Antireflection film laminate, article provided therewith, and method for manufacturing antireflection film laminate

The antireflection film laminate with a hard coat, inorganic multilayer, and adhesive layers addresses the issue of display surface shattering and edge formation, improving visibility and safety in transportation machines.

JP2024161034AInactive Publication Date: 2024-11-15DEXERIALS CORP
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
JP2024139855
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing antireflection films attached to display surfaces in transportation machines like automobiles are insufficient in preventing the display surface from shattering and the formation of sharp edges during accidents, which can cause injuries to passengers.

Method used

An antireflection film laminate comprising a first transparent base material with a hard coat layer, an inorganic multilayer film layer, an antifouling layer, and a two-layer adhesive layer, designed to have a reflectance of 0.8% or less and a breaking force of 5.7N or more, ensuring visibility and edge suppression.

Benefits of technology

The laminate enhances visibility and prevents the formation of sharp edges, reducing the risk of injury during accidents by maintaining structural integrity and optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161034000001_ABST
    Figure 2024161034000001_ABST
Patent Text Reader

Abstract

To provide an antireflection film laminate that has improved visibility and excels in the ability to prevent splashing on display surface and suppress the occurrence of sharp edges.SOLUTION: Provided is an antireflection film laminate comprising: a first transparent substrate having a first face and a second face; an antireflection layer having a hard coat layer, an inorganic multilayered film layer, and an anti-fouling layer that are provided in order on the first face; and an adhesive layer provided on top of the second face. The hard coat layer is a single layer being in contact with the first face. The adhesive layer adjoins the second face, and the inorganic multilayered film layer is a laminate of a low refraction index layer and a high refraction index layer. The adhesive layer is composed of two-layered adhesive layers and a second transparent layer held therebetween and composed of PET film adhered directly to each. The reflectance Y in a visible ray region at an incidence angle 5° is 0.8% or less, the fracture force in a thrust stabbing test is 5.7 N or greater, the thickness of the first transparent substrate is 80 μm or less, and the thickness of the second transparent substrate is less than 12 μm. The two-layered adhesive layers are formed on both sides of the second transparent substrate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anti-reflection film laminate, and more particularly to an anti-reflection film laminate that is suitably used in combination with a display or the like provided in the interior of a transport machine such as an automobile. [Background technology]

[0002] In the cockpits of automobiles and other transport vehicles, displays using liquid crystal panels and the like are becoming more common in order to handle large amounts of information. Anti-reflective films have long been used in displays to improve visibility.

[0003] On the other hand, when a display is used in the cockpit of a transport vehicle, it is known that it is necessary to deal with the possibility of a passenger hitting their head on the display due to impact in an accident, resulting in injury from broken glass. Proposals have been made to improve the bonding structure of the cover glass used for the display and to improve the installation structure of the display. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2017 / 208995 [Patent Document 2] International Publication No. 2002 / 009976 Summary of the Invention [Problem to be solved by the invention]

[0005] In response to these proposals, it is conceivable that an adhesive layer could be provided on an optical film such as an anti-reflective film and attached to a display to improve visibility while protecting passengers by preventing the surface of the display from shattering in the event of an accident and suppressing the occurrence of so-called sharp edges, where broken glass protrudes from the broken surface.

[0006] However, it was found that simply attaching an anti-reflection film to a cover glass on a display surface via an adhesive layer was insufficient to suppress the occurrence of sharp edges. Furthermore, as a result of intensive research, the present inventors have found that in an anti-reflection film laminate in which an adhesive function is imparted to an anti-reflection film, the above problem can be solved by ingeniously devising the configuration of the adhesive layer used when attaching the anti-reflection film to the cover glass on the display surface, and have completed the present invention.

[0007] An object of the present invention is to provide an anti-reflection film laminate that is excellent in preventing scattering on a display surface and suppressing the occurrence of sharp edges while improving visibility, and an article including the same. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention provides the following means.

[0009] An antireflection film laminate according to one embodiment of the present invention comprises a first transparent substrate having a first surface and a second surface opposite to the first surface, an antireflection layer including at least a hard coat layer, an inorganic multilayer film layer, and an antifouling layer, which are provided in that order on the first surface, and an adhesive layer provided on the second surface, the adhesive layer comprising two adhesive layers and a second transparent substrate sandwiched between the two adhesive layers, the adhesive layer having a reflectance Y of 0.8% or less when light having a wavelength of 380 nm to 780 nm by standard light source D65 is incident at an incident angle of 5°, and a breaking force of 5.7 N or more when a conical probe having a diameter of 8 mm is pressed against the antireflection film laminate at a puncture test speed of 500 mm / min.

[0010] In the antireflection film laminate according to the above embodiment, the second transparent substrate may be a PET film having a thickness of less than 12 μm.

