Polysiloxane particle fluid dispersion and method for producing the same

A method for producing polysiloxane particles with controlled size and high concentration addresses the challenge of efficiently creating small-sized polysiloxane particles, enhancing the productivity and reliability of conductive particles for electronic devices.

JP2024161215AActive Publication Date: 2024-11-15NIPPON SHOKUBAI CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024152258
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-15
Estimated Expiration
2040-06-08

AI Technical Summary

Technical Problem

Existing methods struggle to efficiently produce small-sized polysiloxane particles with a narrow particle size distribution for use in conductive fine particles, which are crucial for connecting smaller electrodes and wiring in electronic devices.

Method used

A polysiloxane particle dispersion is produced with a high concentration of polysiloxane particles having a number average diameter of 0.5 μm to 2.0 μm and a coefficient of variation of 7.2% or less, achieved through a method involving the hydrolysis and condensation of a silane coupling agent in the presence of an acid, followed by addition of a base, and subsequent polymerization with a monomer to form resin particles.

Benefits of technology

The method enables the production of polysiloxane particles with precise size control, leading to improved productivity and connection reliability in electronic devices by forming conductive particles with stable electrical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161215000001
    Figure 2024161215000001
  • Figure 2024161215000002
    Figure 2024161215000002
  • Figure 2024161215000003
    Figure 2024161215000003
Patent Text Reader

Abstract

To provide a polysiloxane particle fluid dispersion that contains a high concentration of polysiloxane particles having a small particle size, and to provide a method for producing the same.SOLUTION: The present invention is a polysiloxane particle fluid dispersion, which is a fluid dispersion of a polysiloxane particle having a radically polymerizable group and in which, characterized, the solid content is 4.8 mass% or more, the number average particle size of the polysiloxane particles is 0.5 μm or more and 2.0 μm or less, and the number-based coefficient of variation of the particle sizes of the polysiloxane particles is 7.2% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polysiloxane particle dispersion and a method for producing the same. [Background technology]

[0002] In recent years, electronic devices have become smaller and more functional. Accordingly, electronic components mounted on electrical devices have become smaller and more densely mounted, and electrodes and wiring in electronic circuits have become finer and narrower. Conventionally, in the assembly of electronic devices, a connection method using anisotropic conductive materials has been adopted to electrically connect a large number of opposing electrodes and wiring. Anisotropic conductive materials are materials in which conductive particles are mixed with binder resins, etc., and examples of such materials include anisotropic conductive pastes (ACPs), anisotropic conductive films (ACFs), anisotropic conductive inks, and anisotropic conductive sheets. In addition, the conductive particles used in anisotropic conductive materials are metal particles or resin particles used as a base material, the surfaces of which are coated with a conductive metal layer.

[0003] As described above, with the progress of miniaturization and narrowing of electrodes and wiring of electronic circuits, conductive fine particles used in anisotropic conductive materials are also required to have smaller particle diameters and smaller coefficients of variation of particle diameters. In order to satisfy this requirement in conductive fine particles in which the surface of a base resin particle is coated with a conductive metal layer, it is important that the base particle before being coated with the conductive metal layer also has a small particle diameter and a small coefficient of variation of particle diameter.

[0004] For example, Patent Document 1 describes a method in which 3-methacryloxypropyltrimethoxysilane is subjected to hydrolysis and condensation reaction in the presence of aqueous ammonia to obtain an emulsion of polysiloxane particles, and then a monomer such as styrene is absorbed into the polysiloxane particles, followed by radical polymerization to obtain resin particles, which are used as resin particles that serve as the base material for conductive microparticles. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-146528 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, the demand for electronic devices remains high, and there is a demand for efficient production of conductive microparticles. Patent Document 1 discloses that polysiloxane particles of about 1.85 μm were obtained, but in order to improve the productivity of conductive microparticles, it is important to efficiently obtain polysiloxane particles of such a small particle size when producing resin particles that are the base material of the conductive microparticles.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a polysiloxane particle dispersion containing small-diameter polysiloxane particles at a high concentration, and a method for producing the same. [Means for solving the problem]

[0008] The present invention which achieves the above object is as follows. [1] A dispersion of polysiloxane particles having a radical polymerizable group, The solid content is 4.8% by mass or more, The polysiloxane particles have a number average particle diameter of 0.5 μm or more and 2.0 μm or less, and the number-based coefficient of variation of the particle diameters of the polysiloxane particles is 7.2% or less. [2] The radical polymerizable group is selected from the group consisting of a vinyl group, an acryloyl group, and a methacryloyl group. [3] A polysiloxane particle dispersion liquid according to [1], which is at least one selected from the group consisting of a vinyl group, an acryloyl group, and a methacryloyl group, a solvent containing water, and an acid; A dispersion liquid of polysiloxane particles having a radical polymerizable group, which is obtained by adding a base to the mixed liquid obtained in the step (1) in a step (2). [4] A method for producing a dispersion of polysiloxane particles having a radical polymerizable group, comprising the steps of: A step (1) of mixing a silane coupling agent having a radical polymerizable group, a solvent containing water, and an acid; A method for producing a dispersion of polysiloxane particles having a radical polymerizable group, comprising: a step (2) of adding a base to the mixed liquid obtained in the step (1). Effect of the Invention

[0009] According to the present invention, it is possible to provide a polysiloxane particle dispersion containing small-diameter polysiloxane particles at a high concentration, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The polysiloxane particle dispersion of the present invention is a dispersion of polysiloxane particles having a radically polymerizable group, the solid content being 4.8 mass% or more, the number average particle diameter of the polysiloxane particles being 0.5 μm or more and 2.0 μm or less, and the coefficient of variation of the particle diameter of the polysiloxane particles on a number basis being 7.2% or less.

[0011] 1. Polysiloxane particle dispersion The polysiloxane particles having a radical polymerizable group of the present invention can be obtained by hydrolysis and condensation of a silane coupling agent having a radical polymerizable group, as described later, and have a structure in which a radical polymerizable group is bonded to the silicon atom of a siloxane bond (-Si-O-).

