Manufacturing method of secondary battery and secondary battery

The method uses an elastic press jig to form a flat and curved electrode body with controlled heating and adhesive strength, addressing uneven spacing and adhesion issues to prevent lithium precipitation and ensure effective electrolyte impregnation.

JP2024162047AActive Publication Date: 2024-11-21PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023077211
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

The existing electrode body forming apparatuses cause uneven spacing between positive and negative electrode plates in curved parts, leading to lithium precipitation and poor electrolyte impregnation due to strong adhesion and uneven pressing.

Method used

A method involving a press jig with elastic parts to form a flat and curved electrode body by sandwiching a wound body with elastic press surfaces, heating the curved parts to a controlled temperature, and ensuring appropriate adhesive strength between electrode plates and separators.

Benefits of technology

This method suppresses lithium precipitation and maintains good electrolyte impregnation by ensuring uniform pressing and controlled adhesive strength, particularly in large-sized electrode bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162047000001_ABST
    Figure 2024162047000001_ABST
Patent Text Reader

Abstract

To suppress deposition of a lithium in an electrode body inner part while preferably holding an impregnation property of an electrolyte against an electrode body.SOLUTION: In a step of manufacturing an electrode body 20 by performing a press processing of a winding body in a flat shape, the winding body is nipped by a first fixture 3 having a first press surface F1 containing a first elastic part 7 and a second fixture 4 that includes a second press surface F2 containing a second elastic part 8. The winding body is depressed by the first press surface F1 and the second press surface F2 while elastically deforming at least one part of the first press surface F1 and the second press surface F2. In the step of manufacturing the electrode body 20 by performing the press processing of the winding body, a flat part 22, a first curvature part 24, and a second curvature part 25 are formed to the electrode body 20. In the step of manufacturing the electrode body 20 by performing the press processing of the winding body, each of the first curvature part 24 and the second curvature part 25 are heated to a temperature that is higher than a room temperature via at least one of the first press surface F1 and the second press surface F2.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present technology relates to a manufacturing method of a secondary battery and a secondary battery. [Background technology]

[0002] A prior art document disclosing the configuration of an electrode body forming device is JP 2013-084445 A (Patent Document 1). The electrode body forming device described in Patent Document 1 includes a first press head and a second press head. The first press head and the second press head sandwich and press the electrode body, which is wound into a hollow cylindrical shape, from both sides in the diameter direction, thereby forming a flat portion and a curved portion on the outer peripheral surface of the electrode body and forming the electrode body into a flat shape. The first press head and the second press head are provided with a pressing surface and an R pressing surface. The pressing surface corresponds to the flat portion of the outer peripheral surface of the electrode body when pressed. The R pressing surfaces are located at both ends of the pressing surface, and at least when pressed, protrude from the pressing surface in the height direction and press the curved portion of the outer peripheral surface of the electrode body.

[0003] Furthermore, a prior art document similar to Patent Document 1 is JP 2022-050088 A (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-084445 A [Patent Document 2] Patent Publication No. 2022-050088 Summary of the Invention [Problem to be solved by the invention]

[0005] In the electrode body forming device described in Patent Document 1, the curved part of the electrode body is formed by making the wound body follow the jig shape of the device, so that the distance between the positive and negative plates at the curved part may become uneven. This may cause lithium to precipitate on the negative plate. In addition, when the curved part of the electrode body is strongly pressed to adjust the distance between the positive and negative plates, the positive and negative plates and the separator at the inner part of the stack are strongly bonded, which may deteriorate the impregnation of the electrolyte into the electrode body.

[0006] The present technology has been made to solve the above-mentioned problems, and aims to provide a method for manufacturing a secondary battery and a secondary battery that can suppress lithium precipitation inside the electrode body while maintaining good impregnation of the electrode body with an electrolyte. [Means for solving the problem]

[0007] The present technology provides the following method for producing a secondary battery. [1] preparing a wound body in which a separator is sandwiched between a positive electrode plate and a negative electrode plate, and the positive electrode plate, the negative electrode plate, and the separator are wound around a winding axis that is aligned in a first direction; a step of sandwiching the wound body between a first jig having a first press surface including a first elastic portion and a second jig having a second press surface including a second elastic portion in a second direction perpendicular to the first direction, and pressing the wound body with the first press surface and the second press surface while elastically deforming at least a portion of the first press surface and the second press surface to produce an electrode body by pressing the wound body into a flat shape; and housing the electrode body and the electrolyte in a case. In a step of producing the electrode body by pressing the wound body, a flat portion is formed in the electrode body, the flat portion being located on a central side in a third direction perpendicular to the first direction and the second direction and having a flat outer surface, a first curved portion is located on one end side of the flat portion in the third direction and having a curved outer surface, and a second curved portion is located on the other end side of the flat portion in the third direction and having a curved outer surface, a step of pressing the wound body to produce the electrode body, wherein each of the first curved portion and the second curved portion is heated to a temperature higher than room temperature via at least one of the first press surface and the second press surface. Here, room temperature refers to the temperature of the surrounding atmosphere when the electrode body is pressed. [2] The method for producing a secondary battery according to [1], wherein the temperature higher than room temperature is 50° C. or higher and 110° C. or lower. [3] The method for manufacturing a secondary battery according to [1] or [2], wherein the first press surface and the second press surface abut against the outer surface of 50% or more of an area that will become the first curved portion and the second curved portion after the wound body is pressed. [4] The method for manufacturing a secondary battery according to any one of [1] to [3], wherein each of the first elastic portion and the second elastic portion is made of a porous material.

[0008] The present technology provides the following secondary battery. [5] an electrode assembly in which a separator is sandwiched between a positive electrode plate and a negative electrode plate, and the positive electrode plate, the negative electrode plate, and the separator are wound around a winding axis that is aligned in a first direction; A case is provided to accommodate the electrode assembly and an electrolyte solution, the electrode body is flat and has a short side in a second direction perpendicular to the first direction and a long side in a third direction perpendicular to the first direction and the second direction; The electrode body is a flat portion located on the central side in the third direction and having a flat outer surface; a first curved portion located on one end side of the flat portion in the third direction and having a curved outer surface; a second curved portion located on the other end side of the flat portion in the third direction and having a curved outer surface, In the first curved portion, an adhesive strength between a surface of each of the positive electrode plates in the stacked positive electrode plates from the outermost layer to the third layer counting from the outermost layer and each of the separators adjacent to the outer periphery side is 1.0 N / m or more and 1.9 N / m or less, a secondary battery, in which in the first curved portion, an adhesive strength between a surface of the positive plate located on the outer periphery side for 50% of the total number of stacked positive plates, counting from the innermost positive plate among the stacked positive plates, and the separator adjacent to that outer periphery side is 0.6 N / m or more and 1.5 N / m or less. Note that "each of the positive electrode plates up to the third layer counting from the positive electrode plate located at the outermost periphery among the positive electrode plates" refers to each of the positive electrode plates located in the first layer at the outermost periphery, the second layer one layer inward from the first layer, and the third layer one layer inward from the second layer. In addition, when the total number of laminated positive electrode plates is an even number, "50% of the total number of laminated plates" refers to the total number of laminated plates divided in half. Furthermore, when the total number of laminations of positive electrode plates is an odd number, "50% of the total number of laminations" means the total number of laminations divided in half and rounded off to the nearest whole number. [6] The secondary battery according to [5], wherein in the flat portion, an adhesive strength between a surface of each of the positive plate layers up to the third layer counting from the outermost positive plate among the stacked positive plate layers and each of the separators adjacent to the outer periphery side of the positive plate layers is 1.5 N / m or more and 1.9 N / m or less. [7] The secondary battery according to [5] or [6], wherein in the flat portion, an adhesive strength between a surface of the positive plate located on the outer periphery side of 50% of the total number of stacked positive plate layers, counting from the innermost positive plate among the stacked positive plate layers, and the separator adjacent to that outer periphery side is 1.5 N / m or more and 1.9 N / m or less. Effect of the Invention