[0011] In the antireflection film laminate according to the above embodiment, the second transparent substrate may be a TAC film.

[0012] In the antireflection film laminate according to the above embodiment, the inorganic multilayer film layer may be a laminate of a low refractive index material layer and a high refractive index material layer, and the low refractive index material layer and the high refractive index material layer may be sputtered films.

[0013] In the antireflection film laminate according to the above embodiment, the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer may have a storage modulus at 25° C. of 0.20 to 0.10 MPa and a loss tangent of 0.40 to 0.20.

[0014] The antireflection film laminate according to the above embodiment may have a thickness of 170 μm or less.

[0015] The antireflection film laminate according to the above embodiment may further comprise a protective film on the side of the antifouling layer opposite the first transparent substrate, and may further comprise a release film on the side of the pressure-sensitive adhesive layer away from the first transparent substrate, opposite the second transparent substrate, of the two pressure-sensitive adhesive layers.

[0016] An article according to another aspect of the present invention includes the anti-reflection film laminate of the above aspect. Effect of the Invention

[0017] According to the present invention, it is possible to provide an anti-reflection film laminate which is excellent in preventing scattering on the display surface and suppressing the occurrence of sharp edges while improving visibility. [Brief description of the drawings]

[0018] [Figure 1] 1 is a schematic cross-sectional view of an antireflection film laminate according to one embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view of an antireflection film laminate according to another embodiment of the present invention. [Diagram 3] FIG. 1A is a perspective view showing an overview of a piercing test, and FIG. 1B is a schematic plan view showing a state in which an antireflection film laminate sample used in the piercing test is attached to a sample setting table. [Figure 4]FIG. 4 is a schematic cross-sectional view showing an enlarged portion of the state in which the anti-reflection film laminate sample shown in FIG. 3(a) is sandwiched between a sample setting table and a pressing plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate modifications can be made within the scope of the effects of the present invention. The configuration shown in one embodiment can also be applied to other embodiments.

[0020] FIG. 1 is a schematic cross-sectional view of an antireflection film laminate according to one embodiment of the present invention.

[0021] The antireflection film laminate 100 shown in FIG. 1 comprises a first transparent substrate 10 having a first surface 10a and a second surface 10b which is the reverse surface of the first surface 10a, an antireflection layer 20 including at least a hard coat layer 21, an inorganic multilayer film layer 22, and an antifouling layer 23 which are provided in that order on the first surface 10a, and an adhesive layer 30 provided on the second surface 10b. The adhesive layer 30 comprises two adhesive layers 31, 33 and a second transparent substrate 32 sandwiched between the two adhesive layers 31, 33. The adhesive layer 30 has a luminous reflectance of 0.8% or less when light having a wavelength of 380 nm to 780 nm by a standard light source D65 is incident at an incident angle of 5°, and has a breaking stress of 5.7 N or more when a conical probe having a diameter of 8 mm is pressed against the antireflection film 100 at a puncture test speed of 500 mm / min.

[0022] 2, in terms of ease of handling during transportation and storage, a known protective film 40 may be further provided on the surface 23a of the antifouling layer 23 opposite to the surface 23b on the first transparent substrate 10 side. Examples of the protective film 40 include those using polypropylene, polyethylene, polyethylene terephthalate, or the like as a base material and having an adhesive layer mainly composed of natural rubber, synthetic rubber, acrylic resin, or the like. Furthermore, of the two pressure-sensitive adhesive layers 31 and 33, a surface 33b opposite to a surface 33a on the second transparent substrate side of the pressure-sensitive adhesive layer 33 away from the first transparent substrate 10 may further be provided with a known release film 50. An example of the release film 50 is a polyethylene terephthalate film having a surface coated with a silicone material or a fluorine-based material.

[0023] [First transparent base material] The first transparent substrate 10 has a first surface 10a and a second surface 10b that is the surface on the rear side of the first surface 10a.

[0024] The first transparent substrate 10 may be formed of a transparent material capable of transmitting light in the visible light range, and for example, a plastic film is preferably used. Specific examples of the constituent material of the plastic film include polyester resin, acetate resin, polyethersulfone resin, polycarbonate resin, polyamide resin, polyimide resin, polyolefin resin, (meth)acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin, polyarylate resin, and polyphenylene sulfide resin. In addition, a reinforcing material may be included as long as it does not impair the optical properties, and examples of such materials include cellulose nanofiber and nanosilica. In particular, polyester resin, acetate resin, polycarbonate resin, and polyolefin resin are preferably used, and specifically, a triacetyl cellulose (TAC) substrate and a polymethyl methacrylate substrate are preferably used. In addition, a glass film can be used as the inorganic substrate.

[0025] When the plastic film is a TAC substrate, when a hard coat layer 21 is formed on one side thereof, a permeation layer can be formed in which some of the components constituting the hard coat layer 21 penetrates, and this can suppress the adhesion between the transparent substrate and the hard coat layer 21 and the occurrence of interference fringes due to the difference in refractive index between the layers.

