Laminated sheet for paper container and paper container

The laminated sheet design with a bubbling suppression layer and optimized thickness and lamination strength addresses bubbling issues in paper containers, maintaining sealing integrity and appearance while reducing manufacturing complexity and costs.

JP2024161307AInactive Publication Date: 2024-11-15TOPPAN HOLDINGS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024157673
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing laminated sheets for paper containers face issues with bubbling during heating due to low resistance to water vapor expansion pressure, leading to sealing and appearance defects, and require additional steps that increase manufacturing costs and complexity.

Method used

A laminated sheet design with a bubbling suppression layer made of low density polyethylene or linear low density polyethylene, an adhesive layer, a barrier film layer, and a sealant layer, optimized for thickness and lamination strength, which suppresses bubbling during container molding while minimizing manufacturing steps.

Benefits of technology

The solution effectively prevents bubbling during container molding without increasing manufacturing complexity or costs, ensuring robust sealing and appearance quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161307000001_ABST
    Figure 2024161307000001_ABST
Patent Text Reader

Abstract

To provide a laminated sheet for a paper container capable of suppressing bubbling due to hot air (heating) during molding of the container while suppressing an increase in the number of manufacturing processes.SOLUTION: In a laminated sheet for a paper container, a bubbling suppressing layer, an adhesive layer, a barrier film layer and a sealant layer are laminated in this order on one surface side of a paper layer, and a thermoplastic resin layer is laminated on the other surface side of the paper layer. The bubbling suppressing layer is composed of a resin containing low density polyethylene or linear low density polyethylene. The melt tension of the resin is 0.04 N or more and 0.09 N or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a technology relating to a laminate sheet for paper containers and a paper container using the laminate sheet for paper containers. [Background technology]

[0002] Conventionally, containers such as glass bottles, cans, and plastic bottles have often been used to hold liquids such as beverages and alcohol, and powdery substances. However, in recent years, due to growing awareness of protecting the global environment, paper containers, which are highly recyclable and have a low environmental impact, have come to be widely used as containers for holding beverages, alcohol, and other contents. Generally, paper containers for liquids use packaging materials made of laminated sheets of multiple materials to ensure the storage stability of the contents, the strength of the container, gas barrier properties, etc. Packaging materials (laminated sheets) used in paper containers for liquids are known to have a layer structure in which a thermoplastic resin layer / paper layer / adhesive layer / barrier layer / sealant layer are laminated in this order from the outer surface side of the container. EMAA resin, which has good adhesion to the paper layer and the barrier film layer, is generally used for the adhesive layer.

[0003] When such a laminated sheet is molded into the desired container shape, a heating process is performed in which hot air is applied to heat the sealant layer to melt it. When hot air is applied to the sealant layer in this heating process, the moisture contained in the paper layer is rapidly heated by the heat and turns into water vapor. The expansion pressure of this water vapor may cause a foaming phenomenon (bubbling) that causes separation between the paper layer and the adhesive layer. The EMAA resin used in the adhesive layer has low resistance to expansion pressure, so bubbling is likely to occur. When bubbling as described above occurs, there is a possibility that it may cause a sealing failure and a defective appearance, and therefore, a laminate sheet is required that is less susceptible to bubbling. As a technique for suppressing bubbling, methods such as those described in Patent Documents 1 and 2 have been proposed.

[0004] Patent Document 1 describes a paper container formed by molding a laminated material mainly composed of a paper base material in which at least a paper layer and a barrier film layer are laminated via a melt-extruded resin layer, and the adhesive-coated surface of the paper layer and paper base material has a sizing degree of 400 seconds or more according to the measurement method of JIS P8122, and an adhesive layer made of a two-component curing adhesive having a urethane bond is applied to the adhesive-coated surface at a rate of 0.5 g / m 2 More than 4g / m 2 A paper container has been proposed which is characterized by being formed by coating with the following coating amount and forming a laminate material in which a paper layer and a barrier film layer are laminated so that the adhesive layer is interposed between the paper layer and the melt-extruded resin layer. In this case, the provision of the adhesive layer improves heat resistance or provides strength sufficient to withstand the pressure of water vapor expansion, thereby making it possible to suppress bubbling.