[0012] The radically polymerizable group is preferably at least one selected from the group consisting of a vinyl group, an acryloyl group, and a methacryloyl group, and more preferably at least one selected from the group consisting of an acryloyl group and a methacryloyl group.

[0013] The number-based average particle size of the polysiloxane particles is 0.5 μm or more and 2.0 μm or less, preferably 0.7 μm or more, more preferably 0.9 μm or more, and even more preferably 1.0 μm or more, and preferably 1.8 μm or less, more preferably 1.6 μm or less, and even more preferably 1.4 μm or less.

[0014] The coefficient of variation (CV value) of the particle diameter of the polysiloxane particles based on the number of particles is 7.2% or less, preferably 6.5% or less, more preferably 6.0% or less, and even more preferably 5.5% or less. The lower limit of the coefficient of variation is not particularly limited, but may be about 1.5%. The coefficient of variation is a value expressed as a percentage of the ratio of the coefficient of variation of the particle diameter to the average particle diameter.

[0015] The average particle size and the coefficient of variation can be measured in the manner described in the Examples described later. Specifically, a polysiloxane particle dispersion is prepared so that the polysiloxane particle concentration is about 0.01 to 1%, the surfactant concentration is about 0.1 to 5%, and the proportion of water in the solvent is about 80 to 100%, and the average particle size and the coefficient of variation are measured using a Coulter counter.

[0016] In the present invention, by employing the production method described below, it is possible to obtain a liquid in which polysiloxane particles having a small average particle size of 0.5 μm or more and 2.0 μm or less are dispersed at a high concentration. By obtaining a high-concentration polysiloxane particle dispersion, when the polysiloxane particles are used to produce the resin particles described below, the yield of resin particles obtained from a reaction vessel of a given size can be increased, improving productivity. The solid content (polysiloxane particle concentration) in the dispersion is 4.8% by mass or more, preferably 5.5% by mass or more, more preferably 6.0% by mass or more, and even more preferably 7.0% by mass or more. The upper limit of the solid content is not particularly limited, but may be about 16% by mass. The solid content is a percentage value obtained by dividing the weight of the silane coupling agent described below by the total weight of the dispersion of the present invention.

[0017] The solvent in the dispersion may be the solvent in the step (1) and step (2) described later (i.e., the solvent in the reaction solution of the hydrolysis and condensation reaction of the silane coupling agent), i.e., a solvent containing water, or may be replaced with a different solvent from the solvent in the reaction solution by solvent replacement. The solvent in the dispersion is preferably at least one of water and an organic solvent, and examples of the organic solvent include alcohols such as methanol, ethanol, isopropanol, n-butanol, isobutanol, sec-butanol, t-butanol, pentanol, ethylene glycol, propylene glycol, and 1,4-butanediol; ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate; (cyclo)paraffins such as isooctane and cyclohexane; and aromatic hydrocarbons such as benzene and toluene. These may be used alone or in combination of two or more.

[0018] The solvent preferably contains water, and the proportion of water in the solvent is, for example, 50 to 95% by mass, more preferably 70 to 90% by mass.

[0019] The dispersion may also contain an acid, a base or a surfactant, which will be described later.

[0020] The polysiloxane particle dispersion liquid can be produced by a method including a step (1) of mixing a silane coupling agent having a radical polymerizable group, a solvent containing water, and an acid, and a step (2) of adding a base to the mixture obtained in the step (1). In the step (1), the silane coupling agent having a radical polymerizable group can be hydrolyzed in a solvent containing water in the presence of an acid, and in the step (2), a base can be added to the mixture obtained in the step (1), i.e., the liquid containing the hydrolyzate of the silane coupling agent, to condense the hydrolyzate of the silane coupling agent.

[0021] In the above-mentioned Patent Document 1, the hydrolysis of the silane coupling agent is carried out in the presence of ammonia water, but in the present invention, it is important to mix the silane coupling agent, the solvent containing water, and the acid, and this mixing process allows the hydrolysis of the silane coupling agent in the presence of the acid. Examples of the acid used include acetic acid, citric acid, and formic acid, and more preferably acetic acid.

[0022] The amount of the acid is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.2 parts by mass or more, relative to 100 parts by mass of the silane coupling agent, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 1 part by mass or less.

[0023] Examples of silane coupling agents having a radical polymerizable group include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropylethyldiethoxysilane, 3-acryloxypropylmethyldimethoxysilane, 3-acryloxypropylethyldimethoxysilane, 3-acryloxypropylmethyldiethoxysilane, 3-acryloxypropylethyldiethoxysilane, 3-methacryloxypropylmethyl (Meth)acryloyl group-containing bifunctional silane coupling agents such as diacetoxysilane, 3-methacryloxypropylethyldiacetoxysilane, 3-methacryloxyethoxypropylmethyldimethoxysilane, and 3-methacryloxyethoxypropylmethyldimethoxysilane; vinyl group-containing bifunctional silane coupling agents such as dimethoxymethylvinylsilane and diethoxymethylvinylsilane; Examples of the silane coupling agent include a difunctional silane coupling agent; a trifunctional silane coupling agent containing (meth)acryloyl groups, such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, and 3-acryloxypropyltriethoxysilane; and a trifunctional silane coupling agent containing vinyl groups, such as vinyltrimethoxysilane, vinyltriethoxysilane, and p-styryltrimethoxysilane. At least one of these can be used as a silane coupling agent having a radical polymerizable group. Among them, a trifunctional silane coupling agent containing (meth)acryloyl groups is preferred, and 3-methacryloxypropyltrimethoxysilane is particularly preferred. The (meth)acryloyl group means an acryloyl group or a methacryloyl group.

[0024] The amount of the silane coupling agent charged is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 7 parts by mass or more, relative to 100 parts by mass of water charged, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less.

[0025] In the step (1), it is preferable to mix a surfactant with the silane coupling agent, the solvent containing water, and the acid, and it is preferable to use a surfactant because the hydrolysis can be carried out in the presence of the surfactant together with the acid. By using a surfactant, the particle size of the polysiloxane particles finally obtained can be made smaller. As the surfactant, any of a nonionic surfactant, a cationic surfactant, and an anionic surfactant may be used, but an anionic surfactant is preferable.

