METHOD OF PRODUCING NiTi SHAPE-MEMORY ALLOY

The method of selective laser melting and tailored annealing addresses the poor ductility of NiTi SMAs, enhancing mechanical properties and enabling industrial application by achieving 100% superelasticity and improved tensile strength.

JP2024160979AActive Publication Date: 2024-11-15TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024073910
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-04
Filing Date
2024-04-30
Publication Date
2024-11-15
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

NiTi shape memory alloys (SMAs) face challenges in machining performance and weldability, limiting their industrial application due to poor ductility and mechanical properties when produced via selective laser melting (SLM), necessitating a tailored annealing process to enhance tensile properties.

Method used

A method involving selective laser melting followed by annealing at 750-1050°C for 50-90 minutes, using specific parameters and materials, including gas atomized spherical powder and as-cast NiTi alloy, to improve mechanical properties and achieve superelasticity.

Benefits of technology

The method significantly enhances the mechanical properties of SLM-NiTi SMAs, achieving 100% superelasticity with improved tensile strength and elongation, extending their practical service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160979000001_ABST
    Figure 2024160979000001_ABST
Patent Text Reader

Abstract

To provide a method of producing a high-performance NiTi shape-memory alloy in order to overcome the shortcoming in a prior art technique.SOLUTION: A method of producing high-performance NiTi SMA includes: a step 1 of obtaining a SLM-NiTi printed matter by printing a NiTi shape-memory alloy by a selective laser melting process and naturally cooling it down to room temperature, so as to use as-cast NiTi shape-memory alloy as a base plate with a gas-atomized spherical powder Ni50Ti50 having an equi-atomic ratio used as a raw material; and a step 2 of obtaining high-performance NiTi SMA by keeping warm the SLM-NiTi printed matter obtained at the step 1 at 750-1050°C for 50 min-90 min and then cooling it down. By annealing the SLM-NiTi lamination-molded printed matter according to the method in the present invention, dynamic properties of the printed matter can be conspicuously improved.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of alloy materials, and in particular to a method for producing high performance NiTi shape memory alloys. [Background technology]

[0002] NiTi shape memory alloys (SMAs) are widely used in aerospace, biomedicine and other fields due to their unique shape memory effect and superelasticity. However, NiTi SMAs have poor machining performance and poor weldability, which makes it very difficult to process and prepare parts with arbitrary geometric shapes, greatly limiting their further promotion and application. Selective laser melting (SLM) technology has the ability to mold complex components close to the final shape in one go. Therefore, it is of great importance to conduct research on NiTi SMAs based on selective laser melting technology. Compared with traditional manufacturing methods, NiTi SMA manufactured by SLM technology has poor ductility and cannot meet industrial applications. Therefore, it is necessary to find an effective way to improve the tensile properties of SLM-NiTi SMA. Annealing is one of the most commonly used post-treatment methods for additive manufacturing prints, which can effectively adjust the microstructure of the prints and improve the mechanical properties of the material. At present, the annealing process of traditional metal materials is relatively mature. However, unlike conventional alloys, NiTi SMA has a unique strengthening mechanism that is different from conventional metals due to its unique non-diffusional martensitic transformation process. Due to the difference in strengthening mechanism, its annealing process cannot be obtained by simply slightly modifying the annealing process of conventional alloys, but must be newly designed based on an understanding of the effect of annealing on the strengthening mechanism. Therefore, the annealing process of SLM-NiTi printed products is not mature, and as a result, industrial practical application cannot be realized. Therefore, research on the annealing process of SLM-NiTi SMA is of great importance for its engineering applications. Summary of the Invention

[0003] The objective of the present invention is to provide a method for producing high performance NiTi shape memory alloys to overcome the deficiencies of the existing technology.

[0004] The technical means for achieving the object of the present invention are as follows.

[0005] Step 1: Printing NiTi shape memory alloy by selective laser melting and naturally cooling to room temperature to obtain SLM-NiTi printed object; Step 2: keeping the SLM-NiTi print obtained in step 1 at 750-1050 °C for 50 min-90 min, preferably 1 h, and then cooling to obtain a high-performance NiTi SMA; A method for fabricating high performance NiTi SMAs, including:

[0006] In the above technical means, in step 1, a selective laser melting device of model Renishaw AM400 is used to print NiTi shape memory alloy.

[0007] In the above technical means, in step 1, equiatomic gas atomized spherical powder Ni50Ti50 is used as raw material, and as-cast NiTi shape memory alloy is used as substrate.