[0005] Patent Document 2 proposes a paper container sheet material for liquid packaging, in which at least an outer resin layer is laminated on one side of a main cardboard layer, and an inner sealant resin layer is laminated on the other side of the cardboard layer via an adhesive layer such as a plastic resin layer or a barrier layer, characterized in that the outer resin layer is provided with minute holes that are permeable to water vapor and reach the cardboard layer. According to this method, the holes in the outer resin layer serve as escape routes for water vapor evaporated by hot air, reducing the expansion pressure caused by water vapor, thereby making it possible to suppress bubbling. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 4577001 [Patent Document 2] JP 2000-203565 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the method described in Patent Document 1 requires the provision of an adhesive layer between the paper layer and the melt-extruded resin layer, which increases the material cost and the number of steps, thereby increasing the manufacturing cost. In addition, the method described in Patent Document 2 requires a step of providing holes, which increases the number of steps, and therefore there is a need to further simplify the steps. In addition, the method described in Patent Document 2 also has the risk that moisture and odors in the air may enter the paper layer through the pores when the paper container is in use. The present invention has been made with attention to the above-mentioned points, and aims to provide a laminated sheet for paper containers that can suppress bubbling caused by hot air (heating) during container molding while minimizing an increase in the number of manufacturing steps. [Means for solving the problem]

[0008] One embodiment of the present invention provides a laminate sheet for paper containers, which comprises a bubbling suppression layer, an adhesive layer, a barrier film layer and a sealant layer laminated in that order on one surface of a paper layer, and a thermoplastic resin layer laminated on the other surface of the paper layer, wherein the bubbling suppression layer is composed of a resin containing low-density polyethylene or linear low-density polyethylene, and the melt tension of the resin is 0.04 N or more and 0.09 N or less.

[0009] In addition, the laminated sheet for paper containers may have a sum of the film thicknesses of the bubbling-suppressing layer and the adhesive layer of 20 μm or more and 40 μm or less, a thickness of the bubbling-suppressing layer of 10 μm or more and 35 μm or less, and a thickness of the adhesive layer of 5 μm or more and 10 μm or less. Moreover, in the laminate sheet for paper containers, the adhesive layer and the barrier film layer may have a lamination strength of 2 N / 15 mm or more. In addition, in the laminated sheet for paper containers, the adhesive layer may be made of a resin containing any one of additive-free polyethylene, polyethylene containing an adhesive component, and an ethylene-acrylic acid copolymer.

[0010] The laminate sheet for paper containers is also characterized in that the barrier film layer is any film selected from the following (1) to (3), as described in any one of claims 1 to 4. (1) PET film with a metal vapor deposition layer (2) PET film with a vapor-deposited layer of inorganic oxide (3) Aluminum foil and PET film laminate Moreover, a paper container according to one embodiment of the present invention is obtained by forming the above-mentioned laminated sheet for paper containers into a container shape. Moreover, the shape of the paper container may be any one of a Gagel-top shape, a cup shape, and a cylindrical shape. Effect of the Invention

[0011] According to an aspect of the present invention, it is possible to suppress bubbling caused by hot air during container molding while suppressing an increase in the number of manufacturing steps. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic cross-sectional view illustrating an example of the configuration of a laminate sheet for paper containers according to one embodiment of the present invention. [Diagram 2] 1A to 1C are diagrams showing an example of a process for manufacturing a paper container according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a conceptual diagram illustrating a production example of a laminate sheet for paper containers according to one embodiment of the present invention. [Figure 4] 1A to 1C are diagrams illustrating an example of a manufacturing process for a paper container according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that each drawing is a schematic view, and the size and shape of each part are appropriately exaggerated for easy understanding. Also, the following description relates to an example of the present invention, and the present invention is not limited thereto. (Laminated sheet for paper containers) Fig. 1 is a schematic cross-sectional view illustrating an example of the configuration of a laminate sheet for paper containers according to one embodiment of the present invention. The laminate sheet for paper containers 10 of this embodiment has a structure in which a bubbling suppression layer 3, an adhesive layer 4, a barrier film layer 5, and a sealant layer 6 are laminated in this order on one surface side of a paper layer 2, and a thermoplastic resin layer 1 is laminated on the other surface side of the paper layer 2.