[0026] Examples of the anionic surfactant include carboxylate-type anionic surfactants such as aliphatic monocarboxylates, polyoxyethylene alkyl ether carboxylates, and fatty acid oils; sulfonate-type anionic surfactants such as dialkyl sulfosuccinates, polyoxyethylene alkyl sulfosuccinates, alkanesulfonates, linear alkylbenzene sulfonates, branched alkylbenzene sulfonates, naphthalenesulfonate-formaldehyde condensates, and alkylnaphthalenesulfonates; sulfate-type anionic surfactants such as alkyl sulfates, polyoxyalkylene alkyl ether sulfates, and oil and fat sulfates; and phosphate-type anionic surfactants such as alkyl phosphates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkylaryl ether phosphates. Among these, sulfonate-type anionic surfactants and sulfate-type anionic surfactants are preferred, and sulfate-type anionic surfactants are more preferred.

[0027] Examples of the sulfate ester-type anionic surfactant include polyoxyethylene alkyl ether sulfates such as ammonium polyoxyethylene styrenated phenyl ether sulfate, sodium polyoxyalkylene branched decyl ether sulfate (preferably sodium polyoxyethylene branched decyl ether sulfate), ammonium polyoxyethylene isodecyl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, ammonium polyoxyethylene lauryl ether sulfate, ammonium polyoxyethylene oleyl cetyl ether sulfate, and sodium polyoxyethylene oleyl cetyl ether sulfate, with ammonium polyoxyethylene styrenated phenyl ether sulfate being the most preferred.

[0028] The amount of the surfactant to be added is 100 parts by mass of the silane coupling agent. It is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, and is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less.

[0029] The solvent in the step (1) may contain an organic solvent in addition to the water, acid, and surfactant described above. Examples of the organic solvent include alcohols such as methanol, ethanol, isopropanol, n-butanol, isobutanol, sec-butanol, t-butanol, pentanol, ethylene glycol, propylene glycol, and 1,4-butanediol; ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate; (cyclo)paraffins such as isooctane and cyclohexane; ethers such as dioxane and diethyl ether; and aromatic hydrocarbons such as benzene and toluene. These may be used alone or in combination of two or more. The organic solvent is preferably an alcohol.

[0030] The amount of the organic solvent charged is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 12 parts by mass or more, relative to 100 parts by mass of the water charged, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less.

[0031] In the step (1), the silane coupling agent, water, acid, and other materials used as necessary may be mixed and stirred. The order of adding the materials in the step (1) is not particularly limited, but it is preferable to prepare a liquid in which water, acid, and a surfactant and an organic solvent used as necessary are mixed, and then add the silane coupling agent to the mixed liquid and stir. The temperature during stirring is, for example, 20 to 50°C, preferably 28 to 35°C, and more preferably 30 to 33°C. The stirring time from the start of adding the silane coupling agent is, for example, 10 minutes or more, preferably 20 minutes or more, more preferably 30 minutes or more, and preferably 2 hours or less, more preferably 100 minutes or less, and even more preferably 90 minutes or less. The stirring temperature and time in the above ranges are preferable in terms of reducing the particle size of the resulting polysiloxane particles.

[0032] After the step (1), a base is added to the mixed liquid obtained in the step (1) (i.e., the liquid containing the hydrolyzate of the silane coupling agent) (step (2)). The step (2) condenses the hydrolyzate of the silane coupling agent to form polysiloxane particles having a polymerizable functional group (condensation step).

[0033] The base is preferably NaOH or KOH. The amount of the base is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, relative to 100 parts by mass of the silane coupling agent charged in the step (1).

[0034] After the base is added, stirring is preferably performed, and the stirring time may be, for example, about 5 to 30 minutes. In addition to using the surfactant in the above-mentioned step (1) (particularly adding the surfactant before adding the silane coupling agent), it is also preferable to add a surfactant during stirring in step (2). The surfactant added in step (2) can be one of those exemplified as the surfactant used in the above-mentioned step (1), and the amount is, for example, 3 to 100 times by mass, preferably 5 to 80 times by mass, relative to the amount of the surfactant used in step (1). In this way, by increasing the amount of the surfactant in step (2) relative to the amount of the surfactant in step (1), it is possible to obtain the effect of reducing the particle size and stabilizing the initial nucleation in step (1), and it is preferable to obtain the effect of stabilizing the particles precipitated in step (2). If the amount of the surfactant in step (1) is excessive, the CV value becomes large. This tends to become more common.

[0035] 2. Resin particles For the polysiloxane particles having the above-mentioned radically polymerizable group, it is preferable to employ a seed polymerization method including a step of using the polysiloxane particles as seed particles and causing the seed particles to absorb a monomer having the radically polymerizable group and a group capable of radical polymerization, and a polymerization step, in which the seed polymerization method can be used to form resin particles by combining with the monomer.

[0036] In the absorption step, the polysiloxane particles are made to absorb the monomer component. The absorption method is not particularly limited as long as it proceeds in the presence of the polysiloxane particles and the monomer component. Therefore, the monomer component may be added to a solvent in which the polysiloxane particles are dispersed, or the polysiloxane particles may be added to a solvent containing the monomer component. Among them, as in the former case, it is preferable to add the monomer component to a solvent in which the polysiloxane particles are dispersed in advance. In particular, the method of adding water as necessary and adding the monomer component to the reaction liquid (polysiloxane particle dispersion liquid) without taking out the polysiloxane particles obtained in steps (1) and (2) (i.e., hydrolysis and condensation steps) from the reaction liquid is preferable because it does not complicate the process and has excellent productivity.

[0037] In the absorption step, the timing of adding the monomer component is not particularly limited, and the monomer component may be added all at once, may be added in several portions, or may be fed at any speed. When adding the monomer component, either the monomer component alone or a solution of the monomer component may be added, but it is preferable to mix an emulsion in which the monomer component is emulsified and dispersed in water or an aqueous medium with an emulsifier with the polysiloxane particles, since the absorption into the polysiloxane particles is more efficiently performed.

