system 615 less susceptible to the effect of the outside air temperature.
[0339] 12D, the power storage system 615 is electrically connected to a control circuit 620 via a wiring 621 and a wiring 622. The wiring 621 is electrically connected to a positive electrode of the plurality of lithium ion batteries 616 via a conductive plate 628, and the wiring 622 is electrically connected to a negative electrode of the plurality of lithium ion batteries 616 via a conductive plate 614.
[0340] When the electrolyte and positive electrode active material of the present invention are used in a cylindrical lithium ion battery 100, excellent charge and discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.
[0341] [Other examples of lithium-ion battery structures] An example of the structure of a lithium ion battery will be described with reference to FIGS.
[0342] A lithium ion battery 913 shown in FIG. 13A has a wound body 950 in which terminals 951 and 952 are provided inside a housing 930. The wound body 950 is impregnated with an electrolyte according to one embodiment of the present invention inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 is not in contact with the housing 930 by using an insulating material or the like. Note that in FIG. 13A, the housing 930 is shown separated for convenience, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a resin material.
[0343] Note that as shown in Fig. 13B, the housing 930 shown in Fig. 13A may be formed using a plurality of materials. For example, in a lithium ion battery 913 shown in Fig. 13B, a housing 930a and a housing 930b are bonded together, and a wound body 950 is provided in a region surrounded by the housing 930a and the housing 930b.
[0344] The housing 930a can be made of an insulating material such as organic resin. In particular, by using a material such as organic resin on the surface on which the antenna is formed, it is possible to suppress shielding of the electric field by the lithium ion battery 913. Note that if the shielding of the electric field by the housing 930a is small, the antenna may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material.
[0345] 13(C) shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and an electrolyte layer 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the electrolyte layer 933 sandwiched therebetween, and the laminated sheet is wound. Note that the stack of the negative electrode 931, the positive electrode 932, and the electrolyte layer 933 may be stacked a plurality of times.
[0346] 14(A) to 14(C) may be used as a lithium ion battery 913 having a wound body 950a. The wound body 950a shown in Fig. 14(A) includes a negative electrode 931, a positive electrode 932, and an electrolyte layer 933. The negative electrode 931 includes a negative electrode active material layer 931a. The positive electrode 932 includes a positive electrode active material layer 932a.
[0347] The electrolyte layer 933 has a width wider than the negative electrode active material layer 931a and the positive electrode active material layer 932a, and is wound so as to overlap the negative electrode active material layer 931a and the positive electrode active material layer 932a. From the viewpoint of safety, it is preferable that the width of the negative electrode active material layer 931a is wider than that of the positive electrode active material layer 932a. Moreover, a wound body 950a having such a shape is preferable because of its high safety and productivity.
[0348] 14B, the negative electrode 931 is electrically connected to a terminal 951. The terminal 951 is electrically connected to a terminal 911a. The positive electrode 932 is electrically connected to a terminal 952. The terminal 952 is electrically connected to a terminal 911b.
[0349] 14C, the wound body 950a is covered with the housing 930 to form the lithium ion battery 913. It is preferable that a safety valve, an overcurrent protection element, and the like are provided in the housing 930. The safety valve is a valve that opens when the inside of the housing 930 reaches a predetermined internal pressure in order to prevent the battery from exploding.
[0350] As shown in Fig. 14(B), the lithium ion battery 913 may have a plurality of wound bodies 950a. By using a plurality of wound bodies 950a, the lithium ion battery 913 can have a larger charge / discharge capacity. For other elements of the lithium ion battery 913 shown in Figs. 14(A) and (B), the descriptions of the lithium ion battery 913 shown in Figs. 13(A) to 13(C) can be referred to.
[0351] When the electrolyte and positive electrode active material of the present invention are used in a lithium ion battery 913 having a wound body, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0352] The content of this embodiment mode can be appropriately combined with the content of the other embodiment modes.
[0353] (Embodiment 5) In this embodiment, an example of application to an electric vehicle (EV) will be described with reference to FIG.
[0354] 15(A), an electric vehicle is equipped with first batteries 1301a and 1301b as main driving lithium ion batteries, and a second battery 1311 that supplies power to an inverter 1312 that starts a motor 1304. When the electrolyte and positive electrode active material of the present invention are used for the first batteries 1301a and 1301b, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0355] The second battery 1311 is also called a cranking battery (also called a starter battery). The second battery 1311 only needs to have high output, and does not need to have a large capacity. The capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.