[0014] Next, each layer that constitutes the paper container laminate sheet 10 will be described individually. (Paper layer 2) The paper layer 2 is a layer that mainly provides the formability and rigidity of the container. Examples of the paper layer 2 include surface-treated coated paper and untreated uncoated paper. The paper layer 2 may be made of a known paper material used in paper containers. The paper basis weight of the paper layer 2 is, for example, 200 g / m 2 More than 500g / m 2 The following are preferred, but may be selected appropriately according to the container size. Here, in order to improve adhesion between the surface of the paper layer 2 and the thermoplastic resin layer 1 and the bubbling suppression layer 3, it is preferable that a surface treatment such as a corona treatment is appropriately performed.

[0015] (Bubbling suppression layer 3) The bubbling suppression layer 3 is a layer provided to suppress bubbling. Examples of resins selected for the bubbling suppression layer 3 include low-density polyethylene, linear low-density polyethylene, and resins containing them. The material selected for the bubbling suppression layer 3 is preferably one that has good adhesion to the paper layer 2, is easy to extrude, and is inexpensive. However, polyethylene is easy to co-extrude with the resin used for the adhesive layer 4 described later, and has good adhesion, so that it can obtain good adhesive strength while being excellent in processability. It also has excellent adhesion to the paper layer 2. If a resin other than polyethylene is used, it becomes difficult to achieve both adhesion to the paper layer 2 and the adhesive layer 4, and sufficient adhesive strength cannot be obtained at either interface, which may cause delamination, etc.

[0016] A polyethylene resin with a melt tension in the range of 0.04N to 0.09N is used for the bubbling suppression layer 3. When a resin with a melt tension in the above range is placed in the bubbling suppression layer 3 adjacent to the paper layer, the resistance to the expansion pressure caused by the steam of the moisture in the paper is increased, and the effect of suppressing bubbling is obtained. In this case, if the melt tension is greater than 0.09N, the adhesion with the paper layer 2 decreases and delamination is likely to occur, so bubbling occurs easily. Also, if the melt tension is less than 0.04N, the resin does not have enough tenacity and is unable to resist the expansion pressure of steam.

[0017] The melt tension is a value measured using a capillary rheometer (Rosand RH-7D manufactured by NETZSCH) at a measurement temperature of 200° C., a piston speed of 20 mm / min, and a take-up speed of 10 m / min. The thickness of the bubbling suppression layer 3 is preferably 10 μm or more and 35 μm or less. In terms of maintaining the adhesiveness of the paper layer 2 and the adhesive layer 4, if the thickness is less than 10 μm, the adhesiveness will decrease and delamination may occur. If the thickness is more than 35 μm, problems will occur during the container molding process, such as difficulty in forming creasing lines.

[0018] Examples of a method for laminating the bubbling-suppressing layer 3 include an extrusion coating method and a method of laminating the barrier film layer 5 with the adhesive layer 4 by a co-extrusion lamination method described below. Note that co-extrusion lamination with the adhesive layer 4 is a more preferable lamination method because it allows multiple layers to be laminated at once and simplifies the manufacturing process. When the adhesive layer 4 is extrusion coated in a single layer configuration, the bubbling suppression layer 3 may be appropriately subjected to a corona treatment in order to improve adhesion.

[0019] (adhesive layer 4) The adhesive layer 4 is provided on one surface of the bubbling suppression layer 3 in order to adhere a barrier film layer 5, which will be described later. The laminate strength between the adhesive layer 4 and the barrier film layer 5 is preferably 2N / 15mm or more. If the laminate strength is 2N / 15mm or more, it is possible to prevent liquid leakage due to poor sealing when liquid is poured into the container. The adhesive layer 4 is not particularly limited as long as it is made of a thermoplastic resin that has adhesiveness to the bubbling suppression layer 3 in addition to adhesiveness to the barrier film layer as described above. The reason why a thermoplastic resin is used is that it can be laminated with the bubbling suppression layer 3 by co-extrusion lamination with a small number of steps.

[0020] Examples of the thermoplastic resin constituting the adhesive layer 4 include low-density polyethylene, medium-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-α-olefin copolymer resin, copolymers with ethylene-unsaturated carboxylic acid or its ester compound such as ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, etc., ionomer resin, etc. Among these, additive-free polyethylene having good adhesion to the low-density polyethylene constituting the bubbling-suppressing layer 3, polyethylene containing an adhesive component, ethylene-acrylic acid copolymer, etc. are more preferable.