[0026] The first transparent substrate 10 may be a film having an optical or physical function. Examples of films having optical or physical functions include a polarizing plate, a retardation compensation film, a heat shielding film, a transparent conductive film, and a brightness enhancing film.

[0027] The thickness of the first transparent substrate 10 is not particularly limited, but is preferably, for example, 25 μm or more, and more preferably 40 μm or more. If the thickness of the first transparent substrate 10 is less than 25 μm, wrinkles are likely to occur when stress is applied, which may make it difficult to continuously form the hard coat layer 21 on the first transparent substrate 10 when producing the antireflection film laminate 100. In addition, curling may become large, and scratch hardness may deteriorate.

[0028] In the case where production is performed in a roll, if the thickness of the first transparent substrate 10 exceeds 300 μm, the first transparent substrate 10 cannot be rolled when producing the antireflection film laminate 100, or it may be disadvantageous in terms of thinning, weight reduction, and cost reduction of the antireflection film laminate 100. Furthermore, gas (moisture, organic matter, etc.) is likely to be generated from the first transparent substrate 10 when laminating the hard coat layer 21, which may be an obstruction to the formation of the hard coat layer 21.

[0029] The surface of the first transparent substrate 10 may be previously subjected to an etching treatment such as sputtering, corona discharge, ultraviolet irradiation, electron beam irradiation, chemical conversion, oxidation, or an undercoat treatment. By previously performing these treatments, it is possible to improve the adhesion with the hard coat layer 21 formed on the first transparent substrate 10. In addition, it is also preferable to remove dust and clean the surface of the first transparent substrate 10 by performing solvent cleaning, ultrasonic cleaning, or the like as necessary before forming the hard coat layer 21.

[0030] [Anti-reflection layer] The antireflection layer 20 is provided on the first surface 10a of the first transparent substrate 10, and includes a hard coat layer 21, an inorganic multilayer film layer 22, and an antifouling layer 23 in this order from the first surface 10a side.

[0031] <Hard coat layer> The hard coat layer 21 is a hardened layer of an organic material formed between the first transparent substrate 10 and the inorganic multilayer film layer 22, or a hardened layer of an organic material containing an inorganic material.

[0032] The hard coat layer 21 may contain silica (oxide of silicon) particles or alumina (aluminum oxide) particles as a filler in a binder resin. These silica particles or alumina particles may be exposed from the surface of the hard coat layer 21 on the inorganic multilayer film layer 22 side. With this configuration, the inorganic multilayer film layer 22 can be strongly bonded to the binder resin of the hard coat layer 21, and adheres more firmly to the exposed silica particles or alumina particles, improving the adhesion between the hard coat layer 21 and the inorganic multilayer film layer 22, and improving the scratch resistance of the antireflection film laminate 100.

[0033] Moreover, the silica particles or alumina particles serving as the filler of the hard coat layer 21 preferably have an average particle size of, for example, 800 nm or less, preferably 780 nm or less, and more preferably 100 nm or less, and are dispersed in the form of single particles in the binder resin of the hard coat layer 21. By dispersing the silica particles or alumina particles as such a filler, fine irregularities can be formed on the surface of the hard coat layer 21, and the hardness of the hard coat layer 21 can be increased, and the adhesion to the antireflection film laminate 100 can be improved.

[0034] The binder resin of the hard coat layer 21 is preferably transparent, and for example, an ionizing radiation curable resin that is cured by ultraviolet light or electron beams, a thermoplastic resin, a thermosetting resin, or the like can be used.

[0035] Examples of the ionizing radiation curable resin used as the binder resin of the hard coat layer 21 include ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, and N-vinylpyrrolidone. Examples of the compound that is an ionizing radiation curable resin having two or more unsaturated bonds include trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, dipentaerythritol hexa ... Examples of the polyfunctional compounds include erythritol penta(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerin tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate. Among them, pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), and pentaerythritol tetraacrylate (PETTA) are preferably used. Incidentally, "(meth)acrylate" refers to methacrylate and acrylate. In addition, as the ionizing radiation curable resin, the above-mentioned compounds modified with PO (propylene oxide), EO (ethylene oxide), CL (caprolactone), etc. can also be used.

[0036] Examples of the thermoplastic resin used for the binder resin of the hard coat layer 21 include styrene-based resins, (meth)acrylic resins, vinyl acetate-based resins, vinyl ether-based resins, halogen-containing resins, alicyclic olefin-based resins, polycarbonate-based resins, polyester-based resins, polyamide-based resins, cellulose derivatives, silicone-based resins, and rubber or elastomers. The thermoplastic resin is preferably non-crystalline and soluble in an organic solvent (particularly a common solvent capable of dissolving a plurality of polymers and curable compounds). In particular, from the viewpoint of transparency and weather resistance, styrene-based resins, (meth)acrylic resins, alicyclic olefin-based resins, polyester-based resins, cellulose derivatives (cellulose esters, etc.), and the like are preferred.