[0356] The internal structure of the first battery 1301a may be a wound type or a laminated type. The first battery 1301a may use the all-solid-state battery of embodiment 5. By using the all-solid-state battery of embodiment 5 for the first battery 1301a, it is possible to achieve a high capacity, improve safety, and reduce the size and weight.
[0357] In this embodiment, an example is shown in which two first batteries 1301a and 1301b are connected in parallel, but three or more batteries may be connected in parallel. If the first battery 1301a can store sufficient power, the first battery 1301b may not be necessary. By configuring a battery pack having multiple lithium ion batteries, it is possible to extract large power. The multiple lithium ion batteries may be connected in parallel, in series, or in series after being connected in parallel. A plurality of lithium ion batteries is also called a battery pack.
[0358] In addition, in an on-vehicle lithium ion battery, in order to cut off power from a plurality of lithium ion batteries, a service plug or circuit breaker capable of cutting off high voltage without using tools is provided in the first battery 1301a.
[0359] The power of the first batteries 1301a and 1301b is mainly used to rotate the motor 1304, but also supplies power to 42V in-vehicle components (such as an electric power steering 1307, a heater 1308, and a defogger 1309) via a DCDC circuit 1306. When a rear motor 1317 is provided for the rear wheels, the first battery 1301a is used to rotate the rear motor 1317.
[0360] In addition, the second battery 1311 supplies power to 14V in-vehicle components (such as an audio system 1313, a power window 1314, and lamps 1315) via the DCDC circuit 1310.
[0361] The first battery 1301a will be described with reference to FIG.
[0362] FIG. 15B shows an example in which nine rectangular lithium ion batteries 1300 are used as one battery pack 1415. Nine rectangular lithium ion batteries 1300 are connected in series, one electrode is fixed by a fixing part 1413 made of an insulator, and the other electrode is fixed by a fixing part 1414 made of an insulator. In this embodiment, an example in which the batteries are fixed by the fixing parts 1413 and 1414 is shown, but the batteries may be stored in a battery storage box (also called a housing). Since it is assumed that the vehicle is subjected to vibration or shaking from the outside (such as a road surface), it is preferable to fix a plurality of lithium ion batteries by the fixing parts 1413 and 1414 and the battery storage box. One electrode is electrically connected to the control circuit part 1320 by a wiring 1421. The other electrode is electrically connected to the control circuit part 1320 by a wiring 1422.
[0363] A memory circuit including a transistor using an oxide semiconductor may be used for the control circuit unit 1320. A charge control circuit or a battery control system having a memory circuit including a transistor using an oxide semiconductor may be referred to as a Battery operating system (BTOS) or a Battery oxide semiconductor.
[0364] It is preferable to use a metal oxide that functions as an oxide semiconductor. For example, a metal oxide such as In-M-Zn oxide (wherein element M is one or more selected from aluminum, gallium, yttrium, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium) may be used as the oxide. In particular, the In-M-Zn oxide that can be used as the oxide is preferably CAAC-OS (C-Axis Aligned Crystal Oxide Semiconductor) or CAC-OS (Cloud-Aligned Composite Oxide Semiconductor). In-Ga oxide or In-Zn oxide may be used as the oxide. CAAC-OS is an oxide semiconductor that has a plurality of crystal regions, and the plurality of crystal regions have c-axes oriented in a specific direction. The specific direction is the thickness direction of the CAAC-OS film, the normal direction of the surface on which the CAAC-OS film is formed, or the normal direction of the surface of the CAAC-OS film. The crystalline region is a region in which the atomic arrangement has periodicity. If the atomic arrangement is regarded as a lattice arrangement, the crystalline region is also a region in which the lattice arrangement is uniform. Furthermore, the CAAC-OS has a region in which a plurality of crystalline regions are connected in the ab-plane direction, and the region may have distortion. Note that the distortion refers to a portion in which the direction of the lattice arrangement changes between a region in which the lattice arrangement is uniform and another region in which the lattice arrangement is uniform in a region in which a plurality of crystalline regions are connected. In other words, the CAAC-OS is an oxide semiconductor that is c-axis oriented and does not have a clear orientation in the ab-plane direction.