[0021] The sum of the film thicknesses of the bubbling suppression layer 3 and the adhesive layer 4 is preferably 20 μm or more and 40 μm or less. If the sum of the film thicknesses of the bubbling suppression layer 3 and the adhesive layer 4 is thinner than 20 μm, heat is transferred quickly to the paper, which is the location where bubbling occurs, during heating with hot air, making bubbling more likely to occur. If the sum of the film thicknesses of the bubbling suppression layer 3 and the adhesive layer 4 is thicker than 40 μm, problems such as difficulty in forming creases for forming a container are more likely to occur. The thickness of the adhesive layer 4 is preferably 5 μm or more and 10 μm or less. If it is thinner than 5 μm, the adhesion to the bubbling suppression layer 3 and the barrier film layer 5 decreases, and delamination is likely to occur. If the thickness of the adhesive layer 4 is thicker than 10 μm, when the sum of the film thicknesses of the bubbling suppression layer 3 and the adhesive layer 4 is designed to be within the above-mentioned preferred range, the bubbling suppression layer 3 cannot have a sufficient thickness.

[0022] Examples of a method for laminating the adhesive layer 4 include known methods such as an extrusion lamination method in which the bubbling suppression layer 3 and the barrier film layer 5 are sandwiched in a molten state between the bubbling suppression layer 3 and the barrier film layer 5. Alternatively, a coextrusion lamination method can be applied in which the bubbling suppression layer 3 and the adhesive layer 4 are coextruded and sandwiched in a molten state between the paper layer 2 and the barrier film layer 5. The two-layer coextrusion lamination method is more preferable because it allows the lamination of the barrier film layer 3 and the lamination of the adhesive layer 4 to be carried out simultaneously, thereby eliminating a step.

[0023] (Barrier film layer 5) The barrier film layer 5 is provided to provide the container with gas barrier properties. For the barrier film layer 5, for example, a film obtained by depositing an inorganic material such as silica, alumina, or aluminum on a substrate film such as a biaxially oriented polyester film, a nylon film, a polycarbonate film, a polyvinyl alcohol film, or an ethylene-vinyl alcohol copolymer resin can be used. The thickness of this substrate film is suitably about 5 to 30 μm. The thickness of the deposited film itself may be sufficient to achieve the required gas barrier properties, and for example, when silica is deposited, the thickness is preferably about 30 to 200 nm.

[0024] The barrier film layer 5 may also be prepared by bonding an aluminum foil and the above-mentioned base film by a dry lamination method. When the barrier film layer 5 is laminated with the adhesive layer 4 or the sealant layer 6, the surface may be appropriately subjected to a corona treatment in order to improve adhesion. The barrier film layer 5 is preferably any film selected from the following (1) to (3). (1) PET film with a metal vapor deposition layer (2) PET film with a vapor-deposited layer of inorganic oxide (3) Aluminum foil and PET film laminate Here, the above-mentioned "provided" includes not only the case where the film is provided on one side of the PET film, but also the case where the film is provided on both sides.

[0025] (Sealant layer 6) Resins generally used for sealant layers can be used for the sealant layer 6. Examples of resins constituting the sealant layer 6 include polyethylene-based resins such as low-density polyethylene, medium-density polyethylene, linear low-density polyethylene, ethylene-α-olefin copolymer resins, and ethylene-vinyl acetate copolymers, and polypropylene. The sealant layer 6 can be used as a single layer of these resins, or as a multilayer in which a plurality of resins are combined.

[0026] The thickness of the sealant layer 6 is not particularly limited as long as it has sufficient sealing properties when the container is formed, and any known thickness can be used. The appropriate thickness of the sealant layer 6 is, for example, 30 μm or more and 100 μm or less. The method for laminating the sealant layer 6 is not particularly limited, but generally used are a dry lamination method using a two-component curing adhesive having a urethane bond after film formation, and an extrusion coating method in which the sealant layer 6 is laminated in a molten state on the barrier film layer 5. In the case of extrusion coating, in order to enhance adhesion with the barrier film layer 5, an adhesive may be applied to the barrier film layer 5 in advance, and then the sealant layer 6 in a molten state may be laminated thereon.

