Method for producing sintered ore

The method of continuous component analysis and layer thickness adjustment using LIBS stabilizes RDI in sintered ore, addressing quality inconsistencies caused by lower-quality iron ore, enhancing blast furnace efficiency.

JP2024161838APending Publication Date: 2024-11-20NIPPON STEEL CORPORATION
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023076928
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20

AI Technical Summary

Technical Problem

Conventional sintered ore manufacturing processes struggle to manage compositional fluctuations due to the use of lower-quality iron ore, leading to inconsistent Reduction Degradation Index (RDI) in blast furnace operations, which affects permeability and efficiency.

Method used

A method involving continuous component analysis of finished sintered ore using laser-induced breakdown spectroscopy (LIBS) to adjust the layer thickness of the raw material packed bed based on real-time chemical composition data, stabilizing RDI by controlling the sintered ore's chemical composition.

Benefits of technology

Enables rapid detection and stabilization of RDI, ensuring consistent sintered ore quality by adjusting the layer thickness in response to chemical composition changes, thereby improving blast furnace operation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161838000001_ABST
    Figure 2024161838000001_ABST
Patent Text Reader

Abstract

To provide a method for producing of sintered ore that speedily detects variation of a chemical composition of a sintering raw material to stabilize a reduction degradation index (RDI).SOLUTION: The method for producing sintered ore in the present invention is a method for producing a sintered cake by charging a blending raw material containing a plurality of types of iron ore, auxiliary raw materials, and setting raw material into a sintering machine to sinter the charged blending raw materials to produce a sintered cake, then sieving the sintered cake into a product sintered ore and a return ore with a classifier, the sieved product sintered ore is transferred to a blast furnace, wherein a concentration of at least one component of the product sintered ore being transported to the blast furnace facility is continuously measured, and based on the component concentration data obtained by the measurement, a layer thickness of a raw material filling layer to be formed is adjusted by charging the blending raw material into the sintering machine.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing sintered ore for producing sintered ore for a blast furnace. [Background technology]

[0002] Currently, the main raw material for blast furnace pig iron production is sintered ore. Sintered ore (product sintered ore) used as a blast furnace raw material is generally produced by sintering raw materials for sintered ore production (sintered raw material), including iron ore, in a downward suction type Dwight Lloyd (DL) sintering machine, and then regulating the grain size to a specified size by crushing, sieving, etc. The product sintered ore is sampled every 4 to 7 hours, and the elemental composition is measured by X-ray fluorescence analysis and chemical analysis. The sintered ore production process and blast furnace operation are then managed based on this measurement data.

[0003] In recent years, homogeneous and high-quality iron ore has been depleted, and the quality of iron ore used as sintering raw material has deteriorated, resulting in the content of many components such as gangue. As a result, the components of sintered ore have begun to vary even within the same lot. In order to improve the production efficiency of blast furnace operations, it is necessary to carefully manage the blending ratio of sintering raw materials in the sintered ore manufacturing process, and the blending ratio and operating conditions (furnace temperature, pressure, etc.) of blast furnace raw materials in blast furnace operation, in accordance with the component fluctuations of sintered ore. However, as described above, the conventional management of the sintered ore manufacturing process and blast furnace operation was carried out based on the component analysis results of samples taken from the finished sintered ore during transportation at specified time intervals. Because it takes time to obtain the component analysis results, the component analysis cannot keep up with the component fluctuations of sintered ore, making it difficult to implement appropriate management.

[0004] In response to this, Patent Document 1 discloses a technique for continuously measuring the component concentrations of moisture and CaO contained in the sintering raw material transported on a transport conveyor 30. Specifically, Patent Document 1 discloses a technique having a measuring step for measuring the component concentration of at least one of the iron-containing raw material, the sintering raw material, and the granulated sintering raw material, and an adjustment step for adjusting at least one of the opening degree of the charging gate and the inclination angle of the chute with respect to the horizontal plane, using the component concentration measured in the measuring step, so that the charging density of the charging bed becomes a predetermined charging density. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-173161 A Summary of the Invention [Problem to be solved by the invention]

[0006] The Reduction Degradation Index (RDI) is used as one of the indicators for quality control of sintered ore. If the RDI is high, the sintered ore will be pulverized during the reduction reaction during blast furnace operation, and the air permeability inside the blast furnace will deteriorate. If the thickness of the raw material packed bed is reduced (the bed height is lowered), the flow rate of air (passing air volume) passing through the raw material packed bed will increase, resulting in sintered ore with a low RDI. The thickness of the raw material packed bed, which must be controlled to obtain sintered ore with the target RDI, also depends on the chemical composition of the sintered ore.