[0038] Examples of the monomer components include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and propyl (meth)acrylate; cycloalkyl (meth)acrylates such as cyclopropyl (meth)acrylate and cyclopentyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as phenyl (meth)acrylate and benzyl (meth)acrylate; styrene; alkyl styrenes such as o-methylstyrene, m-methylstyrene, and p-methylstyrene; halogen group-containing styrenes such as o-chlorostyrene, m-chlorostyrene, and p-chlorostyrene; allyl (meth)acrylates such as allyl (meth)acrylate; ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, and the like. Examples of the crosslinking agent include alkanediol di(meth)acrylates such as acrylate and 1,6-hexanediol di(meth)acrylate; di(meth)acrylates such as polyalkylene glycol di(meth)acrylates such as diethylene glycol di(meth)acrylate and triethylene glycol di(meth)acrylate; tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate; tetra(meth)acrylates such as pentaerythritol tetra(meth)acrylate; hexa(meth)acrylates such as dipentaerythritol hexa(meth)acrylate; aromatic hydrocarbon-based crosslinking agents such as divinylbenzene, divinylnaphthalene, and derivatives thereof (preferably styrene-based multifunctional monomers such as divinylbenzene); and the like. Among them, alkanediol diacrylates, styrene or styrene-based multifunctional monomers (particularly, divinylbenzene) are preferred.

[0039] The amount of the monomer component charged may be 1.5 to 10 times by mass the amount of the silane coupling agent charged in the process for producing the polysiloxane particles.

[0040] The emulsifier is not particularly limited, and the surfactants exemplified in the above-mentioned production process of polysiloxane particles can be used.

[0041] In the polymerization step, the monomer component absorbed in the polysiloxane particles is polymerized, and the absorbed monomer component is polymerized with the radical polymerizable group of the polysiloxane particles, and the polysiloxane skeleton and the polymer obtained from the monomer component are composited. The polymerization method is not particularly limited, but for example, a method using a radical polymerization initiator can be mentioned. The radical polymerization initiator is not particularly limited, but for example, a peroxide initiator, an azo initiator, etc. can be used. These radical polymerization initiators may be used alone or in combination of two or more kinds.

[0042] The reaction temperature during radical polymerization is preferably 40°C or higher and 100°C or lower. If the reaction temperature is too low, the degree of polymerization does not increase sufficiently, and the mechanical properties of the composite particles tend to be insufficient. On the other hand, if the reaction temperature is too high, aggregation between particles tends to occur easily during polymerization. The reaction time during radical polymerization may be appropriately changed depending on the type of polymerization initiator used, but is usually 5 minutes or longer and 300 minutes or shorter. If the reaction time is too short, the degree of polymerization may not increase sufficiently, and if the reaction time is too long, aggregation between particles tends to occur easily.

[0043] The number-based average dispersed particle diameter of the resin particles after synthesis is, for example, 1.1 μm or more and 3.0 μm or less, and the number-based coefficient of variation of the dispersed particle diameter measured by the method of the examples described later is, for example, 2% or more and 10% or less. In addition, the compressive elastic modulus (10% K value) when the diameter of the resin particles is displaced by 10% is 2500 N / mm 2 More than 15000N / mm 2 It is preferable that the 10% K value is 2500N / mm 2 By the above, the resin particles are used as a substrate. Therefore, the 10% K value is preferably 3000 N / mm 2 More preferably, 3500N / mm 2 On the other hand, the 10% K value is 15000N / mm 2 This allows for low-voltage connection with the electrodes. The polysiloxane particles obtained by the present invention have a small particle diameter, so that when resin particles of a predetermined particle diameter are obtained, the proportion of the monomer component in the resin particles can be increased, and the 10% K value can be set to a predetermined value or less. The 10% K value is more preferably 14000 N / mm 2 or less, more preferably 13000N / mm 2 The following is the result.

[0044] The 10% K value is the compressive modulus when a load is applied toward the center of a test particle and the compressive displacement is 10% of the particle diameter. The compressive modulus can be determined by measuring the load value at 10% compressive displacement. More specifically, the 10% K value (compressive modulus at 10% compressive displacement) is determined by measuring the compressive load value using the method shown in the Examples below, and then using the following formula:

[0045]

number

[0046] In the above formula, E is the compressive elastic modulus (N / mm 2 ), F is the compression load (N), S is the compression displacement (mm), and R is the radius of the particle (mm).

[0047] 3.Conductive particles The conductive particles can be formed by forming at least one conductive metal layer on the surface of the resin particles. The metal constituting the conductive metal layer is not particularly limited, but examples thereof include gold, silver, copper, platinum, iron, lead, aluminum, chromium, palladium, nickel, rhodium, ruthenium, antimony, bismuth, germanium, tin, cobalt, indium, and nickel- Examples of the metals include phosphorus, nickel-boron, and other metals and metal compounds, as well as alloys thereof.

[0048] The thickness of the conductive metal layer is, for example, 0.01 μm or more and 0.20 μm or less. When the thickness of the conductive metal layer is within the above range, stable electrical connection can be maintained when the conductive fine particles are used as an anisotropic conductive material.

[0049] The method for forming the conductive metal layer is not particularly limited, and can be, for example, a method of plating the surface of the substrate by electroless plating, electrolytic plating, etc., a method of forming a conductive metal layer on the surface of the substrate by a physical vapor deposition method such as vacuum deposition, ion plating, ion sputtering, etc. Among these, the electroless plating method is particularly preferred because it does not require a large-scale device and can easily form a conductive metal layer.

[0050] The number-average particle diameter of the conductive particles is preferably 1.1 μm or more and 2.8 μm or less. If the number-average particle diameter is within this range, it can be suitably used for electrical connections of miniaturized and narrowed electrodes and wiring.