[0009] According to the present technology, it is possible to suppress the deposition of lithium inside the electrode body while maintaining good impregnation of the electrode body with an electrolyte. [Brief description of the drawings]

[0010] [Figure 1] 1 is a perspective view showing a configuration of a secondary battery according to an embodiment of the present technology; [Diagram 2] 1 is a perspective view showing an internal configuration of a secondary battery according to an embodiment of the present technology; [Diagram 3] 1 is a perspective view showing a configuration of an electrode assembly and a current collector included in a secondary battery according to an embodiment of the present technology; [Figure 4] 4 is a cross-sectional view of the electrode body of FIG. 3 as seen from the direction of the arrows IV-IV. [Diagram 5] 2 is a flowchart showing a method for manufacturing a secondary battery according to an embodiment of the present technology. [Figure 6] FIG. 2 is a schematic diagram showing a state before the wound body is pressed. [Figure 7] 10 is a schematic diagram showing a state in which an electrode body is produced by pressing a wound body. FIG. [Figure 8] FIG. 4 is a schematic diagram showing measurement positions for adhesive strength between a positive electrode plate and a separator in an electrode assembly. [Figure 9] FIG. 4 is a schematic diagram showing a method for measuring the adhesive strength between a positive electrode plate and a separator in an electrode assembly. [Figure 10] 10 is a schematic diagram showing a state in which an electrode body is produced by pressing a wound body according to a comparative example. FIG. [Figure 11] FIG. 4 is a cross-sectional view showing the configuration of an electrode body included in a secondary battery according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present technology will be described. Note that the same or corresponding parts are denoted by the same reference characters, and description thereof will not be repeated.

[0012] In the embodiments described below, when referring to the number, amount, etc., the scope of the present technology is not necessarily limited to the number, amount, etc., unless otherwise specified. In addition, in the following embodiments, each component is not necessarily essential to the present technology, unless otherwise specified. In addition, the present technology is not necessarily limited to those that achieve all of the effects and advantages mentioned in the present embodiment.

[0013] In this specification, the words "comprise", "include" and "have" are open-ended, i.e., when a certain configuration is included, other configurations may or may not be included.

[0014] Furthermore, when geometric terms and terms expressing positional and directional relationships, such as "parallel," "orthogonal," "45° diagonal," "coaxial," and "along" are used in this specification, these terms allow for manufacturing errors and slight variations. When terms expressing relative positional relationships, such as "upper side" and "lower side," are used in this specification, these terms are used to indicate relative positional relationships in one state, and the relative positional relationships can be inverted or rotated to any angle depending on the installation direction of each mechanism (for example, by turning the entire mechanism upside down).

[0015] In this specification, the term "secondary battery" is not limited to lithium ion batteries, but may include other secondary batteries such as nickel-metal hydride batteries and sodium ion batteries. In this specification, the term "electrode" may collectively refer to a positive electrode and a negative electrode.

[0016] In addition, a "battery module" including a secondary battery can be mounted on a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), an electric vehicle (BEV), etc. However, the use of the "battery module" is not limited to being mounted on a vehicle.

[0017] In the drawings, the direction along the winding axis of the electrode body of the secondary battery is the X direction as a first direction, the Y direction is the short side direction of the electrode body that is perpendicular to the first direction and seen from the first direction as a second direction, and the Z direction is the long side direction of the electrode body that is perpendicular to the first direction and seen from the first direction as a third direction. In addition, in order to make the invention easier to understand, the dimensions of each component in the drawings are sometimes shown differently from the actual dimensions.

[0018] Fig. 1 is a perspective view showing a configuration of a secondary battery according to an embodiment of the present technology. Fig. 2 is a perspective view showing an internal configuration of a secondary battery according to an embodiment of the present technology. Fig. 3 is a perspective view showing a configuration of an electrode body and a current collector included in the secondary battery according to an embodiment of the present technology.

[0019] 1 to 3, the secondary battery 1 includes a case 10, an electrode assembly 20, a positive electrode current collector 30, a negative electrode current collector 40, a positive electrode terminal 50, a negative electrode terminal 60, a positive electrode external conductive member 70, a negative electrode external conductive member 80, and an insulating sheet (not shown).

[0020] The case 10 includes an exterior body 100 and a sealing plate 110 .

[0021] The exterior body 100 has a bottomed rectangular cylindrical shape having an opening 101. The exterior body 100 is made of metal. Specifically, the exterior body 100 is made of aluminum, an aluminum alloy, iron, an iron alloy, or the like.

[0022] Exterior body 100 has a bottom 102, a pair of first side walls 103a, 103b, and a pair of second side walls 104a, 104b.

[0023] The bottom 102 faces the opening 101. The pair of first side walls 103a, 103b are erected from the edge of the bottom 102 and face each other in parallel. The pair of second side walls 104a, 104b are erected from the edge of the bottom 102 and face each other in parallel. The pair of second side walls 104a, 104b connect the first side walls 103a, 103b to each other. The area of ​​each of the pair of first side walls 103a, 103b is larger than the area of ​​each of the pair of second side walls 104a, 104b.

[0024] Sealing plate 110 seals opening 101 of exterior body 100. Sealing plate 110 is made of, for example, aluminum, an aluminum alloy, iron, or an iron alloy.

[0025] The sealing plate 110 is provided with an electrolyte injection hole 111. The electrolyte injection hole 111 is sealed with a sealing member 112. The sealing plate 110 is provided with a gas exhaust valve 113. The gas exhaust valve 113 breaks when the pressure inside the case 10 reaches or exceeds a predetermined value, and exhausts gas inside the case 10 to the outside.

