Manufacturing method of secondary battery material
The synthesis of nitrogen-containing carbon quantum dots addresses the issues of high volumetric expansion and reduced capacity in lithium ion batteries by enhancing discharge capacity and rate characteristics, resulting in improved battery performance.
Patent Information
- Application Number
- JP2024146456
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-02-21
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium ion secondary batteries face challenges with high volumetric expansion of Si or Si alloy as negative electrode active materials, leading to deteriorated cycle characteristics, and the addition of conductive aids like carbon materials reduces active material content, affecting battery capacity and conductivity.
A method for producing a secondary battery material using carbon nanostructures, specifically carbon quantum dots synthesized with nitrogen-containing amines, which are non-conductive and emit light, improving rate and cycle characteristics.
The use of nitrogen-containing carbon quantum dots enhances the discharge capacity and rate characteristics of lithium ion batteries, providing excellent performance in both charging and discharging processes.
Smart Images

Figure 2024161153000004 
Figure 2024161153000005 
Figure 2024161153000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a secondary battery material containing carbon nanostructures. [Background technology]
[0002] In recent years, electronic devices have become smaller and lighter, and there is a demand for smaller and lighter batteries to serve as their power sources. Non-aqueous electrolyte secondary batteries such as lithium ion batteries have been put to practical use as small, lightweight, high-capacity chargeable and dischargeable batteries, and are used in portable electronic devices and communication devices such as small video cameras, mobile phones, and laptop computers.
[0003] Lithium-ion secondary batteries have excellent advantages such as high energy density, high capacity and operating voltage compared to other batteries. However, due to their high energy density, there is a risk of overheating or fire depending on the usage conditions, so high safety is required. In particular, hybrid cars, which have been attracting attention recently, require higher energy density and output characteristics, so even higher safety is required.
[0004] Generally, a lithium ion secondary battery is composed of a positive electrode, a negative electrode, and an electrolyte. During charging, lithium ions escape from the positive electrode active material into the electrolyte and are inserted into the negative electrode active material such as carbon particles. During discharging, lithium ions escape from the negative electrode active material into the electrolyte and are inserted into the positive electrode active material, allowing current to be taken out to an external circuit. In this way, charging and discharging are performed inside the lithium ion secondary battery by lithium ions moving between the positive electrode and the negative electrode via the electrolyte.
[0005] On the other hand, as the performance of portable electronic devices improves, batteries with higher capacity are required, and Sn and Si, which have a much higher capacity per unit weight than existing carbon, are being actively researched as negative electrode active materials. However, when Si or Si alloys are used as negative electrode active materials, there is a problem that the volume expansion becomes large and the cycle characteristics become worse. To solve this problem, graphite is mixed, but if the graphite is not distributed uniformly during mixing, the cycle characteristics (lifespan) may decrease.
[0006] In recent years, there has been a demand for further improvement in rate characteristics as lithium-ion secondary batteries are increasingly used for a variety of purposes, such as as high-output power sources for plug-in hybrid vehicles, hybrid vehicles, power tools, etc. Batteries used as these high-output power sources are required to be able to charge and discharge at high speeds.
[0007] In the positive electrode active materials currently in practical use, the theoretical capacity of the positive electrode active material is much lower than that of the negative electrode active material. Therefore, in order to realize high capacity and high output of lithium ion batteries, it is necessary to give the positive electrode high electrical conductivity and ionic conductivity. Therefore, in order to improve the electronic conductivity in the positive electrode, a method of adding a carbon material to the electrode as a conductive assistant is used. Examples of such carbon materials include graphite, acetylene black, ketjen black, and in recent years, carbon nanotubes and graphene have been reported. However, if the amount of such a conductive assistant is increased, the amount of active material in the electrode decreases, and the capacity of the battery decreases.
[0008] Also, in order to increase the electronic conductivity of the electrode material, an electrode material has been proposed in which the particle surface of the electrode active material is covered with an organic compound that is a carbon source, and then the organic compound is carbonized to form a carbonaceous coating on the surface of the electrode active material, and the carbon of this carbonaceous coating is interposed as an electronic conductive material (for example, Patent Document 1). However, the carbonization process requires a long-term heat treatment at a high temperature of 500°C or higher in an inert gas atmosphere, and this heat treatment reduces the capacity of the electrode. In addition, since the carbonization process is performed at a high temperature of 500 to 800°C in a reducing atmosphere or an inert atmosphere, there is a possibility that the positive electrode active material itself will be reduced, so that the usable positive electrode active material has been limited to lithium iron phosphate, lithium nickel phosphate, lithium cobalt phosphate, lithium manganese phosphate, etc. In the case of other positive electrode active materials, the carbon source has been limited to a polymer material having electrical conductivity. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2001-15111 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a secondary battery material that can be suitably used as a material for forming batteries such as lithium ion secondary batteries and can improve the rate characteristics of the batteries. [Means for solving the problem]
[0011] As a result of extensive research to achieve the above-mentioned object, the inventors have discovered that a battery manufactured using a secondary battery material containing a luminescent carbon nanostructure (carbon quantum dot) synthesized using a nitrogen source consisting of specific amines as a raw material has excellent rate characteristics, and have completed the present invention.
[0012] That is, the present invention provides the following method for producing a secondary battery material. 1. A method for producing a secondary battery material comprising a carbon nanostructure, an active material, conductive carbon, and a binder, comprising: The method includes a step of synthesizing a carbon nanostructure by mixing and heating a polycarboxylic acid or a sugar, an amine (excluding cysteine), and a solvent, The method for producing a secondary battery material is characterized in that the carbon nanostructure is a carbon quantum dot that is non-conductive and contains nitrogen, the nitrogen being derived from a nitrogen source consisting of amines (excluding cysteine), and emitting light when excited with any wavelength of 300 to 800 nm. 2. A method for producing a secondary battery material according to claim 1, wherein the absolute quantum yield of the carbon nanostructure is 10% or more. 3. A method for producing a secondary battery material according to claim 2, wherein the absolute quantum yield of the carbon nanostructure is 30% or more. 4. The method for producing a secondary battery material according to any one of claims 1 to 3, wherein the nitrogen is obtained from a nitrogen source comprising an aliphatic amine as a raw material. 5. A method for producing a secondary battery material according to any one of 1 to 4, wherein the carbon contained in the carbon nanostructure is obtained by using a carbon source made of a polycarboxylic acid or a sugar as a raw material. 6. The method for producing a secondary battery material according to any one of 1 to 5, wherein the active material is selected from the group consisting of metals, semi-metals, metal alloys, metal oxides, semi-metal oxides, metal phosphates, metal sulfides and metal nitrides. 7. The above active materials are FeS2, TiS2, MoS2, LiFePO4, V2O6, V6O 13 , MnO2, LiCoO2, LiMnO2, LiMn2O4, LiMo2O4, LiV3O8, LiNiO2, Li z Ni y M 1-y O2 (wherein M represents at least one metal element selected from Co, Mn, Ti, Cr, V, Al, Sn, Pb, and Zn, and 0.05≦z≦1.10, 0.5≦y≦1.0), Li(Ni a Co b Mn c)O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), Li4Ti5O 12 Si, SiO x AlO x SnO x SbO x BiO x GeO x AsO x PbO x ZnO x CdO x InO x TiO x and GaO x The manufacturing method of the secondary battery material according to claim 6, which is at least one selected from (where 0 < x ≤ 2). 8. The manufacturing method of the secondary battery material according to any one of 1 to 7, wherein the secondary battery material is for electrode formation. 9. The manufacturing method of the secondary battery material according to any one of 1 to 8, wherein the blending amount of the carbon nanostructure is 0.01 to 1.0 mass% in the solid content. 10. The manufacturing method of the secondary battery material according to any one of 1 to 9, wherein the synthesis is performed by solvothermal synthesis. 11. The manufacturing method of the secondary battery material according to any one of 1 to 9, wherein the synthesis is performed by hydrothermal synthesis. 12. The manufacturing method of the secondary battery material according to 11, which includes a step of replacing the solvent of the carbon nanostructure aqueous solution obtained by hydrothermal synthesis with an organic solvent. 13. The manufacturing method of the secondary battery material according to any one of 1 to 12, After preparing a solution or dispersion liquid containing an active material and a carbon nanostructure, removing the solvent to produce a composite of the active material - carbon nanostructure. The manufacturing method of the secondary battery material including this step.