[0365] In addition, since it can be used in a low-temperature environment, it is preferable that the control circuit unit 1320 uses a transistor using an oxide semiconductor. In order to simplify the process, the control circuit unit 1320 may be formed using a unipolar transistor. The operating ambient temperature of a transistor using an oxide semiconductor in the semiconductor layer is wider than that of single-crystal Si, from -40°C to 150°C, and the characteristic change is smaller than that of a single crystal even when the lithium-ion battery is heated. The off-current of a transistor using an oxide semiconductor is below the lower measurement limit regardless of temperature even at 150°C, but the off-current characteristic of a single-crystal Si transistor is highly temperature-dependent. For example, at 150°C, the off-current of a single-crystal Si transistor increases, and the current on / off ratio does not become sufficiently large. The control circuit unit 1320 can improve safety.
[0366] The control circuit unit 1320 using a memory circuit including a transistor using an oxide semiconductor can function as an automatic control device for a lithium-ion battery against 10 causes of instability such as micro-short circuit. The functions for eliminating the 10 causes of instability include overcharging prevention, overcurrent prevention, overheating control during charging, cell balancing in a battery pack, over-discharging prevention, a remaining capacity meter, automatic control of charging voltage and current amount according to temperature, control of charging current amount according to deterioration degree, detection of abnormal behavior of micro-short circuit, and prediction of abnormality related to micro-short circuit, and the control circuit unit 1320 has at least one of these functions. In addition, the automatic control device for a lithium-ion battery can be made ultra-compact.
[0367] Micro-short circuits are tiny short circuits inside lithium-ion batteries. One of the causes of micro-short circuits is said to be localized current concentration in parts of the positive electrode and negative electrode due to uneven distribution of the positive electrode active material caused by multiple charge and discharge cycles, or the generation of by-products due to side reactions, resulting in micro-short circuits.
[0368] In addition to detecting micro-short circuits, the control circuit unit 1320 can also be said to detect the terminal voltage of the lithium-ion battery and manage the charge / discharge state of the lithium-ion battery. For example, to prevent overcharging, it can turn off both the output transistor and the cutoff switch of the charging circuit almost simultaneously.
[0369] FIG. 15C shows an example of a block diagram of the battery pack 1415 shown in FIG.
[0370] The control circuit unit 1320 has at least a switch unit 1324 including a switch for preventing overcharging and a switch for preventing overdischarging, a control circuit 1322 for controlling the switch unit 1324, and a voltage measurement unit for the first battery 1301a. The control circuit unit 1320 has an upper limit voltage and a lower limit voltage for the lithium ion battery used, and limits the upper limit of the current from the outside and the upper limit of the output current to the outside. The range between the lower limit voltage and the upper limit voltage of the lithium ion battery is within the voltage range recommended for use, and when it is outside that range, the switch unit 1324 operates and functions as a protection circuit. In addition, the control circuit unit 1320 can also be called a protection circuit because it controls the switch unit 1324 to prevent overcharging and overdischarging. For example, when the control circuit 1322 detects a voltage that is likely to cause overcharging, the switch unit 1324 is turned off to cut off the current. Furthermore, a PTC element may be provided in the charge / discharge path to provide a function of cutting off the current in response to an increase in temperature. In addition, the control circuit section 1320 has an external terminal 1325 (+IN) and an external terminal 1326 (-IN).
[0371] The switch unit 1324 can be configured by combining n-channel transistors and p-channel transistors. The switch unit 1324 is not limited to a switch having a Si transistor using single crystal silicon, and may be, for example, Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenide), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), GaOx The switch unit 1324 may be formed of a power transistor having an OS transistor (gallium oxide; x is a real number greater than 0). Memory elements using OS transistors can be freely arranged by stacking them on a circuit using Si transistors, and therefore integration can be easily achieved. A control circuit unit 1320 using an OS transistor can be stacked on the switch unit 1324 and integrated into a single chip, enabling miniaturization.
[0372] The first batteries 1301a and 1301b mainly supply power to 42V (high voltage) in-vehicle devices, and the second battery 1311 supplies power to 14V (low voltage) in-vehicle devices. Lead-acid batteries are often used as the second battery 1311 because they are cost-effective. The second battery 1311 is a lithium-ion battery, which has the advantage of being maintenance-free. However, after a long period of use, for example, three years or more, there is a risk of abnormalities occurring that cannot be detected at the time of manufacture. In particular, if the second battery 1311 that starts the inverter becomes inoperable, even if the first batteries 1301a and 1301b have remaining capacity, in order to prevent the motor from being unable to start, if the second battery 1311 is a lead-acid battery, power is supplied from the first battery to the second battery, and the battery is charged to always maintain a fully charged state.