[0026] The electrode assembly 20 in this embodiment is a flat-shaped electrode assembly having a positive electrode plate, a negative electrode plate, and a separator, which will be described later. Specifically, the electrode assembly 20 is a wound electrode assembly in which a strip-shaped positive electrode plate and a strip-shaped negative electrode plate are wound together with a strip-shaped separator interposed therebetween.

[0027] The thickness T of the electrode body 20 is, for example, 12 mm. The width W of the electrode body 20 is, for example, 290 mm. The height H of the electrode body is, for example, 95 mm. The width of the positive electrode plate in the electrode body 20 is preferably 140 mm or more and 500 mm or less, and more preferably 280 mm or more and 400 mm or less.

[0028] 1, case 10 houses electrode bodies 20. Case 10 in the present embodiment houses three electrode bodies 20. Electrode bodies 20 are housed in exterior body 100 with winding axis A1 of electrode body 20 parallel to bottom 102 and oriented along the longitudinal direction of case 10. The number of electrode bodies 20 arranged in exterior body 100 is not limited to three.

[0029] The case 10 also contains an electrolyte. The electrolyte is a liquid in which a lithium salt is dissolved in a non-aqueous solvent.

[0030] In the electrode body 20, a tab portion 21 is provided on at least one of the positive electrode plate and the negative electrode plate, and extends to the side of the electrode body 20. In the electrode body 20 in this embodiment, a positive electrode tab group 201 including multiple positive electrode tabs is provided as one tab portion 21 at one end of the electrode body 20 in the direction in which the winding axis A1 of the electrode body 20 extends. A negative electrode tab group 211 including multiple negative electrode tabs is provided as the other tab portion 21 at the other end of the electrode body 20 in the direction in which the winding axis A1 of the electrode body 20 extends.

[0031] It is preferable that the electrode body 20 is arranged within the exterior body 100 with an insulating sheet sandwiched between them, with one second side wall 104a facing the positive electrode tab group 201 and the other second side wall 104b facing the negative electrode tab group 211.

[0032] The positive electrode current collector 30 has a plate-like shape. The positive electrode current collector 30 is connected to one of the tab portions 21. The positive electrode current collector 30 in this embodiment is connected to a positive electrode tab group 201. The positive electrode current collector 30 is preferably made of metal, and more preferably made of aluminum or an aluminum alloy.

[0033] The negative electrode current collector 40 has a plate-like shape. The negative electrode current collector 40 is connected to the other tab portion 21. The negative electrode current collector 40 in the present embodiment is connected to a negative electrode tab group 211. The negative electrode current collector 40 is preferably made of metal, and more preferably made of copper or a copper alloy.

[0034] A positive electrode terminal 50 and a negative electrode terminal 60 are attached to the sealing plate 110. The positive electrode terminal 50 is electrically connected to a positive electrode tab group 201 in each of the plurality of electrode bodies 20 via a positive electrode current collector 30. A positive electrode external conductive member 70 is connected to the positive electrode terminal 50. It is to be noted that the secondary battery 1 does not necessarily need to include the positive electrode external conductive member 70.

[0035] Each of the positive electrode terminal 50 and the positive electrode external conductive member 70 is preferably made of a metal, and more preferably made of aluminum or an aluminum alloy.

[0036] The negative electrode terminal 60 is electrically connected to the negative electrode tab group 211 in each of the plurality of electrode bodies 20 via the negative electrode current collector 40. A negative electrode external conductive member 80 is connected to the negative electrode terminal 60. It is to be noted that the secondary battery 1 does not necessarily have to include the negative electrode external conductive member 80.

[0037] The negative electrode terminal 60 is preferably made of a metal, more preferably made of copper or a copper alloy. The negative electrode external conductive member 80 is preferably made of a metal, more preferably made of aluminum or an aluminum alloy. Note that the negative electrode terminal 60 may have a region connected to the negative electrode current collector 40 made of copper or a copper alloy, and a region protruding outward from the sealing plate 110 made of aluminum or an aluminum alloy.

[0038] Fig. 4 is a cross-sectional view of the electrode assembly as viewed from the direction of the arrows IV-IV in Fig. 3. As shown in Fig. 4, the electrode assembly 20 in this embodiment includes a positive electrode plate 200, a negative electrode plate 210, and a separator 220.

[0039] The positive electrode plate 200 is manufactured by processing a positive electrode original plate. The positive electrode original plate includes a positive electrode core, a positive electrode active material layer, and a positive electrode protective layer. The positive electrode core is an aluminum foil or an aluminum alloy foil.

[0040] A positive electrode active material layer is formed on the positive electrode core except for one end of both sides. The positive electrode active material layer is preferably a lithium transition metal composite oxide layer. The transition metal preferably contains at least nickel. The positive electrode active material layer is formed on the positive electrode core by applying a positive electrode active material layer slurry with a die coater.

[0041] The positive electrode active material layer slurry is prepared by kneading lithium nickel cobalt manganese composite oxide as the positive electrode active material, polyvinylidene fluoride (PVDF) as a binder, a carbon material as a conductive material, and N-methyl-2-pyrrolidone (NMP) as a dispersion medium, so that the mass ratio of lithium nickel cobalt manganese composite oxide:PVdF:carbon material is 97.5:1:1.5.

[0042] The positive electrode protective layer is formed on one end of the positive electrode active material layer in the width direction while being in contact with the positive electrode core by applying a positive electrode protective layer slurry by a die coater.

[0043] The positive electrode protective layer slurry is prepared by kneading alumina powder, a carbon material as a conductive material, PVdF as a binder, and NMP as a dispersion medium so that the mass ratio of alumina powder:carbon material:PVdF is 83:3:14.

[0044] The positive electrode core coated with the positive electrode active material layer slurry and the positive electrode protective layer slurry is dried, and the NMP contained in the positive electrode active material layer slurry and the positive electrode protective layer slurry is removed. This forms a positive electrode active material layer and a positive electrode protective layer. Furthermore, the positive electrode active material layer is compressed to obtain a positive electrode original plate including the positive electrode core, the positive electrode active material layer, and the positive electrode protective layer. The positive electrode original plate is cut into a predetermined shape to obtain a positive electrode plate. The positive electrode original plate can be cut by laser processing using energy beam irradiation, die processing, cutter processing, or the like.

[0045] The thickness of the positive electrode plate 200 is preferably 5 μm or more and 30 μm or less, and more preferably 8 μm or more and 20 μm or less.

[0046] The number of layers of the positive electrode plate 200 is preferably 10 or more, more preferably 20 or more, and even more preferably 30 or more. The number of layers of the positive electrode plate 200 is preferably 150 or less, and more preferably 100 or less. In this embodiment, the number of layers of the positive electrode plate 200 is, for example, 33 layers.

[0047] The negative electrode plate 210 is manufactured by processing a negative electrode original plate. The negative electrode original plate includes a negative electrode core and a negative electrode active material layer. The negative electrode core is a copper foil or a copper alloy foil.