Effect of the Invention
[0013] By using the secondary battery material obtained by the manufacturing method of the present invention, a battery excellent in rate characteristics can be provided.
Brief Description of the Drawings
[0014] [Figure 1]FIG. 2 is a diagram showing the fluorescence spectrum of the aqueous solution A1 obtained in Example 1-1. [Diagram 2] FIG. 1 is a diagram showing the fluorescence spectrum of the aqueous solution A2 obtained in Example 1-2. [Diagram 3] FIG. 1 shows the fluorescence spectrum of the aqueous solution A3 obtained in Example 1-3. [Figure 4] FIG. 1 shows the fluorescence spectrum of the aqueous solution A4 obtained in Example 1-4. [Diagram 5] FIG. 1 is a diagram showing the fluorescence spectrum of the aqueous solution A5 obtained in Comparative Example 1-1. [Figure 6] FIG. 13 is a diagram showing the fluorescence spectrum of the aqueous solution A6 obtained in Comparative Example 1-2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The battery material of the present invention contains a carbon nanostructure, which emits light when excited with a wavelength of 300 to 800 nm. In the present invention, a battery excellent in rate characteristics and cycle characteristics can be obtained by using a carbon nanostructure having such characteristics. The emission of the carbon nanostructure can be confirmed using a known measuring device. In the present invention, for example, the emission of the carbon nanostructure can be confirmed by measuring the obtained carbon nanostructure aqueous solution with a spectrofluorometer F-7000 manufactured by Hitachi High-Tech Science Corporation, with the excitation wavelength fixed at any wavelength of 300 to 800 nm. The excitation wavelength can be determined by the maximum absorption wavelength in the absorption spectrum measurement.
[0016] A carbon nanostructure is generally a structure composed primarily of carbon atoms, with at least one of the three dimensions of the structure being in the nanometer range, for example, on the order of a few nm to a few hundred nm.
[0017] From the viewpoint of further improving the discharge capacity of the resulting battery, the absolute quantum yield of the carbon nanostructure is preferably 10% or more, more preferably 30% or more, and even more preferably 50% or more. The upper limit of the absolute quantum yield is not particularly limited, but is usually 90% or less. The absolute quantum yield can be confirmed using a known measuring device. In the present invention, for example, the absolute quantum yield can be confirmed by measuring the maximum absorption wavelength in absorption spectrum measurement as the excitation wavelength with an absolute PL quantum yield meter manufactured by Hamamatsu Photonics K.K. for the obtained carbon nanostructure aqueous solution.
[0018] Examples of carbon nanostructures include carbon quantum dots, graphene quantum dots, and carbon materials containing a fused ring structure that is a partial structure of fibrous π-conjugated polymers and graphene, which have the above-mentioned light-emitting properties. Among these, carbon quantum dots, which are carbon materials with an average particle size of 20 nm or less, are preferred. The above average particle size is a value measured by a transmission electron microscope (TEM).
[0019] In addition, the carbon nanostructure is preferably non-conductive from the viewpoint of further improving the discharge capacity of the resulting battery. In the present invention, "non-conductive" means that the electrical conductivity of the resulting powder of carbon nanostructure measured with a low resistance meter Loresta-GP manufactured by Mitsubishi Chemical Analytech Co., Ltd. is below the detection limit (resistance value is 10 7 Ω).
[0020] The carbon nanostructure preferably contains nitrogen. The nitrogen content of the carbon nanostructure is not particularly limited as long as it contains nitrogen, but in consideration of further improving the discharge capacity of the resulting battery, the nitrogen content is preferably 5 to 30 mass%, more preferably 10 to 25 mass%, and even more preferably 10 to 20 mass%.
[0021] The carbon nanostructure can be produced by known methods, for example, by using a carbon source consisting of a polycarboxylic acid or a sugar and a nitrogen source consisting of an amine as raw materials, mixing these with a solvent, and heating.
[0022] The polycarboxylic acid is not particularly limited as long as it has two or more carboxy groups. Specific examples thereof include quinic acid, galactaric acid, glyceric acid, gluconic acid, glucuronic acid, ascorbic acid, and gallic acid. Among these, citric acid, succinic acid, and oxalic acid are preferred, and citric acid is more preferred. The polycarboxylic acid may be used alone or in combination of two or more.
[0023] The sugars include monosaccharides, disaccharides and polysaccharides. These sugars may be used alone or in combination of two or more.
[0024] As the monosaccharide, those having 3 to 9 carbon atoms, particularly 5 to 6 carbon atoms are preferred. Specific examples include pentoses such as xylose; hexoses such as glucose, mannose, and galactose; deoxyhexoses such as fucose; hexosamines such as glucosamine and galactosamine; hexosamine derivatives such as N-acetylglucosamine and N-acetylgalactosamine; sialic acids such as neuraminic acid, N-acetylneuraminic acid, and N-glycolylneuraminic acid; and uronic acids such as glucuronic acid and iduronic acid. Of these, hexoses are preferred, and glucose is more preferred. The above monosaccharides may be used alone or in combination of two or more.
[0025] Examples of disaccharides include sucrose, lactulose, lactose, maltose, trehalose, cellobiose, etc. The above disaccharides may be used alone or in combination of two or more.
[0026] Examples of polysaccharides include starch, amylose, amylopectin, glycogen, cellulose, chitin, agarose, carrageenan, heparin, hyaluronic acid, pectin, xyloglucan, glucomannan, etc. Among these, those that are soluble in water are preferred from the viewpoint of synthesis. The above polysaccharides may be used alone or in combination of two or more.
[0027] The amines include aliphatic amines, aromatic amines, hydroxyamines, polyamines, heterocyclic amines, amino acids, and amino group-containing polyalkylene glycols. Among these, aliphatic amines, aromatic amines, and amino acids are preferred. The above amines may be used alone or in combination of two or more.
[0028] Examples of the aliphatic amines include methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, s-butylamine, t-butylamine, n-pentylamine, 1-methyl-n-butylamine, 2-methyl-n-butylamine, 3-methyl-n-butylamine, 1,1-dimethyl-n-propylamine, 1,2-dimethyl-n-propylamine, 2,2-dimethyl-n-propylamine, 1-ethyl-n-propylamine, n-hexylamine, 1-methyl-n-pentylamine, 2-methyl-n-pentylamine, 3-methyl-n-pentylamine, 4-methyl-n-pentyl ... monoamines such as 1-ethyl-n-butylamine, 1,2-dimethyl-n-butylamine, 1,3-dimethyl-n-butylamine, 2,2-dimethyl-n-butylamine, 2,3-dimethyl-n-butylamine, 3,3-dimethyl-n-butylamine, 1-ethyl-n-butylamine, 2-ethyl-n-butylamine, 1,1,2-trimethyl-n-propylamine, 1,2,2-trimethyl-n-propylamine, 1-ethyl-1-methyl-n-propylamine, 1-ethyl-2-methyl-n-propylamine, 2-ethylhexylamine, 2-aminoethanol, 1-amino-2-propanol, 2-amino-1-propanol, and 2-aminoethanethiol;Ethylenediamine, N,N-dimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-diethylethylenediamine, N,N'-diethylethylenediamine, N-ethylethylenediamine, diethylenetriamine, 1,2-diaminopropane, 1,3-diaminopropane, 2-(2-aminoethylamino)ethanol, N-isopropylethylenediamine, N-isopropyl-1,3-diaminopropane, triethylenetetramine, N,N'-bis(2-hydroxyethyl)ethylenediamine, 2,2-dimethyl-1,3-propanediamine, 2-methyl-2,3-propanediamine, 1,2-diamino-2-methylpropane, 3,3'-diamino-N-methyldipropylamine, 2,3-dimethyl-2,3-butanediamine, 3,3'-diaminodipropylamine, N,N-bis(2-aminoethyl)-1,3-propanediamine, triethylenetetramine Examples of diamines include tetramethylenediamine, 2,2'-oxybis(ethylamine), tetramethylenediamine, 1,4-diaminobutane, 2,2'-thiobis(ethylamine), 1,5-diaminopentane, 2-methyl-1,5-diaminopentane, 1,6-diaminoheptane, 1,7-diaminopentane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, N,N'-bis(3-aminopropyl)ethylenediamine, diethylene glycol bis(3-aminopropyl)ether, 1,14-diamino-3,6,9,12-tetraoxatetradecane, bis(aminomethyl)cyclohexane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, bis(aminomethyl)norbornane, 1,4-bis(aminomethyl)cyclohexane, and 1,2-bis(2-aminoethoxy)ethane. Among these, compounds having two or more amino groups are preferred, and diamines having two carbon atoms between the amino groups are more preferred.