[0373] In this embodiment, an example in which lithium ion batteries are used for both the first battery 1301a and the second battery 1311 is shown, but a lead storage battery, an all-solid-state battery, or an electric double layer capacitor may be used for the second battery 1311. When the electrolyte and the positive electrode active material of the present invention are used in the above-mentioned lithium ion battery, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0374] Moreover, regenerative energy due to the rotation of the tire 1316 is sent to the motor 1304 via the gear 1305, and is charged into the second battery 1311 from the motor controller 1303 and the battery controller 1302 via the control circuit unit 1321. Alternatively, the first battery 1301a is charged from the battery controller 1302 via the control circuit unit 1320. Alternatively, the first battery 1301b is charged from the battery controller 1302 via the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is desirable that the first batteries 1301a and 1301b are capable of being quickly charged.
[0375] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b. The battery controller 1302 can set charging conditions in accordance with the charging characteristics of the lithium ion battery used, and can perform rapid charging.
[0376] Although not shown, when connecting to an external charger, the charger outlet or the connection cable of the charger is electrically connected to the battery controller 1302. The power supplied from the external charger is charged to the first batteries 1301a and 1301b via the battery controller 1302. Some chargers are provided with a control circuit and may not use the function of the battery controller 1302, but it is preferable to charge the first batteries 1301a and 1301b via the control circuit unit 1320 to prevent overcharging. In some cases, the connection cable or the connection cable of the charger is provided with a control circuit. The control circuit unit 1320 is also called an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. The CAN is one of the serial communication standards used as an in-vehicle LAN. The ECU includes a microcomputer. The ECU uses a CPU or a GPU.
[0377] External chargers installed at charging stations and the like come in a variety of types, including 100V outlets, 200V outlets, and three-phase 200V and 50kW outlets. In addition, charging can also be achieved by receiving power from external charging equipment using a contactless power supply system or the like.
[0378] Next, an example in which the lithium-ion battery according to one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.
[0379] Furthermore, by installing lithium-ion batteries in vehicles, next-generation clean energy automobiles such as hybrid vehicles (HVs), electric vehicles (EVs), plug-in hybrid vehicles (PHVs), etc. Lithium-ion batteries can also be installed in transportation vehicles such as agricultural machinery, motorized bicycles including electrically assisted bicycles, motorcycles, electric wheelchairs, electric carts, small or large ships, submarines, aircraft such as fixed-wing aircraft and rotary-wing aircraft, rockets, artificial satellites, space probes, planetary probes, and spacecraft.
[0380] 16(A) to 16(D) show an example of a transportation vehicle using one embodiment of the present invention. An automobile 2001 shown in FIG. 16(A) is an electric automobile that uses an electric motor as a power source for running. Or, it is a hybrid automobile that can appropriately select and use an electric motor and an engine as a power source for running. When a lithium-ion battery is mounted on a vehicle, an example of the lithium-ion battery shown in the above embodiment is installed in one or more locations. When the electrolyte and the positive electrode active material of the present invention are used in the lithium-ion battery mounted on the vehicle, excellent charge and discharge characteristics can be expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0381] 16A includes a battery pack 2200, which includes a battery module to which a plurality of lithium ion batteries are connected. The battery pack 2200 preferably further includes a charge control device electrically connected to the battery module.
[0382] Moreover, the automobile 2001 can charge the lithium ion battery of the automobile 2001 by receiving power supply from an external charging facility by a plug-in method, a contactless power supply method, or the like. When charging, the charging method and connector standard may be appropriately performed by a predetermined method such as CHAdeMO (registered trademark) or Combo. The lithium ion battery may be a charging station provided in a commercial facility, or may be a home power source. For example, a power storage device mounted on the automobile 2001 can be charged by an external power supply by plug-in technology. Charging can be performed by converting AC power to DC power via a conversion device such as an ACDC converter.
[0383] Although not shown, a power receiving device may be mounted on a vehicle, and charging may be performed by supplying power contactlessly from a ground power transmitting device. In the case of this contactless power supply method, by incorporating a power transmitting device in a road or an exterior wall, charging may be performed not only while the vehicle is stopped but also while it is moving. This contactless power supply method may also be used to transmit and receive power between two vehicles. Furthermore, solar cells may be provided on the exterior of the vehicle, and the lithium ion battery may be charged while the vehicle is stopped and while it is moving. An electromagnetic induction method or a magnetic field resonance method may be used for such contactless power supply.