[0037] Examples of thermosetting resins used as the binder resin of the hard coat layer 21 include phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, unsaturated polyester resins, polyurethane resins, epoxy resins, aminoalkyd resins, melamine-urea co-condensation resins, silicon resins, and polysiloxane resins (including so-called silsesquioxanes such as cage-shaped and ladder-shaped silsesquioxanes).

[0038] The hard coat layer 21 may contain an organic resin and an inorganic material, or may be an organic-inorganic hybrid material. For example, the hard coat layer 21 may be formed by a sol-gel method, and examples of the inorganic material include silica, alumina, zirconia, and titania, and examples of the organic material include acrylic resin.

[0039] The thickness of the hard coat layer 21 is not particularly limited, but is preferably, for example, 0.5 μm or more, more preferably 1 μm or more, and the upper limit is 100 μm or less. If the thickness of the hard coat layer 21 is less than 0.5 μm, there is a concern that the strength will be insufficient and the scratch hardness will be deteriorated. On the other hand, if the thickness of the hard coat layer 21 is too thick, it may be disadvantageous for making the antireflection layer 20 thinner, lighter, and less expensive.

[0040] The hard coat layer 21 may be a single layer or multiple layers. The hard coat layer 21 may further be provided with known functions such as ultraviolet absorbing performance, antistatic performance, refractive index adjusting function, hardness adjusting function, etc. Furthermore, the function to be imparted to the hard coat layer 21 may be imparted to a single hard coat layer 21, or may be imparted to a plurality of separate layers.

[0041] <Inorganic multilayer film layer> The inorganic multilayer film layer 22 is a laminate that exhibits an optical function, and in this embodiment, an anti-reflection function. The inorganic multilayer film layer 22 in this embodiment is a laminate in which a low refractive index layer a and a high refractive index layer b are alternately laminated in this order from the hard coat layer 21 side, and for example, the hard coat layer 21 side and the antifouling layer 23 side are both low refractive index layers a, making a total of five layers. Of these, the low refractive index layer a in contact with the hard coat layer 21 functions as an adhesive layer for the hard coat layer 21 . The number of low refractive index layers a and high refractive index layers b is not limited to five, and any number of low refractive index layers a and high refractive index layers b can be formed.

[0042] The low refractive index layer a is a layer containing SiO2 (oxide of Si) as a main component, etc. The SiO2 single layer film is colorless and transparent, and the refractive index of the low refractive index layer is preferably 1.20 to 1.60, and more preferably 0 to 1.50. The inorganic thin film layer containing an oxide of Si may contain up to 50% of another element. It may contain Na for the purpose of improving durability, and Zr, Al, or N for the purpose of improving hardness. The content is preferably 10% or less. The refractive index of the high refractive index layer is preferably 2.00 to 2.60, and more preferably 2.10 to 2.45. Examples of such high refractive index dielectric materials include niobium pentoxide (Nb2O5, refractive index 2.33), titanium oxide (TiO2, refractive index 2.33 to 2.55), tungsten oxide (WO3, refractive index 2.2), cerium oxide (CeO2, refractive index 2.2), tantalum pentoxide (Ta2O5, refractive index 2.16), zinc oxide (ZnO, refractive index 2.1), and indium tin oxide (ITO, refractive index 2.06).

[0043] By alternately stacking such low refractive index layers a and high refractive index layers b, light incident from the antifouling layer 23 side is diffused, preventing it from being reflected in one direction, thereby achieving an antireflection function.

[0044] The inorganic multilayer film 22 can be formed by sputtering a low refractive index layer a and a high refractive index layer b. In this case, the sputtering target may be changed when forming the low refractive index layer a and when forming the high refractive index layer b. Alternatively, for example, one type of material may be used as the target, and the oxygen flow rate during sputtering may be changed to alternately form layers made of the target material and layers made of an oxide of the target material, forming the low refractive index layer and the high refractive index layer.

[0045] The thickness of the low refractive index layer a constituting the inorganic multilayer film 22 is appropriately selected depending on the wavelength region requiring the antireflection function, and may be, for example, 1 nm to 200 nm, and the thickness of the high refractive index layer b may be in the range of 15 nm to 200 nm.

[0046] The film thicknesses of the low refractive index layers a and the high refractive index layers b do not all need to be the same, and can be appropriately selected depending on the design of the inorganic multilayer film 22. For example, from the hard coat layer 21 side, they can be a low refractive index layer a of 30 to 120 nm, a high refractive index layer b of 10 to 50 nm, a low refractive index layer a of 30 to 120 nm, a high refractive index layer b of 50 to 200 nm, and a low refractive index layer a of 50 to 200 nm.