[0008] In the above technical means, in step 1, the printing process is as follows: First, the substrate is mounted, and before mounting, the surface of the substrate is sandblasted to remove dirt on the substrate surface and form a uniform and fine uneven surface, thereby improving the uniformity of powder scattering and the adhesion of the substrate to the powder; then, the powder is loaded, and before loading, the powder is vibrated and sieved through a 250 mesh standard sieve before being put into the hopper, thereby improving the flowability of the powder; further, the 3D model is sliced, parameter setting and scanning strategy editing are performed by the dedicated software (QuantAM and Material Editor) attached to the selective laser melting device; finally, a 3D data introduction device is generated; in order to avoid the accumulation of thermal stress, a rotation angle of 67° is adopted between successive layers, the laser power is set to 150W, the scanning speed is set to 900mm / s, the scanning pitch is set to 50μm, and the layer thickness is set to 40μm; finally, the oxygen content is adjusted, and the substrate is preheated and printed.

[0009] In the above technical means, in order to prevent oxidation of the molded article, the threshold value of the oxygen content when adjusting the oxygen content is less than 100 ppm.

[0010] In the above technical means, in order to reduce the residual stress generated during the manufacturing process, the preheating temperature when preheating the substrate is 150-170°C.

[0011] In the above technical means, in step 1, the area of ​​the substrate is 248×248×20 (mm), and the size of the SLM-NiTi print is 5×5×5 (mm).

[0012] In the above technical means, in step 2, cooling is performed by water cooling.

[0013] In the above technical means, the high-performance NiTi SMA obtained in step 2 has a grain size of 6.592-150.582 μm, a breaking elongation of 11.92-13.95%, and realizes 100% superelasticity.

[0014] In the above technical means, the austenite crystal orientation of the high-performance NiTi SMA obtained in step 2 is <110> It is.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. By annealing the SLM-NiTi additive manufacturing prints using the method of the present invention, the mechanical properties of the prints can be significantly improved.

[0017] After annealing at 2.750-1050℃ for 50-90min and then water cooling, the tensile strength is reduced by only 2.7%-20.3% compared to the NiTi SMA without annealing process, while the breaking elongation is improved by 17.1%-56.3%, and 100% superelasticity is achieved.

[0018] 3. The annealing process can significantly improve key indicators that determine the use stability of parts, such as plasticity and superelasticity, and improve the reliability of the printed matter in actual use. This method is favorable for extending the actual service life of SLM-NiTi additive manufacturing products. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a schematic diagram of a test piece for tensile and superelastic tests. [Diagram 2] 1 shows SLM-NiTi test pieces in Comparative Example 1 and Examples 1 to 3 in (a) the printed state, (b) the state after heat treatment at 750° C., (c) the state after heat treatment at 950° C., and (d) the state after heat treatment at 1050° C. [Diagram 3] FIG. 2 is a statistical diagram of grain sizes of SLM-NiTi specimens in Comparative Example 1 and Examples 1 to 3. [Figure 4] 1 shows test results of tensile performance of SLM-NiTi test pieces in Comparative Example 1 and Examples 1 to 3. [Diagram 5]1 shows the results of superelasticity tests of SLM-NiTi specimens in Comparative Example 1 and Examples 1 to 3. (a) As printed, (b) As heat-treated at 750°C, (c) As heat-treated at 950°C, and (d) As heat-treated at 1050°C. [Figure 6] 1 shows (a) the phase transition temperatures and Ni contents of the SLM-NiTi specimens in Comparative Example 1 and Examples 1 to 3, and (b) room temperature XRD images. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described in more detail below with reference to specific examples. Note that the specific examples described here are merely for the purpose of illustrating the present invention and are not intended to limit the present invention.

[0021] All the examples are produced using the following method: selective laser melting with Renishaw AM400 is used to produce SLM-NiTi prints, using spherical or near-spherical gas atomized equiatomic Ni50Ti50 powder as raw material, as-cast NiTi alloy as substrate, and the size is 248mm x 248mm x 20mm.

[0022] Comparative Example 1 The as-printed SLM-NiTi SMA is fabricated by the following method. First, the substrate is mounted, and before mounting, the surface of the substrate is sandblasted to remove dirt on the substrate surface and form a uniform and fine uneven surface, thereby improving the uniformity of powder scattering and the adhesion of the substrate to the powder; then, the powder is loaded, and before loading, the powder is vibrated and sieved through a 250 mesh standard sieve before being put into the hopper, thereby improving the flowability of the powder; further, the 3D model is sliced, parameter setting and scanning strategy editing are performed using the dedicated software (QuantAM and Material Editor) provided with the device; finally, a 3D data introduction device is generated; in order to avoid the accumulation of thermal stress, a rotation angle of 67° is adopted between successive layers, the laser power is set to 150W, the scanning speed is set to 900mm / s, the scanning pitch is set to 50μm, and the layer thickness is set to 40μm; finally, the oxygen content is adjusted, and the substrate is preheated and printed. To prevent oxidation of the molded product, the oxygen content threshold during SLM operation was set to less than 100 ppm, and to reduce residual stresses generated during the manufacturing process, the substrate was preheated to 170 °C. After printing was completed, it was cooled together with the chamber for 4 h to obtain the as-printed SLM-NiTiSMA (denoted as As-SLM).