[0048] A negative electrode active material layer is formed on both sides of the negative electrode core except for one end portion by applying a negative electrode active material layer slurry with a die coater.

[0049] The negative electrode active material layer slurry is prepared by kneading graphite or a silicon-containing compound as the negative electrode active material, styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) as binders, and water as a dispersion medium so that the mass ratio of graphite:SBR:CMC is 98:1:1.

[0050] The negative electrode core coated with the negative electrode active material layer slurry is dried to remove water contained in the negative electrode active material layer slurry. This forms a negative electrode active material layer. The negative electrode active material layer is then compressed to obtain a negative electrode master plate including the negative electrode core and the negative electrode active material layer. The negative electrode master plate is cut into a predetermined shape to obtain a negative electrode plate. The negative electrode master plate can be cut by laser processing using energy beam irradiation, die processing, cutter processing, or the like.

[0051] The thickness of the negative electrode plate 210 is preferably 5 μm or more and 30 μm or less, and more preferably 8 μm or more and 20 μm or less.

[0052] The number of layers of the negative electrode plate is preferably 10 or more, more preferably 20 or more, and even more preferably 30 or more. In the present embodiment, the number of layers of the negative electrode plate is, for example, 35.

[0053] The separator 220 is provided to insulate the positive electrode plate 200 from the negative electrode plate 210. The separator 220 preferably includes a base layer and a functional layer. The base layer is preferably made of polyethylene or polyolefin. The base layer is preferably a microporous film. Note that the base layer is not limited to being made of polyethylene or polyolefin, and may be made of other resins.

[0054] The functional layer is preferably formed on at least one surface of the base material layer. The functional layer is, for example, a heat-resistant layer or an adhesive layer. The separator 220 in this embodiment preferably has adhesive layers on both surfaces of the base material layer.

[0055] The adhesive layer is, for example, an acrylic adhesive layer. The adhesive layer is arranged on the entire surface of the base layer in a dot or stripe pattern. The adhesive layer is preferably composed of a layer containing PVDF. The PVDF may be arranged in the adhesive layer in a mesh pattern. The adhesive layer may contain ceramic particles such as alumina.

[0056] Separator 220 may have a configuration in which only an adhesive layer is arranged on the surface of the base material layer, a configuration in which a heat-resistant layer and an adhesive layer are arranged as multiple layers, or a configuration in which a single layer having heat-resistant and adhesive functions is arranged.

[0057] The thickness of the separator 220 is, for example, 16 μm. The thickness of the base layer is, for example, 12 μm. The thickness of the adhesive layer as a functional layer is, for example, 2 μm for a single layer located on one side of the base layer. Note that the thickness of the separator 220 is not limited as long as it can insulate the positive electrode plate 200 and the negative electrode plate 210.

[0058] The separators 220 are disposed at the innermost and outermost peripheries between the positive electrode plates 200 and the negative electrode plates 210. The number of layers of the separators 220 in this embodiment is, for example, 78 layers.

[0059] The electrode body 20 has a separator 220 sandwiched between a positive electrode plate 200 and a negative electrode plate 210. In the electrode body 20, the positive electrode plate 200, the negative electrode plate 210, and the separator 220 are wound around a winding axis A1 along a first direction (X direction).

[0060] The electrode body 20 has a short side in a second direction (Y direction) perpendicular to the first direction (X direction). The electrode body 20 also has a long side in a third direction (Z direction) perpendicular to the first direction (X direction) and the second direction (Y direction). That is, the electrode body 20 is flattened when viewed from the first direction (X direction).

[0061] The electrode body 20 includes a flat portion 22 and a curved portion 23. The flat portion 22 has one flat portion 22a and the other flat portion 22b on both sides in the second direction (Y direction).

[0062] The flat portion 22 is located on the central side in the third direction (Z direction). The flat portion 22 has a flat outer surface. Note that the "flat" of the flat portion 22 does not only mean that it is on the same plane. The "flat" includes a surface shape including steps at the winding end ends of the positive electrode plate 200, the negative electrode plate 210, and the separator 220, and steps such as the winding stop tape of the electrode body 20.

[0063] The curved portion 23 has a first curved portion 24 and a second curved portion 25. The first curved portion 24 is located on one end side of the flat portion 22 in the third direction (Z direction). The first curved portion 24 has a curved outer surface. The second curved portion 25 is located on the other end side of the flat portion 22 in the third direction (Z direction). The second curved portion 25 has a curved outer surface.

[0064] The positive electrode plate 200 and the separator 220 are pressure-bonded to each other at the flat portion 22 and the curved portion 23. The negative electrode plate 210 and the separator 220 are also pressure-bonded to each other at the flat portion 22 and the curved portion 23. This ensures that there is no gap between the positive electrode plate 200 and the separator 220, and between the negative electrode plate 210 and the separator 220, and that there is no gap between the positive electrode plate 200 and the separator 220.

[0065] Hereinafter, a method for manufacturing a secondary battery according to an embodiment of the present technology will be described. Fig. 5 is a flowchart showing a method for manufacturing a secondary battery according to an embodiment of the present technology.

[0066] As shown in FIG. 5, in the method for manufacturing the secondary battery 1 according to the present embodiment, first, a wound body 20A is prepared in which a separator 220 is sandwiched between a positive electrode plate 200 and a negative electrode plate 210, and the positive electrode plate 200, the negative electrode plate 210, and the separator 220 are wound around a winding axis A1 along a first direction (X direction) (step S1).

[0067] Next, the wound body 20A is pressed while being heated to form a flattened shape, thereby producing the electrode body 20 (step S2). Details of this step will be described later.

[0068] Next, the electrode body 20 and the electrolyte are housed in a case (step S3). The electrode body 20 is placed in a bag- or box-shaped insulating sheet. The electrode body 20 covered with the insulating sheet is inserted into the exterior body 100. As a result, the electrode body 20 is housed in the case 10.

[0069] Next, the case 10 is sealed (step S4). The sealing plate 110 is joined to the opening 101 of the exterior body 100 by laser welding or the like.

[0070] Next, an electrolyte is injected into the case 10 (step S5). A non-aqueous electrolyte is injected through an electrolyte injection hole 111 provided in the sealing plate 110, and the electrolyte injection hole 111 is sealed with a sealing member 112. In this way, the secondary battery 1 is completed.

[0071] Hereinafter, the press working of the electrode body 20 according to an embodiment of the present technology will be described in detail. Fig. 6 is a schematic diagram showing a state before the wound body is pressed. Fig. 7 is a schematic diagram showing a state in which the wound body is pressed to produce the electrode body.

[0072] As shown in FIGS. 6 and 7, the wound body 20A is pressed by a press jig 2 to form the electrode body 20.