[0047] <Anti-stain layer> The antifouling layer 23 is formed on the outermost surface of the inorganic multilayer film layer 22 to prevent the inorganic multilayer film layer 22 from being soiled and to suppress wear of the inorganic multilayer film layer 22 due to its abrasion resistance when applied to a touch panel or the like.

[0048] As the fluorine-based organic compound constituting the antifouling layer 23, a compound consisting of a fluorine-modified organic group and a reactive silyl group (e.g., alkoxysilane) is preferably used. One example is perfluorodecyltriethoxysilane (FDTS). Commercially available products include Optool DSX (manufactured by Daikin Corporation) and KY-1901 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0049] In addition, the antifouling layer 23 may further contain additives such as a light stabilizer, an ultraviolet absorber, a colorant, an antistatic agent, a lubricant, a leveling agent, an antifoaming agent, an antioxidant, a flame retardant, an infrared absorber, and a surfactant, as necessary.

[0050] The anti-fouling layer 23 may be formed by diluting the above-mentioned fluorine compound with a soluble solvent, applying the dilution to the inorganic multilayer film layer 22 using a known application device such as a bar coater, and then drying the dilution, or may be formed by a deposition method or the like.

[0051] [Adhesive layer] The adhesive layer 30 is provided on the second surface 10b of the first transparent substrate 10, and is composed of a second transparent substrate 32 and two adhesive layers 31, 33 provided on both surfaces of the second transparent substrate 32.

[0052] <Second transparent base material> The second transparent base material 32 may be formed of a transparent material capable of transmitting light in the visible light range, and for example, a plastic film is preferably used. Specific examples of the constituent material of the plastic film include polyester resin, acetate resin, polyethersulfone resin, polycarbonate resin, polyamide resin, polyimide resin, polyolefin resin, (meth)acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin, polyarylate resin, polyphenylene sulfide resin, etc. In particular, polyester resin, acetate resin, polycarbonate resin, and polyolefin resin are preferably used, and specifically, a triacetyl cellulose (TAC) base material, a polyethylene terephthalate base material, and a polymethyl methacrylate resin are preferably used.

[0053] The material of the second transparent base 32 preferably has a tensile elastic modulus of 490 to 4500 MPa.

[0054] The refractive index of the second transparent substrate 32 preferably has a small difference from that of the first transparent substrate 10 so as not to impair the optical properties of the antireflection film laminate, and can be, for example, less than 0.1.

[0055] <Adhesive layer> In the present embodiment, the adhesive layers 31 and 33 may be made of various pressure-sensitive adhesives such as rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, etc., but acrylic-based adhesives are preferred in terms of their ability to be colorless and transparent, their minimizing loss of optical properties of the anti-reflection film laminate, ease of adjusting adhesiveness, and material selectivity.

[0056] The difference in refractive index between the pressure-sensitive adhesive layers 31, 33 and the second transparent substrate 32 is preferably as small as possible so as not to impair the optical properties of the antireflection film laminate, and can be, for example, 0.12 or less.

[0057] In addition, the adhesive layers 31, 33 formed on both sides of the second transparent substrate 32 may be made of the same composition or different compositions from the viewpoint of desired optical properties and impact resistance, but it is preferable in terms of optical properties that there is a small difference in refractive index between the two sides.

[0058] From the viewpoint of impact resistance, the pressure-sensitive adhesive layers 31, 33 preferably have a storage modulus at 25° C. of 0.20 to 0.10 MPa and a loss tangent of 0.40 to 0.20.

[0059] The method for producing the adhesive layer 30 is not particularly limited, and examples thereof include a method of applying an adhesive composition diluted with a solvent to the second transparent substrate 32 and drying it, a method of applying the adhesive composition to the second transparent substrate 32 and then curing it by irradiating it with ultraviolet light when the adhesive composition is a solventless ultraviolet-curable composition, a method of transferring an adhesive layer from a release sheet having adhesive layers 31 and 33 provided thereon to the second transparent substrate 32, and a combination of these methods may be used. The thickness of the adhesive layer is not particularly limited, but is preferably about 5 to 30 μm.

[0060] [Method for producing anti-reflection film laminate] An example of a method for producing an anti-reflection film laminate includes a method in which an anti-reflection layer is formed on the first surface of a first transparent substrate, and then an adhesive layer produced by the above-mentioned method is laminated to the first surface using one of the adhesive layers. Alternatively, an adhesive layer may be laminated to the second surface of the first transparent substrate, and then an anti-reflection layer may be formed on the first surface.

[0061] Another example is a method in which one side of an adhesive layer is first formed on the second surface of a first transparent substrate, and then a release film is attached for protection, an anti-reflection layer is formed on the first surface of the first transparent substrate, the release film is then peeled off, and a separately manufactured second transparent substrate having an adhesive layer on only one surface thereof is attached.