[0384] Fig. 16(B) shows a large transport vehicle 2002 having an electrically controlled motor as an example of a transport vehicle. The battery module of the transport vehicle 2002 has, for example, a four-cell unit of lithium ion batteries with a nominal voltage of 3.0 V to 5.0 V, with 48 cells connected in series to achieve a maximum voltage of 170 V. Other than the number of lithium ion batteries in the battery pack 2201, the battery pack 2201 has the same functions as those in Fig. 15(B), and therefore a description thereof will be omitted. When the electrolyte and positive electrode active material of the present invention are used in the lithium ion batteries of the battery pack 2201, excellent charge and discharge characteristics can be expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0385] Fig. 16(C) shows, as an example, a large transport vehicle 2003 having an electrically controlled motor. The battery module of the transport vehicle 2003 has, for example, a maximum voltage of 600V, in which 100 or more lithium ion batteries with a nominal voltage of 3.0V to 5.0V are connected in series. Also, except for the number of lithium ion batteries constituting the battery module of the battery pack 2202, the battery module has the same functions as that of Fig. 15(B), and therefore a description thereof will be omitted. If the electrolyte and positive electrode active material of the present invention are used in the lithium ion battery of the module, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0386] Fig. 16(D) shows, as an example, an aircraft 2004 having an engine that burns fuel. The aircraft 2004 shown in Fig. 16(D) has wheels for takeoff and landing, and therefore can be said to be a part of a transportation vehicle, and has a battery pack 2203 including a battery module formed by connecting multiple lithium ion batteries and including a battery module and a charge control device.
[0387] The battery module of the aircraft 2004 is, for example, eight 4 V lithium ion batteries connected in series to produce a maximum voltage of 32 V. Other than the number of lithium ion batteries constituting the battery module of the battery pack 2203, it has the same functions as those in FIG. 15(B), and therefore a description thereof will be omitted.
[0388] The content of this embodiment mode can be appropriately combined with the content of the other embodiment modes.
[0389] (Embodiment 6) In this embodiment, an example will be described in which a lithium-ion battery according to one embodiment of the present invention is mounted on a vehicle such as a motorcycle or a bicycle.
[0390] 17A is an example of an electric bicycle using the lithium-ion battery of one embodiment of the present invention. The lithium-ion battery of one embodiment of the present invention can be applied to an electric bicycle 8700 shown in FIG. 17A. The lithium-ion battery of one embodiment of the present invention may include a protection circuit.
[0391] The electric bicycle 8700 includes a power storage device 8702. The power storage device 8702 can supply electricity to a motor that assists a rider. The power storage device 8702 is portable, and is shown in a state removed from the bicycle in FIG. 17B. The power storage device 8702 includes a plurality of lithium-ion batteries 8701 of one embodiment of the present invention, and the remaining battery charge and the like can be displayed on a display unit 8703. When the electrolyte and positive electrode active material of the present invention are used for the lithium-ion battery 8701, excellent charge and discharge characteristics can be expected in a wide temperature range, including from below freezing to high temperatures.
[0392] The power storage device 8702 also includes a control circuit 8704 capable of controlling charging or detecting an abnormality of the lithium ion battery, an example of which is shown in Embodiment 7. The control circuit 8704 is electrically connected to the positive and negative electrodes of the lithium ion battery 8701. This can greatly contribute to preventing accidents such as fires caused by lithium ion batteries.
[0393] 17C is an example of a two-wheeled vehicle using a lithium-ion battery of one embodiment of the present invention. A scooter 8600 shown in FIG. 17C includes a power storage device 8602, a side mirror 8601, and a turn signal light 8603. The power storage device 8602 can supply electricity to the turn signal light 8603. When the electrolyte and the positive electrode active material of the present invention are used in a lithium-ion battery, excellent charge and discharge characteristics can be expected in a wide temperature range, including from below freezing to high temperatures.
[0394] 17C, a power storage device 8602 can be stored in an under-seat storage compartment 8604. The power storage device 8602 can be stored in the under-seat storage compartment 8604 even if the under-seat storage compartment 8604 is small in size.
[0395] The content of this embodiment mode can be appropriately combined with the content of other embodiment modes.