[0007] The present invention provides a method for producing sintered ore that quickly detects fluctuations in the chemical composition of sinter raw materials and stabilizes the RDI. [Means for solving the problem]

[0008] (1) A mixture of raw materials including multiple types of iron ore, auxiliary materials, and coagulants is charged into a sintering machine; Sintering the charged blended raw materials to produce a sintered cake; The sintered cake is sieved into product sinter and return ore using a classification device, In the method for producing sintered ore, the sieved product sintered ore is transported to a blast furnace facility, Continuously measuring the concentration of at least one component of the product sintered ore being transported to the blast furnace facility; a layer thickness of a raw material packed bed formed by charging the blended raw materials into the sintering machine is adjusted based on the component concentration data obtained by the measurement. (2) The method for producing sintered ore according to (1), wherein the component to be measured is at least one of CaO, SiO2, Al2O3, MgO, and TiO2. (3) The method for producing sintered ore described in (1) above, in which the adjustment of the layer thickness is performed by using the reduction disintegration index (RDI) of the product sintered ore as a target variable and controlling the RDI within a predetermined range based on a prediction equation including the component concentration data and the layer thickness as explanatory variables. (4) In the measurement, The method for producing sintered ore according to any one of (1) to (3), further comprising irradiating the finished sintered ore with a laser beam while the finished sintered ore is being transported to the blast furnace facility, thereby performing a component analysis using laser-induced breakdown spectroscopy to obtain the component concentration data. Effect of the Invention

[0009] According to the present invention, the thickness of the raw material packed bed is adjusted based on the measurement data obtained by continuously measuring the component concentrations of the product sintered ore during transportation, thereby making it possible to quickly detect fluctuations in the chemical composition of the sinter raw material and stabilize the RDI. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a diagram showing a sintered ore manufacturing process according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Embodiment 1> The present invention relates to a method for producing sintered ore, which comprises charging a blended raw material containing multiple types of iron ore, auxiliary raw materials, and aggregating agent into a sintering machine, sintering the charged blended raw material to produce a sintered cake, sieving the sintered cake into a product sintered ore and return ore with a classifier, and transporting the sieved product sintered ore to a blast furnace facility. The method includes continuously measuring the concentration of at least one component of the product sintered ore being transported to the blast furnace facility, and adjusting the concentration based on the component concentration data obtained by the measurement. The present invention will be described below with reference to the drawings. Figure 1 is a diagram showing an example of a sintered ore production process according to the present invention.

[0012] As shown in Figure 1, the sintered ore manufacturing process includes a raw material mixing process S1, a granulation process S2, a sintering process S3, a cooling and crushing process S4, and a classification process S5. After each process, the raw materials and semi-finished products are transported to the next process by a transport device such as a belt conveyor.

[0013] The raw material blending step S1 is a step of blending raw materials for sintered ore (sinter raw materials). The sintering raw materials are iron raw materials such as iron ore (powder) of various brands, iron-containing miscellaneous raw materials such as scale and iron-making dust, SiO2-containing auxiliary raw materials such as silica stone, MgO-containing auxiliary raw materials such as olivine, CaO-containing auxiliary raw materials such as limestone, return ore, and agglomeration materials (carbon materials) that serve as fuel for sintering (agglomeration), etc. Each sintering raw material is stored in each raw material tank installed in the raw material tank group, and a predetermined amount of each sintering raw material is cut out onto a belt conveyor, mixed in a predetermined ratio (mixing ratio), and sent to the granulation process S2.

[0014] The granulation step S2 is a step of granulating the blended sintering raw materials (blended raw materials) (adjusting the particle size distribution) for the purpose of ensuring the air permeability of the raw material packed bed. The mixed raw materials transported by the belt conveyer are fed into a granulator. After mixing for a specified time in the granulator, water is added (humidity control), and granulation is performed by mixing for a specified time, producing pseudo-particles that are aggregates of the primary particles of the raw materials. The mixed raw materials after granulation (hereinafter also referred to as the mixed raw material granules) are sent to the sintering process S3.