[0062] [Goods] The article in this embodiment is, for example, an anti-reflection film laminate provided on the display surface of an image display unit such as a liquid crystal display panel, an organic EL display panel, etc. This makes it possible to impart an effect of reducing injuries caused when a strong force is applied to a liquid crystal display panel or an organic EL display panel, particularly a liquid crystal display panel or an organic EL display panel provided inside or outside a transport machine such as an automobile, during an accident.

[0063] In addition, the article is not limited to an image display device, and examples thereof include window glass or goggles having the antireflection film laminate of the present embodiment on the surface, the light receiving surface of a solar cell, a smartphone screen, a personal computer display, an information input terminal, a tablet terminal, an electric display board, a glass table surface, a game machine, a navigation support device for an aircraft or train, a navigation system, an instrument panel, the surface of an optical sensor, a helmet visor, a mirror, a head mounted display, and the like. EXAMPLES

[0064] Example 1 The first transparent substrate was a TAC film having a thickness of 80 μm. The photocurable resin composition shown in Table 1 below was applied to the first surface of the TAC film using a bar coater, and the resin composition was then photopolymerized and dried to form a hard coat layer having a thickness of 5 μm. [Table 1]

[0065] Next, the glow discharge treatment speed was increased to 8300 W·min / m 2 The hard coat layer was subjected to a surface treatment.

[0066] After the glow treatment, a 10 nm thick adhesion layer (low refractive index layer) made of SiOx was formed by sputtering, and a 200 nm thick AR layer (inorganic multilayer film layer) made of a Nb2O5 film (high refractive index layer), a SiO2 layer (low refractive index layer), a Nb2O5 film (high refractive index layer), and a SiO2 layer (low refractive index layer) was formed on the adhesion layer. Furthermore, a 10 nm thick antifouling layer made of an alkoxysilane compound having a perfluoropolyether group was formed on the AR layer to obtain an antireflection layer.

[0067] On the other hand, a 25 μm thick TAC film (refractive index 1.49) was used as the second transparent substrate, and an acrylic adhesive with a refractive index of 1.47 was applied to both sides of the film with a thickness of 10 μm using a bar coater to form an adhesive layer, thereby obtaining an adhesive layer.

[0068] Thereafter, the first surface of the pressure-sensitive adhesive layer in the pressure-sensitive adhesive layer was attached to the second surface of the first transparent substrate to obtain an antireflection film laminate having a pressure-sensitive adhesive layer.

[0069] Example 2 An antireflection film laminate was obtained in the same manner as in Example 1, except that the second transparent substrate was a transparent PET film (refractive index: 1.58) having a thickness of 6 μm.

[0070] Example 3 An antireflection film laminate was obtained in the same manner as in Example 1, except that the second transparent substrate was a transparent PET film (refractive index: 1.58) having a thickness of 9 μm.

[0071] Comparative Example 1 An acrylic adhesive was applied to a PET film having a thickness of 75 μm that had been subjected to a release treatment to form an adhesive layer having no second transparent substrate, and the adhesive layer was then bonded to the antireflection layer obtained in the same manner as in Example 1 to obtain an antireflection film laminate having an adhesive layer having no second transparent substrate.

[0072] Comparative Example 2 An antireflection film laminate was obtained in the same manner as in Example 1, except that the second transparent substrate was a transparent PET film (refractive index: 1.58) having a thickness of 16 μm.

[0073] Comparative Example 3 An antireflection film laminate was obtained in the same manner as in Example 1, except that the second transparent substrate was a transparent PET film (refractive index: 1.58) having a thickness of 25 μm.

[0074] 〔evaluation〕 The anti-reflection film laminates of the above Examples and Comparative Examples were evaluated for their effect of preventing shattering of a glass panel and their optical properties by the methods described below.

[0075] [Puncture test] In this specification, the piercing test refers to a test in which an antireflection film laminate sample is attached using an adhesive layer over an opening of a sample mounting table (thickness 9 mm) with a circular opening 9 mm high and 9 mm in diameter (see Figure 3(b)), and a pressing plate (thickness 3 mm) with circular openings 3 mm high and 11 mm in diameter is pressed and fixed so that the openings overlap (see Figure 4).A specified piercing tool (probe) is then pressed into the part of the antireflection film laminate sample that overlaps the opening at a constant piercing speed (see Figure 3(a)), and the force (breaking force) at which the antireflection film laminate sample breaks (tears) is measured.