[0029] Examples of aromatic amines include aralkyl monoamines such as benzylamine, p-methoxycarbonylbenzylamine, p-ethoxycarbonylphenylbenzyl, p-methylbenzylamine, m-methylbenzylamine, and o-methoxybenzylamine, aniline, p-methoxycarbonylaniline, p-ethoxycarbonylaniline, p-methoxyaniline, 1-naphthylamine, 2-naphthylamine, anthranilamine, 1-aminopyrene, 4-biphenylylamine, o-phenylaniline, and 4-amino-p-terphenylamine. aryl monoamines such as fluorene, 2-aminofluorene, etc.; 1,2-phenylenediamine, 1,3-phenylenediamine, 1,4-phenylenediamine, 3-nitro-1,2-phenylenediamine, 4-nitro-1,2-phenylenediamine, 3-methyl-1,2-phenylenediamine, 4-methyl-1,2-phenylenediamine, 1,2,4-benzenetriamine, 3,4-dimethyl-1,2-phenylenediamine, 4,5-dimethyl-1,2-phenylenediamine, 3-fluoro-1,2-phenylenediamine, 4-fluoro-1,2 -phenylenediamine, 3,4-difluoro-1,2-phenylenediamine, 3,5-difluoro-1,2-phenylenediamine, 4,5-difluoro-1,2-phenylenediamine, 3-chloro-1,2-phenylenediamine, 4-chloro-1,2-phenylenediamine, 3,4-dichloro-1,2-phenylenediamine, 3,5-dichloro-1,2-phenylenediamine, 4,5-dichloro-1,2-phenylenediamine, 3-bromo-1,2-phenylenediamine, 4-bromo-1,2-phenylenediamine, 3,4-dibu Examples of aryl diamines include aryl diamines such as bromo-1,2-phenylenediamine, 3,5-dibromo-1,2-phenylenediamine, 4,5-dibromo-1,2-phenylenediamine, 2,3-naphthalenediamine, benzidine, 3,3'-diaminobenzidine, 3,4-diaminobenzoic acid, methyl 3,4-diaminobenzoate, ethyl 3,4-diaminobenzoate, 4-(4-aminophenoxy)-1,2-benzenediamine, 3,4-diaminobenzophenone, and 5,6-diamino-1,3-dihydro-2H-benzimidazol-2-one.
[0030] Examples of heterocyclic amines include barbituric acid, aziridine, azetidine, pyrrolidine, piperidine, piperazine, azepane, pyridine, pyridazine, pyrimidine, pyrazine, imidazole, benzimidazole, pyrazole, oxazole, isoxazole, benzoxazole, thiazole, isothiazole, benzothiazole, triazine, azepine, diazepine, benzodiazepine, pyrrole, imidazoline, morpholine, thiazine, indole, isoindole, purine, quinoline, isoquinoline, quinoxaline, pteridine, acridine, carbazole, cinnoline, benzo-C-cinnoline, porphyrin, chlorine, choline, triaminotriazine, trichlorotriazine, and derivatives thereof.
[0031] Examples of amino acids include cysteine, glycine, alanine, valine, phenylalanine, threonine, lysine, asparagine, tryptophan, serine, glutamic acid, aspartic acid, ornithine, thyroxine, cystine, leucine, isoleucine, proline, tyrosine, asparagine, glutamine, histidine, methionine, and threonine. Examples of amino group-containing polyalkylene glycols include amino group-containing polyethylene glycols and amino group-containing polypropylene glycols. In addition, when the above amino acids have optical isomers, the above amino acids may be D- or L-isomers or may be racemic.
[0032] The amount of the amines used is preferably 10 to 300 parts by mass, and more preferably 20 to 150 parts by mass, per 100 parts by mass of the carbon source, from the viewpoint of nitrogen introduction efficiency.
[0033] As the raw material, organic compounds other than the above carbon sources and nitrogen sources may be used. Such organic compounds are not particularly limited as long as they do not impair the effects of the present invention.
[0034] The solvent is not particularly limited as long as it can dissolve the raw materials used. Examples of such solvents include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone (NMP), hexamethylphosphoric triamide, acetonitrile, acetone, alcohols (methanol, ethanol, 1-propanol, 2-propanol, etc.), glycols (ethylene glycol, triethylene glycol, etc.), cellosolves (ethyl cellosolve, methyl cellosolve, etc.), polyhydric alcohols (glycerin, pentaerythritol, etc.), tetrahydrofuran, toluene, ethyl acetate, butyl acetate, benzene, toluene, xylene, pentane, hexane, heptane, chlorobenzene, dichlorobenzene, trichlorobenzene, hexadecane, benzyl alcohol, and oleylamine. In the present invention, water is preferred among these. The above solvents may be used alone or in combination of two or more.
[0035] The amount of the solvent used is preferably 100 to 10,000 parts by mass, and more preferably 400 to 2,500 parts by mass, per 100 parts by mass of the raw material, in order to obtain carbon nanostructures having a uniform particle size.
[0036] When synthesizing the carbon nanostructure, an acid catalyst or a surfactant may be further included, if necessary.
[0037] The acid catalyst may be either a homogeneous acid catalyst or a heterogeneous acid catalyst, but a heterogeneous acid catalyst is preferred from the viewpoint of improving the quantum yield. Examples of homogeneous acid catalysts include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid, and organic acids such as sulfonic acid and p-toluenesulfonic acid. On the other hand, examples of heterogeneous acid catalysts include solid acid catalysts, such as cationic ion exchange resins, cationic ion exchange membranes, and solid acid catalysts described in Nature 438, p. 178 (2005). As the solid acid catalyst, commercially available products can be used, such as ion exchange resins manufactured by Rohm and Haas, such as AMBERLYST (registered trademark) 15, 16, 31, and 35, AMBERLITE (registered trademark) IR120B, IR124, 200CT, and 252, ion exchange membranes manufactured by DuPont, and inorganic solid acid catalysts such as zeolite and polyphosphoric acid. The acid catalysts may be used alone or in combination of two or more.
[0038] When a homogeneous acid catalyst is used, it is usually added at 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.5 to 1 part by mass, per 100 parts by mass of the raw material.
[0039] The heterogeneous acid catalyst is preferably a porous body having pores capable of containing the generated carbon nanostructures. The particle size or disk size of the generated carbon nanostructures can be controlled by the size of the pores. In general, it is preferable to produce carbon quantum dots with a particle size (disk size) of up to 20 nm using a solid acid catalyst of a porous body having a pore size of up to 20 nm.
[0040] When a heterogeneous acid catalyst is used, it is preferable to add about 0.1 to 100 parts by mass, more preferably 1.0 to 50 parts by mass, and even more preferably 5.0 to 10 parts by mass, per 100 parts by mass of the raw material.
[0041] The surfactant may be a cationic surfactant, an anionic surfactant, or a nonionic surfactant.