[0027] (Thermoplastic resin layer 1) The thermoplastic resin layer 1 is the outermost layer after the container is molded, and is provided to protect the paper layer and perform printing. The thermoplastic resin layer 1 must have properties such as heat sealability and printability for heat fusing the thermoplastic resin layers together when the laminated sheet is molded into various container shapes such as square or round. Examples of resins selected for the thermoplastic resin layer 1 include low-density polyethylene, linear low-density polyethylene, ethylene-α-olefin copolymer resins, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-methyl acrylate copolymers, ethylene-methyl methacrylate copolymers, and copolymers of ethylene and unsaturated carboxylic acids or ester compounds thereof, such as ionomer resins.

[0028] The thickness of the thermoplastic resin layer 1 can be a known thickness used for the thermoplastic resin layer of a paper container. The thickness of the thermoplastic resin layer 1 is determined by the thickness of the thermoplastic resin layer when the thermoplastic resin layers are heated together during container molding. It is sufficient that the thermoplastic resin layer 1 has a minimum thickness necessary for fusion and for enduring impact such as dropping after molding of the container. The thickness of the thermoplastic resin layer 1 is generally set to 10 μm or more and 30 μm or less. The extrusion coating method, in which the thermoplastic resin layer 1 is laminated on the paper layer in a molten state, can be used for laminating the thermoplastic resin layer 1. If the dry lamination method is used, the adhesive layer blocks the escape route of the water vapor generated in the paper layer 2 during hot air heating, which tends to increase the internal pressure in the paper layer 2 and cause bubbling, which is not preferable. The order in which each layer is laminated on the paper layer 2 is not particularly limited. The thermoplastic resin layer 1 may be laminated first, and then the bubbling suppression layer 3 may be laminated, or the layers may be laminated in the reverse order. The surface of the thermoplastic resin layer 1 may be subjected to a surface treatment such as a corona treatment, if necessary, and then printing may be carried out.

[0029] (Paper container) Fig. 2 is a diagram showing an example of a process for manufacturing a paper container according to one embodiment of the present invention. A paper container is formed using the paper container laminate sheet 10 described in the above embodiment. The manufacturing process 20 for manufacturing a paper container having a desired container shape from the paper container laminate sheet 10 includes a heating process 20A and a molding process 20B, as shown in Fig. 2. The heating process 20A is a process in which heat is applied from both the sealant layer 6 side of the paper container laminate sheet 10, which will be the inside of the paper container, and the thermoplastic resin layer 1 side of the paper container laminate sheet 10, which will be the outside of the paper container, to temporarily melt the sealant layer 6 and the thermoplastic resin layer 1. The heating process in the heating step 20A is carried out, for example, by blowing hot air at a temperature of 340° C. for one second. In the molding step 20B, a load is applied to the sealant layer 6 and the thermoplastic resin layer 1, which have been temporarily in a molten state after the heating step 20A, to seal and simultaneously mold them three-dimensionally into a container shape. The heating step 20A and the molding step 20B are first performed on the bottom of the container. After molding the bottom of the container, the contents are filled, and then the heating step 20A and the molding step 20B are performed again to seal and mold the top of the container.

[0030] (Example of manufacturing process) An example of a method for manufacturing a laminated sheet for paper containers and a paper container according to this embodiment is shown. Fig. 3 is a conceptual diagram for explaining an example of a manufacturing process of a laminated sheet for paper containers according to one embodiment of the present invention. Fig. 4 is a diagram for explaining an example of a manufacturing process of a paper container according to one embodiment of the present invention.

[0031] <Production Example of Laminated Sheet 10 for Paper Containers> First, as shown in FIG. 3(a), a laminate sheet (5, 6) is produced by laminating a resin constituting a sealant layer 6 by extrusion coating onto a barrier film layer 5 previously coated with an adhesive. Next, as shown in FIG. 3(b), the bubbling suppression layer 3 and adhesive layer 4 are co-extrusion laminated onto the laminated sheets (5, 6) and paper layer 2 produced above to produce laminated sheets (2-6). Next, as shown in FIG. 3(c), the laminate sheets (2-6) produced above and a thermoplastic resin layer 1 are laminated by extrusion molding to sequentially form a laminate sheet 10 for paper containers, and the laminate sheet 10 for paper containers is rolled.