[0076] Samples for the piercing test were prepared by cutting the antireflection film laminates of the above-mentioned Examples and Comparative Examples into 30 mm squares. The piercing tool used was a stainless steel piercing tool (conical probe) with a diameter of 8 mm and a conical tip. The length of the conical part was 6 mm, and the tip of the conical part was sharp. For the measurement, the sample mounting table was set in a testing machine (EZ-SX, manufactured by Shimadzu Corporation) with the pressure plate facing up, and the piercing tool was pressed against the anti-reflective film laminate sample at a piercing speed of 500 mm / min, and the force (breaking force) at which the anti-reflective film laminate sample broke was measured.

[0077] In the anti-reflection film laminate of the present invention, the breaking strength must be 5.7 N or more.

[0078] [Dropping ball test] In this specification, the ball drop test refers to a test sample prepared by laminating the anti-reflection film laminate of the above-mentioned Examples and Comparative Examples to the cover glass of an 8-inch LCD module with cover glass, and then dropping a 6.8 kg iron ball from a height of 2.4 m onto the test sample with the laminated surface facing up, to evaluate the effect of preventing the shattering of the broken cover glass and the effect of preventing the occurrence of sharp edges in the broken cover glass. The above-mentioned LCD module with cover glass is an LCD module having a cover glass made of chemically strengthened soda lime glass with a thickness of 1.1 mm.

[0079] <Shatterproofness evaluation> After the ball drop test, the LCD module was visually inspected for shattered cover glass.

[0080] <Sharp edge evaluation> After the ball drop test, it was confirmed whether the broken cover glass of the LCD module broke through the anti-reflection film laminate.

[0081] [Optical property evaluation] In addition, the reflectance Y (%), total light transmittance (%), and rainbow unevenness of the antireflection film laminate were measured by the following methods.

[0082] <Reflectance Y(%)> Reflectance Y means luminosity-corrected reflectance (luminosity corresponds to the color sensation of the human eye, that is, the sensitivity of the color perception cells of the retina), and specifically, it is the luminosity correction using the color matching function Y(λ) defined by CIE for the spectral reflectance of 380nm to 780nm for the C light source specified in JIS Z8701. Reflected light Y can be measured using a spectrophotometer or the like. Measurements were performed using a spectrophotometer U-4100 (Hitachi High-Tech Science Corporation) under conditions of an incident angle of 5° and standard light source D65.

[0083] In the antireflection film laminate of the present invention, the reflectance Y must be 0.8% or less.

[0084] <Total light transmittance (%)> Total light transmittance refers to all light transmitted when light equivalent to standard light source D65 is incident on the measurement object, and is the value measured using a haze meter manufactured in accordance with the method specified in JIS K7361. The total light transmittance was measured using a haze meter NDH-5000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0085] In the antireflection film laminate of the present invention, the total light transmittance is preferably 94% or more.

[0086] <Rainbow unevenness> Rainbow unevenness refers to rainbow-colored interference unevenness that occurs when light is reflected at each interface and the reflected light interferes with each other. Rainbow unevenness was measured by rotating a laminate of an anti-reflection film and soda-lime glass placed over a liquid crystal display showing white, and checking for any change in color tone.

[0087] <Difference in refractive index between second transparent substrate and pressure-sensitive adhesive layer> In the antireflection film laminate of the present invention, the difference in refractive index between the second transparent substrate and the pressure-sensitive adhesive layer is preferably 0.12 or less.

[0088] The test results are shown in Table 2 below. [Table 2]

[0089] The anti-reflection film laminate according to the embodiment has a reflectance lower than a predetermined value, and therefore has suitable anti-reflection performance, particularly when combined with a display installed in a transport machine such as an automobile, while suppressing the occurrence of sharp edges. Therefore, when an occupant hits his / her head on the display due to an impact during an accident, for example, even if the glass constituting the display is broken, it is expected that injury to the occupant will be reduced.

[0090] Although the antireflection laminate of Comparative Example 1 meets the required performance requirements for reflectivity, it has a low breaking strength in a puncture test and is unable to suppress the occurrence of sharp edges, and it is presumed that its occupant protection performance in the event of an accident is poor.

[0091] The anti-reflection film laminates of Comparative Examples 2 and 3 have a high breaking strength in a puncture test, but have a high reflectance and poor anti-reflection function, and are not suitable for use in combination with displays installed in transportation vehicles such as automobiles. [Explanation of symbols]

[0092] 10 First transparent base material 10a 1st page 10b 2nd side 20 Anti-reflection layer 21 Hard coat layer 22 Inorganic multilayer film layer 23 Antifouling layer 30 Adhesive layer 31, 33 Adhesive layer 32 Second transparent base material