[0051] The conductive particles preferably have an initial resistance of 5 Ω or less, more preferably 2 Ω or less, as measured by the method described in the Examples below, and the resistance increase rate is preferably 5% or less, more preferably 2% or less. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples, and can be modified as long as it satisfies the spirit of the invention, and all such modifications are included in the technical scope of the present invention. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0053] The physical properties shown in the following Examples and Comparative Examples were measured by the following methods.

[0054] <Number average particle size and coefficient of variation (CV value) of polysiloxane particle dispersion and resin particles> In the case of polysiloxane particle dispersion, the dispersion obtained by hydrolysis and condensation reaction of silane coupling agent was diluted with 1% aqueous solution of polyoxyethylene alkyl ether sulfate ammonium salt (Dai-ichi Kogyo Seiyaku Co., Ltd.'s "Hitenol (registered trademark) N-08") to be used as a measurement sample, and in the case of resin particles, 0.1 parts of resin particles were added with 20 parts of 1% aqueous solution of polyoxyethylene alkyl ether sulfate ammonium salt (Dai-ichi Kogyo Seiyaku Co., Ltd.'s "Hitenol (registered trademark) N-08"), which is an emulsifier, and dispersed for 10 minutes by ultrasonic waves to be used as a measurement sample, and the particle diameter (μm) of 30,000 particles was measured using a particle size distribution measuring device (Beckman Coulter Co., Ltd.'s "Coulter Multisizer III") to obtain the number average particle diameter. In addition to the number average particle diameter, the standard deviation of the particle diameter based on the number was obtained, and the coefficient of variation (CV value) of the particle diameter was calculated according to the following formula. Coefficient of variation of particle size (CV value) (%) = 100 x (standard deviation of particle size based on number / number-average particle size)

[0055] <Thickness of conductive metal layer> Using a flow type particle image analyzer (Sysmex Corporation's "FPIA (registered trademark)-3000"), the number average particle diameter X (μm) of 3000 base particles (resin particles) and the number average particle diameter Y (μm) of 3000 conductive fine particles were measured. The measurements were performed after adding 17.5 parts of a 1.4% aqueous solution of polyoxyethylene oleyl ether (Kao Corporation's "Emulgen (registered trademark) 430"), which is an emulsifier, to 0.25 parts of the particles and dispersing the mixture by ultrasonic waves for 10 minutes. The film thickness of the conductive metal layer was then calculated according to the following formula. Conductive metal layer thickness (μm)=(YX) / 2

[0056] <10% K value of base particles for conductive particles> Using a micro-compression tester (Shimadzu Corporation "MCT-W500"), at room temperature (25°C), a single base particle (resin particle) was spread on a sample table (material: SKS plate) and a circular flat indenter (material: diamond) with a diameter of 50 μm was used to apply a load to the center of the base particle at a constant load speed (2.231 mN / sec) up to the maximum load (49.0 mN) in the "soft surface detection" mode, and the load value (10% compression load value) (mN) when the compression displacement became 10% of the number-average particle diameter of the base particle and the displacement amount (μm) at that time were measured. Note that the measurement was performed on 10 different base particles for each sample, and the average value was used as the measured value. The obtained compression load value (mN) was converted to compression load (N), the obtained displacement (μm) was converted to compression displacement (mm), and the radius (mm) of the base particle was calculated from the number average particle diameter (μm) of the base particle for conductive particles, and the above was used to calculate based on the following formula. The above measurement was performed in a constant temperature atmosphere of 25°C.

[0057]

number

[0058] <Productivity of Base Resin Particles> When the maximum ideal yield of base resin particles obtained from a reaction vessel with a capacity of 5 L was set to 5,000 g, the ratio of the yield of base resin particles to the maximum ideal yield was evaluated as "○○" if it was 10% or more, "○" if it was 5% or more but less than 10%, and "×" if it was less than 5%.

[0059] <Initial resistance value> The initial resistance between the electrodes of the connection structures obtained in the following Examples and Comparative Examples was measured, and an initial resistance of 2 Ω or less was evaluated as "○○", an initial resistance of 5 Ω or less was evaluated as "○", and an initial resistance of more than 5 Ω was evaluated as "×".

[0060] <Connection reliability> The initial resistance value A between the electrodes of the connection structure was measured, and the resulting connection structure was then left in an atmosphere of 85°C and 85% RH for 500 hours, after which the resistance value was measured in the same manner as the initial resistance value A and was taken as resistance value B. The resistance increase rate (%) calculated based on the following formula was evaluated as "○○" when it was 2% or less, "○" when it was more than 2% and 5% or less, and "×" when it was more than 5%. Resistance increase rate (%) = [(BA) / A] x 100

[0061] Example 1 <Preparation of Polysiloxane Particle Dispersion No. 1> In a four-neck flask equipped with a condenser, a thermometer, and a dropping nozzle, 2040 parts of ion-exchanged water, 360 parts of methanol, 1.2 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08"), and 1.2 parts of acetic acid were charged and kept at 30°C while stirring. 173 parts of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503"), which is a silane monomer (silane coupling agent), was dropped into the flask, and the internal temperature was kept at 30°C and stirred for 30 minutes to hydrolyze 3-methacryloxypropyltrimethoxysilane. As the hydrolysis proceeded, a colorless and transparent solution was obtained. Subsequently, the mixture was stirred for 50 minutes, and the mixture was heated to 30°C. A condensation reaction of the hydrolyzate of 3-methacryloxypropyltrimethoxysilane was carried out by adding 5.3 parts of a w / v% aqueous sodium hydroxide solution (manufactured by Fuji Film Wako Co., Ltd.), and 10 minutes later, 8.6 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08") was added to obtain polysiloxane particle dispersion No. 1 having a methacryloxy group. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion was 6.7%, the number average particle size was 1.01 μm, and the coefficient of variation (CV value) was 4.6%.