[0015] The sintering step S3 is a step of sintering the blended raw material granules to produce a sintered cake (sinter cake). The mixed raw material granules are stored in a mixed raw material surge hopper from the belt conveyor, and then loaded onto the pallet of a Dwight Lloyd (DL) type sintering machine to form a raw material packed bed. The raw material packed bed is ignited by an ignition furnace and sintered by the combustion heat of the coagulant in the raw material packed bed. The sintered cake obtained by sintering is discharged from the ore discharge end of the sintering machine, roughly crushed into sintered ore with a particle size of less than 200 mm by a crusher (primary crushing), and sent to the cooling and crushing process S4.

[0016] The cooling and crushing step S4 is a step in which the roughly crushed lump-shaped sintered ore is cooled and crushed. The lump sintered ore is cooled by a cooling device to a temperature at which it can be transported by a belt conveyor. The lump sintered ore is then crushed by a crusher (secondary crushing) and sent to the classification step S5 in a finer particle size state.

[0017] The classification step S5 is a step of grading the pulverized sintered ore for use in a blast furnace. The crushed sintered ore is sized by screening using a multi-stage classification device. Sintered ore (product sintered ore) of a particle size suitable for blast furnace charging is selected by the sizing process. The particle size suitable for blast furnace charging is, for example, sintered ore with a particle size of 5 mm or more and less than 50 mm. Here, a particle size of 5 mm or more and less than 50 mm refers to a particle size that is an oversize particle when sieved through a 5 mm sieve and an undersize particle when sieved through a 50 mm sieve. Note that sintered ore with a particle size of 50 mm or more is crushed to a particle size of less than 50 mm, and then sized again.

[0018] Each classifier is, for example, a rocking classifier with an inclined screen (sieve mesh), and a rocking motion is imparted to it by an eccentric drive mechanism. The classification intensity can be adjusted by changing the rotation speed of the motor that rotates this drive mechanism. The product sintered ore selected in the classification process S5 is placed on the blast furnace conveying line L1, and the other sintered ores are placed on the return ore conveying line L2.

[0019] The blast furnace transport line L1 is a line that transports the finished sintered ore to the blast furnace facility. The blast furnace transport line L1 is equipped with conveyors and other transport devices. The product sintered ore with a particle size of 5 mm or more but less than 50 mm is transported to the blast furnace equipment and used as the raw material for blast furnace iron production. The product sintered ore is charged into the blast furnace by multiple belt conveyors together with reducing materials such as coke, limestone, and serpentine produced in a separate process.

[0020] The return ore transport line L2 is a line that returns fine sintered ore that is not suitable for use as a blast furnace raw material to the raw material blending process S1. The return ore transport line L2 is equipped with a transport device such as a conveyor, and transports sintered ore with a particle size of less than 5 mm, which is smaller than the finished sintered ore (hereinafter, sintered ore with a particle size of less than 5 mm is also referred to as -5 mm sintered ore), into the raw material tank for return ore described above. A particle size of less than 5 mm refers to the particle size that falls under the sieve when sieved through a 5 mm sieve. The transported -5 mm sintered ore is mixed into the sintering raw material as return ore.

[0021] The blast furnace conveying line L1 of the present invention is equipped with a component analyzer 1 capable of online analysis. This component analyzer 1 continuously measures the component concentration of the product sintered ore online. In the present invention, the layer thickness of the raw material packed bed in the sintering process S3 is adjusted based on the component concentration data obtained by the component measurement of the product sintered ore on the blast furnace conveying line L1. Note that the "layer thickness of the raw material packed bed" in this embodiment refers to the thickness of only the raw material packed bed formed by the blended raw materials, since the blended raw materials are charged on top of the bedding layer of the pallet on which the bedding is laid.

[0022] Reduction Degradation Index (RDI) is used as one of the indicators for quality control of sintered ore. If the RDI is high, the sintered ore will be pulverized during the reduction reaction in blast furnace operation, and the air permeability inside the blast furnace will deteriorate. In DL-type sintering machines, the utilization of combustion exhaust gas from the upper layer increases in the lower layer, so the maximum temperature of the sintered layer becomes higher and the time that the oxidizing atmosphere at high temperature is maintained is also longer. As a result, the crystals of the generated minerals become coarse in the lower layer, and the coarsening of the crystal grains of secondary hematite, which is the mineral that causes the deterioration of RDI, becomes particularly noticeable. The reduction and disintegration of sintered ore is said to be caused by the volumetric distortion that occurs when secondary hematite is reduced to magnetite. A decrease in the cooling rate in the sintering reaction is one of the factors that deteriorates the RDI. In addition, the RDI also deteriorates due to a decrease in the amount of fusion bonding (the amount of molten liquid generated in the sintering reaction), as well as the drop strength (SI), which is one of the indicators of sintered ore quality. One method for controlling RDI is to adjust the chemical composition of sintered ore, but there are restrictions imposed by blast furnace operation, such as the pig iron composition and the physical properties of blast furnace slag, and the degree of freedom in adjusting the composition is limited.