[0073] The wound body 20A may have a cylindrical shape with a substantially circular cross section as viewed from the first direction (X direction) before being pressed, or may have an elliptical cross section. When the wound body 20A has an elliptical cross section, the wound body 20A is formed into an elliptical shape by performing another press process in advance before being pressed.

[0074] The press jig 2 is provided in a press machine (not shown). The press jig 2 is provided with a heater (not shown). The press jig 2 includes a first jig 3 and a second jig 4. The first jig 3 is provided facing a portion of the wound body 20A where one flat portion 22a is to be formed. The second jig 4 is provided facing a portion of the wound body 20A where the other flat portion 22b is to be formed.

[0075] The first jig 3 has a first head portion 5. The first head portion 5 has a first press surface F1 including a first elastic portion 7. The second jig 4 has a second head portion 6. The second head portion 6 has a second press surface F2 including a second elastic portion 8.

[0076] Each of the first elastic portion 7 and the second elastic portion 8 is made of a porous material. In this embodiment, each of the first elastic portion 7 and the second elastic portion 8 is made of foamed silicone. Each of the first elastic portion 7 and the second elastic portion 8 may be made of a thermosetting elastomer such as natural rubber, urethane rubber, silicone rubber, or fluororubber. Each of the first elastic portion 7 and the second elastic portion 8 is preferably one that undergoes large elastic deformation during press processing.

[0077] Each of the first elastic portion 7 and the second elastic portion 8 preferably has a thickness for shaping the electrode body 20 in order to press the wound body 20A while elastically deforming. The thickness of each of the first elastic portion 7 and the second elastic portion 8 in the second direction (Y direction) is, for example, preferably ½ or more, and more preferably ⅔ or more, of the thickness of the electrode body 20 in the short side direction.

[0078] When the wound body 20A is pressed, the wound body 20A is sandwiched between a first jig 3 and a second jig 4 in a second direction (Y direction) perpendicular to the first direction (X direction). The wound body 20A is pressed by the first press surface F1 and the second press surface F2 while elastically deforming at least a part of the first press surface F1 and the second press surface F2 to produce the electrode body 20. In this embodiment, the wound body 20A is pressed by the first press surface F1 and the second press surface F2 while elastically deforming both the first press surface F1 and the second press surface F2.

[0079] In the electrode body 20, the first pressed surface F1 and the second pressed surface F2 abut against 50% or more of the outer surface of the region that will become the first curved portion 24 and the second curved portion 25 after the wound body 20A is pressed. In the present embodiment, the first pressed surface F1 and the second pressed surface F2 abut against the entire outer surface of the region that will become the first curved portion 24 and the second curved portion 25.

[0080] By pressing the wound body 20A into a flat shape, the electrode body 20 produced has a flat portion 22 and a first curved portion 24 and a second curved portion 25 which are curved portions 23. The positive electrode plate 200 and the separator 220 in each of the flat portion 22 and the curved portion 23 are pressed and bonded by the press jig 2. The negative electrode plate 210 and the separator 220 in each of the flat portion 22 and the curved portion 23 are also pressed and bonded by the press jig 2.

[0081] The pressing pressure of the wound body 20A is preferably, for example, 50 kN or more, more preferably 80 kN or more, and even more preferably 90 kN or more. The pressing pressure of the wound body 20A is preferably, for example, 200 kN or less, and more preferably 150 kN or less. The pressing pressure of the wound body 20A in this embodiment is, for example, 110 kN.

[0082] When the wound body 20A is pressed to produce the electrode body 20, each of the first curved portion 24 and the second curved portion 25 is heated to a temperature higher than room temperature. Specifically, when the wound body 20A is pressed to produce the electrode body 20, each of the first curved portion 24 and the second curved portion 25 is heated to a temperature higher than room temperature via at least one of the first press surface F1 and the second press surface F2. In this embodiment, each of the first curved portion 24 and the second curved portion 25 is heated to a temperature higher than room temperature via both the first press surface F1 and the second press surface F2 by a heater built into the press jig 2.

[0083] Room temperature refers to the ambient temperature when press working is performed on electrode body 20. The temperature higher than room temperature is, for example, preferably 50° C. or higher and 110° C. or lower, more preferably 60° C. or higher and 100° C. or lower, and even more preferably 70° C. or higher and 90° C. or lower. The heating temperature of each of first curved portion 24 and second curved portion 25 in this embodiment is, for example, 70° C.

[0084] The heating time of each of the first bending portion 24 and the second bending portion 25 is preferably, for example, 1 second or more and 30 seconds or less, more preferably, 3 seconds or more and 20 seconds or less, and further preferably, 5 seconds or more and 10 seconds or less. The heating time of each of the first bending portion 24 and the second bending portion 25 in this embodiment is, for example, 10 seconds.

[0085] 7, the flat portion 22 is formed by pressing simultaneously with the curved portion 23. In this embodiment, the flat portion 22 is also heated during the press working, but the flat portion 22 does not necessarily have to be heated during the press working.

[0086] The adhesive strength between the positive electrode plate 200 and the separator 220 inside the electrode assembly 20 will be described below. Fig. 8 is a schematic diagram showing the measurement positions for the adhesive strength between the positive electrode plate and the separator in the electrode assembly. In Fig. 8, only the positive electrode plate of the electrode assembly is shown.

[0087] One of the characteristics required for the electrode body 20 is the adhesive strength between the positive electrode plate 200 or the negative electrode plate 210 and the separator 220. The positive electrode plate 200 or the negative electrode plate 210 and the separator 220 are bonded by pressure applied during press processing. The adhesive strength increases as the pressure applied during press processing increases. The adhesive strength also increases when heated.

[0088] Even if the electrode body 20 is pressed so as not to form a gap between the positive electrode plate 200 or the negative electrode plate 210 and the separator 220 at the curved portion 23 as described above, if the adhesive strength is too high, the impregnation of the electrolyte into the inside of the electrode body 20 decreases. For this reason, it is desirable for the electrode body 20 to have an adhesive strength between the positive electrode plate 200 or the negative electrode plate 210 and the separator 220 within an appropriate range.

[0089] The required adhesive strength is desirably measured on the outer and inner sides of the electrode body 20, since the pressing forces applied to the outer and inner sides of the electrode body 20 during press working are different.

[0090] Therefore, in the electrode body 20 of the present embodiment, the adhesive strength is specified at the following four locations. The four locations are a first outer location 240, a first inner location 241, a second outer location 250, and a second inner location 251.

[0091] The first outer portion 240 is each of the positive electrode plates 200 in the first curved portion 24, counting from the positive electrode plate 200 located at the outermost periphery among the stacked positive electrode plates 200. "Each of the positive electrode plates in the first to third layers counting from the positive electrode plate located at the outermost periphery" refers to each of the positive electrode plates located in the first layer at the outermost periphery, the second layer one layer inward from the first layer, and the third layer one layer inward from the second layer.