[0062] <Preparation of Resin Particles No. 1 Using Polysiloxane Particle Dispersion No. 1> In a 5L glass reactor, 1837 parts of polysiloxane particle dispersion (equivalent to 120 parts of 3-methacryloxypropyltrimethoxysilane) and 941 parts of ion-exchanged water were added to improve dispersion stability by adjusting the solid content, and an emulsion of polysiloxane particles was prepared. Next, a solution of 15 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier dissolved in 600 parts of ion-exchanged water was added to a solution of 600 parts of styrene and 7.2 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., "V-65") as a polymerization initiator, and the mixture was emulsified and dispersed at 13,000 rpm for 15 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare a monomer emulsion. This monomer emulsion was added to the emulsion of polysiloxane particles and further stirred. One hour after the addition of the monomer emulsion, a sample of the reaction liquid was taken and observed under a microscope, and it was confirmed that the polysiloxane particles had absorbed the monomer composition and had become enlarged. Next, 15 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier and 615 parts of ion-exchanged water were added to the reaction solution, and the reaction solution was heated to 65°C under a nitrogen atmosphere and held at 65°C for 2 hours to carry out radical polymerization. After cooling the reaction solution, the resulting emulsion was subjected to solid-liquid separation, and the resulting cake was washed with ion-exchanged water and then with methanol, and then dried under reduced pressure at 80°C for 4 hours under a nitrogen atmosphere to obtain resin particles No. 1. The yield of the obtained resin particles No. 1 was 576 parts, and the ratio of the yield of the base resin particles to the maximum ideal yield was 11.5%. The number average particle size was 2.03 μm, the coefficient of variation (CV value) was 3.6%, and the 10% K value was 5057 N / mm 2 The results are shown in Table 1-2.

[0063] <Preparation of conductive particles (formation of conductive metal layer)> The resin particles No. 1 were etched with sodium hydroxide, and then sensitized by contacting with a tin dichloride solution, and then activated by immersing in a palladium dichloride solution (sensitizing-activation method) to form palladium nuclei. Next, 2 parts of the resin particles with palladium nuclei formed were added to 400 parts of ion-exchanged water, and after ultrasonic dispersion treatment, the resulting resin particle suspension was heated in a warm bath at 70°C. In this heated suspension, 600 parts of an electroless plating solution ("Shumer S680" manufactured by Nippon Kangen Co., Ltd.) separately heated to 70°C was added to cause an electroless nickel plating reaction. After confirming that the generation of hydrogen gas had ended, solid-liquid separation was performed, and the particles were washed with ion-exchanged water and methanol in that order, and vacuum dried at 100°C for 2 hours to obtain nickel-plated particles. Next, the obtained nickel-plated particles were added to a displacement gold plating solution containing potassium gold cyanide, and gold plating was further performed on the surface of the nickel layer to obtain conductive fine particles. The thickness of the conductive metal layer in the obtained conductive fine particles is as shown in Table 1-2.

[0064] Example 2 <Preparation of Polysiloxane Particle Dispersion No. 2> In a four-neck flask equipped with a condenser, a thermometer, and a dropping nozzle, add 2040 parts of ion-exchanged water, 360 parts of methanol, and ammonium polyoxyethylene styrenated phenyl ether sulfate. 1.2 parts of a 20% aqueous solution of methyl methacrylate salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08") and 1.2 parts of acetic acid were charged and kept at 30°C with stirring. 189 parts of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503"), a silane monomer (silane coupling agent), was dropped into the flask, and the mixture was stirred for 30 minutes at an internal temperature of 30°C to hydrolyze 3-methacryloxypropyltrimethoxysilane. As the hydrolysis proceeded, a colorless, transparent solution was obtained. Subsequently, 5.3 parts of a 50 w / v% aqueous sodium hydroxide solution (manufactured by Fuji Film Wako Co., Ltd.) was added while stirring to carry out a condensation reaction of the hydrolyzate of 3-methacryloxypropyltrimethoxysilane, and 10 minutes later, 9.4 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08") was added to obtain polysiloxane particle dispersion No. 2 having a methacryloxy group. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion was 7.3%, the number average particle size was 1.00 μm, and the coefficient of variation (CV value) was 4.9%.

[0065] <Preparation of Resin Particles No. 2 Using Polysiloxane Particle Dispersion No. 2> Into a 5 L glass reactor was placed 1657 parts of the polysiloxane particle dispersion (equivalent to 120 parts of 3-methacryloxypropyltrimethoxysilane). Next, 60 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier was dissolved in 600 parts of ion-exchanged water, to which was added a solution of 300 parts of 1.6-hexanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., "Light Acrylate 1.6-HXA"), 108 parts of divinylbenzene (manufactured by Nippon Steel Chemical Co., Ltd., DVB960), 192 parts of styrene, and 7.2 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., "V-65") as a polymerization initiator, and the mixture was emulsified and dispersed at 13,000 rpm for 30 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare a monomer emulsion. This monomer emulsion was added to the emulsion of polysiloxane particles and further stirred. One hour after the addition of the monomer emulsion, a sample of the reaction liquid was taken and observed under a microscope, and it was confirmed that the polysiloxane particles had absorbed the monomer composition and had become enlarged. Next, 93 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier and 1328 parts of ion-exchanged water were added to the reaction solution, and the reaction solution was heated to 65°C under a nitrogen atmosphere and held at 65°C for 2 hours to carry out radical polymerization. After cooling the reaction solution, the resulting emulsion was separated into solid and liquid, and the resulting cake was washed with ion-exchanged water and then with methanol, and then subjected to a heat treatment at 230°C for 1 hour under a nitrogen atmosphere to obtain resin particles No. 2. The yield of the obtained resin particles No. 2 was 612 parts, and the ratio of the yield of the base resin particles to the maximum ideal yield was 12.2%. The number average particle size was 1.94 μm, the coefficient of variation (CV value) was 3.6%, and the 10% K value was 12652 N / mm 2 The results are shown in Table 1-2.

[0066] <Preparation of conductive particles (formation of conductive metal layer)> Except for using resin particle No. 2 as the base material, conductive fine particles were produced in the same manner as in Example 1. The particle size of the obtained conductive fine particles and the film thickness of the conductive metal layer were as shown in Table 1-2.