[0042] Examples of cationic surfactants include cetyltrimethylammonium bromide and cetyltrimethylammonium chloride. Examples of anionic surfactants include sodium dodecyl sulfate and sodium dodecylbenzenesulfonate. Examples of nonionic surfactants include polyethylene glycol and polypropylene glycol. These surfactants may be used alone or in combination of two or more.
[0043] The amount of the surfactant used is preferably 10 to 2,000 parts by mass, and more preferably 50 to 500 parts by mass, per 100 parts by mass of the raw materials, from the viewpoints of dispersibility of the raw materials and the critical micelle concentration under the synthesis conditions.
[0044] When synthesizing the carbon nanostructure, the components may be mixed in any order. The synthesis may be carried out in a continuous or batch manner. In the present invention, the continuous method is preferably adopted because it allows continuous and efficient mass production of carbon nanostructures having uniform particle sizes.
[0045] As the continuous type, for example, a flow type reaction device (flow reactor) can be suitably adopted. As the flow reactor, a known device can be used, for example, a flow type high temperature reaction system Phoenix Flow Reactor manufactured by Thales Nanotechnology Inc. can be mentioned. By using the flow reactor, a reaction (solvothermal synthesis, hydrothermal synthesis) can be continuously and efficiently carried out under high temperature and pressure.
[0046] The reaction temperature can be appropriately adjusted depending on conditions such as the type of solvent used in the raw material solution, and is not particularly limited, but from the viewpoint of carrying out the reaction efficiently, it is preferably about 100 to 450° C., more preferably 150 to 400° C., and even more preferably 250 to 350° C. If the reaction temperature is too high, a charcoal product insoluble in the reaction solvent may be produced. The reaction time (residence time) is preferably from 1 to 30 minutes, more preferably from 1.5 to 20 minutes, and more preferably from 2 to 16 minutes, from the viewpoints of allowing the reaction to proceed completely and suppressing the formation of carbonized products insoluble in the reaction solvent.
[0047] When a batch system is employed, heating may be performed under normal pressure (atmospheric pressure) or under pressure (solvothermal synthesis, hydrothermal synthesis).
[0048] When the reaction is carried out under normal pressure, the reaction temperature depends on the boiling point of the solvent used, but is usually preferably about 40 to 250° C., more preferably 60 to 200° C., and even more preferably 100 to 150° C. Heating is usually carried out in a water bath or oil bath, but heating with microwaves is also possible. As a result, for example, when water is used as the solvent, the product can be obtained in a shorter time than when heating in a water bath or oil bath.
[0049] When the reaction is carried out under normal pressure, the reaction time is preferably about 1 minute to 240 hours, more preferably about 10 minutes to 48 hours, and even more preferably about 12 to 30 hours.
[0050] When pressurization is performed, for example, an autoclave can be suitably used. By using an autoclave, the reaction temperature can be increased to above the boiling point at normal pressure. For example, even when water is used as a solvent, a reaction temperature of about 200°C can be easily achieved by using an autoclave for the reaction.
[0051] The reaction temperature, similar to the case of reaction under normal pressure, depends on the boiling point of the solvent used, but is usually preferably about 100 to 450° C., more preferably 150 to 400° C., and even more preferably 250 to 350° C. The reaction time is preferably about 30 seconds to 24 hours, more preferably about 1 minute to 1 hour, and even more preferably about 2 minutes to 10 minutes.
[0052] The pressure is not particularly limited as long as the desired reaction temperature can be achieved, but is preferably about 200 kPa to 20.0 MPa, and more preferably about 500 kPa to 15.0 MPa.
[0053] In addition, when using a solid acid catalyst in a batch system, it is preferable to carry out the reaction while stirring, and good results can be obtained by increasing the stirring speed within a range in which the solid catalyst is not crushed. The stirring speed is preferably about 10 to 500 rpm, and more preferably about 50 to 300 rpm.
[0054] The average particle size of the carbon nanostructures obtained by each of the above methods is preferably 20 nm or less, more preferably 15 nm or less, and even more preferably 10 nm or less. The lower limit of the particle size is not particularly limited, but is usually 1 nm or more. If the particle size is within the above range, the carbon nanostructures will not aggregate in a solvent, and no aggregates will be generated during preparation or application of an electrode-forming composition (electrode slurry, etc.). In addition, the particle size of the carbon nanostructures is sufficiently small compared to the size of the active material, so that the carbon nanostructures have excellent coating properties on the active material.
[0055] The obtained product can be purified by removing low molecular weight impurities by dialysis, ultrafiltration, etc., and then removing high molecular weight impurities by centrifugation, etc. The pore size of the dialysis membrane or ultrafiltration membrane and the centrifugal force during centrifugation may be appropriately set according to the molecular weight of the substance to be removed.
[0056] To further purify the mixture to a higher purity, column purification may be performed. In this case, the column packing material may be normal phase or reverse phase. As normal phase packing materials, silica particles, alumina particles, etc. may be used. On the other hand, as reverse phase packing materials, silica particles surface-modified with long-chain alkyl groups, etc. may be used. In addition, pressure may be applied during column purification in order to shorten the time.
[0057] When preparing a battery material using the carbon nanostructure, the carbon nanostructure may be used in the form of a solution after the reaction, or may be isolated by removing the solvent. When preparing a battery material, if a solvent different from that used in synthesizing the carbon nanostructure is used, the solvent may be replaced to obtain the desired solvent system.
[0058] The battery material of the present invention can be used for forming an undercoat layer and an active material layer of an electrode, for producing an electrolyte, etc., and can be particularly suitably used as a material for forming an active material layer of an electrode.
[0059] When the above battery material is used as a material for forming an active material layer, it is preferable to combine the above carbon nanostructure with the following active material, conductive assistant, binder, and, if necessary, solvent (dispersion medium).
[0060] In the battery material, the amount of the carbon nanostructures to be blended varies depending on the required electrical and thermal properties, the viscosity of the material, the production cost, etc., but is preferably 0.01 to 1.0 mass% of the solid content, more preferably 0.01 to 0.75 mass%, and even more preferably 0.05 to 0.5 mass%. By making the amount of the carbon nanostructures blended within the above range, a battery with excellent rate characteristics and cycle characteristics can be obtained. The solid content here means the components other than the solvent contained in the battery material of the present invention.
[0061] As the active material, various active materials that have conventionally been used in electrodes for energy storage devices such as secondary batteries can be used, and examples thereof include metals, semi-metals, metal alloys, metal oxides, semi-metal oxides, metal phosphates, metal sulfides, and metal nitrides.
[0062] Specific examples of the active material include the following. Metal active materials include Al, Sn, and Zn. Metalloid active materials include Si, Ge, and As. Examples of the metal alloy active material include Li-Al based alloys, Li-Mg based alloys, Li-Al-Ni based alloys, Na-Hg based alloys, and Na-Zn based alloys. Metal oxide active materials include AlO x , SnO x , SbO x , BiO x , PbOx , ZnO x , CdO x , InO x , TiO x and GaO x (where 0 < x ≤ 2), V2O6, V6O 13 , MnO2, LiCoO2, LiMnO2, LiMn2O4, LiMo2O4, LiV3O8, LiNiO2, Li z Ni y M 1-y O2 (where M represents at least one metal element selected from Co, Mn, Ti, Cr, V, Al, Sn, Pb, and Zn, 0.05 ≤ z ≤ 1.10, 0.5 ≤ y ≤ 1.0), ternary active material (Li(Ni a Co b Mn c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1)), tin silicate (SnSiO3), lithium bismuth oxide (Li3BiO4), lithium zinc oxide (Li2ZnO2), and lithium titanium oxide (Li4Ti5O 12 ) etc. can be mentioned. As the active material of the half - metal oxide, SiO x , GeO x and AsO x (where 0 < x ≤ 2) etc. can be mentioned. As the active material of the metal phosphate, LiFePO4 etc. can be mentioned. As the active material of the metal sulfide, FeS2, TiS2, MoS2, Li2S, iron sulfide lithium (Li x FeS2 (where 0 < x ≤ 3)) and copper sulfide lithium (Li x CuS (where 0 < x ≤ 3)) etc. can be mentioned. As the active material of the metal nitride, Li x M y N (where M = Co, Ni, Cu, 0 ≤ x ≤ 3, 0 ≤ y ≤ 0.5, and x and y do not become 0 simultaneously) and lithium iron nitride (Li3FeN4) etc. can be mentioned.