[0092] The first outer portion 240 is located outside the stacked electrode body 20 of the first curved portion 24. In the first outer portion 240 of the first curved portion 24, the adhesive strength between the surface of each of the positive electrode plates 200 from the positive electrode plate 200 located at the outermost periphery to the third layer among the stacked positive electrode plates 200 and each separator 220 adjacent to the outer periphery side is 1.0 N / m or more and 1.9 N / m or less. The adhesive strength is more preferably 1.5 N / m or more and 1.9 N / m or less. If the adhesive strength is less than 1.0 N / m, lithium may be precipitated. If the adhesive strength is 1.9 N / m or more, the impregnation of the electrolyte into the electrode body 20 may be deteriorated.

[0093] It is preferable that the adhesive strength between the surface of the positive electrode plate 200 at the first outer location 240 of the first curved portion 24 and the separator 220 adjacent to its outer periphery is similar in the portion corresponding to the first outer location of the second curved portion 25.

[0094] The first inner portion 241 is located inside the stacked electrode body 20 of the first curved portion 24. In the first inner portion 241 of the first curved portion 24, the adhesive strength between the surface of the positive electrode plate 200 located on the outer periphery side of 50% of the total number of stacked positive electrode plates 200 counting from the positive electrode plate 200 located at the innermost circumference of the stacked positive electrode plates 200 and the separator 220 adjacent to the outer periphery side is 0.6 N / m or more and 1.5 N / m or less. If the adhesive strength is 1.5 N / m or more, the impregnation of the electrolyte into the electrode body 20 may deteriorate. If the total number of stacked positive electrode plates is an even number, the "50% of the total number of stacked positive electrode plates" refers to the number of sheets obtained by dividing the total number of stacked positive electrode plates in half. If the total number of stacked positive electrode plates is an odd number, the "50% of the total number of stacked positive electrode plates" refers to the number of sheets obtained by dividing the total number of stacked positive electrode plates in half and rounding off the decimal point.

[0095] It is preferable that the adhesive strength between the surface of the positive electrode plate 200 at the first inner location 241 of the first curved portion 24 and the separator 220 adjacent to its outer periphery is similar in the portion corresponding to the first inner location of the second curved portion 25.

[0096] The second outer portion 250 is located outside the stacked electrode body 20 of the flat portion 22. In the second outer portion 250 of the flat portion 22, the adhesive strength between the surface of each of the positive electrode plates 200 from the positive electrode plate 200 located at the outermost periphery among the stacked positive electrode plates 200 to the third layer counting from the positive electrode plate 200 located at the outermost periphery and each separator 220 adjacent to the outer periphery side is 1.5 N / m or more and 1.9 N / m or less.

[0097] The second inner portion 251 is located inside the stacked electrode body 20 of the flat portion 22. In the second inner portion 251 of the flat portion 22, the adhesive strength between the surface of the positive electrode plate 200 on the outer periphery side for 50% of the total number of stacked positive electrode plates 200, counting from the positive electrode plate 200 located at the innermost periphery among the stacked positive electrode plates 200, and the separator 220 adjacent to that outer periphery side is 1.5 N / m or more and 1.9 N / m or less.

[0098] FIG. 9 is a schematic diagram showing a method for measuring the adhesive strength between the positive electrode plate and the separator in the electrode assembly.

[0099] When measuring the adhesive strength between the positive electrode plate 200 and the separator 220 in the electrode assembly 20, the electrode assembly 20 is measured after it has reached room temperature after pressing. The electrode assembly 20 is disassembled in a state in which the positive electrode plate 200 and the separator 220 are attached to each other.

[0100] A test piece is obtained by cutting a portion from the portion where the positive electrode plate 200 and the separator 220 are stuck to each other and laminated. The test piece of the curved portion 23 is cut to a size of 70 mm in the winding axis direction and 8 mm in the direction perpendicular to the winding axis. The test piece of the flat portion 22 is cut to a size of 70 mm in the winding axis direction and 20 mm in the direction perpendicular to the winding axis.

[0101] Thereafter, the test piece is fixed to a plate (not shown) with double-sided tape so that the positive electrode plate 200 is in contact with the plate. The separator 220 is pulled in a direction perpendicular to the direction in which the positive electrode plate 200 extends. During the test, the plate is moved so that the direction in which the separator 220 is peeled off is always vertical. The adhesive strength is measured when the separator 220 is peeled off at a speed of 50 mm / min.

[0102] A method for manufacturing a secondary battery according to a comparative example will be described below. The method for manufacturing a secondary battery according to this comparative example is different from the method for manufacturing an electrode body by pressing in the secondary battery 1 according to the embodiment of the present technology, and therefore the description of the same configuration as that of the secondary battery 1 according to the embodiment of the present technology will not be repeated.

[0103] FIG. 10 is a schematic diagram showing a state in which an electrode body is produced by pressing a wound body according to a comparative example.

[0104] 10, an electrode body 90 according to the comparative example is formed by a pressing jig 9. The pressing jig 9 includes a first jig 9a and a second jig 9b.

[0105] The first jig 9a has a first head portion 9c. The first head portion 9c has a first press surface F91. The second jig 9b has a second head portion 9d. The second head portion 9d has a second press surface F92. Each of the first head portion 9c and the second head portion 9d is made of, for example, a steel material. Therefore, each of the first press surface F91 and the second press surface F92 is not substantially elastically deformed during the press processing to form the electrode body 90.

[0106] Fig. 11 is a cross-sectional view showing the configuration of an electrode assembly included in a secondary battery according to a comparative example. As shown in Fig. 11, an electrode assembly 90 according to the comparative example includes a positive electrode plate 900, a negative electrode plate 910, and a separator 920. In a flat portion 92, the positive electrode plate 900, the negative electrode plate 910, and the separator 920 are each pressure-bonded.

[0107] In the curved portion 93, a gap G is provided between each of the positive electrode plate 900, the negative electrode plate 910, and the separator 920. As a result, the inter-electrode distance between the positive electrode plate 900 and the negative electrode plate 910 becomes large, and the concentration of lithium increases in the gap G, which may cause lithium to precipitate on the negative electrode plate 910.

[0108] On the other hand, in the electrode body 20 according to the present embodiment, the curved portion 23 is formed by pressing the wound body 20A with the first press surface F1 and the second press surface F2 while elastically deforming the first press surface F1 and the second press surface F2. The curved portion 23 is formed by applying a pressing force of the press process along the shape of the electrode body 20 due to the elastic deformation of the first press surface F1 and the second press surface F2, so that the formation of gaps between the positive electrode plate 200, the negative electrode plate 210, and the separator 220 at the curved portion 23 is suppressed. As a result, the inter-electrode plate distance between the positive electrode plate 200 and the negative electrode plate 210 is appropriately maintained, so that the deposition of lithium at the curved portion 23 is suppressed.