[0396] (Embodiment 7) In this embodiment, an example of mounting a lithium ion battery according to one embodiment of the present invention in an electronic device will be described. Examples of electronic devices mounting a lithium ion battery include television devices (also called televisions or television receivers), monitors for computers, digital cameras, digital video cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices), portable game machines, portable information terminals, audio playback devices, and large game machines such as pachinko machines. Examples of portable information terminals include notebook personal computers, tablet terminals, e-book terminals, and mobile phones.
[0397] 18(A) shows an example of a mobile phone. The mobile phone 2100 includes a display unit 2102 built into a housing 2101, as well as operation buttons 2103, an external connection port 2104, a speaker 2105, a microphone 2106, and the like. The mobile phone 2100 includes a lithium ion battery 2107. When the electrolyte and the positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics can be expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0398] The mobile phone 2100 is capable of executing a variety of applications, such as mobile phone calls, e-mail, document browsing and creation, music playback, Internet communications, and computer games.
[0399] The operation button 2103 can have various functions, such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / cancellation, power saving mode activation / cancellation, etc. For example, the function of the operation button 2103 can be freely set by an operating system built into the mobile phone 2100.
[0400] The mobile phone 2100 is also capable of performing short-range wireless communication according to a communication standard. For example, the mobile phone 2100 can communicate with a wireless headset to enable hands-free calling.
[0401] The mobile phone 2100 also includes an external connection port 2104, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the external connection port 2104. Note that charging may be performed by wireless power supply without using the external connection port 2104.
[0402] It is preferable that the mobile phone 2100 has a sensor. For example, it is preferable that a fingerprint sensor, a pulse sensor, a human body sensor such as a body temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like is mounted as the sensor.
[0403] FIG. 18(B) shows an unmanned aerial vehicle 2300 having a plurality of rotors 2302. The unmanned aerial vehicle 2300 is sometimes called a drone. The unmanned aerial vehicle 2300 includes a lithium ion battery 2301 which is one embodiment of the present invention, a camera 2303, and an antenna (not shown). The unmanned aerial vehicle 2300 can be remotely controlled via the antenna. When the electrolyte and positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics can be expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0404] Fig. 18C shows an example of a robot. The robot 6400 shown in Fig. 18C includes a lithium ion battery 6409, an illuminance sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406, an obstacle sensor 6407, a moving mechanism 6408, a computing device, and the like.
[0405] The microphone 6402 has a function of detecting the user's voice, environmental sounds, etc. The speaker 6404 has a function of emitting sound. The robot 6400 can communicate with the user using the microphone 6402 and the speaker 6404.
[0406] The display unit 6405 has a function of displaying various information. The robot 6400 can display information desired by the user on the display unit 6405. The display unit 6405 may be equipped with a touch panel. The display unit 6405 may be a removable information terminal, and by installing it in a fixed position on the robot 6400, charging and data transfer are possible.
[0407] The upper camera 6403 and the lower camera 6406 have a function of capturing images of the surroundings of the robot 6400. In addition, the obstacle sensor 6407 can detect the presence or absence of an obstacle in the moving direction when the robot 6400 moves forward using the moving mechanism 6408. The robot 6400 can recognize the surrounding environment and move safely using the upper camera 6403, the lower camera 6406, and the obstacle sensor 6407.
[0408] The robot 6400 includes a lithium ion battery 6409 according to one embodiment of the present invention and a semiconductor device or electronic component in its internal area. When the electrolyte and the positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0409] 18(D) shows an example of a cleaning robot. The cleaning robot 6300 has a display unit 6302 arranged on the top surface of a housing 6301, a plurality of cameras 6303 arranged on the side surface, a brush 6304, an operation button 6305, a lithium ion battery 6306, various sensors, and the like. Although not shown, the cleaning robot 6300 is provided with tires, a suction port, and the like. The cleaning robot 6300 can move by itself, detect dust 6310, and suck up the dust from a suction port arranged on the bottom surface.
[0410] For example, the cleaning robot 6300 can analyze an image captured by the camera 6303 and determine the presence or absence of an obstacle such as a wall, furniture, or a step. When an object that may become entangled in the brush 6304, such as a wire, is detected by image analysis, the rotation of the brush 6304 can be stopped. The cleaning robot 6300 includes a lithium ion battery 6306 according to one embodiment of the present invention and a semiconductor device or electronic component in its internal area. When the electrolyte and positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures.