[0063] In the present invention, among these, FeS2, TiS2, MoS2, LiFePO4, V2O6, V6O13 , MnO2, LiCoO2, LiMnO2, LiMn2O4, LiMo2O4, LiV3O8, LiNiO2, Li z Ni y M 1-y O2 (where M represents at least one metal element selected from Co, Mn, Ti, Cr, V, Al, Sn, Pb, and Zn, 0.05 ≦ z ≦ 1.10, 0.5 ≦ y ≦ 1.0), Li(Ni a Co b Mn c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), Li4Ti5O 12 , Si, SiO x , AlO x , SnO x , SbO x , BiO x , GeO x , AsO x , PbO x , ZnO x , CdO x , InO x , TiO x and GaO x (where 0 < x ≦ 2) is preferred, and TiO x (where 0 < x ≦ 2) is more preferred.
[0064] Furthermore, for Li(Ni a Co b Mn c )O2, those satisfying 1 / 3 ≦ a < 1, 0 < b ≦ 1 / 3, 0 < c ≦ 1 / 3, a + b + c = 1 are even more preferred. Note that for the above Li(Ni a Co b Mn c)O2 can also be obtained as a commercially available product, and examples of such commercially available products include NCM111 (manufactured by Beijing Easping Material Technology, manufactured by Toshima Manufacturing Co., Ltd., a=1 / 3, b=1 / 3, c=1 / 3), NCM523 (manufactured by Beijing Easping Material Technology, manufactured by JIANGSU Easping Material Technology, a=0.5, b=0.2, c=0.3), NCM622 (manufactured by Beijing Easping Material Technology, a=0.6, b=0.2, c=0.2), and NCM811 (manufactured by Beijing Easping Material Technology, a=0.8, b=0.1, c=0.1).
[0065] The amount of active material to be used will vary depending on the required electrical and thermal properties, the viscosity of the composition, production costs, etc., but is preferably 80 to 99.8 mass % of the solid content, more preferably 85 to 98.5 mass %, and even more preferably 90 to 98 mass %.
[0066] Examples of the conductive assistant include carbon materials such as graphite, carbon black, acetylene black, vapor-grown carbon fiber, carbon nanotube, carbon nanohorn, and graphene, and conductive polymers such as polyaniline, polypyrrole, polythiophene, polyacetylene, and polyacene. The conductive assistants may be used alone or in combination of two or more.
[0067] The amount of the conductive assistant is not particularly limited, but is preferably 0.05 to 9 mass % of the solid content, more preferably 0.1 to 6 mass %, and even more preferably 0.2 to 3 mass %. By setting the amount of the conductive assistant within the above range, good electrical conductivity can be obtained.
[0068] The binder can be appropriately selected from known materials and is not particularly limited, but examples of binders that can be used in the present invention include polyvinylidene fluoride (PVdF), polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, polyvinyl alcohol, polyimide, ethylene-propylene-diene terpolymer, styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, polyaniline, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, and polypropylene. These can be used alone or in combination of two or more.
[0069] The amount of the binder is not particularly limited, but is preferably 0.14 to 10 mass % of the solid content, more preferably 0.5 to 7 mass %, and even more preferably 1 to 5 mass %. By setting the amount of the binder within the above range, good adhesion to the current collecting substrate can be obtained without decreasing the capacity.
[0070] If necessary, the binder may be dissolved in a suitable solvent, which will be described later, before mixing.
[0071] The solvent is not particularly limited as long as it can disperse or dissolve the raw material used. Examples of such solvents include those exemplified in the description of the carbon nanostructure, but more preferred examples include water, NMP, dimethyl sulfoxide, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, γ-butyrolactone, tetrahydrofuran, dioxolane, sulfolane, dimethylformamide, and dimethylacetamide. These solvents may be appropriately selected depending on the raw material used, but NMP is preferred when using a water-insoluble binder such as PVdF. The above solvents may be used alone or in combination of two or more.
[0072] When preparing the battery material for forming the active material, the preparation method is not particularly limited, and the respective components may be mixed in any order to prepare the battery material. In addition, when the solvent used in the synthesis of the carbon nanostructure is the same as the solvents exemplified above or is a solvent miscible with them, the obtained reaction solution may be used as is. On the other hand, when the solvent used in the synthesis of the carbon nanostructure is a solvent that is not miscible with the solvents exemplified above, it is preferable to use the reaction solution obtained by removing the solvent and isolating it, or to use the reaction solution obtained by solvent replacement with an appropriate solvent. In particular, when water is used as the solvent in the synthesis of the carbon nanostructure, it is preferable to replace the solvent with the organic solvent.
[0073] Furthermore, in the present invention, a composite of the active material and the carbon nanostructure can be produced by preparing a solution or dispersion containing the active material and the carbon nanostructure before mixing the above components, and then removing the solvent. By using this composite as the battery material of the present invention, a battery with excellent rate characteristics and cycle characteristics can be obtained.
[0074] The electrode of the present invention has an active material layer (thin film) made of the battery material described above on a substrate that is a current collector, or the battery material alone is formed into a thin film. When the active material layer is formed on a substrate, the active material layer can be formed by pressing a composition for forming an electrode prepared without using a solvent onto a substrate (dry method), or by preparing a composition for forming an electrode using a solvent, applying it to a current collector, and drying it (wet method). These methods are not particularly limited, and various conventionally known methods can be used. For example, wet methods include various printing methods such as offset printing and screen printing, doctor blade method, dip coating method, spin coating method, bar coating method, slit coating method, inkjet method, etc.
[0075] Examples of substrates used for the electrodes include metal substrates such as platinum, gold, iron, stainless steel, copper, aluminum, and lithium; alloy substrates made of any combination of these metals; oxide substrates such as indium tin oxide (ITO), indium zinc oxide (IZO), and antimony tin oxide (ATO); and carbon substrates such as glassy carbon, pyrolytic graphite, and carbon felt.
[0076] When the battery material is formed into a thin film by itself, a thin film may be formed on a substrate from which the thin film can be peeled off after formation by appropriately using the above-mentioned wet method and dry method, and a method of spreading the battery material thinly on the substrate using a glass rod or the like may also be adopted. As the substrate, a substrate that does not have adhesion to the thin film, such as a glass plate, may be used, and even if the substrate has adhesion to the thin film, it may be used as long as the surface of the substrate is treated to enable peeling of the thin film (such as attaching a release paper or forming a release layer).
[0077] The thickness of the active material layer (thin film) is not particularly limited, but is preferably about 0.01 to 1,000 μm, more preferably about 1 to 100 μm. When the thin film is used alone as an electrode, the thickness is preferably 10 μm or more.
[0078] In order to further suppress the elution of the active material contained in the electrode, the active material layer (thin film) may further contain a polyalkylene oxide and an ion-conductive salt, or the electrode may be covered with a protective film. The protective film preferably contains a polyalkylene oxide and an ion-conductive salt. The polyalkylene oxide is not particularly limited, but polyethylene oxide, polypropylene oxide, and the like are preferred. The number average molecular weight of the polyalkylene oxide is preferably 300,000 to 900,000, and more preferably 500,000 to 700,000. The number average molecular weight is a value measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent.
[0079] Examples of the ion conductive salt include lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), lithium trifluoromethanesulfonate (LiCF3SO3), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), etc. The ion conductive salt is preferably contained in an amount of 5 to 50 parts by mass relative to 100 parts by mass of the polyalkylene oxide.
[0080] The protective film can be formed, for example, by applying a composition containing a polyalkylene oxide, an ion-conductive salt, and a solvent onto the substrate on which the active material layer (thin film) is formed, by a method such as dipping, and drying the composition at 40 to 60°C for 30 to 120 minutes. The solvent is preferably acetonitrile, dichloromethane, or the like. The thickness of the protective film is not particularly limited, but is preferably about 10 to 1,000 μm, and more preferably about 50 to 500 μm.