[0109] The manufacturing conditions of the electrode assembly according to the present embodiment and the comparative example and the test results of the battery characteristics are described below. Table 1 shows the adhesive strength between the positive electrode plate and the separator and the battery characteristics when the electrode assembly is pressed under each manufacturing condition in the examples and the comparative example.

[0110] [Table 1]

[0111] As shown in Table 1, the electrode body was produced by changing the press processing conditions when pressing the wound body to produce the electrode body, such as whether or not the wound body was heated, whether or not the wound body was pressed by the elastic part, and the press pressure.

[0112] The adhesive strength of the electrode assemblies produced under the production conditions of each of Experimental Examples 1 to 3 and Comparative Examples 1 and 2 was measured, and the battery characteristics were evaluated. The battery characteristics were evaluated in terms of the impregnation of the electrode assembly with the electrolyte solution and lithium deposition in the electrode assembly.

[0113] The method for evaluating the impregnation of the electrode assembly with the electrolyte was as follows: first, a secondary battery was fabricated to the state before the electrolyte was poured in, and then the electrolyte was poured in. 24 hours, 48 ​​hours, and 72 hours after the electrolyte was poured in, the secondary batteries were disassembled, and the impregnation of the electrolyte between the positive electrode plate and the separator was visually confirmed.

[0114] To evaluate the presence or absence of lithium precipitation in the electrode assembly, a secondary battery containing the electrode assembly was first prepared. Then, the secondary battery was connected to an external power source in a restrained state, and a lithium precipitation durability test was performed in which charge and discharge cycles were repeated.

[0115] The lithium precipitation durability test was conducted under the following test conditions: charging the battery at a current of 37 A for 10 seconds at −30° C. until the battery reached a charge rate of 80%, and then discharging the battery. This charge / discharge cycle was repeated 500 times.

[0116] After the lithium deposition durability test, the secondary battery was disassembled and the state of the electrode body was visually confirmed. Visual inspection was performed on all layers of the laminated electrode body. In the curved part of the electrode body, the first, second, and third layers counting from the outermost circumference were carefully visually checked to see if lithium had been generated.

[0117] As a result of the test, in Examples 1 to 3, the adhesive strength at each measurement point was not too low and not too high. In addition, good results were obtained in terms of impregnation of the electrolyte and lithium deposition.

[0118] In Comparative Example 1, the adhesive strength was comparable to that of Examples 1 to 3. However, in Comparative Example 1, the wound body was not heated during press processing, and the wound body was pressed with high pressure. This resulted in high adhesive strength on the inner circumference side where the electrode body was laminated, and poor impregnation with the electrolyte.

[0119] In Comparative Example 2, since pressing was not performed using an elastic portion, the curved portion was not sufficiently pressed, and it was not possible to ensure the adhesive strength at the curved portion between the positive electrode plate 200 or the negative electrode plate 210 and the separator 220. Furthermore, in Comparative Example 2, although the impregnation of the electrolyte was good, gaps were formed at the curved portion, causing lithium precipitation.

[0120] In the manufacturing method of the secondary battery 1 according to the embodiment of the present technology, the curved portion 23 of the electrode body 20 is formed while the first press surface F1 and the second press surface F2 are elastically deformed, thereby suppressing the increase in the inter-electrode plate distance between the positive electrode plate 200 and the negative electrode plate 210 at the curved portion 23 of the electrode body 20, thereby suppressing the precipitation of lithium. In addition, by heating the curved portion 23 when pressing, the adhesive strength of the outer periphery side of the electrode body 20, which is easily affected by heating, is ensured. As a result, compared to the case where the electrode body 20 is pressed without heating, the adhesive strength between the positive electrode plate 200 or the negative electrode plate 210 on the inside of the electrode body 20 and the separator 220 is not made too high without applying an excessive load to the inner periphery side of the electrode body 20, and the impregnation of the electrolyte can be maintained in a good condition. As a result, the precipitation of lithium inside the electrode body 20 can be suppressed while maintaining the impregnation of the electrolyte into the electrode body 20 in a good condition.

[0121] In the case of a relatively large electrode body, the adhesive strength between the separator and the positive or negative electrode plate on the outer periphery of the electrode body is likely to be low. Therefore, the effect of suppressing lithium precipitation inside the electrode body while ensuring the impregnation of the electrolyte by pressing the electrode body with the elastic part and heating the electrode body during pressing is more effective in the case of a secondary battery equipped with a relatively large electrode body.

[0122] In the manufacturing method of the secondary battery 1 according to the embodiment of the present technology, the curved portion 23 is heated at a temperature of 50° C. or more and 110° C. or less when the curved portion 23 is press-formed. This makes it easier to keep the adhesive strength between the positive electrode plate 200 or the negative electrode plate 210 and the separator 220 in an appropriate range on the outer circumferential side of the curved portion 23, and also makes it easier to maintain good impregnation with the electrolyte by preventing the adhesive strength between the positive electrode plate 200 or the negative electrode plate 210 and the separator 220 on the inner side of the electrode body 20 from being too high.

[0123] In the manufacturing method of the secondary battery 1 according to the embodiment of the present technology, the first press surface F1 and the second press surface F2 are in contact with the outer surface of 50% or more of the region that will become the first curved portion 24 and the second curved portion 25 after the wound body 20A is pressed. This allows the shape of the curved portion 23 to be formed uniformly compared to the case where the curved portion 23 is pressed locally, making it easier to obtain the required adhesive strength between the positive electrode plate 200 or the negative electrode plate 210 and the separator 220. In addition, the contact area of ​​the first press surface F1 and the second press surface F2 with the curved portion 23 can be increased, making it easier for heat generated by heating to be transmitted from the press jig 2 to the curved portion 23.

[0124] In a manufacturing method of a secondary battery 1 according to one embodiment of the present technology, by constructing each of the first elastic portion 7 and the second elastic portion 8 from a porous material, it is possible to provide a configuration that makes it easy to obtain the elastic modulus of the first press surface F1 and the second press surface F2 required to form the curved portion 23.

[0125] In the secondary battery 1 according to the embodiment of the present technology, in the first curved portion 24, the adhesive strength between the surface of each of the positive electrode plates 200 up to the third layer counting from the positive electrode plate 200 located at the outermost periphery among the stacked positive electrode plates 200 and each separator 220 adjacent to the outer periphery side is 1.0 N / m or more and 1.9 N / m or less. Also, in the first curved portion 24, the adhesive strength between the surface of the positive electrode plate 200 located on the outer periphery side by 50% of the total number of stacked positive electrode plates 200 counting from the positive electrode plate 200 located at the innermost periphery among the stacked positive electrode plates 200 and each separator 220 adjacent to the outer periphery side is 0.6 N / m or more and 1.5 N / m or less. As a result, the adhesive strength between the positive electrode plate 200 and the separator 220 can be set to an appropriate range in the vicinity of the outermost periphery of the first curved portion 24, so that the inter-electrode plate distance between the positive electrode plate 200 and the negative electrode plate 210 can be normally maintained. As a result, the impregnation of the electrolyte in the curved portion 23 can be kept good, and deposition of lithium in the curved portion 23 can be suppressed.