[0023] To study the microstructure and performance of the as-printed (Comparative Example 1) and heat-treated SLM-NiTi SMAs (Examples 1-3), specimens were machined and polished to 5 mm × 5 mm × 5 mm specimens. To test their mechanics and superelasticity, specimens were machined according to the dimensions shown in Figure 1 and tested by a Lishi LD26 type electronic universal testing machine equipped with an extensometer (measurement range 25 mm). Here, the tensile speed was 5 × 10 -4 / s.

[0024] In the superelasticity test method, the specimens were subjected to strains of 2, 4, 6, and 8% at room temperature and then unloaded to 2 MPa.

[0025] The as-printed SLM-NiTi SMA obtained in Comparative Example 1 had a grain size of 8.982 μm, a tensile strength of 921.62±6 MPa, and an elongation at break of 10.18±0.31%, and did not exhibit superelasticity when strained.

[0026] Example 1 The as-printed SLM-NiTi SMA obtained in Comparative Example 1 was annealed at 750°C for 1h and water-cooled to obtain an annealed SLM-NiTiSMA (denoted as S750). Its grain size was 6.592μm, tensile strength was 896.75±7MPa, elongation at break was 11.92±0.84%, superelastic recovery after 2% strain was 90.5%, superelastic recovery after 4% strain was 81%, superelastic recovery after 6% strain was 42.17%, and superelastic recovery after 8% strain was 24.75%.

[0027] Example 2 The as-printed SLM-NiTi SMA obtained in Comparative Example 1 was annealed at 950°C for 1h, and after water cooling, the annealed as-SLM-NiTi SMA (denoted as S950) was obtained. Its grain size was 47.678μm, tensile strength was 816.24±6MPa, elongation at break was 15.91±1.20%, superelastic recovery after 2% strain was 100%, superelastic recovery after 4% strain was 86%, superelastic recovery after 6% strain was 50.33%, and superelastic recovery after 8% strain was 32%.

[0028] Example 3 The as-printed SLM-NiTi SMA obtained in Comparative Example 1 was annealed at 1050°C for 1h and water-cooled to obtain the as-annealed SLM-NiTi SMA (denoted as S1050). Its grain size was 150.582μm, tensile strength was 733.99±6MPa, breaking elongation was 13.95±0.78%, superelastic recovery after 2% strain was applied was 100%, superelastic recovery after 4% strain was applied was 84.75%, superelastic recovery after 6% strain was 47.33%, and expired when 8% strain was applied.

[0029] Regarding the above Comparative Example 1 and Examples 1 to 3 The microstructure, tensile performance and superelasticity tests of the as-printed (Comparative Example 1) and heat-treated SLM-NiTi SMAs (Examples 1-3) were studied, and it was found that with increasing annealing temperature, the grain size and elongation at break gradually increased, whereas the tensile strength tended to decrease (Figs. 3 and 4). In particular, the SLM-NiTi specimens after annealing showed significant superelasticity, with the superelasticity optimal at 950 °C (Fig. 5). Understanding the mechanisms of these phenomena is advantageous for selecting the appropriate annealing process to satisfy practical applications.

[0030] To study the mechanism of the tensile performance and superelasticity change, we first characterized the phase transition behavior, Ni content, and room temperature phase structure of the as-printed and heat-treated SLM-NiTiSMA (Fig. 6). After heat treatment, the Ni content of the specimens increased, the phase transition temperature decreased, and the room temperature structure transformed from martensite to austenite, which caused the heat-treated specimens to exhibit superelasticity.

[0031] As can be seen from Figures 2-4 and 6, at 750 °C, recrystallization occurred in the SLM-NiTi specimen, and the microstructure of the specimen transformed from elongated columnar crystals in the printed state to uniform fine equiaxed crystals. The elongation to failure of the specimen increased by 17.1%, while the strength decreased by only 2.7%. At 950 °C, the structure of the SLM-NiTi specimen was a mixed phase of coarse columnar crystals and equiaxed crystals. In this case, the elongation to failure increased by 56.3%, while the strength decreased by 11.4%. At 1050 °C, the structure of the SLM-NiTi specimen was coarse columnar crystals. In this case, the elongation to failure increased by 37.0%, while the strength decreased by 20.3%. As is evident, the fine crystals enhanced the strength, while the oxides reduced its ductility.

[0032] As can be seen from Figures 2-3, 5 and 6, during the superelasticity test period, the SLM-NiTi specimen fractured early at 1050 °C, because the oxides and coarse crystals reduced the reliability of the SLM-NiTi specimen.