[0081] The secondary battery of the present invention is provided with the above-mentioned electrodes, and more specifically, is provided with at least a pair of positive and negative electrodes, a separator interposed between the electrodes, and an electrolyte, and at least one of the positive and negative electrodes is provided with the above-mentioned electrode. Other components of the battery element may be appropriately selected from conventionally known components.
[0082] Examples of materials used for the separator include porous polyolefin, polyamide, and polyester.
[0083] As the electrolyte, from the viewpoint of easily achieving practically sufficient performance, an electrolytic solution composed of an electrolyte salt, which is the main body of ion conduction, a solvent, etc. can be suitably used.
[0084] Examples of the electrolyte salt include lithium salts such as LiPF6, LiBF4, LiN(C2F5SO2)2, LiAsF6, LiSbF6, LiAlF4, LiGaF4, LiInF4, LiClO4, LiN(CF3SO2)2, LiCF3SO3, LiSiF6, LiN(CF3SO2)(C4F9SO2), metal iodides such as LiI, NaI, KI, CsI, and CaI2, iodide salts of quaternary imidazolium compounds, iodide salts and perchlorates of tetraalkylammonium compounds, metal bromides such as LiBr, NaBr, KBr, CsBr, and CaBr2, etc. These electrolyte salts can be used alone or in combination of two or more kinds.
[0085] The above-mentioned solvent is not particularly limited as long as it does not cause corrosion or decomposition of the materials constituting the battery to deteriorate the performance and dissolves the above-mentioned electrolyte salt. For example, as a non-aqueous solvent, cyclic esters such as ethylene carbonate, propylene carbonate, butylene carbonate, and γ-butyrolactone, ethers such as tetrahydrofuran and dimethoxyethane, and chain esters such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate are used. These solvents can be used alone or in combination of two or more.
[0086] The electrode may be pressed as necessary. In this case, the pressing pressure is preferably 1 kN / cm or more. A commonly used pressing method can be used, but a mold pressing method or a roll pressing method is particularly preferred. The pressing pressure is not particularly limited, but is preferably 2 kN / cm or more, and more preferably 3 kN / cm or more. The upper limit of the pressing pressure is preferably about 40 kN / cm, and more preferably about 30 kN / cm.
[0087] A battery produced using the battery material of the present invention has superior rate characteristics and cycle characteristics compared to general secondary batteries.
[0088] The type of the secondary battery and the type of electrolyte are not particularly limited, and any type of battery such as a lithium ion battery, a nickel hydrogen battery, a manganese battery, or an air battery may be used, but a lithium ion battery is preferred. The lamination method and the production method are also not particularly limited.
[0089] The shape of the cell is not particularly limited, and various types of cells known in the art, such as a cylindrical type, a flat wound rectangular type, a laminated rectangular type, a coin type, a flat wound laminate type, and a laminated type, can be used. When applied to a coin-shaped cell, the electrode of the present invention described above may be punched out into a predetermined disk shape for use. For example, a lithium ion secondary battery can be produced by placing one electrode on a lid of a coin cell to which a washer and spacer are welded, placing a separator of the same shape impregnated with an electrolyte on top of that, and then placing the electrode of the present invention on top with the active material layer facing down, placing a case and a gasket on top, and sealing with a coin cell crimping machine. EXAMPLES
[0090] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The measuring devices used in the examples are as follows. [Flow-type reactor] Equipment: Phoenix Flow Reactor, a high-temperature flow reaction system manufactured by Thales Nanotechnology Inc. [Fluorescence spectrum measurement] Equipment: Hitachi High-Tech Science Co., Ltd., spectrofluorometer F-7000 [Absolute quantum yield analysis] Equipment: Hamamatsu Photonics, absolute PL quantum yield meter [Conductivity measurement] Equipment: Low resistance meter Loresta-GP, manufactured by Mitsubishi Chemical Analytech Co., Ltd. [Elemental analysis] Equipment: Perkin-Elmer fully automated elemental analyzer CHNS / O Analyzer 2400 The resulting solution was placed in an aluminum cup container and dried on a hot plate at 150°C, and the analysis was performed on the resulting powder. [Transmission Electron Microscope (TEM)] Equipment: Hitachi, Ltd., H-8000 A TEM substrate was immersed in the obtained solution and dried, and then observed at an acceleration voltage of 200 kV and a magnification of 20,000 times. The diameters of 10 particles were measured to determine the number-average particle size. [Rotation and revolution mixer] Equipment: Thinky Corporation's Awatori Rentaro ARE-310 [Roll press machine] Equipment: Pressure / heat roll press SA-602, manufactured by Takumi Giken Co., Ltd. [Coin cell crimping machine] Equipment: Manual coin crimping machine CR2032 manufactured by Hosen Co., Ltd. [Micrometer] Equipment: Mitutoyo Corporation, IR54 [Charge / discharge measuring device] Equipment: Toyo Systems Co., Ltd., TOSCAT 3100
[0091] [1] Manufacturing of carbon nanostructures (carbon quantum dots) (1) Preparation of an aqueous solution of carbon nanostructures [Example 1-1] 20.0 g (0.1 mol) of citric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as a carbon source, and 12.5 g (0.2 mol) of ethylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in 292 g of water as a nitrogen source to prepare an aqueous solution with a raw material concentration of 10 mass %. The aqueous solution was continuously synthesized using a flow-type reactor at a flow rate of 4 mL / min. (residence time of 2 minutes) and a temperature of 300°C to obtain an aqueous solution A1 of carbon nanostructures. Elemental analysis revealed that the content was 38.8 mass% carbon, 7.1 mass% hydrogen, and 17.0 mass% nitrogen, and the particle size was 5 nm. Water was distilled off from the obtained aqueous solution A1 under reduced pressure to obtain a brown solid D1. The solid D1 was placed in a high resistance probe unit for powders, and the electrical conductivity was measured by applying a pressure of 20 kN using a low resistance meter Loresta GP, which was below the detection limit.
[0092] [Example 1-2] An aqueous solution A2 was prepared in the same manner as in Example 1-1, except that the reaction temperature was changed to 340°C. Elemental analysis revealed that the composition was 46.0% by mass of carbon, 7.9% by mass of hydrogen, and 17.6% by mass of nitrogen, and the particle size was 5 nm. In the same manner as in Example 1-1, water was distilled off under reduced pressure from the resulting aqueous solution A2 to obtain a brown solid D2, which was then measured for electrical conductivity, which was below the detection limit.
[0093] [Examples 1-3] An aqueous solution A3 was prepared in the same manner as in Example 1-1, except that the raw material ethylenediamine was changed to N-ethylethylenediamine. Elemental analysis revealed that the composition was 57.5% by mass of carbon, 7.6% by mass of hydrogen, and 16.7% by mass of nitrogen, and the particle size was 14 nm. In the same manner as in Example 1-1, water was distilled off under reduced pressure from the resulting aqueous solution A3 to obtain a brown solid D3, which was measured for electrical conductivity, which was below the detection limit.
[0094] [Examples 1-4] An aqueous solution A4 was prepared in the same manner as in Example 1-1, except that the raw material ethylenediamine was changed to 2-(2-aminoethylamino)ethanol. Elemental analysis revealed that the composition was 53.3% by mass of carbon, 7.0% by mass of hydrogen, and 16.0% by mass of nitrogen, and the particle size was 7 nm. In the same manner as in Example 1-1, water was distilled off under reduced pressure from the resulting aqueous solution A4 to obtain a brown solid D4, which was measured for electrical conductivity, which was below the detection limit.