[0126] In the secondary battery 1 according to an embodiment of the present technology, in the flat portion 22, the adhesive strength between the surface of each of the positive electrode plates 200 from the positive electrode plate 200 located at the outermost periphery to the third layer among the stacked positive electrode plates 200 and each separator 220 adjacent to the outer periphery side is 1.5 N / m or more and 1.9 N / m or less. This ensures a necessary adhesive strength in the outer periphery of the flat portion 22 and prevents the plate distance between the positive electrode plate 200 and the negative electrode plate 210 from increasing, so that the impregnation of the electrolyte in the flat portion 22 can be well maintained while suppressing the deposition of lithium.

[0127] In the secondary battery 1 according to an embodiment of the present technology, in the flat portion 22, the adhesive strength between the surface of the positive plate 200 located on the outer periphery side for 50% of the total number of stacked positive plates 200 counting from the innermost positive plate 200 among the stacked positive plate 200 and the separator 220 adjacent to the outer periphery side is 1.5 N / m or more and 1.9 N / m or less. This ensures the necessary adhesive strength in the inner peripheral part of the flat portion 22 and prevents the plate distance between the positive plate 200 and the negative plate 210 from widening, so that the impregnation of the electrolyte in the flat portion 22 can be maintained well while suppressing lithium precipitation.

[0128] Although the embodiment of the present technology has been described above, the embodiment disclosed herein should be considered as illustrative and not restrictive in all respects. The scope of the present technology is defined by the claims, and it is intended to include all modifications within the scope and meaning equivalent to the claims. [Explanation of symbols]

[0129] 1 secondary battery, 2, 9 pressing tool, 3, 9a first tool, 4, 9b second tool, 5, 9c first head portion, 6, 9d second head portion, 7 first elastic portion, 8 second elastic portion, 10 case, 20, 90 electrode body, 20A winding body, 21 tab portion, 22, 22a, 22b, 92 flat portion, 23, 93 curved portion, 24 first curved portion, 25 second curved portion, 30 positive electrode collector, 40 negative electrode collector, 50 positive electrode terminal, 60 negative electrode terminal, 70 positive electrode external conductive member, 80 negative electrode external conductive member, 100 outer casing, 101 opening, 102 bottom, 103a, 103b first side wall, 104a, 104b second side wall, 110 sealing plate, 111 liquid injection hole, 112 Sealing member, 113 gas exhaust valve, 200,900 positive electrode plate, 201 positive electrode tab group, 210,910 negative electrode plate, 211 negative electrode tab group, 220,920 separator, 240 first outer portion, 241 first inner portion, 250 second outer portion, 251 second inner portion, A1 winding shaft, F1,F91 first press surface, F2,F92 second press surface.

Claims

1. preparing a wound body in which a separator is sandwiched between a positive electrode plate and a negative electrode plate, and the positive electrode plate, the negative electrode plate, and the separator are wound around a winding axis that is aligned in a first direction; a step of sandwiching the wound body between a first jig having a first press surface including a first elastic portion and a second jig having a second press surface including a second elastic portion in a second direction perpendicular to the first direction, and pressing the wound body with the first press surface and the second press surface while elastically deforming at least a portion of the first press surface and the second press surface to produce an electrode body by pressing the wound body into a flat shape; and housing the electrode body and the electrolyte in a case. In a step of producing the electrode body by pressing the wound body, a flat portion is formed in the electrode body, the flat portion being located on a central side in a third direction perpendicular to the first direction and the second direction and having a flat outer surface, a first curved portion is located on one end side of the flat portion in the third direction and having a curved outer surface, and a second curved portion is located on the other end side of the flat portion in the third direction and having a curved outer surface, a step of pressing the wound body to produce the electrode body, wherein each of the first curved portion and the second curved portion is heated to a temperature higher than room temperature via at least one of the first press surface and the second press surface.

2. The method for producing a secondary battery according to claim 1 , wherein the temperature higher than room temperature is 50° C. or higher and 110° C. or lower.

3. 3. The method for manufacturing a secondary battery according to claim 1, wherein the first press surface and the second press surface abut against the outer surface of 50% or more of an area that will become the first curved portion and the second curved portion after the wound body is pressed.

4. 3. The method for manufacturing a secondary battery according to claim 1, wherein each of the first elastic portion and the second elastic portion is made of a porous material.

5. an electrode assembly in which a separator is sandwiched between a positive electrode plate and a negative electrode plate, and the positive electrode plate, the negative electrode plate, and the separator are wound around a winding axis that is aligned in a first direction; A case is provided to accommodate the electrode assembly and an electrolyte solution, the electrode body is flat and has a short side in a second direction perpendicular to the first direction and a long side in a third direction perpendicular to the first direction and the second direction; The electrode body is a flat portion located on the central side in the third direction and having a flat outer surface; a first curved portion located on one end side of the flat portion in the third direction and having a curved outer surface; a second curved portion located on the other end side of the flat portion in the third direction and having a curved outer surface, In the first curved portion, an adhesive strength between a surface of each of the positive electrode plates from the outermost positive electrode plate to a third layer counting from the outermost positive electrode plate among the stacked positive electrode plates and each of the separators adjacent to the outer periphery side is 1.0 N / m or more and 1.9 N / m or less, a first curved portion of the positive plate that is located on the outer periphery side of the positive plate and that corresponds to 50% of the total number of stacked positive plates, counting from the innermost positive plate, and an adhesive strength between the surface of the positive plate and the separator adjacent to that outer periphery is 0.6 N / m or more and 1.5 N / m or less.

6. 6. The secondary battery according to claim 5, wherein in the flat portion, an adhesive strength between a surface of each of the positive electrode plates in the first to third layers counting from the outermost positive electrode plate among the stacked positive electrode plates and each of the separators adjacent to the outer periphery side thereof is 1.5 N / m or more and 1.9 N / m or less.

7. 7. The secondary battery according to claim 5, wherein in the flat portion, an adhesive strength between a surface of the positive plate located on the outer periphery side for 50% of a total number of stacked positive plate layers counting from an innermost positive plate among the stacked positive plate layers and the separator adjacent to that outer periphery side is 1.5 N / m or more and 1.9 N / m or less.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    JP2002260663A

  • Flat nonaqueous electrolyte secondary battery and manufacturing method therefor

    JP2004362968A

  • Nonaqueous electrolyte secondary battery

    JP2005285372A

  • Method and device for manufacturing lithium secondary battery, and lithium secondary battery

    JP2009054376A

  • Method of manufacturing sealed battery

    JP2011258493A