[0067] Example 3 <Preparation of Polysiloxane Particle Dispersion No. 3> In a four-neck flask equipped with a condenser, a thermometer, and a dropping nozzle, 8,500 parts of ion-exchanged water, 1,500 parts of methanol, 1.3 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08"), and 5.0 parts of acetic acid were charged and kept at 30°C with stirring. A silane monomer (silane coupling agent), 3-methacryloxypropyltrimethoxysilane, was added to the flask. 1667 parts of silane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503") was dropped, and the mixture was stirred at an internal temperature of 30°C for 30 minutes to hydrolyze 3-methacryloxypropyltrimethoxysilane. A colorless and transparent solution was obtained as the hydrolysis proceeded. Subsequently, 21.2 parts of a 50 w / v% aqueous sodium hydroxide solution (manufactured by Fuji Film Wako Co., Ltd.) was added while stirring to carry out a condensation reaction of the hydrolyzate of 3-methacryloxypropyltrimethoxysilane, and 83.4 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08") were added after 10 minutes to obtain polysiloxane particle dispersion No. 3 having a methacryloxy group. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion was 14.2%, the number average particle size was 1.74 μm, and the coefficient of variation (CV value) was 2.2%.

[0068] Comparative Example 1 <Preparation of Polysiloxane Particle Dispersion No. 4> In a four-neck flask equipped with a cooling tube, a thermometer, and a dropping nozzle, 141.1 parts of ion-exchanged water, 2.9 parts of 25% ammonia water, and 10.1 parts of methanol were charged and kept at 25°C. 26 parts of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503"), which is a crosslinkable silane monomer (silane coupling agent), and 54 parts of methanol were added thereto to carry out hydrolysis and condensation of 3-methacryloxypropyltrimethoxysilane, thereby obtaining a polysiloxane particle dispersion having a methacryloxy group (polysiloxane particle dispersion) No. 4. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion was 11.1%, the number average particle size was 4.02 μm, and the coefficient of variation (CV value) was 3.8%.

[0069] Comparative Example 2 <Preparation of Polysiloxane Particle Dispersion No. 5> In a four-neck flask equipped with a cooling tube, a thermometer, and a dropping nozzle, 141.1 parts of ion-exchanged water, 5.8 parts of 25% ammonia water, and 10.1 parts of methanol were charged and kept at 25°C. 13.2 parts of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503"), which is a crosslinkable silane monomer (silane coupling agent), and 51 parts of methanol were added thereto, and hydrolysis and condensation of 3-methacryloxypropyltrimethoxysilane was performed to obtain polysiloxane particle dispersion No. 5 having a methacryloxy group. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion was 6.0%, the number average particle size was 0.95 μm, and the coefficient of variation (CV value) was 7.3%.

[0070] Comparative Example 3 <Preparation of Polysiloxane Particle Dispersion No. 6> In a four-neck flask equipped with a cooling tube, a thermometer, and a dropping nozzle, 2200 parts of ion-exchanged water, 24 parts of 25% ammonia water, and 200 parts of methanol were charged and kept at 30°C. 120 parts of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503"), a crosslinkable silane monomer (silane coupling agent), was added to the flask to carry out hydrolysis and condensation of 3-methacryloxypropyltrimethoxysilane, thereby obtaining polysiloxane particle dispersion No. 6 having methacryloxy groups. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion was 4.7%, the number average particle size was 0.85 μm, and the coefficient of variation (CV value) was 8.0%.

[0071] Comparative Example 4 <Preparation of Polysiloxane Particle Dispersion No. 7> In a four-neck flask equipped with a condenser, a thermometer, and a dropping nozzle, 2400 parts of ion-exchanged water, 72 parts of 25% ammonia water, and 1200 parts of methanol were charged and kept at 30° C. To the flask, 81 parts of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., “KBM503”), which is a crosslinkable silane monomer (silane coupling agent), was added to obtain 3-methacryloxypropyltrimethoxysilane. After hydrolysis and condensation of dipropyltrimethoxysilane, 96 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08") was added to obtain polysiloxane particle dispersion liquid having methacryloxy groups No. 7. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion liquid was 2.1%, the number average particle size was 1.54 μm, and the coefficient of variation (CV value) was 4.1%.

[0072] <Preparation of Resin Particles No. 7 Using Polysiloxane Particle Dispersion No. 7> 3810 parts of polysiloxane particle dispersion (equivalent to 80 parts of 3-methacryloxypropyltrimethoxysilane) was placed in a 5L glass reactor to prepare an emulsion of polysiloxane particles. Next, 2 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier was dissolved in 80 parts of ion-exchanged water, to which was added a solution of 80 parts of styrene and 0.96 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., "V-65") as a polymerization initiator, and the mixture was emulsified and dispersed at 13,000 rpm for 15 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare a monomer emulsion. This monomer emulsion was added to the emulsion of polysiloxane particles and further stirred. One hour after the addition of the monomer emulsion, a sample of the reaction liquid was taken and observed under a microscope, and it was confirmed that the polysiloxane particles had absorbed the monomer composition and had become enlarged. Next, 20 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier and 800 parts of ion-exchanged water were added to the reaction solution, and the reaction solution was heated to 65°C under a nitrogen atmosphere and held at 65°C for 2 hours to carry out radical polymerization. After cooling the reaction solution, the resulting emulsion was separated into solid and liquid, and the resulting cake was washed with ion-exchanged water and then with methanol, and then dried under reduced pressure at 80°C for 4 hours under a nitrogen atmosphere to obtain resin particles No. 7. The yield of the obtained resin particles No. 7 was 80 parts, and the ratio of the yield of the base resin particles to the maximum ideal yield was 1.6%. The number-average particle diameter was 2.02 μm, and the coefficient of variation (CV value) was 3.2%. The results are shown in Table 1-2.

[0073] <Preparation of conductive particles (formation of conductive metal layer)> Except for using resin particle No. 7 as the base material, conductive fine particles were produced in the same manner as in Example 1. The particle size of the obtained conductive fine particles and the film thickness of the conductive metal layer were as shown in Table 1-2.