[0023] Here, if the layer thickness of the raw material packed bed is reduced (the layer height is reduced), the flow rate (passing air volume) of the air passing through the raw material packed bed increases, so that the maximum temperature of the lower layer is prevented from becoming excessively high, and sintered ore with a low RDI is obtained. The layer thickness of the raw material packed bed, which should be controlled to obtain sintered ore with a target RDI, also depends on the chemical composition of the sintered ore. In the present invention, the layer thickness of the raw material packed bed is controlled using the chemical composition of the product sintered ore measured on the belt based on a relational expression obtained in advance by multiple regression analysis of the relationship between the chemical composition of the product sintered ore, the layer thickness of the raw material packed bed, and the RDI. This makes it possible to stably maintain the target RDI even when the chemical composition of the sintering raw material fluctuates. Next, the measurement of the component concentration of the product sintered ore will be described.

[0024] (Measurement of component concentration in finished sintered ore) The component concentration measurement on the blast furnace conveying line L1 is performed on the product sintered ore being conveyed to the blast furnace facility as the analysis target. The component analyzer 1 is, for example, a laser analyzer, an infrared analyzer, a neutron analyzer, a microwave analyzer, or the like. By continuously measuring the components of the product sintered ore on the conveyor (on belt) being conveyed and performing online analysis, it is possible to sequentially obtain component concentration data of the product sintered ore. Here, continuous measurement means a form in which electromagnetic waves, neutrons, or the like are continuously irradiated to the analysis target to continuously obtain measured values. When the electromagnetic wave is a pulsed laser or the like, the time interval between pulses may be on the order of microseconds to seconds depending on the number of pulse repetitions. In addition, continuous measurements may be performed intermittently. There may be a finite rest period between the continuous measurements and the next continuous measurement. Such a rest period can be appropriately selected so that the desired control is possible. From another perspective, the continuous measurement of the present invention may be a form in which the analysis target moving by a conveying means such as a belt conveyor or pallet is measured in a non-contact manner without sampling.

[0025] For example, if a LIBS (Laser Induced Breakdown Spectroscopy) analyzer is used to measure and analyze the component concentrations of the finished sintered ore, the component concentration data of the finished sintered ore can be obtained by irradiating the finished sintered ore with a laser beam while it is being transported to a blast furnace facility and performing component analysis using laser induced breakdown spectroscopy. Here, before irradiating the finished sintered ore with the analytical laser beam, a pretreatment laser may be irradiated to remove surface deposits and / or moisture from the finished sintered ore. This pretreatment is a process of removing surface deposits and moisture from the finished sintered ore particles by so-called laser ablation.

[0026] The LIBS analysis device is equipped with the components necessary for measurement and analysis, such as a pre-processing laser light source and an analytical laser light source arranged in order in the conveying direction, a spectrometer (e.g., AvanSpec-ULS2048CL-EVO manufactured by Avantes) that detects the wavelengths and intensity of light contained in the emission caused by the analytical laser light, a processing unit, and a control device.The processing unit acquires measurement data regarding the emission generated from the finished sintered ore (data regarding the emission intensity at each wavelength) output from the spectrometer, and analyzes the component composition of the finished sintered ore using LIBS based on this measurement data.

[0027] Here, fine sintered ore particles of micron order size are attached to the surface of the product sintered ore that has been through the classification step S5. The sintered ore particles that are surface attachments have different component concentrations from the product sintered ore particles that are the lump part. When the product sintered ore is analyzed without pretreatment, the target of irradiation with the analysis laser light is biased toward the sintered ore particles that are surface attachments, and the mass ratio of the sintered ore particles that are surface attachments is extremely small compared to the product sintered ore particles that are the lump part, so that the analysis data is highly likely not to represent the component concentrations of the product sintered ore particles that are the lump part.