[0033] Therefore, when the superelastic NiTi SMA requires high strength, it is preferable to anneal at an annealing temperature of 750°C for 1 hour to obtain uniform and fine equiaxed crystals. As a result, the NiTi SMA has superelasticity and high strength. When the superelastic NiTi SMA requires high plasticity, it is preferable to anneal at an annealing temperature of 950 to 1050°C for 1 hour to obtain coarse crystals. As a result, the NiTi SMA has superelasticity and high plasticity. Also, when the superelastic NiTi SMA requires good overall performance, it is preferable to anneal at an annealing temperature of 750 to 950°C for 1 hour to obtain a structure in which coarse crystals and fine crystals are mixed. As a result, the NiTi SMA has high plasticity and excellent reliability in addition to superelasticity.

[0034] As the heat treatment temperature increased, the grain size of the SLM-NiTi specimens decreased and then increased through three processes, namely, recovery, recrystallization, and abnormal growth. In addition, as the heat treatment temperature increased, the crystal orientation of the specimens continued to change, especially <110> As is known, the ductility of SLM-NiTi alloys is closely related to the crystal orientation. <001> In the oriented direction, the specimens fractured prematurely and the tensile performance was significantly reduced. <110> In the orientation, the test specimen has a relatively high elongation rate, which is favorable for tensile performance. When the heat treatment temperature exceeds 750 °C, the test specimen completes the recrystallization process, compared with the alloy test specimen in the printed state. <110> The stronger orientation resulted in higher plasticity of the specimen. In addition, as the heat treatment temperature increased, the diffusion ability of Ti atoms was gradually activated, the supersaturated Ti atoms were activated, and Ti2Ni precipitate phase was precipitated, which resulted in higher Ni atom content in the substrate, lowering the phase transition temperature, and the room temperature phase structure was transformed into the austenite phase, and the specimen showed superelasticity. In addition, since the fine crystals suppress the stress martensitic transformation, the alloy grew larger during the heat treatment process (heat treatment temperature 750-1050°C), the grain size became larger, and the alloy was more likely to generate stress-induced martensite, ultimately achieving excellent superelasticity. However, when the heat treatment temperature exceeded 1050°C, the alloy was more likely to generate oxides, which resulted in poor tensile and functional properties.

[0035] The above description is only the preferred embodiment of the present invention. Those skilled in the art can make multiple improvements and modifications without departing from the principle of the present invention. These improvements and modifications should fall within the protection scope of the present invention.

Claims

1. A method for producing a NiTi SMA comprising the steps of: The NiTi shape memory alloy was printed by selective laser melting and naturally cooled to room temperature to obtain the SLM-NiTi print. 5 0Ti 5 Step 1: Using NiTi0 as raw material and as-cast NiTi shape memory alloy as substrate; Step 2 is to keep the SLM-NiTi printed matter obtained in step 1 at 750-1050°C for 50-90 min and then cool it by water cooling to obtain NiTi SMA; A method comprising:

2. 2. The method of claim 1, wherein in step 1, a Renishaw AM400 selective laser melting machine is used to print the NiTi shape memory alloy.

3. In step 1, the printing process is as follows: The method according to claim 1, characterized in that: first, the substrate is mounted, and before mounting, the surface of the substrate is sandblasted to remove dirt on the substrate surface to form a uniform and fine uneven surface, thereby improving the uniformity of powder scattering and the adhesion between the substrate and the powder; then, the powder is loaded, and before loading, the powder is vibrated and sieved through a 250 mesh standard sieve before being loaded into a hopper, thereby improving the flowability of the powder; and then, the 3D model is sliced, parameter setting and scanning strategy editing are performed through the dedicated software attached to the selective laser melting device, and finally a 3D data introduction device is generated; in order to avoid the accumulation of thermal stress, a rotation angle of 67° is adopted between successive layers, the laser power is set to 150W, the scanning speed is set to 900mm / s, the scanning pitch is set to 50μm, and the layer thickness is set to 40μm; finally, the oxygen content is adjusted, and the substrate is preheated and printed.

4. 2. The method according to claim 1, characterized in that the threshold oxygen content when adjusting the oxygen content is less than 100 ppm.

5. The method according to claim 1, wherein the preheating temperature of the substrate is 150-170°C.

6. 2. The method according to claim 1, wherein in step 1, the area of ​​the substrate is 248×248×20 mm, and the size of the SLM-NiTi print is 5×5×5 mm.

7. The method of claim 1, wherein the high performance NiTi SMA obtained in step 2 has a grain size of 6.592-150.582 μm, a breaking elongation of 11.92-13.95%, and achieves 100% superelasticity.

8. 2. The method of claim 1, wherein the austenite crystal orientation of the high performance NiTi SMA obtained in step 2 is <110>.