[0074] Comparative Example 5 <Preparation of Polysiloxane Particle Dispersion No. 8> In a four-neck flask equipped with a cooling tube, a thermometer, and a dropping port, 8320 parts of ion-exchanged water, 104 parts of 25% ammonia water, and 2080 parts of methanol were charged and kept at 30°C. 171.7 parts of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503"), which is a crosslinkable silane monomer (silane coupling agent), was added thereto to carry out hydrolysis and condensation of 3-methacryloxypropyltrimethoxysilane, and then 8 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol (registered trademark) NF-08") were added to obtain polysiloxane particle dispersion No. 8 having a methacryloxy group. As shown in Table 1-1, the solid content of the obtained polysiloxane particle dispersion was 1.6%, the number average particle size was 1.01 μm, and the coefficient of variation (CV value) was 5.0%.

[0075] <Preparation of Resin Particles No. 8 Using Polysiloxane Particle Dispersion No. 8> 3,125 parts of the polysiloxane particle dispersion (equivalent to 50 parts of 3-methacryloxypropyltrimethoxysilane) was placed in a 5 L glass reactor to prepare an emulsion of polysiloxane particles. Next, 6.3 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier was dissolved in 250 parts of ion-exchanged water, to which was added a solution of 125 parts of 1,6-hexanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., "Light Acrylate 1.6-HXA"), 45 parts of divinylbenzene (manufactured by Nippon Steel Chemical Co., Ltd., DVB960), 80 parts of styrene, and 3 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., "V-65") as a polymerization initiator, and the mixture was emulsified and dispersed at 13,000 rpm for 30 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare a monomer emulsion. This monomer emulsion was added to the emulsion of polysiloxane particles and further stirred. One hour after the addition of the monomer emulsion, a sample of the reaction liquid was taken and observed under a microscope, and it was confirmed that the polysiloxane particles had absorbed the monomer composition and had become enlarged. Next, 33.3 parts of a 20% aqueous solution of polyoxyethylene styrenated phenyl ether sulfate ester ammonium salt (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Hitenol NF-08") as an emulsifier and 1000 parts of ion-exchanged water were added to the reaction solution, and the reaction solution was heated to 65°C under a nitrogen atmosphere and held at 65°C for 2 hours to carry out radical polymerization. After cooling the reaction solution, the resulting emulsion was subjected to solid-liquid separation, and the resulting cake was washed with ion-exchanged water and then with methanol, and then subjected to heat treatment at 230°C for 1 hour under a nitrogen atmosphere to obtain resin particles No. 8. The yield of the obtained resin particles No. 8 was 238 parts, and the ratio of the yield of the base resin particles to the maximum ideal yield was 4.8%. The number average particle size was 2.04 μm, and the coefficient of variation (CV value) was 4.0%. The results are shown in Table 1-2.

[0076] <Preparation of conductive particles (formation of conductive metal layer)> Except for using resin particle No. 8 as the base material, conductive fine particles were produced in the same manner as in Example 1. The particle size of the obtained conductive fine particles and the film thickness of the conductive metal layer were as shown in Table 1-2.

[0077] <Preparation of connection structure> Using the conductive fine particles obtained in Examples 1 and 2 and Comparative Examples 4 and 5, anisotropic conductive materials (anisotropic conductive films) were produced by the following method, and the performance thereof was evaluated by the following method. That is, 100 parts of epoxy resin (Mitsubishi Chemical's "JER828") as a binder resin, 2 parts of a curing agent (Sanshin Chemical's "San-Aid (registered trademark) SI-150"), and 100 parts of toluene were added to 1 part of conductive fine particles, and 50 parts of zirconia beads with a diameter of 1 mm were further added, and the mixture was dispersed by stirring at 300 rpm for 10 minutes using two stainless steel stirring blades. The obtained paste-like composition was then applied to a PET film that had been subjected to a release treatment using a bar coater and dried to obtain an anisotropic conductive film.

[0078] The obtained anisotropic conductive film was sandwiched between a glass substrate with aluminum deposition on the entire surface having lines for resistance measurement and a polyimide film substrate with a copper pattern formed at a pitch of 20 μm, and thermocompression bonded under compression bonding conditions of 1 MPa and 190° C. to obtain a connection structure. The results of the initial resistance value and connection reliability measured by the above-mentioned method are shown in Table 1-2.

[0079] [Table 1-1]

[0080] [Table 1-2]

Claims

1. A dispersion of polysiloxane particles having a radical polymerizable group, The solid content is 4.8% by mass or more, The polysiloxane particles have a number average particle size of 0.5 μm or more and 2.0 μm or less, and the coefficient of variation of the particle size of the polysiloxane particles on a number basis is 7.2% or less.

2. 2. The polysiloxane particle dispersion according to claim 1, wherein the radical polymerizable group is at least one selected from the group consisting of a vinyl group, an acryloyl group, and a methacryloyl group.

3. A step (1) of mixing a silane coupling agent having at least one radical polymerizable group selected from the group consisting of a vinyl group, an acryloyl group, and a methacryloyl group, a solvent containing water, and an acid; A dispersion liquid of polysiloxane particles having a radical polymerizable group, which is obtained by subjecting the mixture obtained in the step (1) to a step (2) of adding a base.

4. A method for producing a dispersion of polysiloxane particles having a radical polymerizable group, comprising the steps of: A step (1) of mixing a silane coupling agent having a radical polymerizable group, a solvent containing water, and an acid; A method for producing a dispersion of polysiloxane particles having a radical polymerizable group, comprising: a step (2) of adding a base to the mixed liquid obtained in the step (1).

Citation Information

Patent Citations

  • Fine polyorganosilsesquioxane particle and production thereof

    JP1989217039A

  • Production of powdered silicone and powdered silicone

    JP1991244636A

  • Production of granular organopolysiloxane

    JP1999130861A

  • Production of polyorganosiloxane microparttcle

    JP1999181095A

  • Production of organic and inorganic composite particle

    JP1999199671A