[0028] In addition, sintered ore may contain moisture due to water sprinkling to prevent dust during storage or transportation, or due to rainfall. When a sample containing moisture is irradiated with a laser, at least a part of the energy required for plasma generation, which is supplied from the irradiated laser light, is used for evaporating the moisture, etc., and there is a concern that the light emission from the sample will be significantly attenuated. Although it may be possible to partially correct the effect of moisture by further applying a method such as multivariate analysis, there is a concern that the reliability of the analysis results will also decrease because the analytical accuracy decreases as the emission intensity decreases.

[0029] Therefore, the above-mentioned pretreatment is performed before the irradiation of the analytical laser light, and the analytical laser light is irradiated to at least a part of the area irradiated with the laser light in the pretreatment to perform the analysis. With this configuration, the analytical laser light is irradiated to the product sintered ore particles, which are the lump parts, and even if the product sintered ore contains moisture, a decrease in the emission signal intensity can be suppressed, making it possible to accurately measure the component concentrations of the product sintered ore.

[0030] It is also preferable to measure the position of the analysis portion to be irradiated with the analysis laser light (e.g., height from the conveying surface of a conveying equipment such as a belt conveyor) by irradiating a position-measuring laser light before irradiating the analysis laser light after pretreatment, and to irradiate the analysis portion with the analysis laser light based on the measured position information. This makes it possible to identify the analysis position of the product sintered ore to be analyzed, and to more reliably focus the analysis laser light on the analysis portion (surface) of the product sintered ore particle to be analyzed. As a result, it becomes possible to measure the component concentrations of the product sintered ore with even greater accuracy.

[0031] (Components to be measured) In the present invention, the component to be measured by the component analyzer 1 is at least one of CaO, SiO2, Al2O3, MgO, and TiO2. SiO2, Al2O3, and MgO are components contained in gangue. When the basicity (CaO / SiO2) is high, the generation of calcium ferrite (CaO·Fe2O3)-based melt is promoted, and the generation of secondary hematite is suppressed. When the component concentration of SiO2 is high, the amount of melt generated increases, and the generation of secondary hematite is suppressed. When the component concentration of MgO is high, magnesioferrite (MgO·Fe2O3) is more likely to crystallize than calcium ferrite because Mg has a smaller ionic radius difference with Fe compared to Ca, and magnesioferrite crystallizes at high temperatures, resulting in the generation of secondary hematite being suppressed. On the other hand, there is no need to measure components among CaO, SiO2, Al2O3, MgO, and TiO2 that are known to have small concentration fluctuations. In the present invention, at least one of CaO, SiO2, Al2O3, MgO and TiO2 is measured, and the layer thickness of the raw material packed bed formed by charging the blended raw materials into the sintering machine is adjusted based on the component concentration data obtained by the measurement. The adjustment of the layer thickness of the raw material packed bed is described below.

[0032] (Adjusting the layer thickness of the raw material packed bed) In the present invention, the layer thickness of the raw material packed bed is controlled using the chemical composition of the product sinter measured on the belt based on the following formula (1) obtained by multiple regression analysis of the relationship between the chemical composition of the product sinter, the layer thickness of the raw material packed bed, and the RDI. Note that A1 to An and B1 are constants previously obtained by multiple regression analysis based on the operational performance. RDI = A1[X1] + A2[X2] + A3[X3] + ··· + An[Xn] + B1 (layer thickness) ··· Equation (1) [Xk]=Xk concentration k:1~n X: CaO, SiO2, Al2O3, MgO or TiO2 In addition, the constants A1 to An and B1 in formula (1) vary depending on the brand of raw material used and the individual difference of the sintering machine, so when applying the present invention, formula (1) may be updated as necessary. Formula (1) may further include a term such as basicity (CaO / SiO2). In addition, the correlation coefficient of multiple regression analysis may be more than 0.5. EXAMPLES