[0095] [Comparative Example 1-1] An aqueous solution A5 was prepared in the same manner as in Example 1-1, except that the raw material was changed to only citric acid. Elemental analysis revealed that the carbon content was 44.5 mass%, hydrogen content was 4.5 mass%, and nitrogen content was 0.0 mass%, and the particle size was 10 nm. In the same manner as in Example 1-1, water was distilled off under reduced pressure from the resulting aqueous solution A5 to obtain a brown solid D5, which was measured for electrical conductivity, which was below the detection limit. In the same manner as in Example 1-1, water was distilled off under reduced pressure from the resulting aqueous solution A3 to obtain a brown solid D3, which was measured for electrical conductivity, which was below the detection limit.
[0096] [Comparative Example 1-2] An aqueous solution A6 was prepared in the same manner as in Example 1-1, except that the raw material was changed to glucose alone and the reaction temperature was changed to 250°C. Elemental analysis revealed that the carbon content was 41.9 mass%, hydrogen content was 6.6 mass%, and nitrogen content was 0.0 mass%, and the particle size was 200 nm. In the same manner as in Example 1-1, water was distilled off under reduced pressure from the resulting aqueous solution A6 to obtain a brown solid D6, which had a conductivity measured to find that it was below the detection limit.
[0097] (2) Measurement of fluorescence spectrum and quantum yield Aqueous solutions A1 to A6 obtained in Examples 1-1 to 1-4 and Comparative Examples 1-1 to 1-2 were each diluted 1,000 times with water, and the fluorescence spectrum and absolute quantum yield were measured. During the measurement, the excitation wavelength was fixed at 360 nm. The results are shown in Table 1. The fluorescence spectra obtained by the measurement are shown in Figures 1 to 6.
[0098] [Table 1] *The maximum fluorescence wavelengths in the table are values automatically detected by the measuring device.
[0099] The carbon nanostructures (carbon quantum dots) synthesized in Examples 1-1 to 1-4 had a maximum fluorescence wavelength in the vicinity of 440 nm, and the quantum yield was also higher than that of the comparative examples.
[0100] (3) Solvent replacement [Example 2-1] An appropriate amount of NMP was added to the aqueous solution A1 obtained in Example 1-1, and water was removed by distillation under reduced pressure using a rotary evaporator. The obtained solution was passed through a 1.0 μm filter to remove aggregates, thereby obtaining an NMP solution B1. The solid content was measured as the dry residue after drying at 150° C. for 2 hours, and was 6.9% by mass.
[0101] [Example 2-2] An NMP solution B2 was obtained in the same manner as in Example 2-1, except that the aqueous solution A2 obtained in Example 1-2 was used instead of the aqueous solution A1. The solid content was 6.2% by mass.
[0102] [Example 2-3] An NMP solution B3 was obtained in the same manner as in Example 2-1, except that the aqueous solution A3 obtained in Example 1-3 was used instead of the aqueous solution A1. The solid content was 6.2% by mass.
[0103] [Example 2-4] An NMP solution B4 was obtained in the same manner as in Example 2-1, except that the aqueous solution A4 obtained in Example 1-4 was used instead of the aqueous solution A1. The solid content was 6.2% by mass.
[0104] [Comparative Example 2-1] An NMP solution B5 was obtained in the same manner as in Example 2-1, except that the aqueous solution A5 obtained in Comparative Example 1-1 was used instead of the aqueous solution A1. The solid content was 5.4% by mass.
[0105] [Comparative Example 2-2] An NMP solution B6 was obtained in the same manner as in Example 2-1, except that the aqueous solution A6 obtained in Comparative Example 1-2 was used instead of the aqueous solution A1. The solid content was 12.6% by mass.
[0106] [2] Manufacturing and evaluation of lithium-ion batteries (1) Electrode manufacturing [Example 3-1] Ternary cathode active material Li(Ni 0.5 Co 0.2 Mn0.3 2.781 g of 1,2-dimethylformamide (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive additive, 0.042 g of solution B1 prepared in Example 2-1, and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.9:1.8:0.1:2.2), and 0.859 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a planetary centrifugal mixer (2,000 rpm, 10 minutes, 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by the doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C1 (film thickness 40 μm).
[0107] [Example 3-2] Ternary positive electrode active material Li(Ni 0.5 Co 0.2 Mn 0.3 2.770 g of 1,2-dichlorophenyl ether (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive assistant, 0.210 g of solution B1 prepared in Example 2-1, and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.5:1.8:0.5:2.2), and 0.692 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a rotation-revolution mixer (2,000 rpm, 10 minutes, 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by a doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C2 (film thickness 40 μm).
[0108] [Example 3-3] Ternary positive electrode active material Li(Ni 0.5 Co 0.2 Mn 0.3 2.770 g of acetylene black (NCM523-5Y, manufactured by Beijing Easping Material Technology Co., Ltd.) as a conductive assistant (0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive assistant, 0.233 g of solution B2 prepared in Example 2-2, and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.5:1.8:0.5:2.2), and 0.669 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a rotation-revolution mixer (2,000 rpm, 10 minutes 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by a doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C3 (film thickness 37 μm).
[0109] [Example 3-4] Ternary positive electrode active material Li(Ni 0.5 Co 0.2 Mn 0.32.770 g of acetylene oxide (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive assistant, 0.065 g of solution B3 prepared in Example 2-3, and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.5:1.8:0.5:2.2), and 0.826 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a rotation-revolution mixer (2,000 rpm, 10 minutes, 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by the doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C4 (film thickness 42 μm).
[0110] [Examples 3-5] Ternary positive electrode active material Li(Ni 0.5 Co 0.2 Mn 0.3 2.770 g of 1,2-dimethylformamide (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive assistant, 0.054 g of solution B4 prepared in Example 2-4, and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.5:1.8:0.5:2.2), and 0.837 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a rotation-revolution mixer (2,000 rpm, 10 minutes, 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by a doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C5 (film thickness 42 μm).
[0111] [Comparative Example 3-1] Ternary cathode active material Li(Ni 0.5 Co 0.2 Mn 0.3 2.784g of O2 (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive assistant, and 1.28g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 96:1.8:2.2), and 0.888g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a rotation-revolution mixer (2,000 rpm, 10 minutes 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by the doctor blade method (wet film thickness 100 μm), and then dried at 80 ° C for 30 minutes and then at 120 ° C for 30 minutes to form an active material layer. This was pressed with a roll press to produce electrode C6 (film thickness 40 μm).
[0112] [Comparative Example 3-2] Ternary cathode active material Li(Ni 0.5 Co 0.2 Mn 0.32.770 g of 1,2-dimethylformamide (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive additive, 0.271 g of solution B3 prepared in Comparative Example 2-1, and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.5:1.8:0.5:2.2), and 0.635 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a planetary centrifugal mixer (2,000 rpm, 10 minutes, 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by a doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C7 (film thickness 40 μm).
[0113] [Comparative Example 3-3] Ternary positive electrode active material Li(Ni 0.5 Co 0.2 Mn 0.3 2.770 g of 02 (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive assistant, 0.115 g of solution B4 prepared in Comparative Example 2-2, and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.5:1.8:0.5:2.2), and 0.787 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a rotation-revolution mixer (2,000 rpm, 10 minutes, 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by a doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C8 (film thickness 41 μm).
[0114] [Comparative Example 3-4] Ternary cathode active material Li(Ni 0.5 Co 0.2 Mn 0.3 2.770 g of 1,2-dichloroethane (NCM523-5Y, manufactured by Beijing Easping Material Technology), 0.052 g of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive assistant, 0.290 g of an NMP solution (solid content concentration 5% by mass) of polyvinylpyrrolidone (manufactured by Tokyo Chemical Industry Co., Ltd., K15, molecular weight 10,000), and 1.28 g of an NMP solution (solid content concentration 5% by mass) of PVdF (manufactured by Kureha Corporation, #7300) as a binder were mixed (solid content mass ratio 95.5:1.8:0.5:2.2), and 0.612 g of NMP was further mixed so that the total solid content concentration became 58% by mass. This was mixed in a rotation-revolution mixer (2,000 rpm, 10 minutes, 3 times) to prepare a slurry for forming an electrode. This was uniformly spread on an aluminum foil (1085, manufactured by UACJ Corporation, substrate thickness 15 μm) by the doctor blade method (wet film thickness 100 μm), and then dried at 80° C. for 30 minutes and then at 120° C. for 30 minutes to form an active material layer. This was pressed with a roll press machine to produce electrode C9 (film thickness 44 μm).