[0032] <Example of paper container manufacturing> As shown in FIG. 4(a), the manufactured laminated sheet for paper containers 10 is cut into sheets to obtain blanks as shown in FIG. 4(b) (punching step). Next, as shown in FIG. 4(c), a scoring process is carried out to add creases to the blank material to make it easier to assemble. Next, it is molded into a cylindrical shape as shown in FIG. 4(d). Next, as shown in Fig. 4(e), the sealant layer 6 side (inner surface) and the thermoplastic resin 1 side (outer surface) on the bottom side of the cylindrical molded product are heated with hot air (heating process 20A), and a molding process is performed to seal and close the bottom of the container (molding process 20B). Next, as shown in FIG. 4(f), the contents are filled from the top side (filling process). Next, as shown in FIG. 4(g), the surface (inner surface) of the sealant layer 6 on the top side and the surface (outer surface) of the thermoplastic resin 1 are heated with hot air (heating process 20A) to seal and close the top part of the container (molding process 20B).

[0033] [Example 1] An LDPE film (thickness 55 μm) that had been previously subjected to a corona treatment on one side was prepared as the sealant layer 6, and a PET film (thickness 12 μm) that had been silica-vapor-deposited on one side and corona-treated on the other side was prepared as the barrier film layer 5, and the silica-vapor-deposited surface and the corona-treated surface of the LDPE film were laminated by a dry lamination method using a urethane adhesive to produce a laminate sheet of barrier film layer 5 / sealant layer 6. In addition, the PET surface exposed on the barrier film layer 5 side of the barrier film layer 5 / sealant layer 6 laminate sheet was subjected to a corona treatment.

[0034] Paper layer 2: basis weight 380g / m 2After corona treatment was performed on both sides of the paper layer 2, LDPE (Suntech L2340, manufactured by Asahi Kasei Corp.) was extrusion coated to a thickness of 18 μm from the first T-die of the tandem extruder on one side of the paper substrate, and the thermoplastic resin layer 1 was laminated on the paper layer 2. Next, LDPE (L2340, manufactured by Asahi Kasei Corp., melt tension 0.08 N, thickness 20 μm) as the bubbling suppression layer 3 and EMAA (AN4228C, manufactured by Mitsui DuPont Polychemicals Co., Ltd., thickness 10 μm) as the adhesive layer 4 were co-extruded from the second T-die onto the opposite side of the paper substrate on which the thermoplastic resin layer 1 was formed and the PET film side of the laminated film of the barrier film layer 5 / sealant layer 6, to produce a laminated sheet.

[0035] The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) (1) / paper (basis weight 380 g / m 2 ) (2) / LDPE (L2340, melt tension 0.08 N, thickness 20 μm) (3) / EMAA (AN4228C, thickness 10 μm) (4) / silica-deposited PET film (thickness 12 μm) (5) / LDPE (thickness 55 μm) (6) (see Figure 1).

[0036] [Example 2] A laminate sheet was produced in the same manner as in Example 1, except that the resin of the bubbling suppression layer 3 in Example 1 was changed to LDPE (L1640 manufactured by Asahi Kasei Corporation, melt tension 0.05 N). The composition of the obtained laminated sheet was L2340 (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (L1640, melt tension 0.05N, thickness 20μm) / EMAA (AN4228C, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm).

[0037] [Example 3] A laminate sheet was produced in the same manner as in Example 1, except that the resin of the bubbling suppression layer 3 in Example 1 was changed to LDPE (LC500 manufactured by Asahi Kasei Corporation, melt tension 0.04 N). The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (LC500, melt tension 0.04N, thickness 20μm) / EMAA (AN4228C, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm).

[0038] [Example 4] A laminate sheet was produced in the same manner as in Example 1, except that the resin of the bubbling suppression layer 3 in Example 1 was changed to LDPE (M2629 manufactured by Asahi Kasei Corporation, melt tension 0.09 N). The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (M2629, melt tension 0.09N, thickness 20μm) / EMAA (AN4228C, melt tension 0.02N, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm).

[0039] [Example 5] A laminate sheet was produced in the same manner as in Example 1, except that the resin of the bubbling suppression layer 3 in Example 1 was changed to LDPE (LC522 manufactured by Japan Polyethylene Corporation, melt tension 0.09 N). The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (LC522, melt tension 0.09N, thickness 20μm) / EMAA (AN4228C, melt tension 0.02N, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm).