[0033] Regarding the adjustment of the layer thickness of the raw material packed bed, two experiments were carried out, an example of the invention and a comparative example. Granulated sinter raw material pseudo particles are charged onto the sinter machine pallet through a drum feeder and a cut-off chute from a surge hopper arranged on the sinter machine. A gate is provided to adjust the layer thickness after the raw material is cut off from the drum feeder, and the layer thickness of the raw material packed bed is controlled by adjusting the height of the gate. The layer thickness of the raw material packed bed is measured and managed by a laser level meter. In this example, a predetermined amount of product sintered ore is sampled from the blast furnace conveying line L1 every two hours, the RDI is measured, and the values ​​of constants A1 to A4 and B1 in the formula (1') described later are obtained by multiple regression analysis. The RDI is calculated by heating sintered ore with a particle size range of -20+16 mm to 550°C, reducing it for 30 minutes with a gas mixture of 30% CO and 70% N2, cooling it, rotating it 900 times in a small tumbler, and then sieving it through a 3 mm sieve, and expressing the percentage of particles 3 mm or less (JIS M 8720 (2009)).

[0034] (Example of the invention) In the invention example, the product sinter on the belt of the blast furnace conveying line L1 was continuously measured online by a LIBS analyzer, and the data was analyzed every 10 minutes, and the average value of the RDI calculated from formula (1') over one hour was calculated, and when the average value was +1% or more of the reference value, the height of the gate was adjusted so that the RDI calculated from formula (1') was equal to or less than the reference value, and the layer thickness of the raw material packed bed was adjusted, and the RDI value of the product sinter after this adjustment was investigated. In the LIBS analysis, a laser light source with pulse energy: 40 mJ, wavelength: 1064 nm, repetition frequency: 100 Hz, and pulse width: 7 ns was used. RDI = A1[CaO] + A2[SiO2] + A3[Al2O3] + A4[MgO] + B1(layer thickness (mm)) ··· formula (1´) [Xk]=Xk concentration (mass%)

[0035] (Comparative Example) In a comparative example, the RDI was calculated from the chemical composition of the finished sintered ore sampled from the blast furnace transport line L1 obtained every 6 hours using formula (1). When the calculated value was +1% or more of the reference value, the gate height was adjusted to adjust the layer thickness of the raw material packed bed so that the RDI was below the reference value, and the RDI value of the finished sintered ore after this adjustment was investigated.

[0036] In each of the invention examples and comparative examples, the RDI values ​​and standard deviations of the adjusted product sintered ore are shown in Table 1.

[0037] [Table 1]

[0038] As shown in Table 1, the RDI value in the example of the invention is lower than that in the comparative example, and the RDI variation is smaller than that in the comparative example. From this, it can be said that the example of the invention, which adjusts the layer thickness of the raw material packed bed by obtaining component concentration data of the product sintered ore almost in real time, improves the RDI and suppresses its variation, and can stably obtain the target RDI even if the chemical composition of the sintering raw material fluctuates.

[0039] Although the present invention has been described in detail above with reference to the drawings, it is of course not limited to the above-mentioned configurations and various modifications can be made without departing from the gist of the present invention. [Explanation of symbols]

[0040] S1: Raw material blending process, S2: Granulation process, S3: Sintering process, S4: Cooling / grinding process, S5: Classification process, L1: Blast furnace conveyance line, L2: Return ore conveyance line, 1: Component analysis device.

Claims

1. A mixed raw material containing multiple types of iron ore, auxiliary materials, and a coagulant is charged into a sintering machine; Sintering the charged blended raw materials to produce a sintered cake; The sintered cake is sieved into product sinter and return ore using a classification device, In the method for producing sintered ore, the sieved product sintered ore is transported to a blast furnace facility, Continuously measuring the concentration of at least one component of the product sintered ore being transported to the blast furnace facility; a layer thickness of a raw material packed bed formed by charging the blended raw materials into the sintering machine is adjusted based on the component concentration data obtained by the measurement.

2. The components to be measured are CaO, SiO 2 , Al 2 O 3 , MgO and TiO 2 The method for producing sintered ore according to claim 1, wherein the sintered ore is at least one of the above.

3. The method for producing sintered ore according to claim 1, wherein the layer thickness is adjusted so as to control the reduction disintegration index (RDI) of the product sintered ore within a predetermined range based on a prediction equation including the component concentration data and the layer thickness as explanatory variables, with the RDI being set as a response variable.

4. In the measurement, The method for producing sintered ore according to any one of claims 1 to 3, wherein the component concentration data is obtained by irradiating the product sintered ore being transported to the blast furnace facility with a laser beam and performing component analysis by laser induced breakdown spectroscopy.

Citation Information

Patent Citations

  • Method for manufacturing sintered ore

    JP2019173161A