[0115] (2) Manufacture of lithium-ion batteries [Example 4-1] The electrode C1 produced in Example 3-1 was punched out into a disk shape with a diameter of 10 mm, and the mass was measured. The disk was then vacuum-dried at 120° C. for 12 hours and transferred to a glove box filled with argon. Six sheets of lithium foil (Honjo Chemical Co., Ltd., thickness 0.17 mm) punched to a diameter of 14 mm were placed on the lid of a 2032-type coin cell (Hosen Co., Ltd.) to which a washer and spacer were welded, and a separator (Celgard Co., Ltd., 2400) punched to a diameter of 16 mm and soaked in electrolyte (Kishida Chemical Co., Ltd., ethylene carbonate: diethyl carbonate = 1: 1 (volume ratio), containing 1 mol / L of lithium hexafluorophosphate (LiPF6) as an electrolyte) for 24 hours or more was placed on top of the six sheets. Electrode C1 was then placed on top of the separator with the active material applied side down. After dropping one drop of electrolyte, a case and a gasket were placed on top and the coin cell was sealed with a crimping machine. It was then left to stand for 24 hours to prepare a secondary battery for testing.
[0116] [Examples 4-2 to 4-5] Test secondary batteries were produced in the same manner as in Example 4-1, except that electrodes C2 to C5 produced in Examples 3-2 to 3-5, respectively, were used instead of electrode C1.
[0117] [Comparative Examples 4-1 to 4-4] Test secondary batteries were produced in the same manner as in Example 4-1, except that electrodes C6 to C9 produced in Comparative Examples 3-1 to 3-4, respectively, were used instead of electrode C1.
[0118] The lithium ion secondary batteries produced in Examples 4-1 to 4-5 and Comparative Examples 4-1 to 4-4 were evaluated for the physical properties of the electrodes using a charge / discharge measuring device under the following conditions. Table 2 shows the ratio of the discharge capacity of each secondary battery at discharge rates of 0.2 C and 10 C to the discharge capacity of Comparative Example 4-1. [Measurement conditions] Rate characteristics: Current: 0.2C constant current charge, 0.2C, 0.5C, 3C, 5C, 10C constant current discharge (Li(Ni 0.5 Co 0.2 Mn 0.3 ) The capacity of O2 was set to 160mAh / g, and the discharge rate was increased every two cycles, and finally the discharge rate was set to 0.5C. Cut-off voltage: 4.20V-3.00V ·Temperature: Room temperature
[0119] [Table 2] *In the table, CA stands for citric acid, EDA stands for ethylenediamine, EEDA stands for N-ethylethylenediamine, AEAE stands for 2-(2-aminoethylamino)ethanol, and AB stands for acetylene black.
[0120] The lithium ion secondary batteries produced in Examples 4-1, 4-4, 4-5 and Comparative Example 4-1 were evaluated for the physical properties of the electrodes using a charge / discharge measuring device under the following conditions. Table 2 shows the charge capacity of each secondary battery at charge rates of 0.2C and 10C, as a ratio based on the charge capacity of Comparative Example 4-1. [Measurement conditions] Rate characteristics: Current: 0.2C, 0.5C, 3C, 5C, 10C constant current charging, 0.2C constant current discharging (Li(Ni 0.5 Co 0.2 Mn 0.3 ) The capacity of O2 was set to 160mAh / g, and the charging rate was increased every two cycles, and finally the charging rate was set to 0.5C. Cut-off voltage: 4.20V-3.00V ·Temperature: Room temperature
[0121] [Table 3] *In the table, CA stands for citric acid, EDA stands for ethylenediamine, EEDA stands for N-ethylethylenediamine, and AEAE stands for 2-(2-aminoethylamino)ethanol.
[0122] From the results in Tables 1 and 2, it was confirmed that a battery with excellent rate characteristics can be obtained by using the battery material containing the carbon nanostructure defined in the present invention. It was also confirmed that the effect is observed in both charging (input) and discharging (output).
Claims
1. A method for producing a secondary battery material comprising a carbon nanostructure, an active material, conductive carbon, and a binder, the method comprising the steps of: The method includes a step of synthesizing a carbon nanostructure by mixing a polyvalent carboxylic acid or a sugar, an amine (excluding cysteine), and a solvent and heating the mixture, The method for producing a secondary battery material is characterized in that the carbon nanostructure is a carbon quantum dot that is non-conductive and contains nitrogen, the nitrogen being derived from a nitrogen source consisting of amines (excluding cysteine), and emitting light when excited with any wavelength from 300 to 800 nm.
2. 2. The method for producing a secondary battery material according to claim 1, wherein the carbon nanostructure has an absolute quantum yield of 10% or more.
3. The method for producing a secondary battery material according to claim 2, wherein the carbon nanostructure has an absolute quantum yield of 30% or more.
4. 4. The method for producing a secondary battery material according to claim 1, wherein the nitrogen is obtained from a nitrogen source comprising an aliphatic amine.
5. The method for producing a secondary battery material according to any one of claims 1 to 4, wherein the carbon contained in the carbon nanostructure is obtained from a carbon source comprising a polycarboxylic acid or a sugar.
6. The method for producing a secondary battery material according to any one of claims 1 to 5, wherein the active material is selected from the group consisting of metals, semi-metals, metal alloys, metal oxides, semi-metal oxides, metal phosphates, metal sulfides and metal nitrides.
7. The active material is FeS 2 , TiS 2 , MoS 2 , LiFePO 4 , V 2 O 6 , V 6 O 13 , MnO 2 , LiCoO 2 , LiMnO 2 , LiMn 2 O 4 , LiMo 2 O 4 , LiV 3 O 8 , LiNiO 2 , Li z Ni y M 1-y O 2 (wherein M represents at least one metal element selected from Co, Mn, Ti, Cr, V, Al, Sn, Pb, and Zn, and 0.05≦z≦1.10, 0.5≦y≦1.0), Li (Ni a Co b Mn c ) O 2 (where 0<a<1, 0<b<1, 0<c<1, a+b+c=1), Li 4 Ti 5 O 12 , Si, SiO x , AlO x , SnO x , SbO x , BiO x , GeO x , AsO x , PbO x , ZnO x , CdO x , InO x , TiO x and GaO x 7. The method for producing a secondary battery material according to claim 6, wherein x is at least one selected from the group consisting of (where 0<x≦2).
8. The method for producing a secondary battery material according to any one of claims 1 to 7, wherein the secondary battery material is for forming an electrode.
9. The method for producing a secondary battery material according to any one of claims 1 to 8, wherein the amount of the carbon nanostructure is 0.01 to 1.0 mass % of the solid content.
10. The method for producing a secondary battery material according to any one of claims 1 to 9, wherein the synthesis is carried out by solvothermal synthesis.
11. The method for producing a secondary battery material according to any one of claims 1 to 9, wherein the synthesis is carried out by hydrothermal synthesis.
12. The method for producing a secondary battery material according to claim 11, further comprising a step of replacing the solvent in the aqueous carbon nanostructure solution obtained by hydrothermal synthesis with an organic solvent.
13. A method for producing the secondary battery material according to any one of claims 1 to 12, comprising the steps of: A method for producing a secondary battery material, comprising the steps of preparing a solution or dispersion containing an active material and a carbon nanostructure, and then removing the solvent to produce a composite of the active material and the carbon nanostructure.
Citation Information
Patent Citations
Carbon quantum dot and cobaltosic oxide composite electrode material and preparation method thereof
CN107195465A
Method for preparing high-quality nitrogen-doped graphene quantum dots
CN108529601A
Production method of luminescent nanocarbon
JP2017043539A
carbazole polymer
JP5983631B2
New high surface conductivity electrode material
JP2001015111A