Claims

1. A first transparent substrate having a first surface and a second surface opposite to the first surface; an antireflection layer including at least a hard coat layer, an inorganic multilayer film layer, and an antifouling layer provided in this order on the first surface; an adhesive layer provided on the second surface, the hard coat layer is a single layer in contact with the first surface, The adhesive layer is in contact with the second surface, The inorganic multilayer film is a laminate of a low refractive index material layer and a high refractive index material layer, each of which is a sputtering film, The adhesive layer includes two adhesive layers and a second transparent substrate made of a PET film sandwiched between the two adhesive layers and directly attached to each of the two adhesive layers; The reflectance Y is 0.8% or less when light having a wavelength of 380 nm to 780 nm by a standard light source D65 is incident at an incident angle of 5°, and The breaking force is 5.7 N or more when a conical probe with a diameter of 8 mm is pressed against the specimen at a penetration test speed of 500 mm / min. The thickness of the first transparent substrate is 80 μm or less, The thickness of the second transparent substrate is less than 12 μm; The two pressure-sensitive adhesive layers are formed on both sides of the second transparent substrate, in the anti-reflection film laminate.

2. A first transparent substrate having a first surface and a second surface opposite to the first surface; an antireflection layer including at least a hard coat layer, an inorganic multilayer film layer, and an antifouling layer provided in this order on the first surface; an adhesive layer provided on the second surface, the hard coat layer is a single layer in contact with the first surface, The adhesive layer is in contact with the second surface, The inorganic multilayer film is a laminate of a low refractive index material layer and a high refractive index material layer, each of which is a sputtering film, the adhesive layer comprises two adhesive layers and a second transparent substrate made of a TAC film sandwiched between the two adhesive layers and directly adhering to each of the two adhesive layers; The reflectance Y is 0.8% or less when light having a wavelength of 380 nm to 780 nm by a standard light source D65 is incident at an incident angle of 5°, and The breaking force is 5.7 N or more when a conical probe with a diameter of 8 mm is pressed against the specimen at a penetration test speed of 500 mm / min. The thickness of the first transparent substrate is 80 μm or less, The two pressure-sensitive adhesive layers are formed on both sides of the second transparent substrate, in the anti-reflection film laminate.

3. The anti-reflection film laminate according to claim 2 , wherein the second transparent substrate has a thickness of 25 μm or less.

4. The anti-reflection film laminate according to any one of claims 1 to 3, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus of 0.20 to 0.10 MPa at 25°C and a loss tangent of 0.40 to 0.

20.

5. The anti-reflection film laminate according to any one of claims 1 to 4, having a thickness of 170 µm or less.

6. The anti-reflection film laminate according to any one of claims 1 to 5, wherein the first transparent substrate is a TAC film.

7. The anti-reflection film laminate according to any one of claims 1 to 6, further comprising a protective film on a surface of the antifouling layer opposite to the first transparent substrate, and further comprising a release film on a surface of the pressure-sensitive adhesive layer of the two pressure-sensitive adhesive layers that is away from the first transparent substrate, opposite to the second transparent substrate.

8. The anti-reflection film laminate according to any one of claims 1 to 7, wherein the refractive index difference between the second transparent substrate and the two pressure-sensitive adhesive layers is 0.12 or less.

9. An article comprising the anti-reflection film laminate according to any one of claims 1 to 8.

10. a preparation step of preparing a first transparent substrate having a first surface and a second surface that is a surface on the reverse side of the first surface and a thickness of 80 μm or less; a hard coat layer forming step of forming a single hard coat layer in contact with the first surface; an inorganic multilayer film forming step of forming an inorganic multilayer film layer, which is a laminate of a low refractive index material layer and a high refractive index material layer, on the hard coat layer by sputtering; An adhesive layer preparation step of preparing an adhesive layer including a second transparent substrate made of a PET film and having a thickness of less than 12 μm, and two adhesive layers directly bonded to both sides of the second transparent substrate to sandwich the second transparent substrate; and a lamination step of laminating one of the two pressure-sensitive adhesive layers to the second surface of the first transparent substrate.

11. a preparation step of preparing a first transparent substrate having a first surface and a second surface that is a surface on the reverse side of the first surface and a thickness of 80 μm or less; a hard coat layer forming step of forming a single hard coat layer in contact with the first surface; an inorganic multilayer film forming step of forming an inorganic multilayer film layer, which is a laminate of a low refractive index material layer and a high refractive index material layer, on the hard coat layer by sputtering; an adhesive layer preparation step of preparing an adhesive layer including a second transparent substrate made of a TAC film and having a thickness of 25 μm or less, and two adhesive layers directly bonded to both sides of the second transparent substrate to sandwich the second transparent substrate; and a lamination step of laminating one of the two pressure-sensitive adhesive layers to the second surface of the first transparent substrate.

Citation Information

Patent Citations

  • Film and glass for preventing dispersion of low-reflection glass

    JP1998086264A

  • Antireflecting film

    JP2002006107A

  • Antireflective transparent substrate and image display device

    JP2004126220A

  • Polarizing plate, its manufacturing method and picture display device

    JP2004318054A

  • Plastic film, functional film, and image display

    JP2005178173A