[0040] [Comparative Example 1] The resin of the bubbling suppression layer 3 in Example 1 was EMAA (manufactured by Mitsui DuPont Polychemicals Co., Ltd.). A laminate sheet was produced in the same manner as in Example 1, except that the melt tension of AN4228C was changed to 0.02 N. The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2) / EMAA (AN4228C, melt tension 0.02N, thickness 20μm) / EMAA (AN4228C, melt tension 0.02N, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm).

[0041] [Comparative Example 2] A laminate sheet was produced in the same manner as in Example 1, except that the resin of the bubbling suppression layer 3 in Example 1 was changed to LDPE (L6810 manufactured by Asahi Kasei Corporation, melt tension 0.03 N). The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (L6810, melt tension 0.03N, thickness 20μm) / EMAA (AN4228C, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm).

[0042] [Comparative Example 3] A laminate sheet was produced in the same manner as in Example 1, except that the resin of the bubbling suppression layer 3 in Example 1 was changed to LDPE (M6520 manufactured by Asahi Kasei Corporation, melt tension 0.007 N). The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / LDPE (M6520, melt tension 0.007N, thickness 20μm) / EMAA (AN4228C, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm).

[0043] [Comparative Example 4] A laminate sheet was produced in the same manner as in Example 1, except that the resin of the bubbling suppression layer 3 in Example 1 was changed to PP (MFX3 manufactured by Japan Polypropylene Corporation, melt tension 0.007 N). The composition of the obtained laminated sheet was LDPE (L2340, thickness 18 μm) / paper (basis weight 380 g / m 2 ) / PP (MFX3, melt tension 0.16N, thickness 20μm) / EMAA (AN4228C, thickness 10μm) / silica-deposited PET film (thickness 12μm) / LDPE (thickness 55μm). The bubbling resistance of the above-prepared Examples 1 to 5 and Comparative Examples 1 to 4 was evaluated, and the results are shown in Table 1.

[0044] [Evaluation method] The time until bubbling occurred was measured when hot air at 240° C. was sprayed from a distance of 2 cm from the sealant layer 6 side using a heat gun 7 (Earthman HG-1450B, manufactured by Takagi Corporation). The time until bubbling occurred for EMAA in Comparative Example 1 was used as the standard, and if the time until bubbling occurred was long, it was judged as ◯, and if it was short, it was judged as ×.

[0045] [Table 1]

[0046] As shown in Table 1, it was confirmed that the time when bubbling occurs was delayed by using a resin having a melt tension of 0.04 to 0.09 N for the bubbling suppression layer 3, and it was made clear that the bubbling resistance was improved. [Explanation of symbols]

[0047] 1...Thermoplastic resin layer 2…Paper layer 3…Bubbling suppression layer 4...Adhesive layer 5...Barrier film layer 6…Sealant layer 10...Laminated sheet for paper containers

Claims

1. A laminated sheet for paper containers, comprising a bubbling suppression layer, an adhesive layer, a barrier film layer and a sealant layer laminated in this order on one surface side of a paper layer, and a thermoplastic resin layer laminated on the other surface side of the paper layer, The bubbling suppression layer is made of a resin containing low-density polyethylene, The sum of the film thicknesses of the bubbling suppression layer and the adhesive layer is 20 μm or more and 40 μm or less, The melt tension of the resin is 0.04 N or more and 0.09 N or less, A laminate sheet for paper containers, characterized in that the thermoplastic resin layer is made of low-density polyethylene.

2. The laminated sheet for paper containers according to claim 1, characterized in that the adhesive layer is composed of a resin containing either additive-free polyethylene, polyethylene containing an adhesive component, or an ethylene-acrylic acid copolymer.

3. 2. The laminate sheet for paper containers according to claim 1, wherein the melt tension of the resin constituting the bubbling suppression layer is equal to that of the resin constituting the thermoplastic resin layer.

Citation Information

Patent Citations

  • Paper cup

    JP2004338773A

  • Laminated sheet for paper container and paper container

    JP2021181331A

  • Paper-made container sheet material for packaging liquid

    JP2000203565A

  • Method for manufacturing paper containers and the laminated materials constituting those containers.

    JP4577001B2