[0411] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0412] (Embodiment 8) In this embodiment, an example in which a lithium-ion battery according to one embodiment of the present invention is mounted on space equipment will be described.
[0413] 19A shows an artificial satellite 6800 as an example of space equipment. The artificial satellite 6800 has a body 6801, a solar panel 6802, an antenna 6803, and a lithium ion battery 6805. The solar panel may be called a solar cell module.
[0414] When the solar panel 6802 is irradiated with sunlight, the power required for the operation of the satellite 6800 is generated. However, for example, in a situation where the solar panel is not irradiated with sunlight or the amount of sunlight irradiated to the solar panel is small, the generated power is small. Therefore, there is a possibility that the power required for the operation of the satellite 6800 is not generated. In order to operate the satellite 6800 even under a situation where the generated power is small, it is preferable to provide a lithium ion battery 6805 in the satellite 6800. When the electrolyte and the positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics are expected in a wide temperature range including from below freezing to high temperatures.
[0415] The satellite 6800 can generate a signal. The signal is transmitted via an antenna 6803, and can be received by, for example, a receiver installed on the ground or another satellite. By receiving the signal transmitted by the satellite 6800, for example, the position of the receiver that received the signal can be measured. Thus, the satellite 6800 can constitute, for example, a satellite positioning system.
[0416] Alternatively, the artificial satellite 6800 can be configured to have a sensor. For example, by configuring the artificial satellite 6800 to have a visible light sensor, the artificial satellite 6800 can have a function of detecting sunlight reflected by an object on the ground. Alternatively, by configuring the artificial satellite 6800 to have a thermal infrared sensor, the artificial satellite 6800 can have a function of detecting thermal infrared rays emitted from the earth's surface. From the above, the artificial satellite 6800 can have a function as, for example, an earth observation satellite.
[0417] FIG. 19(B) shows a probe 6900 having a solar sail (also called a sun sail) as an example of space equipment. The probe 6900 has a body 6901, a solar sail 6902, and a lithium ion battery 6905. When the electrolyte and the positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures. When photons emitted from the sun hit the surface of the solar sail 6902, momentum is transferred to the solar sail 6902. Therefore, the surface of the solar sail 6902 preferably has a thin film with high reflectivity, and further preferably faces the sun.
[0418] The solar sail 6902 may also be designed to be folded up small until it leaves the atmosphere, and then deployed into a large sheet outside the Earth's atmosphere (in outer space) as shown in Figure 19(B).
[0419] FIG. 19(C) shows a spacecraft 6910 as an example of space equipment. The spacecraft 6910 has a body 6911, a solar panel 6912, and a lithium ion battery 6913. When the electrolyte and the positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures. The body 6911 can have, for example, a pressurized compartment and a non-pressurized compartment. The pressurized compartment may be designed to accommodate a crew member. Electricity generated by irradiating the solar panel 6912 with sunlight can be charged into the lithium ion battery 6913.
[0420] 19(D) shows a rover 6920 as an example of space equipment. The rover 6920 has a body 6921 and a lithium ion battery 6923. When the electrolyte and the positive electrode active material of the present invention are used in the lithium ion battery, excellent charge and discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures. The rover 6920 may have a solar panel 6922.
[0421] The rover 6920 may be designed to accommodate a crew member. The lithium ion battery 6923 may be charged with electricity generated by irradiating the solar panel 6912 with sunlight, or may be charged with electricity generated by other power sources, such as a fuel cell, a radioisotope thermoelectric converter, or the like.
[0422] The content of this embodiment mode can be appropriately combined with the content of other embodiment modes. [Explanation of symbols]
[0423] 10a Surface layer 10b Bulk section 10 Cathode active material 15 Grain Boundaries 100 Lithium-ion batteries 101 Negative electrode current collector 102 Negative electrode active material layer 104 Cathode active material layer 105 Positive electrode current collector 106 Negative electrode 107 Positive electrode 108 Separator 109 Electrolytes 301 Positive electrode can 302 Anode can 303 Gasket 304 Positive electrode 305 Positive electrode current collector 306 Positive electrode active material layer 307 Negative electrode 308 Negative electrode current collector 309 Negative electrode active material layer 332 Washer 342 Spacer 508 Adhesive area 509 Exterior body 510 Negative lead electrode 511 Positive lead electrode 550 Current collector 553 Carbon Black 554 Graphene 555 Carbon Fiber 561 Cathode active material 562 Second active material 601 Positive electrode cap 602 Battery Can 603 Positive terminal 604 Positive electrode 605 Electrolyte layer 606 negative electrode 607 Negative terminal 608 Insulating plate 609 Insulating plate 611 PTC element 613 Safety valve mechanism 614 Conductive plate 615 Energy Storage System 616 Lithium-ion battery 620 Control circuit 621 Wiring 622 Wiring 623 Wiring 624 Conductors 625 Insulators 626 Wiring 627 Wiring 628 Conductive plate 903 mixture 904 Mixture 911a Terminal 911b Terminal 913 Lithium-ion battery 930a Case 930b Case 930 Case 931a Negative electrode active material layer 931 negative electrode 932a Cathode active material layer 932 Positive electrode 933 Electrolyte layer 950a Wound body 950 Wound body 951 Terminal 952 Terminal 1300 Square Lithium-ion Battery 1301a First Battery 1301b 1st Battery 1302 Battery Controller 1303 Motor Controller 1304 Motor 1305 Gear 1306 DC-DC circuit 1307 Electric power steering 1308 Heater 1309 Defogger 1310 DC-DC circuit 1311 Second Battery 1312 Inverter 1313 Audio 1314 Power window 1315 Lamps 1316 Tires 1317 Rear motor 1320 Control circuit section 1321 Control circuit section 1322 Control circuit 1324 Switch section 1413 Fixed part 1414 Fixed part 1415 Battery Pack 1421 Wiring 1422 Wiring 2001 Automobiles 2002 Transport vehicle 2003 Transport Vehicles 2004 aircraft 2100 Mobile phone 2101 Case 2102 Display section 2103 Operation button 2104 External connection port 2105 Speaker 2106 Mike 2107 Lithium-ion battery 2200 Battery Pack 2201 Battery Pack 2202 Battery Pack 2203 Battery Pack 2300 Unmanned Aircraft 2301 Lithium-ion battery 2302 Rotor 2303 Camera 6300 Cleaning robot 6301 Case 6302 Display section 6303 Camera 6304 Brush 6305 Operation button 6306 Lithium-ion battery 6310 Garbage 6400 Robot 6401 Light Sensor 6402 Microphone 6403 Upper Camera 6404 Speaker 6405 Display section 6406 Lower Camera 6407 Obstacle Sensor 6408 Moving mechanism 6409 Lithium-ion battery 6800 satellite 6801 Aircraft 6802 Solar Panel 6803 Antenna 6805 Lithium-ion Battery 6900 Probe 6901 Aircraft 6902 Solar Sail 6905 Lithium-ion battery 6910 Spaceship 6911 Aircraft 6912 Solar Panel 6913 Lithium-ion battery 6920 Rover 6921 Aircraft 6922 Solar Panel 6923 Lithium-ion battery 8600 Scooter 8601 Side mirror 8602 Energy storage devices 8603 Turn signal light 8604 Under-seat storage 8700 Electric Bike 8701 Lithium-ion battery 8702 Energy storage devices 8703 Display section 8704 Control circuit
Claims
1. A positive electrode having a positive electrode active material, an electrolyte, and a negative electrode having graphite, The positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in the surface layer portion of the positive electrode active material is higher than the magnesium concentration in the interior of the positive electrode active material, the electrolyte contains a fluorinated cyclic carbonate or a fluorinated chain carbonate; A lithium ion secondary battery in which vinylene carbonate is added to the electrolyte.
2. 2. The lithium ion secondary battery according to claim 1, wherein the positive electrode active material is lithium cobalt oxide further containing aluminum, nickel, and fluorine.
3. 2. The lithium ion secondary battery according to claim 1, wherein the vinylene carbonate is present in an amount of 0.1% by weight or more and 5% by weight or less based on the total weight of the electrolyte.
4. 2. The lithium ion secondary battery according to claim 1, wherein at least a portion of the interface between the positive electrode active material and the electrolyte is coated with a film.
5. 2. The lithium ion secondary battery according to claim 1, further comprising a coating on at least a portion of the interface between the graphite and the electrolyte.
Citation Information
Patent Citations
Method for manufacturing positive electrode active material
JP2019179758A
Secondary battery and electronic apparatus
JP2022070247A
Positive electrode active material and method for producing positive electrode active material
WO2020026078A1